Surface-treated steel sheet
Patent Information
- Application Number
- MYPI2025001087
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-08-31
- Filing Date
- 2023-08-30
- Publication Date
- 2024-02-29
AI Technical Summary
Surface-treated steel sheets face challenges with insufficient adhesion to adhesives, blackening resistance, and dew condensation discoloration, despite improved corrosion resistance from existing coatings.
A surface-treated steel sheet configuration featuring a plating layer with Al and Mg content between 5.0-25.0% and 3.0-12.5% respectively, a chemical conversion coating containing Zr, V, P, and Co, and an acrylic resin, with specific mass ratios and adhesion amounts, which enhances corrosion resistance, adhesion, and blackening resistance, while controlling dew condensation discoloration.
The proposed configuration achieves excellent corrosion resistance, adhesion with adhesives, blackening resistance, and resistance to dew condensation discoloration, ensuring improved performance and appearance of the steel sheets.
Smart Images

Figure PI2025001087_DRAWING_001
Abstract
Description
Surface-treated steel sheet
[0001] The present disclosure relates to a surface-treated steel sheet having a plating layer and a chemical conversion coating on its surface.
[0002] A surface-treated steel sheet comprises a base steel sheet, a plating layer formed on the base steel sheet, and a coating formed on the plating layer. Surface-treated steel sheets are widely used in applications such as building materials, automobiles, and home appliances. The plating layer and coating enhance the corrosion resistance of surface-treated steel sheets.
[0003] As coatings for improving the corrosion resistance of surface-treated steel sheets, coatings made of inorganic materials, organic resin coatings, and coatings made of inorganic materials and organic resins, which are formed by chemical conversion treatments such as chromate treatment and phosphate treatment, have been proposed.
[0004] For example, coatings made of inorganic materials are disclosed in Japanese Patent Laid-Open No. 2002-030460 (Patent Document 1) and International Publication No. 2007 / 123276 (Patent Document 2). Patent Document 1 proposes a metal surface treatment agent containing a vanadium compound and a metal compound containing at least one metal selected from zirconium, titanium, molybdenum, tungsten, manganese, and cerium. Patent Document 2 also proposes a zinc-containing plated steel material treated with a composite coating using a treatment solution containing a basic zirconium compound, a vanadyl-containing compound, a phosphate compound, a cobalt compound, an organic acid, and water.
[0005] Organic resin coatings are disclosed in International Publication Nos. 2007 / 069783 (Patent Document 3) and 2009 / 004684 (Patent Document 4). Patent Document 3 proposes an organic resin coating formed from a surface treatment agent for metal materials comprising an anionic water-dispersible resin and an alkali metal silicate. Patent Document 4 also proposes an organic resin coating formed from a surface treatment agent comprising ammonium zirconium carbonate, a tetravalent vanadium compound, an organic phosphonic acid, and an anionic water-dispersible acrylic resin.
[0006] Coatings made of inorganic materials and organic resins are disclosed in Japanese Patent Laid-Open No. 2003-055777 (Patent Document 5) and Japanese Patent Laid-Open No. 2005-097733 (Patent Document 6). Patent Document 5 proposes a surface-treated steel sheet in which a coating made of a zirconium compound and a vanadium compound is formed on a Zn—Al—Mg—Si alloy plating. Patent Document 6 also proposes a surface-treated steel sheet in which a coating made of an acrylic resin composed of a vanadium compound, a phosphate compound, a metal component, and a specific monomer component is formed on a Zn—Al alloy plating.
[0007] Surface-treated steel sheets having these coatings can have improved corrosion resistance. However, these surface-treated steel sheets sometimes fail to provide sufficient adhesion to adhesives. Furthermore, from the viewpoint of appearance, it is also required to suppress blackening in surface-treated steel sheets, that is, to improve blackening resistance.
[0008] Therefore, WO 2017 / 155028 (Patent Document 7) proposes a surface-treated steel sheet that exhibits corrosion resistance, sufficient adhesion to adhesives, and sufficient resistance to blackening. The surface-treated steel sheet disclosed in Patent Document 7 includes a steel sheet, a zinc-containing plating layer formed on the steel sheet, and a coating formed on the plating layer. The coating contains acrylic resin, zirconium, vanadium, phosphorus, and cobalt, and in a region of the cross section of the coating from the surface to 1 / 5 of the film thickness, the acrylic resin has an area ratio of 80 to 100 area %, and in a region consisting of a region from the film thickness center of the coating to the surface side to 1 / 10 of the film thickness and a region from the film thickness center to the plated layer side to 1 / 10 of the film thickness, the acrylic resin has an area ratio of 5 to 50 area %.
[0009] Japanese Patent Publication No. 2002-030460, International Publication No. 2007 / 123276, International Publication No. 2007 / 069783, International Publication No. 2009 / 004684, Japanese Patent Publication No. 2003-055777, Japanese Patent Publication No. 2005-097733, International Publication No. 2017 / 155028
[0010] The surface-treated steel sheet disclosed in Patent Document 7 has sufficient corrosion resistance, sufficient adhesion to adhesives, and sufficient resistance to blackening.
[0011] Incidentally, when condensation forms on the surface of a surface-treated steel sheet, discoloration of the condensed areas may occur. This phenomenon is referred to as "condensation discoloration" in this specification. Condensation discoloration does not have any particular effect on the mechanical properties of the surface-treated steel sheet. However, since patterns are formed in the condensed areas, the appearance of the surface-treated steel sheet is reduced. Therefore, it is preferable that the surface-treated steel sheet is less susceptible to condensation discoloration. In other words, excellent resistance to condensation discoloration is also required for the surface-treated steel sheet.
[0012] An object of the present disclosure is to provide a surface-treated steel sheet that has excellent corrosion resistance, excellent adhesion to adhesives, excellent resistance to blackening, and further has excellent resistance to condensation discoloration.
[0013] The surface-treated steel sheet according to the present disclosure comprises a base steel sheet, a plating layer formed on the base steel sheet, and a chemical conversion coating formed on the plating layer, and the plating layer has a chemical composition, in mass%, of Al: more than 5.0 and less than 25.0%, Mg: more than 3.0 and less than 12.5%, Sn: 0 to 3.00%, Bi: 0 to 5.00%, In: 0 to 2.00%, Ca: 0 to 3.00%, Y: 0 to 3.00%, La: 0 to 3.00%, Ce: 0 to 3.00%, Si: 0 to 2.50%, Cr: 0 to 0.5%, Ti: 0 to 0.5%, Ni: 0 to 0.5%, Co: 0 to 0.5%, V: 0 to 0.5%, Nb: 0 to 0.5%, The alloy contains Cu: 0-0.5%, Mn: 0-0.5%, Fe: 0-5.0%, Sr: 0-0.5%, Sb: 0-0.5%, Pb: 0-0.5%, and B: 0-0.5%, with the balance consisting of 65.0% or more Zn and impurities, and the chemical conversion coating contains Zr, V, P, and Co, and an acrylic resin, and the coating weight of the chemical conversion coating is 300-1000 mg / m 2 and the mass of V in the conversion coating [V] mg / m 2 and the mass of P in the conversion coating [P] mg / m 2 and satisfy formula (1), and the Mg content [Mg]b mass% of the chemical composition of the plating layer and the V mass [V]mg / m 2and satisfy the formula (2): 0.60≦[V] / [P]≦2.80 (1) 0<[V] / [Mg]b≦20.00 (2)
[0014] The surface-treated steel sheet of the present disclosure has excellent corrosion resistance, excellent adhesion to adhesives, excellent resistance to blackening, and also excellent resistance to condensation discoloration.
[0015] Fig. 1 is a graph of glow luminescence spectroscopy (GDS spectrum) of elements in a chemical conversion coating and a plating layer of a surface-treated steel sheet. Fig. 2 is a cross-sectional view perpendicular to the rolling direction of a surface-treated steel sheet according to the present embodiment. Fig. 3 is a side view of a lap shear test specimen used in an adhesion evaluation test in the examples.
[0016] The present inventors have conducted research and studies to solve the above problems, and as a result, have come to the following findings.
[0017] In a base steel sheet having a plating layer formed thereon that contains primarily Zn and further contains, by mass%, more than 5.0% but less than 25.0% Al and more than 3.0% but less than 12.5% Mg, excellent corrosion resistance may be obtained if the chemical conversion coating formed on the plating layer contains Zr, V, P, and Co, as well as an acrylic resin.
[0018] Therefore, the inventors investigated the corrosion resistance, adhesiveness with adhesives, and blackening resistance of the surface-treated steel sheet having the above-mentioned configuration, and as a result, they further obtained the following findings.
[0019] The adhesive strength with the adhesive depends on the amount of the conversion coating of the above composition. Specifically, the amount of the conversion coating is 300 to 1000 mg / m 2 If so, excellent adhesion can be obtained in the surface-treated steel sheet.
[0020] Furthermore, the mass of V in the chemical conversion coating is [V] (mg / m 2 ) and the P mass is defined as [P] (mg / m 2) In this case, corrosion resistance and blackening resistance are affected by [V] / [P]. Specifically, if [V] / [P] is less than 0.60, sufficient blackening resistance cannot be obtained. Although the mechanism behind this is not clear, it is thought that if the P mass [P] is too high, the oxidation reaction of the plating, which causes blackening, is promoted. On the other hand, if [V] / [P] exceeds 2.80, sufficient corrosion resistance cannot be obtained. This is because if the P mass [P] in the chemical conversion coating is too small relative to the V mass [V], the corrosion-inhibiting effect of the passivation coating formed by P becomes smaller. If [V] / [P] satisfies formula (1), excellent corrosion resistance and excellent blackening resistance can be obtained. 0.60≦[V] / [P]≦2.80 (1)
[0021] However, even with the surface-treated steel sheet having the above-described configuration, there are still cases where sufficient resistance to condensation discoloration cannot be obtained. Therefore, the present inventors conducted further studies. As a result, the present inventors have newly discovered the following.
[0022] Resistance to condensation discoloration is determined by the V mass [V] (mg / m 2 ) and the Mg content [Mg]b (mass%) in the chemical composition of the plating layer. Specifically, the V mass [V] (mg / m 2 Sufficient resistance to condensation discoloration can be obtained if the relationship between the V / Mg content [Mg]b (mass%) in the plating layer and the Mg content [Mg]b (mass%) in the plating layer satisfies the following formula (2): 0<[V] / [Mg]b≦20.00 (2) This point will be explained below.
[0023] The inventors used an electron probe microanalyzer (EPMA) to measure the concentrations of major elements in areas on the surface of a coated steel sheet where condensation discoloration had occurred and areas where condensation discoloration had not occurred. As a result, in areas where condensation discoloration had occurred, [V] / [Mg]b exceeded 20.00. On the other hand, in areas where condensation discoloration had not occurred, [V] / [Mg]b was greater than 0 to 20.00. Therefore, when the above-mentioned chemical conversion coating containing V is formed on the above-mentioned plating layer with a Mg content of more than 3.0%, the occurrence of condensation discoloration can be suppressed and sufficient condensation discoloration resistance can be achieved if [V] / [Mg]b is 20.00 or less.
[0024] The surface-treated steel sheet of this embodiment has been completed based on the above technical concept, and has the following configuration.
