Temporary fixation composition, bonded structure manufacturing method, and use of temporary fixation composition
Patent Information
- Application Number
- MYPI2025001012
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-08-31
- Filing Date
- 2023-07-26
- Publication Date
- 2024-02-29
AI Technical Summary
Conventional temporary fixing agents for semiconductor devices, such as those used in power devices, often fail to solidify quickly, leading to longer processing times and insufficient tackiness due to their liquid state or slow solidification, which can result in penetration into the bonded body and reduced adhesion.
A temporary fixing composition containing a first organic component that is solid at 25°C with a 95% mass reduction temperature of 300°C or less, used in a proportion of 42% to 95% by mass, which quickly solidifies after application and maintains tackiness, allowing for rapid bonding without residue, combined with a second organic component that is liquid at 25°C with a 95% mass reduction temperature of 300°C or less, ensuring fluidity and short solidification time.
The composition enables rapid solidification and maintains tackiness, preventing penetration into the bonded structure over time, ensuring reliable adhesion even with extended processing times, thus improving the efficiency and effectiveness of the bonding process.
Smart Images

Figure PI2025001012_DRAWING_001
Abstract
Description
Temporary fixing composition, method for manufacturing joined structure, and use of temporary fixing composition
[0001] The present invention relates to a composition used for temporarily fixing two workpieces to be joined prior to joining, and its use. The present invention also relates to a method for producing a joined structure using the composition.
[0002] In recent years, semiconductor devices known as power devices have come into widespread use as power conversion and control devices, such as inverters. Unlike integrated circuits such as memories and microprocessors, power devices are designed to control high currents, and therefore generate a great deal of heat during operation. Therefore, it is necessary to use materials with better heat dissipation properties. Instead of using conventional solder, various technologies have been proposed for power devices, which use pastes containing metal particles that limit the use of harmful chemicals. These pastes are then applied to the target object by various coating methods and then fired.
[0003] For example, Patent Document 1 describes a method in which a paste containing silver particles is placed between a semiconductor chip and a chip mounting portion, and the semiconductor chip and the chip mounting portion are bonded by a sintered body of the silver particles. In this method, a temporary bonding agent having tackiness is supplied so that it has a portion that comes into contact with the chip mounting portion, and the semiconductor chip is mounted on the paste so that part of the back surface of the semiconductor chip comes into contact with the temporary bonding agent.
[0004] US2018 / 247884A1
[0005] However, because the temporary fixing agent described in Patent Document 1 is liquid, it may not solidify after application or may take a long time to solidify, lengthening the process time for chip mounting. As a result, there is a problem in that the temporary fixing agent penetrates over time into the dried film of the paste that becomes the bonded body, resulting in insufficient tackiness. Therefore, an object of the present invention is to provide a temporary fixing composition that solidifies quickly after application, a method for producing a bonded structure using the composition, and a method for using the composition.
[0006] The present invention provides a temporary fixing composition used to temporarily fix a first material to be joined and a second material to be joined prior to joining the two materials, the composition comprising a first organic component in a proportion of 42% by mass or more and 95% by mass or less, the first organic component being solid at 25°C and having a 95% mass loss temperature in nitrogen of 300°C or less.
[0007] The present invention also provides a method for manufacturing a bonded structure, comprising the steps of temporarily fixing a first material to be bonded and a second material to be bonded by interposing a temporary fixing composition between them and then firing the temporarily fixed material to bond them together, wherein the temporary fixing composition uses a composition that is solid at 25°C and contains a first organic component in a proportion of 42% by mass or more and 95% by mass or less, the first organic component being solid at 25°C and having a 95% mass reduction temperature in nitrogen of 300°C or less.
[0008] Furthermore, the present invention provides use of a composition containing a first organic component in a proportion of 42% by mass or more and 95% by mass or less, the first organic component being solid at 25°C and having a 95% mass loss temperature in nitrogen of 300°C or less, for temporarily fixing a first material to be joined and a second material to be joined prior to joining the two materials.
[0009] 1(a) to 1(d) are schematic diagrams sequentially showing the steps of joining two members to be joined using the temporary fixing composition of the present invention.
[0010] The present invention relates to a temporary fixing composition. The temporary fixing composition is used to temporarily fix a first material to a second material to be joined prior to joining (i.e., permanently fixing) the two materials. The temporarily fixed first material to be joined and the second material to be joined are then joined to form a bonded structure in a subsequent process, such as a firing process. "Temporarily fixed" refers to a state in which the first material to be joined and the second material to be joined are fixed together, and the fixed state changes when a large external force is applied, but does not change when a small external force is applied (e.g., a force strong enough to cause either the first or second material to fall under its own weight when the temporarily fixed first material to be joined and the second material to be joined are placed so that the joining surfaces of the two materials are oriented vertically).
[0011] There are no particular limitations on the types of the first and second materials to be joined. In general, it is preferable that both the first and second materials to be joined contain a metal on their joining surfaces. For example, at least one of the first and second materials to be joined can be a member having a surface made of metal.
