Plated steel material

MYPI2025000887A0Undetermined Publication Date: 2024-02-29NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025000887
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-08-30
Filing Date
2023-08-30
Publication Date
2024-02-29

AI Technical Summary

Technical Problem

Zn-Al-Mg-based plated steel sheets lack sufficient corrosion resistance in wet and running water environments, leading to reduced product lifespan due to red rust formation and sacrificial corrosion issues.

Method used

A plated steel material with a specific chemical composition and structure, including an Al: 10.0% to 40.0% and Mg: 4.0% to 8.5% content in the plating layer, along with controlled phase ratios of Al, Al-Zn, and Zn-Al phases, and the presence of Si and Ca, to enhance wet and running water corrosion resistance and sacrificial corrosion protection.

Benefits of technology

The material exhibits excellent wet corrosion resistance, running water corrosion resistance, and sacrificial corrosion resistance, preventing red rust formation and extending product lifespan in wet environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

ABSTRACT PLATED STEEL MATERIAL This plated steel material is a plated steel material including: a steel material; and a plating layer disposed on a surface of the steel material, wherein the plating layer has a predetermined average chemical composition, in a cross section of the plating layer perpendicular to the surface of the steel material, a microstructure observed with a scanning electron microscope includes, in terms of area fraction, a MgZn2 phase: 10% or more and 50% or less, a total of an Al phase, an Al-Zn phase, and a Zn-Al phase: 15% or more and 75% or less, a [ternary eutectic structure of Al / MgZn2 / Zn]: 0% or more and 65% or less, and the remainder: 0% or more and 5.0% or less, and an area ratio (([Al] + [Zn - Al]) / [Al - Zn]) of a total of the Al phase and the Zn-Al phase to the Al-Zn phase is 0.8 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Plated steel

[0001] This application claims priority to Japanese Patent Application No. 2022-136497, filed on August 30, 2022, the contents of which are incorporated herein by reference.

[0002] It is widely known that the corrosion resistance of steel materials can be improved by plating the surface with zinc, and among these, Zn-Al-Mg-plated steel sheets, which have improved corrosion resistance by adding Al and Mg to zinc, are widely used in the fields of automobiles, home appliances, building materials, and civil engineering.The environments in these applications include wet environments where rainwater and the like constantly accumulates, and flowing water environments, and in these environments, there is a problem that even Zn-Al-Mg-plated steel sheets do not have sufficient corrosion resistance.

[0003] For example, Patent Document 1 discloses a steel sheet having a steel plate, an alloy layer containing Fe and Si, and a plating layer, in which the average composition of the plating layer and the alloy layer is, in mass %, Al: 45.0 to 65.0%, Si: 0.50 to 5.00%, Mg: 1.00 to 10.00%, with the balance being Zn, Fe, and impurities, the plating layer contains an Mg—Si phase with a volume fraction of 0.1 to 20.0%, and when a range of 1 μm from the surface of the plating layer in the thickness direction of the plating layer is defined as a surface layer portion of the plating layer, the plating layer in the surface layer portion is flat. The document describes a Zn-Al-Mg-based plated steel sheet in which the average equivalent circle diameter of the Mg-Si phase in a planar view direction is 0.1 to 15.0 μm, and when the Si content is measured over the entire thickness of the plated layer, the integrated value of the Si content from the surface of the plated layer to the center of the plated layer thickness is 0.55 times or more the integrated value of the Si content from the surface of the plated layer to the interface between the plated layer and the alloy layer, with the center of the plated layer being defined as a position halfway through the thickness of the plated layer from the surface of the plated layer toward the interface.

[0004] Patent Document 2 describes a hot-dip Al-Zn-Mg-Si plated steel sheet having a plating film on the surface of the steel sheet, the plating film comprising an interfacial alloy layer present at the interface with the base steel sheet and a main layer present on the alloy layer, and containing 25 to 80 mass% Al, more than 0.6 to 15 mass% Si, and more than 0.1 to 25 mass% Mg, and the Mg on the surface of the main layer 2A hot-dip Al-Zn-Mg-Si plated steel sheet having an area ratio of Si of 10% or more is described.

[0005] Patent Document 3 discloses a method for forming a steel strip, which comprises the steps of: (a) passing the strip through a hot dip coating bath containing Al, Zn, Si, and Mg, and optionally other elements, to form a molten Al-Zn-Si-Mg alloy coating on the strip; (b) cooling the coated strip to solidify the molten Al-Zn-Si-Mg alloy on the strip, forming an alpha-Al phase dendrite, a Zn-rich phase in the interdendritic regions, and an Mg alloy in the interdendritic regions; 2 (c) heat treating the coated strip at a temperature and for a time to form an Al-Zn phase solid solution from an as-cast microstructure of alpha-Al phase dendrites and Zn-rich interdendritic phases to form an Al-Zn phase solid solution. 2 A method for forming a metal-coated strip is described, which comprises (a) promoting spheroidization of the Si phase particles; and (b) cooling the heat-treated strip.

[0006] Patent Document 4 describes a highly heat-resistant hot-dip Zn-Al alloy-plated steel sheet in which an alloy plating layer composed of 3.0 to 7.0 mass% Al, 0.05 to 0.5 mass% Si, 0.01 to 0.5 mass% Mg, and the balance Zn is formed on the surface of the steel sheet, and an Fe-Al-Si alloy layer in which Si is concentrated is formed between the alloy plating layer and the steel sheet substrate.

[0007] Patent Document 5 discloses a steel sheet having a plating layer formed on the surface thereof, the plating layer containing, on an average composition, 1 to 10 mass % of Mg, 4 to 22 mass % of Al, and the balance being Zn and impurities, and the plating layer is 2The coating layer has a base material having a ternary eutectic structure of Al / Zn, and the base material contains an Al / Zn mixed structure of 10 to 70% by area in the cross section of the coating layer. The Al / Zn mixed structure includes a first region having a Zn concentration in the range of 75 mass% or more and less than 85 mass%, and a second region inside the first region having a Zn concentration in the range of 67 mass% or more and less than 75 mass%, and the second region contains a mixture of Zn phase and Al phase, and the area of ​​the second region in the cross section of the coating layer is 1 μm 2 The document describes a hot-dip Zn-Al-Mg plated steel material in which the interface length between the Zn phase and the Al phase per unit area is 20 μm or less.

[0008] However, Patent Documents 1 to 5 do not consider corrosion resistance in a water-wet environment or a flowing water environment (hereinafter referred to as water-wet corrosion resistance or flowing water corrosion resistance).

[0009] International Publication No. 2019 / 049307 Japanese Patent Application Laid-Open No. 2016-166414 Japanese Patent Application Laid-Open No. 2012-528244 Japanese Patent Application Laid-Open No. 2000-265255 Japanese Patent Application Laid-Open No. 2021-195564

[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a plated steel material that has excellent water-wet corrosion resistance and running water corrosion resistance, as well as excellent sacrificial corrosion resistance.

[0011] In order to solve the above problems, the following configuration is adopted. [1] A plated steel material having a steel material and a plating layer disposed on a surface of the steel material, wherein the plating layer has an average chemical composition, in mass%, of Al: 10.0% to 40.0%, Mg: over 4.0% to 8.5%, Si: 0% to 5.0%, Ca: 0% to 3.00%, Sn: 0% to 3.00%, Bi: 0% to 1.00%, In: 0% to 1.00%, Y: 0% to 0.50%, La: 0% to 0.50%, Ce: 0% to 0.50%, Sr: 0% to 0.50%, B: 0% to 1.00%, P: 0% to 0.50%, Cr: 0% to 0.25%, Ti: 0% to 0.25%, V: 0% to 0.25%, Zr: 0% to 0.25%, Ni: 0% to 1.00%, Co: 0% to 0.25%, Nb: 0% to 0.25%, Cu: 0% to 1.00%, Mn: 0% to 0.25%, Mo: 0% to 0.25%, W: 0% to 0.25%, Ag: 0% to 1.00%, Li: 0% to 0.50%, Na: 0% to 0.05%, K: 0% to 0.05%, Fe: 0% to 5.00%, Sb: 0% to 0.50%, Pb: 0% to 0.50%, Ba: 0% to 0.25%, and the balance: Zn and impurities; In a cross section of the coating layer perpendicular to the surface of the steel material, the structure observed with a scanning electron microscope is, in terms of area fraction, MgZn 2 phase: 10% or more and 50% or less, the total of Al phase, Al-Zn phase and Zn-Al phase: 15% or more and 75% or less, [Al / MgZn 2[Al] / Zn ternary eutectic structure]: 0% or more and 65% or less, and balance: 0% or more and 5.0% or less, and the area ratio of the total of the Al phase and the Zn-Al phase to the Al-Zn phase (([Al] + [Zn-Al]) / [Al-Zn]) is 0.8 or more. [2] The plated steel material according to [1], wherein the average chemical composition of the plated layer contains 0.05% to 5.0% of Si, and the integrated intensity values ​​of each element in a surface layer from the surface of the plated layer to a depth of 0.5 μm, when depth analysis is performed by GDS method, satisfy the following formula (1): IS(Si) / (ISI(Zn)+ISI(Al))≧0.005 (1) where IS(Si), ISI(Zn), and ISI(Al) in formula (1) are the integrated intensity values ​​of Si, Zn, and Al detected by GDS method, respectively. [3] In the average chemical composition of the plating layer, Ca is 0.01% to 3%, and in the plating layer, Ca 3 Al 2 Si 2 phase, CaAl 2 Si 2 phase, CaAl 2 Si 2 phase, CaAl 1-x Si 1+x The plated steel material according to [1] or [2], which contains any one of the following phases (where x = 0 to 0.2), and wherein, in a surface layer from the surface of the plated layer to a depth of 0.5 μm, when a depth analysis is performed by a GDS method, the integrated intensity values ​​of each element satisfy the following formula (2): IΣ(Ca) / IΣ(Si)≧2.0 (2), where IΣ(Ca) and IΣ(Si) are the integrated intensity values ​​of Ca and Si detected by the GDS method, respectively.

