Laminated core and method for manufacturing laminated core

MYPI2025000886A0Undetermined Publication Date: 2024-03-08NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025000886
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-08
Filing Date
2023-09-08
Publication Date
2024-03-08

AI Technical Summary

Technical Problem

Existing laminated core manufacturing techniques face challenges in achieving high production efficiency due to iron loss from conduction in fixed parts and the need for large-scale cooling mechanisms, which hinder energy efficiency and productivity.

Method used

A laminated core with magnetic steel plates and adhesive insulating coatings alternately laminated, achieving a tensile adhesive strength of 20 MPa or more at 25°C, manufactured using a method involving low-pressure adhesion and controlled temperature increase, allowing for rapid production without high-temperature heating and cooling processes.

Benefits of technology

The method enables the production of high-strength laminated cores with improved energy efficiency and reduced equipment size, enhancing productivity by ensuring necessary adhesive strength without extensive heating or cooling requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025000886_DRAWING_001
    Figure PI2025000886_DRAWING_001
  • Figure PI2025000886_DRAWING_002
    Figure PI2025000886_DRAWING_002
  • Figure PI2025000886_DRAWING_003
    Figure PI2025000886_DRAWING_003
Patent Text Reader

Abstract

ABSTRACT LAMINATED CORE AND METHOD FOR MANUFACTURING LAMINATED CORE A laminated core (10) includes electrical steel sheets (1) and adhesive insulating coatings (2) alternately stacked and has a lamination direction (D) tensile strength of adhesive bond of 20 MPa or more measured under a 25°C condition after a complete reaction of each adhesive insulating coating (2). A method for manufacturing a laminated core (10) includes a punching step of punching an electrical steel sheet coated with an adhesive insulating coating (2) to form an electrical steel sheet (1), an accommodating step of stacking and accommodating electrical steel sheets (1) in a die after the punching step, a low-pressure bonding step of heating the electrical steel sheets (1) in the die at a surface temperature of 60°C or more and 200°C or less and bonding the adjacent electrical steel sheets (1) by pressurization at 3.0 MPa or less to form a laminated core (10), and a take-out step of taking out the laminated core (10) from the die after the low-pressure bonding step. FIG. 3
Need to check novelty before this filing date? Find Prior Art

Description

Laminated core and method of manufacturing the laminated core

[0001] The present invention relates to a laminated core and a method for manufacturing a laminated core. This application claims priority to Japanese Patent Application No. 2022-143134, filed on September 8, 2022, the contents of which are incorporated herein by reference.

[0002] In recent years, CO2 reduction has become a global trend. 2 The trend towards CO 2 The application of zero-emission motors (rotating electric motors, electric motors) is expanding in various fields, including automobiles. This trend is driving demand for motors with greater power savings and higher output than ever before. Known lamination manufacturing techniques for laminated cores used in motors include crimping and laser bonding. Laminated cores manufactured using these lamination manufacturing techniques suffer from iron loss due to conduction through the bonding points, which is one of the factors hindering power savings and higher output. Recently, development of adhesive-based laminated core manufacturing techniques has focused on reducing iron loss. Adhesive-based laminated core manufacturing techniques include a method in which an adhesive is applied to electromagnetic steel sheets before they are punched, and a method in which the electromagnetic steel sheets are punched and then an adhesive is applied to the electromagnetic steel sheets. The assembly process of stacking the adhesive-coated electromagnetic steel sheets is performed either inside or outside the mold. The following prior literature describes these techniques:

[0003] Japanese Patent Publication No. 2010-274625 Japanese Patent Publication No. 2009-297758 Japanese Patent Publication No. 2022-000888 Japanese Patent Publication No. 2021-129453

[0004] In a technique for laminating adhesive-coated electromagnetic steel sheets outside a mold (see Patent Document 3 or Patent Document 4), adjacent electromagnetic steel sheets are bonded to each other by applying high pressure to a plurality of electromagnetic steel sheets housed inside a dedicated jig, temporarily fixing the sheets, and then removing the laminate from the dedicated jig. The laminate, or the laminate secured in the dedicated jig, is heated at high temperature. As described above, the method for manufacturing a laminate outside a mold involves steps of securing and removing the sheets using a dedicated jig, making automation difficult, which reduces productivity. Unlike the technique for laminating outside a mold, the technique for laminating adhesive-coated electromagnetic steel sheets inside a mold (see Patent Document 1 or Patent Document 2) does not include a step of removing the laminate, making automation relatively easy and resulting in high productivity. However, after forming a laminate by high-temperature bonding, if the laminate is not rapidly cooled before being transported to the next process, it takes a long time, approximately 3 to 4 hours, for the temperature of the laminate to drop to a temperature suitable for transport. Furthermore, if rapid cooling is required before transporting the laminate to the next process, a large-scale cooling mechanism for rapid cooling is required depending on the size of the laminate, which increases the overall size of the manufacturing equipment, including the cooling mechanism. As described above, the method of manufacturing a laminate in a mold requires a long time for manufacturing or requires a large-scale manufacturing device, making it difficult to scale up production, which is a factor in reducing productivity. In view of the problems of the above-mentioned known techniques, the present application provides a laminated core and a method of manufacturing a laminated core that can be manufactured with high production efficiency.

[0005] The gist of the present invention is as follows.

[0006] (1) A laminated core according to one aspect of the present invention has magnetic steel sheets and adhesive insulating coatings laminated alternately, and after complete reaction of the adhesive insulating coatings, the tensile adhesive strength in the lamination direction measured at 25°C is 20 MPa or more. (2) In the above (1), the magnetic steel sheet of the uppermost layer may have a protrusion protruding in the lamination direction. (3) A method for manufacturing a laminated core according to one aspect of the present invention is a method for manufacturing a laminated core formed by stacking multiple magnetic steel sheets, and includes: a punching step of punching an magnetic steel strip coated with an adhesive insulating coating to form the magnetic steel sheets; a loading step of stacking the magnetic steel sheets and loading them into a mold after the punching step; a low-pressure bonding step of heating the magnetic steel sheets in the mold to a surface temperature of 60°C or more and 200°C or less while applying a pressure of 3.0 MPa or less to bond adjacent magnetic steel sheets together to form a laminated core; and a removal step of removing the laminated core from the mold after the low-pressure bonding step. (4) In the above (3), the low-pressure bonding step may include an adhesion promotion step of heating the laminated core to a temperature of 100°C or higher and 160°C or lower at a heating rate of 0.5°C / s or higher and 10.0°C / s or lower, and maintaining the temperature for 20 seconds or higher and 120 seconds or lower. (5) In the above (3) or (4), after the removal step, a reheating step of heating the laminated core to a temperature of 160°C or higher and 250°C or lower may be included. (6) In any of the above (3) to (5), the low-pressure bonding step may include applying a pressure of 0.1 MPa or higher to the electromagnetic steel sheets in the mold.

