AI Technical Summary

Technical Problem

Existing methods for imparting antiviral properties to metal surfaces, such as those using photocatalysts, are labor-intensive and costly due to the need for periodic application of antiviral drugs, and there is a need for improved durability and effectiveness.

Method used

A painted metal plate with a zinc-containing metal layer and a photocatalyst layer that allows for the controlled elution of zinc ions, enhancing antiviral properties by forming a photocatalyst layer with specific thickness and composition, including elements like Si, Zr, Cu, Fe, and Ag, to improve antiviral function and durability.

Benefits of technology

The solution results in a coated metal plate with improved antiviral properties, reduced labor and maintenance costs, and enhanced durability by facilitating the controlled release of zinc ions, effectively inhibiting viruses and maintaining corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025000860_DRAWING_001
    Figure PI2025000860_DRAWING_001
  • Figure PI2025000860_DRAWING_002
    Figure PI2025000860_DRAWING_002
  • Figure PI2025000860_DRAWING_003
    Figure PI2025000860_DRAWING_003
Patent Text Reader

Abstract

[Name of Document] Abstract PAINTED METAL PLATE To provide a painted metal plate which can be more simply manufactured, can improve the antiviral function, and has durability. The present invention relates to a painted metal plate including a metal plate and a coating layer located on at least one surface of the metal plate, wherein: the metal plate is a metal plate having a zinc-containing metal layer containing at least zinc on the at least one surface; as the coating layer, is provided a first coating layer which is located at an outermost surface of the painted metal plate and contains at least a compound having photocatalytic activity; an average thickness of the first coating layer is 0.05 to 5.00 μm; a total thickness from a surface of the zinc-containing metal layer to an outermost surface of the first coating layer is 15.00 μm or less; and when an antiviral test defined by JIS R1756: 2020 is carried out for 4 hours, a zinc ion concentration eluted into a virus-containing liquid is 0.60 to 5.00 mass%. FIG. 1
Need to check novelty before this filing date? Find Prior Art

Description

painted metal plate

[0001] The present invention relates to a coated metal sheet.

[0002] Due to the impact of the novel coronavirus (COVID-19) over the past few years, there has been a growing need to impart antiviral properties to various items, and businesses that apply antiviral agents to the surfaces of various items have become popular. The application of antiviral agents can be applied to existing structures. However, applying antiviral agents poses problems such as high labor costs and the need for periodic application due to the agents' insufficient durability, resulting in high running costs.

[0003] Meanwhile, there is a known technique for imparting antiviral properties to steel materials in advance, as described in Patent Document 1. This technique uses a coated steel material as a base and forms a protective layer and a photocatalytic layer in this order on top of the coated steel material.

[0004] JP 2009-131960 A

[0005] However, as a result of investigations by the present inventors, it has been found that there is room for further improvement in the antiviral function of the technology using a photocatalyst as disclosed in Patent Document 1.

[0006] Based on this finding, an object of the present invention is to provide a coated metal sheet that can be produced more simply, has improved antiviral function, and is durable.

[0007] In order to solve the above problems, the present inventors conducted extensive research and experimentally found that when a metal plate having a zinc-containing metal layer and further forming a photocatalytic layer thereon was subjected to an antiviral test specified in JIS R1756:2020, the metal plate exhibited better antiviral properties the more easily zinc was eluted into a virus-containing liquid. Based on this finding, the present inventors conducted further research and found that the antiviral function of a coated metal plate could be further improved by creating conditions that facilitate zinc elution, leading to the completion of the present invention. The gist of the present invention, which was completed based on this finding, is as follows.

[0008] (1) A coated metal sheet comprising a metal sheet and a coating layer located on at least one surface of the metal sheet, wherein the metal sheet has a zinc-containing metal layer containing at least zinc on at least one surface, and the coating layer includes a first coating layer located on the outermost surface of the coated metal sheet and containing at least a compound having photocatalytic activity, the first coating layer having an average thickness of 0.05 to 5.00 μm, a total thickness from the surface of the zinc-containing metal layer to the outermost surface of the first coating layer being 15.0 μm or less, and a zinc ion concentration eluted into a virus-containing liquid when an antiviral test specified in JIS R1756:2020 is performed for 4 hours. (2) The coated metal sheet according to (1), wherein the thickness of the first coating layer is 0.05 to 0.95 μm, and a total thickness from the surface of the zinc-containing metal layer to the outermost surface of the first coating layer is less than 1.0 μm. (3) The coated metal sheet according to (1) or (2), wherein the total content of elements having a potential more noble than zinc in the coating layer is 0 to 20.0 mass %. (4) The coated metal sheet according to (1), wherein the first coating layer further contains at least one element selected from the group consisting of Zn, Cu, Fe, Ni, and Ag. (5) The coated metal sheet according to (1), wherein the first coating layer further contains at least one element of Si or Zr, and the total content of the elements is 5 to 50 mass % for Si, calculated as silica, and for Zr, calculated as zirconia. (6) A coated metal sheet having a metal sheet and a coating layer located on at least one surface of the metal sheet, the coating layer comprising a first coating layer located on the outermost surface of the coated metal sheet and containing a compound having photocatalytic activity and 0.2 to 20.0 mass% zinc elemental, calculated as metallic Zn, the average thickness of the first coating layer being 0.05 to 5.00 μm, the total thickness from the surface of the metal sheet to the outermost surface of the first coating layer being 60.0 μm or less, and the zinc ion concentration eluted into a virus-containing liquid when an antiviral test specified in JIS R1756:2020 is performed for 4 hours is 0.60 to 5.00 mass%. (7) The coated metal sheet according to (6), wherein the total content of elements having a more noble potential than zinc in the coating layer is 0 to 20.0 mass%.(8) The coated metal sheet according to (6) or (7), wherein the first coating layer further contains at least one element selected from the group consisting of Cu, Fe, Ni, and Ag. (9) The coated metal sheet according to (6), wherein the first coating layer further contains at least one element of Si or Zr, and the total content of the elements is 5 to 50 mass% in terms of silica for Si and zirconia for Zr. (10) The coated metal sheet according to (1) or (6), wherein the coating layer further includes a second coating layer located below the first coating layer and made of an inorganic component, the second coating layer containing at least one element of Si or Zr as the inorganic component, and the average thickness of the second coating layer is 0.05 to 5.00 μm. (11) The coated metal sheet according to (10), wherein the second coating layer further contains at least one of P and V as the inorganic component. (12) The coated metal sheet according to (10), wherein the second coating layer further contains at least one element selected from the group consisting of Zn, Cu, Fe, Ni, and Ag. (13) The coated metal sheet according to (10), wherein the coating layer further includes a third coating layer located below the second coating layer and containing a resin component, the third coating layer having an average thickness of 0.50 to 14.00 μm. (14) The coated metal sheet according to (13), wherein the third coating layer further contains a colorant. (15) The coated metal sheet according to (1) or (6), wherein the compound having photocatalytic activity is anatase-type titanium oxide. (16) The coated metal sheet according to (15), wherein the compound having photocatalytic activity is metal-supported titanium oxide in which at least one of Cu and Fe is supported on titanium oxide. (17) The coated metal sheet according to (1), wherein the metal sheet is a zinc-based plated steel sheet having a zinc-based plating layer as the zinc-containing metal layer. (18) The coated metal sheet according to (17), wherein the zinc-based plating layer is a plating layer containing 30% by mass or more of Zn, calculated as metallic Zn. (19) The coated metal sheet according to (17), wherein the zinc-based plating layer is any one of a zinc plating layer, a zinc-aluminum alloy plating layer, a zinc-aluminum-magnesium alloy plating layer, a zinc-nickel alloy plating layer, and a zinc-iron alloy plating layer.(20) The coated metal sheet according to (1) or (6), wherein the surface of the metal sheet has a hairline along the rolling direction of the metal sheet. (21) The coated metal sheet according to (1), wherein the surface of the zinc-containing metal layer has a spangle pattern.

[0009] As described above, according to the present invention, it is possible to provide a coated metal sheet that can be produced more easily, has durability, and has improved antiviral function.

[0010] FIG. 1 is an explanatory diagram schematically showing an example of the structure of a coated metal plate according to a first embodiment of the present invention. FIG. 2 is an explanatory diagram schematically showing another example of the structure of a coated metal plate according to a first embodiment of the present invention. FIG. 3 is an explanatory diagram schematically showing another example of the structure of a coated metal plate according to a first embodiment of the present invention. FIG. 4 is an explanatory diagram schematically showing another example of the structure of a coated metal plate according to a first embodiment of the present invention. FIG. 5 is an explanatory diagram schematically showing another example of the structure of a coated metal plate according to a second embodiment of the present invention. FIG. 6 is an explanatory diagram schematically showing another example of the structure of a coated metal plate according to a second embodiment of the present invention. FIG. 7 is an explanatory diagram schematically showing another example of the structure of a coated metal plate according to a second embodiment of the present invention.

[0011] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In this specification and drawings, components having substantially the same functional configurations are designated by the same reference numerals, and redundant explanations will be omitted.

[0012] First Embodiment Hereinafter, a coated metal sheet according to a first embodiment of the present invention will be described in detail. The first embodiment of the present invention relates to a coated metal sheet having a metal sheet and a coating layer located on at least one surface of the metal sheet, wherein the metal sheet has a zinc-containing metal layer containing at least zinc on at least one surface.

[0013] (Regarding Coated Metal Sheet) <Structure of Coated Metal Sheet> First, the structure of a coated metal sheet according to a first embodiment of the present invention will be described below with reference to Fig. 1. Fig. 1 is an explanatory diagram that schematically shows an example of the structure of a coated metal sheet according to this embodiment.

[0014] As shown schematically in FIG. 1 , a coated metal sheet 1 according to a first embodiment of the present invention has a coating layer on at least one surface of the metal sheet, and includes at least a metal sheet 10 and, as the coating layer, a photocatalytic layer 20 as an example of a first coating layer.

[0015] [Regarding the metal plate 10] In the coated metal plate 1 according to this embodiment, the metal plate 10 has a base metal 11 as the base material of the metal plate 10, and a zinc-containing metal layer 13 which is a metal layer containing at least zinc.

[0016] Here, various metal plates can be used as the base metal 11. Examples of such metal plates include various steel plates, aluminum plates, stainless steel plates, etc., and the type may be selected depending on the strength, properties, etc. required for the base metal 11.

[0017] Furthermore, the zinc-containing metal layer 13 is a metal layer provided on the surface of the base metal 11 and contains at least zinc. The presence of such a zinc-containing metal layer 13 on the surface of the base metal 11 causes zinc to dissolve into a virus-containing liquid in an antiviral test specified in JIS R1756:2020, as discovered by the present inventors. As a result, it is possible to further improve the antiviral function of the coated metal sheet 1 for a longer period of time by a simpler method.

[0018] More specifically, the zinc-containing metal layer 13 preferably contains 30% by mass or more of zinc in terms of metallic Zn. The zinc-containing metal layer 13 may also contain impurities. By ensuring a zinc content of 30% by mass or more in the zinc-containing metal layer 13, it is possible to further increase the amount of zinc eluted into the virus-containing liquid as described above while ensuring the corrosion resistance of the base metal 11. This makes it possible to further improve the antiviral function of the coated metal sheet 1. The zinc content of the zinc-containing metal layer 13 is more preferably 40% by mass or more, and even more preferably 70% by mass or more. The higher the zinc content of the zinc-containing metal layer 13, the better, and the zinc content of the zinc-containing metal layer 13 may be 100% by mass.