[0025] A surface-treated steel sheet of a first configuration includes a base steel sheet, a plating layer formed on the base steel sheet, and a chemical conversion coating formed on the plating layer, and the plating layer has a chemical composition, in mass%, of Al: more than 5.0 and less than 25.0%, Mg: more than 3.0 and less than 12.5%, Sn: 0 to 3.00%, Bi: 0 to 5.00%, In: 0 to 2.00%, Ca: 0 to 3.00%, Y: 0 to 3.00%, La: 0 to 3.00%, Ce: 0 to 3.00%, Si: 0 to 2.50%, Cr: 0 to 0.5%, Ti: 0 to 0.5%, Ni: 0 to 0.5%, Co: 0 to 0.5%, V: 0 to 0.5%, Nb: 0 to 0.5%, The alloy contains Cu: 0-0.5%, Mn: 0-0.5%, Fe: 0-5.0%, Sr: 0-0.5%, Sb: 0-0.5%, Pb: 0-0.5%, and B: 0-0.5%, with the balance consisting of 65.0% or more Zn and impurities, and the chemical conversion coating contains Zr, V, P, and Co, and an acrylic resin, and the coating weight of the chemical conversion coating is 300-1000 mg / m 2 and the mass of V in the conversion coating [V] mg / m 2 and the mass of P in the conversion coating [P] mg / m 2 and satisfy formula (1), and the Mg content [Mg]b mass% of the chemical composition of the plating layer and the V mass [V]mg / m 2 and satisfy the formula (2): 0.60≦[V] / [P]≦2.80 (1) 0<[V] / [Mg]b≦20.00 (2)
[0026] The surface-treated steel sheet of the second configuration is the surface-treated steel sheet of the first configuration, further comprising: an Mg concentration difference Δ[Mg] mass %, which is the difference between the Mg concentration [Mg]s mass % in the surface layer of the plating layer obtained by elemental analysis of the plating layer in the depth direction using glow discharge optical emission spectrometry and the Mg content [Mg]b mass % in the chemical composition of the plating layer; and a Mg concentration difference Δ[Mg] mass %, which is the difference between the Mg concentration [Mg]s mass % in the surface layer of the plating layer obtained by elemental analysis of the plating layer in the depth direction using glow discharge optical emission spectrometry and the Mg content [Mg]b mass % in the chemical composition of the plating layer. 2 and satisfy the formula (3). Δ[Mg]×[V]≦200 (3)
[0027] Fig. 1 is a graph of glow discharge optical emission spectroscopy (GDS) spectra of elements in the chemical conversion coating and plating layer of a surface-treated steel sheet, obtained by glow discharge optical emission spectroscopy from the surface of the chemical conversion coating in the thickness direction. The horizontal axis of Fig. 1 represents the depth from the surface (measurement time), and the vertical axis represents the concentration (emission intensity) of each element.
[0028] In Fig. 1, the emission intensity of carbon (C) is high from the surface of the surface-treated steel sheet (position 0 on the horizontal axis) to a predetermined depth. The region with high emission intensity of C indicates the region of the chemical conversion coating. On the other hand, the region with high emission intensity of Mg and Al indicates the region of the plating layer.
[0029] Referring to Figure 1, the inventors noticed that in surface-treated steel sheets satisfying formulas (1) and (2), Mg is concentrated in the surface region of the coating layer that is in contact with the chemical conversion coating. The inventors then suspected that in surface-treated steel sheets satisfying formulas (1) and (2), condensation discoloration could be further suppressed by a synergistic reaction between the amount of Mg concentrated in the surface region of the coating layer and the components in the chemical conversion coating. Based on the above considerations, the inventors conducted further studies. As a result, the following findings were discovered.
[0030] In surface-treated steel sheets that satisfy formulas (1) and (2), Mg in the plating layer and V in the chemical conversion coating affect condensation discoloration. As shown in Figure 1, when the Mg concentration difference Δ[Mg], which is the difference between the Mg concentration [Mg]s (mass%) in the surface layer of the plating layer and the Mg content [Mg]b (mass%) in the chemical composition of the plating layer, is reduced, or when the V mass [V] in the chemical conversion coating is kept low, the synergistic effect of Mg and V further suppresses condensation discoloration.
[0031] Based on the above findings, the inventors further investigated the relationship between the Mg concentration difference Δ[Mg] in the plating layer, the V mass [V] in the chemical conversion coating, and condensation discoloration, and as a result, the inventors further discovered the following.
[0032] The Mg concentration difference Δ[Mg] (mass%) in the plating layer and the V mass [V] (mg / m 2) satisfies the formula (3), the surface-treated steel sheet can obtain excellent corrosion resistance, excellent adhesion to adhesives, excellent resistance to blackening, and even excellent resistance to condensation discoloration.
[0033] A surface-treated steel sheet of a third configuration is a surface-treated steel sheet of the first or second configuration, wherein the chemical composition of the coating layer is, in mass %, Sn: 0.01 to 3.00%, Bi: 0.01 to 5.00%, In: 0.01 to 2.00%, Ca: 0.01 to 3.00%, Y: 0.01 to 3.00%, La: 0.01 to 3.00%, Ce: 0.01 to 3.00%, Si: 0.01 to 2.50%, Cr: 0.1 to 0.5%, Ti: 0.1 to 0.5%, Ni: 0.1 to 0.5%, Co: 0.1 to 0.5%, V: 0.1 to 0.5%, Nb: 0.1 to 0.5%, Cu: 0.1 to 0.5%, Contains one or more selected from the group consisting of Mn: 0.1 to 0.5%, Fe: 0.1 to 5.0%, Sr: 0.1 to 0.5%, Sb: 0.1 to 0.5%, Pb: 0.1 to 0.5%, and B: 0.1 to 0.5%.
[0034] Hereinafter, the surface-treated steel sheet of this embodiment will be described with reference to the drawings. In the drawings, substantially identical components are denoted by the same reference numerals, and their description will be omitted. When describing the content of each element, "%" means mass % unless otherwise specified.
[0035] [Configuration of Surface-Treated Steel Sheet] Fig. 2 is a cross-sectional view perpendicular to the rolling direction of the surface-treated steel sheet of this embodiment. Referring to Fig. 2, the surface-treated steel sheet 1 includes a base steel sheet 10, a plating layer 20, and a chemical conversion coating 30. The plating layer 20 is formed on the surface of the base steel sheet 10. The chemical conversion coating 30 is formed on the surface of the plating layer 20. The plating layer 20 may be formed on one side of the base steel sheet 10, or may be formed on both sides of the base steel sheet 10. When the plating layer 20 is formed on both sides of the base steel sheet 10, the chemical conversion coating 30 may be formed only on the plating layer 20 on one side, or may be formed on the plating layer 20 on both sides.
[0036] [Regarding the base steel sheet 10] The base steel sheet 10 is not particularly limited. For example, it may be a steel sheet whose microstructure is mainly composed of ferrite. It may be a steel sheet whose microstructure is mainly composed of ferrite and pearlite. It may be a steel sheet whose microstructure is mainly composed of ferrite and one or more of martensite and bainite. The type of base steel sheet 10 does not particularly affect the effect of the surface-treated steel sheet 1 of this embodiment. Therefore, the base steel sheet 10 is not particularly limited.
[0037] [Regarding the plating layer 20] The plating layer 20 is formed on the surface (one side or both sides) of the base steel sheet 10. The plating layer 20 contains, in mass %, more than 5.0% and less than 25.0% Al, more than 3.0% and less than 12.5% Mg, and 65.0% or more Zn. Each element will be described below.
[0038] Al: More than 5.0% and Less than 25.0% Aluminum (Al) is an easily oxidizable element and enhances the corrosion resistance of the plating layer 20 through sacrificial corrosion protection. When the Al content is more than 5.0% and less than 25.0%, the above-mentioned effects are sufficiently achieved. The preferred lower limit of the Al content is 5.1%, more preferably 7.5%, even more preferably 10.0%, and even more preferably 12.0%. The preferred upper limit of the Al content is 24.9%, even more preferably 24.5%, even more preferably 24.0%, even more preferably 22.0%, and even more preferably 20.0%. The preferred range of the Al content is, for example, 5.1 to 24.9%, even more preferably 7.5 to 24.5%, even more preferably 10.0 to 24.0%, even more preferably 12.0 to 22.0%, and even more preferably 12.0 to 20.0%.
[0039] Mg: More than 3.0% and Less than 12.5% Magnesium (Mg) is an easily oxidizable element and enhances the corrosion resistance of the plating layer 20 through sacrificial corrosion protection. When the Mg content is more than 3.0% and less than 12.5%, the above-mentioned effects are sufficiently obtained. The preferred lower limit of the Mg content is 3.1%, more preferably 3.5%, even more preferably 4.0%, even more preferably 4.5%, even more preferably 5.0%, and even more preferably 5.5%. The preferred upper limit of the Mg content is 12.4%, even more preferably 12.0%, even more preferably 11.0%, and even more preferably 10.0%. The preferable range of the Mg content is, for example, 3.1 to 12.4%, more preferably 3.5 to 12.0%, even more preferably 4.0 to 11.0%, even more preferably 4.5 to 10.0%, even more preferably 5.0 to 10.0%, and even more preferably 5.5 to 10.0%.
[0040] The remainder of the chemical composition of the plating layer 20 of this embodiment is made up of 65.0% or more of Zn and impurities.
[0041] As described above, the plating layer 20 primarily contains Zn. Specifically, the plating layer 20 contains 65.0% or more Zn by mass. If the Zn content of the plating layer 20 is 65.0% or more by mass, sufficient corrosion resistance can be obtained. A preferred lower limit of the Zn content is 67.5%, and more preferably 70.0%. A preferred upper limit of the Zn content is less than 92.0%, more preferably 90.0%, even more preferably 85.0%, and even more preferably 80.0%. A preferred range of the Zn content is, for example, 67.5 to less than 92.0%, more preferably 70.0 to 90.0%, even more preferably 70.0 to 85.0%, and even more preferably 70.0 to 80.0%.
[0042] The above-mentioned impurities refer to those that are mixed in from the raw materials of the plating layer 20 or the manufacturing environment, etc., when the surface-treated steel sheet 1 is industrially manufactured, and are acceptable within a range that does not adversely affect the plating layer 20 according to this embodiment.
[0043] [Optional Elements] The chemical composition of the plating layer 20 may further contain one or more elements selected from the following first to sixth groups in place of a portion of Zn. [Group 1 (Sn group)] Sn: 0 to 3.00%, Bi: 0 to 5.00%, and In: 0 to 2.00% [Group 2 (Ca group)] Ca: 0 to 3.00%, Y: 0 to 3.00%, La: 0 to 3.00%, and Ce: 0 to 3.00% [Group 3] Si: 0 to 2.50% [Group 4 (Cr group)] Cr: 0 to 0.5%, Ti: 0 to 0.5%, Ni: 0 to 0.5%, Co: 0 to 0.5%, V: 0 to 0.5%, Nb: 0 to 0.5%, Cu: 0 to 0.5%, and Mn: 0 to 0.5% [Group 5] Fe: 0 to 5.0% [Group 6 (Sr group)] Sr: 0 to 0.5%, Sb: 0 to 0.5%, Pb: 0 to 0.5%, and B: 0 to 0.5%. The first to sixth groups will be explained below.
[0044] [First Group (Sn, Bi, and In)] The chemical composition of the plating layer 20 may further contain one or more elements selected from the group consisting of tin (Sn), bismuth (Bi), and indium (In) in place of a portion of the Zn. These elements are optional and may not be included. That is, the Sn content, Bi content, and In content may each be 0%. When included, these elements form intermetallic compounds with Mg. As a result, the corrosion resistance of the surface-treated steel sheet is improved. The above effects can be achieved to some extent by including even a small amount of one or more of Sn, Bi, and In. However, if the content of these elements is too high, the viscosity of the plating bath increases even if the contents of the other elements are within the ranges of this embodiment. In this case, the appearance quality of the surface-treated steel sheet 1 is degraded. Therefore, the Sn content is 0 to 3.00%, the Bi content is 0 to 5.00%, and the In content is 0 to 2.00%.
[0045] The lower limit of the Sn content is preferably more than 0%, more preferably 0.01%, and even more preferably 0.05%. The upper limit of the Sn content is preferably 2.70%, more preferably 2.50%, even more preferably 2.00%, and even more preferably 1.70%. The preferred range of the Sn content is, for example, more than 0 to 2.70%, more preferably 0.01 to 2.50%, even more preferably 0.05 to 2.00%, and even more preferably 0.05 to 1.70%.
[0046] The lower limit of the Bi content is preferably more than 0%, more preferably 0.01%, and even more preferably 0.05%. The upper limit of the Bi content is preferably 4.80%, more preferably 4.50%, and even more preferably 4.00%. The preferred range of the Bi content is, for example, more than 0 to 4.80%, more preferably 0.01 to 4.50%, and even more preferably 0.05 to 4.00%.
