Winding, method for manufacturing winding, welding electrode, and manufacturing device

MYPI2025000788A0Undetermined Publication Date: 2024-02-03FUJI FILTER MFG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025000788
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-08-03
Filing Date
2023-08-01
Publication Date
2024-02-03

AI Technical Summary

Technical Problem

Existing methods for manufacturing porous winding bodies with spirally wound metal wires face challenges in minimizing the distance between the welding point and the terminal edge, leading to potential damage and delamination issues, while also increasing the number of manufacturing steps.

Method used

A method where the terminal end of the metal wire is resistance spot welded and fused at the welded location, using a welding electrode to ensure a short distance between the weld and the terminal edge without adding manufacturing steps, by melting and cutting the wire under tension.

Benefits of technology

This approach reduces the risk of damage to other parts, prevents delamination, and simplifies the manufacturing process by simultaneously welding and cutting the metal wire, maintaining the integrity of the winding body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025000788_DRAWING_001
    Figure PI2025000788_DRAWING_001
  • Figure PI2025000788_DRAWING_002
    Figure PI2025000788_DRAWING_002
  • Figure PI2025000788_DRAWING_003
    Figure PI2025000788_DRAWING_003
Patent Text Reader

Abstract

To manufacture a winding (10) configured to prevent a terminal end part (30(20n)) of a metal wire (20) from damaging other components and the like by making the distance from a welded part to a terminal edge (35) as short as possible without increasing the number of manufacturing steps, and to prevent manufacturing defective windings (10). The winding is a porous winding (a filter 10) formed by winding at least one continuous metal wire (20) in a helical and multilayered manner. In the winding (10), a terminal end part (30) (a metal wire portion 20n) of the metal wire (20) is resistance spot welded to another portion (a metal wire portion 20m) of the metal wire (20) and is fusion-cut at the welded portion. The terminal end part (30) (the metal wire portion 20n) has a fused solidified part (31n) where entirety of the metal wire (20) in a width direction has been solidified after being fused. Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

Winding body, method for manufacturing winding body, welding electrode, and manufacturing device

[0001] The present invention relates to a porous winding body in which at least one continuous metal wire is wound spirally and in multiple layers, a method for manufacturing the winding body, a welding electrode suitable for manufacturing the winding body, and a manufacturing apparatus equipped with the welding electrode.

[0002] A hollow cylindrical porous winding body made by winding at least one continuous metal wire in a spiral and multiple layers is used in applications such as filters that remove foreign matter exceeding a predetermined size from a fluid, and for cooling the fluid. Patent Document 1 is an example of a document that describes such a winding body. In the above winding body, it is necessary to fix the end of the metal wire at the end of the winding to an appropriate position on the winding body by welding or the like, and to cut the metal wire.

[0003] JP 2001-171472 A

[0004] Here, it is desirable that the terminal edge (cut end) of the metal wire be as close to the weld as possible. If the terminal edge of the metal wire is far away from the weld, the following problems may occur. One example of a problem is that the portion of the metal wire from the weld to the terminal edge may get caught on other components, damaging them. Another example of a problem is that the weld is more likely to peel if the distance from the weld to the terminal edge is long. If nippers, scissors, or the like are used as a tool to cut the metal wire, the cutting blade must be applied in a direction intersecting the longitudinal direction of the metal wire. During cutting, the cutting blade is inserted between the metal wire and the winding, so the portion of the metal wire from the weld to the terminal edge is longer, and the insertion of the cutting blade tends to cause the metal wire to rise in the outer diameter direction. Therefore, to prevent the above-mentioned problems, post-processing is required to shorten the length of the metal wire from the weld to the terminal edge, which increases the number of manufacturing steps.

[0005] Another approach to shortening the length of the metal wire portion from the weld to the terminal edge is to repeatedly bend the metal wire in a direction intersecting its longitudinal direction in the immediate vicinity of the weld, thereby cutting the metal wire. However, this method tends to deform the cut portion in the bending direction and become work-hardened, which does not solve the problem of damaging other components. Furthermore, this cutting method is complicated. Patent Document 1 describes welding the end of the metal wire near the end of winding, but does not describe how to cut the end of the winding. The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a winding body in which the distance from the weld to the terminal edge is as short as possible without increasing the number of manufacturing processes.

[0006] In order to solve the above problems, the present invention provides a porous winding body in which at least one continuous metal wire is wound in a spiral and multi-layered manner, and the terminal end of the metal wire is resistance spot welded to another portion of the metal wire and is melted at the welded location.

[0007] According to the present invention, it is possible to provide a winding body in which the distance from the welded portion to the terminal edge is as short as possible without increasing the number of manufacturing steps.

[0008] 1 is a schematic perspective view of a filter according to an embodiment of the present invention;

[0023] FIG. 1 is a schematic view showing the state of the terminal end portion of the filter, where (a) is a cross-sectional view cut along the longitudinal direction of the metal wire, and (b) is a perspective view observed from the outer diameter side of the filter;

[0024] FIG. 2 is a view showing the vicinity of the terminal end portion of the filter using an actual photograph;

[0025] FIG. 3 is a schematic view mainly showing a winding device among the winding body manufacturing apparatus;

[0026] FIG. 4 is a schematic view particularly showing the downstream side of a guide member among the winding body manufacturing apparatus;

[0027] FIG. 5 is a perspective view showing an example of an electrode;

[0028] FIGS. 1(a) and 1(b) are plan views illustrating the relationship between the electrode tip surface and the metal wire in contact with the electrode tip surface;

[0029] FIGS. 1(a) and 1(b) are schematic views showing the state immediately before the metal wire is cut;

[0029] FIGS. 1(a) and 1(b) are schematic views showing the state immediately before the metal wire is cut;

[0029] FIGS. 1(a) and 1(b) are schematic views showing the state immediately before the metal wire is cut;

[0009] The present invention will be described in detail below using the embodiments shown in the drawings. However, unless otherwise specified, the components, types, combinations, shapes, relative positions, etc. described in these embodiments are merely illustrative examples and do not intend to limit the scope of the present invention. Furthermore, the configurations shown in each embodiment can be implemented in appropriate combinations as long as they are not inconsistent.

[0010] [Overall Shape of the Filter] FIG. 1 is a schematic perspective view of a filter according to one embodiment of the present invention. A hollow cylindrical filter 10 according to the present invention is formed by winding at least one continuous metal wire 20 in a spiral shape and in multiple layers at a constant pitch and at a constant inclination angle relative to the axial direction (the vertical direction in the drawing). The filter 10 is an example of a porous winding body in which at least one continuous metal wire is wound in a spiral shape and in multiple layers. Here, the individual layers in which the metal wire 20 is wound in the same direction are referred to as wire layers L1, L2, L3, etc. The metal wires constituting each of the wire layers L1, L2, L3, etc. extend in the same direction inclined relative to the axial direction (the central axis Ax1) of the hollow cylindrical filter in a front view. Furthermore, the metal wires constituting adjacent wire layers in the inner and outer radial directions extend in directions that intersect with each other (i.e., are not parallel to each other).

[0011] In FIG. 1 , the direction of extension of the metal wire portion 20(n) (thickness not shown) constituting the outermost wire layer Ln (n is a natural number) (the longitudinal direction of the metal wire portion 20(n)) is indicated by a solid arrow, and the direction of extension of the metal wire portion 20(n-1) constituting the immediately inner wire layer Ln-1 (the longitudinal direction of the metal wire portion 20(n-1)) is indicated by a dashed arrow. n is set to approximately 20 to 20,000 (approximately 10 to 10,000 round trips). That is, the filter 10 has one wire layer (e.g., wire layer L1) formed by spirally winding the metal wire 20 at a certain inclination angle with respect to the axial direction, and another wire layer (e.g., wire layer L2) overlapping the outer periphery of the one wire layer L1 and formed by spirally winding a metal wire at an inclination angle different from that of the metal wire constituting the one wire layer L1. The metal wires constituting one wire layer L1 and the adjacent wire layer L2 are configured to be non-parallel to each other in the axial direction and to intersect with each other. Note that the inclination angle of the metal wires constituting the wire layers with respect to the axial direction may be configured to vary within one wire layer.

