Lead-free piezoelectric composition and piezoelectric element

MYPI2025001085A0Undetermined Publication Date: 2024-03-30NITERRA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025001085
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-30
Filing Date
2023-09-11
Publication Date
2024-03-30

AI Technical Summary

Technical Problem

Lead-free piezoelectric compositions with excellent piezoelectric properties face challenges with low dielectric breakdown voltage and insulation issues.

Method used

A lead-free piezoelectric composition featuring a main phase of alkali niobate perovskite oxide and a sub-phase of Mn-Ti-O-based oxide, with controlled particle sizes and compositions, including MnTi2O4 or Mn2TiO4, to enhance both piezoelectric and insulation properties.

Benefits of technology

The composition achieves excellent piezoelectric properties and high dielectric breakdown voltage, improving insulation and structural stability, making it suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025001085_DRAWING_001
    Figure PI2025001085_DRAWING_001
Patent Text Reader

Abstract

ABSTRACT LEAD-FREE PIEZOELECTRIC COMPOSITION AND PIEZOELECTRIC ELEMENT [Means for Solution] The lead-free piezoelectric composition of the present invention has a primary phase containing an alkali niobate perovskite-type oxide and a secondary phase containing an Mn-Ti-O oxide. The Mn-Ti-O oxide contained in the secondary phase has a maximum grain size of 35 µm or smaller and a number-basis 80% cumulative particle size (D80) of 32 µm or smaller.
Need to check novelty before this filing date? Find Prior Art

Description

Lead-free piezoelectric composition and piezoelectric element

[0001] The present invention relates to a lead-free piezoelectric composition and a piezoelectric element.

[0002] Conventionally, most piezoelectric elements are made of PZT (lead zirconate titanate)-based materials. However, the lead contained in PZT is considered problematic because it causes environmental load, and in recent years, development of piezoelectric elements made of lead-free materials has been progressing.

[0003] As this type of lead-free material, for example, a lead-free piezoelectric composition has been proposed that has a main phase formed of a first crystalline phase consisting of an alkali niobate-based perovskite-type oxide and a subphase containing a second crystalline phase consisting of an M-Ti-O-based spinel compound (element M is a monovalent to tetravalent element) (see Patent Document 1).

[0004] The alkali niobate perovskite oxide that constitutes the main phase is inherently a material that is prone to the formation of voids that cause a deterioration in piezoelectric properties. However, the voids in the main phase are filled with a subphase containing a second crystal, stabilizing the structure of the main phase (first crystal phase). Therefore, the lead-free piezoelectric composition has excellent piezoelectric properties. In other words, when force is applied to the lead-free piezoelectric composition, a voltage is generated, and when a voltage is applied, the lead-free piezoelectric composition undergoes dimensional expansion and contraction and changes in shape.

[0005] Patent No. 5715309

[0006] (Problem to be Solved by the Invention) Although the above-mentioned lead-free piezoelectric composition has excellent piezoelectric properties, it has a low dielectric breakdown voltage and therefore has a problem with insulation properties.

[0007] An object of the present invention is to provide a lead-free piezoelectric composition and the like that has excellent piezoelectric properties and insulating properties.

[0008] (Means for Solving the Problems) The means for solving the above problems are as follows: Namely, <1> A lead-free piezoelectric composition having a main phase containing an alkali niobate-based perovskite-type oxide and a subphase containing a Mn—Ti—O-based oxide, wherein the maximum particle size of the Mn—Ti—O-based oxide in the subphase is 35 μm or less and the number-based cumulative 80% particle size (D80) is 32 μm or less.

[0009] <2> The lead-free piezoelectric composition according to <1>, wherein the Mn—Ti—O-based oxide in the subphase has an average particle size of 24 μm or less.

[0010] <3> The Mn—Ti—O-based oxide is MnTi 2 O 4 , or Mn 2 TiO 4 The lead-free piezoelectric composition according to <1> or <2>,

[0011] <4> A piezoelectric element comprising a laminate of a piezoelectric ceramic layer formed from the lead-free piezoelectric composition according to any one of <1> to <3> 2 and an electrode attached to the piezoelectric ceramic layer.

[0012] EFFECTS OF THE INVENTION According to the present invention, it is possible to provide a lead-free piezoelectric composition and the like that has excellent piezoelectric properties and insulating properties.

