Patent Information
- Application Number
- MYPI2025000584
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-05
- Filing Date
- 2023-04-25
- Publication Date
- 2024-02-24
AI Technical Summary
Conventional methods struggle to uniformly and stably supply fibrous fillers with low bulk density and a tendency to aggregate, leading to uneven fiber length distribution and bridging issues in thermoplastic resin compositions, which affects the quality of molded products.
A fibrous filler agitation supply device with a connecting tank and a rotating shaft equipped with an inclined stirring blade, which reduces bulk density and promotes uniform feeding by adjusting the angle and position of the stirring blade to prevent bridging and ensure stable conveyance.
The solution enables uniform and stable conveyance of fibrous fillers with low bulk density, resulting in a thermoplastic resin composition with uniform fiber dispersion and improved product stability during manufacturing.
Smart Images

Figure PI2025000584_DRAWING_001 
Figure PI2025000584_DRAWING_002 
Figure PI2025000584_DRAWING_003
Abstract
Description
Agitation supply device, supply method, and manufacturing method for fibrous filler, and manufacturing method for thermoplastic resin composition
[0001] The present invention relates to an agitation supply device, supply method, and production method for a fibrous filler, and a method for producing a thermoplastic resin composition.
[0002] A widely used method for producing resin compositions is to feed raw resins together with various additives into an extruder, melt-knead them, and form pellets of the resin composition. Fiber-reinforced thermoplastic resin compositions containing fibrous fillers such as carbon fiber and glass fiber as additives produce molded articles with high strength and are widely used in various fields.
[0003] To produce a fiber-reinforced thermoplastic resin composition, resin pellets of the raw thermoplastic resin are fed into an extruder. The resin pellets are melted in the extruder's cylinder and sent forward (downstream) by the screw. The fibrous filler is fed into the extruder's cylinder at a predetermined position by a side feeder. In the extruder, the molten thermoplastic resin and the fibrous filler are kneaded by the rotation of the screw, and the fibrous filler is dispersed and appropriately cut. The extruded pellets are then cooled and cut to produce pellets of the fiber-reinforced thermoplastic resin composition.
[0004] When various additives are supplied from the side feeder, a stirring and supplying device is provided, which is composed of a hopper (measuring tank) for storing the raw material additives, a connecting tank below it, an agitator for stirring the raw materials in the connecting tank, and a screw cylinder at the bottom of the connecting tank with a screw for sending the additives to its discharge section.
[0005] Fibrous fillers are usually provided as chopped fibers. If such fibrous fillers are directly fed from a side feeder to an extruder cylinder, the stress applied to the fibrous fillers during mixing with the thermoplastic resin becomes non-uniform, making the fibrous fillers prone to breaking or cutting, resulting in a thermoplastic resin composition with a non-uniform fiber length distribution.
[0006] However, the agitator in conventional agitation supply devices agitates the raw material in the connecting tank, and its purpose is to prevent bridging, in which the fibrous filler partially or entirely stops falling out of the connecting tank, or the phenomenon of only the center falling out. However, fibrous fillers with low bulk density and easy-to-spread fibers cannot be stably supplied to the cylinder with the screw. Easy-to-spread fibrous fillers easily spread when charged into the hopper (measuring tank), moved downward, and rotated by the agitator, forming a flocculent aggregate that does not fall into the cylinder and forms a bridge at the cylinder opening. As a result, the cylinder cannot be sufficiently filled with the fibrous filler, making uniform transport by the screw difficult.
[0007] In view of the problems of the prior art, the present invention aims to provide an agitating and feeding device for a fibrous filler and a feeding method for a fibrous filler that can uniformly and stably convey with a screw even fibrous fillers that tend to easily open, have low bulk density, and tend to aggregate into a flocculent state. It is also an object of the present invention to provide a method for producing a fibrous filler that has accelerated opening and reduced bulk density using the above agitating and feeding device or feeding method, and a method for stably producing a thermoplastic resin composition containing the fibrous filler obtained by the above production method.
[0008] In order to solve the above problems, the fibrous filler agitation and supply device of the present invention is a device that feeds fibrous filler from a hopper that stores the fibrous filler to a discharge section, and is provided with a connection tank between the hopper and the discharge section. Inside the connection tank, there is a shaft that rotates around a rotation axis, and at the tip of the shaft, an agitation blade for agitating the fibrous filler is provided so as to rotate along the inner surface of the connection tank, and the agitation blade is inclined inward at an angle Θ of 10° to 70° with respect to the rotation direction of the agitation blade.
[0009] The agitation supply device for fibrous filler preferably comprises a connection tank having a substantially hemispherical inner peripheral surface between a hopper and a discharge section, a shaft inside the connection tank that rotates vertically about an axis of rotation that protrudes horizontally from the inner peripheral surface of the connection tank, and an agitation blade for agitating the fibrous filler is provided at the tip of the shaft so that it rotates vertically along the inner peripheral surface of the connection tank, the agitation blade being inclined inward at an angle Θ of 10° to 70° with respect to the rotation direction of the agitation blade. In the agitation supply device, the shortest distance between the agitation blade and the inner peripheral surface of the connection tank is preferably in the range of 0.2 to 5 cm.
[0010] The fibrous filler agitation and supply device preferably includes a connecting tank between a hopper and a discharge section, a circular inclined surface provided at the bottom of the connecting tank facing diagonally upward from the bottom of the connecting tank, a shaft that rotates about an axis of rotation that protrudes inward from the center of the circular inclined surface, and a stirring blade for agitating the fibrous filler provided at the tip of the shaft so as to rotate on the circular inclined surface, the stirring blade being inclined inward at an angle Θ of 10° to 70° with respect to the rotation direction of the stirring blade. The shortest distance between the tip of the stirring blade and the inner wall surface of the connecting tank is preferably in the range of 0.2 to 5 cm.
[0011] The number of stirring blades is preferably 2 to 6. A screw for feeding the fibrous filler to the discharge portion is preferably provided at the bottom of the connecting tank. The area obtained by multiplying the area of the stirring blade by the inclination angle cos Θ is preferably in the range of 0.1 to 1.0 times the area of the opening to the screw at the bottom of the connecting tank when viewed from directly above.
[0012] The method for supplying fibrous filler of the present invention is a method for supplying fibrous filler contained in a hopper to a discharge section, and is characterized in that a connecting tank is provided between the hopper and the discharge section, and inside the connecting tank there is a shaft that rotates around a rotation axis, and at the tip of the shaft there is a stirring blade for stirring the fibrous filler so that it rotates along the inner surface of the connecting tank, and the stirring blade is provided with an agitator that is inclined inward at an angle Θ of 10° to 70° with respect to the rotation direction of the stirring blade, and the fibrous filler is opened by the agitator and supplied to the discharge section by a screw provided at the bottom of the connecting tank.
