Package board
Patent Information
- Application Number
- MYPI1998004731
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 1997-12-10
- Filing Date
- 1998-10-16
- Publication Date
- 1999-04-17
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional package boards face issues with warping due to differences in the area occupied by soldering pads on the IC chip and mother board sides, leading to mechanical stress and potential cracking, which affects connection reliability and signal transmission.
A package board design with a dummy pattern on the IC chip side to adjust the metallic portion ratio, eliminating the need for wires between conductor layers and directly connecting soldering bumps to via-holes, thereby reducing noise and mechanical stress.
The design prevents warping, enhances mechanical strength, reduces noise interference, and ensures reliable connections by adjusting the metallic portion ratio and eliminating wire-related issues.
Abstract
Description
SPECIFICATIONPACKAGE BOARDBACKGROUND ARTThe present invention relates to a package board on which an IC chip is to be mounted, more particularly, a package board provided with soldering pads on its top and bottom surfaces.The soldering pads are connected to the IC chip, as well as to boards such as a mother board, a sub-board, etc.A highly integrated IC chip is mounted on the package board and connected to a mother board, a sub-board, etc. Hereunder, a configuration of this package board will be described with reference to Fig. 23, which is a cross sectional view of the package board 600 provided with an IC chip 80 and mounted on a mother board 90. The package board 600 includes conductor circuits 658A and 658B formed on both surfaces of its core board 630. Furthermore, conductor circuits 658C and 658D are formed in the upper layer of the conductor circuits 658A and 658B with an interlaminar resin insulating layer 650 therebetween respectively. On the upper layer of the conductor circuits 658C and 658D is formed an interlaminar resin insulator 750. In the interlaminar resin insulating layer 650 are formed via-holes 660A and 660B and in the interlaminar resin insulator 750 are formed viarholes 660D and 660C respectively. On the other hand, on the; top surface of the package board on which the IC chip 80 is mounted are formed soldering bumps 676U connected to the pads 82 formed on the IC chip 80 side surface • · of the package board. On the bottom surface of the package board 600 on which a sub-board 90 is mounted are formed soldering bumps 676D connected to the pads 92 formed on the mother boardI side surface of the package board 600. Each of the soldering bumps 676U is formed on a soldering pad 675U. Each of the soldering bumps 676D is formed on a soldering pad 675D. In order to more improve the connection reliability of the soldering bumps 676U and 676D, resin 84 is sealed in a clearance between the IC chip and the package board 600. In the same way, resin 94 is sealed in a clearance between the package board600 and the mother As described connect the highly90. The pads 82 fc board 90.above, the package board 600 is used to integrated IC chip 80 to the mother board irmed on the IC chip 80 side surface are as small as 133 to 170μπι in diameter and the pads 92 formed on the mother board 90 side surface are as large as 600μπι in diameter. Consequently, the IC chip 80 cannot be attached directly to the mother board 90. This is why the package board 600 is disposed between the IC chip 80 and the mother board 90.The package board 600 is formed so as to match both IC chip side soldering pads 675U and mother board side soldering pads 675D with both IC chip side pads 82 and mother board side pads 92 in size respectively. Consequently, the rate of the area occupied by ttie soldering pads 675U on the IC chip side surface of the package board 600 differs from the rate of the area occupied by the soldering pads 675D on the mother board side surface of the package board 600. And, both interlaminar resin insulator 650 and core board 630 are made of resin and the soldering pads 675U and 675D are made of a metal lie material • · · · such as nickel. Consequently, when the resin portions of the interlaminar resin to curing, drying, nsulating layers 650 and 750 are shrunk due etc. in the manufacturing process, the as described above, the package board 6 generated from the shrink repetitively package board is warped toward the IC chip side sometimes. This 5 is because of a difference in the rate of the area occupied by the soldering pads between 675U on the IC chip side surface and675D on the mother board side surface of the package board 600 In addition, when in an actual usage of 10 on which an IC chip is mounted, the heat IC chip makes the package board expand and causing a difference of shrinkage factor between the resin portion and the metallic portion of those soldering pads. And, this results in warping of the package board 600 sometimes.In the case of a multi-layer board used as such a package board, one of a plurality of conductor circuit layers is generally used as i ground layer or a power supply layer to reduce noise or for other purposes. In the case of a multi-layer wiring board manufactured by a conventional technology as showr: in Fig. 23, however, the ground layer (or the power supply layer) is connected to an external terminal via a wire. In other words, wires 658A and 658B (conductor circuits) used as ground layers are formed on the upper layer of the board 630. to the wiring 658DThe wiring (ground layer) 658B is connected -S through a via-hole 660B and the wiring 658D-S is connected to the soldering bump 676U through a via-hole 660D.Since the grdund layer 658D is connected to the soldering bump 676U via the wiring 658D-S in this case, the wiring 658D-S is apt to generate noise and the noise causes malfunctions in electric elements multi-layer wiring such as an IC chip connected to the board. In addition, such the multi-layer wiring board needs a space for wiring in itself and this makes it difficult to r boards.On the other ealize higher integrated printed wiring embodiment as shown 658A and 658B provi are used as a power hand, a package board generally includes capacitors thereiri used to reduce noise from signals transmitted between the IC chip and the mother board. In an inFig. 23, inner layer conductor circuits ded on both surfaces of the core board 630 supply layer and a ground layer, so that capacitors are formed between the core board 630 and the power supply layer and tlie ground layer respectively.Fig. 24A is a top view of the inner conductor circuit layer658B formed on the top surface of the core board 630. On the inner conductor circuit layer 658B are formed a ground layer 638G, as well as land-pads 640 for connecting the top layer to the bottom layer. And, around each of the land-pads 640 is formed an insulating buffer 642.Each of the land-pads 640 consists of a land 640a of a through-hole 636 of the core board 630 shown in Fig. 23, a pad 640b connected to a via-hole 660A going through the upper interlaminar resin insulating layer 650, and a wire 640c connecting the land 640a to the pad 640b.In the case of a package board manufactured by the conventional technology,, the land 640a is connected to the pad640b via the wiring provided between640c. Consequently, the transmission path the upper conductor layer and the lowerΠ ' conductor layer is longer, so that the package board has confronted with prcblems that the signal transmission slows down and the connec Furthermore, at a joint between as at a joint bet respectively. And, corners K due to a the core board 630 / i ting resistance increases, as shown in Fig. 24A, a corner K is formed he wiring 640c and the land 640a, as well ween the wiring 640c and the pad 640b stress is concentrated on each of those difference of thermal expansivity between nterlaminar resin insulating layer 650 made of resin and the land pad 640 made of a metal 1 ic material (copper, a crack Ll to be generated sometimes in the insulating layer 650 as shown in Fig. 23, ng of a wire in the conductor circuit 658D formed in the interlaminar resin insulating etc.). This causes interlaminar resin resulting in breaki or the via-hole 660D 15 layer 650.On the other hand, the mother board 90 side soldering bumps 676D are connected to the inner conductor circuit layer 658C through the via-holes 660D, the wiring 678, and the soldering pads 675. Fig. 24B shows an expanded view (C direction) of both via—hole 660D and soldering bump 675D shown in Fig. 23. A solder ing bump 675 on which a soldering bump 676D formed circularly and connected to a / ia-hole 660D through the wiring 678.repeats the heat cycle between high an operation and cooling down up to the room end of an operation. Since the thermal expansivity differs significantly between the IC chip 80 made of silicon and the package board 600 made of resin, stress is generated in the package board in the heat cycle, causing a crack is mounted is circularly-formed The IC chip temperature during temperature at the n the sealing resin 94 provided between the the mother board 90. And, such a crack by to disconnect the via-hole 660D from the of the package board 600 sometimes. In own in Fig. 24C for an expanded view (D a-hole 660D and the soldering bump 675 shown s a crack L2 causes breaking of the wiring via-hole 660D to the soldering bump 675D on bump 676D is mounted.andL2 to be generated i package board 600 L2 is extended there soldering bump 6751) other words, as sh direction) of the vi in Fig. 23, someti 678 connecting the which the solderingUnder such circumstances, it is an object of the present invention to provide a package board provided with soldering bumps, which can solve the above conventional problems and never ime be warped.It is another object of the present invention to provide a multi-layer wiring board and a multi-layer printed wiring board that are not affected by noise easily.It is also another object of the present invention to provide a package ipoard that can shorten a transmission path upper conductor wiring layer and the lower ayer.nother object of the present invention to formed between the conductor wiring 