Composite copper nanoparticles and method for manufacturing composite copper nanoparticles

MYPI2025000068A0Undetermined Publication Date: 2024-01-27NIPPON SANSO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025000068
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-07-27
Filing Date
2023-07-05
Publication Date
2024-01-27

AI Technical Summary

Technical Problem

Copper nanoparticles used in electronic components and conductive pastes tend to agglomerate due to small particle size and ease of oxidation, leading to poor dispersibility in non-aqueous solvents and uneven film formation, which affects the smoothness and conductivity of electrode films.

Method used

Composite copper nanoparticles with a surface modified by a silane coupling agent, specifically an alkylsilane, are produced, with a controlled mass carbon concentration and surface area, to enhance dispersibility and prevent agglomeration, using a method that involves mixing copper nanoparticles with an organic solvent and silane coupling agent, followed by shear force dispersion and chemical bonding.

Benefits of technology

The modified copper nanoparticles exhibit high dispersibility in organic solvents, preventing agglomeration and ensuring the formation of smooth, conductive electrode films with improved particle size distribution and reduced carbon residue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025000068_DRAWING_001
    Figure PI2025000068_DRAWING_001
Patent Text Reader

Abstract

One object of the present application is to provide composite copper nanoparticles that have high dispersibility in organic solvents and can be used to form a smooth electrode film. The present invention provides composite copper nanoparticles in which the surfaces of copper nanoparticles are modified with a silane coupling agent, wherein the copper nanoparticles have a coating film containing copper oxide on at least a part of the surface, and wherein the mass carbon concentration derived from the silane coupling agent in the composite copper nanoparticles is 0.1 to 1.2% by mass with respect to the total mass of the composite copper nanoparticles or wherein the number of surface groups derived from the silane coupling agent on the surface of the composite copper nanoparticles is 1.0 to 13.0 per 1 nm2 of the surface area of the composite copper nanoparticles. Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Composite copper nanoparticles and method for producing the same

[0001] The present invention relates to composite copper nanoparticles and a method for producing composite copper nanoparticles.

[0002] When applying inks or pastes containing copper nanoparticles as a primary component to bond various electronic components or form wiring, the copper nanoparticles are prone to agglomeration due to their small particle size and susceptibility to oxidation. In particular, maintaining dispersion in non-aqueous solvents is difficult, and when a thin film is formed using the ink or paste, unevenness is likely to occur, resulting in low smoothness. To address this issue, it is known to use copper nanoparticles with improved dispersibility through silane coupling treatment.

[0003] Patent Document 1 discloses a method for improving the dispersibility of copper nanoparticles by modifying the surface of copper nanoparticles with a silane coupling agent having a vinyl group, and then reacting the modified surface with a monomer to form a graft polymer chain.

[0004] Patent Document 2 discloses a method of modifying the surface of copper hydride fine particles synthesized by a wet method with a silane coupling agent.

[0005] JP 2017-165796 A JP 2015-110682 A

[0006] In the examples of Patent Document 1, the proportion of polymer chains is high at 2.8 to 7.0 mass%, which tends to leave carbon residue during electrode film formation, raising concerns about impaired electrode film adhesion and poor conductivity. The composite copper nanoparticles of Patent Document 2 are not surface-modified with a silane coupling agent, raising concerns about poor dispersibility in organic solvents. Furthermore, since the silane coupling agent is not used for the purpose of improving dispersibility, only 0.1 mass% is added to the copper nanoparticles, raising concerns about insufficient dispersibility in organic solvents. In particular, there is a concern that a conductive paste with a higher metal concentration than conductive ink is prone to aggregation.

[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide composite copper nanoparticles that are highly dispersible in organic solvents and can form smooth electrode films, and a method for producing composite copper nanoparticles.