[0019] Examples of such a zinc-containing metal layer 13 include a zinc vapor deposition layer on which metallic zinc or the like is vapor-deposited, and a zinc-based plating layer which is a plating layer containing zinc. Here, it is preferable to provide a zinc-based plating layer as the zinc-containing metal layer 13, from the viewpoint that the zinc-based plating layer can be easily produced at low production costs by using various existing zinc-based plating layer production lines, etc.

[0020] A preferred zinc-based plating layer as the zinc-containing metal layer 13 is a zinc-based plating layer containing 30% by mass or more of zinc in terms of metallic Zn. Furthermore, such a zinc-based plating layer may contain impurities. By ensuring the corrosion resistance of the base metal 11 while increasing the amount of zinc eluted into the virus-containing liquid, the antiviral function of the coated metal sheet 1 can be further improved. The zinc content of the zinc-based plating layer is more preferably 40% by mass or more, and even more preferably 70% by mass or more. The zinc content of the zinc-based plating layer may be 100% by mass.

[0021] Examples of such a zinc-based plating layer include various plating layers such as a zinc plating layer, a zinc-aluminum alloy plating layer, a zinc-aluminum-magnesium alloy plating layer, a zinc-nickel alloy plating layer, a zinc-iron alloy plating layer, etc. From the viewpoint of further increasing the amount of zinc eluted, it is more preferable to provide a zinc-nickel alloy plating layer or a zinc-iron alloy plating layer as the zinc-based plating layer.

[0022] In particular, element Fe is an element that promotes the elution of zinc from the viewpoint of ionization tendency, and the coexistence of metallic Fe and zinc is advantageous in terms of potential from the viewpoint of zinc elution, and is therefore preferred.

[0023] The amount of the zinc-containing metal layer 13 deposited on one side of the base metal 11 is 8 g / m2 in terms of metal Zn. 2 It is preferable that the content is 17 g / m or more. 2 It is more preferable that the coating amount is 8 g / m or more. 2 More preferably, 17 g / m 2 By setting the thickness to the above, it is possible to dissolve a sufficient amount of zinc while ensuring the corrosion resistance of the base metal 11. On the other hand, the amount of the zinc-containing metal layer 13 deposited on one side of the base metal 11 is 250 g / m in terms of metallic Zn. 2 Preferably, the weight is 170 g / m or less. 2 It is more preferable that the coating amount is 250 g / m or less. 2 or less, more preferably 170 g / m 2 By setting the above, it is possible to dissolve a sufficient amount of zinc while ensuring the corrosion resistance of the base metal 11.

[0024] In view of the above, it is more convenient to use various zinc-based plated steel sheets having various zinc-based plating layers as described above as the metal sheet 10 having the zinc-containing metal layer 13 .

[0025] Here, the thickness of the metal plate 10 as described above is not particularly limited, and may be set appropriately depending on the mechanical strength (e.g., tensile strength, etc.) and processability required for the painted metal plate 1 of this embodiment.

[0026] Moreover, various patterns such as a hairline pattern or a spangle pattern may be present on the surface of the zinc-containing metal layer 13 along the rolling direction of the base metal 11. By providing such patterns, it is possible to further improve the design of the coated metal sheet 1.

[0027] In particular, the hairline pattern is a pattern realized by forming fine irregularities on the surface of the zinc-containing metal layer 13, and therefore increases the surface area of ​​the zinc-containing metal layer 13. As a result, it is possible to further increase the amount of zinc eluted from the zinc-containing metal layer 13, which is more preferable not only from the viewpoint of design but also from the viewpoint of antiviral properties.

[0028] Although FIG. 1 illustrates a form in which the zinc-containing metal layer 13 is formed on one surface of the base metal 11, the zinc-containing metal layer 13 may be formed on both surfaces of the base metal 11.

[0029] [Regarding the Photocatalytic Layer 20] In the coated metal sheet 1 according to this embodiment, the photocatalytic layer 20, which serves as an example of a first coating layer, is a layer located on the outermost surface of at least one surface of the metal sheet 10, as shown schematically in FIG. 1 , and contains at least a compound having photocatalytic activity (hereinafter, sometimes abbreviated as "photocatalytic compound"). When the photocatalytic layer 20 contains a compound having photocatalytic activity, the compound causes a photocatalytic reaction in response to light (particularly light in the ultraviolet to visible light range) incident on the photocatalytic layer 20. As a result, the photocatalytic layer 20 according to this embodiment exhibits various photocatalytic effects, including antiviral and bactericidal effects. This allows the coated metal sheet 1 according to this embodiment to achieve various properties, including antiviral and bactericidal effects.

[0030] Compounds having such photocatalytic activity include compounds that react mainly with light in the ultraviolet light range (more specifically, when excited by light in the ultraviolet light range) to exhibit photocatalytic activity, and compounds that react mainly with light in the visible light range (more specifically, when excited by light in the visible light range) to exhibit photocatalytic activity.

[0031] Examples of compounds that react with light in the ultraviolet range to exhibit photocatalytic activity include metal oxides such as titanium oxide (more specifically, anatase titanium oxide), zinc oxide, cerium oxide, tin oxide, bismuth oxide, zirconium oxide, tungsten oxide, chromium oxide, molybdenum oxide, iron oxide, nickel oxide, ruthenium oxide, cobalt oxide, copper oxide, manganese oxide, germanium oxide, lead oxide, cadmium oxide, vanadium oxide, niobium oxide, tantalum oxide, rhodium oxide, and rhenium oxide, metal sulfides such as cadmium sulfide and zinc sulfide, and titanium compounds such as strontium titanate and barium titanate. Among these, anatase titanium oxide, zinc oxide, tin oxide, zirconium oxide, tungsten oxide, iron oxide, niobium oxide, and strontium titanate are particularly preferred as compounds that react with light in the ultraviolet range to exhibit photocatalytic activity, with anatase titanium oxide being even more preferred.

[0032] Furthermore, examples of compounds that react with light in the visible light range to exhibit photocatalytic activity include metal-supported titanium oxide (more specifically, anatase-type titanium oxide) in which at least one metal of Cu or Fe is supported on titanium oxide; anatase-type titanium oxide in which Cr, V, Mn, Ni, or Pt is supported on anatase-type titanium oxide; anatase-type titanium oxide doped with anions such as nitrogen or sulfur; and AgNbO. 3 and SrTiO 3 Among these, anatase type titanium oxide in which at least one metal of Cu or Fe is supported on anatase type titanium oxide is more preferably used.

[0033] In particular, anatase-type titanium oxide carrying Cu is particularly suitable because the attached Cu has the effect of promoting the elution of zinc from the zinc-containing metal layer 13 as described above.

[0034] Among these photocatalytic compounds, the average particle size (primary particle size) of anatase-type titanium oxide (including that in a metal-supported state) is preferably 5 nm or more. By making the average particle size (primary particle size) of anatase-type titanium oxide 5 nm or more, it becomes possible to more uniformly disperse anatase-type titanium oxide in the photocatalytic layer 20. The average particle size (primary particle size) of anatase-type titanium oxide is more preferably 20 nm or more. Furthermore, the average particle size (primary particle size) of anatase-type titanium oxide (including that in a metal-supported state) is preferably 200 nm or less. By making the average particle size (primary particle size) of anatase-type titanium oxide 200 nm or less, it becomes possible to more uniformly disperse anatase-type titanium oxide in the photocatalytic layer 20 while suppressing excessive aggregation of anatase-type titanium oxide in the photocatalytic layer 20. The average particle size (primary particle size) of anatase-type titanium oxide is more preferably 100 nm or less.

[0035] The average particle size of the anatase titanium oxide can be measured, for example, by dynamic light scattering using laser light. This method allows for easy and accurate measurement. However, if the anatase titanium oxide particles are aggregated to a certain extent, it is possible to measure the size of the aggregates (aggregate particle size). Therefore, it is preferable to also directly confirm the primary particle size using a transmission electron microscope (TEM). If the presence of aggregated particles is confirmed as a result of TEM observation, it is preferable to change the dispersion conditions and measure again using dynamic light scattering. Furthermore, if it is difficult to completely disperse the particles to the primary particle level, it is also possible to use the size of the primary particles observed and measured by TEM as the primary particle size. In this case, the inventor's experience has shown that a value representative of the entire particle population can be obtained by measuring approximately 100 or more particles selected at random.

[0036] Furthermore, when measuring the average particle size of anatase-type titanium oxide contained in the photocatalyst layer 20 of a coated metal sheet 1 on which the photocatalyst layer 20 has already been formed, the following procedure can be used. Specifically, a cross section of the photocatalyst layer 20 cut along its thickness direction can be observed or analyzed using a transmission electron microscope (TEM). Using a TEM, the primary particle size of the photocatalyst compound can be measured. Furthermore, performing EDS analysis in combination with the TEM can measure the elements contained in the photocatalyst compound. Furthermore, electron diffraction can determine the crystal structure of the photocatalyst compound (e.g., whether titanium oxide is anatase-type or rutile-type). The inventor's experience has shown that measuring approximately 100 or more randomly selected particles can provide a value representative of the entire particle population.

[0037] Here, the concentration of anatase-type titanium oxide (including that in a metal-supported state) in the photocatalyst layer 20 is preferably 50% by mass or more in titania equivalent. A concentration of anatase-type titanium oxide of 50% by mass or more in the photocatalyst layer 20 makes it possible to reliably exhibit various photocatalytic effects, including antiviral effects. The concentration of anatase-type titanium oxide in the photocatalyst layer 20 is more preferably 60% by mass or more in titania equivalent. Furthermore, the concentration of anatase-type titanium oxide (including that in a metal-supported state) in the photocatalyst layer 20 is preferably 95% by mass or less in titania equivalent. A concentration of anatase-type titanium oxide of 95% by mass or less in the photocatalyst layer 20 makes it possible to exhibit various photocatalytic effects, including antiviral effects, while suppressing increases in manufacturing costs. The concentration of anatase-type titanium oxide in the photocatalyst layer 20 is more preferably 80% by mass or less in titania equivalent.

[0038] Similarly to the above, photocatalytic compounds other than anatase type titanium oxide preferably have an average particle size of 5 to 200 nm, and their concentration is preferably 50 to 95% by mass.

[0039] In addition, the photocatalytic compounds represented by the above-mentioned anatase type titanium oxide and the like can be used, if necessary, not only in particulate form but also in sol-like form that cannot be said to be particulate, and in substances produced by heating metal complexes.

[0040] The photocatalyst layer 20 further contains at least one element of Si or Zr, and the total concentration of such elements is preferably 5% by mass or more in terms of silica for Si and zirconia for Zr. In other words, the photocatalyst layer 20 is an inorganic coating having a skeleton of inorganic components with a three-dimensional network structure containing at least one element of Si or Zr, and possibly impurities, and the total concentration of at least one element of Si or Zr is preferably 5% by mass or more in terms of silica for Si and zirconia for Zr. By containing at least one element of Si or Zr at the above concentrations, it is possible to achieve a photocatalyst layer 20 with better corrosion resistance. The total content of at least one element of Si or Zr is more preferably 10% by mass or more. Here, inorganic components refer to components that do not contain organic resins.