[0012] This filter 10 is used to remove unwanted substances from various fluids, such as liquids and gases, and, in some applications, such as in automobile airbag inflators, to simultaneously cool the fluid passing through the filter. This filter is primarily configured to form a fluid flow path in the direction in which the wire layers overlap, i.e., the radial direction of the filter (the direction in which the wire layers overlap). The fluid may pass from the inner diameter side to the outer diameter side of the filter, or from the outer diameter side to the inner diameter side. Here, the radial direction does not mean the diametric direction (radial direction) in the strict sense, but rather means roughly the radial direction as opposed to the axial and circumferential directions. The size of the filter (e.g., inner diameter, outer diameter, axial dimensions) is determined appropriately depending on the structure and size of the device in which the filter is incorporated. Metals used to make this filter include iron, steel, mild steel, stainless steel, nickel alloys, copper alloys, titanium alloys, and aluminum alloys. The type of metal is selected based on the application of the filter.

[0013] The thickness and cross-sectional shape (cross-sectional shape in a direction perpendicular to the longitudinal direction of the metal wire) of the metal wire used in the filter are determined appropriately depending on the size of the filter, the substances to be removed by the filter, pressure loss, etc. For example, the cross-sectional area of ​​the metal wire used in the inflator filter is about 0.007 to 3.2 mm^2 (the wire diameter is about 0.1 to 2.0 mm when a metal wire with a perfectly circular cross-sectional shape is used as the standard).

[0014] The filter uses metal wires obtained by rolling metal wires having a perfectly circular cross section into a predetermined shape. For example, rectangular wires are used as the metal wires, which are rolled to have a flattened rectangular cross section. Alternatively, deformed wires are used as the metal wires, which are rolled to have a cross section that is approximately W-shaped, U-shaped, J-shaped, L-shaped, X-shaped, or other irregular shapes along their entire length. Alternatively, deformed wires are used as the metal wires, whose cross section and external shape are not constant along their entire length, in other words, deformed wires that are rolled to have different cross sections and external shapes depending on the longitudinal position of the metal wire. Such deformed wires are rolled so that the cross section changes along the longitudinal length, for example, at intervals approximately equal to the width of the metal wire.

[0015] In the filter 10, the metal wire 20 is wound so as not to twist. The filter 10 has a plurality of contact portions where the metal wire portions are in contact with each other. The filter 10 may be subjected to a heat treatment (for example, a heat treatment for sintering) that collectively bonds all of the contact portions (or a plurality of contact portions). Alternatively, of the plurality of contact portions in the filter 10, portions other than the end portion on the winding end side may be left as unbonded portions that are not bonded. If the filter 10 is not subjected to a heat treatment for sintering the entire filter, the manufacturing cost of the filter 10 can be reduced and the manufacturing time of the filter 10 can be shortened.

[0016] [State of Terminal Portion] The filter 10 according to the present embodiment is characterized in that the winding end portion (terminal portion 30) of the metal wire is fused at the welded location. That is, in the filter 10, the welding and fusion of the terminal portion 30 are performed simultaneously.

[0017] In this example, melting (or thermal cutting) refers to heating all or part of the metal wire in the thickness direction (inner diameter side) above the melting point and cutting the metal wire using tension acting on the metal wire. When the entire metal wire in the thickness direction is melted, the melted part is cut. When only part of the metal wire in the thickness direction is melted, the melted part is cut, and the heat-affected zone (mainly the outer diameter side) adjacent to the melted part, where the structure has changed due to heating and the strength has decreased, is cut (torn off). This example differs from cutting methods that use shear force or metal fatigue in that the metal wire is cut by applying force in the longitudinal direction.

[0018] 2A and 2B are schematic diagrams showing the state of the terminal end of the filter, where (a) is a cross-sectional view cut along the longitudinal direction of the metal wire, and (b) is a perspective view observed from the outer diameter side of the filter. Hereinafter, the portion of the metal wire portion 20n that is in contact with the welding electrode will be referred to as the terminal end 30. More specifically, the terminal end 30 is the portion closer to the terminal edge 35 (the cut end) than the indentation 33 of the welding electrode.

[0019] The terminal end 30 of the metal wire 20 is resistance spot welded to an appropriate location (joining target portion 21) of another portion of the metal wire 20 (metal wire portion 20m). This figure shows only the periphery of the terminal end 30 and the metal wire portion 20m belonging to the wire layer Lm located radially inward from the terminal end 30 among the metal wire portions 20n constituting the outermost wire layer Ln (where m is a natural number, m<n). The metal wire portion 20p shown by a dotted line on the right side of the figure is a portion that is separated from the metal wire portion 20n by melting the metal wire 20. The molten portion 32p shown by a dotted line in the figure is a portion of the metal wire portion 20p that is separated from the metal wire portion 20n after melting.

[0020] The terminal end 30, which is a part of the metal wire portion 20n, and the metal wire portion 20m that overlaps it melt during welding and then solidify to form a molten solidified portion 31 (31n, 31m). The metal wire portions 20n and 20m are integrated in the molten solidified portion 31, but for convenience, the molten solidified portions 31 located on the sides of each metal wire portion 20n and 20m will be described separately as molten solidified portions 31n and 31m, respectively. The molten solidified portion 31 and the molten portion 32p are the molten portion 32 that was melted just before the metal wire portion 20p separated. Below, we will describe in detail the traces left on the winding or filter when the metal wire is melted at the welded location or heat-affected zone by the method of the present invention.

[0021] <Melted solidified portion at end portion> The molten solidified portion 31n is solidified after at least a portion of the metal wire portion 20n in the width direction is melted. The molten solidified portion 31n is preferably formed only within the width direction range of the metal wire 20. That is, it is preferable that the molten solidified portion 31n does not leak out beyond the width direction edge of the metal wire portion 20n (does not leak sideways).

[0022] The illustrated terminal end 30 has a molten solidified portion 31n that solidifies after the entire width direction of the metal wire portion 20n (entire width or entire width direction) has melted. This indicates that the entire width direction of the metal wire 20 is covered by the welding electrode during welding, and that the entire width direction of the metal wire 20 is thereby melted. The molten solidified portion 31n is formed from the terminal edge 35 over a predetermined longitudinal length of the metal wire. By melting the entire width direction of the metal wire 20, the metal wire 20 can be reliably melted. In addition, since the entire width direction of the terminal end 30 is melted and joined to the metal wire portion 20m, the required joint strength can be easily ensured.

[0023] Because the molten solidified portion 31 is melted and then solidified, it is softer than other metal wire portions (except for high-carbon steel). If the metal wire 20 is cut using shear force with nippers, scissors, or the like, the vicinity of the cut end of the metal wire will be work-hardened. However, in this embodiment, the metal wire is melted or softened before being torn off, so the terminal end 30 does not work-harden. In other words, even without subjecting the winding body to heat treatment, the molten solidified portion 31 can be prevented from contacting and damaging other components, etc. Furthermore, unlike when cutting the metal wire with nippers, scissors, etc., it is possible to minimize the possibility of the cut end rising in a direction intersecting the longitudinal direction of the metal wire.

[0024] Since the terminal end 30 is joined by resistance spot welding, a trace (indentation 33) of pressure applied by the electrode during welding remains in a portion closer to the beginning of the metal wire 20 (closer to the beginning of winding) than the molten solidified portion 31. The indentation 33 is formed over the entire width of the metal wire portion 20n. The indentation 33 has a shape corresponding to the contact state of the electrode when pressurizing the metal wire 30. As an example, the indentation 33 has a shape in which the portion not pressurized by the electrode and the portion pressurized are continuous via a gentle step. As another example, FIG. 2(b) shows an example in which no step is formed between the portion not pressurized by the electrode and the portion pressurized, and the indentation 33 is recognized as a change point in the inclination angle (or wall thickness) of the outer diameter side surface of both portions.

[0025] <Thinning of Terminal Portion> The overall thickness of the terminal portion 30 is thinner than the thickness t of the other portions of the metal wire 20. This indicates that the metal wire is melted and cut at an appropriate location in the fusion zone 32 to form the terminal edge 35. This characteristic does not appear when the metal wire is cut using nippers or the like, that is, when the welded portion and the cut end are spaced apart in the longitudinal direction of the metal wire. The terminal portion 30 has a portion where the thickness of the metal wire 20 is thinned toward the terminal edge 35 of the metal wire 20 (a portion where the thickness gradually decreases) in the range where the fusion solidified portion 31n is formed. In particular, the thickness of the portion of the fusion solidified portion 31n exposed to the outside gradually decreases toward the terminal edge 35. This indicates that the terminal end 30 has melted or softened and been stretched in the direction of the terminal end edge 35, and that a portion of the thickness of the metal wire 20 located on the outer diameter side near the terminal end 30 has melted and disappeared without remaining on the winding side (the metal wire portion 20p has separated from the metal wire portion 20n). In particular, Figure 2(b) shows an example in which the thickness of the terminal end 30 gradually decreases uniformly as a whole toward the terminal end edge 35.

