Plated steel sheet

MYPI2025000685A0Undetermined Publication Date: 2024-02-18NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025000685
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-08-18
Filing Date
2023-06-07
Publication Date
2024-02-18

AI Technical Summary

Technical Problem

Existing plated steel sheets fail to achieve high levels of both plane corrosion resistance and end face corrosion resistance simultaneously, as improving one often compromises the other.

Method used

A plated steel sheet with a Zn-Al-Mg alloy layer containing specific chemical compositions and Mg21Zn25 phases, which are preferentially corroded to form protective corrosion products, enhancing end face corrosion resistance without compromising plane corrosion resistance.

Benefits of technology

The solution provides both excellent plane and end face corrosion resistance by ensuring the Mg21Zn25 phase is present in the surface layer, forming corrosion products that protect the steel plate's end faces without impairing the plating layer's corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025000685_DRAWING_001
    Figure PI2025000685_DRAWING_001
Patent Text Reader

Abstract

ABSTRACT PLATED STEEL SHEET The plated steel sheet comprises: a steel sheet; and a plated layer arranged on a surface of the steel sheet, wherein the plated layer comprises, as a chemical composition, Al: 10.0% to 25.0%, Mg: 3.0% to 10.0%, Fe: 0.01% to 2.00%, Si: more than 0.00% and 2.00% or less, and a remainder comprising Zn and impurities, and when the plated layer is subjected to grazing incidence X-ray diffraction measurement under conditions where Cu-Kα ray is used, an acceleration voltage as an X-ray output is 50 kV, and an X-ray incident angle against a surface of the plated layer is 1°, an X-ray diffraction intensity ratio between a (300) plane of a Mg21Zn25 phase and a (002) plane of an η-Zn phase (I (Mg21Zn25) / I (η-Zn)) is more than 0.3.
Need to check novelty before this filing date? Find Prior Art

Description

Plated steel sheet

[0001] This application claims priority to Japanese Patent Application No. 2022-130521, filed on August 18, 2022, the contents of which are incorporated herein by reference.

[0002] Zn-Al-Mg hot-dip plated steel sheets having a hot-dip Zn coating layer containing Al and Mg have excellent corrosion resistance, and are therefore widely used as materials for structural members that require corrosion resistance, such as building materials.

[0003] For example, Patent Document 1 describes a plated steel material having a steel material and a plating layer including a Zn—Al—Mg alloy layer disposed on the surface of the steel material, wherein the Zn—Al—Mg alloy layer has a Zn phase and the Zn phase contains an Mg—Sn intermetallic compound phase, and the plating layer contains, in mass %, more than 65.0% Zn, more than 5.0% but less than 25.0% Al, more than 3.0% but less than 12.5% ​​Mg, 0.1% to 20.0% Sn, and impurities, and has a chemical composition that satisfies the following formulas 1 to 5: Formula 1: Bi + In < Sn Formula 2: Y + La + Ce ≦ Ca Formula 3: Si < Sn Formula 4: O ≦ Cr + Ti + Ni + Co + V + Nb + Cu + Mn < 0.25 Formula 5: O ≦ Sr + Sb + Pb + B < 0.5

[0004] Patent Document 2 discloses a plated steel material having a steel material and a plating layer including a Zn—Al—Mg alloy layer disposed on the surface of the steel material, in which the cross section of the Zn—Al—Mg alloy layer is 2 Phase area fraction is 45-75%, MgZn 2 The total area fraction of the Zn-Al-MgZn phase and the Al phase is 70% or more, and 2The area fraction of the ternary eutectic structure is 0 to 5%, and the plating layer is composed of, by mass%, Zn: more than 44.90% to less than 79.90%, Al: more than 15% to less than 35%, Mg: more than 5% to less than 20%, Ca: 0.1% to less than 3.0%, and impurities, and when element group A is Y, La, and Ce, element group B is Cr, Ti, Ni, Co, V, Nb, Cu, and Mn, element group C is Sr, Sb, and Pb, and element group D is Sn, Bi, and In, The document describes a plated steel material having a chemical composition in which the total content of elements selected from element group A is 0% to 0.5%, the total content of Ca and the elements selected from element group A is 0.1% to less than 3.0%, the total content of elements selected from element group B is 0% to 0.25%, the total content of elements selected from element group C is 0% to 0.5%, and the total content of elements selected from element group D is 0% to 20.00%.

[0005] Patent Document 3 describes a hot-dip Al-Zn-Mg-Si plated steel sheet having a plating film on the surface of the steel sheet, the plating film comprising an interfacial alloy layer present at the interface with the base steel sheet and a main layer present on the alloy layer, and containing 25 to 80 mass% Al, more than 0.6 to 15 mass% Si, and more than 0.1 to 25 mass% Mg, and the Mg on the surface of the main layer 2 A hot-dip Al-Zn-Mg-Si plated steel sheet having an area ratio of Si of 10% or more is described.

[0006] In recent years, hot-dip galvanized steel for building applications such as roofing and wall materials is required to have both excellent flat corrosion resistance, which is the corrosion resistance of the coating layer itself, and excellent edge corrosion resistance, which is the corrosion resistance of the cut edge. However, no technology has been developed that can achieve high levels of both flat corrosion resistance and edge corrosion resistance.

[0007] International Publication No. 2018 / 139619 International Publication No. 2018 / 139620 Japanese Patent Application Laid-Open No. 2016-166414

[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a plated steel sheet that is excellent in both flat corrosion resistance and edge corrosion resistance.

