Method of producing iron ore pellets

MYPI2025000852A0Undetermined Publication Date: 2024-03-01JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025000852
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-01
Filing Date
2023-05-10
Publication Date
2024-03-01

AI Technical Summary

Technical Problem

The existing methods for producing iron ore pellets, particularly using low-grade ores with high crystallization water content, face challenges in suppressing bursting and ensuring adequate strength, as the current decrystallization water treatment processes do not adequately control crystallization water removal and particle size distribution, leading to reduced crushability and increased bursting risks.

Method used

A method involving a decrystallization water treatment step where iron ore with an iron content of 63% or less is heated between 100°C and 800°C for 5 to 200 minutes to remove crystallization water, followed by crushing to achieve a particle size distribution of 10% to 70% of particles 10 μm or less, which enhances the strength and suppresses bursting during the firing process.

Benefits of technology

This method effectively increases the strength of green pellets to 1.0 kg or more and reduces bursting, as evidenced by a passing rate of pellet pieces of 3.0% or less through a 5 mm sieve, thereby improving the yield and quality of fired pellets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025000852_DRAWING_001
    Figure PI2025000852_DRAWING_001
  • Figure PI2025000852_DRAWING_002
    Figure PI2025000852_DRAWING_002
Patent Text Reader

Abstract

Provided is a method of producing iron ore pellets that both suppresses bursting and provides strength to the iron ore pellets. The method of producing iron ore pellets includes a water of crystallization removal process of removing water of crystallization from iron ore having an iron content of 63 mass% or less to obtain dewatered ore. In the water of crystallization removal process, the iron ore heated to a temperature of 100 °C or more and 800 °C or less is held at the temperature for a hold time of 5 min or more and 200 min or less.
Need to check novelty before this filing date? Find Prior Art

Description

Iron ore pellet manufacturing method

[0001] The present invention relates to a method for producing iron ore pellets.

[0002] In the shaft furnace reduction process, which is currently the mainstream of direct reduction ironmaking processes, lump ore or pellets are used as the charging materials. Pellets are produced through the processes of crushing, mixing, granulating, and firing the ore. In this production process, iron ore pellets before firing (so-called green pellets) must be strong enough to prevent crumbling and powdering during handling, such as transportation from the granulation process to the firing process.

[0003] To control the strength of green pellets, it is important to control the particle size of the ore powder after crushing, and it is known that the strength of green pellets increases as the proportion of fine powder increases.In addition, it is known that during the firing process, the evaporation of water in the green pellets causes a phenomenon called bursting, in which the green pellets explode or break down into powder, resulting in a decrease in yield.

[0004] For example, Japanese Patent Laid-Open Publication No. 04-099132 (Patent Document 1) discloses a method for producing pellets from iron ore containing a large amount of water of crystallization. In this production method, raw iron ore containing a large amount of water of crystallization is crushed and granulated, followed by drying, dewatering, and preheating processes, and then a firing process is added to produce fired pellets. In this method, at least a portion of the water of crystallization in the raw iron ore is dewatered in advance before crushing a part or all of the raw iron ore. This production method is said to reduce bursting and improve product yield by increasing the crushing strength of the preheated pellets.

[0005] Japanese Patent Application Publication No. 04-099132

[0006] Currently, high-grade ore with little water of crystallization is generally used as the raw ore (iron ore) for pellets. However, as demand for high-grade ore increases, it is predicted that it will become more difficult to secure a stable supply of high-grade ore in the future. Therefore, the use of low-grade ore with an iron content (total Fe content) of 63 mass% or less, produced in Australia, India, etc., is being considered. As the amount of water of crystallization in iron ore pellets (green pellets) increases, they become more prone to bursting, as described above. Therefore, improvements to pellet manufacturing methods that suppress bursting are desired.

