Paper strengthening agent and paper
Patent Information
- Application Number
- MYPI2025000683
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-16
- Filing Date
- 2023-09-06
- Publication Date
- 2024-03-16
AI Technical Summary
In the paper manufacturing industry, the decreasing strength of pulp fibers due to recycling and the reduced effectiveness of aluminum sulfate as a fixing agent in papermaking systems hinder the performance of (meth)acrylamide-based paper strength enhancers, necessitating a more effective solution to enhance paper strength.
A paper strength enhancer is developed by blending a (meth)acrylamide-based polymer with metal inorganic acid salts, such as titanium chloride or iron compounds, to create a mixture with specific viscosity and composition that improves paper strength when added to pulp slurry, reducing the need for aluminum sulfate and enhancing paper properties.
The proposed solution significantly enhances paper strength, achieving better results than previous methods by chemically interacting with the (meth)acrylamide-based polymer and metal inorganic acid salts, resulting in improved viscosity and paper quality.
Abstract
Description
Paper strength enhancer, paper
[0001] The present invention relates to a paper strength agent and paper.
[0002] Paper strength agents are chemicals used to increase the strength of paper itself. In particular, the papermaking industry is moving towards a closed papermaking system (recycling waste paper pulp, etc.), which means that the strength of the resulting paper is more likely to decrease due to a decrease in the strength of the pulp fibers used as raw materials. This makes paper strength agents increasingly important.
[0003] Incidentally, (meth)acrylamide polymers are widely used as paper strength agents, and are classified into anionic, cationic, and amphoteric types depending on their ionicity. Among these, amphoteric (meth)acrylamide polymers, which are the mainstream, are obtained by copolymerizing acrylamide with polymerizable monomers such as cationic monomers and anionic monomers (Patent Document 1).
[0004] When the polymer is added to the pulp slurry of a papermaking system, aluminum sulfate is added as a fixing agent before or after the addition of the polymer. However, as papermaking systems become more closed, the fixing effect of aluminum sulfate decreases. Furthermore, paper mills are also moving to reduce the amount of aluminum sulfate added due to environmental concerns, making it even more difficult for the paper strength agent itself to exert its paper strength effect. As a solution to this problem, a method has long been known in which a paper strength agent premixed with a (meth)acrylamide polymer and a water-soluble aluminum compound such as aluminum sulfate is added to the pulp slurry (Patent Documents 2 and 3). While such a mixed paper strength agent has the advantage of reducing the amount of aluminum sulfate added to the pulp slurry and increasing the paper strength effect, its effectiveness has been insufficient.
[0005] JP 2012-251252 A JP 2001-011787 A JP 8-226092 A
[0006] An object of the present invention is to provide a paper strength agent having excellent paper strength effects.
[0007] The present inventors have conducted extensive research and found that the above-mentioned problems can be solved by blending a specific metal inorganic acid salt with a (meth)acrylamide polymer, thereby completing the present invention. That is, the present invention relates to the following paper strength agent and paper.
[0008] 1. A paper strength agent comprising a mixture of a (meth)acrylamide polymer (A) containing, as essential components, (meth)acrylamide (a1), a polymerizable monomer (a2) having an amino group, and a polymerizable monomer (a3) having a carboxy group, and a metal inorganic acid salt (B) containing a divalent or trivalent metal atom with an atomic weight of 30 to 80.
[0009] 2. The paper strength agent according to the preceding paragraph 1, wherein the viscosity of the mixture (at 25°C) when made into an aqueous solution (pH = 6) containing 1% by weight of component (A) in terms of nonvolatile content is 5 mPa s or more and 5,000 mPa s or less.
[0010] 3. The paper strength agent according to item 1 or 2 above, wherein the constituent components further comprise a polymerizable monomer (a4) having a sulfonic acid group and / or a polymerizable monomer (a5) having a crosslinkable group.
[0011] 4. The paper strength agent according to item 1 or 2 above, wherein component (B) is at least one selected from the group consisting of titanium chloride, titanium sulfate, titanium phosphate, iron nitrate, iron chloride, polyiron chloride, iron sulfate, polyiron sulfate, iron phosphate, polyiron phosphate, iron silicate, and polyiron silicate.
[0012] 5. The paper strength agent according to item 1 or 2 above, wherein the mixture further contains a water-soluble aluminum compound (C).
[0013] 6. Paper containing the paper strength agent according to the preceding paragraph 1 or 2.
[0014] The paper strength agent of the present invention exhibits excellent paper strength when made into paper.
