Lead-free piezoelectric composition and piezoelectric element
Patent Information
- Application Number
- MYPI2025001084
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-30
- Filing Date
- 2023-09-20
- Publication Date
- 2024-03-30
AI Technical Summary
Lead-free piezoelectric compositions exhibit low insulation properties under high temperature conditions, which is a concern for applications requiring high reliability and insulation integrity.
A lead-free piezoelectric composition with a main phase of alkali niobate perovskite oxide and a subphase containing Mn oxide, where the Mn oxide includes 0.05 mol% to 5 mol% Sc, and the crystal grains of the subphase have a maximum particle diameter of 94 μm or less, is used to enhance insulation and piezoelectric properties.
The composition achieves excellent piezoelectric and insulation properties under high-temperature conditions, making it suitable for various applications including vibration detection and piezoelectric devices.
Smart Images

Figure PI2025001084_DRAWING_001
Abstract
Description
Lead-free piezoelectric composition and piezoelectric element
[0001] The present invention relates to a lead-free piezoelectric composition and a piezoelectric element.
[0002] Conventionally, most piezoelectric elements are made of PZT (lead zirconate titanate)-based materials. However, the lead contained in PZT is considered problematic because it causes environmental load, and in recent years, development of piezoelectric elements made of lead-free materials has been progressing.
[0003] As this type of lead-free material, for example, a lead-free piezoelectric composition has been proposed that has a main phase formed of a first crystalline phase consisting of an alkali niobate-based perovskite-type oxide and a subphase containing a second crystalline phase consisting of an M-Ti-O-based spinel compound (element M is a monovalent to tetravalent element) (see Patent Document 1).
[0004] The alkali niobate perovskite oxide that constitutes the main phase is inherently a material that is prone to the formation of voids that cause a deterioration in piezoelectric properties. However, the voids in the main phase are filled with a subphase containing a second crystal, stabilizing the structure of the main phase (first crystal phase). Therefore, the lead-free piezoelectric composition has excellent piezoelectric properties. In other words, when force is applied to the lead-free piezoelectric composition, a voltage is generated, and when a voltage is applied, the lead-free piezoelectric composition undergoes dimensional expansion and contraction and changes in shape.
[0005] Furthermore, as shown in Patent Document 2, a conventionally known piezoelectric element is a multilayer piezoelectric element having a laminate in which internal electrodes mainly composed of Ni and lead-free piezoelectric ceramic layers are alternately stacked. In this type of multilayer piezoelectric element, Ni is used as the material (main component) of the internal electrodes in order to reduce costs.
[0006] Patent No. 5715309 Patent No. 5862983
[0007] (Problem to be Solved by the Invention) Although the above-mentioned lead-free piezoelectric composition has excellent piezoelectric properties, it has a problem of poor insulating properties under high temperature conditions (e.g., 100° C.) For example, in the case of the above-mentioned multilayer piezoelectric element, high reliability is required in terms of insulating properties, etc., but poor insulating properties under high temperature conditions (e.g., 100° C.) have been a problem.
[0008] An object of the present invention is to provide a lead-free piezoelectric composition and the like which has excellent piezoelectric properties and excellent insulating properties under high temperature conditions.
[0009] (Means for Solving the Problems) The means for solving the problems are as follows: <1> A lead-free piezoelectric composition having a main phase containing an alkali niobate perovskite-type oxide and a subphase containing a manganese oxide, wherein the manganese oxide contains 0.05 mol % to 5 mol % of Sc.
[0010] <2> The Mn oxide is Mn 4 Nb 2 O 9 , MnTi 2 O 4 , Mn 2 TiO 4 The lead-free piezoelectric composition according to <1>, which contains at least one of the following:
[0011] <3> The lead-free piezoelectric composition according to <1> or <2>, wherein the maximum particle size of the crystal grains of the subphase is 94 μm or less.
[0012] <4> A piezoelectric element having a structure in which the lead-free piezoelectric composition according to any one of <1> to <3> and electrodes are alternately laminated.
[0013] EFFECTS OF THE INVENTION According to the present invention, it is possible to provide a lead-free piezoelectric composition and the like that has excellent piezoelectric properties and excellent insulating properties under high temperature conditions.
[0014] 1 is a perspective view of a piezoelectric element according to a first embodiment; FIG. 2 is a cross-sectional view of a piezoelectric element according to a second embodiment;
[0015] The lead-free piezoelectric composition and piezoelectric element according to the embodiment will be described below.
