AI Technical Summary
Conventional catalysts for hydrogenating carboxylic acids and carboxylic acid esters often produce unwanted by-products, such as C-C and C-O bond cleavage products, which reduce the yield of the desired alcohol and require complex purification processes.
A metal-supported catalyst comprising ruthenium, tin, and platinum, further supported with iron, chromium, and/or molybdenum, which suppresses the formation of by-products while maintaining high catalytic activity, specifically by controlling the active sites that cleave C-C and C-O bonds.
The catalyst significantly reduces the yield of by-products, improving the yield of the target alcohol and simplifying the purification process, making it suitable for industrial applications like resin synthesis.
Abstract
Description
Metal-supported catalyst, alcohol production method and hydrogenation method
[0001] The present invention relates to a supported metal catalyst, and more particularly to a supported metal catalyst capable of hydrogenating carboxylic acids and / or carboxylic acid esters with high selectivity, a method for producing alcohols using the supported metal catalyst, and a hydrogenation method.
[0002] As a catalyst for reducing carboxylic acids and / or carboxylic acid esters to the corresponding alcohols, catalysts have been proposed in which ruthenium, tin, and platinum are supported on a carrier and then reduced with hydrogen or the like (e.g., Patent Documents 1 and 2). This catalyst is an excellent catalyst, exhibiting high reaction activity and reaction selectivity in the hydrogenation of carboxylic acids and / or carboxylic acid esters. Patent Document 3 also discloses a catalyst in which iron is further supported on a reduction catalyst. More specifically, the document discloses a supported catalyst in which nitrates of iron, cobalt, and nickel are added to a reduction catalyst supported on ruthenium, platinum, and tin as the main metal components, and the catalyst is used to produce 1,4-cyclohexanedimethanol.
[0003] Japanese Patent Publication No. 2001-9277 International Publication No. 2015 / 178459 Chinese Patent No. 104722321
[0004] When hydrogenation reactions of carboxylic acids and / or carboxylic acid esters are carried out using the conventional catalysts described in Patent Documents 1 and 2, although the hydrogenation activity is high, by-products accompanied by cleavage of C-C bonds and C-O bonds are generated, resulting in a decrease in the yield of the target product and requiring precise operations to remove the by-products in some cases. The catalyst disclosed in Patent Document 3 suppresses the generation of by-products compared to the catalysts described in Patent Documents 1 and 2, but the degree of suppression is insufficient, and further improvement has been desired. In view of the above circumstances, an object of the present invention is to provide a catalyst that further reduces the yield of by-products while maintaining high catalytic activity.
[0005] The present inventors have discovered that a metal-supported catalyst comprising ruthenium, tin, and platinum supported on a carrier, and further comprising iron, chromium, and / or molybdenum, can significantly reduce the yield of by-products while maintaining high catalytic activity. Although the details are not clear, it is presumed that iron, chromium, and molybdenum exert an effect of selectively suppressing active sites on the catalyst that cleave C-C bonds and C-O bonds, rather than active sites that reduce carbonyls. The inventors have discovered that the above effect can be significantly exhibited by a combination of iron and chromium, a combination of iron and molybdenum, or a combination of the three components iron, chromium, and molybdenum.
[0006] The gist of the present invention is as follows. [1] A metal-supported catalyst used for the hydrogenation of carboxylic acids and / or carboxylic acid esters, comprising ruthenium, tin, and platinum supported on a support, wherein the metal-supported catalyst further supports iron, and chromium and / or molybdenum. [2] The metal-supported catalyst according to [1] above, wherein the amount of iron supported is 0.01% by mass or more and 4% by mass or less, and the total amount of chromium and / or molybdenum supported is 0.01% by mass or more and 2% by mass or less, relative to the total mass of the metal-supported catalyst. [3] The metal-supported catalyst according to [1] or [2] above, wherein the support is a carbonaceous support. [4] The metal-supported catalyst according to any one of [1] to [3] above, wherein the total amount of ruthenium, tin, platinum, iron, molybdenum, and chromium supported is 5% by mass or more, relative to the total mass of the metal-supported catalyst. [5] The metal-supported catalyst according to any one of [1] to [4] above, which is prepared via hydrogen reduction. [6] A method for producing an alcohol, comprising contacting a carboxylic acid and / or a carboxylic acid ester with the metal-supported catalyst according to any one of [1] to [5] above and reducing the carboxylic acid and / or the carboxylic acid ester to obtain an alcohol corresponding to the carboxylic acid and / or the carboxylic acid ester. [7] A method for hydrogenating a carboxylic acid and / or a carboxylic acid ester, comprising contacting the metal-supported catalyst according to any one of [1] to [5] above with the carboxylic acid and / or the carboxylic acid ester. [8] The method for producing an alcohol according to [6] above, wherein the carboxylic acid is 1,4-cyclohexanedicarboxylic acid and the carboxylic acid ester is an ester of 1,4-cyclohexanedicarboxylic acid.
[0007] According to the present invention, it is possible to provide a catalyst that maintains high catalytic activity while further reducing the yield of by-products, and a method for producing an alcohol from a carboxylic acid and / or a carboxylic acid ester, and a method for hydrogenating a carboxylic acid and / or a carboxylic acid ester, using the catalyst.
[0008] Hereinafter, embodiments of the present invention will be described in detail. However, the following description of the constituent elements is merely an example (typical example) of an embodiment of the present invention, and the present invention is not limited to these details and can be implemented in various modifications within the scope of the present invention. In this application, metals (ruthenium, tin, platinum, and other metals such as iron, which are used as needed) supported on a carrier are sometimes collectively referred to as "metal components." Furthermore, the term "metal-supported catalyst" refers to a catalyst in which the metal components are supported on a carrier, a catalyst in which the metal components have been subjected to a reduction treatment, or a catalyst in which the metal components have been further subjected to an oxidation stabilization treatment. Furthermore, the term "metal-supported catalyst" also refers to a catalyst in which a metal component is further supported on a "metal-supported catalyst" that has been subjected to such an oxidation stabilization treatment. Regarding metal-supported catalysts, the catalyst in the stage before the reduction treatment is sometimes referred to as a "metal-supported material."
[0009] [Metal-supported catalyst] The metal-supported catalyst of the present invention (hereinafter sometimes simply referred to as "the catalyst") is obtained by reducing a metal-supported material, in which the metal component is supported on a carrier, usually with a reducing gas. The metal-supported catalyst of the present invention also includes catalysts obtained by subjecting the reduced metal-supported catalyst to an oxidation treatment. Furthermore, catalysts to which a metal component is further added after these treatments are also included in the metal-supported catalyst.
[0010] The metal-supported catalyst of the present invention is a catalyst (hereinafter, sometimes referred to as a "reduction catalyst") containing ruthenium, tin, and platinum as essential elements, and further supports iron, chromium, and / or molybdenum. Specifically, the reduction catalyst may be a combination of iron and chromium, a combination of iron and molybdenum, or a three-component combination of iron, chromium, and molybdenum. By using a metal-supported catalyst of this configuration, it is possible to further reduce the yield of by-products associated with C-C bond and C-O bond cleavage while maintaining hydrogenation activity. For example, when 1,4-cyclohexanedicarboxylic acid is hydrogenated as a carboxylic acid, cyclohexanemethanol, which involves C-C cleavage, and 4-methylcyclohexanemethanol, which involves C-O cleavage, are produced as by-products along with the target product, 1,4-cyclohexanedimethanol, resulting in a decrease in the yield of the target product. In contrast, the use of the catalyst of the present invention effectively suppresses the production of by-products. In addition, the diol compound 1,4-cyclohexanedimethanol is often used as a resin raw material for polyesters, polyurethanes, etc., and in this case, monoalcohols such as cyclohexanemethanol and 4-methylcyclohexanemethanol act as polymerization terminators, so contamination during resin synthesis must be avoided and removal procedures are required. On the other hand, reducing the amount of by-products produced in the hydrogenation reaction has the advantage that the purification procedures for removing the monoalcohols can be simplified or skipped.