[0007] According to the present invention, it is possible to provide a laminated core that can be manufactured with high production efficiency and a method for manufacturing a laminated core.

[0008] Fig. 3 is a perspective view of a laminated core. Fig. 4 is a plan view of the laminated core. Fig. 5 is a cross-sectional view taken along the arrow A in Fig. 2. Fig. 6 is a table showing the relationship between test specimens, test conditions, and test results for a tensile adhesion test.

[0009] To improve productivity of laminated cores, a manufacturing technique in which adhesive-coated magnetic steel sheets are laminated in a mold is suitable. However, this manufacturing technique involves a process of heating the laminate (laminated core) at high temperatures and a process of cooling it, which necessitates the need for larger manufacturing facilities.

[0010] The reason for heating the laminate at a high temperature is to obtain the necessary strength using a thermosetting adhesive.

[0011] In order to reduce the size or simplify the manufacturing equipment, it is effective to use an adhesive that has high strength when the laminate is completed without heating the laminate to a high temperature.

[0012] Conventional knowledge has led to the design of laminate manufacturing technologies by lowering the glass transition temperature (Tg) of the adhesive used in the adhesive coating of magnetic steel sheets (the temperature at which the adhesive hardens from a flexible state) (low Tg) to accelerate the adhesive's curing reaction even at low temperatures and complete curing (development of the desired strength) early. However, in the case of manufacturing technologies that manufacture laminates by laminating magnetic steel sheets using an adhesive coating, there has been a concern that the adhesive's curing reaction may be accelerated during transportation and storage of the manufactured laminate, resulting in unintended adhesion between materials, known as blocking. Therefore, conventional laminate manufacturing technologies require temperature control and stacking volume control, which ultimately hinders improvements in production efficiency.

[0013] To manufacture a laminate at low temperatures without lowering the Tg, a tensile test was conducted in which a tensile force was applied to the completed laminate in the lamination direction of the steel sheets. The tensile adhesive strength in the lamination direction (hereinafter, the tensile adhesive strength in the lamination direction may be referred to as lamination direction tensile strength) required for a laminate used in a motor was examined, as well as the relationship between the temperature of the adhesive and the reaction progress and strength. The lamination direction tensile strength is an evaluation index uniquely defined by the present application and is the adhesive strength of the entire laminate in the lamination direction (the direction perpendicular to the adhesive bonding surfaces of the laminate sheets). Specifically, the lamination direction tensile strength is the value obtained by dividing the load at which the laminate breaks when a tensile load is applied to the laminate in the lamination direction by the cross-sectional area of ​​the laminate perpendicular to the lamination direction D (the adhesive area on one of the plate surfaces of the plate sheets constituting the laminate). On the other hand, strengths measured by conventional methods include the tensile bond strength of JIS K 6849:1994 and the tensile shear bond strength of JIS K 6850:1999, but these are the bond strength of the adhesive alone. Furthermore, the tensile shear bond strength is the bond strength when a shear stress parallel to the adhesive surface is applied. Here, we explain the necessity of the lamination direction tensile strength specified in this disclosure and its differences from conventional methods. First, resins used as adhesives have phase directionality (orientation, anisotropy). Therefore, evaluation in the required direction is necessary. However, shear tensile strength, which evaluates tensile strength in a direction parallel to the adhesive surface, is insufficient when tensile strength in the lamination direction is required, as in this case. Furthermore, when testing test specimens containing resin, the bonding and compatibility at the interface between the resin and the steel sheet are important, and the tensile bond strength of JIS K 6849:1994 is insufficient because it does not allow for evaluation of the strength at the interface. Thus, lamination direction tensile strength and conventional strength represent different strengths. Using the tensile strength in the lamination direction that we discovered this time, we were able to measure the adhesive strength of the entire laminate in the lamination direction, as follows. As a result of investigating the relationship between the tensile strength in the lamination direction and the temperature of the adhesive and the progress of the reaction and strength, we obtained the following findings: 1) The tensile strength in the lamination direction required for a laminate used in a motor varies depending on the application of the motor.Even for motors used in electric vehicles (EVs), drones, or vacuum cleaners, the laminates used in motors operated at high speeds require a high tensile strength in the lamination direction of about 1 MPa, which is higher than the 0.5 MPa that is the bonding strength of typical laminates bonded by caulking. 2) As the temperature rises, the adhesive progresses and hardens from a soft state (1), through a reaction-promoting state (2), and then to a reaction-end state (3) (adhesive hardening mechanism).

[0014] In some cases, emphasis is placed on the strength exhibited at the end of the reaction (3), and adhesives are designed based on this strength. However, if an adhesive can ensure sufficient strength in the reaction promotion process (2) without waiting for the end of the reaction (3), then the required strength can be ensured without subsequent heating.

[0015] Based on this technical concept, it was discovered that by using an adhesive having a lamination direction tensile strength of 20 MPa or more at the end of the reaction, which is about 20 times the lamination direction tensile strength of approximately 1 MPa required for laminates for general motors, it is possible to ensure sufficient strength in the reaction promotion state (2) without waiting for the reaction completion state (3).

[0016] <<First embodiment>> A laminated core 10 according to an embodiment will be described. Fig. 1 is a perspective view of the laminated core 10. Fig. 2 is a plan view of the laminated core 10. Fig. 3 is a cross-sectional view taken along the arrow A in Fig. 2 .

