AI Technical Summary
Existing thick film resistors using ruthenium-based conductive particles and glass powder struggle to achieve a temperature coefficient of resistance (TCR) close to zero, especially in both low and high temperature ranges, with a significant difference between low-temperature and high-temperature TCR values, which affects resistance value accuracy and stability.
A ruthenium oxide powder with a rutile crystal structure and a specific lattice constant ratio (Lc/La ≥ 0.6913) and crystallite diameter of 10 nm to 80 nm is used, allowing for the adjustment of TCR to near zero and minimizing the difference between low-temperature and high-temperature coefficients, when incorporated into thick film resistor compositions.
The approach results in thick film resistors with highly accurate resistance values, reduced resistance variations, and improved electrical characteristics, including low current noise and excellent performance in short-time overload tests, by achieving TCR values within ±50 ppm/°C and minimizing the difference between low-temperature and high-temperature coefficients.
Smart Images

Figure PI2025000659_DRAWING_001
Abstract
Description
Ruthenium oxide powder, composition for thick film resistors, paste for thick film resistors, thick film resistors
[0001] The present invention relates to a ruthenium oxide powder, a composition for a thick film resistor, a paste for a thick film resistor, and a thick film resistor.
[0002] 2. Description of the Related Art Resistors such as chip resistors, hybrid ICs, and resistor networks generally use thick film resistors formed by applying a thick film resistor paste to a ceramic substrate and firing the paste.
[0003] A widely used composition for thick film resistors contains, as main components, ruthenium-based conductive particles, typically ruthenium oxide, and glass powder.
[0004] Ruthenium-based conductive particles and glass powder are used for thick-film resistors because they can be fired in air, the temperature coefficient of resistance (TCR) can be brought close to zero, and resistors with a wide range of resistance values can be formed.
[0005] In a thick-film resistor composition containing ruthenium-based conductive particles and glass powder, the resistance value of the thick-film resistor changes depending on the compounding ratio. Specifically, increasing the compounding ratio of ruthenium-based conductive particles decreases the resistance value of the thick-film resistor, while decreasing the compounding ratio of ruthenium-based conductive particles increases the resistance value of the thick-film resistor. Taking advantage of this, the compounding ratio of ruthenium-based conductive particles and glass powder is adjusted to produce a desired resistance value in a thick-film resistor.
[0006] In recent years, the number of resistors mounted in electrical and electronic devices has been increasing, and it is desired that each resistor has a high resistance value precision and a temperature coefficient of resistance (TCR) close to zero.
[0007] As described above, in a thick-film resistor composition containing ruthenium-based conductive particles and glass powder, when a low resistance value is desired, the ruthenium-based conductive particles are mixed in a large amount and the glass powder is mixed in a small amount, and when a high resistance value is desired, the resistance value is adjusted by mixing in a small amount of ruthenium-based conductive particles and a large amount of glass powder.
[0008] However, in the low resistance range where a large amount of ruthenium-based conductive particles is incorporated, the temperature coefficient of resistance (TCR) tends to be positive, while in the high resistance range where a small amount of ruthenium-based conductive particles is incorporated, the temperature coefficient of resistance (TCR) tends to be negative. The temperature coefficient of resistance (TCR) represents the change in resistance value with temperature and is one of the important characteristics of thick-film resistors. The temperature coefficient of resistance can be adjusted by adding a regulator, primarily a metal oxide, to the thick-film resistor composition. Adjusting the temperature coefficient of resistance to a negative value is relatively easy, and examples of regulators include manganese oxide, niobium oxide, tantalum oxide, and titanium oxide. However, adjusting the temperature coefficient of resistance to a positive value is difficult. Therefore, it is desirable for conductive particles for thick-film resistors to have a temperature coefficient of resistance close to zero or large positive values when used in thick-film resistors.
[0009] The temperature coefficient of resistance (TCR) of a thick film resistor is evaluated based on the room temperature as a reference, using the cold temperature coefficient of resistance (COLD-TCR) at a lower temperature side and the hot temperature coefficient of resistance (HOT-TCR) at a higher temperature side.
[0010] In recent years, there has been an increasing demand for higher precision in electronic components, and both the cold temperature coefficient of resistance (COLD-TCR) and the hot temperature coefficient of resistance (HOT-TCR) must be close to zero.
[0011] In thick-film resistors containing ruthenium-based conductive particles and glass powder, the low-temperature temperature coefficient of resistance (COLD-TCR) on the low-temperature side and the high-temperature temperature coefficient of resistance (HOT-TCR) on the high-temperature side are generally not the same, and it has been difficult to make either of them approach zero.
[0012] Patent Document 1 discloses a resistor paste containing at least a glass composition that is substantially free of lead and a conductive material that is substantially free of lead, which are mixed with an organic vehicle, and which is characterized in that the conductive material has an average particle size of 5 μm or more and 50 μm or less.
[0013] According to Patent Document 1, the average particle size of the conductive material is set to 5 μm or more and 50 μm or less, so that while it has a high resistance value of 10 kΩ / □ or more, it is possible to achieve small variation in the resistance value, a small absolute value of the temperature coefficient of resistance (TCR), and good withstand voltage characteristics (STOL).
[0014] Japanese Patent Publication No. 2005-129806 Japanese Patent Publication No. 2005-209742
[0015] There is a need for ruthenium-based conductive particles that, when used in a thick-film resistor, can bring both the low-temperature temperature coefficient of resistance (COLD-TCR) on the low-temperature side and the high-temperature temperature coefficient of resistance (HOT-TCR) on the high-temperature side closer to 0 and reduce the difference between them. However, Patent Document 1 does not evaluate the low-temperature temperature coefficient of resistance on the low-temperature side or the difference between the low-temperature temperature coefficient of resistance and the high-temperature temperature coefficient of resistance.
[0016] In view of the problems of the conventional technology described above, one aspect of the present invention aims to provide a ruthenium oxide powder that, when used in a thick-film resistor, can bring the temperature coefficient of resistance close to 0 and can reduce the difference between the low-temperature temperature coefficient of resistance and the high-temperature temperature coefficient of resistance.
[0017] In order to solve the above problems, the present invention provides a ruthenium oxide powder having a rutile crystal structure, in which, where La is the lattice constant of the a-axis and Lc is the lattice constant of the c-axis measured by X-ray diffraction, Lc / La is 0.6913 or more, and the crystallite diameter is 10 nm or more and 80 nm or less.
[0018] According to one aspect of the present invention, it is possible to provide a ruthenium oxide powder that, when used in a thick-film resistor, can bring the temperature coefficient of resistance close to 0 and reduce the difference between the low-temperature temperature coefficient of resistance and the high-temperature temperature coefficient of resistance.
[0019] FIG. 1 is an explanatory diagram of the relationship between the a-axis lattice constant and the c-axis lattice constant of the ruthenium oxide powder used in the examples and comparative examples.
[0020] The ruthenium oxide powder of this embodiment has a rutile crystal structure, and has a crystallite diameter of 10 nm to 80 nm, where Lc is the lattice constant of the a-axis measured by X-ray diffraction and Lc is the lattice constant of the c-axis measured by X-ray diffraction.
