Surface-treated steel sheet

MYPI2025000459A0Undetermined Publication Date: 2024-04-06NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025000459
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-06
Filing Date
2023-10-06
Publication Date
2024-04-06

AI Technical Summary

Technical Problem

Existing surface-treated steel sheets lack sufficient corrosion resistance and electrical conductivity, particularly in galvanized steel sheets without Mg or Al, and those with chemical conversion coatings that contain organic resins, which compromise on corrosion resistance or conductivity.

Method used

A surface-treated steel sheet with a chromate-free chemical conversion coating on a zinc-based plated steel material, where the Zn concentration is 40% by mass or more, and Mg concentration is 0% to 4.0% by mass, with specific elemental concentration profiles in the plating layer and coating to enhance barrier properties and inhibitor effects, ensuring excellent corrosion resistance and conductivity.

Benefits of technology

The described surface-treated steel sheet achieves improved corrosion resistance and electrical conductivity by optimizing elemental concentrations in the plating layer and coating, providing enhanced barrier properties and inhibitor effects, thus addressing the limitations of prior art in both flat and processed parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025000459_DRAWING_001
    Figure PI2025000459_DRAWING_001
  • Figure PI2025000459_DRAWING_002
    Figure PI2025000459_DRAWING_002
Patent Text Reader

Abstract

ABSTRACT SURFACE-TREATED STEEL SHEET The surface-treated steel sheet is a surface-treated steel sheet including a base steel sheet, a plating layer formed on a surface of the base steel sheet, and a coating formed on a surface of the plating layer, in which the plating layer has a Zn concentration of 40 mass% or more and 100 mass% or less, and a Mg concentration of 0 mass% or more and less than 4.0 mass%, and a maximum concentration of Ti in mass%, a maximum concentration of Zr in mass%, and a maximum concentration of V in mass% from the interface to a center in the thickness direction from the interface to the surface satisfy a predetermined relationship, and an average concentration of C in mass% in the center portion of the coating, a maximum concentration of Mg in mass% in the boundary region of the coating, an average concentration of Mg in mass% in the center portion of the coating, a maximum concentration of F in mass% in the boundary region of the coating, an average concentration of F in mass% in the center portion of the coating, and an average concentration of Si in mass% in the center portion of the coating satisfy a predetermined relationship. FIG. 1
Need to check novelty before this filing date? Find Prior Art

Description

Surface-treated steel sheet

[0001] The present invention relates to a surface-treated steel sheet. This application claims priority based on Japanese Patent Application No. 2022-161691 filed on October 6, 2022, and Japanese Patent Application No. 2022-161692 filed on October 6, 2022, the contents of which are incorporated herein by reference.

[0002] Conventionally, plated steel sheets (zinc-plated steel sheets) having a plating layer mainly composed of zinc formed on the surface of the steel sheet have been used in a wide range of applications, such as automobiles, building materials, and home appliances. Furthermore, for the purpose of imparting corrosion resistance, paint adhesion, and the like to the surface of such zinc-plated steel sheets, methods such as chromate treatment using a treatment solution containing chromic acid, dichromic acid, or a salt thereof as a main component, treatment using a metal surface treatment agent that does not contain chromium, phosphate treatment, treatment using a silane coupling agent alone, and organic resin coating treatment are commonly known and in practical use.

[0003] In recent years, in response to various legal restrictions on hexavalent chromium compounds, which may have adverse effects on the environment and human health, development of chromium-free metal surface treatment agents has been promoted. Examples of chromium-free metal surface treatment agents include technologies using oxides or hydroxides of Group 4 metals such as Ti and Zr. For example, Patent Document 1 discloses a chromate-free chemically treated steel sheet having a zinc-plated or zinc-alloy-plated steel sheet as a substrate, in which a chemical conversion coating containing a valve metal oxide or hydroxide and a fluoride, both of which exhibit high insulation resistance, is formed on the surface of the substrate. Patent Document 2 also discloses a hot-dip zinc alloy-plated steel sheet with excellent corrosion resistance, in which a chemical conversion coating containing one or more of a valve metal hydroxide, oxide, oxyacid, oxyacid acid salt, and fluoride as the main components is formed on a Mg-containing zinc alloy plating layer via an interfacial reaction layer containing one or more compounds selected from magnesium fluoride, magnesium phosphate, and a composite compound of magnesium and a valve metal oxyacid acid salt. In Patent Document 2, a zinc alloy plating layer containing Mg is used as a base, and an interfacial reaction layer containing Mg is formed, thereby achieving high white rust resistance (corrosion resistance). Also, Patent Document 3 discloses a hot-dip zinc alloy-plated steel sheet with excellent corrosion resistance, in which a composite chemical conversion coating of Ti and V is formed on a Zn-Al alloy plating layer via an interfacial reaction layer of Al-F. In Patent Document 3, a zinc alloy plating layer containing Al is used as a base, and an Al-F reaction layer is formed, thereby achieving high white rust resistance. Patent Document 4 also describes a chromate-free precoated metal sheet having an upper coating film (α) formed on at least one side of the metal sheet, wherein (1) a silane coupling agent (A) containing an amino group in the molecule and a silane coupling agent (B) containing a glycidyl group in the molecule are blended and reacted between the metal sheet and the upper coating film (α), and the silane coupling agent (A) has a cyclic siloxane bond and a chain siloxane bond in its structure, and the abundance ratio of the cyclic siloxane bond and the chain siloxane bond is 1090 to 1100 cm, which indicates a cyclic siloxane bond by FT-IR reflection method. -1 The absorbance (C1) and the linear siloxane bond at 1030-1040 cm -1and (2) an inhibitor component (Y) containing at least one metal compound (E) selected from titanium compounds and zirconium compounds, a phosphate compound (J), and a fluorine compound (F), wherein the ratio of the absorbance (C1) of the metal compound (C) to the absorbance (C2) of the metal compound (C) [C1 / C2] is 0.4 to 2.5; and (3) an inhibitor component (Y) containing at least one metal compound (E) selected from titanium compounds and zirconium compounds, a phosphate compound (J), and a fluorine compound (F), provided that when the metal compound (E) is a fluorometal complex compound (E'), the fluorine compound (F) may not be contained.

