Method of producing iron ore pellets

MYPI2025000866A0Undetermined Publication Date: 2024-03-28JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025000866
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-28
Filing Date
2023-07-11
Publication Date
2024-03-28

AI Technical Summary

Technical Problem

Current methods for producing iron ore pellets face challenges in achieving high strength while minimizing emissions, as traditional calcination processes rely on combustion, leading to greenhouse gas emissions and insufficient internal heating, and existing binders either degrade at high temperatures or require additional processing steps.

Method used

A method involving the use of solid carbon, such as charcoal, produced from greenhouse gases like CO2 and CH4, which is mixed with iron ore and a binder, then granulated and fired, allowing internal heating and reducing emissions by consuming these gases as raw materials, thereby enhancing pellet strength and achieving carbon neutrality.

Benefits of technology

This method produces high-strength iron ore pellets while contributing to carbon neutrality by utilizing solid carbon generated from greenhouse gases, improving internal heating and reducing emissions during the calcination process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025000866_DRAWING_001
    Figure PI2025000866_DRAWING_001
  • Figure PI2025000866_DRAWING_002
    Figure PI2025000866_DRAWING_002
  • Figure PI2025000866_DRAWING_003
    Figure PI2025000866_DRAWING_003
Patent Text Reader

Abstract

Provided is a method of producing iron ore pellets that can obtain high-strength iron ore pellets and contribute to carbon neutrality. The method of producing iron ore pellets includes: a mixing process of mixing iron ore having a total Fe content of 63 mass% or less, solid carbon, binder, and auxiliary material to obtain a mixture; a granulation process of granulating the mixture to obtain green pellets; and a firing process of firing the green pellets to obtain iron ore pellets by burning CH4 gas to heat the green pellets from outside while burning the solid carbon to heat the green pellets from inside. The solid carbon includes carbon produced from one or more gases selected from the group consisting of CO2 gas, CO gas, and CH4 gas. Figure 4A, 4B, 4C
Need to check novelty before this filing date? Find Prior Art

Description

Iron ore pellet manufacturing method

[0001] The present invention relates to a method for producing iron ore pellets.

[0002] Iron ore pellets are made by granulating iron ore powder to have properties (e.g., size, strength, reducibility, etc.) suitable for charging into a blast furnace or a solid reduction furnace. Iron ore pellets are generally produced by the following steps: mixing iron ore powder, a binder, and optional auxiliary materials to obtain a mixture; granulating the mixture to obtain green pellets; and firing the green pellets to obtain iron ore pellets. In this specification, pellets as granulated before firing are referred to as "green pellets." Here, as described in Non-Patent Document 1, it is known that a carbonaceous material such as anthracite is added to the mixture. In the firing step, CH 4 Natural gas, which is primarily composed of gas, is burned to heat the green pellets, but the heat generated by this combustion is transferred from the surface of the green pellets to the inside. This can result in insufficient heating inside the pellets, which can lead to a decrease in strength. Therefore, to compensate for the heat inside the pellets, a carbonaceous material such as anthracite is added to the green pellets, and by burning the carbonaceous material during the firing process, the green pellets are heated from the inside as well.

[0003] Volodymyr Shatokha, “Iron Ores and Iron Oxide Materials”, IntechOpen, published July 11, 2018, p41-59

[0004] Ensuring the strength of green pellets, and therefore the strength of iron ore pellets, is important to prevent the green pellets from pulverizing during handling before being placed in the sintering furnace, and the resulting powder from adhering to the inside of the sintering furnace. Therefore, improvements are always being sought.

[0005] In addition, recent CO 2 In response to public demand for carbon-neutral carbon dioxide emissions reduction, carbon dioxide emissions from iron ore pellets are being reduced during the firing process. 4 Gas and carbonaceous combustion are the main sources of CO 2 It is a cause of CO emissions. 2As a method for producing iron ore pellets without emissions, it has been proposed to use unburned green pellets as iron ore pellets by using organic and inorganic binders. However, unburned green pellets have the following quality problems: When the organic binder is heated to a high temperature, it is carbonized and the CO2 generated by carbonization occurs. 2 Gasification reaction with (C + CO 2 Therefore, it is expected that organic binders cannot function as binders due to the formation of SiO2 (→2CO2), making it difficult to achieve their binding properties when used at high temperatures. Furthermore, silicates (sodium silicate, calcium silicate) are examples of inorganic binders, but the silica itself must be separated as slag from the pig iron or molten steel during either the ironmaking or steelmaking process, requiring excess heat to melt the pig iron. Another issue arises: the inorganic binder is discharged as slag, i.e., as excess material. Furthermore, while the sodium in sodium silicate is solid at low temperatures, it vaporizes below 1000°C, making it undesirable as a substance remaining in a blast furnace. No carbon-neutral technology has been known to date that involves the production of iron ore pellets through a firing process.