[0007] In the pellet production method of Patent Document 1, it is believed that the water of crystallization cannot be appropriately reduced unless the ore is subjected to a dehydration treatment at an appropriate treatment temperature and time. However, the pellet production method of Patent Document 1 does not take such appropriate treatment temperature and time into consideration. Furthermore, excessive dehydration treatment deteriorates the grindability of the ore, making it difficult to control the particle size to an appropriate level in the grinding process, and may make it difficult to ensure the strength of the iron ore pellets. Therefore, it is desired to provide a method for producing iron ore pellets that can achieve both suppression of bursting and strength of the iron ore pellets.

[0008] The present disclosure has been made in view of the above circumstances, and its purpose is to provide a method for producing iron ore pellets that achieves both suppression of bursting and strength of the iron ore pellets.

[0009] To achieve the above object, the method for producing iron ore pellets according to the present disclosure is as follows.

[0010] [1] A method for producing iron ore pellets, comprising a dehydration treatment step of removing water of crystallization from iron ore having an iron content of 63% by mass or less to obtain dehydrated ore, wherein in the dehydration treatment step, the iron ore is heated to 100°C or more and 800°C or less and held in that state for 5 minutes or more and 200 minutes or less.

[0011] The method for producing iron ore pellets according to the present disclosure may further be as follows.

[0012] [2] The method for producing iron ore pellets according to [1], further comprising a crushing step of crushing the dehydrated ore to obtain ore powder, wherein the proportion of particles having a particle diameter of 10 μm or less as determined by sieving is 10% by mass or more and 70% by mass or less.

[0013] [3] The method for producing iron ore pellets according to [2] above, wherein the proportion of the particle diameter of 10 μm or less is 25% by mass or more and 60% by mass or less.

[0014] [4] The method for producing iron ore pellets according to the above [2] or [3], wherein the proportion of the particle diameter of 10 μm or less is 25% by mass or more and 60% by mass or less.

[0015] [5] The method for producing iron ore pellets according to any one of [1] to [4] above, wherein the content of water of crystallization in the iron ore is 3.0 mass% or more.

[0016] According to the method for producing iron ore pellets of the present disclosure, it is possible to provide a method for producing iron ore pellets that achieves both suppression of bursting and strength of the iron ore pellets.

[0017] 1 is a graph showing the relationship between the strength of the green pellet and the proportion of particles with a diameter of 10 μm or less in the ore powder, and the relationship between the passing rate of pellet fragments of the green pellet and the proportion of particles with a diameter of 10 μm or less in the ore powder.

[0018] A method for producing iron ore pellets according to an embodiment of the present disclosure will be described.

[0019] First, an overview of the method for producing iron ore pellets according to this embodiment will be described. The iron ore pellets according to this embodiment are so-called green pellets (pellets before calcination). The method for producing iron ore pellets according to this embodiment includes a dehydration treatment step in which water of crystallization is removed from iron ore having an iron content of 63% by mass or less (so-called low-grade ore) to obtain dehydrated ore. In the following description, iron ore having an iron content of 63% by mass or less will be simply referred to as iron ore.

[0020] In the crystal water removal treatment step, the iron ore is heated to 100° C. or more and 800° C. or less and held in that state for 5 minutes or more and 200 minutes or less.

[0021] The method for producing iron ore pellets may further include a crushing step of crushing the dehydrated ore to obtain ore powder. In the crushing step, the ore powder may be crushed so that the proportion of particles with a particle diameter of 10 μm or less is 10% by mass to 70% by mass.

[0022] According to the method for producing iron ore pellets according to this embodiment, it is possible to suppress bursting while also achieving strength of the iron ore pellets.

[0023] Bursting is a phenomenon in which iron ore pellets (green pellets) explode or break into powder when heated due to evaporation of water in the green pellets.

[0024] The method for producing iron ore pellets according to this embodiment will be described in detail below.

[0025] The method for producing iron ore pellets according to this embodiment may further include a granulation step in which the ore powder is granulated to obtain iron ore pellets (green pellets) in addition to the above-described decrystallization water treatment step and pulverization step. The green pellets may then be fired in a firing step to form fired pellets. In the following description, to distinguish between pellets before and after firing, the iron ore pellets according to this embodiment (pellets before firing) may be referred to as green pellets, and the pellets after firing may be referred to as fired pellets. The green pellets and fired pellets may contain raw materials other than iron ore (e.g., bentonite).