[0011] <Carrier> The carrier used in the present invention is not particularly limited as long as it has a large surface area and can support a metal component, and examples thereof include carbonaceous carriers such as activated carbon and carbon black; inorganic porous carriers such as alumina, silica, diatomaceous earth, zirconia, titania, and hafnia; silicon carbide, gallium nitride, etc. Among these, carbonaceous carriers such as activated carbon, graphite, titania, and zirconia are preferred, and carbonaceous carriers are more preferred in terms of excellent stability and industrial availability, and activated carbon is even more preferred in terms of a large surface area, excellent metal dispersibility, and easy enhancement of reaction activity. Note that one type of carrier may be used, or two or more types may be used in combination.
[0012] The support may be used as is, or may be pretreated to a form suitable for loading. For example, when a carbonaceous support is used, the carbonaceous support may be heat-treated with nitric acid before use, as described in JP-A-10-71332. This method improves the dispersibility of the metal components on the support, thereby improving the activity of the resulting catalyst. The shape and size of the support used in the present invention are not particularly limited, but when converted to a spherical shape, the average primary particle diameter is usually 50 μm or more and 5 mm or less, preferably 4 mm or less. The particle diameter is measured using the sieving test method described in JIS standard JIS Z8815.
[0013] The suitable particle size of the support varies depending on the reaction using the catalyst, and is therefore preferably adjusted according to the reaction. Specifically, when the reaction using the catalyst is a completely mixed reaction, the particle size of the support is usually 50 μm or more, preferably 100 μm or more, and usually 3 mm or less, preferably 2 mm or less. The smaller the particle size of the support, the higher the activity per unit mass of the resulting catalyst, which is preferable; however, if it is too small, it may be difficult to separate the catalyst from the reaction liquid. That is, a particle size of the support equal to or greater than the above lower limit is preferable in terms of reaction activity, and a particle size equal to or less than the above upper limit is preferable because it is easy to separate the catalyst from the reaction liquid. Note that when the shape of the support is not spherical, the volume of the support is determined and converted into the diameter of a spherical particle of the same volume.
[0014] When the reaction using the catalyst is a fixed bed reaction, the particle size of the carrier is usually 0.5 mm or more and 5 mm or less, preferably 4 mm or less, and more preferably 3 mm or less. If the particle size is above the lower limit, operation will not be difficult due to the pressure difference, and if the particle size is below the upper limit, sufficient reaction activity can be obtained.
[0015] <Metal Components> The metal-supported catalyst of the present invention is a catalyst in which ruthenium, tin, and platinum are supported on a carrier as essential elements, and the catalyst further supports iron, chromium, and / or molybdenum (hereinafter sometimes referred to as "other metals such as iron"). By additionally supporting iron and chromium and / or molybdenum, the generation of by-products can be further suppressed. The effect of suppressing the generation of by-products is enhanced by supporting iron and chromium and / or molybdenum. Furthermore, in addition to ruthenium, tin, platinum, iron, chromium, and molybdenum, the catalyst may further contain other metals as needed, as long as they do not adversely affect the reduction reaction or other reactions using the catalyst. Preferably, the catalyst contains at least one metal selected from metal species such as rhodium, tungsten, rhenium, barium, and boron, and more preferably contains rhenium. The raw materials for each metal component will be described later.
[0016] (Amount of Supported Metal Component) The amount of supported metal component in the present catalyst is not particularly limited and is determined for each metal. The amount of supported ruthenium, expressed as a mass ratio relative to the total mass of the metal-supported catalyst, is usually 1 mass% or more, preferably 3 mass% or more, usually 10 mass% or less, and preferably 8 mass% or less. Similarly, the amount of supported tin, expressed as a mass ratio relative to the total mass of the metal-supported catalyst, is usually 1 mass% or more, preferably 2 mass% or more, usually 15 mass% or less, and preferably 10 mass% or less. Similarly, the amount of supported platinum, expressed as a mass ratio relative to the total mass of the metal-supported catalyst, is usually 0.5 mass% or more, usually 7 mass% or less, and preferably 5 mass% or less. These ranges are preferred because they enhance the ability as a hydrogenation catalyst. The amounts of supported iron and chromium and / or molybdenum are preferably 0.01 mass% or more and 4 mass% or less, more preferably 2 mass% or less, respectively. By setting them within these ranges, the generation of by-products can be significantly reduced. That is, the amount of iron supported is preferably 0.01 mass% or more and 4 mass% or less, more preferably 0.01 mass% or more and 2 mass% or less. Regarding the amount of chromium and / or molybdenum supported, when either one is supported, the preferred range of the amount of each metal supported is 0.01 mass% or more and 4 mass% or less, more preferably 0.01 mass% or more and 2 mass% or less. When both chromium and molybdenum are supported, the total amount of both supported is preferably within the above-mentioned range. Furthermore, in order to fully obtain the by-product suppression effect of the combined use of iron and chromium, their composition ratio is not particularly limited as long as it is within the above-mentioned range, but for example, 100:1 to 1:100 is used, more preferably 10:1 to 1:10, and even more preferably 10:1 to 1:5. The same range is also preferred when iron and molybdenum are used in combination. On the other hand, chromium and molybdenum are more expensive than iron in terms of cost, so in this sense, it is preferable that they be less than iron.
[0017] The total amount of other metals, such as ruthenium, tin, platinum, and iron, supported relative to the total mass of the metal-supported catalyst is not particularly limited, but is usually 5% by mass or more, preferably 8% by mass or more, more preferably 10% by mass or more, and usually 40% by mass or less, preferably 30% by mass or less, and more preferably 20% by mass or less. The amount of supported metal is calculated by converting all of the supported metals into metal atoms. The size of the reduced metal-supported catalyst of the present invention is not particularly limited, but is basically the same as the size of the support. The amount of supported metal (hereinafter sometimes referred to as "metal") can be measured, for example, by the following method. The catalyst can be powdered and stirred to form a homogeneous state, and if necessary, formed into a disk, which can then be analyzed in its solid state by X-ray fluorescence analysis. Alternatively, the catalyst can be subjected to alkali fusion decomposition or microwave pressure decomposition to form a homogeneous solution, which can then be analyzed by ICP atomic emission spectroscopy (inductively coupled plasma atomic emission spectroscopy). Of these, ICP atomic emission spectrometry (inductively coupled plasma atomic emission spectrometry) is preferred because more accurate measurement results can be obtained by preparing a homogeneous solution.
[0018] <Catalyst Manufacturing Method> In the present invention, the catalyst manufacturing method includes a step of supporting the metal component on a support (hereinafter referred to as a metal supporting step), followed by a step of reducing the obtained metal-supported material with a reducing gas. Each step will be described below in order.
[0019] <<Metal Supporting Step>> The metal supporting step is a step of supporting the above-mentioned metal component on the above-mentioned support to obtain a metal-supported material. The method for supporting the metal component is not particularly limited, and known methods can be used. During the supporting step, a solution or dispersion of various metal compounds that serve as raw materials for the above-mentioned metal component can be used.