[0026] Here, the molten portion of the metal wire portion 20n (the portion that will later become the molten solidified portion 31n) may aggregate due to the surface tension of the molten metal material and deform into a rounded shape such as a sphere before solidifying to form the terminal edge 35. For example, the thickness of the downstream portion of the terminal end 30 gradually decreases toward the terminal edge, but there may be a portion where the thickness locally increases near the terminal edge (the upstream portion of the terminal end). Depending on the conditions during fusing, the upstream portion of the terminal end 30 may have a portion that is thicker than the downstream portion.

[0027] <Stretching marks> Stretching marks 37 are formed in the terminal end 30, indicating that the softened metal wire portion 20n has been stretched toward the terminal end edge 35 of the metal wire 20. Alternatively, the stretching marks 37 indicate that the softened metal material has been cut as if being torn toward the terminal end edge 35. The softened portion is a portion whose strength has been reduced by heating during welding, and is a heat-affected zone. In order to form the metal wire 20 into a predetermined winding shape, a predetermined tension is applied to the metal wire when it is wound. The stretching marks 37 indicate that the metal wire has been melted and cut using the tension applied during winding. In other words, the stretching marks 37 are marks remaining on the metal wire portion 20n as a result of the metal wire portion 20n, which has been softened by welding, being stretched and cut toward the upstream direction (the supply side of the metal wire) by the tension acting on the metal wire portion 20n. The drawing marks 37 are stretching marks, and can be visually distinguished from rolling marks left on other parts of the metal wire rod 20 .

[0028] <Exposed molten solidified portion> At least a portion of the molten solidified portion 31n formed in the terminal end portion 30 is exposed to the outside. In FIG. 2(b), the exposed molten solidified portion 31n is indicated by diagonal lines. At least a portion of the molten solidified portion 31n near the terminal end edge 35 of the metal wire is exposed to the outside. The terminal end edge 35 is the molten solidified portion 31n. In this figure, the terminal end edge 35 of the metal wire portion 20n is welded to the metal wire portion 20m, and the distance between the welded joint and the terminal end edge 35 is zero. The molten solidified portion 31n is exposed from the terminal end edge 35 over a predetermined longitudinal length of the metal wire. The molten solidified portion 31n formed within the width direction range of the metal wire portion 20n is exposed to the outside. The molten solidified portion 31n exposed to the outside constitutes the surface on the outer diameter side of the terminal end portion 30. This indicates that a portion of the thickness located on the outer diameter side of the metal wire portion 20n has disappeared due to elongation and melting. In particular, this indicates that the metal wire portion 20p has been separated from the metal wire portion 20n, accompanied by a molten portion 32p, which is a part of the molten portion melted during heating. Alternatively, this indicates that at least a portion of the heat-affected zone (non-molten portion) formed on the surface of the metal wire portion 20n near the terminal edge 35 has been torn off by welding. When the molten solidified portion 31 is formed over the entire width of the metal wire portion 20n, the terminal end 30 has a portion where the molten solidified portion 31 is exposed over the entire width of the terminal end 30. Of the molten solidified portion 31, the portion closest to the terminal edge 35 in particular exposes the molten solidified portion 31 over the entire width. This indicates that the metal wire portion 20p has been torn off along the longitudinal direction of the metal wire. The molten solidified portions 31n and 31m have a size that can exert a joining force that can withstand the tension acting on the metal wire portion 20n.

[0029] <Joining target portion> The portion of the metal wire portion 20m to be joined to the terminal end 30 is referred to as the joining target portion 21. The joining target portion 21 will be described as a concept including the portion joined to the terminal end 30 (joined portion) and the portion that could have been joined to the metal wire portion 20n by overlapping with the metal wire portion 20n that becomes the terminal end 30. The joining target portion 21 has a molten solidified portion 31m in which at least a portion of the width direction w of the metal wire portion 20m is melted and solidified. In FIG. 2(b), the exposed molten solidified portion 31m is indicated by diagonal lines. In this example, at least a portion of the molten solidified portion 31m is exposed to the outside. That is, at least a portion of the molten solidified portion 31n formed in the terminal end 30 and at least a portion of the molten solidified portion 31m formed in the joining target portion 21 are both exposed to the outside. The molten solidified portions 31n, 31m exposed to the outside form the outer diameter side surface of the winding body. This indicates that the metal wire portion 20p was separated from the metal wire portion 20n, along with a portion of the molten portion 32 (molten portion 32p) that was melted during heating, thereby exposing the molten solidified portion 31m.

[0030] [Actual Photograph] Figure 3 is a diagram showing an actual photograph of the vicinity of the terminal end of the filter. The thickness of the metal wire 20 used in this figure is 0.2 mm. The right side of the arrow A in the figure is the part where the molten solidified portion 31 is exposed. As shown in the figure, it can be seen that the features shown in Figure 2 (b) also appear in the actual photograph taken around the terminal end 30 of the filter.

[0031] [Winding Body Manufacturing Apparatus] Fig. 4 is a diagram that shows a schematic view of the winding body manufacturing apparatus, mainly showing the winding device. Fig. 5 is a diagram that shows a schematic view of the winding body manufacturing apparatus, particularly showing the downstream side of the guide member. Fig. 5 corresponds to a view of the manufacturing apparatus shown in Fig. 4 as seen from the left side of the figure.

[0032] The winding body manufacturing apparatus 100 includes at least a winding device 130 and a welding device 150 .

[0033] The winding device 130 includes a mandrel 131 that rotates in a fixed direction at a predetermined speed, and a guide member 132 that unwinds the metal wire 20 toward the mandrel 131 with a predetermined tension and moves back and forth at a predetermined speed along the axis Ax2 of the mandrel 131 to guide the metal wire 20. The mandrel 131 is generally columnar or cylindrical, and is generally made of metal such as stainless steel, copper alloy, or aluminum alloy. A tension unit is disposed upstream of the winding device 130 and applies a predetermined tension to the metal wire 20.

[0034] Welding device 150 joins and fixes a suitable location on the winding end side of metal wire 20 to a suitable location on already wound metal wire 20 by resistance spot welding. Welding device 150 includes an electrode (welding electrode) 160 that contacts the workpiece and applies pressure to it while passing welding current I through the workpiece, a power source 155 that supplies power to electrode 160, and a contact electrode 157 that is connected to power source 155 and serves as a port for receiving welding current I. Welding device 150 also includes a welding head 151 that holds electrode 160, first driving means 153 that drives welding head 151, and second driving means 159 that moves contact electrode 157 toward or away from the workpiece. 5, a tangent line TL (of the mandrel 131) is defined in the direction of the metal wire 20 extending from the guide member 132 toward the mandrel 131, and a virtual line passing through the axis Ax2 and perpendicular to both the tangent line TL and the axis Ax2 is defined as a normal line NL (of the mandrel 131). The X-axis, Y-axis, and Z-axis are defined along the axis Ax2, the tangent line TL, and the normal line NL, respectively. Based on the supply direction of the metal wire 20, the guide member 132 side is referred to as the upstream side, and the mandrel 131 side or the side already wound around the mandrel 131 is referred to as the downstream side. The welding device 150 shown in this example applies pressure to the electrode 160 in the direction of the normal line NL of the mandrel 131.

[0035] The first driving means 153 reciprocates the welding head 151 holding the electrode 160 along the axis Ax2 direction (X direction) of the mandrel 131, along the tangent TL direction (Y direction) of the mandrel 131, and moves the electrode 160 toward or away from the mandrel 131 in the Z direction in the figure. The first driving means 153 drives the electrode 160 in the X-Y directions to move the electrode 160 to a position where the metal wire portion 20n and the metal wire portion 20m overlap. The first driving means 153 preferably includes a servo motor or a stepping motor as a means for moving at least the electrode 160 in the X-Y directions. If the electrode 160 can be precisely positioned at least in the X-Y directions by the servo motor or the stepping motor, an air cylinder, which does not require high positioning accuracy, may be used as a means for reciprocating the electrode 160 in the Z direction. The first driving means 153 drives the welding head 151 along the normal NL direction to apply pressure to the welded portion with the electrode 160. The welding head 151 holds the electrode 160 with the central axis Ax3 of the electrode 160 aligned with the pressure direction P, but the welding head 151 can hold the electrode 160 with the central axis Ax3 tilted relative to the pressure direction P as needed. The power source 155 appropriately controls the magnitude, current application time, application cycle, waveform, and other parameters of the welding current I and supplies the current to the electrode 160. Suitable well-known contact electrode 157 and second driving means 159 are used. The shape and other parameters of the electrode 160 will be described later.