[0013] In the above-mentioned feeding method, it is preferable that the rotation speed of the agitator is 1 to 20% of the rotation speed of the screw. 0 is 0.3 to 0.7 g / cm 3 and the bulk density V of the discharged fibrous filler 1 is V 0 Smaller than 0.1 to 0.5 g / cm 3 It is preferable that the temperature is in the range of
[0014] The method for producing a fibrous filler of the present invention is a method for producing a fibrous filler with a reduced bulk density by opening a fibrous filler contained in a hopper, and is characterized in that a connection tank is provided between the hopper and a discharge section, and the connection tank contains a shaft that rotates about its axis of rotation, and a stirring blade for stirring the fibrous filler is provided at the tip of the shaft so that it rotates along the inner circumferential surface of the connection tank, and the stirring blade is provided with an agitator that is inclined inward at an angle Θ of 10° to 70° with respect to the rotation direction of the stirring blade, and the fibrous filler is opened by the agitator and supplied to the discharge section by a screw provided at the bottom of the connection tank. Here, the bulk density V of the fibrous filler contained in the hopper 0 is 0.3 to 0.7 g / cm 3 and the bulk density V of the discharged fibrous filler 1 is V 0 Smaller than 0.1 to 0.5 g / cm 3 It is preferable that the temperature is in the range of
[0015] The method for producing a thermoplastic resin composition is a method for producing a thermoplastic resin composition in which a fibrous filler is blended with a thermoplastic resin using an extruder, and is characterized in that the fibrous filler with reduced bulk density obtained by the method for producing a fibrous filler is side-fed from a side feeder located downstream of the main inlet for raw materials containing the thermoplastic resin, and melt-kneaded.
[0016] The fibrous filler agitation supply device of the present invention enables uniform and stable conveyance by a screw, even for fibrous fillers that tend to open easily, have low bulk density, and tend to aggregate like flocs. Furthermore, the fibrous filler supply method of the present invention enables stable supply to the discharge section, even for fibrous fillers that tend to open easily and have low bulk density. Furthermore, the fibrous filler production method of the present invention enables stable production of fibrous fillers that have opened easily and have low bulk density. Furthermore, the thermoplastic resin composition production method of the present invention enables stable production of thermoplastic resin compositions in which the fibrous filler is uniformly dispersed.
[0017] Fig. 4 is an exploded perspective view showing one embodiment of the agitation supply device of the present invention; Fig. 5 is a partial cross-sectional view of one embodiment of the agitation supply device of the present invention; Fig. 6 is a plan view and a side view showing one embodiment of an agitation blade used in the agitation supply device of the present invention; Fig. 7 is an exploded perspective view showing an embodiment in which the lower part of the connection tank has a circular inclined surface; Fig. 8 is a partial cross-sectional view of the embodiment in Fig. 4 having the circular inclined surface; Fig. 9 is a plan view and a side view showing one embodiment of an agitation blade used when the circular inclined surface is shown in Fig. 4.
[0018] The agitation supply device, supply method, production method for a fibrous filler, and production method for a thermoplastic resin composition of the present invention will be described below with reference to the drawings. The embodiments shown here are merely examples and are not necessarily limited to these.
[0019] FIG. 1 is an exploded perspective view showing one embodiment of the agitation feeder of the present invention. FIG. 2 is a partial cross-sectional view of one embodiment of the agitation feeder of the present invention. In FIGS. 1 and 2, a connecting tank having a substantially hemispherical inner periphery is provided between a hopper and a discharge section. Inside the connecting tank, a shaft that rotates vertically around a rotation axis that protrudes horizontally from the inner periphery of the connecting tank. A stirring blade for stirring the fibrous filler is provided at the tip of the shaft so that it rotates vertically along the inner periphery of the connecting tank. As shown in FIGS. 1 and 2, the agitation feeder of the present invention includes a hopper 1 that accommodates the introduced fibrous filler, a connecting tank 2 that has a substantially hemispherical inner periphery below the hopper 1, and a screw 5 that supplies the fibrous filler to a discharge section 3 through an opening 6 at the bottom of the connecting tank 2. The hopper 1 may be conical as shown in FIG. 1 or cylindrical. The connecting tank 2 may be substantially hemispherical, and a portion of the connecting tank may have a curved surface, such as an oval sphere, as long as it does not come into contact with the rotating stirring blade 10.
[0020] An agitator 4 is provided inside the connecting tank 2, and the agitator 4 has a shaft 9 that rotates vertically around a rotation axis 8 that protrudes horizontally from the inner circumferential surface of the connecting tank 2 into the interior, and an agitator blade 10 for agitating the fibrous filler is provided at the tip of the shaft 9 so as to rotate (swivel) vertically along the inner circumferential surface of the connecting tank 2. The fibrous filler contained in the hopper 1 falls into the connecting tank 2 by gravity, and is agitated and spread by the agitator blade 10 provided at the tip of the shaft 9 of the agitator 4 that rotates (swivels) vertically.
[0021] FIG. 3 shows one embodiment of the agitator blades in the agitator 4, with FIG. 3(a) being a plan view and FIG. 3(b) being a right side view. Note that in FIG. 3(b), the shafts 9 extending left and right in FIG. 3(a) and the agitating blades 10 at their tips are omitted. The shafts 9 may be formed in a cross shape with two shafts joined around the rotation axis 8, as shown in FIG. 3(a), and have a total of four agitating blades 10. Alternatively, three shafts may be joined crosswise around the rotation axis 8, with a total of six agitating blades 10 at their tips, arranged symmetrically around the rotation axis 8. Alternatively, three shafts 9 may extend radially from the center of the rotation axis 8 at 120° intervals, each with one agitating blade at its tip, for a total of three agitating blades 10. Alternatively, one shaft 9 may have one agitating blade at each end. The number of agitating blades 10 is preferably 2 to 6.
[0022] The stirring blades 10 may extend from the same side of the shaft 9 as shown in Fig. 3, or may extend alternately from the front and back sides as shown in Fig. 2. When there are a plurality of shafts 9 as described above, it is preferable that the stirring blades 10 are provided alternately in the order of front side → back side → front side with respect to the rotation plane of the shaft 9, for example as shown in Fig. 3(a).
[0023] As shown in FIG. 3( a), the agitator blade 10 is inclined at an angle Θ inward toward the rotation axis 8 with respect to the rotation direction D (the tangent direction of the rotating circumference) of the agitator blade 10, with the angle Θ being 10° to 70°. By setting such an angle, uneven supply from the bottom of the connecting tank 2 to the discharge section 3 is suppressed, enabling uniform feeding. If the angle Θ is less than 10°, the force sending the fibrous filler to the cylinder 7 is weak, and a sufficient amount of fibrous filler cannot be loaded into the screw 5 that supplies the fibrous filler from the bottom of the connecting tank 2 to the supply section 3, making uniform feeding by the screw difficult. If the angle Θ is greater than 70°, the force applied to the agitator's rotating shaft becomes too strong, making the rotating shaft more susceptible to damage. The angle Θ is more preferably in the range of 20° to 60°. The angle Θ is preferably 20° or more, preferably 60° or less, and more preferably 50° or less.
