Method for manufacturing semiconductor device having dolmen structure, method for manufacturing support piece, and laminate film for support piece formation
Patent Information
- Application Number
- MYPI2021005377
- Authority / Receiving Office
- MY · MY
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-04-25
- Publication Date
- 2026-02-25
- Estimated Expiration
- 2039-04-25
AI Technical Summary
The existing methods for manufacturing semiconductor devices with a dolmen structure are complex and costly, requiring multiple steps and using expensive semiconductor wafers as support pieces, which complicates the process and increases costs.
A method involving a laminated film with a base film, an adhesive layer, and a thermosetting resin layer is used to form support pieces, which are then divided and arranged around a first chip, simplifying the process and eliminating the need for semiconductor wafers, with the thermosetting resin layer providing stability and adhesion.
This approach simplifies the manufacturing process, reduces costs by eliminating the use of expensive semiconductor wafers, and ensures stable support for stacked semiconductor chips with improved shear viscosity and adhesion properties.
Smart Images

Figure PI2021005377_DRAWING_001 
Figure PI2021005377_DRAWING_002 
Figure PI2021005377_DRAWING_003
Abstract
Description
Manufacturing method for semiconductor device having dolmen structure, manufacturing method for support piece, and laminated film for forming support piece
[0001] The present disclosure relates to a method for manufacturing a semiconductor device having a dolmen structure including a substrate, a first chip arranged on the substrate, a plurality of support pieces arranged on the substrate around the first chip, and a second chip supported by the plurality of support pieces and arranged to cover the first chip. The present disclosure also relates to a method for manufacturing a support piece and a laminated film for forming the support piece. A dolmen is a type of stone tomb, comprising a plurality of supporting stones and a slab-shaped rock placed on top of the supporting stones. In a semiconductor device having a dolmen structure, the supporting pieces correspond to the "pillar stones" and the second chip corresponds to the "slab-shaped rock."
[0002] In recent years, there has been a demand for higher integration, smaller size, and faster speeds in the field of semiconductor devices. As one aspect of semiconductor devices, a structure in which a semiconductor chip is stacked on a controller chip disposed on a substrate has attracted attention. For example, Patent Document 1 (Patent Document 1) discloses a semiconductor die assembly including a controller die and a memory die supported by a support member on the controller die. The semiconductor assembly 100 shown in FIG. 1A of Patent Document 1 can be said to have a dolmen structure. That is, the semiconductor assembly 100 includes a package substrate 102, a controller die 103 disposed on its surface, memory dies 106a and 106b disposed above the controller die 103, and support members 130a and 130b supporting the memory die 106a.
[0003] Special table 2017-515306 publication
[0004] Patent Document 1 discloses that semiconductor materials such as silicon can be used as the support member (support piece), and more specifically, that fragments of semiconductor material obtained by dicing a semiconductor wafer can be used (see
[0012] ,
[0014] and FIG. 2 of Patent Document 1). To manufacture a support piece for a dolmen structure using a semiconductor chip, the following steps are required, similar to the manufacture of a normal semiconductor chip: (1) a step of attaching a backgrinding tape to the semiconductor wafer; (2) a step of backgrinding the semiconductor wafer; (3) a step of attaching a film having an adhesive layer and an adhesive layer (a dicing / die bonding integrated film) to a dicing ring and the backgrinded semiconductor wafer placed therein; (4) a step of peeling the backgrinding tape from the semiconductor wafer; (5) a step of dividing the semiconductor wafer; and (6) a step of picking up the support piece, which is a stack of semiconductor chips and adhesive pieces, from the adhesive layer.
[0005] The present disclosure provides a method for manufacturing a semiconductor device that can simplify the process of fabricating support pieces in a manufacturing process of a semiconductor device having a dolmen structure and can stably support stacked semiconductor chips. The present disclosure also provides a method for manufacturing the support pieces and a laminated film for forming the support pieces.
[0006] One aspect of the present disclosure relates to a method for manufacturing a semiconductor device having a dolmen structure including a substrate, a first chip arranged on the substrate, a plurality of support pieces arranged on the substrate around the first chip, and a second chip supported by the plurality of support pieces and arranged to cover the first chip. The method for manufacturing the semiconductor device includes the following steps: (A) preparing a laminated film including, in this order, a base film, an adhesive layer, and a support piece-forming film; (B) forming a plurality of support pieces on the surface of the adhesive layer by dividing the support piece-forming film; (C) picking up the support pieces from the adhesive layer; (D) arranging the first chip on the substrate; (E) arranging a plurality of support pieces on the substrate around the first chip; (F) preparing a chip with adhesive pieces including a second chip and an adhesive piece provided on one side of the second chip; and (G) constructing the dolmen structure by arranging the chip with adhesive pieces on the surfaces of the plurality of support pieces.
[0007] According to a semiconductor device manufacturing method according to one aspect of the present disclosure, support pieces can be obtained by singulating a support piece-forming film. This simplifies the process of producing the support pieces compared to conventional manufacturing methods that use fragments of semiconductor material obtained by dicing a semiconductor wafer as the support pieces. In other words, while conventional methods required the above-described steps (1) to (6), the support piece-forming film does not include a semiconductor wafer, so steps (1), (2), and (4) related to back-grinding the semiconductor wafer can be omitted. Furthermore, because semiconductor wafers, which are more expensive than resin materials, are not used, costs can be reduced.
[0008] The support piece-forming film has a shear viscosity of 4000 Pa·s or more at 120°C. When the support piece-forming film has a shear viscosity of 4000 Pa·s or more at 120°C, the support piece-forming film is less susceptible to flow deformation, and as a result, the support piece-forming film can stably support the stacked semiconductor chips. The support piece-forming film may include a thermosetting resin layer.
