Method for producing iron ore pellet

MYPI2025000522A0Undetermined Publication Date: 2024-03-02JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025000522
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-02
Filing Date
2023-05-10
Publication Date
2024-03-02

AI Technical Summary

Technical Problem

The existing methods for producing iron ore pellets face challenges in preventing bursting during the drying or firing process, especially when using low-grade ores with higher crystallized water content, which leads to a decrease in pellet strength and stability.

Method used

A method involving pulverizing low-grade iron ore with an iron content of 63% or less to obtain ore powder with specific particle size distribution characteristics, including a cumulative 90% diameter of 150 μm or less and a particle size distribution index between 14,700 and 510,000, to suppress bursting and enhance pellet strength.

Benefits of technology

The method effectively reduces the likelihood of bursting and maintains sufficient strength in green pellets, allowing for stable handling and firing, even with low-grade ores, by optimizing the particle size distribution and volatile content.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A pellet production method that can suppress bursting of green pellets can be provided. The method for producing an iron ore pellet includes grinding iron ore with iron content of 63 mass% or less to obtain ore powder, in which a volatile matter of the iron ore is 3.3 mass% or more, the ore powder has a cumulative 90 % diameter of 150 μm or less in a volume-based particle size distribution and a particle size distribution index based on the harmonic mean diameter of 14,700 or more and 510,000 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Iron ore pellet manufacturing method

[0001] The present disclosure relates to a method for producing iron ore pellets.

[0002] In the shaft furnace reduction process, which is currently the mainstream direct reduction ironmaking process, lump ore or pellets are used as the charging materials. Pellets are produced through the processes of crushing, mixing, granulating, and firing the ore. In this production process, iron ore pellets before firing (so-called green pellets) must be strong enough to prevent crumbling and powdering during handling, such as transportation from the granulation process to the firing process. Therefore, efforts are being made to improve the strength of green pellets.

[0003] Japanese Patent Laid-Open Publication No. 2000-273552 (Patent Document 1) discloses a method for producing reducing agent-mixed pellets. In this pellet production method, at least one of carboxymethyl cellulose and polyvinyl alcohol, or tar, is added to powdered iron ore and coal as a reducing agent, and moisture is added in a granulator to form pellets, producing reducing agent-mixed pellets. The reducing agent-mixed pellets are then dried in a dryer at an ambient temperature of 150°C to 170°C. The dropping strength of the dried reducing agent-mixed pellets is said to be significantly improved by using a hydrocarbon binder such as carboxymethyl cellulose, polyvinyl alcohol, or tar.

[0004] Japanese Patent Laid-Open Publication No. 2002-206120 (Patent Document 2) discloses pellets for a reducing furnace, a manufacturing method thereof, and a method for reducing metal oxides. In this pellet manufacturing method, raw materials discharged from a raw material storage tank are mixed in a mixer, and pellets are produced in a pan-type granulator using fine powder containing metal oxides and carbon as raw materials. These pellets are classified in a pellet sieve, dried in a pellet dryer, and then fired and reduced in a rotary hearth-type reducing furnace, preventing the raw material pellets from collapsing.

[0005] Japanese Patent Laid-Open No. 2009-161791 (Patent Document 3) discloses a method for producing carbon-containing unburned pellets for blast furnaces. This pellet production method involves adding a hydraulic binder to finely powdered iron-containing raw materials and finely powdered carbonaceous materials, adjusting the blending ratio of the finely powdered carbonaceous materials so that the carbon content in all raw materials is 15 to 25 mass %, and then mixing and granulating while adjusting the moisture content, followed by curing, to produce pellets with a cold crushing strength of 85 kg / cm. 2 In this method for producing carbon-containing uncalcined pellets for blast furnaces, the curing treatment involves leaving the pellets after granulation in the air for 12 to 48 hours in a primary curing yard, then loading the pellets into a shaft furnace for secondary curing, where they are subjected to steam injection treatment at a temperature of 60 to 90°C for a treatment time of 5 hours or more, followed by a continuous drying treatment, with the total treatment time for the steam injection treatment and drying treatment being within 8 hours.