[0021] The inventors of the present invention have investigated ruthenium oxide powder that, when used in a thick film resistor, can bring the temperature coefficient of resistance close to 0 and can reduce the difference between the low-temperature temperature coefficient of resistance and the high-temperature temperature coefficient of resistance.
[0022] As a result, it was found that by setting the ratio of the a-axis lattice constant to the c-axis lattice constant of ruthenium oxide powder to a predetermined value or more, the temperature coefficient of resistance (TCR) of a thick film resistor formed using a composition for a thick film resistor containing the ruthenium oxide powder and a glass powder can be made to approach 0. In other words, it was found that the low-temperature temperature coefficient of resistance and the high-temperature temperature coefficient of resistance of the thick film resistor can be made to approach 0, and the difference between them can also be made small.
[0023] Furthermore, it was found that by adjusting the crystallite size of the ruthenium oxide powder to fall within a predetermined range, it is possible to form a thick film resistor with small variations in resistance value and good electrical characteristics.
[0024] Based on the above findings, the present invention was completed. The ruthenium oxide powder of this embodiment will be described below. (Ratio of the c-axis lattice constant Lc to the a-axis lattice constant La) The lattice constant and crystallite size of ruthenium oxide powder vary depending on the manufacturing method, manufacturing conditions, etc. The inventors of the present invention discovered that the lattice constant of ruthenium oxide powder affects the properties of a thick-film resistor formed using a thick-film resistor composition containing ruthenium oxide powder and glass powder, as described above, and completed the present invention.
[0025] According to the investigations of the present inventors, it is preferable that the ruthenium oxide powder has a rutile crystal structure. The ratio of the c-axis lattice constant Lc to the a-axis lattice constant La of the ruthenium oxide powder is important. Specifically, by using ruthenium oxide powder with an Lc / La ratio of 0.6913 or more, it is possible to make the temperature coefficient of resistance (TCR) of a thick-film resistor formed using the ruthenium oxide powder approach zero.
[0026] For example, ruthenium oxide in a bulk state having a tetragonal rutile crystal structure and sufficiently large crystals has an a-axis lattice constant of 4.499 Å and a c-axis lattice constant of 3.107 Å. The a-axis lattice constant La and the c-axis lattice constant Lc of bulk ruthenium oxide, Lc / La, are 0.6906. The lattice constant of the bulk ruthenium oxide is taken from the International Centre for Diffraction Data.
[0027] In contrast to this, the lattice constants of the ruthenium oxide powder of this embodiment can be made smaller than those in the bulk state, for example, in both the a-axis and c-axis, and Lc / La can be within the range described above.
[0028] According to the investigations of the inventors of the present invention, thick film resistors using ruthenium oxide powder with an Lc / La ratio of less than 0.6913 have a large difference between the low-temperature temperature coefficient of resistance (COLD-TCR) and the high-temperature temperature coefficient of resistance (HOT-TCR). For this reason, thick film resistors using ruthenium oxide powder with an Lc / La ratio of less than 0.6913 cannot reduce the difference between the low-temperature temperature coefficient of resistance (COLD-TCR) and the high-temperature temperature coefficient of resistance (HOT-TCR) and cannot bring both closer to zero.
[0029] The upper limit of Lc / La, which is the ratio of the lattice constant Lc of the c-axis to the lattice constant La of the a-axis of the ruthenium oxide powder of this embodiment, is not particularly limited, but can be set to 0.692 or less, for example, when the crystallite diameter satisfies the range of 10 nm or more and 80 nm or less.
[0030] The ratio Lc / La of the c-axis lattice constant Lc to the a-axis lattice constant La increases as the c-axis lattice constant increases and the a-axis lattice constant decreases. However, according to the investigations of the inventors of the present invention, no clear correlation is found between the a-axis lattice constant and the c-axis lattice constant of the ruthenium oxide powder, and the Lc / La ratio cannot be controlled simply by controlling the a-axis or c-axis lattice constant, for example.
[0031] Patent Document 2 discloses that the a-axis and b-axis of ruthenium oxide are focused on and set within a predetermined range. However, according to studies by the inventors of the present invention, simply setting the lattice constants of the a-axis and b-axis of ruthenium oxide powder within a predetermined range does not make it possible to bring both the low-temperature temperature coefficient of resistance (COLD-TCR) and the high-temperature temperature coefficient of resistance (HOT-TCR) of a thick-film resistor using the ruthenium oxide powder close to 0. Furthermore, even if the lattice constants of the a-axis and b-axis of ruthenium oxide powder are set within a predetermined range, it is not possible to reduce the difference between the high-temperature temperature coefficient of resistance and the low-temperature temperature coefficient of resistance.
[0032] Therefore, when used in a thick film resistor, in order to bring both the low-temperature temperature coefficient of resistance (COLD-TCR) and the high-temperature temperature coefficient of resistance (HOT-TCR) closer to zero and to reduce the difference between the high-temperature temperature coefficient of resistance and the low-temperature temperature coefficient of resistance, it is important to set Lc / La to a predetermined value or greater. (Crystallite Diameter) By setting the crystallite diameter of the ruthenium oxide powder of this embodiment to 10 nm or more and 80 nm or less (100 Å or more and 800 Å or less), the precision of the resistance value of a thick film resistor formed using a composition for a thick film resistor containing the ruthenium oxide powder can be increased. In other words, the variation in resistance value can be suppressed. Furthermore, by using a ruthenium oxide powder whose crystallite diameter to lattice constant ratio Lc / La is within a predetermined range, the difference between the low-temperature temperature coefficient of resistance and the high-temperature temperature coefficient of resistance of a thick film resistor formed using a composition for a thick film resistor containing the ruthenium oxide powder can be reduced, and both can be made to approach zero in particular. Furthermore, by using ruthenium oxide powder that satisfies the above crystallite size range, it becomes possible to form a thick film resistor with good electrical properties.
[0033] Generally, fine ruthenium oxide powder is used in thick-film resistors. In fine ruthenium oxide powder, the primary particles are composed almost entirely of single crystals, and the crystallite diameter is close to the particle diameter of the primary particles. However, if the crystallite diameter of the ruthenium oxide powder is less than 10 nm, the difference between the low-temperature temperature coefficient of resistance (COLD-TCR) and the high-temperature temperature coefficient of resistance (HOT-TCR) of the thick-film resistor becomes large, making it impossible to approach both values to zero. Furthermore, if the crystallite diameter of the ruthenium oxide powder exceeds 80 nm, the resistance value of the thick-film resistor varies greatly, the precision of the resistance value decreases, and the resistance value changes significantly with the load voltage, resulting in poor electrical characteristics. (Lattice Constant) For ruthenium oxide powder with a crystallite diameter of 10 nm to 80 nm, the lattice constant of the a-axis is explained using the examples and comparative examples of the present invention. The lattice constant is 4.491 Å to 4.4918 Å. Therefore, in order to make the ratio of the c-axis lattice constant Lc to the a-axis lattice constant La, Lc / La, of this embodiment equal to or greater than 0.6913, the c-axis lattice constant can be set to 3.105 Å or greater. The upper limit of the c-axis lattice constant of the ruthenium oxide powder of this embodiment is not particularly limited, but can be set to, for example, 3.108 Å or less.