[0012] Furthermore, a structure containing metal fine particles can be used as at least one of the first and second materials to be joined. This structure can be, for example, a dried paste or sheet containing metal fine particles and at least one of a resin and an organic solvent. Specifically, a member having a metal surface can be used as the first material to be joined, and the structure can be used as the second material to be joined. When a dried paste is used as the structure, it is preferable to apply the paste to a supporting substrate made of a metal such as copper and dry it to obtain a dried paste. When a sheet is used as the structure, the sheet can be pressure-bonded to a supporting substrate made of a metal such as copper, or it can be used without pressure-bonding. When used without pressure-bonding, it is preferable to use a temporary fixing composition between the sheet and the supporting substrate made of a metal such as copper.
[0013] In addition, when the above-mentioned "structure" is heated in the next step, for example, the metal fine particles contained in the structure are sintered together, so the structure can be considered a sintering precursor. Therefore, in this specification, the "structure" will also be referred to as a "sintering precursor" hereinafter.
[0014] When the first material to be joined is a member having a metal surface and the second material to be joined is a sintered precursor, the metal in the first material to be joined and the metal of the metal fine particles in the second material to be joined may be the same or different. The term "metal" as used herein refers to a metal itself that does not form a compound with other elements, or an alloy of two or more metals. While there are no particular limitations on the type of metal, considering that the temporary fixing composition of the present invention is used in combination with a solder-substitute joining member, it is advantageous to use a metal with a melting point higher than that of solder. Examples of such metals include copper, silver, gold, aluminum, titanium, nickel, and alloys of two or more of these.
[0015] When at least one of the first and second workpieces has a metal surface, the metal surface may be made of a single metal, or may be made of two or more metals. When made of two or more metals, the surface may be an alloy. The metal surface is generally preferably flat, but may be curved in some cases.
[0016] The metal fine particles contained in the structure may be composed of one kind of metal, an alloy of two or more kinds of metals, or a mixture of two or more kinds of metal fine particles of different metal species.
[0017] Volume cumulative particle size D of metal fine particles SEM50 It is preferable that the thickness of the first material to be joined and the second material to be joined be 0.01 μm or more and 30 μm or less in order to maintain a good bond between the first material to be joined and the second material to be joined. SEM50 The volume cumulative particle diameter D is more preferably 0.03 μm or more and 20 μm or less, and even more preferably 0.05 μm or more and 15 μm or less. SEM50can be determined, for example, by the following measurement method. Metal fine particles with clear contours are photographed using a scanning electron microscope (SEM) at a magnification of 10,000 times or more and 150,000 times or less. After the SEM image of the metal fine particles is read using Mac-View manufactured by Mountech Co., Ltd., 50 or more metal fine particles on the SEM image are randomly selected and the particle diameters (Heywood diameters) of the particles are measured. Next, the volume of the particles is calculated from the obtained Heywood diameter assuming that the particles are spherical, and the particle diameter at 50% by volume of the cumulative volume is determined as the volume cumulative particle diameter D SEM50 Let's say.
[0018] There is no particular limitation on the shape of the metal fine particles, and examples thereof include spherical, polyhedral, flat, amorphous, and combinations thereof. The metal fine particles may have two or more peaks in their particle size distribution.
[0019] The metal fine particles may have a surface treatment agent attached to their surfaces, which can prevent excessive aggregation and oxidation of the metal fine particles.
[0020] The surface treatment agent is not particularly limited, and examples thereof include fatty acids, aliphatic amines, silane coupling agents, titanate coupling agents, and aluminate coupling agents. The use of these agents interacts with the particle surfaces, improving compatibility with the organic solvents contained in the paste and the resins in the sheet, thereby improving paste fluidity and preventing oxidation of the particle surfaces. Specific examples of fatty acids or aliphatic amines include benzoic acid, pentanoic acid, hexanoic acid, octanoic acid, nonanoic acid, decanoic acid, lauric acid, palmitic acid, oleic acid, stearic acid, pentylamine, hexylamine, octylamine, decylamine, laurylamine, oleylamine, and stearylamine. These fatty acids and aliphatic amines can be used alone or in combination of two or more.
[0021] The paste and its dried sinter precursor may contain an adjuster to adjust various properties of the paste or sinter precursor. Examples of adjusters include reducing agents, viscosity adjusters, and surface tension adjusters. Reducers that promote sintering of copper particles are preferred, such as monoalcohols, polyhydric alcohols, amino alcohols, citric acid, oxalic acid, formic acid, ascorbic acid, aldehydes, hydrazine and its derivatives, hydroxylamine and its derivatives, dithiothreitol, phosphites, hydrophosphites, phosphorous acid and its derivatives, etc. Viscosity adjusters can be used to adjust the viscosity of the paste, such as ketones, esters, alcohols, glycols, hydrocarbons, and polymers. Surface tension adjusters can be used to adjust the surface tension of the paste, such as acrylic surfactants, silicone surfactants, polymers such as alkyl polyoxyethylene ethers and fatty acid glycerol esters, and monomers such as alcohols, hydrocarbons, esters, and glycols.
[0022] When obtaining a dried product from the paste, it is not necessary to remove all of the organic solvent; it is sufficient to remove only enough of the organic solvent to cause the paste coating to lose fluidity. Therefore, the organic solvent may remain in the sinter precursor. The proportion of the organic solvent contained in the sinter precursor can be, for example, 15% by mass or less, and particularly 10% by mass or less.