[0013] 1 is a perspective view of a piezoelectric element according to a first embodiment; FIG. 2 is a cross-sectional view of a piezoelectric element according to a second embodiment;

[0014] The lead-free piezoelectric composition and piezoelectric element according to the embodiment will be described below.

[0015] The lead-free piezoelectric composition has a main phase containing an alkali niobate-based perovskite oxide and a subphase containing an Mn—Ti—O-based oxide.

[0016] The main phase is formed of a first crystalline phase made of an alkali niobate perovskite oxide, which is represented by the following composition formula (1):

[0017] (A1 a M1 b ) c (Nb d1 Mn d2 Tid3 Zr d4 ) O 3+e ...(1)

[0018] The element A1 is at least one of alkali metals Li, Na, and K. The element M1 is at least one of alkaline earth metals Ba (barium), Ca (calcium), and Sr (strontium).

[0019] In the above composition formula (1), the elements A1 and M1 are arranged at the A site of the perovskite structure, and Nb (niobium), Mn (manganese), Ti (titanium), and Zr (zirconium) are arranged at the B site.

[0020] The values ​​of the coefficients a to e in the composition formula (1) are those that establish a perovskite structure and are suitable for the electrical or piezoelectric properties (particularly the piezoelectric constant d 33 ) is selected as a preferable value.

[0021] Specifically, the coefficients a and b satisfy 0<a<1, 0<b<1, and a+b=1, and a=0 (i.e., a composition containing no alkali metals) and b=0 (i.e., a composition containing none of Ba, Ca, and Sr) are excluded.

[0022] The coefficient c for all A sites satisfies 0.80<c<1.10, preferably 0.84≦c≦1.08, and more preferably 0.88≦c≦1.07.

[0023] The coefficients d1, d2, d3, and d4 satisfy the following conditions: 0<d1<1, 0<d2<1, 0<d3<1, 0≦d4<1, and d1+d2+d3+d4=1. The cases where d1=0 (a composition that does not contain Nb), d2=0 (a composition that does not contain Mn), and d3=0 (a composition that does not contain Ti) are excluded. The coefficient d4 of Zr may be zero (i.e., the composition may not contain Zr).

[0024] In the oxygen coefficient 3+e, the coefficient e is a positive or negative value indicating a deficiency or excess of oxygen, with the oxygen coefficient usually being 3. The oxygen coefficient 3+e can take a value such that the main phase constitutes a perovskite-type oxide. A typical value of the coefficient e is e=0, and 0≦e≦0.1 is preferred. The value of the coefficient e can be calculated from the electrical neutrality condition of the composition of the main phase. However, a composition that slightly deviates from the electrical neutrality condition is also acceptable as the composition of the main phase.

[0025] Among the alkali niobate perovskite oxides represented by the above composition formula (1), oxides containing K, Na, and Nb as main metal components are called "KNN" or "KNN material," and are excellent in piezoelectric properties, electrical properties, etc.

[0026] The above composition formula (1) can be rewritten as the following composition formula (1A).

[0027] (K a1 Na a2 Li a3 Ca b1 Sr b2 Ba b3 ) c (Nb d1 Mn d2 Ti d3 Zr d4 ) O 3+e ... (1A)

[0028] The composition formula (1) and the composition formula (1A) are equivalent, and a1 + a2 + a3 = a, and b1 + b2 + b3 = b. The coefficient a1 of K is 0 < a1 ≦ 0.6, and the coefficient a2 of Na is 0 < a1 ≦ 0.6. The coefficient a3 of Li is 0 ≦ a3 ≦ 0.2 (preferably, 0 ≦ a3 ≦ 0.1).

[0029] The subphase is formed of a second crystalline phase containing an Mn—Ti—O-based oxide, which is an oxide containing Mn (manganese) and Ti (titanium), and is represented, for example, by the following composition formula (2):

[0030] MnTiO y ...(2)

[0031] The coefficient y satisfies 2≦y≦8.

[0032] Furthermore, as the Mn-Ti-O-based oxide, MnTi 2 O 4 may be.

[0033] Furthermore, the Mn-Ti-O-based oxides include Mn 2 TiO 4 may be.

[0034] In addition, Mn-Ti-O-based oxides (e.g., MnTi 2 O 4 , Mn 2 TiO 4 The Mn and Ti compositions in the alloy may deviate from the desired values ​​within a range of ±0.2.