[0009] The adhesive layer of the laminated film prepared in step (A) may be pressure-sensitive or UV-curable. That is, the adhesive layer may or may not be cured by UV irradiation; in other words, it may or may not contain a resin having a photoreactive carbon-carbon double bond. The pressure-sensitive adhesive layer may contain a resin having a photoreactive carbon-carbon double bond. For example, the adhesive layer may have its adhesiveness reduced by irradiating a predetermined region with UV light; for example, the resin having a photoreactive carbon-carbon double bond may remain in that region. When the adhesive layer is UV-curable, the adhesive layer's adhesiveness can be reduced by irradiating the adhesive layer with UV light between steps (B) and (C).
[0010] When the support piece-forming film includes a thermosetting resin layer, the step of heating the support piece-forming film or the support piece to harden the thermosetting resin layer or adhesive piece can be performed at an appropriate time, for example, before step (G). In the stage of arranging chips with adhesive pieces so that they contact the surfaces of the multiple support pieces, the thermosetting resin layer has already hardened, which can prevent the support pieces from deforming due to the placement of the chips with adhesive pieces. Note that, because the thermosetting resin layer has adhesive properties to other components (e.g., substrates), it is not necessary to provide a separate adhesive layer or the like on the support pieces.
[0011] The thickness of the support piece-forming film may be, for example, 5 to 180 μm or 20 to 120 μm. By having the thickness of the support piece-forming film within this range, a dolmen structure of appropriate height can be constructed for the first chip (e.g., controller chip). The support piece-forming film may include a thermosetting resin layer. The thermosetting resin layer preferably includes, for example, an epoxy resin and an elastomer. By including an elastomer in the thermosetting resin layer constituting the support piece, stress within the semiconductor device can be alleviated.
[0012] One aspect of the present disclosure relates to a method for manufacturing a support piece used in a manufacturing process of a semiconductor device having a dolmen structure. The method includes the following steps: (A) preparing a laminated film including, in this order, a base film, an adhesive layer, and a support piece-forming film; (B) forming a plurality of support pieces on the surface of the adhesive layer by dividing the support piece-forming film; and (C) picking up the support pieces from the adhesive layer. The shear viscosity of the support piece-forming film at 120°C is 4000 Pa s or more.
[0013] One aspect of the present disclosure relates to a support piece-forming laminate film used in a manufacturing process for a semiconductor device having a dolmen structure including a substrate, a first chip disposed on the substrate, a plurality of support pieces disposed on the substrate around the first chip, and a second chip supported by the plurality of support pieces and disposed so as to cover the first chip, the support piece-forming laminate film including, in this order, a base film, an adhesive layer, and a support piece-forming film, the support piece-forming film having a shear viscosity of 4000 Pa s or more at 120°C. The support piece-forming film may include a thermosetting resin layer.
[0014] According to the present disclosure, a method for manufacturing a semiconductor device that can simplify the process of manufacturing a support piece in a manufacturing process of a semiconductor device having a dolmen structure and that can stably support stacked semiconductor chips is provided. Also, according to the present disclosure, a method for manufacturing a support piece and a laminated film for forming the support piece are provided.
[0015] FIG. 1 is a cross-sectional view schematically illustrating a first embodiment of a semiconductor device. FIGS. 2(a), 2(b), and 2(c) are plan views schematically illustrating an example of the positional relationship between a first chip and multiple support pieces. FIG. 3(a) is a plan view schematically illustrating one embodiment of a support piece-forming laminate film, and FIG. 3(b) is a cross-sectional view taken along line b-b in FIG. 3(a). FIG. 4 is a cross-sectional view schematically illustrating a process of bonding an adhesive layer and a support piece-forming film. FIGS. 5(a), 5(b), 5(c), and 5(d) are cross-sectional views schematically illustrating a support piece fabrication process. FIG. 6 is a cross-sectional view schematically illustrating a state in which multiple support pieces are arranged around a first chip on a substrate. FIG. 7 is a cross-sectional view schematically illustrating an example of a chip with adhesive pieces attached. FIG. 8 is a cross-sectional view schematically illustrating a dolmen structure formed on a substrate. FIG. 9 is a cross-sectional view schematically illustrating a second embodiment of a semiconductor device. Figure 10(a) is a top view showing an example of a substrate with support pieces used in the examples, Figure 10(b) is a cross-sectional view taken along line b-b in Figure 10(a), and Figure 10(c) is a cross-sectional view showing an example of a laminate used in the examples.
[0016] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings. However, the present invention is not limited to the following embodiments. In this specification, "(meth)acrylic acid" means acrylic acid or methacrylic acid, and "(meth)acrylate" means acrylate or the corresponding methacrylate. "A or B" may include either A or B, or may include both.
[0017] In this specification, the term "layer" encompasses not only a structure with a shape formed over the entire surface when observed in a plan view, but also a structure with a shape formed on a portion of the surface. Furthermore, in this specification, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the intended effect of the process is achieved. Furthermore, a numerical range indicated using "to" indicates a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively.
[0018] In this specification, the content of each component in a composition refers to the total amount of the components present in the composition unless otherwise specified, when the composition contains multiple substances corresponding to each component. Furthermore, unless otherwise specified, the exemplified materials may be used alone or in combination of two or more. Furthermore, in the numerical ranges described in stages in this specification, the upper or lower limit of a certain numerical range may be replaced with the upper or lower limit of another numerical range. Furthermore, in the numerical ranges described in this specification, the upper or lower limit of that numerical range may be replaced with the value shown in the examples.