1 It is also a provide a package board that will never cause breaking of a wire between solderingIn Claim 1 o on the IC chip side the rate of the me pads is also small.jump and via-hole.the present invention, the soldering pads surface of the package board are small, so tallic portion occupied by those soldering On the other hand, the soldering pads on the mother board side surface of the package board are large, so the rate of the metallic portion occupied by those solderingThis is why a dummy pattern is formed ircuit patterns on the IC chip side surface pads is also large between conductor c of the package board thereby to increase the metallic portion and adjust the rate of the metallic portion between the IC chip side surface and the mother board side surface of the package board so as to pro dummy pattern ment meaning such as an just means a patter According to soldering pads on t are small. Thus, ect the package board from warping. The ioned above does not have any functional electrical connection and a capacitor. It n formed mechanically.the invention defined in Claim 2, the re IC chip side surface of the package board the metallic portion occupied by the soldering pads is less than that of the mother board side surface of the package boa’d, where the soldering pads are large and the metallic portion occupied;by the soldering pads is large. This is why a dummy pattern is formed at the outer periphery of each conductor circuit on the IC chip side surface of the package board thereby to increase the metallic portion thereon and adjust the rate of the metallic portion on the package board surface between the IC chip side and the mother board side. This metallic dummy pattern is also effective to improve the mechanical strength of the outer periphery of the package board, the package board from warping, the package board defined in Claim 3, a power as well as protect According to supply layer and / or a ground layer is formed as an inner layer conductor circuit supports the oute formed under an insulating layer that most layer conductor circuits. Then, avia-hole is connected directly to the second conductor circuit and a solder bump is formed in the via-hole. It is therefore not necessary to prcvide a wire for connecting the power supply layer or the ground layer to the soldering bumps. Consequently, s free of any noise to be mixed in wires, he package board defined in Claim 4, a power supply and / or a grohnd layer is formed as the second conductor circuit disposed unqer the second interlaminar resin insulating s the conductor circuits formed in the A via-hole is connected directly to the rcuit and a soldering bump is formed in the via-hole. It is therefore not necessary to provide a wire for connecting the power supply layer or the ground layer to the soldering bumps. Consequently, the package board is free of ed in wires.the package board defined in claims 5 and the package board i According to layer that support outermost layer, second conductor ci any noise to be mi According to6, each land and ea,ch pad are formed integrally and connected directly to each other without using a wire. It is thus possible to shorten the transmission path provided between upper and lower conductor layers, as well as to reduce the connecting resistance significantly. In addition, since the land and the pad aie connected directly to each other without 'ess is concentrated at a joint between wiring is at a joint between wiring and pad. It is using a wire, no str and land, as well a thus possible to protect the package board from breaking of a wire to be caused stress.According tc soldering bump is by a crack generated by such concentrated the package board defined in Claim 7, a ormed in a via-hole, so that each soldering •ft ·· ·· · ········ • ···· ··· · · • · · · ·· ····· · ·bump is connected direct ly to a via-hole. Therefore, even when the package board is cracked, it is prevented that breaking of a wire occurs between the soldering bump and the via-hole. In other words, the conventional package board, where a soldering a via-hole through a wire and a soldering bump is formed on έ soldering pad, cannot avoid crack-caused breaking of a wire connecting via-holes to soldering pads. A soldering bump is thus disconnected from a via-hole due to such a crack generated inside the package board. The package board defined in Claim f, however, is completely protected from caused by such a crack.the package board defined in Claim 8, a breaking of a wire According to soldering bump is formed in a via-hole, so that each soldering bump is connected possible to prevent directly to each via-hole. It is thus breaking of a wire between a soldering bump and a via-hole even when the package board is cracked. Such a soldering bump is also formed in a plurality of via-holes respectively in this case. It is possible to utilize a fail-safe, since the soldering bump can be connected to another via-hole when one of the via-holes is disconnected from the soldering bump. In addition, since a soldering bump is formed on a plurality of via-holes, a soldering bump can be formed larger to each via-holeIn the pres ent invention, a dummy pattern may be electrically connec ted to a power supply layer or a ground layer, or may be the power supply layer or a ground layer, for reducing noise in signal lines.• · · · · · ·ίοBRIEF Fig. 1 is a c a first embodiment Fig. 2 is anX board shown in Fig.Figs. 3 to F the package board invention.Fig. 10 is a in a second embodinlent of the present invention.DESCRIPTION OF THE DRAWINGS oss sectional view of the package board in of the present invention.-XI 1 ine cross sectional view of the package 1.ig. 9 illustrate manufacturing processes of in the first embodiment of the present cross sectional view of the package boardFig. 1 IA is a embodiment and Fig.Fig. 12 is a shown in Fig. 10 whe thereon is attachec top view of the package board in the second11B is a bottom view of an IC chip, cross sectional view of the package board n the package board with an IC chip mounted to a mother board.Fig. 13 is a cross sectional view of a mul ti-layer printed wiring board in a Fig. 14 is a a variation of the m embodiment of the present invention, hird embodiment of the present invention, cross sectional view of a configuration of nlti-layer printed wiring board in the thirdFig. 15 is a cross sectional view of the package board in the fourth embodiment of the present invention.Fig. 16A is a in the fourth embod board is formed an top view of a core board of the package board ment of the present invention. On the core inner layer copper pattern. Fig. 16B is an expanded partial top view of Fig. 16A.Fig. 17 is a cross sectional view of a package board composed as a variation of the package board in the fourth embodiment of the present invention.Fig. 18A is a top view of a conductor circuit formed on a package board composed as a variation of the package board in the fourth embodiment of the present invention. Fig. 18B is an expanded partial top view of Fig. 18A.Fig. 19 is a cross sectional view of the package board in a fifth embodiment of the present invention.Fig. 20 is a cross sectional view of the package board shown in Fig. 19 when the package board with an IC chip mounted thereon is attached to a mother board.Fig. 21 is 8-cross sectional view of a package board ation of the package board in the fifth embodiment of the bresent invention.Fig. 22 is an X5-X5 line cross sectional view of the package board shown in Fig. 21.Fig. 23 is a cross sectional view of a prior art package board.Fig. 24A is a shown in Fig. 23, F composed as a var top view of an inner layer conductor circuit g. 24B is a C-l ine view of Fig. 23, and Fig.24C is a D-line view of Fig. 23BEST MOD' (First Embodiment) Hereunder, a first embodiment of reference to Fig. the package board in this first embodFOR CARRYING OUT THE INVENTION configuration of the package board in the the present invention will be described wi th 1. Fig. 1 shows a cross sectional view of in the first embodiment. The package board iment is a so-called IC package provided wi th an IC (not i 1 lust rated) mounted thereon and attached to a mother board (not illustr ated). The package board is provided with • ·Both soldering bumps the IC and the moth soldering bumps 76U on its top surface and soldering bumps 76D on its bottom surface. Each of the soldering bumps 76U is connected to a soldering bump of the IC and each of the soldering bumps 76D is connected to a soldering bump of the mother board.76U and 76D are used to pass signals between er board, as well as relay a supply power from the mother board to other parts.On both top and bottom surfaces of a core board 30 of the package board are formed inner layer copper patterns 34U and 34D, which are usee as ground layers. In the upper layer of the inner layer copper pattern 34U is formed a conductor circui t 58U, as well as a dummy pattern 58M for forming a signal line with an interlaminar resin insulating layer 50 therebetween. In addition, avia-hole 60U is formed through the interlaminar resin insulating layer 50. In the upper layer of the conductor circuit 58U and the dummy pattern 58M is formed a via-hole 160U respectively with an interlaminar resin insulating layer 150 therebetween. The via-hole 160U goes through both outermost conductor circuit 158U and interlaminar resin insulating layer 150. And, a soldering pad 75U is formed both in the conductor circuit 158U and ir the via-hole 160U. The soldering pad 75U is used to support a soldering bump 76U. Each IC chip side soldering pad 75U ia formed so as to be 133 to 170μπι in diameter.On the other band, in the upper layer of the ground layer (inner layer copper pattern) 34D formed on the bottom surface of the core board 30 (the upper layer mentioned here means a layer formed on the top surface and the lower layer means a layer formed on the bottom surface of the board 30 respectively) is formed a conductor circuit 58D for forming a signal line with ·· ·· ·· · ···!