[0035] The lead-free piezoelectric composition of the present embodiment may contain a crystalline phase other than the second crystalline phase (such as a third crystalline phase) as long as the object of the present invention is not impaired.

[0036] In the lead-free piezoelectric composition of this embodiment, the maximum particle size of the Mn—Ti—O oxide in the subphase is 35 μm or less. The method for measuring the maximum particle size of the Mn—Ti—O oxide will be described later.

[0037] In the lead-free piezoelectric composition of this embodiment, the Mn—Ti—O-based oxide in the subphase has a cumulative 80% particle size (D80) based on the number of particles of 32 μm or less. The method for measuring the cumulative 80% particle size (D80) based on the number of particles will be described later.

[0038] When the maximum particle size of the Mn—Ti—O-based oxide in the subphase and the number-based cumulative 80% particle size (D80) of the Mn—Ti—O-based oxide in the subphase are each within the above ranges, a lead-free piezoelectric composition having excellent piezoelectric properties and excellent insulating properties (i.e., a high dielectric breakdown voltage) can be obtained.

[0039] In the lead-free piezoelectric composition of this embodiment, the average particle size of the Mn—Ti—O oxide in the subphase is preferably 24 μm or less. The method for measuring the average particle size of the Mn—Ti—O oxide will be described later.

[0040] When the average particle size of the Mn--Ti--O based oxide in the subphase is within the above range, the piezoelectric properties and insulating properties of the lead-free piezoelectric composition are easily improved.

[0041] The subphase, which includes the second crystalline phase satisfying the above-mentioned conditions, is dispersed in a scattered manner within the main phase, which is made of the first crystalline phase. The subphase fills the voids (gaps) formed between the fine crystals of the main phase. Although the subphase does not have piezoelectric properties, its presence in the main phase improves the sinterability and structural stability of the lead-free piezoelectric composition, as well as the insulating properties.

[0042] In this embodiment, the proportion of the subphase contained in the lead-free piezoelectric composition is not particularly limited as long as it does not impair the object of the present invention, but is preferably, for example, 0.5% by volume or more and 5% by volume or less.

[0043] Next, a piezoelectric element 200 according to embodiment 1 will be described with reference to FIG. 1 . FIG. 1 is a perspective view of the piezoelectric element 200 according to embodiment 1. As shown in FIG. 1 , the piezoelectric element 200 according to this embodiment has a disk-shaped appearance and includes a disk-shaped piezoelectric layer (an example of a piezoelectric ceramic layer) 100 and electrodes 301 and 302 attached to the upper and lower surfaces of the piezoelectric layer 100. The piezoelectric layer 100 is formed from the lead-free piezoelectric composition described above. The piezoelectric layer 100 is polarized in the thickness direction. The electrodes 301 and 302 are made of, for example, Au.

[0044] Here, an example of a manufacturing method of the piezoelectric element 200 according to the first embodiment will be described. First, multiple types of raw material powders necessary for forming the main phase are prepared, and these raw material powders are weighed out to obtain the desired composition. The raw material powders may be oxides, carbonates, hydroxides, etc., of the elements contained in the main phase. Ethanol is added to a mixture of the weighed raw material powders, and the mixture is wet-mixed using a ball mill, preferably for 15 hours or more, to obtain a slurry. The obtained slurry is dried, and the mixed powder obtained after drying is calcined, for example, in an air atmosphere at a temperature of 600 to 1000°C for 1 to 10 hours, to obtain a powdered calcined main phase.

[0045] Furthermore, multiple types of raw material powders necessary for forming the subphase are prepared, and these raw material powders are weighed out to achieve the desired composition. The raw material powders may be oxides, carbonates, hydroxides, etc., of the elements contained in the subphase. Ethanol is added to a mixture of the weighed raw material powders, and the mixture is wet-mixed using a ball mill, preferably for 15 hours or more, to obtain a slurry. The resulting slurry is dried, and the mixed powder obtained after drying is calcined, for example, in an air atmosphere at a temperature of 600 to 1000°C for 1 to 10 hours to obtain a powdered calcined subphase.