[0004] Japanese Patent Publication No. 2002-194558 Japanese Patent Publication No. 2007-23309 Japanese Patent Publication No. 2003-306777 Japanese Patent Publication No. 2012-237065

[0005] The technologies disclosed in Patent Documents 1 to 3 are excellent technologies that have been put to practical use as surface-treated steel sheets that have undergone chromate-free surface treatments with excellent corrosion resistance. To improve the corrosion resistance of chromate-free treatments, technologies for forming a reaction layer containing metal elements contained in the plating layer have been used, as described in Patent Documents 2 and 3. However, due to the recent increasing sophistication of customer needs, it has become clear that these prior art technologies may not provide sufficient corrosion resistance. For example, with zinc-plated steel sheets using plating that does not contain Mg or Al, it is difficult to form the reaction layer described in Patent Documents 2 or 3, resulting in insufficient corrosion resistance in flat (planar) and processed areas. Furthermore, even in the case of zinc-plated steel sheets using plating containing Mg and Al in the plating layer, when a chemical conversion coating (film) is formed in a continuous hot-dip galvanized steel sheet production line, from the viewpoint of productivity, the time from applying a chemical conversion treatment solution to the surface of a zinc-based plated steel sheet to drying to form a chemical conversion coating is very short, within 5 seconds. Therefore, since the Zn phase of the zinc alloy plating contains only trace amounts of Mg and Al, it is difficult to form the reaction layer on the Zn phase of the plating, resulting in insufficient corrosion resistance. Furthermore, Patent Document 4 requires the inclusion of an organic resin as a film-forming component. Therefore, even if the coating exhibits excellent corrosion resistance and coating adhesion, it suffers from the problem of poor electrical conductivity. For these reasons, there is a demand for surface-treated steel sheets that exhibit excellent corrosion resistance (white rust resistance) and electrical conductivity in both processed and flat areas.

[0006] An object of the present invention is to provide a surface-treated steel sheet having excellent corrosion resistance and electrical conductivity, based on the premise that the surface of a zinc-based plated steel material has a plating layer containing zinc or a zinc alloy on the surface of the steel material and a chromate-free chemical conversion coating on the surface of the zinc-based plated steel material.

[0007] The corrosion resistance of surface-treated steel materials bearing a chemical conversion coating improves with increasing barrier properties (i.e., the ability to block the penetration of corrosion factors such as moisture and chloride ions) of the chemical conversion coating. Furthermore, in areas where the chemical conversion coating is damaged due to scratches or other defects, the greater the inhibitor effect (the ability of substances (mainly metal elements) in the chemical conversion coating to dissolve and prevent corrosion of the plating layer when moisture adheres) is increased, the better the corrosion resistance, including white rust resistance, improves. As described above, the chemical conversion coatings disclosed in Patent Documents 1 to 3 possess both barrier and inhibitor properties. However, in environments requiring higher white rust resistance than conventional coatings, these properties are insufficient, raising concerns that they may corrode the plating layer and cause early white rust formation. In light of these circumstances, the present inventors investigated methods for improving the barrier properties and inhibitor effect of chemical conversion coatings, assuming that the chemical conversion coating does not contain organic resins from the perspective of electrical conductivity. As a result, they discovered that when a chemical conversion coating is formed on the surface of a zinc plating layer or zinc alloy plating layer in a short period of time, the barrier properties of the chemical conversion coating can be improved and corrosion resistance can be dramatically increased by forming multiple locations where specific elements are concentrated in addition to controlling the concentration of each element between the vicinity of the interface between the Zn phase of the zinc plating layer or zinc alloy plating layer and the chemical conversion coating and the surface of the chemical conversion coating.

[0008] The present invention has been made in light of the above findings. The gist of the present invention is as follows. [1] A surface-treated steel sheet according to one embodiment of the present invention is a surface-treated steel sheet comprising: a base steel sheet; a plating layer formed on the surface of the base steel sheet; and a coating formed on the surface of the plating layer, wherein the Zn concentration of the plating layer is 40 mass% or more and 100 mass% or less, and the Mg concentration is 0 mass% or more and less than 4.0 mass%, and when the concentrations of C, O, F, Mg, Al, Si, P, Ti, V, Zn, and Zr are continuously measured by linear analysis in the thickness direction from the plating layer toward the surface of the surface-treated steel sheet, the position where the Zn concentration first becomes 35.0 mass% or less is defined as the interface between the plating layer and the coating, and a region including the interface and extending from a range of 10 nm from the interface toward the plating layer in the thickness direction to a range of 15 nm toward the coating in the thickness direction is defined as a boundary region, and a region 10 nm from the center of the interface and the surface of the coating toward the surface in the thickness direction is defined as a center part of the coating. One or more of the following formulae (1) to (3) and (4) to (12) are satisfied.Dti≧5.0 (1) Dzr≧5.0 (2) Dv≧5.0 (3) Dti+Dzr+Dv≦25.0 (4) Bc<10.0 (5) 5.0 / M≦Amg≦25.0 (6) 0.5≦Bmg≦5.0 (7) 15.0 / M≦Af≦40.0 (8) 0.5≦Bf≦15.0 (9) Amg / Bmg≧2.0 (10) Af / Bf≧2.0 (11) Bsi<5.0 (12) where Dti is the maximum concentration of Ti in mass % from the interface to the center in the thickness direction between the interface and the surface, Dzr is the maximum concentration of Zr in mass % from the interface to the center in the thickness direction between the interface and the surface, Dv is the maximum concentration of V in mass % from the interface to the center in the thickness direction between the interface and the surface, Bc is the average concentration of C in mass % in the center of the coating, Amg is the maximum concentration of Mg in mass % in the boundary region of the coating, Bmg is the average concentration of Mg in mass % in the center of the coating, Af is the maximum concentration of F in mass % in the boundary region of the coating, Bf is the average concentration of F in mass % in the center of the coating, Bsi is the average concentration of Si in mass % in the center of the coating, and M is a constant that is 1 when the Mg concentration of the plating layer is 0 mass % or more and less than 1.0 mass %, and is 2 when the Mg concentration of the plating layer is 1.0 mass % or more and less than 4.0 mass %. [2] The surface-treated steel sheet according to [1] may further satisfy the following formula (13): 0≦Cmg<5.0 (13), where Cmg is the Mg concentration in mass % at a position 10 nm from the interface toward the coating layer in the thickness direction of the coating layer. [3] The surface-treated steel sheet according to [1] or [2] may further satisfy the following formulas (14) to (16).5.0≦Aal≦20.0 (14) 0.2≦Bal≦5.0 (15) Aal / Bal≧5.0 (16) where Aal is the maximum concentration of Al in mass% in the boundary region, and Bal is the average concentration of Al in mass% in the central portion of the coating. [4] The surface-treated steel sheet according to any of [1] to [3] may further satisfy the following formulas (17) to (18): 10.0≦Ap≦25.0 (17) 0.5≦Bp≦8.0 (18) where Ap is the maximum concentration of P in mass% in the boundary region, and Bp is the average concentration of P in mass% in the central portion of the coating. [5] The surface-treated steel sheet according to any of [1] to [4] may further satisfy the following formula (19): 1.0≦Bzn≦30.0 (19), where Bzn is the average concentration of Zn in mass % in the central portion of the coating. [6] The surface-treated steel sheet according to any one of [1] to [5] may further satisfy the following formula (20): Af / Bf≧2.5 (20).