[0008] In order to achieve the above-mentioned object, the present invention employs the following configurations. [1] Composite copper nanoparticles, the surfaces of which are modified with a silane coupling agent, wherein the copper nanoparticles have a coating containing copper oxide on at least a portion of their surfaces, and the mass carbon concentration attributable to the silane coupling agent in the composite copper nanoparticles is 0.1 to 1.2 mass% relative to the total mass of the composite copper nanoparticles. [2] The composite copper nanoparticles according to [1], wherein the mass carbon concentration attributable to the silane coupling agent in the composite copper nanoparticles is 0.2 to 0.5 mass% relative to the total mass of the composite copper nanoparticles. [3] The composite copper nanoparticles according to [1] or [2], wherein the mass carbon concentration attributable to the copper nanoparticles in the composite copper nanoparticles is 0.3 mass% or less relative to the total mass of the composite copper nanoparticles. [4] Composite copper nanoparticles, the surfaces of which are modified with a silane coupling agent, wherein the copper nanoparticles have a coating containing copper oxide on at least a portion of their surfaces, and the surface groups derived from the silane coupling agent on the surfaces of the composite copper nanoparticles are 0.1 to 1.2 mass% relative to the total mass of the composite copper nanoparticles. 2[5] The composite copper nanoparticles according to any one of [1] to [4], wherein the silane coupling agent is an alkylsilane. [6] The composite copper nanoparticles according to [5], wherein the silane coupling agent is an alkylsilane having an alkyl chain containing 3 to 10 carbon atoms. [7] The composite copper nanoparticles according to [6], wherein the silane coupling agent is n-octyltrimethoxysilane. [8] The composite copper nanoparticles according to any one of [1] to [7], wherein the average particle size of the copper nanoparticles is 200 nm or less. [9] A method for producing composite copper nanoparticles whose surfaces have been modified with the silane coupling agent, comprising: preparing copper nanoparticles having a coating containing copper oxide on at least a portion of their surfaces; an organic solvent; and a silane coupling agent; preparing a mixture of the copper nanoparticles, the organic solvent, and the silane coupling agent; pressurizing the mixture and feeding it into a capillary flow path; and dispersing the mixture by applying a collision and shear force to the mixture to obtain a dispersion; wherein the amount of the silane coupling agent added is 0.6 to 3.3 times the amount equivalent to forming a monomolecular film on the surface of the copper nanoparticles.

[0009] According to the present invention, it is possible to provide composite copper nanoparticles that are highly dispersible in organic solvents and that can form smooth electrode films, and a method for producing composite copper nanoparticles.

[0010] FIG. 1 is a graph showing the relationship between the mass carbon concentration (horizontal axis, unit: mass%) derived from the silane coupling agent of the composite copper nanoparticles and the median diameter (vertical axis, unit: μm) of the composite copper nanoparticles. FIG. 2 is a graph showing the relationship between the number of surface groups derived from the silane coupling agent on the surface of the composite copper nanoparticles (horizontal axis, unit: number / nm 2 ) and the median diameter (vertical axis, unit: μm) of composite copper nanoparticles.

[0011] Although the embodiments of the present invention will be described in detail below, the present invention is not limited to the embodiments described below, and various modifications are possible without departing from the gist of the present invention.

[0012] The meanings and definitions of terms used in this specification are as follows. A numerical range represented by "to" means a numerical range with the numbers before and after "to" as the lower and upper limits. The modification of the surface of copper nanoparticles with a silane coupling agent means that the hydroxyl groups present on the surface of the particles undergo a dehydration condensation reaction with the silane coupling agent, resulting in silanol being bonded to the surface. Alternatively, even in the absence of hydroxyl groups, the alkoxy groups of the silane coupling agent are hydrolyzed by electrostatic interaction to form silanol groups, which are then adsorbed onto the particle surface, and a monomolecular film is formed on the surface by subsequent dehydration condensation between the silane coupling agents.

[0013] [Composite Copper Nanoparticles] The composite copper nanoparticles of the present invention are composite copper nanoparticles in which the surfaces of copper nanoparticles are modified with a silane coupling agent, and the copper nanoparticles have a coating containing copper oxide on at least a portion of their surfaces.