[0034] As mentioned above, the Lc / La ratio of the a-axis lattice constant La to the c-axis lattice constant Lc of bulk ruthenium oxide is 0.6906. In contrast, in the ruthenium oxide powder of this embodiment, the Lc / La ratio of the c-axis lattice constant Lc to the a-axis lattice constant La is 0.6913 or more. Therefore, the ruthenium oxide powder of this embodiment is characterized by a relatively long c-axis, provided that the a-axis has the same length as that of the bulk.
[0035] The lattice constant of the ruthenium oxide powder varies depending on the raw materials and manufacturing conditions used to manufacture the ruthenium oxide powder. It is known from the inventor's experimental results and prior art document 2 that the a-axis lattice constant of the ruthenium oxide powder is 4.475 Å or greater. The ruthenium oxide powder of this embodiment has a ratio of the c-axis lattice constant Lc to the a-axis lattice constant La, Lc / La, of 0.6913 or greater, as long as the Lc / La ratio is within the range of lattice constants that the ruthenium oxide particles can achieve. (Specific Surface Area Diameter) The particle size of the ruthenium oxide powder of this embodiment is not particularly limited, but the specific surface area diameter of the ruthenium oxide powder of this embodiment is preferably 10 nm or greater and 115 nm or less.
[0036] The specific surface area diameter of the ruthenium oxide powder can be calculated from the specific surface area. Specifically, the particle size, which is the specific surface area diameter of the ruthenium oxide powder, is D (nm), and the density is ρ (g / cm 3 ), the specific surface area is S (m 2 / g) and the particles contained are considered to be perfect spheres, the following relational expression (1) holds true.
[0037] In this embodiment, the density ρ of ruthenium oxide is set to 7.05 g / cm 3 The particle size, which is the specific surface area diameter, can be calculated by equation (1) using the following formula: (Regarding the characteristics of the thick film resistor formed using the ruthenium oxide powder) As described above, for the thick film resistor formed using the ruthenium oxide powder of this embodiment, the low-temperature temperature coefficient of resistance and the high-temperature temperature coefficient of resistance can be made to approach 0, and the difference between them can also be made small.
[0038] Specifically, the thick film resistor preferably has a temperature coefficient of resistance of −50 ppm / ° C. or more and +50 ppm / ° C. or less, more preferably −40 ppm / ° C. or more and +40 ppm / ° C. or less, and even more preferably −30 ppm / ° C. or more and +30 ppm / ° C. or less. The above ranges are suitable for both the high-temperature temperature coefficient of resistance and the low-temperature temperature coefficient of resistance.
[0039] Furthermore, for the thick film resistor, the difference between the high-temperature temperature coefficient of resistance and the low-temperature temperature coefficient of resistance is preferably 70 ppm / °C or less, and more preferably 60 ppm / °C or less. As will be shown in the examples described later, in the thick film resistor manufactured from the composition for a thick film resistor containing the ruthenium oxide powder of this embodiment, the low-temperature temperature coefficient of resistance and the high-temperature temperature coefficient of resistance can be -30 ppm / °C or more and +30 ppm / °C or less. Furthermore, with this thick film resistor, the difference between the high-temperature temperature coefficient of resistance and the low-temperature temperature coefficient of resistance can be made small.
[0040] Furthermore, a thick film resistor formed using a composition for a thick film resistor containing the ruthenium oxide powder of this embodiment can achieve a highly accurate temperature coefficient of resistance and resistance value, as well as excellent characteristics in current noise and short time overload tests (STOL).
[0041] Thus, a thick film resistor formed from a thick film resistor composition or thick film resistor paste using the ruthenium oxide powder of this embodiment can achieve excellent characteristics in terms of temperature coefficient of resistance, resistance value accuracy, current noise, and short-term overload test. [Method for manufacturing ruthenium oxide powder] Below, an example of the configuration of the method for manufacturing ruthenium oxide powder of this embodiment will be described. Note that, since the method for manufacturing ruthenium oxide powder of this embodiment can manufacture the ruthenium oxide powder already described, a description of the matters already described will be omitted.
[0042] The method for producing the ruthenium oxide powder of this embodiment is not particularly limited, and the production method and production conditions can be selected so that the ratio La / Lc of the lattice constant Lc of the c-axis to the lattice constant La of the a-axis and the crystallite diameter fall within the aforementioned ranges.
[0043] A common method for producing ruthenium oxide powder used in a composition for a thick film resistor is to heat-treat hydrated ruthenium oxide powder synthesized from a liquid containing ruthenium ions. In this production method, the lattice constant and crystallite size can also be adjusted and selected by changing the production conditions.
[0044] In the method of heat treating hydrated ruthenium oxide powder, the lattice constant and crystallite size can be selected by combining the wet synthesis method and conditions for the hydrated ruthenium oxide powder and the method and conditions for the heat treatment, and the ruthenium oxide particles of this embodiment can be synthesized.
[0045] More specifically, the method for producing the ruthenium oxide powder can include, for example, the following steps.
[0046] A ruthenium oxide hydrate production step in which ruthenium oxide hydrate is synthesized by a wet method.
[0047] a ruthenium oxide hydrate recovery step of separating and recovering ruthenium oxide hydrate from the solution;
[0048] A drying step for drying the ruthenium oxide hydrate.
[0049] A heat treatment step for heat treating ruthenium oxide hydrate.
[0050] Note that the conventionally commonly used method of producing ruthenium oxide powder, in which ruthenium oxide having a large particle size is produced and then crushed, is not suitable for the method of producing ruthenium oxide powder of the present embodiment, because it is difficult to reduce the particle size and the particle size variation is large.
[0051] In the ruthenium oxide hydrate production step, the method for synthesizing ruthenium oxide hydrate is not particularly limited, but examples thereof include a method in which ruthenium oxide hydrate is precipitated or precipitated in a ruthenium-containing aqueous solution. 2 Ru 2 O 4 A method of adding ethanol to an aqueous solution to obtain a precipitate of ruthenium oxide hydrate, or RuCl 3 For example, the aqueous solution is neutralized with KOH or the like to obtain a precipitate of ruthenium oxide hydrate.
[0052] Then, as described above, in the ruthenium oxide hydrate recovery step and the drying step, the precipitate of ruthenium oxide hydrate is separated into solid and liquid, washed as necessary, and then dried, whereby ruthenium oxide hydrate powder can be obtained.
[0053] The conditions for the heat treatment step are not particularly limited, but for example, ruthenium oxide hydrate powder can be heat-treated in an oxidizing atmosphere at a temperature of 400° C. or higher to remove water of crystallization and produce highly crystalline ruthenium oxide powder. The oxidizing atmosphere here refers to a gas containing 10% by volume or more of oxygen, and air, for example, can be used.
[0054] The temperature at which the ruthenium oxide hydrate powder is heat-treated is set to 400°C or higher as described above, thereby obtaining ruthenium oxide (RuO 2 Although there is no particular upper limit to the heat treatment temperature, excessively high temperatures may result in the crystallite size and specific surface area of the resulting ruthenium oxide powder becoming large, or may result in the ruthenium becoming a hexavalent or octavalent oxide (RuO 3 and RuO 4 ) and the rate of volatilization may increase. For this reason, it is preferable to perform the heat treatment at a temperature of, for example, 1100° C. or less.
