Corrosion-resistant alloy steel bar and preparation method therefor

MYPI2025000144A0Undetermined Publication Date: 2023-12-22INST OF RES OF IRON & STEEL JIANGSU PROVINCE +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025000144
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-06-22
Filing Date
2023-01-18
Publication Date
2023-12-22

AI Technical Summary

Technical Problem

The existing alloy corrosion-resistant steel bars have high Cr and Mo contents, which results in high production costs and limits their application.

Method used

By optimizing the chemical composition, reducing the Cr content, and through the related design of Si, Mn, Ti, Al and other elements, combined with the smelting, refining, continuous casting, and rolling processes, we can prepare alloys with excellent mechanical properties and corrosion resistance. Steel bars avoid the use of Mo elements.

Benefits of technology

It is possible to obtain alloy corrosion-resistant steel bars with excellent mechanical properties and corrosion resistance while reducing production costs, which is suitable for actual production and processing and reduces production difficulty.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided in the present application are a corrosion-resistant alloy steel bar and a preparation method therefor, wherein the corrosion-resistant alloy steel bar comprises, in percentage by weight: 0.05-0.25% of C, 1.05-2% of Si, 0.3-1.5% of Mn, 0.5-2.5% of Cr, 0.05-1% of Ni, 0.001-0.005% of O, 0.001-0.0035% of S, 0.005-0.1% of Ti, 0.005-0.1% of Al, 0.005-0.03% of V, and 0.005-0.03% of Nb, with the balance being Fe and inevitable impurities. The preparation method therefor comprises the successive steps of smelting, refining, continuous casting, rolling and cooling. In the present application, elements such as Si, Ti, Al and Mn are used for compensating for the reduction in corrosion resistance caused by a decrease in the content of Cr, such that the production cost of the corrosion-resistant alloy steel bar are greatly reduced. No drawing accompanying abstract
Need to check novelty before this filing date? Find Prior Art

Description

A kind of corrosion-resistant alloy steel bar and its preparation method

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to the Chinese patent application filed with the China Patent Office on June 22, 2022, with application number 202210708417.8 and invention name “A kind of alloy corrosion-resistant steel bar and its preparation method”, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present application relates to the technical field of steel bars, and in particular to an alloy corrosion-resistant steel bar and a preparation method thereof. Background Art

[0004] Reinforced concrete structures are the most important building structures, and their insufficient durability has become a major industry challenge. Alloy corrosion-resistant steel bars, which combine the appearance, mechanical properties, processing capabilities, and corrosion resistance of ordinary steel bars, have become an important means of addressing the durability issues faced by reinforced concrete structures. However, existing alloy corrosion-resistant steel bars still present some challenges that hinder their widespread adoption.

[0005] For example, patent CN112375995A discloses a 400MPa-grade corrosion-resistant steel bar and its production method. The steel bar's composition, by mass percentage, includes: Cr: 9.5-10.4%, Mo: 1.0-1.2%, Mn: 0.3-0.6%, Ni: 0.01-1%, Cu: 0.01-0.5%, C ≤ 0.014%, N ≤ 0.004%, Nb: 0.01-0.05%, Si: 0.2-0.6%, with the balance being Fe and unavoidable impurities. The steel bar has a microstructure of bainite and ferrite, and is classified as an ultra-low-carbon, high-alloy corrosion-resistant steel bar with excellent mechanical properties and corrosion resistance.

[0006] However, the high content of Cr and Mo in the alloying elements of the above-mentioned corrosion-resistant steel bars leads to high production costs, which greatly limits the application of corrosion-resistant steel bars.

[0007] Summary of the Invention

[0008] The technical problem to be solved by the present application is to overcome the defect in the prior art that the Cr and Mo contents in the alloy elements of the corrosion-resistant steel bars are high, resulting in high production costs and greatly limiting the application of the corrosion-resistant steel bars.

[0009] To this end, the present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage: C: 0.05-0.25%, Si: 1.05-2%, Mn: 0.3-1.5%, Cr: 0.5-2.5%, Ni: 0.05-1%, O: 0.001-0.005%, S: 0.001-0.0035%, Ti: 0.005-0.1%, Al: 0.005-0.1%, V: 0.005-0.03%, Nb: 0.005-0.03%; the balance is Fe and unavoidable impurities;

[0010] The contents of Si and Mn satisfy 2≤Si / Mn≤5; the contents of Si and Cr satisfy 0.75≤Si / Cr≤1.5; and the contents of Ti and Al satisfy 0.02%≤Ti+Al≤0.2%.

[0011] Optionally, the Si is 1.2-1.8%;

[0012] And / or, the Mn is 0.4-1%;

[0013] And / or, the Cr content is 0.85-2%.

[0014] Optionally, the Si content is 1.35-1.65%;

[0015] And / or, the Mn is 0.45-0.75%;

[0016] And / or, the Cr content is 1.35-1.75%.

[0017] Optionally, the C is 0.05-0.15%.

[0018] Optionally, the C is 0.07-0.12%.

[0019] Optionally, the Ti content is 0.01-0.075%;

[0020] And / or, the Al content is 0.01-0.075%.

[0021] The present application also provides a method for preparing the aforementioned alloy corrosion-resistant steel bar, comprising the steps of smelting, refining, continuous casting, rolling and cooling performed in sequence.