[0009] In order to solve the above problems, the present invention employs the following configuration: [1] A steel sheet and a plating layer disposed on a surface of the steel sheet, wherein the chemical composition of the plating layer contains, in mass %, Al: 10.0 to 25.0%, Mg: 3.0 to 10.0%, Fe: 0.01 to 2.00%, Si: more than 0.00% but not more than 2.00%, and one or more elements selected from the group consisting of Group A, Group B, and Group C below, with the balance consisting of Zn and impurities, wherein grazing incidence X-ray diffraction measurement of the plating layer is performed using Cu-Kα radiation under conditions of an X-ray output, an acceleration voltage of 50 kV, and an X-ray incident angle to the surface of the plating layer of 1°, and wherein Mg is 21 Zn 25 The X-ray diffraction intensity ratio (I(Mg 21 Zn 25 ) / I(η-Zn)) is greater than 0.3. [Group A] Ni: 0-1.000% [Group B] Ca: 0-0.05% [Group C] Sb: 0-0.50%, Pb: 0-0.50%, Cu: 0-1.00%, Sn: 0-1.00%, Ti: 0-1.00%, Cr: 0-1.00%, Nb: 0-1.00%, Zr: 0-1.00%, Mn: 0-1.00%, Mo: 0-1.00%, Ag: 0-1.00%, Li: 0-1.00%, La: 0-0.50%, Ce: 0-0.50%, B: 0-0.50%, Y: 0-0.50%, P: 0-0.50%, [2] The chemical composition of the plating layer contains, in mass%, Mg: 4.5% or more, and the X-ray diffraction intensity ratio (I(Mg 21 Zn 25 [3] The plated steel sheet according to [1], wherein the chemical composition of the plated layer contains, in mass %, 4.5% or more of Mg, and the X-ray diffraction intensity ratio (I(Mg 21 Zn 25[4] The plated steel sheet according to [1], wherein the chemical composition of the plated layer contains, in mass %, 4.5% or more of Mg, and the X-ray diffraction intensity ratio (I(Mg 21 Zn 25 [5] The plated steel sheet according to [1], wherein the chemical composition of the plating layer contains, in mass %, Sn: 0.05 to 0.5%, and X-ray diffraction measurement of the plating layer by the θ-2θ method reveals that the plating layer contains Mg 2 [6] The plated steel sheet according to any one of [1] to [4], in which a Sn phase is detected. [6] The plated steel sheet according to any one of [1] to [4], in which the chemical composition of the plating layer contains Group A. [7] The plated steel sheet according to any one of [1] to [4], in which the chemical composition of the plating layer contains Group B. [8] The plated steel sheet according to any one of [1] to [4], in which the chemical composition of the plating layer contains Group C.

[0010] According to the present invention, a plated steel sheet having excellent corrosion resistance on both the flat surface and the edge surface can be provided.

[0011] 1 is a cross-sectional schematic view of a hot-dip plated steel material according to an embodiment of the present invention. FIG.

[0012] When a plated steel sheet is cut, the edge of the steel sheet is exposed at the cut edge of the plated steel sheet. The corrosion resistance of this edge of the steel sheet (hereinafter referred to as edge corrosion resistance) is generally achieved as follows: A plating layer containing an element (e.g., Zn, Mg, etc.) with a higher ionization tendency than the base steel is formed on the surface of the steel sheet, and the plating layer corrodes preferentially relative to the base steel to generate corrosion products, which then protect the edge of the steel sheet from corrosion. Therefore, improving edge corrosion resistance by the plating layer and improving planar corrosion resistance, which is the corrosion resistance of the plating layer itself, are mutually exclusive.

[0013] Therefore, the present inventors have conducted extensive research to improve both the planar corrosion resistance and the edge corrosion resistance of a plating layer containing Al and Mg. In a plating layer containing Al, Mg, Si, and Zn, various Mg-Zn compounds containing Mg and Zn are formed. Among these Mg-Zn compounds, Mg 21 Zn 25 contains a relatively large amount of Mg, which can contribute to the corrosion resistance of the steel sheet end surface. 21 Zn 25 As a result of further investigation by the present inventors, it was found that by adjusting the manufacturing conditions of the plating layer, Mg 21 Zn 25 It was found that a large amount of Mg can be crystallized on the surface of the plating layer, thereby improving the corrosion resistance of the edge. 21 Zn 25 The presence of many Mg phases prevents corrosion of the plating layer from the early stage. 21 Zn 25 The phase becomes corroded. 21 Zn 25 As the phase corrodes, Mg ions are produced as corrosion products, and these Mg ions protect the end surface of the steel sheet from corrosion.

[0014] Also, Mg 21 Zn 25 Since there are many Mg phases on the surface of the plating layer, Mg 21 Zn 25 Since the corrosion products of the phases improve the edge corrosion resistance, the edge corrosion resistance can be increased without sacrificing the flat corrosion resistance of the plating layer, thereby achieving both flat corrosion resistance and edge corrosion resistance of the plating layer.

[0015] Hereinafter, a plated steel sheet according to an embodiment of the present invention will be described. The plated steel sheet according to this embodiment includes a steel sheet and a plating layer disposed on the surface of the steel sheet, and the plating layer has a chemical composition, in mass %, of Al: 10.0 to 25.0%, Mg: 3.0 to 10.0%, Fe: 0.01 to 2.00%, and Si: more than 0.00% but not more than 2.00%, and further contains one or more elements selected from the group consisting of Group A, Group B, and Group C below, with the balance consisting of Zn and impurities. When a glancing angle incidence X-ray diffraction measurement was performed on the plating layer using Cu-Kα radiation under conditions of an X-ray output, accelerating voltage, of 50 kV, and an X-ray incident angle to the surface of the plating layer of 1°, it was found that Mg 21 Zn 25 The X-ray diffraction intensity ratio (I(Mg 21 Zn 25 ) / I(η-Zn)) is greater than 0.3.

[0016] [Group A] Ni: 0-1.000% [Group B] Ca: 0-0.05% [Group C] Sb: 0 to 0.50%, Pb: 0 to 0.50%, Cu: 0 to 1.00%, Sn: 0 to 1.00%, Ti: 0 to 1.00%, Cr: 0 to 1.00%, Nb: 0-1.00%, Zr: 0-1.00%, Mn: 0-1.00%, Mo: 0-1.00%, Ag: 0-1.00%, Li: 0-1.00%, La: 0- 0.50%, Ce: 0 to 0.50%, B: 0 to 0.50%, Y: 0 to 0.50%, P: 0 to 0.50%, Sr: 0 to 0.50%, Co: 0 to 0.500%, Bi: 0 to 0.500%, In: 0 to 0.500%, V: 0 to 0.500%, and W: 0 to 0.500%, with a total of 0 to 5.000% of one or more of the above.