[0055] In particular, the temperature at which the ruthenium oxide hydrate powder is heat-treated is more preferably 500°C or higher and 1100°C or lower.
[0056] As described above, the lattice constant and crystallite size of the resulting ruthenium oxide powder can be changed by changing the synthesis conditions when producing ruthenium oxide hydrate, the heat treatment conditions, etc. For this reason, it is preferable to select conditions, for example, by conducting a preliminary test, so as to obtain ruthenium oxide powder having the desired lattice constant, lattice constant ratio (Lc / La), and crystallite size.
[0057] The lattice constant and crystallite size of ruthenium oxide powder can be determined by analyzing a diffraction pattern obtained by powder X-ray diffraction. In recent years, Rietveld analysis in powder X-ray diffraction has made it possible to accurately measure and calculate the lattice constant and crystallite size of powder.
[0058] The ruthenium oxide powder of this embodiment can be combined with a glass powder to form a composition for a thick-film resistor, as described below, and used to manufacture a thick-film resistor. By using the ruthenium oxide powder of this embodiment in a composition for a thick-film resistor, the temperature coefficient of resistance can be brought close to 0, regardless of the composition of the glass powder, and a thick-film resistor can be obtained with a small difference between the low-temperature temperature coefficient of resistance and the high-temperature temperature coefficient of resistance. That is, with the ruthenium oxide powder of this embodiment, a thick-film resistor with a high-precision temperature coefficient of resistance close to 0 can be formed, regardless of whether it is made of, for example, a conventionally used lead-containing glass powder or a lead-free glass powder that reduces the impact on the human body and pollution. Furthermore, the difference between the low-temperature temperature coefficient of resistance and the high-temperature temperature coefficient of resistance can be reduced.
[0059] Furthermore, a thick film resistor obtained using the ruthenium oxide powder of this embodiment has small variations in resistance value and can achieve excellent characteristics in current noise and short time overload tests (STOL), etc. [Thick Film Resistor Composition] Next, an example of the composition for a thick film resistor of this embodiment will be described.
[0060] The thick-film resistor composition of this embodiment can contain the above-mentioned ruthenium oxide powder, which is a conductive particle, and a glass powder. The thick-film resistor composition of this embodiment can also be composed of ruthenium oxide powder and a glass powder, but even in this case, it does not exclude the inclusion of unavoidable impurities.
[0061] The components contained in the composition for a thick film resistor of this embodiment will be described below. (1) Ruthenium oxide powder As described above, the ruthenium oxide powder has a rutile-type crystal structure, and when the lattice constant of the a-axis measured by X-ray diffraction is La and the lattice constant of the c-axis is Lc, the Lc / La ratio is 0.6913 or more, and the crystallite diameter can be 10 nm or more and 80 nm or less.
[0062] Other aspects of the ruthenium oxide powder have already been described, and therefore will not be described here. (2) Glass Powder As the glass powder, glass powders conventionally used in compositions for thick film resistors can be used. (Example of Glass Powder Composition) As the glass powder that can be used in this embodiment, for example, one or more types selected from aluminoborosilicate lead glass, zinc borosilicate glass, calcium borosilicate glass, and barium borosilicate glass can be used. Furthermore, lead-free glass, for example, one or more types selected from zinc borosilicate glass, calcium borosilicate glass, and barium borosilicate glass can also be used.
[0063] Glass can generally be produced by mixing predetermined components or their precursors according to the desired composition, melting the resulting mixture, and rapidly cooling it. The melting temperature is not particularly limited, but is typically around 1400°C. Rapid cooling is often achieved by placing the molten material in cold water or flowing it over a cold belt. Glass is crushed to the desired particle size using a ball mill, vibration mill, planetary mill, or bead mill.
[0064] Although lead-containing glass powders that have generally been used in compositions for thick film resistors can be used, in recent years, due to concerns about environmental issues, it has become desirable to use lead-free glass powders.
[0065] In the composition of the glass powder for the lead-free thick film resistor composition, the skeleton of SiO 2 The fluidity during firing is adjusted by blending a metal oxide other than SiO 2 As the metal oxide other than B 2 O 3 and RO (R represents one or more alkaline earth elements selected from Ca, Sr, and Ba). For this reason, the glass powder used in the thick film resistor composition of this embodiment is preferably SiO 2 , B 2 O 3 , RO. The glass powder preferably contains SiO in the glass composition. 2 , B 2O 3 and RO is 100 parts by mass, 2 20 parts by mass or more and 50 parts by mass or less, B 2 O 3 and RO in an amount of 35 parts by mass or more and 65 parts by mass or less. By using such a glass powder, the temperature coefficient of resistance of the obtained thick film resistor can be particularly easily brought close to 0.
[0066] SiO in the glass composition of the glass powder 2 , B 2 O 3 and RO is 100 parts by mass, 2 By making the amount of SiO 20 parts by mass or more, it is possible to easily obtain glass and improve weather resistance. 2 By making the content of the glass powder 50 parts by mass or less, the softening temperature of the glass powder can be suppressed and the fluidity can be increased.
[0067] In the glass powder, B 2 O 3 By making the content of B 10 parts by mass or more, the softening temperature of the glass powder can be suppressed and the fluidity can be increased. 2 O 3 By making the amount 30 parts by mass or less, weather resistance can be improved.
[0068] In the glass powder, by adjusting the RO content to 35 parts by mass or more, the softening temperature of the glass powder can be suppressed and the flowability can be increased, and by adjusting the RO content to 65 parts by mass or less, crystallization can be suppressed and the glass can be easily produced.
[0069] The glass powder of the lead-free thick film resistor composition is 2 , B 2 O 3 Preferably, the glass powder contains SiO, RO as an essential component. 2 , B 2 O 3 Although the glass may be composed of only RO, other components may be contained in order to adjust the weather resistance of the glass and the fluidity during firing. Examples of other components include Al, 2 O 3, ZrO 2 , TiO 2 , SnO 2 , ZnO, Li 2 O, Na 2 O.K. 2 O and the like. 2 O 3 can suppress the phase separation of glass, and ZrO 2 , TiO 2 improves the weather resistance of the glass, SnO 2 , ZnO, Li 2 O, Na 2 O.K. 2 O and the like have the function of increasing the fluidity of the glass. (Softening Point) The softening point is a measure that influences the fluidity of the glass when firing the composition for a thick film resistor.
[0070] In general, when a thick film resistor is produced, the temperature at which a thick film resistor composition or a thick film resistor paste is fired is 800°C or higher and 900°C or lower.
[0071] In this way, when the firing temperature of the composition for a thick film resistor or the like when producing a thick film resistor is 800°C or higher and 900°C or lower, the softening point of the glass powder used in the composition for a thick film resistor according to this embodiment is preferably 600°C or higher and 800°C or lower, more preferably 600°C or higher and 750°C or lower.
[0072] Here, the softening point is the temperature at which the next differential thermal curve decreases at a peak higher than the temperature at which the lowest differential thermal curve decreases when the glass is heated in air by differential thermal analysis (TG-DTA) at a rate of 10°C / min. (Particle size) The particle size of the glass powder is not particularly limited, but if it is too large, it can cause an increase in the resistance value variation of the thick-film resistor and a decrease in the load characteristics. To avoid these, the 50% volume cumulative particle size of the glass powder is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1.5 μm or less. Glass can be pulverized using a ball mill, planetary mill, bead mill, etc., but wet pulverization is preferable to achieve a sharp particle size.