[0041] The photocatalytic layer 20 further contains at least one element selected from the group consisting of Si and Zr, and the total concentration of these elements is preferably 50% by mass or less, calculated as silica for Si and zirconia for Zr. By including at least one element selected from the group consisting of Si and Zr at the above-mentioned concentrations, a photocatalytic layer 20 with superior corrosion resistance can be achieved. The total content of at least one element selected from the group consisting of Si and Zr is more preferably 40% by mass or less. The Si or Zr preferably has excellent light transmittance and is an inorganic component that is less susceptible to decomposition by the photocatalyst. Examples of inorganic components containing Si and Zr include silica and zirconia.

[0042] In addition to the above-described photocatalytic compound and at least one element selected from the group consisting of Si and Zr, the photocatalytic layer 20 preferably further contains at least one element selected from the group consisting of Zn, Cu, Fe, Ni, and Ag. Here, the elements Cu, Fe, Ni, and Ag are elements that promote the elution of zinc from the zinc-containing metal layer 13 described above, so by further containing these elements in the photocatalytic layer 20, more zinc is eluted from the zinc-containing metal layer 13, which is preferable. Furthermore, the elements Cu, Zn, and Ag are particularly preferable because they also exhibit antibacterial effects. Furthermore, by further containing the element Zn in the photocatalytic layer 20, the amount of zinc eluted from the coated metal sheet 1 can be further increased, which is more preferable.

[0043] The total content of at least one element selected from the group consisting of Zn, Cu, Fe, Ni, and Ag in the photocatalytic layer 20 is preferably 0.2 mass% or more, calculated as metal elements. A total content of the metal elements of 0.2 mass% or more makes it possible to more favorably exhibit the above-described effects. The total content of the metal elements is more preferably 0.6 mass% or more, and even more preferably 1.0 mass% or more. On the other hand, the total content of at least one element selected from the group consisting of Zn, Cu, Fe, Ni, and Ag in the photocatalytic layer 20 is preferably 5.0 mass% or less, calculated as metal elements. A total content of the metal elements of 5.0 mass% or less makes it possible to ensure the content of the photocatalytic compound while exhibiting the above-described effects without saturating the effects. The total content of the metal elements is more preferably 3.5 mass% or less, and even more preferably 2.5 mass% or less.

[0044] The photocatalyst layer 20 containing the above-mentioned photocatalyst compound may contain an antibacterial agent or an adsorbent such as activated carbon or zeolite, if necessary, within a range that does not impair the effects of the present invention.

[0045] The average thickness d of the photocatalytic layer 20 1 (In the case of the layer structure shown in FIG. 1, the total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 20 (which can also be regarded as the outermost surface of the coating layer)T The average thickness d of the photocatalytic layer 20 is 0.05 μm or more. 1 If the average thickness d is less than 0.05 μm, it becomes difficult to uniformly form the photocatalytic layer 20 as described above, and the obtained photocatalytic effect becomes uneven, which is not preferable. 1 By making the thickness 0.05 μm or more, it is possible to secure a route for elution of zinc from the zinc-containing metal layer 13, thereby allowing zinc to be sufficiently eluted, and also to make the desired photocatalytic effect appear uniformly throughout the photocatalytic layer 20.

[0046] On the other hand, the average thickness d of the photocatalytic layer 20 1 (In the case of the layer structure shown in FIG. 1, the total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 20 is T The average thickness d of the photocatalytic layer 20 is 5.00 μm or less. 1 If the average thickness d exceeds 5.00 μm, the photocatalytic effect obtained will be saturated, but the manufacturing cost will increase, which is not preferable. Also, it will be difficult to ensure a sufficient amount of zinc eluted from the zinc-containing metal layer 13, which is also not preferable from this point of view. Furthermore, since the photocatalytic layer is an inorganic coating, its processability will be reduced. 1 By making the thickness 5.00 μm or less, it is possible to suppress the deterioration of ease of manufacturing and processability, and also to ensure a route for elution of zinc from the zinc-containing metal layer 13, thereby allowing zinc to be sufficiently eluted, and further to make it possible to uniformly exhibit the desired photocatalytic effect over the entire photocatalytic layer 20.

[0047] Normally, there is a certain probability that light passes through the photocatalytic layer 20 without hitting the photocatalytic compound. Conventionally, such light that does not interact with the photocatalytic compound is light that does not provide a photocatalytic effect. In this embodiment, by reflecting such light on the surface of the metal plate 10, it is possible to increase the probability that light incident on the photocatalytic layer 20 will hit the photocatalytic compound. As a result, in this embodiment, the photocatalytic effect can be further improved. In the case of the layer structure shown in FIG. 1, the total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 20 is Tis naturally 5.00 μm or less, and as a result, the incident light reflected on the surface of the metal plate 10 (in other words, the interface between the metal plate 10 and the photocatalytic layer 20) can be used for the photocatalytic reaction by the photocatalytic compound, thereby further improving the photocatalytic effect.

[0048] The average thickness d of the photocatalytic layer 20 1 is preferably 0.10 μm or more, and more preferably 0.15 μm or more. 1 is preferably 2.00 μm or less, more preferably 1.00 μm or less, even more preferably less than 1.0 μm, and even more preferably 0.80 μm or less, 0.60 μm or less, or 0.50 μm or less.

[0049] Although FIG. 1 illustrates a configuration in which the photocatalytic layer 20 is formed on one surface of the metal plate 10, the photocatalytic layer 20 may be formed on both surfaces of the metal plate 10.

[0050] <Zinc ion concentration eluted into virus-containing liquid in antiviral test> The structure of coated metal sheet 1 as described above is one of the conditions for ensuring that the zinc ion concentration eluted into virus-containing liquid falls within the range of 0.60 to 5.00 mass % when an antiviral test specified in JIS R1756:2020 is carried out for 4 hours.

[0051] The reason why the above-described structure is one of the conditions is that in the coated metal plate 1 according to this embodiment, the zinc-containing metal layer 13 is provided in an appropriate state, and further, the total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 20 is T is within a specific range, an appropriate amount of zinc can be eluted from the zinc-containing metal layer 13. In this way, in the coated metal sheet 1 according to this embodiment, the zinc-containing metal layer 13, which is originally provided to ensure the corrosion resistance of the metal sheet 10, also functions to improve the antiviral properties of the coated metal sheet 1.

[0052] The amount of zinc eluted from the zinc-containing metal layer 13 depends on the amount of zinc attached to the zinc-containing metal layer 13 and the total thickness d TIt is possible to control the amount of zinc eluted from the zinc-containing metal layer 13 to a desired state by adjusting the density of the coating layer present on the path from the zinc-containing metal layer 13 to the outermost surface of the photocatalytic layer 20.

[0053] Here, if the zinc ion concentration in the virus-containing liquid is less than 0.60% by mass, this means that the amount of zinc eluted from the zinc-containing metal layer 13 is insufficient, making it impossible to further improve the antiviral function of the coated metal sheet 1. The zinc ion concentration in the virus-containing liquid is preferably 0.90% by mass or more, and more preferably 1.20% by mass or more.

[0054] On the other hand, if the zinc ion concentration in the virus-containing liquid exceeds 5.00% by mass, the amount of zinc eluted from the zinc-containing metal layer 13 becomes too large, making it impossible to ensure the corrosion resistance of the metal plate 10. The zinc ion concentration in the virus-containing liquid is preferably 4.50% by mass or less, and more preferably 3.50% by mass or less.

[0055] In the coated metal sheet 1 according to this embodiment, the total content of elements (more specifically, ions) having a potential more noble than zinc present in the coating layer is preferably 20.0 mass% or less in terms of metal elements. Examples of elements having a potential more noble than zinc include Cu and Ag. By setting the total content of elements having a potential more noble than zinc in the coating layer to 20.0 mass% or less, the zinc ion concentration in the virus-containing liquid described above can be set to 5.00 mass% or less, thereby achieving both excellent antiviral properties and excellent corrosion resistance. The total content of elements having a potential more noble than zinc in the coating layer is more preferably 15.0 mass% or less, even more preferably 11.0 mass% or less, and even more preferably 7.5 mass% or less. The lower limit of the total content of elements having a potential more noble than zinc in the coating layer is not particularly specified and may be 0 mass%.

[0056] The antiviral test is carried out for 4 hours in accordance with the method specified in JIS R1756: 2020. The concentration of zinc ions dissolved in the virus-containing solution may be measured by inductively coupled plasma (ICP) atomic emission spectrometry.

[0057] <Modification 1> The coated metal sheet 1 according to this embodiment, which has a layer structure as shown in Fig. 1, may have an additional coating layer that functions as a chemical conversion coating layer between the metal sheet 10 and the photocatalytic layer 20. By providing a chemical conversion coating layer between the metal sheet 10 and the photocatalytic layer 20, it is possible to further improve the adhesion between the metal sheet 10 and the photocatalytic layer 20. Furthermore, it is also possible to further improve the corrosion resistance and the like of the coated metal sheet 1 according to this embodiment.

[0058] The additional coating layer that functions as a chemical conversion coating layer will be described in detail below with reference to Figures 2A and 2B, which are explanatory diagrams that schematically show another example of the structure of a coated metal sheet according to this embodiment.

[0059] 2A and 2B are schematic diagrams showing the layer structure of the coated metal sheet 1 when an inorganic coating layer 30 functioning as a chemical conversion coating layer as an example of a second coating layer is provided. In this case, the coated metal sheet 1 according to this embodiment has the inorganic coating layer 30 as an example of a second coating layer between the metal sheet 10 and the photocatalyst layer 20 as described above.

[0060] Photocatalytic compounds, such as anatase titanium oxide, have extremely excellent oxidizing properties, so when a coating layer is formed below the layer containing the photocatalytic compound, a protective layer is often formed to protect the coating layer. However, as explained below, by forming the chemical conversion coating layer from inorganic components, it becomes possible to arrange the chemical conversion coating layer without providing a protective layer. Here, inorganic components mean components that do not contain organic resins.

[0061] The inorganic coating layer 30 is formed by chemical conversion treatment after removing impurities such as oil and surface oxides adhering to the surface of the metal plate 10 by known degreasing and cleaning processes. The inorganic coating layer 30 is preferably made of an inorganic component such as a silane compound or a zirconia compound containing at least one element of Si or Zr. The inorganic coating layer 30 may further contain an inorganic component containing at least one element of P or V.

[0062] The inorganic coating layer 30 contains inorganic components having the elements described above, which improves the film-forming properties after application of the chemical conversion treatment solution, the barrier properties (density) of the coating against corrosion factors such as moisture and corrosive ions, and the adhesion of the coating to the metal sheet surface, thereby contributing to improving the corrosion resistance of the coating.

[0063] Examples of inorganic components containing Si include γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, etc. Examples of inorganic components containing Zr include zirconium carbonate, ammonium zirconium carbonate, potassium zirconium carbonate, sodium zirconium carbonate, ammonium zirconium carbonate, etc.