[0022] Optionally, the raw materials for preparing the corrosion-resistant alloy steel bar include ferrosilicon alloy and silicon-manganese alloy, and the mass ratio of the ferrosilicon alloy to the silicon-manganese alloy is (2-5):1.

[0023] Optionally, in the continuous casting process, the casting speed is 2.5-3.5 m / min;

[0024] And / or, in the cooling process, the temperature of the upper cooling bed is 820°C-1000°C;

[0025] And / or, the rolling process includes the steps of heating the continuous casting steel billet, starting rolling, and finishing rolling.

[0026] Optionally, the heating temperature of the continuous casting billet is 1150-1250°C; the starting rolling temperature is 1000-1120°C; and the finishing rolling temperature is ≥1000°C.

[0027] The technical solution of this application has the following advantages:

[0028] 1. The present application provides an alloy corrosion-resistant steel bar. Through the associated design of Si, Mn, Cr, Al, and Ti in the formula of the present application, elements such as Si, Ti, Al, and Mn are used to compensate for the decrease in corrosion resistance caused by the reduction in Cr content. As a result, without adding Mo to the formula and greatly reducing the Cr content, alloy corrosion-resistant steel bars with excellent mechanical properties and corrosion resistance can be obtained, thereby greatly reducing the production cost of the alloy corrosion-resistant steel bars.

[0029] 2. The alloy corrosion-resistant steel bar provided in this application is designed based on the chemical composition of this application, which can not only achieve the excellent corrosion resistance of the alloy corrosion-resistant steel bar, but also make the alloy corrosion-resistant steel bar have excellent mechanical properties, lower production costs, and is suitable for actual production and processing.

[0030] 3. The present application provides an alloy corrosion-resistant steel bar. Based on the chemical composition design scheme of the present application, combined with the smelting technology and controlled rolling and cooling process in the preparation method, it ensures the strengthening effect of the alloy elements and the acquisition of the ferrite + pearlite complex phase structure. While ensuring the corrosion resistance and mechanical properties of the alloy corrosion-resistant steel bar, it reduces the production difficulty and production cost. DETAILED DESCRIPTION

[0031] The following examples are provided to further better understand the present application, but are not limited to the best implementation mode described herein, and do not limit the content and protection scope of the present application. Any product identical or similar to the present application obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the scope of protection of the present application.

[0032] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in this field can be used. If the manufacturer of the reagents or instruments is not specified, they are all commercially available conventional reagents.

[0033] The particle size of the ferrosilicon alloy in this application is 10-30 mm, and its main components are calculated by weight percentage as follows: Si: 75%, S: 0.002%, C: 0.01%, Al: 0.1%, Ti: 0.01%, P: 0.02%, and the rest are iron and impurities, which were purchased from Qinghai Baitong High Purity Materials Co., Ltd.

[0034] The particle size of the silicon manganese alloy in this application is 10-30 mm, and its main components are, by weight percentage, Mn: 83%, Si: 1.94%, C: 0.65%, P: 0.15%, S: 0.005%, and the rest are iron and impurities, which were purchased from Ningxia Yitong Industrial Co., Ltd.

[0035] The ferrochrome alloy in this application has a particle size of 30-50 mm, and its main components are, by weight percentage, Cr: 60%, Si: 0.87%, C: 0.14%, S: 0.002%, P: 0.034%, and the rest are iron and impurities, which were purchased from Tianjin Haoyuan Metal Materials Co., Ltd.

[0036] The particle size of the titanium-iron alloy in this application is 10-30 mm, and its main components are, by weight percentage, Si: 1.85%, S: 0.014%, C: 0.04%, Al: 1.35%, Ti: 32.94%, P: 0.042%, Mn: 1.57%, and the rest are iron and impurities, which were purchased from Jinzhou Haixin Metal Materials Co., Ltd.

[0037] The particle size of the niobium-iron alloy in the present application is 5-30 mm, and its main components, by weight percentage, are: Nb: 65.92%, Si: 1.97%, C: 0.12%, Al: 0.94%, S: 0.018%, P: 0.258%, and the rest are iron and impurities. It was purchased from Beijing Gaoke New Material Technology Co., Ltd.

[0038] The particle size of the vanadium-nitrogen alloy in this application is 5-10 mm, and its main components are, by weight percentage, V: 77.69%, S: 0.075%, C: 5.53%, N: 14.1%, P: 0.045%, and the rest are iron and impurities, which were purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd.

[0039] In this application, nickel is added from nickel plate, with a nickel content of 99.9% and the rest being iron and impurity elements, purchased from Jiangsu Guoyan Special Steel Co., Ltd.

[0040] In this application, aluminum is added in the form of aluminum particles, with an aluminum content of 99.5% and the rest being iron and impurity elements, purchased from Xuchang Shengtong Metal Materials Co., Ltd.