[0017] In the following description, the "%" used to indicate the content of each element in the chemical composition means "mass %." The numerical ranges described below, separated by "to" include the lower and upper limits. Values ​​marked with "less than" and "more than" do not include the numerical range. The content of elements in the chemical composition may be expressed as element concentration (e.g., Zn concentration, Mg concentration, etc.). "Plane corrosion resistance" refers to the corrosion-resistant properties of the coating layer (specifically, the Zn-Al-Mg alloy layer) itself. "Edge corrosion resistance" refers to the property of inhibiting corrosion of the steel sheet at the exposed portion of the steel sheet (e.g., the cut edge of the coated steel sheet). "Coating layer" refers to a coating film produced by a so-called hot-dip coating process.

[0018] As shown in Fig. 1 , the plated steel sheet 1 according to this embodiment has a steel sheet 11. There are no particular limitations on the shape of the steel sheet 11. The steel sheet 11 may also be a base steel sheet that has been formed into, for example, steel pipes, civil engineering and construction materials (fences, corrugated pipes, drainage ditch covers, sand-flying prevention plates, bolts, wire mesh, guardrails, water cut-off walls, etc.), home appliance components (casings for air conditioner outdoor units, etc.), automobile parts (suspension components, etc.), etc. The forming process may be any of various plastic processing techniques, such as pressing, roll forming, and bending.

[0019] The material of the steel plate 11 is not particularly limited. The steel plate 11 can be various steel plates such as general steel, Al-killed steel, ultra-low carbon steel, high carbon steel, various high-tensile steels, and some high-alloy steels (steels containing strengthening elements such as Ni and Cr). The steel plate 11 may also be a hot-rolled steel plate, hot-rolled steel strip, cold-rolled steel plate, or cold-rolled steel strip described in JIS G 3302:2010. There are also no particular limitations on the manufacturing method of the steel plate (hot rolling method, pickling method, cold rolling method, etc.) and the specific manufacturing conditions thereof.

[0020] As will be described later, a steel sheet 11 with adjusted surface roughness is used as the steel sheet to be used as the base sheet for plating. The surface roughness of the steel sheet can be adjusted, for example, by adjusting the surface of a reduction roll or a roll for skin pass to a predetermined surface roughness and then transferring the surface shape of the roll during rolling or skin pass.

[0021] The plated steel sheet 1 according to this embodiment has a plating layer 12 disposed on the surface of a steel sheet 11. The plating layer 12 of the plated steel sheet 1 according to this embodiment is mainly composed of a Zn—Al—Mg alloy layer due to its chemical composition, which will be described later. The plating layer 12 of the plated steel sheet 1 according to this embodiment may also include an interfacial alloy layer containing Fe and Al as main components between the steel sheet 11 and the Zn—Al—Mg alloy layer. That is, the plating layer 12 may have a single-layer structure of a Zn—Al—Mg alloy layer, or a laminate structure including a Zn—Al—Mg alloy layer and an interfacial alloy layer.

[0022] The chemical composition of the plating layer according to this embodiment is composed of Zn and other alloying elements. The chemical composition of the plating layer will be described in detail below. Note that elements described as having a lower limit of 0% concentration are optional elements that are not essential for solving the problems of the plated steel sheet according to this embodiment, but are allowed to be included in the plating layer for the purpose of improving characteristics, etc.

[0023] <Al: 10.0 to 25.0%> Al contributes to improving flat surface corrosion resistance, edge corrosion resistance, and workability. Therefore, the Al concentration is set to 10.0% or more. The Al concentration may be set to 11.0% or more, 12.0% or more, or 15.0% or more. On the other hand, if Al is excessive, the Mg concentration and Zn concentration decrease relatively, deteriorating edge corrosion resistance. Therefore, the Al concentration is set to 25.0% or less. The Al concentration may also be set to 24.0% or less, 22.0% or less, or 20.0% or less.

[0024] <Mg: 3.0 to 10.0%> Mg is an essential element for ensuring flat surface corrosion resistance and edge corrosion resistance. Therefore, the Mg concentration is set to 3.0% or more. The Mg concentration may be set to 4.0% or more, 5.0% or more, or 6.0% or more. On the other hand, if the Mg concentration is excessive, workability, particularly powdering resistance, may deteriorate, and flat surface corrosion resistance may also deteriorate. Therefore, the Mg concentration is set to 10.0% or less. The Mg concentration may also be set to 8.0% or less or 7.0% or less.

[0025] <Fe: 0.01 to 2.00%> The Fe concentration may be 0%, but the coating layer may contain Fe at 0.01% or more. It has been confirmed that an Fe concentration of 2.00% or less does not adversely affect the performance of the coating layer. The Fe concentration may be, for example, 0.05% or more, 0.10% or more, 0.50% or more, or 1.00% or more. The Fe concentration is set to 2.00% or less. The Fe concentration may be 1.80% or less or 1.50% or less. Because Fe may be mixed in from the base steel sheet, the Fe concentration may be 0.05% or more.

[0026] <Si: More than 0.00% and 2.00% or less> Si contributes to improving flat surface corrosion resistance. Therefore, the Si concentration may be more than 0.00%, 0.01% or more, 0.02% or more, or 0.06% or more. On the other hand, excessive Si concentration deteriorates flat surface corrosion resistance and edge corrosion resistance. Therefore, the Si concentration is set to 2.00% or less. The Si concentration may also be set to 1.80% or less, 1.60% or less, 1.20% or less, or 1.00% or less.

[0027] Furthermore, the plating layer of this embodiment may contain one or more elements selected from the group consisting of Group A, Group B, and Group C below.

[0028] [Group A] Ni: 0-1.000% [Group B] Ca: 0-0.05% [Group C] Sb: 0 to 0.50%, Pb: 0 to 0.50%, Cu: 0 to 1.00%, Sn: 0 to 1.00%, Ti: 0 to 1.00%, Cr: 0 to 1.00%, Nb: 0-1.00%, Zr: 0-1.00%, Mn: 0-1.00%, Mo: 0-1.00%, Ag: 0-1.00%, Li: 0-1.00%, La: 0- 0.50%, Ce: 0 to 0.50%, B: 0 to 0.50%, Y: 0 to 0.50%, P: 0 to 0.50%, Sr: 0 to 0.50%, Co: 0 to 0.500%, Bi: 0 to 0.500%, In: 0 to 0.500%, V: 0 to 0.500%, and W: 0 to 0.500%, with a total of 0 to 5.000% of one or more of the above.