[0019] 1 is a cross-sectional view schematically illustrating a first embodiment of a semiconductor device. The semiconductor device 100 shown in FIG. 1 includes a substrate 10, a chip T1 (first chip) disposed on the surface of the substrate 10, a plurality of support pieces Dc disposed around the chip T1 on the surface of the substrate 10, a chip T2 (second chip) disposed above the chip T1, an adhesive piece Tc sandwiched between the chip T2 and the plurality of support pieces Dc, chips T3 and T4 stacked on the chip T2, a plurality of wires w electrically connecting electrodes (not shown) on the surface of the substrate 10 to the chips T1 to T4, and a sealant 50 filled in gaps between the chips T1 and T2.
[0020] In this embodiment, a dolmen structure is formed on the substrate 10 by a plurality of support pieces Dc, chips T2, and adhesive pieces Tc located between the support pieces Dc and chips T2. The chips T1 are spaced apart from the adhesive pieces Tc. By appropriately setting the thickness of the support pieces Dc, it is possible to ensure space for the wires w that connect the upper surfaces of the chips T1 to the substrate 10.
[0021] The substrate 10 may be an organic substrate or a metal substrate such as a lead frame. From the viewpoint of suppressing warpage of the semiconductor device 100, the thickness of the substrate 10 is, for example, 90 to 300 μm, and may be 90 to 210 μm.
[0022] The chip T1 is, for example, a controller chip, and is adhered to the substrate 10 by an adhesive piece Tc and electrically connected to the substrate 10 by a wire w. The shape of the chip T1 in a plan view is, for example, rectangular (square or oblong). The length of one side of the chip T1 is, for example, 5 mm or less, and may be 2 to 5 mm or 1 to 5 mm. The thickness of the chip T1 is, for example, 10 to 150 μm, and may be 20 to 100 μm.
[0023] The chip T2 is, for example, a memory chip and is adhered onto the support piece Dc via an adhesive piece Tc. In a plan view, the chip T2 is larger than the chip T1. In a plan view, the shape of the chip T2 is, for example, rectangular (square or oblong). The length of one side of the chip T2 is, for example, 20 mm or less, and may be 4 to 20 mm or 4 to 12 mm. The thickness of the chip T2 is, for example, 10 to 170 μm, and may be 20 to 120 μm. The chips T3 and T4 are also, for example, memory chips and are adhered onto the chip T2 via an adhesive piece Tc. The length of one side of the chips T3 and T4 may be the same as that of the chip T2, and the thickness of the chips T3 and T4 may also be the same as that of the chip T2.
[0024] The support pieces Dc serve as spacers that form a space around the chip T1. The support pieces Dc include a cured product of the support piece-forming film (a cured product of a thermosetting resin composition). The shear viscosity of the support piece-forming film at 120°C is 4000 Pa·s or greater, as described below. As shown in FIG. 2(a), two support pieces Dc (rectangular in shape) may be arranged at separate positions on both sides of the chip T1. As shown in FIG. 2(b), one support piece Dc (square in shape, four in total) may be arranged at each position corresponding to a corner of the chip T1. As shown in FIG. 2(c), one support piece Dc (rectangular in shape, four in total) may be arranged at each position corresponding to a side of the chip T1. The length of one side of the support pieces Dc in a planar view is, for example, 20 mm or less, and may be 1 to 20 mm or 1 to 12 mm. The thickness (height) of the support pieces Dc is, for example, 10 to 180 μm, and may be 20 to 120 μm.
[0025] (Method for manufacturing support piece) An example of a method for manufacturing a support piece will be described. The manufacturing method according to this embodiment includes the following steps (A) to (C). (A) A step of preparing a laminate film 20 for forming a support piece (hereinafter sometimes referred to as "laminate film 20") including a base film 1, an adhesive layer 2, and a film D for forming a support piece in this order (see FIGS. 3 and 4). (B) A step of forming a plurality of support pieces Da on the surface of the adhesive layer 2 by dividing the film D for forming a support piece (see FIG. 5(b)). (C) A step of picking up the support pieces Da from the adhesive layer 2 (see FIG. 5(d)).
[0026] The support piece Dc shown in Fig. 1 is in a state where the adhesive piece (thermosetting resin composition) contained therein has hardened, while the support piece Da is in a state where the adhesive piece (thermosetting resin composition) contained therein has not yet completely hardened (see, for example, Fig. 5(b)).
[0027] Steps (A) to (C) are a process for manufacturing a plurality of support pieces Da. Steps (A) to (C) will be described below with reference to FIGS.
[0028] [Step (A)] Step (A) is a step of preparing a laminate film 20. The laminate film 20 includes a base film 1, an adhesive layer 2, and a support piece-forming film D. The base film 1 is, for example, a polyethylene terephthalate (PET) film. The adhesive layer 2 is formed into a circular shape by punching or the like (see FIG. 3(a)). The adhesive layer 2 may be made of a pressure-sensitive adhesive or an ultraviolet-curing adhesive. When the adhesive layer 2 is made of an ultraviolet-curing adhesive, the adhesive layer 2 has the property of decreasing in adhesiveness when irradiated with ultraviolet light. The support piece-forming film D is formed into a circular shape by punching or the like and has a smaller diameter than the adhesive layer 2 (see FIG. 3(a)). The support piece-forming film D may include a thermosetting resin layer 5 made of a thermosetting resin composition.
[0029] The thermosetting resin composition constituting the thermosetting resin layer 5 in the support piece-forming film D can go through a semi-cured (B-stage) state and then become a fully cured (C-stage) state by a subsequent curing treatment. The thermosetting resin composition contains an epoxy resin, a curing agent, and an elastomer (e.g., an acrylic resin) because the shear viscosity can be easily adjusted to a predetermined range, and may further contain an inorganic filler, a curing accelerator, etc., as necessary. Details of the thermosetting resin composition constituting the thermosetting resin layer 5 in the support piece-forming film D will be described later.