[0047] The lower limit of the In content is preferably more than 0%, more preferably 0.01%, and even more preferably 0.05%. The upper limit of the In content is preferably 1.90%, more preferably 1.80%, and even more preferably 1.70%. The preferred range of the In content is, for example, more than 0 to 1.90%, more preferably 0.01 to 1.80%, and even more preferably 0.05 to 1.70%.
[0048] [Second Group (Ca, Y, La, and Ce)] The chemical composition of the coating layer 20 may further contain one or more elements selected from the group consisting of calcium (Ca), yttrium (Y), lanthanum (La), and selenium (Ce) in place of a portion of the Zn. These elements are optional and may not be present. That is, the content of these elements may be 0%. When present, these elements form intermetallic compounds with Al and Zn in the coating layer 20. As a result, the corrosion resistance of the surface-treated steel sheet 1 is improved. Even if even a small amount of these elements is present, the above-mentioned effects can be achieved to some extent. However, if the content of these elements is too high, oxide dross increases even if the contents of the other elements are within the ranges of this embodiment. In this case, the appearance quality of the surface-treated steel sheet 1 deteriorates. Therefore, the Ca content is 0 to 3.00%, the Y content is 0 to 3.00%, the La content is 0 to 3.00%, and the Ce content is 0 to 3.00%.
[0049] The lower limit of each of the contents of Ca, Y, La, and Ce is preferably greater than 0%, more preferably 0.01%, even more preferably 0.05%, and even more preferably 0.10%. The upper limit of each of the contents of Ca, Y, La, and Ce is preferably 2.80%, even more preferably 2.50%, and even more preferably 2.00%. The preferred range of each of the contents of Ca, Y, La, and Ce is, for example, greater than 0% to 2.80%, even more preferably 0.01 to 2.50%, even more preferably 0.05 to 2.00%, and even more preferably 0.10 to 2.00%.
[0050] [Third Group (Si)] The chemical composition of the coating layer 20 may further contain silicon (Si) in place of a portion of the Zn. Si is an optional element and does not necessarily need to be contained. That is, the Si content may be 0%. When contained, Si enhances the corrosion resistance of the surface-treated steel sheet 1. Even if even a small amount of Si is contained, the above effect can be obtained to some extent. However, if the Si content is too high, the viscosity of the coating bath increases even if the contents of other elements are within the ranges of this embodiment. In this case, the appearance quality of the surface-treated steel sheet 1 deteriorates. Therefore, the Si content is 0 to 2.50%.
[0051] The lower limit of the Si content is preferably more than 0%, more preferably 0.01%, even more preferably 0.05%, and even more preferably 0.10%. The upper limit of the Si content is preferably 2.00%, more preferably 1.50%, even more preferably 1.00%, and even more preferably 0.50%. The preferred range of the Si content is, for example, more than 0 to 2.00%, more preferably 0.01 to 1.50%, even more preferably 0.05 to 1.00%, and even more preferably 0.10 to 0.50%.
[0052] [Fourth Group (Cr, Ti, Ni, Co, V, Nb, Cu, and Mn)] The chemical composition of the plating layer 20 may further contain, in place of a portion of Zn, one or more elements selected from the group consisting of chromium (Cr), titanium (Ti), nickel (Ni), cobalt (Co), vanadium (V), niobium (Nb), copper (Cu), and manganese (Mn). These elements are optional and may not be present. That is, the content of these elements may be 0%. When present, these elements improve the appearance quality of the surface-treated steel sheet 1. These elements also form intermetallic compounds with Al in the plating layer 20. As a result, the corrosion resistance of the surface-treated steel sheet 1 is improved. Even if even a small amount of these elements is present, the above-mentioned effects can be achieved to some extent. However, if the content of these elements is too high, the viscosity of the plating bath increases even if the content of other elements is within the range of this embodiment. In this case, the appearance quality of the surface-treated steel sheet 1 is degraded. Therefore, the Cr content is 0 to 0.5%, the Ti content is 0 to 0.5%, the Ni content is 0 to 0.5%, the Co content is 0 to 0.5%, the V content is 0 to 0.5%, the Nb content is 0 to 0.5%, the Cu content is 0 to 0.5%, and the Mn content is 0 to 0.5%.
[0053] The lower limit of the content of each of the elements Cr, Ti, Ni, Co, V, Nb, Cu, and Mn is preferably more than 0%, more preferably 0.1%. The upper limit of the content of each of the elements Cr, Ti, Ni, Co, V, Nb, Cu, and Mn is preferably less than 0.5%, more preferably 0.4%. The preferred range of the content of each of the elements Cr, Ti, Ni, Co, V, Nb, Cu, and Mn is, for example, more than 0% to less than 0.5%, more preferably 0.1 to 0.4%.
[0054] [Group 5 (Fe)] The chemical composition of the plating layer 20 may further contain Fe in place of a portion of the Zn. That is, the Fe content may be 0%. When contained, Fe increases the hardness of the plating layer 20 and improves the workability of the surface-treated steel sheet 1. Even if even a small amount of Fe is contained, the above effects can be obtained to some extent. However, if the Fe content is too high, the hardness of the plating layer becomes too high even if the contents of other elements are within the ranges of this embodiment. In this case, the workability of the surface-treated steel sheet 1 will actually decrease. Therefore, the Fe content is 0 to 5.0%.
[0055] The lower limit of the Fe content is preferably more than 0%, more preferably 0.1%, and even more preferably 0.5%. The upper limit of the Fe content is preferably 4.5%, more preferably 4.0%, and even more preferably 3.5%. The Fe content is preferably in the range of more than 0 to 4.5%, more preferably 0.1 to 4.0%, and even more preferably 0.5 to 3.5%, for example.
[0056] [Group 6 (Sr, Sb, Pb, and B)] The chemical composition of the coating layer 20 may further contain, in place of a portion of the Zn, one or more elements selected from the group consisting of strontium (Sr), antimony (Sb), lead (Pb), and boron (B). These elements are optional and may not be present. That is, the content of these elements may be 0%. When present, these elements enhance the metallic luster of the coating layer 20 and improve the appearance quality of the surface-treated steel sheet 1. Even if even a small amount of these elements is present, the above effects can be achieved to some extent. However, if the content of these elements is too high, oxide dross increases even if the contents of the other elements are within the ranges of this embodiment. In this case, the appearance quality of the surface-treated steel sheet 1 deteriorates. Therefore, the Sr content is 0 to 0.5%, the Sb content is 0 to 0.5%, the Pb content is 0 to 0.5%, and the B content is 0 to 0.5%.
[0057] The lower limit of each of the Sr, Sb, Pb, and B elements is preferably more than 0%, more preferably 0.1%. The upper limit of each of the Sr, Sb, Pb, and B elements is preferably less than 0.5%, more preferably 0.4%. The preferred range of each of the Sr, Sb, Pb, and B elements is, for example, more than 0% to less than 0.5%, more preferably 0.1 to 0.4%.
[0058] [Preferable Coating Weight of Plating Layer 20] The coating weight of the plating layer 20 (mg / m 2 The preferred coating weight of the plating layer 20 is, for example, 20 to 500 mg / m 2 A more preferable lower limit of the coating weight of the plating layer 20 is 30 mg / m 2 and more preferably 40 mg / m 2 and more preferably 50 mg / m 2 The preferred upper limit of the coating weight of the plating layer 20 is 400 mg / m 2 and more preferably 300 mg / m 2 and more preferably 200 mg / m 2 The preferred range of the coating weight of the plating layer 20 is, for example, 30 to 400 mg / m 2 and more preferably 40 to 300 mg / m2 and more preferably 50 to 200 mg / m 2 is.
[0059] [Method for measuring the chemical composition and coating weight of the plating layer 20] The content (mass%) of each element in the chemical composition of the plating layer 20 and the coating weight (mg / m 2 ) can be measured in the following way:
[0060] First, the thickness of the plating layer 20 and the thickness of the chemical conversion coating 30 of the surface-treated steel sheet 1 are measured. Specifically, a test piece is taken that includes a cross section perpendicular to the surface of the surface-treated steel sheet 1, with this cross section serving as the observation surface. The observation surface is mirror-polished. After mirror polishing, a region of the observation surface that includes the chemical conversion coating 30, the plating layer 20, and at least the surface layer portion of the base steel sheet 10 is observed with a scanning electron microscope (SEM). The magnification is 400x.
[0061] In the observation field, the chemical conversion coating 30 and the plating layer 20 can be clearly distinguished by contrast. The thickness (μm) of the plating layer 20 and the thickness (μm) of the chemical conversion coating 30 are determined at any five locations in the observation field. The arithmetic mean value of the thicknesses of the plating layer 20 determined at the five locations is defined as the thickness (μm) of the plating layer 20. Similarly, the arithmetic mean value of the thicknesses of the chemical conversion coating 30 determined at the five locations is defined as the thickness (μm) of the chemical conversion coating 30.
[0062] Next, a plurality of test pieces including the chemical conversion coating 30, the plating layer 20, and the base steel sheet 10 are taken from the surface-treated steel sheet 1. Hereinafter, these test pieces are referred to as basic test pieces. The thickness of the basic test piece is the thickness of the surface-treated steel sheet 1. In one basic test piece, the plating layer 20 and the chemical conversion coating 30 are completely dissolved with hexamethylenetetramine hydrochloric acid. Elemental analysis is performed on the solution using ICP-MS (Inductively Coupled Plasma Mass Spectrometry). This allows the total deposition amount (mg / m) of the plating layer 20 and the chemical conversion coating 30 to be determined. 2 ), and the mass (mg / m) of each element contained in the plating layer 20 and the chemical conversion coating 30 2 ) is required.
[0063] Next, a test piece for plating layer analysis is prepared using another basic test piece. Specifically, the chemical conversion coating 30 of the other basic test piece is removed by polishing. At this time, a depth of the chemical conversion coating 30 + (thickness of the plating layer 20 × 0.05) μm is removed from the surface of the basic test piece by polishing. By the above method, a test piece for plating layer analysis composed of the plating layer 20 and the base steel sheet 10 is prepared.
[0064] In the test piece for plating layer analysis, the plating layer 20 is completely dissolved with hexamethylenetetramine hydrochloric acid. The solution is subjected to elemental analysis by ICP-MS. This allows the provisional coating weight (mg / m) of the plating layer 20 to be determined. 2 ), and the provisional mass (mg / m) of each element contained in the plating layer 20 2 ) is required.
[0065] Here, the thickness of the plating layer 20 of the test piece for plating layer analysis corresponds to 0.95 times the thickness of the plating layer 20 of the surface-treated steel sheet 1. Therefore, the provisional coating weight (mg / m 2 ) multiplied by 1 / 0.95 to obtain the coating mass (mg / m 2 ) and the provisional mass of each element (mg / m 2 ) multiplied by 1 / 0.95 to obtain the mass (mg / m) of each element in the plating layer 20. 2 ) The coating weight (mg / m 2 ) and the mass (mg / m) of each element in the plating layer 20 2 ) and calculate the content (mass %) of each element in the plating layer 20.
[0066] [Regarding Chemical Conversion Coating 30] The chemical conversion coating 30 is formed on the surface of the plating layer 20. The chemical conversion coating 30 contains Zr, V, P, Co, and an acrylic resin.
[0067] [Regarding Zr, V, P, and Co] Zirconium (Zr), vanadium (V), phosphorus (P), and cobalt (Co) all function as corrosion inhibitors for the surface-treated steel sheet 1, improving the corrosion resistance of the surface-treated steel sheet 1. Zr, V, P, and Co each function as a corrosion inhibitor effectively in different corrosive environments. Therefore, Zr, V, P, and Co are contained as corrosion inhibitors. This allows the surface-treated steel sheet 1 to inhibit corrosion in various corrosive environments, resulting in excellent corrosion resistance.
[0068] [Regarding Zr in the Chemical Conversion Coating 30] The Zr in the chemical conversion coating 30 forms a cross-linked structure with the acrylic resin. Therefore, the chemical conversion coating 30 has excellent barrier properties. As a result, the surface-treated steel sheet 1 achieves excellent corrosion resistance. It is believed that Zr also forms Zr-O-M bonds (M: metal element in the plating layer) with the surface of the plating layer 20. Therefore, Zr also improves the adhesion of the chemical conversion coating 30 to the plating layer 20.