[0017] As shown in FIGS. 1 to 3 , the laminated core 10 is formed by alternately stacking magnetic steel sheets 1 and adhesive insulating coatings 2 in the stacking direction D. After the adhesive insulating coatings 2 have completely reacted, the tensile strength in the stacking direction D measured at 25°C is 20 MPa or more. The tensile strength in the stacking direction is preferably 40 MPa or more. Here, complete reaction refers to a 100% cure rate, i.e., a state in which no peaks due to heat generation appear in a differential scanning calorimetry (DSC) curve. As described above, the tensile strength in the stacking direction is calculated by dividing the load at which the laminate breaks when a tensile load is applied to the laminate in the stacking direction by the cross-sectional area of ​​the laminate perpendicular to the stacking direction D (the adhesive area on one of the plate surfaces of the plate constituting the laminate). For example, the maximum tensile load may be calculated by applying a tensile load in the lamination direction D to a test specimen with a uniform cross section cut out from a laminated core 10 (e.g., a cubic test specimen measuring 45.0 mm long, 3.6 mm wide, and 12.25 mm long along the lamination direction D) as shown by the dashed line in FIG. 1 using a tensile tester. The maximum tensile load until fracture occurs may be divided by the cross-sectional area of ​​the test specimen perpendicular to the lamination direction D. As shown in FIG. 1 , the test specimen is a laminate formed by stacking magnetic steel sheets 1 and adhesive insulating coatings 2. The magnetic steel sheets constituting the test specimen are fully bonded by the adhesive insulating coating. The fracture refers to the fracture of at least one of the adhesive insulating coatings formed between the plates constituting the laminate. The tensile tester used is a tensile tester capable of tensile testing No. 5 test specimens as described in JIZ Z 2241:2022. The tensile tester used is, for example, a fully automatic tensile tester with a capacity of 100 kN. The dimensions of the test specimen are not limited to those described above, and the test specimen may be cut out from the laminated core 10 so as to include two or more layers of adhesive insulating coating 2 (three or more layers of the adherend magnetic steel sheet 1). There are also no particular restrictions on the lamination direction of the test specimen and the cut-out position on a plane perpendicular to the lamination direction. However, the test specimen is cut out from the laminated core 10 so as not to include the protrusions 3.In this case, it is assumed that three or more electromagnetic steel sheets 1 are laminated, due to the ease of conducting tests and the frequency of lamination. This allows the laminated core 10 for a motor to achieve the required adhesive strength (e.g., 1 MPa) even at relatively low temperatures (60°C or higher and 200°C or lower). Therefore, a high-strength laminated core 10 can be manufactured without further heating after bonding the electromagnetic steel sheets 1 together to form a laminate (laminated core). This allows the laminated core 10 to be removed from the manufacturing equipment at a low temperature, simplifying the mechanisms for high-temperature heating and cooling in the manufacturing equipment, thereby enabling the manufacturing equipment for the laminated core 10 to be made more compact. Therefore, a laminated core 10 and a manufacturing method for the laminated core 10 that can be manufactured with high production efficiency can be provided.

[0018] The electromagnetic steel sheet 1 is, for example, an electromagnetic steel sheet 1 suitable for a high-efficiency motor. The electromagnetic steel sheet 1 may be, for example, a non-oriented electromagnetic steel sheet (for example, proprietary standard 25HX1300) having a yield strength of 394 MPa, low iron loss (13.0 W / kg or less), high magnetic flux density, and a thickness of 0.25 mm.

[0019] The adhesive insulating coating 2 may be an adhesive that is coated on the magnetic steel sheet 1 in advance before the punching step described below.

[0020] The adhesive insulating coating 2 may be coated on the surface of the electrical steel sheet to a thickness of, for example, 3 μm. The adhesive insulating coating 2 may be an adhesive resin containing a thermosetting resin as shown below. The compounding ratio of the thermosetting resin, organic components other than the thermosetting resin, inorganic components, etc. shown below is adjusted so that after complete reaction, the tensile strength in the lamination direction when measured at 25°C is 20 MPa or more.

[0021] <Thermosetting Resin> Specific examples of thermosetting resins include crosslinked resins such as epoxy resins, thermosetting acrylic resins, urethane resins, unsaturated polyester resins, phenolic resins, melamine resins, urea resins, and thermosetting polyimide resins. In the present invention, these resins can be used alone or in combination of two or more.

[0022] (Epoxy Resin) An epoxy resin is a resin containing two or more epoxy groups, which are crosslinked by an appropriate curing agent to form a three-dimensional resin and harden. Examples of epoxy group-containing resins include bisphenol-based (bisphenol A, bisphenol F, bisphenol AD), naphthalene-based, and cardo-skeleton epoxy resins.

[0023] (Thermosetting Acrylic Resin) Examples of thermosetting acrylic resins include copolymers of acrylic acid esters or methacrylic acid esters with acrylic monomers having reactive functional groups such as hydroxyl groups, amino groups, N-methylol, N-alkoxymethylcarboxylate, allyl groups, or epoxy groups. Specific examples include copolymers of methyl acrylate or methyl methacrylate with one or more acrylic monomers having reactive functional groups such as acrylic acid, methacrylic acid, acrylamide, N-methylolacrylamide, N-(methoxymethyl)acrylamide, allyl methacrylate, acrylic glycidyl ether, and glycidyl methacrylate. Thermosetting acrylic resins crosslink by utilizing the self-reactivity of the reactive functional groups, or crosslink and harden by the reaction of the reactive functional groups with curing agents such as amines.

[0024] (Urethane Resin) Examples of urethane resins include resins composed of residues of polyfunctional isocyanate compounds and hydroxyl group-containing compounds. Specific examples include resins composed of aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane isocyanate, or polymethylene polyphenylene polyisocyanate, aliphatic polyisocyanates such as hexamethylene diisocyanate or xylene isocyanate, or mixtures thereof, and residues of hydroxyl group-containing compounds such as polyether polyol, polyester polyol, polyacrylate polyol, or polycarbonate polyol. Urethane resins crosslink and harden by reaction with curing agents such as isocyanate-based curing agents or polyol-based curing agents.