[0030] The thickness of the support piece forming film D may be, for example, 5 to 180 μm or 20 to 120 μm. When the thickness of the support piece forming film is in this range, a dolmen structure of an appropriate height can be constructed for the first chip (for example, the controller chip).
[0031] The shear viscosity of the support piece forming film D at 120°C is 4000 Pa·s or more. The shear viscosity of the support piece forming film D at 120°C may be 4500 Pa·s or more, 5000 Pa·s or more, 7000 Pa·s or more, 10000 Pa·s or more, 15000 Pa·s or more, 18000 Pa·s or more, 20000 Pa·s or more, or 23000 Pa·s or more. When the shear viscosity of the support piece forming film D at 120°C is 4000 Pa·s or more, the degree of flow deformation of the support piece forming film is reduced, and as a result, the support stability of the semiconductor chip can be improved. The upper limit of the shear viscosity of the support piece-forming film D at 120°C is not particularly limited, but may be 100,000 Pa s or less, 70,000 Pa s or less, or 50,000 Pa s or less. The shear viscosity of the support piece-forming film D at 120°C can be adjusted, for example, by appropriately adjusting the types and contents of the components contained in the thermosetting resin composition described below.
[0032] The laminate film 20 can be produced, for example, by bonding a first laminate film having a base film 1 and an adhesive layer 2 on its surface with a second laminate film having a cover film 3 and a support piece-forming film D on its surface (see FIG. 4). The first laminate film is obtained through a process of forming an adhesive layer on the surface of the base film 1 by coating, and processing the adhesive layer into a predetermined shape (e.g., circular) by punching or the like. The second laminate film is obtained through a process of forming a support piece-forming film on the surface of a cover film 3 (e.g., a PET film or polyethylene film) by coating, and processing the support piece-forming film into a predetermined shape (e.g., circular) by punching or the like. When using the laminate film 20, the cover film 3 is peeled off at an appropriate time.
[0033] [Step (B)] Step (B) is a step of forming a plurality of support pieces Da on the surface of the adhesive layer 2 by dividing the support piece-forming film D. As shown in FIG. 5( a), a dicing ring DR is attached to the laminate film 20. That is, the dicing ring DR is attached to the adhesive layer 2 of the laminate film 20, and the support piece-forming film D is arranged inside the dicing ring DR. The support piece-forming film D is divided into individual pieces by dicing (see FIG. 5( b)). As a result, a large number of support pieces Da are obtained from the support piece-forming film D.
[0034] [Step (C)] Step (C) is a step of picking up the support pieces Da from the adhesive layer 2. As shown in Fig. 5(c), the base film 1 is expanded to separate the support pieces Da from each other. Next, as shown in Fig. 5(d), the support pieces Da are pushed up by a push-up jig 42 to peel the support pieces Da from the adhesive layer 2, and the support pieces Da are picked up by suction with a suction collet 44.
[0035] (Method for Manufacturing Semiconductor Device) A method for manufacturing the semiconductor device 100 will be described. The manufacturing method according to this embodiment includes steps (A) to (C) and further includes the following steps (D) to (H): (D) a step of arranging a first chip T1 on the substrate 10; (E) a step of arranging a plurality of support pieces Da (support pieces Da including at least metal pieces 6p) obtained by the above manufacturing method around the first chip T1 on the substrate 10 (see FIG. 6); (F) a step of preparing a chip with adhesive pieces T2a including a second chip T2 and an adhesive piece Ta provided on one surface of the second chip T2 (see FIG. 7); (G) a step of constructing a dolmen structure by arranging the chip with adhesive pieces T2a on the surfaces of a plurality of support pieces Dc (see FIG. 8); and (H) a step of sealing gaps between the chips T1 and T2 with a sealant 50 (see FIG. 1).
[0036] Steps (D) to (H) are processes in which a dolmen structure is constructed on the substrate 10 using a plurality of support pieces Da. Steps (D) to (H) will be described below with reference to FIGS. 6 to 8.
[0037] [Step (D)] Step (D) is a step of placing a first chip T1 on the substrate 10. For example, first, the chip T1 is placed at a predetermined position on the substrate 10 via an adhesive layer T1c. Thereafter, the chip T1 is electrically connected to the substrate 10 by a wire w.
[0038] [Step (E)] Step (E) is a step of arranging multiple support pieces Da on the substrate 10 around the first chip T1. Through this step, the structure 30 shown in FIG. 6 is produced. The structure 30 includes the substrate 10, the chip T1 arranged on its surface, and multiple support pieces Da. The support pieces Da may be arranged by a pressure bonding process. The pressure bonding process is preferably performed, for example, under conditions of 80 to 180°C, 0.01 to 0.50 MPa, and for 0.5 to 3.0 seconds. The adhesive pieces 5p contained in the support pieces Da may be completely cured to become support pieces Dc at the time of step (E), or may not be completely cured at this time. It is preferable that the adhesive pieces 5p contained in the support pieces Da be completely cured to become adhesive pieces 5c before the start of step (G).
[0039] [Step (F)] Step (F) is a step of preparing the chip T2a with adhesive pieces shown in Figure 7. The chip T2a with adhesive pieces includes the chip T2 and an adhesive piece Ta provided on one surface of the chip T2. The chip T2a with adhesive pieces can be obtained, for example, by using a semiconductor wafer and a dicing / die bonding integrated film through a dicing step and a pick-up step.