[0020] (Metal Supporting Method) The method of supporting a metal component on a carrier is not particularly limited, but various impregnation methods can usually be applied. For example, there are adsorption methods that utilize the adsorption force of metal ions on a carrier to adsorb metal ions below the saturated adsorption amount; equilibrium adsorption methods that immerse a carrier in a solution of metal ions above the saturated adsorption amount and remove excess solution; pore filling methods that add a metal ion solution in an amount equal to the pore volume of the carrier and adsorb it all on the carrier; incipient wetness methods that add a metal ion solution until it matches the water absorption amount of the carrier, and finish when the carrier surface is uniformly wet and there is no excess solution; evaporation to dryness methods that impregnate a carrier with a metal ion solution and evaporate the solvent while stirring; and spray methods that dry the carrier and spray the solution. Among the above methods, pore filling methods, incipient wetness methods, evaporation to dryness methods, and spray methods are preferred, and more preferred are pore filling methods, incipient wetness methods, and evaporation to dryness methods. By the above-mentioned method, ruthenium, tin, platinum, and other metal components such as iron can be supported in a relatively uniformly dispersed state.
[0021] The loading may be carried out by preparing a solution of all the metals to be loaded and then loading them all at once, or by splitting each metal into separate loadings. In the case of split loading, each metal may be loaded separately, or multiple metal solutions may be used for separate loading. In order to shorten the loading process, it is preferable to load all the metal solutions at once, or to separately load multiple metals. The timing of split loading is not particularly limited; multiple metals may simply be loaded in separate steps, or they may be loaded partway through the process up to hydrogen reduction, or they may be separately loaded on a metal-supported catalyst after hydrogen reduction.
[0022] (Metal Compound) The metal compound used for loading is not particularly limited and can be appropriately selected depending on the loading method. For example, halides such as chlorides, bromides, and iodides; mineral acid salts such as nitrates and sulfates; organic acid salts such as acetates; metal hydroxides, metal oxides, organometallic compounds, metal complexes, etc. can be used. Among these, halides, mineral acid salts, and organic acid salts are preferred, with halides and mineral acid salts being more preferred, and halides being even more preferred. Among halides, chlorides such as hydrochlorides are particularly preferred. Furthermore, it is preferable that at least one of the above metal compounds is a chloride, and it is more preferable that all of them are chlorides. The use of chlorides is thought to complex the metals in solution, resulting in uniform dispersion of each metal on the loaded support, thereby ensuring stable loading. Furthermore, the growth of alloy particles due to other metal components such as ruthenium, tin, platinum, and iron in the resulting catalyst is suppressed, improving activity and selectivity, as well as catalyst stability during the reaction.
[0023] More specifically, in the case of ruthenium, ruthenium chloride, ruthenium nitrosyl nitrate, tris(acetylacetonato)ruthenium, etc. may be mentioned. These ruthenium salts may be used alone or in combination of two or more. In the case of tin, specific examples include tin compounds such as tin(II) chloride, tin(IV) chloride, tin(II) acetate, tin(IV) acetate, dibutyltin dilaurate, dibutyltin oxide, and dibutyltin dimethoxide. Tin compounds may be used alone or in combination of two or more. In the case of platinum, a platinum precursor compound is used, and examples of the platinum precursor compound include hexachloroplatinic acid (hexahydrate, etc.), potassium tetrachloroplatinic acid (II), potassium hexachloroplatinic acid (IV), potassium tetracyanoplatinic acid (II), sodium hexachloroplatinic acid (IV) (hexahydrate), hydrogen hexahydroxyplatinic acid (IV), potassium tetracyanoplatinic acid (II) (hydrate), tetrabutylammonium hexachloroplatinic acid (IV), etc. One type of platinum precursor compound may be used alone, or two or more types may be used in combination.
[0024] Examples of other metal compounds such as iron include iron salts, chromium compounds, and molybdenum compounds, as exemplified below. The iron salt is preferably selected from the group consisting of iron chloride, iron nitrate, iron sulfate, and iron acetylacetonate. The chromium compound may be an inorganic acid salt such as chromium nitrate, chromium sulfate, or chromium chloride; an organic acid salt such as chromium acetate, chromium oxalate, or chromium acetylacetonate; or various compounds known to be used in the production of chromium oxide catalysts. The molybdenum compound is preferably a molybdenum compound containing oxidized molybdenum, such as molybdenum trioxide, molybdic acid, molybdates, and heteropolyacids. Among these, molybdenum trioxide and molybdates are more preferred. Examples of molybdates include ammonium paramolybdate, ammonium dimolybdate, and ammonium tetramolybdate. The molybdenum raw material may be used alone or in combination of two or more.
[0025] (Solvent) When the metal compound is supported on a support, various solvents can be used to dissolve or disperse the metal compound and to use various support methods. The type of solvent used is not particularly limited as long as it can dissolve or disperse the metal compound and does not adversely affect the subsequent calcination and hydrogen reduction of the metal-supported material, or the hydrogenation reaction using the catalyst of the present invention. Examples of the solvent include ketone solvents such as acetone, alcohol solvents such as methanol and ethanol, ether solvents such as tetrahydrofuran and ethylene glycol dimethyl ether, and water. These solvents may be used alone or as a mixed solvent. As described above, in the present invention, a halide, more preferably a chloride, is preferably used as the metal compound. However, water is preferably used because of the high solubility of these halides. Furthermore, when dissolving or dispersing the metal compound, various additives may be added in addition to the solvent. For example, as described in JP-A-10-15388, the addition of a carboxylic acid and / or carbonyl compound solution can improve the dispersibility of each metal component on the support when the metal compound is supported on the support.
[0026] <Metal-supported material> The metal-supported material in which the metal component is supported on a carrier can be dried before use as necessary, and is preferably dried before use. If the metal-supported material is subjected to a subsequent reduction treatment without being dried, the reaction activity may be reduced. In particular, when a dehalogenation treatment described below is subsequently performed, drying is preferable in that it can suppress elution of metal salts in the presence of an alkali typically used in the dehalogenation treatment. The drying method is not particularly limited as long as it removes the solvent used during the supporting process. It is usually carried out in the presence of an inert gas or under a flow of an inert gas. The drying pressure is not particularly limited, but is usually carried out under normal pressure or reduced pressure conditions. The drying temperature is not particularly limited, but is usually carried out at 300°C or less, preferably 250°C or less, more preferably 200°C or less, and usually 80°C or more.
[0027] <Dehalogenation Treatment and Washing> The metal-supported material may be subjected to a dehalogenation treatment, if necessary, before the reduction step described below. During the metal-supporting step, particularly when a halide such as a chloride is used as the raw material for the metal component, halogen compounds may be generated in the reduction apparatus during the reduction step described below. While this is not a problem in laboratory-scale processing volumes, when performing large-scale reduction on an industrial scale, a large amount of halogen compounds may be generated in the reduction apparatus, which may require exhaust gas treatment and may cause corrosion of the apparatus. Therefore, it is preferable to perform a dehalogenation treatment before performing the reduction step. The dehalogenation treatment method is not particularly limited, but typically, the metal-supported material is contacted with an alkaline compound in the gas phase or liquid phase to react with the halogen compounds in the metal-supported material, and then the halogen compounds can be removed by gas-phase treatment or washing. Among these, due to ease of operation and high efficiency of removing halogen compounds from the metal-supported material, it is preferable to treat the metal-supported material by contacting it with an alkaline compound in the liquid phase and then remove the halogen compounds by washing. Specifically, it is more preferable to contact the metal-supported material with an alkaline aqueous solution and then wash it with water.
[0028] The temperature for the dehalogenation treatment is not particularly limited, but is usually 10° C. or higher, preferably 20° C. or higher, and usually 150° C. or lower, preferably 100° C. or lower, more preferably 80° C. or lower. When the temperature is equal to or higher than the lower limit, the dehalogenation treatment can be carried out efficiently, and when the temperature is equal to or lower than the upper limit, volatilization, thermal decomposition, etc. of the solvent and the alkali compound used in the treatment do not occur.