[0023] The organic solvent is not particularly limited in type, as long as it can disperse metal particles to form a paste. Examples of organic solvents include monoalcohols, polyhydric alcohols, polyhydric alcohol alkyl ethers, polyhydric alcohol aryl ethers, polyethers, esters, nitrogen-containing heterocyclic compounds, amides, amines, terpene alcohols, ketones, and saturated hydrocarbons. These organic solvents can be used alone or in combination of two or more.
[0024] Examples of monoalcohols that can be used include 1-propanol, 1-butanol, 1-pentanol, 1-hexanol, cyclohexanol, 1-heptanol, 1-octanol, 1-nonanol, 1-decanol, glycidol, benzyl alcohol, methylcyclohexanol, 2-methyl-1-butanol, 3-methyl-2-butanol, 4-methyl-2-pentanol, 2-propanol, 2-ethylbutanol, 2-ethylhexanol, 2-octanol, 2-methoxyethanol, 2-ethoxyethanol, 2-n-butoxyethanol, and 2-phenoxyethanol.
[0025] Examples of polyhydric alcohols that can be used include ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tetraethylene glycol, and hexylene glycol.
[0026] Examples of polyhydric alcohol alkyl ethers that can be used include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, and propylene glycol monobutyl ether.
[0027] Examples of polyhydric alcohol aryl ethers that can be used include ethylene glycol monophenyl ether and the like. Examples of polyethers that can be used include polyethylene glycol and polypropylene glycol. Examples of esters that can be used include ethyl cellosolve acetate, butyl cellosolve acetate, and γ-butyrolactone. Examples of nitrogen-containing heterocyclic compounds that can be used include N-methylpyrrolidone and 1,3-dimethyl-2-imidazolidinone. Examples of amides that can be used include formamide, N-methylformamide, and N,N-dimethylformamide. Examples of amines that can be used include monoethanolamine, diethanolamine, triethanolamine, tripropylamine, and tributylamine. Examples of terpene alcohols that can be used include isobornylcyclohexanol and terpineol. Examples of ketones that can be used include methyl ethyl ketone. Examples of saturated hydrocarbons that can be used include heptane, octane, nonane, decane, undecane, dodecane, tridecane, tetradecane, pentadecane, and hexadecane.
[0028] In addition, in the case of a sintered precursor consisting of a sheet in which metal fine particles are dispersed in a resin, examples of the resin include various polyolefin resins such as polyethylene, polypropylene, polymethylpentene, and copolymers thereof, various polyamide resins such as nylon 6, nylon 66, nylon 12, nylon 11, metaxylylene adipamide (mXD6), hexamethylene terephthalamide (6T), and copolymers thereof, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene-2,6-naphthalate (PEN), polymethylene terephthalate (PMT), polypropylene terephthalate (PPT), polyethylene-p-oxybenzoate, and the like. Examples of suitable resins include various polyester resins such as poly(ethylene oxide) terephthalate (PEOB), poly-1,4-cyclohexylene dimethylene terephthalate (PCT), and copolymerized polyesters with diol components such as diethylene glycol, neopentyl glycol, and polyalkylene glycol, and dicarboxylic acid components such as adipic acid, sebacic acid, phthalic acid, isophthalic acid, and 2,6-naphthalenedicarboxylic acid, as well as thermoplastic resins such as acrylic resin, methacrylic resin, polyacetal (POM) resin, polyphenylene sulfide (PPS) resin, polycarbonate resin, and chlorine-containing resins such as polyvinyl chloride (PVC) and polyvinylidene chloride (PVdC). Thermosetting resins such as phenolic resin, epoxy resin, urea resin, melamine resin, and silicone resin may also be used.
[0029] In the present invention, a bonded structure is produced by temporarily fixing a first material to be bonded and a second material to be bonded together using a temporary fixing composition, and then bonding the temporarily fixed materials together. The components of the temporary fixing composition are preferably selected in relation to the types of organic solvent and resin contained in the paste or sheet of the structure used to form the sintered precursor, and the type of surface treatment agent adhered to the surfaces of the metal fine particles contained in the paste or resin.
[0030] The temporary fixing composition contains a first organic component that is solid at 25°C and has a 95% mass loss temperature in nitrogen of 300°C or lower, preferably 280°C or lower. Being solid at 25°C allows the temporary fixing composition to solidify after application. Furthermore, the inclusion of such a first organic component allows the temporary fixing composition to be applied, solidify quickly after application, and have tackiness, and to be baked without leaving any residue. Note that "application" refers to attaching the temporary fixing composition to a target object or target portion by methods such as dripping or dispensing, pin transfer, inkjet printing, or screen printing. "Solid" refers to a rigid substance that undergoes no or very little deformation or volume change, does not flow to conform to the shape of a container, and does not diffuse to fill the entire container. Examples include stone-like, rock-like, wax-like, and wax-like substances.