[0016] The lead-free piezoelectric composition has a main phase containing an alkali niobate perovskite oxide and a subphase containing a manganese oxide.
[0017] The main phase is formed of a first crystalline phase made of an alkali niobate perovskite oxide, which is represented by the following composition formula (1):
[0018] (A1 a M1 b ) c (Nb d1 Mn d2 Ti d3 Zr d4 ) O 3+e ...(1)
[0019] The element A1 is at least one of alkali metals Li, Na, and K. The element M1 is at least one of alkaline earth metals Ba (barium), Ca (calcium), and Sr (strontium).
[0020] In the above composition formula (1), the elements A1 and M1 are arranged at the A site of the perovskite structure, and Nb (niobium), Mn (manganese), Ti (titanium), and Zr (zirconium) are arranged at the B site.
[0021] The values of the coefficients a to e in the composition formula (1) are those that establish a perovskite structure and are suitable for the electrical or piezoelectric properties (particularly the piezoelectric constant d 33 ) is selected as a preferable value.
[0022] Specifically, the coefficients a and b satisfy 0<a<1, 0<b<1, and a+b=1, and a=0 (i.e., a composition containing no alkali metals) and b=0 (i.e., a composition containing none of Ba, Ca, and Sr) are excluded.
[0023] The coefficient c for all A sites satisfies 0.80<c<1.10, preferably 0.84≦c≦1.08, and more preferably 0.88≦c≦1.07.
[0024] The coefficients d1, d2, d3, and d4 satisfy the following conditions: 0<d1<1, 0<d2<1, 0<d3<1, 0≦d4<1, and d1+d2+d3+d4=1. The cases where d1=0 (a composition that does not contain Nb), d2=0 (a composition that does not contain Mn), and d3=0 (a composition that does not contain Ti) are excluded. The coefficient d4 of Zr may be zero (i.e., the composition may not contain Zr).
[0025] In the oxygen coefficient 3+e, the coefficient e is a positive or negative value indicating a deficiency or excess of oxygen, with the oxygen coefficient usually being 3. The oxygen coefficient 3+e can take a value such that the main phase constitutes a perovskite-type oxide. A typical value of the coefficient e is e=0, and 0≦e≦0.1 is preferred. The value of the coefficient e can be calculated from the electrical neutrality condition of the composition of the main phase. However, a composition that slightly deviates from the electrical neutrality condition is also acceptable as the composition of the main phase.
[0026] Among the alkali niobate perovskite oxides represented by the above composition formula (1), oxides containing K, Na, and Nb as main metal components are called "KNN" or "KNN material," and are excellent in piezoelectric properties, electrical properties, etc.
[0027] The above composition formula (1) can be rewritten as the following composition formula (1A).
[0028] (K a1 Na a2 Li a3 Ca b1 Sr b2 Ba b3 ) c (Nb d1 Mn d2 Ti d3 Zr d4 ) O 3+e ... (1A)
[0029] The composition formula (1) and the composition formula (1A) are equivalent, and a1 + a2 + a3 = a, and b1 + b2 + b3 = b. The coefficient a1 of K is 0 < a1 ≦ 0.6, and the coefficient a2 of Na is 0 < a1 ≦ 0.6. The coefficient a3 of Li is 0 ≦ a3 ≦ 0.2 (preferably, 0 ≦ a3 ≦ 0.1).
[0030] The subphase is formed of a second crystalline phase containing Mn oxide. The Mn oxide is an oxide containing Mn (manganese) and Sc (scandium) in a proportion of 0.05 mol % to 5 mol %. The method for determining the Sc content (mol %) in the subphase will be described later.
[0031] The Mn oxide is Mn 2 TiO 4 In the case where the Mn oxide contains Sc, the Mn oxide preferably contains 0.05 mol % or more and 1 mol % or less of Sc.
[0032] As the Mn oxide, Mn 4 Nb 2 O 9 , MnTi 2 O 4 , Mn 2 TiO 4 Examples of Mn oxides include Mn 4 Nb 2 O 9 , MnTi 2 O 4 , Mn 2 TiO 4 It is preferable to include at least one of the following.
