A resin-coated metal sheet with higher vivid reflectivity having excellent workable adhesion
Patent Information
- Application Number
- MYPI1997002096
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 1996-05-14
- Filing Date
- 1997-05-13
- Publication Date
- 1997-11-14
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Decorative metal sheets with high vivid reflectivity and excellent workable adhesion are challenging to achieve due to issues with surface roughness, coefficient of friction, and delamination during processes like stretch-forming and deep drawing, as existing solutions either result in inadequate anchor effects or compromised reflectivity.
A resin-coated metal sheet with a metal base having a surface roughness of 0.1-10 μm, featuring a soft resin layer, an adhesive layer with metal powder pigments, and a transparent biaxial oriented polyethylene terephthalate resin film, where the soft resin layer absorbs ruggedness and ensures excellent adhesion and reflectivity.
The solution provides a resin-coated metal sheet with remarkable vivid reflectivity and excellent workable adhesion, preventing delamination even under intense working conditions like stretch-forming and deep drawing, while maintaining economic efficiency.
Abstract
Description
HIGHER VIVID REFLECTIVITY HAVING EXCELLENT WORKABLE ADHESION [Detailed description of the Invention]
[0001] [Field of the Invention]The present invention relates to a resin-coated metal sheet with higher vivid reflectivity having excellent workable adhesion property.
[0002] [Description of the Prior Art]Recently, decorative design of higher grade is being pursued, together with the grade of articles such as domestic electrical machinery and apparatus, audio, kitchen appliance, and interior finish materials being made higher. Decorative design of higher grade can be expressed by the shape of package which is formed by stretch-forming or deep drawing of its material and by the decorativeness of the surface of packing materials, especially expressed by print patterns printed on the packing materials with higher reflectivity. Accordingly, the requirement for a decorative steel sheet with higher vivid reflectivity having excellent workable adhesion fit for working such as stretch-forming and deep drawing is being increased.
[0003] -1'97$05£03B (i) 17^35# 0-0041-603-243-4063 $=:O$ SBR:858 P. 03 / 34So far, polished sheet whose arithmetical mean deviation of profile (Ra) which indicates the surface roughness of metal sheet is small has been recommended as a metal base to be used for this kind of decorative metal sheet with higher vivid reflectivity, because the surface roughness of metal sheet affects largely the vivid reflectivity. However, when a polished sheet is produced by rolling-forming, it will easily slip because its coefficient of friction is small due to its small roughness. Therefore, such polished sheet with a small arithmetical mean deviation of profile (Ra) is not at all productive and too expensive for materials. Moreover, when such polished sheet is used as a metal base, it does not have enough anchor effect on a coating layer which is formed on such base, and therefore the workable adhesion of the coating layer will be insufficient.On the other hand, in order to use a rather cheep metal sheet having a little larger surface roughness as a base sheet for decorative metal board with higher vivid reflectivity, it is proposed by Japanese Patent Publication (Kokai) (Heisei 6)23909 that a transparent thermoplastic resin film provided with an adhesive layer or a printing layer is overlaid on the base sheet, which is thereafter heat-pressed by mirror finish roll to produce a laminated metal sheet with higher vivid reflectivity.However, when such laminated metal sheet is heat-pressed by rolling, it is not avoidable that the thermoplastic resin-2• · · · • · · '97105^030 (i) 17^35# 0-0041-603-243-4063 ΜβR:858 P. 04 / 34 layer has external waviness caused by the heat and therefore the obtained metal sheet does not always have satisfactory high vivid reflectivity. Another problem is that the ruggedness resulting from partially arranged printing pattern and shading pattern rises up to the surface of the transparent thermoplastic resin layer, which does not allow the laminated metal sheet to have sufficiently vivid reflectivity .
[0004] [Problem to be solved by the Invention]In view of the problems encountered in the prior art, it is an object of the present invention to provide a resin-coated metal sheet which has an excellent workable adhesion property and high vivid reflectivity.
[0005] [Means for solving the Problem]A resin-coated metal sheet of the present invention comprises: a metal sheet, whose surface roughness of arithmetical mean deviation of profile (Ra) is more than OAm and not more than 10Am, as a base sheet; a coloring paint layer; a soft resin layer; an adhesive layer; and a transparent resin film, wherein at least one surface side of the metal sheet is overlaid by the above mentioned layers which are laid one over another in order from the side of the metal sheet toward the transparent resin film.Further, in the resin-coated metal sheet of the present invention, the above mentioned soft resin layer consists of a • · ·· · ·· ·· · · · · ···· · · ·· ····· · • ·· ·· ···· • · · · · · · • · · · · · • ··· ··· ·-3'97$05£03Β (i) 17^35^ 0-0041-603-243-4063 fflR:858 P. 05 / 34 transparent resin and is a layer consisting of a soft resin which is prepared by painting's’ paint of resin mixed with such amount of curing agent as not to be perfectly cured by afterheating, on a resin mixed with curing agent to be perfectly cured by after-heating, and then heating them to have low hardness, or a polyester resin paint layer, or a film consisting of polyolefin resin.Further, in the resin-coated metal sheet of this invention, the above mentioned adhesive layer contains pigment and the pigment includes metal powder especially such as aluminum powder or mica powder.Furthermore, in the resin-coated metal sheet of this invention, the above mentioned transparent resin film has both surfaces visually mirror finished and is a biaxial oriented film of polyethylene terephthalate.Furthermore, in the resin-coated metal sheet of this invention, a pattern printing layer or a pattern and solid printing layer is / are provided between the adhesive layer and the soft resin layer, or a pattern printing layer or a pattern and solid printing layer is / are provided between the adhesive layer and the transparent resin film.