[0029] When an alkaline aqueous solution is used for the dehalogenation treatment, the pH of the alkaline aqueous solution is not particularly limited, but is usually 7.5 or higher, preferably 8.0 or higher, and usually 13.0 or lower, preferably 12.5 or lower. If the pH is below the upper limit, there is no risk of the supported metal being altered due to an excessively high pH, and the supported metal is less likely to be eluted during the washing process described below. If the pH is above the lower limit, sufficient dehalogenation is achieved.
[0030] As the type of alkaline compound, for example, carbonates, bicarbonates, ammonia, ammonium carbonate, ammonium bicarbonate, etc. of alkaline metals can be used. These can be used alone or in combination of two or more. Among them, weakly basic alkaline compounds are preferred. The use of weakly basic alkaline compounds such as ammonia and ammonium salts tends to produce a catalyst with higher activity than the use of strongly basic alkaline compounds.
[0031] The amount of alkaline compound used is usually 0.1 to 50 equivalents, preferably 1 to 20 equivalents, and more preferably 1 to 10 equivalents relative to the halogen ions contained in the carrier. The alkaline compound is usually used as an aqueous solution, but water-soluble solvents such as methanol, ethanol, acetone, and even ethylene glycol dimethyl ether, or even mixtures of these with water, may also be used. The alkaline aqueous solution is preferably used in an amount that completely fills the pores of the carrier supporting the metal component of the metal-supported material, i.e., in an amount equal to or greater than the pore volume of the carrier. The amount of alkaline aqueous solution used is not particularly limited, as it also depends on the concentration of the alkaline aqueous solution. However, it is usually 0.8 to 20 times, preferably 1 to 10 times, and more preferably 1 to 5 times the pore volume of the carrier of the metal-supported material used.
[0032] It is preferable to wash the metal-supported material after treatment with an alkali compound to remove excess alkali compound and generated halide. For washing, any solution that dissolves excess alkali compound and generated halide can be used, but water is preferred. In this case, the washing temperature is not particularly limited, and washing is usually carried out at 10°C or higher and 100°C or lower, but because washing efficiency is good with warm water, it is preferably 40°C or higher, more preferably 50°C or higher. After the alkali treatment or washing, further drying may be carried out as necessary. Drying conditions are the same as those for drying the above-mentioned metal-supported material.
[0033] <Reduction Treatment and Reducing Gas> The metal-supported material is preferably reduced with a reducing gas to form a metal-supported catalyst. The reducing gas in the present invention is not particularly limited as long as it has reducing properties, and examples thereof include hydrogen, methanol, hydrazine, etc., with hydrogen being preferred. In other words, the metal-supported catalyst of the present invention is preferably prepared via hydrogen reduction. In the reduction treatment of the present invention, a reduction reaction occurs regardless of the type of reducing gas, resulting in a metal-supported catalyst. The amount of reducing gas required for the reduction treatment is expressed as the "hydrogen absorption amount." In the present invention, the reduction treatment of the metal-supported material may be performed in one stage or in multiple stages, although this is not particularly limited.
[0034] (Reduction Treatment Temperature) During the production of the metal-supported catalyst of the present invention, it is preferable to carry out the reduction treatment by controlling the treatment temperature range. The reduction treatment temperature is not particularly limited and may be constant or variable. It is usually 80°C or higher, preferably 100°C or higher, more preferably 150°C or higher, and usually 650°C or lower, preferably 600°C or lower, more preferably 580°C or lower. When the temperature is below the upper limit, there is no sintering of the metal component or adverse effects on the support. On the other hand, when the temperature is above the lower limit, the reduction reaction proceeds sufficiently. Specifically, the reduction treatment may be carried out by maintaining a specific temperature within a preferred temperature range for a certain period of time, or by increasing the temperature within a preferred temperature range for a certain period of time. From the viewpoint of improving the efficiency of the reaction time, the reduction treatment generates heat from the metal-supported material and increases the temperature of the reaction system, so it is preferable to carry out the reduction treatment while increasing the temperature over a certain period of time. On the other hand, when intense heat is generated, a method of maintaining a constant temperature is preferred so that the reaction can be accurately controlled.
[0035] (Reducing Gas Concentration) The concentration of the reducing gas during the reduction treatment of the present catalyst is not particularly limited, and may be 100% by volume of reducing gas or may be diluted with an inert gas. The inert gas referred to here is a gas that does not react with the metal support or the reducing gas, and examples thereof include nitrogen and water vapor, with nitrogen being typically used. The concentration of the reducing gas when diluted with an inert gas is typically 5% by volume or more, preferably 15% by volume or more, more preferably 30% by volume or more, and even more preferably 50% by volume or more, based on the total gas components. Alternatively, a low concentration reducing gas may be used at the beginning of the reduction, and the reducing gas concentration may then be gradually increased to perform the reduction treatment.
[0036] (Flow Rate) In order to determine the flow rate of the reducing gas, it is preferable to know in advance the amount of hydrogen absorbed by the catalyst during reduction. While there are no particular limitations on the method for measuring the amount of hydrogen absorbed, it is usually preferable to perform reduction while adjusting the amount of hydrogen supplied per unit time and the temperature rise time per unit time, i.e., the temperature programmed reduction method (hereinafter referred to as the TPR method). Using this method, the amount of hydrogen absorbed by the catalyst and the absorption temperature can be precisely measured. In the TPR method, the catalyst to be measured is placed in a container, the container is heated while a constant flow rate of hydrogen is passed through it, and the amount of hydrogen at the inlet and outlet of the container is continuously measured. This method makes it possible to determine the amount of hydrogen absorbed by the metal-supported catalyst during reduction. Specifically, it can be measured using the method described in the Examples.
[0037] During the reduction treatment of the present catalyst, the reducing gas may be used in a sealed reactor or may be circulated through the reactor, but it is preferable to circulate the reducing gas through the reactor. The reduction treatment generates by-products such as water and ammonium chloride in the reactor, and these by-products may adversely affect the metal-supported material before the reduction treatment, the metal-supported material after the reduction treatment, and the obtained catalyst, which can be prevented. In other words, by circulating the reducing gas, the by-products can be discharged outside the reaction system.
[0038] The amount of reducing gas required for the reduction treatment is not particularly limited as long as the object of the present invention is achieved, and can be appropriately set depending on the reduction apparatus, the size of the reactor during reduction, and the flow conditions. Typically, the flow rate is 1.5 times or more, preferably 2 times or more, more preferably 3 times or more, and particularly preferably 5 times or more the amount of hydrogen required for each reduction treatment, relative to the hydrogen absorption amount determined by the TPR method, under conditions of high contact efficiency such that hydrogen flows through the catalyst layer. At or above the lower limit, reduction is sufficiently performed, especially when the contact efficiency with hydrogen is sufficient. There is no particular upper limit, but from the viewpoints of avoiding problems with exhaust gas treatment, preventing the scattering of metal supports or produced catalysts by the reducing gas, and avoiding waste of excess reducing gas, the flow rate is usually 500 times or less, preferably 200 times or less.