[0025] (Unsaturated polyester resin) Examples of unsaturated polyester resins include dehydration condensates of unsaturated dibasic acids such as maleic anhydride, fumaric acid, or itaconic acid, or compounds in which a portion of the unsaturated dibasic acid is substituted with a saturated dibasic acid such as phthalic anhydride, isophthalic acid, or terephthalic acid, and dihydric alcohols such as ethylene glycol, diethylene glycol, or propylene glycol, or compounds in which a portion of the unsaturated polyester resin is substituted with a polyhydric alcohol such as glycerin or pentaerythritol. The unsaturated polyester resin crosslinks and hardens by reaction with a curing agent such as an isocyanate-based curing agent.

[0026] (Other Thermosetting Resins) Phenolic resins include resins containing two or more phenols (such as phenol and cresol). Examples include resins composed of residues of phenols and formaldehydes or aldehydes. Specific examples of phenolic resins include phenol novolac resins, cresol novolac resins, cresol naphthol formaldehyde polycondensates, and triphenylmethane-type polyfunctional phenyl resins. Examples of phenolic resins include phenol aralkyl resins. Examples of melamine resins include alkyl etherified melamine resins and their substituted derivatives. Examples of urea resins include ethylene urea resins. Examples of thermosetting polyimide resins include resins composed of residues of polycarboxylic dianhydrides and diamine compounds. Specific examples include thermosetting polyimide resins such as maleimide polymers, bismaleimide polymers, aminobismaleimide polymers, and bismaleimide triazine polymers. These resins also cure through a crosslinking reaction with a curing agent.

[0027] (Preferred Examples of Thermosetting Resins) Among the above-mentioned thermosetting resins, it is preferred that the thermosetting resin contains one or more selected from the group consisting of epoxy resins, acrylic resins, urethane resins, and unsaturated polyester resins, as these resins have many options for achieving a glass transition temperature Tg of 30° C. or higher, exhibit a fast curing reaction at high temperatures, and are easy to prepare a dispersed state of the curing agent. Among these, it is most preferred that the thermosetting resin contains an epoxy resin, from the viewpoints of economy, versatility, and ease of handling.

[0028] <Suitable Examples of Adhesive Resins> One suitable adhesive resin is one in which the thermosetting resin contains one or more thermosetting resins selected from the group consisting of epoxy resins, acrylic resins, urethane resins, and unsaturated polyester resins, and the total content (total mass of thermosetting resins / mass of adhesive resins x 100 (%)) is 20 mass% or more. If the adhesive resin contains 20 mass% or more of these thermosetting resins, the properties of these thermosetting resins can be fully utilized. Among these, an adhesive resin containing 50 mass% or more of epoxy resin is most preferred in terms of economy, versatility, and ease of handling.

[0029] The adhesive resin may contain a thermosetting resin, and may also contain organic or inorganic components other than the thermosetting resin, such as a thermoplastic resin, an impact modifier such as core-shell rubber or natural rubber, a curing accelerator such as dimethylurea, boron trifluoride, or triphenylphosphine, a known epoxy resin modifier, a reaction control agent (such as a catalyst), a surfactant, a rust inhibitor, a lubricant, an antioxidant, an antifoaming agent, or a color pigment.

[0030] <Examples of Curing Agents> Specific examples of curing agents include amine-based, amide-based, imidazole-based, acid anhydride-based, phenol-based, catalyst-based, etc. In the present invention, for example, it is possible to select a crystalline curing agent that crystallizes at room temperature from the following specific examples, either alone or in combination of two or more types.

[0031] (Amine-Based Curing Agent) Examples of the amine-based curing agent include, but are not limited to, aliphatic amines, aromatic amines, and guanidine compounds.

[0032] [Aliphatic Amines] Examples of aliphatic amines include, but are not limited to, diethylenetriamine, triethylenetetraamine, tetraethylenepentamine, m-xylenediamine, trimethylhexamethylenediamine, 2-methylpentamethylenediamine, isophoronediamine, 1,3-bisaminomethylcyclohexane, bis(4-aminocyclohexyl)methane, norbornenediamine, 1,2-diaminocyclohexane, benzoylamine, methylcyclohexylamine, and diazabicycloundecene.

[0033] [Aromatic Amine] Examples of aromatic amines include, but are not limited to, diaminodiphenylmethane, m-phenylenediamine, diaminodiphenylsulfone (DDS), diethyltoluenediamine, trimethylenebis(4-aminobenzoate), polytetramethyleneoxide-di-p-aminobenzoate, methylaniline, and dimethylaniline.

[0034] [Guanidine Compound] Examples of guanidine compounds include, but are not limited to, dicyandiamide (DICY, cyanoguanidine) and its derivatives, methylguanidine, ethylguanidine, propylguanidine, butylguanidine, dimethylguanidine, trimethylguanidine, phenylguanidine, diphenylguanidine, and toluylguanidine.

[0035] (Amide-Based Curing Agent) The amide-based curing agent is not limited to the following, but examples thereof include an amine-based curing agent to which an acid anhydride is added, and a hydrazide-based compound.

[0036] [Hydrazide Compounds] Examples of hydrazide compounds include, but are not limited to, succinic acid dihydrazide, adipic acid dihydrazide, phthalic acid dihydrazide, isophthalic acid dihydrazide, terephthalic acid dihydrazide, p-oxybenzoic acid hydrazide, salicylic acid hydrazide, phenylaminopropionic acid hydrazide, and maleic acid dihydrazide.

[0037] (Imidazole-Based Curing Agent) Examples of imidazole-based curing agents include imidazole-isocyanuric acid compounds, diamino-6-[2-(2-methyl-1-imidazolyl)ethyl]-1,3,5-triazine (2MZ-AZINE), 1-cyanoethyl-2-ethyl-4-methylimidazole (CEMI), 2-ethyl-4-methylimidazole, and 2-undecylimidazole (C11Z).

[0038] (Acid Anhydride Curing Agent) Examples of acid anhydride curing agents include, but are not limited to, phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, and methylhexahydrophthalic anhydride.