[0012] According to the present invention, a plated steel material can be provided that has excellent water-wet corrosion resistance and flowing water corrosion resistance, as well as excellent sacrificial corrosion protection.

[0013] Conventionally, pure aluminum-plated materials known as Type 2 for corrugated pipes have been known as plating materials suitable for wet and flowing water environments. However, aluminum has poor sacrificial corrosion protection, and red rust develops on the end faces of steel materials, resulting in poor appearance. Furthermore, as the thickness of steel materials increases, corrosion from the end faces becomes more pronounced, resulting in a shortened product life.

[0014] On the other hand, Zn-Al-Mg plated materials have sufficient sacrificial corrosion protection performance and superior corrosion resistance compared to Zn plating in normal environments, but have the problem that corrosion products are easily washed away in wet or flowing water environments, making it difficult to demonstrate high corrosion resistance compared to normal environments.

[0015] The Zn-Al-Mg based plating layer is formed from a number of constituent phases, including an Al phase, an Al-Zn phase, a Zn-Al phase, and an Mg phase, as will be described in detail later. 2 Zn phase, Mg 2 Zn 11 phase, Zn phase, [Al / MgZn 2 Phases and structures such as the above-mentioned ternary eutectic structure of Fe / Zn account for the majority of the phase composition ratio.

[0016] The present inventors have focused on the relationship between the wet corrosion resistance and running water corrosion resistance of Zn-Al-Mg based plating in a water-wet environment and the constituent phases and structural structures of the plating layer, and as a result of extensive investigation, have found that the wet corrosion resistance and running water corrosion resistance can be improved by optimizing the proportions of the constituent phases and structural structures.

[0017] It is known that Al, a plating component, precipitates as multiple phases during solidification, namely, Al phase, Al-Zn phase, and Zn-Al phase. Of these, the Al phase has the best water resistance and running water resistance, but poor sacrificial corrosion protection. Furthermore, the Al-Zn phase has the highest sacrificial corrosion protection of the three phases, but is poor in water wetting corrosion resistance and running water corrosion resistance. Furthermore, the Zn-Al phase has intermediate properties compared to the previous two phases in terms of water wetting corrosion resistance, running water corrosion resistance, and sacrificial corrosion protection.

[0018] Therefore, the inventors have conducted extensive research, thinking that a plated steel material with excellent corrosion resistance can be obtained by appropriately adjusting the proportion of Al phase in a Zn-Al-Mg-based coating layer, and have found that by controlling the phase proportion in the coating layer, a plated steel material with excellent water wetting corrosion resistance, running water corrosion resistance, and sacrificial corrosion protection can be obtained. Steel structures manufactured from the plated steel material according to the present invention have excellent water wetting corrosion resistance, running water corrosion resistance, and sacrificial corrosion protection. The plated steel material according to an embodiment of the present invention will be described below.

[0019] The plated steel material of this embodiment is a plated steel material having a steel material and a plating layer disposed on the surface of the steel material, and the plating layer has an average chemical composition, in mass %, of Al: 10.0% to 40.0%, Mg: over 4.0% to 8.5%, Si: 0% to 5.0%, Ca: 0% to 3.00%, Sn: 0% to 3.00%, Bi: 0% to 1.00%, In: 0% to 1.00%, Y: 0% to 0.50%, La: 0% to 0.50%, Ce: 0% to 0.50%, Sr: 0% to 0.50%, B: 0% to 1.00%, P: 0% to 0.50%, Cr: 0% to 0.25%, Ti: 0% to 0.25%, V: 0% to 0.25%, Z: r: 0% to 0.25%, Ni: 0% to 1.00%, Co: 0% to 0.25%, Nb: 0% to 0.25%, Cu: 0% to 1.00%, Mn: 0% to 0.25%, Mo: 0% to 0.25%, W: 0% to 0.25%, Ag: 0% to 1.00%, Li: 0% to 0.50%, Na: 0% to 0.05%, K: 0% to 0.05%, Fe: 0% to 5.00%, Sb: 0% to 0.50%, Pb: 0% to 0.50%, Ba: 0% to 0.25%, and the balance: Zn and impurities, and the structure observed with a scanning electron microscope in a cross section of the plating layer perpendicular to the surface of the steel material is, in terms of area fraction, MgZn 2 phase: 10% or more and 50% or less, the total of Al phase, Al-Zn phase and Zn-Al phase: 15% or more and 75% or less, [Al / MgZn 2 / Zn ternary eutectic structure]: 0% or more and 65% or less, and the balance: 0% or more and 5.0% or less, and the total area ratio of the Al phase and the Zn—Al phase to the Al—Zn phase (([Al] + [Zn—Al]) / [Al—Zn]) is 0.8 or more. Furthermore, in the plated steel material of this embodiment, the average chemical composition of the coating layer contains 0.05% to 5.0% Si, and it is preferable that the integrated intensity values ​​of each element in a surface layer from the surface of the coating layer to a depth of 0.5 μm, when a depth analysis is performed by the GDS method, satisfy the following formula (1): IS(Si) / (ISI(Zn)+ISI(Al))≧0.005 (1) where IS(Si), ISI(Zn), and ISI(Al) in formula (1) are the integrated intensity values ​​of Si, Zn, and Al detected by the GDS method, respectively. Furthermore, in the plated steel material of this embodiment, the average chemical composition of the plated layer contains 0.01% to 3% of Ca, and the plated layer contains 3 Al 2 Si 2 phase, CaAl 2 Si 2 phase, CaAl 2 Si 2 phase, CaAl 1-x Si 1+x phase (where x = 0 to 0.2), and in the surface layer from the surface of the plating layer to a depth of 0.5 μm, when depth analysis is performed by the GDS method, the integrated intensity value of each element preferably satisfies the following formula (2): IΣ(Ca) / IΣ(Si)≧2.0 (2) where IΣ(Ca) and IΣ(Si) are the integrated intensity values ​​of Ca and Si detected by the GDS method, respectively.

[0020] In the following description, the "%" used to indicate the content of each element in the chemical composition means "mass %." Furthermore, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. When the numerical values ​​before and after "to" are followed by "greater than" or "less than," the numerical range does not include these numerical values ​​as the lower or upper limit.

[0021] "Corrosion resistance" refers to the corrosion resistance of the plating layer itself. Zn-based plating layers have a sacrificial corrosion protection effect on steel materials, so the plating layer corrodes and turns white rust before the steel material corrodes. After the white rust disappears, the steel material corrodes and turns red rust. This is the corrosion process of plated steel sheets. "Sacrificial corrosion protection" refers to the ability to inhibit corrosion of exposed steel material (e.g., cut end surfaces of plated steel material, or areas where the steel material is exposed due to cracks in the hot-dip coating layer during processing). "Water-wet corrosion resistance, running water corrosion resistance" refers to the ability of the plating layer itself to resist corrosion when water is dripped onto the surface of the plating layer and then flowed over it.

[0022] There are no particular limitations on the quality of the steel material. Various types of steel material can be used, such as general steel, Ni pre-plated steel, Al-killed steel, extra-low carbon steel, high carbon steel, various high-tensile steels, and some high alloy steels (steels containing strengthening elements such as Ni and Cr). Furthermore, there are no particular limitations on the conditions for the steel material manufacturing method and the steel sheet manufacturing method (hot rolling method, pickling method, cold rolling method, etc.). Furthermore, the steel material can be used in a range of 3 g / m of Zn, Ni, Sn, or alloys thereof. 2 Steel materials on which the following metal or alloy films are formed may also be used.

[0023] Next, the plating layer will be described. The plating layer according to this embodiment includes a Zn—Al—Mg alloy layer. The plating layer may also include an Al—Fe alloy layer. A Zn—Al—Mg alloy layer, in which alloy elements such as Al and Mg are added to Zn, has improved corrosion resistance compared to a normal Zn plating layer. For example, even if the Zn—Al—Mg alloy layer is about half the thickness of a normal Zn plating layer, it has corrosion resistance equivalent to that of a Zn plating layer. Therefore, the plating layer according to this embodiment also has corrosion resistance equivalent to or greater than that of a Zn plating layer.

[0024] The Zn—Al—Mg alloy layer is made of a Zn—Al—Mg alloy, which means a ternary alloy containing Zn, Al, and Mg.

[0025] The Al--Fe alloy layer is an interface alloy layer between the steel material and the Zn--Al--Mg alloy layer.