[0040] [Step (G)] Step (G) is a step of placing the adhesive-piece-attached chip T2a above the chip T1 so that the adhesive pieces Ta contact the upper surfaces of the multiple support pieces Dc. Specifically, the chip T2 is pressure-bonded to the upper surfaces of the support pieces Dc via the adhesive pieces Ta. This pressure-bonding process is preferably carried out, for example, at 80 to 180°C and 0.01 to 0.50 MPa for 0.5 to 3.0 seconds. Next, the adhesive pieces Ta are hardened by heating. This hardening process is preferably carried out, for example, at 60 to 175°C and 0.01 to 1.0 MPa for 5 minutes or more. As a result, the adhesive pieces Ta harden and become adhesive pieces Tc. Through this process, a dolmen structure is constructed on the substrate 10 (see Figure 8).
[0041] After step (G) and before step (H), chip T3 is placed on chip T2 via an adhesive strip, and chip T4 is then placed on chip T3 via an adhesive strip. The adhesive strip may be a thermosetting resin composition similar to the adhesive strip Ta described above, and becomes adhesive strip Tc upon heat curing (see FIG. 1). Meanwhile, chips T2, T3, and T4 are electrically connected to substrate 10 via wires w. Note that the number of chips stacked above chip T1 is not limited to three as in this embodiment and may be set as appropriate.
[0042] [Step (H)] Step (H) is a step of sealing the gap between the chip T1 and the chip T2 with the sealing material 50. Through this step, the semiconductor device 100 shown in FIG.
[0043] (Thermosetting Resin Composition) As described above, the thermosetting resin composition constituting the thermosetting resin layer 5 in the support piece-forming film D contains an epoxy resin, a curing agent, and an elastomer, because the shear viscosity can be easily adjusted to a predetermined range, and may further contain an inorganic filler, a curing accelerator, etc., as necessary. According to the studies of the present inventors, it is preferable that the support piece Da and the support piece Dc after curing further have the following properties. - Property 1: When the support piece Da is thermocompression bonded to a predetermined position on the substrate 10, misalignment is unlikely to occur. - Property 2: The adhesive piece 5c exhibits stress relaxation properties within the semiconductor device 100 (the thermosetting resin composition contains an elastomer (rubber component)). - Property 3: The adhesive strength of the chip with the adhesive piece to the adhesive piece Tc is sufficiently high (the die shear strength (shear strength) of the adhesive piece 5c (i.e., the cured product of the film made of the thermosetting resin layer) to the adhesive piece Tc is, for example, 2.0 to 7.0 MPa or 3.0 to 6.0 MPa). - Property 4: The shrinkage rate associated with curing is sufficiently small. - Property 5: The support piece Da is easily visible by camera in the pick-up process (the thermosetting resin composition contains, for example, a colorant). - Property 6: The adhesive piece 5c has sufficient mechanical strength.
[0044] [Epoxy Resin] The epoxy resin is not particularly limited as long as it has adhesive properties upon curing. Bifunctional epoxy resins such as bisphenol A epoxy resin, bisphenol F epoxy resin, and bisphenol S epoxy resin, as well as novolac epoxy resins such as phenol novolac epoxy resin and cresol novolac epoxy resin, can be used. Also applicable are commonly known epoxy resins such as multifunctional epoxy resins, glycidylamine epoxy resins, heterocycle-containing epoxy resins, and alicyclic epoxy resins. These may be used alone or in combination of two or more.
[0045] [Curing Agent] Examples of curing agents include phenolic resins, ester compounds, aromatic amines, aliphatic amines, acid anhydrides, and the like. Among these, phenolic resins are preferred from the viewpoint of achieving high die shear strength (shear strength). Commercially available phenolic resins include, for example, LF-4871 (trade name, BPA novolac phenolic resin) manufactured by DIC Corporation, HE-100C-30 (trade name, phenylarakyl phenolic resin) manufactured by Air Water Inc., Phenolite KA and TD series manufactured by DIC Corporation, Milex XLC-series and XL series (e.g., Milex XLC-LL) manufactured by Mitsui Chemicals, Inc., HE series (e.g., HE100C-30) manufactured by Air Water Inc., MEHC-7800 series (e.g., MEHC-7800-4S) manufactured by Meiwa Kasei Co., Ltd., JDPP series manufactured by JEF Chemical Co., Ltd., and PSM series (e.g., PSM-4326) manufactured by Gun-ei Chemical Industry Co., Ltd. These may be used alone or in combination of two or more.
[0046] From the viewpoint of achieving high die shear strength (shear strength), the blending amounts of the epoxy resin and phenolic resin are preferably such that the equivalent ratio of the epoxy equivalent to the hydroxyl equivalent is 0.6 to 1.5, more preferably 0.7 to 1.4, and even more preferably 0.8 to 1.3. By keeping the blending ratio within the above range, it is easy to achieve sufficiently high levels of both curability and fluidity.
[0047] [Elastomer] Examples of the elastomer include acrylic resin, polyester resin, polyamide resin, polyimide resin, silicone resin, polybutadiene, acrylonitrile, epoxy-modified polybutadiene, maleic anhydride-modified polybutadiene, phenol-modified polybutadiene, and carboxy-modified acrylonitrile.
[0048] From the viewpoint of film formability, acrylic resins are preferred as elastomers, and more preferred are acrylic resins such as epoxy group-containing (meth)acrylic copolymers obtained by polymerizing functional monomers having epoxy or glycidyl groups as crosslinkable functional groups, such as glycidyl acrylate or glycidyl methacrylate. Among acrylic resins, epoxy group-containing (meth)acrylic acid ester copolymers and epoxy group-containing acrylic rubbers are preferred, and epoxy group-containing acrylic rubbers are more preferred. Epoxy group-containing acrylic rubbers are rubbers containing epoxy groups, primarily consisting of acrylic acid esters as the main component, such as copolymers of butyl acrylate and acrylonitrile, or copolymers of ethyl acrylate and acrylonitrile. The acrylic resins may contain not only epoxy groups but also crosslinkable functional groups such as alcoholic or phenolic hydroxyl groups and carboxyl groups.