[0039] (Reduction Treatment Time) The time required for the reduction treatment varies depending on the amount of metal-supported material to be treated, the equipment used, etc., but is usually 7 minutes or more, preferably 15 minutes or more, more preferably 30 minutes or more, even more preferably 1 hour or more, and most preferably 2 hours or more, and is usually 40 hours or less, preferably 30 hours or less. The degree of reduction of the metal-supported material can be determined by the halogen concentration in the oxidized and stabilized metal-supported catalyst after the reduction treatment described below. The halogen concentration in the metal-supported catalyst is not particularly limited, but is usually 0.8 mass% or less, more preferably 0.7 mass% or less, and even more preferably 0.5 mass% or less. A lower halogen concentration is preferable because it suppresses the elution of halogen into the reaction solution during the reduction reaction using this catalyst. The lower limit of the halogen concentration is not particularly limited, but is usually 0.005 mass% or more, preferably 0.01 mass% or more. When the halogen concentration is within the above range, the reduction treatment of the metal support is sufficiently carried out, the elution of halogen into the reaction solution is kept low, and the activity of the reduction reaction using the present catalyst is improved, the reaction selectivity is also improved, and the stability of the catalyst is also improved.
[0040] <Preferred Production Method> As described above, the production method of the catalyst of the present invention involves a metal supporting step, a dehalogenation step, a washing step, and a reduction step. Preferred production method embodiments include a method in which a reducing gas is passed through the catalyst in a fixed bed in the reduction step, a method in which a reducing gas is passed through the catalyst placed stationary on a tray or belt, and a method in which a reducing gas is passed through a fluidized catalyst. Of these, it is preferable to carry out the reduction treatment while fluidizing the metal-supported material in the reduction treatment. By carrying out the reduction treatment while fluidizing the material, the surface area in contact with the reducing gas during the reduction treatment increases, thereby improving the efficiency of the reduction treatment.
[0041] The specific fluidization method is not particularly limited, and it is sufficient that the metal-supported material to be reduced is moved in a manner that increases the contact surface area with the reducing gas. For example, there is a method of rotating a reactor containing the metal-supported material to be reduced, or a method of incorporating an apparatus configuration that stirs or moves the metal-supported material in the reactor up and down. Specific fluidization methods include treatment methods using various kilns (heating furnaces). Specific preferred production methods include, for example, modes that use a continuous kiln or a batch kiln.
[0042] (Continuous Kiln) A continuous kiln refers to a kiln that can continuously supply a metal-supported material, perform reduction, and continuously discharge the reduced catalyst. Specific examples include a continuous rotary kiln, a roller hearth kiln, a belt kiln, a tunnel kiln, etc., but among these, in the production method of the present invention, a continuous rotary kiln is preferred because it provides high fluidity of the metal-supported material and high contact efficiency with the reducing gas.
[0043] The operating conditions of the continuous kiln are not particularly limited as long as they satisfy the above-mentioned conditions for the reduction treatment, and can be set appropriately depending on the equipment used. Typically, a continuous kiln can be operated so as to satisfy the above-mentioned conditions for the reduction treatment by controlling the flow rate and temperature of the reducing gas. Since a continuous kiln can continuously supply a metal support and a reducing gas, it is possible to control the method of supplying the metal support into the continuous kiln and the flow rate of the reducing gas.
[0044] The flow rate of the reducing gas in the continuous kiln is not particularly limited, but the amount of hydrogen required for reduction, calculated by TPR measurement of the metal support, is referred to as "hydrogen absorption amount A (m 3 / kg) and the amount of metal support fed into the continuous kiln is B (kg / h), the hydrogen flow rate is usually (1.5 x A x B) m 3 / h or more, preferably (2×A×B)m 3 / h or more, more preferably (5×A×B)m 3When the hydrogen flow rate is equal to or higher than the lower limit, a sufficient amount of hydrogen is absorbed by the catalyst, and the performance of the resulting catalyst is maintained at a high level. The upper limit is not particularly limited, but it is preferable to set the hydrogen flow rate at (1000×A×B) m 3 / h or less, preferably (500 x A x B) m 3 / h or less, more preferably (300 x A x B) m 3 / h or less.
[0045] The flow direction of the metal-supported material to be reduced in the continuous kiln and the flow direction of the reducing gas such as hydrogen can be adjusted appropriately depending on the conditions of the reduction treatment, and the flow direction of the reducing gas can be either parallel or countercurrent to the flow direction of the metal-supported material. In particular, it is preferable that the flow direction of hydrogen is countercurrent to the flow direction of the metal-supported material (opposite to each other) so that the catalyst that reaches the outlet of the continuous kiln can come into contact with high-purity hydrogen.
[0046] The rotation speed of the continuous rotary kiln is not particularly limited. A higher rotation speed improves the contact efficiency between the metal support and hydrogen, but causes catalyst wear, so the rotation speed is usually 0.5 rpm or more and 10 rpm or less, preferably 5 rpm or less.
[0047] (Batch kiln) A batch kiln is a kiln in which a predetermined amount of metal-supported material is charged in advance, and the temperature is gradually increased to the desired reduction temperature under the flow of reducing gas, thereby carrying out reduction at the predetermined temperature. Specific examples include fixed-bed heating furnaces in which metal-supported material is filled and treated, shelf-type heating furnaces in which the material is heated on shelves, shuttle kilns in which a firing cart enters and exits an electric furnace, and batch rotary kilns. Considering the contact efficiency of the metal-supported material with the reducing gas, fixed-bed heating furnaces and batch rotary kilns in which the metal-supported material is filled and treated are preferred, and for uniform reduction, a batch rotary kiln having a device for fluidizing the catalyst is preferred. Due to equipment constraints, continuous kilns are usually operated at a constant flow rate when introducing reducing gas, whereas batch kilns have a reaction vessel for each batch, allowing the temperature-raising method, flow rate, and concentration of the reducing gas to be changed for each batch.
[0048] (Operating Conditions of Batch Kiln) The operating conditions of the batch kiln are not particularly limited and can be set appropriately depending on the configuration of the apparatus, etc. The batch rotary kiln preferably used in the present invention starts heating after a predetermined amount of metal-supported material is charged in advance, allowing for more precise control of the heating time to the final reduction temperature than a continuous rotary kiln. The reduction treatment time is not particularly limited, but is usually at least 1 hour, preferably at least 2 hours, and usually at most 40 hours, preferably at most 30 hours, and more preferably at most 10 hours. If the reduction treatment time is shorter than the lower limit, if sudden hydrogen absorption occurs, a large amount of metal-supported material is reduced at once, resulting in intense heat generation and massive hydrogen absorption, which may cause catalyst sintering and make stable operation difficult. Furthermore, if the reduction treatment time is above the lower limit, the reduction time is ensured, sufficient reduction is achieved, and sufficient reaction activity and selectivity as a catalyst can be obtained. On the other hand, if the reduction treatment time is below the upper limit, catalyst productivity can be ensured, hydrogen loss is eliminated, and this is industrially advantageous.
[0049] When a batch rotary kiln is used, the concentration, flow rate, etc. of the reducing gas can be changed for each batch as appropriate depending on the conditions of the reduction treatment. The preferred reducing gas concentration in the operation of the batch rotary kiln is the same as described above.
[0050] The flow rate of the reducing gas is not particularly limited and can be set appropriately depending on the conditions of the reduction reaction. However, the amount of hydrogen required until the reduction is completed is calculated by TPR analysis of the unreduced catalyst, and the amount of hydrogen used is typically at least 5 times, preferably at least 10 times, and more preferably at least 20 times the required amount of hydrogen. It is also typically 5,000 times or less, preferably 1,000 times or less. If the flow rate is above the lower limit, hydrogen deficiency does not occur, and if it is below the upper limit, excess reducing gas is not consumed, which is economically advantageous. The rotation speed of the batch rotary kiln is not particularly limited, but a faster speed improves the contact efficiency with hydrogen, but catalyst wear occurs. Therefore, the rotation speed is typically 0.5 to 10 rpm, preferably 0.5 to 5 rpm.