[0009] According to the above aspect of the present invention, it is possible to provide a surface-treated steel sheet having excellent corrosion resistance and electrical conductivity.

[0010] 1 is a schematic diagram showing an example of a cross section of a surface-treated steel sheet according to an embodiment of the present invention, and FIG. 2 is a diagram showing an example of an elemental analysis result in the thickness direction obtained using an FE-TEM equipped with an energy dispersive X-ray analyzer.

[0011] A surface-treated steel sheet according to one embodiment of the present invention (surface-treated steel sheet according to this embodiment) will be described. In the following description, the numerical ranges enclosed by "to" are defined by the symbols "to" and "less than," and the values ​​at both ends are included as the lower and upper limits of the range. On the other hand, values ​​indicated as "greater than" or "less than" are not included in the numerical range. Furthermore, all ratios (e.g., A mg / B mg, which is the ratio of A mg to B mg, as described below) are dimensionless. As shown in FIG. 1 , the surface-treated steel sheet 1 according to this embodiment includes a base steel sheet 10, a plating layer 20 formed on the surface of the base steel sheet 10, and a coating 30 formed on the surface of the plating layer 20. The plating layer 20 is a zinc plating layer or zinc alloy plating layer containing 0% or more and less than 4.0% Mg. From the viewpoint of electrical conductivity, it is not preferable to further include a coating containing an organic resin on the coating 30. Therefore, the steel sheet 10 may include a base steel sheet 10, a plating layer 20 formed on the surface of the base steel sheet 10, and a coating 30 formed on the surface of the plating layer 20. The coating 30 is, for example, a chemical conversion coating. In this embodiment, when the concentrations (concentration distributions) of C, O, F, Mg, Al, Si, P, Ti, V, Zn, and Zr are continuously measured by linear analysis in the thickness direction from the plating layer toward the surface of the coated steel sheet, the position where the Zn concentration first becomes 35.0 mass% or less is defined as the interface 25 between the plating layer 20 and the coating 30. In addition, a region including the interface 25 and extending from the interface 25 in the thickness direction between a range of 10 nm toward the plating layer 20 and a range of 15 nm toward the coating 30 is defined as a boundary region A. The plating layer 20 and the coating 30 may be formed on one side or both sides of the base steel sheet 10.

[0012] The X-ray analysis is performed using a field emission-transmission electron microscope (FE-TEM) equipped with an energy dispersive X-ray analyzer, for example, under the following conditions: A test piece is cut out from the surface-treated steel sheet on which a coating has been formed by a cryo-focused ion beam (FIB) method, and the cross-sectional structure of the cut out test piece is observed with a transmission electron microscope (TEM) at a magnification (100,000 to 1,000,000 times) that allows the entire coating and part of the Zn phase of the plating layer to be seen in the field of view. To identify the constituent elements of each layer, TEM-EDS (Energy Dispersive X-ray Spectroscopy) is used to continuously measure the concentrations of C, O, F, Mg, Al, Si, P, Ti, V, Zn, and Zr in the thickness direction from the plating layer toward the surface of the coating, which is also the surface of the coated steel sheet. The acceleration voltage during observation and EDS analysis is 200 kV. When observed with an FE-TEM, the plating layer is clearly different from the coating, so that when observed with an FE-TEM, a position that is clearly different from the coating can be determined to be the plating layer. The starting point of the line analysis may be, for example, any position in the plating layer observed with the FE-TEM. Furthermore, even if the plating layer cannot be sufficiently identified by FE-TEM observation, if, for example, the Zn concentration is 85 mass% or higher and the Mg concentration and Al concentration are both 1.0 mass% or lower at the start point of the EDS line analysis, the start point is certainly the plating layer, and there is no need to repeat the FE-TEM observation or the EDS line analysis. The end point of the line analysis may be a position at which the below-described Bmg (average concentration of Mg and the like in the center portion B of the coating described below) can be measured and calculated. For example, the end point of the line analysis may be a position 30%, 20%, or 10% of the thickness of the coating from the surface of the coated steel sheet, or may be the surface of the coating (the surface of the coated steel sheet).

[0013] Although line analysis is also possible with EPMA, EPMA cannot perform observations at higher magnifications than TEM, and therefore cannot analyze the concentration distribution of each element in the coating of the surface-treated steel sheet according to this embodiment with high precision. Therefore, in this embodiment, line analysis is performed using an FE-TEM equipped with an energy dispersive X-ray analyzer.

[0014] The base steel sheet, the plating layer, and the coating will each be described below.

[0015] <Base Steel Sheet> The surface-treated steel sheet according to this embodiment has excellent corrosion resistance due to the plating layer and coating. Therefore, the base steel sheet is not particularly limited. The base steel sheet may be determined depending on the product to which it is applied, the required strength, plate thickness, etc. For example, hot-rolled mild steel sheets and steel strips, or hot-rolled steel sheets and steel strips for automotive structures (sometimes collectively referred to as hot-rolled steel sheets) described in JIS G 3131:2018 or JIS G 3113:2018, or cold-rolled steel sheets and steel strips, or automotive workable cold-rolled high-tensile steel sheets and steel strips (sometimes collectively referred to as cold-rolled steel sheets) described in JIS G 3141:2021 or JIS G 3135:2018, may be used.