[0014] The mass carbon concentration attributable to the silane coupling agent in the composite copper nanoparticles is 0.1 to 1.2 mass%, preferably 0.2 to 0.5 mass%, and more preferably 0.25 to 0.4 mass%, relative to the total mass of the composite copper nanoparticles. If the mass carbon concentration attributable to the silane coupling agent is less than 0.1 mass%, the composite copper nanoparticles cannot be imparted with sufficient hydrophobicity, and aggregation begins from the non-hydrophobic portions, inhibiting dispersibility and resulting in a large particle size distribution. If the mass carbon concentration attributable to the silane coupling agent exceeds 1.2 mass%, aggregation begins between the excess silane coupling agent particles, inhibiting dispersibility and resulting in a large particle size distribution. Furthermore, if the mass carbon concentration attributable to the silane coupling agent exceeds 1.2 mass%, carbon residues are likely to remain during the formation of the electrode film, which may result in a deterioration in conductivity or damage to the electrode film during degassing.

[0015] Here, the mass carbon concentration attributable to the silane coupling agent is determined by measuring the mass carbon concentration of the composite copper nanoparticles and the mass carbon concentration of the copper nanoparticles in their raw state before reaction with the silane coupling agent by a method described below, and calculating the difference between the measured values ​​of the composite copper nanoparticles and the measured values ​​of the copper nanoparticles.

[0016] <Copper Nanoparticles> Copper nanoparticles have a coating containing copper oxide on at least a portion of their surface. Examples of such copper nanoparticles include those produced by a dry method using a reducing flame. Copper nanoparticles produced by a dry method exhibit little thermal shrinkage even when sintered at 300°C or higher. In contrast, copper nanoparticles synthesized by a wet method exhibit large thermal shrinkage. Examples of the copper oxide include copper(I) oxide, copper(II) oxide, and mixtures thereof. When the copper oxide is a mixture of copper(I) oxide and copper(II) oxide, the ratio of these is not particularly limited. The copper nanoparticles preferably have an average particle size of 10 to 200 nm, more preferably 10 to 150 nm. When the average particle size of the copper nanoparticles is 200 nm or less, the composite copper nanoparticles exhibit excellent dispersibility when made into a paste, and when it is 150 nm or less, the dispersibility is even better. On the other hand, if the average particle diameter of the copper nanoparticles exceeds 200 nm, the weight per particle increases, so the steric effect of the alkyl chain of the silane coupling agent does not function sufficiently, and the dispersibility of the composite copper nanoparticles when made into a paste tends to decrease.

[0017] "Average Particle Diameter" The average particle diameter of copper nanoparticles can be measured using a scanning electron microscope (SEM). For example, the particle diameters of 250 copper nanoparticles present in one field of view in an electron microscope image are measured, and the number average value is calculated to determine the average particle diameter of the copper nanoparticles. The criteria for selecting particles to be measured among those shown in a scanning electron microscope image (photograph) are as follows: (1) Particles whose parts extend outside the field of view of the photograph are not measured. (2) Particles whose outlines are clearly defined and exist in isolation are measured. (3) Particles that deviate from the average particle shape are measured if they are independent and can be measured as individual particles. (4) Particles that overlap but have clear boundaries and whose overall shape can be determined are measured as individual particles. (5) Particles that overlap with each other, with unclear boundaries, and whose overall shape cannot be determined, are not measured because their shape cannot be determined. (6) For particles that are not perfectly round, such as ellipses, the major axis was taken as the particle size.

[0018] The surface of the copper nanoparticles is covered with a coating containing copper oxide. The copper oxide contained in the coating functions as a reaction site with a silane coupling agent. The coating on the surface of the copper nanoparticles may contain copper carbonate in addition to copper oxide as a copper compound, but copper carbonate does not react with a silane coupling agent. Therefore, the mass carbon concentration attributable to the copper nanoparticles is preferably 0.3 mass% or less.

[0019] "Mass carbon concentration" The mass carbon concentration in copper nanoparticles and composite copper nanoparticles can be measured using a carbon-sulfur analyzer (for example, "EMIA-920V" manufactured by Horiba, Ltd.). The mass carbon concentration in copper nanoparticles and composite copper nanoparticles is the number average value of three samples.