[0036] [Filter Manufacturing Method] To manufacture the filter 10, first, one end (starting end, winding start) of the metal wire 20 is secured in a suitable position on a mandrel 131 constituting a winding device 130. With a tension of 0.01 to 20 kgf applied to the metal wire 20, the mandrel 131 is rotated at a predetermined speed in a fixed direction about the central axis Ax2, and a guide member 132 that supplies the metal wire 20 is reciprocated at a predetermined speed along the central axis Ax2 of the mandrel 131. This operation causes the metal wire 20 to be wound around the outer periphery of the mandrel 131 in a spiral and multi-layered manner at a predetermined pitch while tilting at a predetermined angle θ with respect to the central axis Ax2. Furthermore, the metal wires (portions of the metal wire) constituting adjacent wire layers intersect with each other to form a mesh. Furthermore, the meshes overlap in a regular radial arrangement to achieve the desired filtration accuracy. For example, if each metal wire 20 in the first metal wire layer wound directly around the periphery of the mandrel 131 is inclined clockwise by a predetermined angle θ with respect to the axial direction of the mandrel 131, the metal wire 20 constituting the second metal wire layer wound around the periphery of the first metal wire layer will be inclined counterclockwise by the predetermined angle θ with respect to the axial direction of the mandrel 131. After that, after the metal wire 20 has been wound a predetermined number of times (a predetermined number of layers), the rotation of the mandrel 131 is stopped, and the other end (terminal end, winding end side) of the metal wire 20 is joined and fixed to an appropriate position of the wound metal wire 20 by resistance spot welding.

[0037] The welding device 150 brings the electrode 160 and the contact electrode 157 into contact with the winding body 11. As shown in FIG. 8( a) and other figures, the power supply 155 applies a predetermined welding current I while the electrode 160 presses the metal wire portion 20 n against the metal wire portion 20 m with a predetermined pressure. The welding current I is set to a current greater than a current sufficient to join the metal wire portions together. The metal wire portion 20 n is welded to the metal wire portion 20 m while the tension Tp applied during winding is still applied. The welding current I is set to a magnitude that melts the metal wire portion 20 n to the extent that the metal wire portion 20 n can no longer withstand the tension.

[0038] The portion of the metal wire located directly below the electrode 160 is cut by the tension acting on that portion. The metal wire portion 20p located upstream of the electrode 160 is separated from the winding body 11 while the electrode 160 is energized. At this time, the metal wire 20p is separated from the winding body 11 so that a molten solidified portion 31n (see FIG. 2) large enough to exert a bonding force capable of withstanding the tension acting on the metal wire portion 20n remains on the winding body 11 side. Since the metal wire is cut using the tension acting on the metal wire, none of the electrode 160, the mandrel 131, or the tension unit operates during cutting, and the electrode 160 holds down and fixes the welded portion. Furthermore, since the metal wire is melted and cut using the tension acting on the metal wire, welding and cutting can be performed simultaneously, simplifying the manufacturing process.

[0039] After the metal wire is melted, the power supply 155 is turned off. The electrode 160 maintains the pressure until the molten portion 32 of the metal wire portions 20 n and 20 m cools and resolidifies. After the molten portion 32 cools and resolidifies, the electrode 160 and the contact electrode 157 are separated from the winding body 11, and the winding body 11 is removed from the mandrel 131.

[0040] To fuse the metal wire, it is desirable to utilize the tension that has been continuously applied to the metal wire since the time of winding. However, if the metal wire can be fused, since the welded portion is fixed by the electrode 160, the tension applied to the metal wire located upstream of the electrode 160 may be controlled to be greater during fusion than during winding. If the tension is to be changed between during winding and fusion, the tension of the metal wire is adjusted by a tension unit located upstream of the guide member 132. In the above embodiment, the current is stopped after the metal wire is fused, but the metal wire portion 20p may be separated from the winding body 11 after the current to the electrode 160 is stopped and while the electrode is pressing the metal wire.

[0041] The angle (winding angle) of the metal wire 20 relative to the axial direction of the mandrel 131 and the spacing (pitch) between adjacent metal wires 20 in the axial direction can be changed by appropriately adjusting the ratio between the rotation speed of the mandrel 131 and the movement speed of the guide member 132. By appropriately changing the thickness of the metal wire, the winding angle, the pitch, and the number of windings, the pressure loss of the fluid passing through the filter can be controlled to an appropriate value. The inner diameter of the filter 10 corresponds to the outer diameter of the mandrel 131, and the outer diameter of the filter 10 is appropriately adjusted depending on the thickness and number of windings of the metal wire 20. The winding body manufactured by the above method is used as a filter as is, without being sintered as a whole. Alternatively, if necessary, the winding body removed from the mandrel 131 may be subjected to a heat treatment such as sintering to metallurgically bond the contact portions where adjacent metal wire portions contact each other, and then used as a filter.

[0042] [Electrode Shape] Fig. 6 is a perspective view showing an example of an electrode, and Figs. 7(a) and 7(b) are plan views illustrating the relationship between the electrode tip surface and the metal wire rod in contact with the electrode tip surface.

[0043] The electrode 160 has an electrode tip surface 161 that can come into contact with the metal wire during welding. The electrode tip surface 161 has a shape and size that can cover the entire width of the metal wire 20 over a predetermined longitudinal length of the metal wire. That is, the electrode tip surface 161 has a first length Le1 that can cover the entire width (length W) of the metal wire during welding, and a second length Le2 that covers a predetermined longitudinal length of the metal wire and is longer than the first length. However, the length Le1 of the electrode tip surface 161 is set to a length that does not come into contact with other portions of the metal wire that are not to be welded. The "other metal wire portion that is not to be welded" referred to here is a metal wire portion that extends in the same direction as the metal wire portion 20n (terminal end 30) that contacts the electrode tip surface 161, that forms the surface on the outer diameter side of the winding body 11 (exposed on the outer diameter side), and that is adjacent to the terminal end 30 in the axial direction of the winding body 11, and does not necessarily mean a metal wire portion that belongs to the wire layer Ln (see Figure 1).

[0044] The length Le1 of the electrode tip surface 161 is set to a length that melts the entire width of the metal wire 20 and ensures reliable melting of the metal wire. Therefore, the length Le1 is set to be longer than the widthwise length w of the metal wire 20. The length Le2 of the electrode tip surface 161 is set to a length that forms a melted portion that can melt the metal wire portion located upstream of the electrode 160 and leaves a melted portion necessary for securing the end of the metal wire 20 on the winding side after the upstream metal wire portion is separated. The entire width of the metal wire portion 20n can be melted and joined to the metal wire portion 20m, ensuring sufficient joint strength. The illustrated electrode 160 is rectangular with a roughly rectangular electrode tip surface 161, but the shape of each part of the electrode 160 is not limited to this. Furthermore, although the figure shows an electrode having an electrode tip surface 161 perpendicular to the central axis Ax3, the central axis Ax3 and the electrode tip surface 161 do not have to be perpendicular to each other (e.g., FIG. 9(b)).

[0045] As long as the electrode 160 can separate the portion of the metal wire 20 located upstream of the electrode 160 and can fix the remaining portion of the metal wire 20 to the winding, the metal wire 20 may assume any orientation (angle) within the electrode tip surface 161. For example, if the electrode tip surface 161 is rectangular, the metal wire 20 may be brought into contact with the electrode tip surface 161 so that its longitudinal direction coincides with the longitudinal direction (length Le1 direction) of the electrode tip surface 161, as shown in FIG. 7( a). Alternatively, as shown in FIG. 7( b), the metal wire 20 may be brought into contact with the electrode tip surface 161 at an angle so that its longitudinal direction does not coincide with the longitudinal direction (length Le1 direction) of the electrode tip surface 161. The same applies when the electrode tip surface is not rectangular. In this way, the electrode 160 only needs to apply pressure to the metal wire 20 with its longitudinal direction generally aligned with the longitudinal direction of the electrode tip surface 161.

[0046] 8 to 10 are schematic diagrams showing the state immediately before the metal wire is cut, in which the metal wire to be welded is pressed with the electrode and a current is passed through the electrode to form a molten zone.

[0047] <Pressure Application of Metal Wire by Electrode 1> An electrode 160 shown in FIGS. 8( a ) and 8 ( b ) corresponds to the electrode shown in FIG. 6 and has an electrode tip surface 161 perpendicular to the central axis Ax3 .

