Method of producing iron ore pellets
Patent Information
- Application Number
- MYPI2025000578
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-16
- Filing Date
- 2023-07-11
- Publication Date
- 2024-03-16
AI Technical Summary
The existing methods for producing iron ore pellets face challenges in simultaneously ensuring the strength of green pellets and suppressing bursting, which affects the quality and durability of the final iron ore pellets.
The method involves mixing iron ore with a core ore having a particle size of more than 1 mm and fine ore with a particle size of 1 mm or less, with a specific mass ratio of core ore to total iron ore, to create green pellets that are strong and less prone to bursting during the firing process.
This approach results in high-strength green pellets that are resistant to bursting, maintaining strength and reducing porosity, thereby enhancing the quality and performance of the iron ore pellets post-firing.
Smart Images

Figure PI2025000578_DRAWING_001 
Figure PI2025000578_DRAWING_002 
Figure PI2025000578_DRAWING_003
Abstract
Description
Iron ore pellet manufacturing method
[0001] The present invention relates to a method for producing iron ore pellets.
[0002] Iron ore pellets are produced by granulating iron ore powder to have properties (e.g., size, strength, reducibility, etc.) suitable for charging into a blast furnace or a solid reduction furnace. As described in Patent Document 1, for example, iron ore pellets are generally produced by the steps of crushing iron ore raw material to obtain fine ore, mixing the fine ore with a binder and optional auxiliary materials to obtain a mixture, granulating the mixture to obtain green pellets, and firing the green pellets to obtain iron ore pellets. In this specification, pellets as granulated before firing are referred to as "green pellets."
[0003] In the production of iron ore pellets, ensuring the strength of green pellets is important to prevent the green pellets from pulverizing during handling before being placed in a sintering furnace, resulting in the powder adhering to the inside of the sintering furnace. Suppressing bursting of green pellets is also important to ensure the strength of iron ore pellets after sintering. Bursting is a phenomenon in which green pellets burst due to the pressure of steam generated from within the green pellets as they are dried and dehydrated. Bursting causes cracks in the green pellets, significantly reducing the strength of the iron ore pellets after sintering. In particular, if the particle size of the crushed fine ore is reduced to ensure the strength of the green pellets, the green pellets become highly densified, making them more susceptible to bursting. In other words, it has been difficult to simultaneously ensure the strength of green pellets and suppress bursting.
[0004] Japanese Patent Application Laid-Open No. 2022-34210
[0005] In order to ensure the strength of the green pellets or to suppress the bursting of the green pellets, bentonite or various organic or inorganic binders have been added as binders. However, there is room for improvement in terms of ensuring the strength of the green pellets and suppressing the bursting.
[0006] In view of the above problems, an object of the present invention is to provide a method for producing iron ore pellets that can produce green pellets that are high in strength and can suppress bursting.
[0007] In order to achieve this object, the inventors have conducted extensive research and have discovered that by using iron ore having a particle size of 1 mm or less obtained by crushing iron ore raw material, and iron ore having a particle size of more than 1 mm obtained without crushing the iron ore raw material, and mixing and granulating these to produce green pellets, it is possible to ensure the drop strength of the green pellets and suppress bursting.
[0008] The gist and configuration of the present invention, which has been completed based on the above findings, is as follows.
[0009] [1] A method for producing iron ore pellets, comprising the steps of: mixing iron ore having a total Fe content of 63% by mass or less with a binder to obtain a mixture; granulating the mixture to obtain green pellets; and firing the green pellets to obtain iron ore pellets, wherein the iron ore comprises core ore having a particle size of more than 1 mm and fine ore having a particle size of 1 mm or less.
[0010] [2] The method for producing iron ore pellets according to [1], wherein the mass ratio of the core ore to the iron ore is 15 mass% or more.
[0011] [3] The method for producing iron ore pellets according to [2], wherein the mass ratio of particles having a particle size of more than 2.8 mm among the core ores is 15 mass% or more relative to the iron ore.
