Lead-free piezoelectric composition, and piezoelectric element

MYPI2025001086A0Undetermined Publication Date: 2024-03-30NITERRA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025001086
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-30
Filing Date
2023-09-11
Publication Date
2024-03-30

AI Technical Summary

Technical Problem

Conventional lead-free piezoelectric compositions exhibit poor insulation properties under high-temperature conditions, despite showing good piezoelectric properties under high electric fields.

Method used

A lead-free piezoelectric composition based on an alkali niobate perovskite oxide containing Mn, Ti, and Sc, with a specific compositional formula and particle size range, is developed to enhance both piezoelectric and insulation properties. The composition is represented by (A1_a M1_b)_c (Nb_d1 Mn_d2 Ti_d3 Zr_d4 Sc_d5)O_{3+e}, where A1 and M1 are specific alkali and alkaline earth metals, and the coefficients a to e are within defined ranges to maintain the perovskite structure and optimize electrical properties.

Benefits of technology

The composition achieves excellent piezoelectric properties and insulation properties under high-temperature conditions, with a Sc to Ti molar ratio of 0.004 to 8, and average particle sizes between 1.2 μm and 8.1 μm, enabling effective performance in applications such as vibration detection and pressure sensing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025001086_DRAWING_001
    Figure PI2025001086_DRAWING_001
Patent Text Reader

Abstract

ABSTRACT LEAD-FREE PIEZOELECTRIC COMPOSITION, AND PIEZOELECTRIC ELEMENT [Means for Solution] The lead-free piezoelectric composition of the present invention contains, as a main component, an alkali niobate perovskite-type oxide containing Mn, Ti, and Sc, and has a ratio of Sc content to Ti content of 0.004 or more and 8 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Lead-free piezoelectric composition and piezoelectric element

[0001] The present invention relates to a lead-free piezoelectric composition and a piezoelectric element.

[0002] Conventionally, most piezoelectric elements are made of PZT (lead zirconate titanate)-based materials. However, the lead contained in PZT is considered problematic because it causes environmental load. In recent years, development of piezoelectric elements made of lead-free materials has been promoted. For example, alkali niobate-based perovskite oxides have been proposed as such lead-free materials.

[0003] In recent years, piezoelectric elements used in stacked actuators and the like have been required to be driven under high electric fields and to have high reliability. This type of piezoelectric element includes a laminate in which internal electrodes and piezoelectric ceramic layers made of lead-free alkali niobate perovskite oxide are alternately stacked (see, for example, Patent Document 1). This piezoelectric element exhibits good piezoelectric properties under high electric fields because the piezoelectric ceramic expands and contracts in response to the applied voltage.

[0004] Patent No. 3945536

[0005] (Problem to be Solved by the Invention) Lead-free piezoelectric compositions used in conventional piezoelectric elements exhibit good piezoelectric properties under high electric fields, but have the problem of poor insulating properties under high temperature conditions.

[0006] An object of the present invention is to provide a lead-free piezoelectric composition and the like which has excellent piezoelectric properties and excellent insulating properties under high temperature conditions.

[0007] (Means for Solving the Problems) The means for solving the above problems are as follows: <1> A lead-free piezoelectric composition containing, as a main component, an alkali niobate perovskite oxide containing Mn, Ti, and Sc, in which the content ratio of Sc relative to Ti is 0.004 to 8.

[0008] <2> The lead-free piezoelectric composition according to <1>, wherein the alkali niobate perovskite oxide is represented by the following composition formula (1): (A1 a M1 b ) c (Nbd1 Mn d2 Ti d3 Zr d4 Sc d5 ) O 3+e ....(1) where element A1 is at least one of Li, Na, and K, element M1 is at least one of Ba, Ca, and Sr, 0<a<1, 0<b<1, a+b=1, 0.80<c<1.10, 0<d1<1, 0<d2<1, 0<d3<1, 0≦d4<1, 0<d5<1, d1+d2+d3+d4+d5=1, and e is any value that can maintain a perovskite-type crystal structure.