[0006] [Mode of carrying out the Invention]The resin-coated metal sheet of this invention with high vivid reflectivity has a soft resin layer provided between the coloring paint layer formed on the metal sheet and the·· · ·· ·· · · ·· ·· ·· '97^05^03B (±) 17^35» 0-0041-603-243-4063 Μβ tfflR:858 P. 06 / 34 outermost transparent resin film whose both surfaces are visually mirror finished so^that the soft resin layer is transformed to absorb the ruggedness due to the roughness of metal sheet, and the ruggedness of coloring paint layer affected by the ruggedness of the metal sheet or the ruggedness by printing patterns or shading patterns when the metal sheet and the above mentioned resin layers are heat-pressed. Besides, the soft resin layer allows the transparent resin film to be heat-pressed without its outermost visually mirror finished surface deformed. As a result, the resin-coated metal sheet of this invention has remarkably high vivid reflectivity and such excellent workable adhesion property that delamination between the layers is not caused even in intense working such as stretch-forming or deep drawing.
[0007] [Embodiment]The present invention is explained in detail according to the following embodiments.Figures 1 to 3 show the composition of one side of the resin coated metal sheet in a cace where the metal sheet is provided with a resin coating layer.Figure 1 shows an embodiment according to the invention as claimed in claim 1, wherein A is a transparent resin film, B Is an adhesive layer, C is a soft resin layer, O is a coloring paint layer, and S is a metal sheet.
[0008] • · '97£05£03B (i) 17^35» 0-0041-603-243-4063R:858 P. 07 / 34In Figure 1, A is a transparent resin film forming the outermost layerof the resin coated metal sheet. This transparent resin film is formed by extrusion method, calendering method, casting method and the like, or oriented uniaxially or biaxially after casting.It is essentially required to obtain a resin-coated metal sheet of this invention with higher vivid reflectivity that the transparent resin film has both surfaces visually mirror finished whose surface roughness Ra max after forming is not more than 5 μιη . When the film surfaces become rougher with its surface roughness Ra max more than 5μπι, the vivid reflectivity of resin-coated metal sheet is inferior due to the diffused reflection by the film surfaces.The thickness of transparent resin film is preferably 5100μm, and more desirably 12μπι to 80μπι. When the thickness of the transparent resin film i9 less than 5μπι, the vivid reflectivity of the whole of the resin-coated metal sheet is inferior, and besides, handling of the transparent resin film in laminating work is extremely difficult. On the other hand, when the thickness of the transparent resin film is more than 100μη, the workable adhesion property of the resin-coated metal sheet is inferior.Transparent resin film A includes films formed of polyester resin, polycarbonate resin, polyvinyl alcohol resin, polypropylene resin, and nonplasticized or plasticized vinylchloride resin, polymethylpentane resin, cellulose • · ·· · ·· ·· ···· ···· · · ·· ····· ·-6• · • · '97$O5£O30 (i) 17$35# Β: 0-0041-603-243-4063 ΟR: 858 Ρ. 08 / 34 triacetate resin, cellulose diacetate resin etc, to which a stabilizing agent and a plasticizing agent may be added to an extent so far as the vivid reflectivity is not lowered, if necessary. Further the polyester film includes films formed of polyethylene terephthalate resin and copolymer resin thereof. Above all, biaxial oriented polyethylene terephthalate resin film is practically preferable to be used for the resin-coated metal sheet of this invention with high vivid reflectivity.
[0009] In order to improve scratch resistance and slip resistance of the resin-coated metal sheet in forming it or handling it, the transparent resin film forming the outermost layer of the resin-coated metal sheet of this invention is preferably coated with a top coat of thermosetting paint or ultraviolet irradiated resin paint such as silicon resin paint, fluoride resin paint, acrylic resin paint, melamine resin paint or urethane resin paint with a thickness of 0.1 50Pm and more desirably 0.3Pm to 30Pm. When the thickness of the top coat is less than 0.2Pm, an interference color is noticeably seen, and the scratch resistance is reduced. On the other hand, when the thickness of the top coat is more than 50Pm, the workability thereof decreases, and besides the economical efficiency is lowered.