[0046] Next, a dispersant, a binder, and ethanol are added to the obtained main phase calcined product and the subphase calcined product, and the mixture is pulverized and mixed to obtain a slurry. The obtained slurry is then dried, and the obtained dried product is appropriately granulated and uniaxially pressed under a pressure condition of, for example, 20 MPa to obtain a disk-shaped pre-molded product. The pre-molded product is then subjected to a CIP (cold isostatic pressing) treatment under a pressure condition of, for example, 150 MPa to obtain a molded product.

[0047] The resulting compact is then subjected to a binder removal process by, for example, holding it for 2 to 10 hours at a temperature of 200 to 400° C. The compact after the binder removal process is then fired for 2 to 5 hours at a temperature of, for example, 1000 to 1200° C. in a reducing atmosphere in which the pressure is controlled to be one order of magnitude or more lower than the equilibrium oxygen partial pressure of Ni / NO, thereby obtaining a piezoelectric layer.

[0048] Electrodes made of Au are formed on both the front and back surfaces of the obtained piezoelectric layer, for example, by sputtering. Then, the laminate with the electrodes formed on the piezoelectric layer is subjected to a polarization process in which a DC voltage of 5 kV / mm is applied in silicone oil at 50°C, thereby developing the voltage characteristics of the piezoelectric layer. In this way, the piezoelectric element 200 is obtained.

[0049] In the lead-free piezoelectric composition used in the voltage element 200, the subphase is formed of a second crystalline phase containing an Mn—Ti—O-based oxide, as described above. The size of the crystal grains in this subphase (maximum grain size, D80, average grain size, etc.) can be controlled to a desired size by appropriately setting the grain size of the subphase calcined product and the firing temperature of the compact after the binder removal treatment under a reducing atmosphere. For example, the larger the grain size of the subphase calcined product, the larger the crystal grains of the subphase in the final lead-free piezoelectric composition. Furthermore, the higher the firing temperature of the compact after the binder removal treatment under a reducing atmosphere, the larger the crystal grains of the subphase in the final lead-free piezoelectric composition.

[0050] Next, a piezoelectric element 10 according to a second embodiment will be described with reference to FIG. 2 . FIG. 2 is a cross-sectional view of the piezoelectric element 10 according to the second embodiment. As shown in FIG. 2 , the piezoelectric element 10 of this embodiment includes a piezoelectric layer (an example of a piezoelectric ceramic layer) 11, a plurality of internal electrodes 12, 13 in contact with the piezoelectric layer 11, and two external electrodes 14, 15 connected to the internal electrodes 12, 13. The piezoelectric layer 11 is formed from the lead-free piezoelectric composition described above. The internal electrodes 12, 13 are primarily composed of a base metal (e.g., nickel). The piezoelectric layer 11 and the internal electrodes 12, 13 are alternately stacked. More specifically, the piezoelectric layer 11 and the internal electrodes 12, 13 are stacked in the following order: piezoelectric layer 11, internal electrode 12, piezoelectric layer 11, internal electrode 13, piezoelectric layer 11, etc., with one piezoelectric layer 11 sandwiched between the two internal electrodes 12, 13. Two external electrodes 14, 15 are disposed on the outer surfaces of the laminate of the piezoelectric layer 11 and the internal electrodes 12, 13. The external electrodes 14, 15 are made mainly of, for example, Au. Of the two internal electrodes 12, 13 in contact with one piezoelectric layer 11, one end of one internal electrode 12 is connected to one external electrode 14, and one end of the other internal electrode 13 is connected to the other external electrode 15. When a voltage is applied between the external electrodes 14, 15, the piezoelectric layer 11 expands and contracts, causing the entire piezoelectric element 10 to expand and contract.

[0051] Here, an example of a manufacturing method of the piezoelectric element 10 according to the second embodiment will be described. First, multiple types of raw material powders necessary for forming the main phase are prepared, and these raw material powders are weighed out to obtain the desired composition. The raw material powders may be oxides, carbonates, hydroxides, etc., of the elements contained in the main phase. Ethanol is added to a mixture of the weighed raw material powders, and the mixture is wet-mixed using a ball mill, preferably for 15 hours or more, to obtain a slurry. The obtained slurry is dried, and the mixed powder obtained after drying is calcined, for example, in an air atmosphere at a temperature of 600 to 1000°C for 1 to 10 hours, to obtain a powdered calcined main phase.