···· ······· * · • ···· · · · · · ···· ·· ····· · ·• · · · · · · · · · an interlaminar res upper layer of the n insulating layer 50 therebetween. In the conductor circuit 58D is formed a via-hole160D through both an outermost layer conductor circuit 158D and an interlaminar res resin insulating la 75D is formed both in insulating layer 150 with an interlaminar yer 150 therebetween. And, a soldering pad in the conductor circuit 158D and in the via-hole 160D. The soldering pad 75D is used to support a soldering bump 76D. is formed so as toFig. 2 shows 1. In other words,Each mother board side soldering pad 75D be 600μπι in diameter, an Xl-Xl line cross sectional view of Fig. Fig. 2 shows a cross sectional view of the package board. The Xl-Xl line cross sectional view in Fig. 2 is equal to Fig. 1. As shown in Fig. 2, a dummy pattern 58M is formed between conductor circuits 58U forming signal lines. A dummy pattern mentioned here means a pattern just formed mechanical ly; i t has no functional meaning such as an electrical connection, a capacitor, etc.Just 1 ike the prior art package board described above wi th reference to Fig. 23, according to the package board in the first embodiment of the present invention, each soldering pad disposed on the IC chip side surface is small (133 to 170μπι in diameter), so the metallic portion occupied by such soldering pads is also small pad is large (600μπι (bottom) of the pi occupied by the soOn the other hand, since each soldering in diameter) on the mother board side surface ckage board, a larger metallic portion is ldering pads. This is why a dummy pattern58M is formed between conductor circuits 58U forming a signal line respectively on the IC chip side surface of the package board thereby to increase the metallic portion and adjust the • · rate of the metal 1ic between the IC chip possible to protec portion on the surface of the package board side and the mother board side. It is thus :t the package board from warping in the manufacturing processes to be described later, as we 11 as during a usage of the package board.Next, how to manufacture the package board shown in Fig.wi11 be described concretely. At first, descript ion wi11 be made for A. Electroless Plating Binding Material, B.Interlaminar ResinA. Raw MaterialInsulating Material, C. Resin Filler, andD. Solder Resist Composition in orderCompositions for Manufacturing a BindingMaterial for Electroless Plat ing (Upper Layer Binding Material) [Resin Composition This resin stirring 35 weight (1)] composition was obtained by mixing and parts of a resin solution obtained by dissolving 25% acrylic-modified cresol novolac epoxy resin (Nippon Kayaku, mol ar weight 2500) into DMDG at a concentration of 80wt%; 3. 15 weight parts of photosensitive monomer (Toagosei,ARONIX M315); 0. 5 we ight part of an anti-forming agent (SANN0PC0,S-65); and 3. 6 weight parts of NMP.[Resin Composition (2)]This resin composition was obtained by mixing 12 weight parts of polyether-sulfone (PES); 7.2 weight parts of epoxy resin particles (Saiyo Chemical Industries, Polymer Pole) 1. Ομίη in average diameter; and 3.09 weight parts of the same epoxy resin particles 0. 5 am in average particle diameter; then adding 30 weight parts of NMP to the mixture and stirring the mixture using a beads mill.[Hardener Composition (3)]This hardener composition was obtained by mixing and stirring 2 weight parts of an imidazole hardener (ShikokuChemicals, 2E4MZ0CN); 2 weight parts of a photo-initiator (CibaGeigy, Irgacure 1-907); 0.2 weight part of a photosensitizer (Nippon Kayaku, DE1X-S); and 1.5 weight parts of NMP.B. Raw Material Compositions for Manufacturing anInsulating Material (Lower Layer BindingInterlaminar Resin Material) [Resin Composition (1)]This resin composition (1) was obtained by mixing and stirring 35 weight parts of a resin solution obtained by dissolving 25% acrylated cresol novolac epoxy resin (Nippon Kayaku, molar weigit 2500) into DMDG at a concentration of 80wt%; 4 weight parts of photosensitive monomer (Toagosei, AR0NIXM315); 0.5 weight part of an ant i-forming agent (SANN0PC0, S-65); and 3.6 weight parts of NMP.[Resin Composition This resin c (2)] :omposition (2) was obtained by mixing 12 weight parts of polyether-sulfone (PES); 14. 49 weight parts of epoxy resin particles (Sanyo Chemical Industries, Polymer Pole) 0. 5μπι in average diameter; then adding 30 weight parts of NMP to the mixture and [Hardener Compos it stirring the mixture using a beads mill, on (3)]This hardened· composition (3) was obtained by mixing and stirring 2 weight parts of an imidazole hardener (Shikoku Chemicals, 2E4MZ0CL·); 2 weight parts of a photo-initiator (Ciba Geigy, Irgacure 1-907); 0.2 weight part of a photosensitizer (Nippon Kayaku, DETX-S); and 1.5 weight parts of NMP.C. Raw Material Compositions for Manufacturing a Resin FiHer [Resin Composition This compos it100 weight parts of (1)] ion (1) was obtained by mixing and stirring bisphenol F type epoxy monomer (Yuka Shell, molecular weight 310, YL983U); 170 weight parts of SiO, ball-like particles (Admatec, CRS 1101-CE, the maximum size of particles should be the thickness (15μΐη) of the inner layer copper pattern to be described later) 1. 6μΐη in average diameter, when their surfaces are coated with a silane coupling agent; and 1. 5 weight parts of a leveling agent (SANN0PC0, PERENOL S4); then adjusting the viscosity of the mixture to 45, 000 to 49, 000 cps at 23 ± 1 °C.[Hardener Composition (2)]6. 5 weight parts of imidazole hardener (Shikoku Chemicals, 2E4MZ-CN)D. Solder Resist GompositionThis solder resist composition was obtained by mixing46. 67g of photosensitive oligomer (molecular weight 4000) obtained by acrylic-modifying 50% of epoxy groups of 60 percentage by weight of cresol novolac dissolved into DMDG of 50% epoxy resin (Nippon Kayaku); 15. Og of 80 percentage by weight of bisphenol A type epoxy resin (Yuka Shell, Epikote 1001) dissolved into methyl ethyl ketone; 1. 6g of imidazole Chemicals, 2E4MZ-CN); 3g of multivalent ppon Kayaku, R604) which is photoreceptive ; same multivalent acryl ic monomer (KY0EISHA 0. 71g of a scattering anti-foaming agent then adding 2g of benzophenone (ΚΑΝΤΟ photoinitiator; and 0.2g of Michler’s ketone ;ed as a photosensitizer to the mixture and hardener (Shikoku acrylic monomer (N monomer; 1. 5g of th CHEMICAL, DPE6A); (SANNOPCO, S-65) ; CHEMICAL) used as a (ΚΑΝΤ0 CHEMICAL) u adjusting the viscosity to 2. OPa-s at 25 °C.A rotor No. 4 \ used to measure the viscosity meter (To iscosi ty meter (Tokyo Keiki, DVL-B type) was viscosity at 60 rpm and a rotor No. 3 B type kyo Keiki, DVL-B type) was used to measure the viscosity at 6ifpm.Next, description will be made for how to manufacture a package board 100 with reference to Figs. 3 to 9.Manufacturing a Package Board (1) A copper-clad laminate 30A was obtained at first by laminating 18μΐπ copper foil 32 on both surfaces of a board 30 made of glass epoxy resin or BT (bismaleimide triazine) resin of 1mm in thickness (process A in Fig. 3). After this, the copper-clad laminate 30A was drilled to make holes, then e1ectro1ess-plated and etched for patterning thereby to form inner layer copper patterns 34U and 34D on both surfaces of the board 30 and make through-holes 36 in the board 30 (process (B) in Fig. 3)).(2) After forming the inner layer copper patterns 34U and ough-holes 36, the board 30 was washed inThen, the board was treated with34D, as well as th water and dried.oxidation-reduction using NaOH (10g / l), NaC102 (40g / l), andNa3P04 (6g / l) as ox idation bathing (blackening bathing) agents and using NaOH (10g / l) and NaBH4 (6g / l) as reduction agents thereby to form a rough layer 38 on the surface of each of the inner layer copper patterns 34U and 34D, as well as the through-holes 36 (process (C) in Fig. 3)).(3) The raw material compositions for adjusting the resin filler in C were mixed and stirred to obtain a resin filler.(4) The res in filler 40 obtained in (3) was coated on both surfaces of the board 30 within 24 hours after the manufacturing using a roll coating device thereby to fill a clearance between the conductor circuits (inner layer copper patterns) 34U, as well as in the through-holes 36. The filler was then dried at 70 °C for 20 minutes. On the other surface, the resin filler 40 was filled in a clearance between the conductor circuits 34D or in the through-f.oles 36 and dried at 70 °C for 20 minutes (process (D) in Fig. 3)).(5) After the treatment (4), one surface of the board 30 was sanded using a belt sanding machine and a #600 belt sand paper (Sankyo Ri kagaku) to remove the resin f i 1 ler 40 completely from the surfaces of both inner layer copper patterns 34U and 34D, as well as from the surface of the land 36a of each through-hole 36. After this, the surface of the board 30 was buffed to remove scratches made by the belt sanding. Such a series of sanding was also carried out for the other surface of the board in the same way (process (E) in Fig. 4)).;he resin filler 40 was hardened by baking ur, at 120 °C for three hours, at 150 °C for °C for seven hours respectively, the surface layer of the resin filler 40 wasAfter this, at 100 °C for one hc one hour, and at 1In this way, removed from the through-holes 36, etc., and the rough layer of the top surface and 34D was removed of the inner layer conductor circuits 34U thereby to smooth both surfaces of the board30. It was thus possible to obtain a wire board on which the resin filler 40 was of the inner layer therebetween, as we in close contact with side surfaces of each conductor circuits 34 with a rough layer 38 11 as the resin fi 1 ler 40 was in close contact with the inner wall of each through-hole 36 with a rough layer therebetween, to align the surface copper pattern 34 cIn other words, this process was effective s of the resin filler 40 and the inner layer n the same level.(6) After forming the conductor circuits 34U and 34D, the 5 board 30 was alkaline-degreased for soft-etching, then the board 30 was treated with a catalyst solvent consisting of pal ladium chloride and organic acid thereby to add a Pd catalyst. The catalyst was then activated, and the board 30 was dipped in an electroless plating solvent consisting of 3. 2 χ 10'2mol / 1 of copper sulfate, 3. 9 χ 10-3mol / 1 of nickel sulfate, 5. 