[0026] That is, the plating layer according to this embodiment may have a single-layer structure of a Zn—Al—Mg alloy layer, or a laminate structure including a Zn—Al—Mg alloy layer and an Al—Fe alloy layer. In the case of a laminate structure, the Zn—Al—Mg alloy layer is preferably the layer that constitutes the surface of the plating layer. However, although an oxide film of the plating layer constituent elements is formed on the outermost surface of the plating layer with a thickness of less than 1 μm, this is thin compared to the overall thickness of the plating layer and is therefore often ignored by the main body of the plating layer.

[0027] The total thickness of the plating layer is preferably 5 to 70 μm. However, since the total thickness of the plating layer depends on the plating conditions, the total thickness of the plating layer is not limited to the range of 5 to 70 μm. In a typical hot-dip plating method, the total thickness of the plating layer is affected by the viscosity and specific gravity of the plating bath. The total thickness of the plating layer is adjusted by the drawing speed of the steel material (base sheet for plating) and the strength of wiping.

[0028] The Al-Fe alloy layer is formed on the surface of the steel material (specifically, between the steel material and the Zn-Al-Mg alloy layer), and has an Al structure. 5 Fe 2 The Al-Fe alloy layer is formed by mutual atomic diffusion between the base steel (steel material) and the coating bath. When hot-dip coating is used as the manufacturing method, the Al-Fe alloy layer is likely to be formed in the coating layer containing Al element. Since the coating bath contains Al at a certain concentration or more, the Al 5 Fe 2 However, atomic diffusion takes time, and there are also areas where the Fe concentration is high near the base steel. Therefore, the Al-Fe alloy layer is partially composed of AlFe phase, Al 3 Fe phase, Al 2 It may contain a small amount of Fe phase, etc. Furthermore, since the plating bath also contains a certain concentration of Zn, the Al—Fe alloy layer also contains a small amount of Zn.

[0029] When the plating layer contains Si, Si is particularly likely to be incorporated into the Al-Fe alloy layer, and may form an Al-Fe-Si intermetallic compound phase. Identified intermetallic compound phases include the AlFeSi phase, and isomers such as α-, β-, q1-, and q2-AlFeSi phases exist. Therefore, these AlFeSi phases may be detected in the Al-Fe alloy layer. An Al-Fe alloy layer containing these AlFeSi phases is also referred to as an Al-Fe-Si alloy layer.

[0030] Next, the average chemical composition of the plating layer will be described. When the plating layer has a single-layer structure of a Zn—Al—Mg alloy layer, the average chemical composition of the entire plating layer is the average chemical composition of the Zn—Al—Mg alloy layer. When the plating layer has a laminated structure of an Al—Fe alloy layer and a Zn—Al—Mg alloy layer, the average chemical composition is the combined average chemical composition of the Al—Fe alloy layer and the Zn—Al—Mg alloy layer.

[0031] Typically, in hot-dip galvanizing, the chemical composition of the Zn—Al—Mg alloy layer is almost identical to that of the galvanizing bath, since the reaction for forming the coating layer is almost always completed within the coating bath. Furthermore, in hot-dip galvanizing, the Al—Fe alloy layer is instantaneously formed and grows immediately after immersion in the coating bath. The reaction for forming the Al—Fe alloy layer is already completed within the coating bath, and its thickness is often sufficiently smaller than that of the Zn—Al—Mg alloy layer. Therefore, unless special heat treatment such as a thermal alloying treatment is performed after coating, the average chemical composition of the entire coating layer is substantially identical to that of the Zn—Al—Mg alloy layer, and components such as the Al—Fe alloy layer can be ignored.

[0032] Al: 10.0% or more, 40.0% or less Like Zn, Al is an element that mainly constitutes the coating layer. Although Al has a small sacrificial corrosion protection effect, the inclusion of Al in the coating layer improves wet corrosion resistance, running water corrosion resistance, and flat surface corrosion resistance. Furthermore, without Al, Mg cannot be stably maintained in the coating bath, so Al is included in the coating bath as an element essential for manufacturing. The Al content of 10.0% or more is the content necessary to contain a large amount of Mg, as described below, or the content necessary to ensure a certain level of corrosion resistance. If the Al content is below this level, it becomes difficult to prepare the coating bath and furthermore, it becomes difficult to ensure corrosion resistance. Furthermore, the Al content is set to 40.0% or less because Al has a weak sacrificial corrosion protection effect on steel sheet, and if the Al content exceeds this level, sufficient sacrificial corrosion protection cannot be obtained. Therefore, the upper limit is set to 40.0%.

[0033] Mg: more than 4.0% and not more than 8.5% Mg is an element that has a sacrificial anticorrosion effect and enhances the corrosion resistance of the plating layer. When Mg is contained at a certain level or more, the plating layer 2 The higher the Mg content in the plating layer, the more the MgZn phase is formed. 2 More phases are formed. MgZn 2 The phase is known to have a structure called the Laves phase, and its hardness is known to be high. The Mg content of more than 4.0% is the concentration necessary to exhibit corrosion resistance, and if it is 4.0% or less, sufficient corrosion resistance cannot be obtained. 2 If the Mg content is too high, the plating layer will not be sufficiently formed, and the corrosion resistance of the plating layer itself will be low. Since an excessive Mg content makes it difficult to manufacture the plating layer and reduces the workability of the plating layer, the upper limit is 8.5%. A more preferable Mg content is 5.0% or more and 7.0% or less.

[0034] Si: 0% to 5.0% When Si is contained in the plating bath, a single Si phase or a Mg 2Si precipitates, and when Ca is also present together with Si, an Al-Ca-Si compound precipitates. Because Si has excellent wet corrosion resistance and running water corrosion resistance, the precipitation of Si or Si-based compounds on the surface of the coating layer can further improve wet corrosion resistance and running water corrosion resistance. Si is an optional additive element and may be 0%, but adding 0.05% or more further improves wet corrosion resistance and running water corrosion resistance. However, if Si exceeds 5.0%, a large amount of dross is generated and bare spots frequently occur. Therefore, the Si concentration is 0 to 5.0%, and may be 0.05% to 5.0%, 0.05% to less than 1.0%, or 0.10% to 0.50%.

[0035] Ca: 0% to 3.00%. Calcium easily oxidizes in the atmosphere. When present in the plating bath, it forms a dense oxide film on the bath surface, preventing the oxidation of magnesium. This effect stabilizes the magnesium concentration, facilitating the production of plated steel sheets with the target composition. Because Ca is an optional additive, 0% is acceptable. However, to optimally exert the aforementioned effects, the Ca content should be greater than 0%, more preferably 0.01% or greater. Furthermore, when Ca is present at 0.01% or greater, Al-Ca-Si compounds or Ca-Al-Zn compounds are likely to form. Of these, Al-Ca-Si compounds have excellent wet corrosion resistance and running water corrosion resistance. Therefore, the concentration of these compounds in the plating surface layer can improve wet corrosion resistance and running water corrosion resistance. The upper limit of Ca is 3.00%.

[0036] Element Group A Sn: 0% to 3.00%, Bi: 0% to 1.00%, In: 0% to 1.00% Elements in element group A function to improve sacrificial corrosion protection. However, Mg tends to bond more strongly than Zn, reducing the effect of the contained Mg, so there is an upper limit to the content of these elements. If the upper limit is exceeded, adhesion of dross and the like increases, and water-wet corrosion resistance, running water corrosion resistance, workability, and weldability all tend to deteriorate. Therefore, Sn is set to 0 to 3.00%, more preferably more than 0 and less than 3.00%. Bi is set to 0% to 1.00%, more preferably more than 0 and less than 1.00%. In is set to 0% to 1.00%, more preferably more than 0 and less than 1.00%.

[0037] Element Group B Y: 0% to 0.50% La: 0% to 0.50% Ce: 0% to 0.50% Sr: 0% to 0.50% Element Group B, Y, La, Ce, and Sr, are easily oxidized in the atmosphere. When present in a coating bath, they form a dense oxide film on the bath surface, preventing oxidation of Mg. This effect stabilizes the Mg concentration and facilitates the production of coated steel sheets with the target composition. To optimally achieve this effect, the content of these elements is set to more than 0%, more preferably 0.01% or more. However, there is an upper limit to the content of each element. Exceeding the upper limit tends to make the preparation of the coating bath difficult. Furthermore, the deposition of dross and the like tends to increase, and the water-wet corrosion resistance, running water corrosion resistance, workability, and weldability also tend to deteriorate. Therefore, the content of each of Y, La, Ce, and Sr is set to 0% to 0.50%, preferably more than 0% and less than 0.50%, and more preferably 0.01% or more and less than 0.50%.

[0038] Element Group C B: 0% to 1.00% P: 0% to 0.50% B and P, which belong to element group C, are elements belonging to the metalloid group. These elements generally do not affect wet corrosion resistance or running water corrosion resistance, but there is an upper limit to the content of each element, and if the upper limit is exceeded, adhesion of dross and the like increases, tending to deteriorate corrosion resistance. Therefore, the contents of B and P are set to 0% to 1.0% and 0% to 0.50%, respectively.