[0041] Example 1

[0042] The present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage: C: 0.07%, Si: 1.35%, Mn: 0.45%, Cr: 1.35%, Ni: 0.05%, O: 0.001%, S: 0.001%, Ti: 0.01%, Al: 0.01%, V: 0.005%, Nb: 0.005%; the balance is Fe and unavoidable impurities;

[0043] The contents of Si and Mn satisfy Si / Mn=3; the contents of Si and Cr satisfy Si / Cr=1; the contents of Ti and Al satisfy Ti+Al=0.02%;

[0044] The method for preparing the above-mentioned corrosion-resistant alloy steel bar comprises the following steps:

[0045] Smelting process: smelting ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, ferrosilicon, silicon-manganese alloy, nickel plates, and aluminum pellets at 1610° C. to obtain molten steel; wherein the mass ratio of ferrosilicon to silicon-manganese alloy is 3.3:1, the mass ratio of ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, and silicon-manganese alloy is 3.3:0.05:0.1:0.05:1, the amount of nickel plates added is 60 kg, the amount of aluminum pellets added is 25 kg, and the amount of silicon-manganese alloy added is 750 kg.

[0046] Refining process: argon is introduced into the molten steel and the steel is further refined at 1550°C for 40 minutes;

[0047] Continuous casting process: The refined molten steel is made into continuous casting billets using a continuous casting machine. The casting speed is set to 3m / min during continuous casting. The cross-sectional size of the obtained continuous casting billet is 140mm. 2 ;

[0048] Rolling process: The continuous casting billet obtained in the continuous casting process is heated to 1190°C for 100 minutes, and then the starting rolling temperature is set to 1035°C and the finishing rolling temperature is set to 1000°C to obtain steel bars with a diameter of 14 mm.

[0049] Cooling process: After the steel bars obtained in the rolling process are cooled to 920℃, they are first moved to the cooling bed for cooling and then air-cooled. The conveying speed of the cooling bed is 2m / min.

[0050] Example 2

[0051] The present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage: C: 0.1%, Si: 1.5%, Mn: 0.55%, Cr: 1.5%, Ni: 0.5%, O: 0.003%, S: 0.0025%, Ti: 0.05%, Al: 0.05%, V: 0.015%, Nb: 0.015%; the balance being Fe and unavoidable impurities;

[0052] The contents of Si and Mn satisfy Si / Mn=2.7; the contents of Si and Cr satisfy Si / Cr=1; the contents of Ti and Al satisfy Ti+Al=0.1%;

[0053] The method for preparing the above-mentioned corrosion-resistant alloy steel bar comprises the following steps:

[0054] Smelting process: smelting ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, ferrosilicon, silicon-manganese alloy, nickel plates, and aluminum pellets at 1630° C. to obtain molten steel; wherein the mass ratio of ferrosilicon to silicon-manganese alloy is 3.1:1, the mass ratio of ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, and silicon-manganese alloy is 3.1:0.15:0.5:0.15:1, the amount of nickel plates added is 600 kg, the amount of aluminum pellets added is 130 kg, and the amount of silicon-manganese alloy added is 920 kg.

[0055] Refining process: argon is introduced into the molten steel and the refining is continued at 1555℃ for 40 minutes;

[0056] Continuous casting process: The refined molten steel is made into continuous casting billets using a continuous casting machine. The casting speed is set to 2.7m / min during continuous casting. The cross-sectional size of the obtained continuous casting billet is 140mm. 2 ;

[0057] Rolling process: The continuous casting billet obtained in the continuous casting process is heated to 1210℃ for 110 minutes, and then the starting rolling temperature is set to 1025℃ and the finishing rolling temperature is set to 1010℃, and steel bars with a diameter of 25mm are obtained by rolling;

[0058] Cooling process: After the steel bars obtained in the rolling process are cooled to 930℃, they are first moved to the cooling bed for cooling and then air-cooled. The conveying speed of the cooling bed is 1.5m / min.

[0059] Example 3

[0060] The present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage: C: 0.12%, Si: 1.65%, Mn: 0.75%, Cr: 1.75%, Ni: 1%, O: 0.005%, S: 0.0035%, Ti: 0.075%, Al: 0.075%, V: 0.03%, Nb: 0.03%; the balance is Fe and unavoidable impurities;

[0061] The contents of Si and Mn satisfy Si / Mn=2.2; the contents of Si and Cr satisfy Si / Cr=0.94; the contents of Ti and Al satisfy Ti+Al=0.15%;

[0062] The method for preparing the above-mentioned corrosion-resistant alloy steel bar comprises the following steps:

[0063] Smelting process: smelting ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, ferrosilicon, silicon-manganese alloy, nickel plates, and aluminum pellets at 1635° C. to obtain molten steel; wherein the mass ratio of ferrosilicon to silicon-manganese alloy is 2.5:1, the mass ratio of ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy to silicon-manganese alloy is 2.7:0.3:0.8:0.3:1, the amount of nickel plates added is 1200 kg, the amount of aluminum pellets added is 250 kg, and the amount of silicon-manganese alloy added is 1250 kg.

[0064] Refining process: argon is introduced into the molten steel and the refining is continued at 1515℃ for 50min;

[0065] Continuous casting process: The refined molten steel is made into continuous casting billets using a continuous casting machine. The casting speed is set to 2.6m / min during continuous casting. The cross-sectional size of the obtained continuous casting billet is 140mm. 2 ;

[0066] Rolling process: The continuous casting billet obtained in the continuous casting process is heated to 1210°C for 110 minutes, and then the starting rolling temperature is set to 1025°C and the finishing rolling temperature is set to 1010°C to obtain steel bars with a diameter of 32 mm;

[0067] Cooling process: After the steel bars obtained in the rolling process are cooled to 880℃, they are first moved to the cooling bed for cooling and then air-cooled. The conveying speed of the cooling bed is 1.1m / min.