[0064] Examples of inorganic components containing P include phosphoric acids such as phosphoric acid, orthophosphoric acid, metaphosphoric acid, pyrophosphoric acid, triphosphoric acid, and tetraphosphoric acid, and salts thereof, ammonium dihydrogen phosphate, etc. Examples of inorganic components containing V include ammonium metavanadate (V), potassium metavanadate (V), sodium metavanadate (V), vanadyl sulfate (IV), etc.

[0065] The inorganic coating layer 30 according to this embodiment may contain the above-described various inorganic components either singly or in combination. The content of the above-described various inorganic components may also be adjusted as appropriate.

[0066] The average thickness d of the inorganic coating layer 302 is preferably 0.05 μm or more, and more preferably 0.10 μm or more. This allows the inorganic coating layer 30 to be uniformly formed on the surface of the metal sheet 10, while stably achieving the various effects achieved by providing the chemical conversion coating layer as described above. In addition, the average thickness d of the inorganic coating layer 30 2 is preferably 5.00 μm or less, more preferably 1.00 μm or less, even more preferably less than 1.00 μm, and even more preferably 0.80 μm or less, 0.60 μm or less, or 0.50 μm or less. This allows the inorganic coating layer 30 to be formed uniformly on the surface of the metal sheet 10, while stably achieving the various effects achieved by providing the chemical conversion coating layer as described above.

[0067] Similarly to the photocatalytic layer 20, the inorganic coating layer 30 according to this embodiment preferably further contains at least one element selected from the group consisting of Zn, Cu, Fe, Ni, and Ag.

[0068] The total content of at least one element selected from the group consisting of Zn, Cu, Fe, Ni, and Ag in the inorganic coating layer 30 is preferably 0.2 mass% or more, calculated as metal elements. A total content of the metal elements of 0.2 mass% or more makes it possible to more favorably exhibit the above-described effects. The total content of the metal elements is more preferably 0.6 mass% or more, and even more preferably 1.0 mass% or more. On the other hand, the total content of at least one element selected from the group consisting of Zn, Cu, Fe, Ni, and Ag in the inorganic coating layer 30 is preferably 10.0 mass% or less, calculated as metal elements. A total content of the metal elements of 10.0 mass% or less makes it possible to ensure the content of the photocatalytic compound while exhibiting the above-described effects without saturating the effects. The total content of the metal elements is more preferably 7.5 mass% or less, and even more preferably 5.0 mass% or less.

[0069] Furthermore, the coated metal sheet 1 according to this embodiment may further include various known layers between the photocatalytic layer 20 and the inorganic coating layer 30, as schematically shown in FIG. 2B .

[0070] Here, even in the cases shown in FIGS. 2A and 2B, the total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 20 is T (=d 1 +d 2 +α) is set to 15.00 μm or less. This prevents a decrease in ease of manufacturing and a decrease in processability, secures a route for zinc elution from the zinc-containing metal layer 13, and allows zinc to be sufficiently eluted. Furthermore, it becomes possible to uniformly exhibit the desired photocatalytic effect throughout the entire photocatalytic layer 20. The total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 20 T (=d 1 +d 2 +α) is preferably 10.00 μm or less, more preferably 7.00 μm or less, and even more preferably 1.00 μm or less, less than 1.00 μm, 0.90 μm or less, 0.80 μm or less, or 0.70 μm or less.

[0071] <Modification 2> The coated metal sheet 1 according to this embodiment may have, in addition to the inorganic coating layer 30 located between the metal sheet 10 and the photocatalytic layer 20, a resin coating layer 40 as an example of a third coating layer further below the inorganic coating layer 30. The resin coating layer 40 will be described in detail below with reference to Figures 3A and 3B. Figures 3A and 3B are explanatory diagrams that schematically show another example of the structure of a coated metal sheet according to this embodiment.

[0072] 3A and 3B are schematic diagrams showing the layer structure of the coated metal sheet 1 when a resin coating layer 40, which is an example of a third coating layer, is provided. In this case, the coated metal sheet 1 according to this embodiment has the resin coating layer 40, which is an example of a third coating layer, below the inorganic coating layer 30 as described above.

[0073] The resin coating layer 40 is formed by chemical conversion treatment after impurities such as oil and surface oxides adhering to the surface of the metal plate 10 are removed by a known degreasing process and cleaning process.

[0074] The resin coating layer 40 according to this embodiment contains, for example, a resin, and may further contain one or more selected from the group consisting of a silane coupling agent, a zirconium compound, silica, phosphoric acid and its salts, fluoride, a vanadium compound, and tannin or tannic acid. The inclusion of these substances further improves the film-forming properties after application of the chemical conversion treatment solution, the barrier properties (density) of the coating against corrosion factors such as moisture and corrosive ions, and the adhesion of the coating to the surface of the metal sheet, thereby contributing to raising the corrosion resistance of the coating.

[0075] In particular, when the resin coating layer 40 contains one or more of a silane coupling agent or a zirconium compound, a cross-linked structure is formed within the resin coating layer 40, which also strengthens the bond with the metal plate surface, making it possible to further improve the adhesion and barrier properties of the coating.

[0076] Furthermore, when the resin coating layer 40 contains one or more of silica, phosphoric acid and its salts, fluorides, or vanadium compounds, it functions as an inhibitor and forms a precipitated film or a passive film on the surface of the metal plate, thereby further improving corrosion resistance.

[0077] Hereinafter, the components that may be contained in the resin coating layer 40 will be described in detail with examples.

[0078] [Resin] As the resin, for example, known organic resins such as polyester resin, polyurethane resin, epoxy resin, phenolic resin, acrylic resin, polyolefin resin, etc. can be used. In order to further improve adhesion to the metal plate, it is preferable to use at least one resin having a forced moiety or a polar functional group in the molecular chain (polyester resin, urethane resin, epoxy resin, acrylic resin, etc.). The resin may be used alone or in combination of two or more types.

[0079] The resin content in the resin coating layer 40 is, for example, preferably 0% by mass or more, and more preferably 1% by mass or more, relative to the solid content of the coating. This allows for improved corrosion resistance. Furthermore, the resin content in the resin coating layer 40 is, for example, preferably 85% by mass or less, more preferably 60% by mass or less, and even more preferably 40% by mass or less, relative to the solid content of the coating. By setting the resin content to 85% by mass or less, the corrosion resistance of the coating can be improved while ensuring the performance required of the coating other than corrosion resistance.

[0080] [Silane Coupling Agent] Examples of the silane coupling agent include γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropylmethyldiethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropyltriethoxysilane, Silane, γ-methacryloxypropylmethyldiethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltriethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropylmethyldiethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane Silane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropyltriethoxysilane, γ-mercaptopropylmethyldiethoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, vinyltriacetoxysilane, γ-chloropropyltrimethoxysilane, γ-chloropropylmethyldimethoxysilane dimethylsilane, γ-chloropropyltriethoxysilane, γ-chloropropylmethyldiethoxysilane, hexamethyldisilazane, γ-anilinopropyltrimethoxysilane, γ-anilinopropylmethyldimethoxysilane, γ-anilinopropyltriethoxysilane, γ-anilinopropylmethyldiethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, vinyltriethoxysilane, vinylmethyldiethoxysilane, octadecyldimethyl[3-(trimethoxysilyl)propyl]ammonium chloride,Examples of suitable silane coupling agents include octadecyldimethyl[3-(methyldimethoxysilyl)propyl]ammonium chloride, octadecyldimethyl[3-(triethoxysilyl)propyl]ammonium chloride, octadecyldimethyl[3-(methyldiethoxysilyl)propyl]ammonium chloride, γ-chloropropylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, methyltrichlorosilane, dimethyldichlorosilane, and trimethylchlorosilane. The amount of silane coupling agent added to the chemical conversion treatment agent for forming the resin coating layer 40 can be, for example, 2 to 80 g / L. By adding 2 g / L or more of the silane coupling agent, adhesion to the metal sheet surface can be improved, thereby improving the processing adhesion of the coating film. Furthermore, by adding 80 g / L or less of the silane coupling agent, the cohesive strength of the coating film can be maintained, thereby improving the processing adhesion of the coating film. The silane coupling agents exemplified above may be used alone or in combination of two or more.

[0081] [Zirconium Compound] Examples of zirconium compounds include zirconium normal propylate, zirconium normal butylate, zirconium tetraacetylacetonate, zirconium monoacetylacetonate, zirconium bisacetylacetonate, zirconium monoethylacetoacetate, zirconium acetylacetonate bisethylacetoacetate, zirconium acetate, zirconium monostearate, zirconium carbonate, ammonium zirconium carbonate, potassium zirconium carbonate, and sodium zirconium carbonate. The amount of zirconium compound added to the chemical conversion treatment agent for forming the resin coating layer 40 can be, for example, 2 to 80 g / L. By adding the zirconium compound in an amount of 2 g / L or more, adhesion to the metal sheet surface can be improved, thereby improving the processing adhesion of the coating film. Furthermore, by adding the zirconium compound in an amount of 80 g / L or less, the cohesive strength of the coating can be maintained, thereby improving the processing adhesion of the coating film. Such zirconium compounds may be used alone or in combination of two or more.

[0082] [Silica] Examples of silica that can be used include commercially available silica gels such as "Snowtex N," "Snowtex C," "Snowtex UP," and "Snowtex PS" manufactured by Nissan Chemical Industries, Ltd., and "Adelite AT-20Q" manufactured by ADEKA Corporation, as well as powdered silica such as Aerosil #300 manufactured by Nippon Aerosil Co., Ltd. The type of silica can be selected appropriately depending on the required performance of the coated metal sheet. The amount of silica added to the chemical conversion treatment agent for forming the resin coating layer 40 is preferably 1 to 40 g / L. By adding silica in an amount of 1 g / L or more, it is possible to improve the processing adhesion of the coating film. Furthermore, by adding silica in an amount of 40 g / L or less, it is possible to achieve both processing adhesion and corrosion resistance while suppressing cost increases.

[0083] [Phosphoric Acid and Salts Thereof] Examples of phosphoric acid and salts thereof include phosphoric acids such as orthophosphoric acid, metaphosphoric acid, pyrophosphoric acid, triphosphoric acid, and tetraphosphoric acid, and salts thereof; ammonium salts such as triammonium phosphate and diammonium hydrogen phosphate; phosphonic acids such as aminotri(methylenephosphonic acid), 1-hydroxyethylidene-1,1-diphosphonic acid, ethylenediaminetetra(methylenephosphonic acid), and diethylenetriaminepenta(methylenephosphonic acid), and salts thereof; and organic phosphoric acids such as phytic acid and salts thereof. Examples of phosphoric acid salts other than ammonium salts include metal salts with Na, Mg, Al, K, Ca, Mn, Ni, Zn, Fe, and the like. Phosphoric acid and salts thereof may be used alone or in combination of two or more.

[0084] The content of phosphoric acid and its salts is preferably 0% by mass or more, and more preferably 1% by mass or more, based on the solid content of the coating. Furthermore, the content of phosphoric acid and its salts is preferably 20% by mass or less, and more preferably 10% by mass or less, based on the solid content of the coating. By keeping the content of phosphoric acid and its salts at 20% by mass or less, embrittlement of the coating can be prevented, and a decrease in the processing adhesion of the coating when the coated metal sheet is formed can be prevented.