[0020] <Silane Coupling Agent> The silane coupling agent is not particularly limited as long as it can be chemically bonded to the surface of copper nanoparticles by a silane coupling reaction and improves dispersibility in a solvent. Examples of such silane coupling agents include alkylsilanes having only alkyl chains as surface groups, aminoalkylsilanes having amino groups, and arylsilanes having phenyl groups. Specific examples of each silane coupling agent include alkylsilanes such as n-octyltrimethoxysilane, n-octyltriethoxysilane, dodecyltriethoxysilane, octadecyltrimethoxysilane, and octadecyltriethoxysilane. Examples of aminoalkylsilanes include 3-aminopropyltrimethoxysilane and 3-(2-aminoethylamino)propyltrimethoxysilane. Examples of arylsilanes include phenyltrimethoxysilane. Among the silane coupling agents mentioned above, alkylsilanes are preferred for use in modifying the surface of copper nanoparticles, with n-octyltrimethoxysilane being more preferred. By using alkylsilane, the carbon content of the composite copper nanoparticles can be reduced without impairing the dispersibility of the composite copper nanoparticles in organic solvents.

[0021] The alkyl chain of the silane coupling agent is preferably an alkyl chain having 3 or more carbon atoms, more preferably an alkyl chain having 6 or more carbon atoms, and even more preferably an alkyl chain having 8 or more carbon atoms. If the alkyl chain has 3 or more carbon atoms, the alkyl chain can exert a steric effect by bonding an amount of silane coupling agent equivalent to the formation of a monomolecular film to the surface of the copper nanoparticles. On the other hand, if the alkyl chain is longer than necessary, it will cause an increase in carbon residue when the composite copper nanoparticles are sintered and applied to electrode applications. Therefore, it is preferable that the alkyl chain of the silane coupling agent has 10 or less carbon atoms.

[0022] The composite copper nanoparticles whose surfaces have been modified using a silane coupling agent have a number of surface groups derived from the silane coupling agent on the surface of the composite copper nanoparticles, i.e., a number of surface groups of the silane coupling agent attached to the copper nanoparticle surface of 1 nm or less. 2 The number of particles per particle is 1.0 to 13.0 particles or less, preferably 1.0 to 5.0 particles, and more preferably 2.0 to 4.0 particles.

[0023] Here, the number of surface groups is calculated by the following formula (A).

[0024]

[0025] As a result of extensive research, the inventors have found that when the surface of copper nanoparticles, which have a coating containing copper oxide on at least a portion of their surface, is modified with alkylsilane, a silane coupling agent, so that the entire surface of one copper nanoparticle is covered with a single layer of alkylsilane, a silane coupling agent (hereinafter referred to as monolayer formation), the area occupied by one molecule of alkylsilane, a silane coupling agent, is 0.33 nm 2 Alkylsilanes are generally R-Si(OR') 3It is a compound represented by the chemical formula: [R represents an alkyl group, and R' represents an alkyl group which may be different from each other.] When alkylsilane bonds to the surface of copper nanoparticles, the silane coupling agent, which is alkylsilane, is thought to be chemically bonded vertically from the surface of the copper nanoparticles. Since the alkoxy group (OR') is hydrolyzed, the type of R' has no effect. In other words, if the silane coupling agent is an alkylsilane, the area occupied by one molecule of the silane coupling agent on the surface of the copper nanoparticles is the same, 0.33 nm, regardless of the length of the alkyl chain. 2 From this value, the number of molecules of the silane coupling agent when forming a monolayer of the silane coupling agent on the surface of the copper nanoparticles is 1 nm 2 The number of surface groups of the silane coupling agent is 1 nm. 2 When the number of surface groups of the silane coupling agent is 1.0 or more, the area of ​​the hydrophobicized copper nanoparticle surface is 30% or more. Since the non-hydrophobic portion is 30% or more, aggregation is unlikely to start, dispersibility is unlikely to be hindered, and the particle size distribution is narrow. In addition, the number of surface groups of the silane coupling agent is 1 nm 2 When the number of particles per particle is 13.0 or less, the silane coupling agent particles are less likely to aggregate, so that good dispersibility is maintained and the particle size distribution becomes narrow.