[0068] Example 4

[0069] The present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage: C: 0.05%, Si: 1.2%, Mn: 0.4%, Cr: 0.85%, Ni: 0.05%, O: 0.001%, S: 0.001%, Ti: 0.005%, Al: 0.025%, V: 0.005%, Nb: 0.005%; the balance is Fe and unavoidable impurities;

[0070] The contents of Si and Mn satisfy Si / Mn=3; the contents of Si and Cr satisfy Si / Cr=1.41; the contents of Ti and Al satisfy Ti+Al=0.03%;

[0071] The method for preparing the above-mentioned corrosion-resistant alloy steel bar comprises the following steps:

[0072] Smelting process: smelting ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, ferrosilicon, silicon-manganese alloy, nickel plates, and aluminum pellets at 1600° C. to obtain molten steel; wherein the mass ratio of ferrosilicon to silicon-manganese alloy is 3.5:1, the mass ratio of ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, and silicon-manganese alloy is 2.5:0.05:0.05:0.05:1, the amount of nickel plates added is 60 kg, the amount of aluminum pellets added is 70 kg, and the amount of silicon-manganese alloy added is 670 kg.

[0073] Refining process: argon is introduced into the molten steel and the refining is continued at 1540℃ for 30min;

[0074] Continuous casting process: The refined molten steel is made into continuous casting billets using a continuous casting machine. The casting speed is set to 3m / min during continuous casting. The cross-sectional size of the obtained continuous casting billet is 140mm. 2 ;

[0075] Rolling process: The continuous casting billet obtained in the continuous casting process is heated to 1230℃ for 120 minutes, and then the starting rolling temperature is set to 1070℃ and the finishing rolling temperature is set to 1050℃ to obtain steel bars with a diameter of 28mm.

[0076] Cooling process: After the steel bars obtained in the rolling process are cooled to 920℃, they are first moved to the cooling bed for cooling and then air-cooled. The conveying speed of the cooling bed is 1.2m / min.

[0077] Example 5

[0078] The present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage: C: 0.15%, Si: 1.8%, Mn: 0.9%, Cr: 2%, Ni: 1%, O: 0.005%, S: 0.0035%, Ti: 0.1%, Al: 0.1%, V: 0.03%, Nb: 0.03%; the balance being Fe and unavoidable impurities;

[0079] The contents of Si and Mn satisfy Si / Mn=2; the contents of Si and Cr satisfy Si / Cr=0.9; the contents of Ti and Al satisfy Ti+Al=0.2%;

[0080] The method for preparing the above-mentioned corrosion-resistant alloy steel bar comprises the following steps:

[0081] Smelting process: smelting ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, ferrosilicon, silicon-manganese alloy, nickel plates, and aluminum pellets at 1639°C to obtain molten steel; wherein the mass ratio of ferrosilicon to silicon-manganese alloy is 2:1, and the mass ratio of ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy to silicon-manganese alloy is 2.5:0.3:1.2:0.3:1; the amount of nickel plates added is 1200 kg, the amount of aluminum pellets added is 30 kg, and the amount of silicon-manganese alloy added is 1500 kg;

[0082] Refining process: argon is introduced into the molten steel and the refining is continued at 1560℃ for 45 minutes;

[0083] Continuous casting process: The refined molten steel is made into continuous casting billets using a continuous casting machine. The casting speed is set to 2.5m / min during continuous casting. The cross-sectional size of the obtained continuous casting billet is 140mm. 2 ;

[0084] Rolling process: The continuous casting billet obtained in the continuous casting process is heated to 1150°C for 90 minutes, and then the starting rolling temperature is set to 1000°C and the finishing rolling temperature is set to 1000°C to obtain steel bars with a diameter of 10 mm;

[0085] Cooling process: After the steel bars obtained in the rolling process are cooled to 820℃, they are first moved to the cooling bed for cooling and then air-cooled. The conveying speed of the cooling bed is 2.2m / min.

[0086] Example 6

[0087] The present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage: C: 0.05%, Si: 1.05%, Mn: 0.3%, Cr: 0.8%, Ni: 0.05%, O: 0.001%, S: 0.001%, Ti: 0.025%, Al: 0.005%, V: 0.005%, Nb: 0.005%; the balance is Fe and unavoidable impurities;

[0088] The contents of Si and Mn satisfy Si / Mn=3.5; the contents of Si and Cr satisfy Si / Cr=1.31; the contents of Ti and Al satisfy Ti+Al=0.03%;

[0089] The method for preparing the above-mentioned corrosion-resistant alloy steel bar comprises the following steps:

[0090] Smelting process: smelting ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, ferrosilicon, silicon-manganese alloy, nickel plates, and aluminum pellets at 1650° C. to obtain molten steel; wherein the mass ratio of ferrosilicon to silicon-manganese alloy is 3.8:1, the mass ratio of ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, and silicon-manganese alloy is 2.6:0.05:0.3:0.05:1, the amount of nickel plates added is 60 kg, the amount of aluminum pellets added is 20 kg, and the amount of silicon-manganese alloy added is 500 kg;