[0031] The first organic component is contained in a proportion of 42% by mass or more, preferably 55% by mass or more, and more preferably 60% by mass or more, relative to 100% by mass of the temporary fixing composition. By containing 42% by mass or more relative to 100% by mass of the temporary fixing composition, the temporary fixing composition can be solidified in a short time, for example, within 240 seconds, after application in a 25°C atmosphere. On the other hand, the first organic component is preferably contained in a proportion of 95% by mass or less, more preferably 85% by mass or less, relative to 100% by mass of the temporary fixing composition. If the temporary fixing composition contains more than 95% by mass of the first organic component relative to 100% by mass of the temporary fixing composition, the fluidity during application may decrease, resulting in nozzle clogging and making application impossible. By containing the first organic component, the solidification time can be shortened, specifically to 240 seconds or less, preferably 40 seconds or less, and more preferably 5 seconds or less. This can suppress the penetration of the composition into the structure, i.e., the sintering precursor, over time, and ensure tackiness to the first and second bonded bodies, even if the process time for bonding the first and second bonded bodies is long. The above-mentioned 95% mass loss temperature is the temperature at which a sample loses 95% of its mass when it is subjected to thermogravimetric differential thermal analysis under the following conditions: in a nitrogen atmosphere (e.g., in a nitrogen flow), the sample is heated from 25°C to 40°C at a heating rate of 2°C / min, maintained at this temperature for 15 minutes, and then the temperature is increased at a heating rate of 10°C / min, and the sample has a mass of 30 mg.
[0032] Examples of the first organic component include monoalcohols, polyhydric alcohols, polyhydric alcohol alkyl ethers, polyhydric alcohol aryl ethers, esters, heterocyclic compounds, amides, amines, saturated hydrocarbons, cyclic terpene alcohols and their derivatives, ketones, and carboxylic acids. These organic components can be used alone or in combination of two or more. Among these, saturated aliphatic monoalcohols, saturated aliphatic polyhydric alcohols, saturated fatty acid esters, cyclic terpene alcohol derivatives, oxygen-containing heterocyclic compounds, and saturated aliphatic monocarboxylic acids are preferred. Preferably, these have 6 to 21 carbon atoms. Among these, myristyl alcohol, palmityl alcohol, stearyl alcohol, 1,6-hexanediol, 2,2,4-trimethyl-1,3-pentanediol, trimethylolpropane, methyl stearate, borneol, 2,4,6-triisopropyl-1,3,5-trioxane, capric acid, lauric acid, myristic acid, and palmitic acid are particularly preferred. These compounds can be used alone or in combination of two or more.
[0033] The temporary fixing composition preferably contains, in addition to the first organic component, a second organic component that is different from the first organic component. The second organic component contained in the temporary fixing composition is a substance that is unlikely to alter the first and second materials to be joined when the first and second materials are temporarily fixed together, and that can easily volatilize while the two materials are in a temporarily fixed state.
[0034] The second organic component is desirably liquid at 25°C and has a temperature at which it loses 95% of its mass in nitrogen of 300°C or less, preferably 280°C or less. By using such a second organic component in combination with the first organic component, the temporary fixing composition can be made fluid during application while retaining its tackiness, and can be baked with good workability and without leaving any residue. The temperature at which it loses 95% of its mass is measured using the same procedure as for the first organic component.
[0035] The second organic component is contained in an amount of 5% by mass or more, preferably 15% by mass or more, based on 100% by mass of the temporary fixing composition, thereby ensuring fluidity during application. Meanwhile, the second organic component is contained in an amount of 58% by mass or less, preferably 45% by mass or less, and more preferably 40% by mass or less, based on 100% by mass of the temporary fixing composition. By making the content of the second organic component 58% by mass or less based on 100% by mass of the temporary fixing composition, the solidification time after application is shortened and tackiness can be ensured.
[0036] The second organic component is preferably selected so that, in combination with the first organic component, the solidification time of the temporary fixing composition is shortened, specifically, 240 seconds or less, preferably 40 seconds or less, and more preferably 5 seconds or less. This shortens the solidification time of the temporary fixing composition as described above, thereby suppressing the penetration of the composition into the above-described structure, i.e., the sintering precursor, over time, and ensuring tackiness to these materials to be joined, even if the process time for joining the first and second objects to be joined is long.
[0037] As described above, the second organic component may be any component that does not change the state of the sintering precursor and ensures fluidity during application. Examples of such components include monoalcohols, polyhydric alcohols, polyhydric alcohol alkyl ethers, polyhydric alcohol aryl ethers, esters, heterocyclic compounds, amides, amines, saturated hydrocarbons, cyclic terpene alcohols and their derivatives, ketones, carboxylic acids, and other components similar to those listed above as organic solvents. These organic components may be used alone or in combination of two or more. Among these, saturated aliphatic polyhydric alcohols, unsaturated aliphatic monoalcohols, unsaturated fatty acid esters, tertiary amines, cyclic terpene alcohol derivatives, unsaturated aliphatic monocarboxylic acids, and saturated aliphatic hydrocarbons are preferred. Preferably, these organic components have 3 to 21 carbon atoms. Among these, particularly preferred are glycerin, 1,2,4-butanetriol, oleyl alcohol, methyl oleate, triethanolamine, 4-(1'-acetoxy-1'-methylethyl)-cyclohexanol acetate, isobornylcyclohexanol, oleic acid, and normal decane. These compounds can be used alone or in combination of two or more. The phrase "does not change the state of the sintered precursor" refers to the fact that, when 1 μL of an organic component is dropped onto the sintered precursor and the sintered precursor is dried at 110°C or less, no change is observed in the sintered precursor before and after the dropping when observed under a microscope at 140x magnification. Furthermore, this "no change is observed" also includes not only the fact that no change is observed in the sintered precursor before and after the dropping, but also the fact that no traces of the dropping are observed in the ultrasonic flaw detection image after bonding.