[0039] Element group D Cr: 0% to 0.25% Ti: 0% to 0.25% V: 0% to 0.25% Zr: 0% to 0.25% Ni: 0% to 1.00% Co: 0% to 0.25% Nb: 0% to 0.25% Cu: 0% to 1.00% Mn: 0% to 0.25% Mo: 0% to 0.25% W: 0% to 0.25% Ag: 0% to 1.00% Li: 0% to 0.50% Na: 0% to 0.05% K: 0% to 0.05% Fe: 0% to 5.00% Element group D, consisting of Cr, Ti, V, Zr, Ni, Co, Nb, Cu, Mn, Mo, W, Ag, Li, Na, K, and Fe, is a metal element. When these elements are incorporated into the coating layer, they form substitutional solid solutions and new high-melting-point intermetallic compounds. This improves wet corrosion resistance and running water corrosion resistance. Each element has an upper limit, and exceeding the upper limit tends to increase the adhesion of dross and other substances. Therefore, Na and K are each limited to 0% to 0.05%, preferably more than 0% and less than 0.05%. Cr, Ti, V, Zr, Co, Nb, Mn, Mo, and W are each limited to 0% to 0.25%, preferably more than 0% and less than 0.25%. Li is limited to 0% to 0.50% or less, preferably more than 0% and less than 0.50%. The contents of Ni, Cu, and Ag are each 0% to 1.00% or less, and preferably more than 0% and less than 1.00%. Furthermore, Fe may be unavoidably contained in the coating layer. This is because Fe may diffuse from the base steel into the coating layer during coating production. Therefore, the Fe content is 0% to 5.00% or less, and may be more than 0% and less than 5.00%.

[0040] Element Group E Sb: 0% to 0.50% Pb: 0% to 0.50% Ba: 0% to 0.25% Element Group E, consisting of Sb, Pb, and Ba, are elements with properties similar to Zn. Therefore, the inclusion of these elements does not generally provide any special effects, but they do have the effect of facilitating the formation of a spangle pattern on the plating's appearance. However, excessive inclusion of these elements may result in a decrease in corrosion resistance. Therefore, the contents of Sb and Pb are each limited to 0% to 0.50%, preferably greater than 0% and less than 0.50%. Ba is limited to 0% to 0.25%, preferably greater than 0% and less than 0.25%.

[0041] Balance: Zn and impurities Zn is a low-melting-point metal that exists on the steel material as the main phase of the plating layer. Zn is an element necessary for ensuring corrosion resistance and providing sacrificial corrosion protection to the steel material. Zn is the balance, and it is preferably contained in an amount of 50.00% or more. If the Zn content is less than 50.00%, the metal structure of the Zn-Al-Mg alloy layer will be dominated by the Al phase, and the Zn phase that exhibits sacrificial corrosion protection may be insufficient. More preferably, it is 65.00% or more, or 70.00% or more. The upper limit of the Zn content is the amount that constitutes the balance excluding elements other than Zn and impurities.

[0042] Furthermore, impurities in the coating layer refer to components contained in the raw materials or components mixed in during the manufacturing process, but not intentionally added. For example, trace amounts of components other than Fe may be mixed into the coating layer as impurities due to mutual atomic diffusion between the steel material (base steel) and the coating bath.

[0043] To identify the average chemical composition of the plating layer, the plating layer is stripped and dissolved using an acid containing an inhibitor that suppresses corrosion of the base steel (steel material) to obtain an acid solution. The resulting acid solution is then measured using ICP atomic emission spectroscopy or ICP-MS to obtain the chemical composition. There are no particular restrictions on the type of acid, as long as it can dissolve the plating layer. By measuring the area and weight before and after stripping, the plating deposition amount (g / m 2 ) can also be obtained at the same time.

[0044] Next, we will explain the microstructural morphology of the plating layer. The proportions of phases and structures contained in the plating layer significantly affect the wet corrosion resistance and flowing water corrosion resistance of plated steel. Even plating layers with the same component composition can have different properties due to the phases or structures contained in their metallographic structure, which vary depending on the manufacturing method. The metallographic structure of the plating layer can be easily confirmed using a scanning electron microscope with an energy dispersive X-ray analyzer (SEM-EDS). The approximate state of the metallographic structure of the plating layer can be confirmed by, for example, obtaining a backscattered electron image of any vertical cross section of a mirror-finished plating layer. A vertical cross section of the plating layer refers to a cross section in the thickness direction of the plating layer perpendicular to the surface of the steel material. In this embodiment, the thickness of the plating layer is 3 to 80 μm, preferably 5 to 70 μm. Therefore, it is preferable to confirm the metallographic structure using an SEM at a magnification of 500 to 5000 times. The reason for setting the lower limit of the plating layer thickness to 3 μm or more is that it may be difficult to ensure corrosion resistance at thicknesses below this limit. The reason why the upper limit of the thickness of the plating layer is set at 80 μm is that if the thickness exceeds this limit, there is a concern that the plating may peel off when the plated steel material is processed, and it may not be practical. For example, when a plating layer with a thickness of 25 μm is observed at a magnification of 2000 times, the thickness per field of view is 25 μm (plating thickness) × 40 μm (SEM field width) = 1000 μm 2 In this embodiment, since the SEM field of view for the plating layer may be a local field of view, 25 fields of view may be selected from any cross section to obtain average information on the plating layer. That is, a total of 25,000 μm 2 The metal structure in the field of view can be observed to determine the area ratio of the phase or structure that constitutes the metal structure of the plating layer.

[0045] Backscattered electron images taken by SEM are preferred because they allow easy identification of the phases or structures contained in the plating layer. Elements with small atomic numbers, such as Al, appear black, while elements with large atomic numbers, such as Zn, appear white, making it easy to determine the proportions of these structures.

[0046] To confirm each phase, the composition of the phase can be pinpointed using EDS analysis, and the phase can be identified by reading phases with approximately the same components using elemental mapping, etc. For materials for which EDS analysis can be used, elemental mapping can be used to distinguish phases with approximately the same composition. If a phase with approximately the same composition can be identified, it is possible to know the area of ​​that crystalline phase in the observation field. Once the area is known, the average crystal grain size can be calculated by calculating the equivalent circular diameter.

[0047] Furthermore, the area ratio of each phase in the observed field of view can be determined. The area ratio of a specific phase in the plating layer corresponds to the volume ratio of that phase in the plating layer.

[0048] Al Phase In this embodiment, the Al phase is a region in the plating layer where the Al content exceeds 35 mass %. This Al phase may contain Zn, but the Zn content is less than 65%. The Al phase can be clearly distinguished from other phases and structures in a SEM backscattered electron image. That is, the Al phase is often shown as the darkest phase in a SEM backscattered electron image. In this embodiment, the Al phase takes various forms in any cross section, such as a block, or a dendritic cross section such as a circular or flat shape. In this embodiment, the Al phase is referred to as [Al / MgZn 2 The Al contained in the Al-Zn / Zn ternary eutectic structure is not included in the Al phase. The Al phase has excellent water-wet corrosion resistance and running water corrosion resistance. The Al in the bath precipitates as the Al phase, the Al-Zn phase, and the Zn-Al phase described below, but it is desirable to precipitate it as the Al phase in order to ensure water-wet corrosion resistance and running water corrosion resistance.

[0049] Al—Zn Phase In this embodiment, the Al—Zn phase is a phase containing 65 to 75 mass% Zn and Al. The Al—Zn phase is an aggregate of a fine Zn phase with a grain size of approximately 1 μm (hereinafter referred to as the fine Zn phase) and a fine Al phase with a grain size of less than 1 μm (hereinafter referred to as the fine Al phase). In a molten coating layer, Al has a different crystal structure from that at room temperature, allowing a large amount of Zn phase to be dissolved, and the Al exists as a high-temperature stable phase containing the Zn phase. Meanwhile, at room temperature, the content of the Zn phase in this high-temperature stable phase is drastically reduced, and Al and Zn are equilibrium separated to exist as an Al—Zn phase containing a fine Al phase and a fine Zn phase. That is, the Al—Zn phase is a phase containing a fine Zn phase in a proportion of 65 to 75 mass%. This Al-Zn phase has a composition equivalent to the β-phase in the Al-Zn phase diagram, and has properties different from the Al phase and Zn-Al phase contained in the coating layer, so it can be distinguished in backscattered electron SEM images and wide-angle X-ray diffraction. Therefore, in this embodiment, the Al-Zn phase is defined as a phase having an Al component of 25 to 35 mass % and a Zn component of 65 to 75 mass %.

[0050] Furthermore, since the Al-Zn phase is inferior to the Al phase and the Zn-Al phase in wet corrosion resistance and corrosion resistance in running water, it is desirable to prevent the crystallization of the Al-Zn phase as much as possible in order to ensure the running water resistance of the coating. Therefore, the relationship between the area ratios of the Al-Zn phase, Al phase, and Zn-Al phase in the structure needs to satisfy the following formula (A):

[0051] ([Al]+[Zn-Al]) / [Al-Zn] is ≧0.8...(A)

[0052] In the formula (A), [Al] is the area ratio (%) of the Al phase, [Zn-Al] is the area ratio (%) of the Zn-Al phase, and [Al-Zn] is the area ratio (%) of the Al-Zn phase.

