Plated steel material and method for manufacturing plated steel material
Patent Information
- Application Number
- MYPI2025001088
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-08-31
- Filing Date
- 2022-12-16
- Publication Date
- 2024-02-29
AI Technical Summary
Zn-Al-Mg alloy-plated steel materials with high Al and Mg concentrations exhibit superior corrosion resistance but are prone to early white rust and oxidative discoloration, and high Mg concentrations lead to poor workability and discoloration issues.
A plated steel material with a Zn-Al-Mg alloy layer and an Mg-enriched layer on its surface, where the Zn concentration is above 65%, Al between 5-25%, Mg between 3-12.5%, and additional elements within specific ranges, along with a laminated structure including an Al-Fe alloy layer, is developed. The manufacturing process involves immersing the base steel in a plating bath and controlling cooling rates, followed by skin pass rolling to achieve the desired layer thickness and structure.
The solution provides excellent corrosion resistance in severe environments, maintains workability, and prevents discoloration, forming a dense corrosion product film that reduces corrosion rates and ensures processability.
Smart Images

Figure PI2025001088_DRAWING_001
Abstract
Description
Plated steel product and method for manufacturing the same
[0001] The present disclosure relates to plated steel products and methods for manufacturing plated steel products.
[0002] For example, in the field of building materials, a wide variety of plated steels are used. Most of these are zinc-plated steels. Due to the need for longer life spans for building materials, research into improving the corrosion resistance of zinc-plated steels has been conducted for a long time, and various plated steels have been developed. The first highly corrosion-resistant plated steel for building materials was Zn-5% Al-plated steel (galvanized steel), which had improved corrosion resistance due to the addition of Al to the zinc-based plating layer. It is well known that adding Al to a plating layer improves corrosion resistance, and the addition of 5% Al forms Al crystals in the plating layer (specifically, the Zn phase), improving corrosion resistance. Zn-55% Al-1.6% Si-plated steel (galvalume steel) is also a plated steel with improved corrosion resistance for essentially the same reason.
[0003] The appeal of zinc-based plated steel is its sacrificial corrosion protection effect on the base steel. That is, at the cut end of plated steel, at areas where the plating layer breaks during processing, and at areas where the base steel is exposed due to peeling of the plating layer, the surrounding plating layer dissolves before the base steel corrodes, and the eluted components form a protective film. This makes it possible to prevent red rust from forming on the base steel to some extent.
[0004] Generally, a low Al concentration and a high Zn concentration are preferable for this effect. Therefore, highly corrosion-resistant plated steel materials with a relatively low Al concentration of about 5% to 25% have been put into practical use in recent years. In particular, plated steel materials with a low Al concentration and containing about 1% to 3% Mg have superior corrosion resistance to Galvanic Acid Plated Steel. For this reason, they have become a market trend for plated steel materials and are now widely known on the market.
[0005] As a plated steel material containing a certain amount of Al and Mg, for example, the plated steel material disclosed in Patent Document 1 has been developed.
[0006] Specifically, Patent Document 1 describes a method for producing a plated steel material having a plating layer on the surface of the steel material, the plating layer comprising Al: 5 to 18 mass %, Mg: 1 to 10 mass %, Si: 0.01 to 2 mass %, the balance being Zn and unavoidable impurities, in which an Al phase is formed to a thickness of 1 mm. 2 The publication discloses a hot-dip Zn-Al-Mg-Si plated steel material in which 200 or more particles exist per one particle.
[0007] Furthermore, Patent Document 2 describes a plated steel material having a steel material and a plating layer including a Zn—Al—Mg alloy layer disposed on the surface of the steel material, wherein the plating layer has a chemical composition containing more than 65.0% Zn, more than 5.0% to less than 25.0% Al, more than 3.0% to less than 12.5% Mg, and 0.1% to 20.0% Sn, and wherein the surface of the Zn—Al—Mg alloy layer is polished to half its thickness, and then observed with a scanning electron microscope at a magnification of 100 times. In a backscattered electron image of the Zn—Al—Mg alloy layer, Al crystals are present, and the average cumulative perimeter of the Al crystals is 88 to 195 mm / mm. 2 "Plated steel material which is
[0008] Patent Document 1: JP 2001-355053 A Patent Document 2: WO2019 / 221193
[0009] Zn-Al-Mg alloy-plated steel with high Al and Mg concentrations has better corrosion resistance than Zn-based alloy-plated steel in heavily salt-damaged areas with high levels of airborne salt and a severely corrosive environment, but it still tends to develop white rust soon after application. Furthermore, plating with a high Mg concentration is prone to oxidation and discoloration, and its hardness can make it difficult to work.