[0033] In the case where the Mn oxide is an Mn—Ti—O-based oxide, the Mn—Ti—O-based oxide may be any oxide having the above-mentioned composition formula (MnTiO) as long as it can maintain a spinel structure and the change in the properties of the compound is within an acceptable range. 2 O 4 , Mn 2 TiO 4 ) may have deviated values of the standard coefficients, and may have a composition represented by the following formula (2) or (3), for example. The Mn—Ti—O-based oxide represented by the following formula (2) or (3) may contain impurity elements such as Na, K, Nb, Zr, Ba, Ca, Sr, Sc, and Ni.
[0034] Mn a Ti 2b O 4±e ... (2) Mn 2c Ti d O 4±e ...(3)
[0035] In the composition formula (2), 0.8<a<1.2, 0.8<b<1.2, and e are values indicating oxygen deficiency or excess. In the composition formula (3), 0.8<c<1.2, 0.8<d<1.2, and e are values indicating oxygen deficiency or excess.
[0036] In addition, when the Mn oxide is an Mn—Nb—O-based oxide, the Mn—Nb—O-based oxide may be any oxide having the above-mentioned composition formula (Mn) as long as it can maintain a spinel structure and the change in the properties of the compound is within an acceptable range. 4 Nb 2 O 9 ) may have deviated values of the standard coefficients, and may have a composition represented by the following formula (4), for example: The Mn—Nb—O-based oxide represented by the following formula (4) may contain impurity elements such as Na, K, Ti, Zr, Ba, Ca, Sr, Sc, and Ni.
[0037] Mn 4f Nb 2g O 9±h ...(4)
[0038] In the above composition formula (4), 0.8<f<1.2, 0.8<g<1.2, and h is a value indicating oxygen deficiency or excess.
[0039] It is presumed that Sc is dissolved in the subphase (second crystal phase) and that Sc is present in some of the sites of the main metal elements in the crystal structure of the Mn oxide.
[0040] For example, Mn oxide is Mn 4 Nb 2 O 9 In this case, it is presumed that Sc exists in some of the Mn (manganese) sites and some of the Nb (niobium) sites. 2 O 4 In this case, it is presumed that the metal is present in a part of the Mn (manganese) site or a part of the Ti (titanium) site.
[0041] In the lead-free piezoelectric composition of the present embodiment, the subphase crystal grains preferably have a maximum particle size of 94 μm or less. The lower limit of the maximum particle size is not particularly limited as long as it does not impair the object of the present invention, but is preferably, for example, 0.8 μm or more.
[0042] In the lead-free piezoelectric composition of this embodiment, the subphase crystal grains preferably have a D80 of 83 μm or less. There is no particular restriction on the lower limit of D80 as long as the object of the present invention is not impaired. However, for example, it is preferably 0.6 μm or more.
[0043] In the lead-free piezoelectric composition of the present embodiment, the average particle size of the subphase crystal grains is preferably 65 μm or less. There is no particular restriction on the lower limit of the average particle size as long as it does not impair the object of the present invention, but it is preferably 0.4 μm or more, for example.
[0044] The methods for measuring the maximum particle size, D80, and average particle size of the subphase crystal particles will be described later.
[0045] The lead-free piezoelectric composition of this embodiment may contain two or more types of Mn oxides as subphases, as long as the object of the present invention is not impaired.
[0046] Furthermore, the lead-free piezoelectric composition of this embodiment may contain, as a subphase, a crystalline phase other than the second crystalline phase containing Mn oxide (such as a third crystalline phase), as long as the object of the present invention is not impaired.
[0047] The subphase, which includes the second crystalline phase satisfying the above-mentioned conditions, is dispersed in a scattered manner within the main phase, which is made of the first crystalline phase. The subphase fills the voids (gaps) formed between the fine crystals of the main phase. Although the subphase does not have piezoelectric properties, its presence in the main phase improves the sinterability and structural stability of the lead-free piezoelectric composition, as well as the insulating properties under high temperature conditions.
[0048] In this embodiment, the proportion of the subphase contained in the lead-free piezoelectric composition is not particularly limited as long as it does not impair the object of the present invention, but is preferably, for example, 0.5% by volume or more and 5% by volume or less.