[0009] <3> The lead-free piezoelectric composition according to <2>, wherein the element M1 contains Ba, and 0.06≦b≦0.20 and 0.06≦d4≦0.20 are satisfied.

[0010] <4> The lead-free piezoelectric composition according to <1> or <2>, wherein the average particle size of the crystal particles of the alkali niobate perovskite oxide is 1.2 μm or more and 8.1 μm or less.

[0011] <5> A piezoelectric element having a structure in which the lead-free piezoelectric composition according to any one of <1> to <4> and electrodes are alternately laminated.

[0012] EFFECTS OF THE INVENTION According to the present invention, it is possible to provide a lead-free piezoelectric composition and the like that has excellent piezoelectric properties and excellent insulating properties under high temperature conditions.

[0013] 1 is a perspective view of a piezoelectric element according to a first embodiment; FIG. 2 is a cross-sectional view of a piezoelectric element according to a second embodiment;

[0014] The lead-free piezoelectric composition and piezoelectric element according to the embodiment will be described below.

[0015] The lead-free piezoelectric composition is mainly composed of an alkali niobate-based perovskite oxide containing Mn (manganese), Ti (titanium), and Sc (scandium), that is, the lead-free piezoelectric composition has the alkali niobate-based perovskite oxide as a main phase.

[0016] The alkali niobate perovskite oxide is represented by the following composition formula (1).

[0017] (A1 aM1 b ) c (Nb d1 Mn d2 Ti d3 Zr d4 Sc d5 ) O 3+e ...(1)

[0018] The element A1 is at least one of alkali metals Li (lithium), Na (sodium), and K (potassium), and the element M1 is at least one of alkaline earth metals Ba (barium), Ca (calcium), and Sr (strontium).

[0019] In the above composition formula (1), the elements A1 and M1 are arranged at the A site of the perovskite structure, and Nb (niobium), Mn (manganese), Ti (titanium), and Zr (zirconium) are arranged at the B site.

[0020] As the values ​​of the coefficients a to e in the composition formula (1), values ​​that are preferable in terms of the electrical properties or piezoelectric properties of the lead-free piezoelectric composition are selected from among values ​​that establish a perovskite structure.

[0021] Specifically, the coefficients a and b satisfy 0<a<1, 0<b<1, and a+b=1, and a=0 (i.e., a composition containing no alkali metals) and b=0 (i.e., a composition containing none of Ba, Ca, and Sr) are excluded.

[0022] The coefficient c for all A sites satisfies 0.80<c<1.10, and preferably 0.90≦c≦1.05.

[0023] The coefficients d1, d2, d3, d4, and d5 satisfy the following conditions: 0<d1<1, 0<d2<1, 0<d3<1, 0≦d4<1, 0<d5<1, and d1+d2+d3+d4+d5=1. The following cases are excluded: d1=0 (composition not containing Nb), d2=0 (composition not containing Mn), d3=0 (composition not containing Ti), and d5=0 (composition not containing Sc). The coefficient d4 of Zr may be zero (i.e., the composition may not contain Zr).

[0024] The coefficient d1 of Nb is preferably 0.745≦d1≦0.950, and more preferably 0.830≦d1≦0.959. The coefficient d2 of Mn is preferably 0.001≦d2≦0.07. The coefficient d3 of Ti is preferably 0.005≦d3≦0.06. The coefficient d4 of Zr is preferably 0≦d4≦0.2, and more preferably 0≦d4≦0.1. The coefficient d5 of Sc is preferably 0.0002≦d5≦0.05.

[0025] In the oxygen coefficient 3+e, the coefficient e is a positive or negative value indicating a deficiency or excess of oxygen, with the oxygen coefficient usually being 3. The oxygen coefficient 3+e can take a value such that the main phase constitutes a perovskite-type oxide. A typical value of the coefficient e is e=0, and 0≦e≦0.1 is preferred. The value of the coefficient e can be calculated from the electrical neutrality condition of the composition of the main phase. However, a composition that slightly deviates from the electrical neutrality condition is also acceptable as the composition of the main phase.