[0038] Examples of preferred combinations of the first organic component and the second organic component include: a combination of a C8-C21 saturated aliphatic monocarboxylic acid as the first organic component and a C8-C21 saturated aliphatic hydrocarbon as the second organic component; a combination of a C8-C21 saturated aliphatic monocarboxylic acid as the first organic component and a C8-C21 cyclic terpene alcohol derivative as the second organic component; a combination of a C8-C21 saturated fatty acid ester as the first organic component and a C8-C21 cyclic terpene alcohol derivative as the second organic component; a combination of a C8-C21 saturated aliphatic monocarboxylic acid as the first organic component and a C8-C21 unsaturated aliphatic monoalcohol as the second organic component; a combination of a C8-C21 saturated aliphatic monocarboxylic acid as the first organic component and a C8-C21 unsaturated aliphatic monocarboxylic acid as the second organic component. a combination of a C8-C21 saturated aliphatic monoalcohol as the first organic component and a C8-C21 cyclic terpene alcohol derivative as the second organic component; a combination of a C8-C21 saturated aliphatic monoalcohol as the first organic component and a C8-C21 saturated aliphatic hydrocarbon as the second organic component; a combination of a C8-C21 saturated aliphatic monoalcohol as the first organic component and a C8-C21 unsaturated aliphatic monoalcohol as the second organic component; a combination of a C8-C21 saturated aliphatic monoalcohol as the first organic component and a C8-C21 unsaturated aliphatic monocarboxylic acid as the second organic component. Preferably, for reasons of tackiness and short solidification time, the following is used: a combination of a C8-C21 saturated aliphatic monocarboxylic acid as the first organic component and a C8-C21 saturated aliphatic hydrocarbon as the second organic component. a combination of a C8-21 saturated aliphatic monocarboxylic acid as the first organic component and a C8-21 cyclic terpene alcohol derivative as the second organic component; a combination of a C8-21 saturated fatty acid ester as the first organic component and a C8-21 cyclic terpene alcohol derivative as the second organic component; a combination of a C8-21 saturated aliphatic monocarboxylic acid as the first organic component and a C8-21 unsaturated aliphatic monoalcohol as the second organic component.A combination of a C8-21 saturated aliphatic monocarboxylic acid as the first organic component and a C8-21 unsaturated aliphatic monocarboxylic acid as the second organic component, or a combination of a C8-21 saturated aliphatic monoalcohol as the first organic component and a C8-21 cyclic terpene alcohol derivative as the second organic component is preferred.
[0039] The temporary fixing composition may contain other components in addition to the first organic component and the second organic component described above, as long as the effects of the present invention are not impaired.
[0040] It is preferable that the temporary fixing composition be substantially free of organic polymer compounds. Organic polymer compounds are generally nonvolatile or hardly volatilizable substances. Therefore, the absence of organic polymer compounds in the temporary fixing composition can, for example, shorten the solidification time and suppress the permeation of the composition over time. This ensures tackiness to the materials to be joined, even when the process time for joining the first and second objects to be joined is relatively long. From this perspective, it is preferable that the temporary fixing composition be substantially free of organic polymer compounds. From a similar perspective, it is also preferable that the temporary fixing composition be substantially free of inorganic compounds. "Substantially free of organic polymer compounds" means that the temporary fixing composition is not intentionally made to contain organic polymer compounds, but the unavoidable inclusion of organic polymer compounds in the temporary fixing composition is acceptable. "Substantially free of inorganic compounds" has a similar meaning.
[0041] Examples of the organic polymer compound include polyolefins such as polyethylene, polypropylene, and ethylene-α-olefin copolymers; polyesters such as polyethylene terephthalate and polybutylene terephthalate; vinyl polymers such as polyvinyl chloride and polystyrene; (meth)acrylic acid polymers such as poly(meth)acrylic acid and polyalkyl(meth)acrylate; terpene polymers such as polyethylene glycol, terpene polymers, and terpene phenol polymers; polycarbonate, polyethersulfone, and the like.
[0042] The temporary fixing composition can be prepared by mixing the first organic component and the second organic component in a heated state at 30°C or more and 70°C or less, or by mixing the first organic component and the second organic component and then heating the mixture to 30°C or more and 70°C or less.
[0043] Next, a method for using the temporary fixing composition of the present invention will be described. Figures 1(a) to 1(d) schematically show the steps of joining a first material to be joined and a second material to be joined using the temporary fixing composition. First, as shown in Figure 1(a), a paste containing metal fine particles and an organic solvent is applied to a substrate 10 to form a coating film, and the organic solvent is removed from the coating film to form a sintered precursor, i.e., a second material to be joined 11, which is a dried product of the paste. Alternatively, a sheet containing metal fine particles dispersed in a resin is disposed on the substrate 10 to form the sintered precursor, i.e., the second material to be joined 11.
[0044] 1(a) shows a state in which a sintering precursor is formed as a second material to be joined 11 on the surface of a single substrate 10. Examples of the substrate 10 include metals such as copper, silver, nickel, gold, and aluminum, and ceramics such as alumina, silicon carbide, silicon nitride, and aluminum nitride. Metal plating or a metal pattern of copper, silver, nickel, gold, aluminum, etc. may also be formed on one or both sides of the metal or ceramic.