[0006] JP 2000-273552 A JP 2002-206120 A JP 2009-161791 A

[0007] As described above, iron ore pellets (green pellets) are produced using ore powder, which is obtained by crushing iron ore into a powder. However, if the particle size of the ore powder is reduced to increase the strength of the green pellets, the green pellets become denser, making them more susceptible to bursting during the drying or firing process. Bursting refers to the phenomenon in which the green pellets burst, explode, or break into powder due to the pressure of the vapor generated inside the green pellets when the volatile components of the iron ore in the green pellets evaporate. The volatile components of the iron ore in the green pellets include, for example, the water of crystallization of the iron ore in the green pellets. Bursting causes cracks in the pellets, significantly reducing their strength after firing.

[0008] As described above, since the presence of crystallization water can cause bursting, currently, high-grade ore with little crystallization water is generally used as the raw ore (iron ore) for pellets. However, as demand for high-grade ore increases in the future, it is predicted that it will become difficult to secure a stable supply of high-grade ore. Therefore, the use of low-grade ore produced in Australia, India, etc., with an iron content (total Fe content) of 63 mass% or less, is being considered. However, as the crystallization water in iron ore pellets (green pellets) increases, they become more prone to bursting, as described above. Therefore, it is desirable to provide a pellet manufacturing method that can suppress bursting of green pellets.

[0009] The present disclosure has been made in view of the above circumstances, and its object is to provide a method for producing pellets that can suppress bursting of green pellets.

[0010] To achieve the above object, the method for producing iron ore pellets according to the present disclosure is as follows.

[0011] [1] A method for producing iron ore pellets, comprising: a crushing step of crushing iron ore having an iron content of 63% by mass or less to obtain ore powder, wherein the iron ore has a volatile content of 3.3% by mass or more, and the ore powder has a cumulative 90% diameter of 150 μm or less in a volume-based particle size distribution, and a particle size distribution index defined by the following formulas (1) to (4) of 14,700 or more and 510,000 or less. where Dp is the harmonic mean diameter (μm), Isp is the particle size distribution index, wi is the particle ratio, and di (μm) is the representative particle diameter.

[0012] The method for producing iron ore pellets according to the present disclosure may further be as follows.

[0013] [2] The method for producing iron ore pellets according to the above [1], wherein the volatile content of the iron ore is 12.0 mass% or less.

[0014] [3] The method for producing iron ore pellets according to the above [1] or [2], wherein the ore powder has a cumulative 50% diameter in a volume-based particle size distribution of less than 61 μm.

[0015] [4] The method for producing iron ore pellets according to any one of [1] to [3], wherein the ore powder has a cumulative 10% diameter in a volume-based particle size distribution of less than 7.1 μm.

[0016] [5] The method for producing iron ore pellets according to any one of [1] to [4] above, wherein the ore powder has a harmonic mean diameter of less than 13 μm.

[0017] According to the iron ore pellet manufacturing method of the present disclosure, it is possible to provide a pellet manufacturing method that can suppress bursting of green pellets.

[0018] A method for producing iron ore pellets according to an embodiment of the present disclosure will be described.

[0019] First, an overview of a method for producing iron ore pellets according to this embodiment will be described. The iron ore pellets according to this embodiment are so-called green pellets (pellets before calcination). The method for producing iron ore pellets according to this embodiment includes a crushing step in which iron ore having an iron content of 63% by mass or less (so-called low-grade ore) is crushed to obtain ore powder. In the following description, iron ore having an iron content of 63% by mass or less will be simply referred to as iron ore.

[0020] In the method for producing iron ore pellets according to this embodiment, the volatile content of the iron ore used to obtain the ore powder is 3.3 mass % or more.