[0010] Therefore, an object of the present disclosure is to provide a plated steel material that has excellent corrosion resistance even in areas subject to heavy salt damage, and that is compatible with workability and discoloration resistance, and a method for manufacturing the same.
[0011] The above-mentioned problems are solved by the following means. <1> A plated steel material having a base steel material and a plating layer including a Zn-Al-Mg alloy layer disposed on a surface of the base steel material and a Mg-enriched layer disposed on the surface of the Zn-Al-Mg alloy layer, wherein the plating layer contains, in mass %,: Zn: more than 65.00%, Al: more than 5.00% and less than 25.00%, Mg: more than 3.00% and less than 12.50%, Sn: 0% to 3.0%, Bi: 0% to less than 5.00%, In: 0% to less than 2.00%, Ca: 0% to 3.00%, Y: 0% to 0.50%, La: 0% to less than 0.50%, Ce: 0% to less than 0.50%, Si: 0% to less than 2.5%, Cr: 0% to less than 0.25%, Ti: 0% to less than 0.25%, Zr: 0% to less than 0.25%, Mo: 0% to less than 0.25%, W: 0% to less than 0.25%, Ag: 0% to less than 0.25%, P: 0% to less than 0.25%, Ni: 0% to less than 0.25%, Co: 0% to less than 0.25%, V: 0% to less than 0.25%, Nb: 0% to less than 0.25%, Cu: 0% to less than 0.25%, Mn: 0% to less than 0.25%, Li: 0% to less than 0.25%, Na: 0% to less than 0.25%, K: 0% to less than 0.25%, Fe: 0% to 5.0%, Sr: 0% to less than 0.5%, The Zn-Al-Mg alloy layer has a chemical composition consisting of Sb: 0% to less than 0.5%, Pb: 0% to less than 0.5%, B: 0% to less than 0.5%, and impurities. 2 Crystal, Zn / Al / MgZn 2A plated steel material, in which the total area ratio of ternary eutectic is 90% or more, and the thickness of the Mg-enriched layer is 0.8 μm or more (½ times the thickness of the plated layer) or less.<2> The plated steel material according to <1>, in which the plated layer includes an Al-Fe alloy layer between the base steel material and the Zn-Al-Mg alloy layer.<3> A method for producing a plated steel material according to <1> or <2>, comprising the steps of: immersing the base steel material in a coating bath and withdrawing it from the coating bath; cooling it at an average cooling rate of 15°C / s or less in a temperature range of 450 to 395°C; cooling it at an average cooling rate of 3°C / s or less in a temperature range of 395 to 340°C; and cooling it at an average cooling rate of 10 to 20°C / s or more in a temperature range of 340 to 280°C; and, after cooling, skin-pass rolling it under conditions of a skin-pass roll surface roughness Ra of 1 to 5 μm and a skin-pass rolling force of 100 to 500 tons.
[0012] According to the present disclosure, it is possible to provide a plated steel material that has excellent corrosion resistance even in areas with heavy salt damage, and that is both workable and resistant to discoloration, and a method for manufacturing the same.
[0013] FIG. 1 is a graph illustrating a method for measuring the thickness of the Mg-enriched layer.
[0014] An example of the present disclosure will be described below. In this disclosure, the "%" representation of the content of each element in a chemical composition means "mass %." A numerical range expressed using "to" means a range that includes the numerical values written before and after "to" as the lower and upper limits. When "greater than" or "less than" is added to the numerical values written before and after "to", the numerical range does not include these numerical values as the lower or upper limit. The content of an element in a chemical composition may be expressed as an element concentration (e.g., Zn concentration, Mg concentration, etc.).
[0015] The plated steel material of the present disclosure has a base steel material, a Zn—Al—Mg alloy layer disposed on the surface of the base steel material, and a plating layer including an Mg-enriched layer disposed on the surface of the Zn—Al—Mg alloy layer. 2 Crystal, Zn / Al / MgZn 2 The total area ratio of the ternary eutectic is 90% or more, and the thickness of the Mg-enriched layer is 0.8 μm or more (½ of the thickness of the plating layer) or less.
