AI Technical Summary
Conventional water-absorbing resins made from polysaccharides have insufficient water-absorbing performance, which limits their effectiveness in absorbent articles.
Development of an absorbent article containing a water-soluble polymer with acidic groups introduced into starch or its partial decomposition products, specifically carboxyalkyl, carboxyalkenyl, or sulfoalkyl groups, with a weight average molecular weight of 500,000 to 40,000,000, and a crosslinked structure forming a physical gel for enhanced water absorption and retention.
The resulting absorbent article exhibits excellent water-absorbing performance with non-pressure water absorption capacities and retention rates, and the ability to be recycled, reducing environmental impact.
Smart Images

Figure PI2025000634_DRAWING_001 
Figure PI2025000634_DRAWING_002
Abstract
Description
absorbent articles
[0001] The present invention relates to an absorbent article.
[0002] Absorbent articles are used in the hygiene and medical fields as disposable diapers, sanitary products, wound dressings, etc., as well as in the food, agriculture, forestry, civil engineering, and other fields. These absorbent articles exhibit liquid absorbency by containing a water-absorbent resin. Partially neutralized salts of polyacrylic acid and polymethacrylic acid are widely used as water-absorbent resins, and water-absorbent resins made from polysaccharides such as starch are also known.
[0003] Patent Document 1 discloses a method for producing a water-absorbent resin by heating and drying carboxyalkylated starch to crosslink the starch particles, and describes that it is preferable to suppress a reduction in the molecular weight of the starch during the carboxyalkylation reaction.
[0004] Patent Document 2 discloses a method for producing a water-absorbent resin by surface-treating carboxyalkylated polysaccharide particles with a non-crosslinking acid such as hydrochloric acid, and then crosslinking the polysaccharides together by heating and drying or by using a crosslinking agent.
[0005] Patent Document 3 discloses a method for producing a water-absorbing material by reacting starch with an acid anhydride of a polybasic acid in an extruder, and describes that it is preferable to suppress reduction in the molecular weight of the starch during the reaction with the acid anhydride of the polybasic acid.
[0006] U.S. Patent No. 5,079,354, JP-A-2010-504414, JP-A-2007-222704
[0007] Conventional water-absorbent resins made from polysaccharides have not been found to have sufficient water-absorbing properties. An object of the present invention is to provide an absorbent article containing a water-absorbent resin with excellent water-absorbing properties.
[0008] The present inventors have studied the chemical structure of water-absorbent resins made from polysaccharides and discovered a water-absorbent resin with excellent water-absorbing properties. The present invention has been accomplished by applying this water-absorbent resin to absorbent articles.
[0009] That is, the present invention relates to an absorbent article comprising a water-absorbent resin made of a water-soluble polymer in which an acidic group is introduced into starch or a partially hydrolyzed product thereof.
[0010] The acidic group is preferably a carboxyalkyl group, a carboxyalkenyl group, or a sulfoalkyl group.
[0011] The starch or its partial hydrolyzate preferably has a weight average molecular weight (Mw) of 7,500,000 or less and / or a dispersity (weight average molecular weight (Mw) / number average molecular weight (Mn)) of 5 or more.
[0012] The weight average molecular weight (Mw) of the water-soluble polymer, calculated as pullulan by aqueous size exclusion chromatography, is preferably 500,000 to 40,000,000.
[0013] The water-absorbent resin preferably has the following characteristics: (a) a water absorption capacity of ion-exchanged water under no pressure of 100 to 500 g / g, (b) a water retention rate of ion-exchanged water of 80 to 300 g / g, (c) a water absorption capacity of physiological saline under no pressure of 10 to 70 g / g, and / or (d) a water retention rate of physiological saline of 5 to 60 g / g.
[0014] It is preferably any one selected from the group consisting of hygiene products, medical products, food preservation products, civil engineering products, and agricultural and horticultural products.
[0015] The sanitary product is preferably any one selected from the group consisting of disposable diapers, sanitary products, incontinence pads, breast pads, portable toilets, and pet toilets.
[0016] The medical product is preferably any one selected from the group consisting of a hemostatic sponge, a wound protection material, a wound healing material, a medical waste solidification agent, a cooling agent, a carrier for a drug delivery system, and an artificial joint.
[0017] The present invention also relates to a regenerated water-soluble polymer obtained by treating the absorbent article with alkali.
[0018] The present invention also relates to a water-absorbent resin which is a crosslinked product of the recycled water-soluble polymer.
[0019] The present invention also relates to a water-absorbent article containing the water-absorbent resin.
[0020] The present invention also relates to a method for recovering hydrophilic fibers from an absorbent article containing hydrophilic fibers and a water-absorbent resin made of a water-soluble polymer in which an acidic group has been introduced into starch or a partial hydrolyzate thereof, the method comprising a step of treating a part or all of the water-absorbent article with an alkali to decompose the water-absorbent resin.
[0021] The water-absorbent article of the present invention has excellent water-absorbing performance. In addition, the water-absorbent resin made from polysaccharides can be decomposed and reused, which reduces the environmental impact.
[0022] 1 shows the results of gel filtration chromatography of the water-soluble polymer, and 2 shows the infrared absorption spectrum of the water-soluble polymer.
[0023] <Absorbent Article> The absorbent article of the present invention is characterized by including a water-absorbent resin made of a water-soluble polymer in which an acidic group is introduced into starch or a partially hydrolyzed product thereof.
[0024] <Starch or Partially Hydrolyzed Starch or Its Partially Hydrolyzed Product> In the present invention, starch or a partially hydrolyzed starch product is used as the main material of the water-absorbent resin. By using starch, it is possible to obtain a water-absorbent resin that is highly safe for the human body, has excellent water absorbency, and has a small environmental impact when disposed of. The starch raw material is not particularly limited, and examples include tapioca starch, potato starch, corn starch such as waxy corn starch and high-amylose starch, wheat starch, rice starch, and sweet potato starch. Partially hydrolyzed starch is starch, i.e., a polymer formed by linking a large number of α-glucose molecules via glycosidic bonds, in which some of the glycosidic bonds have been decomposed, but the position and manner of decomposition are not limited. A method for producing a water-absorbent resin will be described later, and starch and a partially hydrolyzed starch product may be used in combination when producing a water-absorbent resin.
[0025] When a partial starch hydrolysate is used, the weight-average molecular weight (Mw) of the partial starch hydrolysate is not particularly limited, but is preferably 7.5 million or less, more preferably 5 million or less, even more preferably 4.5 million or less, and even more preferably 4 million or less. The lower limit of the weight-average molecular weight of the partial starch hydrolysate is not particularly limited, but is preferably 50,000 or more, more preferably 100,000 or more, and even more preferably 200,000 or more. If the weight-average molecular weight is less than 50,000, the water absorption capacity of the water-absorbent resin tends to decrease. When the viscosity of the starch affects the operability during production, two or more types of starch and / or partial starch hydrolysate having different weight-average molecular weights, or other additives, may be used in combination depending on the application and cost. The method for measuring the weight-average molecular weight is not particularly limited, but it can be determined, for example, by aqueous size exclusion chromatography based on a calibration curve of molecular weight vs. elution time prepared using pullulan with a known molecular weight.
[0026] The degree of dispersion (weight average molecular weight (Mw) / number average molecular weight (Mn)) of the partial starch hydrolysate is not particularly limited, but is generally 5 or more, and if it is less than 5, the water absorption capacity of the water-absorbent resin tends to decrease. The upper limit of the degree of dispersion is not particularly limited. The method for measuring the number average molecular weight is not particularly limited, but for example, it can be determined by aqueous size exclusion chromatography based on a calibration curve of molecular weight and elution time prepared using pullulan with a known molecular weight.
[0027] The weight-average molecular weight and dispersity of starch or its partial hydrolyzates are as described above. When starch is used alone, starch derived from waxy corn, tapioca, corn, or potato is preferred, and starch derived from waxy corn, tapioca, or corn is more preferred. When a partial starch hydrolyzate is used alone, the weight-average molecular weight is preferably 50,000 to 7,500,000, more preferably 50,000 to 5,000,000, and even more preferably 100,000 to 4,000,000. The dispersity is preferably 5 or more, more preferably 7 or more.
[0028] <Water-soluble polymer, acidic group> As used herein, the term "water-soluble polymer" refers to a polymer in which an acidic group has been introduced into starch or a partially hydrolyzed product thereof.
[0029] Examples of the acidic group include acidic groups having a carboxyl group, such as a carboxyalkyl group and a carboxyalkenyl group; acidic groups having a sulfo group, such as a sulfoalkyl group and a sulfoalkenyl group; and acidic groups having a phospho group, such as a phosphoalkyl group and a phosphoalkenyl group.
[0030] A carboxyalkyl group is an alkyl group substituted with a carboxyl group. The number of carbon atoms in the alkyl group substituted with a carboxyl group is preferably 1 to 8, and more preferably 1 to 5. The alkyl group may be either linear or branched. Specific examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, an s-butyl group, a t-butyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, and a 1-ethyl-n-propyl group.
[0031] Specific examples of the carboxyalkyl group include a carboxymethyl group, a carboxyethyl group, a carboxypropyl group, a carboxybutyl group, and a carboxypentyl group.
[0032] A carboxyalkenyl group is an alkenyl group substituted with a carboxyl group. The alkenyl group substituted with a carboxyl group preferably has 2 to 8 carbon atoms, more preferably 2 to 4 carbon atoms. The alkenyl group may be either linear or branched. Specific examples of the alkenyl group include ethenyl, 1-propenyl, 2-propenyl, 1-methyl-1-ethenyl, 1-butenyl, 2-butenyl, 3-butenyl, 2-methyl-1-propenyl, 2-methyl-2-propenyl, 1-ethylethenyl, 1-methyl-1-propenyl, and 1-methyl-2-propenyl.
[0033] Specific examples of the carboxyalkenyl group include a carboxyethenyl group, a carboxypropenyl group, and a carboxybutenyl group.
[0034] A sulfoalkyl group is an alkyl group substituted with a sulfo group. Examples of the alkyl group substituted with a sulfo group include the alkyl groups mentioned in relation to the carboxyalkyl group. Specific examples of sulfoalkyl groups include a sulfomethyl group, a sulfoethyl group, and a sulfopropyl group.
[0035] The sulfoalkenyl group is an alkenyl group substituted with a sulfo group. The alkenyl group substituted with a sulfo group can be any of the alkenyl groups described above for the carboxyalkenyl group. Specific examples of the sulfoalkenyl group include a sulfoethenyl group and a sulfopropenyl group.
[0036] A phosphoalkyl group is an alkyl group substituted with a phospho group. The alkyl groups substituted with a phospho group can be the same as those mentioned for the carboxyalkyl group. Specific examples of the phosphoalkyl group include a phosphomethyl group, a phosphoethyl group, and a phosphopropyl group.
[0037] A phosphoalkenyl group is an alkenyl group substituted with a phospho group. The alkenyl group substituted with a phospho group can be any of the alkenyl groups described above for the carboxyalkenyl group. Specific examples of phosphoalkenyl groups include phosphoethenyl and phosphopropenyl groups.