[0085] [Fluoride] Examples of fluorides include ammonium zirconate fluoride, ammonium silicofluoride, ammonium titanium fluoride, sodium fluoride, potassium fluoride, calcium fluoride, lithium fluoride, titanium hydrofluoric acid, zirconate hydrofluoric acid, etc. Such fluorides may be used alone or in combination of two or more.

[0086] The fluoride content is preferably 0% by mass or more, and more preferably 1% by mass or more, based on the solid content of the coating. The fluoride content is preferably 20% by mass or less, and more preferably 10% by mass or less, based on the solid content of the coating. A fluoride content of 20% by mass or less can prevent embrittlement of the coating and can prevent a decrease in the coating's adhesion during forming of the coated metal sheet.

[0087] [Vanadium Compound] Examples of vanadium compounds include vanadium compounds obtained by reducing pentavalent vanadium compounds such as vanadium pentoxide, metavanadic acid, ammonium metavanadate, sodium metavanadate, and vanadium oxytrichloride with a reducing agent to divalent to tetravalent vanadium compounds, and vanadium trioxide, vanadium dioxide, vanadium oxysulfate, vanadium oxyoxalate, vanadium oxyacetylacetonate, vanadium acetylacetonate, vanadium trichloride, vanadium phosphomolybdic acid, vanadium sulfate, vanadium dichloride, and vanadium oxide, and other vanadium compounds having a tetravalent to divalent oxidation number. These vanadium compounds may be used alone or in combination of two or more.

[0088] The content of the vanadium compound is preferably 0% by mass or more, and more preferably 1% by mass or more, based on the solid content of the coating. Furthermore, the content of the vanadium compound is preferably 20% by mass or less, and more preferably 10% by mass or less, based on the solid content of the coating. By keeping the vanadium compound content at 20% by mass or less, it is possible to prevent embrittlement of the coating and to prevent a decrease in the processing adhesion of the coating when the coated metal sheet is formed.

[0089] [Tannin or Tannic Acid] Tannin or tannic acid can be either hydrolyzable tannin or condensed tannin. Examples of tannin and tannic acid include ham meta tannin, Chinese gall tannin, gall nut tannin, myrobalan tannin, dividivi tannin, algarovila tannin, valonia tannin, and catechin. The amount of tannin or tannic acid added to the chemical conversion treatment agent for forming the resin coating layer 40 can be 2 to 80 g / L. By adding tannin or tannic acid in an amount of 2 g / L or more, adhesion to the metal sheet surface can be improved, thereby improving the processing adhesion of the coating film. Furthermore, by adding tannin or tannic acid in an amount of 80 g / L or less, the cohesive strength of the coating can be maintained, improving the processing adhesion of the coating film.

[0090] Furthermore, the resin coating layer 40 may further contain a colorant in addition to the components described above, which allows the appearance of the coated metal sheet 1 according to this embodiment to have a desired color tone, thereby further improving the design of the coated metal sheet 1.

[0091] The type and content of the colorant contained in the resin film layer 40 are not particularly limited and may be adjusted as appropriate.

[0092] Furthermore, an acid, alkali, or the like may be added to the chemical conversion treatment agent for forming the resin film layer 40 to adjust the pH, within a range that does not impair performance.

[0093] The average thickness d of the resin coating layer 40 3 is preferably 0.20 μm or more, more preferably 0.50 μm or more, and even more preferably 2.50 μm or more. This allows the resin coating layer 40 to be uniformly formed on the surface of the metal sheet 10, while stably achieving the various effects achieved by providing the coating layer as described above. In addition, the average thickness d of the resin coating layer 40 3is preferably 60.00 μm or less, more preferably 30.00 μm or less, and even more preferably 15.00 μm or less, 1.00 μm or less, less than 1.00 μm, or 0.80 μm or less. This allows the resin coating layer 40 to be formed uniformly on the surface of the metal sheet 10, while stably achieving the various effects achieved by providing the coating layer as described above.

[0094] Furthermore, the coated metal sheet 1 according to this embodiment may further include various known layers between the inorganic coating layer 30 and the resin coating layer 40, as schematically shown in FIG. 3B .

[0095] 3A and 3B, the total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 20 is T (=d 1 +d 3 +d 4 +α) is set to 60.00 μm or less. This prevents a decrease in ease of manufacturing and processability, ensures a zinc elution path from the zinc-containing metal layer 13, and allows zinc to be sufficiently eluted. Furthermore, it becomes possible to uniformly exhibit the desired photocatalytic effect throughout the photocatalytic layer 20. The total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 20 T (=d 1 +d 3 +d 4 +α) is preferably 15.00 μm or less, more preferably 10.00 μm or less, even more preferably 7.00 μm or less, and even more preferably 1.00 μm or less, less than 1.00 μm, 0.90 μm or less, 0.80 μm or less, or 0.70 μm or less.

[0096] In each of the modified examples described above, when the antiviral test specified in JIS R1756:2020 is performed on the coated metal sheet 1 for 4 hours, the concentration of zinc ions eluted into the virus-containing liquid falls within the range of 0.60 to 5.00 mass%.

[0097] 2A to 3B show the case where each layer is provided on one side of the metal plate 10, but each layer may be provided on both sides of the metal plate 10. In this case, the total thickness d from the surface of the metal plate 10 to the surface of the photocatalytic layer 20 is T The thickness of each surface of the coated metal sheet 1 should be 60.00 μm or less.

[0098] The coated metal sheet according to the first embodiment of the present invention has been described in detail above with reference to FIGS. 1 to 3B.

[0099] <Method for measuring the average thickness of each layer> Here, the average thickness of each layer, including the photocatalytic layer, can be measured by observing the layer of interest from the cross-sectional direction using a microscope. As a method for preparing a sample for cross-sectional observation, known methods can be used, such as embedding the sample in resin and polishing the observation surface, FIB processing, and microtome method. Furthermore, known devices such as SEM and TEM can be used as the type of microscope.

[0100] (Regarding the manufacturing method of the coated metal plate) The coated metal plate according to the present embodiment as described above can be manufactured by subjecting the surface of the base metal plate 10 to various pretreatments such as cleaning as necessary, and then applying a photocatalytic treatment agent for forming the photocatalytic layer 20, an inorganic chemical conversion treatment agent for forming the inorganic coating layer 30, an organic chemical conversion treatment agent for forming the resin coating layer 40, or the like, so as to form the desired layer configuration, followed by drying and baking.

[0101] Here, various coating materials can be applied by commonly known coating methods such as roll coating, curtain flow coating, air spraying, airless spraying, dipping, bar coating, brush coating, etc. Roll coating, which is a feature of the present product and allows stable application of a thin film, is particularly preferred.

[0102] The drying and baking conditions are not particularly limited and may be set appropriately depending on the paint used, etc.

[0103] Second Embodiment Next, a coated metal sheet according to a second embodiment of the present invention will be described in detail. The second embodiment of the present invention relates to a coated metal sheet having a metal sheet and a coating layer located on at least one surface of the metal sheet, the coating layer having a first coating layer located on the outermost surface of the coated metal sheet and containing a compound having photocatalytic activity and 0.2 to 20.0 mass % zinc elemental metal, calculated as metallic Zn.

[0104] (Regarding Coated Metal Sheet) <Structure of Coated Metal Sheet> First, the structure of a coated metal sheet according to a second embodiment of the present invention will be described below with reference to Fig. 4. Fig. 4 is an explanatory diagram that schematically shows an example of the structure of a coated metal sheet according to this embodiment.

[0105] As shown in FIG. 4, a coated metal sheet 3 according to a second embodiment of the present invention has a coating layer on at least one surface of the metal sheet, and includes at least a metal sheet 10 and, as the coating layer, a photocatalytic layer 25 as an example of a first coating layer.

[0106] [Regarding the Metal Plate 10] In the coated metal plate 3 according to this embodiment, the metal plate 10 is constructed by using various types of base metal 11 as the base material of the metal plate 10. Here, various types of metal plates can be used as the base metal 11. Examples of such metal plates include various types of steel plates, aluminum plates, stainless steel plates, etc., and the base metal 11 may be selected depending on the strength, properties, etc. required for the base metal 11.

[0107] Furthermore, in the coated metal sheet 3 according to this embodiment, various plating layers may be provided on the surface of the base metal 11 constituting the metal sheet 10. Here, the various plating layers may include plating layers that do not contain zinc.

[0108] Here, the thickness of the metal plate 10 as described above is not particularly limited, and may be set appropriately depending on the mechanical strength (e.g., tensile strength, etc.) and processability required for the painted metal plate 3 of this embodiment.

[0109] Furthermore, various patterns such as a hairline pattern or a spangle pattern may be present on the surface of the metal sheet 10 along the rolling direction of the base metal 11. By providing such patterns, it is possible to further improve the design of the coated metal sheet 3.

[0110] [Regarding the Photocatalytic Layer 25] In the coated metal sheet 3 according to this embodiment, the photocatalytic layer 25, which is an example of a first coating layer, is a layer located on the outermost surface of the coating layer on at least one surface of the metal sheet 10, as schematically shown in Fig. 4. The photocatalytic layer 25 is a layer containing at least a compound having photocatalytic activity (hereinafter sometimes abbreviated as "photocatalytic compound") and the element Zn.

[0111] The photocatalytic layer 25 according to this embodiment contains a compound having photocatalytic activity, and the compound having photocatalytic activity causes a photocatalytic reaction in response to light (particularly light in the ultraviolet to visible light range) incident on the photocatalytic layer 25. As a result, the photocatalytic layer 25 according to this embodiment exhibits various photocatalytic effects, including an antiviral effect and a bactericidal effect. This allows the coated metal sheet 3 according to this embodiment to achieve various properties, including an antiviral effect and a bactericidal effect.

[0112] Furthermore, since the photocatalytic layer 25 according to this embodiment contains the element Zn, the element Zn contained in the photocatalytic layer 25 fulfills the same function as the Zn contained in the zinc-containing metal layer 13 described in the first embodiment. As a result, zinc elution into a virus-containing liquid occurs in the antiviral test specified in JIS R1756:2020, as discovered by the present inventors. This allows the coated metal sheet 3 according to this embodiment to achieve the same effects as the coated metal sheet 1 according to the first embodiment, and makes it possible to further improve the antiviral function of the coated metal sheet 3 for a longer period of time by a simpler method.

[0113] The photocatalytic compound contained in the photocatalytic layer 25 according to this embodiment is the same as the photocatalytic compound contained in the photocatalytic layer 20 according to the first embodiment, and exhibits the same effects as the photocatalytic compound contained in the photocatalytic layer 20 according to the first embodiment. Therefore, detailed description of the photocatalytic compound will be omitted below.

[0114] In the photocatalytic layer 25 according to this embodiment, the content of element Zn contained in the photocatalytic layer 25 is 0.2 mass% or more, calculated as metallic Zn. If the Zn content is less than 0.2 mass%, the amount of zinc eluted from the photocatalytic layer 25 is too small, and the antibacterial effect described above cannot be achieved. If the Zn content is 0.2 mass% or more, the antibacterial effect described above can be achieved. The content of the element Zn is more preferably 0.6 mass% or more, and even more preferably 1.0 mass% or more.