[0010] In Figure 1, B is an adhesive layer, which contains one of'97^05^030 (i) 175^35^ 0-0041-603-243-4063R:858 P. Q9 / 34 the resins of polyester resin, acrylic resin, urethane resin, epoxy resin, and melamine resin as chief ingredients of the adhesive. Further, adhesive assistant having adhesive effect, for instance, silane coupling agent can be used as ingredients in addition to the above mentioned resin.The adhesive layer can be transparent, or contain pigment in order to attain higher decorativeness of the coloring paint layer which is formed as the lower layer thereof. The pigment to be contained in the adhesive layer can be organic or inorganic matter. In particular, when the adhesive layer is given a so-called metallic color tone with metallic luster, pigment containing metal powder, especially such as aluminum powder or mica powder, which may be paint colored metal powder or non-colored metal powder, is preferably used.The ratio of pigments to solid matter in adhesive resin is preferably 1 ,- 30% by weight and more desirably 3 - 20% by weight. When the ratio of pigment to solid matter in adhesive is less than 1% by weight, color tone by pigment (metallic luster) cannot be obtained and when the ratio of pigment to solid matter in adhesive is more than 30% by weight, the adhesive layer becomes fragile and besides the workable adhesion strength is inferior in severe working.The particles of the above mentioned pigment may have a glovelike shape or scalelike shape. The average particle size thereof is preferably 0.1 - 90 Am, and more desirably 1 - 80 Am. When the average particle size is less than 0.1 Am, the• · ···· · · • · '97.W03B(±)17W 0-0041-603-243-4063 Μβ WR-· 858 p. 10 / 34 metallic tone is inferior and when the average particle size is more than 100 P m, the vivid reflectivity of the resin-coated metal sheet becomes lowered.The thickness of the above-mentioned adhesive layer is preferably 1 - 50Am and more desirably 3 - 30Am. When the thickness of the adhesive layer is less than lAm, the boiling water resistance and the workable adhesion property of the resin-coated metal sheet are inferior and moreover when the pigment is added thereto, the pigment is hardly to be diffused uniformly in the paint. On the other hand, when the thickness of the adhesive layer is more than 50Am, it takes economical disadvantage, and moreover when the pigment is added thereto, the external appearance of the resin-coated metal sheet will be worsened resulting from the residual solvent contained in the adhesive at the time of heating for lamination. Thus, the vivid reflectivity thereof becomes lowered.
[0011] In Figure 1, C is a soft resin layer significantly provided to produce the excellent workable adhesion property and high vivid reflectivity of the resin-coated metal sheet of this invention. According to the present invention, when a metal sheet having a rough surface is used as base sheet, or when coloring paint is painted on the metal sheet with its thickness partially uneven so that the coated metal sheet has the ruggedness, or when even a transparent resin film provided with a pattern or / and solid printing layer (there is naturally-9• a · · ·· ·· ·· ·· • · · · · ·· · · · · · · ··· · · · · · · ··· · ·· · ·· ···· ·· ·· ··'97.^05^030 (±) 17^35# 5^:0-0041-603-243-4063 MiM fflR;858 p, n / 34 formed ruggedness) is overlaid on the metal sheet, soft resin layer C can absorb such ruggedness.That is, the ruggedness resulting from the surface roughness of the metal sheet, coloring paint layer and printing layer is absorbed by this soft resin layer C so as not to appear up to the surface of transparent resin film A. Otherwise, if the ruggedness comes up to the surface of transparent resin film A, it causes diffused reflection, thereby lowering the vivid reflectivity of the resin-coated metal sheet.When the layers are laminated, soft resin layer C is transformed by the laminating roll pressure to thereby prevent transparent resin film A from being deformed due to the ruggedness of the metal sheet, coloring paint layer or printing layer.On the other hand, soft resin layer C requires to have an excellent workable adhesion property so that delamination between soft resin layer C and the other layers is not caused, even when the laminate is subjected to intense working such as stretch-forming or deep drawing.
[0012] In view of the above mentioned requirement, the soft resin layer of the resin-coated metal sheet according to the present invention includes, for example, a resin with two liquid mixture curing type resin not perfectly cured ( under cured). That is, a resin which would be perfectly cured by curing agent with after-heating is mixed with such amount of the curing• · a · '97£O5£O30 (i) 17B335# 5^:0-0041-603-243-4063 50» fflR:858 P. 12 / 34 agent as not to be perfectly cured with after-heating to form an under cured soft resin, which is suitable for the soft resin layer of this invention.Or, a film consisting of the above soft resin is preferably used as soft resin layer C.The transparent resin layer may be a transparent layer or opaque or semi-transparent layer with pigment added thereto. However, the transparent layer may most desirably be selected so as to make clear the decorative design of a surface treated layer which is formed as the lower layer thereof.
[0013] When soft resin layer C is formed of an under cured resin, such resin includes one of polyester resin, acrylic resin, urethane resin, epoxy resin, and melamine resin as chief ingredients. Above all, it is preferable that polyester resin is used as chief ingredients, since when it is applied to the soft resin layer, the most excellent workable adhesion strength and the vivid reflectivity are attained. In this case of using polyester resin, urethane resin is added as curing agent into polyester resin with the ratio of 0.5 - 15% of urethane resin by wight to 100% of polyester resin by weight. The thus prepared polyester resin is painted on a surface treated layer formed on the metal base sheet and thereafter heated at a temperature of 230 - 280^ for 0.3-2 minutes to be semi-cured. When the curing agent is less than 0.5 % by weight, the workable adhesion strength with regard to the metal• · '97.^05^030 (i) 17B335# 0-0041-603-243-4063 Μ»R:858 p. 13 / 34 sheet is not enough. On the other hand, when the ratio of the curing agent is more than 15% by weight and not more than 20% by weight, excellent workable adhesion property can be obtained but the resin becomes harder so that the soft resin layer can no longer absorb the ruggedness of the base metal and / or printing layer. Further, when the ratio of the curing agent is more than 20% by weight, the resin is excessively hardened so that the soft resin layer becomes fragile and its workable adhesion property is deteriorated.