[0053] Zn—Al Phase In this embodiment, the Zn—Al phase is a phase containing 75 to 85 mass% Zn and Al. The Zn—Al phase is an aggregate of a fine Zn phase with a grain size of approximately 1 μm (hereinafter referred to as the fine Zn phase) and a fine Al phase with a grain size of less than 1 μm. The β phase, which is a high-temperature stable phase, separates into Zn and Al phases at temperatures below 250°C, incorporating surrounding Zn to form the Zn—Al phase. Although the Zn—Al phase is inferior to the Al phase, it has better water-wet corrosion resistance and running water corrosion resistance than the Al—Zn phase. Furthermore, if the Al concentration in the plating bath is 15% or less, the Al phase is unlikely to precipitate. Therefore, by controlling the precipitation of the Zn—Al phase, the water-wet corrosion resistance and running water corrosion resistance can be improved.

[0054] In order to improve the wet corrosion resistance and flowing water corrosion resistance while ensuring sacrificial corrosion protection, the total area fraction of the Al phase, Al-Zn phase, and Zn-Al phase must be 15% or more and 75% or less. Note that it is not always necessary for all of the Al phase, Al-Zn phase, and Zn-Al phase to crystallize, and any of the phases may account for 0%.

[0055] MgZn 2 Phase MgZn according to this embodiment 2 The MgZn phase is a region in the plating layer where Mg is 11 to 21 mass %, preferably 16 mass %, and Zn is 81 to 89 mass %, preferably 84 mass %. 2 In SEM backscattered electron images, the MgZn phase is often photographed as a gray color between Al and Zn. 2 The phases are Al-Zn phase, Al phase, [Al / MgZn 2 / Zn ternary eutectic structure).

[0056] MgZn 2 The MgZn phase has higher sacrificial corrosion resistance than the Al phase, but is inferior in wet corrosion resistance and running water corrosion resistance. 2 The more phases there are, the better. 2 If the phase becomes too large, the water corrosion resistance and running water corrosion resistance will decrease. 2 There is an upper limit to the area ratio of the MgZn phase in the plating layer. 2The proportion of the phase must balance both properties, so MgZn 2 The area ratio of the phase must be 10% or more and 50% or less.

[0057] [Al / MgZn 2 / Zn ternary eutectic structure] [Al / MgZn 2 / Zn ternary eutectic structure] is Al phase, MgZn 2 The eutectic structure is composed of MgZn and Zn phases, and in the backscattered electron image of the SEM, the MgZn contained as the main phase of the plating layer is 2 It is clearly distinguishable from the Al phase and the Al phase.

[0058] Zn phase [Al / MgZn 2 By having a certain degree of the ternary eutectic structure of Al / MgZn, sacrificial corrosion protection can be ensured and the end surface corrosion resistance can be improved. On the other hand, the water wetting corrosion resistance and the running water corrosion resistance are reduced. 2 The upper limit of the area ratio of the Al / MgZn ternary eutectic structure is 65% by area or less, preferably 40% by area or less. 2 There is no particular lower limit to the area ratio of the ternary eutectic structure of Ni / Zn, and it may be 0%.

[0059] Mg 2 Si phase When the plating layer contains Si, Si is 2 It may precipitate as a Si phase. 2 The Si phase has excellent corrosion resistance against water wetting and running water, so Mg 2 The presence of the Si phase acts as a barrier layer against water, which has the effect of suppressing the wear of the plating layer. 2 It is preferable to precipitate Si.

[0060] Mg 2 The presence of Si can be confirmed by X-ray diffraction measurement. In the X-ray diffraction measurement, Cu-Kα rays are used and the X-ray output is measured under the conditions of 50 kV and 300 mA. In the X-ray diffraction pattern of the plating layer surface, Mg 2The determination can be made by determining whether or not a diffraction peak of the Si phase appears. There are no particular limitations on the X-ray diffraction device, but for example, a horizontal sample type high-power X-ray diffraction device RINT-TTR III manufactured by Rigaku Corporation can be used.

[0061] The concentration of Si in the surface layer of the plating layer can be confirmed by GDS (glow discharge optical emission spectroscopy). To improve wet corrosion resistance and running water corrosion resistance, it is desirable for a Si compound to be present in the surface layer of the plating layer. Specifically, Si should be present within a range of 0.5 μm from the surface of the plating layer. The depth direction can be calculated using GDS by deriving the relationship between the number of seconds for Zn sputtering and the depth. The amount of Si required to improve wet corrosion resistance and running water corrosion resistance can be determined by comparing the intensity ratio with the main components Al and Zn. Specifically, when the integrated intensity value of element X when GDS measurement is performed to a depth of 0.5 μm from the surface of the plating layer is taken as IS(X), it is preferable that the following formula (1) be satisfied. This further improves wet corrosion resistance and running water corrosion resistance. The integrated intensity value of element X shown in the present invention refers to the strength of the plating layer and does not include the integrated intensity values ​​of the paint coating or chemical conversion coating. To confirm the GDS strength integrated value of the coating layer of a painted or chemically treated plated steel material, the paint coating, the chemical conversion coating, or both can be removed by chemical treatment, grinding, or the like, and then measurement can be performed using GDS. If it is difficult to remove the coating, the surface of the coating layer can be defined based on the GDS measurement results. Specifically, GDS measurements are performed from the surface of the plated steel material to the steel material, and the first position where the intensities of all of the main components of the coating layer, Zn, Al, and Mg, satisfy at least one-third of their respective peak intensity values, is considered to be the coating surface layer.

[0062] In the following formula (1), IΣ(Si), IΣ(Zn), and IΣ(Al) are the integrated intensities of Si, Zn, and Al detected by the GDS method within a range from the surface of the plating layer to a depth of 0.5 μm, respectively.

[0063] IΣ(Si) / (IΣ(Zn)+IΣ(Al))≧0.005…(1)

[0064] The Si intensity appears as a peak in the range from the surface of the plating layer to a depth of 0.5 μm and at the interface between the plating layer and the steel material. The peak Si intensity on the surface side of the plating layer is five times or more stronger than the Si intensity at a position halfway through the thickness of the plating layer.

[0065] Al-Ca-Si phase When Ca and Si are contained in the plating bath, an Al-Ca-Si phase precipitates as a Si compound in the plating layer. 3 Al 2 Si 2 phase, CaAl 2 Si 2 phase, CaAl 2 Si 2 phase, CaAl 1-x Si 1+x The Al-Ca-Si phase precipitates as the Mg phase (where x = 0 to 0.2). 2 The Al-Ca-Si phase has even better water-wet corrosion resistance and running water corrosion resistance than the Si phase. Therefore, when the Al-Ca-Si phase is present in the range from the surface of the plating layer to a depth of 0.5 μm, it acts as a barrier layer against water and has the effect of suppressing wear of the plating layer. More specifically, it is preferable that the following formula (2) is satisfied:

[0066] In the following formula (2), IΣ(Ca) and IΣ(Si) are the integrated intensities of Ca and Si detected by the GDS method within a range from the surface of the plating layer to a depth of 0.5 μm, respectively.

[0067] IΣ(Ca) / IΣ(Si)≧2.0…(2)

[0068] The above phases and structures constitute the main phase of the plating layer, accounting for 90% or more of the area fraction of the plating layer. Meanwhile, elements other than Zn, Mg, and Al are contained in the plating layer to form other metal phases. While some of these are effective in improving water wetting resistance, running water resistance, and corrosion resistance, their effects are not significant. Because it is difficult for the composition of the plating layer to make the total of these balances exceed 5.0 area%, the balance is 5.0 area% or less. The balance may be 0%.

[0069] As already mentioned above, the method for measuring the area ratio of the phases and structures in the coating layer is to expose a cross section of the coating layer in the thickness direction perpendicular to the surface of the steel material, and check the metal structure in a field of view of 500 to 5000 times. 25 points of view are selected from any cross section and used as the average information. That is, a total of 25,000 μm 2 The metal structure in the field of view is observed to determine the area ratio of the phase or structure that makes up the metal structure of the plating layer. To confirm each phase, the composition of the phase is pinpointed using EDS analysis, and phases with approximately the same components are identified by elemental mapping, etc. In cases where EDS analysis can be used, elemental mapping makes it possible to distinguish phases with approximately the same composition. Once a phase with approximately the same composition has been identified, it is possible to determine the area of ​​that crystalline phase in the observation field. Once the area is known, the equivalent circular diameter can be calculated to calculate the average crystal grain size, and the area ratio of each phase in the observation field can also be determined.

[0070] When performing depth-wise component analysis of the plating layer using GDS analysis, a glow discharge optical emission spectrometer (GDS) is used. For example, a LECO Japan 850A glow discharge optical emission spectrometer may be used, but the measurement device is not limited to this. When performing depth-wise analysis using argon sputtering, the analysis conditions are: argon pressure: 0.27 MPa, output power: 30 W, output voltage: 1000 V, and discharge area: within a circular area with a diameter of 4 mm. Measurements are performed using GDS analysis, which involves etching the plating layer from the surface to a depth of 0.5 μm, and obtaining an integrated value of the emission intensity of each element. Based on this integrated value, it is determined whether the above conditions (1) and (2) are met.

[0071] In addition, the Al-Ca-Si phase (Ca 3 Al 2 Si 2 phase, CaAl 2 Si 2 phase, CaAl 2 Si 2 phase, CaAl 1-x Si 1+xThe presence of the Al-Ca-Si phase can be confirmed by X-ray diffraction measurement in addition to SEM and ESD measurement. In X-ray diffraction measurement, Cu-Kα radiation is used, and the presence can be confirmed by whether or not a diffraction peak of the Al-Ca-Si phase appears in the X-ray diffraction pattern of the plating layer surface measured under conditions of an X-ray output of 50 kV and 300 mA. The X-ray diffraction device is not particularly limited, and for example, a horizontal sample type high-power X-ray diffractometer RINT-TTR III manufactured by Rigaku Corporation can be used, but is not limited thereto.