[0029] <Ni: 0 to 1.000%> The Ni concentration as group A may be 0%. On the other hand, Ni contributes to improving edge corrosion resistance. Therefore, the Ni concentration may be 0.050% or more, 0.080% or more, or 0.100% or more. On the other hand, if the Ni concentration is excessive, flat surface corrosion resistance deteriorates. Therefore, the Ni concentration is set to 1.000% or less. The Ni concentration may also be 0.800% or less, 0.600% or less, 0.500% or less, 0.100% or less, or 0.010% or less.

[0030] <Ca: 0 to 0.05%> The Ca concentration as a B group element may be 0%. On the other hand, Ca is an element that can adjust the amount of Mg elution that is optimal for imparting flat surface corrosion resistance. Therefore, the Ca concentration may be 0.005% or more, or 0.01% or more. On the other hand, if the Ca concentration is excessive, flat surface corrosion resistance and workability will deteriorate. Therefore, the Ca concentration is set to 0.05% or less. The Ca concentration may also be set to 0.04% or less.

[0031] Furthermore, the plating layer according to this embodiment contains the following elements of group C: Sb: 0 to 0.50%, Pb: 0 to 0.50%, Cu: 0 to 1.00%, Sn: 0 to 1.00%, Ti: 0 to 1.00%, Cr: 0 to 1.00%, Nb: 0 to 1.00%, Zr: 0 to 1.00%, Mn: 0 to 1.00%, Mo: 0 to 1.00%, Ag: 0 to 1.00%, Li: 0 to 1.00% The alloy may contain one or more of the following elements: 0.00%, La: 0-0.50%, Ce: 0-0.50%, B: 0-0.50%, Y: 0-0.50%, P: 0-0.50%, Sr: 0-0.50%, Co: 0-0.500%, Bi: 0-0.500%, In: 0-0.500%, V: 0-0.500%, and W: 0-0.500%. The total of these elements is 0-5.000%. If the total exceeds 5.000%, flat surface corrosion resistance or edge corrosion resistance may be reduced.

[0032] <Sb, Pb: 0 to 0.50% each> The concentrations of Sb and Pb may be 0%. On the other hand, Sb and Pb contribute to improving edge corrosion resistance. Therefore, the concentrations of Sb and Pb may be 0.05% or more, 0.10% or more, or 0.15% or more. On the other hand, excessive Sb and Pb concentrations deteriorate flat surface corrosion resistance. Therefore, the concentrations of Sb and Pb are set to 0.50% or less. The concentrations of Sb and Pb may also be 0.40% or less, 0.30% or less, 0.25% or less, or 0.10% or less.

[0033] <Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li: 0 to 1.00% each> The concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li may each be 0%. On the other hand, these elements contribute to improving edge corrosion resistance. Therefore, the concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li may each be 0.05% or more, 0.08% or more, or 0.10% or more. On the other hand, excessive concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li deteriorate plane corrosion resistance. Therefore, the concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li are each set to 1.00% or less. The concentration of each of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li may be 0.80% or less, 0.70% or less, 0.60% or less, 0.10% or less, or 0.05% or less.

[0034] <Sn: 0 to 1.00%> The Sn concentration may be 0%. On the other hand, Sn is an element that forms an intermetallic compound with Mg and improves the edge corrosion resistance of the plating layer. Therefore, the Sn concentration may be 0.05% or more, 0.10% or more, or 0.20% or more. However, if the Sn concentration is excessive, planar corrosion resistance will deteriorate. Therefore, the Sn concentration is set to 1.00% or less. The Sn concentration may also be 0.80% or less, 0.60% or less, 0.50% or less, or 0.10% or less.

[0035] <La, Ce, B, Y, P, and Sr: 0 to 0.50% Each> The concentrations of La, Ce, B, Y, P, and Sr may be 0%. Meanwhile, La, Ce, B, Y, P, and Sr contribute to improving edge corrosion resistance. Therefore, the concentrations of La, Ce, B, Y, P, and Sr may each be 0.10% or more, 0.15% or more, or 0.20% or more. Meanwhile, excessive concentrations of La, Ce, B, Y, P, and Sr deteriorate planar corrosion resistance. Therefore, the concentrations of La, Ce, B, Y, P, and Sr each are set to 0.50% or less. The concentrations of La, Ce, B, Y, P, and Sr each may be set to 0.40% or less, 0.30% or less, 0.10% or less, or 0.05% or less.

[0036] <Co, Bi, In, V, W: 0 to 0.500% each> The concentrations of Co, Bi, In, V, and W may each be 0%. Meanwhile, Co, Bi, In, V, and W contribute to improving end face corrosion resistance. Therefore, the concentrations of Co, Bi, In, V, and W may each be 0.100% or more, 0.150% or more, or 0.200% or more. Meanwhile, excessive concentrations of Co, Bi, In, V, and W degrade planar corrosion resistance. Therefore, the concentrations of Co, Bi, In, V, and W are each set to 0.5% or less. The concentrations of Co, Bi, In, V, and W may each be set to 0.400% or less, 0.300% or less, 0.100% or less, 0.050% or less, or 0.010% or less.

[0037] <Balance: Zn and Impurities> The balance of the components of the plating layer according to this embodiment is Zn and impurities. Zn is an element that provides the plating layer with flat corrosion resistance and edge corrosion resistance. Impurities refer to components contained in raw materials or components mixed in during the manufacturing process that are not intentionally added, and components that do not adversely affect the plated steel sheet according to this embodiment. For example, trace amounts of components other than Fe may be mixed into the plating layer as impurities due to mutual atomic diffusion between the base steel sheet and the plating bath.

[0038] The chemical composition of the plating layer is measured by the following method. First, an acid containing an inhibitor that suppresses corrosion of the steel sheet is used to peel and dissolve the plating layer to obtain an acid solution. Next, the obtained acid solution is subjected to ICP analysis. This allows the chemical composition of the plating layer to be obtained. There are no particular restrictions on the type of acid, as long as it is an acid that can dissolve the plating layer. Note that the chemical composition measured by the above-mentioned means is the average chemical composition of the entire plating layer.