[0014] Resin film for the soft resin layer includes a film of polyester resin blended with elastmer to soften it, a film of modified polyolefin resin prepared by having at least one functional group selected from the groups consisting of carboxyl group, hydroxyl group, hydrolyzable group, and acid anhydrous group contained within a molecule, and a film of polyvinylchloride resin prepared by adding a known platicizing agent thereto to soften it. Above all, the film of polyolefin resin or the polyvinylchloride resin is preferable for soft resin layer C of the resin-coated metal sheet of the present invention.
[0015] The thickness of above-mentioned soft resin layer C is preferably 10 - 100Pm and more preferably 20 - 70Pm. When the thickness of the soft resin layer is less than 10Pm, the vivid reflectivity of the whole resin-coated metal sheet is inferior-12• · · · · · • · '97^0.5^030 (±) 17^35# B:0-0041-603-243-4063 ®R:858 P. 14 / 34 because the soft resin layer can no longer absorb the ruggedness o¥the metal sheetTand / or printing layer perfectly. On the other hand, when the thickness of the soft resin layer is more than 100Am, the surface rigidity and the workable adhesion strength of the whole resin-coated metal sheet are inferior.Incidentally, when the soft resin film is used as soft resin layer C, it is possible to improve the adhesive strength between the laminated resin layers (films) by effecting anchor treatment with silane coupling agent on the upper or lower layer (or both upper and lower layers) of the soft resin film.
[0016] In Figure 1, D is a coloring paint layer. This coloring paint layer is provided for forming a coloring layer to express decorative design. For this coloring paint layer, resin for paint Includes one of polyester resin, acrylic resin, urethane resin, epoxy resin, and melamine resin as chief ingredients. In particular, it is preferable that polyester resin is used as chief ingredients, because the workable adhesion strength is extremely good. For pigment to be contained in this paint, a known organic and inorganic pigment are applicable.The ratio of pigment to solid matter in resin paint is preferable 1 - 30% by weight, more desirably 3 - 20% by weight. When the ratio of pigment to solid matter is less than 1% by weight, coloring tone cannot be given by the pigment. When the ratio of pigment to solid matter is more than 30% by weight,-13• · • · '97£05£03B (±) 17B£35# 0-0041-603-243-4063 1:$® fflR:858 p. 15 / 34 the coloring paint layer becomes fragile and its workable adhesion strength is ba*d whei?subjected to severe working. The particle of the pigment may have a globelike shape or scalelike shape. The average particle size thereof is preferably 0.1 100 μ m, more desirably 1 - 80 μ m. when the average particle size is less than Ο.ίμαι, handling it is extremely difficult and when the average particle size is more than 100μπι, the coating property is inferior and the vivid reflectivity of the resin-coated metal sheet is lowered.The thickness of coloring paint layer D including the above-mentioned pigments is preferably 1 - 60μιη, and more desirably 3 - 30μιη. When the thickness of coloring paint layer D is less than ΐμπι, masking by pigment is inferior. On the other hand, when the thickness of the coloring paint layer is more than 60μπι, the economical efficiency is lowered.Further, coloring paint layer D includes a layer composed of two or more layers. That is, coloring paint layer D includes a laminate formed of plural layers having an under coating including rust preventing pigment in order to increase the rust resistance of the metal base.
[0017] In Figure 1, S is a metal sheet as base sheet. This metal sheet includes: steel sheet, stainless steel sheet, galvanized steel sheet, galvanized alloy steel sheet, composite galvanized steel sheet, nickel-plated steel sheet, those further surface-treated steel sheet with chemical conversion-14•··· ·« ····• · · '97$0·5 / ]03B (i) 17B£35# 5$: 0-0041-603-243-4063R:858 ρ. 16 / 34 treatment such as known chrome treatment, phosphate chrome treatment, and electrochemical chrome treatment; surfacetreated steel sheet such as tin-free steel that is directly treated on its steel sheet surface; nonferrous metal sheets such as aluminum alloy sheet and copper steel; and those further treated steel sheet with the above mentioned chemical conversion treatment.In addition, it is essentially required for the resincoated metal sheet of this invention that the arithmetical mean deviation of profile (Ra) thereof is more than O#m and not more than 10(tm. When a metal sheet has a mirror-finished surface with Ra of O^m, the anchor effect on coloring paint layer D cannot be obtained and therefore the workable adhesion strength is insufficient. Moreover, manufacturing the metal sheet having a mirror-finished surface with Ra of 0#m is not at all productive and thus such metal sheet becomes too expensive.On the other hand, when a metal sheet whose Ra exceeds10#m is used as base sheet, the vivid reflectivity decreases, because the ruggedness due to the surface roughness of the metal sheet cannot be perfectly absorbed by soft resin layer B.It is more desirable that Ra of the metal sheet is 0.1 - 2 / Zm.