[0115] On the other hand, the Zn content in the photocatalytic layer 25 is 20.0 mass% or less, calculated as metallic Zn. If the Zn content exceeds 20.0 mass%, the amount of zinc eluted from the photocatalytic layer 25 becomes too large, reducing the density of the photocatalytic layer 25 and making it easier for corrosion factors to penetrate from the outside, resulting in reduced corrosion resistance of the coated metal sheet 3. By ensuring that the total content of the Zn element is 20.0 mass% or less, it is possible to ensure the content of the photocatalytic compound while still achieving the above-mentioned effects without saturating, and it is also possible to ensure the corrosion resistance of the coated metal sheet 3. The total content of the Zn element is preferably 18.0 mass% or less, more preferably 16.0 mass% or less, even more preferably 5.0 mass% or less, and even more preferably 3.5 mass% or less, or 2.5 mass% or less.

[0116] The photocatalytic layer 25 further contains at least one element selected from the group consisting of Si and Zr, and the total concentration of such elements is preferably 5% by mass or more in terms of silica for Si and zirconia for Zr. In other words, the photocatalytic layer 25 is an inorganic coating having a three-dimensional network structure of inorganic components containing at least one element selected from the group consisting of Si and Zr, and possibly impurities. The total concentration of at least one element selected from the group consisting of Si and Zr is preferably 5% by mass or more in terms of silica for Si and zirconia for Zr. By including at least one element selected from the group consisting of Si and Zr at the above concentrations, a photocatalytic layer 25 with superior corrosion resistance can be achieved. The total content of at least one element selected from the group consisting of Si and Zr is more preferably 10% by mass or more. Here, "inorganic components" refers to components that do not contain organic resins.

[0117] The photocatalytic layer 25 further contains at least one element selected from the group consisting of Si and Zr, and the total concentration of these elements is preferably 50% by mass or less, calculated as silica for Si and zirconia for Zr. By including at least one element selected from the group consisting of Si and Zr at the above-mentioned concentrations, a photocatalytic layer 25 with superior corrosion resistance can be achieved. The total content of at least one element selected from the group consisting of Si and Zr is more preferably 40% by mass or less. The Si or Zr preferably has excellent light transmittance and is an inorganic component that is less susceptible to decomposition by the photocatalyst. Examples of inorganic components containing Si and Zr include silica and zirconia.

[0118] Furthermore, the photocatalytic layer 25 preferably contains at least one element selected from the group consisting of Cu, Fe, Ni, and Ag in addition to the above-mentioned photocatalytic compound and at least one element of Si or Zr. Here, the elements Cu, Fe, Ni, and Ag are elements that promote the elution of zinc from the photocatalytic layer 25, so by further containing these elements in the photocatalytic layer 25, more zinc is eluted from the photocatalytic layer 25, which is preferable. Furthermore, the elements Cu and Ag are particularly preferable because they also exhibit antibacterial effects.

[0119] The total content of at least one element selected from the group consisting of Cu, Fe, Ni, and Ag in the photocatalytic layer 25 is preferably 0.2 mass% or more, calculated as metal elements. A total content of the metal elements of 0.2 mass% or more enables the above-described effects to be exhibited in a more favorable manner. The total content of the metal elements is more preferably 0.6 mass% or more, and even more preferably 1.0 mass% or more. On the other hand, the total content of at least one element selected from the group consisting of Cu, Fe, Ni, and Ag in the photocatalytic layer 25 is preferably 5.0 mass% or less, calculated as metal elements. A total content of the metal elements of 5.0 mass% or less enables the above-described effects to be exhibited without saturating while ensuring the content of the photocatalytic compound. The total content of the metal elements is more preferably 3.5 mass% or less, and even more preferably 2.5 mass% or less.

[0120] The photocatalyst layer 25 containing the above-mentioned photocatalyst compound may contain an antibacterial agent or an adsorbent such as activated carbon or zeolite, if necessary, within a range that does not impair the effects of the present invention.

[0121] The average thickness d of the photocatalytic layer 25 1 4 ′ (In the case of the layer structure shown in FIG. 4 , the total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 25 (which can also be regarded as the outermost surface of the coating layer) T The average thickness d of the photocatalytic layer 25 is 0.05 μm or more. 1If the average thickness d' is less than 0.05 μm, it becomes difficult to uniformly form the photocatalytic layer 25 as described above, and the obtained photocatalytic effect becomes uneven, which is not preferable. 1 By making the thickness ' 0.05 μm or more, it is possible to secure a path for zinc to dissolve from the photocatalytic layer 25, thereby allowing zinc to be sufficiently dissolved, and to make the desired photocatalytic effect appear uniformly throughout the photocatalytic layer 25.

[0122] On the other hand, the average thickness d of the photocatalytic layer 25 1 ' (In the case of the layer structure shown in FIG. 4, the total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 25 T The average thickness d of the photocatalytic layer 25 is 5.00 μm or less. 1 If the average thickness d' exceeds 5.00 μm, the photocatalytic effect obtained will be saturated, but the manufacturing cost will increase, which is not preferable. Also, it will be difficult to ensure a sufficient amount of zinc elution from the photocatalytic layer 25, which is also not preferable from this point of view. Furthermore, since the photocatalytic layer is an inorganic coating, its processability will be reduced. 1 By setting the thickness ' to 5.00 μm or less, it is possible to suppress a decrease in ease of manufacturing and a decrease in processability, to ensure a route for elution of zinc from the photocatalytic layer 25, to allow sufficient elution of zinc, and further to make it possible to uniformly exhibit the desired photocatalytic effect throughout the entire photocatalytic layer 25.

[0123] Normally, there is a certain probability that light passes through the photocatalytic layer 25 without hitting the photocatalytic compound. Conventionally, such light that does not interact with the photocatalytic compound is light that does not provide a photocatalytic effect. In this embodiment, by reflecting such light on the surface of the metal plate 10, it is possible to increase the probability that light incident on the photocatalytic layer 25 hits the photocatalytic compound. As a result, in this embodiment, the photocatalytic effect can be further improved. In the case of the layer structure shown in Figure 4, the total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 25 is Tis naturally 5.00 μm or less, and as a result, it becomes possible to utilize the reflected light that is incident on the surface of the metal plate 10 (in other words, the interface between the metal plate 10 and the photocatalytic layer 25) for the photocatalytic reaction by the photocatalytic compound, thereby making it possible to further improve the photocatalytic effect while suppressing costs.

[0124] The average thickness d of the photocatalytic layer 25 1 The average thickness d′ of the photocatalytic layer 20 is preferably 0.10 μm or more, and more preferably 0.15 μm or more. 1 is preferably 2.00 μm or less, more preferably 1.00 μm or less, even more preferably less than 1.00 μm, and even more preferably 0.80 μm or less, 0.60 μm or less, or 0.50 μm or less.

[0125] Although Figure 4 illustrates a configuration in which the photocatalytic layer 25 is formed on one surface of the metal plate 10, the photocatalytic layer 25 may be formed on both surfaces of the metal plate 10.

[0126] <Zinc ion concentration eluted into virus-containing liquid in antiviral test> The structure of coated metal sheet 3 as described above is one of the conditions for ensuring that the zinc ion concentration eluted into virus-containing liquid falls within the range of 0.60 to 5.00 mass % when an antiviral test specified in JIS R1756:2020 is carried out for four hours.

[0127] The reason why the above-described structure is one of the conditions is that in the coated metal plate 3 according to this embodiment, the photocatalytic layer 25 is provided in an appropriate state, and further, the total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 25 is T , and the Zn content in the photocatalytic layer 25 are each within a specific range, so that an appropriate amount of zinc can be eluted from the photocatalytic layer 25.

[0128] The amount of zinc eluted from the photocatalytic layer 25 depends on the Zn content in the photocatalytic layer 25 and the total thickness d T By adjusting the above, it is possible to control the temperature to a desired state.

[0129] Here, if the zinc ion concentration in the virus-containing liquid is less than 0.60 mass%, this means that the amount of zinc eluted from the photocatalyst layer 25 is insufficient, making it impossible to further improve the antiviral function of the coated metal sheet 3. The zinc ion concentration in the virus-containing liquid is preferably 0.90 mass% or more, and more preferably 1.20 mass% or more.

[0130] On the other hand, if the zinc ion concentration in the virus-containing liquid exceeds 5.00 mass%, the amount of zinc eluted from the photocatalytic layer 25 becomes too large, making it impossible to ensure the corrosion resistance of the metal plate 10. The zinc ion concentration in the virus-containing liquid is preferably 4.50 mass% or less, and more preferably 3.50 mass% or less.

[0131] In the coated metal sheet 3 according to this embodiment, the total content of elements (more specifically, ions) having a potential more noble than zinc present in the coating layer is preferably 20.0 mass% or less in terms of metal elements. Examples of elements having a potential more noble than zinc include Cu and Ag. By setting the total content of elements having a potential more noble than zinc in the coating layer to 20.0 mass% or less, the zinc ion concentration in the virus-containing liquid described above can be set to 5.00 mass% or less, thereby achieving both excellent antiviral properties and excellent corrosion resistance. The total content of elements having a potential more noble than zinc in the coating layer is more preferably 15.0 mass% or less, even more preferably 11.0 mass% or less, and even more preferably 7.5 mass% or less. The lower limit of the total content of elements having a potential more noble than zinc in the coating layer is not particularly specified and may be 0 mass%.

[0132] The antiviral test is carried out for 4 hours in accordance with the method specified in JIS R1756: 2020. The concentration of zinc ions dissolved in the virus-containing solution may be measured by inductively coupled plasma (ICP) atomic emission spectrometry.

[0133] <Modification 3> The coated metal sheet 3 according to this embodiment, which has the layer structure shown in Fig. 4, may have an additional coating layer that functions as a chemical conversion coating layer between the metal sheet 10 and the photocatalytic layer 25. By providing a chemical conversion coating layer between the metal sheet 10 and the photocatalytic layer 25, it is possible to further improve the adhesion between the metal sheet 10 and the photocatalytic layer 25. Furthermore, it is also possible to further improve the corrosion resistance and the like of the coated metal sheet 3 according to this embodiment.

[0134] The additional coating layer that functions as a chemical conversion coating layer will be described in detail below with reference to Figures 5A and 5B, which are explanatory diagrams that schematically show another example of the structure of a coated metal sheet according to this embodiment.

[0135] 5A and 5B are schematic diagrams showing the layer structure of a coated metal sheet 3 when an inorganic coating layer 30 functioning as a chemical conversion coating layer, as an example of a second coating layer, is provided. In this case, the coated metal sheet 3 according to this embodiment has the inorganic coating layer 30, as an example of a second coating layer, between the metal sheet 10 and the photocatalyst layer 25.

[0136] Furthermore, the coated metal sheet 3 according to this embodiment may further include various known layers between the photocatalytic layer 25 and the inorganic coating layer 30, as schematically shown in FIG. 5B.

[0137] Here, the inorganic coating layer 30 of the painted metal plate 3 according to this embodiment has the same configuration as the inorganic coating layer 30 of the painted metal plate 1 according to the first embodiment of the present invention, and also has the same effects, so detailed explanation will be omitted below.