[0048] FIG. 8( a) shows a state in which the metal wire portions 20 n and 20 m are welded by pressing the electrode 160 in a pressure direction P along the central axis Ax3 with the electrode 160 aligned with the normal line NL. The fusion zone 32 is uniformly formed on the upstream side (right side in the figure) and downstream side (left side in the figure) of the normal line NL. Although the fusion zone 32 shown does not reach the outer diameter surface of the metal wire portion 20 n, depending on the welding conditions, including the magnitude of the welding current I, the metal wire portion 20 n may be melted to the outer diameter surface, and the fusion zone 32 may come into contact with the electrode tip surface 161. Note that in FIGS. 8( b) to 10 , the metal wire portion 20 n may also be melted to the outer diameter surface.

[0049] The metal wire 20 is melted at the upstream portion of the fusion zone 32 by the tension Tp acting in the longitudinal direction. Then, the metal wire portion 20p located upstream of the electrode 160 is separated from the winding 11. The tension Tn=Tp also acts on the metal wire portion 20n located downstream of the electrode 160, but the unwinding force has a Z-direction component and is pressed in the Z direction by the electrode 160, so the downstream portion of the fusion zone 32 (to the left of the normal line NL in the figure) does not melt and this portion is eventually joined to the winding 11 to become the termination portion 30.

[0050] Because spot welding is performed while tension is applied to the metal wire 20, when the electrode 160 starts to apply pressure, an equal tension Tp = Tn acts on the upstream and downstream sides of the fusion zone 32. Therefore, in this example, in which the fusion zone 32 is evenly formed on the upstream and downstream sides of the normal line NL, the metal wire 20 may melt at both the downstream and upstream parts of the fusion zone 32. To prevent this situation, as shown in FIG. 8( a ), it is desirable to operate the tension unit so that the tension Tp > Tn after the electrode 160 applies pressure to the metal wire portions 20 n and 20 m. This prevents the downstream part of the fusion zone 32 and the unmelted part of the metal wire portion 20 n from being torn off by the tension Tn acting on the metal wire portion 20 n, and allows the metal wire portion 20 p to be separated from the winding 11.

[0051] 8(b) shows a state in which the metal wire portions 20n and 20m are welded together by pressing the electrode 160 in a pressing direction P along the central axis Ax3 with the electrode 160, with the central axis Ax3 of the electrode 160 positioned downstream of the normal line NL. In this figure, the normal line NL is located outside the electrode tip surface 161, but the electrode 160 may be positioned so that the normal line NL is located within the plane of the electrode tip surface 161. Because the central axis Ax3 of the electrode 160 is positioned downstream of the normal line NL, the pressing force applied by the electrode 160 to the metal wire portions 20n and 20m is relatively large in the upstream portion of the electrode 160 and relatively small in the downstream portion of the electrode 160. This pressing force changes continuously depending on the distance from the normal line NL.

[0052] At the upstream portion of the electrode 160, sufficient pressing force reduces the electrical resistance between the metal wire portions 20n and 20m, allowing the welding current I to flow efficiently. At the downstream portion of the electrode 160, the pressing force is smaller than at the upstream portion, resulting in a higher electrical resistance. Therefore, the welding current I flowing between the metal wire portions 20n and 20m is smaller than at the upstream portion. The molten zone 32 formed between the metal wire portions 20n and 20m is relatively large on the upstream side and relatively small on the downstream side. This makes it easier to melt the metal wire portion 20p located upstream of the electrode 160, while preventing unnecessary melting of the metal wire portion 20n located downstream of the electrode 160, ensuring the necessary joint strength between the metal wire portions 20n and 20m.

[0053] Since the metal wire 20 has an oxide coating on its surface in most cases, by taking advantage of the relatively large pressure in the upstream portion of the electrode 160, the oxide coating of the metal wire in the upstream portion of the electrode 160 can be destroyed, effectively reducing the electrical resistance in that portion.

[0054] Depending on the distance between the central axis Ax3 and the normal line NL and the pressure applied by the electrode 160 to the metal wire 20, it is also possible to prevent the welding current I from flowing in the downstream portion of the electrode tip surface 161. In this case, the non-current-carrying portion of the electrode tip surface 161 functions as a pressure cooling portion that presses and cools the metal wire portions 20n, 20m. Conversely, the current-carrying portion of the electrode tip surface 161 functions as a pressure current-carrying portion that presses and applies current to the metal wire portions 20n, 20m. The pressure cooling portion presses the metal wire portions 20n, 20m, and the tension Tn acting on the metal wire portion 20n prevents the metal wire portion 20n from separating from the metal wire portion 20m.

[0055] <Pressure application 2 of metal wire rod by electrode> FIGS. 9(a) and 9(b) show an example in which pressure is applied to metal wire rod portions 20n and 20m in a state in which the electrode tip surface 161 is inclined with respect to the tangent line TL.

[0056] FIG. 9( a) illustrates an example using an electrode 160 having an electrode tip surface 161 perpendicular to the central axis Ax3, as shown in FIG. 6 . In this example, the pressure direction P coincides with the direction of the normal line NL, and the intersection of the electrode tip surface 161 and the central axis Ax3 is on the normal line NL. However, because the central axis Ax3 of the electrode 160 is inclined upstream by an angle φ with respect to the normal line NL, the pressure applied by the electrode 160 to the metal wire portions 20 n and 20 m is greater in the upstream portion of the electrode 160 and smaller in the downstream portion. Therefore, for the same reason as in FIG. 8( b), the fusion zone 32 formed between the metal wire portions 20 n and 20 m is relatively larger in the upstream portion and relatively smaller in the downstream portion. This example achieves the same effect as in FIG. 8( b). The pressure direction P may also coincide with the direction of the central axis Ax3.

[0057] FIG. 9( b ) shows an example using an electrode 160 having an electrode tip surface 161 that is not perpendicular to the central axis Ax3. In this electrode 160, the axis Ax4, which is perpendicular to the electrode tip surface 161, is inclined upstream by an angle λ with respect to the central axis Ax3. In this example, the pressure direction P coincides with the direction of the normal line NL, and the intersection of the electrode tip surface 161 and the central axis Ax3 is on the normal line NL. However, because the upstream portion of the electrode tip surface 161 protrudes toward the tip of the electrode 160, the pressure applied to the metal wire by the electrode 160 is greater in the upstream portion of the electrode 160 and smaller in the downstream portion. Therefore, for the same reason as in FIG. 8( b ), the fusion zone 32 formed between the metal wire portions 20 n and 20 m is relatively large on the upstream side and relatively small on the downstream side. This example achieves the same effect as in FIG. 8( b ). The pressure direction P may also coincide with the direction of the axis Ax4.

[0058] <Pressing of metal wire by electrode 3> The electrode 160 shown in Figures 10(a) and (b) has a pressing and current-carrying section 163 at the upstream side that applies pressure to the metal wire portions 20n and 20m while passing current through them, and a pressing and cooling section 165 at the downstream side that cools the metal wire portions 20n and 20m while pressing them.

[0059] The electrode 160 shown in FIG. 10( a) is entirely made of a conductor and is integrally formed. The pressure conducting portion 163 protrudes toward the tip of the electrode 160 beyond the pressure cooling portion 165. A step 164 is formed between the pressure conducting portion 163 and the pressure cooling portion 165. The electrode tip surface 161 on the pressure conducting portion 163 side and the electrode tip surface 161 on the pressure cooling portion 165 side are each approximately rectangular and are flat surfaces perpendicular to the central axis Ax3. This figure shows how the metal wire portions 20 n and 20 m are welded together by pressing the electrode 160 in a pressure direction P along the central axis Ax3 with the central axis Ax3 and the normal line NL aligned. Because the pressure current conducting portion 163 protrudes toward the tip of the electrode 160, even if the central axis Ax3 of the electrode 160 and the normal line NL are aligned, the force with which the pressure current conducting portion 163 applies pressure to the metal wire portion can be greater than the force with which the pressurizing and cooling portion 165 presses the metal wire portion. Because there is a step between the pressure current conducting portion 163 and the pressurizing and cooling portion 165, the pressure with which the pressure current conducting portion 163 applies pressure to the metal wire and the pressure with which the pressurizing and cooling portion 165 press the metal wire portion can be made to differ stepwise (discontinuously). Furthermore, the central axis Ax5 of the pressure current conducting portion 163 is located upstream of the normal line NL. Therefore, the pressure current conducting portion 163 applies a sufficient pressure to sufficiently reduce the electrical resistance between the metal wire portions 20n and 20m, allowing the welding current I to flow efficiently. In the pressure cooling portion 165, the pressure is clearly smaller than that in the pressure conducting portion 163, so the electrical resistance is large and it is possible to prevent the welding current I from flowing.