[0039] Next, the metal structure of the plating layer will be described. 21 Zn 25 The surface layer of the plating layer is, strictly speaking, the depth region within which X-rays penetrate and diffraction lines are obtained in a grazing incidence X-ray diffraction measurement with an X-ray incidence angle of 1°. Approximately, it can also be said to be the region from the outermost surface of the plating layer to a depth of 3 μm. 21 Zn 25 The phase may be present in regions other than the surface of the plating layer, but must be present in the surface layer. 21 Zn 25 The Mg phase is present on the surface of the plating layer, which prevents corrosion of the plating layer in the early stages. 21 Zn 25 The phase corrodes to form corrosion products, which improve the corrosion resistance of the edge of the steel sheet, thereby improving the edge corrosion resistance without impairing the plane corrosion resistance of the coating layer.

[0040] Mg 21 Zn 25 The presence of the Mg phase was confirmed by performing oblique incidence X-ray diffraction measurement on the plating layer using Cu-Kα rays, setting the acceleration voltage (X-ray output) to 50 kV, and setting the X-ray incident angle to the surface of the plating layer to 1°. 21 Zn 25 This is confirmed by detecting the Mg phase. 21 Zn 25 The presence of the phase can be confirmed by, specifically, Mg 21 Zn 25 This is done by checking whether or not there is a diffraction peak on the (300) plane of the Mg phase. 21 Zn 25The diffraction peak of the (300) plane of the phase is observed in the diffraction angle range of 11.92°±0.4°. Grazing incidence X-ray diffraction (GIXD) is a measurement method in which the angle of incidence of X-rays is fixed at a low angle, so it is possible to detect intermetallic compounds contained in the surface layer of the plating layer with high sensitivity.

[0041] In addition, Mg 21 Zn 25 The presence or absence of the phase was judged by the X-ray diffraction intensity ratio (I(Mg 21 Zn 25 ) / I(η-Zn)) is more than 0.3, Mg 21 Zn 25 It can be said that phases exist.

[0042] As mentioned above, Mg 21 Zn 25 The Mg phase may be present in the surface layer of the plating layer, but it is not necessary to add Mg 21 Zn 25 phases may be present, namely Mg 21 Zn 25 The Mg phase is detected by grazing incidence X-ray diffraction measurement, and may also be detected by X-ray diffraction measurement using the normal θ-2θ method. 21 Zn 25 When a large amount of phases are formed, the Mg 21 Zn 25 Since the amount of the phase may decrease, it is necessary to appropriately control the cooling conditions when forming the plating layer, as will be described later.

[0043] The grazing incidence X-ray diffraction measurement method is also called grazing incidence X-ray diffraction, glancing incidence X-ray diffraction, or thin film X-ray diffraction. Unlike the usual θ-2θ measurement method, this method performs X-ray diffraction measurement by moving the X-ray detector while keeping the X-ray incident angle on the sample fixed.

[0044] Mg on the surface of the plating layer 21 Zn 25The number density of the phases may be affected by the average chemical composition of the plating layer. When the chemical composition of the plating layer contains, in mass %, 4.5% or more of Mg, when a grazing incidence X-ray diffraction measurement is performed on the plating layer using Cu-Kα rays under the conditions of an acceleration voltage (X-ray output) of 50 kV and an X-ray incident angle to the surface of the plating layer of 1°, the number density of Mg 21 Zn 25 The X-ray diffraction intensity ratio (I(Mg 21 Zn 25 The X-ray diffraction intensity ratio (I(Mg ) / I(η-Zn)) may be 1.0 or more, 5.0 or more, 10.0 or more, 15.0 or more, or 20.0 or more. 21 Zn 25 By increasing the value of I(η-Zn) / I(η-Zn), it is possible to achieve both high levels of flat surface corrosion resistance and edge corrosion resistance.

[0045] In addition, I(Mg 21 Zn 25 ) is Mg 21 Zn 25 I(η-Zn) is the peak intensity of the diffraction peak of the (300) plane of the η-Zn phase, more specifically, the maximum diffraction intensity within a diffraction angle range of 11.92°±0.4°. I(η-Zn) is the peak intensity of the diffraction peak of the (002) plane of the η-Zn phase, more specifically, the maximum diffraction intensity within a diffraction angle range of 36.24°±0.4°.

[0046] In the chemical composition of the plating layer of this embodiment, the η-Zn phase is a metal phase that is present in relatively large amounts not only in the surface layer of the plating layer but also throughout the entire plating layer, so it is preferable to use the diffraction intensity of the η-Zn phase as the basis. 21 Zn 25 The higher the diffraction intensity ratio of the phase, the more Mg is present in the surface layer of the plating layer. 21 Zn 25 It can be said that the surface of the plating layer contains a lot of Mg 21 Zn 25 The presence of many Mg phases contributes to the early corrosion of the plating layer. 21 Zn 25More corrosion products of the I(Mg) phase are formed, which further improves the corrosion resistance of the edge surface of the steel sheet. 21 Zn 25 There is no particular upper limit to the value of I(η-Zn) / I(η-Zn), but it may be, for example, 50.0 or less, 45.0 or less, 40.0 or less, 35.0 or less, or 30.0 or less.

[0047] Mg 21 Zn 25 The method for measuring the diffraction intensity of the η-Zn phase and the η-Zn phase is described below. Using an X-ray diffractometer (Rigaku Corporation (Model RINT1500)), oblique incidence X-ray diffraction measurements were performed in the range of 2θ = 5 to 90° under the following conditions: X-ray output: (accelerating voltage) 50 kV, (accelerating current) 200 mA, X-ray source: copper target, X-ray irradiation angle: 1°, attachment: thin film rotating sample stage, filter: none, monochromator: used. 21 Zn 25 The diffraction intensity of the (300) plane of the η-Zn phase (maximum intensity in the range of 11.92°±0.4°) and the diffraction intensity of the (002) plane of the η-Zn phase (maximum intensity in the range of 36.24°±0.4°) are measured. The diffraction intensity is the intensity excluding the background intensity. From the obtained diffraction intensities, I(Mg 21 Zn 25 ) / I(η-Zn). As long as the measurement conditions are met, accelerating voltage: 50 kV, X-ray source: Cu, and X-ray incident angle: 1°, even if other measurement conditions are different, Mg 21 Zn 25 Phase detection and Mg 21 Zn 25 The diffraction intensity ratio of the η-Zn phase and the η-Zn phase is not affected.