[0138] The average thickness d of the inorganic coating layer 30 2 is preferably 0.05 μm or more, and more preferably 0.10 μm or more. This allows the inorganic coating layer 30 to be uniformly formed on the surface of the metal sheet 10, while stably achieving the various effects achieved by providing the chemical conversion coating layer as described above. In addition, the average thickness d of the inorganic coating layer 30 2is preferably 5.00 μm or less, more preferably 1.00 μm or less, even more preferably less than 1.00 μm, and even more preferably 0.80 μm or less, 0.60 μm or less, or 0.50 μm or less. This allows the inorganic coating layer 30 to be formed uniformly on the surface of the metal sheet 10, while stably achieving the various effects achieved by providing the chemical conversion coating layer as described above.

[0139] 5A and 5B, the total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 25 is T (=d 1 '+d 2 +α) is set to 60.00 μm or less. This prevents a decrease in ease of manufacturing and processability, ensures a zinc elution path from the photocatalytic layer 25, and allows zinc to be sufficiently eluted. Furthermore, it becomes possible to uniformly exhibit the desired photocatalytic effect throughout the photocatalytic layer 25. The total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 25 T (=d 1 '+d 2 +α) is preferably 15.00 μm or less, more preferably 10.00 μm or less, even more preferably 7.00 μm or less, and even more preferably 1.00 μm or less, less than 1.00 μm, 0.90 μm or less, 0.80 μm or less, or 0.70 μm or less.

[0140] <Modification 4> The coated metal sheet 3 according to this embodiment may have, in addition to the inorganic coating layer 30 located between the metal sheet 10 and the photocatalytic layer 25, a resin coating layer 40 as an example of a third coating layer further below the inorganic coating layer 30. The resin coating layer 40 will be described in detail below with reference to Figures 6A and 6B. Figures 6A and 6B are explanatory diagrams that schematically show another example of the structure of a coated metal sheet according to this embodiment.

[0141] 6A and 6B are schematic diagrams showing the layer structure of a coated metal sheet 3 when a resin coating layer 40, which is an example of a third coating layer, is provided. In this case, the coated metal sheet 3 according to this embodiment has the resin coating layer 40, which is an example of a third coating layer, below the inorganic coating layer 30 as described above.

[0142] Furthermore, the coated metal sheet 3 according to this embodiment may further include various known layers between the inorganic coating layer 30 and the resin coating layer 40, as schematically shown in FIG. 6B .

[0143] Here, the resin film layer 40 of the painted metal plate 3 of this embodiment has the same configuration as the resin film layer 40 of the painted metal plate 1 of the first embodiment of the present invention and has the same effects, so detailed explanation will be omitted below.

[0144] The average thickness d of the resin coating layer 40 3 is preferably 0.20 μm or more, more preferably 0.50 μm or more, and even more preferably 2.50 μm or more. This allows the resin coating layer 40 to be uniformly formed on the surface of the metal sheet 10, while stably achieving the various effects achieved by providing the coating layer as described above. In addition, the average thickness d of the resin coating layer 40 3 is preferably 60.00 μm or less, more preferably 30.00 μm or less, even more preferably 12.00 μm or less, and even more preferably 1.00 μm or less, less than 1.00 μm, or 0.90 μm or less. This allows the resin coating layer 40 to be formed uniformly on the surface of the metal sheet 10, while stably achieving the various effects achieved by providing the coating layer as described above.

[0145] 6A and 6B, the total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 25 is T (=d 1 '+d 3 +d 4+α) is set to 60.00 μm or less. This prevents a decrease in ease of manufacturing and processability, ensures a zinc elution path from the photocatalytic layer 25, and allows zinc to be sufficiently eluted. Furthermore, it becomes possible to uniformly exhibit the desired photocatalytic effect throughout the photocatalytic layer 25. The total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalytic layer 25 T (=d 1 '+d 3 +d 4 +α) is preferably 15.00 μm or less, more preferably 10.00 μm or less, even more preferably 7.00 μm or less, and even more preferably 1.00 μm or less, less than 1.00 μm, 0.90 μm or less, 0.80 μm or less, or 0.60 μm or less.

[0146] In each of the modified examples described above, when the antiviral test specified in JIS R1756:2020 is performed on the coated metal sheet 3 for four hours, the concentration of zinc ions eluted into the virus-containing liquid falls within the range of 0.60 to 5.00 mass%.

[0147] 5A to 6B show the case where each layer is provided on one side of the metal plate 10, but each layer may be provided on both sides of the metal plate 10. In this case, the total thickness d from the surface of the metal plate 10 to the surface of the photocatalytic layer 25 is T The thickness of each surface of the coated metal plate 3 should be 60.00 μm or less.

[0148] The coated metal sheet according to the second embodiment of the present invention has been described in detail above with reference to FIGS. 4 to 6B.

[0149] <Method for measuring the average thickness of each layer> Here, the average thickness of each layer, including the photocatalytic layer, can be measured by observing the layer of interest from the cross-sectional direction using a microscope. As a method for preparing a sample for cross-sectional observation, known methods can be used, such as embedding the sample in resin and polishing the observation surface, FIB processing, and microtome method. Furthermore, known devices such as SEM and TEM can be used as the type of microscope.

[0150] (Regarding the manufacturing method of the coated metal plate) The coated metal plate according to the present embodiment as described above can be manufactured by subjecting the surface of the base metal plate 10 to various pretreatments such as cleaning as necessary, and then applying a photocatalytic treatment agent for forming the photocatalytic layer 25, an inorganic chemical conversion treatment agent for forming the inorganic coating layer 30, an organic chemical conversion treatment agent for forming the resin coating layer 40, or the like, to the desired layer configuration, followed by drying and baking.

[0151] Here, various coating materials can be applied by commonly known coating methods such as roll coating, curtain flow coating, air spraying, airless spraying, dipping, bar coating, brush coating, etc. Roll coating, which is a feature of the present product and allows stable application of a thin film, is particularly preferred.

[0152] The drying and baking conditions are not particularly limited and may be set appropriately depending on the paint used, etc.

[0153] The coated metal sheet according to the present invention will be specifically described below with reference to examples and comparative examples. Note that the examples shown below are merely examples of the coated metal sheet according to the present invention, and the coated metal sheet according to the present invention is not limited to the examples below.

[0154] Nine types of metal sheets shown in Table 1 below were prepared as base metal sheets for the coated metal sheets. In Table 1, the six types of metal sheets designated SD, ZL, GI, GL, AL, and GA are various types of plated steel sheets using steel sheets as the base material. The thickness of each metal sheet, as well as the plating composition and coating weight / specification of each plated steel sheet, are as shown in Table 1 below. In addition, a zinc-containing coating layer using zinc was separately formed on the stainless steel sheet by vapor deposition at a rate of 20 g / m. 2 The coating was formed with a deposition amount of 0.01g and designated as Stainless Steel-2.

[0155]

[0156] Seven types of compounds shown in Table 2 below were prepared as compounds having photocatalytic activity (photocatalytic compounds). All photocatalytic compounds used were commercially available. The supported metals and average particle sizes are also shown in Table 2.

[0157]

[0158] <Organic Chemical Conversion Treatment Agent> The raw materials of the water-based paint (chemical conversion treatment agent) for forming the organic chemical conversion treatment film used to form the resin film layer, and the concentrations in the dried film, are shown in Table 3 below. The amount added was adjusted so that the concentration of each component would be the specified concentration in the dried film. Ion-exchanged water was added to adjust the solids concentration of the treatment agent to 20 mass %. Each treatment agent was applied to achieve the dry film thickness shown in Tables 4-1, 4-2, and 6 below. The metal sheet was then dried in an induction heating furnace so that the temperature reached was 150°C, and then water-cooled using a spray.

[0159]

[0160] <Photocatalytic Treatment Agent, Inorganic Chemical Conversion Treatment Agent> The photocatalytic treatment agent used and the method for preparing the inorganic chemical conversion treatment agent will be described. The inorganic chemical conversion treatment agent for forming the inorganic coating layer was adjusted to have a solids concentration of 8 mass % in consideration of storage stability. The concentration was adjusted by diluting with n-butanol. In addition, in some examples, ammonium dihydrogen phosphate was added as the P source and sodium metavanadate was added as the V source to the inorganic chemical conversion treatment agent described below. The photocatalytic treatment agent was prepared by adding a predetermined amount of the compound shown in Table 2 to the inorganic chemical conversion treatment agent described below. The solids concentrations of the photocatalytic compounds are as shown in Tables 4-1, 4-2, and 6 below.

[0161] (1) Inorganic chemical conversion treatment agent (Si-based): Tetraethoxysilane (22.5 parts by mass), methacryloxypropyltrimethoxysilane (2.8 parts by mass), and n-butanol (26 parts by mass) were mixed and stirred at 60°C for 2 hours. While stirring this mixture, a mixed solution of 26% by mass of hydrochloric acid (3 parts by mass) and n-butanol (26 parts by mass) was added dropwise at a rate of 1 drop / second. Thereafter, the mixture was kept stirred at 60°C for 2 hours to obtain a treatment agent. This series of operations was carried out in a nitrogen atmosphere.

[0162] (2) Inorganic chemical conversion treatment agent (Zr-based): Zirconium n-butoxide (34.5 parts by mass), n-butanol (11.6 parts by mass), 1,5-diaminopentane (0.5 parts by mass), and yttrium nitrate (2.8 parts by mass) were mixed and stirred for 1 hour. Glacial acetic acid (4.8 parts by mass) was then added and stirred for 40 hours. Concentrated nitric acid (0.6 parts by mass) was then added dropwise at a rate of 1 drop / second, and the mixture was stirred for 2 hours to obtain a treatment agent. This series of operations was carried out in a nitrogen atmosphere.

[0163] In some examples, the photocatalytic treatment agent and the inorganic conversion treatment agent may be used with ultrafine zinc oxide (trade name: FZO) manufactured by Ishihara Sangyo Kaisha, Ltd. as a Zn source, nanoparticle cuprous oxide (trade name: FRC-N10) manufactured by Furukawa Chemicals Co., Ltd. as a Cu source, and Fe (trade name: Fe) manufactured by Sigma-Aldrich Co., Ltd. as an Fe source. 2 O 3 The Ni source was nickel nanopowder (product name: 544884) manufactured by Iwatani Corporation, which was targeted to have a particle size of 50 nm, and the Ag source was Ag nanopowder (product name: 576832) manufactured by Sigma-Aldrich Corporation.

[0164] Using the metal sheets and photocatalytic compounds described above, two coated metal sheets having the structures shown in Tables 4-1, 4-2, and 6 were produced by roll coating for each level. Each layer was formed on one side of the metal sheet. For some of the coated metal sheets, a decorative finish was applied to the surface of the metal sheet to form a hairline pattern. For some of the coated metal sheets, a hot-dip galvanized bath containing 0.1 mass % Sb and 0.2 mass % Al was used, and a plated steel sheet on which a spangle pattern had been formed by adjusting the solidification rate of the hot-dip galvanized coating was used as the substrate.

[0165] The average film thickness of each layer in the above-mentioned coated metal sheet was measured by embedding the obtained coated metal sheet in resin, polishing the cross section, and observing the obtained observation surface under a microscope.