[0073] If the particle size of the glass powder is too small, productivity may decrease and the inclusion of impurities may increase, so the 50% volume cumulative particle size of the glass powder is preferably 0.5 μm or more.
[0074] The 50% volume cumulative particle size means the particle size at 50% of the volume cumulative value in the particle size distribution determined by a laser diffraction / scattering method. (3) Mixing Ratio of Ruthenium Oxide Powder and Glass Powder Since the ratio of the ruthenium oxide powder and the glass powder contained in the composition for a thick film resistor can be changed depending on the desired resistance value, etc., the mass ratio of the ruthenium oxide powder and the glass powder contained in the composition for a thick film resistor of this embodiment is not particularly limited.
[0075] However, in the composition for a thick film resistor of this embodiment, the mass ratio of ruthenium oxide powder to glass powder is preferably in the range of 60:40 to 5:95. In other words, when the total mass of the ruthenium oxide powder and the glass powder is taken as 100%, the mass ratio of the ruthenium oxide powder is preferably 5% to 60%.
[0076] When the total mass of the ruthenium oxide powder and the glass powder is taken as 100%, by setting the mass ratio of the ruthenium oxide powder to 60% or less, it is possible to prevent the fired film obtained by firing the thick film resistor composition or the like from becoming brittle, and also to prevent the occurrence of cracks and the like.
[0077] Furthermore, when the total mass of the ruthenium oxide powder and the glass powder is taken as 100%, by setting the mass ratio of the ruthenium oxide powder to 5% or more, the resistance value of the thick film resistor obtained using the thick film resistor composition or the like can be prevented from becoming excessively high, and stability can be improved. (4) Regarding Additives The thick film resistor composition of this embodiment can be composed of the above-mentioned ruthenium oxide powder and glass powder, but it can also contain additives. The thick film resistor composition of this embodiment can also be composed of ruthenium oxide powder, glass powder, and additives. Note that even in the above case, it is not excluded that the thick film resistor composition may contain inevitable impurities.
[0078] When a thick film resistor having a lower resistance value is desired, the composition for a thick film resistor of this embodiment may also contain Ag powder or Pd powder.
[0079] The thick film resistor composition of this embodiment contains the above-mentioned ruthenium oxide powder and glass powder, and also contains Ag powder or Pd powder, and even in a thick film resistor with a reduced resistance value, it is possible to make both the low-temperature temperature coefficient of resistance and the high-temperature temperature coefficient of resistance approach zero.
[0080] The thick film resistor composition of this embodiment may also contain additives that are generally used for the purpose of improving or adjusting the resistance value, temperature coefficient of resistance, voltage load characteristics, and trimming properties of the thick film resistor.
[0081] A typical example of the additive is Nb. 2 O 5 , Ta 2 O 5 , TiO 2 , MnO 2 , CuO, ZrO 2 , Al 2 O 3 , SiO 2 , ZrSiO 4 One or more types selected from the above can be mentioned.
[0082] Nb 2 O 5 , Ta 2 O 5 , TiO 2 , MnO 2 Although ZrO has the effect of reducing the resistance value fluctuation when a voltage load is applied to a thick film resistor, it also shifts the temperature coefficient of resistance to the negative side. CuO has the effect of reducing the resistance value of the thick film resistor and shifting the temperature coefficient of resistance to the positive side. 2 , Al 2 O 3 , SiO 2 , ZrSiO 4 This has the effect of suppressing the extension of microcracks that tend to occur during laser trimming to adjust the resistance value of the thick film resistor.
[0083] By including these additives in the thick film resistor composition of this embodiment, a thick film resistor having better characteristics can be produced.
[0084] The content of the additives in the composition for thick film resistors of this embodiment is adjusted depending on the purpose, but it is preferable that the content be, for example, in the range of 0 to 20 parts by mass, where the total amount of the ruthenium oxide powder and the glass powder is 100 parts by mass. [Thick Film Resistor Paste] Next, the paste for thick film resistors of this embodiment will be described.
[0085] The thick film resistor paste of this embodiment can contain ruthenium oxide powder, glass powder, and an organic vehicle. The thick film resistor paste of this embodiment can also be composed of ruthenium oxide powder, glass powder, and an organic vehicle, but even in this case, it does not exclude the inclusion of unavoidable impurities.
[0086] Both the ruthenium oxide powder and the glass powder can be mixed and dispersed in an organic vehicle to form a paste for a thick film resistor for printing.
[0087] The thick film resistor paste of this embodiment may further contain the additives described in the thick film resistor composition. In this case, the ruthenium oxide powder, glass powder, and additives contained in the thick film resistor paste of this embodiment are preferably mixed and dispersed in an organic vehicle to form a thick film resistor paste for printing.
[0088] The thick film resistor paste of this embodiment can also be composed of ruthenium oxide powder, glass powder, additives, and an organic vehicle, but even in this case, it does not exclude the inclusion of unavoidable impurities.
[0089] The components contained in the thick film resistor paste of this embodiment are described below. (1) Components Contained in the Thick Film Resistor Paste (1-1) Ruthenium Oxide Powder The ruthenium oxide powder can be the ruthenium oxide powder described above. That is, as described above, the ruthenium oxide powder has a rutile crystal structure, and when the lattice constant of the a-axis measured by X-ray diffraction is La and the lattice constant of the c-axis is Lc, the Lc / La can be 0.6913 or more, and the crystallite diameter can be 10 nm or more and 80 nm or less.
[0090] Other aspects of the ruthenium oxide powder have already been described, and therefore will not be described here. (1-2) Glass Powder As the glass powder, glass powders that have conventionally been used in pastes for thick film resistors can be used.
[0091] Examples of glass powder include SiO 2 and B 2 O 3 and RO (wherein R represents one or more alkaline earth elements selected from Ca, Sr, and Ba), and SiO 2 and B 2 O 3 and RO is 100 parts by mass, 2 20 parts by mass or more and 50 parts by mass or less, B 2 O 3 and RO in an amount of 35 parts by mass or more and 65 parts by mass or less. By using such a glass powder, the temperature coefficient of resistance of the obtained thick film resistor can be particularly easily brought close to 0.
[0092] The glass powder may have the same composition, properties, etc. as those described for the thick film resistor composition, and therefore further description will be omitted here. (1-3) Mixing Ratio of Ruthenium Oxide Powder and Glass Powder The ratio of the ruthenium oxide powder and glass powder contained in the thick film resistor paste can be changed depending on the desired resistance value, etc., so the mass ratio of the ruthenium oxide powder and glass powder contained in the thick film resistor paste of this embodiment is not particularly limited.
[0093] However, in the thick film resistor paste of this embodiment, the mass ratio of ruthenium oxide powder to glass powder is preferably in the range of 60:40 to 5:95. In other words, when the total mass of the ruthenium oxide powder and the glass powder is taken as 100%, the mass ratio of the ruthenium oxide powder is preferably 5% to 60%.