4 χ 10'2xing agent, 3.3 χ 10'1mol / 1 of sodium χ 10'1mol / 1 of boracic acid, 0. lg / 1 of a surface active agent (Nissin Chemical Industry, Surfynol 465), and PH=9. One minute later, the board 30 was vibrated in both ital directions once every 4 seconds thereby ike alloy coating layer consisting of Cutr 42 on the surfaces of each of the conductor 1 as on the surface of the land 36a of each mol / 1 of a comple hypophosphite, 5.0 vertical and horizo to form a needle-1 Ni-P and a rough lay circuits 34, as wel of the through-holes 36 (process (F)) in Fig. 4).Furthermore, an Sn layer of 0. 3μΐη in thickness (not illustrated) was formed on the surface of the rough layer by a Cu-Sn substitution reaction on the conditions of 0. 1 mol / 1 of boracic stannoup fluoride, 1.0 mol / 1 of thiocarbamide, 35 °C, and PH= 1. 2.(7) The raw interlaminar resin mixed thereby to o lower layers). Th to 1. 5 Pa-s.material compositions used to adjust the insulator obtained in B were stirred and btain an interlaminar resin insulator (for e viscosity of the layer was then adjusted • · · · · 9 9 · tt · · ·After this, the raw material compositions used to manufacture a binding material of electroless plating obtained in A were stirred ani mixed thereby to obtain a binding solution (for the upper layer) for electroless plating. The viscosity of the solution was then adjusted to 7 Pa-s.(8) Both surfaces of the board obtained in (6) were coated with an interlaminar resin insulation material (for lower layers) 44 of 1. 5 Pa-s in viscosity using a roll coating device wi thin 24 hours after the solution was manufactured. Then, the board was left horizontally for 20 minutes, then dried (prebaking) at 60 °C for 30 minutes. After this, the board was coated with a sensitive binding solution 46 (for upper layers) of 7 Pa-s in viscosity obtained in (7) within 24 hours after the solution was manufactured, then the board was left horizontally for 20 minutes. Then, the board was dried (prebaking) at 60 °C for 30 minutes thereby to form a binding material layer 50a of 35μΐη in thickness (process (G) in Fig. 4)).(9) A photo-masking film (not illustrated) provided with85μπιφ printed black circles was stuck fast to each surface of the board 30 on which a binding layer was formed respectively in (8), then exposed at 500 mJ / cm2using a super high voltage mercury lamp. A DI1TG solution was then sprayed on the black circle for developing. Furthermore, the board 30 was exposed at 3000 mJ / cm2using a super high voltage mercury lamp, then heated (post-baking) at 100 °C for one hour, at 120 °C for one hour, and at 150 °C for 3 hours thereby to form an interlaminar resin insulating layer (two-layer structure) of 35μΐη in thickness. The layer was thus provided with 85 μπιφ openings (used to form via-ho functioning equally les), which were excel lent in size accuracy, to a photo-masking film (process (H) inFig. 5)). The tinned lafer (not illustrated) was partially exposed in each of the openings 48 to be used as via-holes.(10) The board 30 provided with the openings 48 was then id for 19 minutes thereby to melt and remove the surface of the interlaminar resin and make the surface rough (process (I) in dipped in chromic ac epoxy resin from insulation layer 50Fig. 5)). After this, the board 30 was dipped in a neutral ized solution (SHIPLEY), then washed by water.A palladium catalyst (Atotech) was thus applied to the roughened surface ( catalytic nuclei o insulating layer 50 oughened depth 6μπι) of the board 30 to stick n the surface of the interlaminar resin as well as the inner wall surface of each of the via-hole openings 48 (11) The boai plating water solut d was then dipped in an electroless copper on consisting of the following compositions thereby to form an electroless copper plating film 52 of 0. 6μπι in thickness on the whole rough surface of the board 30 (process (J) in Fig. 5)).[Electroless Plating Water Solution]EDTA... 150 Copper sulfa HCHO...g / 1e...g / 1 ml / 1 40 g / 1NaOH...a, a’ - bipyridyl... 80 mg / 1PEG... 0. 1 g / 1 [Electroless Plating Conditions] min. at a solution temperature of 70 °C > · · « » · · · • · · · « • · « • · · · (12) A market-sold photosensitive dry film was stuck on the electroless copper plating film 52 formed in (11), then a mask was put on the film for exposing at 100 mJ / cm2and for developing using 0.8% sodium thereby to form a plating resist 54 of 15pun in thickness (process (K) in Fig. 6)).(13) After this, the no-resist-formed portion was plated with electrolytic copper thereby to form an electrolytic copper plated film 56 of 15μΐη in thickness (process (L) in Fig. 6)).ng Water Solution]180 g / 1 ;e... 80 g / 1Additive (Atdtech Japan, Cupracid GL)... 1 ml / 1 [Electrolytic Plat ng Conditions]Current density... lA / dm2Time... 30 inin.Temperature... Room temp.(14) The plat ing resist 54 was separated and removed wi th 5%K0H, then the electroless plated film 52 under the plating resist was melted and removed with etching treatment using a mixed solution of sulfuric acid and hydrogen peroxide thereby [Electrolytic PlatSulfuric acid... Copper sulfa to form conductor circuits 58U and 58D of 18μΐη in thickness respectively, as well as via-holes 60U and 60D consisting of er plated film 52 and an electrolytic copper oectively (process (M) in Fig. 6)).an electroless copp plated film 56 res (15) The same treatments as those in (6) were carried out to form a rough sur of the conductor ci ace 62 consisting of Cu—Ni—P on the surfaces rcuits 58U and 58D, as well as the surfaces of the via-holes 60U and 60D. Furthermore, Sn displacement was carried out for the rough surface 62 (process (N) in Fig. 7)).► · · · to · · · • · · · (16) The pro conductor circuits ;esses (7) to (15) were repeated to form in a further upper layer. In other words, both surfaces of the board 30 were coated with an interlaminar resin insulating material (for lower layers) using a roll coating device to form an insulating layer 144. In addition, this insulating layer 144 was coated with a photosensitive binding material (for upper layers) using a rol 1 coating device to form a binding material layer 146 (process (0) in Fig. 7)). After this, a photo-masking film was stuck fast to both surfaces of the board 30 on then exposed and which the layers 144 and 146 were formed, developed to form an interlaminar resin insulating layer 150 provided with openings (via-holes 148).The surface of the then roughened (pi electroless copper surface of the boa nterlaminar resin insulating layer 150 was ocess (P) in Fig. 7)). After this, an plated film 152 was formed on the roughened rd 30 (process (Q) in Fig. 8)). It was followed by forming of a plating resist 154 on the electroless copper plated film copper plated film152, then by forming of an electrolytic156 on the no-resist-coated portion of the film 152 (process (R) in Fig. 8)). The plating resist 154 was then separated and removed with KOH, and the electroless plated plating resist 54 was melted and removed thereby to form conductor circuits 158U and 158D, as well as via-holes 160U and 1601) (process (S) in Fig. 8)). Then, aI roughened layer 162 was formed on the roughened surface 162 formed on the surfaces of the conductor circuits 158 and the via-holes 160 (process (T) in Fig. 9)). No Sn displacement was carried out for the roughened surface 162 at this time.(17) Both surfaces of the board 30 obtained in (16) werecoated with a solder resist composition 70a described in D at a thickness of 45μπι. The board 30 was then dried at 70 °C for 20 minutes, then at 70 °C for 30 minutes. After this, a photo-masking film (not illustrated) of 4mm in thickness on which circles (masking pattern) were drawn was stuck fast to both surfaces of ttie board 30 respectively, then exposed with an ultraviolet beam' of 1000 mJ / cm2and developed with DMTG. In addition, the board 30 was baked at 80 °C for 1 hour, at 100 °C for 1 hour, at 120 °C for 1 hour, and at 150 °C for 3 hours thereby to form a solder resist layer (20μπι thick) provided with an opening (200μΐη diameter) 71 at each soldering pad (including the via-hole and i (18) After th nickel plating solu plated layer 72 of s land) (process (U) in Fig. 9)). is, the board 30 was dipped in an electroless ion of pH=4. 5 for 20 minutes to form a nickel 5μΐη in thickness. The electroless nickel plating solution consisted of 2. 31x10'1mol / 1 of nickel chloride,2. 8x10_1mol / 1 of s sodium citrate. TI gold plating soluti jdium hypophosphite, and 1.85x10'* mol / 1 of e board 30 was then dipped in an electroless on for 7 minutes 20 seconds at 80 °C to form a gold plated layer 74 of 0. 03μπι in thickness on the nickel plated layer, so t hat soldering pads 75U and 75D were formed on the via-holes 160U and 160D, as well as on the conductor circuits 158U and 158D (see Fig. 1). The electroless gold plating solution consisted of 4. lxlO'2mol / 1 of gold potassium cyanide, 1. 87x10'* Lo 1 / 1 of ammonium chloride, 1. 16x10* mol / 1 of sodium citrate, and 1. 7x10'* mol / 1 of sodium hypophosphite.(19) Soldering paste was printed in the openings 71 of the solder resist 1 soldering bumps (so lyer 70 and reflowed at 200 °C thereby to form ldering bodies) 76U and 76D. This completed • · · ·« manufacturing of the package board 10 (see Fig. 1).Although the additive process in the present inventi formed with the fu package board was formed with the semithe above embodiment, the configuration of on may also apply to a package board to be 1-additive process, of course.Although a dunmy pattern 58M is formed between conductor circuits 58U formed between the interlaminar resin insulating layer 50 and the interlaminar resin insulating layer 150 in the first embodiment, such a dummy pattern 58M may also be formed between the inner layer copper patterns 34D formed on the core board 30 or between outermost layer conductor circuits 158U.As described above, according to the package board in the first embodiment, a dummy pattern is formed between conductor circuits that form signal lines on the IC chip side surface of the package board thereby to increase the metallic portion on the IC chip side surface of the package board and adjust the rate of the metallic portion between the IC chip side and the mother board side on the package board. It is thus possible to protect the package board from warping in the manufacturing processes, as well (Second Embodiment) Hereunder, a second embodiment o wi th reference to Fi view of the package is a top view of the as during operation.configuration of the package board in the f the present invention will be described gs. 10 to 12. Fig. 10 is a cross sectional board in the second embodiment. Fig. 11A package board and Fig. 1 IB is a bottom view of an IC chip mounted on the package board. Fig. 12 illustrates how the IC chip 80 shown inFig. 