[0091] Refining process: argon is introduced into the molten steel and the refining is continued at 1550℃ for 35min;

[0092] Continuous casting process: The refined molten steel is made into continuous casting billets using a continuous casting machine. The casting speed is set to 2.5m / min during continuous casting. The cross-sectional size of the obtained continuous casting billet is 140mm. 2 ;

[0093] Rolling process: The continuous casting billet obtained in the continuous casting process is heated to 1180°C for 100 minutes, and then the starting rolling temperature is set to 1020°C and the finishing rolling temperature is set to 1000°C to obtain steel bars with a diameter of 18 mm;

[0094] Cooling process: After the steel bars obtained in the rolling process are cooled to 860℃, they are first moved to the cooling bed for cooling and then air-cooled. The conveying speed of the cooling bed is 1.4m / min.

[0095] Example 7

[0096] The present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage: C: 0.25%, Si: 2%, Mn: 1%, Cr: 2.5%, Ni: 1%, O: 0.005%, S: 0.0035%, Ti: 0.1%, Al: 0.1%, V: 0.03%, Nb: 0.03%; the balance being Fe and unavoidable impurities;

[0097] The contents of Si and Mn satisfy Si / Mn=2; the contents of Si and Cr satisfy Si / Cr=0.8; the contents of Ti and Al satisfy Ti+Al=0.2%;

[0098] The method for preparing the above-mentioned corrosion-resistant alloy steel bar comprises the following steps:

[0099] Smelting process: smelting ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, ferrosilicon, silicon-manganese alloy, nickel plates, and aluminum pellets at 1600° C. to obtain molten steel; wherein the mass ratio of ferrosilicon to silicon-manganese alloy is 2.2:1, the mass ratio of ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, and silicon-manganese alloy is 3:0.3:1.1:0.3:1, the amount of nickel plates added is 1200 kg, the amount of aluminum pellets added is 250 kg, and the amount of silicon-manganese alloy added is 1665 kg.

[0100] Refining process: argon is introduced into the molten steel and the steel is further refined at 1540°C for 40 minutes;

[0101] Continuous casting process: The refined molten steel is made into continuous casting billets using a continuous casting machine. The casting speed is set to 2.7m / min during continuous casting. The cross-sectional size of the obtained continuous casting billet is 140mm. 2 ;

[0102] Rolling process: The continuous casting billet obtained in the continuous casting process is heated to 1250℃ for 120 minutes, and then the starting rolling temperature is set to 1120℃ and the finishing rolling temperature is set to 1100℃ to obtain steel bars with a diameter of 22mm.

[0103] Cooling process: After the steel bars obtained in the rolling process are cooled to 1000℃, they are first moved to a cooling bed for cooling and then air-cooled. The conveying speed of the cooling bed is 1.45m / min.

[0104] Example 8

[0105] The present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage, C: 0.1%, Si: 1.05%, Mn: 0.35%, Cr: 0.75%, Ni: 0.15%, O: 0.0025%, S: 0.0025%, Ti: 0.03%, Al: 0.03%, V: 0.01%, Nb: 0.01%; the balance being Fe and unavoidable impurities;

[0106] The contents of Si and Mn satisfy Si / Mn=3; the contents of Si and Cr satisfy Si / Cr=1.4; the contents of Ti and Al satisfy Ti+Al=0.06%;

[0107] The method for preparing the above-mentioned corrosion-resistant alloy steel bar comprises the following steps:

[0108] Smelting process: smelting ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, ferrosilicon, silicon-manganese alloy, nickel plates, and aluminum pellets at 1620° C. to obtain molten steel; wherein the mass ratio of ferrosilicon to silicon-manganese alloy is 3.3:1, the mass ratio of ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, and silicon-manganese alloy is 2.1:0.1:0.3:0.1:1, the amount of nickel plates added is 180 kg, the amount of aluminum pellets added is 250 kg, and the amount of silicon-manganese alloy added is 585 kg.

[0109] Refining process: argon is introduced into the molten steel and the refining is continued at 1545℃ for 40 minutes;

[0110] Continuous casting process: The refined molten steel is made into continuous casting billets using a continuous casting machine. The casting speed is set to 3.5m / min during continuous casting. The cross-sectional size of the obtained continuous casting billet is 140mm. 2 ;

[0111] Rolling process: The continuous casting billet obtained in the continuous casting process is heated to 1200°C for 100 minutes, and then the starting rolling temperature is set to 1020°C and the finishing rolling temperature is set to 1000°C to obtain steel bars with a diameter of 16 mm.

[0112] Cooling process: After the steel bars obtained in the rolling process are cooled to 880℃, they are first moved to the cooling bed for cooling and then air-cooled. The conveying speed of the cooling bed is 1.6m / min.