[0026] In the composition formula (1), it is preferable that the element M1 contains Ba, and that 0.06≦b≦0.20 and 0.06≦d4≦0.20 are satisfied. When the composition formula (1) satisfies these conditions, the piezoelectric characteristics (displacement characteristics) are particularly excellent. In this case, it is preferable that the conditions further satisfy 0.80≦a≦0.94, a+b=1, 0.80<c<1.10 (preferably 0.90≦c≦1.05), 0.745≦d1≦0.885, 0.01≦d2≦0.07, 0.005≦d3≦0.06, 0.06≦d4≦0.2, 0.001≦d5≦0.04, d1+d2+d3+d4+d5=1, and 0≦e≦0.1.

[0027] Among the alkali niobate perovskite oxides represented by the above composition formula (1), oxides containing K, Na, and Nb as main metal components are called "KNN" or "KNN material," and are excellent in piezoelectric properties, electrical properties, etc.

[0028] The above composition formula (1) can be rewritten as the following composition formula (1A).

[0029] (K a1 Na a2 Li a3Ba b1 Ca b2 Sr b3 ) c (Nb d1 Mn d2 Ti d3 Zr d4 Sc d5 ) O 3+e ...(1A)

[0030] The composition formula (1) and the composition formula (1A) are equivalent, and a1 + a2 + a3 = a, and b1 + b2 + b3 = b. The coefficient a1 of K is 0 < a1 ≦ 0.7 (preferably, 0.095 ≦ a1 ≦ 0.665), the coefficient a2 of Na is 0 < a1 ≦ 0.9 (preferably, 0.285 ≦ a2 ≦ 0.855), and the coefficient a3 of Li is 0 ≦ a3 ≦ 0.2 (preferably, 0 ≦ a3 ≦ 0.1). The coefficient b1 of Ba is 0 ≦ b1 ≦ 0.05, the coefficient b2 of Ca is 0 ≦ b2 ≦ 0.05, and the coefficient b3 of Sr is 0 ≦ b3 ≦ 0.05.

[0031] In the alkali niobate perovskite oxide represented by the composition formula (1) or (1A), the molar ratio of Sc to Ti (Sc / Ti) is from 0.004 to 8. When the Sc to Ti content is in this range, a lead-free piezoelectric composition having excellent piezoelectric properties and excellent insulating properties under high-temperature conditions can be obtained.

[0032] In the composition formula (1A), it is preferable that 0.06≦b1≦0.20 and 0.06≦d4≦0.20. When the composition formula (1A) satisfies these conditions, the piezoelectric properties (displacement properties) are particularly excellent. In this case, the conditions are preferably further as follows: 0.400≦a1≦0.470, 0.400≦a2≦0.470, 0≦b2≦0.02, b3=0, a1+a2+b1+b2+b3=1, 0.80<c<1.10 (preferably 0.90≦c≦1.05), 0.745≦d1≦0.885, 0.01≦d2≦0.07, 0.005≦d3≦0.06, 0.06≦d4≦0.2, 0.001≦d5≦0.04, d1+d2+d3+d4+d5=1, 0≦e≦0.1.

[0033] In this embodiment, the proportion of the main phase contained in the lead-free piezoelectric composition is not particularly limited as long as it does not impair the object of the present invention, but is, for example, preferably 50 vol% or more, more preferably 70 vol% or more, and even more preferably 90 vol% or more.

[0034] The lead-free piezoelectric composition of this embodiment may have a subphase consisting of another crystalline phase in addition to the crystalline phase of the alkali niobate perovskite oxide, as long as it does not impair the object of the present invention.

[0035] In the lead-free piezoelectric composition of this embodiment, the average particle size of the crystal grains of the alkali niobate perovskite oxide forming the main phase is preferably 1.2 μm or more and 8.1 μm or less. When the average particle size is in this range, the insulating properties are particularly excellent under high-temperature conditions (e.g., 150° C.). The method for measuring the average particle size will be described later.