[0038] Among the acidic groups, from the viewpoint of ease of introduction into starch or its partial hydrolyzates, acidic groups having a carboxyl group or a sulfo group are preferred, a carboxyalkyl group, a carboxyalkenyl group or a sulfoalkyl group is more preferred, and a carboxyalkyl group having 1 to 5 carbon atoms is even more preferred.
[0039] In the water-soluble polymer, in addition to the introduction of an acidic group into starch or a partial hydrolyzate thereof, the hydrogen atom of the hydroxyl group of the glucose unit may be substituted with a functional group other than the acidic group. Examples of the functional group other than the acidic group include hydrocarbon groups such as methyl groups and ethyl groups, and substituents having a hydroxyl group such as hydroxypropyl groups and hydroxyethyl groups. The position of the hydroxyl group substituted with the functional group other than the acidic group may be any of the 1-, 2-, 3-, 4-, and 6-positions of the glucose unit, but the 2-, 3-, and 6-positions are preferred.
[0040] The molecular weight of the water-soluble polymer is not particularly limited, but the weight-average molecular weight in terms of pullulan as determined by aqueous size exclusion chromatography analysis is preferably 500,000 to 40,000,000, and more preferably 800,000 to 35,000,000. If the weight-average molecular weight is less than 500,000, the water absorption performance of the water-absorbent resin tends to decrease, while if it exceeds 40,000,000, the viscosity tends to be high and handling during production tends to decrease. The weight-average molecular weight in terms of pullulan as determined by aqueous size exclusion chromatography analysis can be determined based on a calibration curve of molecular weight and elution time created using pullulan with a known molecular weight in aqueous size exclusion chromatography.
[0041] The water-soluble polymer preferably has a total acid value of 50 to 350 mgKOH / g, more preferably 70 to 300 mgKOH / g. As will be described later, during the production of a water-absorbent resin, the salts of acidic groups added to starch or partial starch hydrolysates are partially neutralized. The total acid value means the acid value measured after returning the neutralized acidic groups to an unneutralized state, and indicates the amount of all acidic groups possessed by the water-soluble polymer. If the total acid value is less than 50 mgKOH / g or exceeds 350 mgKOH / g, the water-absorbent resin after crosslinking the water-soluble polymer tends to have reduced water absorption performance for aqueous solutions containing electrolytes, such as physiological saline.
[0042] When acidic groups are introduced by reacting a haloalkyl group having an acidic group with hydroxyl groups of starch to produce a water-soluble polymer, the amount of introduced acidic groups can also be expressed by the degree of etherification. The degree of etherification is preferably 0.1 to 2.0, more preferably 0.2 to 1.5. The degree of etherification can be determined by ashing titration or the like. Furthermore, the total acid value is detected by the introduction of acidic groups. If the raw starch or partial starch hydrolysate does not contain acidic groups, the acidic groups detected by measuring the total acid value are considered to be equal to those introduced by the etherification reaction. Therefore, if the raw starch or partial starch hydrolysate does not contain acidic groups, the degree of etherification can be simply calculated from the total acid value. For example, if the acidic groups are carboxymethyl groups and all of them are neutralized as sodium salts, the degree of etherification can be calculated by the formula: (162 × total acid value) ÷ (56100 − 80 × total acid value). The unit of the total acid value is mgKOH / g.
[0043] The free acid value of the water-soluble polymer is preferably 5 to 50 mgKOH / g, more preferably 7 to 25 mgKOH / g. The free acid value means the acid value measured for unneutralized acid groups. If the free acid value is less than 5 mgKOH / g or more than 50 mgKOH / g, the water absorption performance of the water-absorbent resin tends to decrease.
[0044] The dispersity (weight average molecular weight / number average molecular weight) of the water-soluble polymer is not particularly limited, but is preferably 5 to 110, and more preferably 7 to 70. If it is less than 5 or exceeds 110, the water absorption performance of the water-absorbent resin tends to decrease. The number average molecular weight of the water-soluble polymer can be determined by aqueous size exclusion chromatography based on a calibration curve of molecular weight and elution time prepared using pullulan with a known molecular weight.
[0045] <Cross-linked structure of water-absorbent resin> Generally, water-absorbent resins having polyacrylic acid as a main constituent unit have a network structure formed by covalent bonds, and form a chemical gel upon absorbing water. In contrast, the water-absorbent resin used in the present invention is characterized by forming a physical gel upon absorbing water. The cross-linked points of a physical gel disappear relatively easily due to thermal motion of molecular chains or changes in pH or ionic strength, and the physical gel can be converted into a fluid sol. Therefore, the physical gel is easily decomposed by adding alkali or acid, heating, shaking, etc., which leads to a reduction in the environmental impact upon disposal.
[0046] The formation of a physical gel can be confirmed by confirming a sol-gel transition due to the disappearance of the crosslinking points. For example, in the case of crosslinking by ionic bonds and / or hydrogen bonds, it can be confirmed by fluidization after alkali or acid treatment. Specifically, when a water-absorbent resin is suspended in a 1% aqueous sodium hydroxide solution to a final concentration of 5% by weight, stirred for 60 minutes, and then sieved through a sieve with an opening of 500 μm, it can be determined that a physical gel is formed by water absorption when the dry weight of the water-absorbent resin remaining on the sieve is less than 2% by weight of the dry weight of the water-absorbent resin contained in the aqueous solution.
[0047] More specifically, 0.5 g of water-absorbent resin was suspended in 9.5 g of 1% aqueous sodium hydroxide solution and stirred for 60 minutes. The suspension was then naturally filtered through a 30-mesh wire mesh (500 μm mesh size) measuring approximately 50 mm x 50 mm, and the mesh was washed with ion-exchanged water. After washing, the wire mesh was dried for 2 hours in a 120°C air dryer. When the weight of the wire mesh before filtration is Wm1 and the weight of the wire mesh after filtration and drying is Wm2, it can be determined that a physical gel has formed by water absorption if the 30-mesh pass residue calculated using the following formula is less than 2 wt%. The 500 μm mesh sieve is a 30-mesh sieve specified by JIS. Residue passing 30 mesh (%)=(Wm2-Wm1) / 0.5×100 The residue passing 30 mesh is preferably less than 2% by weight, more preferably less than 1.5% by weight, even more preferably less than 1.0% by weight, and even more preferably less than 0.5% by weight.
[0048] The water-absorbent resin is a crosslinked product of the water-soluble polymer described above. The crosslinking consists of internal crosslinking and, optionally, surface crosslinking. However, it is preferable that the water-absorbent resin does not have an internal crosslinked structure via an ether bond or an ester bond. Furthermore, it is preferable that the water-absorbent resin does not have an internal crosslinked structure via a covalent bond. Examples of the covalent bond include ester bonds, ether bonds, carbon-carbon covalent bonds, double bonds, etc. Internal crosslinked structures constituting the water-absorbent resin include, for example, ionic bonds between acidic groups and neutralized acidic groups on the water-soluble polymer, ionic bonds with compounds having an opposite charge to the water-soluble polymer (when the acidic group of the water-soluble polymer is carboxylic acid, compounds containing basic groups such as cationic groups or amino groups), ionic bonds with divalent alkali metal ions, coordinate bonds via metal ions, and hydrogen bonds such as carboxylic acid dimerization when the acidic group is a carboxylic acid group. The method of forming surface crosslinks will be described later.
[0049] The water-absorbent resin may optionally contain a structural unit other than the water-soluble polymer described above. Examples of structural units other than the water-soluble polymer include compounds having an opposite charge to that of the water-soluble polymer, such as polymers having amino groups such as chitosan, polyethyleneimine, and vinylpyrrolidone-N,N-dimethylaminoethyl methacrylic acid copolymers, or salts thereof, and polymers having quaternary ammonium groups such as dimethylamine-epichlorohydrin copolymers and polydiallyldimethylammonium chloride. When the water-absorbent resin contains a structural unit other than the water-soluble polymer, the content of the structural unit other than the water-soluble polymer is preferably 90% by weight or less, more preferably 50% by weight or less, based on the total amount of the water-soluble polymer used as the main component.
[0050] The water-absorbent resin may contain water and / or a hydrophilic solvent. Examples of hydrophilic solvents include methanol, ethanol, n-propanol, isopropanol, acetone, ethylene glycol, propylene glycol, diethylene glycol, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol dimethyl ether, and dimethyl sulfoxide. The content of water and / or hydrophilic solvent in the water-absorbent resin is preferably 0.1 to 20%, and more preferably 1 to 19%. If the content is less than 0.1%, the water absorption rate tends to decrease, and if it exceeds 20%, the water-absorbent resin particles tend to aggregate during water absorption. The content of water and / or hydrophilic solvent can be adjusted by subjecting the water-absorbent resin to treatments such as heating and drying.
[0051] <Physical Properties of Water-Absorbent Resin> The water absorption capacity of a water-absorbent resin under no load is determined by measuring the absorbency of physiological saline or ion-exchanged water when no load is applied to the water-absorbent resin using the method described in the Examples. The water-absorbent resin used in the present invention, in its solid state, preferably has a water absorption capacity for ion-exchanged water under no load of 100 to 500 g / g, more preferably 100 to 400 g / g, and even more preferably 120 to 350 g / g. Furthermore, the water-absorbent resin used in the present invention preferably has a water absorption capacity for physiological saline under no load of 10 to 70 g / g, more preferably 20 to 65 g / g.
[0052] The ratio (A / B) of the absorbency of the water-absorbent resin for ion-exchanged water without load (A) to the absorbency of physiological saline without load (B) is preferably 7 or less, more preferably 5 or less.
[0053] The water retention rate of a water-absorbent resin can be determined by measuring the absorbency of physiological saline or ion-exchanged water when a load of 150 G is applied to the water-absorbent resin, using the method described in the Examples. The water-absorbent resin of the present invention, in its solid state, preferably has a water retention rate for ion-exchanged water of 80 to 300 g / g, more preferably 100 to 250 g / g. Furthermore, the water-absorbent resin of the present invention preferably has a water retention rate for physiological saline of 5 to 60 g / g, more preferably 10 to 60 g / g, and even more preferably 20 to 60 g / g.
[0054] <Method for producing water-absorbent resin> The method for producing the water-absorbent resin is not particularly limited as long as it has the above-mentioned structure, but it can be obtained, for example, by a step of forming an internal crosslinked structure in starch or a partially hydrolyzed product thereof. Furthermore, before the step of forming the internal crosslinked structure, the method may include a step of partially hydrolyzing the starch and / or a step of introducing an acidic group, as necessary. Note that when the step of partially hydrolyzing the starch and the step of introducing an acidic group are included, these steps may be performed in any order, and either step may be performed first.
[0055] In the process of partially hydrolyzing starch, the α-1,4-glucosidic bond of the α-glucose molecules constituting the starch is often degraded, but the position and manner of degrading are not limited. The degrading method is not particularly limited, and examples include enzyme treatment, acid treatment, physical crushing, and the like. These methods may also be combined. The enzyme treatment may be carried out after gelatinization of the starch, or may be carried out simultaneously with gelatinization. An example of a method of carrying out the enzyme treatment after gelatinization of the starch is a method in which the starch is first suspended in water and heated to gelatinize it, and then an enzyme is added to carry out the enzymatic reaction. An example of a method of carrying out the enzyme treatment simultaneously with the starch gelatinization is a method in which the starch is suspended in water, and the mixture to which the enzyme is added is heated within a temperature range in which the enzyme is not completely inactivated. Among these methods, it is preferable to carry out the enzyme treatment while gelatinizing the starch by heating and kneading it at 70 to 110°C.