[0012] [4] The method for producing iron ore pellets according to [2], wherein the mass ratio of particles having a particle size of more than 2.8 mm among the core ores is 30 mass% or more relative to the iron ore.
[0013] [5] The method for producing iron ore pellets according to [1], wherein the mass ratio of particles having a particle size of more than 4.8 mm among the core ores is 10 mass% or more relative to the iron ore.
[0014] [6] The method for producing iron ore pellets according to [5], wherein the mass ratio of particles having a particle size of more than 4.8 mm among the core ores is 25 mass% or more relative to the iron ore.
[0015] [7] The particle size and mass ratio of the core ore are set so that the number of core ores contained per iron ore pellet is an average of 0.9 to 1.0. [1] to [6] The method for producing iron ore pellets according to any one of the above.
[0016] [8] The iron ore raw material is sieved using a sieve with 1 mm openings, and the oversized ore is used as the core ore, and the undersized ore is crushed and used as the fine ore. [1] to [7] The method for producing iron ore pellets according to any one of the above.
[0017] [9] In the mixture, the mass of the fine ore is W1, the mass of the binder is W2, and W2 / W1×100 is 1.0 or more. [1] to [8] A method for producing iron ore pellets according to any one of the above.
[0018]
[10] The method for producing iron ore pellets according to any one of [1] to [9], wherein the binder is bentonite.
[0019] According to the method for producing iron ore pellets of the present invention, it is possible to obtain green pellets that are high in strength and can suppress bursting.
[0020] The present invention relates to an iron ore pellet manufacturing method, a method for manufacturing an iron ore pellet, and a comparative example.
[0021] Hereinafter, an embodiment of the method for producing iron ore pellets according to the present invention will be described. Note that the embodiment described below is an example of the present invention, and the configuration of the present invention is not limited to this specific example.
[0022] A method for producing iron ore pellets according to one embodiment of the present invention includes the steps of: mixing iron ore having a total Fe content of 63% by mass or less with a binder to obtain a mixture; granulating the mixture to obtain green pellets; and firing the green pellets to obtain iron ore pellets. The iron ore used to obtain the mixture is characterized by comprising core ore having a particle size of more than 1 mm and fine ore having a particle size of 1 mm or less.
[0023] In this specification, iron ore particles having a particle size of more than 1 mm that are obtained without crushing the iron ore raw material are referred to as "nuclear ore," and iron ore particles having a particle size of 1 mm or less that are obtained by crushing the iron ore raw material are referred to as "fine ore."
[0024] In this embodiment, core ore is used in addition to fine ore as the iron ore that constitutes the green pellets. The inclusion of high-strength core ore in the green pellets ensures the strength of the green pellets. Furthermore, compared to conventional techniques in which the iron ore that constitutes the green pellets is composed solely of fine ore, the green pellets in this embodiment contain large-grained core ore, which reduces the speed of drying and decrystallization water. The inclusion of core ore reduces the porosity of the green pellets, making them dense and less likely to retain moisture. Furthermore, the small gas path makes it difficult for steam to be generated from inside the green pellets. As a result, bursting can be sufficiently suppressed.
[0025] In the present invention, the "particle size" of iron ore corresponds to the nominal mesh size of a sieve mesh conforming to JIS Z 8801:2019. That is, iron ore having a particle size exceeding X mm is iron ore that remains on the sieve when sieved using a sieve with a nominal mesh size of X mm. Iron ore having a particle size of Y mm or less is iron ore that passes through a sieve with a nominal mesh size of Y mm and falls below the sieve size.
[0026] The type and characteristics of the core ore are not particularly limited as long as it is iron ore having a particle size of more than 1 mm and a total Fe content of 63 mass% or less. Furthermore, the particle size of the core ore is preferably 9.5 mm or less. A particle size of 9.5 mm or less ensures that the size of the finished iron ore pellets is suitable, allowing subsequent reduction treatments and other processes to be performed uniformly.