[0016] <Plated Layer> The chemical composition of the plated layer provided on the surface-treated steel sheet according to this embodiment has a zinc (Zn) concentration (content) of 40 mass% or more and 100 mass% or less, and a Mg concentration (content) of 0 mass% or more and less than 4.0 mass%. The plated layer is a zinc plated layer or a zinc alloy plated layer. Regarding the chemical composition of the plating layer, elements other than Zn and Mg are not limited, but may be, for example, in mass %, Al: 0% or more and less than 25.0%, Sn: 0% or more and less than 20%, Bi: 0% or more and less than 5.0%, In: 0% or more and less than 2.0%, Ca: 0% or more and less than 3.0%, Y: 0% or more and less than 0.5%, La: 0% or more and less than 0.5%, Ce: 0% or more and less than 0.5%, Si: 0% or more and less than 2.5%, Cr: 0% or more and less than 0.25%, Ti: 0% or more and less than 0.25%, Ni: 0% or more and less than 0.25%, Co: 0% or more and less than 0.25%, V: 0% or more and less than 0.25%, Nb: 0% or more and less than 0.25%, The plating layer may contain Cu: 0% or more but less than 0.25%, Mn: 0% or more but less than 0.25%, Fe: 0% or more but less than 5.0%, Sr: 0% or more but less than 0.5%, Sb: 0% or more but less than 0.5%, Pb: 0% or more but less than 0.5%, B: 0% or more but less than 0.5%, and the balance: impurities. Elements other than Zn, including Mg and Al, are all optional elements, with their lower limits being 0%. In other words, the chemical composition of the plating layer may consist only of Zn and impurities. If necessary, the Mg concentration may be 0.1% or more, 0.5% or more, or 1.0% or more, and the Mg concentration may be 3.5% or less, 3.0% or less, or 2.5% or less. If necessary, the Al concentration may be 0.1% or more, 0.2% or more, 1.0% or more, or 4.0% or more, and the Al concentration may be 21.0% or less, 17.0% or less, or 12.0% or less. If necessary, the Zn concentration may be 50% or more, 60% or more, 70% or more, 80% or more, or 85% or more, and the Zn concentration may be less than 100%, less than 99%, less than 97%, or less than 95%. It is preferable that the total concentration of impurities is less than 1.0%.

[0017] The chemical composition of the plating layer can be determined by dissolving the plating layer in, for example, a 10% HCl aqueous solution containing an inhibitor that suppresses corrosion of the base steel (base steel sheet) (for example, IBIT manufactured by Asahi Chemical Industry Co., Ltd.), and then performing composition analysis by ICP atomic emission spectrometry.

[0018] The coating weight of the plating layer is not limited, but in order to improve corrosion resistance, it is recommended to use 10 g / m per side. 2 On the other hand, the amount of adhesion per side is preferably 200 g / m or more. 2 If the coating amount exceeds 200 g / m, the corrosion resistance will be saturated and it will be economically disadvantageous. 2 It is preferable that:

[0019] The type of the plated layer is not limited, and may be, for example, a hot-dip plated layer or an electroplated layer.

[0020] <Coating> In the surface-treated steel sheet according to this embodiment, the coating is present on the plating layer (the surface opposite to the base steel sheet). The coating may be referred to as a chemical conversion coating, a primer coating, a surface treatment coating, or the like. In this embodiment, the central portion B of the coating is defined as a range extending 10 nm from the center of the interface between the plating layer and the coating and the surface of the coating toward the surface in the thickness direction. The coating is a chemical conversion coating formed by applying a chemical conversion solution containing an aqueous solution containing any of Ti, Zr, or V, Mg, and F, to which phosphoric acid and nitric acid have been added, and then drying the solution, as described below. The coating contains any of Ti, Zr, or V, Mg, and F, and may also contain P and Si. In terms of electrical conductivity, the coating does not contain an organic resin.

[0021] In the coating provided on the surface-treated steel sheet according to this embodiment (the coating according to this embodiment), where Dti (unit: mass %) is the maximum concentration of Ti, Dzr (unit: mass %) is the maximum concentration of Zr in mass %, and Dv (unit: mass %) is the maximum concentration of V in mass %, from the interface to the center in the thickness direction between the interface and the surface, one or more selected from Dti, Dzr, and Dv are 5.0% or more, and the total of one or more is 25.0% or less. In this case, the barrier properties of the coating are enhanced. Since increasing each value makes the coating brittle and reduces the barrier properties, the total of Dti, Dzr, and Dv is preferably 20.0% or less. That is, the surface-treated steel sheet according to this embodiment satisfies one or more of formulas (1) to (3) and formula (4). Dti≧5.0 (1) Dzr≧5.0 (2) Dv≧5.0 (3) Dti+Dzr+Dv≦25.0 (4)

[0022] In the coating according to this embodiment, the average concentration of C (Bc (unit: mass %)) at the center portion B of the coating described above is less than 10.0%. That is, the surface-treated steel sheet according to this embodiment satisfies formula (5). Bc<10.0 (5) If Bc is 10.0% or more, the barrier properties of the coating are reduced, resulting in poor corrosion resistance. As mentioned above, in terms of electrical conductivity, the coating is substantially free of organic resin (1 mass % or less). There is no simple measurement method that can confirm that the organic resin content is 1 mass % or less through coating analysis. However, as the amount of organic resin in the surface treatment solution increases, the C concentration in the coating increases. For this reason, in this embodiment, Bc is set to less than 10.0% as an indicator that the organic resin content is 1 mass % or less. To obtain excellent corrosion resistance, Bc is more preferably 6.0% or less, 4.5% or less, or 3.0% or less. Since the lower limit of Bc is not limited, the lower limit of Bc is 0%. If necessary, Bc may be set to 0.5% or more, 1.0% or more, or 1.5% or more.

[0023] Furthermore, in the coating according to this embodiment, the maximum Mg concentration Amg (unit: mass %) in the boundary region A is 2.5 to 25.0%, the average Mg concentration Bmg (unit: mass %) in the central portion B of the coating is 0.5 to 5.0%, and the ratio of Amg to Bmg, Amg / Bmg, is 2.0 or greater. In other words, Mg is concentrated near the interface. By containing a predetermined amount of Mg and concentrating Mg near the interface, the barrier properties of the coating are improved, and its corrosion resistance is enhanced. If Amg is less than 2.5%, Bmg is less than 0.5%, or Amg / Bmg is less than 2.0, the effect of improving corrosion resistance is not sufficiently achieved. However, if the Mg concentration in the plating layer is less than 1.0 mass%, an Amg of less than 5.0% will not be effective. This is thought to be because, due to the large volume fraction of Zn in the coating structure, in order to suppress the occurrence of white rust, it is necessary to form a stronger Mg-enriched layer than a coating layer containing a higher amount of Mg (1.0% or more). Therefore, when the Mg concentration of the coating layer is 0% or more but less than 1.0% by mass, Amg is 5.0 to 25.0%. On the other hand, if Amg exceeds 25.0%, the adhesion between the coating and the coating decreases, resulting in a decrease in corrosion resistance. If Bmg exceeds 5.0%, no Mg-enriched portion is formed, resulting in a decrease in corrosion resistance.