[0094] The reason why the above range is preferable has already been explained in the thick film resistor composition, so the explanation will be omitted here. (1-4) Organic Vehicle The organic vehicle contained in the thick film resistor paste of this embodiment is not particularly limited, and various organic vehicles can be used.
[0095] As the organic vehicle, for example, a solution in which a resin such as ethyl cellulose, acrylic acid ester, methacrylic acid ester, rosin, or maleic acid ester is dissolved in a solvent such as terpineol, butyl carbitol, or butyl carbitol acetate can be suitably used.
[0096] A dispersant, a plasticizer, or the like can be added to the organic vehicle as needed. (1-5) Additives The thick film resistor paste of this embodiment can contain the various additives described in the thick film resistor composition in addition to the dispersant and plasticizer described in the organic vehicle above. (2) Dispersion Method As described above, the ruthenium oxide powder, the glass powder, and, if necessary, the additives are preferably mixed and dispersed in the organic vehicle.
[0097] The method for dispersing the ruthenium oxide powder, glass powder, additives, etc. is not particularly limited. For example, dispersion is generally performed using a three-roll mill, a bead mill, a planetary mill, or the like, which are used to disperse fine particles. The blending ratio of the organic vehicle is not particularly limited, as it can be appropriately adjusted depending on the printing or application method of the thick-film resistor paste. For example, when the total amount of the ruthenium oxide powder, glass powder, and additives is 100 parts by mass, the thick-film resistor paste preferably contains, for example, 20 parts by mass or more and 200 parts by mass or less of the organic vehicle. [Thick-Film Resistor] Next, the thick-film resistor of this embodiment will be described.
[0098] The thick film resistor of this embodiment is a thick film resistor formed from the above-described thick film resistor composition or thick film resistor paste. That is, the thick film resistor of this embodiment can be produced using the above-described thick film resistor composition or thick film resistor paste.
[0099] Therefore, the thick film resistor of this embodiment can contain the above-mentioned ruthenium oxide powder and the glass component derived from the above-mentioned glass powder.
[0100] The thick film resistor of this embodiment can be manufactured using, for example, the above-described paste for a thick film resistor by a manufacturing method for a thick film resistor including the following printing step, drying step, and firing step.
[0101] In the printing step, the above-described paste for thick film resistors can be printed between a pair of electrodes formed by a known thick film technique, for example.
[0102] In the drying step, solvents such as organic vehicles contained in the paste for forming the thick film resistor that constitutes the printed film printed in the printing step can be volatilized by heating and drying.
[0103] In the firing step, the printed film dried in the drying step can be fired under temperature conditions such that the peak temperature is 800°C or higher and 900°C or lower.
[0104] By carrying out the above firing step, the thick film resistor of this embodiment can be manufactured.
[0105] A coating glass may be formed on the surface of the obtained thick film resistor by a known thick film technique, and the resistance value may be adjusted by known laser trimming.
[0106] As described above, in the thick-film resistor composition or thick-film resistor paste, the ratio of the ruthenium oxide powder to the glass powder is preferably 5% by mass or more and 60% by mass or less. The thick-film resistor of this embodiment can be produced using the thick-film resistor composition or thick-film resistor paste, and the glass component in the resulting thick-film resistor is derived from the glass powder in the thick-film resistor composition or thick-film resistor paste.
[0107] Therefore, in the thick film resistor of this embodiment, similarly to the thick film resistor composition and the thick film resistor paste, the proportion of ruthenium oxide is preferably 5% by mass or more and 60% by mass or less, when the total mass of ruthenium oxide and the glass component is taken as 100% by mass.
[0108] The glass component contained in the thick film resistor of this embodiment is derived from the glass powder used in the thick film resistor composition, as described above. Therefore, the glass component contained in the thick film resistor of this embodiment is not particularly limited, but may be, for example, SiO 2 and B 2 O 3 and RO (wherein R represents one or more alkaline earth elements selected from Ca, Sr, and Ba). In this case, SiO 2 and B 2 O 3 and RO is 100 parts by mass, 2 20 parts by mass or more and 50 parts by mass or less, B 2 O 3 and RO in a proportion of 35 parts by mass to 65 parts by mass.
[0109] The method for producing the thick film resistor of this embodiment is not particularly limited, but for example, the resistor can be formed by firing the above-mentioned thick film resistor composition on a ceramic substrate. Alternatively, as described above, the resistor can be formed by applying the above-mentioned thick film resistor paste to a ceramic substrate, followed by drying and firing.
[0110] According to the thick film resistor of this embodiment, the low-temperature resistance temperature coefficient and the high-temperature resistance temperature coefficient can be made close to 0, and the difference between them can also be made small.
[0111] Specifically, in the thick film resistor of this embodiment, the temperature coefficient of resistance is preferably −50 ppm / ° C. or more and +50 ppm / ° C. or less, more preferably −40 ppm / ° C. or more and +40 ppm / ° C. or less, and even more preferably −30 ppm / ° C. or more and +30 ppm / ° C. or less. The above ranges are suitable for both the high-temperature temperature coefficient of resistance and the low-temperature temperature coefficient of resistance.
[0112] In the thick film resistor of this embodiment, the difference between the high temperature coefficient of resistance and the low temperature coefficient of resistance is preferably 70 ppm / °C or less, and more preferably 60 ppm / °C or less.
[0113] Furthermore, the thick film resistor of this embodiment can achieve the above-mentioned high-precision temperature coefficient of resistance, and also has small variations in resistance value and can achieve excellent characteristics in current noise and short-time overload tests (STOL).
[0114] As described above, the thick film resistor of this embodiment can achieve excellent characteristics in terms of temperature coefficient of resistance, resistance value accuracy, current noise, and short-time overload test.
[0115] The low-temperature temperature coefficient of resistance (COLD-TCR) can be calculated by the following formula (2).
[0116] The high temperature coefficient of resistance (HOT-TCR) can be calculated by the following formula (3).
[0117]
[0118] Here, R -55 is the resistance value at a temperature of -55°C, R 25 is the resistance value at a temperature of 25°C, R 125 is the resistance value at a temperature of 125°C.
[0119] The present invention will be described below with reference to specific examples and comparative examples, but is not limited to these examples. [Evaluation Methods] (1) Evaluation Methods for Ruthenium Oxide Powder and Glass Powder (1-1) Lattice Constant and Crystallite Diameter The lattice constant and crystallite diameter of the ruthenium oxide powder were determined by Rietveld analysis in an X-ray diffraction method.
[0120] Furthermore, the lattice constant of the a-axis thus obtained was defined as La, and the lattice constant of the c-axis as Lc, and Lc / La was calculated. (1-2) Specific Surface Area Diameter The specific surface area diameter of the ruthenium oxide powder was calculated from the specific surface area and density of the ruthenium oxide powder. The BET single-point method, which allows for easy measurement, was used to measure the specific surface area. The specific surface area diameter was defined as D (nm) and the density as ρ (g / cm 3 ), the specific surface area is S (m 2 / g) and the particles contained are considered to be true spheres, the following relational expression (A) holds: The specific surface area diameter calculated from this D was taken as the specific surface area diameter of the ruthenium oxide powder.