[0026] The type and blend (ore blend) of iron ore used as the raw material for green pellets are not particularly limited. The raw material for green pellets may consist of a single iron ore or may be a mixture of multiple ores in any blend.

[0027] The content of water of crystallization in iron ore (before the water of crystallization removal step) used as a raw material for green pellets is not particularly limited. The content of water of crystallization can be measured as the weight loss (LOI: Loss On Ignition) of the iron ore when the iron ore is held at 1000°C for 30 minutes.

[0028] The water of crystallization removal process is a process for removing water of crystallization from iron ore to obtain dehydrated ore. In the water of crystallization removal process, the iron ore is heated to remove water of crystallization from the iron ore.

[0029] In the dewatering treatment step, the iron ore is heated to a dewatering treatment temperature of 100°C or higher and 800°C or lower and maintained at this temperature. In this dewatering treatment, the holding time for maintaining the iron ore at a temperature within the above temperature range (hereinafter referred to as dewatering time) is 5 minutes or higher and 200 minutes or lower. If the dewatering time is shorter than 5 minutes, the water of crystallization may not be sufficiently removed from the iron ore. Furthermore, if the dewatering time is longer than 200 minutes, the crushability of the iron ore may deteriorate. In these cases, the strength of the green pellets may decrease. Therefore, the dewatering time is set to 5 minutes or higher and 200 minutes or lower.

[0030] The time for removing water of crystallization is preferably 180 minutes or less. When the time for removing water of crystallization is 180 minutes or less, a decrease in strength of the green pellets can be appropriately avoided.

[0031] In the water of crystallization removal process, the water of crystallization removal temperature and time are important factors for removing water of crystallization. If the water of crystallization removal temperature is less than 100°C, water of crystallization cannot be sufficiently removed from the iron ore. If the water of crystallization removal temperature is higher than 800°C, the grindability of the iron ore deteriorates, and the strength of the green pellets is insufficient. Therefore, the water of crystallization removal temperature is set to 100°C or higher and 800°C or lower. If the water of crystallization removal temperature is within this range and the water of crystallization removal time is 5 minutes or higher and 200 minutes or lower as described above, it is possible to suppress bursting and obtain green pellets with sufficient strength.

[0032] The temperature for the crystallization water removal treatment is preferably 200° C. or higher and 500° C. or lower. When the crystallization water removal treatment temperature is in this range, the strength of the green pellets can be sufficiently increased, and bursting can be more effectively suppressed.

[0033] The content of water of crystallization of the dehydrated ore is not particularly limited. The content of water of crystallization of the dehydrated ore can be measured as LOI, similarly to the content of water of crystallization of the iron ore before the water of crystallization removal step. The content of water of crystallization of the dehydrated ore is preferably reduced by 10 mass% or more from the content of water of crystallization of the iron ore before the water of crystallization removal step.

[0034] The crushing step is a step in which the dehydrated ore is crushed to obtain ore powder. In this embodiment, the crushing method of the dehydrated ore in the crushing step and the crushing time required for crushing are not particularly limited. When crushing the dehydrated ore by batch processing, the crushing time is preferably 15 minutes or more and 75 minutes or less.

[0035] The shape of the ore powder is not particularly limited. It is preferable that the particle diameter of the ore powder is, for example, 300 μm or less in proportion of 95 mass % or more.

[0036] The particle size distribution of the ore powder is preferably such that the proportion of particles with a diameter of 10 μm or less is 10% by mass or more and 70% by mass or less. The particle size or particle size distribution of the ore powder is an important factor that affects the strength of the green pellets. The ore powder can be obtained by crushing iron ore. The crushing method of the iron ore is not particularly limited.