[0069] Preferably, the Zr mass [Zr] in the chemical conversion coating 30 is 4.0 to 510.0 mg / m 2 Unit area (1 m 2 ) Zr mass [Zr] per 4.0 mg / m 2 If the Zr mass [Zr] is 510.0 mg / m or more, adhesion is further improved due to bonding between the Zr in the chemical conversion coating 30 and the surface of the plating layer 20. Furthermore, the cross-linked structure formed by the Zr and the acrylic resin in the chemical conversion coating 30 further improves the barrier properties of the chemical conversion coating 30 and further improves corrosion resistance. 2 If the thickness is less than this, the occurrence of cracks in the chemical conversion coating 30 can be suppressed, and the corrosion resistance can be further improved.
[0070] A more preferable lower limit of the Zr mass [Zr] is 50.0 mg / m 2 and more preferably 100.0 mg / m 2 and more preferably 120.0 mg / m 2 A more preferable upper limit of the Zr mass [Zr] is 500.0 mg / m 2 and more preferably 400.0 mg / m 2and more preferably 350.0 mg / m 2 A preferred range of the Zr mass [Zr] is, for example, 50.0 to 500.0 mg / m 2 and more preferably 100.0 to 400.0 mg / m 2 and more preferably 120.0 to 350.0 mg / m 2 is.
[0071] [V in the chemical conversion coating 30] The V in the chemical conversion coating 30 is preferentially eluted into the plating layer 20 in a corrosive environment. This suppresses an increase in pH due to dissolution of the plating layer 20. As a result, the corrosion resistance of the surface-treated steel sheet 1 is improved.
[0072] Preferably, the V mass [V] in the chemical conversion coating 30 is 5.0 to 110.0 mg / m 2 Unit area (1 m 2 ) V mass [V] per 5.0 mg / m 2 If the V mass [V] is 110.0 mg / m or more, the corrosion resistance of the surface-treated steel sheet 1 is further improved. 2 If it is less than this, the resistance to condensation discoloration of the surface-treated steel sheet 1 is further improved.
[0073] The preferred lower limit of the V mass [V] is 7.0 mg / m 2 and more preferably 10.0 mg / m 2 and more preferably 30.0 mg / m 2 and more preferably 50.0 mg / m 2 The preferred upper limit of the V mass [V] is 100.0 mg / m 2 and more preferably 90.0 mg / m 2 and more preferably 80.0 mg / m 2 The preferred range of the V mass [V] is, for example, 7.0 to 100.0 mg / m 2 and more preferably 10.0 to 90.0 mg / m 2 and more preferably 30.0 to 80.0 mg / m 2 and more preferably 50.0 to 80.0 mg / m 2 is.
[0074] [Regarding P in the chemical conversion coating 30] The P in the chemical conversion coating 30 forms a passivation coating such as zinc phosphate on the surface of the plating layer 20. This passivation coating enhances the corrosion resistance of the surface-treated steel sheet 1. The passivation coating is formed by a reaction between P and metal ions produced by dissolving a portion of the plating layer 20. The passivation coating is formed by applying an aqueous surface treatment agent containing P, which is a raw material for the chemical conversion coating 30, to the surface of the plating layer 20, and / or by dissolving a portion of the plating layer 20 in a corrosive environment after the formation of the chemical conversion coating 30.
[0075] Preferably, the P mass [P] in the chemical conversion coating 30 is 20.0 to 200.0 mg / m 2 Unit area (1 m 2 ) P mass [P] per 20.0 mg / m 2 If the P mass [P] is 200.0 mg / m or more, the corrosion resistance of the surface-treated steel sheet 1 is further improved. 2 If it is less than this, the blackening resistance of the surface-treated steel sheet 1 is further improved.
[0076] The preferred lower limit of the P mass [P] is 20.0 mg / m 2 and more preferably 30.0 mg / m 2 and more preferably 40.0 mg / m 2 and more preferably 50.0 mg / m 2 The preferred upper limit of the P mass [P] is 190.0 mg / m 2 and more preferably 180.0 mg / m 2 and more preferably 150.0 mg / m 2 and more preferably 100.0 mg / m 2 The preferred range of the P mass [P] is, for example, 20.0 to 190.0 mg / m 2 and more preferably 30.0 to 180.0 mg / m 2 and more preferably 40.0 to 150.0 mg / m 2 and more preferably 50.0 to 100.0 mg / m 2 is.
[0077] [Regarding Co in the chemical conversion coating 30] Co in the chemical conversion coating 30 improves the blackening resistance and corrosion resistance of the surface-treated steel sheet 1. Al and Mg in the plating layer 20 exhibit sacrificial corrosion protection in a corrosive environment. In this case, Zn in the plating layer 20 oxidizes in an oxygen-deficient state and turns black. This phenomenon is called blackening. Blackening is likely to occur in parts of the plating layer 20 that are easily dissolved. Co in the chemical conversion coating 30 slows the oxidation rate (corrosion rate) of Zn in the plating layer 20. This suppresses blackening and improves the blackening resistance of the surface-treated steel sheet 1.
[0078] Preferably, the Co mass [Co] in the chemical conversion coating 30 is 1.0 to 20.0 mg / m 2 Unit area (1 m 2 ) Co mass [Co] per 2 If the Co mass [Co] is 20.0 mg / m or more, the blackening resistance of the surface-treated steel sheet 1 is further improved. 2 If it is less than this, the corrosion resistance of the surface-treated steel sheet 1 is further improved.
[0079] The preferred lower limit of the Co mass [Co] is 2.0 mg / m 2 and more preferably 3.0 mg / m 2 and more preferably 4.0 mg / m 2 and more preferably 5.0 mg / m 2 The preferred upper limit of the Co mass [Co] is 15.0 mg / m 2 and more preferably 12.0 mg / m 2 and more preferably 10.0 mg / m 2 and more preferably 8.0 mg / m 2 The preferred range of the Co mass [Co] is, for example, 2.0 to 15.0 mg / m 2 and more preferably 3.0 to 12.0 mg / m 2 and more preferably 4.0 to 10.0 mg / m 2 and more preferably 5.0 to 8.0 mg / m 2 is.
[0080] [Method for measuring the mass of Zr, V, P, and Co in the chemical conversion coating 30] The masses of Zr, V, P, and Co in the chemical conversion coating 30 can be measured by the following method. The masses (mg / m) of each element contained in the plating layer 20 and the chemical conversion coating 30 are calculated in accordance with the method described in the above-mentioned [Method for measuring the chemical composition and coating weight of the plating layer 20]. 2 Furthermore, the mass (mg / m) of each element in the plating layer 20 is calculated. 2 ) is required.
[0081] The mass (mg / m) of each element contained in the plating layer 20 and the chemical conversion coating 30 2 ) to calculate the mass (mg / m) of each element in the plating layer 20. 2 ) to obtain the Zr mass [Zr] (mg / m 2 ), V mass [V] (mg / m 2 ), P mass [P] (mg / m 2 ) and Co mass [Co] (mg / m 2 ) is required.
[0082] [Regarding Acrylic Resin] In this embodiment, the "acrylic resin" is a resin containing a polymer of a (meth)acrylic acid ester. Preferably, the acrylic resin is a resin containing a polymer of a (meth)acrylic acid alkyl ester. The acrylic resin may be a polymer obtained by polymerizing only a (meth)acrylic acid alkyl ester, or may be a copolymer obtained by polymerizing a (meth)acrylic acid alkyl ester and another monomer. In this specification, "(meth)acrylic" means "acrylic" or "methacrylic".
[0083] The acrylic resin enhances the adhesiveness between the chemical conversion coating 30 and the adhesive. The acrylic resin also enhances the corrosion resistance of the surface-treated steel sheet 1.
[0084] When the acrylic resin is a copolymer of a (meth)acrylic acid alkyl ester and another monomer, the copolymer is, for example, a copolymer of styrene (b1), (meth)acrylic acid (b2), a (meth)acrylic acid alkyl ester (b3), and acrylonitrile (b4).
[0085] Preferably, the acrylic resin is a copolymer containing 15 to 25 mass% of styrene (b1), 1 to 10 mass% of (meth)acrylic acid (b2), 40 to 58 mass% of a (meth)acrylic acid alkyl ester (b3), and 20 to 38 mass% of acrylonitrile (b4). When the acrylic resin is the copolymer, adhesion to an adhesive is further improved. In addition, the corrosion resistance of the surface-treated steel sheet 1 is further improved.
[0086] Styrene (b1) improves the adhesion of the chemical conversion coating 30 to the adhesive. Styrene (b1) further improves the corrosion resistance of the surface-treated steel sheet 1. When the styrene (b1) content relative to the total mass of the monomer components (i.e., when the acrylic resin is taken as 100% by mass) is 15% by mass or more, the above-mentioned effects obtained by styrene (b1) are further improved. When the styrene (b1) content is 25% by mass or less, excessive hardening of the chemical conversion coating 30 can be suppressed. As a result, the adhesion of the chemical conversion coating 30 to the adhesive is further improved, and the corrosion resistance of the surface-treated steel sheet 1 is further improved. Therefore, the styrene (b1) content is preferably in the range of 15 to 25% by mass. A more preferable lower limit of the styrene (b1) content is 17% by mass. A more preferable upper limit of the styrene (b1) content is 23% by mass. A more preferable range of the styrene (b1) content is, for example, 17 to 23% by mass.
[0087] The (meth)acrylic acid (b2) improves the adhesion between the chemical conversion coating 30 and the plating layer 20 and adhesive, thereby improving the corrosion resistance of the surface-treated steel sheet 1. When the (meth)acrylic acid (b2) content is 1% by mass or more relative to the total mass of the monomer components (i.e., when the acrylic resin is taken as 100% by mass), the effects obtained by the (meth)acrylic acid (b2) are further improved. When the (meth)acrylic acid (b2) content is 10% by mass or less, the water resistance of the chemical conversion coating 30 is improved, and as a result, the corrosion resistance is further improved. Therefore, the preferred range of the (meth)acrylic acid (b2) content is 1 to 10% by mass. A more preferred lower limit of the (meth)acrylic acid (b2) content is 2% by mass. A more preferred upper limit of the (meth)acrylic acid (b2) content is 6% by mass. A more preferred range of the (meth)acrylic acid (b2) content is, for example, 2 to 6% by mass.
[0088] The (meth)acrylic acid alkyl ester (b3) enhances the corrosion resistance of the surface-treated steel sheet 1. When the (meth)acrylic acid alkyl ester (b3) is 40 mass% or more relative to the total mass of the monomer components (i.e., when the acrylic resin is taken as 100 mass%), corrosion resistance is further improved. Furthermore, when the content of the (meth)acrylic acid alkyl ester (b3) is 58 mass% or less, corrosion resistance is further improved. Therefore, the preferred range of the (meth)acrylic acid alkyl ester (b3) is 40 to 58 mass%. A more preferred lower limit of the (meth)acrylic acid alkyl ester (b3) content is 43 mass%. A more preferred upper limit of the (meth)acrylic acid alkyl ester (b3) content is 55 mass%. A more preferred range of the (meth)acrylic acid alkyl ester (b3) content is, for example, 43 to 55 mass%.
[0089] The (meth)acrylic acid alkyl ester (b3) is, for example, one or more selected from the group consisting of methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-methylhexyl acrylate, and isomers thereof. Preferably, the (meth)acrylic acid alkyl ester (b3) is ethyl acrylate and / or butyl acrylate. In this case, corrosion resistance is further improved.
[0090] Acrylonitrile (b4) improves the adhesion between the chemical conversion coating 30 and the adhesive. If the acrylonitrile (b4) content is 20% by mass or more relative to the total mass of the monomer components (i.e., when the acrylic resin is taken as 100% by mass), the adhesion between the chemical conversion coating 30 and the adhesive is further improved. If the acrylonitrile (b4) content is 38% by mass or less, the water resistance and corrosion resistance of the chemical conversion coating 30 are improved. Therefore, the preferred range of acrylonitrile (b4) is 20 to 38% by mass. A more preferred lower limit of the acrylonitrile (b4) content is 22% by mass. A more preferred upper limit of the acrylonitrile (b4) content is 35% by mass. A more preferred range of the acrylonitrile (b4) content is, for example, 22 to 35% by mass.