[0072] Mg 2 The presence of Si can be confirmed by X-ray diffraction measurement in addition to SEM and ESD measurement. In the X-ray diffraction measurement, Cu-Kα rays are used and the X-ray output is set to 50 kV and 300 mA. In the X-ray diffraction pattern of the plating layer surface, Mg 2 The presence of the Si phase can be confirmed by whether or not a diffraction peak of the Si phase appears. As the X-ray diffraction device, for example, a horizontal sample type high-power X-ray diffraction device RINT-TTR III manufactured by Rigaku Corporation can be used, but is not limited to this.

[0073] Next, a method for producing a plated steel material according to an embodiment of the present invention will be described. The plated steel material according to this embodiment can be produced by either an immersion hot-dip galvanizing method (batch hot-dip galvanizing method) or a continuous hot-dip galvanizing method.

[0074] There are no particular restrictions on the size, shape, surface configuration, etc. of the steel material to be plated. Regular steel, high-tensile steel, stainless steel, and other steel materials are all applicable. More specifically, various steel materials are applicable, such as general steel, Ni-preplated steel, Al-killed steel, ultra-low carbon steel, high carbon steel, various high-tensile steels, and some high-alloy steels (steels containing strengthening elements such as Ni and Cr). Steel strips of general structural steel are most preferred.

[0075] The steel material may be subjected to a surface finishing process in advance using shot blasting, abrasive brushes, etc., and the surface may be plated with Ni, Zn, Sn, etc. at a concentration of 3 g / m. 2 There is no problem if the following metal or alloy film is attached before plating. As a pretreatment of the steel material, it is preferable to thoroughly clean the steel material by degreasing and pickling.

[0076] The steel surface is 2 After thorough heating and reduction using a reducing gas such as ammonium hydroxide, the steel material is immersed in a coating bath formulated to the specified composition. For high-tensile steels, etc., the atmosphere during annealing is humidified, and internal oxidation methods are generally used to ensure coating adhesion, even on high-Si, high-Mn steels. By performing such treatments, it is possible to produce coated steel products with minimal bare spots or poor appearance, similar to ordinary steel products. Although fine-grained steel surfaces and internal oxide coating layers are observed on the base steel side of such steel products, these do not affect the performance of the present invention.

[0077] In the case of hot-dip plating, the composition of the plating layer can be controlled by the composition of the plating bath to be prepared. The plating bath is prepared by mixing predetermined amounts of pure metals to prepare an alloy of the plating bath components, for example, by a melting method in an inert atmosphere.

[0078] Immersing a steel material whose surface has been reduced in a plating bath maintained at a predetermined concentration forms a plating layer with approximately the same composition as the plating bath. If the immersion time is prolonged or if it takes a long time for solidification to be completed, the formation of the interfacial alloy layer becomes active, and the Fe concentration may become high. However, at temperatures below 500°C, the reaction with the plating layer rapidly slows, and the Fe concentration in the plating layer is usually kept below 5.00%.

[0079] To form the hot-dip coating layer, the coating bath is preferably kept at a temperature of 450°C to 550°C. The reduced steel material is then preferably immersed in the coating bath for several seconds. On the surface of the reduced steel material, Fe diffuses into the coating bath and reacts with the coating bath, which may result in the formation of an interfacial alloy layer (mainly an Al-Fe alloy layer) at the interface between the coating layer and the steel material. When an interfacial alloy layer is formed, the steel material below the interfacial alloy layer and the coating layer above are metallochemically bonded more firmly.

[0080] After immersing the steel material in the plating bath for a predetermined time, the steel material is removed from the plating bath, and the metal adhering to the surface is in a molten state. 2By wiping, the plating layer is adjusted to a predetermined thickness. The thickness of the plating layer is preferably adjusted to 3 to 80 μm. This corresponds to a coating weight of the plating layer of 10 to 500 g / m. 2 The thickness of the plating layer may be adjusted to 5 to 70 μm. This corresponds to a coating weight of approximately 20 to 400 g / m. 2 (One-sided).

[0081] After adjusting the coating weight of the coating layer, the deposited molten metal is solidified. The cooling method for solidifying the molten metal may be spraying nitrogen, air, or a mixed gas of hydrogen and helium, mist cooling, or submersion in water. Mist cooling is preferred, and mist cooling using nitrogen containing water is preferable. The cooling rate may be adjusted by adjusting the water content in the mist.

[0082] Under normal coating solidification conditions, for example, cooling from the coating bath temperature to 150°C at an average cooling rate of 5 to 20°C / sec, it may be difficult to control the structure, making it difficult to achieve the desired performance. Therefore, cooling conditions that enable the coating layer of this embodiment to be obtained are described below. As described below, under these cooling conditions, it is preferable to adjust the average cooling rate for each temperature range.

[0083] Average cooling rate between bath temperature and 380°C: 10°C / sec to 20°C / sec When Si is contained in the coating, Si compounds precipitate between the bath temperature and 380°C. A fast cooling rate tends to cause solidification of the coating without sufficient Si precipitation, resulting in uniform dispersion of Si throughout the coating layer. On the other hand, a slow cooling rate tends to cause coarsening of the Si compounds, resulting in Si concentration at the interface between the coating layer and the steel material, resulting in less Si compounds precipitating in the surface layer of the coating layer. Therefore, in order to precipitate Si compounds in the surface layer, the average cooling rate between the bath temperature and 380°C must be 10°C / sec to 20°C / sec. Even if the coating layer does not contain Si, the average cooling rate between the bath temperature and 380°C should preferably be 10°C / sec to 20°C / sec. The preferred lower limit of the average cooling rate is 15°C / sec, and the preferred upper limit is 20°C / sec. By setting the average cooling rate to the preferred lower limit or more, the Si compound tends to concentrate on the surface, and the MgZn 2By setting the average cooling rate to the preferred upper limit or less, Si compounds tend to concentrate on the surface, and Mg, which precipitates when the degree of supercooling is large, is reduced. 2 Zn 11 The effect of suppressing the precipitation of SiC and improving the workability is obtained.

[0084] Average cooling rate between 380°C and 250°C: 20°C / sec or more Between 380°C and 250°C, precipitation of Al phase occurs from the liquid phase of the molten metal attached to the steel material, and Zn-Al-MgZn 2 A ternary eutectic reaction of the phases occurs, and finally the liquid phase disappears and the coating layer is completely solidified. In addition, in the temperature range between 400°C and 300°C, the Al phase changes to the Al-Zn phase, which is a high-temperature stable phase. In other words, the precipitated Al phase contains [Al / MgZn 2 The Zn phase formed as a ternary eutectic structure of Al / MgZn is absorbed into the 2 / Zn ternary eutectic structure] is reduced. To improve water-wet corrosion resistance and flowing water corrosion resistance, the average cooling rate between 380°C and 250°C is set to at least 20°C / sec. More preferably, the average cooling rate is set to 30°C / sec or more. By setting the average cooling rate to 30°C / sec or more, the area ratio of the Al phase tends to increase. In other words, it is preferable to set the average cooling rate between 380°C and 250°C faster than the average cooling rate between the bath temperature and 380°C. The upper limit of the average cooling rate is not particularly limited, but it may be, for example, 50 / sec.

[0085] Average cooling rate between 250°C and 150°C: 20°C / sec or less The Al-Zn phase is unstable in the temperature range of 250°C to 150°C and separates into the Zn phase and the Al phase. That is, the Al-Zn phase transforms into the Al phase or the Zn-Al phase. Therefore, to improve water-wet corrosion resistance and running water corrosion resistance, it is preferable to cool slowly in this temperature range to promote the precipitation of the Al phase. Therefore, the cooling rate between 250°C and 150°C is set to 20°C / sec or less. This causes the Al-Zn phase to separate into the Al phase and the Zn phase and transform into the Al phase or the Zn-Al phase. This tendency is particularly strong when the Al concentration is high. More preferably, the cooling rate is set to 10°C / sec or less, more preferably less than 5°C / sec. By setting the average cooling rate to 10°C / sec or less, the area ratio of the Al-Zn phase is reduced, resulting in stable and excellent water-wet corrosion resistance and running water corrosion resistance. The lower limit of the average cooling rate is not particularly limited, but may be 2.5°C / sec. If the average cooling rate is less than 2.5°C, the MgZn in the coating structure may be easily cooled. 2 The phase tends to become coarse and the workability tends to become poor.

[0086] Average Cooling Rate in Temperature Range Below 150°C The average cooling rate in the temperature range below 150°C during the solidification process does not affect the constituent phases in the plating layer, so there is no need to particularly limit it, and natural cooling may be used.

[0087] The plating layer of this embodiment is formed under the above cooling conditions.

[0088] After cooling the plating layer, various chemical conversion treatments and painting treatments may be performed. In addition, to further improve corrosion resistance, welded parts, processed parts, etc. may be subjected to touch-up paint application or thermal spraying treatment.