10 as s mounted on the top of the package board i cross sectional view of the package board ··· ··· · mounted on a mother board 90. The package board is provided with soldering bumps 76U on its top surface and soldering bumps 76D on the bottom surface as shown in Fig. 12. Those bumps are connected to the bumps 82 of the IC chip 80 and the bumps 92 of the mother board 90 respectively. Those bumps are used to pass signals between the IC chip 80 and the mother board 90, as well as relay a supply power from the mother board to other parts.As shown in Fig. 10, on both top and bottom surfaces of the core board 30 o copper patterns 341 In the upper layer formed a conductor50.the f the package board are formed inner layer and 34D, which are used as ground layers, of the inner layer copper pattern 34U is circuit 58U for forming a signal line with an interlaminar re^in insulating layer 50 therebetween and a via-hole 60U through the interlaminar resin insulating layer In the upper layer of the conductor circuit 58U are formed lalyer conductor circuits 158U with an outermost interlaminar resin as via-holes 160U interlaminar resin insulating layer 150 therebetween, as well through both a dummy pattern 159 and an nsulating layer 150. The dummy pattern 159 is formed at the outer periphery of each of the conductor circuits 158U as shown in Fig. 11, that is, along the circumference of the package board. On each of the conductor circuits 158U and via-holes 160U is formed a soldering pad 75U for supporting a scldering bump 76U. The soldering pads 75U on the IC chip side surface are formed so as to be 120 to 170μπι in diameter.On the other hand, in the upper layer of the ground layer (inner layer copper pattern) on the bottom side of the core board • · · · • · • · · • · • · are formed conductor circuits 58D for forming signal lines with the interlaminar resin insulating layer 50 therebetween. In the upper layer of the conductor circuits 58D are formed the outermost layer conductor circuits 158D with the interlaminar resin insulating layer 150 therebetween, as well as via-holes 160D through the interlaminar resin insulating layer 150. On each of the conductor circuits 158D and the via-holes 160D is formed a soldering pad 75D for supporting a soldering bump 76D.75D on the mother board side surface are 600 to 700μπι in diameter.top view of the package board 200, that is, ig. 10. Fig. 10 is equal to the X2-X2 line ional view of Fig. 11A. As shown in Fig. the outer periphery of each of the conductor orming signal lines on the lower layer of the solder resist 70 is formed a lOmm-wide dummy pattern 159. The dummy pattern mentioned here means a pattern formed just mechanically; it has no functional meaning such as an electric connection, capacitor, etc.Like the package board manufactured with the prior art h reference to Fig. 23, according to the second embodiment, the IC chip 80 side (top) surface of the package board is provided wi th smaller soldering pads 76U (120 to 170μΐη in diameter), so the metallic portion occupied by those soldering pads on the surface of the package board is also small. On the other hand, the mother board 90 side (bottom) surface of the package board is provided with larger soldering pads 75D (600 to 700μΐη in diameter), so the metal 1 ic portion occupied by those soldering pads on the surfaceThe soldering pads formed so as to be Fig. 11A is a an A-line view of F vertical cross sec 11A and Fig. 10, at circuits 158U for :described above wi package board in the • · · » · · · · · of the package board is also large. This is why the package board in this embodiment forms a dummy pattern 159 at the outer periphery of each of the outermost layer conductor circuits 158U on the IC chip side surface of the package board thereby to increase the metal 1 of the metallic por board side on the iC portion on the surface and adjust the rate ion between the IC chip side and the mother surface of the package board. The dummy patterns 159 are also effective to improve the mechanical strength of the circumference of the package board, protecting the package board from warping in the manufacturing processes, as well as during operation.Fig. 11A shows a top view (A-line view of Fig. 10) of a completed package board and Fig. 1 IB shows a bottom view of an IC chip. The package board 100, while the IC chip 80 is put thereon, is passed through a reflowing oven to fix the IC chip on the package board through the soldering bumps 76U as shown in Fig. 12. After Ihis, the package board 100 with the IC chip mounted thereon is mounted on a mother board 90, then passed in a reflowing oven thereby to fix the package board on the mother board 90.How to manufacture the package board in this second embodiment to the fifth embodiment to be described later will be omitted here, since it is the same as the method described in the first embodiment with reference to Figs. 3 to 9.In the second embodiment described above, a dummy pattern 159 is formed around each of the outermost layer conductor circuits 158U formec. on the interlaminar resin insulating layer 150. However, the dummy pattern 159 may also be formed around each conductor circuit 58U formed between inner layer copper ···· ··· 4 »· · ·· ····· · » · · · · · ··· ···· 4 • · · 4 • · · ·As described second embodiment, and adjust the rate side and the mothe board, protectingHereunder, a third embodiment of reference to Fig.patterns 34D or around each of the conductor circuits 58U formed between the interliminar resin insulating layers 50 and 150.above, according to the package board in the a dummy pattern is formed around each conductor circuit on the IC chip side surface of the package board thereby to increase the metallic portion on the surface of the metallic portion between the IC chip : board side on the surface of the package the package board from warping in the manufacturing processes, as well as during operation.(Third Embodiment) configuration of the package board in the the present invention will be described wi th3.The core board 30 of the package board 300 is provided with inner layer copper patterns 34U used as signal lines and formed on its top surface, as well as inner layer copper patterns 34D used as signal lines and formed on its bottom surface respectively. In the upper layer of each inner layer copper pattern 34U is formed a conductor circuit 58U that forms a power isupply layer with the interlaminar resin insulating layer 50 therebetween. In the upper layer of each conductor circuit 58U is formed an outermost layer conductor circuit 158 with the interlaminar resin as a via-hole 160U layer 150. In the v insulating layer 150 therebetween, as well through the interlaminar resin insulating ia-hole 160U is formed a soldering bump 76U.In other words, the package board is composed in the third embodiment so that hole 160U connected a soldering bump 76U is formed on a viato a conductor circui t 58U that forms a powerΓ supply layer. The power supply layer can thus be connected directly to an external bump (not illustrated).On the other hand, a conductor circuit 58D used as a ground layer is formed in the upper layer of a signal line (inner layer ID with the interlaminar resin insulating ;en on the bottom side of the core board 30. of each conductor circuit 58D is formed an outermost layer conductor circuit 158D with the interlaminar resin insulating layer therebetween 150, as well as a via-hole 160D through the interlaminar resin insulating layer 150. A soldering bump 76D is formed on the via-hole 160D. In other words, the package tioard is composed in this embodiment so that a soldering bump 76p is formed on a via-hole 160D connected to 58D composing a ground layer. The ground layer can thus be connected directly to an external bump (not i1 lustrated).According to the package board configuration in this embodiment, the conductor circuits 58U and 58D disposed under the interlaminar resin insulating layer 150 supporting the conductor circuits 158U and 158D in the outermost layer are used as a power supply layer and a ground layer. And, via-holes 160U ted directly to the conductor circuits 58U ing bumps 76U and 76D are formed in the ely. Consequently, it is not necessary to supply layer or ground layer directly to The package board is thus protected from copper pattern) 34 layer 50 therebetwe In the upper layer and 160D are connec and 58D, and solde via-holes respectiv connect any power soldering bumps, noise mixed in wires. It is thus possible to reduce the influence of noise expected while passing signals between theIC and the mother board, as well as while relaying a supply power from the mother board to other parts. In addition, since there are less wires, the multi-layer printed wiring board (package board) can be packed more densely. According to the multilayer printed wiring board in this embodiment, a conductor circuit 58U is used as a power supply layer and a conductor circuit 58D is used as a ground layer. The conductor circuit 58U or 58D, however, may be formed in the same layer together with other conductor circuits functioning as a power supply layer and a ground layer respectively.Next, a description wil 1 be made for a multi-layer printed wiring board composed as a variation of the third embodiment with reference to Fig. 14.Fig. 14 is a cross sectional view of a configuration of the multi-layer printed wiring board in the second embodiment of the present invention. On both top and bottom surfaces of the core board 230 are formed inner layer copper patterns 234U and 234D used as ground layers. In other words, capacitors are formed wi th the ground layers (inner layer copper pat terns) 234U and 234D that face each other with the