[0018] Figure 2 corresponds to an invention described in claim 12 and has the similar composition to that shown in Figure 1 except that a pattern and / or solid printing layer is provided-15• 9999 99 9999 9 99 99 99999 9 9 9 9 9 9 9 9 9 9 9'97WO30 (i) 17#35# 0-0041-603-243-4063 $1:0$ ®R:858 P. 17 / 34 between adhesive layer B and soft resin layer C.
[0019] Figure 3 corresponds to an invention described in claim 13 and has the similar composition to that shown in Figure 1 except that a pattern and / or solid printing layer is provided between adhesive layer B and transparent resin film A.
[0020] Next, method of manufacturing the resin-coated metal sheet of this invention is explained.(1) Formation of soft resin layerIn a case of the resin-coated metal sheet shown in Figure 1 (described in claim 1), a paint containing pigment is painted on the surface of metal sheet S one time or two times by roll coating or the like to form coloring paint layer D. When the thickness of the paint layer needs to be increased, further times of painting is increased. Then, soft resin layer C is formed on that coloring paint layer. In a case where soft resin layer C is formed of a paint coat, a resin, which has a curing agent added thereto perfectly to be cured by afterheating, is coated with a paint consisting of another resin, which has a curing agent added thereto to such an extent as not to be perfectly cured by after-heating, and they are dried to be then heated. In another case where soft resin layer C ls formed of a film consisting of a soft resin, the soft resin is formed into a film by extrusion coating to be overlaid on the paint layer. Alternately, the above mentioned painted metal-16• · · * · ·· ·· · · · 9 ···· · * · · · · · · ·• · · · · ·97.105^030 (i) 17B335# & 0-0041-603-243-4063 5MM fflR:858 P. 18 / 34 sheet provided with coloring paint layer D is heated, and then contacted*··with a film'formedof a soft resin and they are pressed using a pair of laminating rolls to be laminated, thereby producing soft resin layer C.(2) Production of resin coating filmIn a case of the resin coating film shown in Figure 1 (described in claim 1), adhesive mixed with pigment consisting of metal powder, especially aluminum powder or mica powder, or non-mixed adhesive is painted on transparent resin film A and they are dried, thereby producing adhesive layer B.In a case of the resin coating film shown in Figure 2 (described in claim 12), adhesive mixed with pigment consisting of metal powder, especially aluminum powder or mica powder, or non-mixed adhesive is painted on transparent resin film A and they are dried to form adhesive layer B, and thereafter pattern printing layer P2, or pattern printing layer P2 and solid printing layer Pl is / are provided.In a case of the resin coating film shown in Figure 3 (described in claim 13), first, pattern printing layer P2, or pattern printing layer and solid printing layer Pl is / are formed on transparent resin film A, sequentially, as described above, adhesive mixed with pigment consisting of metal powder, particularly aluminum powder or mica powder, or non-mixed adhesive is painted on the above mentioned printing layer and dried to form adhesive layer B.(3) Overlay • · ·· ·· ·· ·· ·· • · ·· · · · ·· ···· ··· · · · · · · ···· · ·· ··· ·· · · · «· · ·· ···· ·· ·· ··'97.^05^030 (i) 17$35# Β:0-0041-603-243-4063 fflR:858 p. 19 / 34The soft resin coated metal sheet produced as described above is heated, then contacted with the resin coating film and they are pressed using a pair of laminating rolls. They are still further heated and then pressed using a pair of mirror rolls thereafter to be cooled.In this time, the suitable roll pressure of the laminating roll is 1 - 80kg / cm2 and more desirably 5 - 60kg / cm2. When the roll pressure is less than 5kg / cm2, the coating resin film cannot be pressed uniformly over the width of the metal sheet, resulting in unevenness of the appearance (vivid reflectivity). On the other hand, when the roll pressure is more than 60kg / cm2, the abrasion of the roll occurs heavily so that the laminating roll needs to be frequently replaced, therefore the productivity being decreased.
[0021] (Example 1)Formation of soft resin layerPolyester copolymer paint including white pigment was painted, with a thickness of 12Pm, on galvanized steel sheet having a thickness of 0.5mm, 12g / m2 galvanizing amount,0.08g / dm2 chromate film layer (as amount of chromium), and average surface roughness Ra of 0.55Pm and dried. Further, a mixture of 100 % by weight of transparent polyester resin and 3% by weight of urethane resin as curing agent was painted thereon with a thickness of 10Pm and dried, and then baked at a temperature of 260^ for one minute to produce a metal sheet18'97$05£030 (i) 170^35# 0-0041-603-243-4063 Μβ fflR;858 p. 20 / 34 provided with soft resin layer.
[0022] Production of resin coating filmPolyester copolymer resin adhesive containing the pigment consisting of gold colored scalelike aluminum powder having average particle size of 3 Am with a ratio of 15% by weight of pigment to solid matter in resin adhesive, was painted on a transparent biaxial oriented polyethylene terephthalate film having a thickness of 25 Am and average surface roughness Ra of 0.8Am, which was beforehand top-coated with acrylic resin of 3 Am thickness, with a thickness of 10 Am, and dried to produce a resin coating film.