[0166] Furthermore, one of the obtained coated metal sheets was subjected to an antiviral test specified in JIS R1756:2020 for 4 hours, and then the concentration of zinc ions eluted into the virus-containing liquid was measured in accordance with the method described above.

[0167] A test piece was prepared using the other half of the obtained coated metal sheet, and the test piece was evaluated from the viewpoints of antiviral properties, processing adhesion, and corrosion resistance. The detailed evaluation methods are as follows.

[0168] <Antiviral Activity> The antiviral activity was verified by measuring the viral infectivity value by the following antiviral test in accordance with the antiviral standard stipulated by the Photocatalyst Industry Association of Japan. More specifically, test specimens (dimensions: 50 × 50 mm) prepared from each coated metal plate were used. 2 The test specimen was placed in a petri dish with the test surface facing up, and a virus suspension containing bacteriophage Qβ was dropped onto the test surface. A film was then placed over the test specimen to allow the virus suspension to adhere to the entire test surface, and the petri dish was then covered with a lid. The petri dish was then left to stand for 4 hours in a room at 25°C with an illuminance of 500 lux, simulating a typical office environment. The virus on the film surface and the test surface was then washed away, and the virus infectivity (unit: PFU, PFU: Plaque Forming Units) in the resulting washing solution was measured by a plaque measurement method. The concentration of dissolved zinc ions in the washing solution was also measured using an inductively coupled plasma (ICP) emission spectrometer (Agilent 7700X).

[0169] Apart from the coated metal sheets, the antiviral test was also carried out on each metal sheet not provided with a photocatalytic layer in the same manner, and the extent to which the viral infectivity of the coated metal sheet had decreased compared to the viral infectivity of the metal sheet not provided with a photocatalytic layer was evaluated as an activity value. 2 If the activity value is reduced by more than 1 × 10 2 If the activity value is 1 × 10 or more, the use of the certification seal prescribed by the Photocatalyst Industry Association is permitted. 2 Those having the above value were judged to be acceptable. In the following Tables 5-1, 5-2 and 7, the obtained activity values ​​are shown in logarithmic form.

[0170] <Processing Adhesion> A test piece was subjected to 0T bending (180° bending), the coating on the outside of the bent portion was peeled off with adhesive tape (Cellotape (registered trademark) manufactured by Nichiban Co., Ltd., tape width 15 mm), and the state of adhesion of the coating to the tape side was observed. The processing adhesion was then evaluated according to the following evaluation criteria. In this adhesion test, a pass level was rated as 3 or higher. Specifically, a score of 4 or higher was judged to be excellent in adhesion, and a score of 3 or higher was judged to be acceptable (pass level).

[0171] (Evaluation criteria) 5: No coating adhered to the tape side 4: Coating peeled off in several places on the tape side, and the peeled length on the steel plate side was less than 5% of the total length of the processed part on one side of the test piece 3: Coating peeled off in several places on the tape side, and the peeled length on the steel plate side was 5% or more but less than 10% of the total length of the processed part on one side of the test piece 2: Coating peeled off on the tape side, and the peeled length on the steel plate side was 10% or more but less than 20% of the total length of the processed part on one side of the test piece 1: Coating peeled off on the tape side, and the peeled length on the steel plate side was 20% or more of the total length of the processed part on one side of the test piece

[0172] <Corrosion resistance of flat plate> The end faces of the test specimens were sealed with tape and subjected to a salt spray test (SST) in accordance with JIS Z 2371:2015 for 72 hours. After the test, the state of rust on the flat plate was observed, and the corrosion resistance was evaluated according to the following evaluation criteria. A pass level was 3 or higher.

[0173] (Evaluation criteria) 5: The area where white rust has occurred is less than 1% of the total area on one side of the test piece. 4: The area where white rust has occurred is 1% or more but less than 5% of the total area on one side of the test piece. 3: The area where white rust has occurred is 5% or more but less than 10% of the total area on one side of the test piece. 2: The area where white rust has occurred is 10% or more but less than 30% of the total area on one side of the test piece. 1: The area where white rust has occurred is 30% or more of the total area on one side of the test piece.

[0174] <Corrosion resistance of processed portion> For each test piece, a test material was obtained by processing (7 mm extrusion) in accordance with the Erichsen test (JIS Z2247:2006). The end faces of the test material were sealed with tape and subjected to a salt spray test (SST) in accordance with JIS Z 2371 for 72 hours. After the test, the state of rust formation in the processed portion was observed, and the corrosion resistance was evaluated according to the following evaluation criteria. A pass level was 3 or higher.

[0175] (Evaluation criteria) 5: The area where white rust has occurred is less than 5% of the total area of ​​the processed part of the test piece. 4: The area where white rust has occurred is 5% or more but less than 10% of the total area of ​​the processed part of the test piece. 3: The area where white rust has occurred is 10% or more but less than 30% of the total area of ​​the processed part of the test piece. 2: The area where white rust has occurred is 30% or more but less than 50% of the total area of ​​the processed part of the test piece. 1: The area where white rust has occurred is 50% or more of the total area of ​​the processed part of the test piece.

[0176] The results obtained are summarized in the following Tables 5-1, 5-2, and 7. As is clear from the following Tables 5-1, 5-2, and 7, the coated metal sheets corresponding to the examples of the present invention exhibited excellent antiviral properties, adhesion during processing, and corrosion resistance, while the coated metal sheets corresponding to the comparative examples of the present invention failed the evaluation results for antiviral properties or adhesion during processing.

[0177]

[0178]

[0179]

[0180]

[0181]

[0182]

[0183] Although the preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings, the present invention is not limited to these examples. It is clear that a person skilled in the art to which the present invention pertains can conceive of various modifications and alterations within the scope of the technical ideas set forth in the claims, and it is understood that these also naturally fall within the technical scope of the present invention.

[0184] The embodiments disclosed herein are illustrative in all respects and are not limiting. The above-described embodiments may be omitted, substituted, or modified in various ways without departing from the scope of the appended claims, the technical scope of the present invention as described below, and the spirit thereof. For example, the components of the above-described embodiments may be arbitrarily combined within the scope that does not impair the effects of the components. Furthermore, such an arbitrary combination naturally provides the functions and effects of each of the components involved in the combination, and also provides other functions and effects that are apparent to those skilled in the art from the description of this specification.

[0185] Furthermore, the effects described in this specification are merely descriptive or exemplary and are not limiting. In other words, the technology according to the present invention may achieve other effects that will be apparent to those skilled in the art from the description of this specification, in addition to or in place of the above-described effects.

[0186] REFERENCE SIGNS LIST 1, 3 Coated metal plate 10 Metal plate 11 Base metal 13 Zinc-containing metal layer 20, 25 Photocatalytic layer (first coating layer) 30 Inorganic coating layer (second coating layer) 40 Resin coating layer (third coating layer)

Claims

1. A coated metal sheet comprising a metal sheet and a coating layer located on at least one surface of the metal sheet, wherein the metal sheet has a zinc-containing metal layer containing at least zinc on at least one surface, and the coating layer comprises a first coating layer located on the outermost surface of the coated metal sheet and containing at least a compound having photocatalytic activity, the first coating layer having an average thickness of 0.05 to 5.00 μm, the total thickness from the surface of the zinc-containing metal layer to the outermost surface of the first coating layer being 15.00 μm or less, and the coated metal sheet having a zinc ion concentration of 0.60 to 5.00 mass% eluted into a virus-containing liquid when an antiviral test specified in JIS R1756:2020 is carried out for 4 hours.

2. The coated metal sheet according to claim 1, wherein the thickness of the first coating layer is 0.05 to 0.95 μm, and the total thickness from the surface of the zinc-containing metal layer to the outermost surface of the first coating layer is less than 1.0 μm.

3. A coated metal sheet according to claim 1 or 2, wherein the total content of elements having a more noble potential than zinc in the coating layer is 0 to 20.0 mass %.

4. The coated metal sheet according to claim 1, wherein the first coating layer further contains at least one element selected from the group consisting of Zn, Cu, Fe, Ni, and Ag.

5. The coated metal sheet according to claim 1, wherein the first coating layer further contains at least one of the elements Si and Zr, and the total content of the elements is 5 to 50 mass % in terms of silica for Si and zirconia for Zr.

6. A coated metal sheet comprising a metal sheet and a coating layer located on at least one surface of the metal sheet, wherein the coating layer comprises a first coating layer located on the outermost surface of the coated metal sheet and containing a compound having photocatalytic activity and 0.2 to 20.0 mass% zinc elemental, calculated as metallic Zn, wherein the average thickness of the first coating layer is 0.05 to 5.00 μm, and the total thickness from the surface of the metal sheet to the outermost surface of the first coating layer is 60.0 μm or less, and wherein when an antiviral test specified in JIS R1756:2020 is carried out for 4 hours, the concentration of zinc ions eluted in a virus-containing liquid is 0.60 to 5.00 mass%.

7. The coated metal sheet according to claim 6, wherein the total content of elements having a more noble potential than zinc in the coating layer is 0 to 20.0 mass %.

8. A coated metal sheet according to claim 6 or 7, wherein the first coating layer further contains at least one element selected from the group consisting of Cu, Fe, Ni, and Ag.

9. A coated metal sheet according to claim 6, wherein the first coating layer further contains at least one of the elements Si and Zr, and the total content of said elements is 5 to 50 mass % in terms of silica for Si and zirconia for Zr.

10. A coated metal sheet as set forth in claim 1 or 6, further comprising a second coating layer located below the first coating layer and made of an inorganic component, the second coating layer containing at least one of Si and Zr as the inorganic component, and the average thickness of the second coating layer being 0.05 to 5.00 μm.

11. The coated metal sheet according to claim 10, wherein the second coating layer further contains at least one of P and V as the inorganic component.

12. The coated metal sheet according to claim 10, wherein the second coating layer further contains at least one element selected from the group consisting of Zn, Cu, Fe, Ni, and Ag.

13. The coated metal sheet according to claim 10, further comprising a third coating layer located below the second coating layer and containing a resin component, the third coating layer having an average thickness of 0.50 to 14.00 μm.

14. The coated metal sheet according to claim 13, wherein the third coating layer further contains a colorant.

15. A coated metal sheet according to claim 1 or 6, wherein the compound having photocatalytic activity is anatase-type titanium oxide.

16. A coated metal sheet according to claim 15, wherein the compound having photocatalytic activity is a metal-supported titanium oxide in which at least one of Cu and Fe is supported on titanium oxide.

17. The coated metal sheet according to claim 1, wherein the metal sheet is a zinc-based plated steel sheet having a zinc-based plated layer as the zinc-containing metal layer.

18. The coated metal sheet according to claim 17, wherein the zinc-based plating layer is a plating layer containing Zn in an amount of 30 mass % or more calculated as metallic Zn.

19. The coated metal sheet according to claim 17, wherein the zinc-based plating layer is any one of a zinc plating layer, a zinc-aluminum alloy plating layer, a zinc-aluminum-magnesium alloy plating layer, a zinc-nickel alloy plating layer, or a zinc-iron alloy plating layer.

20. A coated metal sheet according to claim 1 or 6, wherein the surface of the metal sheet has a hairline extending in the rolling direction of the metal sheet.

21. The coated metal sheet according to claim 1, wherein the zinc-containing metal layer has a spangle pattern on its surface.