[0021] The ore powder has a cumulative 90% diameter of 150 μm or less in the volume-based particle size distribution. The particle size distribution index of the ore powder, as defined by the above-mentioned formulas (1) to (4), is 14,700 or more and 510,000 or less. Note that the particle ratio wi in formulas (1), (3), and (4) is the particle ratio in the range of the representative particle diameter di when the particle size distribution is evaluated by dividing it into predetermined particle diameter ranges.

[0022] According to the iron ore pellet manufacturing method of this embodiment, it is possible to provide a pellet manufacturing method that can suppress bursting of green pellets.

[0023] In this embodiment, bursting refers to a phenomenon in which, when the volatile components of the iron ore in the green pellets evaporate, the green pellets burst, explode, or break into powder due to the pressure of the vapor of the volatile components generated inside the green pellets.

[0024] The method for producing iron ore pellets according to this embodiment will be described in detail below.

[0025] In the present embodiment, the iron ore pellets are pellets before firing, so-called green pellets. In the following description, to distinguish between pellets before and after firing, the iron ore pellets according to the present embodiment (pellets before firing) may be referred to as green pellets, and the pellets after firing may be referred to as fired pellets. In the present embodiment, the green pellets and the fired pellets may contain auxiliary materials other than iron ore (e.g., bentonite).

[0026] In addition to the above-described crushing step, the method for producing iron ore pellets according to this embodiment may further include a granulation step of granulating the ore powder to obtain green pellets. The green pellets may then be fired in a firing step to form fired pellets.

[0027] The type and blend (ore blend) of iron ore used as the raw material for green pellets are not particularly limited. The raw material for green pellets may consist of a single iron ore or may be a mixture of multiple ores in any blend.

[0028] In this embodiment, the volatile content of the iron ore used as the raw material for the green pellets refers to the moisture adsorbed by the iron ore and the water of crystallization contained in the iron ore crystals. That is, the volatile content of the iron ore in the green pellets refers to, for example, the moisture adsorbed by the iron ore in the green pellets and the water of crystallization of the iron ore in the green pellets. The content of the volatile content can be measured as the weight loss of the iron ore (LOI: Loss On Ignition) when the iron ore is held at 1000°C for 30 minutes.

[0029] In this embodiment, iron ore having a volatile content of 3.3% by mass or more is used as the raw material for green pellets. This allows the use of inexpensive or readily available iron ore raw material. The volatile content of the iron ore is preferably 12.0% by mass or less.

[0030] The pulverization step is a step of pulverizing iron ore to obtain ore powder (iron ore powder) in which the iron ore is pulverized. In this embodiment, the pulverization method of the iron ore in the pulverization step and the pulverization time required for pulverization are not particularly limited. The iron ore can be pulverized using, for example, a ball mill, a hammer mill, a roll pulverizer, or the like.

[0031] The shape of the ore powder is not particularly limited. The particle size (particle diameter) of the ore powder is preferably, for example, 250 μm or less (for example, passing through a 250 μm sieve, so-called 250 μm pass). If the ore powder contains coarse particles with a particle size exceeding 250 μm, the strength of the green pellets may decrease.

[0032] In this embodiment, the particle size distribution of the ore powder is a value measured using a laser diffraction particle size measurement device (Malvern, Mastersizer 3000). Water is used as the dispersion medium when measuring the particle size distribution.

[0033] The particle size distribution of the ore powder is such that the cumulative 90% diameter in the volumetric particle size distribution is 150 μm or less. Furthermore, in this embodiment, as described above, the particle size distribution index of the ore powder is defined by the above formulas (1) to (4), i.e., the particle size distribution index based on the harmonic mean diameter, is 14,700 or more and 510,000 or less. These factors can suppress pellet bursting.

[0034] As described above, bursting is a phenomenon in which the green pellets explode or break into powder due to the evaporation of volatiles from the iron ore in the green pellets when the green pellets are heated. More specifically, bursting is a phenomenon in which the green pellets burst, explode, or break into powder due to the pressure of steam generated inside the green pellets when the green pellets dry or when water of crystallization is released from the iron ore crystals in the green pellets.