[0036] Next, a piezoelectric element 200 according to embodiment 1 will be described with reference to FIG. 1 . FIG. 1 is a perspective view of the piezoelectric element 200 according to embodiment 1. As shown in FIG. 1 , the piezoelectric element 200 according to this embodiment has a disk-shaped appearance and includes a disk-shaped piezoelectric layer (an example of a piezoelectric ceramic layer) 100 and electrodes 301 and 302 attached to the upper and lower surfaces of the piezoelectric layer 100. The piezoelectric layer 100 is formed from the lead-free piezoelectric composition described above. The piezoelectric layer 100 is polarized in the thickness direction. The electrodes 301 and 302 are made of, for example, Au.

[0037] Here, an example of a manufacturing method of the piezoelectric element 200 according to the first embodiment will be described. First, multiple types of raw material powders necessary for forming the main phase are prepared, and these raw material powders are weighed out to obtain the desired composition. The raw material powders may be oxides, carbonates, hydroxides, etc., of the elements contained in the main phase. Ethanol is added to a mixture of the weighed raw material powders, and the mixture is wet-mixed using a ball mill, preferably for 15 hours or more, to obtain a slurry. The obtained slurry is dried, and the mixed powder obtained after drying is calcined, for example, in an air atmosphere at a temperature of 600 to 1000°C for 1 to 10 hours, to obtain a powdered calcined main phase.

[0038] Next, a dispersant, a binder, and ethanol are added to the calcined main phase, and the mixture is pulverized and mixed to obtain a slurry. The resulting slurry is then dried, and the dried product is appropriately granulated and uniaxially pressed under a pressure of, for example, 20 MPa to obtain a disk-shaped pre-form. The pre-form is then subjected to a CIP (cold isostatic pressing) process under a pressure of, for example, 150 MPa to obtain a compact.

[0039] The resulting compact is then subjected to a binder removal process by, for example, holding it for 2 to 10 hours at a temperature of 200 to 400° C. The compact after the binder removal process is then fired for 2 to 5 hours at a temperature of, for example, 1000 to 1200° C. in a reducing atmosphere in which the pressure is controlled to be one order of magnitude or more lower than the equilibrium oxygen partial pressure of Ni / NO, thereby obtaining a piezoelectric layer.

[0040] Electrodes made of Au are formed on both the front and back surfaces of the obtained piezoelectric layer, for example, by sputtering. Then, the laminate with the electrodes formed on the piezoelectric layer is subjected to a polarization process in which a DC voltage of 5 kV / mm is applied in silicone oil at 50°C, thereby developing the voltage characteristics of the piezoelectric layer. In this way, the piezoelectric element 200 is obtained.

[0041] Next, a piezoelectric element 10 according to a second embodiment will be described with reference to FIG. 2 . FIG. 2 is a cross-sectional view of the piezoelectric element 10 according to the second embodiment. As shown in FIG. 2 , the piezoelectric element 10 of this embodiment includes a piezoelectric layer (an example of a piezoelectric ceramic layer) 11, a plurality of internal electrodes 12, 13 in contact with the piezoelectric layer 11, and two external electrodes 14, 15 connected to the internal electrodes 12, 13. The piezoelectric layer 11 is formed from the lead-free piezoelectric composition described above. The internal electrodes 12, 13 are primarily composed of a base metal (e.g., nickel). The piezoelectric layer 11 and the internal electrodes 12, 13 are alternately stacked. More specifically, the piezoelectric layer 11 and the internal electrodes 12, 13 are stacked in the following order: piezoelectric layer 11, internal electrode 12, piezoelectric layer 11, internal electrode 13, piezoelectric layer 11, etc., with one piezoelectric layer 11 sandwiched between the two internal electrodes 12, 13. Two external electrodes 14, 15 are disposed on the outer surfaces of the laminate of the piezoelectric layer 11 and the internal electrodes 12, 13. The external electrodes 14, 15 are made mainly of, for example, Au. Of the two internal electrodes 12, 13 in contact with one piezoelectric layer 11, one end of one internal electrode 12 is connected to one external electrode 14, and one end of the other internal electrode 13 is connected to the other external electrode 15. When a voltage is applied between the external electrodes 14, 15, the piezoelectric layer 11 expands and contracts, causing the entire piezoelectric element 10 to expand and contract.