[0049] Next, a piezoelectric element 200 according to embodiment 1 will be described with reference to FIG. 1 . FIG. 1 is a perspective view of the piezoelectric element 200 according to embodiment 1. As shown in FIG. 1 , the piezoelectric element 200 according to this embodiment has a disk-shaped appearance and includes a disk-shaped piezoelectric layer (an example of a piezoelectric ceramic layer) 100 and electrodes 301 and 302 attached to the upper and lower surfaces of the piezoelectric layer 100. The piezoelectric layer 100 is formed from the lead-free piezoelectric composition described above. The piezoelectric layer 100 is polarized in the thickness direction. The electrodes 301 and 302 are made of, for example, Au.
[0050] Here, an example of a manufacturing method of the piezoelectric element 200 according to the first embodiment will be described. First, multiple types of raw material powders necessary for forming the main phase are prepared, and these raw material powders are weighed out to obtain the desired composition. The raw material powders may be oxides, carbonates, hydroxides, etc., of the elements contained in the main phase. Ethanol is added to a mixture of the weighed raw material powders, and the mixture is wet-mixed using a ball mill, preferably for 15 hours or more, to obtain a slurry. The obtained slurry is dried, and the mixed powder obtained after drying is calcined, for example, in an air atmosphere at a temperature of 600 to 1000°C for 1 to 10 hours, to obtain a powdered calcined main phase.
[0051] Additionally, multiple types of raw material powders necessary for forming the subphase are prepared and weighed to achieve the desired composition. In this process, a Mn-containing compound and a Sc-containing compound are used as the essential raw material powders. The amount of the raw material powder containing Sc is adjusted so that the Sc content in the subphase is 0.05 mol% or more and 5 mol% or less. The raw material powder may be an oxide, carbonate, hydroxide, or the like of each element contained in the subphase. Ethanol is added to the mixture of the weighed raw material powders, and the mixture is wet-mixed using a ball mill, preferably for 15 hours or more, to obtain a slurry. The resulting slurry is dried, and the resulting mixed powder is calcined, for example, in an air atmosphere at a temperature of 600 to 1000°C for 1 to 10 hours to obtain a calcined subphase.
[0052] Next, a dispersant, a binder, and ethanol are added to the obtained main phase calcined product and the subphase calcined product, and the mixture is pulverized and mixed to obtain a slurry. The obtained slurry is then dried, and the obtained dried product is appropriately granulated and uniaxially pressed under a pressure condition of, for example, 20 MPa to obtain a disk-shaped pre-molded product. The pre-molded product is then subjected to a CIP (cold isostatic pressing) treatment under a pressure condition of, for example, 150 MPa to obtain a molded product.
[0053] The resulting compact is then subjected to a binder removal process by, for example, holding it for 2 to 10 hours at a temperature of 200 to 400° C. The compact after the binder removal process is then fired for 2 to 5 hours at a temperature of, for example, 1000 to 1200° C. in a reducing atmosphere in which the pressure is controlled to be one order of magnitude or more lower than the equilibrium oxygen partial pressure of Ni / NO, thereby obtaining a piezoelectric layer.
[0054] Electrodes made of Au are formed on both the front and back surfaces of the obtained piezoelectric layer, for example, by sputtering. Then, the laminate with the electrodes formed on the piezoelectric layer is subjected to a polarization process in which a DC voltage of 5 kV / mm is applied in silicone oil at 50°C, thereby developing the voltage characteristics of the piezoelectric layer. In this way, the piezoelectric element 200 is obtained.
[0055] Next, a piezoelectric element 10 according to a second embodiment will be described with reference to FIG. 2 . FIG. 2 is a cross-sectional view of the piezoelectric element 10 according to the second embodiment. As shown in FIG. 2 , the piezoelectric element 10 of this embodiment includes a piezoelectric layer (an example of a piezoelectric ceramic layer) 11, a plurality of internal electrodes 12, 13 in contact with the piezoelectric layer 11, and two external electrodes 14, 15 connected to the internal electrodes 12, 13. The piezoelectric layer 11 is formed from the lead-free piezoelectric composition described above. The internal electrodes 12, 13 are primarily composed of a base metal (e.g., nickel). The piezoelectric layer 11 and the internal electrodes 12, 13 are alternately stacked. More specifically, the piezoelectric layer 11 and the internal electrodes 12, 13 are stacked in the following order: piezoelectric layer 11, internal electrode 12, piezoelectric layer 11, internal electrode 13, piezoelectric layer 11, etc., with one piezoelectric layer 11 sandwiched between the two internal electrodes 12, 13. Two external electrodes 14, 15 are disposed on the outer surfaces of the laminate of the piezoelectric layer 11 and the internal electrodes 12, 13. The external electrodes 14, 15 are made mainly of, for example, Au. Of the two internal electrodes 12, 13 in contact with one piezoelectric layer 11, one end of one internal electrode 12 is connected to one external electrode 14, and one end of the other internal electrode 13 is connected to the other external electrode 15. When a voltage is applied between the external electrodes 14, 15, the piezoelectric layer 11 expands and contracts, causing the entire piezoelectric element 10 to expand and contract.