[0006] In view of the above problems, the present invention aims to provide a method for producing iron ore pellets that can obtain high-strength iron ore pellets and contributes to carbon neutrality.

[0007] In order to achieve this object, the present inventors have focused on improving the carbonaceous material to be added to the green pellets. 2 gas, CO gas, and CH 4 In this case, the carbon generated from the combustion of the carbon material is CO 2 Although CO is generated, the greenhouse gases are consumed as raw materials for the carbonaceous material, which contributes to carbon neutrality. 2 gas, CO gas, and CH 4It has been found that the strength of iron ore pellets can be unexpectedly increased by using solid carbon (carbonaceous material) containing carbon generated from one or more gases selected from the group consisting of:

[0008] The gist and configuration of the present invention, which has been completed based on the above findings, is as follows.

[0009] [1] A mixing step of mixing iron ore having a total Fe content of 63% by mass or less, solid carbon, a binder, and auxiliary materials to obtain a mixture; a granulation step of granulating the mixture to obtain green pellets; 4 a calcination step of calcining the green pellets by burning a gas to heat the green pellets from the outside and burning the solid carbon to heat the green pellets from the inside, thereby obtaining iron ore pellets, wherein the solid carbon is 2 gas, CO gas, and CH 4 1. A method for producing iron ore pellets, comprising: producing carbon from one or more gases selected from the group consisting of:

[0010] [2] The solid carbon is CO 2 The method for producing iron ore pellets according to [1], wherein the carbon is generated from one or both of gas and CO gas.

[0011] [3] The CH used in the production of the carbon 4 The gas is CO 2 CH generated from one or both of gas and CO 4 The method for producing iron ore pellets according to [1], which contains gas.

[0012] [4] The method for producing iron ore pellets according to any one of [1] to [3], wherein the carbon contains carbon produced using iron as a catalyst.

[0013] [5] The method for producing iron ore pellets according to any one of [1] to [4], wherein the proportion of the carbon in the solid carbon is 10% by mass or more.

[0014] [6] The CH used in the firing step 4 The gas is CO 2 CH generated from one or both of gas and CO 4The method for producing iron ore pellets according to any one of [1] to [5], which contains gas.

[0015] According to the method for producing iron ore pellets of the present invention, high-strength iron ore pellets can be obtained and contribute to carbon neutrality.

[0016] A schematic diagram of a vertical reactor used in a carbon production test using CO gas as a raw material is shown. Photographs of the appearance of (a) sintered ore and (b) solid carbon after the carbon production test are shown. (a) and (b) show the appearance of the sintered ore and solid carbon after the carbon production test. 4 The schematic diagram of the apparatus used in the carbon production tests using gas as a raw material is shown. (a) to (c) show the TEM observation results of the solid carbon obtained in each carbon production test.

[0017] Hereinafter, an embodiment of the method for producing iron ore pellets according to the present invention will be described. Note that the embodiment described below is an example of the present invention, and the configuration of the present invention is not limited to this specific example.

[0018] A method for producing iron ore pellets according to one embodiment of the present invention includes a mixing step of mixing iron ore, solid carbon (carbon material), a binder, and auxiliary materials to obtain a mixture, a granulation step of granulating the mixture to obtain green pellets, and a CH 4 and a calcination step of calcining the green pellets by burning the gas to heat them from the outside and the solid carbon to heat them from the inside, thereby obtaining iron ore pellets. 2 gas, CO gas, and CH 4 The carbon dioxide gas is characterized by containing carbon generated from one or more gases selected from the group consisting of:

[0019] The mixture used to produce iron ore pellets includes iron ore, solid carbon, a binder, and auxiliary materials. In this embodiment, the iron ore contains iron with a total iron content (T.Fe) of 63% by mass or less. Iron ore with a T.Fe content of 63% by mass or less is inexpensive and suitable for production.

[0020] The amount of solid carbon in the iron ore pellets is preferably 0.80% by mass or more relative to the amount of iron ore in the iron ore pellets in order to sufficiently improve the strength of the green pellets. On the other hand, if the amount of solid carbon is excessive, excessive heat occurs in the firing process, causing the iron ore pellets to melt. Therefore, the amount of solid carbon in the iron ore pellets is preferably 2.00% by mass or less relative to the amount of iron ore in the iron ore pellets.