[0016] The plated steel material disclosed herein has a Mg-enriched layer on the surface of the Zn-Al-Mg alloy layer, which allows a dense corrosion product film containing Mg to form early in the early stages of corrosion. The dense corrosion product film reduces the corrosion rate. Therefore, the steel material exhibits excellent corrosion resistance even in heavily salt-damaged areas with high levels of airborne salt, resulting in a severely corrosive environment. Furthermore, by appropriately adjusting the chemical composition of the plated layer and the extent of the Mg-enriched layer, both workability and discoloration resistance can be achieved. In addition, the presence of a Zn-Al-Mg alloy layer having the above-described structure beneath the Mg-enriched layer ensures workability while supplying Mg ions and Al ions to the corrosive environment from the middle to late stages of corrosion. This maintains a dense corrosion product film, thereby improving corrosion resistance.
[0017] Hereinafter, the plated steel material of the present disclosure will be described in detail.
[0018] (Base Steel Material) There are no particular limitations on the shape of the base steel material. Examples of the base steel material include steel plates, as well as formed base steel materials such as steel pipes, civil engineering and construction materials (fences, corrugated pipes, drainage ditch covers, sand-blocking plates, bolts, wire mesh, guardrails, water-blocking walls, etc.), home appliance components (casings for outdoor units of air conditioners, etc.), and automobile parts (suspension components, etc.). For the forming, various plastic processing techniques such as press working, roll forming, and bending can be used.
[0019] The material of the base steel is not particularly limited. Various types of base steel can be used, such as general steel, pre-plated steel, Al-killed steel, extra-low carbon steel, high carbon steel, various high-tensile steels, and some high-alloy steels (steels containing strengthening elements such as Ni and Cr). The manufacturing conditions for the base steel, such as the manufacturing method for the base steel and the manufacturing method for the base steel sheet (hot rolling, pickling, cold rolling, etc.), are also not particularly limited. Hot-rolled steel sheets, hot-rolled steel strips, cold-rolled steel sheets, and cold-rolled steel strips specified in JIS G 3302 (2010) can also be used as the base steel.
[0020] The base steel may be a pre-plated steel material that has been pre-plated. Pre-plated steel materials can be obtained, for example, by an electrolytic treatment method or a displacement plating method. In the electrolytic treatment method, the base steel material is immersed in a sulfate bath or chloride bath containing metal ions of various pre-plating components for electrolytic treatment to obtain the pre-plated steel material. In the displacement plating method, the base steel material is immersed in an aqueous solution containing metal ions of various pre-plating components and the pH of which is adjusted with sulfuric acid to cause displacement precipitation of the metal to obtain the pre-plated steel material. A typical example of a pre-plated steel material is pre-Ni-plated steel material.
[0021] (Plated layer) The plated layer includes a Zn—Al—Mg alloy layer and a Mg-enriched layer disposed on the surface of the Zn—Al—Mg alloy layer. In addition to the Zn—Al—Mg alloy layer and the Mg-enriched layer, the plated layer may also include an Al—Fe alloy layer. The Al—Fe alloy layer is disposed between the base steel and the Zn—Al—Mg alloy layer.
[0022] That is, the plating layer may have a laminated structure including a Zn-Al-Mg alloy layer, an Mg-enriched layer, and an Al-Fe alloy layer. However, although an oxide film of the plating layer constituent elements having a thickness of about 50 nm may be formed on the surface of the plating layer, it is considered to be thin relative to the overall thickness of the plating layer (about 8 to 60 μm) and not to constitute the main part of the plating layer.
[0023] The coating weight of the plating layer is 40 to 300 g / m per side. 2 The coating weight of the plating layer is preferably 40 g / m 2 If the coating weight of the plating layer is 300 g / m or more, corrosion resistance can be more reliably ensured. 2 If the thickness is set to the above range, poor appearance such as sagging of the plating layer can be suppressed.