[0060] The electrode 160 forms a molten zone 32 only between the metal wire portions 20n, 20m on the pressurizing and current-carrying portion 163 side. The pressurizing and cooling portion 165 presses and cools the metal wire portions 20n, 20m. The pressurizing and cooling portion 165 presses the metal wire portions 20n, 20m, and the tension Tn acting on the metal wire portion 20n keeps the metal wire portion 20n from separating from the metal wire portion 20m. This makes it possible to melt only the portion of the metal wire 20 located upstream of the electrode 160. Since the metal wire 20 almost always has an oxide film formed on its surface, the oxide film of the metal wire can be destroyed at the pressurizing and current-carrying portion 163, which is the side with the larger pressurizing force, thereby effectively reducing the electrical resistance in that portion.

[0061] The electrode 160 shown in FIG. 10( b) includes an insulating member 167 disposed between the pressure conducting portion 163 and the pressure cooling portion 165. The entire tip surface of the electrode 160 is a flat surface perpendicular to the central axis. The tip surface on the pressure conducting portion 163 side is the electrode tip surface 161, which can be electrically conducted, and the tip surface on the pressure cooling portion 165 side is the non-electrical pressing surface 169. The pressure conducting portion 163 and the pressure cooling portion 165 can be made of the same material. The pressure cooling portion 165 is preferably made of a material with high thermal conductivity. Note that the insulating member 167 can be omitted by making the pressure cooling portion 165 itself an insulator. This figure shows the metal wire portions 20 n and 20 m being welded by pressing them with the electrode 160 in the pressure direction P along the central axis Ax3 with the central axis Ax3 and the normal line NL aligned. The molten zone 32 is formed only between the metal wire portions 20n and 20m on the side of the pressurizing and current-carrying portion 163. The function of the pressurizing and cooling portion 165 is the same as that of the electrode shown in FIG.

[0062] According to this example, it is possible to melt and cut only the portion of the metal wire portion 20n located in the upstream portion of the electrode 160. Note that, similar to FIG. 10(a), the pressurizing and energizing portion 163 may be made to protrude further toward the tip side than the pressurizing and cooling portion 165.

[0063] [Effects] In the filter 10 according to this embodiment, the terminal end 30 is fused at the welded location. That is, during the manufacture of the filter 10, the welding and fusion of the terminal end 30 are performed simultaneously. Therefore, according to this embodiment, it is possible to provide a winding in which the distance from the weld to the terminal edge is as short as possible without increasing the number of manufacturing processes. By making the distance from the weld to the terminal edge as short as possible, particularly zero, it is possible to manufacture a winding in which the terminal end of the metal wire will not damage other components, and it is also possible to prevent the occurrence of defective windings in which the weld has peeled off.

[0064] [Summary of Embodiments, Functions, and Effects of the Present Invention] <Winding> <<First Embodiment>> This embodiment is a porous winding (filter 10) in which at least one continuous metal wire 20 is wound in a spiral and multilayered manner. In the winding, the terminal end 30 of the metal wire (metal wire portion 20n) is resistance spot welded to another portion of the metal wire (metal wire portion 20m) and is melt-cut at the welded location. Here, the terminal end is defined as the portion closer to the terminal edge 35 than the welding electrode indentation 33. This embodiment provides a winding in which the distance from the weld to the terminal edge is minimized without increasing the number of manufacturing steps. It is also possible to use the terminal edge as the weld. Such a winding has the external features shown in the third to eleventh embodiments, which are traces of the metal wire being cut.

[0065] <<Second Embodiment>> This embodiment is a porous winding (filter 10) in which at least one continuous metal wire 20 is wound helically and in multiple layers. In the winding, the terminal end 30 of the metal wire (metal wire portion 20n) is resistance spot welded to another portion of the metal wire (metal wire portion 20m), melted at the welded location, and a heat-affected zone near the welded location is torn off. Here, the terminal end is defined as the portion closer to the terminal edge 35 than the welding electrode indentation 33. This embodiment provides a winding in which the distance from the weld to the terminal edge is minimized without increasing the number of manufacturing steps. It is also possible to use the terminal edge as the weld. Such a winding has the external features shown in the third to eleventh embodiments, which are traces of the metal wire being cut.

[0066] <<Third embodiment>> In the winding body (filter 10) according to this embodiment, the terminal end 30 (metal wire portion 20n) is characterized by having a molten solidified portion 31n formed after the entire width of the metal wire is melted and then solidified. More specifically, the molten solidified portion is formed over a predetermined longitudinal length from the terminal edge of the metal wire. According to this embodiment, since the entire width is melted, the metal wire can be reliably melted at that portion. Furthermore, since the terminal end is joined to another portion of the metal wire by melting the entire width, the joining strength can be ensured.

[0067] <<Fourth Embodiment>> In the winding (filter 10) according to this embodiment, the terminal end 30 (metal wire portion 20n) is characterized in that the thickness of the metal wire gradually decreases toward the terminal end edge 35 of the metal wire. The external feature of the winding according to this embodiment indicates that a portion of the thickness of the metal wire near the terminal end, particularly that located on the outer diameter side, does not remain on the winding due to melting. This external feature also appears when the terminal end is stretched toward the terminal end due to melting or softening. Because nippers, scissors, etc. cannot cut the metal wire at the welded portion, this feature according to this embodiment does not appear in cutting methods that utilize shear force using nippers, scissors, etc. In other words, if the metal wire is not cut at the spot-welded portion, the entire indentation remains on the metal wire, and therefore, when the metal wire is cut with nippers, scissors, etc., the thickness does not gradually decrease toward the terminal end.

[0068] <<Fifth Embodiment>> The winding (filter 10) according to this embodiment is characterized in that the terminal end 30 (metal wire portion 20n) has a drawing mark 37 formed thereon, which indicates that the softened metal wire has been drawn toward the terminal end edge 35. In order to shape the metal wire into a predetermined winding shape, a predetermined tension is applied to the metal wire during winding. The drawing mark indicates that the metal wire has been melted down using the tension applied during winding.

[0069] <<Sixth embodiment>> In the winding body (filter 10) according to this embodiment, the terminal end 30 (metal wire portion 20n) has a molten solidified portion 31n formed by melting at least a portion of the metal wire in the width direction and then solidifying, and at least a portion of the molten solidified portion is exposed to the outside. Normally, a molten solidified portion that appears on the outside in spot welding indicates a poor weld, so when spot welding is performed, the molten solidified portion is generally not exposed to the outside. However, in this embodiment, the metal wire is melted, so at least a portion of the molten solidified portion is exposed to the outside.

[0070] <<Seventh embodiment>> In the winding body (filter 10) according to this embodiment, the terminal end 30 (metal wire portion 20n) has a molten solidified portion 31n formed after at least a portion of the metal wire in the width direction has melted and solidified, and the terminal end edge 35 of the metal wire is a molten solidified portion, and the molten solidified portion is exposed to the outside from the terminal end over a predetermined longitudinal length of the metal wire. In this embodiment, the metal wire is melted, so the molten solidified portion is exposed to the outside. Since a portion of the molten portion melted during heating is separated from the winding body, the molten solidified portion is exposed to the outside from the terminal end over a predetermined longitudinal length.

[0071] <<Eighth embodiment>> In the winding body (filter 10) according to this embodiment, the terminal end 30 (metal wire portion 20n) has a molten solidified portion 31n formed after at least a portion of the metal wire in the width direction has melted and solidified, and at least a portion of the molten solidified portion is exposed to the outside, and the portion of the molten solidified portion exposed to the outside has a portion whose thickness gradually decreases toward the terminal edge 35 of the metal wire. The above-mentioned external characteristics of the winding body according to this embodiment indicate that the terminal end is extended in the direction of the terminal edge, and that a portion of the thickness of the metal wire located on the outer diameter side near the terminal end does not remain on the winding body side due to melting. Such characteristics do not appear when the metal wire is cut using shear force, such as with scissors or nippers.

[0072] <<Ninth embodiment>> In the winding body (filter 10) according to this embodiment, the terminal end 30 (metal wire portion 20n) and another portion of the metal wire (metal wire portion 20m) each have a molten solidified portion 31 (31n, 31m) that solidifies after melting, and at least a portion of the molten solidified portion 31m formed in another portion of the metal wire is exposed to the outside. The above-mentioned feature of the winding body according to this embodiment indicates that the upstream metal wire portion 20p is separated from the metal wire portion 20n together with a portion of the molten portion (molten portion 32p) that was melted during heating.