[0021] Solid carbon is CO 2 gas, CO gas, and CH 4 The carbon material (solid carbon) added to the green pellets includes carbon generated from one or more selected from the group consisting of CO 2 gas, CO gas, and CH 4 In this case, carbon generated from one or more gases selected from the group consisting of CO 2 Although CO is generated, the greenhouse gases mentioned above are consumed as raw materials for carbonaceous materials, which contributes to carbon neutrality. 2 gas, CO gas, and CH 4 By adding carbon generated from one or more gases selected from the group consisting of gases to the green pellets, it is possible to obtain the effect of increasing the strength of the green pellets and iron ore pellets.

[0022] The proportion of the carbon in the solid carbon added to the green pellets is preferably 10% by mass or more, more preferably 50% by mass or more, and most preferably 100% by mass. The greater the amount of carbon added, the greater the effect of increasing strength and the greater the contribution to carbon neutrality. Furthermore, when the proportion of the carbon in the solid carbon added to the green pellets is less than 100% by mass, the remainder of the solid carbon may be, for example, anthracite.

[0023] Solid carbon is CO 2 Preferably, the solid carbon comprises carbon generated from one or both of CH 3 gas and CO 2 gas. 4 If carbon generated from the gas is included, the CH 4 The gas is CO2 CH generated from one or both of gas and CO 4 Preferably, the gas contains CO 2 gas, CO gas, or CH 4 The reaction for producing solid carbon from gas is not particularly limited, but examples thereof include the following reactions:

[0024] [Reaction for Producing Solid Carbon from CO Gas] Solid carbon may be produced from CO gas by the Boudouard reaction shown in reaction formula (1). The Boudouard reaction can produce solid carbon from CO gas at temperatures of about 700°C or less: 2CO = C + CO 2 ...(1)

[0025] Solid carbon may be produced from CO gas by the reverse water-gas reaction shown in reaction formula (2). The reverse water-gas reaction can produce solid carbon from CO gas at temperatures of about 650°C or less: CO + H 2 =C+H 2 O... (2)

[0026] CO gas is converted to CH by the methanation reaction shown in reaction formula (3). 4 The gas is generated and converted to CH by the thermal decomposition reaction shown in reaction formula (4). 4 The methanation reaction may produce solid carbon from the gas at temperatures below about 650°C from CO gas to CH 4 Gas can be generated, and the thermal decomposition reaction occurs in air at temperatures above 500°C. 4 It is possible to produce solid carbon from gas. CO + 3H 2 =CH 4 +H 2 O...(3)CH 4 =C+2H 2 ...(4)

[0027] Solid carbon may be produced from CO gas by the decomposition reaction shown in reaction formula (5). The decomposition reaction can produce solid carbon from CO gas under low oxygen partial pressure: 2CO = 2C + O 2 ...(5)

[0028] [CO 2Reaction to generate solid carbon from gas] CO is generated by the reverse water-gasification reaction shown in reaction formula (6). 2 Solid carbon may be produced from the gas. The reverse water-gasification reaction produces CO 2 It is possible to produce solid carbon from the gas. 2 +2H 2 =C+2H 2 O... (6)

[0029] CO is produced by the reverse water gas shift reaction shown in reaction formula (7). 2 The reverse water-gas shift reaction may be carried out at temperatures above about 850° C. to produce CO gas, and solid carbon may be produced from the CO gas by the reverse water-gas shift reaction shown in reaction formula (2). 2 CO gas can be produced from the gas. 2 +H 2 =CO+H 2 O...(7) CO+H 2 =C+H 2 O... (2)

[0030] CO is produced by the methanation reaction shown in reaction formula (8). 2 Gas to CH 4 The gas is generated and converted to CH by the thermal decomposition reaction shown in reaction formula (4). 4 The methanation reaction may produce solid carbon from the gas at temperatures below about 600°C. 2 Gas to CH 4 Gas production is possible. 2 +4H 2 =CH 4 +2H 2 O...(8) CH 4 =C+2H 2 ...(4)

[0031] CO is decomposed by the decomposition reaction shown in reaction formula (9). 2 Solid carbon may be produced from the gas. The decomposition reaction occurs under low oxygen partial pressure. 2 It is possible to produce solid carbon from the gas. 2 = C + O 2 ...(9)

[0032] [CH 4Reaction to generate solid carbon from gas] CH 4 Solid carbon may be produced from the gas. 4 =C+2H 2 ...(4)

[0033] The gas used in the carbon production reaction is CO 2 gas, CO gas, or CH 4 The gas may be any one of the three types of gases alone, or may be a mixture of two or more of the three types of gases. 2 Gas and N 2 A mixed gas containing CO, H, etc. may be used. For example, a mixed gas containing CO, H, etc. may be used. 2 : 19%, N 2 : A 50% mixed gas may be used.