[0039] (Phenol-Based Curing Agent) Examples of the phenol-based curing agent include, but are not limited to, phenol novolac resin, cresol novolac resin, phenol aralkyl resin, cresol aralkyl resin, naphthol aralkyl resin, biphenyl-modified phenol resin, biphenyl-modified phenol aralkyl resin, dicyclopentadiene-modified phenol resin, aminotriazine-modified phenol resin, naphthol novolac resin, naphthol-phenol co-condensed novolac resin, naphthol-cresol co-condensed novolac resin, and allyl acrylic phenol resin.

[0040] (Catalytic Curing Agent) Examples of catalytic curing agents include, but are not limited to, cationic thermosetting catalysts, BF3-amine complexes, and 1,8-diazabicyclo[5.4.0]undec-7-ene.

[0041] The curing agent preferably contains one or more crystalline curing agents selected from the group consisting of amine-based curing agents, amide-based curing agents, and imidazole-based curing agents, because this allows for a fast curing reaction rate of the adhesive resin composition coating during thermocompression bonding, thereby enabling relatively easy short-term curing of the adhesive resin composition coating. The use of such curing agents allows for a difference between the storage temperature of the adhesive resin composition-coated electrical steel sheet and the heating temperature during thermocompression bonding, making it easier to control the temperature rise rate during thermocompression bonding. From the perspective of ease of handling and versatility, the curing agent most preferably contains one or more selected from the group consisting of dicyandiamide (DICY), diaminodiphenyl sulfone (DDS), and diamino-6-[2-(2-methyl-1-imidazolyl)ethyl]-1,3,5-triazine (2MZ-AZINE).

[0042] The laminated core 10 is formed by alternately laminating electromagnetic steel sheets 1 and adhesive insulating coatings 2. The laminated core 10 is made up of, for example, 600 electromagnetic steel sheets 1 and has a total thickness of approximately 150 mm.

[0043] Here, the electromagnetic steel sheet 1 in the uppermost layer preferably has a protrusion 3 protruding in the stacking direction D. As a result, after the first laminated core 10 is formed in a mold with the stacking direction D aligned vertically, if the electromagnetic steel sheet 1 in the lowermost layer of the second laminated core 10 formed on the first laminated core 10 in the same mold is placed in direct contact with the electromagnetic steel sheet 1 in the uppermost layer of the first laminated core 10 and then pressed vertically, the lower surface of the electromagnetic steel sheet 1 in the lowermost layer of the second laminated core 10 will only come into contact with the upper end of the protrusion 3 formed on the upper surface of the electromagnetic steel sheet 1 in the uppermost layer of the first laminated core 10. Therefore, the adhesive force at the contact area between the upper end of the protrusion 3 and the lower surface of the electromagnetic steel sheet 1 in the lowermost layer of the second laminated core 10 can be made smaller than the weight of the first laminated core 10, which is the lowest. Therefore, when the laminated cores 10 are mass-produced one after another in the mold, the first laminated core 10 falls naturally due to the action of gravity, so that the first laminated core 10 can be separated from the second laminated core 10 and easily removed from the mold alone. This allows the laminated cores 10 to be manufactured with high production efficiency.

[0044] The conditions for allowing the first laminated core 10 to fall naturally under the action of gravity and separate from the second laminated core 10 as described above are as follows: The number Q of protrusions 3 formed on the upper surface of the uppermost electromagnetic steel sheet 1 and the contact area A (m 2 ) and the tensile strength σ (N / m 2 The relationship between the weight W (N) of the laminated core 10 and the measured value A×Q can be expressed by the inequality σ×A×Q<W. In this case, the adhesive area may be calculated using either a measurement value based on the manufactured core size or an area based on the equipment design, and it is best to use whichever is more preferable.

[0045] Second Embodiment Next, a method for manufacturing a laminated core 10 will be described. The method for manufacturing a laminated core 10 formed by stacking multiple electromagnetic steel sheets 1 includes a punching step in which an electromagnetic steel strip coated with an adhesive insulating coating 2 is punched to form the electromagnetic steel sheets 1; a housing step in which, after the punching step, the electromagnetic steel sheets 1 are stacked and housed in a mold; a low-pressure bonding step in which the electromagnetic steel sheets 1 in the mold are heated to a surface temperature of 60°C to 200°C while applying a pressure of 3.0 MPa or less to bond adjacent electromagnetic steel sheets 1 together to form a laminated core; and a removal step in which, after the low-pressure bonding step, the laminated core 10 is removed from the mold. This allows the laminated core 10 to be integrally formed by applying pressure under relatively low temperature and relatively low pressure conditions, ensuring the required tensile strength in the lamination direction (e.g., 1 MPa) for the laminated core 10. Furthermore, because the applied pressure is low, no special pressure device for applying high pressure is required. Furthermore, since the temperature is low, the laminated core 10 can be removed from the mold quickly without relying on the cooling rate, and without having to be cooled naturally over a long period of time or using a special cooling device to accelerate the cooling. Therefore, a method for manufacturing the laminated core 10 that can be produced with high productivity can be provided. Each step will be described in detail below.

[0046] (1) Preparation Step: An electromagnetic steel strip coated with an adhesive insulating coating 2 is prepared. Here, an adhesive resin is used as the adhesive insulating coating 2 so that the laminated core 10 can exhibit a tensile strength in the lamination direction of 20 MPa after complete reaction. As a result, even if the laminated core 10 is formed by applying pressure at low temperature and low pressure in the low-pressure bonding step, as will be described later, the laminated core 10 can have a tensile strength in the lamination direction of 1 MPa or more when removed in the removal step, which is required for a laminated core 10 for a motor.

[0047] (2) Punching Step Next, the electromagnetic steel strip coated with the adhesive insulating coating 2 is punched to form the electromagnetic steel sheet 1 (punching step). In detail, a hollow cylindrical mold is placed with its central axis aligned vertically. A punch for punching, shaped to match the outer shape of the electromagnetic steel sheet 1, is placed above the mold. The electromagnetic steel strip is moved horizontally toward the mold with the thickness direction of the electromagnetic steel sheet 1 aligned vertically, until it is positioned between above the mold and below the punch. The punch is lowered and acts on the electromagnetic steel strip, punching it out.