[0073] <<Tenth embodiment>> In the winding body (filter 10) according to this embodiment, the terminal end 30 (metal wire portion 20n) and the other portion of the metal wire (metal wire portion 20m) each have a molten solidified portion 31 (31n, 31m) that solidifies after melting, and at least a portion of the molten solidified portion 31n formed at the terminal end and at least a portion of the molten solidified portion 31m formed in the other portion of the metal wire are both exposed to the outside. The above-mentioned feature of the winding body according to this embodiment indicates that the upstream metal wire portion 20p is separated from the metal wire portion 20n along with a portion of the molten portion (molten portion 32p) that was melted during heating. In addition, in this embodiment, the metal wire is melted, and the molten solidified portion 31n is exposed to the outside.

[0074] <<Eleventh embodiment>> In the winding body (filter 10) according to this embodiment, the terminal end 30 has a molten solidified portion 31n formed after the metal wire 20 melts and solidifies, and the molten solidified portion formed within the width of the metal wire portion 20n constituting the terminal end is exposed to the outside. The molten solidified portion exposed to the outside constitutes the outer diameter side surface of the winding body. The external feature of the winding body according to this embodiment indicates that a portion of the thickness of the metal wire located on the outer diameter side near the terminal end did not remain on the winding body side due to melting. Furthermore, at least the molten solidified portion constituting the outer diameter side surface of the winding body does not leak sideways.

[0075] <Method for Manufacturing a Winding Body> <<Twelfth Embodiment>> This embodiment is a method for manufacturing a porous winding body (filter 10) in which at least one continuous metal wire 20 is wound in a spiral and in multiple layers. This embodiment includes a winding process in which the metal wire is wound in a spiral and in multiple layers around a mandrel 131 while applying a predetermined tension to the metal wire, and a welding process in which the winding end portion of the metal wire (metal wire portion 20n, terminal end 30) is welded to the wound metal wire portion 20m by resistance spot welding. The welding process is characterized in that the tension continuously applied to the metal wire is used to fuse the supply-side metal wire portion from the wound metal wire portion. In this embodiment, the metal wire is fuse-cut using the tension acting on the metal wire, allowing welding and cutting to be performed simultaneously, thereby simplifying the winding body manufacturing process. The tension applied to the metal wire during the fuse-cutting process may be the same as or different from the tension applied to the metal wire in the winding process. According to this aspect, it is possible to provide a winding body in which the distance from the welded portion to the terminal edge is as short as possible without increasing the number of manufacturing steps.

[0076] <<Thirteenth Embodiment>> In the manufacturing method according to this embodiment, when the side where the metal wire 20 is supplied to the mandrel 131 is defined as the upstream side and the side where the metal wire 20 has already been wound around the mandrel is defined as the downstream side, the welding step is characterized in that the welding electrode 160 is brought into contact with the metal wire portion 20n so that the pressure applied by the welding electrode 160 at the upstream side is greater than the pressure applied by the welding electrode at the downstream side (FIGS. 8(b) to 10). According to this embodiment, the molten portion is made larger at the upstream side where the pressure is greater and smaller at the downstream side where the pressure is less. As a result, the metal wire portion at the upstream side is more likely to melt. Furthermore, unnecessary melting of the metal wire portion at the downstream side can be prevented.

[0077] <<Fourteenth Embodiment>> In the manufacturing method according to this embodiment, the extension direction of the metal wire 20 supplied toward the mandrel 131 is defined as the tangent line TL direction, and an imaginary line passing through the mandrel axis Ax2 and perpendicular to both the tangent line and the axis is defined as the mandrel normal line NL. In the welding process, the welding electrode 160 is positioned so that its central axis Ax3 is downstream of the normal line. With the normal line and the central axis aligned, the metal wire (metal wire portion 20n) is pressed in the normal direction by the welding electrode to weld the winding end of the metal wire to the already wound metal wire portion 20m ( FIG. 8( b) ). According to this embodiment, because the central axis of the welding electrode is positioned downstream of the normal line, the pressure applied at the upstream portion of the welding electrode can be greater than the pressure applied at the downstream portion of the welding electrode. Therefore, the same effect as that of the eleventh embodiment can be achieved.

[0078] <<Fifteenth Embodiment>> In the manufacturing method according to this aspect, the extension direction of the metal wire 20 supplied toward the mandrel 131 is defined as the tangent line TL direction, and an imaginary line passing through the mandrel axis Ax2 and perpendicular to both the tangent line and the axis is defined as the mandrel normal line NL. In the welding step, the normal lines Ax3 and Ax4 to the electrode tip surface 161 of the welding electrode 160 are inclined toward the supply side of the metal wire relative to the mandrel normal line NL, and the metal wire is pressed by the welding electrode to weld the winding end portion of the metal wire to the already wound metal wire portion 20m. In this aspect, by inclining the normal line to the electrode tip surface, the pressure applied at the upstream portion of the welding electrode is made greater than the pressure applied at the downstream portion of the welding electrode. This example also achieves the same effects as the eleventh embodiment.

[0079] <Welding Electrode> <<Sixteenth Embodiment>> The welding electrode 160 according to this embodiment is a welding electrode used when winding at least one continuous metal wire 20 around a rotating mandrel 131 to produce a porous winding (filter 10) in which the metal wire is wound in a spiral and multilayered configuration. The welding electrode 160 is characterized by having an electrode tip surface 161 having a first length Le1 sufficient to cover the entire width of the metal wire during welding ( FIGS. 6 to 10 ). According to this embodiment, the entire width of the metal wire can be melted, thereby ensuring reliable melt-cutting of the metal wire. According to this embodiment, a winding can be provided in which the distance from the weld to the terminal edge is minimized without increasing the number of manufacturing steps. According to this embodiment, the entire width of the metal wire, for example, the terminal end 30, can be melted and joined to another portion of the metal wire (metal wire portion 20m), thereby ensuring joint strength.

[0080] Seventeenth Embodiment In a welding electrode 160 according to this embodiment, the electrode tip surface 161 has a second length Le2 that can cover a predetermined length in the longitudinal direction of the metal wire 20, and is characterized in that it is provided with a pressure current-carrying portion 163 on one side in the second length direction that applies pressure to two overlapping metal wire portions 20 n, 20 m to be welded while applying current to both metal wire portions, and a pressure cooling portion 135 on the other side in the second length direction that presses and cools one metal wire portion in contact with the electrode tip surface ( FIGS. 10 and 9( b)). According to this embodiment, the metal wire can be melted in the pressure current-carrying portion while not being melted in the pressure cooling portion.

[0081] <<Eighteenth embodiment>> In the welding electrode 160 according to this embodiment, the pressure conducting portion 163 is characterized in that it protrudes further toward the tip of the welding electrode than the press cooling portion 165 (FIGS. 10(a) and 9(b)). According to this embodiment, by having the pressure conducting portion protrude further toward the tip of the welding electrode than the press cooling portion, the pressure and melting portion of the metal wire portion by the pressure conducting portion can be increased, and the pressure and melting portion of the metal wire portion by the press cooling portion can be decreased. As a result, the metal wire portion on the pressure conducting portion side can be more easily melted. Furthermore, unnecessary melting of the metal wire portion can be prevented in the press cooling portion.

[0082] <<Nineteenth embodiment>> In the welding electrode 160 according to this embodiment, the press cooling portion 165 is configured so as not to be electrified ( FIG. 10( b) ). According to this embodiment, the metal wire can be welded and melted in the press electrification portion, while the metal wire can be prevented from melting in the press cooling portion.

[0083] <Apparatus for Manufacturing a Winding Body> <<Twentieth Embodiment>> This embodiment is a manufacturing apparatus 100 that manufactures a porous winding body (filter 10) by winding at least one continuous metal wire 20 in a spiral and multiple layers. The manufacturing apparatus includes a mandrel 131 that rotates in a fixed direction at a predetermined speed and around which the metal wire is wound in a spiral and multiple layers, and a welding device 150 that welds the winding end of the metal wire (metal wire portion 20n) to the already wound metal wire portion 20m by resistance spot welding. The welding device is characterized by including a welding electrode 160 (shown) described in any of the fourteenth to seventeenth embodiments. This manufacturing apparatus achieves the effects described in the fourteenth to seventeenth embodiments.