core board therebetween.Furthermore, on the upper layer of the inner layer copper pattern 234U are formed a conductor circuits 258U that form signal lines with the interlaminar resin insulating layer 250 therebetween. In the upper layer of the conductor circuits 258U are formed via-holes 360U through the interlaminar resin insulating layer 350. And, a soldering bump 376U is formed on each of those via-holes 360U.On the other hand, in the upper layer of the ground layer (inner layer copper pattern) 234D formed on the bottom surface of the board 230 is formed a conductor circuit 258D that forms• · · · · · · · ·· · a signal 1ine wi th the interlaminar resin insulating layer 250 therebetween. In the upper layer of the conductor circuit 258D is formed a conduct with the interlamin In the upper layer or circuit 388D used as a power supply layer ar resin insulating layer 350 therebetween, of the conductor circuit 388D is formed a via-hole 380D throrgh the interlaminar resin insulating layer 390. And, a solder ing bump 376D is formed in the via-hole 380D. In other words, a soldering bump 376D is formed in a via-hole 380D connected to a conductor circuit 388D used as a power supply layer. The power supply layer can thus be connected directly to an external bump (not illustrated).embodiment, a via-hole 380D is connected directly to the conductor circuit 388D used as a power supply layer and a soldering bump 376D is formed in a via-hole.s not necessary to provide a wire for connecting the powdr supply layer to soldering bumps. It is thus possible to mate the package board free of noise mixed in wires.As described ibove, according to the package board in the 20 third embodiment, an inner layer conductor circuit formed in the lower layer of tlie insulating layer supporting the conductor circuits formed in the outermost layer is used as a power supply layer and / or a ground layer, and a via-hole is connected directly to a second conductor circuit and a soldering bump is 25 formed in each of those via-holes. The package board can a wire for connecting the power supply layer to soldering bumps. Consequently, it is package board free of noise mixed in wires, ring-eliminated space can be used to pack formed in each of therefore eliminate or the ground layer possible to make the Furthermore, the wi the multi-layer printed wiring board in a higher density.Furthermore, according to the package board in the third embodiment, a second conductor circuit formed under the second interlaminar resin insulating layer supporting the outermost layer conductor circuits is used as a power supply layer or a ground layer, and avia-hole is connected directly to the second conductor circuit and a soldering bump is formed on the via-hole. The package board can thus eliminate a wire for connecting the power supply layer or the ground layer to soldering bumps.Consequently, it is possible to make the package board free of noise mixed in wires. Furthermore, the wiring-eliminated space can be used to pack the multi-layer printed wiring board more densely.(Fourth Embodiment)Hereunder, a configuration of the package board in the fourth embodiment of the present invention will be described with reference to Fig. 15. On both top and bottom surfaces of the core board 30 of the package board 400 are formed inner layer copper patterns 34U and 34D used as a ground layer respectively.In the upper layer of the inner layer copper pattern 34U are formed a conductor circuit 58U that forms a signal line with an interlaminar resin insulating layer 50 therebetween, as well as a via-hole 60U through the interlaminar resin insulating layer 50. In the upper layer of the conductor circuit 58U is formed an outermost layer conductor circuit 158U with an interlaminar resin insulating layer 150 therebetween, as well as a via-hole 160U through the interlaminar resin insulating layer 150. And, a soldering pad 75U for support ing a solder ing bump 76U is formed on the conductor circui t 158U and the via-hole• · » · · · · · ·160U respectively. Each of the soldering pads 75U on the IC chip side surface of the package board is formed so as to be 133 to 170μΐη in diameter.On the other hand, in the upper layer of the inner layer copper pattern 34D formed on the bottom surface of the core board 30 is formed a conductor circuit 58D that forms a signal line with the interlaminar resin insulating layer 50 therebetween.of the conductor circuit 58D is formed an iductor circuit 158D with the interlaminarIn the upper layer outermost layer co resin insulating layer 150 therebetween, as well as avia-hole160D through the in a soldering pad 75D ;erlaminar resin insulating layer 150. And, for supporting a soldering bump 76D is formed on the conductor circuit 158D and the via-hole 160D respectively. Each of those soldering pads 75D on this mother board side surface of the package board is formed so as to be 600μΐη in tion, a ground (electrode) layer is formed ayer copper patterns 34U and 34D that face le core board 30 therebetween, so that a capacitor is formed with those inner layer copper patterns 34U and 34D.i top view of an inner layer copper pattern top surface of the core board 30. On this pattern 34U are formed a ground layer 34G sed to connect the upper layer to the lower Fig. 16B shows an expanded land-pad 41 inFig. 16A. The X3-X3 1 ine cross sect ional equal to the X3-X3 line cross sectional view diameter. In addi on each of the inne each other with tFig. 16A is 34U formed on the inner layer copper and land-pads 41 u layer respectively formed in the B area, view in Fig. 16B is in Fig. 15.As shown in ig. 16B, each land-pad 41 is a combination • · of the land 41a of a through-hole 36 shown in Fig. 15 and a pad41b connected to a interlaminar resin via-hole 60U that goes through the upper insulating layer 50. Around the lad pad 41 is disposed an insi.lating buffer 43 of about 200μΐη in width.According to 41a is united with the package board in this embodiment, a land a pad 41b as shown in Fig. 16B, so that the land 41a is connected directly to the pad 41b without using a wire. It is thus between the lower upper conductor wir possible to shorten the transmission path layer (the conductor circuit 58D) and the ing 58U in the upper layer (the interlaminar resin insulating layer 50) thereby to speed up the signal transmission, as we addition, since the 41b without using a wire and a land or t is thus protected c a crack generated as reduce the connection resistance. In land 41a is connected directly to the pad wire, no stress is concentrated between a etween a wire and a pad. The package board ompletely from breaking of a wire caused by by concentrated stress at such a place, although the packalge board manufactured with the prior art technology describ ed above with reference to Fig. 24A has confronted with such a problem. And, although a description was made for only t the top surface of pattern 34D on the ie inner layer copper pattern 34U formed on the core board 30, the inner layer copper bottom surface of the core board 30 is also composed in the sabae way.Next, a description will be made for a package board composed as a variation of the fourth embodiment of the present invention with reference to Figs. 17 and 18. According to the fourth embodiment described above with reference to Fig. 15, the ground layer (electrode layer) 34G and the land-pad 41 are » · · · · · formed on the inner layer copper patterns 34U and 34D formed on both top and bo tom surfaces of the core board 30. On the contrary, in the second embodiment, the power supply layer (electrode layer) conductor circuits interlaminar resin Fig. 17 is a composed as a varia58G and the land-pad 61 are formed on the 58U and 58D formed in the upper layer of the insulating layer 50 as shown in Fig. 16A. cross sectional view of the package board tion of the fourth embodiment. Fig. 18A is a top view of the conductor circuit 58U formed on the top surface of the interlamin ar resin insulating layer 50. On this conductor circuit 58U are formed a power supply layer 58G, as well as land-pads 6 layer respectively used to connect the upper layer to the lower Fig. 18B shows an expanded land-pad 61 in the B area shown i| Fig. 18A. The X4-X4 line cross sectional view shown in Fig. 1]8B is equal to the X4-X4 line cross sectional17.Fig. 17, each of those land-pads 61 is a land 61a of a via-hole 60U connected to an pattern 34U and a pad 61b connected to a ng through the upper interlaminar resin 50. Around each of those land pad 61 is ing buffer 63 of about 200μπι in width as shown view shown in Fig.As shown in combination of the inner layer copper via-hole 160U goi insulating layer disposed an insulat i n F i g. 18B.Also in the case of this package board composed as a variation of the fourth embodiment, a land 61a is united with a pad 61b, so that the land 61a is connected directly to the pad 61b wi thou t using a wire. This makes it possible to shorten the transmission between the lower layer (an inner layer copper pattern 34U on the (top surface of the core board 30) and an upper • · first conductor wirk 158U formed on the top of the upper layer (the interlaminar resin insulating layer 150), as well as to speed up the signal transmission and reduce the connection resistance. In acdition, since the land 61a is connected 5 directly to the pad 61b without using a wire, no stress is concentrated between a wire and a land or between a wire and a pad. The package board is thus protected completely from breaking of a wire caused by a crack generated by concentrated stress at such a place, although the package board manufactured with the prior art technology described above with reference to Fig. 24A has confronted with such a problem.Al though each circular ly-formed land is united wi th a pad in the above embodiment, the land may be formed as an ellipse, a polygon, etc. and united with a pad in this invention.According to the fourth embodiment described above, each land is connected cirectly to a pad without using a wire. It is thus possible to shorten the transmission between the lower layer and each conductor wiring (conductor layer) formed in the upper layer, as well as to speed up the signal transmission