[0091] When the acrylic resin is a copolymer, it may be a copolymer containing styrene (b1), (meth)acrylic acid (b2), a (meth)acrylic acid alkyl ester (b3), acrylonitrile (b4), and other vinyl group-containing monomers.
[0092] The other vinyl group-containing monomer is not particularly limited. Examples of the other vinyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, ethoxy-diethylene glycol (meth)acrylate, 2-hydroxyethyl (meth)allyl ether, 3-hydroxypropyl (meth)allyl ether, 4-hydroxybutyl (meth)allyl ether, 2-dimethylaminoethyl acrylate, acrylamide, allyl alcohol, and methyl acrylate. The other vinyl group-containing monomer is at least one selected from the group consisting of leic acid, maleic anhydride, fumaric acid, crotonic acid, itaconic acid, citraconic acid, cinnamic acid, vinyltrimethoxysilane, vinyltriethoxysilane, allyl glycidyl ether, glycidyl (meth)acrylate, 2-(1-aziridinyl)ethyl acrylate, iminol methacrylate, acryloylmorpholine, vinyl formate, vinyl acetate, vinyl butyrate, vinyl acrylate, vinyl toluene, cinnamonitrile, (meth)acryloxyethyl phosphate, and bis-(meth)acryloxyethyl phosphate. Preferably, the other vinyl group-containing monomer is at least one selected from the group consisting of 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, ethoxydiethylene glycol acrylate, and acrylamide. In this case, the emulsion stability is enhanced.
[0093] As used herein, "(meth)acrylate" means "acrylate" or "methacrylate." "(meth)allyl ether" means "allyl ether" or "methallyl ether." "(meth)acrylo" means "acrylo" or "methacrylo."
[0094] [Method for measuring the content of each component in the acrylic resin in the chemical conversion coating 30] The content (mass %) of each component, styrene (b1), (meth)acrylic acid (b2), (meth)acrylic acid alkyl ester (b3), and acrylonitrile (b4), in the acrylic resin is measured by an FT-IR reflectance method, specifically, by Fourier transform infrared spectroscopy using a high-sensitivity reflectance method (RAS method), as follows.
[0095] A test piece including the chemical conversion coating 30 (hereinafter referred to as test piece for resin component analysis) is taken from the surface-treated steel sheet 1. The thickness of the test piece for resin component analysis is the same as that of the surface-treated steel sheet 1. Measurement is carried out by Fourier transform infrared spectroscopy on a 40 mm x 40 mm area of the test piece for resin component analysis, with an accumulation number of 16. At this time, the angle of incidence of infrared light on the chemical conversion coating 30 is set to 70 to 75°. From the measurement, the horizontal axis is plotted as wavenumber (cm -1 ), and create a graph of the infrared absorption spectrum with the vertical axis representing transmittance (%).
[0096] In the infrared absorption spectrum graph, the heights of the main peaks of styrene (b1), (meth)acrylic acid (b2), (meth)acrylic acid alkyl ester (b3), and acrylonitrile (b4) are determined.
[0097] Next, calibration curves for styrene (b1), (meth)acrylic acid (b2), (meth)acrylic acid alkyl ester (b3), and acrylonitrile (b4) are prepared. For example, in the case of styrene (b1), multiple chemical conversion coating samples are prepared with different styrene (b1) contents (mass %) in the chemical conversion coating 30. The prepared chemical conversion coating samples are measured using Fourier transform infrared spectroscopy under the same conditions as described above, and the height of the main peak of styrene (b1) is determined. A calibration curve is prepared based on the obtained height of the main peak and the styrene (b1) content in the chemical conversion coating sample. Calibration curves for (meth)acrylic acid (b2), (meth)acrylic acid alkyl ester (b3), and acrylonitrile (b4) are also prepared using the same method as for styrene (b1).
[0098] The contents (% by mass) of styrene (b1), (meth)acrylic acid (b2), (meth)acrylic acid alkyl ester (b3), and acrylonitrile (b4) are determined based on the height of the main peak of each component obtained from the test piece for resin component analysis and the calibration curves of each component.
[0099] Preferably, the glass transition temperature of the acrylic resin is −12 to 24° C. If the glass transition temperature is −12° C. or higher, the corrosion resistance of the chemical conversion coating 30 is further improved. If the glass transition temperature is 24° C. or lower, the adhesion to the adhesive is further improved. The preferred lower limit of the glass transition temperature of the acrylic resin is −10° C. The preferred upper limit of the glass transition temperature of the acrylic resin is 20° C.
[0100] The glass transition temperature of the acrylic resin is calculated by the following formula: 1 / Tg(K)=W 1 / Tg 1 +W 2 / Tg 2 +...+W n / Tg n (1) In the formula, Tg is the glass transition temperature (K) of the acrylic resin (A), and W 1 , W 2 , ..., W n (n is a natural number) is the content (mass%) of the homopolymer of each monomer constituting the acrylic resin, and Tg 1 , Tg 2 , ..., Tg n (n is a natural number) is the glass transition temperature of the homopolymer of each monomer.
[0101] [Preferred Acrylic Resin Content in Chemical Conversion Coating 30] The preferred acrylic resin content in the entire chemical conversion coating 30 is 20.0 to 60.0 mass%. If the acrylic resin content is 20.0 mass% or more, the effects of including the acrylic resin are more effectively achieved. If the acrylic resin content is 60.0 mass% or less, the corrosion resistance is further improved due to the synergistic effect of including Zr and the acrylic resin. A more preferred lower limit of the acrylic resin content is 25.0 mass%, and even more preferably 30.0 mass%. A more preferred upper limit of the acrylic resin content is 55.0 mass%, and even more preferably 50.0 mass%. A more preferred range of the acrylic resin content is, for example, 25.0 to 55.0 mass%, and even more preferably 30.0 to 50.0 mass%.
[0102] [Method for Confirming Acrylic Resin in Chemical Conversion Coating 30 and Measuring the Amount] The presence or absence of acrylic resin contained in the chemical conversion coating 30 and the amount (mass %) of acrylic resin can be confirmed by the following method.
[0103] A test piece including the chemical conversion coating 30, the plating layer 20, and the base steel sheet 10 is taken from the surface-treated steel sheet 1. The thickness of the test piece is the thickness of the surface-treated steel sheet 1.
[0104] The test specimen is subjected to pyrolysis gas chromatography mass spectrometry (GC-MS) analysis. Specifically, the test specimen is heated to 600°C in a GC-MS device. At this time, the resin in the chemical conversion coating 30 is thermally decomposed, generating decomposition products. The decomposition products are analyzed by GC-MS to determine the type and amount of the decomposition products. The presence or absence of acrylic resin in the chemical conversion coating 30 can be confirmed from the type of decomposition products.
[0105] The content (mass %) of acrylic resin in the chemical conversion coating is determined based on the amount of the analyzed decomposition products and the mass of the chemical conversion coating 30. The mass of the chemical conversion coating 30 is the total coating mass (mg / m) of the plating layer 20 and the chemical conversion coating 30 obtained by the method described in [Method for measuring the chemical composition and coating mass of the plating layer 20]. 2 ) and the coating weight (mg / m 2 ) and can be found from
[0106] [Regarding the deposition amount of the chemical conversion coating 30] The deposition amount of the chemical conversion coating 30 is 300 to 1000 mg / m 2 The coating amount of the chemical conversion coating 30 is 300 mg / m 2 If the coating weight of the chemical conversion coating 30 is less than 1000 mg / m, the formed chemical conversion coating 30 will be too thin. In this case, the adhesion and corrosion resistance will also decrease. 2 If the coating weight exceeds 300 to 1000 mg / m, the formed chemical conversion coating 30 will be too thick, resulting in a decrease in adhesion. 2 The thickness of the chemical conversion coating 30 is appropriate, so that sufficient adhesion and corrosion resistance can be obtained. The preferred lower limit of the coating weight of the chemical conversion coating 30 is 350 mg / m 2 and more preferably 400 mg / m 2 and more preferably 450 mg / m 2 The preferred upper limit of the coating amount of the chemical conversion coating 30 is 950 mg / m 2 and more preferably 900 mg / m 2 and more preferably 850 mg / m 2 The preferred range of the coating weight of the chemical conversion coating 30 is 350 to 950 mg / m 2 and more preferably 400 to 900 mg / m 2 and more preferably 450 to 850 mg / m 2 is.
[0107] [Method for measuring the coating weight of the chemical conversion coating 30] The coating weight of the chemical conversion coating 30 can be determined by the following method. The total coating weight (mg / m) of the plating layer 20 and the chemical conversion coating 30 is determined in accordance with the method described in the above [Method for measuring the chemical composition and coating weight of the plating layer 20]. 2 Furthermore, the coating weight (mg / m 2 ) is required.
[0108] The total coating weight (mg / m) of the plating layer 20 and the chemical conversion coating 30 2 ) to the coating amount (mg / m 2 ) to obtain the coating amount (mg / m 2 ) is required.
[0109] [Regarding formula (1)] In the surface-treated steel sheet 1 of this embodiment, the V mass [V] mg / m in the chemical conversion coating 30 2 and the P mass [P] mg / m in the chemical conversion coating 30 2 and satisfy the formula (1). 0.60≦[V] / [P]≦2.80 (1)
[0110] F1 is defined as follows: F1 = [V] / [P]. If F1 is less than 0.60, the P mass [P] is excessively high relative to the V mass [V] in the chemical conversion coating 30. In this case, the blackening resistance of the surface-treated steel sheet 1 is reduced. If the P mass [P] is too high relative to the V mass [V], it is believed that the oxidation reaction of the plating, which causes blackening, is accelerated. On the other hand, if F1 exceeds 2.80, sufficient corrosion resistance cannot be obtained. This is because if the P mass [P] is too low relative to the V mass [V], the corrosion-inhibiting effect of the passivation coating formed by P is reduced. If F1 is 0.60 to 2.80, excellent blackening resistance and excellent corrosion resistance can be obtained. The preferred lower limit of F1 is 0.65, more preferably 0.70, and even more preferably 0.80. The preferred upper limit of F1 is 2.40, more preferably 2.00, and even more preferably 1.80. A preferred range for F1 is, for example, 0.65 to 2.40, more preferably 0.70 to 2.00, and even more preferably 0.80 to 1.80.
[0111] The V mass [V] (mg / m 2 ), and P mass [P] (mg / m 2 ) can be determined by the method described above in [Method for measuring the Zr mass, V mass, P mass, and Co mass in the chemical conversion coating 30].
[0112] [Regarding formula (2)] In the surface-treated steel sheet 1 of this embodiment, when the Mg content in the chemical composition of the plating layer 20 is defined as [Mg]b (mass%), the Mg content [Mg]b (mass%) and the V mass [V] (mg / m 2 ) satisfy the formula (2). 0<[V] / [Mg]b≦20.00 (2)
[0113] F2 is defined as follows: F2 = [V] / [Mg]b When the Mg content in the chemical composition of the plating layer 20 exceeds 3.0 mass%, if the V mass [V] in the chemical conversion coating 30 relative to the Mg content [Mg]b in the plating layer 20 is high, condensation discoloration will occur. Specifically, if F2 exceeds 20.00, the V mass in the chemical conversion coating 30 relative to the Mg mass in the plating layer 20 will be excessively high. In this case, sufficient resistance to condensation discoloration cannot be obtained. If F2 is greater than 0 to 20.00, the surface-treated steel sheet 1 will have excellent resistance to condensation discoloration. The preferred lower limit of F2 is 5.00, more preferably 6.00, and even more preferably 7.00. The preferred upper limit of F2 is 19.00, more preferably 18.00, and even more preferably 17.00. A preferred range for F2 is, for example, 5.00 to 19.00, more preferably 6.00 to 18.00, and even more preferably 7.00 to 17.00.