[0027] The mass ratio of the core ores to the total iron ore is preferably 15 mass% or more. This is because the more core ores there are, which have a larger volume than normal crushed iron ore powder, the more effective the binder such as bentonite can be even in a small amount, and the better the strength improvement and bursting suppression effects can be obtained.
[0028] Similarly, from the viewpoint of more fully obtaining the effects of the present invention, the mass ratio of particles having a particle size of more than 2.8 mm among the core ores is more preferably 15 mass% or more, and even more preferably 30 mass% or more, based on the total iron ore. In this case, the mass ratio of the core ores having a particle size of more than 1 mm and not more than 2.8 mm is not particularly limited and may be 0 mass%.
[0029] Similarly, from the viewpoint of more fully obtaining the effects of the present invention, the mass ratio of particles having a particle size of more than 4.8 mm in the core ore is preferably 10 mass% or more, more preferably 25 mass% or more, based on the total iron ore. In this case, the mass ratio of the core ore having a particle size of more than 1 mm and not more than 4.8 mm is not particularly limited and may be 0 mass%.
[0030] The mass ratio of the core ore is preferably 99% by mass or less, more preferably 75% by mass or less, based on the total iron ore. In general iron ore raw material, the mass ratio of particles having a particle size of more than 1 mm is at most about 75% by mass.
[0031] The fine ore is obtained by crushing iron ore using a general ball mill or the like. The average particle size of the fine ore is preferably about several tens of μm. The Blaine index of the fine ore is 2000 to 4000 cm 2 / g, and 2500 to 3500 cm 2 / g. It is more preferable that the Blaine index is 2000 cm 2 / g or more, the efficiency of powder production is more favorable. 2 / g or less, shrinkage due to sintering during firing is suppressed, and strength is more suitable. The Blaine index is measured using a Blaine air permeability tester specified in JIS R 5201:2015 and represents the specific surface area of the powder. In the pellet manufacturing process, the Blaine index is used as a control index for ore particle size, and a higher value indicates finer powder.
[0032] Although there is no particular restriction on the method for producing the core ore and the fine ore, it is preferable to sieve the iron ore raw material through a sieve with 1 mm openings, use the oversized ore as the core ore, and crush the undersized ore to use as the fine ore. Alternatively, each of them may be prepared separately from the iron ore raw material.
[0033] As shown in Figure 1, each iron ore pellet obtained in this embodiment preferably contains one core ore 10, with fine ore 12 attached to the surface of the core ore 10. The same is preferably true for the green pellets. When the green pellets and iron ore pellets each contain one core ore, favorable strength can be obtained.
[0034] The inventors believe that the reason why high strength is achieved when green pellets and iron ore pellets contain only one core ore is as follows. Figure 2 shows a schematic diagram (cross-sectional view) of the growth process during the granulation process of green pellets. When the number of core ores contained in one pellet is one, as in the present invention, layering granulation occurs, in which fine ore 12 and binder, etc., adhere in layers to the surface of the core ore 10. When green pellets do not contain core ore, nuclei 14 of powder agglomerates made of fine ore are formed instead of the core ore, and the fine ore coats these, leading to granulation. However, the binder is dispersed within the green pellet, resulting in a decrease in strength. Furthermore, when green pellets contain more than one core ore, a layer of fine ore must surround multiple core ores at once during the growth process. This rapid particle growth leaves insufficient time for the coating layer to densify, resulting in lower strength than when there is only one core ore.