[0024] The agitating blade 10 is configured to fit along the approximately hemispherical inner peripheral surface of the connecting tank 2, and the shortest distance between the agitating blade 10 and the inner peripheral surface of the connecting tank is preferably in the range of 0.2 to 5 cm, more preferably 0.3 to 3 cm. If it is more than 5 cm, the force pushing the fibrous filler into the cylinder 7 will be weak, making it difficult to fill the cylinder 7 with a sufficient amount of fibrous filler and making it difficult to feed uniformly by the screw 5. If it is less than 0.2 cm, the agitating blade 10 will come into contact with the inner surface of the hopper, potentially damaging the agitator 4. The connecting tank 2 is approximately hemispherical, and the diameter of the inner surface of its upper part is usually 15 to 50 cm, and preferably 20 to 40 cm.
[0025] In the present invention, examples of the fibrous filler include inorganic fibers such as carbon fiber, glass fiber, alumina fiber, boron fiber, and ceramic fiber, and organic fibers such as plant fibers (including kenaf and bamboo fiber), polyester fiber, aramid fiber, polyoxymethylene fiber, aromatic polyamide fiber, polyparaphenylene benzobisoxazole fiber, and ultra-high molecular weight polyethylene fiber. Of these, carbon fiber and glass fiber are preferred, and carbon fiber is particularly preferred.
[0026] The fibrous filler used preferably has a number average fiber length of 20 mm or less, more preferably 10 mm or less, and more preferably 1 mm or more. Specifically, chopped fiber and milled fiber are preferred. The bulk density V of the raw fibrous filler contained in the hopper is 0 is 0.3 to 0.7 g / cm 3 is preferably 0.35 to 0.65 g / cm 3 , and further 0.4 to 0.6 g / cm 3 It is preferable that the bulk density is in the range of V 0 is 0.3 / cm 3 If it is smaller than this, the stirring blades will not be able to push enough of the stirring bulk-increasing raw material into the cylinder, which will easily cause non-uniform feeding. 3If the agitator temperature exceeds this value, a strong force is applied to the rotating shaft of the agitator, which can easily damage the rotating shaft. In particular, in the present invention, it is preferable to use a fibrous filler that is easy to open and whose bulk increases easily upon agitation (the bulk density decreases), as the raw material, since this invention is more effective. Examples of fibrous fillers that increase bulk easily upon agitation include fibrous fillers that do not use a sizing agent or that are treated with only a small amount of a sizing agent.
[0027] In the present invention, bulk density represents the weight of a fibrous filler per certain volume, and is the same as loose bulk specific gravity, loose bulk density, or loose apparent density, and refers to the bulk density when lightly and quietly packed into a receiver. 0 , V 1 The bulk density (B) is measured in accordance with ISO 60. Specifically, a metal cylinder with a volume of 100 cc, an inner diameter of 50 mm, and a smoothly finished inner surface is used as the receiver, and the fibrous filler is slowly and gently filled into the receiver. When the receiver is full, the material that has risen from the receiver is scraped off with a straight plate, and the weight of the contents of the receiver is measured to the nearest 0.1 g to determine the bulk density.
[0028] The fibrous filler that has been opened and agitated by the agitator 4 comes out from an opening 6 provided at the bottom of the connection tank 2 and is supplied to the discharge section 3 by a screw 5 for feeding the fibrous filler to the discharge section 3. The screw 5 may be a single-axis screw or may be configured with two screws. The screw 5 is disposed in a cylinder 7, and the fibrous filler from the opening 6 is filled into the cylinder 7, and the screw 5 is driven to rotate and is supplied to the discharge section 3.
[0029] The opening 6 has a rectangular shape corresponding to the screw 5 located directly below, and it is preferable that its longitudinal centerline coincides with the rotation axis 8 of the agitator 4 located above. Agitator blades 10 with an inclination angle of 10 to 70 degrees rotate downward on the inner peripheral surface of the connecting tank 2, and the fibrous filler is sufficiently pushed from the opening 6 into the cylinder 7 containing the screw 5, making it possible to uniformly feed the fibrous filler with a reduced bulk density.
[0030] The area obtained by multiplying the area of one stirring blade 10 by the inclination angle cos Θ is preferably in the range of 0.1 to 1.0 times the area of the opening 6 as viewed from directly above, and more preferably in the range of 0.2 to 0.8 times. If it is less than 0.1 times, the force pushing the fibrous filler into the cylinder 7 will be weak, and a sufficient amount of fibrous filler will not be filled into the cylinder 7, making it difficult to uniformly feed the fibrous filler by the screw 5. If it is more than 1.0 times, the force applied to the agitator 4 will be strong, and the rotating shaft 8 will be easily damaged. The size of the opening 6 is preferably about 10 to 25 cm in long sides and about 5 to 15 cm in short sides, and the opening area is 50 to 350 cm. 2 The area of one stirring blade 10 multiplied by the inclination angle cos Θ is 10 to 350 cm 2 The degree is preferable.
[0031] The rotation speed of the agitator 4 is preferably 1 to 20% of the rotation speed of the screw 5, more preferably 2 to 15%, and even more preferably 3 to 10%. If it is less than 1%, the amount of fibrous filler pushed into the agitator 4 will be small, making uniform feeding difficult, and if it exceeds 20%, the fibrous filler will be opened too much, causing pilling and making it difficult to push into the cylinder 7, making it difficult to fill a sufficient amount of fibrous filler into the cylinder 7, and making uniform feeding by the screw 5 difficult. The rotation speed of the screw 5 is preferably about 10 to 600 rpm, and the rotation speed of the agitator 4 is preferably about 2 to 90 rpm.
[0032] The distance traveled in the axial direction when the screw makes one revolution is called "lead", and in a single-start screw, the lead and pitch are equal. In a double-start screw, the lead is twice the pitch. If the screw diameter (outer diameter) is D, the lead of the screw 5 is preferably 0.5D to 1.5D. If it is greater than 1.5D, the force conveying the fibrous filler will be weak and uniform feeding will be difficult, and even if it is less than 0.5D, the conveying force will be weak and uniform feeding will be difficult. The lead of the screw 5 is more preferably 0.6D to 1.4D, and even more preferably 0.7D to 1.3D.
[0033] The bulk density V of the fibrous filler supplied to the discharge section 31 is the bulk density V of the fibrous filler contained in the hopper 0 (preferably 0.3 to 0.7 g / cm 3 ) and is 0.1 to 0.5 g / cm 3 It is preferable that the density is in the range of 0.15 to 0.45 g / cm 3 , and further 0.2 to 0.4 g / cm 3 According to the present invention, even if the raw material is a fibrous filler that has not been treated with a sizing agent or that has been treated with only a small amount of a sizing agent, by opening and stirring the raw material with the agitator having the above configuration, sending it to the screw 5, and feeding it to the discharge section 3, the opening proceeds and a fibrous filler with a low bulk density can be obtained.