[0114] [Effects of Surface-Treated Steel Sheet 1] In the surface-treated steel sheet 1 of this embodiment, the plating layer 20 and the chemical conversion coating 30 have the above-described chemical compositions, and the coating weight of the chemical conversion coating 30 is 300 to 1000 mg / m 2 and further satisfies formula (1) and formula (2). Therefore, the surface-treated steel sheet 1 of this embodiment has sufficient corrosion resistance, sufficient adhesion to an adhesive, sufficient resistance to blackening, and further has sufficient resistance to condensation discoloration.
[0115] [Regarding a preferred embodiment of the surface-treated steel sheet 1] In the surface-treated steel sheet 1 of this embodiment, the difference between the Mg concentration [Mg]s mass% in the surface layer of the plating layer 20 obtained by elemental analysis of the plating layer 20 in the depth direction using glow discharge optical emission spectrometry and the Mg content [Mg]b mass% in the chemical composition of the plating layer 20 is defined as the Mg concentration difference Δ[Mg] (mass%).
[0116] Preferably, in the surface-treated steel sheet 1 of this embodiment, the Mg concentration difference Δ[Mg] (mass%) and the V mass [V] (mg / m 2 ) satisfies the formula (3). Δ[Mg]×[V]≦200 (3)
[0117] F3 is defined as follows: F3 = Δ[Mg] × [V] The Mg concentration difference Δ[Mg] in the plating layer 20 and the V mass [V] in the chemical conversion coating 30 have a synergistic effect on resistance to condensation discoloration. If the Mg concentration difference Δ[Mg] is low and the V mass [V] is small, the concentrated Mg in the surface layer of the plating layer 20 and the V concentration in the chemical conversion coating 30 act synergistically to further improve resistance to condensation discoloration. Therefore, F3 is an index of resistance to condensation discoloration.
[0118] If F3 is 200 or less, it is possible to sufficiently suppress the interaction between concentrated Mg in the surface layer of the plating layer 20 and V in the chemical conversion coating 30. As a result, resistance to condensation discoloration is significantly improved.
[0119] A more preferred upper limit of F3 is 180, more preferably 160, even more preferably 150, even more preferably 140, even more preferably 130, and even more preferably 120. The lower limit of F3 is not particularly limited. A preferred lower limit of F3 is, for example, 5, more preferably 10, even more preferably 20, even more preferably 25, and even more preferably 30. A more preferred range of F3 is, for example, 5 to 180, more preferably 10 to 160, even more preferably 20 to 150, even more preferably 25 to 140, even more preferably 30 to 130, and even more preferably 30 to 120.
[0120] [Method for Measuring Mg Concentration Difference Δ[Mg]] The Mg concentration difference Δ[Mg] in the surface layer of the plating layer 20 can be determined by the following method. A test specimen is taken from the surface-treated steel sheet 1. The test specimen includes the base steel sheet 10, the plating layer 20, and the chemical conversion coating 30. The thickness of the test specimen is the thickness of the surface-treated steel sheet. Glow discharge optical emission spectroscopy is performed from the surface of the chemical conversion coating 30 of the test specimen in the thickness direction of the base steel sheet 10 to measure the glow discharge optical emission spectra (GDS spectra) of Mg and C. Specifically, using a high-frequency glow discharge optical emission spectroscopy device (GD-OES, product name: GDA750 manufactured by Rigaku Corporation) in an argon atmosphere (Ar pressure: 3 hPa), the test specimen is used as the cathode and a power output of 30 W is applied to measure the GDS spectrum of Mg and the GDS spectrum of C. The measurement area is 4 mmφ, the measurement time is 100 seconds, and the measurement interval is 0.025 seconds.
[0121] Referring to Figure 1, the position P0 where the obtained GDS spectrum of Mg and the GDS spectrum of C intersect is defined as the surface of the plating layer 20 (i.e., the interface between the chemical conversion coating 30 and the plating layer 20). The region SF within 10 seconds of measurement from the surface of the plating layer 20 is defined as the surface region SF of the plating layer 20. The maximum Mg concentration in the surface region SF of the plating layer 20 is defined as the Mg concentration [Mg]s (mass%). Furthermore, the Mg content in the chemical composition of the plating layer 20 obtained by the "Method for Measuring the Chemical Composition and Coating Weight of the Plating Layer 20" is defined as [Mg]b (mass%).
[0122] Using the obtained Mg concentration [Mg]s and Mg content [Mg]b, the Mg concentration difference Δ[Mg] (mass%) is calculated using the following formula: Δ[Mg]=[Mg]s-[Mg]b
[0123] [Regarding the adhesive to be applied to the surface-treated steel sheet 1] Examples of adhesives that provide good adhesion to the chemical conversion coating 30 of the surface-treated steel sheet 1 include silicone-based (including acrylic-modified and epoxy-modified), epoxy-based, acrylic resin-based, phenol-based, urethane-based, vinyl acetate-based, cyanoacrylate-based, and styrene-butadiene rubber-based adhesives. Note that there are no particular limitations on the material that can be bonded to the chemical conversion coating 30 of the surface-treated steel sheet 1 via the adhesive. Examples of the above-mentioned materials include steel sheet, mortar, float glass, ceramic tile, porcelain tile, and MDF (medium-density fiberboard).
[0124] [Method for manufacturing the surface-treated steel sheet 1] An example of a method for manufacturing the surface-treated steel sheet of this embodiment will be described. The surface-treated steel sheet having the above-described configuration may be manufactured by a manufacturing method other than the manufacturing method described below. However, the manufacturing method described below is a preferred example of the method for manufacturing the surface-treated steel sheet according to this embodiment.
[0125] An example of the method for manufacturing a surface-treated steel sheet according to this embodiment includes the following steps: (Step 1) Base steel sheet preparation step (Step 2) Plating layer formation step (Step 3) Skin-pass rolling step (Step 4) Chemical conversion coating formation step Steps 1 to 4 will be described below.
[0126] [(Step 1) Base Steel Plate Preparation Step] In the base steel plate preparation step, the above-described base steel plate 10 is prepared. The base steel plate 10 may be supplied from a third party.
[0127] [(Step 2) Coating Layer Forming Step] In the coating layer forming step, a coating process (hot-dip coating process) is performed on the base steel sheet 10 to form a coating layer 20 on the surface of the base steel sheet 10. Specifically, a coating bath is prepared. The composition of the coating bath is adjusted depending on the composition of the coating layer 20 to be formed. After the base steel sheet 10 is immersed in the coating bath for a certain period of time, the base steel sheet 10 is pulled up from the coating bath by a well-known method. For example, a sink roll is placed in the coating bath. The direction of travel of the base steel sheet 10 immersed in the coating bath is changed upward by the sink roll.
[0128] The base steel sheet 10 has a coating adhered to its surface after being pulled out of the coating bath. A known gas wiping device is used to adjust the amount of coating adhered to the base steel sheet 10. The coating adhered to the base steel sheet 10 after being pulled out of the coating bath is cooled. The coating is solidified by cooling to form a coating layer 20.
[0129] [Preferable Cooling Conditions in the Coating Layer Forming Step] The coating layer forming step preferably satisfies the following manufacturing condition 1. (Preferable Manufacturing Condition 1) When the surface temperature of the coated base steel sheet 10 is pulled up from the coating bath, the average cooling rate CR1 is set to 16 to 46°C / sec from 450°C to 340°C, and the average cooling rate CR2 is set to 21 to 51°C / sec from 340°C to 250°C.
[0130] When the average cooling rate CR1 is 16°C / sec or more and the average cooling rate CR2 is 21°C / sec or more, the structure of the coating layer 20 after solidification becomes fine. Therefore, Mg concentration in the surface layer of the coating layer 20 is sufficiently suppressed, and the Mg concentration difference Δ[Mg] becomes sufficiently low. As a result, F3 satisfies formula (3).
[0131] The upper limits of the average cooling rate CR1 and the average cooling rate CR2 are not particularly limited. The upper limit of the average cooling rate CR1 is preferably 46°C / sec. The upper limit of the average cooling rate CR2 is preferably 51°C / sec.
[0132] [(Step 3) Skin-pass Rolling Step] In the skin-pass rolling step, the steel sheet after the coating layer forming step is subjected to skin-pass rolling. In the skin-pass rolling, the steel sheet on which the coating layer 20 has been formed is cold-rolled using a rolling stand having a pair of skin-pass rolls.
[0133] [Preferred Manufacturing Conditions in the Skin-Pass Rolling Step] In the skin-pass rolling step, the following manufacturing conditions 2 and 3 are preferably satisfied. (Preferred Manufacturing Condition 2) The arithmetic mean roughness Ra of the surface of the skin-pass roll in the roll axial direction is 1.0 to 5.0 μm, and the rolling force P(t) in skin-pass rolling is 100 to 500 t. (Preferred Manufacturing Condition 3) The average cooling rates CR1 and CR2 (° C. / sec), the arithmetic mean roughness Ra (μm) of the surface of the skin-pass roll, and the rolling force P(t) in skin-pass rolling satisfy formula (A): (CR1+CR2) / {2(Ra×P)}≧0.020 (A) Manufacturing Condition 2 and Manufacturing Condition 3 will be explained below.
[0134] [Regarding Preferred Manufacturing Condition 2] The surface roughness of the skin-pass roll affects the Mg concentration in the surface layer of the plating layer 20. If the arithmetic mean roughness Ra is 5.0 μm or less, the surface roughness of the plating layer 20 is sufficiently suppressed. In this case, excessive Mg concentration in the surface layer of the plating layer 20 is suppressed, and the Mg concentration difference Δ[Mg] becomes sufficiently low. As a result, F3 satisfies formula (3). Therefore, the arithmetic mean roughness Ra of the surface of the skin-pass roll is preferably 5.0 μm or less.
[0135] The arithmetic mean roughness Ra is measured as follows. For each of a pair of skin-pass rolls, the arithmetic mean roughness Ra of the surface in the roll axis direction is measured in accordance with JIS B 0601:2013. A contact roughness meter is used to measure the arithmetic mean roughness Ra. The conditions for calculating the roughness curve are cutoff value λc: 80 mm, cutoff value λs: 80 μm, measurement speed: 0.5 mm / sec, reference length: 1 mm, and evaluation length: 10 mm. The arithmetic mean value of the arithmetic mean roughnesses (total of two) obtained for each skin-pass roll is defined as the arithmetic mean roughness Ra (μm).
[0136] In view of the Mg concentration difference Δ[Mg], the lower limit of the arithmetic mean roughness Ra is not particularly limited. However, if the arithmetic mean roughness Ra is excessively small, the base steel sheet 10 on which the coating layer 20 is formed will be less likely to be caught in the skin-pass roll. Therefore, the lower limit of the arithmetic mean roughness Ra is 1.0 μm.
[0137] The rolling force P during skin-pass rolling affects the Mg concentration in the surface layer of the coating layer 20. If the rolling force P is 100 to 500 t, the Mg concentration in the surface layer of the coating layer 20 is sufficiently suppressed, and the Mg concentration difference Δ[Mg] becomes sufficiently low. As a result, F3 satisfies formula (3). Therefore, the rolling force P is preferably 100 to 500 t.
[0138] [Regarding preferred manufacturing condition 3] FA is defined as follows: FA = (CR1 + CR2) / {2 (Ra × P)} FA is an index related to Mg concentration in the surface layer of the coating layer 20. As described above, the average cooling rates CR1 and CR2, the arithmetic mean roughness Ra, and the rolling force P affect the Mg concentration difference Δ[Mg]. If FA is 0.020 or more, the Mg concentration difference Δ[Mg] in the surface layer of the coating layer 20 of the surface-treated steel sheet 1 after manufacturing will be sufficiently low, provided that manufacturing conditions 1 and 2 are met. As a result, F3 satisfies formula (3).
[0139] [(Step 4) Chemical Conversion Coating Formation Step] In the chemical conversion coating formation step, an aqueous surface treatment agent containing each component contained in the chemical conversion coating 30 is prepared. The prepared aqueous surface treatment agent is applied to the plating layer 20. The applied aqueous surface treatment agent is dried to form the chemical conversion coating 30 on the plating layer 20.