[0034] In addition, CO is used as solid carbon to be added to the green pellets. 2 Carbon generated from CO gas, carbon generated from CO gas, and CH 4 Any one of the carbons produced from the gas may be used alone, or two or more of them may be used in combination.

[0035] The solid carbon is preferably produced using iron as a catalyst. 4 It is known that iron can be used as a catalyst for the thermal decomposition reaction of CH3CO4 shown in reaction formula (4). It is also known that iron oxide can be used as a catalyst for the reverse water gas shift reaction shown in reaction formula (7). Therefore, when producing solid carbon, sintered ore or direct reduced iron may be charged into a furnace, and the iron or iron oxide contained in the sintered ore or direct reduced iron may be used as a catalyst. In addition, the CH3CO4 shown in reaction formula (4) 4 In high temperature reactions such as the thermal decomposition reaction of the above, alumina may be charged into the furnace to maintain the temperature inside the furnace.

[0036] The solid carbon is preferably in a fibrous form, and preferably has an aspect ratio (length / diameter) of 10 or more. When the solid carbon is in a fibrous form, the strength of the iron ore pellets can be suitably obtained. The solid carbon may also be in a spherical form. When the solid carbon is in a spherical form, the binder effect of the fine particles is obtained, and the strength of the iron ore pellets can be suitably obtained. When the solid carbon is in a spherical form, the cumulative particle size D90 is preferably about 10 to 50 μm. CO 2 gas, CO gas, and CH 4 The solid carbon (carbonaceous material) produced from one or more gases selected from the group consisting of gases preferably has a carbon content of 50 mass % or more, and the remainder may contain Fe, FeO, and the like.

[0037] Bentonite is preferred as a binder for iron ore pellets, but any known or arbitrary binder, such as an organic or inorganic binder, that provides a similar effect may also be used. To fully obtain the effect, the binder is preferably contained in an amount of 0.1% by mass or more relative to the amount of iron ore in the iron ore pellets. On the other hand, excessive binder content increases production costs, and the effect decreases with increasing content. Therefore, the binder is preferably contained in an amount of 4.0% by mass or less relative to the amount of iron ore in the iron ore pellets.

[0038] Iron ore pellets are used with quicklime and limestone (CaCO 3 ), dolomite (CaMg(CO 3 ) 2 The basicity of the iron ore pellets is adjusted by the auxiliary raw material. The basicity of the iron ore pellets is determined by the CaO / SiO 2 The basicity of the iron ore pellets is preferably 0.01 to 1.5.

[0039] The iron ore pellets are produced by a general crushing, mixing, granulation, and firing process. A general crusher such as a ball mill may be used for the crushing process. A general concrete mixer or a high-speed agitating mixer may be used for the mixing process. A general pelletizer or a drum mixer may be used for the granulation process.

[0040] The Blaine index of the crushed iron ore is 2000 to 4000 cm 2 / g. The Blaine index is measured using a Blaine air permeability tester specified in JIS R 5201:2015 and represents the specific surface area of ​​the powder. In the pellet manufacturing process, the Blaine index is used as a control index for ore particle size, and a higher value indicates finer powder.

[0041] The granulated green pellets preferably have a particle size of about 9.5 to 12 mm. If the particle size of the green pellets is less than 9.5 mm, the gas permeability will be deteriorated when the pellets are filled into a blast furnace as fired pellets. If the particle size of the green pellets exceeds 12 mm, the reducibility will be reduced.

[0042] The firing step may be performed using a general rotary kiln or electric furnace. 4 The green pellets are heated from the inside by burning solid carbon while the gas is burned to heat the green pellets from the outside. The firing conditions are preferably a furnace temperature of 1200 to 1350°C and a holding time at the furnace temperature of 5 to 30 minutes.