[0113] Example 9

[0114] The present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage: C: 0.25%, Si: 1.5%, Mn: 0.3%, Cr: 1%, Ni: 0.05%, O: 0.001%, S: 0.001%, Ti: 0.1%, Al: 0.05%, V: 0.005%, Nb: 0.005%;

[0115] The contents of Si and Mn satisfy Si / Mn=5; the contents of Si and Cr satisfy Si / Cr=1.5; the contents of Ti and Al satisfy Ti+Al=0.15%;

[0116] The method for preparing the above-mentioned corrosion-resistant alloy steel bar comprises the following steps:

[0117] Smelting process: smelting ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, ferrosilicon, silicon-manganese alloy, nickel plates, and aluminum pellets at 1650° C. to obtain molten steel; wherein the mass ratio of ferrosilicon to silicon-manganese alloy is 5:1, the mass ratio of ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, and silicon-manganese alloy is 3.3:0.05:1.1:0.05:1, the amount of nickel plate added is 60 kg, the amount of aluminum pellets added is 125 kg, and the amount of silicon-manganese alloy added is 500 kg;

[0118] Refining process: argon is introduced into the molten steel and the steel is further refined at 1560°C for 60 minutes;

[0119] Continuous casting process: The refined molten steel is made into continuous casting billets using a continuous casting machine. The casting speed is set to 3.1m / min during continuous casting. The cross-sectional size of the obtained continuous casting billet is 140mm. 2 ;

[0120] Rolling process: The continuous casting billet obtained in the continuous casting process is heated to 1230°C for 120 minutes, and then the starting rolling temperature is set to 1060°C and the finishing rolling temperature is set to 1000°C to obtain steel bars with a diameter of 22 mm;

[0121] Cooling process: After the steel bars obtained in the rolling process are cooled to 1000℃, they are first moved to a cooling bed for cooling and then air-cooled. The conveying speed of the cooling bed is 1.45m / min.

[0122] Example 10

[0123] The present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage: C: 0.05%, Si: 1.86%, Mn: 0.93%, Cr: 2.48%, Ni: 1%, O: 0.005%, S: 0.0035%, Ti: 0.005%, Al: 0.015%, V: 0.03%, Nb: 0.03%;

[0124] The contents of Si and Mn satisfy Si / Mn=2; the contents of Si and Cr satisfy Si / Cr=0.75; the contents of Ti and Al satisfy Ti+Al=0.02%;

[0125] The method for preparing the above-mentioned corrosion-resistant alloy steel bar comprises the following steps:

[0126] Smelting process: smelting ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, ferrosilicon, silicon-manganese alloy, nickel plates, and aluminum pellets at 1600° C. to obtain molten steel; wherein the mass ratio of ferrosilicon to silicon-manganese alloy is 2.2:1, the mass ratio of ferrochrome, ferroniobium, ferrotitanium, vanadium-nitrogen alloy, and silicon-manganese alloy is 3.0:0.3:0.2:0.3:1, the amount of nickel plates added is 1200 kg, the amount of aluminum pellets added is 325 kg, and the amount of silicon-manganese alloy added is 1550 kg;

[0127] Refining process: argon is introduced into the molten steel and the refining is continued at 1540℃ for 30min;

[0128] Continuous casting process: The refined molten steel is made into continuous casting billets using a continuous casting machine. The casting speed is set to 2.8m / min during continuous casting. The cross-sectional size of the obtained continuous casting billet is 140mm. 2;

[0129] Rolling process: The continuous casting billet obtained in the continuous casting process is heated to 1180°C for 90 minutes, and then the starting rolling temperature is set to 1020°C and the finishing rolling temperature is set to 1000°C to obtain steel bars with a diameter of 22 mm;

[0130] Cooling process: After the steel bars obtained in the rolling process are cooled to 950℃, they are first moved to the cooling bed for cooling and then air-cooled. The conveying speed of the cooling bed is 1.45m / min.

[0131] Comparative Example 1

[0132] The present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage: C: 0.1%, Si: 2.15%, Mn: 0.3%, Cr: 1%, Ni: 0.05%, O: 0.001%, S: 0.0035%, Ti: 0.08%, Al: 0.07%, V: 0.005%, Nb: 0.005%;

[0133] The contents of Si and Mn satisfy Si / Mn=7.17; the contents of Si and Cr satisfy Si / Cr=2.15; the contents of Ti and Al satisfy Ti+Al=0.15%;

[0134] The only difference between the above-mentioned method for preparing corrosion-resistant alloy steel bars and Example 8 is that in the smelting step, the mass ratio of ferrosilicon alloy to silicon-manganese alloy is 6.5:1, the mass ratio of ferrochromium alloy, ferroniobium alloy, ferrotitanium alloy, vanadium-nitrogen alloy and silicon-manganese alloy is 3.6:0.05:0.8:0.05:1, the amount of nickel plate added is 60 kg, the amount of aluminum particles added is 180 kg, and the amount of silicon-manganese alloy added is 500 kg.

[0135] Comparative Example 2

[0136] The present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage: C: 0.1%, Si: 1.5%, Mn: 1.65%, Cr: 1%, Ni: 0.05%, O: 0.001%, S: 0.0035%, Ti: 0.08%, Al: 0.07%, V: 0.005%, Nb: 0.005%;

[0137] The contents of Si and Mn satisfy Si / Mn=0.91; the contents of Si and Cr satisfy Si / Cr=1.5; the contents of Ti and Al satisfy Ti+Al=0.15%;

[0138] The only difference between the above-mentioned method for preparing corrosion-resistant alloy steel bars and Example 8 is that in the smelting step, the mass ratio of ferrosilicon alloy to silicon-manganese alloy is 0.8:1, the mass ratio of ferrochromium alloy, ferroniobium alloy, ferrotitanium alloy, vanadium-nitrogen alloy and silicon-manganese alloy is 0.6:0.05:0.8:0.05:1, the amount of nickel plate added is 60 kg, the amount of aluminum particles added is 180 kg, and the amount of silicon-manganese alloy added is 2750 kg.