[0051] (Oxidation Stabilization of Catalyst) In the production of the metal-supported catalyst of the present invention, the oxidation state of the metal-supported catalyst obtained by reducing the metal-supported material is usually controlled. Oxidation stabilization of the catalyst is preferable, particularly when producing a large amount of catalyst. The metal-supported material catalyst obtained by reduction is in a state in which the metal components have been reduced and are highly dispersed. Compared to directly discharging the catalyst into air, oxidative stabilization is preferable because it reduces the possibility of metal sintering due to sudden heat generation and also reduces the possibility of fire (fire of the support itself if the support is combustible, and also fire of surrounding combustible materials). Stabilization under controlled conditions can maintain high dispersion and exhibit high activity in the subsequent hydrogenation reaction. The oxidation stabilization method is not particularly limited, but includes adding water to the catalyst or pouring the catalyst into water, oxidative stabilization in a low-oxygen-concentration gas diluted with an inert gas under flow, and stabilization with carbon dioxide. Among these, the method of adding water to the catalyst or the method of putting the catalyst into water, and the method of oxidative stabilization with a gas having a low oxygen concentration are preferred, and the method of oxidative stabilization with a gas having a low oxygen concentration (hereinafter referred to as the "gradual oxidation method") is more preferred, and oxidative stabilization under flow of a gas having a low oxygen concentration is particularly preferred.
[0052] The oxygen concentration when oxidatively stabilizing with a low-oxygen gas is not particularly limited, but the oxygen concentration at the start of gradual oxidation is usually 0.2% by volume or more, preferably 0.5% by volume or more, and 10% by volume or less, preferably 8% by volume or less, and more preferably 7% by volume or less. If the oxygen concentration is above the lower limit, the time required for complete oxidative stabilization can be shortened and stabilization is sufficient. On the other hand, if the oxygen concentration is below the upper limit, the catalyst does not reach a high temperature, so there is no risk of deactivation. In order to produce a low-oxygen gas, it is preferable to dilute air with an inert gas, and nitrogen is preferably used as the inert gas.
[0053] The oxygen concentration during gradual oxidation may be maintained at the oxygen concentration at the start of gradual oxidation, but as long as the catalyst internal temperature is high and no catalyst deterioration occurs, the oxygen concentration may be gradually increased after the start of gradual oxidation. When gradual oxidation is stable at a low oxygen concentration, it is preferable to control the catalyst temperature so that it does not exceed 130 ° C. If the catalyst temperature is 130 ° C or less, rapid oxidation does not proceed, so sintering of the catalyst does not proceed, and the strength of the support is maintained without decreasing. From the above perspective, it is preferable to control the oxygen concentration and flow rate so that the catalyst temperature does not exceed 120 ° C, more preferably 110 ° C.
[0054] Methods for oxidative stabilization using a gas with a low oxygen concentration include passing a gas with a low oxygen concentration through a catalyst in a fixed bed, passing a gas with a low oxygen concentration through a catalyst placed stationary on a tray or belt, and passing a gas with a low oxygen concentration through a fluidized catalyst. The better the dispersion of the supported metal on the metal-supported catalyst, the more rapidly the oxidative stabilization progresses and the greater the amount of oxygen that reacts. Therefore, of the above methods, passing a gas with a low oxygen concentration through a catalyst in a fixed bed and passing a gas with a low oxygen concentration through a fluidized catalyst are preferred, and passing a gas with a low oxygen concentration through a fluidized catalyst is particularly preferred.
[0055] (Method of storing catalyst) When storing the metal-supported catalyst of the present invention, it is preferable to store it in an atmosphere with an oxygen concentration of 15% by volume or less. By storing it in such an atmosphere, if oxidation proceeds slowly even after oxidation stabilization, oxidation can proceed slowly in a sealed container. The lower limit of the oxygen concentration is not particularly limited, but it is usually preferable that it be 0.2% by volume or more in order to proceed with oxidation. In addition, since gas-stabilized catalysts are highly hygroscopic, which can be a major problem in non-aqueous reactions, it is preferable to store it in a sealed container.
[0056] <Uses> The catalyst of the present invention is suitable as a catalyst for reduction reactions, and is suitably used, for example, in the hydrogenation of carboxylic acids and / or carboxylic acid esters. That is, it is suitably used in a method for producing alcohols, in which a carboxylic acid and / or a carboxylic acid ester is brought into contact with the metal-supported catalyst of the present invention and reduced to obtain an alcohol corresponding to the carboxylic acid and / or the carboxylic acid ester, respectively. Any carboxylic acid or carboxylic acid ester that is easily available industrially can be used as the target carboxylic acid or carboxylic acid ester for the reduction reaction. Examples of carboxylic acids and / or carboxylic acid esters that can be subjected to a reduction reaction using the catalyst of the present invention include aliphatic chain carboxylic acids such as acetic acid, butyric acid, lauric acid, oleic acid, linoleic acid, linolenic acid, stearic acid, and palmitic acid; aliphatic cyclic carboxylic acids such as cyclohexanecarboxylic acid, naphthenic acid, and cyclopentanecarboxylic acid; aliphatic polycarboxylic acids such as oxalic acid, malonic acid, succinic acid, methylsuccinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, sebacic acid, cyclohexanedicarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,3,4-cyclohexanetricarboxylic acid, bicyclohexyldicarboxylic acid, and decahydronaphthalenedicarboxylic acid; and aromatic carboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, and trimesic acid.
[0057] The carboxylic acid is not particularly limited, but is preferably a linear or cyclic saturated aliphatic carboxylic acid, more preferably a carboxylic acid having 20 or less carbon atoms and containing no functional groups other than carboxyl groups, and even more preferably a dicarboxylic acid having 20 or less carbon atoms and containing no functional groups other than carboxyl groups and represented by formula (2): HOOC-R 1 -COOH (2) (in the formula R 1may have a substituent and is an aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms other than the substituent.) Particularly preferred are aliphatic or alicyclic polycarboxylic acids having 4 to 14 carbon atoms or esters thereof, which are suitable because of their high activity and high selectivity in the reduction reaction. In the present invention, it is particularly preferred to use 1,4-cyclohexanedicarboxylic acid or an ester thereof as a reactant to produce the corresponding alcohol by a reduction reaction. That is, a preferred method for producing an alcohol is to use 1,4-cyclohexanedicarboxylic acid or an ester (diester) of 1,4-cyclohexanedicarboxylic acid as a raw material and bring it into contact with the catalyst of the present invention to reduce it.
[0058] When using esters of these carboxylic acids, examples of the alcohol component include lower alcohols such as methanol, ethanol, i-propanol, and n-butanol. Esterification can also be performed with the same alcohol as the alcohol obtained by reduction. This has the advantage of eliminating the need to separate the alcohol produced in the subsequent hydrogenation reaction.
[0059] The reduction reaction using the catalyst of the present invention can be carried out without a solvent or in the presence of a solvent, but is typically carried out in the presence of a solvent. Examples of solvents that can be used include water, lower alcohols such as methanol and ethanol, alcohols from the reaction product, ethers such as tetrahydrofuran, dioxane, and ethylene glycol dimethyl ether, and hydrocarbons such as hexane and decalin. These solvents can be used alone or in combination of two or more. When reducing a carboxylic acid, it is preferable to use a solvent containing water for reasons such as solubility. The amount of solvent used is not particularly limited, but is typically about 0.1 to 20 times by mass, preferably 0.5 to 10 times by mass, and more preferably about 1 to 10 times by mass, relative to the carboxylic acid or carboxylic acid ester used as the starting material.