[0024] That is, the surface-treated steel sheet according to this embodiment satisfies the following formulas (6), (7), and (10): 5.0 / M≦Amg≦25.0 (6) 0.5≦Bmg≦5.0 (7) Amg / Bmg≧2.0 (10) Here, M is a constant such that M=1 when the Mg concentration in the chemical composition of the coating layer is 0% or more and less than 1.0%, in mass%, and M=2 when the Mg concentration is 1.0% or more and less than 4.0%. If necessary, Amg may be set to 20.0% or less, 15.0% or less, 12.0% or less, 10.0% or less, or 8.0% or less. In particular, only when the Mg concentration in the chemical composition of the coating layer is 1.0% or more and less than 4.0% by mass, the upper limit of Amg may be limited; for example, Amg may be set to 12.0% or less, 10.0% or less, 8.0% or less, or 6.0% or less. Furthermore, B mg may be set to 4.0% or less, 3.0% or less, or 2.0% or less, as needed. There is no need to particularly set an upper limit for A mg / B mg, but A mg / B mg may be set to 20.0 or less, 15.0 or less, or 10.0 or less. As needed, A mg / B mg may be set to 2.5 or more, 3.5 or more, or 4.5 or more.

[0025] F also enhances the barrier properties of the coating, and like Mg, it is contained in a predetermined amount in the coating and then concentrated near the interface. Specifically, in the coating, the maximum F concentration Af (unit: mass %) in the boundary region A is 7.5 to 40.0%, the average F concentration Bf (unit: mass %) in the central portion B of the coating is 0.5 to 15.0%, and the ratio of Af to Bf, Af / Bf, is 2.0 or greater. When Af is less than 7.5%, Bf is less than 0.5%, or Af / Bf is less than 2.0, the effect of improving corrosion resistance is not sufficiently achieved. However, when the Mg concentration of the coating layer is less than 1.0 mass%, the effect is not achieved when Af is less than 15.0%. This is thought to be because the volume fraction of Zn in the coating structure is large, and therefore, to suppress the occurrence of white rust, it is necessary to form a stronger F-concentrated layer than a coating layer containing more Mg. Therefore, when the Mg concentration in the plating layer is 0% or more and less than 1.0% by mass, Af is 15.0 to 40.0%. On the other hand, if Af exceeds 40.0%, excess F impairs the barrier properties and reduces corrosion resistance. If Bf exceeds 15.0%, no F-enriched areas are formed, and excellent corrosion resistance cannot be obtained.

[0026] That is, the surface-treated steel sheet according to this embodiment satisfies the following formulas (8), (9), and (11): 15.0 / M≦Af≦40.0 (8) 0.5≦Bf≦15.0 (9) Af / Bf≧2.0 (11) Here, M is a constant that is 1 (i.e., M=1) when the Mg concentration in the chemical composition of the coating layer is 0% or more and less than 1.0%, in mass%, and is 2 (i.e., M=2) when the Mg concentration is 1.0% or more and less than 4.0%. Furthermore, preferably, the surface-treated steel sheet satisfies the following formula (20): Af / Bf≧2.5 (20) If necessary, Af may be set to 38.0% or less, 35.0% or less, 30.0% or less, 25.0% or less, or 20.0% or less. In particular, only when the Mg concentration in the chemical composition of the plating layer is 1.0 mass% or more and less than 4.0 mass%, the upper limit of Af may be limited. For example, Af may be set to 25.0% or less, 20.0% or less, 16.0% or less, or 12.0% or less. Furthermore, Bf may be set to 12.0% or less, 10.0% or less, or 7.5% or less, as needed. There is no particular need to set an upper limit for Af / Bf, but Af / Bf may be set to 50.0 or less, 30.0 or less, 20.0 or less, or 10.0 or less. As needed, Af / Bf may be set to 3.0 or more, 3.5 or more, or 4.5 or more.

[0027] In the coating according to this embodiment, Bsi (unit: mass%), which is the average concentration of Si in the central portion B of the coating, is less than 5.0%. That is, the surface-treated steel sheet according to this embodiment satisfies the following formula (12): Bsi<5.0 (12) If Bsi is 5.0% or more, a coating with barrier properties will not be formed and corrosion resistance will decrease. From the viewpoint of improving corrosion resistance, Bsi is more preferably 2.0% or less. If necessary, Bsi may be set to 1.5% or less, 1.0% or less, or 0.5% or less. The lower limit of Bsi is 0%, but Bsi may be set to 0.1% or more.

[0028] In the surface-treated steel sheet according to this embodiment, the average Zn concentration Bzn (unit: mass%) in the center portion B of the coating is preferably 1.0 to 30.0%. That is, the surface-treated steel sheet according to this embodiment preferably satisfies the following formula (19): 1.0≦Bzn≦30.0 (19) The inclusion of Zn in the coating improves corrosion resistance. If Bzn is less than 1.0%, this effect cannot be sufficiently obtained. On the other hand, if Bzn exceeds 30.0%, corrosion resistance decreases, which is not preferable. If necessary, Bzn may be set to 25.0% or less, 21.0% or less, or 18.0% or less, or Bzn may be set to 1.5% or more, 2.0% or more, 3.5% or more, or 5.0% or more.

[0029] In the surface-treated steel sheet according to this embodiment, it is preferable that the maximum Al concentration, Aal (unit: mass%), in the boundary region A is 5.0 to 20.0%, the average Al concentration, Bal (unit: mass%), in the central portion B of the coating is 0.2 to 5.0%, and the ratio of Aal to Bal, Aal / Bal, is 5.0 or more. Bal is more preferably 0.2 to 1.0%. That is, the surface-treated steel sheet according to this embodiment preferably satisfies the following formulas (14) to (16): 5.0≦Aal≦20.0 (14) 0.2≦Bal≦5.0 (15) Aal / Bal≧5.0 (16) In this case, corrosion resistance (white rust resistance) is improved. Taking the Al concentration in the coating layer into consideration, Aal may be set to 20.0% or less or 15.0% or less. Aal may be 0.5% or more, 1.0% or more, 3.0% or more, 7.0% or more, or 10.0% or more. Bal may be 3.0% or less, 2.0% or less, or 1.0% or less, and Bal may be 0.1% or more, or 0.3% or more. There is no need to particularly set an upper limit for Aal / Bal, but Aal / Bal may be 80.0 or less, 60.0 or less, or 30.0 or less. If necessary, Aal / Bal may be 7.0 or more, 10.0 or more, or 15.0 or more.