and reduce the connect ipn resistance. In addition, since each land is connected direc is concentrated at as at a junction be ly to a pad without using a wire, no stress a junction between wiring and land, as well ;ween wiring and pad. The package board can thus be protected completely from breaking of a wire caused by a crack generated (Fifth Embodiment) Hereunder, a of the package boa by concentrated stress at such a place.description will be made for a configuration rd in the fifth embodiment of the present invention with reference to Figs. 19 and 20. Fig. 19 is a cross sectional view of the package board 500 in the fifth embodiment. Fig. 20 shows how the package board 500 provided with an IC chip 80 mounted on its top surface thereof is mounted on a mother board 90 thereby to compose a so-called integrated circuit package.On both top and bottom surfaces of the core board 30 of the package board 500 are formed inner layer copper patterns 34U and 34D used as ground layers. In the upper layer of .the inner layer copper pattern 34U is formed a conductor circuit 58U forming a signa. line with an interlaminar resin insulating layer 50 therebetween, as well as a via-hole 60U through the interlaminar resin insulating layer 50. In the upper layer of the conductor circuit 58U is formed an outermost layer conductor circuit 158U with an interlaminar resin insulating layer 150, as well as a via-hole 160U through the interlaminar resin insulating layer 150. And, a soldering pad 75U for supporting a soldering bump 75U is formed on the conductor circuit 158U and the via-hole 160U respectively. Each of the soldering pads side surface of the package board is formed 170p,m in diameter.hand, in the upper layer of the ground layer pattern) on the bottom side of the core board75U on the IC chip so as to be 133 to On the other (inner layer copper is formed a conductor circuit 58D forming a signal line with an interlaminar res upper layer of the layer conductor < insulating layer 1 through the interl in insulating layer 50 therebetween. In the conductor circuit 58D is formed an outermost ircuit 158D with an interlaminar resin 50 therebetween, as well as a via-hole 160D aminar resin insulating layer 150. And, a soldering pad 75D for supporting a soldering bump 76D is formed • · · · in the via-hole 160 mother board side diameter.According toD. Each of the soldering pads 75D on the surface is formed so as to be 600μπι in this package board in the fifth embodiment, a soldering bump 76D is formed on each via-hole 160D on the mother board side connected directly board is completely urface 60, so that the soldering bump is o the via-hole. Consequently, the package protected from breaking of a wire, otherwise to occur between the soldering bump 76D and the via-hole 160D if the package boari is cracked. In other words, according to the package board 600 manufactured with the prior art technology described above with reference to Fig. 23B, each soldering pad 375D is connected ;o a via-hole 360 through a wire 378 and a soldering bump 3761) is disposed on a soldering pad 375D. If :rated in the package board 600, therefore, the wire 378 connecting the via-hole 376D pad 376D. The soldering bump 376D can nnected from the via-hole 360D. On the contrary, according to the package board in the fifth embodiment, no breaking of a wire occurs between the soldering bump 376D and the via-hole 160D even when a crack is generated in the package board.Next, a description will be made for how the IC chip 80 is mounted on the package board 500 in the fifth embodiment of the present invention shown in Fig. 19. As shown in Fig. 20, the IC chip 80 is nounted on the package board 500 so that the soldering pads 82 of the IC chip 80 are aligned to the soldering bumps 76U of the package board 500. Then, the package board 500 with the IC chip 80 mounted thereon is passed through a a crack L2 is gene the crack L2 breaks to the soldering therefore be discc process. In this chlorothen is flown 500 to remove the so the IC chip 80 and heating oven thereby to weld the soldering pads 76U to the soldering pads 82. The IC chip 80 is thus connected to the package board 500.The package board 500 is then washed to remove the soldering flux seeoed out when the soldering bumps 76U are welded to and set μρ at the soldering pads 82 in the heating embodiment, an organic solution such as between the IC chip 80 and the package board ldering flux. Resin is then filled between the package board 500 to seal the portion.Although not illustrated, the whole IC chip 80 is molded with resin at this time thereby to finish the mounting of the IC chip 80 on the package board 500.After this, the soldering pads 92 of the mother board 90 are aligned to the soldering bumps 76D to mount the package board 500 on a mother board 90. Then, the package board is passed through a heating oven to fuse the soldering pads 76D to the soldering pads 92. The package board 500 is then connected to the mother board 90. After this, resin 94 is filled in a clearance between 90 as shown in Fig.the package board 500 and the mother board 20 to seal the clearance. This completes the mounting of the package board 500 on the mother board 90.Next, a description will be made for a package board 501 composed as a variation of the fifth embodiment of the present invention with reference to Figs. 20 and 21.the package board 500 in the fifth embodiment described above wHh reference to Fig. 19, a solder ing bump 76D is formed on a vii-hole 160D. Meanwhile, according to the package board 501 in the fifth embodiment, a soldering bump 276 »» · • · • · · · is formed on a plurality of (three) via-holes 260 as shown in Fig. 21. In other words, three via-holes 260 are formed closely to each other as shown in Fig. 22, which is equal to the X5-X5 line cross sectional view shown in Fig. 21 (the X6-X6 line in Fig. 22 is equal to the X5-X5 line in Fig. 21). Then, a nickel plated layer 72 and a gold plated layer 74 are formed respectively on a c thereby to form one276 is formed on the large land 275.ommon land 260a of the three via-holes 260 large land 275. And, a large soldering bumpIn the case variation of the f formed on a plurali of this package board 501 composed as a ifth embodiment, a soldering bump 276 is ty of via-holes 260, so that the soldering bump 276 is coniiected directly to the via-holes 260. Consequently, it is prevented that the soldering bump 276 is disconnected from tpe via-holes 260, for example, even when the s cracked. In addition, since a soldering n a plurality of (three) via-holes 260, the package board 501 i bump 276 is formed package board 501 can have a phase safe function. Because, when one of those via-ho conductor circuit connection with th conductor circuit 58D.Furthermore, es 260 is disconnected from the inner layer 58D, another via-hole 260 can keep the e soldering bump 27 and the inner layer as described above, each soldering pad 75U on the IC chip 80 side surface is formed so as to be 133 to 170μΐη in diameter and eac surface is formed s i soldering pad 75D on the mother board side o as to be 600μΐη in diameter. Thus, there is generated a difference in soldering pad size 4 to 5 times between the IC chip side and the mother board side. It is thus difficult to form a large soldering pad 75D on a via-hole like • · those formed on the this package board mother board side surface. In the case of 501 composed as a variation of the fifth embodiment, therefore, a soldering bump 276 is formed on a plurality of (three' via-holes 260, 260, and 260 thereby to form such a large soldering bump. Although one soldering bump is formed on three via-holes in this variation described above, to form one soldering bump on two via-holes via-holes.the package board in the fifth embodiment a soldering bump is formed on a via-hole, so that the soldering bump is connected directly to the via-hole. This can prevent breaking of a wire even when the package board is cracked between the soldering bump and the via-hole. In addition, since a soldering bump is formed on a plurality of via-holes, the package board can have a phase safe function.it is also possible or on four or more According to as described above,Because, when one soldering bump insi keep the connectio soldering bump is of the via-holes is disconnected from the de the package board, another via-hole can n with the soldering bump. And, since a formed on a plurality of via-holes, the soldering bump cah be formed larger with respect to the via-hole.package board is connected directly to the e embodiment described above, the presentAlthough the mother board in th invention also allows the package board to be connected to the mother board via a sub-board, etc.
Claims
CLAIMS 1. A package board (1C plurality of conductor circu insulating layer (50) therebet formed on an IC chip mourn connected to another board, are larger than those on said a dummy pattern (58 board (100) is formed betwei said IC chip mounted side su; IC 0) having a core board (30) on each surface of which a its (58U, 58D)) are formed with an interlaminar resin Aveen, wherein a plurality of soldering pads (75U, 75D) are ed side surface, as well as on an other side surface to be 50 that said soldering pads (75D) on the other side surface chip side surface of said package board (100), and M) for improving the mechanical strength of the package en signal line conductor circuit patterns (58U) formed on rface of said core board (30).
2. A package board (1()0) having a core board (30) on each surface of which a plurality of conductor circuits (58U, 58D) are formed with an interlaminar resin insulating layer (50) therebetween, wherein a plurality of soldering pads (75U, 75D) are formed on an IC chip mourned side surface, as well as on an other side surface to be connected to another board, so that said soldering pads (75D) on the other side surface are larger than those on said IC chip side surface of said package board (100), and a dummy pattern (58M) for improving the mechanical strength of the package board (100) is formed between signal line conductor circuit patterns (58D) of an outmost layer (158D) formed on said 1C chip mounted side surface of said core board (30).