[0015] The paper strength agent of the present invention comprises a mixture of a (meth)acrylamide polymer (A) (hereinafter referred to as component (A)), which contains as essential components (meth)acrylamide (a1) (hereinafter referred to as component (a1)), a polymerizable monomer (a2) having an amino group (hereinafter referred to as component (a2)), and a polymerizable monomer (a3) having a carboxy group (hereinafter referred to as component (a3)), and a metal inorganic acid salt (B) (hereinafter referred to as component (B)), which contains a divalent or trivalent metal atom with an atomic weight of 30 to 80.
[0016] The component (a1) is methacrylamide or acrylamide, which may be used alone or in combination.
[0017] The molar ratio of the component (a1), with all constituent components taken as 100 mol %, is preferably 50 to 99.45 mol %, more preferably 61 to 98.88 mol %, and even more preferably 68 to 97.48 mol %.
[0018] The component (a2) is a polymerizable monomer having an amino group. Examples of the component (a2) include polymerizable monomers having a primary amino group, polymerizable monomers having a secondary amino group, polymerizable monomers having a tertiary amino group, and quaternary salts of these polymerizable monomers. These may be used alone or in combination of two or more.
[0019] Examples of polymerizable monomers having a primary amino group include vinylamine, allylamine, etc. These may be used alone or in combination of two or more.
[0020] Examples of the polymerizable monomer having a secondary amino group include diallylamine, etc. These may be used alone or in combination of two or more.
[0021] Examples of polymerizable monomers having a tertiary amino group include (meth)acrylates having a tertiary amino group, such as N,N-dimethylaminoethyl (meth)acrylate and N,N-diethylaminoethyl (meth)acrylate, and (meth)acrylamides having a tertiary amino group, such as N,N-dimethylaminopropyl (meth)acrylamide and N,N-diethylaminopropyl (meth)acrylamide. These may be used alone or in combination of two or more.
[0022] The quaternized salts of these monomers refer to those obtained by reacting the polymerizable monomer having a primary amino group, the polymerizable monomer having a secondary amino group, or the polymerizable monomer having a tertiary amino group with a quaternizing agent, and the quaternized salts may be inorganic acid salts such as hydrochlorides and sulfates, or organic acid salts such as acetates. Examples of the quaternizing agent include methyl chloride, benzyl chloride, dimethyl sulfate, epichlorohydrin, and the like. These may be used alone or in combination of two or more.
[0023] Among these components (a2), it is preferable to include a (meth)acrylate having a tertiary amino group and / or a quaternary salt of the (meth)acrylate. Note that "(meth)acrylate" means methacrylate or acrylate (the same applies hereinafter).
[0024] The molar ratio of the component (a2) is preferably 0.5 to 20 mol %, more preferably 1 to 18 mol %, and even more preferably 2 to 16 mol %, with the total of all constituent components being 100 mol %.
[0025] The component (a3) is a polymerizable monomer having a carboxy group. Examples of the component (a3) include (meth)acrylic acid, acrylic anhydride, 2-(meth)acrylamido-N-glycolic acid, N-(meth)acryloylglycine, 3-(meth)acrylamidopropanoic acid, 4-(meth)acrylamidobutanoic acid, itaconic acid, itaconic anhydride, fumaric acid, maleic acid, and maleic anhydride. These components (a3) may be used in the form of salts such as alkali metal salts (e.g., sodium, potassium, etc.); ammonium salts (e.g., ammonia, etc.); and organic amine salts (e.g., trimethylamine, triethylamine, trimethanolamine, and triethanolamine, etc.). These may be used alone or in combination of two or more. Among these, (meth)acrylic acid, acrylic anhydride, 2-(meth)acrylamido-N-glycolic acid, and itaconic acid are preferred.
[0026] The molar ratio of the component (a3) is preferably 0.05 to 20 mol %, more preferably 0.1 to 15 mol %, and even more preferably 0.5 to 12 mol %, with the total of all constituent components being 100 mol %.
[0027] The above-mentioned constituent components may further contain a polymerizable monomer (a4) having a sulfonic acid group (hereinafter also referred to as component (a4)).
[0028] The component (a4) is a polymerizable monomer having a sulfonic acid group. Examples of the component (a4) include vinyl sulfonic acid, methallyl sulfonic acid, and p-styrene sulfonic acid. These components (a4) may be used in the form of a salt such as an alkali metal salt (e.g., sodium or potassium) or an ammonium salt. These may be used alone or in combination of two or more.