[0139] Comparative Example 3

[0140] The present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage: C: 0.1%, Si: 1.5%, Mn: 0.3%, Cr: 3%, Ni: 0.05%, O: 0.001%, S: 0.0035%, Ti: 0.08%, Al: 0.07%, V: 0.005%, Nb: 0.005%;

[0141] The contents of Si and Mn satisfy Si / Mn=5; the contents of Si and Cr satisfy Si / Cr=0.5; the contents of Ti and Al satisfy Ti+Al=0.15%;

[0142] The only difference between the above-mentioned method for preparing corrosion-resistant alloy steel bars and Example 8 is that in the smelting step, the mass ratio of ferrosilicon alloy to silicon-manganese alloy is 4.5:1, the mass ratio of ferrochromium alloy, ferroniobium alloy, ferrotitanium alloy, vanadium-nitrogen alloy and silicon-manganese alloy is 10:0.05:0.8:0.05:1, the amount of nickel plate added is 60 kg, the amount of aluminum particles added is 180 kg, and the amount of silicon-manganese alloy added is 500 kg.

[0143] Comparative Example 4

[0144] The present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage: C: 0.1%, Si: 1.5%, Mn: 0.3%, Cr: 1%, Ni: 0.05%, O: 0.001%, S: 0.0035%, Ti: 0.15%, Al: 0.07%, V: 0.005%, Nb: 0.005%;

[0145] The contents of Si and Mn satisfy Si / Mn=5; the contents of Si and Cr satisfy Si / Cr=1.5; the contents of Ti and Al satisfy Ti+Al=0.22%;

[0146] The only difference between the above-mentioned method for preparing corrosion-resistant alloy steel bars and Example 8 is that in the smelting step, the mass ratio of ferrosilicon alloy to silicon-manganese alloy is 4.5:1, the mass ratio of ferrochromium alloy, ferroniobium alloy, ferrotitanium alloy, vanadium-nitrogen alloy and silicon-manganese alloy is 3.3:0.05:1.55:0.05:1, the amount of nickel plate added is 60 kg, the amount of aluminum particles added is 180 kg, and the amount of silicon-manganese alloy added is 500 kg.

[0147] Comparative Example 5

[0148] The present application provides an alloy corrosion-resistant steel bar, comprising, by weight percentage: C: 0.1%, Si: 1.5%, Mn: 0.3%, Cr: 1%, Ni: 0.05%, O: 0.001%, S: 0.0035%, Ti: 0.08%, Al: 0.15%, V: 0.005%, Nb: 0.005%;

[0149] The contents of Si and Mn satisfy Si / Mn=5; the contents of Si and Cr satisfy Si / Cr=1.5; the contents of Ti and Al satisfy Ti+Al=0.22%;

[0150] The only difference between the above-mentioned method for preparing corrosion-resistant alloy steel bars and Example 8 is that in the smelting step, the mass ratio of ferrosilicon alloy to silicon-manganese alloy is 4.5:1, the mass ratio of ferrochromium alloy, ferroniobium alloy, ferrotitanium alloy, vanadium-nitrogen alloy and silicon-manganese alloy is 3.3:0.05:0.8:0.05:1, the amount of nickel plate added is 60 kg, the amount of aluminum particles added is 380 kg, and the amount of silicon-manganese alloy added is 500 kg.

[0151] Test Example 1

[0152] The mechanical properties of the corrosion-resistant alloy steel bars prepared in the examples and comparative examples were tested according to the national standard GB / T228.1-2010 Metallic Materials Tensile Tests Part 1: Room Temperature Test Methods, and the strength-to-yield ratio (i.e., tensile strength / yield strength) was calculated. The test results are shown in Table 1.

[0153] Table 1. Test results of Test Example 1

[0154] It can be seen from the data in Table 1 that only when the proportions of various elements are met in this application can the yield strength be guaranteed to be ≥430 MPa, the elongation after fracture be ≥20.5%, the strength-to-yield ratio be ≥1.26, and the total elongation at maximum force be ≥10.6%. This allows excellent mechanical properties to be achieved without adding Mo to the formula and by greatly reducing the content of Cr.

[0155] Test Example 2

[0156] The microstructures of the corrosion-resistant alloy steel bars prepared in the embodiment and the comparative example were observed at a magnification of 200 times using a Zeiss optical microscope, and the volume proportion of ferrite therein was calculated. The test results are shown in Table 2.

[0157] Test Example 3

[0158] The critical chloride ion concentration for rupture of the passive film on the surface of the corrosion-resistant alloy steel bars prepared in the embodiment and the comparative example was tested using an electrochemical workstation equipped with a working electrode, a reference electrode, and a counter electrode system, and the improvement factor of the critical chloride ion concentration compared with the HRB400 steel bar was calculated. The specific testing method is as follows: the test sample is immersed in a saturated sodium hydroxide solution for 48 hours, and then loaded into the electrochemical workstation and used as a working electrode; 0.01 mol / L sodium chloride solution is added to the electrochemical workstation solution every 24 hours, and the voltage / current-chloride ion concentration curve is tested; when the current or voltage changes sharply, the corresponding chloride ion concentration value is the critical chloride ion concentration value; the calculation formula is improvement factor = critical chloride ion solubility value of the corrosion-resistant alloy steel bar / critical chloride ion concentration value of the HRB400 steel bar; the test results are shown in Table 2; the composition ratio of the HRB400 steel bar is C: 0.24%, Si: 0.40%, Mn: 1.40%, V: 0.025%, P≤0.04%, and S≤0.04%.