[0049] Commercially available acrylic resins include SG-70L, SG-708-6, WS-023 EK30, SG-280 EK23, and SG-P3 solvent-modified product (trade name, acrylic rubber, weight-average molecular weight: 800,000, Tg: 12°C, solvent: cyclohexanone), all manufactured by Nagase ChemteX Corporation, and SG-P3 low molecular weight product (trade name, acrylic rubber, weight-average molecular weight: 300,000, Tg: 12°C, solvent: cyclohexanone).
[0050] From the viewpoint of film formability, the glass transition temperature (Tg) of the acrylic resin is preferably -50 to 50°C, more preferably -30 to 30°C. From the viewpoint of film formability, the weight average molecular weight (Mw) of the acrylic resin is preferably 100,000 to 3,000,000, more preferably 500,000 to 2,000,000. Here, Mw refers to a value measured by gel permeation chromatography (GPC) and converted using a calibration curve based on standard polystyrene. Note that the use of an acrylic resin with a narrow molecular weight distribution tends to enable the formation of highly elastic adhesive pieces.
[0051] From the viewpoint of achieving high die shear strength (shear strength), the amount of the acrylic resin contained in the thermosetting resin composition is preferably 10 to 200 parts by mass, and more preferably 20 to 100 parts by mass, per 100 parts by mass of the epoxy resin and the epoxy resin curing agent in total.
[0052] From the viewpoint of achieving a high shear viscosity, the amount of the acrylic resin contained in the thermosetting resin composition is preferably 50 parts by mass or more per 100 parts by mass of the epoxy resin and the epoxy resin curing agent combined.
[0053] [Inorganic Filler] Examples of inorganic fillers include aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whisker, boron nitride, crystalline silica, amorphous silica, etc. These may be used alone or in combination of two or more.
[0054] The average particle size of the inorganic filler is preferably 0.005 μm to 1.0 μm, more preferably 0.05 to 0.5 μm, from the viewpoint of achieving high die shear strength (shear strength). The surface of the inorganic filler is preferably chemically modified from the viewpoint of achieving high die shear strength (shear strength). Examples of materials for chemically modifying the surface include silane coupling agents. Examples of types of functional groups of silane coupling agents include vinyl groups, acryloyl groups, epoxy groups, mercapto groups, amino groups, diamino groups, alkoxy groups, and ethoxy groups.
[0055] From the viewpoint of achieving high die shear strength (shear strength), the content of the inorganic filler is preferably 20 to 200 parts by mass, and more preferably 30 to 100 parts by mass, per 100 parts by mass of the resin component of the thermosetting resin composition.
[0056] [Curing Accelerator] Examples of curing accelerators include imidazoles and their derivatives, organic phosphorus compounds, secondary amines, tertiary amines, and quaternary ammonium salts. From the viewpoint of achieving high die shear strength (shear strength), imidazole compounds are preferred. Examples of imidazoles include 2-methylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-cyanoethyl-2-methylimidazole. These may be used alone or in combination of two or more.
[0057] From the viewpoint of achieving high die shear strength (shear strength), the content of the curing accelerator in the thermosetting resin composition is preferably 0.04 to 3 parts by mass, and more preferably 0.04 to 0.2 parts by mass, per 100 parts by mass of the epoxy resin and the epoxy resin curing agent in total.
[0058] Second Embodiment Figure 9 is a cross-sectional view schematically illustrating a second embodiment of a semiconductor device. While the semiconductor device 100 according to the first embodiment has the chip T1 spaced apart from the adhesive piece Tc, the semiconductor device 200 according to this embodiment has the chip T1 in contact with the adhesive piece Tc. In other words, the adhesive piece Tc is in contact with the top surface of the chip T1 and the top surface of the support piece Dc. For example, by appropriately setting the thickness of the support piece-forming film D, the position of the top surface of the chip T1 can be aligned with the position of the top surface of the support piece Dc.
[0059] In the semiconductor device 200, the chip T1 is flip-chip connected to the substrate 10, not by wire bonding. If the chip T1 is configured to be embedded in the adhesive piece Ta that constitutes the adhesive piece-attached chip T2a together with the chip T2, the chip T1 can be in contact with the adhesive piece Tc even if the chip T1 is wire-bonded to the substrate 10.
[0060] The present disclosure will be described below with reference to examples, but the present invention is not limited to these examples.
[0061] [Preparation of Film for Forming Support Piece] <Preparation of Varnish> The materials shown in Table 1 were used in the composition ratios (unit: parts by mass) shown in Table 1. Cyclohexanone was added to the epoxy resin, phenolic resin, and inorganic filler, and the mixture was stirred and mixed. The cyclohexanone content was adjusted so that the solids content of the final varnish was 40 mass%. To this was added an elastomer, followed by a coupling agent and a curing accelerator, and the components were stirred until uniform, to prepare varnishes A to E.