[0029] The molar ratio of the component (a4) is preferably 5 mol % or less, more preferably 0.01 to 3 mol %, and even more preferably 0.01 to 2 mol %, with the total of all constituent components being 100 mol %.
[0030] The above-mentioned constituent components may further contain a polymerizable monomer (a5) having a crosslinkable group (hereinafter also referred to as component (a5)).
[0031] Examples of the component (a5) include N-alkyl(meth)acrylamides such as N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, and N-t-butyl(meth)acrylamide; N,N-dialkyl(meth)acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, and N,N-diisopropyl(meth)acrylamide; N,N'-alkylenebis(meth)acrylamides such as N,N'-methylenebis(meth)acrylamide and N,N'-ethylenebis(meth)acrylamide; crosslinkable monomers having a triallyl group such as triallyl isocyanurate, triallyl trimellitate, triallylamine, and triallyl(meth)acrylamide; and triazines having a (meth)acryloyl group such as 1,3,5-triacryloyl-1,3,5-triazine and 1,3,5-triacryloylhexahydro-1,3,5-triazine. These may be used alone or in combination of two or more. Among these, N,N-dimethyl(meth)acrylamide and N,N'-methylenebis(meth)acrylamide are preferred.
[0032] The molar ratio of the component (a5) is preferably 5 mol % or less, more preferably 0.01 to 3 mol %, and even more preferably 0.01 to 2 mol %, with the total of all constituent components being 100 mol %.
[0033] The constituent components may further include a monomer (a6) (hereinafter referred to as component (a6)) other than the components (a1) to (a5).
[0034] Examples of component (a6) include polymerizable monomers having an aromatic ring, such as styrene, α-methylstyrene, and vinyltoluene; alkyl (meth)acrylates, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate; vinyl carboxylates, such as vinyl acetate and vinyl propionate; nitriles, such as acrylonitrile; mercaptans, such as 2-mercaptoethanol and n-dodecyl mercaptan; alcohols, such as ethanol, isopropyl alcohol, and n-pentyl alcohol; aromatic compounds, such as α-methylstyrene dimer, ethylbenzene, isopropylbenzene, and cumene; and carbon tetrachloride. These may be used alone or in combination of two or more. Furthermore, the molar ratio of component (a6), based on 100 mol% of all constituents, is preferably 10 mol% or less, more preferably 8 mol% or less, and even more preferably 5 mol% or less.
[0035] In producing a (meth)acrylamide polymer, additives such as organic acids such as acetic acid, propionic acid, butanoic acid, citric acid, succinic acid, oxalic acid, glycolic acid, and glyoxylic acid; inorganic acids such as hydrochloric acid, sulfuric acid, and phosphoric acid; inorganic acid salts not belonging to the component (B) described below, such as sodium sulfate, potassium sulfate, and ammonium sulfate; inorganic bases such as sodium hydroxide, potassium hydroxide, and calcium hydroxide; starches such as oxidized starch, starch phosphate, urea phosphate, etherified starch, crosslinked starch, APS-modified starch, enzyme-modified starch, cationized starch, and amphoteric starch; polyvinyl alcohol, urea, antifoaming agents, antioxidants, preservatives, and bactericides may be added. These may be used alone or in combination of two or more, and the content thereof is preferably 10 parts by weight or less, and more preferably 5 parts by weight or less, per 100 parts by weight of all constituents.
[0036] The (meth)acrylamide polymer of the present invention can be obtained by appropriately adjusting the amounts of the components (a1) to (a6) used.
[0037] The (meth)acrylamide polymer is obtained by polymerizing the components (a1), (a2), and (a3) as essential components, and optionally the components (a4), (a5), and (a6), and the additives, in a solvent in the presence of a polymerization initiator.
[0038] Examples of the polymerization method include a method using only a dropping polymerization method, a method using only a simultaneous polymerization method (charging a monomer mixture all at once), and a method combining a simultaneous polymerization method and a dropping polymerization method.
[0039] The dropping polymerization method is a method of dropping a monomer mixture into a reaction system that has been charged with a solvent such as water in advance, and examples of methods that use only this polymerization method include the following (1) to (3). The dropping may be continuous, or may be stopped midway and allowed to polymerize for a certain period of time before restarting the dropping. (1) A method of dropping a monomer mixture in which all the monomer components are mixed. (2) A method of separately preparing two or more types of monomer mixtures and then dropping them simultaneously. (3) A method of separately preparing two or more types of monomer mixtures and then dropping them sequentially.