[0084] L...wire layer, w...width of metal wire, t...thickness of metal wire, Le1, Le2...length of electrode tip surface, Tn, Tp...tension, Ax1...center axis of filter, Ax2...axis of mandrel, Ax3...center axis of electrode, Ax4...axis perpendicular to electrode tip surface, Ax5...center axis of pressurized current-carrying part, 10...filter, 20...metal wire, 20n, 20m...metal wire part, 20p...(separated) metal wire part, 21...(part to be joined of metal wire part 20m), 30...termination part, 31, 31n, 31m... Melted solidified portion, 32... molten portion, 32p... (separated) molten portion, 33... indentation, 35... terminal edge, 37... drawing mark, 100... manufacturing apparatus, 130... winding apparatus, 131... mandrel, 132... guide member, 150... welding apparatus, 151... welding head, 153... first driving means, 155... power source, 157... contact electrode, 159... second driving means, 160... electrode (welding electrode), 161... electrode tip surface, 163... pressurizing current-carrying portion, 164... step, 165... pressure cooling portion, 167... insulating member, 169... pressing surface

Claims

1. A multi-hole winding in which at least one continuous metal wire is wound in a spiral and in multiple layers, wherein the end of the metal wire is resistance spot welded to another portion of the metal wire and is melted at the welded point.

2. A multi-hole winding in which at least one continuous metal wire is wound in a spiral and in multiple layers, wherein the end of the metal wire is resistance spot welded to another portion of the metal wire, and is melted at the welded point, and the heat-affected zone in the vicinity of the welded point is torn off.

3. A porous winding in which at least one continuous metal wire is wound in a spiral and in multiple layers, wherein the terminal end of the metal wire is resistance spot welded to another portion of the metal wire and is melted at the welded location or at the welded location and a heat-affected zone in the vicinity of the welded location, and wherein the terminal end has a molten solidified portion formed by melting the entire width of the metal wire over a predetermined longitudinal length range from the terminal edge of the metal wire and then solidifying.

4. A porous winding in which at least one continuous metal wire is wound in a spiral and in multiple layers, wherein the terminal end of the metal wire is resistance spot welded to another portion of the metal wire and is melted at the welded location or at the welded location and a heat-affected zone adjacent to the welded location, and wherein the thickness of the metal wire at the terminal end gradually decreases toward the terminal edge of the metal wire.

5. A porous winding in which at least one continuous metal wire is wound in a spiral and in multiple layers, wherein the terminal end of the metal wire is resistance spot welded to other parts of the metal wire and is melted at the welded point and at a heat-affected zone in the vicinity of the welded point, and wherein the terminal end has a drawing mark indicating that the softened metal wire has been drawn toward the terminal edge.

6. A porous winding in which at least one continuous metal wire is wound in a spiral and in multiple layers, wherein the terminal end of the metal wire is resistance spot welded to another portion of the metal wire and is melted at the welded location or at the welded location and a heat-affected zone in the vicinity of the welded location, and the terminal end has a molten solidified portion formed by melting at least a portion of the metal wire in the width direction and then solidifying, and at least a portion of the molten solidified portion is exposed to the outside.

7. A porous winding in which at least one continuous metal wire is wound in a spiral and in multiple layers, wherein a terminal end of the metal wire is resistance spot welded to another portion of the metal wire and is melted at the welded location or at the welded location and a heat-affected zone in the vicinity of the welded location, and wherein the terminal end has a molten solidified portion formed after at least a portion of the metal wire in the width direction has melted and solidified, and the terminal edge of the metal wire is the molten solidified portion, and the molten solidified portion is exposed to the outside from the terminal edge over a predetermined longitudinal length of the metal wire.

8. A porous winding in which at least one continuous metal wire is wound in a spiral and in multiple layers, wherein the terminal end of the metal wire is resistance spot welded to another portion of the metal wire and is melted at the welded location or at the welded location and a heat-affected zone in the vicinity of the welded location, wherein the terminal end has a molten solidified portion that has solidified after at least a portion of the metal wire in the width direction has melted, at least a portion of the molten solidified portion is exposed to the outside, and the exposed portion of the molten solidified portion has a portion whose thickness gradually decreases toward the terminal edge of the metal wire.

9. A porous winding in which at least one continuous metal wire is wound in a spiral and in multiple layers, wherein the terminal end of the metal wire is resistance spot welded to another portion of the metal wire and is melted at the welded location or at the welded location and a heat-affected zone in the vicinity of the welded location, and the terminal end and the other portion of the metal wire each have a molten solidified portion that has solidified after melting, and at least a portion of the molten solidified portion formed on the other portion of the metal wire is exposed to the outside.

10. A porous winding in which at least one continuous metal wire is wound in a spiral and in multiple layers, wherein the terminal end of the metal wire is resistance spot welded to another portion of the metal wire and is melted at the welded location or at the welded location and a heat-affected zone in the vicinity of the welded location, and the terminal end and the other portion of the metal wire each have a molten solidified portion that has solidified after melting, and at least a portion of the molten solidified portion formed at the terminal end and at least a portion of the molten solidified portion formed on the other portion of the metal wire are both exposed to the outside.

11. A porous winding in which at least one continuous metal wire is wound in a spiral and in multiple layers, wherein the terminal end of the metal wire is resistance spot welded to another portion of the metal wire and is melted at the welded location or at the welded location and a heat-affected zone in the vicinity of the welded location, wherein the terminal end has a molten solidified portion formed after the metal wire has melted and solidified, and wherein the molten solidified portion formed within the width of the metal wire portion constituting the terminal end is exposed to the outside.

12. A method for manufacturing a porous winding body in which at least one continuous metal wire is wound in a spiral and in multiple layers, comprising: a winding step in which the metal wire is wound in a spiral and in multiple layers around a mandrel while applying a predetermined tension to the metal wire; and a welding step in which the winding end of the metal wire is welded by resistance spot welding to the wound metal wire portion, wherein the welding step utilizes the tension continuously applied to the metal wire to fuse the supply side metal wire portion from the wound metal wire portion.

13. A method for manufacturing a winding body as described in claim 12, characterized in that, when the side where the metal wire is supplied to the mandrel is the upstream side and the side where the metal wire has already been wound around the mandrel is the downstream side, in the welding process, the welding electrode is brought into contact with the metal wire portion so that the pressure applied to the metal wire portion at the upstream side of the welding electrode is greater than the pressure applied to the metal wire portion at the downstream side of the welding electrode.

14. A method for manufacturing a winding body as described in claim 13, characterized in that, when the extension direction of the metal wire supplied toward the mandrel is defined as the tangential direction and an imaginary line passing through the axis of the mandrel and perpendicular to both the tangent line and the axis line is defined as the normal line to the mandrel, in the welding process, the welding electrode is positioned so that its central axis is downstream of the normal line, and with the normal line and the central axis line aligned, the metal wire is pressed in the normal direction by the welding electrode to weld the end of the winding of the metal wire to the already wound portion of the metal wire.

15. A method for manufacturing a winding body as described in claim 13, characterized in that, when the extension direction of the metal wire being supplied toward the mandrel is defined as the tangential direction and an imaginary line passing through the axis of the mandrel and perpendicular to both the tangential line and the axis is defined as the normal line to the mandrel, in the welding process, the normal line to the electrode tip surface of the welding electrode is tilted toward the supply side of the metal wire with respect to the normal line to the mandrel, and the metal wire is pressed by the welding electrode to weld the end of the winding of the metal wire to the part of the metal wire that has already been wound.

16. A welding electrode used when winding at least one continuous metal wire around a rotating mandrel to produce a porous winding body in which the metal wire is wound in a spiral and multi-layered manner, the welding electrode having an electrode tip surface with a first length capable of covering the entire width of the metal wire during welding.

17. A welding electrode as described in claim 16, characterized in that the electrode tip surface has a second length capable of covering a predetermined length in the longitudinal direction of the metal wire, and is provided on one side of the second length direction with a pressure conducting section that applies pressure to two overlapping metal wire portions to be welded while passing current through both metal wire portions, and on the other side of the second length direction with a pressure cooling section that cools the metal wire portion in contact with the electrode tip surface while pressing it.

18. A welding electrode according to claim 17, characterized in that the pressure conducting portion protrudes further in the direction of the tip of the welding electrode than the pressure cooling portion.

19. The welding electrode according to claim 17, wherein the press cooling portion is configured so as not to be energized.

20. A manufacturing apparatus for manufacturing a porous winding body by winding at least one continuous metal wire in a spiral and in multiple layers, comprising: a mandrel that rotates in a fixed direction at a predetermined speed and around which the metal wire is wound in a spiral and in multiple layers; and a welding device that welds the winding end of the metal wire to the wound metal wire portion by resistance spot welding, wherein the welding device is equipped with a welding electrode as defined in any one of claims 16 to 19.