[0045] Next, as shown in FIG. 1( b), a temporary fixing composition 12 is applied to the surface of the second material to be joined 11. The temperature of the temporary fixing composition during application is preferably 30°C to 70°C, and the second material to be joined 11 to which the temporary fixing composition is applied is preferably not preheated or heated, but is at 20°C to 25°C. The room temperature in the room where this step is performed is preferably 20°C to 25°C. The temporary fixing composition 12 may be applied only to a part of the second material to be joined 11 (for example, a corner of the sintering precursor 11) as shown in the figure, or may be applied to the entire second material to be joined 11. The temporary fixing composition 12 can be applied by a known method, such as dispensing, pin transfer, inkjet printing, or screen printing.
[0046] 1(c), the first material to be joined 13 is superimposed on the second material to be joined 11. The surface of the first material to be joined 13 facing the second material to be joined 11 is made of metal. This superposition causes a temporary fixing composition 12 to be interposed between the two materials to be joined 11, 13. The temporary fixing composition 12 preferably does not contain any component that changes the state of the sintered precursor, which is the second material to be joined 11, so the shape of the second material to be joined 11 is stably maintained. In addition, the temporary fixing composition 12 preferably contains a component with high adhesiveness, so the temporary fixed state of the two materials to be joined 11, 13 is stably maintained.
[0047] Next, the temporarily fixed materials 11 and 13 are heated. The heating sinters the metal particles contained in the second material 11, i.e., the sintering precursor, and the materials 11 and 13 are bonded together. This process is shown in FIG. 1( d ). Since heating is typically performed in a heating furnace (not shown), the temporarily fixed materials 11 and 13 shown in FIG. 1( c ) are transported from one stage to another by a transport means (not shown). The materials 11 and 13 are reliably and quickly fixed together by the temporary fixing composition 12, effectively preventing misalignment between the materials 11 and 13 during transport. As a result, the materials 11 and 13 are reliably bonded together in the intended positions in the heating furnace.
[0048] When heating the two materials to be joined 11, 13, pressure may be applied using a pressure member 14. In particular, when the first material to be joined 13 is a semiconductor device, it is necessary to increase the bonding reliability between the first material to be joined 13 and the second material to be joined 11, and therefore the pressure member 14 may be used for the purpose of forming a dense sintered structure. When the pressure member 14 is used, misalignment is likely to occur between the two materials to be joined 11, 13 in a temporarily fixed state. However, if the two materials to be joined 11, 13 are temporarily fixed using the temporary fixing composition 12 of the present invention, misalignment is less likely to occur between the two materials to be joined 11, 13 even when the materials to be joined 11, 13 are pressed by the pressure member 14.
[0049] The pressure applied by the pressure member 14 during heating is preferably 0.01 MPa or more and 40 MPa or less in order to reliably bond the two workpieces 11, 13. The heating temperature is preferably 200°C or more and 300°C or less. Heating at this temperature ensures that the metal microparticles in the sintering precursor, which is the second workpiece 11, are sintered reliably, and the temporary fixing composition 12 can be removed by heat. The firing atmosphere can be any of an oxygen-containing atmosphere such as air, an inert atmosphere such as nitrogen, and a hydrogen-containing atmosphere. This heating process bonds the substrate 10 and the workpieces 11 and 13 together.
[0050] The present disclosure also encompasses the following inventions. [1] A temporary fixing composition used to temporarily fix a first material to be joined and a second material to be joined prior to joining the two materials, the temporary fixing composition comprising a first organic component that is solid at 25°C and has a 95% mass loss temperature in nitrogen of 300°C or lower, in a proportion of 42% by mass or more and 95% by mass or less. [2] The temporary fixing composition according to [1], comprising a second organic component that is liquid at 25°C and has a 95% mass loss temperature in nitrogen of 300°C or lower, in a proportion of 5% by mass or more and 58% by mass or less. [3] The temporary fixing composition according to [1] or [2], which has a solidification time of 240 seconds or less after application. [4] The temporary fixing composition according to any one of [1] to [3], which is substantially free of an organic polymer compound. [5] A method for manufacturing a bonded structure, comprising the steps of: temporarily fixing a first material to be joined and a second material to be joined by interposing a temporary fixing composition between them; and firing the temporarily fixed material to bond them together, wherein the temporary fixing composition uses a composition that is solid at 25°C and contains a first organic component in a proportion of 42% by mass to 95% by mass, the first organic component being solid at 25°C and having a 95% mass reduction temperature in nitrogen of 300°C or lower. [6] The manufacturing method according to [5], wherein the temporary fixing composition contains a second organic component that is liquid at 25°C and has a 95% mass reduction temperature in nitrogen of 300°C or lower, the second organic component being liquid at 25°C and having a 95% mass reduction temperature in nitrogen of 300°C or lower, the second organic component being liquid at 5% by mass to 58% by mass. [7] The manufacturing method according to [5] or [6], wherein at least one of the first material to be joined and the second material to be joined comprises a sintered precursor of a structure containing metal fine particles. [8] Use of a composition containing 42% by mass or more and 95% by mass or less of a first organic component that is solid at 25°C and has a 95% mass loss temperature in nitrogen of 300°C or less, for temporarily fixing a first material to be joined and a second material to be joined prior to joining the two. [9] Use of the composition according to [8], containing 5% by mass or more and 58% by mass or less of a second organic component that is liquid at 25°C and has a 95% mass loss temperature in nitrogen of 300°C or less, for temporarily fixing the first material to be joined and the second material to be joined prior to joining the two.