[0030] Furthermore, it is preferable that the maximum P concentration Ap (unit: mass %) in the boundary region A is 10.0 to 25.0%, and the average P concentration Bp (unit: mass %) in the central portion B of the coating is 0.5 to 8.0%. That is, it is preferable that the surface-treated steel sheet according to this embodiment satisfies the following formulas (17) and (18): 10.0≦Ap≦25.0 (17) 0.5≦Bp≦8.0 (18) In this case, corrosion resistance is improved.

[0031] The coating amount is 150 to 800 mg / m 2 Preferably, the coating amount is 150 mg / m 2 If the coating amount is less than 800 mg / m, the corrosion resistance may decrease. 2 If it exceeds 10 ...

[0032] Furthermore, it is preferable that the Mg concentration Cmg (unit: mass%) at the position in the boundary region A closest to the coating layer (a position 10 nm from the interface to the coating layer in the thickness direction) is 0% or more and less than 5.0%. That is, it is preferable that the surface-treated steel sheet according to this embodiment satisfies the following formula (13): 0≦Cmg<5.0 (13) In this case, cracks in the coating due to processing are reduced, thereby improving the corrosion resistance of the processed portion.

[0033] <Manufacturing Method> Next, a preferred manufacturing method of the surface-treated steel sheet according to this embodiment will be described. The surface-treated steel sheet according to this embodiment can obtain the effects as long as it has the above-mentioned characteristics regardless of the manufacturing method, but the manufacturing method described below is preferred because it can be manufactured stably.

[0034] That is, the surface-treated steel sheet according to this embodiment can be produced by a production method including the following steps: (I) a plating step of forming a plating layer containing zinc or a zinc alloy on the surface of a steel sheet, and (II) a coating formation step of applying a chemical conversion treatment solution to the steel sheet having the plating layer, and then heating and drying the applied solution to form a coating.

[0035] [Plating Process] In the plating process, a steel material such as a steel sheet is immersed in a plating bath containing Zn or a Zn alloy, or electroplated, to form a plating layer on the surface. The method for forming the plating layer is not particularly limited. A conventional method may be used so long as sufficient plating adhesion is obtained. The steel sheet subjected to the plating process and its manufacturing method are also not limited. Examples of steel sheets that can be immersed in the plating bath include hot-rolled mild steel sheets and steel strips described in JIS G 3131:2018 or JIS G 3113:2018, hot-rolled steel sheets and steel strips for automotive structures, cold-rolled steel sheets and steel strips described in JIS G 3141:2021 or JIS G 3135:2018, and workable cold-rolled high-tensile steel sheets and steel strips for automobiles. The composition of the plating bath can be adjusted according to the chemical composition of the desired plating layer. After the steel material is pulled out of the coating bath, the coating weight of the coating layer can be adjusted by wiping, if necessary. When Cmg is set to 0% or more and less than 5.0%, the Mg concentration in the coating layer is preferably set to 0% by mass or more and 3.0% by mass or less. When Aal / Bal is set to 5.0 or more, the Al concentration in the coating layer is preferably set to 0.1% by mass or more.

[0036] [Coating Formation Process] In this process, a chemical conversion treatment solution is applied to a steel sheet having a plating layer, and then heated and dried to form a coating (chemical conversion coating). When forming the coating according to this embodiment, the chemical conversion treatment solution is an aqueous solution containing any one of Ti, Zr, or V, Mg, and F, and optionally Si, to which phosphoric acid and nitric acid are further added. Applying such a treatment solution makes it possible to concentrate specific elements at the interface between the plating layer and the coating. Specifically, the concentrations of each element and the concentrations of phosphoric acid and nitric acid in the chemical conversion treatment solution are set as follows. Here, the concentrations of phosphoric acid and nitric acid do not include the concentrations of phosphates, nitrates, etc. By simultaneously including phosphoric acid and nitric acid within the above-mentioned ranges, dissolution of the plating proceeds and specific substances are concentrated at the interface between the chemical conversion coating and the plating, thereby significantly improving adhesion. One or more of Ti, V, Zr: 5.0 to 20.0 g / L Mg: 0.7 to 7.0 g / L F: 14.4 to 46.1 g / L P: 6.8 to 32.9 g / L Si: 0.0 to 0.4 g / L Phosphoric acid: 10.0 to 80.0 g / L Nitric acid: 5.0 to 40.0 g / L When Ap and Bp are to be within the specified ranges, it is preferable that the P concentration in the chemical conversion treatment solution be 10.0 g / L or higher.

[0037] Furthermore, when Bzn is set to 1.0 to 30.0% in order to improve corrosion resistance, it is preferable to control the contact time between the treatment solution and the plated steel sheet when applying the chemical conversion treatment solution using a roll coater, thereby setting the Zn concentration in the treatment solution to 0.5 to 5.0 g / L on a mass basis. The Zn concentration can be adjusted by immersing the plated steel sheet in the treatment solution or by adding Zn powder. To increase Bzn, Zn powder or a Zn compound may be added to the chemical conversion treatment solution. Even when Zn powder or a Zn compound is not added to the chemical conversion treatment solution, Zn diffuses from the plating layer, so Bzn often does not reach 0%.

[0038] Examples of magnesium that can be contained in the chemical conversion treatment solution include magnesium fluoride, magnesium nitrate, magnesium sulfate, magnesium chloride, and magnesium acetate.

[0039] The F contained in the chemical conversion treatment solution is a fluorine compound, such as hydrofluoric acid HF or hydrofluoroboric acid BF. 4 H, hydrosilicofluoric acid H 2 SiF 6 , fluorozirconium chloride H 2 ZrF 6 , Titanium Hydrofluoric Acid H 2 TiF 6 Examples of compounds include the following. The compound may be one type or a combination of two or more types. Among these, hydrofluoric acid is more preferred. When hydrofluoric acid is used, better corrosion resistance and paintability can be obtained.