[0026] The composite copper nanoparticles of the present invention can be efficiently surface-treated with an optimal amount of silane coupling agent, so there is no aggregation due to the residual silane coupling agent, they are highly dispersible in organic solvents, and a smooth electrode film can be formed.

[0027] [Method for producing composite copper nanoparticles] The method for producing composite copper nanoparticles of the present invention is a method for producing composite copper nanoparticles by modifying the surface of copper nanoparticles with a silane coupling agent, in which copper nanoparticles having a coating containing copper oxide on at least a portion of their surface are prepared, and the copper nanoparticles, an organic solvent, and a silane coupling agent are mixed and dispersed in a dispersion, which is then reacted while being heated and stirred.

[0028] <Preparation Step> First, in the preparation step, copper nanoparticles having a coating containing copper oxide on at least a portion of the surface, i.e., copper nanoparticles produced by a dry method using a reducing flame, are prepared. Copper nanoparticles can be produced, for example, by the method described in Japanese Patent No. 6130616. Furthermore, commercially available copper nanoparticles may also be used. Copper nanoparticles produced by a dry method are not limited to the above-mentioned production method. For example, copper nanoparticles can also be obtained by a method of reducing a copper compound gas with a reducing gas or a method of cooling copper vaporized by plasma.

[0029] <Mixing Step> Copper nanoparticles, an organic solvent, and a silane coupling agent are mixed, and the mixture is subjected to a dispersion treatment to obtain a copper nanoparticle mixture dispersion. Methods for dispersing copper nanoparticles include a method of feeding the mixture into a capillary channel under pressure and applying collision and shear forces to the mixture, a method of dispersing using a bead mill, and a method of dispersing using a blade or roll. The organic solvent is not particularly limited as long as it can dissolve the silane coupling agent and disperse the copper nanoparticles. Examples of the organic solvent include alcohols such as methanol, ethanol, 1-propanol, 2-propanol, and terpineol; polyols such as ethylene glycol, dimethylene glycol, and triethylene glycol; ethers such as diethylene glycol monobutyl ether; N,N-dimethylformamide, and N-methylpyrrolidone.

[0030] <Reaction Step> Next, in the reaction step, the resulting copper nanoparticle mixture dispersion is heated and stirred to chemically bond the silane coupling agent to the surface of the copper nanoparticles. The resulting copper nanoparticle mixture dispersion is preferably stirred at 30 to 250°C, more preferably at 50 to 150°C. The amount of silane coupling agent added to the dispersion is 0.6 to 3.3 times, and preferably 0.6 to 1.25 times, the amount equivalent to the amount of monolayer formed on the surface of the copper nanoparticles in the dispersion. When the amount of silane coupling agent added is 0.6 times or more the amount equivalent to the amount of monolayer formed on the surface of the copper nanoparticles, the silane coupling agent can be sufficiently attached to the surface of the copper nanoparticles. When the amount of silane coupling agent added is 3.3 times or less the amount equivalent to the amount of monolayer formed on the surface of the copper nanoparticles, the occurrence of aggregation due to reaction between silane coupling agents can be suppressed. Furthermore, the effect of easily removing unreacted silane coupling agent is obtained. The mixing step and the reaction step may be performed simultaneously. For example, the dispersion treatment may be carried out while the mixed liquid is heated with a heater or the like, or the reaction step may be carried out by utilizing heat generated by shear during the dispersion treatment.

[0031] The monolayer formation equivalent amount is the amount added that results in the silane coupling agent adhering to all surfaces of the copper nanoparticles. Specifically, the "surface area of ​​copper nanoparticles / area occupied by one molecule of silane coupling agent = number of molecules of silane coupling agent" is calculated, and the monolayer formation equivalent amount is calculated from this number of molecules and the mass per molecule of silane coupling agent. [How to determine the total surface area of ​​copper nanoparticles] The specific surface area of ​​copper nanoparticles to be silane-coupling treated is measured using a specific surface area meter (e.g., Macsorb HM model-1201 manufactured by Mountec Co., Ltd.). The obtained measurement result is multiplied by the weight fraction of the copper nanoparticles to be silane-coupling treated to determine the total surface area of ​​the copper nanoparticles. (Calculation example) Measured specific surface area: 6.0 m 2 / g Weight of copper nanoparticles 100 g Total surface area of ​​copper nanoparticles = 6.0 x 100 = 600 m 2

[0032] Here, the amount equivalent to the formation of the monomolecular film is calculated by the following formula (B).