[0048] (3) Accommodation Step Next, after the punching step, the electromagnetic steel sheets 1 are stacked and accommodated in a mold (accommodation step). In detail, the electromagnetic steel sheets 1 punched out in the punching step are dropped into the mold and accommodated therein. The electromagnetic steel strip is moved horizontally to punch out the next electromagnetic steel sheet 1. Then, the next electromagnetic steel sheet 1 is punched out in the punching step. The next electromagnetic steel sheet 1 is dropped into the mold and accommodated in the mold stacked on top of the previous electromagnetic steel sheet 1. By repeating these steps, the number of electromagnetic steel sheets 1 required to form the laminated core 10 is stacked in the mold.

[0049] (4) Low-Pressure Bonding Process: Next, the electromagnetic steel sheets 1 in the mold are heated to a surface temperature (heating temperature) of 60°C to 200°C while applying pressure of 3.0 MPa or less, thereby bonding adjacent electromagnetic steel sheets 1 together to form the laminated core 10 (low-pressure bonding process). Heating the electromagnetic steel sheets 1 in the mold at 200°C or less allows for heating without requiring complex or large-scale equipment. Here, the adhesive insulating coating 2 of the laminated core 10 uses an adhesive resin that allows the laminated core 10 to exhibit a tensile strength in the lamination direction of 20 MPa after complete reaction. Therefore, the laminated core 10 can be integrally formed by applying pressure under relatively low temperature and pressure conditions, ensuring the required tensile strength in the lamination direction (e.g., 1 MPa). Furthermore, because the pressure is low, no special pressurizing device is required for applying pressure at high pressure. Furthermore, because the pressure is low, the laminated core 10 can be quickly removed from the mold without requiring natural cooling over time or the use of a special cooling device. The heating temperature may be 150°C or less, or 130°C or less. The pressure may be, for example, 0.1 MPa or more, 0.5 MPa or more, or 1.0 MPa or more. The pressure may be 2.0 MPa or less, or 1.5 MPa or less. It is preferable to apply pressure to more reliably ensure tensile adhesion of the laminated core in the lamination direction, but pressure need not be applied (in this case, the pressure is 0 MPa).

[0050] (4-1) Adhesion Promotion Step Here, in the low-pressure bonding step, the magnetic steel sheets may be heated to a temperature (heating temperature) of 100°C to 160°C at a heating rate of 0.5°C / s to 5.0°C / s, and then held at this temperature for 20 seconds to 120 seconds (adhesion promotion step). If the heating rate is too low, bonding takes a long time, reducing cost competitiveness. Furthermore, if the heating rate is too high, equipment is required to achieve a high heating rate. Therefore, the heating rate is preferably 0.5°C / s to 5.0°C / s. This further promotes bonding between adjacent magnetic steel sheets 1 even when heated to a temperature of 60°C to 200°C under low pressure and low temperature conditions in the low-pressure bonding step. The heating temperature may be 150°C or less, or 130°C or less. The holding time may be 100 seconds or less, or 80 seconds or less. The temperature rise rate may be 4.0°C / s or less, or 3.0°C / s or less. The temperature at which the temperature rise in the adhesion promotion step is started is not limited. For example, it may be a temperature 5°C or more lower than the temperature rise temperature, or it may be room temperature (20°C). The order in which the heating to the heating temperature of the low-pressure bonding step and the temperature rise and holding in the adhesion promotion step are performed is not limited. For example, the heating to the heating temperature of the low-pressure bonding step may be performed after the temperature rise and holding in the adhesion promotion step, or the temperature rise and holding in the adhesion promotion step may be performed during the temperature rise to the heating temperature of the low-pressure bonding step (at least a portion of the time from the start of the temperature rise to the heating temperature). Furthermore, the difference between the heating temperature of the low-pressure bonding step and the temperature rise in the adhesion promotion step is not limited. For example, the temperature rise in the adhesion promotion step may be lower than the heating temperature of the low-pressure bonding step. Cooling may be performed during the temperature rise to the heating temperature of the low-pressure bonding step or the temperature rise in the adhesion promotion step, or two or more heating and temperature rise processes may be performed in the low-pressure bonding step or the adhesion promotion step. However, from the viewpoint of improving production efficiency, it is preferable to carry out a single heating / temperature increase treatment through the low-pressure bonding step and the adhesion promotion step without cooling.

[0051] (5) Removal Step Next, after the low-pressure bonding step, the laminated core 10 is removed from the mold (removal step). At this time, the tensile strength of the laminated core 10 in the lamination direction at the time of removal is 1 MPa or more, which is the level required for laminated cores 10 for motors. Therefore, the step of further heating to enhance the adhesive strength of the adhesive insulating coating 2 is no longer necessary. In this way, the laminated core 10 can be manufactured using simple equipment, and the takt time and manufacturing lead time can be shortened.

[0052] (6) Reheating Step After the removal step, the laminated core 10 may be heated to 160°C or higher and 250°C or lower (reheating step). This allows the laminated core 10 to have a higher tensile strength in the lamination direction, depending on the requirements for the laminated core 10. When the adhesive insulating coating is completely reacted, the tensile strength in the lamination direction measured at 25°C is 20 MPa or higher, so the laminated core 10 can have a higher tensile strength in the lamination direction than conventional laminated cores.

[0053] Other Embodiments One embodiment has been described in detail above with reference to the drawings, but the specific configuration is not limited to that described above, and various design modifications and the like are possible.

[0054] The protrusions 3 may be formed, for example, by the following method: For example, the protrusions may be formed by a punch without punching by press working.

[0055] The laminated core 10 according to this embodiment is formed by alternately laminating magnetic steel sheets 1 and adhesive insulating coatings 2. After the adhesive insulating coatings 2 have completely reacted, the tensile strength in the lamination direction measured at 25°C is 20 MPa or more. This allows the laminated core 10 to achieve the adhesive strength (e.g., 1 MPa) required for the finished motor laminated core 10, even at relatively low temperatures (60°C or higher and 200°C or lower). Therefore, a high-strength laminated core 10 can be manufactured without further heating after bonding the magnetic steel sheets 1 together to form the laminate (laminated core). This allows the laminated core 10 to be removed from the manufacturing equipment at a low temperature, simplifying the mechanisms for high-temperature heating and cooling in the manufacturing equipment, thereby enabling the manufacturing equipment for the laminated core 10 to be made more compact. This allows for the provision of a laminated core 10 that can be manufactured with high production efficiency.