[0140] [About the Water-Based Surface Treatment Chemical] The water-based surface treatment chemical contains Zr, V, P, Co, and an acrylic resin. The water-based surface treatment chemical contains, for example, an acrylic resin (A), a zirconium carbonate compound (B), a vanadium compound (C), a phosphorus compound (D), a cobalt compound (E), and water, and the pH of the water-based surface treatment chemical is 8.0 to 11.0.
[0141] [Regarding Acrylic Resin (A)] The acrylic resin (A) becomes the acrylic resin contained in the chemical conversion coating 30 by applying and drying an aqueous surface treatment agent. The preferred content of the acrylic resin (A) in the aqueous surface treatment agent is 20.0 to 60.0 mass% based on the total solids content of the aqueous surface treatment agent. Here, "based on the total solids content" refers to the mass% when the components other than water in the aqueous surface treatment agent are taken as 100.0 mass%. A more preferred lower limit of the acrylic resin (A) content in the aqueous surface treatment agent is 25.0%. A more preferred upper limit of the acrylic resin (A) content in the aqueous surface treatment agent is 40.0%. A more preferred range of the acrylic resin (A) content in the aqueous surface treatment agent is 25.0 to 40.0%.
[0142] The polymerization method for the acrylic resin (A) contained in the aqueous surface treatment agent is not particularly limited. For example, the acrylic resin (A) can be polymerized using suspension polymerization, emulsion polymerization, and solution polymerization. A solvent and / or a polymerization initiator may be used when polymerizing the acrylic resin (A). The polymerization initiator is not particularly limited. Examples of the polymerization initiator include radical polymerization initiators such as azo compounds and peroxide compounds. The polymerization initiator is preferably used in an amount of 0.1 to 10% by mass relative to the total solid content of the acrylic resin. The reaction temperature and reaction time may be well-known conditions. The reaction temperature is, for example, room temperature to 200°C, and the reaction time is 30 minutes to 8 hours.
[0143] [Zirconium Carbonate Compound (B)] The zirconium carbonate compound (B) in the aqueous surface treatment agent undergoes a crosslinking reaction with the acrylic resin (A) when the aqueous surface treatment agent is applied and dried. As a result, a chemical conversion coating 30 having a crosslinked structure between Zr and the acrylic resin (A) is formed. Furthermore, carbonate ions in the zirconium carbonate compound (B) volatilize when the aqueous surface treatment agent is applied and dried. Furthermore, the remaining Zr bonds with each other via oxygen, resulting in a high molecular weight. As a result, the -Zr-OH groups form Zr-O-M bonds (M: metal element in the plating layer) with the surface of the plating layer 20.
[0144] The type of zirconium carbonate compound (B) is not particularly limited. The zirconium carbonate compound (B) is, for example, one or more compounds selected from the group consisting of zirconium carbonate, ammonium zirconium carbonate, potassium zirconium carbonate, and sodium zirconium carbonate. Preferably, the zirconium carbonate compound (B) is zirconium carbonate and / or ammonium zirconium carbonate. In this case, corrosion resistance is further improved.
[0145] [Vanadium Compound (C)] The vanadium compound (C) contained in the aqueous surface treatment agent is, for example, vanadium pentoxide (V 2 O 5 ), metavanadic acid (HVO 3 ), ammonium metavanadate, sodium metavanadate, vanadium oxytrichloride (VOCl 3 ), which are pentavalent vanadium compounds such as vanadium trioxide (V), which are reduced to divalent, trivalent or tetravalent vanadium compounds with a reducing agent, 2 O 3 ), vanadium dioxide (VO 2 ), vanadium oxysulfate (VOSO 4 ), vanadium oxyoxalate [VO(COO) 2 ], vanadium oxyacetylacetonate [VO(OC(CH 3 ) = CHCOCH 3 ) 2 ], vanadium acetylacetonate [V(OC(CH 3 ) = CHCOCH 3 ) 3 ], vanadium trichloride (VCl 3 ), phosphovanadomolybdic acid {H 15-X [PV 12-x Mo x O 40 ]・nH 2 O (6<x<12, n<30)}, vanadium sulfate (VSO 4 ・8H 2 O), vanadium dichloride (VCl 2 ), and vanadium compounds having an oxidation number of 4 to 2, such as vanadium oxide (VO).
[0146] [Phosphorus Compound (D)] The phosphorus compound (D) contained in the aqueous surface treatment agent is, for example, an inorganic acid anion having a phosphorus-containing acid group and / or an organic acid anion having a phosphorus-containing acid group.
[0147] The inorganic acid anion having a phosphorus-containing acid group is, for example, one or more selected from the group consisting of inorganic acid anions in which at least one hydrogen atom of an inorganic acid such as orthophosphoric acid, metaphosphoric acid, condensed phosphoric acid, pyrophosphoric acid, tripolyphosphoric acid, tetraphosphoric acid, hexametaphosphoric acid, etc. is liberated, and salts thereof.
[0148] Examples of organic acid anions having a phosphorus-containing acid group include 1-hydroxymethane-1,1-diphosphonic acid, 1-hydroxyethane-1,1-diphosphonic acid, 1-hydroxypropane-1,1-diphosphonic acid, 1-hydroxyethylene-1,1-diphosphonic acid, 2-hydroxyphosphonoacetic acid, aminotri(methylenephosphonic acid), ethylenediamine-N,N,N',N'-tetra(methylenephosphonic acid), hexamethylenediamine-N,N,N',N'-tetra(methylenephosphonic acid), diethylenetriamine-N,N,N',N'',N''-penta(methylenephosphonic acid), 2-phosphonic acid butane-1,2,4-tricarboxylic acid, inositol hexaphosphonic acid, phytic acid, and other organic phosphonic acids; and organic phosphoric acids; and salts thereof.
[0149] [Cobalt Compound (E)] The cobalt compound (E) contained in the aqueous surface treatment agent is, for example, one or more compounds selected from the group consisting of cobalt sulfate, cobalt nitrate, and cobalt carbonate.
[0150] [Lubricant] The water-based surface treatment agent may contain a lubricant. That is, the lubricant is an optional component. When contained, the lubricant enhances the scratch resistance of the surface-treated steel sheet 1. The lubricant is, for example, one or more selected from the group consisting of polyethylene wax, oxidized polyethylene wax, and oxidized polypropylene wax.
[0151] [Regarding the pH of the aqueous surface treatment agent] Preferably, the pH of the aqueous surface treatment agent is 8.0 to 11.0. If the pH of the aqueous surface treatment agent is 8.0 or higher, the zirconium carbonate compound (B) dissolves stably in the aqueous surface treatment agent. On the other hand, if the pH of the aqueous surface treatment agent is 11.0 or lower, excessive dissolution of the plating layer 20 can be prevented when the aqueous surface treatment agent is applied to the plating layer 20. Furthermore, if the pH is within the above range, the aqueous surface treatment agent is stable. A more preferable lower limit of the pH of the aqueous surface treatment agent is 8.5. A more preferable upper limit of the pH of the aqueous surface treatment agent is 10.0. A more preferable range of the pH of the aqueous surface treatment agent is 8.0 to 11.0. The pH of the aqueous surface treatment agent can be measured, for example, using a Toa DKK Corporation (HM-30R) at a measurement temperature of 25°C.
[0152] The pH adjuster used to adjust the pH of the aqueous surface treatment agent is not particularly limited, and may be, for example, one or more selected from the group consisting of ammonia, guanidine carbonate, carbonic acid, acetic acid, and hydrofluoric acid.
[0153] The aqueous surface treatment agent can be obtained by mixing the above-mentioned components with water such as deionized water or distilled water.
[0154] If necessary, the aqueous surface treatment agent may contain alcohols, ketones, cellosolve-based water-soluble solvents, surfactants, antifoaming agents, leveling agents, antibacterial and antifungal agents, thickeners, conductive substances for improving weldability, coloring pigments and matting materials for improving design, etc. The amount of these components added is preferably less than 5% by mass based on the total solid content of the aqueous surface treatment agent.
[0155] The above-mentioned water-based surface treatment agent is applied to the surface of the plating layer 20 by a well-known method to form a coating film. For example, the water-based surface treatment agent is applied using a roll coater. In this case, the thickness of the coating film can be adjusted by adjusting the peripheral speed ratio of the roll coater. The deposition amount of the chemical conversion coating 30 is 300 to 1000 mg / m 2 After the coating film is formed on the surface of the plating layer 20, the coating film is dried.
[0156] Through the above steps, the surface-treated steel sheet 1 of this embodiment is manufactured.
[0157] The effects of the surface-treated steel sheet of this embodiment will be described more specifically with reference to examples. The conditions in the following examples are one example of conditions adopted to confirm the feasibility and effects of the surface-treated steel sheet of this embodiment. Therefore, the surface-treated steel sheet of this embodiment is not limited to this one example of conditions.
[0158] A base steel sheet having a plating layer formed thereon and having the chemical composition shown in Table 1 (Table 1-1 and Table 1-2) was prepared.
[0159]
[0160]
[0161] The plating layer was formed by hot-dip plating. The coating weight of the plating layer was 40 to 300 mg / m 2 was within the range.
[0162] In the hot dip coating process, the average cooling rate CR1 (°C / sec) when the surface temperature of the steel sheet pulled up from the coating bath was 450 to 340°C and the average cooling rate CR2 (°C / sec) when the surface temperature was 340 to 250°C were as shown in Table 2.
[0163]
[0164] The steel sheet on which the coating layer was formed was subjected to skin-pass rolling. The arithmetic mean roughness Ra (μm) and rolling force P (t) of the skin-pass roll used in the skin-pass rolling were as shown in Table 2. Furthermore, the FA value (= (CR1 + CR2) / {2 (Ra × P)}) was as shown in Table 2.
[0165] An aqueous surface treatment agent having the blending ratio shown in Table 3 was prepared by the following method. Each component shown in Table 3 was added to a certain amount of deionized water while stirring using a propeller stirrer, to prepare a solids concentration of 15% by mass. The pH of the aqueous surface treatment agent was adjusted to 8.0 to 11.0. Carbonate and / or ammonia were used as pH adjusters for the aqueous surface treatment agent.
[0166]
[0167] The types of each component shown in Table 3 were prepared as follows:
[0168] [Acrylic Resin] Styrene (b1), (meth)acrylic acid (b2), (meth)acrylic acid alkyl ester (b3), and acrylonitrile (b4), whose abbreviations are shown in Table 4, were used in the ratios shown in Table 5 to obtain copolymers (acrylic resins) A1 to A17 shown in Table 5. The content of the acrylic resin in the aqueous surface treatment agent in Table 3 is expressed by mass (% by mass) relative to the total solid content of the aqueous surface treatment agent.
[0169]
[0170]
[0171] The following compounds were prepared as Zr compounds, V compounds, P compounds, and Co compounds. [Zr compounds] The following three compounds were prepared as Zr compounds. B1: Potassium zirconium carbonate B2: Ammonium zirconium carbonate B3: Ammonium zirconium fluoride [V compounds] C1: Vanadium acetylacetonate C2: Vanadium oxyoxalate [P compounds] D1: Phosphoric acid D2: 1-hydroxyethane-1,1-diphosphonic acid [Co compounds] E1: Cobalt carbonate E2: Cobalt nitrate
[0172] Steel sheets having plating layers of the respective test numbers shown in Table 1 (Table 1-1 and Table 1-2) formed on both sides were degreased using a degreaser (alkaline degreaser manufactured by Nihon Parkerizing Co., Ltd., trade name: Fine Cleaner E6406) (20 g / L make-up bath, 60°C), and then rinsed with water for 10 seconds using a spray (spray pressure 50 kPa).
[0173] The aqueous surface treatment chemicals shown in Table 3 were applied to both surfaces of degreased steel sheets having plating layers on both sides. Specifically, the aqueous surface treatment chemicals were applied using a roll coater. At this time, the peripheral speed ratio of the roll coater was adjusted to control the film thickness of the coating. The steel sheets with the coating film formed on the plating layer were heated using a warm air circulation oven (heating furnace) while supplying hot air onto the coating film, and the coating film formed on the plating layer was dried.
[0174] The surface-treated steel sheets of each test number were manufactured by the above steps. The thickness of each surface-treated steel sheet of each test number was 2.3 mm.