[0089] In the plated steel material of this embodiment, a coating may be formed on the plating layer. The coating may be one layer or two or more layers. Examples of types of coatings that may be formed directly on the plating layer include chromate coatings, phosphate coatings, and chromate-free coatings. The chromate treatment, phosphate treatment, and chromate-free treatment for forming these coatings can be performed by known methods. However, since many chromate treatments can deteriorate the weldability of the plating layer surface, it is preferable that the thickness of the chromate treatment be less than 1 μm.

[0090] Chromate treatments include electrolytic chromate treatments that form a chromate film by electrolysis, reactive chromate treatments that form a film by utilizing a reaction with the material and then wash away excess treatment solution, and paint-on chromate treatments that apply a treatment solution to the substrate and dry it without rinsing with water to form a film. Any of these treatments may be used.

[0091] Examples of electrolytic chromate treatments include electrolytic chromate treatments using chromic acid, silica sol, resins (phosphoric acid, acrylic resins, vinyl ester resins, vinyl acetate acrylic emulsions, carboxylated styrene butadiene latex, diisopropanolamine-modified epoxy resins, etc.), and hard silica.

[0092] Examples of the phosphate treatment include zinc phosphate treatment, zinc calcium phosphate treatment, and manganese phosphate treatment.

[0093] Chromate-free treatments are particularly suitable because they do not place a burden on the environment. Chromate-free treatments include electrolytic chromate-free treatments that form a chromate-free film by electrolysis, reactive chromate-free treatments that form a film by utilizing a reaction with the material and then wash away excess treatment liquid, and paint-on chromate-free treatments that apply a treatment liquid to the substrate and dry it without rinsing with water to form a film. Any of these treatments may be used.

[0094] Furthermore, one or more organic resin coatings may be provided on the coating directly on the plating layer. The organic resin is not limited to a specific type, and examples thereof include polyester resins, polyurethane resins, epoxy resins, acrylic resins, polyolefin resins, and modified versions of these resins. Here, the term "modified version" refers to a resin obtained by reacting a reactive functional group contained in the structure of these resins with another compound (such as a monomer or a crosslinking agent) containing a functional group capable of reacting with the functional group.

[0095] Such organic resins may be a mixture of one or more unmodified organic resins, or a mixture of one or more organic resins obtained by modifying at least one other organic resin in the presence of at least one organic resin. The organic resin film may also contain any coloring pigment or anti-rust pigment. Water-based organic resins obtained by dissolving or dispersing them in water may also be used.

[0096] The original plates of the plated steel materials were cut out to a size of 180 mm x 100 mm from cold-rolled steel plates with a thickness (t) of 3.2 mm and a thickness (t) of 0.8 mm. Both were SS400 (general steel). A batch-type hot-dip galvanizing simulator (manufactured by Rhesca Co., Ltd.) was used, and a K thermocouple was attached to a part of the steel plate. 2 Contains 5% of N 2 The steel sheet surface was annealed at 800°C in a reducing atmosphere to fully reduce the surface, and then immersed in a plating bath of various compositions for 3 seconds. 2 The plating thickness was adjusted to 10 to 30 μm by gas wiping. However, in Examples 55 to 58, the plating thickness was 3 μm, 5 μm, 70 μm, and 80 μm. The plating thickness on the front and back of the original sheet was the same. After being pulled out of the plating bath, plated steel materials were produced under various cooling conditions A to F below.

[0097] The average chemical composition of the plating layer was measured as follows. The plating layer was stripped and dissolved using an acid containing an inhibitor that suppresses corrosion of the base steel (steel material) to obtain an acid solution. The obtained acid solution was then measured using ICP atomic emission spectroscopy or ICP-MS to obtain the average chemical composition of the plating layer.

[0098] Condition A: After the steel material was removed from the plating bath, the average cooling rate between the bath temperature and 150°C was set to any value less than 5°C / sec (comparative conditions).

[0099] Condition B: After the steel material was removed from the plating bath, the average cooling rate from the bath temperature to 150°C was set to any value between 5 and 20°C / sec (comparative conditions).

[0100] Condition C: After the steel material was removed from the plating bath, the average cooling rate between the bath temperature and 150°C was set to any value of 20°C / sec or more (comparative conditions).

[0101] Condition D: After the steel material was removed from the coating bath, the average cooling rate between the bath temperature and 380°C (range T1) was set to any value between 10°C / sec and 20°C / sec, the average cooling rate between 380°C and 250°C (range T2) was set to any value between 20°C / sec and 50°C / sec, and the average cooling rate between 250°C and 150°C (range T3) was set to any value less than 5°C / sec (preferred conditions). Therefore, in Condition D, the average cooling rates were adjusted for each temperature range. Condition D-2: After the steel material was removed from the coating bath, the average cooling rate between the bath temperature and 380°C (range T1) was set to any value between 10°C / sec and 20°C / sec, the average cooling rate between 380°C and 250°C (range T2) was set to any value between 20°C / sec and 50°C / sec, and the average cooling rate between 250°C and 150°C (range T3) was set to any value less than 10°C / sec. Therefore, in condition D-2, the average cooling rate was adjusted for each temperature range.

[0102] Condition E: After the steel material was pulled out of the coating bath, the average cooling rate between the bath temperature and 380°C (range T1) was set to any value less than 10°C / sec, the average cooling rate between 380°C and 250°C (range T2) was set to any value between more than 20°C / sec and 50°C / sec, and the average cooling rate between 250°C and 150°C (range T3) was set to any value less than 5°C / sec (comparative conditions). Therefore, under condition E, the average cooling rate was adjusted for each temperature range.

[0103] Condition F: After the steel material was pulled out of the coating bath, the average cooling rate between the bath temperature and 380°C (range T1) was set to any value of 20°C / sec or more, the average cooling rate between 380°C and 250°C (range T2) was set to any value of less than 20°C / sec, and the average cooling rate between 250°C and 150°C (range T3) was set to any value of 5°C / sec or more (comparative conditions). Therefore, under condition F, the average cooling rate was adjusted for each temperature range.

[0104] Phase and structure in the plating layer (MgZn 2 phase, Al-containing phase, [Al / MgZn 2 / Zn ternary eutectic structure], Mg 2 The area ratio of the Al-Si phase, Al-Ca-Si phase, and the remainder was measured as described above by exposing a cross section of the plating layer in the thickness direction perpendicular to the surface of the steel material, and observing the metal structure in a field of view of 500 to 5000 times. 2 The metal structure was observed in the field of view to determine the area ratio of the phases or structures that make up the metal structure of the plating layer. To confirm each phase, the composition of the phase was pinpointed using EDS analysis, and phases with approximately the same components were identified by reading them using elemental mapping, etc. Elemental mapping made it possible to distinguish phases with approximately the same composition.

[0105] Mg 2 The presence of Si was also confirmed by X-ray diffraction measurement. In the X-ray diffraction measurement, Cu-Kα rays were used and the X-ray output was measured under conditions of 50 kV and 300 mA. The X-ray diffraction pattern of the plating layer surface showed Mg 2 The determination was made based on whether or not a diffraction peak of the Si phase appeared. The X-ray diffractometer used was a horizontal sample type high-power X-ray diffractometer RINT-TTR III manufactured by Rigaku Corporation.

[0106] IS(Si) / (IS(Zn)+IS(Al)) and IS(Ca) / IS(Si) were measured by performing GDS analysis on the plating layer in the depth direction. Specifically, the analysis conditions for depth direction analysis using argon sputtering were argon pressure: 0.27 MPa, output power: 30 W, output voltage: 1000 V, and discharge region: within a circular region with a diameter of 4 mm. GDS measurement was performed while etching to a depth of 0.5 μm from the surface of the plating layer, and the integrated intensity values ​​of Si, Zn, and Al were obtained to calculate IS(Si) / (IS(Zn)+IS(Al)) and IS(Ca) / IS(Si).

[0107] Al-Ca-Si phase (Ca 3 Al 2 Si 2 phase, CaAl 2 Si 2 phase, CaAl 2 Si 2 phase, CaAl 1-x Si 1+x The presence of the Al-Ca-Si phase was confirmed by X-ray diffraction measurement. The X-ray diffraction measurement was performed using Cu-Kα radiation at an X-ray output of 50 kV and 300 mA. The X-ray diffraction pattern of the plating layer surface was measured, and the Al-Ca-Si phase was determined by whether a diffraction peak of the Al-Ca-Si phase appeared. The X-ray diffraction device used was a horizontal sample-mounted high-power X-ray diffractometer RINT-TTR III manufactured by Rigaku Corporation.

[0108] (Evaluation of sacrificial corrosion protection) A test piece with a plate thickness (t) of 3.2 mm was cut into a size of 120 mm x 50 mm, and one end surface that came into contact with the frame was painted, while the other cut end surfaces were left uncured. The JASO M609 test was then performed to evaluate sacrificial corrosion protection. The occurrence of red rust on the flat surface was confirmed in a combined cycle test. Red rust was considered to have occurred when the red rust area ratio was 5% or more. The sacrificial corrosion protection was evaluated as follows: "B" was considered a failure, and "A" to "S" were considered passing.