[0056] Here, an example of a manufacturing method of the piezoelectric element 10 according to the second embodiment will be described. First, multiple types of raw material powders necessary for forming the main phase are prepared, and these raw material powders are weighed out to obtain the desired composition. The raw material powders may be oxides, carbonates, hydroxides, etc., of the elements contained in the main phase. Ethanol is added to a mixture of the weighed raw material powders, and the mixture is wet-mixed using a ball mill, preferably for 15 hours or more, to obtain a slurry. The obtained slurry is dried, and the mixed powder obtained after drying is calcined, for example, in an air atmosphere at a temperature of 600 to 1000°C for 1 to 10 hours, to obtain a powdered calcined main phase.
[0057] Additionally, multiple types of raw material powders necessary for forming the subphase are prepared and weighed to achieve the desired composition. In this process, a Mn-containing compound and a Sc-containing compound are used as the essential raw material powders. The amount of the raw material powder containing Sc is adjusted so that the Sc content in the subphase is 0.05 mol% or more and 5 mol% or less. The raw material powder may be an oxide, carbonate, hydroxide, or the like, of each element contained in the subphase. Ethanol is added to the mixture of the weighed raw material powders, and the mixture is wet-mixed using a ball mill, preferably for 15 hours or more, to obtain a slurry. The resulting slurry is dried, and the resulting mixed powder is calcined, for example, in an air atmosphere at a temperature of 600 to 1000°C for 1 to 10 hours, to obtain a powdered calcined subphase.
[0058] Next, a dispersant, a binder, and an organic solvent (e.g., toluene) are added to the obtained main phase calcined product and subphase calcined product, and the mixture is pulverized and mixed to obtain a slurry, which is then processed into a sheet shape using a doctor blade method or the like to produce a ceramic green sheet.
[0059] Next, an electrode layer that will become an internal electrode is formed on one surface of the ceramic green sheet by, for example, screen printing using a conductive paste for the internal electrode. The electrode layer is mainly composed of a base metal, for example, nickel (Ni).
[0060] Next, multiple ceramic green sheets with electrode layers formed thereon are stacked so that the electrode layers are exposed alternately from both sides, and ceramic green sheets without electrode layers are stacked on both the front and back sides of the resulting laminate. The resulting laminate is then pressed together to obtain a laminate in which ceramic green sheets and electrode layers are alternately stacked. This laminate is then cut into a desired shape and then subjected to a binder removal treatment, for example, by holding it at a temperature of 200 to 400°C for 2 to 10 hours.
[0061] The laminate after the binder removal treatment is fired, for example, at a temperature of 1000 to 1200°C for 2 to 5 hours in a reducing atmosphere in which the pressure is controlled to be one order of magnitude or more lower than the equilibrium oxygen partial pressure of Ni / NO.
[0062] After the fired laminate has been polished appropriately, a pair of external electrodes made of Au are formed on the side surfaces of the laminate, for example by sputtering. The pair of external electrodes are formed facing each other with the laminate interposed therebetween. The laminate with the external electrodes formed thereon is subjected to a polarization process to obtain a piezoelectric element 10. In this way, a piezoelectric element (multilayer piezoelectric element) 10 having a structure in which piezoelectric layers made of a lead-free piezoelectric composition and electrodes (internal electrodes) are alternately stacked is obtained.
[0063] The manufacturing methods of the first and second embodiments described above are merely examples, and various other steps and processing conditions for manufacturing a piezoelectric element can be employed. For example, instead of separately producing the main phase and subphase calcined products and then mixing and firing the powders of the two, raw materials may be mixed in a quantitative ratio appropriate for the final composition of the lead-free piezoelectric composition, and the mixture may be fired. However, by separately producing the main phase and subphase calcined products and then mixing them, the compositions of the main phase and subphase can be more precisely controlled, thereby increasing the yield of the lead-free piezoelectric composition. The subphase may also be composed of two types of crystalline phases. Furthermore, metals or alloys such as platinum (Pt), silver-palladium (Ag-Pd), and silver (Ag) may be used as the electrode material.