[0040] When Zr is contained in the chemical conversion treatment solution, examples of Zr compounds include ammonium zirconium carbonate, hexafluorozirconic acid, and ammonium zirconium hexafluorooxide. When V is contained, examples of V compounds include vanadium pentoxide V. 2 O 5 , metavanadate HVO 3 , ammonium metavanadate, sodium metavanadate, vanadium oxytrichloride VOCl 3 , vanadium trioxide V 2 O 3 , vanadium dioxide VO 2 , vanadium oxysulfate VOSO 4 , vanadium oxyacetylacetonate VO(OC(=CH 2 ) CH 2 COCH 3 )) 2 , vanadium acetylacetonate V(OC(=CH 2 ) CH 2 COCH 3 )) 3 , vanadium trichloride VCl 3Examples of suitable vanadium compounds include phosphovanadomolybdic acid and phosphonic acid. It is also possible to use a pentavalent vanadium compound reduced to a tetravalent or divalent vanadium using an organic compound having at least one functional group selected from the group consisting of a hydroxyl group, a carbonyl group, a carboxyl group, a primary to tertiary amino group, an amide group, a phosphate group, and a phosphonic acid group. When titanium is contained, examples of suitable titanium compounds include ammonium hexafluorotitanate, titanium hydrofluoric acid, and titanium nitrate.

[0041] There are no limitations on the method for applying the chemical conversion treatment solution, and it can be applied using, for example, a roll coater, a bar coater, a sprayer, or the like.

[0042] After the chemical conversion treatment liquid is applied, it is heated to the maximum heating temperature (maximum reached temperature (PMT)) within 5 seconds after application and dried. The average heating rate during heating up to PMT -10°C is preferably 5 to 50°C / s. When Aal / Bal is set to 5.0 or more, it is preferable to use two-stage heating, with the heating rate in the latter half being faster than the heating rate in the first half. Specifically, if the time from the start of heating to the temperature reaching a temperature (PMT -10°C) 10°C lower than the maximum heating temperature (PMT) is defined as t, the average heating rate V2 in the latter half from the start of heating to 0.5t to 1.0t is preferably 1.25 times or more the average heating rate V1 in the first half from the start of heating to 0.5t, i.e., V2 / V1 ≧ 1.25. Furthermore, when two-stage heating is used to set Aal / Bal to 5.0 or more, it is preferable that the heating rate V1 in the first half be 5°C / s or more. Furthermore, if the furnace time for heating and drying is long, F tends to concentrate near the interface, resulting in a large Af / Bf ratio. For example, if the furnace time is set to 15 seconds or longer, the Af / Bf ratio can be set to 2.5 or higher. Furthermore, when heating, it is preferable to spray the solution onto the steel sheet through a punched metal (a steel sheet having multiple through holes).

[0043] A metal sheet (plated steel sheet) having a plating layer composition shown in Table 1 was prepared. The coating weight of the plating layer was 70 g / m 2Metal sheet No. 1 was produced by electroplating, Nos. 2 to 8 by hot-dip galvanizing, and No. 4 by heat treatment (alloying treatment) after hot-dip galvanizing. In Table 1, for example, 99.6% Zn-0.2% Al indicates a composition containing 99.6% Zn and 0.2% Al, and the same applies to other compositions. The remainder of the plating layer composition is impurities. The base material of the plated steel sheet was a cold-rolled steel sheet that satisfied JIS G3141:2021.

[0044]

[0045] Chemical conversion treatment solutions having the compositions shown in Tables 4-1, 4-2, and 5 were applied to these plated steel sheets. The chemical conversion treatment solutions were applied using a roll coater. However, for No. 48 and No. 118, the chemical conversion treatment solution contained 1.1% by weight of polyurethane resin as an organic resin component. The element concentrations in the chemical conversion treatment solutions were as shown in Tables 2-1, 2-2, and 3 (NH 4 ) 2 TiF 6 , (NH 4 ) 2 ZrF 6 , V 2 O 5 , MgHPO 4 ・3H 2 O, H 3 P.O. 4 , N.H. 4 F, HNO 3 , Ca(NO 3 ) 2 ・4H 2 O.C. 5 H 12 O 3The temperature was adjusted by mixing Si (vinyltrimethoxysilane) as needed. After applying the chemical conversion treatment solution, hot air was blown onto the steel plate through a punched metal (a steel plate having a plurality of through holes) within 5 seconds, and the steel plate was heated to the dry plate temperature (PMT) shown in Tables 4-1, 4-2, and 5 under the conditions shown in Tables 4-1, 4-2, and 5, and then cooled to 20°C by air cooling by blowing air through the punched metal or by water cooling. In this manner, surface-treated steel plates Nos. 1 to 50 and 101 to 120 were obtained. Here, in Tables 4-1, 4-2, and 5, "heating rate V1" refers to the average temperature rising rate in the first half of the time until a temperature 10°C lower than the maximum heating temperature (PMT) (PMT - 10°C) is reached, and "heating rate V2" refers to the average temperature rising rate in the second half of the time until a temperature 10°C lower than the maximum heating temperature (PMT) (PMT - 10°C) is reached. The coating weight of the chemical conversion coating was 400 mg / m, except for No. 40 and No. 41. 2 No. 40 was 150 mg / m 2 No. 41 is 800 mg / m 2 It was decided.

[0046]

[0047]

[0048]

[0049]

[0050]

[0051]

[0052] Test pieces were cut out from the prepared chemical conversion treated steel sheets by a cooling function equipped FIB (Focused Ion Beam) processing method, and the cross-sectional structure of the cut out test piece was observed with a field emission transmission electron microscope (FE-TEM) equipped with an energy dispersive X-ray analyzer at a magnification that allowed the entire coating and plating layer to be included in the observation field. 2Since a Zn phase and a Zn phase were present, the Zn phase was identified by contrast (the relatively bright portion of the dark-field image was determined to be the Zn phase). EDS analysis showed that the Zn phase had a Zn concentration of 85% or more and both the Mg and Al concentrations were 1.0% or less, and the concentration distributions of C, O, F, Mg, Al, Si, P, Ti, V, Zn, and Zr from the position confirmed to be the coating layer to the surface of the coated steel sheet were measured using an energy dispersive X-ray analyzer. The results are shown in Tables 6-1 to 9. Furthermore, Figure 2 shows the results of measuring the depth profile of element distribution for Example Test No. 40.

[0053]

[0054]

[0055]

[0056]

[0057]

[0058]

[0059] Furthermore, the white rust resistance (flat corrosion resistance) of the flat portion, the corrosion resistance of the processed portion, and the electrical conductivity were evaluated by the following methods. The results are shown in Tables 10-1, 10-2, and 11.