[0048] In addition, when the plating layer contains 0.05 to 0.5% Sn, the plating layer contains Mg 2 It is preferable that the Sn phase is contained. 2 Since the Sn phase is present in a small amount, its presence can be detected and confirmed by X-ray diffraction measurement using the θ-2θ method. 2 The inclusion of the Sn phase further improves the corrosion resistance of the edge of the plating layer. 2X-ray diffraction measurement for detecting the Sn phase may be performed by the θ-2θ measurement method. In addition, the X-ray diffraction measurement uses Kα rays from a Cu tube, and when a peak is detected at 23.4±0.3°, it is determined that the Sn phase is Mg. 2 It is determined that a Sn phase is present.

[0049] The coating weight of the plating layer per side is, for example, 20 to 150 g / m 2 The amount of adhesion per side should be within the range of 20 g / m 2 By setting the coating weight per side to 150 g / m or more, the flat surface corrosion resistance and edge corrosion resistance of the plated steel sheet can be further improved. 2 By setting the following, the workability of the plated steel sheet can be further improved.

[0050] Next, a method for producing the plated steel sheet according to this embodiment will be described, but the method for producing the plated steel sheet according to this embodiment is not particularly limited. For example, the plated steel sheet according to this embodiment can be obtained under the production conditions described below.

[0051] In the method for producing a plated steel sheet according to this embodiment, a steel sheet with an adjusted surface roughness is annealed in a reducing atmosphere, and the annealed steel sheet is immersed in a hot-dip galvanizing bath and then pulled out to form a coating layer on the surface of the steel sheet. Next, cooling is performed by blowing a cooling gas onto the steel sheet until the temperature of the coating layer drops from the bath temperature to 300°C or less. The gas flux when blowing the cooling gas is 5,000 to 80,000 L / min / m from the bath temperature to the controlled cooling temperature. 2 The gas flow rate from the controlled cooling temperature to 300°C or less is set to 0 to 5000 L / min / m 2 The range is as follows.

[0052] The controlled cooling temperature is Mg 21 Zn 25 The temperature is set within the range of -10°C to -30°C relative to the phase crystallization temperature.

[0053] The roughness of the surface of the steel sheet to be used as the base sheet for plating is set to 0.1 to 3.5 μm in terms of calculated surface roughness Ra. If it is outside this range, Mg may be present near the interface between the plating layer and the steel sheet. 21 Zn 25 Many phases are crystallized, and Mg 21 Zn25 The adjustment of the surface roughness of the steel sheet is not particularly limited, but may be performed, for example, by rolling the original steel sheet to be plated with a rolling roll or a roll for temper rolling whose surface has been adjusted to the desired roughness, thereby transferring the surface shape of the roll to the original steel sheet. Alternatively, the adjustment may be performed by pickling.

[0054] The arithmetic mean roughness is measured, for example, using a shape measuring laser microscope (model number: VK-8700) manufactured by Keyence Corporation. Measurement conditions are, for example, measurement mode: laser confocal, measurement quality: high precision, pitch: 0.75 μm, double scan: ON, optical zoom: 1x, objective lens name: Plan, γ coefficient: 0.45, offset: 0%. Note that the measuring device used to measure the arithmetic mean roughness is not limited to the above example.

[0055] Annealing of the steel sheet to be used as the base sheet for plating is carried out in a reducing atmosphere. The reducing atmosphere and annealing conditions are not particularly limited. By this annealing, oxides present on the surface of the steel sheet are removed as much as possible.

[0056] Next, the annealed steel sheet is immersed in a hot-dip galvanizing bath. The chemical composition of the hot-dip galvanizing bath may be appropriately adjusted so as to obtain the chemical composition of the coating layer described above. The temperature of the hot-dip galvanizing bath is not particularly limited, and a temperature at which hot-dip galvanizing can be performed may be appropriately selected. For example, the temperature of the galvanizing bath may be set to a value approximately 20°C or more higher than the melting point of the galvanizing bath.

[0057] Next, the steel sheet is pulled out of the hot-dip galvanizing bath. The coating weight of the coating layer can be controlled by controlling the pulling speed of the steel sheet. If necessary, the coating weight of the coating layer may be controlled by wiping the steel sheet to which the coating layer is attached. The coating weight of the coating layer is not particularly limited and can be, for example, within the above-mentioned range.

[0058] The coating layer is then cooled. Cooling is performed by spraying cooling gas onto the steel sheet immediately after it has been pulled out of the hot-dip coating bath. Cooling by spraying cooling gas is performed continuously until the temperature of the steel sheet drops from the bath temperature to 300°C. The cooling conditions for temperatures below 300°C are not particularly limited, and cooling by spraying cooling gas may be continued or the steel sheet may be allowed to cool naturally.

[0059] Cooling by spraying cooling gas is performed by arranging a cooling zone along the steel sheet transport path. The cooling zone is equipped with multiple spray nozzles for the cooling gas. The shape of the gas nozzle from which the cooling gas is sprayed is, for example, in the range of 1 to 50 mm in diameter. The angle between the tip of the gas nozzle and the steel sheet is, for example, in the range of 70 to 110°, more preferably 90° (right angle). The distance between the tip of the gas nozzle and the steel sheet is in the range of 30 to 1000 mm. Note that the shape, angle, and distance of the gas nozzle are merely examples and are not limited to the above ranges.

[0060] The cooling gas to be sprayed is not particularly limited, and may be a non-oxidizing gas such as nitrogen, an inert gas such as argon, or air, or a mixture of these gases.

[0061] In this embodiment, the gas flux when blowing the cooling gas is controlled in two stages. That is, the temperature of the steel sheet is used as a reference, and the cooling temperature is changed from the coating bath temperature to the controlled cooling temperature (Mg 21 Zn 25 The gas flux up to the temperature (temperature in the range of -10 to -30 ° C. relative to the phase crystallization temperature) is 5,000 to 80,000 L / min / m 2 The gas flow rate from the controlled cooling temperature to 300°C or less is set to 0 to 5000 L / min / m 2 The controlled cooling temperature is in the range of Mg 21 Zn 25 The gas flux can be adjusted by changing the shape of the gas nozzle or controlling the compressor output.