[0062] Details of each component shown in Table 1 are as follows: Epoxy resin: YDCN-700-10 (trade name, manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., o-cresol novolac epoxy resin, epoxy equivalent: 209 g / eq) EXA-830CRP (trade name, manufactured by DIC Corporation, bisphenol F epoxy resin, epoxy equivalent: 159 g / eq) Phenolic resin (curing agent): HE-100C-30 (trade name, manufactured by Air Water Inc., phenolnoaralkyl phenolic resin, hydroxyl equivalent: 170 g / eq) Phenolic resin (curing agent): PSM-4326 (trade name, manufactured by Gunei Chemical Industry Co., Ltd., phenol novolac phenolic resin, hydroxyl equivalent: 105 g / eq) Inorganic filler: Aerosil R972 (trade name, manufactured by Nippon Aerosil Co., Ltd., silica, average particle size 0.016 μm) Inorganic filler: SC2050-HLG (trade name, manufactured by Admatechs Co., Ltd., silica filler dispersion, average particle size 0.50 μm) Elastomer: SG-P3 solvent-change product (trade name, manufactured by Nagase ChemteX Corporation, acrylic rubber, weight-average molecular weight: 800,000, Tg: 12°C, solvent: cyclohexanone) Elastomer: SG-P3 low molecular weight product (trade name, manufactured by Nagase ChemteX Corporation, acrylic rubber, weight-average molecular weight: 300,000, Tg: 12°C, solvent: cyclohexanone) Coupling agent: A-189 (trade name, manufactured by GE Toshiba Corporation, γ-mercaptopropyltrimethoxysilane) Coupling agent: A-1160 (trade name, manufactured by GE Toshiba Corporation, γ-ureidopropyltriethoxysilane) Curing accelerator: Curesol 2PZ-CN (trade name, manufactured by Shikoku Chemicals Corporation, 1-cyanoethyl-2-phenylimidazole)
[0063]
[0064] <Preparation of Support Piece-Forming Film> (Example 1) Varnish A was filtered through a 100-mesh filter and vacuum-degassed. A 38 μm-thick polyethylene terephthalate (PET) film that had been subjected to a release treatment was prepared as a substrate film, and the vacuum-degassed varnish A was applied to the PET film. The applied varnish A was heated and dried in two stages: at 90°C for 5 minutes and then at 130°C for 5 minutes, to obtain a support piece-forming film of Example 1 in a B-stage state. The amount of varnish A applied was adjusted to a thickness of 50 μm.
[0065] Example 2 A support piece-forming film of Example 2 was obtained in the same manner as in Example 1, except that varnish A was changed to varnish B.
[0066] Example 3 A support piece-forming film of Example 3 was obtained in the same manner as in Example 1, except that varnish A was changed to varnish C.
[0067] Comparative Example 1 A film for forming a support piece of Comparative Example 1 was obtained in the same manner as in Example 1, except that varnish A was changed to varnish D.
[0068] Comparative Example 2 A film for forming a support piece of Comparative Example 2 was obtained in the same manner as in Example 1, except that varnish A was changed to varnish E.
[0069] [Evaluation of Support Piece-Forming Films] <Measurement of Shear Viscosity> Each of the support piece-forming films (50 μm thick) of Examples 1 to 3 and Comparative Examples 1 and 2 was cut to a predetermined size to prepare four film pieces. The four film pieces were laminated using a rubber roll on a hot plate at 60°C to prepare a 200 μm-thick sample. The obtained sample was punched out with a φ9 mm punch, and the shear viscosity of each support piece-forming film at a measurement temperature of 120°C was measured using a shear viscometer (manufactured by TA Instruments Japan Co., Ltd., product name: ARES-G2) under the following conditions. The results are shown in Table 1. Measurement frequency: 1 Hz; Heating rate: 5°C / min; Measurement temperature: 35 to 130°C; Axial force: 100 gf (0.98 N).
[0070] <Evaluation of Support Stability> (Preparation of Substrate with Support Piece) Each of the support piece-forming films (50 μm thick) of Examples 1 to 3 and Comparative Examples 1 and 2 was attached to an adhesive film (adhesive layer thickness: 10 μm, manufactured by Hitachi Chemical Co., Ltd.) having a base film and an adhesive layer to prepare a laminated film. The resulting laminated film was singulated using a fully automatic dicer DFD-6361 (manufactured by Disco Corporation). A dicing blade ZH05-SD4000-N1-xx-BB (both manufactured by Disco Corporation) was used. The cutting conditions were a blade rotation speed of 4000 rpm, a cutting speed of 50 mm / sec, and a size of 6 mm x 3 mm. Next, the support pieces were picked up using a pickup collet.
[0071] Next, the two obtained support pieces were placed on a solder resist substrate (Taiyo Holdings Co., Ltd., product name: AUS-308) and thermocompression bonded to obtain the support piece-attached substrates of Examples 1 to 3 and Comparative Examples 1 and 2. The thermocompression bonding conditions were a temperature of 120°C, a time of 1 second, and a pressure of 0.1 MPa. FIG. 10(a) is a top view showing an example of the support piece-attached substrate used in the examples, and FIG. 10(b) is a cross-sectional view taken along line b-b in FIG. 10(a). As shown in FIG. 10, the support piece-attached substrate 300 includes a substrate 310 and two support pieces Da arranged on the substrate 310 so as to contact both opposing sides of the substrate 310.
[0072] (Preparation of chip with adhesive piece) A dicing / die bonding integrated adhesive film (film adhesive: thickness 50 μm, adhesive film: thickness 110 μm, manufactured by Hitachi Chemical Co., Ltd.) equipped with a film adhesive and an adhesive film, and a silicon wafer having a thickness of 400 μm were prepared. A dicing sample was prepared by laminating a silicon wafer onto the film adhesive of the dicing / die bonding integrated adhesive film at a stage temperature of 70° C.