[0042] Here, an example of a manufacturing method of the piezoelectric element 10 according to the second embodiment will be described. First, multiple types of raw material powders necessary for forming the main phase are prepared, and these raw material powders are weighed out to obtain the desired composition. The raw material powders may be oxides, carbonates, hydroxides, etc., of the elements contained in the main phase. Ethanol is added to a mixture of the weighed raw material powders, and the mixture is wet-mixed using a ball mill, preferably for 15 hours or more, to obtain a slurry. The obtained slurry is dried, and the mixed powder obtained after drying is calcined, for example, in an air atmosphere at a temperature of 600 to 1000°C for 1 to 10 hours, to obtain a powdered calcined main phase.

[0043] Next, a dispersant, a binder, and an organic solvent (e.g., toluene) are added to the calcined main phase, and the mixture is pulverized and mixed to obtain a slurry, which is then processed into a sheet shape using a doctor blade method or the like to produce a ceramic green sheet.

[0044] Next, an electrode layer that will become an internal electrode is formed on one surface of the ceramic green sheet by, for example, screen printing using a conductive paste for the internal electrode. The electrode layer is mainly composed of a base metal, for example, nickel (Ni).

[0045] Next, multiple ceramic green sheets with electrode layers formed thereon are stacked so that the electrode layers are exposed alternately from both sides, and ceramic green sheets without electrode layers are stacked on both the front and back sides of the resulting laminate. The resulting laminate is then pressed together to obtain a laminate in which ceramic green sheets and electrode layers are alternately stacked. This laminate is then cut into a desired shape and then subjected to a binder removal treatment, for example, by holding it at a temperature of 200 to 400°C for 2 to 10 hours.

[0046] The laminate after the binder removal treatment is fired, for example, at a temperature of 1000 to 1200°C for 2 to 5 hours in a reducing atmosphere in which the pressure is controlled to be one order of magnitude or more lower than the equilibrium oxygen partial pressure of Ni / NO.

[0047] After the fired laminate has been polished appropriately, a pair of external electrodes made of Au are formed on the side surfaces of the laminate, for example by sputtering. The pair of external electrodes are formed facing each other with the laminate interposed therebetween. The laminate with the external electrodes formed thereon is subjected to a polarization process to obtain a piezoelectric element 10. In this way, a piezoelectric element (multilayer piezoelectric element) 10 having a structure in which piezoelectric layers made of a lead-free piezoelectric composition and electrodes (internal electrodes) are alternately stacked is obtained.

[0048] The manufacturing methods of the first and second embodiments described above are merely examples, and various other steps and processing conditions for manufacturing a piezoelectric element can be adopted. For example, when the lead-free piezoelectric composition contains a subphase, multiple types of raw material powders necessary for forming the subphase may be prepared, and a powdered subphase calcined product may be produced using these raw material powders as appropriate. The resulting subphase calcined product may then be mixed with the main phase calcined product in a predetermined ratio as appropriate to form the desired piezoelectric element. Furthermore, metals or alloys such as platinum (Pt), silver-palladium (Ag-Pd), and silver (Ag) may be used as the electrode material.

[0049] The lead-free piezoelectric composition and piezoelectric element disclosed herein have excellent piezoelectric properties under high electric fields and excellent insulating properties even under high-temperature conditions (e.g., 150°C). Such lead-free piezoelectric compositions and piezoelectric elements can be widely used in vibration detection, pressure detection, oscillation, piezoelectric device applications, etc. For example, they can be used in sensors that detect various vibrations (e.g., Knox sensors and combustion pressure sensors), piezoelectric devices such as vibrators, actuators, and filters, high-voltage generators, micropower sources, various driving devices, position control devices, vibration suppression devices, fluid ejection devices (e.g., paint ejection, fuel ejection), etc.

[0050] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples in any way.