[0024] Next, the chemical composition of the plating layer will be described. The chemical composition of the plating layer is, in mass %, as follows: Zn: more than 65.00%, Al: more than 5.00% but less than 25.00%, Mg: more than 3.00% but less than 12.50%, Sn: 0% to 3.00%, Bi: 0% to less than 5.00%, In: 0% to less than 2.00%, Ca: 0% to 3.00%, Y: 0% to 0.50%, La: 0% to less than 0.50%, Ce: 0% to less than 0.50%, Si: 0% to less than 2.5%, Cr: 0% to less than 0.25%, Ti: 0% to less than 0.25%, Zr: 0% to less than 0.25%, Mo: 0% to less than 0.25%, W: 0% to less than 0.25%, The chemical composition is Ag: 0% to less than 0.25%, P: 0% to less than 0.25%, Ni: 0% to less than 0.25%, Co: 0% to less than 0.25%, V: 0% to less than 0.25%, Nb: 0% to less than 0.25%, Cu: 0% to less than 0.25%, Mn: 0% to less than 0.25%, Li: 0% to less than 0.25%, Na: 0% to less than 0.25%, K: 0% to less than 0.25%, Fe: 0% to 5.00%, Sr: 0% to less than 0.50%, Sb: 0% to less than 0.50%, Pb: 0% to less than 0.50%, B: 0% to less than 0.50%, and impurities.
[0025] In the chemical composition of the plating layer, Sn, Bi, In, Ca, Y, La, Ce, Si, Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, K, Fe, Sr, Sb, Pb, and B are optional components. In other words, these elements do not have to be contained in the plating layer. When these optional components are contained, the content of each optional element is preferably within the range described below.
[0026] Here, the chemical composition of the plating layer is the average chemical composition of the entire plating layer (the average chemical composition of the total of the Zn—Al—Mg alloy layer and the Mg-enriched layer, or the average chemical composition of the total of the Al—Fe alloy layer, the Zn—Al—Mg alloy layer, and the Mg-enriched layer).
[0027] Each element in the plating layer will be described below.
[0028] Zn: More than 65.00% Zn is an element necessary for obtaining corrosion resistance. When considering the Zn concentration in terms of atomic composition ratio, since the plating layer is composed of elements with low specific gravity such as Al and Mg, Zn must be the main component in terms of atomic composition ratio as well. Therefore, the Zn concentration is set to more than 65.00%. The Zn concentration is preferably 70.00% or more. The upper limit of the Zn concentration is the concentration that is the remainder excluding elements other than Zn and impurities.
[0029] Al: More than 5.00% to Less than 25.00% Al is an essential element for forming Al crystals and ensuring corrosion resistance. Furthermore, Al is also an essential element for improving the adhesion of the coating layer and ensuring workability. Therefore, the lower limit of the Al concentration is set to more than 5.00% (preferably 10.00% or more). On the other hand, if the Al concentration increases too much, corrosion resistance tends to deteriorate. Therefore, the upper limit of the Al concentration is set to less than 25.00% (preferably 23.00% or less).
[0030] Mg: more than 3.00% to less than 12.50% Mg is an essential element for ensuring corrosion resistance. Therefore, the lower limit of the Mg concentration is set to more than 3.00% (preferably more than 4.00%). On the other hand, if the Mg concentration increases too much, workability tends to deteriorate. Therefore, the upper limit of the Mg concentration is set to less than 12.50% (preferably 10.00% or less).
[0031] Sn: 0 to 3.00% Sn is an element that contributes to corrosion resistance and initial discoloration resistance. Therefore, the lower limit of the Sn concentration is preferably more than 0.00% (preferably 0.05% or more, more preferably 0.10% or more). On the other hand, if the Sn concentration increases too much, corrosion resistance and initial discoloration resistance tend to deteriorate. Therefore, the upper limit of the Sn concentration is set to 3.00% or less.
[0032] Bi: 0% to less than 5.00% Bi is an element that contributes to corrosion resistance. Therefore, the lower limit of the Bi concentration is preferably more than 0.00% (preferably 0.10% or more, more preferably 3.00% or more). On the other hand, if the Bi concentration increases too much, corrosion resistance tends to deteriorate. Therefore, the upper limit of the Bi concentration is set to less than 5.00% (preferably 4.80% or less).
[0033] In: 0% to less than 2.00% In is an element that contributes to corrosion resistance. Therefore, the lower limit of the In concentration is preferably more than 0.00% (preferably 0.10% or more, more preferably 1.00% or more). On the other hand, if the In concentration increases too much, corrosion resistance tends to deteriorate. Therefore, the upper limit of the In concentration is set to less than 2.00% (preferably 1.80% or less).