[0033]

[0034] <Washing step> Next, in the washing step, the copper nanoparticle mixture after the reaction step is washed by adding an organic solvent and stirring. Stirring can be performed using a stirrer, ultrasonic bath, shaker, etc. The washing step can also be omitted.

[0035] <Drying step> Next, as a drying step, the copper nanoparticle mixture after the reaction step or the washing step can be dried by filtration, reduced pressure drying, air drying, spray drying, etc. These methods can be used alone or in combination of two or more.

[0036] As described above, according to the method for producing composite copper nanoparticles of the present invention, composite copper nanoparticles in which the surface of the copper nanoparticles is modified with a silane coupling agent can be obtained, thereby producing composite copper nanoparticles with high dispersibility in organic solvents. Furthermore, in the method for producing composite copper nanoparticles of the present invention, it is preferable to use copper nanoparticles produced by a dry method. Composite copper nanoparticles obtained using copper nanoparticles produced by a dry method have little thermal shrinkage even when sintered at 300°C or higher, and can form particularly smooth electrode films.

[0037] [Effects] In the present invention, in composite copper nanoparticles in which the surface of the copper nanoparticles is modified with a silane coupling agent, the mass carbon concentration attributable to the silane coupling agent is set to the range of 0.1 to 1.2 mass% relative to the total mass of the composite copper nanoparticles. Alternatively, the surface groups derived from the silane coupling agent on the surface of the composite copper nanoparticles are set to a value within a range of 1 nm2 surface area of ​​the composite copper nanoparticles. 2 The particle size is set to a range of 1.0 or more and 13.0 or less per particle. This results in excellent dispersibility in organic solvents and suppression of aggregation. As a result, the median diameter of the composite copper nanoparticles of the present invention is small, and electrode films formed using the composite copper nanoparticles of the present invention have excellent smoothness. In the present invention, in the production of composite nanoparticles, the amount of the silane coupling agent added is set to 0.6 to 3.3 times the amount equivalent to forming a monomolecular film on the surface of the copper nanoparticles. This makes it possible to produce composite copper nanoparticles with high dispersibility in organic solvents.

[0038] The effects of the present invention will be explained below using examples, but the present invention is not limited to the configurations of the examples.

[0039] [Production Example 1] Production of Copper Nanoparticles Copper nanoparticles were produced by the production method described in Japanese Patent No. 6130616. The production conditions were as follows: Powder raw material: copper powder copper oxide (I) (manufactured by Nippon Atomize Processing Co., Ltd., average particle size 10 μm); Fuel gas supplied to burner: liquefied natural gas; Combustion-supporting gas: oxygen; First cooling gas forming a swirling flow in the furnace: nitrogen; Oxygen ratio: 0.9; Raw material supply rate: 0.36 kg / h. As a result, copper nanoparticles with an average particle size of 110 nm and a mass carbon concentration of 0.16 mass% were obtained.

[0040] [Example 1] 20 g of copper nanoparticles with an average particle size of 110 nm and a mass carbon concentration of 0.16% by mass and 15.8 g of ethanol were weighed into a beaker, and 0.16 g of n-octyltrimethoxysilane (OTMS) (= equivalent amount to form a monolayer) was added as a silane coupling (SC) agent. After stirring these mixtures with a magnetic stirrer for 10 minutes, the mixture was pressurized to a pressure of 100 MPa using a "NanoVeita B-ED" manufactured by Yoshida Kikai Kogyo Co., Ltd., and sent into a capillary channel. The mixture was subjected to collision and shear force dispersion 10 times. The resulting dispersion was placed in a pressure-resistant container and stirred with a magnetic stirrer for 30 minutes while immersed in an 80 ° C water bath. After 30 minutes, the resulting mixture was subjected to solid-liquid separation by filtration, 50 g of ethanol was added, and the mixture was stirred in an ultrasonic bath for 10 minutes. The resulting mixture was again filtered for solid-liquid separation, and dried by blowing air to obtain a powder of composite copper nanoparticles. The obtained composite copper nanoparticle powder was prepared by the above-mentioned method, with the copper nanoparticles having a surface area of ​​1 nm 2 The number of surface groups per particle was calculated, and the particle size distribution was measured in an organic solvent as described below, and the compactness of the particles was observed.