[0040] Examples of methods combining the simultaneous polymerization method and the dropping polymerization method include the following (4) to (7): (4) A method in which the respective monomer mixtures are separately simultaneously polymerized, and then the respective polymers are mixed; (5) A method in which the remaining monomer mixture is added dropwise after the simultaneous polymerization of one or more monomer mixtures is completed; (6) A method in which the remaining monomer mixture is added dropwise during the simultaneous polymerization of one or more monomer mixtures, and then polymerized; (7) A method in which one or more monomer mixtures are dropwise polymerized, and then the remaining monomer mixture is added all at once, and then polymerized simultaneously.
[0041] Examples of the solvent include water and organic solvents, which may be used alone or in combination of two or more. Examples of water include tap water, pure water, ultrapure water, ion-exchanged water, and industrial water. Examples of the organic solvent include alcohols such as methanol, ethanol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, sec-butyl alcohol, t-butyl alcohol, isobutyl alcohol, n-hexyl alcohol, n-octyl alcohol, ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, and diacetone alcohol; and ethers such as ethylene glycol monobutyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether. The content of the solvent is adjusted so that the polymerization concentration is preferably 5 to 50% by weight, more preferably 10 to 35% by weight.
[0042] Examples of polymerization initiators include persulfates such as ammonium persulfate, potassium persulfate, and sodium persulfate; azo compounds such as 2,2'-azobis(2-amidinopropane) hydrochloride and 2,2'-azobis[2(2-imidazolin-2-yl)propane] hydrochloride; and hydrogen peroxide. These may be used alone or in combination. Among these, ammonium persulfate, potassium persulfate, and 2,2'-azobis(2-amidinopropane) hydrochloride are preferred from the viewpoint of ensuring sufficient progress of solution polymerization. The method of adding the polymerization initiator is not particularly limited, and can be selected as appropriate, such as all-at-once addition, divided addition, or continuous dropwise addition. The content of the polymerization initiator is also not particularly limited, and is typically about 0.001 to 5 parts by weight, and preferably about 0.01 to 1 part by weight, per 100 parts by weight of all constituents.
[0043] As for polymerization conditions, for example, the reaction temperature is usually 50 to 100° C. (preferably 60 to 90° C.) and the reaction time is usually 1 to 10 hours (preferably 1 to 6 hours).
[0044] The physical properties of the resulting component (A) include, for example, a weight-average molecular weight of typically 1,000,000 to 10,000,000, and preferably 1,500,000 to 7,000,000, in order to ensure that the paper strength agent is likely to have excellent paper strength effects. The "weight-average molecular weight" here refers to a value obtained by gel permeation chromatography (GPC).
[0045] The viscosity of component (A) is typically 1,000 to 20,000 mPa s, and preferably 3,000 to 15,000 mPa s. Here, the "viscosity" refers to the value measured with a Brookfield viscometer on a solution with a solids concentration of 20% by weight, which has been adjusted to a temperature of 25°C.
[0046] The component (A) may be one type, or two or more different types of component (A) that have been separately produced may be used in combination.
[0047] In the present invention, a (meth)acrylamide polymer (A') (hereinafter referred to as component (A')) that does not belong to component (A) may also be used in combination. Component (A') refers to a polymer that does not contain component (a2) and / or component (a3) as constituent components.
[0048] Component (B) is a metal inorganic acid salt having a divalent or trivalent metal atom with an atomic weight of 30 to 80. When component (B) is added, it chemically interacts with component (A) to increase the viscosity of the resulting paper strength agent, allowing paper with excellent paper strength to be obtained.
[0049] Examples of the metal atoms include calcium, scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, and gallium.
[0050] Examples of inorganic acid salts include nitrates, hydrochlorides (hydrochlorides), polyhydrochlorides (polyhydrochlorides), sulfates, polysulfates, phosphates, polyphosphates, silicates (silica salts), and polysilicates (polysilica salts).
[0051] Any combination of the above-mentioned metal atom and inorganic acid salt can be used as component (B). A hydrate can also be used as component (B). These components (B) can be used alone or in combination of two or more. Among these, inorganic titanium acid salts and inorganic iron acid salts are preferred because they chemically interact with component (A) and tend to provide excellent paper strength. More preferred are at least one selected from the group consisting of titanium chloride, titanium sulfate, titanium phosphate, iron nitrate, iron chloride, polyiron chloride, iron sulfate, polyiron sulfate, iron phosphate, polyiron phosphate, iron silicate, and polyiron silicate.