[0037] In the particle size distribution of the ore powder, the proportion of fine powder with a particle size of 10 μm or less has a large effect on the strength of the green pellets. If the proportion of fine powder with a particle size of 10 μm or less in the particle size distribution of the ore powder is less than 10 mass%, it may be impossible to obtain green pellets with sufficient strength.

[0038] The reason why bursting may not be suppressed when the proportion of fine powder with a particle diameter of 10 μm or less in the particle size distribution of the ore powder is greater than 70% by mass is unclear. However, the following reason is predicted, for example. That is, when the proportion of fine powder in the particle size distribution of the ore powder is excessive, the structure of the green pellet becomes dense. Therefore, the diffusion paths (flow paths leading from the inside of the green pellet to the outside of the pellet) of the crystallization water desorbed by heating during firing are reduced. This makes it easier for the water vaporized inside the green pellet to increase the pressure inside the green pellet. Therefore, it is thought that bursting may not be suppressed when the proportion of fine powder with a particle diameter of 10 μm or less in the particle size distribution of the ore powder is greater than 70% by mass.

[0039] In the particle size distribution of the ore powder, the proportion of fine powder with a particle size of 10 μm or less is preferably 20% by mass or more and 60% by mass or less, which makes it possible to obtain an appropriate strength of the green pellets while suppressing bursting.

[0040] The granulation process is a process of granulating ore powder to obtain iron ore pellets (green pellets). The granulation method in the granulation process is not limited. In the granulation process, the ore powder may be granulated using, for example, a pelletizer. As the pelletizer, for example, a pan-type granulator (so-called pan pelletizer) may be used.

[0041] In this embodiment, the shape and size (e.g., particle size and average particle size) of the iron ore pellets are not particularly limited and may be any value. The size of the green pellets may be evaluated by measuring the major axis diameter and minor axis diameter using a vernier caliper, and averaging the measured diameters to determine the particle size of the green pellets. The particle size of the green pellets is preferably 9 mm to 16 mm, which is commonly used in this technical field.

[0042] The green pellets are then fired in a firing process to form fired pellets. The firing temperature in the firing process is, for example, 1200°C to 1350°C.

[0043] In the method for producing iron ore pellets according to this embodiment, when the decrystallization water treatment temperature and decrystallization water time are within the above-mentioned ranges, the green pellets have a strength generally required in this technical field (e.g., 1.0 kg / pellet or more). The strength of the green pellets is preferably 1.0 kg / pellet or more. Furthermore, in the method for producing iron ore pellets according to this embodiment, when the particle size distribution of the raw ore powder is a predetermined distribution, i.e., when the proportion of particle diameters of 10 μm or less is 10% by mass or more and 70% by mass or less, the strength of the green pellets tends to be higher. The strength of the green pellets can be measured by the method described in the Examples below.

[0044] In the method for producing iron ore pellets according to the present embodiment, bursting can be suppressed if the temperature and time for removing the water of crystallization are within the above-described ranges. In the method for producing iron ore pellets according to the present embodiment, bursting can be suppressed even more effectively if the particle size distribution of the ore powder used as the raw material is the above-described predetermined distribution.

[0045] As described above, bursting refers to the phenomenon in which green pellets explode or pulverize due to evaporation of moisture in the green pellets when heated. The likelihood of bursting, i.e., bursting property, can be evaluated, for example, based on the percentage of pellets of 5 mm or less generated after heat treatment of the green pellets at a predetermined temperature (e.g., 300°C) or after firing of the green pellets. More specifically, if bursting occurs during the firing process or when heat treatment of the green pellets at a predetermined temperature (hereinafter referred to as the firing process, etc.), the green pellets explode or pulverize, generating fine pellet fragments (e.g., 5 mm or less). Therefore, if the amount of pellet fragments generated during the firing process, etc. is large, bursting is likely to occur (high bursting property), and the result can be evaluated as being unsatisfactory from the perspective of bursting suppression. Conversely, if the amount of pellet fragments generated during the firing process, etc. is small, bursting is unlikely to occur (low bursting property), and the result can be evaluated as being good from the perspective of bursting suppression.