[0034] Ca: 0% to 3.00% Ca is an element that can adjust the optimal amount of Mg elution to impart corrosion resistance. Therefore, the lower limit of the Ca concentration is preferably more than 0.00% (preferably 0.05% or more). On the other hand, if the Ca concentration increases too much, corrosion resistance and workability tend to deteriorate. Therefore, the upper limit of the Ca concentration is set to 3.00% or less (preferably 1.00% or less).
[0035] Y: 0% to 0.50% Y is an element that contributes to corrosion resistance. Therefore, the lower limit of the Y concentration is preferably more than 0.00% (preferably 0.10% or more). On the other hand, if the Y concentration increases too much, corrosion resistance tends to deteriorate. Therefore, the upper limit of the Y concentration is set to 0.50% or less (preferably 0.30% or less).
[0036] La and Ce: 0% to less than 0.50% La and Ce are elements that contribute to corrosion resistance. Therefore, the lower limit of each of the La concentration and the Ce concentration is preferably more than 0.00% (preferably 0.10% or more). On the other hand, if the La concentration and the Ce concentration are too high, corrosion resistance tends to deteriorate. Therefore, the upper limit of each of the La concentration and the Ce concentration is set to less than 0.50% (preferably 0.40% or less).
[0037] Si: 0% to less than 2.50% Si is an element that suppresses the growth of the Al—Fe alloy layer and contributes to improving corrosion resistance. Therefore, the Si concentration is preferably greater than 0.00% (preferably 0.05% or more, more preferably 0.10% or more). In particular, when Sn is not included (i.e., when the Sn concentration is 0%), the Si concentration is preferably 0.10% or more (preferably 0.20% or more) from the viewpoint of ensuring corrosion resistance. On the other hand, if the Si concentration is too high, corrosion resistance and workability tend to deteriorate. Therefore, the upper limit of the Si concentration is set to less than 2.50%. In particular, from the viewpoint of corrosion resistance, the Si concentration is preferably 2.40% or less, more preferably 1.80% or less, and even more preferably 1.20% or less.
[0038] Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K: 0% to less than 0.25% Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K are elements that contribute to corrosion resistance. Therefore, the lower limit of the concentration of Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K is preferably more than 0% (preferably 0.05% or more, more preferably 0.10% or more). On the other hand, if the concentrations of Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K increase too much, corrosion resistance tends to deteriorate. Therefore, the upper limits of the concentrations of Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K are each set to less than 0.25%.The upper limits of the concentrations of Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K are preferably set to 0.22% or less.
[0039] Fe: 0% to 5.00% When a plating layer is formed by hot-dip plating, a certain concentration of Fe is contained in the Zn—Al—Mg alloy layer and the Al—Fe alloy layer. It has been confirmed that Fe contained in the plating layer (particularly the Zn—Al—Mg alloy layer) with a concentration of up to 5.00% does not adversely affect performance. Since most of the Fe is often contained in the Al—Fe alloy layer, the thicker this layer is, the higher the Fe concentration will generally be.
[0040] Sr, Sb, Pb, and B: 0% to less than 0.50% Sr, Sb, Pb, and B are elements that contribute to corrosion resistance. Therefore, the lower limit of the concentration of Sr, Sb, Pb, and B is preferably more than 0% (preferably 0.05% or more, more preferably 0.10% or more). On the other hand, if the concentrations of Sr, Sb, Pb, and B increase too much, corrosion resistance tends to deteriorate. Therefore, the upper limit of the concentration of Sr, Sb, Pb, and B is each set to less than 0.50%.
[0041] Impurities are components contained in raw materials or components mixed in during the manufacturing process, but are not intentionally added. For example, trace amounts of components other than Fe may be mixed into the coating layer as impurities due to atomic diffusion between the base steel and the coating bath.
[0042] The chemical composition of the plating layer is measured by the following method. First, the plating layer is stripped and dissolved using an acid containing an inhibitor that suppresses corrosion of the base steel material to obtain an acid solution. Next, the obtained acid solution is measured using ICP analysis to obtain the chemical composition of the plating layer. There are no particular restrictions on the type of acid, as long as it is an acid that can dissolve the plating layer. The chemical composition is measured as an average chemical composition. In ICP analysis, the Zn concentration is calculated using the formula: Zn concentration = 100% - concentration of other elements (%).