[0062] Gas flux: 5000 L / min / m 2 When the gas flux is set to a range of less than 5000 L / min / m, it is possible to prevent the surface of the coating layer from vibrating during cooling. 2When the temperature is within the above range, it becomes possible to apply minute vibrations to the surface of the plating layer during cooling.

[0063] The gas flow rate from the plating bath temperature to the controlled cooling temperature is 5000 to 80000 L / min / m 2 By setting the range to , vibration is applied to the surface of the plating layer, and Mg 21 Zn 25 Then, the gas flow rate is controlled from 0 to 5000 L / min / m to cool the mixture to a temperature of 300°C or less. 2 By setting the range of 21 Zn 25 If the gas flux range is outside the above range, Mg 21 Zn 25 It is preferable to set the gas flux from the controlled cooling temperature to 300°C or less to a lower value than the gas flux from the coating bath temperature to the controlled cooling temperature. When the gas flux is constant in both temperature ranges (gas flux from the coating bath temperature to the controlled cooling temperature is 5000 L / min / m 2 The gas flow rate from the controlled cooling temperature to 300°C or less is 5000 L / min / m 2 In this case, it is preferable to set the average cooling rates in both temperature ranges to different values. By setting such conditions, Mg 21 Zn 25 The phase can be preferably formed.

[0064] Mg 21 Zn 25 The phase crystallization temperature varies depending on the chemical composition of the plating bath, and is therefore calculated using a calculated phase diagram. Specifically, a calculated phase diagram database is constructed that accumulates thermodynamic data on intermetallic compound phases and metal phases that may be contained in Al-Mg-Zn alloys, and calculations are performed using the CALPHAD (CALculation of PHAseDiagram) method to determine the Mg phase crystallization temperature for each chemical composition of the plating bath. 21 Zn 25More specifically, the phase crystallization temperature is calculated by using the thermodynamic equilibrium calculation software "Thermo-Calc" (Thermo-Calc is a registered trademark, manufactured by Thermo-Calc Software). 21 Zn 25 The phase crystallization temperature can be estimated. The thermodynamic equilibrium calculation software used for the calculation is not limited to "Thermo-Calc" (registered trademark), and other software may be used. 21 Zn 25 The controlled cooling temperature is set to a temperature within the range of -10 to -30°C relative to the phase crystallization temperature.

[0065] In the above manufacturing method, the surface roughness of the steel sheet surface is adjusted in advance to prevent Mg from being mixed with the surface of the coating layer near the interface between the steel sheet and the coating layer. 21 Zn 25 This suppresses the nucleation of the Mg phase near the interface between the coating layer and the steel sheet. 21 Zn 25 By hot-dipping such a steel sheet and controlling the cooling conditions after plating as described above, it is possible to suppress the crystallization of Mg phases on the surface of the plating layer. 21 Zn 25 This allows a large amount of Mg phase to crystallize on the surface of the plating layer. 21 Zn 25 It is presumed that many phases can be formed.

[0066] As long as the requirements of the present invention are met, the method for producing a plated steel sheet is not limited to the above, and electroplating, vapor deposition plating, thermal spraying, cold spraying, etc. may be used instead of hot-dip plating.

[0067] Examples of the present invention will be described below. However, the conditions in the examples are merely examples adopted to confirm the feasibility and effects of the present invention. The present invention is not limited to these examples. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.

[0068] Cold-rolled steel sheets (0.05C-0.1Si-0.2Mn) with a thickness of 2.3 mm were used as the base sheets for plating. The surface roughness of some of the base sheets for plating was controlled using a skin-pass mill or the like. The steel sheets with the adjusted surface roughness were then annealed. The annealed steel sheets were immersed in various hot-dip coating baths and then pulled out, thereby adhering a coating layer to the steel sheet surface. Next, various coated steel sheets were produced by cooling using cooling gas from immediately after pulling out of the coating bath until the coating layer reached 300°C.

[0069] The arithmetic mean roughness Ra of the surface of the steel sheet to be plated was as shown in the table.

[0070] The arithmetic mean roughness was measured using a shape measuring laser microscope (model number: VK-8700) manufactured by Keyence Corporation. The measurement conditions were as follows: measurement mode: laser confocal, measurement quality: high precision, pitch: 0.75 μm, double scan: ON, optical zoom: 1x, objective lens name: Plan, γ coefficient: 0.45, offset: 0%.

[0071] The annealing conditions for annealing the steel sheet in a reducing atmosphere were a soaking temperature of 600°C and a soaking time of 10 seconds. The annealing atmosphere was a reducing atmosphere consisting of a mixed gas of 5% hydrogen and the balance nitrogen. The annealed steel sheet was then air-cooled with nitrogen gas until the immersion temperature reached the bath temperature + 20°C, after which it was immersed in a hot-dip galvanizing bath and then pulled up. The pulling-up speed was 20 to 200 mm / sec.

[0072] The chemical composition of the plating layer was as shown in Table 1. The production conditions were as shown in Table 2. The metal structure of the plating layer was evaluated, and the results are shown in Table 3. Furthermore, the flat corrosion resistance and edge corrosion resistance of the plated steel sheet were evaluated, and the results are shown in Table 3.

[0073] The chemical composition and metal structure of the plating layer were evaluated by the methods described above.

[0074] The flat corrosion resistance was evaluated as follows. The obtained hot-dip plated steel material was cut into 100 mm x 50 mm pieces and subjected to a flat corrosion resistance evaluation test. The flat corrosion resistance was evaluated by an accelerated corrosion test specified in JASO-CCT-M609, and the corrosion weight loss was compared after 90 cycles. The evaluation criteria were as follows, with "AAA", "AA" and "A" being considered as passing.