[0060] <Flat Corrosion Resistance> A neutral salt spray test conforming to JIS Z 2371:2015 was conducted on flat test specimens (rectangular test specimens measuring 70 mm x 150 mm) at a salt concentration of 70 g ± 5 g / L for 72, 120, 168, and 240 hours, and the corrosion resistance was evaluated based on the occurrence of white rust (area ratio) on the test specimens after the test. The evaluation criteria for corrosion resistance are as follows. If the specimens were SSS or SS after 168 hours, they were judged to have sufficient corrosion resistance. (Evaluation Criteria for Corrosion Resistance) SSS: 3% or less SS: More than 3% and 5% or less S: More than 5% and 10% or less A: More than 10% and 30% or less B: More than 30% and 50% or less C: More than 50%

[0061] <Corrosion resistance of processed parts (white rust resistance)> The center of a flat test piece (a rectangular test piece of 70 mm x 150 mm) was subjected to an Erichsen test (7 mm extrusion), and then a salt spray test according to JIS Z 2371:2015 was performed for 72 hours, and the occurrence of white rust in the extruded part was observed. The evaluation criteria were the same as for the corrosion resistance of the flat part, and if it was SS or S, it was determined that the material had sufficient corrosion resistance. (Evaluation criteria for corrosion resistance) SS: more than 5% and 10% or less S: more than 10% and 30% or less A: more than 30% and 50% or less B: more than 50%

[0062] <Conductivity> Using JIS C 2550-4:2011 A method, the total area of ​​10 contact electrodes is 1000 mm 2 The interlaminar resistance coefficient was measured under the following conditions. If it was rated A, it was determined that the electrical conductivity was sufficient. (Evaluation criteria for electrical conductivity) A: Interlaminar resistance coefficient was 300 Ω mm 2 Less than C: Interlayer resistance coefficient is 300 Ω mm 2 End

[0063]

[0064]

[0065]

[0066] As can be seen from Tables 1 to 11, Test Nos. 1 to 23, 40 to 42, 50, 101 to 106, and 120, which have a steel sheet, a plating layer, and a coating, and in which the elements are distributed as specified in the present invention from the plating layer to the surface of the coating, are excellent in both corrosion resistance and electrical conductivity. On the other hand, Test Nos. 24 to 39, 43 to 49, and 107 to 119, in which the element distribution is outside the range of the present invention, are poor in corrosion resistance. Furthermore, Test Nos. 48 and 118, which contain an organic resin, are also poor in electrical conductivity.

[0067] INDUSTRIAL APPLICABILITY According to the present invention, a surface-treated steel sheet having excellent corrosion resistance and electrical conductivity can be provided, and the present invention has high industrial applicability.

[0068] REFERENCE SIGNS LIST 1 Surface-treated steel sheet 10 Base steel sheet (steel sheet) 20 Plated layer (zinc plated layer or zinc alloy plated layer) 30 Coating (chemical conversion coating) 25 Interface A Boundary region B Center of coating

Claims

1. A surface-treated steel sheet comprising: a base steel sheet; a plating layer formed on the surface of the base steel sheet; and a coating formed on the surface of the plating layer, wherein the Zn concentration of the plating layer is 40 mass% or more and 100 mass% or less, and the Mg concentration is 0 mass% or more and less than 4.0 mass%, and when the concentrations of C, O, F, Mg, Al, Si, P, Ti, V, Zn, and Zr are continuously measured by linear analysis in the thickness direction from the plating layer toward the surface of the surface-treated steel sheet, the position where the Zn concentration becomes 35.0 mass% or less is defined as the interface between the plating layer and the coating, and a region including the interface and extending in the thickness direction from a range of 10 nm toward the plating layer side to a range of 15 nm toward the coating side is defined as a boundary region, and a region in the thickness direction from the center between the interface and the surface of the coating toward a range of 10 nm toward the surface is defined as a center of the coating, A surface-treated steel sheet, characterized by satisfying one or more of the following formulae (1) to (3) and (4) to (12):Dti≧5.0 (1) Dzr≧5.0 (2) Dv≧5.0 (3) Dti+Dzr+Dv≦25.0 (4) Bc<10.0 (5) 5.0 / M≦Amg≦25.0 (6) 0.5≦Bmg≦5.0 (7) 15.0 / M≦Af≦40.0 (8) 0.5≦Bf≦15.0 (9) Amg / Bmg≧2.0 (10) Af / Bf≧2.0 (11) Bsi<5.0 (12) where Dti is the maximum concentration of Ti in mass % from the interface to the center in the thickness direction between the interface and the surface, Dzr is the maximum concentration of Zr in mass % from the interface to the center in the thickness direction between the interface and the surface, Dv is the maximum concentration of V in mass % from the interface to the center in the thickness direction between the interface and the surface, Bc is the average concentration of C in mass % in the center of the coating, Amg is the maximum concentration of Mg in mass % in the boundary region of the coating, Bmg is the average concentration of Mg in mass % in the center of the coating, Af is the maximum concentration of F in mass % in the boundary region of the coating, Bf is the average concentration of F in mass % in the center of the coating, Bsi is the average concentration of Si in mass % in the center of the coating, and M is a constant that is 1 when the Mg concentration of the plating layer is 0 mass % or more and less than 1.0 mass %, and is 2 when the Mg concentration of the plating layer is 1.0 mass % or more and less than 4.0 mass %.

2. The surface-treated steel sheet according to claim 1, further satisfying the following formula (13): 0≦Cmg<5.0 (13), where Cmg is the Mg concentration in mass % at a position 10 nm from the interface toward the coating layer in the thickness direction of the coating layer.

3. The surface-treated steel sheet according to claim 1 or 2, further satisfying the following formulae (14) to (16): 5.0≦Aal≦20.0 (14) 0.2≦Bal≦5.0 (15) Aal / Bal≧5.0 (16), where Aal is the maximum concentration of Al in mass% in the boundary region, and Bal is the average concentration of Al in mass% in the central portion of the coating.

4. The surface-treated steel sheet according to any one of claims 1 to 3, further satisfying the following formulas (17) and (18): 10.0≦Ap≦25.0 (17) 0.5≦Bp≦8.0 (18) wherein Ap is the maximum concentration of P in mass % in the boundary region, and Bp is the average concentration of P in mass % in the central portion of the coating.

5. The surface-treated steel sheet according to any one of claims 1 to 4, further satisfying the following formula (19): 1.0≦Bzn≦30.0 (19), where Bzn is the average concentration of Zn in mass % in the central portion of the coating.

6. The surface-treated steel sheet according to any one of claims 1 to 5, further satisfying the following formula (20): Af / Bf≧2.5 (20)