[0052] The content of component (B) is preferably 0.01 to 50 parts by weight, more preferably 0.05 to 35 parts by weight, and even more preferably 0.1 to 20 parts by weight, of the nonvolatile content relative to 100 parts by weight of component (A), in order to facilitate the paper strength agent to have excellent paper strength effects. Here, the nonvolatile content refers to the components remaining after removing volatile components such as water and organic solvents (the same applies hereinafter).
[0053] The paper strength agent of the present invention may be a mixture further containing a water-soluble aluminum compound (C) (hereinafter referred to as component (C)). Examples include aluminum sulfate, aluminum chloride, basic aluminum sulfate, basic aluminum chloride, aluminum silicate, polyaluminum chloride, and polyaluminum hydroxide. A hydrate may also be used as component (C). These may be used alone or in combination of two or more. Among these, aluminum sulfate, aluminum chloride, and polyaluminum chloride are preferred because of their easy availability.
[0054] The content of component (C), in terms of nonvolatile weight, is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, and even more preferably 2 parts by weight or less, per 100 parts by weight of component (A).
[0055] The paper strength agent of the present invention may further contain additives such as inorganic acid salts not belonging to component (B), such as sodium sulfate, potassium sulfate, and ammonium sulfate; starches, such as oxidized starch, phosphated starch, urea phosphated starch, etherified starch, crosslinked starch, APS-modified starch, enzyme-modified starch, cationized starch, and amphoteric starch; and polyvinyl alcohol, urea, antifoaming agents, antioxidants, preservatives, and bactericides.
[0056] The paper strength agent of the present invention can be obtained as a mixture by stirring or mixing component (A) and component (B), and optionally component (A'), component (C), and the additives at room temperature. The mixture may be heated or cooled as needed during preparation. Regarding the mixing method, component (A) and component (B), and optionally component (A') and component (C), may be mixed as is, or one or more selected from component (A) and component (B), and optionally component (A') and component (C) may be diluted with water before mixing. Further dilution with water may be performed after mixing. When two or more different (meth)acrylamide polymers are used in combination as component (A), the polymers may be mixed with the aforementioned components all at once, or the (meth)acrylamide polymers to be used in combination may be mixed together (optionally with component (A')), and the remaining components may be added and mixed.
[0057] Examples of water include tap water, pure water, ultrapure water, ion-exchanged water, industrial water, etc. The non-volatile concentration of each component after dilution is preferably adjusted as follows, in order to obtain a paper strength agent with an appropriate viscosity while dispersing each component well: Component (A): preferably 0.1 to 10% by weight, more preferably 0.3 to 5% by weight Component (B): preferably 0.1 to 10% by weight, more preferably 0.3 to 5% by weight Component (C): preferably 0.1 to 10% by weight, more preferably 0.3 to 5% by weight
[0058] As for the physical properties of the resulting paper strength agent, when the mixture is made into an aqueous solution (pH = 6) containing 1% by weight of component (A) in nonvolatile concentration, the viscosity of the mixture (at 25°C) is preferably 5 mPa·s or more and 5000 mPa·s or less, more preferably 10 mPa·s or more and 3000 mPa·s or less, and even more preferably 15 mPa·s or more and 2000 mPa·s or less, in order to obtain a paper strength agent that has an appropriate viscosity and high paper strength effect while well dispersing each component. Note that the viscosity here is a value measured with a B-type viscometer.
[0059] When measuring the viscosity, for example, inorganic acids such as hydrochloric acid, sulfuric acid, phosphoric acid, etc.; inorganic bases such as sodium hydroxide, potassium hydroxide, calcium hydroxide, etc. can be used as pH adjusters to adjust the pH.
[0060] The paper of the present invention contains the paper strength agent, and its production method includes, for example, adding the paper strength agent to a raw pulp slurry (hereinafter also referred to as internal addition), spraying it onto the surface of a wet paper, or coating it on the surface of base paper. The paper strength agent may be used as is at the nonvolatile content concentration described above, but it can also be further diluted with water to adjust the nonvolatile content concentration to 0.1 to 10% by weight before use.
[0061] When the strength agent is added internally to the raw pulp slurry, the strength agent is added to the pulp slurry and paper is made. The amount of the strength agent (based on the nonvolatile content of component (A)) is about 0.01 to 4% by weight based on the dry weight of the pulp. Examples of pulp include chemical pulps such as hardwood pulp (LBKP) and softwood pulp (NBKP); mechanical pulps such as groundwood pulp (GP), refiner ground pulp (RGP), and thermomechanical pulp (TMP); and recycled paper pulp such as recycled corrugated cardboard. When the strength agent is added internally, other additives may be added, such as fixing agents, pH adjusters such as aluminum sulfate, sulfuric acid, and sodium hydroxide; papermaking chemicals such as sizing agents and wet strength agents; and fillers such as talc, clay, kaolin, titanium dioxide, and calcium carbonate.