[0056] When partial degradation of starch is carried out by enzymatic treatment, the enzyme used is not particularly limited as long as it can degrade starch, and may be either an exo-enzyme or an endo-enzyme. Specific examples of enzymes include α-amylase, amylomaltase, cyclomaltodextrin glucanotransferase, 4-α-glucanotransferase, 4,6-α-glucanotransferase, neopullulanase, and amylopullulanase. These enzymes may also be used in combination. The pH during the enzymatic treatment is not particularly limited, but a pH of 5.0 to 7.0 is preferred. The pH can be adjusted by adding hydrochloric acid, acetic acid, sodium hydroxide, potassium hydroxide, or the like.
[0057] When partial decomposition of starch is carried out by acid treatment, the acid to be used is not particularly limited as long as it can decompose starch, and specific examples include hydrochloric acid, sulfuric acid, oxalic acid, acetic acid, formic acid, trifluoroacetic acid, etc. The temperature during the acid treatment is preferably 150 to 160°C.
[0058] When starch is partially decomposed by physical crushing, specific means include irradiation, shearing, grinding, high-pressure treatment, ultrasonic waves, thermal decomposition, photolysis, and combinations thereof.
[0059] The starch or its partial hydrolyzates may be a derivative in which the hydrogen atom of the hydroxyl group of the glucose unit is substituted with a functional group (also called processed starch or chemically modified starch), or bleached starch. The position of the hydroxyl group where the hydrogen atom is substituted may be any of the 1st, 2nd, 3rd, 4th, and 6th positions of the glucose unit, with the 2nd, 3rd, and 6th positions being preferred. Examples of the functional group include hydrocarbon groups such as methyl and ethyl groups; substituents having a hydroxyl group such as hydroxypropyl and hydroxyethyl groups; and substituents having a carboxyl group such as carboxymethyl groups. Examples of derivatives of starch or its partial hydrolyzates include acetylated adipate cross-linked starch, acetylated phosphate cross-linked starch, acetylated oxidized starch, sodium octenylsuccinate starch, starch acetate, oxidized starch, hydroxypropyl starch, hydroxypropylphosphate cross-linked starch, phosphate monoesterified phosphate cross-linked starch, phosphated starch, phosphate cross-linked starch, cationized starch, and urea phosphate esterified starch, which are used in food and industrial applications and are known as modified starches. Also usable are methylethylated starch and hydroxypropylmethylated starch substituted with two or more functional groups. Among these, starch acetate, oxidized starch, hydroxypropyl starch, and sodium octenylsuccinate starch are preferred because of the ease of controlling the properties of the water-absorbent resin.
[0060] When the starch or its partial hydrolyzate is a derivative in which the hydrogen atom of the hydroxyl group of the glucose unit is substituted with an acidic group, a step of introducing an acidic group may be carried out to further add an acidic group, or a step of forming an internal crosslinked structure may be carried out without carrying out the step of introducing an acidic group.
[0061] In the step of introducing acidic groups, starch or a partial starch hydrolysate is reacted with an acidic group-containing compound or its precursor. This reaction introduces acidic groups into the hydroxyl groups of the starch or partial starch hydrolysate. The acidic group-containing compound is not particularly limited as long as it can introduce the aforementioned acidic group, and examples thereof include haloalkyl compounds having an acidic group, haloalkenyl compounds having an acidic group, acid anhydrides, and salts thereof. Examples of halogens constituting haloalkyl compounds and haloalkenyl compounds include chlorine and bromine.
[0062] Specific examples of the acidic group-containing compound include monochloroacetic acid, monobromoacetic acid, 3-bromopropionic acid, 6-bromohexanoic acid, succinic anhydride, maleic anhydride, vinyl sulfonic acid, phosphorus oxychloride, ethyl monochloroacetate, and sodium salts and potassium salts thereof. Specific examples of the salts include sodium monochloroacetate, potassium monochloroacetate, and sodium vinyl sulfonate.
[0063] Examples of the precursor of the acidic group-containing compound include acrylonitrile, etc. Examples of the method using acrylonitrile include a method in which acrylonitrile is first reacted with starch or a partial decomposition product thereof under basic conditions to introduce a cyanoethyl group, which is then converted into an amide group (Synthesis; 1989(12):949-950), and the resulting amide is then subjected to alkaline hydrolysis.
[0064] The reaction scheme for producing a water-soluble polymer by reacting starch or a partial starch hydrolysate with monochloroacetic acid is shown in formula (I).
[0065] The reaction scheme for producing a water-soluble polymer by reacting starch or a partial starch hydrolysate with 3-bromopropionic acid is shown in formula (II).
[0066] The reaction scheme for producing a water-soluble polymer by reacting starch or a partial starch hydrolysate with 6-bromohexanoic acid is shown in formula (III).
[0067] The reaction scheme for producing a water-soluble polymer by reacting starch or a partial starch hydrolysate with succinic anhydride is shown in formula (IV).
[0068] The reaction scheme for producing a water-soluble polymer by reacting starch or a partial starch hydrolysate with maleic anhydride is shown in formula (V).
[0069] The reaction scheme for producing a water-soluble polymer by reacting starch or a partially hydrolyzed starch product with sodium vinyl sulfonate is shown in formula (VI).
[0070] Although formulas (I) to (VI) show water-soluble polymers in which sodium salts of acidic groups have been introduced into all hydroxyl groups at the 6-position of glucose units, hydroxyl groups to which no acidic group has been introduced may remain. Furthermore, acidic groups that have not been neutralized by salts may also exist. The position at which the acidic group is introduced is not limited as long as it is a hydroxyl group present in starch or a partial starch hydrolysate, and may be any of the 1-, 2-, 3-, 4-, and 6-positions.
[0071] When a haloalkyl compound or a haloalkenyl compound is used as the acidic group-containing compound, it is preferable to use 1 to 1.5 equivalents of an alkaline agent relative to the haloalkyl compound or haloalkenyl compound. Examples of alkaline agents include sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, sodium carbonate, and potassium carbonate. The acidic groups introduced into the starch or partial starch hydrolysate preferably form salts with the sodium, potassium, lithium, ammonia, or the like derived from the alkaline agent. For this reason, it is preferable to use an amount of alkaline agent necessary for both the reaction of the haloalkyl compound or haloalkenyl compound with the starch or its partial hydrolysate and the neutralization of the acidic groups of the haloalkyl compound or haloalkenyl compound. For example, when chloroacetic acid is used as the acidic group-containing compound, it is theoretically preferable to use at least 2 equivalents of the alkaline agent relative to the chloroacetic acid. When sodium chloroacetate is used, the acidic groups are neutralized in advance, so it is preferable to use at least 1 equivalent of the alkaline agent relative to the sodium chloroacetate.
[0072] The amount of the acidic group-containing compound used can be set arbitrarily depending on the desired total acid value (degree of etherification) of the water-soluble polymer. Typically, 0.5 to 5.0 equivalents per mole of hydroxyl groups in the starch or starch partial hydrolysate are preferred, with 0.5 to 2 equivalents being more preferred. When a haloalkyl compound such as chloroacetic acid is used and the reaction is carried out in an aqueous solution, the acidic group introduction reaction and the hydrolysis reaction of the haloalkyl compound compete with each other, so the haloalkyl compound is required in excess of the theoretical amount. The amount of the haloalkyl compound used in the aqueous solution reaction is preferably set to 5 equivalents or less relative to the theoretical value.
[0073] The reaction temperature between starch or a partial starch hydrolysate and an acidic group-containing compound is not particularly limited, but is preferably 0 to 120°C. The reaction time is not particularly limited, but is preferably 1 to 24 hours. The reaction may be carried out in water, or in a mixed solvent of water and an alcohol such as methanol, ethanol, isopropanol, butanol, ethylene glycol, diethylene glycol, propylene glycol, or ethylene glycol monoethyl ether, or a glycol ether such as ethylene glycol dimethyl ether. Alternatively, the reaction may be carried out by dispersing a dried powder of the partial starch hydrolysate in a hydrophilic solvent such as an alcohol such as methanol, ethanol, isopropanol, or butanol, or a glycol ether such as ethylene glycol dimethyl ether. When a mixed solvent is used, the proportion of the solvent other than water in the mixed solvent is preferably 50% by volume or less. A reaction vessel, an extruder, or the like can be used as the reaction apparatus.
[0074] When a haloalkyl compound such as chloroacetic acid or a salt thereof is used as the acidic group-containing compound, the reaction temperature with starch or a partial starch hydrolysate is not particularly limited, but is preferably 0 to 100°C.
[0075] In particular, when chloroacetic acid or a salt thereof is used as the haloalkyl compound, the reaction is preferably carried out at 25 to 90°C to prevent hydrolysis by water in the reaction solution. The reaction time is preferably the time until the raw material haloalkyl compound is consumed, and more preferably 1 to 12 hours to ensure the stability of the haloalkyl compound and the efficiency of the process. The reaction may be carried out in water, or in a mixed solvent of water with an alcohol such as methanol, ethanol, isopropanol, or butanol, or a glycol ether such as ethylene glycol dimethyl ether. Alternatively, the reaction may be carried out by dispersing a powder of the dried starch partial hydrolyzate in a hydrophilic solvent such as an alcohol such as methanol, ethanol, isopropanol, or butanol, or a glycol ether such as ethylene glycol dimethyl ether. When a mixed solvent is used, the proportion of the solvent other than water in the mixed solvent is preferably 50% by volume or less. A reaction vessel, extruder, or the like can be used as the reaction apparatus.
[0076] Furthermore, when an acid anhydride is used as the acidic group-containing compound, the reaction proceeds simply by mixing the starch partial hydrolyzate with the acid anhydride and heating, but to promote the reaction, a catalyst such as sodium carbonate, sodium hydroxide, or a tertiary amine such as triethylamine, an imidazole such as 2-methylimidazole, a quaternary ammonium salt such as tetrabutylammonium bromide, or a phosphonium salt such as tetrabutylphosphonium bromide may be used. The amount of these catalysts added is preferably 0.1 equivalents or less relative to the acidic group-containing compound. These catalysts may be used alone or in combination of two or more.
[0077] The reaction time is preferably the time until the raw material acid anhydride is consumed, more preferably 1 to 12 hours. The end point of the reaction can be determined by acid value measurement or IR measurement. The reaction may be carried out in water, but to prevent hydrolysis or alcoholysis of the acid anhydride, aprotic solvents such as dimethyl sulfoxide, dimethylformamide, dimethylacetamide, and N-methylpyrrolidone are preferred as the reaction solvent. When a mixed solvent is used, the proportion of solvents other than water in the mixed solvent is preferably 50% by volume or more. When the reaction is carried out without a solvent, the acid anhydride can function as a solvent, so the reaction temperature is preferably above the melting point of the acid anhydride. When a solvent is used in the reaction, the reaction temperature is preferably 50 to 100°C, more preferably 70 to 90°C. A reaction kettle, extruder, or the like can be used as the reaction apparatus.