[0035] Therefore, in this embodiment, it is preferable to set the particle size and mass ratio of the core ore so that the number of core ores contained per iron ore pellet is an average of 0.9 to 1.0. The weight ratio G of the core ore can be calculated from the sizes of the core ore and the green pellets as follows: The weight ratio G of the core ore in the green pellet is considered to be equal to the effective volume ratio of the core ore in the green pellet (the volume ratio excluding the pores in the fine ore agglomerates). The weight ratio G can be expressed as follows: G = T / {(1 - T) * (1 - K) + T} (1) where "(1 - T) * (1 - K)" is the volume ratio of the fine ore agglomerates in the green pellet excluding the pores. By adjusting the weight ratio of the core ores and the particle size of the core ores so as to satisfy formula (1), it is possible to make the green pellets contain an average of one core ore. The porosity K of the green pellets is generally determined by the crushed particle size of the fine ore, and can be, for example, 0.33.
[0036] Bentonite is preferred as the binder used during granulation, but any known or arbitrary binder, such as an organic or inorganic binder, that provides a similar effect may also be used. Furthermore, in the mixing step, limestone, dolomite, or the like may be mixed as an auxiliary material in addition to the iron ore and binder. Furthermore, various reducing agents and additives may be added as auxiliary materials depending on the type of furnace used in the reduction treatment after firing. Specifically, carbon materials such as coal and coke may be used as reducing agents.
[0037] The amount of binder in the mixture is preferably an amount that satisfies the following equation: W2 / W1×100≧1.0, where W1 is the mass of the fine ore and W2 is the mass of the binder. Within this range, the binder amount is suitable for the fine ore, the binder effect is favorably obtained, and strength can be ensured. The range is more preferably 1.4 or more, and even more preferably 1.6 or more. The greater the binder amount, the easier it is to ensure pellet strength, but the purity of the reduced iron decreases, so the binder amount is preferably in the range of 3.0 or less.
[0038] Iron ore pellets are produced by a general crushing, mixing, granulation, and firing process. The crushing process may be carried out using a general crusher such as a ball mill, and is only carried out on iron ore to be used as fine ore. The mixing process may be carried out using a general concrete mixer, etc. The granulation process may be carried out using a general pelletizer or drum mixer, etc. The firing process may be carried out using a general shaft furnace or rotary kiln, etc.
[0039] The granulated green pellets preferably have a size of about 9.5 to 12 mm. If the size of the green pellets is less than 9.5 mm, the gas permeability will be deteriorated when the pellets are filled into a blast furnace as fired pellets. If the size of the green pellets is more than 12 mm, the reducibility will be reduced.
[0040] After drying at 105°C for 24 hours, the iron ore was sieved using a rotary tap through sieves with openings of 1.0 mm, 2.8 mm, 4.8 mm, 6.7 mm, 8.0 mm, and 9.5 mm, and the iron ore remaining on these sieves was designated as core ore. Table 1 shows the composition of the iron ore used as raw material. Note that T.Fe is the total iron content in the iron ore, and LOI (Loss on Ignition) is the loss on ignition at the time of measurement. Iron ore with the same composition as above was similarly dried at 105°C for 24 hours and then pulverized in a ball mill to obtain iron ore powder, which was designated as fine ore. The fine ore passed entirely through a sieve with openings of 1.0 mm, i.e., had a particle size of 1 mm or less. The Blaine index of the fine ore was 2560 cm 2 / g.
[0041]
[0042] The core ore and fine ore were prepared in a total weight ratio of 5,000 g, and then mixed with a specified proportion of bentonite using a concrete mixer at 20 rpm for 3 minutes. The amount of bentonite added (mass%) relative to the total iron ore (total of core ore and fine ore) is shown in the "Bentonite Ratio" column in Table 2. The mixed raw materials were then placed in a 1.2 mφ pelletizer and granulated while adding water. Pellets measuring 9.5 to 12 mm were collected and rolled in the pelletizer for an additional 10 minutes to obtain green pellets. In the inventive example, the blending amounts of core ore and fine ore were adjusted so that the average number of core ores contained in each green pellet was 1.0. The volume ratio of core ore to green pellets and the number of core ores per green pellet are shown in Table 2. The porosity was set to 33%.