[0046] If the amount of pellet fragments generated in the firing process etc. is 3.0 mass % or less, preferably 1.5 mass % or less, and more preferably 1.0 mass % or less, a decrease in the yield of fired pellets can be suppressed. Therefore, if the amount of pellet fragments generated in the firing process etc. is 1.0 mass % or less, the green pellets can be evaluated as being of good quality with suppressed bursting.

[0047] Green pellets were produced according to the following procedure, and the bursting properties were evaluated.

[0048] Ores (Ore A, Ore B) having the chemical compositions shown in Table 1 were used as the iron ore (raw ore) used as the raw material for the green pellets. As described above, "LOI" in Table 1 indicates the content (mass%) of water of crystallization. Furthermore, in Table 1, "T.Fe" indicates the mass% of the iron content (total Fe content) in the iron ore. Furthermore, "T.Fe" is a value determined based on the total iron determination method for iron ore specified in JIS M 8212:2022. As shown in Table 1, both Ore A and Ore B used as raw materials for the green pellets are iron ores with a T.Fe content of 63 mass% or less (so-called low-grade ores).

[0049]

[0050] Table 2 shows information on the ores used for the green pellets (ore properties), as well as the conditions and evaluation results for the decrystallization water treatment step, pulverization step, granulation step, and firing step. Green pellets of Experiments No. 1 to 16 were obtained using the ore blends shown in Table 2 and through the decrystallization water treatment step, pulverization step, granulation step, and firing step described below.

[0051]

[0052] Each raw ore was blended in the ore blending ratio shown in Table 2, and dehydrated ore was obtained by dehydration treatment at the temperature and time shown in Table 2 (dehydration step). The dehydration treatment was carried out in the atmosphere. Table 2 shows the LOI of the dehydrated ore as the content of water of crystallization in the dehydrated ore.

[0053] Next, the dehydrated ore was pulverized (batch processing) in a ball mill for the pulverization time shown in Table 2 to obtain ore powder (pulverization step). The proportion of fine powder with a particle size of 10 μm or less in the ore powder was then measured as the percentage (mass %) that passed through a 10 μm mesh sieve. In Table 2, the proportion of fine powder with a particle size of 10 μm or less in the ore powder is shown as the "-10 μm proportion" in the pulverization step.

[0054] Table 3 shows the particle size distribution of the ore powder, including the cumulative 10% diameter (D10), cumulative 50% diameter (D50: median diameter), and cumulative 90% diameter (D90) on a volume basis. These cumulative 10% diameter, cumulative 50% diameter, and cumulative 90% diameter were derived based on the volume-based particle size distribution of the ore powder measured using a laser diffraction particle size measurement (Malvern, Mastersizer 3000). The dispersion medium used in measuring the particle size distribution was water. For ease of reference, Table 3 also lists the "-10 μm ratio" as shown in Table 2.

[0055]

[0056] Next, 1.0% by mass of bentonite was added to the ore powder to obtain a mixed powder. Although bentonite was added as a binder during granulation, it is not essential in this embodiment. This mixed powder was granulated in a pan-type granulator (pelletizer) to obtain green pellets (granulation process). During granulation, the mixed powder was tumbled while adding water so that the granulation moisture (amount of water added) was 10% to 10.5% by mass of the weight of the green pellets. The granulation moisture can be determined by measuring the weight change before and after holding the green pellets at 105°C for 24 hours. For example, if the weight change rate of the green pellets after holding them at 105°C for 24 hours is minus 10% by mass, the granulation moisture is 10%.

[0057] The particle size of the green pellets was determined by measuring the major axis diameter and minor axis diameter using a vernier caliper and taking the average value (arithmetic mean) of the measurements. For each green pellet of each experiment number, the particle sizes of 10 pellets were measured and the average value (arithmetic mean) of the measurements was used as the particle size of the green pellets of that experiment number.