[0051] [Examples 1 to 48 and Comparative Examples 1 to 8] (Preparation of Main Phase Calcined Product) As raw material powder, K 2 CO 3 Powder, Na 2 CO 3 powder, Nb 2 O 5 Powder, TiO 2 Powder, ZrO 2 Powder, MnCO 3 Powder, BaCO 3 Powder, Sc 2 O 3Powders were prepared, and each of these raw material powders was weighed out so as to obtain the compositions shown in Tables 1 to 4. An appropriate amount of ethanol was added to the mixture of the weighed raw material powders, and the mixture was wet-mixed in a ball mill for 15 hours to obtain a slurry. The obtained slurry was dried, and the mixed powder obtained after drying was calcined in an air atmosphere at a temperature of 600 to 1100°C for 1 to 10 hours to obtain a powdery calcined main phase product.

[0052] (Fabrication of Piezoelectric Elements) A dispersant, a binder, and ethanol were added to the calcined main phase, and the mixture was pulverized and mixed to obtain a slurry. The resulting slurry was then dried, and the dried product was appropriately granulated and uniaxially pressed under a pressure of 20 MPa to obtain a disk-shaped pre-formed body. The pre-formed body was then subjected to a CIP (cold isostatic pressing) process under a pressure of 150 MPa to obtain a compact.

[0053] The obtained compact was subjected to a binder removal treatment by holding it for 2 to 10 hours at a temperature condition of 200 to 400° C. Then, the compact after the binder removal treatment was fired by holding it for 2 to 5 hours at a temperature condition of 1000 to 1200° C. in a reducing atmosphere in which the pressure was controlled so that it was one order of magnitude or more on the reducing side compared to the equilibrium oxygen partial pressure of Ni / NO, to obtain a piezoelectric layer.

[0054] Au electrodes were formed on both the front and back surfaces of the piezoelectric layer by sputtering. Then, the laminate with the electrodes formed on the piezoelectric layer was subjected to a polarization treatment in which a DC voltage of 5 kV / mm was applied in silicone oil at 50° C., thereby developing the voltage characteristics of the piezoelectric layer and obtaining a piezoelectric element.

[0055] [Evaluation of Piezoelectric Properties] For each piezoelectric element (piezoelectric layer) of each Example and Comparative Example, a laser Doppler vibrometer was used to apply an electric field of 1 to 10 kV / mm, measure the vertical displacement S of the element at a measurement frequency of 100 Hz, calculate the S / E value for each electric field by dividing this displacement S by the electric field E, and evaluate the displacement characteristics (piezoelectric properties) using the maximum S / E value Smax / Emax. The results are shown in Tables 1 to 4.

[0056] [Measurement of Insulation Resistance] The insulation resistance (Ω m) of each piezoelectric element in each Example and Comparative Example was measured by the method described below. A DC voltage of 5 kV / mm was applied to the piezoelectric element for 1 minute in a state where the piezoelectric element was placed in silicone oil at 150°C, and the insulation resistance (Ω m) was measured. The results are shown in Tables 1 to 4.

[0057] [Analysis of the Main Phase] For each piezoelectric element (piezoelectric layer) of each Example and Comparative Example, a compositional analysis of the main phase was performed using a scanning electron microscope-energy dispersive X-ray analyzer (SEM-EDS) according to the method described below. The piezoelectric layer of the piezoelectric element was cut in the thickness direction, and the cut surface was polished. The polished surface was then photographed at 3000x magnification using an SEM. From the resulting image, three random crystal grains in the main phase were selected, and quantitative analysis of each element was performed on those three crystal grains using EDS. The electron beam measurement probe diameter was approximately 1 μm. The composition of each Example and Comparative Example was then determined from the average of the quantitative values ​​of each element in the three crystal grains. The results are shown in Tables 1 to 4. Note that "-" in Tables 1 to 4 indicates that the value was below the detection limit of the instrument.