[0023] OverlayThe metal sheet provided with the above mentioned soft resin layer was heated to a temperature of 200°C, contacted with the above mentioned resin coating film, and pressed using a pair of laminating rolls under the roll pressure of 20kg / cm2. Further, the metal sheet provided with soft resin layer was pressed using a pair of mirror rolls in an atmosphere of 200“£ and then cooled, thereby producing a resin-coated metal sheet.
[0024] EvaluationThe characteristics of the thus obtained resin-coated metal sheet was evaluated according to the following standard for evaluation.• · · · » · ·I · · · · • · · · 4-19'9MO30(±) 17B335# 0-0041-603-243-4063 Μ »R:858 P. 21 / 34 (1) Vivid ReflectivityThe vivid reflectivitjTof a reflected image, namely the vivid reflectivity of a normal reflected image, on a decorative surface of the resin-coated metal sheet was measured by means of a portable distinctness of image glossmeter PGD-4 type (made by Japan Color Research Institute). The higher the measured value is, the higher the vivid reflectivity is.(ii) Workable Adhesion StrengthIn the present invention, valuation of workable adhesion strength is made by taking the following two measurements and judging the results thereof synthetically.(a) Erichsen testCheckered cuts reaching a base metal are made in a resincoated surface of the resin-coated metal sheet by a cutter knife, and 8mm stretch-forming of the resin-coated metal sheet is made from the backside of the resin-coated metal sheet byErichsen tester. Thereafter, the extent of delamination is valuated by heating continuously the resin-coated metal sheet at 1OO°C for one hour and thereafter observing the existing of delamination.(b) Cup-deep drawing testDeep drawing of a resin-coated metal sheet into a cup is made by Yamada-way deep drawing tester, with drawing ratio r-2.2. Checkered cuts reaching a base metal are made in a resin surface of the resin-coated metal sheet formed into a cylindrical part of cup, with the space of 5mm. Thereafter,• · · · · ····· • · · • · '97Λ05£03Β (±) 17Β|35^ 5^:0-0041-603-243-4063 5Οί» »r:858 Ρ. 22 / 34 the extent of delamination is valuated by heating continuously the resin-coated metal sheet formed into a cup by deep drawing at lOO'C for one hour and thereafter observing the existing of delamination.Numerical value indicating the vivid reflectivity of the resin-coated metal sheet produced as above described was 0.8 and good, and in addition, the workable adhesion strength was also good.
[0025] (Comparative example 1)The same polyester copolymer paint including white pigment as that of Example 1 was painted on a galvanized steel sheet as used in Example 1 with a thickness of 12(tm, and dried. Further, a mixture of 100 % by weight of transparent polyester resin and 17% by weight of urethane resin as curing agent was painted thereon with a thickness of 10(tm and dried, and then baked at a temperature of 280^ for 0.3 minutes to prepare a resin layer. This resin layer was overlaid by the same resin coating film as that of Example 1 in the same condition as in Example 1 to produce a resin-coated metal sheet. The characteristics of the thus obtained resin-coated metal sheet was evaluated using the same evaluation method as described in Example 1. As a result, the workable adhesion strength was good but numerical value indicating the vivid reflectivity was 0.1 and this was inferior.
[0026] • ·97^05^030 (i) 17(835# 0-0041-603-243-4063R:858 Ρ. 23 / 34 (Example 2)Formation of^soft resin layer’”Polyester copolymer paint including white pigment was painted, with a thickness of 5 μπι, on galvanized steel sheet having a thickness of 0.5mm, 14g / m2 galvanizing amount,0.07g / dm2 chromate film layer (as amount of chromium), and average surface roughness Ra of 8.5X*m and dried. This painted metal sheet was heated to a temperature of 200*£, contacted with a transparent maleic acid modified polyethylene film having a thickness of 100 μπι, pressed using a pair of laminating rolls under the pressure of 20kg / cm2, and then cooled to produce a metal sheet provided with soft resin layer.
[0027] Production of resin coating filmPolyester copolymer resin adhesive paint containing the pigment consisting of scalelike aluminum powder having average particle size of 3Mm with a ratio of 20% by weight of pigment to solid matter in resin adhesive, was painted on a transparent biaxial oriented polyethylene terephthalate film having a thickness of 20μm and average surface roughness Ra of O.Qfim, which was beforehand top-coated with fluoride resin of ίμιη thickness, with a thickness of 12 and dried to produce a resin coating film.
[0028] OverlayThe metal sheet provided with the above mentioned soft'97^05^030 (±) 17B335# $$:0-0041-603-243-4063 $ί;»R:858 P. 24 / 34 resin layer was heated to a temperature of 200°C, contacted with the above mentioned coating resin film, pressed using a pair of laminating rolls under the pressure of 20kg / cm2, and furthermore pressed using a pair of mirror rolls in an atmosphere of 200“C and then cooled to produce a resin-coated metal sheet.The characteristics of the thus obtained resin-coated metal sheet was evaluated according to the same evaluation method as described in Example 1. As a result, numerical value indicating the vivid reflectivity of the resin-coated metal sheet was 1.0 and good and also the workable adhesion strength was good.