[0051] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "% by mass."
[0052] Examples 1-5 and Comparative Examples 1-2 (1) Preparation of Temporary Fixing Compositions Lauric acid (solid at 25°C, 95% reduction temperature 256°C) was used as the first organic component. Normal decane (liquid at 25°C, 95% reduction temperature 144°C) was used as the second organic component. Both were mixed at 50°C to prepare temporary fixing compositions. The ratios of the first organic component and the second organic component in the temporary fixing compositions are as shown in Table 1. These temporary fixing compositions did not contain organic polymer compounds or inorganic compounds.
[0053] (2) Preparation of bonding paste Two types of copper particles (spherical, D) synthesized by a wet method were used. SEM50 = 0.14 μm; flake D SEM50 A bonding paste was prepared by mixing copper powder (particle size: 4.7 μm), organic solvents (hexylene glycol and polyethylene glycol (number average molecular weight: 300)), and other adjusters such as a solid reducing agent. Bis(2-hydroxyethyl)iminotris(hydroxymethyl)methane (hereinafter also referred to as "BIS-TRIS") was used as the solid reducing agent. The proportion of copper particles in the bonding paste was 74%, the proportion of hexylene glycol was 23.4%, and the proportion of polyethylene glycol was 0.74%. Furthermore, the proportion of spherical particles among the copper particles was 70%, and the proportion of flake particles was 30%. Furthermore, the proportion of BIS-TRIS used as the solid reducing agent was 1.85%.
[0054] (3) Formation of second bonded material made of sintered precursor The bonding paste was applied by screen printing to a copper plate (20 mm × 20 mm, thickness 0.5 mm) substrate to form a rectangular coating film with dimensions of 0.6 cm × 0.6 cm and a thickness of 100 μm. This coating film was dried in the air at 110 ° C for 20 minutes to remove the organic solvent, thereby forming a second bonded material made of a dried sintered precursor.
[0055] (4) Dripping or Application of Temporary Fixing Composition and Laminating the First Material to Be Bonded The temporary fixing composition was dripped as soon as the temperature of the sintered precursor formed in (3) reached room temperature (22°C). An Ag-plated alumina chip (0.5 cm x 0.5 cm, 0.5 mm thick, 50 mg mass) was prepared as the first material to be bonded as a model component of a semiconductor device. A compact mounter (SMT-64RH, manufactured by Okuhara Electric Co., Ltd.) was used to laminate this alumina chip and the sintered precursor formed in (3). The temporary fixing composition prepared in (1) was injected into a 10 ml syringe equipped with a plastic needle (both manufactured by Musashi Engineering), and the syringe was set in the temperature control unit attached to the mounter. A fan-type Peltier temperature control unit, PELTIER MASTER (manufactured by Musashi Engineering), was used as the temperature control unit. The temperature was set to 50°C, and the device was left standing for 30 minutes until the temperature of the temporary fixing composition stabilized. The discharge pressure, discharge time, and back pressure were then adjusted to achieve a coating amount of 0.04 mg per drop. The temporary fixing composition was applied drop by drop to the corner of the sintered precursor using the mounter's program. The Ag-plated surface of the alumina chip was then placed on top of the sintered precursor, and a load of 0.8 MPa was applied for 2 seconds. The alumina chip was positioned so that the intersection of the diagonals of the alumina chip and the sintered precursor coincided, and the alumina chip and the sintered precursor were parallel on each side. The temporary fixing composition was applied so that each end of the alumina chip was at the center of each coating. This alignment was performed using image processing within the mounter program. Note that these operations, including application, were performed at room temperature of 22°C, and the second workpiece was not preheated.
[0056] [Examples 6-10] As shown in Table 2, examples 6-10 were produced in the same manner as in Example 1-5 up to (4) superposition of the first bonded material, except that 4-(1'-acetoxy-1'-methylethyl)-cyclohexanol acetate (liquid at 25°C, 95% reduction temperature 236°C) was used instead of normal decane as the second organic component.
[0057] [Example 11] As shown in Table 3, a bonding agent was produced in the same manner as in Example 6-10 up to (4) superposition of the first bonded material, except that methyl stearate (solid at 25°C, 95% reduction temperature 298°C) was used instead of lauric acid as the first organic component.
[0058] [Example 12] As shown in Table 3, a bonding method was prepared in the same manner as in Example 1-5 up to (4) superposition of the first bonded material, except that oleyl alcohol (liquid at 25°C, 95% reduction temperature 295°C) was used instead of normal decane as the second organic component.
[0059] [Example 13] As shown in Table 3, a bonding method was prepared in the same manner as in Example 1-5 up to (4) superposition of the first bonded material, except that oleic acid (liquid at 25°C, 95% reduction temperature 321°C) was used instead of normal decane as the second organic component.