[0121] When calculating the specific surface area diameter, the density ρ of ruthenium oxide was set to 7.05 g / cm 3 (1-3) Softening Point The softening point of the glass powder was determined by heating the glass powder in air at a rate of 10°C per minute using differential thermal analysis (TG-DTA). The softening point of the glass powder was determined as the peak temperature at which the next differential thermal curve, which is higher than the temperature at which the lowest differential thermal curve decreases, was obtained. (2) Evaluation Method of Thick Film Resistors (2-1) Film Thickness The film thickness of the thick film resistor was measured using a stylus thickness roughness meter on five thick film resistors fabricated under the same conditions in each Example and Comparative Example. The film thicknesses of the five thick film resistors were then averaged to calculate the film thickness (fired film thickness) of the thick film resistor in each Example and Comparative Example. (2-2) Sheet Resistivity and CVR (Coefficient of Variation of Sheet Resistivity) The sheet resistance was calculated by averaging the sheet resistance values of 25 thick film resistors fabricated under the same conditions in each Example and Comparative Example.
[0122] The sheet resistance of each thick film resistor was measured using a digital multimeter (manufactured by Keithley, No. 2001). 3 , "M" is 10 6 respectively.
[0123] The coefficient of variation (CVR) of the sheet resistance was calculated by dividing the standard deviation of the sheet resistance of 25 thick film resistors manufactured under the same conditions in each Example and Comparative Example by the average value, and expressing it as a percentage. CVR indicates the variation in resistance value, and a smaller value means a smaller variation in resistance value. Therefore, it is preferable that the CVR is, for example, 5% or less. (2-3) Temperature Coefficient of Resistance For five thick film resistors manufactured under the same conditions in each Example and Comparative Example, the resistance value was measured after holding them at -55°C, 25°C, and 125°C for 15 minutes, and each resistance value was expressed as R -55 , R 25 , R 125 It was decided.
[0124] Then, the low-temperature temperature coefficient of resistance (COLD-TCR) and the high-temperature temperature coefficient of resistance (HOT-TCR) were calculated for each thick-film resistor using the following formulas (B) and (C), and the average of the five thick-film resistors was calculated. The low-temperature temperature coefficient of resistance is shown in the "C-TCR" column in Tables 3 and 4, and the high-temperature temperature coefficient of resistance is shown in the "H-TCR" column in Tables 3 and 4.
[0125] It is desirable that the temperature coefficient of resistance be close to 0 for both COLD-TCR and HOT-TCR, and a target for a high precision resistor is that the temperature coefficient of resistance be between -50 ppm / °C and +50 ppm / °C.
[0126]
[0127] The difference between COLD-TCR and HOT-TCR was calculated for each Example and Comparative Example, and is shown in the "H / C Difference" column in Tables 3 and 4. (2-4) Short-Term Overload Test (STOL) The resistance change rate in the short-term overload test (STOL) was calculated by applying an overload voltage 2.5 times the voltage equivalent to 0.25 W (400 V if it exceeded 400 V) to the thick-film resistors prepared in each Example and Comparative Example for 5 seconds. The resistance was measured using the same procedure as for the area resistance value described above, but for the STOL evaluation, measurements were made and calculated for 10 thick-film resistors for each Example and Comparative Example. The absolute value of the resistance change rate in the short-term overload test (STOL) is preferably 1% or less, and more preferably 0.5% or less. (2-5) Current Noise In each example and comparative example, the current noise of five thick film resistors fabricated under the same conditions was measured, and the average value was calculated.
[0128] The current noise was measured using a noise meter (Model: 315c manufactured by Quan-Tech) by applying a voltage equivalent to 1 / 10 W. The current noise of a thick film resistor is related to its overload characteristics and reliability, and the lower the value, the better the electrical characteristics of the thick film resistor.
[0129] The current noise is simply referred to as noise in Tables 3 and 4. [Examples 1 to 10] (1) Thick-film resistor composition In Examples 1 to 10, ruthenium oxide powder, glass powder, and additive powder (MnO 2 , TiO 2 , CuO, SiO 2 ) were mixed to prepare a thick film resistor composition.
[0130] In addition, "RuO 2 " indicates the blending ratio of ruthenium oxide powder, and "glass" indicates the blending ratio of glass powder. 2 ", "TiO 2 ”, “CuO”, “SiO 2 " indicates the blending ratio of each additive component.
[0131] For example, in Example 1, as shown in the "Type of ruthenium oxide powder" column of Table 3, ruthenium oxide powder A in Table 1 is used. Also, in Example 1, as shown in the "Type of glass powder" column of Table 3, glass powder a in Table 2 is used.
[0132] Therefore, in Example 1, 50 parts by mass of ruthenium oxide powder A, 50 parts by mass of glass powder a, and MnO 2 and 1 part by mass of CuO were mixed to prepare a composition for a thick film resistor. (Ruthenium Oxide Powder) The specific surface area, crystallite size, and lattice constant of ruthenium oxide powders A to G used in each example are shown in Table 1. In Table 1, the "c-axis lattice constant / a-axis lattice constant" corresponds to Lc / La, which is the ratio of the lattice constant of the c-axis, Lc, to the lattice constant of the a-axis, La.
[0133] The relationship between the a-axis lattice constant and the c-axis lattice constant of the ruthenium oxide powder used in the Examples and Comparative Examples is shown in Figure 1. As shown in Figure 1, it was confirmed that there is no clear correlation between the a-axis lattice constant and the c-axis lattice constant. (Glass Powder) The composition of the glass powder used in each Example is shown in Table 2.
[0134] In the examples and comparative examples, lead-free glass powders were used as glass powders a to c from the viewpoint of preventing environmental pollution, but conventionally used lead-containing glass may also be used.
[0135] All of the glass powders a to c were pulverized so that the median diameter was 1.3 μm or more and 1.5 μm or less in particle size distribution measured by a laser diffraction particle size distribution analyzer. That is, the 50% volume cumulative particle size of each of the glass powders a to c was 1.3 μm or more and 1.5 μm or less. (Additives) As mentioned above, the additives used were MnO 2 , TiO 2 , CuO, SiO 2 One or more types selected from the above are used.
[0136] The particle size of the additive is MnO 2 is 0.5 μm, TiO 2 is 0.3 μm, CuO is 0.5 μm, SiO 2 was 15 nm.
[0137] MnO 2 , TiO 2 The particle size of CuO refers to the median diameter in the particle size distribution measured using a laser diffraction particle size distribution analyzer, as in the case of glass powder. That is, the particle size refers to the 50% volume cumulative particle size.
[0138] SiO 2 The specific surface area of SiO was measured by the BET method, and specifically, it was calculated in the same manner as the specific surface area diameter of the ruthenium oxide powder described above. 2 The density ρ is 2.2 g / cm 3 (2) Thick Film Resistor Paste To the thick film resistor composition of each Example, 43 parts by mass of an organic vehicle was added to 100 parts by mass of the total of the ruthenium oxide powder, glass powder, and additives, and the mixture was dispersed using a three-roll mill to prepare a thick film resistor paste.