[0043]
[0044] [Drop Strength Measurement] In each of the invention examples and comparative examples, drop strength measurements were performed on 10 green pellets, simulating the transportation and charging that occur during actual operation. The green pellets were repeatedly dropped from a height of 50 cm, and the test was stopped when cracks or breakage were observed in the green pellets. The number of times before the test was stopped (i.e., when cracks or breakage were observed) was taken as the drop strength, and the average drop strength of the 10 pellets is shown in Table 2.
[0045] [Burst Temperature Measurement] The temperature at which the green pellets burst in the furnace (hereinafter referred to as the bursting temperature) was measured for each of the invention examples and comparative examples. FIG. 3 shows a schematic diagram of the electric furnace used in this example. A green pellet-filled basket 32 filled with 200 g of green pellets was placed in the electric furnace 30, and hot air (air) at 200°C (measured by a thermocouple 34) was flowed from a heating gas source 36 at a flow rate of 1.2 m / sec and maintained for 10 minutes. After the hold, the sample was removed and checked for bursting. If no bursting was observed, the hot air temperature was increased in 40°C increments, and a new sample was placed in the furnace and the same test was repeated. The temperature at which the sample burst was confirmed was taken as the bursting temperature, and the results are shown in Table 2.
[0046] Referring to Table 2, when comparing the invention examples and comparative examples with the same bentonite ratio, it can be seen that the invention examples containing core ores have higher drop strength and bursting temperature, demonstrating the effectiveness of the invention. It can also be seen that increasing the ratio of high-grain core ores or increasing the bentonite ratio improves strength and bursting temperature, demonstrating more favorable manufacturing conditions.
[0047] According to the present invention, it is possible to provide a method for producing iron ore pellets that can obtain green pellets that are high in strength and can suppress bursting.
[0048] 10 Core ore having a particle size of more than 1 mm 12 Fine ore having a particle size of 1 mm or less 14 Core of agglomerate made of fine ore having a particle size of 1 mm or less 30 Electric furnace 32 Green pellet filling basket 34 Thermocouple 36 Heating gas source
Claims
1. A method for producing iron ore pellets, comprising the steps of: mixing iron ore having a total Fe content of 63% by mass or less with a binder to obtain a mixture; granulating the mixture to obtain green pellets; and firing the green pellets to obtain iron ore pellets, wherein the iron ore comprises core ore having a particle size of more than 1 mm and fine ore having a particle size of 1 mm or less.
2. The method for producing iron ore pellets according to claim 1, wherein the mass ratio of the core ore to the iron ore is 15 mass% or more.
3. A method for producing iron ore pellets as described in claim 2, wherein the mass ratio of particles having a particle size of more than 2.8 mm among the core ore is 15 mass % or more relative to the iron ore.
4. A method for producing iron ore pellets as described in claim 2, wherein the mass ratio of particles having a particle size of more than 2.8 mm among the core ore is 30 mass% or more relative to the iron ore.
5. A method for producing iron ore pellets as described in claim 1, wherein the mass ratio of particles having a particle size of more than 4.8 mm among the core ore is 10 mass % or more relative to the iron ore.
6. A method for producing iron ore pellets according to claim 5, wherein the mass ratio of particles having a particle size of more than 4.8 mm among the core ore is 25 mass % or more relative to the iron ore.
7. A method for producing iron ore pellets according to any one of claims 1 to 6, wherein the particle size and mass ratio of the core ores are set so that the number of core ores contained in each iron ore pellet is an average of 0.9 to 1.
0.
8. A method for producing iron ore pellets according to any one of claims 1 to 7, wherein the iron ore raw material is sieved through a sieve with 1 mm openings, the oversized ore is used as the core ore, and the undersized ore is crushed and used as the fine ore.
9. A method for producing iron ore pellets according to any one of claims 1 to 8, wherein in the mixture, the mass of the fine ore is W1, the mass of the binder is W2, and W2 / W1 x 100 is 1.0 or more.
10. A method for producing iron ore pellets according to any one of claims 1 to 9, wherein the binder is bentonite.