[0060] The reduction reaction using the catalyst of the present invention is usually carried out under pressurized hydrogen gas. The reaction is usually carried out at 100 to 300°C, preferably 150 to 300°C. The reaction pressure is 1 to 30 MPa, preferably 1 to 25 MPa, and more preferably 5 to 25 MPa. The reduction reaction using the catalyst of the present invention can be carried out in either a liquid phase or a gas phase. However, vaporizing the carboxylic acid / carboxylic acid ester and carrying out the reduction reaction while maintaining the gaseous state requires large equipment and a large amount of energy, so it is preferably carried out in a liquid phase.
[0061] Also included within the scope of the present invention is a method for hydrogenating a carboxylic acid and / or a carboxylic acid ester, in which the carboxylic acid and / or the carboxylic acid ester is brought into contact with the catalyst of the present invention.
[0062] The present invention will be explained in more detail below by way of examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention.
[0063] <TPR measurement method> 0.1 g of catalyst was placed in a narrow quartz tube and heated in 10% H 2 / He was flowed at 20 ml / min, and hydrogen substitution in the system was completed. 2 The temperature was maintained until the concentration stabilized, and then the temperature was raised at a constant rate to 700° C. over 60 minutes. During this time, the amount of hydrogen at the outlet was continuously measured with a mass spectrometer, and the amount of absorbed hydrogen was calculated.
[0064] <Method for Confirming Catalyst Reaction Activity> The reaction activity and selectivity of the catalyst obtained in the present invention were confirmed using the hydrogenation reaction of 1,4-cyclohexanedicarboxylic acid (CHDA) to produce 1,4-cyclohexanedimethanol (CHDM). A 200 mL Hastelloy C (registered trademark) induction-stirred autoclave (hereinafter sometimes referred to as the "reactor") was charged with 40 g of water, 10 g of CHDA (a mixture of cis and trans isomers: manufactured by Tokyo Chemical Industry Co., Ltd.), and 2 g of the catalyst to be evaluated. The atmosphere inside the reactor was purged with hydrogen, and the hydrogen partial pressure was adjusted to 1 MPa. The reactor was heated with stirring at 1,000 rpm (a stirring speed that was set so that the hydrogen supply rate was not limited by an excessively slow stirring speed, but was not so high that the catalyst cracked). The reaction pressure was adjusted to 8.5 MPa at the specified temperature, and the reaction was initiated at 240°C. Hydrogen was continuously supplied to the reactor from a hydrogen pressure accumulator, and the reaction was carried out for 3 hours at a constant pressure of 8.5 MPa at 240°C. After the reaction was completed, the catalyst was visually inspected for cracks. Reactions in which catalyst cracks occurred were excluded because the apparent reaction rate increased and selectivity could not be accurately compared. The resulting reaction solution was neutralized with NaOH to determine the carboxyl group conversion rate, and the products were analyzed using a gas chromatograph. The main product was the target product, CHDM, and the main by-products were two types: cyclohexanemethanol (CHM) and 4-methylcyclohexanemethanol (MCHM). Since almost the entire product, other than the two by-products, was CHDM, the catalyst performance was compared in terms of the carboxyl group conversion rate and by-product yield.
[0065] Comparative Example 1 A catalyst was prepared using a cylindrical activated carbon support (R1 EXTRA manufactured by Cabot Norit) having a diameter of 1 mm and a length of 2 to 5 mm, according to Example 4 of JP-A 2001-9277. Specifically, ruthenium chloride hydrate (RuCl 3 ・xH 2 O), hexachloroplatinic acid (IV) (hexahydrate, etc.) (H 2 PtCl 6 ・6H 2 O), tin(II) chloride (SnCl 2 ・2H 2O) was dissolved in a dilute hydrochloric acid solution, and activated carbon treated with nitric acid was added thereto. The solvent was removed and the catalyst was dried. The dried catalyst was then added to an ammonium bicarbonate solution, followed by filtration, washing, and drying to prepare a metal-supported catalyst. In the preparation method for the metal-supported catalyst, 1.1 ml of 0.3% dilute hydrochloric acid was used per gram of activated carbon used as the water solution for dissolving the metal chlorides. The metal chlorides were charged in amounts such that, when the entire amount was loaded, reduced with hydrogen, and stabilized by oxidation, the metal contents in the supported catalyst would be 5.5 mass% Ru, 2.4 mass% Pt, and 6.4 mass% Sn (all metal loadings are expressed in mass %). Furthermore, ammonium bicarbonate was used in an 11 mass% aqueous solution in an amount 1.7 times the molar amount of the chlorine in the metal chlorides, and water at 90°C was used for washing. The resulting metal-supported catalyst was reduced at 500°C under a hydrogen stream, and then stabilized by oxidation in a diluted oxygen atmosphere to obtain a catalyst. Hereinafter, this catalyst will be referred to as the "reduced catalyst." Reactions were carried out using this catalyst. The conversion rate and the yield of by-products are shown in Table 1. In Table 1, the column for metal species indicates the compounds used for metal species other than ruthenium, platinum, and tin.
[0066] (Comparative Example 2) The reduction catalyst obtained in Comparative Example 1 was treated with Fe(III) acetylacetonate (Fe(acac) 3 After reduction, the catalyst was prepared so that the amount of supported Fe was 0.1% by mass. Specifically, a predetermined amount of Fe(acac) was added to 0.86 ml of tetrahydrofuran solvent per 1 g of the reduced catalyst. 3 The mixture was dissolved in 10 g of the reduction catalyst obtained in Comparative Example 1, added, stirred, and left for 1 hour. The mixture was then evaporated under reduced pressure of 1 kPa at 80°C for 1 hour, then placed in a glass tube, placed in an electric furnace, and dried at 150°C for 2 hours under a flow of argon at 5 L / hour. 2.5 g of the dried catalyst was then placed in a glass tube again, placed in an electric furnace, and reduced at 500°C for 2 hours under a flow of hydrogen at 5 L / hour. The mixture was then cooled under a flow of argon and stabilized at room temperature under a flow of 6% oxygen / nitrogen by volume to obtain a 0.1% Fe-supported catalyst. Using this catalyst (a catalyst amount equivalent to 2 g of the reduction catalyst used in the preparation) a reaction similar to that of Comparative Example 1 was carried out. The results are shown in Table 1.
[0067] (Comparative Example 3) In Comparative Example 2, Fe(III) acetylacetonate (Fe(acac) 3 ) instead of iron (III) chloride hexahydrate (FeCl 3 ・6H 2 An Fe-supported catalyst was obtained in a concentration of 0.2 mass% in terms of Fe metal in the same manner as in Example 1, except that a hydroxybenzoate (HPO) was used and water was used as the solvent. Using this catalyst, a reaction was carried out in the same manner as in Comparative Example 1. The results are shown in Table 1.
[0068] (Comparative Example 4) In Comparative Example 2, Fe(acac) was added so that the Fe metal content was 0.5 mass %. 3 A 0.5% Fe-supported catalyst was obtained in the same manner as in Comparative Example 2, except that a 0.5% Fe-supported catalyst was used. Using this catalyst, a reaction was carried out in the same manner as in Comparative Example 1. The results are shown in Table 1.
[0069] (Comparative Example 5) In Comparative Example 3, FeCl was added to the mixture to a concentration of 0.5 mass % as Fe metal. 3 ・6H 2 A 0.5% Fe-supported catalyst was obtained in the same manner as in Comparative Example 3, except that O was used. Using this catalyst, a reaction was carried out in the same manner as in Comparative Example 1. The results are shown in Table 1.