[0034] The resulting fibrous filler can be side-fed into an extruder to obtain a fibrous filler that can stably produce a thermoplastic resin composition in which the fibrous filler is uniformly dispersed.
[0035] The raw thermoplastic resin used is not particularly limited in type, and may be any thermoplastic resin.The thermoplastic resin suitable for use in the present invention can include crystalline thermoplastic resins and amorphous thermoplastic resins, and specifically includes polycarbonate resins; polyester-based resins such as polybutylene terephthalate resins and polyethylene terephthalate resins; styrene-based resins such as polystyrene resins, high-impact polystyrene resins (HIPS), ABS resins, AES resins and AS resins; polyolefin-based resins such as polyethylene resins and polypropylene resins; polyamide-based resins such as polyamide 6, polyamide 66 and polyamide MXD6; polyoxymethylene resins; polyphenylene sulfide resins; methacrylic resins such as PMMA resins; polyphenylene ether resins; polysulfone resins; polyethersulfone resins; polyarylate resins; polyetherimide resins; polyamideimide resins; polyimide-based resins; polyetherketone resins; polyetheretherketone resins; polyestercarbonate resins; liquid crystal polymers, etc.
[0036] The extruder is preferably a single-screw or twin-screw extruder, particularly a twin-screw extruder, and may be either vented or non-vented, but a vented extruder is preferred.
[0037] Raw materials containing thermoplastic resin and optional resin additives are fed into the cylinder of the extruder (not shown) in pellet or powder form through the main inlet of the base hopper and then transported to the first kneading section. The raw materials are heated in the first kneading section, with the heating temperature set based on the melting point and glass transition temperature of the thermoplastic resin, which is the main component. The raw materials melt-kneaded in the first kneading section are then pushed by the resin that is fed later. The fibrous filler obtained by the agitation feeder is then fed into the cylinder of the extruder through a side feeder located downstream of the main inlet and melt-kneaded in the second kneading section.
[0038] The screw configuration of the kneading section is preferably configured by a combination of two or more elements selected from a forward kneading disc, a reverse kneading disc, and an orthogonal kneading disc.
[0039] The forward kneading disc element is also called R kneading (hereinafter also referred to as R), and typically has two or more blades, with the blade twist angle preferably being 10° to 75°. By displacing the blades at a predetermined angle in this manner, a pseudo-screw structure is formed, which applies a strong shear force while feeding the resin in the feed direction, forming a kneading zone. The reverse kneading disc element is also called L kneading (hereinafter also referred to as L), and typically has two or more blades, with the blade twist angle preferably being -10° to -75°. The reverse kneading disc element is an element with the ability to block the incoming resin or act in the direction of returning the incoming resin, and by being installed downstream of an element that promotes kneading, it blocks the resin and exerts a powerful kneading effect. The orthogonal kneading disc element is also called N kneading (hereinafter sometimes referred to as N), and usually has two or more blades with a twist angle of 75 to 105 degrees. Because the blades are installed offset by approximately 90 degrees, the resin delivery force is weak but the kneading force is strong.
[0040] The screw configuration of the first kneading section is preferably composed of a combination of two or more types of elements, and it is preferable that an element that promotes kneading is arranged upstream and an element that has the ability to increase pressure is arranged downstream. Therefore, in the kneading zone of the first step, it is preferable to arrange two or more types selected from R, N, and L in the order R → N → L from the upstream side, and it is also preferable to arrange multiple elements of each R, N, and L. The screws of the second kneading section are preferably composed of elements selected from a forward kneading disk (R), a reverse kneading disk (L), an orthogonal kneading disk (N), a forward notched mixing screw, and a reverse notched mixing screw.
[0041] The resin composition melt-kneaded in the second kneading section and having the fibrous filler sufficiently dispersed therein is extruded in the form of strands from a nozzle at the tip of the extruder, cooled, and then cut with a cutter to produce pellets of the thermoplastic resin composition. This allows for the stable production of a thermoplastic resin composition having a uniformly dispersed fibrous filler.
[0042] Figures 4 to 6 are diagrams illustrating another embodiment of the present invention, in which a circular inclined surface is provided at the bottom of the connecting tank facing diagonally upward from the bottom of the connecting tank, a shaft rotates around an axis of rotation protruding inward from the center of the circular inclined surface, and a stirring blade for stirring the fibrous filler is provided at the tip of the shaft so as to rotate on the circular inclined surface.
[0043] As shown in Figures 4-5, the agitation supply device includes a hopper 1 that stores the introduced fibrous filler, a connecting tank 2 below the hopper 1, and a screw 5 that supplies the fibrous filler to a discharge section 3 through an opening 6 at the bottom of the connecting tank 2. The hopper 1 is preferably conical or cylindrical as shown in Figure 4, but may also be prismatic. The connecting tank 2 is connected to the hopper 1 at its upper part, and the sidewall of the connecting tank 2 may be circular in plan view and formed into a conical shape, or may be elliptical in plan view and formed with the same or different cross-sectional shapes in the upper and lower directions. It is also preferable that the sidewall of the connecting tank 2 have a cross-sectional shape that is larger at the bottom than at the top.
[0044] Inside the connecting tank 2, a circular inclined surface 11 is provided at the lower part of the connecting tank, preferably from the bottom, facing diagonally upward, and is equipped with a shaft 9 that rotates around a rotation axis 8 that protrudes diagonally inward from the center of the circular inclined surface 11, and an agitator 4 at the tip of the shaft 9, with a stirring blade 10 for stirring the fibrous filler rotating on the circular inclined surface 11. The fibrous filler contained in the hopper 1 falls into the connecting tank 2 by gravity, and is stirred and spread by the stirring blade 10 attached to the tip of the shaft 9 of the agitator 4 rotating (turning) along the inclined surface 11.
[0045] FIG. 6 shows one embodiment of the agitator blades in the agitator 4, with FIG. 6( a) being a plan view, FIG. 6( b) being a right side view, and FIG. 6( c) being a front view. Note that in FIG. 6( b), the shafts 9 extending left and right in FIG. 6( a) and the agitating blades 10 at their tips are omitted. Also, in FIG. 6( c), the shafts 9 extending left and right and rearward in FIG. 6( a) and the agitating blades 10 at their tips are omitted. As shown in FIG. 6( a), two shafts 9 may be joined around the rotation axis 8 to form a cross shape, with a total of four agitating blades 10. Alternatively, three shafts may be joined crosswise around the rotation axis 8, with a total of six agitating blades 10 at their tips, point-symmetrically arranged around the rotation axis 8. Alternatively, three shafts 9 may extend radially from the center of the rotation axis 8 at 120° intervals, with one agitating blade 10 at the tip of each shaft, for a total of three agitating blades 10. It is also possible to have one stirring blade on each end of one shaft 9. The number of stirring blades 10 is preferably 2 to 6.