[0078] It is preferable to neutralize a portion of the salt of the acidic group added to the starch or partial starch hydrolysate. Neutralization converts some of the acidic groups that formed salts into free acidic groups. For example, when monochloroacetic acid is used as the acidic group-containing compound and sodium hydroxide is used as the alkaline agent, sodium salts of carboxyl groups are added to the starch or partial starch hydrolysate. Adding an acid to this converts some of the carboxyl groups into free carboxylic acids.
[0079] The acid used for neutralization is not particularly limited, but when the acidic group is a carboxyl group, an acid with a pKa equal to or lower than that of the carboxyl group is preferred, such as hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, acetic acid, formic acid, or trichloroacetic acid. A strong acid is preferably used to neutralize a sulfo or phospho group, and a mineral acid such as hydrochloric acid or sulfuric acid, or a strongly acidic ion exchange resin, etc., is used. Neutralization can be carried out using known devices such as a reaction kettle or extruder. After the addition of the acid, the mixture is preferably stirred at 0 to 50°C for 0.2 to 1 hour to allow for the neutralization reaction. The neutralization reaction is preferably carried out under conditions of pH 6.8 to 7.2.
[0080] During the acidic group introduction process and the subsequent neutralization reaction, salts may be formed between the halogen derived from the acidic group-containing compound and the metal or ammonia derived from the alkaline agent, so desalting is preferred. Desalting methods include a method in which a water-soluble polymer is dissolved in water to form an aqueous solution, which is then dropped into a hydrophilic solvent such as methanol, ethanol, isopropanol, acetone, or acetonitrile to reprecipitate the water-soluble polymer and recover it by filtration. The water-soluble polymer recovered by filtration is then redispersed in aqueous methanol (water content of approximately 70 to 90%), stirred, and the water-soluble polymer particles are recovered by filtration. Another desalting method includes a method in which an aqueous solution of the hydrophilic polymer is treated with a filter having an ultrafiltration membrane. Water or a mixture of water and a hydrophilic organic solvent such as methanol, ethanol, propanol, acetone, or acetonitrile can be used as the washing liquid during desalting. Desalting is preferably carried out until the salt concentration in the water-soluble polymer is 1% or less.
[0081] In the step of forming an internal crosslinked structure, water-soluble polymers are crosslinked with each other. Crosslinking can be formed without using a crosslinking agent, for example, by a method of heating and drying a water-soluble polymer in which some of the acidic groups are free acid groups under water-containing conditions. The temperature during heating and drying is preferably 50 to 150°C, more preferably 60 to 130°C. The pressure during heating and drying is not particularly limited, and can be performed at normal pressure, specifically, preferably 0.9 to 1.1 atm. The drying method is not particularly limited, and can be performed using a drum dryer, spray dryer, Nauta mixer, etc.
[0082] During heat drying, the water-soluble polymer may contain a hydrophilic solvent in addition to water. Examples of hydrophilic solvents include lower aliphatic alcohols such as methanol, ethanol, n-propanol, and isopropanol; ketones such as acetone; ethers such as dioxane, tetrahydrofuran, and methoxy(poly)ethylene glycol; and amides such as ε-caprolactam and N,N-dimethylformamide. The proportion of the hydrophilic solvent other than water in the total solvent is preferably adjusted based on the boiling point of the solvent. When the boiling point of the solvent is 100°C or less, the proportion is preferably 70% by volume or more, and when the boiling point is higher than 100°C, the proportion is preferably 30% by volume or less. Furthermore, the water-soluble polymer at the start of heat drying may be in the form of an aqueous solution or a powder containing a water-containing solvent with a water content of 1% by weight or more. When drying a powder containing a water-containing solvent, the wet ratio of the powder at the start of drying is preferably 1 to 85% by weight, more preferably 20 to 80% by weight, and even more preferably 55 to 75% by weight. The wet ratio here refers to the ratio of the total amount of water and hydrophilic solvent in the powder.
[0083] When producing a water-absorbent resin, surface cross-linking may be carried out in addition to internal cross-linking. Surface cross-linking can improve the strength of the water-absorbent resin. Examples of cross-linking agents used for surface cross-linking include epoxy compounds, polyhydric alcohol compounds, polyvalent amine compounds, polyisocyanate compounds, alkylene carbonate compounds, haloepoxy compounds, halohydrin compounds, polyvalent oxazoline compounds, carbodiimide compounds, silane coupling agents, and polyvalent metal compounds.
[0084] Examples of the epoxy compound include succinic acid glycidyl ester, sorbitol polyglycidyl ether, trimethylolpropane polyglycidyl ether, polyethylene glycol diglycidyl ether, glycerol polyglycidyl ether, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and glycidol.
[0085] Examples of the polyhydric alcohol compound include ethylene glycol, diethylene glycol, propylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, 1,3-propanediol, dipropylene glycol, 2,2,4-trimethyl-1,3-pentanediol, polypropylene glycol, glycerin, polyglycerin, 2-butene-1,4-diol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,2-cyclohexanediol, trimethylolpropane, diethanolamine, triethanolamine, polyoxypropylene, oxyethylene-oxypropylene block copolymer, pentaerythritol, and sorbitol.
[0086] Examples of the polyvalent amine compound include ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, polyethyleneimine, inorganic salts or organic salts (such as azithinium salts) of these polyvalent amine compounds, and the like.
[0087] Examples of the polyisocyanate compound include 2,4-tolylene diisocyanate and hexamethylene diisocyanate, and examples of the polyoxazoline compound include 1,2-ethylenebisoxazoline.
[0088] Examples of the alkylene carbonate compound include 1,3-dioxolan-2-one, 4-methyl-1,3-dioxolan-2-one, 4,5-dimethyl-1,3-dioxolan-2-one, 4,4-dimethyl-1,3-dioxolan-2-one, 4-ethyl-1,3-dioxolan-2-one, 4-hydroxymethyl-1,3-dioxolan-2-one, 1,3-dioxan-2-one, 4-methyl-1,3-dioxan-2-one, and 4,6-dimethyl-1,3-dioxan-2-one.
[0089] Examples of the haloepoxy compound include epichlorohydrin, epibromohydrin, α-methylepichlorohydrin, and polyamine adducts thereof (eg, Kaimen (registered trademark) manufactured by Hercules).
[0090] Other known crosslinking agents that can be used include aqueous carbodiimide compounds (e.g., Carbodilite manufactured by Nisshinbo Chemical Inc.), silane coupling agents such as γ-glycidoxypropyltrimethoxysilane and γ-aminopropyltriethoxysilane, and polyvalent metal compounds such as hydroxides and chlorides of zinc, calcium, magnesium, aluminum, iron, zirconium, and the like.
[0091] Among these, epoxy compounds are preferred, and ethylene glycol diglycidyl ether, sorbitol polyglycidyl ether, and succinic acid glycidyl ester are more preferred.
[0092] The surface crosslinking can be formed by spraying a surface crosslinking agent onto a water absorbent resin, mixing by a known method using a cylindrical mixer, a V-shaped mixer, a ribbon mixer, a screw mixer, a double-arm mixer, a pulverizing kneader, etc., and then crosslinking. During spraying and mixing, a surfactant can be added as necessary.
[0093] Furthermore, for the purpose of imparting various functions to the water absorbent resin, it may contain other additives such as disinfectants, deodorants, antibacterial agents, fragrances, various inorganic powders, foaming agents, pigments, dyes, hydrophilic short fibers, fertilizers, oxidizing agents, reducing agents, water, and salts. The amounts of these additives to be added are appropriately selected by those skilled in the art.
[0094] <Uses of Absorbent Article> The absorbent article of the present invention can be used as a sanitary product, a medical product, a civil engineering product, a food preservation product, an agricultural or horticultural product, or the like.
[0095] Because the absorbent article of the present invention is capable of absorbing and retaining protein-containing liquids, it can be used in hygiene and medical applications to absorb and retain not only urine but also protein-containing liquids such as blood, menstrual blood, and breast milk. Specific hygiene products include disposable diapers, sanitary products, incontinence pads, breast milk pads, masks for packs, portable toilets, pet toilets, and cat litter. Medical products include hemostatic sponges (medical pads), wound protection materials, wound healing materials, medical waste solidifying agents, ice packs, carriers for drug delivery systems, artificial joints, and compresses.
[0096] Food preservation products include ice packs, cooling gels, moisture retaining materials, anti-condensation sheets, drip absorbers, and freshness preserving agents.
[0097] Civil engineering products include waterproofing materials, waste liquid solidifying agents, soil surplus solidifying agents, and anti-condensation building materials.
[0098] Examples of agricultural and horticultural products include soil conditioners, soil water-retaining materials, seedling pots, seedbeds, hydroponic cultivation supports, fertilizer-retaining materials, and fertilizer slow-release agents.
[0099] Other uses include as a thickener for fragrances, disposable body warmers, portable toilets, cosmetics, etc.
[0100] <Disposable diapers and napkins> The absorbent article of the present invention may have a structure suitable for each application, as long as it contains the water-absorbent resin described above. For example, when the absorbent article is a disposable diaper or napkin, the disposable diaper or napkin is made of a laminate in which a top sheet, an absorbent body, and a back sheet are laminated in this order.
[0101] The top sheet is a sheet that comes into contact with the wearer's body when the disposable diaper or napkin is worn. The top sheet is preferably liquid-permeable, and can be made of a hydrophilic nonwoven fabric, a porous resin film, or the like. The back sheet is a sheet that does not come into contact with the wearer's body when the disposable diaper or napkin is worn, and is positioned on the outside. The back sheet is preferably liquid-impermeable, and can be made of a hydrophobic nonwoven fabric, a resin film, a laminate of a nonwoven fabric and a resin film, or the like.
[0102] The absorbent body contains the water-absorbent resin described above. The absorbent body may be a molded body obtained by molding the water-absorbent resin into a predetermined shape. Alternatively, the water-absorbent resin may be wrapped in a core wrap and used as the absorbent body. The core wrap may be a paper sheet or a liquid-permeable nonwoven fabric.
[0103] In addition to the water-absorbent resins described above, the absorbent may contain other hydrophilic fibers, such as absorbent paper, pulp, acetate, tissue, hydrophilic nonwoven fabric, natural hydrophilic fibers such as cotton, naturally derived cellulose-based hydrophilic fibers such as lyocell, rayon, and cupra, and petroleum-derived hydrophilic fibers obtained by processing acrylic fibers, as well as water-absorbent resins such as polyacrylic acid, polyaspartic acid, and starch-acrylonitrile. The proportion of the water-absorbent resin in the absorbent, which is a water-soluble polymer in which acidic groups have been introduced into starch or its partial hydrolyzates, is preferably 35% by weight or more, more preferably 40% by weight or more, for disposable diapers. For napkins, it is preferably 5% by weight or more, more preferably 10% by weight or more. For both disposable diapers and napkins, the upper limit is not particularly limited, and is 100% by weight or less.
[0104] When the absorbent contains hydrophilic fibers, the content thereof is preferably 10 to 500 parts by weight, more preferably 20 to 300 parts by weight, per 100 parts by weight of the water-absorbent resin.