[0109] Red rust was observed in less than 200 cycles: "B" Red rust was observed in 200 cycles: "A" Red rust was observed in 200 to 350 cycles: "AA" Red rust was observed in 350 to 500 cycles: "AAA" No red rust was observed in 500 cycles: "S"

[0110] (Evaluation of Water Wet Corrosion Resistance and Flowing Water Corrosion Resistance) A test piece with a plate thickness (t) of 0.8 mm was cut into a size of 120 mm x 60 mm, and a vinyl plate was attached to create a flow path with a width of 20 mm and a length of 100 mm, which was used as a sample. The sample was set at an angle of 15° from the horizontal, and artificial rainwater (Cl) was intermittently injected at 6 ml / min from the upstream of the flow path through a droplet nozzle. - : 10 ppm, SO 4 2- : 40 ppm, NO 3 - (Adjusted to a concentration of 20 ppm. Further, an aqueous NaOH solution was added to adjust the pH to 5). The amount of droplets was adjusted to 100 to 200 μl per drop. When red rust was observed on 5% or more of the flow path area, it was considered that red rust had occurred, and the time until the red rust had occurred was evaluated as follows. In terms of pass / fail for water corrosion, "B" below was considered a failure, and "A" to "S" were considered pass.

[0111] If red rust appeared in less than 8 weeks: "B" If red rust appeared in 8 to 12 weeks: "A" If red rust appeared in 12 to 14 weeks: "AA" If red rust appeared in 14 to 16 weeks: "AAA" If red rust did not appear for 16 weeks or more: "S"

[0112] (Workability Evaluation) Test specimens with a thickness (t) of 0.8 mm were cut into 30 mm x 100 mm pieces, subjected to a 2t 180° bending process (a test in which a spacer twice the thickness of the specimen was inserted and a 180° bending process was performed), and then bent back to a flat state. A Cellotape (registered trademark) peeling test was performed on the inner bent section. After the peeling test, the area of ​​peeled plating on the inner bent surface was measured. The inner bent section was defined as a region within 3 mm from the apex of the bent section on the inner bent surface, i.e., an area of ​​30 mm x 6 mm, and the workability was evaluated as the area ratio of the peeled plating area to the inner bent section. In the workability evaluation, a "B" below was deemed a failure, and "A" to "S" were deemed a pass.

[0113] Peeled area is over 10%: "B" Peeled area is over 5% but not more than 10%: "A" Peeled area is 5% or less: "AA" No peeling: "S"

[0114] As shown in Tables 1A to 5B, Nos. 4 to 25, 27, 28, 30, 32, 33, 35 to 37, 39, 40, 43 to 45, 47, 48, and 53 to 58 (all examples) were manufactured using the preferred cooling conditions of the present invention, and the average chemical composition of the plating layer was within the appropriate range, and the area ratio of the phase and structure of the plating layer was within the appropriate range. This resulted in excellent sacrificial corrosion protection, wet corrosion resistance, running water corrosion resistance, and workability. The Zn content of the plating layer in each example was 50% or more.

[0115] Nos. 1 to 3 (comparative examples) have low Al and Mg contents, and MgZn 2 phase and [Al / MgZn 2 The area ratio of the ternary eutectic structure of Cu / Zn was outside the appropriate range. In addition, the manufacturing conditions were outside the preferred range. As a result, the sacrificial corrosion resistance, wet corrosion resistance, running water corrosion resistance, and workability were inferior.

[0116] No. 26 (comparative example) has a small amount of Mg and MgZn 2 The area ratio of the phase was outside the appropriate range, which resulted in inferior sacrificial corrosion resistance, wet corrosion resistance, running water corrosion resistance, and workability.

[0117] No. 29 (Comparative Example) had an excessive amount of Sn, which resulted in inferior sacrificial corrosion protection, wet corrosion resistance, running water corrosion resistance, and workability.

[0118] No. 31 (Comparative Example) had an excessive amount of Bi, which resulted in inferior sacrificial corrosion protection, wet corrosion resistance, running water corrosion resistance, and workability.

[0119] No. 34 (Comparative Example) had an excessive amount of In. The manufacturing conditions were outside the preferred range. Furthermore, the ([Al] + [Zn - Al]) / [Al - Zn] ratio was less than 0.8. This resulted in inferior sacrificial corrosion resistance, wet corrosion resistance, running water corrosion resistance, and workability.

[0120] No. 38 (Comparative Example) had excessive amounts of La and Ce. Furthermore, the manufacturing conditions were outside the preferred ranges. Furthermore, the ([Al] + [Zn-Al]) / [Al-Zn) ratio was less than 0.8. This resulted in inferior sacrificial corrosion resistance, wet corrosion resistance, running water corrosion resistance, and workability.

[0121] No. 41 (Comparative Example) had an excessive Sr content and the manufacturing conditions were outside the preferred ranges, resulting in inferior sacrificial corrosion resistance, wet corrosion resistance, running water corrosion resistance, and workability.

[0122] No. 42 (comparative example) had an excessive amount of Mg. 2 The area ratio of the phase was outside the appropriate range, which resulted in inferior sacrificial corrosion resistance, wet corrosion resistance, running water corrosion resistance, and workability.

[0123] No. 46 (Comparative Example) had an excessive amount of P. This resulted in inferior sacrificial corrosion protection, wet corrosion resistance, running water corrosion resistance, and workability.

[0124] No. 49 (Comparative Example) had excessive amounts of Al and Ca. Furthermore, the manufacturing conditions were outside the preferred ranges. Furthermore, the ([Al] + [Zn - Al]) / [Al - Zn] ratio was less than 0.8. This resulted in inferior sacrificial corrosion resistance, wet corrosion resistance, running water corrosion resistance, and workability.

[0125] No. 50 (Comparative Example) had excessive amounts of Al and Mg. In addition, the manufacturing conditions were outside the preferred ranges. As a result, the sacrificial corrosion resistance, wet corrosion resistance, running water corrosion resistance, and workability were inferior.

[0126] No. 51 (Comparative Example) had an excessive amount of Al, which resulted in inferior sacrificial corrosion protection, wet corrosion resistance, running water corrosion resistance, and workability.

[0127] No. 52 (Comparative Example) had an excessive amount of Al. The manufacturing conditions were outside the preferred range. Furthermore, the total of the Al phase, Al—Zn phase, and Zn—Al phase exceeded 75%. This resulted in inferior sacrificial corrosion protection, wet corrosion resistance, running water corrosion resistance, and workability.

[0128]

[0129]

[0130]

[0131]

[0132]

[0133]

[0134]

[0135]

[0136]

[0137]

[0138]

[0139]

[0140]

Claims

1. A plated steel material having a steel material and a plating layer arranged on the surface of the steel material, wherein the average chemical composition of the plating layer is, in mass %, Al: 10.0% to 40.0%, Mg: more than 4.0% to 8.5%, Si: 0% to 5.0%, Ca: 0% to 3.00%, Sn: 0% to 3.00%, Bi: 0% to 1.00%, In: 0% to 1.00%, Y: 0% to 0.50%, La: 0% to 0.50%, Ce: 0% to 0.50%, Sr: 0% to 0.50%, B: 0% to 1.00%, P: 0% to 0.50%, Cr: 0% to 0.25%, Ti: 0% to 0.25%, V: 0% to 0.25%, Zr: 0% to 0.25%, Ni: 0% to 1.00%, Co: 0% to 0.25%, Nb: 0% to 0.25%, Cu: 0% to 1.00%, Mn: 0% to 0.25%, Mo: 0% to 0.25%, W: 0% to 0.25%, Ag: 0% to 1.00%, Li: 0% to 0.50%, Na: 0% to 0.05%, K: 0% to 0.05%, Fe: 0% to 5.00%, Sb: 0% to 0.50%, Pb: 0% to 0.50%, Ba: 0% to 0.25%, The remainder: consists of Zn and impurities, In a cross section of the coating layer perpendicular to the surface of the steel material, the structure observed with a scanning electron microscope is, in terms of area fraction, MgZn 2 phase: 10% or more and 50% or less, the total of Al phase, Al-Zn phase and Zn-Al phase: 15% or more and 75% or less, [Al / MgZn 2 and the area ratio (([Al] + [Zn-Al]) / [Al-Zn]) of the total of the Al phase and the Zn-Al phase to the Al-Zn phase is 0.8 or more.

2. The plated steel material according to claim 1, wherein in the average chemical composition of the plating layer, Si is 0.05% to 5.0%, and the integrated strength value of each element when depth analysis is performed by the GDS method in the surface layer from the surface of the plating layer to a depth of 0.5 μm satisfies the following formula (1). IΣ(Si) / (IΣ(Zn)+IΣ(Al))≧0.005 (1) However, IΣ(Si), IΣ(Zn), and IΣ(Al) in equation (1) are the integrated intensity values of Si, Zn, and Al detected by the GDS method, respectively.

3. In the average chemical composition of the plating layer, Ca is 0.01% to 3%, and in the plating layer, Ca 3 Al 2 Si 2 phase, CaAl 2 Si 2 phase, CaAl 2 Si 2 phase, CaAl 1-x Si 1+x 3. The plated steel material according to claim 1 or 2, comprising any one of the following phases (where x = 0 to 0.2), wherein the integrated intensity values ​​of each element in a surface layer from the surface of the plated layer to a depth of 0.5 μm, when depth analysis is performed by the GDS method, satisfy the following formula (2): IΣ(Ca) / IΣ(Si)≧2.0 (2), where IΣ(Ca) and IΣ(Si) are the integrated intensity values ​​of Ca and Si detected by the GDS method, respectively.