[0058] The strength of the green pellets was measured using an autograph. The strength of the green pellets was measured by deforming the green pellets at a displacement rate of 1 mm / min to obtain a load-displacement curve. The load corresponding to the first displacement peak position in the load-displacement curve was used as the strength of the green pellets. For each green pellet of each experiment number, the strength of 10 pellets was measured, and the average value (arithmetic mean) of these values ​​was used as the strength of the green pellet of that experiment number.

[0059] The bursting property was evaluated based on the amount of pellet fragments generated after the firing process. Specifically, the bursting property was evaluated as follows. First, 500 g of green pellets were charged into a vertical furnace (cylindrical shape with a diameter of 60 mm), and 300°C air was passed from below the green pellet layer upward at a wind speed of 1.0 m / sec (converted to 300°C / 1 atmosphere) for 10 minutes. Next, the green pellets exposed to the 300°C air were heated to 1250°C in an electric furnace separate from the above furnace and fired at this temperature for 25 minutes (firing process). Thereafter, the green pellets were removed from the furnace and sieved through a 5 mm sieve, and the passing fraction (mass%) of pellet fragments that passed through the sieve was measured to evaluate the bursting property. In Table 2, the passing fraction of pellet fragments is indicated as "-5 mm fraction."

[0060] As shown in Table 2, the green pellets of Experiments 1 to 5, 8 to 14, 17, and 18, in which the crystallization water removal temperature was 100°C or higher and 800°C or lower and the crystallization water removal time was 5 minutes or higher and 200 minutes or lower, had a strength of 1.0 kg / pellet or higher. Furthermore, the green pellets of these Experiments had a passing pellet fragment rate (-5 mm rate), which is an index of bursting properties, of 3.0 mass% or lower, specifically 1.5 mass% or lower. That is, the green pellets of these Experiments according to this embodiment achieved both high green pellet strength and high bursting properties.

[0061] In the green pellet manufacturing processes of Experiments 1 to 5, 8 to 14, 17, and 18, the content of water of crystallization in the dehydrated ore (LOI of the dehydrated ore) was reduced by 14% by mass or more in the dehydrated water treatment step from the content of water of crystallization in the iron ore (raw ore) before the dehydrated water treatment step (LOI of the raw ore). Compared with Experiments 6 and 15, which did not achieve both strength and bursting properties in the green pellets, it is considered preferable that the content of water of crystallization in the dehydrated ore be reduced by 10% by mass or more from the content of water of crystallization in the iron ore before the dehydrated water treatment step.

[0062] As shown by the green pellets of Experiments 1 to 5, 8 to 14, 17, and 18, even if the iron ore had a crystallization water content of 4.9% by mass or more before the crystallization water removal process, both strength and bursting properties of the green pellets could be achieved. Therefore, even if the iron ore had a crystallization water content of less than 4.9% by mass, for example, 3.0% by mass or more before the crystallization water removal process, it is considered that both strength and bursting properties of the green pellets can be achieved as long as the crystallization water removal temperature is 100°C or higher and 800°C or lower, and the crystallization water removal time is 5 minutes or higher and 200 minutes or lower. Note that the high-grade ores used in conventional direct reduction ironmaking processes often have a crystallization water content of around 1.0% by mass or less. Furthermore, iron ore pellets for blast furnaces typically contain at most just under 3.0% by mass of crystallization water.

[0063] Furthermore, among the green pellets of Experiments 1 to 5, 8 to 14, 17, and 18, the green pellets of Experiments 1 to 5, 10 to 14, 17, and 18, in which the proportion of particles with a diameter of 10 μm or less (-10 μm proportion) in the ore powder was 10% by mass or more and 70% by mass or less, had a particularly good pellet fragment passing proportion (-5 mm proportion), which is an indicator of bursting properties, of 1.0% by mass or less. Furthermore, the green pellets of Experiments 8 and 9, in which the proportion of particles with a diameter of 10 μm or less (-10 μm proportion) in the ore powder was not 10% by mass or more and 70% by mass or less, were also superior in terms of the strength of the green pellets.