3. A package board (ICO) having a core board (30) on each surface of which a plurality of conductor circvits (58U, 58D) are formed with an interlaminar resin insulating layer (50) therebetween, wherein a plurality of soldering pads (75U, 75D) are formed on an IC chip mourn ed side surface, as well as on an other side surface to be connected to another board, so that said soldering pads (75D) on the other side surface are larger than those on said IC chip side surface of said package board (100), and a dummy pattern (58M) for improving the mechanical strength of the package board (100) is formed between signal line conductor circuit patterns (58U) on the core board (30) formed on said IC chip mounted side surface of said core board (30). V4. A package board (200) comprising: a core board (30), the core board having an IC chip (80) side surface and an other surface opposed to the IC chip (80) side surface; a first plurality of conductor circuits (158U) formed on the IC chip (80) side surface and a second plurality of conductor circuits (158D) formed on the other surface (90), the first plurality of conductor circuits (158U) being constructed and adapted to be electrically connected to an 1(} chip; a first interlaminar resin insulating layer (50) disposed between the IC chip (80) side surface and the first plurality of conductor circuits (158U); a second interlaminar resin insulating layer (50) disposed between the other surface (90) and the second plurality of conductor circuits (158D); a first plurality of soldering pads (75U) formed on the IC chip (80) side surface; a second plurality of soldering pads (75D) formed on the other surface, the soldering pads (75D) of the second plurality being larger than the soldering pads (75U) of the first plurality; and a dummy pattern (159) constructed and adapted to improve the mechanical strength of the package board (200), the dummy pattern (159) being formed at an outer periphery of the first plurality of conductor circuits (158U).
5. A package board (200) a core board (30), the surface (90) opposed to the IC one or more layers of surface and one or more layer: (90), the one or more layers o surface being constructed and a first interlaminar res (30) and the one or more surface; a second interlaminar (30) and the one or more layejr: (90); layer: , comprising: core board having an IC chip (80) side surface and an other chip (80) side surface; conductor circuits (158U) formed on the IC chip (80) side s of conductor circuits (158D) formed on the other surface f conductor circuits (158U) formed on the IC chip (80) side adapted to be electrically connected to an IC chip (80); in insulating layer (150) disposed between the core board s of conductor circuits (158U) formed on the IC chip side esin insulating layer (150) disposed between the core board s of conductor circuits (158D) formed on the other surface additional interlaminar insulating layers disposed between ones of the one or more layers of conductor circuits (158U, 158D) formed on the IC chip (80) side surface and the other surface (90); a first plurality of soldering pads (75U) formed on a top one of the one or more 58U) on the IC chip (80) side surface; jaldering pads (75D) formed on a top one of the one or more 58D) on the other surface (90), the soldering pads (75D) of layers of conductor circuits (] a second plurality of s layers of conductor circuits ( the second plurality being larger than the soldering pads (75U) of the first plurality; and a dummy pattern (159) constructed and adapted to improve the mechanical strength of the package board (200), the dummy pattern (159) being formed at an outer periphery of at least one of th^e one or more layers of conductor circuits (158U) on the IC chip (80) side surface.
6. The package board (10' at the outer periphery of each the IC chip side surface. »0) of claim 4, wherein the dummy pattern (58M) is formed of the one or more layers of conductor circuits (158U) on7. A package board (300) a core board (30), surface opposed to the IC chip one or more layers surface and one or more layer, the one or more layers of co: being constructed and adapted a first interlaminar (30) and the one or more laye surface; a second interlaminar (30) and the one or more lay eh additional interlamina more layers of conductor cir the other surface; of , comprising: core board having an IC chip side surface and an other side surface; conductor circuits (158U) formed on the IC chip side s of conductor circuits (158D) formed on the other surface, nductor circuits (158U) formed on the IC chip side surface to be electrically connected to an IC chip; in insulating layer (150) disposed between the core board rs of conductor circuits (158U) formed on the IC chip side resin insulating layer (150) disposed between the core board s of conductor circuits (158D) formed on the other surface; r insulating layers disposed between ones of the one or huits (158U, 158D) formed on the IC chip side surface and a first plurality of so layers of conductor circuits ( a second plurality of layers of conductor circuits second plurality being larger a dummy pattern ( strength of the package board periphery of the core board ( ldering pads (75U) formed on a top one of the one or more 58U) on the IC chip side surface; Soldering pads (75D) formed on a top one of the one or more (158D) on the other surface, the soldering pads (75D) of the than the soldering pads (75U) of the first plurality; and 159) constructed and adapted to improve the mechanical (300), the dummy pattern (159) being formed at an outer 0) on the IC chip side surface. A package board (400), comprising: a core board (30) having a first surface and a second surface opposite the first surface, with first and second conductor layers formed on each of the first and second surfaces, respectively; a third conductor layer formed on at least one of said first and second conductor layers with a first interlaminar resin insulating layer (50) therebetween; at least one of the first, second, and third conductor layers functioning as an electrode layer; and at least one of a pair consisting of the first and third conductor layers and a pair consisting of the second anc third conductor layers, along with the interlaminar resin insulating layer (50) between the at least one of the pairs, having a plurality of throughholes (36) extending therethrough; wherein a land (41a) of each of the plurality of through-holes (36) is formed as a (34G) and is united with a pad (41b) connected to a via-hole and interlaminar resin insulating layer (50) formed on an board (400); and portion of the electrode layer (60U) formed through a sec opposite side of said package wherein the land (41a) and pad (41b) are united as a union of circular areas.
9. The package board (43) area is disposed around t (400) of claim 8, wherein the electrically insulating buffer ie united land (41a) and pad (41b).
10. The package board ( (43) area is about 200 microni 00) of claim 9, wherein the electrically insulating buffer eters in width.
11. A package board, comprising a core board (30) having a first surface and a second surface opposite the first surface, with first and second conductor layers (58U, 58D) formed on each of the first and second surfaces, respectively; a third conductor layer formed on at least one of said first and second conductor layers with a first interlamina at least one of the firsi at least one of a pair • resin insulating layer (50) therebetween; , second, and third conductor layers on said core board (30) functioning as an electrode layer (58G); and ;onsisting of the first and third conductor layers and a pair consisting of the second and third conductor layers, along with the interlaminar resin insulating layer (50) between the at least one of the pairs, having a plurality of via-holes (160U) extending therethrough; wherein a land (61a) resin insulating layer (150) disposed in the at least one c of via-hole (60U) formed through a second interlaminar adjacent to said first surface of said package board (30), inductor layer functioning as said electrode layer (58G), is united with a pad (61b) connected to a via-hole (160U) formed through the first interlaminar resin insulating board (30); and wherein the land (61 a12. The package board of is disposed around the united ayer (150) adjacent to said second surface of said package and the pad (61b) are united as a union of circular areas. claim 11, wherein an electrically insulating buffer (63) area land ( 61a) and pad (61b).
13. The package board of claim 12, wherein the electrically insulating buffer (63) area is about 200 micrometers in width.
14. A package board (500) in the form of a multi-layer wiring board, the package board having a first side and i. second side opposed to the first side, comprising: layers of conductor circuits (58U, 58D) on the first and second sides of the package board (500), the layers of conductor circuits (58U, 58D) including, on each of the first and second sides of the package board (500), inner layers of conductor circuits (58U), the inner layers of conductor circuits being configured and adapted to be one or more of a power supply layer and a ground layer, and outer layers of conductor circuits (58D); insulating layers (50) Supporting the outer layers of conductor circuits (58D); via holes (60U) forme d through the insulating layers (50) on the first and second sides of the package board (500), the via holes (60U) on the first side directly electrically connecting the inner and outer layers of conductor circuits (58U) on the first side and the via holes (60U) on the second side directly electrically connecting the inner and outer layers of conductor circuits (58D) on the second side; soldering bumps (76U, 76D) on the first and second sides of the package board 10 (500), the soldering bumps (76U) on the first side configured and adapted to be connected to an IC chip (80) and the soldering bumps (76D) of the second side configured and adapted to be connected to an outer board (90), each one of the soldering bumps (76U) on the first side disposed in a via hole (160U) , and ones of the soldering bumps (76D) on the second side disposed in two or more via holes (160D).
15. A package board (501) in the form of a multi-layer wiring board, the package board having a first side and a second side opposed to the first side, comprising: a core board (30) having a first side and a second side opposed to the first side; first and second plura ities of layers of conductor circuits (58U, 58D) formed on the first and second sides of the core board (30), the first and second pluralities of layers of conductor circuits (58U, 58D) each including at least one outer layer of conductor circuits (58U), the at least one inner layer of the first and second pluralities of conductor circuits (58D) being configured and adapted as one or more of a power layer and a ground layer; first and second insulating layers (50) supporting the at least one outer layer of the first and second pluralities of layers of conductor circuits (58U, 58D); first and second pluralities of via holes (260) extending through the first and second insulating layers (50), the first plurality of via holes (260) directly electrically connecting the at least one outer layer and the at least one inner layer of the first plurality of conductor circuits (58U) and the second plurality of via holes (260) directly least one outer layer and the at least one inner layer of the circuits (58D); and electrically connecting the at second plurality of conductor ities of soldering bumps (276) disposed on the first and board (501), the first plurality of soldering bumps (276) be connected to an IC chip and the second plurality of red and adapted to be connected to an outer board, each of bumps (276) being disposed in one of the first plurality of e second plurality of soldering bumps (276) being disposed plurality of via holes (260). first and second plural second sides of the package configured and adapted to soldering bumps (276) configu the first plurality of soldering via holes (260) and each of tty in two or more of the second