[0062] When sprayed onto the surface of a wet paper, the paper strength agent is sprayed onto the surface of one or more layers of wet paper before the paper is combined, and then the paper is combined. The paper strength agent is diluted to a non-volatile content of about 0.1 to 7% by weight. The viscosity after dilution is about 2 to 50 mPa·s at 25°C (non-volatile content of 1.0% by weight at 25°C), and the amount used (in terms of non-volatile content) is usually 0.05 to 10% by weight of the total pulp (non-volatile weight).
[0063] When coating the surface of base paper, the paper strength agent is applied to the surface of the base paper by various known means. Here, the paper strength agent applied to the surface of the base paper is called the "coating liquid." The viscosity of the coating liquid is usually 1 to 50 mPa·s at a temperature of 50°C. As the type of base paper, uncoated paper made from wood cellulose fiber can be used, and as the coating means, for example, a bar coater, a knife coater, an air knife coater, a calendar, a gate roll coater, a blade coater, a two-roll size press, a rod metering, etc. can be mentioned. Furthermore, the amount of coating liquid applied (in terms of non-volatile content) is usually 0.001 to 2 g / m 2 about 0.005 to 1 g / m 2 That's about it.
[0064] The paper of the present invention can be used for a variety of products, such as coated base paper, newsprint, liner, medium, paper tube, printing and writing paper, form paper, PPC paper, cup base paper, inkjet paper, and thermal paper.
[0065] The present invention will be described below with reference to examples, but the present invention is not limited thereto. In the examples and comparative examples, "parts" and "%" are by weight unless otherwise specified.
[0066] The following compounds are abbreviated: AM: Acrylamide DM: N,N-dimethylaminoethyl methacrylate DML: N,N-dimethylaminoethyl methacrylate benzyl chloride BQ: N,N-dimethylaminoethyl acrylate benzyl chloride APDM: Dimethylaminopropyl acrylamide IA: Itaconic acid AA: Acrylic acid AGA: 2-acrylamido-N-glycolic acid SMAS: Sodium methallylsulfonate DMAA: N,N-dimethylacrylamide MBAA: N,N'-methylenebisacrylamide APS: Ammonium persulfate
[0067] Production Example 1 A reactor equipped with a stirrer, a thermometer, a reflux condenser, a nitrogen gas inlet tube, and three dropping funnels was charged with 276.5 parts of ion-exchanged water, and oxygen was removed from the reaction system by passing nitrogen gas through it, followed by heating to 90° C. 70.5 parts (21.3 mol %) of AM, 58.7 parts (8.0 mol %) of DM, 2.4 parts (0.40 mol %) of IA, 1.11 parts (0.15 mol %) of SMAS, 28.7 parts of 62.5% sulfuric acid, 0.23 parts (0.05 mol %) of DMAA, 0.36 parts (0.05 mol %) of MBAA, and 218.9 parts of ion-exchanged water were charged into the dropping funnel (1), and the pH was adjusted to around 3.0 with sulfuric acid (monomer mixed solution (I)). In addition, 203.9 parts (61.4 mol%) of AM, 58.7 parts (8.0 mol%) of DM, 2.4 parts (0.40 mol%) of IA, 1.11 parts (0.15 mol%) of SMAS, 0.23 parts (0.05 mol%) of DMAA, 0.36 parts (0.05 mol%) of MBAA, and 466.6 parts of ion-exchanged water were charged into the dropping funnel (2), and the pH was adjusted to about 3.0 with sulfuric acid (monomer mixture (II)). 0.6 parts of APS and 180 parts of ion-exchanged water were charged into the dropping funnel (3). Next, the catalyst in the system was added dropwise from the dropping funnel (3) over about 3 hours. In parallel, the monomer mixtures (I) and (II) from the dropping funnels (1) and (2) were added dropwise in this order at a constant flow rate over about 3 hours. After the dropwise addition was completed, 0.4 parts of APS and 10 parts of ion-exchanged water were added, and the mixture was kept warm for 1 hour. 580 parts of ion-exchanged water was then added to obtain an aqueous solution of component (A-1) with a non-volatile content of 20.0%. The molar ratios of all monomer components are shown in Table 1, and the molar ratios of the monomer components charged in each monomer mixture are shown in Table 2.