[0029] (Comparative example 2)The same polyester copolymer paint including white pigment as that of Example 2 was painted on a galvanized steel sheet as used in Example 2 with a thickness of 5Am, and dried. This painted metal sheet was heated to a temperature of 200^, contacted with a polyethylene film having a thickness of 100Am, pressed using a pair of laminating rolls under the pressure of 20kg / cm2, and then cooled to produce a transparent resin-coated metal sheet. This transparent resin-coated metal sheet was overlaid by the same resin coating film as that of Example 1 in the same condition as in Example 1 to produce a resin-coated metal sheet. The characteristics of the thus obtained resin-coated metal sheet was evaluated using the same-23• ·I · » · ♦ · · • · '97^05^030 (±) 17^35# 0-0041-603-243-4063R:858 Ρ. 25 / 34 evaluation method as described in Example 1. As a result, numericalvalue indicating the vivid reflectivity was 0.9 and good but the workable adhesion strength was bad.
[0030] (Example 3)Formation of soft resin layerPolyester copolymer paint including red pigment was painted, with a thickness of 10Pm, on galvanized steel sheet having a thickness of 0.5mm, 15g / m2 galvanizing amount,0.06g / dm2 chromate film layer (as amount of chromium), and average surface roughness Ra of 0.1 Pm and dried. This painted metal sheet was heated to a temperature of 200°C, contacted with a transparent polyvinylchloride film having a thickness of 50Pm, pressed using a pair of laminating rolls under the pressure of 20kg / cm2, and then cooled to produce a metal sheet provided with soft resin layer.
[0031] Production of resin coating filmPolyester copolymer resin adhesive paint containing the pigment consisting of scalelike mica powder having average particle size of 2Pm with a ratio of 20% by weight of pigment to solid matter in resin adhesive, was painted on a transparent biaxial oriented polyethylene terephthalate film having a thickness of 25Pra and average surface roughness Ra of 0.8Pm, which was beforehand top-coated with melamine resin of 4Pm thickness, with a thickness of 10 Pm, and dried to produce a'9^05^030 (1) 170335# 5$:0-0041-603-243-4063 Μ» fflR:858 ρ. 26 / 34 resin coating film.
[0032] 'The metal sheet provided with the above mentioned soft resin layer was heated to a temperature of 200^, contacted with the above mentioned coating resin film, pressed using a pair of laminating rolls under the pressure of 20kg / cm2, and furthermore pressed using a pair of mirror rolls in an atmosphere of 200“€ and then cooled to produce a resin-coated metal sheet.The characteristics of the thus obtained resin-coated metal sheet was evaluated according to the same evaluation method as described in Example 1. As a result, numerical value indicating the vivid reflectivity of the resin-coated metal sheet was 0.9 and good and also the workable adhesion strength was good.
[0033] (Comparative example 3)Formation of soft resin layerPolyester copolymer paint including red pigment was painted, with a thickness of 10 Am, on galvanized steel sheet having a thickness of 0.5mm, 15g / m2 galvanizing amount,0.06g / dm2 chromate film layer (as amount of chromium), and average surface roughness Ra of 11.5Am and dried. This painted metal sheet was further overlaid by the same transparent polyvinylchloride film as that of Example 3 in the same condition as in Example 3 to produce a resin-coated metal97S05£03B (±) 17(835# 0-0041-603-243-4063R:858 P. 27 / 34 sheet. This resin-coated metal sheet was overlaid by the same resin coatiricpETlm ^as that OfExample 3 in the same condition as in Example 3 to produce a resin-coated metal sheet. The characteristics of the thus obtained resin-coated metal sheet was evaluated using the same evaluation method as described inExample 1. As a result, the workable adhesion strength is good but numerical value indicating the vivid reflectivity was 0.1 and this was bad.
[0034] (Example 4)The same polyester copolymer paint including brown pigment as that of Example 1 was painted on a galvanized steel sheet as used in Example 1 with a thickness of 5Am, and dried. Further, a transparent soft resin layer consisting of the same polyester resin as used in Example 1 was formed on the above painted metal sheet with a thickness of lOAm. Next, silane coupling agent was painted, with a thickness of 0.3Am, on one side of a transparent biaxial oriented polyethylene terephthalate film having 25 Am thickness and surface roughness Ra of 0.8 which has the other side beforehand top-coated with silicon resin with thickness 2Am, and dried. Thereafter, transparent polyester copolymer resin adhesive was painted thereon with thickness 30Am and dried, and further thereon, grain pattern printing was made with thickness lAm using polyester resin ink to form a resin coating film. The metal sheet provided with the above mentioned soft resin layer was-26·· · · ···· • · • · '97^05^030 (±) 17H35# 0-0041-603-243-4063 fflR:858 P. 28 / 34 further overlaid by the thus prepared resin coating film in the same conuxtiOn as in Example’!’to produce a resin-coated metal sheet. The characteristics of the thus obtained resin-coated metal sheet was evaluated using the same evaluation method as described in Example 1. As a result, numerical value indicating the vivid reflectivity was 0.8 and good and the workable adhesion strength is also good.