[0075] AAA: Corrosion weight loss 30g / m 2 Less than AA: Corrosion weight loss 30g / m 2 60g / m or more 2 Less than A: Corrosion weight loss 60g / m 2 90g / m or more 2 Less than B: Corrosion weight loss 90g / m 2 End

[0076] The edge corrosion resistance was determined as follows. The obtained hot-dip plated steel material was cut into a size of 50 mm x 50 mm to obtain a rectangular test piece. Then, the coating layer in a region with a diameter of 15 mm centered on the intersection of the diagonal lines of the test piece was removed by milling to form an exposed region of the steel sheet (base steel). The exposed region of the base steel with a diameter of 15 mm was subjected to a neutral salt spray test specified in JIS Z 2371:2015, and evaluation was performed based on the occurrence of red rust in the exposed region of the base steel. The evaluation criteria for the red rust area ratio are shown below. "AAA", "AA", and "A" were considered to be acceptable.

[0077] AAA: Red rust area ratio 10% or less after 1300 hours AA: Red rust area ratio 10% or less after 800 hours A: Red rust area ratio 20% or less after 400 hours B: Red rust area ratio over 20% after 400 hours

[0078] As shown in Tables 1 to 3, Examples 1 to 27 according to the present invention, in which the chemical composition and metal structure of the plating layer were appropriately controlled, were excellent in both flat surface corrosion resistance and edge corrosion resistance. The coating weight of the plating layer per side in the examples was 20 to 150 g / m 2 The range was.

[0079] In Comparative Example 28, the amount of Al in the plating layer was insufficient. Therefore, in Comparative Example 28, the flat corrosion resistance was insufficient.

[0080] In Comparative Example 29, the amount of Al in the plating layer was excessive. 21 Zn 25 Although the phase was crystallized, the corrosion resistance of the edge surface was reduced.

[0081] In Comparative Example 30, the amount of Mg in the plating layer was insufficient. 21 Zn 25 The phase did not crystallize, and the plane corrosion resistance and edge corrosion resistance decreased.

[0082] In Comparative Example 31, the amount of Mg in the plating layer was excessive, and therefore, in Comparative Example 31, the electrically less noble Mg—Zn phase was produced in excess, resulting in a decrease in planar corrosion resistance.

[0083] In Comparative Example 32, the cooling gas flux from the bath temperature to the controlled cooling temperature was insufficient. 21 Zn 25 The phase could not be crystallized, and the corrosion resistance of the edge surface decreased.

[0084] In Comparative Example 33, the cooling gas flux from the controlled cooling temperature to 300°C was excessive. Therefore, in Comparative Example 33, Mg 21 Zn 25 Many phases crystallize, and Mg 21 Zn 25 In Comparative Example 34, the arithmetic mean roughness Ra of the surface of the steel sheet to be used as the base sheet for plating was outside the preferred range. 21 Zn 25 Many phases are crystallized, and Mg 21 Zn 25 In Comparative Example 35, the cooling gas flux from the controlled cooling temperature to 300°C was excessive. Therefore, in Comparative Example 35, the Mg phase was reduced in the surface layer of the coating layer. 21 Zn 25 In Comparative Example 36, the amount of Al in the plating layer was excessive. Therefore, in Comparative Example 29, the Mg phase was not crystallized in the surface layer of the plating layer. 21 Zn 25 The phase did not crystallize, and the plane corrosion resistance decreased.

[0085]

[0086]

[0087]

[0088] 1...plated steel sheet, 11...steel sheet, 12...plated layer

Claims

1. A steel sheet comprising a steel sheet and a plating layer disposed on the surface of the steel sheet, wherein the chemical composition of the plating layer contains, in mass %, Al: 10.0 to 25.0%, Mg: 3.0 to 10.0%, Fe: 0.01 to 2.00%, Si: more than 0.00% but not more than 2.00%, and one or more elements selected from the group consisting of Group A, Group B, and Group C below, with the balance consisting of Zn and impurities, and wherein when a glancing angle incidence X-ray diffraction measurement is performed on the plating layer using Cu-Kα rays, with an acceleration voltage (X-ray output) of 50 kV, and an X-ray incident angle to the surface of the plating layer of 1°, the following is found: Mg 21 Zn 25 The X-ray diffraction intensity ratio (I(Mg 21 Zn 25 ) / I(η-Zn)) is greater than 0.

3. [Group A] Ni: 0-1.000% [Group B] Ca: 0-0.05% [Group C] Sb: 0-0.50%, Pb: 0-0.50%, Cu: 0-1.00%, Sn: 0-1.00%, Ti: 0-1.00%, Cr: 0-1.00%, Nb: 0-1.00%, Zr: 0-1.00%, Mn: 0-1.00%, Mo: 0-1.00%, Ag: 0-1.00%, Li: 0-1.00%, La: 0-0.50%, Ce: 0-0.50%, B: 0-0.50%, Y: 0-0.50%, P: 0-0.50%, Sr: 0 to 0.50%, Co: 0 to 0.500%, Bi: 0 to 0.500%, In: 0 to 0.500%, V: 0 to 0.500%, and W: 0 to 0.500%, with a total of 0 to 5.000% of one or more of these.

2. The chemical composition of the plating layer contains, in mass%, 4.5% or more of Mg, and the X-ray diffraction intensity ratio (I(Mg 21 Zn 25 2. The plated steel sheet according to claim 1, wherein I(η-Zn) / I(η-Zn)) is 1.0 or more.

3. The chemical composition of the plating layer contains, in mass%, 4.5% or more of Mg, and the X-ray diffraction intensity ratio (I(Mg 21 Zn 25 2. The plated steel sheet according to claim 1, wherein I(η-Zn) / I(η-Zn)) is 5.0 or more.

4. The chemical composition of the plating layer contains, in mass%, 4.5% or more of Mg, and the X-ray diffraction intensity ratio (I(Mg 21 Zn 25 2. The plated steel sheet according to claim 1, wherein I(η-Zn) / I(η-Zn)) is 10.0 or more.

5. The chemical composition of the plating layer contains, in mass%, Sn: 0.05 to 0.5%, and when X-ray diffraction measurement of the plating layer using the θ-2θ method is performed, Mg is not present in the plating layer. 2 The plated steel sheet according to claim 1 , wherein an Sn phase is detected.

6. The plated steel sheet according to any one of claims 1 to 4, wherein the chemical composition of the plating layer contains the Group A element.

7. The plated steel sheet according to any one of claims 1 to 4, wherein the chemical composition of the plated layer contains the B group element.

8. The plated steel sheet according to any one of claims 1 to 4, wherein the chemical composition of the plating layer contains the Group C element.