[0046] As shown in FIG. 6( b), the agitator blade 10 preferably extends from the shaft 9 upward along the inclined surface 11, following the side wall of the connecting tank 2. As shown in FIG. 6( c), the agitator blade 10 is inclined at an angle Θ inward toward the rotation axis 8 relative to the rotation direction D (the tangent direction of the rotating circumference) of the agitator blade 10, with the angle Θ being 10° to 70°. By setting the angle in this manner, uneven supply from the bottom of the connecting tank 2 to the discharge section 3 is suppressed, enabling uniform feeding. If the angle Θ is less than 10°, the force conveying the fibrous filler to the cylinder 7 is weakened, and a sufficient amount of fibrous filler cannot be loaded into the screw 5 for supplying the fibrous filler from the bottom of the connecting tank 2 to the discharge section 3, making uniform feeding by the screw difficult. If the angle Θ is greater than 70°, the force applied to the agitator's rotating shaft becomes too strong, making the rotating shaft more susceptible to damage. A more preferable angle is between 20° and 60°. The angle Θ is preferably 20° or more, and is preferably 60° or less, and more preferably 50° or less.
[0047] 5, the agitating blade 10 rotates on an inclined surface 11 along the side wall of the connecting tank 2, and the shortest distance between the agitating blade 10 and the inner wall surface of the connecting tank is preferably in the range of 0.2 to 5 cm, more preferably 0.3 to 3 cm. If it is more than 5 cm, the force pushing the fibrous filler into the cylinder 7 will be weak, making it difficult to fill the cylinder 7 with a sufficient amount of fibrous filler and making it difficult to feed uniformly by the screw 5. If it is less than 0.2 cm, the agitating blade 10 will come into contact with the inner surface of the hopper, which may damage the agitator 4.
[0048] The connecting tank 2 is preferably circular and conical in plan view, or elliptical in plan view, and the diameter of its inner wall surface is usually 15 to 60 cm, preferably 20 to 50 cm. The diameter of the inclined surface 11 is preferably 15 to 60 cm, more preferably 20 to 50 cm. The length from the rotation axis 8 of the shaft 9 to the connection part of the stirring blade 10 is preferably 8 to 30 cm, more preferably 10 to 25 cm.
[0049] The fibrous filler that has been opened and agitated by the agitator 4 comes out from an opening 6 provided in the bottom of the connecting tank 2 and is supplied to the discharge section 3 by a screw 5 for feeding it to the discharge section 3. The opening 6 is provided between the bottom of the connecting tank 2 and the inclined surface 11, at a position where an agitating blade 10 pushes the fibrous filler from directly above. The screw 5 may be a single-shaft screw or may be configured with two screws. The screw 5 is arranged in a cylinder 7, and the fibrous filler from the opening 6 is filled into the cylinder 7, and the screw 5 is driven to rotate and supplied to the discharge section 3.
[0050] The opening 6 has a rectangular shape corresponding to the screw 5 located directly below, and the stirring blades 10, which have an inclination angle of 10° to 70°, sufficiently push the fibrous filler from the opening 6 into the cylinder 7, making it possible to uniformly feed the fibrous filler whose bulk density has been reduced.
[0051] The area obtained by multiplying the area of one stirring blade 10 by the inclination angle cos Θ is preferably in the range of 0.1 to 1.0 times the area of the opening 6 as viewed from directly above, and more preferably in the range of 0.2 to 0.8 times. If it is less than 0.1 times, the force pushing the fibrous filler into the cylinder 7 will be weak, and a sufficient amount of fibrous filler will not be filled into the cylinder 7, making it difficult to feed uniformly by the screw 5. If it is more than 1.0 times, the force applied to the agitator 4 will be strong, and the rotating shaft 8 will be easily damaged. The size of the opening 6 is preferably about 8 to 25 cm for the long side and about 4 to 15 cm for the short side, and the opening area is 35 to 350 cm. 2 The area of one stirring blade 10 multiplied by the inclination angle cos Θ is 5 to 350 cm 2 The degree is preferable.
[0052] The rotation speed of the agitator 4 is preferably 1 to 20% of the rotation speed of the screw 5, more preferably 2 to 15%, and even more preferably 3 to 10%. If it is less than 1%, the amount of fibrous filler pushed into the agitator 4 will be small, making uniform feeding difficult, and if it exceeds 20%, the fibrous filler will be opened too much, causing pilling and making it difficult to push into the cylinder 7, making it difficult to fill a sufficient amount of fibrous filler into the cylinder 7, and making uniform feeding by the screw 5 difficult. The rotation speed of the screw 5 is preferably about 10 to 600 rpm, and the rotation speed of the agitator 4 is preferably about 2 to 90 rpm.
[0053] The distance traveled in the axial direction when the screw makes one revolution is called "lead", and in a single-start screw, the lead and pitch are equal. In a double-start screw, the lead is twice the pitch. If the screw diameter (outer diameter) is D, the lead of the screw 5 is preferably 0.5D to 1.5D. If it is greater than 1.5D, the force conveying the fibrous filler will be weak and uniform feeding will be difficult, and even if it is less than 0.5D, the conveying force will be weak and uniform feeding will be difficult. The lead of the screw 5 is more preferably 0.6D to 1.4D, and even more preferably 0.7D to 1.3D.
[0054] The bulk density V of the fibrous filler supplied to the discharge section 31 is the bulk density V of the fibrous filler contained in the hopper 0 (preferably 0.3 to 0.7 g / cm 3 ) and is 0.1 to 0.5 g / cm 3 It is preferable that the density is in the range of 0.15 to 0.45 g / cm 3 , and further 0.2 to 0.4 g / cm 3 The range is preferred.
[0055] Even when a circular inclined surface is provided at the bottom of the connecting tank facing diagonally upward from the bottom of the connecting tank, according to the present invention, even if the raw material is a fibrous filler that has not been treated with a sizing agent or has only been treated with a small amount of sizing agent, it can be opened and stirred by an agitator of the above configuration, sent to the screw 5, and fed to the discharge section 3, thereby making it possible to obtain a fibrous filler that has been opened well and has a low bulk density.
[0056] First, the following experiment was conducted to determine the extent to which the bulk density of the raw fibrous filler increases (decreases) due to stirring. A Kubota "gravimetric screw feeder CE-W-1 (two shafts)" stirring and feeding device (connecting tank hemispherical with an inner diameter of 25 cm) was used, and the agitator was a Kubota "CE-W-1 Agitator 2" (a 12.2 cm long rotating shaft extending from the hemispherical side of the connecting tank, a 22.2 cm long, 3.2 cm wide shaft with two 11.8 cm long, 1.0 cm wide stirring blades attached, with an inclination angle Θ = 0° in the direction of rotation) connected to it. The screw was not connected, and the opening was sealed so that the stirred fibrous filler would remain. The bulk density V before charging was added to the hopper. 0 1 kg of the fibrous filler having the measured bulk density V was charged into the hopper 1, and the agitator 4 was rotated at a speed of 1 revolution / second for 15 minutes, after which the bulk density V 1 The bulk density after stirring was determined. 1 is the raw material bulk density V 0 A fibrous filler having a viscosity of 0.8 times or less is particularly preferred as a raw material to which the present invention is applied.