[0056] The manufacturing method for the laminated core 10 according to this embodiment is a method for manufacturing a laminated core 10 formed by stacking multiple electromagnetic steel sheets 1. The manufacturing method for the laminated core 10 includes a punching step in which an electromagnetic steel strip coated with an adhesive insulating coating 2 is punched to form the electromagnetic steel sheets 1; a housing step in which, after the punching step, the electromagnetic steel sheets 1 are stacked and housed in a mold; a low-pressure bonding step in which the electromagnetic steel sheets 1 in the mold are heated to a surface temperature of 60°C to 200°C while applying a pressure of 3.0 MPa or less to bond adjacent electromagnetic steel sheets 1 together to form a laminated core; and a removal step in which, after the low-pressure bonding step, the laminated core 10 is removed from the mold. This allows the laminated core 10 to be integrally formed under pressure at a relatively low temperature and pressure, ensuring the required tensile strength in the lamination direction (e.g., 1 MPa) for the laminated core 10. Furthermore, because the pressure is low, no special pressurizing device is required for high-pressure pressurization. Furthermore, because the pressure is low, the laminated core 10 can be quickly removed from the mold without requiring natural cooling over time or the use of a special cooling device to promote cooling. Therefore, a method for manufacturing the laminated core 10 can be provided that allows for high production efficiency.

[0057] (Lamination Direction Tensile Strength Test) A test was conducted to measure the tensile strength in the lamination direction for laminated cores manufactured under different manufacturing conditions. A fully automatic metal tensile testing machine manufactured by Shimadzu Corporation was used for this test. FIG. 4 is a table showing the relationship between the test specimens, test conditions, and test results for the tensile adhesion test. In FIG. 4 , from the left column, "No." indicates the number of the test specimen, "Example or Comparative Example" indicates whether it is an Example or a Comparative Example, "Heating Temperature" indicates the temperature in °C at which the stacked electromagnetic steel sheets are heated in the low-pressure bonding step in the process of forming the laminated core, "Pressure Force" indicates the pressure in MPa at which the stacked electromagnetic steel sheets are pressed in the low-pressure bonding step in the process of forming the laminated core, "Temperature Rise Rate" indicates the rate at which the temperature is raised from the temperature rise start temperature (room temperature (20°C)) to the heating temperature in the adhesion promotion step in °C / s, and "Temperature Rise Amount" indicates the temperature at which the temperature is raised from the temperature rise start temperature (room temperature (20°C)) in the adhesion promotion step in °C / s. The temperature range (= heating temperature (°C) - 20 (°C)) from the initial temperature (maximum temperature reached) to the heating temperature is shown in °C, the "holding time" is the holding time in seconds at a temperature between 60°C and 120°C, which is the heating temperature, and the "reheating temperature" is the temperature reached by reheating after removal from the mold. The "90°C lamination direction tensile strength" is shown as "B" if the lamination direction tensile strength of the manufactured laminated core at 90°C is 1 MPa or more, "A" if the lamination direction tensile strength of the manufactured laminated core at 90°C is 3 MPa or more, and "C" if the lamination direction tensile strength is less than 1 MPa. Note that under all test conditions, the heating temperature in the low-pressure bonding process was the same as the heating temperature in the adhesion promotion process. The test details are as follows.

[0058] The laminated core was a stator core used as a stator for a motor. The electromagnetic steel sheets used to manufacture the laminated core were 25HX1300 (0.25 mm thick, low-core-loss, high-magnetic-flux-density non-oriented electromagnetic steel sheets). The laminated core was made by laminating 600 electromagnetic steel sheets. The laminated core had a lamination thickness (length along the lamination direction D) of 150 mm. The laminated core was formed by heating multiple electromagnetic steel sheets stacked in a mold at a predetermined heating rate (shown in FIG. 4 ) while applying a predetermined pressure (see FIG. 4 ), starting from room temperature (20°C), to a predetermined surface temperature (the heating temperature shown in FIG. 4 = the heating temperature) for a predetermined time (see FIG. 4 ).

[0059] The test specimens were cut into cubes from the laminated core as shown by the dashed lines in Figure 1. The dimensions of the test specimens were 45.0 mm long along the lamination direction D, 3.6 mm wide, and 12.25 mm long. The 90°C lamination direction tensile strength was determined by gradually increasing the tensile load applied to the test specimen heated to 90°C in the longitudinal direction while holding both longitudinal ends of the specimen with the chucks of a tensile testing machine, and dividing the maximum load by the cross-sectional area of ​​the test specimen. Note that each of the electrical steel sheets constituting the test specimen was fully bonded with an adhesive insulating coating.