[0043] CH used in the above firing process 4 From a carbon-neutral perspective, gas is CO 2 CH generated from one or both of gas and CO 4 Preferably, the gas contains CH 4 There are no particular limitations on the method for producing the gas, but it may be produced by, for example, the methanation reaction shown in reaction formulas (3) and (8). 2 +4H 2 =CH 4 +2H 2 O...(8) CO+3H 2 =CH 4 +H 2 O... (3)

[0044] Iron ore, binder, and auxiliary materials were prepared as raw materials for iron ore pellets. Table 1 shows the composition of the iron ore used. The iron ore was dried at 105°C for 24 hours and then crushed to obtain a pellet with a Blaine index of 2560 cm2 The iron ore powder was obtained with a particle size of 95 μm and a volume average particle size of 95 μm. Bentonite was used as a binder and limestone was used as an auxiliary material.

[0045]

[0046] The solid carbon is then mixed with CO gas or CH 4 The details are described below. 2 Gas, CH 4 Anthracite was prepared as solid carbon that was not produced from any of the gases. The anthracite was in the form of particles with a particle size of 1 mm or less and a carbon content of 85 mass %.

[0047] [Carbon Generation Test from CO Gas] Carbon was generated from CO gas using a vertical reactor. Figure 1 shows a schematic diagram of the vertical reactor. An alumina support 12, alumina balls 14, and sintered ore 16 were loaded into a furnace core tube 10 with an inner diameter of 80 mm in the order shown. A gas inlet tube 18 was introduced containing CO: 31%, H: 10% by volume, and CO: 10% by volume. 2 : 19%, N 2 A 50% CO mixed gas (hereinafter referred to as CO mixed gas) was passed through the sintered ore at 550°C or 800°C (heated by heater 20, measured by thermocouple 22) for 3 hours at a gas flow rate of 17 L / min to generate solid carbon. The iron contained in the sintered ore was used as a catalyst for carbon generation.

[0048] The reduced sample was sieved through a 0.125 mm sieve to separate it into sintered ore and solid carbon. The solid carbon accounted for 1.5 wt% of the reduced sample. Figure 2 shows photographs of (a) sintered ore and (b) solid carbon after a carbon generation test from CO mixed gas at 800°C. The solid carbon was a fine powder, and the cumulative particle sizes were D10: 2.1 μm, D50: 6.61 μm, and D90: 14.8 μm. That is, more than 90% of the cumulative number of powder particles had particle sizes of 14.8 μm or less. Table 2 shows the results of the component analysis of the solid carbon.

[0049]

[0050] [CH 4 Carbon generation test from gas] Using the apparatus shown in Figures 3(a) and 3(b),4 First, 30 g (approximately 20 to 30 pieces) of direct reduced iron (DRI) 32, which was prepared by reducing iron ore pellets with a diameter of 10 mm, was charged into an electric furnace 30 shown in FIG. 3(a), and 100% CH 4 The gas was introduced from the gas inlet 34 at 900° C. for 1 hour at a gas flow rate of 1.0 L / min to generate solid carbon. Next, 500 g of φ6 mm alumina balls 38 were placed in a furnace core tube (alumina tube) 36 with a diameter of 80 mm shown in FIG. 3( b), and a soaking zone with a height of about 50 mm was formed. 4 Gas was introduced from gas inlet 40 at a gas temperature of 1400 (±10)°C (heated by heater 42) for 1 hour at a gas flow rate of 1.0 L / min to produce solid carbon. The post-reduced samples obtained in each test were sieved through a 0.125 mm sieve to separate the DRI or alumina balls from the solid carbon.

[0051] Table 3 shows the morphology and carbon content of the solid carbon and anthracite produced under each condition. Figure 4 shows (a) solid carbon produced from CO mixed gas at 550 °C, (b) solid carbon produced from CH mixed gas at 900 °C, and (c) solid carbon produced from CO mixed gas at 900 °C. 4 (c) Solid carbon formed from gases, (d) CH 4 The results of TEM observation of solid carbon produced from gas are shown below. The solid carbon obtained in the reaction at 900°C or below was fibrous, with an aspect ratio of 10 or more. The solid carbon obtained in the reaction at 1400°C was spherical, with a particle size of about 0.2 to 2.0 μm. This is because at 1400°C, the high temperature makes the reactivity high and carbon is produced in the gas phase as the main reaction, but at 900°C or below, CH 4 This is thought to be because the thermal decomposition reaction of the gas is difficult to proceed, and the iron-catalyzed production reaction occurs as the main reaction.