[0064] Furthermore, when comparing the green pellets of Experiments Nos. 1 to 5, 10 to 14, 17, and 18 with the green pellets of Experiments Nos. 8 and 9, it can be seen that the strength of the green pellets tends to be high when D90 is 50 μm or more and 200 μm or less.

[0065] In addition, the green pellets of Experiments 6 and 7, in which the crystallization water removal temperature was from 100°C to 800°C, and Experiments 15 and 16, in which the crystallization water removal time was from 5 minutes to 200 minutes, had a strength of less than 1.0 kg / pellet or a passing rate of pellet fragments (-5 mm rate) of more than 1.0 mass%. In other words, the green pellets of Experiments 6, 7, 15, and 16 did not achieve both strength and bursting properties.

[0066] Figure 1 shows the relationship between the strength of the green pellets and the proportion of particles with a diameter of 10 μm or less (-10 μm proportion) in the ore powder for Experiments Nos. 1 to 5, 8 to 14, 17, and 18. Figure 2 shows the relationship between the passing fraction of pellet fragments (-5 mm fraction) of the green pellets and the proportion of particles with a diameter of 10 μm or less (-10 μm proportion) in the ore powder for Experiments Nos. 1 to 5, 8 to 14, 17, and 18.

[0067] The graph in Figure 1 shows that when the proportion of particles with a diameter of 10 μm or less (-10 μm proportion) in the ore powder is 10% by mass or more and 70% by mass or less, the strength of the green pellets is 1.0 kg / pellet or more. In particular, when the proportion of particles with a diameter of 10 μm or less in the ore powder is 25% by mass or more and 60% by mass or less, the strength of the green pellets is particularly high. As shown by the solid line in Figure 1, the strength of the green pellets generally becomes convex upward as the proportion of particles with a diameter of 10 μm or less in the ore powder increases from a smaller side to a larger side.

[0068] According to the graph shown in Figure 2, when the proportion of particles of 10 μm or less in the ore powder (-10 μm proportion) is 10% by mass or more and 70% by mass or less, the passing proportion of pellet fragments (-5 mm proportion) is 1% by mass or less. As shown by the dashed line in Figure 2, as the proportion of particles of 10 μm or less in the ore powder moves from the small side to the large side, the passing proportion of pellet fragments generally becomes convex downward.

[0069] Comparing the graphs in Figures 1 and 2, it can be said that, overall, when the proportion of particles with a diameter of 10 μm or less (-10 μm proportion) in the ore powder is 25 mass% or more and 60 mass% or less, the strength of the pellet is particularly high, and the passing proportion of pellet fragments is stably low, and bursting is well suppressed, which is particularly preferable.

[0070] In this way, a method for producing iron ore pellets can be provided.

[0071] It should be noted that the embodiments disclosed in this specification are merely examples, and the embodiments of the present disclosure are not limited to these, and can be modified as appropriate within the scope of the purpose of the present disclosure.

[0072] The present disclosure is applicable to methods for producing iron ore pellets.

Claims

1. A method for producing iron ore pellets, comprising a dehydration treatment step of removing water of crystallization from iron ore having an iron content of 63% by mass or less to obtain dehydrated ore, wherein in the dehydration treatment step, the iron ore is heated to 100°C or higher and 800°C or lower and held at this temperature for 5 minutes or higher and 200 minutes or lower.

2. The method for producing iron ore pellets according to claim 1, further comprising a crushing step of crushing the dehydrated ore to obtain ore powder, wherein the proportion of particles having a particle diameter of 10 μm or less as determined by sieving is 10% by mass or more and 70% by mass or less.

3. A method for producing iron ore pellets according to claim 2, wherein the proportion of particles with a diameter of 10 μm or less is 25% by mass or more and 60% by mass or less.

4. A method for producing iron ore pellets according to claim 2 or 3, wherein the ore powder has a cumulative 90% diameter in a volumetric particle size distribution of 50 μm or more and 200 μm or less.