[0064] The lead-free piezoelectric composition and piezoelectric element disclosed herein have excellent piezoelectric properties and excellent insulating properties under high-temperature conditions. Such lead-free piezoelectric composition and piezoelectric element can be widely used for vibration detection, pressure detection, oscillation, piezoelectric device applications, etc. For example, they can be used in sensors that detect various vibrations (e.g., Knox sensors and combustion pressure sensors), piezoelectric devices such as vibrators, actuators, and filters, high-voltage generators, micropower sources, various driving devices, position control devices, vibration suppression devices, fluid discharge devices (e.g., paint discharge, fuel discharge), etc.
[0065] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples in any way.
[0066] [Examples 1 to 9, Examples 11 to 20 and Comparative Examples 1 to 6] (Preparation of Main Phase Calcined Product) As raw material powder, K 2 CO 3 Powder, Na 2 CO 3 powder, Nb 2 O 5 Powder, TiO 2 Powder, ZrO 2 Powder, MnCO 3 Powder, BaCO 3 Powders were prepared, and each of these raw material powders was weighed so that the content (mol%) of each element was the value shown in Table 1. An appropriate amount of ethanol was added to the mixture of the weighed raw material powders, and the mixture was wet-mixed in a ball mill for 15 hours to obtain a slurry. The obtained slurry was dried, and the mixed powder obtained after drying was calcined in an air atmosphere at a temperature condition of 600 to 1100°C for 1 to 10 hours to obtain a powdery calcined main phase product.
[0067] (Preparation of subphase calcined product) MnCO 3 Powder, TiO 2 powder, Nb 2 O 5 Powder, Li 2 CO 3 Powder, Sc 2 O 3 Powders were prepared. From these raw material powders, the necessary raw material powders were selected corresponding to each Example, and each raw material powder was weighed so as to have a composition shown in Table 2, Table 4, or Table 5 and a Sc content (mol %) corresponding to that composition. An appropriate amount of ethanol was added to the mixture of the weighed raw material powders, and the mixture was wet-mixed using a ball mill for 15 hours to obtain a slurry. The obtained slurry was dried, and the mixed powder obtained after drying was calcined in an air atmosphere at a temperature condition of 600 to 1100°C for 1 to 10 hours to obtain a powdery subphase calcined product.
[0068] (Fabrication of Piezoelectric Element) A dispersant, a binder, and ethanol were added to the obtained main phase calcined product and the subphase calcined product, and the mixture was pulverized and mixed to obtain a slurry. The obtained slurry was then dried, and the obtained dried product was appropriately granulated and uniaxially pressed under a pressure condition of 20 MPa to obtain a disk-shaped pre-molded body. The pre-molded body was then subjected to a CIP (cold isostatic pressing) treatment under a pressure condition of 150 MPa to obtain a molded body. The mixing ratio of the main phase calcined product to the subphase calcined product was adjusted so that the ratio (volume %) of the main phase to the subphase was 97:3.
[0069] The resulting compact was subjected to a binder removal treatment by holding it at a temperature of 200 to 400°C for 2 to 10 hours. The binder-removed compact was then fired for 2 hours at a temperature of 1000 to 1200°C in a reducing atmosphere where the pressure was controlled to be one order of magnitude or more lower than the equilibrium oxygen partial pressure of Ni / NO, yielding a piezoelectric layer. The particle size of the subphases and other components contained in the piezoelectric layer was adjusted by appropriately setting the firing temperature. For example, a higher firing temperature results in a larger particle size.
[0070] Au electrodes were formed on both the front and back surfaces of the piezoelectric layer by sputtering. Then, the laminate with the electrodes formed on the piezoelectric layer was subjected to a polarization treatment in which a DC voltage of 5 kV / mm was applied in silicone oil at 50° C., thereby developing the voltage characteristics of the piezoelectric layer and obtaining a piezoelectric element.
[0071] Example 10 is a piezoelectric element using a lead-free piezoelectric composition containing two types of subphases (subphase a and subphase b). As will be described later, the piezoelectric element of Example 10 was produced in the same manner as in Example 1, etc., except that two types of subphase calcined products were used.