[0041] The amount of n-octyltrimethoxysilane (OTMS) equivalent to forming a monolayer was calculated to be 0.14 g using the above-mentioned formula (B). In formula (B), the area occupied by one molecule of n-octyltrimethoxysilane (OTMS) is set to 0.33 nm 2 , molecular weight 234 g / mol, Avogadro constant 6.02 × 10 23The amount was determined as particles / mol.

[0042] "Particle size distribution in organic solvent" The particle size distribution of copper nanoparticles and composite copper nanoparticles in organic solvents was measured using a laser diffraction wet particle size distribution meter (for example, "SALD-7100" manufactured by Shimadzu Corporation). The sample used for particle size distribution measurement was a dispersion in which 0.1 g of copper nanoparticles or composite copper nanoparticles were dispersed in 23.7 g of ethanol using an ultrasonic homogenizer. As an evaluation index for particle size distribution measurement in organic solvents, the same sample was measured three times, and the average value of the median diameters calculated from the particle size distribution was used. It has been found that when the median diameter in organic solvents is 0.3 μm or less, the density of the coating film of the pasted particles is improved (surface roughness is low).

[0043] The obtained composite copper nanoparticle powder was prepared by the above-mentioned method, with the copper nanoparticles having a surface area of ​​1 nm 2 The number of surface groups per particle was calculated, and the particle size distribution was measured in an organic solvent as described below, and the compactness of the particles was observed.

[0044] The amount of n-octyltrimethoxysilane (OTMS) equivalent to forming a monolayer was calculated to be 0.14 g using the above-mentioned formula (B). In formula (B), the area occupied by one molecule of n-octyltrimethoxysilane (OTMS) is set to 0.33 nm 2 , molecular weight 234 g / mol, Avogadro constant 6.02 × 10 23 The amount was determined as particles / mol.

[0045] [Example 2] The amount of n-octyltrimethoxysilane added was changed to 0.6 times that of Example 1. The other conditions were the same as those of Example 1.

[0046] Example 3 The amount of n-octyltrimethoxysilane added was changed to 0.7 times that of Example 1. The other conditions were the same as in Example 1.

[0047] Example 4 The amount of n-octyltrimethoxysilane added was changed to 1.5 times that of Example 1. The other conditions were the same as those of Example 1.

[0048] Example 5 The amount of n-octyltrimethoxysilane added was changed to 3.3 times that of Example 1. The other conditions were the same as those of Example 1.

[0049] Example 6 The other conditions were the same as in Example 1, except that n-octyltrimethoxysilane was changed to n-propyltrimethoxysilane (PTMS).

[0050] Example 7 The other conditions were the same as in Example 1, except that n-octyltrimethoxysilane was changed to n-hexyltrimethoxysilane (HTMS).

[0051] Example 8 The other conditions were the same as in Example 1, except that n-octyltrimethoxysilane was changed to n-decyltrimethoxysilane (DTMS).

[0052] Comparative Example 1 Copper nanoparticles that had not been surface-modified with a silane coupling agent were evaluated. The evaluation items were the same as those in Example 1.

[0053] Comparative Example 2 The amount of n-octyltrimethoxysilane added was changed to five times that of Example 1. The other conditions were the same as those of Example 1.

[0054] The results of Examples 1 to 5 and Comparative Example 1 are shown in Table 1.

[0055]

[0056] <Evaluation 1> Figure 1 is a graph showing the relationship between the mass carbon concentration derived from the silane coupling agent and the median diameter for the above-mentioned Examples 1 to 8 and Comparative Examples 1 and 2. In Figure 1, the X axis represents the mass carbon concentration derived from the silane coupling agent, and the Y axis represents the median diameter of the copper nanoparticles and composite copper nanoparticles dispersed in an organic solvent.