[0139] The organic vehicle used was a mixture of 5% by mass or more and 25% by mass or less of ethyl cellulose and 75% by mass or more and 95% by mass or less of terpineol. The proportions of the above components in the organic vehicle were adjusted within the above ranges so that the viscosity of the thick-film resistor pastes of Examples 1 to 10 was approximately the same value. (3) Thick-film Resistor The thick-film resistor paste prepared in each Example was printed between a pair of Ag / Pd electrodes, which were 1% by mass Pd and 99% by mass Ag thick films that had been previously formed on an alumina substrate (aluminum oxide substrate) by firing, to form a printed film (printing process).
[0140] The printed film obtained in the printing step was dried at 150° C. for 5 minutes (drying step).
[0141] Next, the printed film (dried film) obtained in the drying step was fired so that the peak temperature reached 850° C. and the holding time at the peak temperature was 9 minutes, thereby forming a thick film resistor (firing step).
[0142] The size of the thick film resistor was set to a resistor width of 1.0 mm and a resistor length (between electrodes) of 1.0 mm.
[0143] The thick film resistors thus obtained were evaluated as described above. The evaluation results are shown in Table 3.
[0144]
[0145]
[0146] [Comparative Examples 1 to 8] Thick film resistor compositions and thick film resistor pastes were prepared using the ruthenium oxide powder, glass powder, and additives shown in Table 4, with the addition amounts of each component being in the proportions shown in Table 4, in the same manner as in Examples 1 to 10. Thick film resistors were prepared and evaluated in the same manner as in Examples 1 to 10, except that the thick film resistor pastes prepared in each comparative example were used. The evaluation results are shown in Table 4.
[0147] According to the results shown in Tables 3 and 4, the thick film resistors of Examples 1 to 10 have both COLD-TCR and HOT-TCR within ±30 ppm / °C, which is close to 0, and the H / C difference is small, at 70 ppm / °C or less, so it was confirmed that a highly accurate temperature coefficient of resistance was achieved.
[0148] Furthermore, it was confirmed that the thick film resistors of Examples 1 to 10 had excellent characteristics, with a resistance change rate of within ±0.5% in a short time overload test (STOL) and sufficiently small current noise.
[0149] Therefore, it was confirmed that by using ruthenium oxide powder having a rutile crystal structure, an Lc / La ratio of 0.6913 or more, and a crystallite diameter of 10 nm or more and 80 nm or less, it is possible to bring the low-temperature temperature coefficient of resistance and the high-temperature temperature coefficient of resistance closer to 0 and to reduce the difference between them.
[0150] Furthermore, it was confirmed that because the crystallite diameter of the ruthenium oxide powder was 10 nm or more and 80 nm or less, the rate of change in resistance value in a short time overload test (STOL) was small, within ±0.5%.
[0151] On the other hand, the thick film resistors of Comparative Examples 1 to 7 used ruthenium oxide powder with an Lc / La ratio of less than 0.6913. Therefore, the thick film resistors obtained in these Comparative Examples tended to exhibit a large difference between the low-temperature temperature coefficient of resistance and the high-temperature temperature coefficient of resistance, and it was confirmed that it was not possible to keep both values within ±30 ppm / °C. Furthermore, in Comparative Examples 6 and 7, TiO 2 , MnO 2 It was confirmed that the temperature coefficient of resistance became significantly negative despite the absence of any additives.
[0152] In Comparative Example 8, the Lc / La of the ruthenium oxide powder used was 0.69181, and the COLD-TCR and HOT-TCR of the resulting thick film resistor were both within ±30 ppm / ° C. However, the crystallite diameter of the ruthenium oxide powder used was as large as 86.2 nm, and the coefficient of variation (CVR), which indicates the variation in resistance value of the resulting thick film resistor, exceeded 5%, and it was confirmed that the rate of change in resistance value in a short time overload test (STOL) exceeded ±0.5%.
[0153] From the results of the above examples and comparative examples, it was confirmed that by using ruthenium oxide powder with predetermined properties, it is possible to easily adjust the temperature coefficient of resistance to within ±30 ppm / °C, which was previously difficult to achieve, and that it is possible to produce a thick film resistor with a highly accurate temperature coefficient of resistance.
[0154] This application claims priority based on Japanese Patent Application No. 2022-119727 filed with the Japan Patent Office on July 27, 2022, the entire contents of which are incorporated herein by reference.
Claims
1. Ruthenium oxide powder having a rutile crystal structure, in which, when the lattice constant of the a-axis measured by X-ray diffraction is La and the lattice constant of the c-axis is Lc, the Lc / La ratio is 0.6913 or more, and the crystallite diameter is 10 nm or more and 80 nm or less.
2. A composition for a thick film resistor comprising ruthenium oxide powder and glass powder, wherein the ruthenium oxide powder has a rutile crystal structure, and wherein, when the lattice constant of the a-axis measured by X-ray diffraction is La and the lattice constant of the c-axis is Lc, Lc / La is 0.6913 or more, and the crystallite diameter is 10 nm or more and 80 nm or less.
3. A composition for a thick film resistor according to claim 2, wherein the mass ratio of the ruthenium oxide powder is 5% or more and 60% or less, when the total mass of the ruthenium oxide powder and the glass powder is 100%.
4. A composition for a thick film resistor according to claim 2 or 3, wherein the 50% volume cumulative particle size of the glass powder is 5 μm or less.
5. The glass powder is SiO 2 and B 2 O 3 and RO (R represents one or more alkaline earth elements selected from Ca, Sr, and Ba), and SiO 2 and B 2 O 3 and RO is 100 parts by mass, 2 20 parts by mass or more and 50 parts by mass or less, B 2 O 3 4. The composition for a thick film resistor according to claim 2, comprising 10 parts by mass or more and 30 parts by mass or less of the above compound and 35 parts by mass or more and 65 parts by mass or less of RO.
6. A paste for thick film resistors comprising ruthenium oxide powder, glass powder, and an organic vehicle, wherein the ruthenium oxide powder has a rutile crystal structure, and wherein, when the lattice constant of the a-axis measured by X-ray diffraction is La and the lattice constant of the c-axis is Lc, Lc / La is 0.6913 or more, and the crystallite diameter is 10 nm or more and 80 nm or less.
7. A paste for a thick film resistor according to claim 6, wherein the mass ratio of the ruthenium oxide powder is 5% or more and 60% or less when the total mass of the ruthenium oxide powder and the glass powder is 100%.
8. The glass powder is SiO 2 and B 2 O 3 and RO (R represents one or more alkaline earth elements selected from Ca, Sr, and Ba), and SiO 2 and B 2 O 3 and RO is 100 parts by mass, 2 20 parts by mass or more and 50 parts by mass or less, B 2 O 3 8. The paste for a thick film resistor according to claim 6, comprising 10 parts by mass or more and 30 parts by mass or less of the above compound and 35 parts by mass or more and 65 parts by mass or less of RO.
9. A thick film resistor formed from the thick film resistor composition according to claim 2 or 3.
10. The glass powder is SiO 2 and B 2 O 3 and RO (R represents one or more alkaline earth elements selected from Ca, Sr, and Ba), and SiO 2 and B 2 O 3 and RO is 100 parts by mass, 2 20 parts by mass or more and 50 parts by mass or less, B 2 O 3 10 parts by mass or more and 30 parts by mass or less of SiO and 35 parts by mass or more and 65 parts by mass or less of RO.