[0060] The adhesive insulating coating (adhesive coat) used was an adhesive resin that had a tensile strength in the lamination direction of 20 MPa or more at 25°C after complete reaction, or an adhesive resin that had a tensile strength of 14 MPa under the same conditions. The tensile strength in the lamination direction at 25°C after complete reaction of the adhesive resin was measured in advance using the same method as for measuring the tensile strength in the lamination direction at 90°C. Specifically, No. In Examples 1, 4, 5, 8, 9, and 11-18, 44 parts by mass of a phenol novolac epoxy resin (PPN201, manufactured by Nippon Kayaku Co., Ltd.), 12 parts by mass of a cresol novolac epoxy resin (YDCN-700-10, manufactured by Nippon Steel Chemical & Materials Co., Ltd.), 10 parts by mass of a trifunctional epoxy resin (EP-3950E, manufactured by ADEKA Corporation), 30 parts by mass of a tetrafunctional epoxy resin (YH-404, manufactured by Nippon Steel Chemical & Materials Co., Ltd.), and 4 parts by mass of a bisphenol A epoxy resin (Epikote, manufactured by Mitsubishi Chemical Corporation) were used as the thermosetting resin, 40 parts by mass (based on the thermosetting resin) of a phenoxy resin (YPS-007A30, manufactured by Nippon Steel Chemical & Materials Co., Ltd.) as the thermoplastic resin, 10 parts by mass (based on the thermosetting resin) of core-shell rubber, and 12 parts by mass (based on the thermosetting resin) of DICY as the curing agent were used. After the reaction was complete, the adhesive resin had a tensile strength in the lamination direction at 25° C. of 24 MPa. In Example 2, 44 parts by mass of a phenol novolac epoxy resin (PPN201, manufactured by Nippon Kayaku Co., Ltd.), 12 parts by mass of a cresol novolac epoxy resin (YDCN-700-10, manufactured by Nippon Steel Chemical & Materials Co., Ltd.), 10 parts by mass of a trifunctional epoxy resin (EP-3950E, manufactured by ADEKA Corporation), 30 parts by mass of a tetrafunctional epoxy resin (YH-404, manufactured by Nippon Steel Chemical & Materials Co., Ltd.), and 4 parts by mass of a bisphenol A epoxy resin (Epikote, manufactured by Mitsubishi Chemical Corporation) were used as the thermoplastic resin, 40 parts by mass (based on the thermosetting resin) of a phenoxy resin (YPS-007A30, manufactured by Nippon Steel Chemical & Materials Co., Ltd.), 10 parts by mass (based on the thermosetting resin) of core-shell rubber, and 41 parts by mass of DDS and 2 parts by mass of DCMU (based on the thermosetting resin) were used as the curing agent. After the reaction was complete, the adhesive resin had a tensile strength in the lamination direction at 25° C. of 83 MPa.In Examples No. 3, 6, and 10, 56 parts by mass of a phenol novolac epoxy resin (PPN201, manufactured by Nippon Kayaku Co., Ltd.) and 44 parts by mass of a tetrafunctional epoxy resin (YH-404, manufactured by Nippon Steel Chemical & Materials Co., Ltd.) were used as the thermosetting resin, 33 parts by mass (based on the thermosetting resin) of a phenoxy resin (YP-50, manufactured by Nippon Steel Chemical & Materials Co., Ltd.) were used as the thermoplastic resin, 5 parts by mass (based on the thermosetting resin) of core-shell rubber were used, and 12 parts by mass of DICY and 5 parts by mass of DCMU (based on the thermosetting resin) were used as the curing agent. The tensile strength in the lamination direction of this adhesive resin at 25°C after complete reaction was 14 MPa.

[0061] The heating temperature (surface temperature) was selected from 200°C, 120°C, and 60°C and combined with other conditions.

[0062] The pressure was selected from 1.0 MPa, 0 MPa, and 3.0 MPa and combined with other conditions.

[0063] The temperature rise rate was selected from 3°C / s, 5°C / s, 0.15°C / s, 10°C / s, and 0.1°C / s and combined with other conditions.

[0064] The temperature rise amount, which is the temperature range from room temperature (20°C) to the heating temperature, was selected from 100°C, 40°C, and 180°C and combined with other conditions.

[0065] The holding time at the elevated temperature of 60° C. or more and 200° C. or less was selected from 20 seconds, 0 seconds, 120 seconds, and 200 seconds, and was combined with other conditions.

[0066] The reheating temperature, which is the temperature at which the molded article is reheated after being removed from the mold, was selected from among no reheating, 160°C, and 250°C, and was combined with other conditions.

[0067] A test of the tensile strength in the lamination direction was performed, and a test result of 1 MPa or more was judged to be pass, and a test result of less than 1 MPa was judged to be fail. In Fig. 4, a pass case is indicated by "A" or "B", and a fail case is indicated by "C".

[0068] As shown in Figure 4, the test results showed that Example Nos. 1, 2, 4, 5, 8, 9, and 11-18 passed the test, while Comparative Example Nos. 3, 6, and 10 failed the test. Thus, it was confirmed that if the lamination direction tensile strength in the lamination direction D measured at 25°C after the adhesive insulating coating 2 has completely reacted is 20 MPa or more, the lamination direction tensile strength at the time of removal from the mold (90°C) can be ensured to be 1 MPa or more, even when pressurized at low temperature and low pressure in the mold. Furthermore, since the laminated cores of the Examples have a lamination direction tensile strength of 20 MPa or more at 25°C after the adhesive insulating coating has completely reacted, laminated cores with higher lamination direction tensile strength than conventional laminated cores were obtained. Measurements were also conducted using test specimens cut from some of the manufactured laminated cores of the Examples, confirming that the lamination direction tensile strength at 25°C was 20 MPa or more.

[0069] REFERENCE SIGNS LIST 1 electromagnetic steel sheet 2 adhesive insulating coating 3 protrusion 10 laminated core D lamination direction

Claims

1. A laminated core in which magnetic steel sheets and adhesive insulating coatings are alternately laminated, and after the adhesive insulating coatings have completely reacted, the tensile adhesive strength in the lamination direction is 20 MPa or more when measured at 25°C.

2. The laminated core according to claim 1, wherein the electromagnetic steel sheet in the uppermost layer has a protrusion that protrudes in the lamination direction.

3. A method for manufacturing a laminated core formed by stacking a plurality of electromagnetic steel sheets, comprising: a punching step of punching an electromagnetic steel strip coated with an adhesive insulating coating to form the electromagnetic steel sheets; a containing step of stacking the electromagnetic steel sheets and accommodating them in a mold after the punching step; a low-pressure bonding step of heating the electromagnetic steel sheets in the mold to a surface temperature of 60°C or more and 200°C or less while applying a pressure of 3.0 MPa or less to bond adjacent electromagnetic steel sheets together to form a laminated core; and a removal step of removing the laminated core from the mold after the low-pressure bonding step.

4. A method for manufacturing a laminated core according to claim 3, wherein the low-pressure bonding process includes an adhesion promotion process in which the temperature is raised to 100°C or higher and 160°C or lower at a heating rate of 0.5°C / s or higher and 5.0°C / s or lower, and the temperature is maintained for 20 seconds or higher and 120 seconds or lower.

5. The method for manufacturing a laminated core according to claim 3 or 4, further comprising a reheating step of heating the laminated core to a temperature of 160°C or higher and 250°C or lower after the removal step.

6. The method for manufacturing a laminated core according to claim 3 or 4, wherein in the low-pressure bonding step, the electromagnetic steel sheets in the mold are pressurized at 0.1 MPa or more.