[0057] For the following raw materials, the bulk density V 0 and bulk density V after stirring1 is calculated, and the bulk density ratio (V 1 / V 0 The results were as follows: 1. Mitsubishi Chemical Corporation carbon fiber chopped fiber "Dialed K6371T" V 0 : 0.48 g / cm 3 , V 1 : 0.31 g / cm 3 , V 1 / V 0 : 0.65 2. Mitsubishi Chemical Corporation carbon fiber chopped fiber "Pyrofil TR06U" V 0 : 0.47 g / cm 3 , V 1 : 0.39 g / cm 3 , V 1 / V 0 : 0.83 3. Glass fiber "Chopped Strand T-187 V" manufactured by Nippon Electric Glass Co., Ltd. 0 : 0.62 g / cm 3 , V 1 : 0.54 g / cm 3 , V 1 / V 0 : 0.87 From the above results, it can be seen that "K6371T" is a raw material that increases in bulk upon stirring.
[0058] Example 1: The agitation supply device used was a conical hopper 1 with a lower inner diameter of 35 cm, a height of 65 cm, and an upper inner diameter of 60 cm, and a hemispherical connection tank 2 with an inner diameter of 35 cm. The agitator 4 used had a shaft 9 with a length of 16.0 cm (from the rotation axis to the outermost periphery) and a width of 4.0 cm, and an agitator blade 10 with a length of 17.0 cm and a tip width of 1.0 cm. As shown in (A1) Figure 3, the tip of the cross-shaped shaft 9 had a total of four agitator blades 10 inclined 30° in the direction of rotation, arranged alternately on the front and back sides of the shaft surface. The agitator blades 10 were arc-shaped and rotated along the inner surface of the hemispherical connection tank 2, and were installed so that each position was spaced 1.5 cm from the inner surface of the connection tank 2. The opening 6 had a long side of 17.0 cm and a short side of 8.5 cm, with an opening area of 144.5 cm. 2 The area of one stirring blade 10 is 47.8 cm 2The area multiplied by the inclination angle cos Θ (= 30°) is 41.4 cm 2 which is 0.29 times the area of the opening 6. The screw 5 in the cylinder 7 was a single-start screw with a screw diameter (D) of 45 mm and a lead of 42 mm (0.93D).
[0059] 40 kg of carbon fiber chopped fiber "K6371T" was charged into hopper 1. The motor ratio of the rotational speed of screw 5 (the value obtained by dividing the agitator rotational speed rpm by the screw rotational speed rpm) was set to 5%. The discharge rate to discharge section 3 was set to 20 kg / h, and constant weight operation was performed. The discharge amount after 60 to 100 minutes was calculated as follows: After 60 minutes, a container was placed under discharge section 3, and the weight W60 of the carbon fiber discharged over 36 seconds was calculated. Next, after 70 minutes, the weight was measured in the same way and calculated as W70. W80, W90, and W100 were calculated in the same way. The maximum and minimum values of W, the difference between the maximum and minimum values, the average value of W for the five measurements, and the rate of variation (%, = the difference between the maximum and minimum values of W for the five measurements / the average value of W for the five measurements) for W60 to W100 are shown in Table 1 below. 40 kg of the carbon fiber chopped fiber "K6371T" discharged to the discharge section 3 was recovered, and 40 kg of new "K6371T" was added to the hopper 1 and discharged under the same conditions, obtaining a total of 80 kg of "K6371T". The bulk density was measured to be 0.19 g / cm 3 As described above, it was found that the opening of "K6371T" was promoted by the rotation of the agitator 4 and the rotation of the screw 5 of the agitation supply device of the present invention, and the bulk density was significantly reduced. This discharged "K6371T" is referred to as "opened K6371T."
[0060] [Example 2] The same procedure as in Example 1 was carried out, except that the agitator (A1) in Example 1 was changed to an agitator (A2) having two agitating blades 10 inclined at 30° in the direction of rotation on both ends of a single shaft 9, one on the front side and one on the back side of the shaft surface. The area of one agitating blade 10 was 47.8 cm 2 The area multiplied by the inclination angle cos Θ (= 30°) is 41.4 cm 2 which is 0.29 times the area of the opening 6.
[0061] Comparative Example 1 The same procedure as in Example 1 was carried out except that the agitator 4 was changed to an agitator (AX) having two non-inclined stirring blades 10 on both ends of a single shaft 9, one on the front side and one on the back side of the shaft surface.
[0062] [Example 3] Carbon fiber chopped fiber "K6371T" (bulk density 0.48 g / cm 3 ) was "Open Fiber K6371T" (bulk density 0.19 g / cm 3 The procedure of Example 1 was repeated except that the temperature was changed to 100°C.
[0063] [Comparative Example 2] Carbon fiber chopped fiber "K6371T" (bulk density 0.48 g / cm 3 ) was "Open Fiber K6371T" (bulk density 0.19 g / cm 3 The same procedure as in Comparative Example 1 was carried out except that the temperature was changed to 100°C.
[0064] The results are shown in Table 1 below. In Table 1, the evaluation was based on the fluctuation rate (difference between the maximum and minimum values of five W measurements / average value of five W measurements) and judged according to the following criteria: A: Fluctuation rate is 7% or less B: Fluctuation rate is more than 7% to 10% or less C: More than 10% to 15% or less D: More than 15%
[0065]
[0066] [Example 1 for producing a thermoplastic resin composition] A twin-screw extruder "TEX44αII" manufactured by The Japan Steel Works, Ltd. was used as the extruder. The screw configuration was RRNNL for the first kneading section and RNL for the second kneading section. R denotes a forward kneading disc, N denotes an orthogonal kneading disc, and L denotes a reverse kneading disc, each with five paddles and a length of 44 mm. The cylinder temperature was set to 260°C. Polybutylene terephthalate resin "Novaduran 5008" manufactured by Mitsubishi Engineering Plastics Corporation was used as the main raw material. It was fed to the base of the screw at 180 kg / h using a belt feeder and melted in the first kneading section. A side feed screw was installed between the first and second kneading sections, and carbon fiber chopped fiber "K6371T" obtained by the method of Example 1 was fed at 20 kg / h and kneaded in the second kneading section. The screw rotation was 250 rpm. The strand was removed from the die, cooled in a water bath, and cut with a pelletizer to obtain pellets. Extrusion was continued for 1 hour, but the extrusion and strand were stable, and there was no torque over or strand breakage. 1 g of the pellet was dissolved in a good solvent, a 1 / 1 mixed solvent of phenol / tetrachloroethane, and the carbon fiber was filtered, dried, and weighed. The weight of the extracted carbon fiber was 0.097 g (the carbon content excluding the sizing agent in 0.1 g of carbon fiber was 0.098 g). This confirmed that the carbon fiber chopped fiber "K6371T" was fed uniformly.