[0060] [Example 14] As shown in Table 3, a bonding agent was prepared in the same manner as in Example 6-10 up to (4) superposition of the first bonded material, except that palmityl alcohol (solid at 25°C, 95% reduction temperature 270°C) was used instead of lauric acid as the first organic component.
[0061] Comparative Example 3 As shown in Table 4, a comparative example was produced in the same manner as in Example 6-10 up to (4) superposition of the first bonded material, except that stearic acid (solid at 25°C, 95% reduction temperature 314°C) was used instead of lauric acid as the first organic component.
[0062] Comparative Example 4 As shown in Table 4, a comparative example was produced in the same manner as in Example 6-10 up to (4) superposition of the first bonded material, except that lauryl alcohol (liquid at 25°C, 95% reduction temperature 229°C) was used instead of lauric acid as the first organic component.
[0063] <95% Mass Loss Temperature of First Organic Component and Second Organic Component> The first organic component and the second organic component were heated from 25° C. to 40° C. at a heating rate of 2° C. / min in a nitrogen flow, maintained for 15 minutes, and then subjected to thermogravimetric differential thermal analysis using a TG-DTA2000SA simultaneous differential thermal analyzer manufactured by Bruker AXS under the conditions of a heating rate of 10° C. / min in a nitrogen flow, a sample mass of 30 mg, and the 95% mass loss temperature was determined.
[0064] <Evaluation of Solidification Time> The solidification time was the time from when the temporary fixing composition was dropped or applied to the sintering precursor at 50°C to when the temporary fixing composition solidified. Solidification was defined as the time when the temporary fixing composition became cloudy due to increased viscosity after dropping or application, as visually confirmed. Furthermore, after solidification, there was no penetration into the sintering precursor, and the size of the dropped or applied material did not change over time. In Comparative Example 1, the amount of the first organic component added was 96% by mass, which meant that fluidity during application was not ensured, making application impossible. Therefore, evaluation of the solidification time was not possible, and data was omitted (-). In Comparative Example 3, the first organic component used had a 95% mass reduction temperature in nitrogen of 314°C, which meant that fluidity during application was not ensured, making application impossible. Therefore, evaluation of the solidification time was not possible, and data was omitted (-). Comparative Examples 2 and 4 were applied but did not solidify, and therefore were marked with an X.
[0065] <Evaluation of Tackiness> After stacking the alumina chips, the alumina chips were left standing for 24 hours. Thereafter, the copper plate and the alumina chips were stood up so that the bonding surface between the copper plate and the alumina chips faced vertically, and after being left standing for 5 seconds, the plate was returned to a horizontal position. This operation was carried out a total of six times. The case where the alumina chips did not fall off the copper plate in any of the six operations was rated A, and the case where the alumina chips fell off at any stage of the operation was rated B. Note that, since coating was not possible for Comparative Examples 1 and 3, evaluation of tackiness could not be carried out and no data was recorded (-).
[0066]
[0067]
[0068]
[0069]
[0070] As is clear from each table, the examples have a short solidification time and excellent tackiness.
[0071] According to the present invention, the temporary fixing composition can have a short solidification time, which makes it possible to suppress the penetration of the temporary fixing composition into the joining material over time, and ensure tackiness to the joined materials even if the process time for joining two joined materials is long.
Claims
1. A temporary fixing composition used to temporarily fix a first material to be joined and a second material to be joined prior to joining the two materials, the composition containing 42% by mass or more and 95% by mass or less of a first organic component that is solid at 25°C and has a temperature at which it loses 95% of its mass in nitrogen of 300°C or less.
2. The temporary fixing composition according to claim 1, containing a second organic component that is liquid at 25°C and has a 95% mass loss temperature in nitrogen of 300°C or lower, in an amount of 5% by mass or more and 58% by mass or less.
3. The temporary fixing composition according to claim 1 or 2, which has a solidification time of 240 seconds or less after application.
4. The temporary fixing composition according to claim 1 or 2, which is substantially free of organic polymer compounds.
5. A method for manufacturing a bonded structure, comprising the steps of temporarily fixing a first material to be bonded and a second material to be bonded by interposing a temporary fixing composition between them, and then firing the temporarily fixed material to bond them together, wherein the temporary fixing composition is a composition containing a first organic component in a proportion of 42% by mass or more and 95% by mass or less, the first organic component being solid at 25°C and having a 95% mass reduction temperature in nitrogen of 300°C or less.
6. The manufacturing method described in claim 5, wherein the temporary fixing composition contains a second organic component that is liquid at 25°C and has a 95% mass loss temperature in nitrogen of 300°C or less, in an amount of 5% by mass or more and 58% by mass or less.
7. The manufacturing method according to claim 5 or 6, wherein at least one of the first material to be joined and the second material to be joined is made of a sintered precursor of a structure containing metal fine particles.
8. Use of a composition containing 42% by mass or more and 95% by mass or less of a first organic component that is solid at 25°C and has a 95% mass loss temperature in nitrogen of 300°C or less, for temporarily fixing a first material to be joined and a second material to be joined prior to joining the two.
9. Use of the composition according to claim 8, which contains a second organic component in a proportion of 5% by mass or more and 58% by mass or less, the second organic component being liquid at 25°C and having a 95% mass loss temperature in nitrogen of 300°C or less, for temporarily fixing the first and second materials to be joined prior to joining the two.