[0058] [Average Particle Diameter of Main Phase Crystal Grains] The polished surface of each of the piezoelectric elements (piezoelectric layers) of Example 12, Examples 45 to 48, and Comparative Examples 6 to 8 was photographed at 3000x magnification using a scanning electron microscope (SEM). A square measurement range with a side length of 250 μm was set for the resulting SEM image (backscattered electron image). Then, using image analysis software, the major axis diameter and minor axis diameter of each of the multiple crystal grains present within the measurement range were determined. The major axis diameter and minor axis diameter of the crystal grain were perpendicular to each other, and the major axis diameter and minor axis diameter were the maximum values ​​for each axis. The average value of the major axis diameter and minor axis diameter for each crystal grain was then used as the grain size (particle diameter) of each crystal grain. The average value of the grain size of each crystal grain within the measurement range thus determined was used as the average grain size (μm) of the main phase crystal grains.

[0059]

[0060]

[0061]

[0062]

[0063] As shown in Tables 1 and 2, the lead-free piezoelectric compositions used in the piezoelectric elements of Examples 1 to 34 have an alkali niobate perovskite oxide containing Mn, Ti, and Sc as the main component (main phase), and the molar ratio of Sc to Ti in the alkali niobate perovskite oxide is 0.004 to 8. Examples 1 to 34 have an insulation resistance of 4×10 under high-temperature conditions (150°C). 8 The maximum S / E value (Smax / Emax) in Examples 1 to 34 was 132 pm / V or more, and it was confirmed that Examples 1 to 34 had excellent piezoelectric properties (displacement characteristics).

[0064] The lead-free piezoelectric composition of Comparative Example 1 is composed of an alkali niobate perovskite oxide containing Mn and Sc but not Ti. The piezoelectric element of Comparative Example 1 had excellent insulation properties under high temperature conditions, but the maximum S / E value Smax / Emax was 98 pm / V, which meant that the piezoelectric characteristics were problematic.

[0065] The lead-free piezoelectric composition of Comparative Example 2 is composed of an alkali niobate perovskite oxide containing Mn and Ti but not Sc. The piezoelectric element of Comparative Example 2 had problems with insulation properties under high temperature conditions. In the case of Comparative Example 2, the insulation resistance could not be measured. Furthermore, the piezoelectric element of Comparative Example 2 had problems with piezoelectric properties.

[0066] The lead-free piezoelectric composition of Comparative Example 3 is composed of an alkali niobate perovskite oxide containing Ti and Sc but not Mn. Since the lead-free piezoelectric composition of Comparative Example 3 does not contain Mn, it has poor sinterability and has problems with insulation and piezoelectric properties under high temperature conditions. In the case of Comparative Example 3, the S / E value and insulation resistance could not be measured.

[0067] The lead-free piezoelectric composition of Comparative Example 4 has an excessively large Sc content relative to Ti (Sc / Ti=10). The piezoelectric element of Comparative Example 4 has excellent insulation properties under high temperature conditions, but the maximum S / E value (Smax / Emax) was 104 pm / V, which means that the piezoelectric characteristics were poor.

[0068] The lead-free piezoelectric composition of Comparative Example 5 has an excessively small Sc to Ti content (Sc / Ti=0.003). The piezoelectric element of Comparative Example 5 has excellent insulation properties under high temperature conditions, but the maximum S / E value (Smax / Emax) was 106 pm / V, which means that the piezoelectric characteristics were poor.

[0069] Although the lead-free piezoelectric composition can achieve high piezoelectric properties by including Ti, an excessive Ti content reduces the insulating properties. Furthermore, the lead-free piezoelectric composition can achieve high insulating properties under high-temperature conditions by including Sc. However, since a large amount of Sc tends to cause a loss of ferroelectricity (i.e., a decrease in piezoelectric properties), a low Ti content reduces the piezoelectric properties. Furthermore, since a high Ti content makes it difficult to lose ferroelectricity, a large amount of Sc does not reduce the piezoelectric properties. Therefore, in the case of a lead-free piezoelectric composition made of an alkali niobate perovskite oxide, the ratio of Sc to Ti is presumed to be important for achieving both piezoelectric properties and insulating properties under high-temperature conditions. Furthermore, the addition of Mn to the lead-free piezoelectric composition improves sinterability and exhibits piezoelectric properties.