[0067] [Comparative Example 1 for the Production of Thermoplastic Resin Composition] The same procedure as in Production Example 1 was carried out, except that the feeding of chopped carbon fiber was that obtained in Comparative Example 2. Torque fluctuations were large, and a torque overload occurred once within 1 hour, causing the extruder to stop. In addition, the strand broke three times. The weight of carbon fiber extracted from 1 g was 0.089 g, clearly demonstrating that the feeding of chopped carbon fiber was fluctuating.
[0068] [Thermoplastic Resin Composition Production Example 2] The same procedure as in Thermoplastic Resin Composition Production Example 1 was carried out, except that the main raw material was a polycarbonate resin "Iupilon S3000F" manufactured by Mitsubishi Engineering Corporation, and the dissolving solvent was methylene chloride. The extrusion and strand were stable, with no torque over or strand breakage. The weight of the extracted carbon fiber was 0.096 g, and it was confirmed that the carbon fiber chopped fiber K6371T had been fed uniformly.
[0069] [Production Example 3 of Thermoplastic Resin Composition] The same procedure as in Production Example 1 was carried out, except that the main raw material was a polyamide resin "MXD Nylon 6000" manufactured by Mitsubishi Gas Chemical Company, Inc., and the solvent was hexafluoroisopropanol. The extrusion and strand were stable, and there was no torque over or strand breakage. The weight of the extracted carbon fiber was 0.097 g, and it was confirmed that the carbon fiber chopped fiber K6371T was fed uniformly.
[0070] Example 4 The agitation supply device used was a conical hopper 1 with a bottom diameter of 29 cm, a height of 65 cm, and a top diameter of 60 cm, a connection tank 2 extending downward from an upper opening circle with a diameter of 29 cm in a generally conical shape with a bottom diameter of approximately 40 cm, and a conical connection tank 2 with a circular inclined surface 11 with a diameter of 26 cm at a 45° angle from the bottom upward at the bottom. The agitator 4 used was an agitator having a shaft 9 that rotates around a rotation axis 8 at the center of the circular inclined surface 11, and an agitator blade 10 attached to the tip of the shaft 9 that rotates on the circular inclined surface. The shaft 9 was 13 cm long from the rotation axis and 2.5 cm wide, and the agitator blade 10 was 10 cm long, 2.9 cm wide at the base, and 2.3 cm wide at the tip. The agitator (A1) used had a total of four agitating blades 10 inclined at 30° in the direction of rotation at the tip of the cross-shaped shaft 9, as shown in Figure 3. The tip of the stirring blade 10 is installed so that the closest distance from the inner wall surface of the connecting tank 2 is 0.7 cm. The opening 6 has a long side of 11.0 cm and a short side of 5.5 cm, and the opening area is 60.5 cm. 2 The area of one stirring blade 10 is 26.0 cm 2The area multiplied by the inclination angle cos Θ (= 30°) is 22.5 cm 2 which is 0.37 times the area of the opening 6. The screw 5 in the cylinder 7 was a single-start screw with a screw diameter (D) of 25.5 mm and a lead of 26 mm (1.02D).
[0071] 20 kg of carbon fiber chopped fiber "K6371T" was charged into hopper 1. The motor ratio of the rotational speed of screw 5 (the value obtained by dividing the agitator rotational speed rpm by the screw rotational speed rpm) was set to 5%. The discharge rate to discharge section 3 was set to 10 kg / h, and constant weight operation was performed. The discharge amount after 60 to 100 minutes was calculated as follows: After 60 minutes, a container was placed under discharge section 3, and the weight W60 of the carbon fiber discharged over 36 seconds was calculated. Next, after 70 minutes, the weight was measured in the same way and calculated as W70. W80, W90, and W100 were calculated in the same way. The maximum and minimum values of W, the difference between the maximum and minimum values, the average value of W for the five measurements, and the fluctuation rate (%, = the difference between the maximum and minimum values of W for the five measurements / the average value of W for the five measurements) for W60 to W100 are shown in Table 2 below. 20 kg of the carbon fiber chopped fiber "K6371T" discharged to the discharge section 3 was recovered, and 20 kg of new "K6371T" was added to the hopper 1 and discharged under the same conditions, obtaining a total of 40 kg of "K6371T". The bulk density was measured to be 0.19 g / cm 3 As described above, it was found that the opening of "K6371T" was promoted by the rotation of the agitator 4 and the rotation of the screw 5 of the agitation supply device of the present invention, and the bulk density was significantly reduced. This discharged "K6371T" is referred to as "opened K6371T."
[0072] [Example 5] The same procedure as in Example 4 was carried out, except that the agitator (A1) in Example 4 was changed to an agitator (A2) having two agitating blades 10 inclined at 30° in the direction of rotation on both ends of a single shaft 9. The area of one agitating blade 10 was 26.0 cm 2 The area multiplied by the inclination angle cos Θ (= 30°) is 22.5 cm 2 which is 0.37 times the area of the opening 6.
[0073] Comparative Example 3 The same procedure as in Example 4 was carried out except that the agitator 4 was changed to an agitator (AX) having a total of two non-inclined agitating blades 10 on both ends of a single shaft 9 .
[0074] The results are shown in Table 2. In Table 2, the evaluation was based on the fluctuation rate (the difference between the maximum and minimum values of W measured five times / the average value of W measured five times) and was judged according to the same criteria (A to D) as above.
[0075]
[0076] [Example 4 for producing a thermoplastic resin composition] A twin-screw extruder "TEX44αII" manufactured by The Japan Steel Works, Ltd. was used as the extruder. The screw configuration was RRNNL for the first kneading section and RNL for the second kneading section. R denotes a forward kneading disc, N denotes an orthogonal kneading disc, and L denotes a reverse kneading disc, each with five paddles and a length of 44 mm. The cylinder temperature was set to 260°C. Polybutylene terephthalate resin "Novaduran 5008" manufactured by Mitsubishi Engineering Plastics Corporation was used as the main raw material. It was fed to the base of the screw at 180 kg / h using a belt feeder and melted in the first kneading section. A side feed screw was installed between the first and second kneading sections, and carbon fiber chopped fiber "K6371T" obtained by the method of Example 1 was fed at 20 kg / h and kneaded in the second kneading section. The screw rotation was 250 rpm. The strand was removed from the die, cooled in a water bath, and cut with a pelletizer to obtain pellets. Extrusion was continued for 1 hour, but the extrusion and strand were stable, and there was no torque over or strand breakage. 1 g of the pellet was dissolved in a good solvent, a 1 / 1 mixed solvent of phenol / tetrachloroethane, and the carbon fiber was filtered, dried, and weighed. The weight of the extracted carbon fiber was 0.096 g (the carbon content excluding the sizing agent in 0.1 g of carbon fiber was 0.098 g). This confirmed that the carbon fiber chopped fiber "K6371T" was fed uniformly.