[0035] (Example 5)The same polyester copolymer paint including brown pigment as that of Example 1 was painted on a galvanized steel sheet as used in Example 1 with a thickness of 5Am, and dried. Further, a transparent soft resin layer consisting of the same polyester resin as used in Example 1 was formed on the above painted metal sheet with a thickness of 10 Am in the same manner as in Example 1. Next, pattern printing was made, using polyester resin ink, on one side of the same transparent biaxial oriented polyethylene terephthalate film as that of Example 4 which has the other side beforehand top-coated in the same manner as in Example 4, and sequentially solid printing was made thereon (with total thickness of 7Am). Then, the same silane coupling agent as used in Example 4 was painted in the same manner as in Example 4, and thereafter the same transparent polyester copolymer resin adhesive was painted thereon with thickness 30Am and dried. The metal sheet provided with the above mentioned soft resin layer was overlaid-27TO05W(±)17TO 5^:0-0041-603-243-4063 fflR:858 P. 29 / 34 by the thus prepared resin coating film in the same condition as in ΕχβδϊρϊίΓΤ’Χο proaucfe'5”resin-coated metal sheet. The characteristics of the thus obtained resin-coated metal sheet was evaluated using the same evaluation method as described in Example 1. As a result, numerical value indicating the vivid reflectivity was 0.8 and good and the workable adhesion strength is also good.
[0036] [Effect of the Invention]The resin-coated metal sheet of the present invention has a soft resin layer provided between a coloring paint layer and an adhesive layer, or between a coloring paint layer and a printing layer, so that the soft resin layer can absorb the ruggedness due to the surface roughness of metal sheet or the ruggedness of coloring paint layer and printing layer to allow the resin-coated metal sheet to have excellent vivid reflectivity.In addition, the soft resin layer has excellent adhesion strength with regard to the coloring paint layer, printing layer, and adhesive layer, and besides the adhesive layer and the printing layer have excellent adhesion strength with the transparent resin layer so that delamination between the above layers is not at all caused even in severe working such as stretch-forming and deep drawing of the resin-coated metal sheet. Thus, the resin-coated metal sheet of the present invention has excellent workable adhesion strength.• · · 9 9 9 • · · ·· ···· 9 · » 9 99 9 9 9 99 9 9 9 9 9 99 9 9 99 9 9 9999 999 99 99 9 9 9 '97$05^030 (i) 17W S$:0-0041-603-243-4063 fflR:S58 Ρ. 30 / 34 [Brief description of the Drawings]Figure lis‘a schematic ^Section view showing a composition of the resin-coated metal sheet of the present invention;Figure 2 is a schematic section view showing another composition of the resin-coated metal sheet; andFigure 3 is a schematic section view showing still another composition of the resin-coated metal sheet.[Explanation of Reference characters]A : transparent resin filmB : adhesive layerC : sot resin layerD : coloring paint layerPl : solid printing layerP2 ; pattern printing layerS : metal sheet
Claims
CLAIMS 1. A resin coated metal sheet comprising a metal sheet (S) having a surface roughness with the center line average roughness (Ra) greater than 0 Am and not more than 10 Am, in which a coloring paint layer (D), a soft resin layer (C), an adhesive layer (B) and a transparent resin film (A) are laminated at least on one surface of the substrate in this order sequentially from the substrate.
2. A resin-coated metal sheet according to claim 1, wherein the soft resin layer (C) comprises a transparent resin (A).
3. A resin-coated metal sheet according to claim 1, wherein the soft resin layer (C) comprises a mixed resin layer in a not-cured state.
4. A resin-coated metal sheet according to any one of claims 1 to 3, wherein the soft resin layer (C) is a layer coated with a polyester resin.
5. A resin-coated metal sheet according to claim 1 or 2, wherein the soft resin layer (C) is a film comprising polyolefin.
6. A resin-coated metal sheet according to claim 1, wherein the adhesive layer (B) contains a pigment. 7 . A wherein resin-coated metal sheet according the pigment is a metal powder. to claim 6, 8. A wherein resin-coated metal sheet according the pigment is an aluminum powder. to claim 7, 9. A wherein resin-coated metal sheet according the pigment is a mica powder. to claim 7, 10. A resin-coated metal sheet according to claim 1, wherein on both the transparent resin film (A) has a front and back surfaces. mirror surface 11. A resin-coated metal sheet according to claim 1, wherein the transparent resin film (A) is a film formed by biaxially stretching and orienting terephthalate. polyethylene 12. A resin-coated metal sheet according to claim 1, wherein a pattern printed layer (P2), or a pattern printed layer and a solid printed layer (Pl) is disposed between the adhesive layer (B) and the soft resin layer (C).
13. A resin-coated metal sheet according to claim 1, wherein a pattern printed layer (P2), or a pattern printed layer and a multiple negative printed layer is disposed between the adhesive layer (B) and the transparent resin film (A). '97^05^030 (i) 17(835# 0-0041-603-243-4063