[0105] <Recycled Water-Soluble Polymer> The recycled water-soluble polymer can be obtained by treating the absorbent article or the water-absorbent resin contained in the absorbent article with alkali. During the alkali treatment, the absorbent article or the water-absorbent resin contained in the absorbent article is kept at a pH of preferably 9.0 or higher, more preferably 10.0 or higher. The alkali treatment cleaves the cross-linked structure and glycoside bonds of the water-absorbent resin, decomposing it into a water-soluble polymer, thereby reducing the environmental impact at the time of disposal.
[0106] The alkaline agent used in the alkaline treatment is not particularly limited, but examples include sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, sodium carbonate, and potassium carbonate. When the alkaline treatment is carried out using an alkaline aqueous solution, the concentration of the alkaline agent in the aqueous solution is preferably 0.01 to 20% by weight, more preferably 0.1 to 5% by weight. The temperature during the alkaline treatment is not particularly limited, but the treatment can be carried out, for example, under conditions of 5 to 70°C. The alkaline treatment time is preferably 1 to 120 minutes. After the alkaline treatment, the regenerated water-soluble polymer may be neutralized by adding an acid, concentrated, washed, filtered, or the like, as necessary. The regenerated water-soluble polymer preferably has the molecular weight, dispersity, total acid number, free acid number, and dispersity described above for the water-soluble polymer.
[0107] A water-absorbent resin can be obtained by crosslinking a recycled water-soluble polymer. The crosslinking method and crosslinking structure of the recycled water-soluble polymer are preferably the same as those described above for the water-soluble polymer. The water-absorbent resin obtained by crosslinking a recycled water-soluble polymer preferably has the physical properties of the water-absorbent resin described above. The water-absorbent resin obtained by crosslinking a recycled water-soluble polymer preferably has the absorbency under no pressure for ion-exchanged water, the water retention rate for ion-exchanged water, the absorbency under no pressure for physiological saline, and the water retention rate for physiological saline, each of which is preferably 60 to 140%, more preferably 80 to 120%, even more preferably 90 to 110%, and particularly preferably 95 to 105%, of the same absorbency properties of a water-absorbent resin obtained by crosslinking a non-recycled water-soluble polymer.
[0108] The water-absorbent resin obtained by crosslinking the recycled water-soluble polymer can be used to obtain absorbent articles, the structure and uses of which are as described above.
[0109] <Method for recovering hydrophilic fibers> The method for recovering hydrophilic fibers of the present invention is a method for recovering hydrophilic fibers from an absorbent article containing hydrophilic fibers and a water-absorbent resin made of a water-soluble polymer in which an acidic group has been introduced into starch or a partial hydrolyzate thereof, and is characterized by including a step of treating a part or all of the water-absorbent article with alkali to decompose the water-absorbent resin.
[0110] The water-absorbent resin, hydrophilic fiber, and absorbent article can be those described above. In the process of decomposing the water-absorbent resin, the target of the alkali treatment may be the entire water-absorbent article, or it may be only a portion of the water-absorbent article. When a portion of the water-absorbent article is alkali-treated, the target of the treatment includes the water-absorbent resin and hydrophilic fiber. The alkali treatment conditions described for the recycled water-soluble polymer can be used. By alkali-treating a portion or the entire water-absorbent article, the water-absorbent resin is decomposed and dissolved, and hydrophilic fiber is obtained as a solid residue. The hydrophilic fiber obtained as a solid residue in the process of decomposing the water-absorbent resin is then dried and, if necessary, defibrated and defibrated, and can be used, like virgin pulp, to manufacture absorbent articles such as disposable diapers. In addition to water-absorbent articles, the recovered hydrophilic fiber can also be used for applications commonly used for hydrophilic fibers, such as industrial wipers, waste liquid absorbents, and filters.
[0111] The present invention will be described below with reference to examples, but is not limited to the following examples. Hereinafter, "parts" and "%" mean "parts by weight" and "% by weight", respectively, unless otherwise specified.
[0112] (1) Materials used (1-1) Starch raw materials Corn starch Waxy corn starch Tapioca
[0113] (1-2) Hydrolases α-amylase (Spitase (registered trademark) HK / R, manufactured by Nagase ChemteX Corporation), 12,200 units / g amylomaltase: Thermus thermophilus was aerobically cultured, and the collected cells were disrupted and the extract was centrifuged, and the supernatant was used as a crude enzyme solution. The crude enzyme solution was subjected to column chromatography in a conventional manner, and a sample purified to an electrophoretically homogeneous state was used as a purified enzyme solution.
[0114] The activity of amylomaltase was measured as follows: A reaction solution containing 10% by weight maltotriose, 50 mM sodium acetate buffer (pH 6.0), and the enzyme was incubated at 60°C for 20 minutes. The reaction was then stopped by heating at 100°C for 10 minutes. The amount of glucose in the reaction solution was measured by the glucose oxidase method. The unit amount of amylomaltase was defined as 1 unit of amylomaltase activity that produces 1 μmol of glucose per minute.
[0115] (2) Production of Partial Starch Hydrolysates (Production Examples 1 to 6) Partial starch hydrolysates were produced by the following method. The weight-average molecular weights of the obtained partial starch hydrolysates were determined by aqueous size exclusion chromatography based on a calibration curve of molecular weight and elution time prepared using pullulan with a known molecular weight. The weight-average molecular weights and dispersities of the partial starch hydrolysates are shown in Table 1.
[0116] (Production Example 1) Cornstarch-Derived Partial Starch Hydrolysate Cornstarch was suspended in city water to a concentration of 30% by weight, and then a 1N aqueous solution of sodium hydroxide was added to adjust the pH to 6.0 to obtain starch milk. To this starch milk, an amylomaltase crude enzyme solution was added at 2.0 units per gram of starch solids, and the mixture was stirred at room temperature for 30 minutes, followed by reaction at 80°C for 6 hours with stirring to prepare liquefied starch. The resulting partial starch hydrolysate had a weight-average molecular weight of 6,000,000 and a dispersity of 30.2.
[0117] (Production Example 2) Cornstarch-Derived Partial Starch Hydrolysate Cornstarch was suspended in city water to a concentration of 30% by weight, and then a 1N aqueous solution of sodium hydroxide was added to adjust the pH to 6.0 to obtain starch milk. To this starch milk, an amylomaltase crude enzyme solution was added in an amount of 0.1 units per gram of starch solids, and the mixture was stirred at room temperature for 30 minutes, followed by reaction at 90°C for 4.5 hours with stirring to prepare liquefied starch. The weight-average molecular weight of the resulting partial starch hydrolysate was 2,260,000, and the dispersity was 14.9.
[0118] (Production Example 3) Tapioca-derived partial starch hydrolysate Tapioca was adjusted to a concentration of 15 wt %, and an amylomaltase crude enzyme solution was added at 0.1 units per gram of starch solids, followed by stirring at room temperature for 30 minutes and then reacting with stirring at 80°C for 4 hours to prepare liquefied starch. The resulting partial starch hydrolysate had a weight-average molecular weight of 1,180,000 and a dispersity of 22.6.
[0119] (Production Example 4) Tapioca-derived partial starch hydrolysate Liquefied starch was prepared by the same procedure as in Production Example 3, except that the reaction time was changed to 12 hours. The weight-average molecular weight of the obtained partial starch hydrolysate was 440,000 and the dispersity was 17.3.
[0120] (Production Example 5) Partial Starch Hydrolysate Derived from Waxy Cornstarch Waxy cornstarch was suspended in city water to a concentration of 15% by weight, and then a 1N aqueous solution of sodium hydroxide was added to adjust the pH to 6.0 to obtain a starch milk. α-Amylase was added to this starch milk at 0.5 units per gram of starch solids, and the mixture was stirred at room temperature for 30 minutes, followed by a reaction at 100°C for 20 minutes with stirring to prepare a liquefied starch. The resulting partial starch hydrolysate had a weight-average molecular weight of 610,000 and a dispersity of 35.2. The aqueous solution of the partial starch hydrolysate was vacuum-dried at 80°C, and the resulting dried product was pulverized to obtain a dry powder with a 1 mm pass filter. The moisture content of the dry powder was 4.8%.
[0121] (Production Example 6) Cornstarch-derived starch partial hydrolyzate Cornstarch was suspended in city water to a concentration of 30% by weight, and then a 1N aqueous solution of sodium hydroxide was added to adjust the pH to 6.0 to obtain starch milk. To this starch milk, an amylomaltase crude enzyme solution was added at 0.2 units per gram of starch solids, and the mixture was stirred at room temperature for 30 minutes, followed by reaction at 90°C for 4.5 hours with stirring to prepare liquefied starch. The resulting partial starch hydrolyzate had a weight-average molecular weight of 1,910,000 and a dispersity of 10.1.
[0122]
[0123] (3) Production of Water-Soluble Polymer (Production Example 7) 140 g of the 30 wt % aqueous solution of the starch partial hydrolysate produced in Production Example 1 (0.78 mol of hydroxyl groups in the starch partial hydrolysate) was charged into a 500 ml separable flask equipped with a stirrer, thermometer, and condenser. Next, 37.6 g of a 48.8% aqueous solution of sodium hydroxide (0.46 mol, 0.59 equivalents relative to the hydroxyl groups in the starch partial hydrolysate) was charged, and the solution was stirred at 60°C or below until it became completely homogeneous. After confirming that the solution was homogeneous, an aqueous solution prepared by dissolving 20.6 g of monochloroacetic acid (0.44 mol, 0.8 equivalents relative to the hydroxyl groups in the starch partial hydrolysate) in 5.2 g of ion-exchanged water was added dropwise at 50-60°C over 30 minutes. After charging the aqueous monochloroacetic acid solution, the temperature was adjusted to 45-50°C, and the mixture was stirred for 12 hours. The reaction was terminated when the chloride ion content in the reaction solution was measured by potentiometric titration using a 0.01 N silver nitrate solution, and reached 98% or more of the calculated chloride ion content of 3.8% when all the monochloroacetic acid had reacted. In this production example, the chloride content was 3.75%.
[0124] After the reaction was completed, the reaction solution was diluted with 600 g of ion-exchanged water. The diluted reaction solution was cooled to room temperature and added to 5,000 ml of methanol over approximately 30 minutes to precipitate and reprecipitate the water-soluble polymer. After the entire reaction solution was added, the mixture was stirred for 30 minutes, and the water-soluble polymer dispersed in the methanol was subjected to solid-liquid separation by vacuum filtration.
[0125] Subsequently, in order to remove sodium chloride contained in the water-soluble polymer, the recovered water-soluble polymer was redispersed in 1000 ml of aqueous methanol (methanol / water 80 / 20 (volume ratio)), stirred at room temperature for 30 minutes, washed, and then subjected to solid-liquid separation by vacuum filtration, and the water-soluble polymer was recovered again. The chlorine content of the recovered water-soluble polymer was measured by potentiometric titration using a 0.01 N aqueous silver nitrate solution, and the washing process was repeated until the chlorine content was less than 1%. The total acid number of the obtained water-soluble polymer was 128 mg KOH / g, the degree of etherification calculated from the total acid number was 0.45, the weight average molecular weight was 30,310,000, and the dispersity was 25.7.