[0175] [Evaluation Tests] The following evaluation tests were carried out on the surface-treated steel sheets with each test number: (Test 1) Chemical composition analysis test of the plating layer (Test 2) Measurement test of the deposition weight of the chemical conversion coating (Test 3) Measurement test of [V] and [P] (Test 4) Measurement test of the Mg concentration difference Δ[Mg] (Test 5) Evaluation test of corrosion resistance (Test 6) Evaluation test of adhesion (Test 7) Evaluation test of blackening resistance (Test 8) Evaluation test of resistance to discoloration due to condensation Tests 1 to 8 are explained below.
[0176] [(Test 1) Chemical Composition Analysis Test of Plating Layer] Based on the method described in the above-mentioned [Method for Measuring Chemical Composition and Coating Weight of Plating Layer 20], the content (mass %) of each element in the chemical composition of the plating layer of each test number was determined. As a result, the chemical composition of the plating layer of each test number was as shown in Table 1 (Table 1-1 and Table 1-2).
[0177] [(Test 2) Test for Measuring the Adhesion Weight of Chemical Conversion Coating] The adhesion weight of the chemical conversion coating for each test number was measured based on the method described in the above-mentioned [Method for Measuring the Adhesion Weight of Chemical Conversion Coating 30]. The results obtained are shown in Table 6 under the heading "Adhesion weight of chemical conversion coating (mg / m)." 2 ) column.
[0178]
[0179] (Test 3) [V] and [P] Measurement Test Based on the method described in the above [Method for measuring the Zr mass, V mass, P mass, and Co mass in the chemical conversion coating 30], the V mass [V] (mg / m 2 ) and P mass [P] (mg / m 2 ) was calculated. Using the obtained V mass [V] and P mass [P], F1 (= [V] / [P]) was calculated. Furthermore, using the Mg content [Mg]b in the chemical composition of the plating layer and the V mass [V], F2 (= [V] / [Mg]b) was calculated. The obtained V mass [V] (mg / m 2 ), P mass [P] (mg / m 2 ), F1 value, and F2 value are shown in Table 6.
[0180] The components of the chemical conversion coating were measured according to the "Method for Measuring the Zr Mass, V Mass, P Mass, and Co Mass in Chemical Conversion Coating 30" and the "Method for Identifying and Measuring the Acrylic Resin Content in Chemical Conversion Coating 30." The results showed that the chemical conversion coating contained Zr, V, P, and Co, as well as acrylic resin, for all test numbers. Furthermore, the Zr content (mass%), V content (mass%), P content (mass%), Co content (mass%), and acrylic resin content (mass%) in the chemical conversion coating were as shown in Table 3. Furthermore, the content of each component in the acrylic resin in the chemical conversion coating 30 was determined according to the method described in the "Method for Measuring the Content of Each Component in the Acrylic Resin in Chemical Conversion Coating 30." As a result, the content of each component in the acrylic resin was as shown in Table 5.
[0181] [(Test 4) Mg concentration difference Δ[Mg] measurement test] The Mg concentration difference Δ[Mg] (mass %) was determined based on the method described in the above [Method for measuring Mg concentration difference Δ[Mg]]. Furthermore, the obtained Mg concentration difference Δ[Mg] (mass %) and the V mass [V] (mg / m) in the chemical conversion coating were compared. 2 ) and F3 (= Δ[Mg] × [V]) was calculated based on the above. The obtained Mg concentration difference Δ[Mg] (mass%) is shown in the "Δ[Mg] (mass%)" column in Table 6. Furthermore, the obtained F3 value is shown in the "F3" column in Table 6.
[0182] [(Test 5) Corrosion Resistance Evaluation Test] Flat test specimens were collected from the surface-treated steel sheets of each test number. The size of the flat test specimens was 50 mm × 100 mm × plate thickness. The flat test specimens were subjected to a salt spray test in accordance with JIS Z 2371:2015 for 240 hours. After the test, the surfaces of the flat test specimens were observed to determine the area ratio of white rust. Based on the obtained area ratio of white rust, the specimens were evaluated as follows: E (Excellent): Area ratio of white rust was 5.0% or less B (Bad): Area ratio of white rust was more than 5.0% The results obtained are shown in the "Corrosion Resistance" column in Table 6.
[0183] (Test 6) Adhesion Evaluation Test Two test pieces were taken from the surface-treated steel sheet for each test number, each having a width of 25 mm, a thickness of the sheet, and a length of 100 mm.
[0184] As shown in Figure 3, two test pieces 100 were arranged so that their ends overlapped, and an adhesive 120 was applied to the overlapping portion of the two test pieces 100. The area of the bonded portion was 25 mm wide x 12.5 mm long. The acrylic adhesive Hardlock (manufactured by Denka Co., Ltd., product name: c355-20) was used as the adhesive. After applying the adhesive and bonding the two test pieces 100 as shown in Figure 3, a cover plate 150 was placed on the end of each test piece 100 to prepare a lap shear test piece 200.
[0185] A tensile shear test was carried out using the prepared lap shear test specimen. At this time, the distance between chucks was set to 112.5 mm, and the tensile speed was set to 2 mm / min. The tensile shear load (N) was determined by the tensile shear test under the above conditions. Based on the obtained tensile shear load, the specimen was evaluated as follows: E: Tensile shear load was 5.2 × 10 3 N or more B: Tensile shear load is 5.2 x 10 3 Less than N The results obtained are shown in the "Adhesion" column in Table 6.
[0186] [(Test 7) Evaluation Test for Blackening Resistance] Test pieces measuring 50 mm × 100 mm × thickness were taken from the surface-treated steel sheets of each test number, and were left to stand for 144 hours in an atmosphere of 70°C and 85% relative humidity (RH) using a constant temperature and humidity tester.
[0187] The surface of the test piece before the test and the surface of the test piece after the test were measured. * Value, a * value, and b * Specifically, the surface of the test piece before the test and the surface of the test piece after the test were measured using the CIE standard illuminant D65 as the light source, with a viewing angle of 10°, and the CIELAB display color was measured using the SCE method. * Value, a * value, and b * The definition of the SCE method is specified in JIS Z 8722:2009. * Value, a * value, and b * Based on the value, the color difference ΔE is calculated by the following formula: * ΔE was calculated. * = {(ΔL * )2 + (Δa * ) 2 + (Δb * ) 2} 1/2 ΔL * = L after the test * -L before the exam * Δa * = a after the test * - a before the exam * Δb * = b after the test * - Before the exam * In addition, L before and after the test * Value, a * value, and b * The values were measured using a colorimeter manufactured by Konica Minolta, Inc. (product name: CM-2600d). * Based on the above, the blackening resistance was evaluated as follows: E: ΔE * ≦3.0 B:ΔE * >3.0 The results are shown in the "Blackening Resistance" column in Table 6.
[0188] [(Test 8) Evaluation Test of Condensation Discoloration Resistance] Test pieces measuring 50 mm x 100 mm x thickness were taken from the surface-treated steel sheets of each test number. Six drops of pure water were dropped onto the surface of the test piece. Each drop was dropped on a different area. After the drops were dropped, the test piece was left in the air at room temperature for 12 hours to allow the water droplets to dry. After 12 hours, the surface of the test piece was observed to determine how many of the 12 drop areas were discolored. The condensation discoloration resistance was evaluated according to the number of discolored areas as follows: E: Two or fewer discolored areas; G: Three to five discolored areas; B: Six or more discolored areas. The results are shown in the "Condensation Discoloration Resistance" column in Table 6.
[0189] [Evaluation Results] Referring to Table 6, the surface-treated steel sheets of test numbers 1 to 44 had appropriate chemical compositions for the plating layers, and the chemical conversion coatings contained Zr, V, P, and Co, as well as an acrylic resin. Furthermore, the coating weights of the chemical conversion coatings were appropriate, and F1 and F2 were also appropriate. Therefore, excellent corrosion resistance, excellent adhesion to adhesives, and excellent resistance to blackening were obtained, as well as excellent resistance to condensation discoloration.
[0190] In particular, the surface-treated steel sheets of test numbers 1 to 35 satisfied the preferred manufacturing conditions 1 to 3. Therefore, F1 and F2 were appropriate, and F3 was also appropriate. Therefore, even better resistance to condensation discoloration was obtained compared to test numbers 36 to 44.
[0191] On the other hand, in test numbers 45 and 46, the amount of the chemical conversion coating applied was too small, and therefore sufficient corrosion resistance and adhesion were not obtained.
[0192] In test numbers 47 and 48, the amount of the chemical conversion coating attached was too large, and therefore sufficient adhesion was not obtained.
[0193] In test numbers 49 and 50, F1 was too low, and therefore sufficient blackening resistance was not obtained.
[0194] In test numbers 51 and 52, F1 was too high, and therefore sufficient corrosion resistance was not obtained.
[0195] In test numbers 53 and 54, F2 was too high, and therefore sufficient condensation discoloration resistance was not obtained.
[0196] In test number 55, the Mg content in the plating layer was low, and therefore sufficient corrosion resistance was not obtained.
[0197] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments within the scope of the present disclosure.
Claims
1. A steel sheet comprising: a base steel sheet; a plating layer formed on the base steel sheet; and a chemical conversion coating formed on the plating layer, wherein the chemical composition of the plating layer is, in mass%, Al: more than 5.0 and less than 25.0%, Mg: more than 3.0 and less than 12.5%, Sn: 0 to 3.00%, Bi: 0 to 5.00%, In: 0 to 2.00%, Ca: 0 to 3.00%, Y: 0 to 3.00%, La: 0 to 3.00%, Ce: 0 to 3.00%, Si: 0 to 2.50%, Cr: 0 to 0.5%, Ti: 0 to 0.5%, Ni: 0 to 0.5%, Co: 0 to 0.5%, V: 0 to 0.5%, Nb: 0 to 0.5%, Cu: 0 to 0.5%, The alloy contains Mn: 0 to 0.5%, Fe: 0 to 5.0%, Sr: 0 to 0.5%, Sb: 0 to 0.5%, Pb: 0 to 0.5%, and B: 0 to 0.5%, with the balance being 65.0% or more of Zn and impurities, and the chemical conversion coating contains Zr, V, P, and Co, and an acrylic resin, and the coating weight of the chemical conversion coating is 300 to 1000 mg / m 2 and the mass of V in the chemical conversion coating [V] mg / m 2 and the mass of P in the chemical conversion coating [P] mg / m 2 and satisfy formula (1), and the Mg content [Mg]b mass % and the V mass [V]mg / m 2 and satisfy the formula (2): 0.60≦[V] / [P]≦2.80 (1) 0<[V] / [Mg]b≦20.00 (2) 2. The surface-treated steel sheet according to claim 1, further comprising: a Mg concentration difference Δ[Mg] mass%, which is the difference between the Mg concentration [Mg]s mass% in the surface layer of the plating layer obtained by elemental analysis of the plating layer in the depth direction using glow discharge optical emission spectrometry and the Mg content [Mg]b mass% in the chemical composition of the plating layer; and a V mass [V] mg / m 2 A surface-treated steel sheet, wherein the formula (3) is satisfied: Δ[Mg]×[V]≦200 (3) 3. A surface-treated steel sheet according to claim 1 or 2, wherein the chemical composition of the plating layer is, in mass %, Sn: 0.01 to 3.00%, Bi: 0.01 to 5.00%, In: 0.01 to 2.00%, Ca: 0.01 to 3.00%, Y: 0.01 to 3.00%, La: 0.01 to 3.00%, Ce: 0.01 to 3.00%, Si: 0.01 to 2.50%, Cr: 0.1 to 0.5%, Ti: 0.1 to 0.5%, Ni: 0.1 to 0.5%, Co: 0.1 to 0.5%, V: 0.1 to 0.5%, Nb: 0.1 to 0.5%, Cu: 0.1 to 0.5%, A surface-treated steel sheet containing one or more elements selected from the group consisting of Mn: 0.1 to 0.5%, Fe: 0.1 to 5.0%, Sr: 0.1 to 0.5%, Sb: 0.1 to 0.5%, Pb: 0.1 to 0.5%, and B: 0.1 to 0.5%.