[0057] As shown in FIG. 1, from the intersection of the approximation curve derived from the results of Examples 1 to 8 and Comparative Examples 1 and 2 and the straight line with a median diameter of 0.30 μm, it was confirmed that the median diameter of the composite copper nanoparticles in an organic solvent was 0.30 μm or less when the mass carbon concentration derived from the silane coupling agent was in the range of 0.1 to 1.2% by mass.

[0058] <Evaluation 2> Figure 2 is a graph showing the relationship between the number of surface groups and the median diameter for the above-mentioned Examples 1 to 8 and Comparative Examples 1 and 2. In Figure 2, the X axis represents the number of silane coupling agents attached to the copper nanoparticle surface in 1 nm. 2 The Y axis represents the number of surface groups per nanoparticle, and the Y axis represents the median diameter of the copper nanoparticles and composite copper nanoparticles dispersed in an organic solvent.

[0059] As shown in FIG. 2, the intersection of the approximation curve derived from the results of Examples 1 to 8 and Comparative Examples 1 and 2 with the line of the median diameter of 0.30 μm indicates a 1 nm 2 It was confirmed that the median diameter of the composite copper nanoparticles in an organic solvent was 0.30 μm or less when the number of surface groups per nanoparticle was in the range of 1.0 to 13.0.

[0060] The composite copper nanoparticles of the present invention can be used as electrode film materials for various electronic components. In particular, they are suitable for electrode film materials that use oxides or ceramics as base materials and are sintered at 300°C or higher to form films. Specifically, they can be used as electrode materials for mounting electronic components such as sensors, batteries, capacitors, and resistors on printed circuit boards.

Claims

1. Composite copper nanoparticles in which the surfaces of copper nanoparticles are modified with a silane coupling agent, the copper nanoparticles having a coating containing copper oxide on at least a portion of their surfaces, and the mass carbon concentration attributable to the silane coupling agent in the composite copper nanoparticles is 0.1 to 1.2 mass% relative to the total mass of the composite copper nanoparticles.

2. The composite copper nanoparticles according to claim 1, wherein the mass carbon concentration attributable to the silane coupling agent in the composite copper nanoparticles is 0.2 to 0.5 mass% relative to the total mass of the composite copper nanoparticles.

3. The composite copper nanoparticles according to claim 1 or 2, wherein the mass carbon concentration attributable to the copper nanoparticles in the composite copper nanoparticles is 0.3 mass% or less relative to the total mass of the composite copper nanoparticles.

4. Composite copper nanoparticles in which the surface of copper nanoparticles is modified with a silane coupling agent, wherein the copper nanoparticles have a coating containing copper oxide on at least a portion of the surface, and the surface groups derived from the silane coupling agent on the surface of the composite copper nanoparticles are 1 nm or less in surface area of ​​the composite copper nanoparticles. 2 Composite copper nanoparticles having 1.0 or more and 13.0 or less per nanoparticle.

5. The composite copper nanoparticles according to claim 1 or 4, wherein the silane coupling agent is an alkylsilane.

6. The composite copper nanoparticles according to claim 5, wherein the silane coupling agent is an alkylsilane having an alkyl chain having 3 to 10 carbon atoms.

7. The composite copper nanoparticles according to claim 6, wherein the silane coupling agent is n-octyltrimethoxysilane.

8. The composite copper nanoparticles according to claim 1 or 4, wherein the average particle size of the copper nanoparticles is 200 nm or less.

9. A method for producing composite copper nanoparticles whose surfaces have been modified with a silane coupling agent, comprising: preparing copper nanoparticles having a coating containing copper oxide on at least a portion of their surfaces, an organic solvent, and a silane coupling agent; preparing a mixture of the copper nanoparticles, the organic solvent, and the silane coupling agent; pressurizing the mixture and feeding it into a capillary flow path; and dispersing the mixture by applying collision and shear force to obtain a dispersion; wherein the amount of the silane coupling agent added is 0.6 to 3.3 times the amount equivalent to forming a monomolecular film on the surface of the copper nanoparticles.