[0070] As shown in Table 3, the lead-free piezoelectric compositions used in the piezoelectric elements of Examples 35 to 43 have an alkali niobate perovskite oxide containing Mn, Ti, and Sc as the main component (main phase), and the molar ratio of Sc to Ti in the alkali niobate perovskite oxide is 0.004 to 8. In particular, in Examples 35 to 43, the alkali niobate perovskite oxide constituting the main phase of the lead-free piezoelectric composition contains Ba and Zr, and the coefficient b in the composition formula (1) is in the range of 0.06≦b≦0.20, and the coefficient d4 is in the range of 0.06≦d4≦0.20. Furthermore, the coefficient b1 in the composition formula (1A) is in the range of 0.06≦b≦0.20, and the coefficient d4 is in the range of 0.06≦d4≦0.20. In the case of Examples 35 to 43, the maximum value of the S / E value, Smax / Emax, is 248 pm / V or more, and the piezoelectric characteristics (displacement characteristics) are particularly excellent.

[0071] In contrast, as shown in Table 3, in the case of Comparative Example 6, the alkali niobate perovskite oxide constituting the main phase of the lead-free piezoelectric composition has a larger value of coefficient b in the composition formula (1) than in Example 35, etc., and also a larger value of coefficient d4 than in Example 35, etc. In the case of Comparative Example 6, the maximum value of the S / E value, Smax / Emax, was 91 pm / V, and there was a problem with the piezoelectric characteristics (displacement characteristics).

[0072] Furthermore, as shown in Table 4, the average particle size of the crystal particles of the alkali niobate perovskite oxide is 1.2 μm or more and 8.1 μm or less in the cases of Example 12 and Examples 44 to 48. It was confirmed that the insulating properties are particularly excellent under high temperature conditions (150° C.) in the cases of Example 12 and Examples 44 to 48.

[0073] In contrast, as shown in Table 4, Comparative Example 7 has an average crystal particle size of 4.3 μm, but the molar ratio of Sc to Ti in the alkali niobate perovskite oxide is 0.003. In Comparative Example 7, the insulation resistance value was low and there were problems with insulation. In Comparative Example 8, the average crystal particle size was too large, and there were problems with insulation.

[0074] Table 4 shows the production conditions (baking temperature (° C.), holding time (hrs)) for Example 12, Examples 44 to 48, Comparative Example 7, and Comparative Example 8.

[0075] 10, 200... Piezoelectric element, 11, 100... Piezoelectric layer (piezoelectric ceramic layer), 12, 13... Internal electrode, 14, 15... External electrode, 301, 302... Electrode

Claims

1. A lead-free piezoelectric composition whose main component is an alkali niobate perovskite oxide containing Mn, Ti, and Sc, in which the Sc content relative to Ti is 0.004 or more and 8 or less.

2. The lead-free piezoelectric composition according to claim 1, wherein the alkali niobate perovskite oxide is represented by the following composition formula (1): (A1 a M1 b ) c (Nb d1 Mn d2 Ti d3 Zr d4 Sc d5 ) O 3+e ....(1) where element A1 is at least one of Li, Na, and K, element M1 is at least one of Ba, Ca, and Sr, 0<a<1, 0<b<1, a+b=1, 0.80<c<1.10, 0<d1<1, 0<d2<1, 0<d3<1, 0≦d4<1, 0<d5<1, d1+d2+d3+d4+d5=1, and e is any value that can maintain a perovskite-type crystal structure.

3. The lead-free piezoelectric composition according to claim 2, wherein the element M1 includes Ba, and 0.06≦b≦0.20 and 0.06≦d4≦0.

20.

4. The lead-free piezoelectric composition according to claim 1 or 2, wherein the average particle size of the crystal particles of the alkali niobate perovskite oxide is 1.2 μm or more and 8.1 μm or less.

5. A piezoelectric element having a structure in which the lead-free piezoelectric composition according to any one of claims 1 to 4 and electrodes are alternately laminated.