[0070] (Reference Example 1) In Comparative Example 3, iron chloride (III) hexahydrate (FeCl 3 ・6H 2 Chromium (III) chloride hexahydrate (CrCl) was used instead of chromium (III) chloride hexahydrate (CrCl). 3 ・6H 2 A 0.2% by mass Cr-supported catalyst was obtained in the same manner as in Comparative Example 3, except that 0.2% by mass Cr-supported catalyst was used. Using this catalyst, a reaction was carried out in the same manner as in Comparative Example 1. The results are shown in Table 1.
[0071] (Reference Example 2) In Comparative Example 2, Fe(III) acetylacetonate (Fe(acac) 3 ) instead of Cr(III) acetylacetonate (Cr(acac) 3 A 0.5% Cr-supported catalyst was obtained in the same manner as in Comparative Example 2, except that a 0.5% Cr-supported catalyst was used. Using this catalyst, a reaction was carried out in the same manner as in Comparative Example 1. The results are shown in Table 1.
[0072] (Comparative Example 6) In Comparative Example 2, Fe(III) acetylacetonate (Fe(acac) 3) instead of ammonium paramolybdate (ammonium molybdate (VI) tetrahydrate ((NH 4 ) 6 Mo 7 O 24 ・4H 2 A 0.5% Mo-supported catalyst was obtained in the same manner as in Comparative Example 2, except that 0)) was used and water was used as the solvent. Using this catalyst, a reaction was carried out in the same manner as in Comparative Example 1. The results are shown in Table 1.
[0073] (Comparative Example 7) RuCl 3 ・xH 2 O (Ru content 41.9%) 1.131g, H 2 PtCl 6 ・6H 2 O 0.547g, SnCl 2 ・2H 2 O 0.883g, FeCl 3 ・6H 2 1.196 g of ammonium bicarbonate was dissolved in a 0.3% hydrochloric acid solution. 7.41 g of the same nitric acid-treated activated carbon as in Comparative Example 1 was added to this solution, thoroughly stirred, and then left for 3 hours. After 3 hours, the mixture was dried in an evaporator, then transferred to a calcination tube, and dried for 2 hours at 150°C under argon gas flow. This catalyst was added to an 11% by mass aqueous solution of ammonium bicarbonate, equivalent to 1.7 equivalents of the total chlorine content of the metal chlorides used, treated for 1 hour, filtered, washed with water at 90°C, and dried in an evaporator. The dried catalyst was transferred to a calcination tube and further dried at 150°C under a flow of argon gas. 2.5 g of the further dried catalyst was reduced at 500°C under a flow of hydrogen, cooled, and then stabilized with 6% oxygen / nitrogen to prepare a 5.5%Ru-2.4%Pt-5.4%Sn-0.47%Fe / activated carbon (calculated values on a charged basis) catalyst supporting all four components at once (in Table 1, "FeCl 3 Using 2 g of this catalyst, a reaction similar to that in Comparative Example 1 was carried out. The results are shown in Table 1.
[0074] (Example 1) The reduction catalyst obtained in Comparative Example 1 was added with FeCl 2 to a concentration of 0.2% as Fe metal and 0.2% as Cr metal. 3 ・6H 2 O, CrCl 3 ・6H 2A 0.2% Fe-0.2% Cr supported catalyst was obtained in the same manner as in Comparative Example 2, except that O was used and water was used as the solvent. Using this catalyst, a reaction was carried out in the same manner as in Comparative Example 1. The results are shown in Table 1.
[0075] Example 2 The reduction catalyst obtained in Comparative Example 1 was added with FeCl 2 to give a concentration of 0.4% as Fe metal and 0.1% as Cr metal. 3 ・6H 2 O, CrCl 3 ・6H 2 A 0.4% Fe-0.1% Cr supported catalyst was obtained in the same manner as in Comparative Example 2, except that O was used and water was used as the solvent. Using this catalyst, a reaction was carried out in the same manner as in Comparative Example 1. The results are shown in Table 1.
[0076] Example 3: The reduction catalyst obtained in Comparative Example 1 was added with FeCl 2 to a concentration of 0.2% as Fe metal and 0.2% as Mo metal. 3 ・6H 2 O, (NH 4 ) 6 Mo 7 O 24 ・4H 2 A 0.2% Fe-0.2% Mo supported catalyst was obtained in the same manner as in Comparative Example 2, except that O was used and water was used as the solvent. Using this catalyst, a reaction was carried out in the same manner as in Comparative Example 1. The results are shown in Table 1.
[0077] Example 4: The reduction catalyst obtained in Comparative Example 1 was added with FeCl 2 to a concentration of 0.4% as Fe metal and 0.1% as Mo metal. 3 ・6H 2 O, ammonium molybdate (VI) tetrahydrate ((NH 4 ) 6 Mo 7 O 24 ・4H 2 A 0.4% Fe-0.1% Mo supported catalyst was obtained in the same manner as in Comparative Example 2, except that a 0.4% Fe-0.1% Mo supported catalyst was used, and a 3% HCl aqueous solution was used as the solvent. Using this catalyst, a reaction was carried out in the same manner as in Comparative Example 1. The results are shown in Table 1.
[0078]
[0079] As is clear from Table 1, the catalyst of the present invention supporting Fe and Cr and the catalyst of the present invention supporting Fe and Mo can reduce the yield of the main by-products, cyclohexanemethanol (CHM) and 4-methylcyclohexanemethanol (MCHM), while maintaining a high conversion. In contrast, Comparative Examples 2 to 5 supporting only iron and Comparative Example 6 supporting only molybdenum show some degree of effectiveness when compared to unmodified catalysts not modified with iron or the like, but are inferior to the catalyst of the present invention. As described above, the catalyst of the present invention maintains a high conversion and suppresses the by-product yield to 60% or less compared to the unmodified catalyst, demonstrating excellent effectiveness.
[0080] According to the present invention, by adding a combination of new specific metals to a conventional reduction catalyst, the yield of by-products is drastically reduced and the yield of the target product is improved. The drastically reduced yield of by-products makes it possible to omit or simplify the detailed purification process when the product is subsequently used as a polymer raw material, making the present invention an extremely useful technology from an industrial perspective.
Claims
1. A supported metal catalyst for use in the hydrogenation of carboxylic acids and / or carboxylic acid esters, comprising ruthenium, tin, and platinum supported on a carrier, wherein the supported metal catalyst further comprises iron, and chromium and / or molybdenum.
2. The metal-supported catalyst according to claim 1, wherein the amount of iron supported is 0.01 mass% or more and 4 mass% or less, and the total amount of chromium and / or molybdenum supported is 0.01 mass% or more and 2 mass% or less, relative to the total mass of the metal-supported catalyst.
3. The metal-supported catalyst according to claim 1 or 2, wherein the support is a carbonaceous support.
4. The metal-supported catalyst according to claim 1 or 2, wherein the total amount of ruthenium, tin, platinum, iron, molybdenum, and chromium supported is 5 mass% or more based on the total mass of the metal-supported catalyst.
5. The metal-supported catalyst according to claim 1 or 2, wherein the metal-supported catalyst is prepared via hydrogen reduction.
6. A method for producing an alcohol, comprising contacting a carboxylic acid and / or a carboxylic acid ester with the metal-supported catalyst according to claim 1 or 2 and reducing the carboxylic acid and / or the carboxylic acid ester to obtain an alcohol corresponding to the carboxylic acid and / or the carboxylic acid ester, respectively.
7. A method for hydrogenating a carboxylic acid and / or a carboxylic acid ester, which comprises contacting the carboxylic acid and / or the carboxylic acid ester with the supported metal catalyst according to claim 1 or 2.
8. The method for producing an alcohol according to claim 6, wherein the carboxylic acid is 1,4-cyclohexanedicarboxylic acid and the carboxylic acid ester is an ester of 1,4-cyclohexanedicarboxylic acid.