[0035] The harmonic mean diameter is often used, for example, when evaluating the permeability of particle beds or packed beds. Therefore, it is considered suitable for evaluating the ease of steam escape from the inside to the outside of green pellets. Furthermore, in general, in a powder-packed bed, for example, the broader the particle size distribution, the larger the particle size ratio between the largest and smallest particles. This results in relatively small particles filling the spaces between the relatively large particles, resulting in a decrease in the porosity of the powder-packed bed. Therefore, the particle size distribution index, which represents the broadness of the particle size distribution, is considered suitable for evaluating the ease of steam escape from the inside to the outside of green pellets.

[0036] The particle size distribution of the ore powder is preferably such that the cumulative 50% diameter in the volumetric particle size distribution is less than 61 μm, which can better suppress pellet bursting. Furthermore, the particle size distribution of the ore powder is preferably such that the cumulative 10% diameter in the volumetric particle size distribution is less than 7.1 μm, which can also better suppress pellet bursting.

[0037] The particle size distribution of the ore powder preferably has a harmonic mean diameter of less than 13 μm.

[0038] The granulation process is a process of granulating ore powder to obtain iron ore pellets (green pellets). The granulation method in the granulation process is not limited. In the granulation process, the ore powder may be granulated using, for example, a pelletizer. As the pelletizer, for example, a pan-type granulator (so-called pan pelletizer) may be used.

[0039] In this embodiment, the shape and size (e.g., particle size and average particle size) of the iron ore pellets are not particularly limited and may be any value. The size of the green pellets may be evaluated by measuring the major axis diameter and minor axis diameter using a vernier caliper, and averaging the measured diameters to determine the particle size of the green pellets. The particle size of the green pellets is preferably 9 mm to 16 mm, which is commonly used in this technical field.

[0040] The green pellets are then fired in a firing process to form fired pellets. The firing temperature in the firing process is, for example, 1200°C to 1350°C.

[0041] The likelihood of bursting, i.e., bursting property, can be evaluated based on the temperature at which bursting occurs when the temperature of the green pellets is increased by gradually heating them, for example. That is, if the temperature at which bursting occurs is low, bursting is likely to occur (bursting property is high), and it can be evaluated as not being good from the viewpoint of bursting suppression. Conversely, if the temperature at which bursting occurs is high, bursting is unlikely to occur (bursting property is low), and it can be evaluated as being good from the viewpoint of bursting suppression.

[0042] Green pellets were produced according to the following procedure, and the strength and bursting properties of the pellets were evaluated.

[0043] Ores (A, B) with chemical compositions shown in Table 1 were used as the iron ore used as the raw material (raw ore) for the green pellets. Note that "LOI" in Table 1 indicates the content (mass%) of volatile matter such as crystal water, as described above. Also, in Table 1, "T.Fe" represents the mass% iron content (total Fe content) in the iron ore. Note that "T.Fe" is a value determined based on the total iron determination method for iron ore specified in JIS M 8212:2022. As shown in Table 1, both Ore A and Ore B used as raw materials for the green pellets are iron ores with a T.Fe content of 63 mass% or less (so-called low-grade ores). The following examples illustrate the cases where the raw material for the green pellets is only ore A or only ore B, but by mixing ore A and ore B in any ratio, the volatile content of the iron ore used as the raw material for the green pellets can be changed or adjusted within the range of 3.3 mass% or more and 12.0 mass% or less.

[0044]

[0045] Ore A or Ore B shown in Table 1 was pulverized in a ball mill to obtain ore powders No. 1 to No. 13 having particle size distributions shown in Table 2. In pulverizing Ore A or Ore B, the particle size distribution of the ore powder was differentiated by adjusting the pulverization time and sieving.