[0052] Furthermore, multiple types of raw material powders necessary for forming the subphase are prepared, and these raw material powders are weighed out to achieve the desired composition. The raw material powders may be oxides, carbonates, hydroxides, etc., of the elements contained in the subphase. Ethanol is added to a mixture of the weighed raw material powders, and the mixture is wet-mixed using a ball mill, preferably for 15 hours or more, to obtain a slurry. The resulting slurry is dried, and the mixed powder obtained after drying is calcined, for example, in an air atmosphere at a temperature of 600 to 1000°C for 1 to 10 hours to obtain a powdered calcined subphase.

[0053] Next, a dispersant, a binder, and an organic solvent (e.g., toluene) are added to the obtained main phase calcined product and subphase calcined product, and the mixture is pulverized and mixed to obtain a slurry, which is then processed into a sheet shape using a doctor blade method or the like to produce a ceramic green sheet.

[0054] Next, an electrode layer that will become an internal electrode is formed on one surface of the ceramic green sheet by, for example, screen printing using a conductive paste for the internal electrode. The electrode layer is mainly composed of a base metal, for example, nickel (Ni).

[0055] Next, multiple ceramic green sheets with electrode layers formed thereon are stacked so that the electrode layers are exposed alternately from both sides, and ceramic green sheets without electrode layers are stacked on both the front and back sides of the resulting laminate. The resulting laminate is then pressed together to obtain a laminate in which ceramic green sheets and electrode layers are alternately stacked. This laminate is then cut into a desired shape and then subjected to a binder removal treatment, for example, by holding it at a temperature of 200 to 400°C for 2 to 10 hours.

[0056] The laminate after the binder removal treatment is fired, for example, at a temperature of 1000 to 1200°C for 2 to 5 hours in a reducing atmosphere in which the pressure is controlled to be one order of magnitude or more lower than the equilibrium oxygen partial pressure of Ni / NO.

[0057] After the fired laminate is polished appropriately, a pair of external electrodes made of Au are formed on the side surfaces of the laminate by, for example, sputtering. The pair of external electrodes are formed facing each other with the laminate interposed therebetween. The laminate with the external electrodes formed thereon is subjected to a polarization process to obtain the piezoelectric element 10.

[0058] In the lead-free piezoelectric composition used in the voltage element 10, the subphase is formed of a second crystalline phase containing an Mn—Ti—O-based oxide, as described above. The size of the crystal grains in this subphase (maximum grain size, D80, average grain size, etc.) can be controlled to a desired size by appropriately setting the grain size of the subphase calcined product and the firing temperature of the compact after the binder removal treatment under a reducing atmosphere. For example, the larger the grain size of the subphase calcined product, the larger the crystal grains of the subphase in the final lead-free piezoelectric composition. Furthermore, the higher the firing temperature of the compact after the binder removal treatment under a reducing atmosphere, the larger the crystal grains of the subphase in the final lead-free piezoelectric composition.

[0059] The manufacturing methods of the first and second embodiments described above are merely examples, and various other steps and processing conditions for manufacturing a piezoelectric element can be adopted. For example, instead of separately producing the calcined products of the main phase and the subphase and then mixing and firing the powders of the two, raw materials may be mixed in a quantitative ratio corresponding to the final composition of the lead-free piezoelectric composition, and the mixture may be fired. However, by separately producing the calcined products of the main phase and the subphase and then mixing them, it is easier to more strictly control the compositions of the main phase and the subphase, and therefore it is possible to increase the yield of the lead-free piezoelectric composition. Furthermore, metals or alloys such as platinum (Pt), silver-palladium (Ag-Pd), and silver (Ag) may be used as the material for the electrodes.

[0060] The lead-free piezoelectric composition and piezoelectric element disclosed herein have excellent piezoelectric properties, a high breakdown voltage, and excellent insulating properties. Such lead-free piezoelectric composition and piezoelectric element can be widely used in vibration detection, pressure detection, oscillation, piezoelectric device applications, etc. For example, they can be used in sensors that detect various vibrations (e.g., Knox sensors and combustion pressure sensors), piezoelectric devices such as vibrators, actuators, and filters, high-voltage generators, micropower sources, various driving devices, position control devices, vibration suppression devices, fluid discharge devices (e.g., paint discharge, fuel discharge), etc.

[0061] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples in any way.