[0126] (Production Example 8) 200 g of the 30 wt % aqueous solution of the partial starch hydrolysate produced in Production Example 2 (1.11 mol of hydroxyl groups in the partial starch hydrolysate) was charged into a 500 ml separable flask equipped with a stirrer, thermometer, and condenser. Next, 79.4 g of a 48.8% aqueous solution of sodium hydroxide (0.96 mol, 0.86 equivalents relative to the hydroxyl groups in the partial starch hydrolysate) was charged, and the solution was stirred at 60°C or below until it became completely homogeneous. After confirming that the solution was homogeneous, 89.9 g of 6-bromohexanoic acid crystals (0.46 mol, 0.4 equivalents relative to the hydroxyl groups in the partial starch hydrolysate) were added in small portions over 30 minutes at 50-60°C. After the addition of 6-bromohexanoic acid, the temperature was adjusted to 45-50°C, and the mixture was stirred for 10 hours. The reaction was terminated when the bromide ion content in the reaction solution was measured by potentiometric titration using a 0.01 N aqueous solution of silver nitrate, and reached 98% or more of the calculated bromide ion content of 9.8% when all 6-bromohexanoic acid had reacted. In this production example, the bromine content was 10.1%.
[0127] After the reaction was completed, the reaction solution was diluted with 250 g of ion-exchanged water. The diluted reaction solution was cooled to room temperature and added to 1600 ml of ethanol over approximately 30 minutes to precipitate and reprecipitate the water-soluble polymer. After the entire reaction solution was added, the mixture was stirred for 30 minutes, and the water-soluble polymer dispersed in the ethanol was subjected to solid-liquid separation by vacuum filtration.
[0128] Subsequently, to remove sodium bromide contained in the water-soluble polymer, the recovered water-soluble polymer was redispersed in 500 ml of aqueous ethanol (ethanol / water 90 / 10 (volume ratio)), stirred at room temperature for 30 minutes, washed, and then subjected to solid-liquid separation by vacuum filtration, and the water-soluble polymer was recovered again. The bromine content of the recovered water-soluble polymer was measured by potentiometric titration using a 0.01 N aqueous silver nitrate solution, and the washing process was repeated until the bromide ion content was less than 1%. The total acid number of the obtained water-soluble polymer was 133 mg KOH / g, the degree of etherification calculated from the total acid number was 0.55, the weight-average molecular weight was 10,420,000, and the dispersity was 24.7.
[0129] (Production Example 9) 200 g of the 30 wt % aqueous solution of the starch partial hydrolysate produced in Production Example 3 (1.11 mol of hydroxyl groups in the starch partial hydrolysate) was charged into a 500 ml separable flask equipped with a stirrer, thermometer, and condenser. Next, 47.8 g of a 48.8% aqueous solution of sodium hydroxide (0.58 mol, 1.1 equivalents relative to the hydroxyl groups in the starch partial hydrolysate) was charged, and the solution was stirred at 60°C or below until it became completely homogeneous. After confirming that the solution was homogeneous, an aqueous solution prepared by dissolving 77.7 g of sodium monochloroacetate (0.67 mol, 1.2 equivalents relative to the hydroxyl groups in the starch partial hydrolysate) in 111 g of water was added in small portions over 30 minutes at 50-60°C. After the addition of the aqueous sodium monochloroacetate solution, the temperature was adjusted to 90-95°C, and the mixture was stirred for 5 hours. The reaction was terminated when the chloride ion content in the reaction solution was measured by potentiometric titration using a 0.01 N silver nitrate solution, and reached 98% or more of the calculated chloride ion content of 5.4% when all the sodium monochloroacetate had reacted. In this production example, the chloride content was 5.3%.
[0130] After the reaction was completed, the reaction mixture was cooled to room temperature and added to 2000 ml of methanol over about 30 minutes to precipitate and reprecipitate the water-soluble polymer. After the entire reaction mixture was added, the mixture was stirred for 30 minutes, and the water-soluble polymer dispersed in the methanol was subjected to solid-liquid separation by filtration under reduced pressure.
[0131] Subsequently, in order to remove the sodium chloride contained in the water-soluble polymer, the recovered water-soluble polymer was redispersed in 1000 ml of methanol, stirred at room temperature for 30 minutes, washed, and then subjected to solid-liquid separation by vacuum filtration, and the water-soluble polymer was recovered again. The chlorine content of the recovered water-soluble polymer was measured by potentiometric titration using a 0.01 N aqueous silver nitrate solution, and the washing process was repeated until the chloride ion content was less than 1%. The total acid number of the obtained water-soluble polymer was 152 mg KOH / g, the degree of etherification calculated from the total acid number was 0.56, the weight-average molecular weight was 8,680,000, and the dispersity was 18.3.
[0132] (Production Example 10) A water-soluble polymer was obtained by carrying out the reaction and post-treatment in the same manner as in Production Example 9, except that the starch partial hydrolyzate was changed to the starch partial hydrolyzate produced in Production Example 4. The total acid value of the obtained water-soluble polymer was 148 mg KOH / g, the degree of etherification calculated from the total acid value was 0.54, the weight-average molecular weight was 3,070,000, and the dispersity was 9.5.
[0133] (Production Example 11) 50 g of the powder of the partial starch hydrolysate (water content: 4.8%) produced in Production Example 5 (0.88 mol of hydroxyl groups in the partial starch hydrolysate) and 140 g of water were charged into a 1000 ml separable flask equipped with a stirrer, thermometer, and condenser. Next, 94.7 g of a 48.8% aqueous solution of sodium hydroxide (1.2 mol, 1.3 equivalents relative to the hydroxyl groups in the partial starch hydrolysate) was charged, and the mixture was stirred at 60°C or below until the solution became completely homogeneous. After confirming that the solution was homogeneous, an aqueous solution of 154 g of sodium monochloroacetate (1.3 mol, 1.5 equivalents relative to the hydroxyl groups in the partial starch hydrolysate) in 300 g of water was added in small portions over 30 minutes at 50-60°C. After the addition of the aqueous sodium monochloroacetate solution, the temperature was adjusted to 90-95°C, and the mixture was stirred for 5 hours. The reaction was terminated when the chloride ion content in the reaction solution was measured by potentiometric titration using a 0.01 N silver nitrate aqueous solution, and reached 98% or more of the calculated chloride ion content of 6.3% when all the sodium monochloroacetate had reacted. In this production example, the chloride content was 6.3%.
[0134] After the reaction was completed, the reaction mixture was cooled to room temperature and added to 5,000 ml of methanol over about 30 minutes to precipitate and reprecipitate the water-soluble polymer. After the entire reaction mixture was added, the mixture was stirred for 30 minutes, and the water-soluble polymer dispersed in the methanol was subjected to solid-liquid separation by filtration under reduced pressure.
[0135] Subsequently, in order to remove the sodium chloride contained in the water-soluble polymer, the recovered water-soluble polymer was redispersed in 2000 ml of methanol, stirred at room temperature for 30 minutes, washed, and then subjected to solid-liquid separation by vacuum filtration, and the water-soluble polymer was recovered again. The chlorine content of the recovered water-soluble polymer was measured by potentiometric titration using a 0.01 N aqueous silver nitrate solution, and the washing process was repeated until the chloride ion content was less than 1%. The total acid number of the obtained water-soluble polymer was 192 mg KOH / g, the degree of etherification calculated from the total acid number was 0.76, the weight-average molecular weight was 2,300,000, and the dispersity was 22.3.
[0136] (Production Example 12) An aqueous polymer was obtained by carrying out the reaction and post-treatment in the same manner as in Production Example 7, except that the starch partial hydrolyzate was changed to 140 g of the partial starch hydrolyzate produced in Production Example 6, the amount of 48.8% sodium hydroxide aqueous solution was changed to 55.6 g (0.68 mol, 0.87 equivalents relative to the hydroxyl groups of the partial starch hydrolyzate), the amount of monochloroacetic acid was changed to 30.5 g (0.32 mol, 0.4 equivalents relative to the hydroxyl groups of the partial starch hydrolyzate), and the amount of ion-exchanged water for dissolving the monochloroacetic acid was changed to 8 g. The total acid value of the obtained water-soluble polymer was 137 mg KOH / g, the degree of etherification calculated from the total acid value was 0.49, the weight-average molecular weight was 11,890,000, and the dispersity was 15.3.
[0137] (4) Production of water-absorbent resin (Production Example 13) 170 g of the water-soluble polymer obtained in Production Example 7 (wet product of hydrous methanol, wet ratio 69%) was placed in a 1000 ml beaker, and 550 ml of hydrous methanol with a methanol / water ratio of 80 / 20 (volume ratio) was added to disperse the water-soluble polymer. While stirring with a magnetic stirrer, 5.8 ml of 1N hydrochloric acid aqueous solution was gradually added with a measuring pipette. After adding hydrochloric acid, the mixture was stirred for 15 minutes and subjected to vacuum suction filtration to recover a water-soluble polymer that was partially neutralized to free acid. The recovered water-soluble polymer was wet crystals containing hydrous alcohol. The wet crystals were transferred to a petri dish, placed in a blower dryer set at 70 ° C., dried for 20 hours, and subjected to a crosslinking treatment. The solid obtained after the treatment was crushed in a mortar and sieved using sieves with openings of 150 μm and 850 μm to recover water-absorbent resin particles with particle sizes of 150 to 850 μm.
[0138] (Production Example 14) 170 g of the water-soluble polymer obtained in Production Example 8 (wet product with aqueous ethanol, wet ratio 61%) was placed in a 1000 ml beaker, and 500 ml of ethanol was added to disperse the water-soluble polymer. While stirring with a magnetic stirrer, 82.2 ml of a 1N aqueous hydrochloric acid solution was gradually added using a measuring pipette. After the addition of hydrochloric acid, the mixture was stirred for 15 minutes and subjected to vacuum suction filtration to recover a water-soluble polymer that had been partially neutralized to free acid. The recovered water-soluble polymer was wet crystals containing aqueous alcohol. The wet crystals were transferred to a petri dish, placed in a blower dryer set at 150 °C, dried for 1 hour, and subjected to a crosslinking treatment. The solid obtained after the treatment was pulverized in a mortar and sieved using sieves with openings of 150 μm and 850 μm, and water-absorbent resin particles with particle sizes of 150 to 850 μm were recovered.
[0139] (Production Examples 15 to 21) Water-absorbent resins were obtained by the same procedure as in Production Example 13, except that the raw materials and amounts thereof were changed as shown in Table 2.
[0140]
[0141] Comparative Production Example 1: Preparation of a water-absorbent resin composed of sodium polyacrylate. 155 parts by mass (2.15 mol parts) of acrylic acid, 0.62 parts by mass (0.0024 mol parts) of pentaerythritol triallyl ether as an internal crosslinker, and 340.27 parts by mass of deionized water were stirred and mixed while maintaining the temperature at 1°C. Nitrogen was introduced into the mixture to reduce the dissolved oxygen content to 0.1 ppm or less, and then 0.31 parts by mass of a 1% by mass aqueous solution of hydrogen peroxide, 1.16 parts by mass of a 1% by mass aqueous solution of ascorbic acid, and 2.325 parts by mass of a 0.5% by mass aqueous solution of 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide] were added and mixed to initiate polymerization. After the temperature of the mixture reached 85°C, polymerization was carried out at 85±2°C for approximately 10 hours to obtain a hydrogel. Next, 502.27 parts by mass of this hydrogel was shredded with a mincer (manufactured by ROYAL, "12VR-400K"), and 128.42 parts by mass of a 48.5% by mass aqueous solution of sodium hydroxide was added and mixed, and 3 parts by mass of a 1% by mass aqueous solution of ethylene glycol diglycidyl ether was added and mixed to obtain a shredded gel. The shredded gel was then dried in a ventilated band dryer {200 ° C., air speed 5 m / sec} to obtain a dried body. The dried body was pulverized in a juicer mixer (manufactured by Oster, "OSTERIZERBLENDER") and then adjusted to a particle size of 150 μm to 710 μm using sieves with openings of 150 μm and 710 μm, to obtain dried particles.