[0046] In Table 2, "D10" indicates the cumulative 10% diameter on a volume basis, "D50" indicates the cumulative 50% diameter (median diameter) on a volume basis, and "D90" indicates the cumulative 90% diameter on a volume basis. Also in Table 2, "Dp" indicates the harmonic mean diameter, and "Isp" indicates the particle size distribution index (see Equation 2) based on the harmonic mean diameter. The particle size distributions shown in Table 2 were derived based on the particle diameters of the ore powder measured using a laser diffraction particle size analyzer (Malvern, Mastersizer 3000). The dispersion medium used in measuring the particle size distribution was water. The measurement range for the particle size distribution was 0.01 μm to 3500 μm, and this range was divided into 101 intervals for measurement. As shown in Table 2, the ore powders of Production Nos. 1 to 13 had a cumulative 90% diameter of 150 μm or less in the volume-based particle size distribution.

[0047]

[0048] Next, the ore powders of Production Nos. 1 to 13 were granulated in a pan-type granulator (pelletizer, pan diameter 1.2 m) to obtain green pellets (granulation process). Granulation was performed by gradually adding water while rolling the ore powder on a rotating pan (rotation speed 10 rpm). The rolling ore powder was gradually granulated with the addition of water and rolling, and when it grew into pellets with diameters of 9.5 mm to 12 mm, these were collected. The pellets that grew to 9.5 mm to 12 mm were further rolled on the pan for 10 minutes to obtain roughly spherical green pellets. The amount of water added during the above granulation was approximately 10% of the weight of the green pellets.

[0049] Table 3 shows the evaluation results of the strength ("Drop Strength" in Table 3) and bursting property ("Burst Temperature" in Table 3) of green pellets of Production Nos. 1 to 13. For ease of reference, Table 3 lists the same "Isp" as in Table 2.

[0050]

[0051] In Table 3, "Drop Strength" indicates the evaluation results of the strength of the green pellets based on a drop test. In this example, the drop test was performed by dropping each green pellet of each production number from a height of 50 cm and measuring the number of times (number of drops) until the green pellet cracked or broke. The number of drops was used as the drop strength. That is, the higher the drop strength value, the higher the strength of the green pellet. Conversely, the lower the drop strength value, the lower the strength of the green pellet. Note that the number of drops used as the drop strength does not include the number of drops that resulted in cracks or breakage of the green pellet. In other words, the drop strength is the number of times the green pellet could be dropped without cracking or breaking. In this example, the average (arithmetic mean) of 10 green pellets was used as the drop strength.

[0052] In Table 3, "bursting temperature" indicates the evaluation results regarding bursting properties. The bursting temperature indicates the temperature at which bursting occurs when the green pellets are gradually heated to increase their temperature. That is, when the bursting temperature is low, the bursting properties are high. On the other hand, when the bursting temperature is high, the bursting properties are low.

[0053] In this example, the "bursting temperature" is a temperature measured as follows. First, 200 g of green pellets are loaded into a vertical cylindrical furnace (diameter 50 mm). Then, hot air heated to 200°C is passed from below the layer of green pellets to above it at a velocity of 1.0 m / sec (converted to 0°C / 1 atmosphere) for 10 minutes. Thereafter, the presence or absence of bursting of the green pellets is confirmed. If bursting or pulverization of the green pellets occurs during or at the end of the period in which the air heated to 200°C is passed through the layer of green pellets, the bursting temperature of the green pellets is determined to be 200°C. If no bursting of the green pellets is confirmed, the temperature of the hot air is further increased by 20°C and passed for 10 minutes, and the presence or absence of bursting of the green pellets is confirmed. Thereafter, the temperature is similarly increased by 20°C increments (i.e., the green pellets are gradually heated) to determine the temperature at which the green pellets burst. After repeated heating of the hot air, the temperature at which the green pellets burst is determined as the bursting temperature of the green pellets, as described above.

[0054] In this example, from the perspective of whether the green pellets have enough strength to prevent disintegration or powdering due to handling such as transportation until they are made into fired pellets (from the granulation process to the firing process), if the drop strength is 5 or more times, the strength is judged to be good, and if the drop strength is less than 5 times, the strength is judged to be poor.