[0077] [Comparative Example 2 for the Production of Thermoplastic Resin Composition] The same procedure as in Production Example 4 was carried out, except that the feeding of chopped carbon fiber was that obtained in Comparative Example 3. Torque fluctuations were large, and a torque overload occurred once within 1 hour, causing the extruder to stop. In addition, the strand broke three times. The weight of carbon fiber extracted from 1 g was 0.085 g, clearly demonstrating that the feeding of chopped carbon fiber was fluctuating.
[0078] [Thermoplastic Resin Composition Production Example 5] The same procedure as in Thermoplastic Resin Composition Production Example 1 was carried out, except that the main raw material was a polycarbonate resin "Iupilon S3000F" manufactured by Mitsubishi Engineering Plastics Corporation, and the dissolving solvent was methylene chloride. The extrusion and strand were stable, with no torque over or strand breakage. The weight of the extracted carbon fiber was 0.096 g, and it was confirmed that the carbon fiber chopped fiber K6371T had been fed uniformly.
[0079] [Thermoplastic Resin Composition Production Example 6] The same procedure as in Production Example 4 was carried out, except that the main raw material was a polyamide resin "MXD Nylon 6000" manufactured by Mitsubishi Gas Chemical Company, Inc., and the solvent was hexafluoroisopropanol. The extrusion and strand were stable, and there was no torque over or strand breakage. The weight of the extracted carbon fiber was 0.099 g, and it was confirmed that the carbon fiber chopped fiber K6371T was fed uniformly.
[0080] The stirring and feeding device, feeding method, and manufacturing method for a fibrous filler of the present invention, and the manufacturing method for a thermoplastic resin composition, enable uniform and stable conveyance with a screw, even for fibrous fillers that tend to open easily and have low bulk density, and can stably produce thermoplastic resin compositions in which the fibrous filler is uniformly dispersed.
[0081] 1: Hopper 2: Connection tank 3: Discharge section 4: Agitator 5: Screw 6: Opening 7: Cylinder 8: Rotating shaft 9: Shaft 10: Agitating blade 11: Inclined surface
Claims
1. A device for feeding fibrous filler from a hopper containing the fibrous filler to a discharge section, which is provided with a connecting tank between the hopper and the discharge section, and inside the connecting tank is a shaft that rotates around a rotation axis, and at the tip of the shaft is a stirring blade for stirring the fibrous filler that is installed so that it rotates along the inner surface of the connecting tank, and the stirring blade is inclined inward at an angle Θ of 10° to 70° with respect to the rotation direction of the stirring blade.
2. The agitation and supply device for fibrous filler according to claim 1, further comprising a connection tank between the hopper and the discharge section, the connection tank having an approximately hemispherical inner surface, a shaft inside the connection tank that rotates vertically around a rotation axis that protrudes horizontally from the inner surface of the connection tank, and a stirring blade for stirring the fibrous filler at the tip of the shaft that rotates vertically along the inner surface of the connection tank, the stirring blade being inclined inward at an angle Θ of 10° to 70° relative to the rotation direction of the stirring blade.
3. The agitation supply device according to claim 2, wherein the shortest distance between the agitation blade and the inner peripheral surface of the connection tank is in the range of 0.2 to 5 cm.
4. The fibrous filler agitation and supply device according to claim 1, further comprising a connecting tank between the hopper and the discharge section, a circular inclined surface provided at the bottom of the connecting tank facing diagonally upward from the bottom of the connecting tank, a shaft that rotates around an axis of rotation that protrudes inward from the center of the circular inclined surface, and a stirring blade for agitating the fibrous filler provided at the tip of the shaft so as to rotate on the circular inclined surface, the stirring blade being inclined inward at an angle Θ of 10° to 70° relative to the rotation direction of the stirring blade.
5. The agitation supply device according to claim 4, wherein the shortest distance between the tip of the agitation blade and the inner wall surface of the connection tank is in the range of 0.2 to 5 cm.
6. The agitation supply device according to claim 1, wherein the number of agitation blades is 2 to 6.
7. The agitation and feeding device according to claim 1, further comprising a screw at the bottom of the connecting tank for feeding the fibrous filler to the discharge portion.
8. The agitation supply device according to claim 1, wherein the area of each agitation blade multiplied by the inclination angle cos Θ is in the range of 0.1 to 1.0 times the area of the opening to the screw at the bottom of the connecting tank when viewed from directly above.
9. A method for supplying fibrous filler contained in a hopper to a discharge section, comprising: a connecting tank between the hopper and the discharge section; a shaft rotating around an axis of rotation inside the connecting tank; a stirring blade for stirring the fibrous filler at the tip of the shaft so that it rotates along the inner surface of the connecting tank; the stirring blade is equipped with an agitator inclined inward at an angle Θ of 10° to 70° relative to the rotation direction of the stirring blade; the fibrous filler is opened by the agitator and supplied to the discharge section by a screw provided at the bottom of the connecting tank.
10. The method for feeding a fibrous filler according to claim 9, wherein the rotation speed of the agitator is 1 to 20% of the rotation speed of the screw.
11. Bulk density V of the fibrous filler contained in the hopper 0 is 0.3 to 0.7 g / cm 3 and the bulk density V of the discharged fibrous filler 1 is V 0 Smaller than 0.1 to 0.5 g / cm 3 11. The method for supplying a fibrous filler according to claim 9 or 10, wherein the range is 12. A method for producing a fibrous filler with a reduced bulk density by opening up a fibrous filler contained in a hopper, comprising: a connecting tank between the hopper and a discharge section; a shaft rotating around an axis of rotation inside the connecting tank; and a stirring blade for stirring the fibrous filler at the tip of the shaft, which is provided so as to rotate along the inner surface of the connecting tank; the stirring blade is provided with an agitator inclined inward at an angle Θ of 10° to 70° relative to the rotation direction of the stirring blade; the fibrous filler is opened up by the agitator and supplied to the discharge section by a screw provided at the bottom of the connecting tank.
13. Bulk density V of the fibrous filler contained in the hopper 0 is 0.3 to 0.7 g / cm 3 and the bulk density V of the discharged fibrous filler 1 is V 0 Smaller than 0.1 to 0.5 g / cm 3 The method for producing a fibrous filler according to claim 12, wherein the range is 14. A method for producing a thermoplastic resin composition by using an extruder, in which a fibrous filler is blended with a thermoplastic resin, characterized in that the fibrous filler with reduced bulk density obtained by the production method described in claim 12 or 13 is side-fed from a side feeder located downstream of the main inlet for raw materials containing the thermoplastic resin, and melt-kneaded.