[0142] (5) Production of Disposable Diapers (Examples 1 to 7) 4 g of water-absorbent resin and 5 g of crushed wood pulp were mixed in a batch-type air paper-making machine, and a 100 mm x 133 mm water-absorbent resin / pulp mixed absorbent material (with a pulp basis weight of 0.0375 g / cm 2 , water-absorbent resin basis weight 0.03 g / cm 2 ) was prepared. The top and bottom of the water-absorbent resin / pulp mixed absorbent body were sandwiched between tissue paper and pressed 10 times with a 15 kg roller to obtain an absorbent layer. The absorbent layer was sandwiched between a thermal bond nonwoven fabric (18 gsm) and a polyethylene sheet, and the periphery was fixed with packing tape to prepare a disposable diaper sample. The water-absorbent resins used are shown in Table 3.
[0143] Comparative Example 1 A disposable diaper was produced in the same manner as in Examples 1 to 7, except that the water-absorbing resin of Comparative Production Example 1 was used as the water-absorbing resin.
[0144] The absorption rate, return amount, and diffusion length of the disposable diapers were measured by the methods described below. The results are shown in Table 3.
[0145] In Examples 1 to 7, the absorption rate, return amount, and diffusion length were all sufficient for practical use in disposable diapers. In some Examples, the performance was significantly superior to that of Comparative Example 1, which used conventional sodium polyacrylate.
[0146] (6) Production of napkins (Examples 8 to 10) A batch-type air papermaking machine was used to produce a 50 mm x 70 mm absorbent body made of water-absorbent resin (basis weight of water-absorbent resin: 0.0143 g / cm 2 The absorbent body was sandwiched between tissue paper sheets and pressed 10 times with a 15 kg roller to obtain an absorbent layer. The absorbent layer was sandwiched between polyethylene sheets and fixed around the edges with packing tape to prepare a napkin sample. The water-absorbent resins used are shown in Table 4.
[0147] Comparative Example 2 A napkin was produced in the same manner as in Examples 8 to 10, except that the water-absorbent resin of Comparative Production Example 1 was used as the water-absorbent resin.
[0148] The absorption rate, return amount, absorption amount and water retention capacity of the napkins were measured by the methods described below. The results are shown in Table 4.
[0149] In Examples 8 to 10, the absorption rate, return amount, absorption amount, and water retention capacity all exceeded those of Comparative Example 2, which used conventional sodium polyacrylate.
[0150] (7) Evaluation Method of Water-Soluble Polymers (7-1) Total Acid Number of Water-Soluble Polymers Approximately 0.3 g of water-soluble polymer was weighed into a 100 ml beaker and dissolved in 40 ml of ion-exchanged water. This aqueous solution was placed in a potentiometric titrator (AT-610, manufactured by Kyoto Electronics Manufacturing Co., Ltd.) equipped with a glass electrode (C-171, manufactured by Kyoto Electronics Manufacturing Co., Ltd.). If the sample was entirely sodium salt, the potential at this stage would be approximately 30 mV or less. A 1N aqueous hydrochloric acid solution was added until the potential reached 320 mV or more, converting all carboxylic acid groups in the water-soluble polymer into a free acid state (resulting in an excess of hydrochloric acid). After confirming that the potential was 320 mV or more, neutralization titration was performed with a 0.1 N aqueous sodium hydroxide solution. In this titration, two inflection points were detected: the first inflection point was detected near 220 mV, and the second inflection point was detected near 0 to -30 mV. The former is the neutralization point of excess hydrochloric acid in the sample, and the latter is the neutralization point of carboxylic acid in the water-soluble polymer. Therefore, the total acid number is calculated by the following formula 1: Total acid number (mg KOH / g) = [{(Vb - Va) x 0.1 x fa x 56.11} / Sa] / (1 - wr) (Formula 1) where Va is the volume (ml) of 0.1 N sodium hydroxide aqueous solution consumed up to the first inflection point, Vb is the volume (ml) of 0.1 N sodium hydroxide aqueous solution consumed up to the second inflection point, fa is the titer of the 0.1 N sodium hydroxide aqueous solution, and Sa is the amount of sample collected. wr is the wet ratio of the water-soluble polymer measured by the method described below.
[0151] (7-2) Wet Ratio of Water-Soluble Polymer The wet ratio refers to the percentage of weight loss relative to the initial weight of a sample when the sample is dried at a drying temperature of 130°C using a halogen moisture meter. In this example, 0.5 to 1.0 g of the water-soluble polymer was set in a halogen moisture meter HC103 manufactured by Mettler Toledo K.K., and measurement was performed at a drying temperature of 130°C, a switch-off standard of 1 mg / 50 seconds, and in % MC mode (a mode in which the MC value = (initial sample weight - dry weight) ÷ initial sample weight × 100) . The displayed MC value was the wet ratio.
[0152] (7-3) Degree of Etherification of Water-Absorbent Resin Degree of Etherification=(162×TAV)÷(56100−80×TAV) Here, TAV is the total acid value (unit: mgKOH / g) of the water-soluble polymer.
[0153] (8) Evaluation Method of Disposable Diapers (8-1) Absorption Rate A disposable diaper is placed on a horizontal surface with the top sheet facing up, and an acrylic plate (weight 200 g) with a measurement cylinder is placed in the center, and 25 g of saline solution (salt concentration 0.9 wt%) is poured into the central cylinder at once. The time required for the saline solution in the cylinder to be absorbed into the disposable diaper is measured and taken as the absorption rate.
[0154] (8-2) Amount of Backflow After the absorption rate test, leave it for 5 minutes, then remove the acrylic plate with the measurement tube, place about 20 g of filter paper (weigh it precisely and call it W1 (g)) on it, and then place a 3.5 kg weight on it and apply pressure for 3 minutes. After 3 minutes, remove the filter paper and measure its weight (W2 (g)). Calculate the amount of backflow using the following formula: Amount of backflow (g) = W2 - W1
[0155] (8-3) Diffusion Length Repeat the steps of (8-1) Absorption rate and (8-2) Backflow amount two more times for a total of three measurements. Measure the spreading length (maximum length) of the saline solution on the disposable diaper.
[0156] (9) Evaluation method for napkins (9-1) Absorption capacity A napkin was soaked in 1000 ml of milk without stirring for 1 hour, and then hung up for 10 minutes to drain. The weight (h5) was measured and the absorption capacity was calculated using the following formula. The temperature of the milk used and the measurement atmosphere was 25°C ± 2°C. Absorption capacity (g / sheet) = (h5) - (h6) where (h6) is the weight of the napkin before soaking.
[0157] (9-2) Water retention capacity After the absorption capacity test, the sheet was placed in a centrifuge and centrifuged at 150 G for 120 seconds to remove excess milk. The weight (h7) was measured and the water retention capacity was calculated using the following formula: Water retention capacity (g / sheet) = (h7) - (h6)
[0158] (9-3) Absorption rate: The napkin is placed on a horizontal surface with the top sheet facing up, and a cylindrical acrylic measuring tool (weight: 200 g) is placed in the center. 5 g of milk is poured into the central cylinder at once. The time required for the milk in the cylinder to be absorbed into the napkin is measured and used as the absorption rate.
[0159] (9-4) Amount of Backflow After the absorption rate test, leave it for 5 minutes, then remove the cylindrical acrylic jig used for measurement, place about 20 g of filter paper (weigh it precisely and call it W1 (g)) on it, and then place a 0.5 kg weight on it and apply pressure for 3 minutes. After 3 minutes, remove the filter paper and measure its weight (W2 (g)). Calculate the amount of backflow using the following formula: Amount of backflow (g) = W2 - W1
[0160] (10) Decomposition and Regeneration of Water-Absorbent Resin (10-1) Production of Disposable Diapers (10-1-1) Production of Tapioca-Derived Starch Partial Hydrolyzate (Production Example 22) Tapioca starch was suspended in city water to a concentration of 30% by weight, and then a 1N aqueous solution of sodium hydroxide was added to adjust the pH to 6.0 to obtain starch milk. To this starch milk, an amylomaltase crude enzyme solution was added so as to give 8.0 units per gram of starch solids, and the mixture was stirred at room temperature for 30 minutes, followed by reaction at 80°C for 5 hours with stirring to prepare liquefied starch. The weight-average molecular weight of the obtained starch partial hydrolyzate was 2,820,000, and the dispersity was 9.82.
[0161] (10-1-2) Preparation of Water-Soluble Polymer (Production Example 23) 140 g of a 30 wt % aqueous solution of the starch partial hydrolysate from Production Example 22 (0.78 mol of hydroxyl groups in the starch partial hydrolysate) was charged into a 500 ml separable flask equipped with a stirrer, thermometer, and condenser. Next, 37.6 g of a 48.8% aqueous solution of sodium hydroxide (0.46 mol, 0.59 equivalents relative to the hydroxyl groups in the starch partial hydrolysate) was charged, and the solution was stirred at 60°C or below until it became completely homogeneous. After confirming that the solution was homogeneous, an aqueous solution prepared by dissolving 20.6 g of monochloroacetic acid (0.44 mol, 0.8 equivalents relative to the hydroxyl groups in the starch partial hydrolysate) in 5.2 g of ion-exchanged water was added dropwise at 60-70°C over 30 minutes. After charging the aqueous monochloroacetic acid solution, the temperature was adjusted to 80-90°C, and the mixture was stirred for 1 hour. The reaction was terminated when the chloride ion content in the reaction solution was measured by potentiometric titration using a 0.01 N silver nitrate solution, and reached 98% or more of the calculated chloride ion content of 3.8% when all the monochloroacetic acid had reacted. In this production example, the chloride content was 3.81%.
[0162] After the reaction was completed, the reaction solution was diluted with 600 g of ion-exchanged water. The diluted reaction solution was cooled to room temperature and added to 5,000 ml of methanol over approximately 30 minutes to precipitate and reprecipitate the water-soluble polymer. After the entire reaction solution was added, the mixture was stirred for 30 minutes, and the water-soluble polymer dispersed in the methanol was subjected to solid-liquid separation by vacuum filtration.
[0163] Subsequently, in order to remove the sodium chloride contained in the water-soluble polymer, the recovered water-soluble polymer was redispersed in 1000 ml of aqueous methanol (methanol / water 80 / 20 (volume ratio)), stirred at room temperature for 30 minutes, washed, and then subjected to solid-liquid separation by vacuum filtration, and the water-soluble polymer was recovered again. The chlorine content of the recovered water-soluble polymer was measured by potentiometric titration using a 0.01 N silver nitrate aqueous solution, and the washing process was repeated until the chlorine content was less than 1%. The total acid number of the obtained water-soluble polymer was 131.7 mg KOH / g, the weight-average molecular weight was 9,420,000, and the dispersity was 15.3.