[0159] Test Example 4

[0160] The chloride corrosion resistance of the alloy corrosion-resistant steel bars prepared in the Examples and Comparative Examples was tested, and the improvement in chloride corrosion resistance compared to HRB400 steel bars was calculated. The specific testing method was as follows: a 100 mm long end of the alloy corrosion-resistant steel bars in each Example and Comparative Example was cut and turned using a lathe to obtain a test specimen with a diameter of 8 mm. The test specimen was then placed in a corrosion solution at a temperature of 35°C and a humidity of 80% for a salt spray corrosion test. The chloride salt in the test solution was a 5 wt % sodium chloride solution with a pH of 7.0. The test lasted for 14 days, and the weight of the test specimens before and after corrosion was measured using an electronic microbalance. The calculation formula was: improvement = weight change of the alloy corrosion-resistant steel bar before and after corrosion / weight change of the HRB400 before and after corrosion. The test results are shown in Table 2. The composition ratio of the HRB400 steel bar is C: 0.24%, Si: 0.40%, Mn: 1.40%, V: 0.025%, P≤0.04%, S≤0.04%.

[0161] Table 2. Test results of test examples 2-4

[0162] From the results in Table 2 above, it can be seen that in the alloy corrosion-resistant steel bar of the present application, the proportion of ferrite in the microstructure type reaches 53-73%. Compared with HRB400, the critical chloride ion concentration value is increased by more than 2.1 times, the chloride salt corrosion resistance is increased by more than 2.7 times, and the overall performance is significantly improved.

[0163] From the data in Tables 1 and 2, it can be concluded that the composition ratio of the present application can take into account both mechanical properties and corrosion resistance, and the comprehensive performance is significant; and the composition ratio of the present application does not contain Mo elements and the content of Cr elements is greatly reduced, which significantly reduces the cost.

[0164] Obviously, the above embodiments are merely examples for clarity of explanation and are not intended to limit the implementation methods. Those skilled in the art will readily appreciate that other variations or modifications based on the above descriptions are possible. It is not necessary and impossible to enumerate all implementation methods here. Obvious variations or modifications arising therefrom remain within the scope of protection of the present invention.

Claims

1. A corrosion-resistant alloy steel bar, characterized in that: Calculated by weight percentage, it comprises: C: 0.05-0.25%, Si: 1.05-2%, Mn: 0.3-1.5%, Cr: 0.5-2.5%, Ni: 0.05-1%, O: 0.001-0.005%, S: 0.001-0.0035%, Ti: 0.005-0.1%, Al: 0.005-0.1%, V: 0.005-0.03%, Nb: 0.005-0.03%; the balance is Fe and unavoidable impurities; The contents of Si and Mn satisfy 2≤Si / Mn≤5; the contents of Si and Cr satisfy 0.75≤Si / Cr≤1.5; and the contents of Ti and Al satisfy 0.02%≤Ti+Al≤0.2%.

2. The corrosion-resistant alloy steel bar according to claim 1, characterized in that: The Si content is 1.2-1.8%; And / or, the Mn is 0.4-1%; And / or, the Cr content is 0.85-2%.

3. The corrosion-resistant alloy steel bar according to claim 2, characterized in that: The Si content is 1.35-1.65%; And / or, the Mn is 0.45-0.75%; And / or, the Cr content is 1.35-1.75%.

4. The corrosion-resistant alloy steel bar according to claim 1, characterized in that: The C content is 0.05-0.15%.

5. The corrosion-resistant alloy steel bar according to claim 4, characterized in that: The C content is 0.07-0.12%.

6. The corrosion-resistant alloy steel bar according to claim 1, characterized in that: The Ti content is 0.01-0.075%; And / or, the Al content is 0.01-0.075%.

7. The method for preparing the corrosion-resistant alloy steel bar according to any one of claims 1 to 6, characterized in that: It includes the processes of smelting, refining, continuous casting, rolling and cooling in sequence.

8. The preparation method according to claim 7, characterized in that The raw materials for preparing the corrosion-resistant alloy steel bar include ferrosilicon alloy and silicon-manganese alloy, and the mass ratio of the ferrosilicon alloy to the silicon-manganese alloy is (2-5):

1.

9. The preparation method according to claim 7, characterized in that In the continuous casting process, the casting speed is 2.5-3.5 m / min; And / or, in the cooling process, the temperature of the upper cooling bed is 820°C-1000°C; And / or, the rolling process includes the steps of heating the continuous casting steel billet, starting rolling, and finishing rolling.

10. The preparation method according to claim 9, characterized in that The continuous casting billet is heated at a temperature of 1150-1250° C.; the start rolling temperature is 1000-1120° C.; and the finish rolling temperature is ≥1000° C.