[0062] Examples 1 to 7 (Preparation of Main Phase Calcined Product) As raw material powder, K 2 CO 3 Powder, Na 2 CO 3 powder, Nb 2 O 5 Powder, TiO 2 Powder, ZrO 2 Powder, MnCO 3 Powder, BaCO 3Powders were prepared, and each of these raw material powders was weighed so that the content (mol%) of each element was the value shown in Table 1. An appropriate amount of ethanol was added to the mixture of the weighed raw material powders, and the mixture was wet-mixed in a ball mill for 15 hours to obtain a slurry. The obtained slurry was dried, and the mixed powder obtained after drying was calcined in an air atmosphere at a temperature condition of 600 to 1100°C for 1 to 10 hours to obtain a calcined main phase product.

[0063] (Preparation of subphase calcined product) MnCO 3 Powder, TiO 2 Powders were prepared, and each of these raw material powders was mixed with the composition shown in Table 2 (MnTi 2 O 4 ) were weighed out. An appropriate amount of ethanol was added to the mixture of the weighed raw material powders, and the mixture was wet-mixed for 15 hours using a ball mill to obtain a slurry. The obtained slurry was dried, and the mixed powder obtained after drying was calcined in an air atmosphere at a temperature of 600 to 1100°C for 1 to 10 hours to obtain a subphase calcined product.

[0064] (Fabrication of Piezoelectric Element) A dispersant, a binder, and ethanol were added to the obtained main phase calcined product and the subphase calcined product, and the mixture was pulverized and mixed to obtain a slurry. The obtained slurry was then dried, and the obtained dried product was appropriately granulated and uniaxially pressed under a pressure condition of 20 MPa to obtain a disk-shaped pre-molded body. The pre-molded body was then subjected to a CIP (cold isostatic pressing) treatment under a pressure condition of 150 MPa to obtain a molded body. The mixing ratio of the main phase calcined product to the subphase calcined product was adjusted so that the ratio (volume %) of the main phase to the subphase was 97:3.

[0065] The obtained compact was subjected to a binder removal treatment by holding it for 2 to 10 hours at a temperature condition of 200 to 400° C. Then, the compact after the binder removal treatment was fired by holding it for 2 to 5 hours at a temperature condition of 1000 to 1200° C. in a reducing atmosphere in which the pressure was controlled so that it was one order of magnitude or more on the reducing side compared to the equilibrium oxygen partial pressure of Ni / NO, to obtain a piezoelectric layer.

[0066] Au electrodes were formed on both the front and back surfaces of the piezoelectric layer by sputtering. Then, the laminate with the electrodes formed on the piezoelectric layer was subjected to a polarization treatment in which a DC voltage of 5 kV / mm was applied in silicone oil at 50° C., thereby developing the voltage characteristics of the piezoelectric layer and obtaining the piezoelectric element of each example.

[0067] In Examples 1 to 7, the particle size of the subphase calcined product and the firing temperature of the compact after the binder removal treatment in a reducing atmosphere were adjusted appropriately so as to be different from one another.

[0068] Comparative Example 1 A piezoelectric element of Comparative Example 1 was produced in the same manner as in Example 7, except that the particle size of the subphase calcined product was set larger than that of Example 7 and the firing temperature of the compact after the binder removal treatment in a reducing atmosphere was set higher than that of Example 7.

[0069] Comparative Example 2 A calcined main phase product was prepared in the same manner as in Example 1. A calcined subphase product was prepared in the following manner. 2 CO 3 Powder, TiO 2 Powders were prepared, and each of these raw material powders was mixed with the composition shown in Table 3 (LiTi 2 O 4 A subphase calcined product was produced in the same manner as in Example 1, etc., except that the main phase calcined product and the subphase calcined product were weighed so that the weight of the calcined product was 10 ...

[0070] Comparative Example 3 A calcined main phase product was prepared in the same manner as in Example 1. A calcined subphase product was prepared in the following manner. 2 CO 3 Powder, Fe 2 O 3 powder, MgO powder, TiO 2 Powders were prepared, and each of these raw material powders was mixed with the composition shown in Table 3 (LiFeMgTiO 4 A subphase calcined product was produced in the same manner as in Example 1, etc., except that the main phase calcined product and the subphase calcined product were weighed so that the weight of the calcined product was 10 ...