[0055] Whether or not bursting was suppressed was determined based on whether the bursting temperature was 250° C. or higher or lower than 250° C. That is, if the bursting temperature was 250° C. or higher, the bursting tendency was low and good, and if the bursting temperature was lower than 250° C., the bursting tendency was high and poor.

[0056] In addition, when the bursting property is good but the strength is poor, it is judged as poor in comprehensive evaluation. This is because when the bursting property is good but the strength is poor, it cannot be properly fired and used thereafter. Similarly, when the strength is good but the bursting property is poor, it is judged as poor in comprehensive evaluation. This is because when the strength is good but the bursting property is poor, it cannot be properly used after firing.

[0057] When the green pellets of each production number were evaluated according to the above, green pellets Nos. 1 and 7 were poor in terms of strength. Green pellets Nos. 6 and 13 were poor in terms of bursting resistance. The other green pellets (Nos. 2-5 and 8-12) were good in strength and bursting resistance. Taking these evaluations into consideration, in Tables 2 and 3, Nos. 1, 6, 7, and 13 are listed as Comparative Examples 1 to 4, in that order. Furthermore, Nos. 2-5 and 8-12 are listed as Examples 1 to 9, in that order.

[0058] In general, the smaller the particle size distribution index (the sharper the particle size distribution) of the green pellets from Production No. 1 to No. 13, the higher the bursting temperature. In other words, the smaller the particle size distribution index of the green pellets from Production No. 1 to No. 13, the better the bursting properties.

[0059] Furthermore, for the green pellets of Production Nos. 1 to 13, the larger the particle size distribution index (the broader the particle size distribution), the higher the drop strength. In other words, for the green pellets of Production Nos. 1 to 13, the larger the particle size distribution index, the better the strength.

[0060] Considering the particle size distribution index of the green pellets of Production Nos. 2-5 and 8-12, which have good strength and bursting resistance, the particle size distribution index needs to be 14,700 or more and 510,000 or less in order to suppress bursting of the green pellets while maintaining good strength.

[0061] Regarding particle size distribution, it can be determined that both strength and bursting resistance can be achieved if the cumulative 50% diameter is 5.0 μm or more and 61.0 μm or less, or at least 5.2 μm or more and 60.1 μm or less. Also, it can be determined that both strength and bursting resistance can be achieved if the cumulative 10% diameter is at least 0.6 μm or more and 7.1 μm or less.

[0062] With regard to the harmonic mean diameter, it can be determined that both strength and bursting resistance can be achieved if the harmonic mean diameter is at least 1.7 μm or more and less than 13.0 μm.

[0063] In this way, a method for producing iron ore pellets can be provided.

[0064] It should be noted that the embodiments disclosed in this specification are merely examples, and the embodiments of the present disclosure are not limited to these, and can be modified as appropriate within the scope of the purpose of the present disclosure.

[0065] The present disclosure is applicable to methods for producing iron ore pellets.

Claims

1. A method for producing iron ore pellets, comprising a crushing step of crushing iron ore having an iron content of 63% by mass or less to obtain ore powder, wherein the volatile content of the iron ore is 3.3% by mass or more, and the ore powder has a cumulative 90% diameter in a volumetric particle size distribution of 150 μm or less, and a particle size distribution index defined by the following formulas (1) to (4) of 14,700 or more and 510,000 or less. where Dp is the harmonic mean diameter (μm), Isp is the particle size distribution index, wi is the particle ratio, and di (μm) is the representative particle diameter.

2. The method for producing iron ore pellets according to claim 1, wherein the volatile content of the iron ore is 12.0% by mass or less.

3. A method for producing iron ore pellets according to claim 1 or 2, wherein the ore powder has a cumulative 50% diameter in a volumetric particle size distribution of less than 61 μm.

4. A method for producing iron ore pellets according to any one of claims 1 to 3, wherein the ore powder has a cumulative 10% diameter in a volumetric particle size distribution of less than 7.1 µm.

5. A method for producing iron ore pellets according to any one of claims 1 to 4, wherein the ore powder has a harmonic mean diameter of less than 13 µm.