[0052]

[0053] 1000 g of iron ore powder was prepared, and various solid carbons were added in the amounts shown in Table 4 relative to the amount of iron ore, along with 1% by mass of bentonite relative to the amount of iron ore. Furthermore, limestone was added to the iron ore powder in an amount set so that the basicity of the iron ore pellets was 0.1, and the mixture was mixed for 3 minutes at 20 rpm using a concrete mixer. The amount of solid carbon in Nos. 2 to 7 was set to be the same as the amount of carbon contained in the anthracite in No. 1. The percentage of carbon contained in the anthracite replaced by the carbon contained in solid carbons 1 to 4 is shown in the "Carbon Replacement Ratio" column in Table 4. Next, the mixed raw materials were placed in a 1.2 mφ pelletizer and granulated while adding water. Pellets with particle sizes of 9.5 to 12 mm were collected and further rolled in the pelletizer for 10 minutes to obtain green pellets.

[0054]

[0055] [Measurement of Drop Strength of Green Pellets] In each of the invention examples and comparative examples, drop strength measurements were performed on 10 green pellets, simulating transportation, charging, and the like during actual operation. The green pellets were repeatedly dropped from a height of 50 cm, and the test was stopped when cracks or breakage were observed in the green pellets. The number of times before the test was stopped (i.e., the number of times when cracks or breakage were observed) was taken as the drop strength, and the average drop strength of the 10 pellets is shown in Table 3.

[0056] Green pellets not used in the above test were charged into an electric furnace and fired. In an air atmosphere, the temperature was increased at 10°C / min, held at 1300°C for 10 minutes, and then decreased at 10°C / min. After the temperature decrease, the sample was taken out to obtain iron ore pellets. In the firing process in actual operation, CH 4 The green pellets are heated by burning natural gas, which is primarily composed of coal, but in this test, an electric furnace was used to simulate this heating.

[0057] [Measurement of crushing strength of iron ore pellets] In each of the invention examples and comparative examples, the crushing strength (kgf) of 10 iron ore pellets was measured using an autograph. The displacement rate was 2 mm / min, and the average value for the 10 pellets is shown in Table 3.

[0058] From Table 4, it can be seen that the invention examples are superior to the comparative examples in both the drop strength of the green pellets and the crushing strength of the iron ore pellets. 2 gas, CO gas, and CH 4 By replacing the carbon with carbon generated from one or more selected from the group consisting of CO 2 Furthermore, assuming that the solid carbon substitution rate is 100 mass%, 2 CH produced from one or both of CO gas and CO 4 It is clear that carbon neutrality can be achieved in the production of iron ore pellets by using gas in the carbon generation and calcination process.

[0059] According to the present invention, it is possible to provide a method for producing iron ore pellets that can obtain high-strength iron ore pellets and contribute to carbon neutrality.

[0060] REFERENCE SIGNS LIST 10 furnace core tube 12 alumina support 14 alumina balls 16 sintered ore 18 gas inlet tube 20 heater 22 thermocouple 30 electric furnace 32 DRI reduced from iron ore pellets 34 gas inlet 36 furnace core tube 38 alumina balls 40 gas inlet 42 heater

Claims

1. A mixing step of mixing iron ore having a total Fe content of 63% by mass or less, solid carbon, a binder, and auxiliary materials to obtain a mixture; a granulation step of granulating the mixture to obtain green pellets; 4 a calcination step of calcining the green pellets by burning a gas to heat the green pellets from the outside and burning the solid carbon to heat the green pellets from the inside, thereby obtaining iron ore pellets, wherein the solid carbon is 2 gas, CO gas, and CH 4 1. A method for producing iron ore pellets, comprising: producing carbon from one or more gases selected from the group consisting of:

2. The solid carbon is CO 2 2. The method for producing iron ore pellets according to claim 1, wherein the carbon is produced from one or both of gas and CO gas.

3. The CH used in the production of the carbon 4 The gas is CO 2 CH generated from one or both of gas and CO 4 The method for producing iron ore pellets according to claim 1 , further comprising a gas.

4. The method for producing iron ore pellets according to any one of claims 1 to 3, wherein the carbon comprises carbon produced using iron as a catalyst.

5. A method for producing iron ore pellets according to any one of claims 1 to 4, wherein the proportion of carbon in the solid carbon is 10 mass% or more.

6. The CH used in the firing step 4 The gas is CO 2 CH generated from one or both of gas and CO 4 The method for producing iron ore pellets according to any one of claims 1 to 5, further comprising a gas.