[0071] [Piezoelectric constant d33 For each of the piezoelectric elements (piezoelectric layers) of Example 3, Comparative Example 2, and Comparative Example 3, d 33 The piezoelectric constant (pC / N) was measured using a piezoelectric meter (product name "ZJ-4B", manufactured by the Institute of Vocal Music, Chinese Academy of Sciences). The results are shown in Table 3.

[0072] [Breakdown voltage] The breakdown voltage (kV / mm) of each voltage element of each example and each comparative example was measured by the following method. With the voltage element placed in silicone oil at 25 ° C, a DC voltage was applied at 1 kV / mm for 1 minute, and then the DC voltage was applied for 1 minute each time the applied voltage was increased by 1 kV / mm. The applied voltage (kV / mm) when the voltage element broke down was taken as the breakdown voltage (breakdown electric field) of the voltage element. The results are shown in Tables 2 and 3.

[0073] [Analysis of the Main Phase] For each piezoelectric element (piezoelectric layer) of each Example and Comparative Example, a compositional analysis of the main phase was performed using an electron probe microanalyzer (EPMA) according to the method described below. The piezoelectric layer of the piezoelectric element was cut in the thickness direction, and the cut surface was polished. The polished surface was then photographed at 5000x magnification using an EPMA. From the obtained image, three arbitrary crystal grains in the main phase were selected, and quantitative analysis was performed on these three crystal grains. The average value of the content of each element in the three crystal grains was then taken as the content (mol%) of each element in the main phase. The results are shown in Table 1.

[0074] [Analysis of Subphases] Qualitative analysis of the subphases was performed using an EPMA for each piezoelectric element (piezoelectric layer) in each Example and Comparative Example, using the method described below. For each Example, the polished surface of the piezoelectric layer used in the analysis of the main phase was photographed at 5000x magnification, and elemental mapping of Mn (manganese) and Ti (titanium) was performed using the obtained image. The obtained elemental mapping image confirmed the presence of Mn and Ti in the subphases. For Comparative Example 2, elemental mapping of Li (lithium), Fe (iron), Mg (magnesium), and Ti (titanium) was performed, and the obtained elemental mapping image confirmed the presence of Li, Fe, Mg, and Ti in the subphases. For Comparative Example 3, elemental mapping of Mn (manganese) and Ti (titanium) was performed, and the obtained elemental mapping image confirmed the presence of Mn and Ti in the subphases.

[0075] Furthermore, the composition of the compounds contained in the subphases was identified for the polished surfaces of each example and comparative example using powder X-ray diffraction (XRD). The measurement conditions for XRD were as follows:

[0076] <XRD measurement conditions> Measurement device: Powder X-ray diffractometer Range: 50.00° to 70.00° Wavelength: 0.7 angstroms

[0077] [Grain size (maximum grain size, average grain size, D80) of subphase crystal grains] The polished surface of each example and comparative example was photographed at 1000x or 10000x magnification using a scanning electron microscope (SEM), and a square measurement range with a side length of 250 μm was set for the obtained SEM image (backscattered electron image). Then, for multiple crystal grains present within the measurement range, the major axis diameter and minor axis diameter were determined using image analysis software. The major axis diameter and minor axis diameter of the crystal grain were perpendicular to each other, and the major axis diameter and minor axis diameter were each the maximum value for each axis. The average value of the major axis diameter and minor axis diameter for each crystal grain was then taken as the grain size (particle size) of each crystal grain. The average value of the grain size of each crystal grain within the measurement range thus determined was taken as the average grain size (μm) of the subphase crystal grains.

[0078] The magnification for taking SEM images was first 1000x. Then, when each crystal particle could not be identified from the obtained SEM image, the magnification was changed to 10000x. As a result, only in Example 1, SEM images were taken at a magnification of 10000x, and in the other cases, SEM images were taken at a magnification of 1000x.

[0079] The largest major axis diameter of each crystal grain within the measurement range was taken as the maximum grain size (μm) of the subphase crystal grains. The results are shown in Tables 2 and 3.

[0080] Furthermore, a particle size distribution was created for each crystal particle within the measurement range, arranged in order of particle size from smallest to largest, and the cumulative 80% particle size (D80) based on the number of particles in the particle size distribution was calculated. The results are shown in Tables 2 and 3.