[0068] Production Examples 2 to 18 Using the compositions shown in Tables 1 and 2, synthesis was carried out in the same manner as in Production Example 1 to obtain aqueous solutions of paper strength agents with a non-volatile content of 20.0%.
[0069] <Viscosity> Using a Brookfield viscometer (manufactured by Toki Sangyo Co., Ltd.), the viscosity of component (A) of each production example adjusted to a temperature of 25° C. was measured. The results are shown in Table 2.
[0070] <Weight-Average Molecular Weight> The weight-average molecular weight of component (A) was measured by gel permeation chromatography (GPC) under the following measurement conditions. The results are shown in Table 2. Column: One guard column PWXL and two GMPWXL, manufactured by Tosoh Corporation. Eluent: Phosphate buffer solution (0.05 mol / L phosphoric acid (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) + 0.13 mol / L sodium dihydrogen phosphate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) aqueous solution, pH approximately 2.5). Flow rate: 0.8 ml / min. Temperature: 40°C. RI detector: Shodex RI-101, manufactured by Showa Denko K.K. MALS detector: DAWN HELEOS-II, manufactured by WYATT. Measurement sample: The sample was diluted with the above eluent so that the nonvolatile content of component (A) was 0.1%, and then measured.
[0071]
[0072]
[0073] Deionized water was added to the component (A) of each Production Example, and the components (B) and (C) shown in Table 2 so that the nonvolatile content of each was 2%. Note that for Example 6, an aqueous solution was used in which deionized water was added to the components (A-1) and (B-1) so that the nonvolatile content of each was 4%.
[0074] Example 1 500 parts of a 2% aqueous solution of component (A-1) (10.0 parts non-volatile content), 150 parts of a 2% aqueous solution of polyferric sulfate (trade name: "Polytetsu", manufactured by Nittetsu Mining Co., Ltd.) (3.0 parts non-volatile content), and 350 parts of ion-exchanged water were charged and mixed at room temperature for 30 minutes to obtain a paper strength agent.
[0075] Examples 2 to 5, 7 to 36 and Comparative Examples 1 to 4 The same procedure as in Example 1 was carried out except that the components and amounts used were changed as shown in Table 2, to obtain the respective paper strength agents.
[0076] Example 6 250 parts of a 4% aqueous solution of component (A-1) (10.0 parts nonvolatile content), 500 parts of a 4% aqueous solution of polyferric sulfate (trade name: "Polytetsu", manufactured by Nittetsu Mining Co., Ltd.) (20.0 parts nonvolatile content), and 250 parts of ion-exchanged water were charged and mixed at room temperature for 30 minutes to obtain a paper strength agent.
[0077] <Viscosity> Aqueous sodium hydroxide solution (non-volatile concentration: 10%, 5%, 1% in combination) was added to each paper strength agent to adjust the pH to 6, and then the temperature was adjusted to 25°C, and the viscosity was measured using a B-type viscometer (manufactured by Toki Sangyo Co., Ltd.). The results are shown in Table 3.
[0078] (Papermaking Evaluation 1: Evaluation by Difference in Paper Strengthening Agents) Waste corrugated cardboard was beaten in a Niagara beater, and calcium chloride was added to the pulp slurry adjusted to 350 ml of Canadian Standard Freeness (C.S.F.) to adjust the electrical conductivity to 2.0 mS / cm. Aluminum sulfate was added to this slurry in an amount of 1.0% (non-volatile content) based on the non-volatile content weight of the pulp slurry and stirred for 30 seconds, after which each of the above paper strength enhancing agents was added in an amount of 1.0% (non-volatile content) of component (A) based on the non-volatile content weight of the pulp slurry. The pH of each pulp slurry was adjusted to 6.5 and evaluated. The slurry was dewatered in a tapping sheet machine and subjected to a pressure of 5 kg / cm. 2 Pressed for 2 minutes at 150 g / m² 2 The sheets were then dried in a rotary dryer at 105°C for 4 minutes and then conditioned at 23°C and 50% humidity for 24 hours to obtain Paper 1. The formation, burst strength, tensile strength and compressive strength of Paper 1 were measured using the following methods. The results are shown in Table 3.