[0073] The obtained diced sample was cut using a fully automatic dicer DFD-6361 (manufactured by Disco Corporation). Cutting was performed using a step-cut method using two blades, and dicing blades ZH05-SD3500-N1-xx-DD and ZH05-SD4000-N1-xx-BB (both manufactured by Disco Corporation) were used. The cutting conditions were a blade rotation speed of 4000 rpm, a cutting speed of 50 mm / sec, and a chip size of 6 mm x 12 mm. The first cutting step was performed so that about 200 μm of the silicon wafer remained, and then the second cutting step was performed so that about 20 μm of incision was made in the adhesive film. Next, the chip was picked up using a pickup collet to obtain a chip with an adhesive piece.
[0074] (Preparation of Evaluation Samples) In Examples 1 to 3 and Comparative Examples 1 and 2, adhesive pieces of the chips with adhesive pieces were placed on the support pieces of the substrates with support pieces, respectively, so that the substrates of the substrates with support pieces and the chips of the chips with adhesive pieces overlapped, followed by thermocompression bonding. The thermocompression bonding conditions were a temperature of 120°C, a time of 1 second, and a pressure of 0.1 MPa. Figure 10(c) is a cross-sectional view showing an example of a laminate used in the examples. As shown in Figure 10(c), the laminate 400 includes a substrate with support piece 300, an adhesive piece-attached chip T300a consisting of an adhesive piece Ta and a chip T300, and two support pieces Da arranged between the substrate with support piece 300 and the adhesive piece-attached chip T300a. The laminate obtained by thermocompression bonding was then placed in a dryer and heat-cured at 170°C for 1 hour, thereby obtaining evaluation samples for Examples 1 to 3 and Comparative Examples 1 and 2.
[0075] (Cross-section observation by microscope) The cross sections of the evaluation samples prepared in Examples 1 to 3 and Comparative Examples 1 and 2 were observed by microscope, and the variation in the height of the support piece was evaluated. Those in which the support piece did not deform or shrink and the substrate and chip remained parallel were evaluated as "A", and those in which the support piece deformed or shrank and the substrate and chip were no longer parallel were evaluated as "B". The results are shown in Table 2.
[0076]
[0077] As shown in Table 2, the evaluation samples of Examples 1 to 3, which used support piece-forming films with a shear viscosity of 4000 Pa·s or more at 120° C., had reduced variation in support piece height compared to the evaluation samples of Comparative Examples 1 and 2, which used support piece-forming films with a shear viscosity of less than 4000 Pa·s at 120° C. From the above, it was confirmed that the semiconductor device manufacturing method of the present invention is capable of manufacturing a semiconductor device that can stably support stacked semiconductor chips.
[0078] According to the present disclosure, a method for manufacturing a semiconductor device that can simplify the process of manufacturing a support piece in a manufacturing process of a semiconductor device having a dolmen structure and that can stably support stacked semiconductor chips is provided. Also, according to the present disclosure, a method for manufacturing a support piece and a laminated film for forming the support piece are provided.
[0079] 1...base material film, 2...adhesive layer, 5...thermosetting resin layer, 10, 310...substrate, 20...laminated film for forming support piece, 50...sealing material, 100, 200...semiconductor device, 300...substrate with support piece, 400...laminated body, D...film for forming support piece, Da...support piece, Dc...support piece (cured product), T1...first chip, T2...second chip, T300...chip, T2a, T300a...chip with adhesive piece, Ta...adhesive piece, Tc...adhesive piece (cured product).
Claims
1. A method for manufacturing a semiconductor device having a dolmen structure including a substrate, a first chip arranged on the substrate, a plurality of support pieces arranged on the substrate around the first chip, and a second chip supported by the plurality of support pieces and arranged to cover the first chip, the method comprising: (A) preparing a laminated film including, in this order, a base film, an adhesive layer, and a support piece forming film; (B) forming a plurality of support pieces on the surface of the adhesive layer by dividing the support piece forming film; (C) picking up the support pieces from the adhesive layer; (D) arranging the first chip on the substrate; (E) arranging the plurality of support pieces on the substrate around the first chip; (F) preparing a chip with adhesive pieces including a second chip and an adhesive piece provided on one surface of the second chip; and (G) constructing a dolmen structure by arranging the chip with adhesive piece on the surfaces of the plurality of support pieces. The method for manufacturing a semiconductor device, wherein the support piece-forming film has a shear viscosity of 4000 Pa·s or more at 120°C.
2. The method for manufacturing a semiconductor device according to claim 1, wherein the support piece forming film includes a thermosetting resin layer, and the method includes a step of heating the support piece forming film or the support piece prior to step (G).
3. A method for manufacturing a support piece used in a manufacturing process for a semiconductor device having a dolmen structure including a substrate, a first chip arranged on the substrate, a plurality of support pieces arranged on the substrate around the first chip, and a second chip supported by the plurality of support pieces and arranged to cover the first chip, the method comprising: (A) a step of preparing a laminated film having, in this order, a base film, an adhesive layer, and a support piece forming film; (B) a step of forming a plurality of support pieces on the surface of the adhesive layer by individualizing the support piece forming film; and (C) a step of picking up the support pieces from the adhesive layer, wherein the shear viscosity at 120°C of the support piece forming film is 4000 Pa·s or more.
4. The method for manufacturing a support piece according to claim 3, wherein the support piece-forming film includes a thermosetting resin layer.
5. A laminated film for forming a support piece used in the manufacturing process of a semiconductor device having a dolmen structure including a substrate, a first chip arranged on the substrate, a plurality of support pieces arranged on the substrate around the first chip, and a second chip supported by the plurality of support pieces and arranged so as to cover the first chip, the laminated film for forming a support piece comprising, in this order: a base film; an adhesive layer; and a film for forming a support piece, wherein the shear viscosity of the film for forming a support piece at 120°C is 4000 Pa·s or more.
6. The laminated film for forming a support piece according to claim 5, wherein the film for forming a support piece includes a thermosetting resin layer.