[0081]

[0082]

[0083]

[0084] As shown in Table 2, the lead-free piezoelectric composition used in the piezoelectric elements of Examples 1 to 7 was MnTi. 2 O 4 The alloys have a subphase consisting of Mn—Ti—O-based oxides. In Examples 1 to 7, the maximum grain size of the crystal grains in the subphase is 35 μm or less, and the cumulative 80% grain size (D80) based on the number is 32 μm or less. The alloys of Examples 1 to 7 have a breakdown voltage of 16 kV / mm or more, demonstrating excellent insulating properties.

[0085] Furthermore, as shown in Table 3, the measurement results of the piezoelectric constant of Example 3, which was carried out as a representative of the Examples, confirmed that the lead-free piezoelectric composition used in the piezoelectric elements of Example 3 and the like has excellent piezoelectric properties.

[0086] Comparative Example 1 is MnTi 2 O 4In Comparative Example 1, the breakdown voltage was 13 kV / mm, indicating that the insulating properties were poor.

[0087] In addition, Comparative Example 2 contains a compound (LiTi) that contains Ti (titanium) but does not contain Mn (manganese) as a subphase. 2 O 4 In Comparative Example 2, like Example 3 and the like, the piezoelectric characteristics are excellent, but the dielectric breakdown voltage is 10 kV / mm, and it was confirmed that the insulating properties are low.

[0088] In addition, Comparative Example 3 is a compound (LiFeMgTiO 4 In Comparative Example 3, like Example 3, the piezoelectric characteristics are excellent, but the dielectric breakdown voltage is 12 kV / mm, and it was confirmed that the insulating properties are low.

[0089] Examples 8 to 10 The same main phase calcined products as in Example 1 were prepared. The subphase calcined products were produced by the following method. 3 Powder, TiO 2 Powders were prepared, and each of these raw material powders was mixed with the composition shown in Table 2 (Mn 2 TiO 4 ) were weighed out. An appropriate amount of ethanol was added to the mixture of the weighed raw material powders, and the mixture was wet-mixed for 15 hours using a ball mill to obtain a slurry. The obtained slurry was dried, and the mixed powder obtained after drying was calcined in an air atmosphere at a temperature of 600 to 1100°C for 1 to 10 hours to obtain a subphase calcined product. Using these main phase calcined products and subphase calcined products, piezoelectric elements of Examples 8 to 10 were fabricated in the same manner as in Example 1, etc.

[0090] For each of the piezoelectric elements of Examples 8 to 10, the main phase, the subphase, the breakdown voltage (kV / mm), and the grain size (maximum grain size, average grain size, D80) of the subphase crystal grains were measured by the same methods as in Example 1, etc. The results are shown in Table 4.

[0091]

[0092] As shown in Table 4, the lead-free piezoelectric compositions used in the piezoelectric elements of Examples 8 to 10 contained Mn 2 TiO 4 The alloys of Examples 8 to 10 have a subphase consisting of a Mn—Ti—O-based oxide. In Examples 8 to 10, the maximum grain size of the crystal grains in the subphase is 35 μm or less, and the cumulative 80% grain size (D80) based on the number is 32 μm or less. The alloys of Examples 8 to 10 have a breakdown voltage of 16 kV / mm or more, demonstrating excellent insulating properties.

[0093] 10, 200... Piezoelectric element, 11, 100... Piezoelectric layer (piezoelectric ceramic layer), 12, 13... Internal electrode, 14, 15... External electrode, 301, 302... Electrode

Claims

1. A lead-free piezoelectric composition having a main phase containing an alkali niobate perovskite oxide and a subphase containing an Mn-Ti-O oxide, wherein the maximum particle size of the Mn-Ti-O oxide in the subphase is 35 μm or less and the cumulative 80% particle size (D80) based on number is 32 μm or less.

2. The lead-free piezoelectric composition according to claim 1, wherein the average particle size of the Mn-Ti-O oxide in the subphase is 24 μm or less.

3. The Mn-Ti-O oxide is MnTi 2 O 4 , or Mn 2 TiO 4 The lead-free piezoelectric composition according to claim 1 or claim 2, comprising:

4. A piezoelectric element comprising a laminate of a piezoelectric ceramic layer formed from the lead-free piezoelectric composition according to claim 1 or 2 and an electrode attached to the piezoelectric ceramic layer.