[0072] As raw material powder, MnCO 3 Powder, TiO 2 powder, Nb 2 O 5 Powder, Sc 2 O 3Powders were prepared, and the necessary raw material powders were selected from these raw material powders for each subphase (subphase a, subphase b), and then each raw material powder was weighed out so as to have the composition and Sc content (mol %) shown in Table 3. Then, for each subphase (subphase a, subphase b), two types of powdered subphase calcined products were obtained from two types of mixtures of the weighed raw material powders by the same manufacturing method as in Example 1, etc.
[0073] During the production of the piezoelectric layer of the piezoelectric element, the mixing ratio of the main phase calcined product, the subphase calcined product for one subphase (subphase a), and the subphase calcined product for the other subphase (subphase b) was adjusted so that the ratio (volume %) of the main phase to the subphase a to the subphase b in the lead-free piezoelectric composition was 97:1.5:1.5.
[0074] [Piezoelectric constant d 33 For the piezoelectric elements (piezoelectric layers) of each example and each comparative example, 33 The piezoelectric constant (pC / N) was measured using a meter (product name "ZJ-4B", manufactured by the Institute of Vocal Music, Chinese Academy of Sciences). The results are shown in Tables 2 to 5.
[0075] [Insulation Resistance Under High Temperature Conditions] The insulation resistance (Ω m) under high temperature conditions was measured for the voltage elements of each Example and Comparative Example using the method described below. The voltage elements were placed in silicone oil at 100°C, and a DC voltage of 5 kV / mm was applied for 1 minute to measure the insulation resistance (Ω m). The results are shown in Tables 2 to 5.
[0076] [Analysis of the Main Phase] For each piezoelectric element (piezoelectric layer) of each Example and Comparative Example, a compositional analysis of the main phase was performed using an electron probe microanalyzer (EPMA) according to the method described below. The piezoelectric layer of the piezoelectric element was cut in the thickness direction, and the cut surface was polished. The polished surface was then photographed at 5000x magnification using an EPMA. From the obtained image, three arbitrary crystal grains in the main phase were selected, and quantitative analysis was performed on these three crystal grains. The average value of the content of each element in the three crystal grains was then taken as the content (mol%) of each element in the main phase. The results are shown in Table 1.
[0077] [Analysis of Subphases] The compositions of compounds contained in the subphases of the polished surfaces of each Example and Comparative Example were identified using powder X-ray diffraction (XRD). The measurement conditions for XRD were as follows:
[0078] <XRD measurement conditions> Measurement device: Powder X-ray diffractometer Range: 5.00° to 70.00° Wavelength: 0.7 angstroms
[0079] Furthermore, for each piezoelectric element (piezoelectric layer) of each Example and Comparative Example, a qualitative analysis of the subphase was performed using an EPMA according to the method described below. For each Example, the polished surface of the piezoelectric layer used in the analysis of the main phase was photographed at 5000x magnification, and elemental mapping of Sc (scandium) was performed using the obtained image. The presence or absence of Sc in the subphase was confirmed from the obtained elemental mapping image. In all of Examples 1 to 20, the presence of Sc in the subphase was confirmed. Furthermore, the presence of Sc in the subphase was also confirmed in Comparative Examples 4 and 5. Note that the presence of Sc was not observed in the subphase in Comparative Examples 1 to 3 and Comparative Example 6.
[0080] [Particle size (maximum particle size, average particle size, D80) of subphase crystal grains] The polished surfaces of Example 5, Examples 14 to 20, and Comparative Example 6 were photographed at 5000x magnification using a scanning electron microscope (SEM). A square measurement range with a side length of 250 μm was set for the resulting SEM image (backscattered electron image). Then, using image analysis software, the major axis diameter and minor axis diameter of each of the multiple crystal grains present within the measurement range were determined. The major axis diameter and minor axis diameter of the crystal grain were perpendicular to each other, and the major axis diameter and minor axis diameter were the maximum values for each axis. The average value of the major axis diameter and minor axis diameter for each crystal grain was then used as the particle size (particle size) of each crystal grain. The average value of the particle size of each crystal grain within the measurement range thus determined was used as the average particle size (μm) of the subphase crystal grains. The results are shown in Table 5.
[0081] The largest major axis diameter of each crystal grain within the measurement range was taken as the maximum particle diameter (μm) of the subphase crystal grains. The results are shown in Table 5.