[0079] <Electrical conductivity> Measured using a pH / COND METER D-54 (manufactured by Horiba, Ltd.). <Formation (formation variation coefficient)> The light (brightness) transmitted through the paper obtained above was input into a commercially available measuring device (trade name "Personal Image Processing System Hyper-700", manufactured by OBS), and the value obtained by statistically analyzing the brightness distribution was taken as the formation variation coefficient. The smaller the value of the formation variation coefficient, the better the formation. <Burst Ratio> Using the paper obtained above, the burst ratio (kPa m 2 <Tensile strength> Using the paper obtained above, the tensile strength (N·m / g) was measured in accordance with JIS P 8113. <Compressive strength> Using the paper obtained above, the compressive strength (N·m 2 / g) was measured.
[0080]
[0081] The symbols in Table 3 represent the following components. <Component (A)> A-1 to A-18: Acrylamide polymers of Production Examples 1 to 18 (composite in the same order) <Component (B)> B-1: Polyferric sulfate (trade name: "Polytetsu", manufactured by Nittetsu Mining Co., Ltd.) B-2: Iron (III) chloride (trade name: "Ferric Chloride Liquid", manufactured by Taiki Pharmaceutical Co., Ltd.) B-3: Polysilica iron (trade name: "PSI-025", manufactured by Naoji Pharmaceutical Co., Ltd.) B-4: Titanium (IV) sulfate (n-hydrate) (manufactured by Kishida Chemical Co., Ltd.) <Component (C)> C-1: Aluminum sulfate (liquid aluminum sulfate, manufactured by Asada Chemical Co., Ltd.) C-2: Polyaluminum chloride (manufactured by Asada Chemical Co., Ltd.) <Component (D)> D-1: Zirconium sulfate (tetrahydrate) (manufactured by Kishida Chemical Co., Ltd.)
[0082] (Papermaking Evaluation 2: Evaluation by Difference in Chemical Addition Order) Evaluation Example 1, Comparative Evaluation Examples 1 to 3 Waste corrugated cardboard was beaten in a Niagara beater, and calcium chloride was added to the pulp slurry adjusted to 350 ml of Canadian Standard Freeness (C.S.F.) to adjust the electrical conductivity to 2.0 mS / cm. Aluminum sulfate was added to this slurry in an amount of 1.0% (non-volatile content) based on the weight of the non-volatile content of the pulp slurry, and 15 seconds, 30 seconds, and 45 seconds after that point, the components listed in Table 4 were added and stirred. The pH of each pulp slurry was adjusted to 6.5 and evaluated. The pulp slurry was dewatered in a tapping sheet machine and 5 kg / cm 2 Pressed for 2 minutes at 150 g / m² 2 The paper was then dried in a rotary dryer at 105°C for 4 minutes and then conditioned at 23°C and 50% humidity for 24 hours to obtain Paper 2. The formation, burst strength, tensile strength and compressive strength of Paper 2 were measured in the same manner as above. The results are shown in Table 4.
[0083] *1: Expressed as the amount of non-volatile content of component (A-1) used.
[0084] The symbols shown in Table 4 represent the following components: Example 1: Paper strength agent of Example 1 A-1: Acrylamide polymer of Production Example 1 B-1: Polyferric sulfate (trade name: "Polytetsu", manufactured by Nittetsu Mining Co., Ltd.)
[0085] Table 4 shows that the paper strength agent (Example 1) which was a mixture of components (A) and (B) exhibited superior paper strength effects compared to when components (A) and (B) were added separately to the pulp slurry.
Claims
1. A paper strength agent comprising a mixture of a (meth)acrylamide polymer (A) having as essential components (meth)acrylamide (a1), a polymerizable monomer (a2) having an amino group, and a polymerizable monomer (a3) having a carboxy group, and a metal inorganic acid salt (B) having a divalent or trivalent metal atom with an atomic weight of 30 to 80.
2. A paper strength agent as described in claim 1, wherein the viscosity of the mixture (at 25°C) when made into an aqueous solution (pH = 6) containing 1% by weight of component (A) in non-volatile concentration is 5 mPa·s or more and 5000 mPa·s or less.
3. A paper strength agent according to claim 1 or 2, wherein the constituent components further comprise a polymerizable monomer (a4) having a sulfonic acid group and / or a polymerizable monomer (a5) having a crosslinkable group.
4. A paper strength agent according to claim 1 or 2, wherein component (B) is one or more selected from the group consisting of titanium chloride, titanium sulfate, titanium phosphate, iron nitrate, iron chloride, polyiron chloride, iron sulfate, polyiron sulfate, iron phosphate, polyiron phosphate, iron silicate, and polyiron silicate.
5. The paper strength agent according to claim 1 or 2, wherein the mixture further contains a water-soluble aluminum compound (C).
6. Paper containing the paper strength agent according to claim 1 or 2.