[0164] (10-1-3) Production of water-absorbent resin (Production Example 24) 170 g of the water-soluble polymer obtained in Production Example 23 (wet product with hydrous methanol, wet ratio 68%) was placed in a 1000 ml beaker, and 550 ml of hydrous methanol with a methanol / water ratio of 80 / 20 (volume ratio) was added to disperse the water-soluble polymer. While stirring with a magnetic stirrer, 10.5 ml of 1N aqueous hydrochloric acid solution was gradually added with a measuring pipette. After adding hydrochloric acid, the mixture was stirred for 15 minutes and subjected to vacuum suction filtration to recover a water-soluble polymer that was partially neutralized to free acid. The recovered water-soluble polymer was wet crystals containing hydrous alcohol. The wet crystals were transferred to a petri dish, placed in a blower dryer set at 70 ° C., dried for 20 hours, and subjected to a crosslinking treatment. The solid obtained after the treatment was crushed in a mortar and sieved using sieves with openings of 150 μm and 850 μm to recover water-absorbent resin particles with particle sizes of 150 to 850 μm.
[0165] Preparation of Water-Absorbent Resin Made of Sodium Polyacrylate (Comparative Preparation Example 2) 155 parts by mass (2.15 mol parts) of acrylic acid, 0.62 parts by mass (0.0024 mol parts) of pentaerythritol triallyl ether as an internal crosslinking agent, and 340.27 parts by mass of deionized water were stirred and mixed while maintaining the temperature at 1°C. Nitrogen was introduced into the mixture to reduce the dissolved oxygen content to 0.1 ppm or less, and then 0.31 parts by mass of a 1% by mass aqueous solution of hydrogen peroxide, 1.16 parts by mass of a 1% by mass aqueous solution of ascorbic acid, and 2.325 parts by mass of a 0.5% by mass aqueous solution of 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide] were added and mixed to initiate polymerization. After the temperature of the mixture reached 85°C, polymerization was carried out at 85±2°C for approximately 10 hours to obtain a hydrogel. Next, 502.27 parts by mass of this hydrogel was shredded with a mincer (manufactured by ROYAL, "12VR-400K"), and 128.42 parts by mass of a 48.5% by mass aqueous solution of sodium hydroxide was added and mixed, and 3 parts by mass of a 1% by mass aqueous solution of ethylene glycol diglycidyl ether was added and mixed to obtain a shredded gel. The shredded gel was then dried in a ventilated band dryer {200 ° C., air speed 5 m / sec} to obtain a dried body. The dried body was pulverized in a juicer mixer (manufactured by Oster, "OSTERIZERBLENDER") and then adjusted to a particle size of 150 μm to 710 μm using sieves with openings of 150 μm and 710 μm, to obtain dried particles.
[0166] (10-1-4) Production of Disposable Diaper (Example 11) 5.0 g of the water-absorbent resin obtained in Production Example 24 was placed on 5.0 g of a 10 x 40 cm pulp water-absorbent sheet, and the pulp water-absorbent sheet was folded in half to a size of 10 x 20 cm, to produce a water-absorbent resin / pulp mixed absorbent body. The top and bottom of the water-absorbent resin / pulp mixed absorbent body were sandwiched between tissue paper, and pressed back and forth 10 times with a 15 kg roller to obtain an absorbent layer. The absorbent layer was sandwiched between a top sheet (air-through nonwoven fabric (18 gsm)) and a back sheet (polyethylene sheet), and the periphery was secured with packing tape to prepare a disposable diaper sample.
[0167] (10-1-5) Production of disposable diaper (Comparative Example 3) A disposable diaper was produced in the same manner as in Example 11, except that the water-absorbent resin obtained in Comparative Production Example 2 was used instead of the water-absorbent resin obtained in Production Example 24.
[0168] (10-1-6) Absorption Capacity of Disposable Diapers 40 ml of saline solution was applied to the disposable diapers of Example 11 and Comparative Example 3 in three separate doses every 5 minutes, resulting in a total absorption of 120 ml. All disposable diapers were able to absorb a total of 120 ml of saline solution. The saline solution used and the temperature of the measurement atmosphere were 25°C ± 2°C.
[0169] (10-1-7) Water Retention Capacity of Disposable Diapers After the absorption capacity test, the disposable diapers were placed in a centrifuge and centrifuged at 150 G for 120 seconds to remove excess saline, and then weighed. The water retention capacity was calculated by subtracting the weight before water absorption from the measured weight. The result was 106.5 g / diaper for Example 11 and 111.9 g / diaper for Comparative Example 3.
[0170] (10-2) Decomposition of Water-Absorbent Resin (Production Example 25) After measuring the water retention capacity, the water-absorbent resin / pulp mixed absorbent body was removed from the disposable diaper of Example 11, and immersed in 1000 ml of an aqueous sodium hydroxide solution (concentration: 0.5 wt %) at 25°C ± 2°C for 30 minutes.
[0171] The solid residue of the absorbent body was washed with water and centrifugal dewatered, and then the ash content was measured in accordance with JIS P8251:2003 "Paper, paperboard and pulp -- Ash content test method -- 525°C combustion method." If all of the water-absorbent resin remains in the solid residue of the absorbent body, it is estimated that the ash content would be measured at about 6% due to the presence of sodium in the aqueous sodium hydroxide solution used in producing the water-soluble polymer.
[0172] For comparison, the ash content of virgin pulp was measured and found to be -0.7%. The theoretical ash content of virgin pulp is 0, and the measured value is presumed to be within the margin of error. In contrast, the measured ash content of the solid residue of the absorbent body was 0.8%, which was equivalent to that of virgin pulp. This result confirmed that the water-absorbent resin contained in the absorbent body was almost completely decomposed by the alkali treatment.
[0173] After immersing the water-absorbent resin / pulp mixed absorbent body in an aqueous sodium hydroxide solution, the decomposition product of the water-absorbent resin exists in the aqueous solution as a regenerated water-soluble polymer. The recovered regenerated water-soluble polymer was analyzed by GPC and IR, and the results are shown in Figures 1 and 2, comparing it with the unused water-soluble polymer obtained in Production Example 23. The molecular weight and dispersity are also shown in Table 5. As shown in Table 5 and Figures 1 and 2, the molecular weight distribution and chemical structure of the regenerated water-soluble polymer contained in the decomposition product of the water-absorbent resin were equivalent to those of the unused water-soluble polymer.
[0174] (10-3) Regeneration of water-absorbent resin from decomposition product Hydrochloric acid was added dropwise to an aqueous solution containing the regenerated water-soluble polymer derived from the decomposition product obtained in Production Example 25 (weight 427 g, solids content 1.4 wt%, alkali content 26.1 meg / g) to neutralize and adjust the pH to 7-8. Water was distilled off using an evaporator until the solids content reached 10 wt%. Reprecipitation was carried out in methanol, and 10.5 g of a wet product of the regenerated water-soluble polymer (solids content 39.6%, pure content 4.2 g) was recovered by vacuum suction filtration. 300 ml of aqueous methanol (methanol / water = 80 / 20 (volume ratio)) was added to the recovered wet product of the regenerated water-soluble polymer to disperse the regenerated water-soluble polymer. While stirring with a magnetic stirrer, 0.8 ml of 1N aqueous hydrochloric acid was gradually added using a measuring pipette. After the addition of hydrochloric acid, the mixture was stirred for 15 minutes and then subjected to vacuum suction filtration to recover the regenerated water-soluble polymer that had been partially neutralized to free acid. The recovered recycled water-soluble polymer was transferred to a petri dish, placed in a blower dryer set at 70°C, and dried for 20 hours to carry out a crosslinking treatment. The solid obtained after the treatment was pulverized in a mortar and sieved using sieves with openings of 150 μm and 850 μm, and water-absorbent resin particles with particle sizes of 150 to 850 μm were recovered. The water absorption properties of this water-absorbent resin and a water-absorbent resin produced from unused water-soluble polymer by the same method are shown in Table 6.
[0175]
[0176] As shown in Table 6, even when a water-absorbent resin was produced again from the recycled water-soluble polymer, which was a decomposition product of the water-absorbent resin, sufficient water-absorbing properties were obtained.
[0177] (10-4) Pulp Recovery (Production Examples 26 to 27, Comparative Production Examples 3 to 4) The solid residue (recovered pulp) of the absorbent body recovered from the alkali treatment of the absorbent body in Production Example 25 was dried at 120°C in a blower dryer and then defibrated. Using the defibrated recovered pulp or virgin pulp in combination with the absorbent resins shown in Table 7, disposable diapers with the same configuration as in Example 11 were produced, and the water absorption rate and return amount were evaluated. The results are shown in Table 7.
[0178]
[0179] As shown in Table 7, when recycled pulp was used, performance equivalent to that of virgin pulp was obtained. It was confirmed that recycled pulp can be used to manufacture absorbent articles in the same way as virgin pulp.
Claims
1. An absorbent article comprising a water-absorbent resin made of a water-soluble polymer in which acidic groups have been introduced into starch or its partial hydrolyzate.
2. The absorbent article of claim 1, wherein said acidic group is a carboxyalkyl group, a carboxyalkenyl group, or a sulfoalkyl group.
3. The absorbent article according to claim 1 or 2, wherein the starch or its partially hydrolyzed product has a weight average molecular weight (Mw) of 7.5 million or less and / or a dispersity (weight average molecular weight (Mw) / number average molecular weight (Mn)) of 5 or more.
4. The absorbent article according to any one of claims 1 to 3, wherein the weight average molecular weight (Mw) of the water-soluble polymer, calculated as pullulan by aqueous size exclusion chromatography analysis, is 500,000 to 40,000,000.
5. An absorbent article according to any one of claims 1 to 4, wherein the water-absorbent resin has the following characteristics: (a) a water absorption capacity of ion-exchanged water without pressure of 100 to 500 g / g, (b) a water retention rate of ion-exchanged water of 80 to 300 g / g, (c) a water absorption capacity of saline without pressure of 10 to 70 g / g, and / or (d) a water retention rate of saline of 5 to 60 g / g.
6. The absorbent article according to any one of claims 1 to 5, which is any one selected from the group consisting of hygiene products, medical products, food preservation products, civil engineering products, and agricultural and horticultural products.
7. The absorbent article according to claim 6, wherein the sanitary product is any one selected from the group consisting of disposable diapers, sanitary products, incontinence pads, nursing pads, portable toilets, and pet toilets.
8. The absorbent article according to claim 6, wherein the medical product is any one selected from the group consisting of a hemostatic sponge, a wound dressing, a wound healing material, a medical waste solidification agent, an ice pack, a carrier for a drug delivery system, and an artificial joint.
9. A regenerated water-soluble polymer obtained by treating the absorbent article according to any one of claims 1 to 5 with alkali.
10. A water-absorbent resin which is a crosslinked product of the recycled water-soluble polymer according to claim 9.
11. A water-absorbent article comprising the water-absorbent resin according to claim 10.
12. A method for recovering hydrophilic fibers from an absorbent article containing hydrophilic fibers and a water-absorbent resin made of a water-soluble polymer in which acidic groups have been introduced into starch or its partial hydrolyzate, the method comprising the step of treating a part or all of the absorbent article with alkali to decompose the water-absorbent resin.