[0082] Furthermore, a particle size distribution was created for each crystal particle within the measurement range, arranged in order of particle size from smallest to largest, and the cumulative 80% particle size (D80) based on the number of particles in the particle size distribution was calculated. The results are shown in Table 5.
[0083]
[0084]
[0085]
[0086]
[0087]
[0088] As shown in Tables 2 and 3, the lead-free piezoelectric compositions used in the piezoelectric elements of Examples 1 to 10 were Mn oxide (MnTi 2 O 4 and / or Mn 4 Nb 2 O 9 In Examples 1 to 10, the Mn oxide contains Sc in a proportion of 0.05 mol % or more and 5 mol % or less. In Examples 1 to 10, the insulation resistance under high temperature conditions is 1×10 10 The resistance was Ω·m or more, confirming that the material has excellent insulating properties under high temperature conditions.
[0089] Comparative Example 1 is MnTi 2 O 4 In Comparative Example 1, the insulation resistance was 5×10 5 Ω·m, and it was confirmed that the insulating properties under high temperature conditions were low.
[0090] Comparative Example 2 is Mn 4 Nb 2 O 9 In Comparative Example 2, the insulation resistance was 5×106 Ω·m, and it was confirmed that the insulating properties under high temperature conditions were low.
[0091] Comparative Example 3 is not a Mn oxide, but LiTiO 4 In Comparative Example 3, the insulation resistance was 4×10 4 Ω·m, and it was confirmed that the insulating properties under high temperature conditions were low.
[0092] Comparative Example 4 is not a Mn oxide, but LiTiO 4 In Comparative Example 4, the insulation resistance was 2×10 5 Ω·m, and it was confirmed that the insulating properties under high temperature conditions were low.
[0093] Comparative Example 5 has a subphase containing Mn oxide similar to Example 1, but the content of Sc (scandium) contained in the subphase is too high. It was confirmed that the insulating properties of Comparative Example 5 were so low that the insulation resistance could not be measured.
[0094] As shown in Tables 2 and 3, in Examples 1 to 10, the piezoelectric constant d 33 The measurement results confirmed that the piezoelectric properties were excellent.
[0095] Furthermore, as shown in Tables 4 and 5, the lead-free piezoelectric compositions used in the piezoelectric elements of Examples 11 to 20 were Mn oxide (Mn 2 TiO 4 In Examples 11 to 20, the Mn oxide contains Sc in a proportion of 0.05 mol % or more and 3 mol % or less. In Examples 11 to 20, the insulation resistance under high temperature conditions is 7×10 8 As shown in Tables 4 and 5, Examples 11 to 20 have a piezoelectric constant d 33 The measurement results confirmed that the piezoelectric properties were excellent.
[0096] Comparative Example 6 is a manganese oxide (Mn 2 TiO 4 ) does not contain Sc. In Comparative Example 6, there were problems with the piezoelectric characteristics and insulating properties.
[0097] As shown in Table 4, the Mn oxide subphase is Mn 2 TiO 4 In this case, if the Mn oxide contains 0.05 mol % to 1 mol % of Sc, the insulating properties are further improved.
[0098] Furthermore, as shown in Table 5, when the maximum particle size of the subphase crystal particles is 94 μm or less (or the D80 of the subphase crystal particles is 83 μm or less, or the average particle size of the subphase crystal particles is 65 μm or less), the insulating properties are even better.
[0099] 10, 200... Piezoelectric element, 11, 100... Piezoelectric layer (piezoelectric ceramic layer), 12, 13... Internal electrode, 14, 15... External electrode, 301, 302... Electrode
Claims
1. A lead-free piezoelectric composition having a main phase containing an alkali niobate perovskite-type oxide and a subphase containing a manganese oxide, wherein the manganese oxide contains 0.05 mol % or more and 5 mol % or less of Sc.
2. The Mn oxide is Mn 4 Nb 2 O 9 , MnTi 2 O 4 , Mn 2 TiO 4 The lead-free piezoelectric composition according to claim 1, comprising at least one of:
3. The lead-free piezoelectric composition according to claim 1 or 2, wherein the maximum particle size of the crystal grains of the subphase is 94 μm or less.
4. A piezoelectric element having a structure in which the lead-free piezoelectric composition according to any one of claims 1 to 3 and electrodes are alternately laminated.