[0043] Here, when a pre-plated steel material is used as the base steel material, the components of the pre-plating are also detected. For example, when a pre-Ni plated steel material is used, ICP analysis detects not only Ni in the plating layer but also Ni in the pre-Ni plating. Specifically, for example, when the Ni deposition amount is 1 g / m, 2 ~3g / m 2When pre-plated steel (thickness: approximately 0.1 to 0.3 μm) is used as a base steel, even if the Ni concentration in the plating layer is 0%, the Ni concentration is detected as 0.1 to 15% when measured by ICP analysis. The method for determining whether a base steel is pre-Ni-plated steel is as follows: A sample is taken from the target steel, with the cross section cut along the thickness direction of the plating layer serving as the measurement surface. An electron probe microanalyzer (FE-EPMA) is used to perform line analysis of the sample's measurement surface near the interface between the plating layer and the base steel to measure the Ni concentration. The measurement conditions are an acceleration voltage of 15 kV, a beam diameter of approximately 100 nm, an irradiation time per point of 1000 ms, and a measurement pitch of 60 nm. The measurement distance may be any distance that allows confirmation of whether or not the Ni concentration is enriched at the interface between the plating layer and the base steel material in the steel material. If the Ni concentration is enriched at the interface between the plating layer and the base steel material in the steel material, the base steel material is determined to be a pre-Ni-plated steel material.
[0044] Furthermore, when pre-Ni-plated steel is used as the base steel, the Ni concentration of the plating layer is defined as the value measured as follows. First, the Ni emission intensity is measured for three or more standard samples (BAS Zn alloy standard samples IMN ZH1, ZH2, and ZH4) with different Ni concentrations using a high-frequency glow discharge optical emission surface analyzer (GDS: manufactured by HORIBA, Ltd., model number: GD-Profiler 2). A calibration curve is created from the relationship between the Ni emission intensity and the Ni concentration of the standard samples. Next, the surface of the plating layer of the sample is polished in the thickness direction of the plating layer (hereinafter also referred to as the "Z-axis direction"). Specifically, the surface of the plating layer is dry-polished with a #1200 grit polishing sheet, and then finish-polished using a finishing solution containing alumina with an average particle size of 3 μm, a finishing solution containing alumina with an average particle size of 1 μm, and a finishing solution containing colloidal silica, in that order. The Zn intensity on the surface of the plating layer is measured before and after polishing using XRF (X-ray fluorescence analysis), and the point at which the Zn intensity after polishing is half of the Zn intensity before polishing is defined as half the thickness of the plating layer. Next, the Ni emission intensity at a position half the thickness of the plating layer of the plated steel material to be measured is measured using a high-frequency glow discharge optical emission surface analyzer (GDS: manufactured by HORIBA, Ltd., model number: GD-Profiler2). The Ni concentration at the position half the thickness of the plating layer is determined from the obtained Ni emission intensity and the created calibration curve. When pre-Ni plated steel material is used as the base steel material, the Zn concentration of the plating layer is defined as the Zn concentration calculated using the following formula: Formula: Zn concentration = 100 - (concentration of elements other than Zn and Ni determined by ICP analysis + Ni concentration determined by GDS)
[0045] The measurement conditions for the high-frequency glow discharge optical emission surface analyzer are as follows: H.V.: 630 V, anode diameter: φ4 mm, gas: Ar, gas pressure: 600 Pa, output: 35 W.
[0046] Next, the structure of the Zn—Al—Mg alloy layer will be described. 2 Crystal, Zn / Al / MgZn 2The total area ratio of the ternary eutectic is 90% or more. From the viewpoint of improving corrosion resistance, the lower limit of the area ratio is preferably 92%, 95%, or 98%. Ideally, the area ratio is particularly preferably 100%. In addition, like Zn crystals, the above-mentioned Al crystals, MgZn 2 Crystal, Zn / Al / MgZn 2 The area ratio of the structure excluding the ternary eutectic is preferably 0 to 10%, more preferably 0 to 8%, 0 to 5%, or even more preferably 0 to 2%. Ideally, the area ratio of Zn crystals is particularly preferably 0% (that is, it is particularly preferable that Zn crystals are not included). Here, Al crystals and Zn crystals each mean crystals that are independently crystallized.
[0047] The structure of the Zn-Al-Mg alloy layer is measured as follows: First, a sample is taken from the plated steel material to be measured. The sample is taken from a location that is free of defects in the plating layer and is not near the punched end surface of the plated steel material (2 mm from the end surface).
[0048] Next, the surface of the plating layer of the sample is polished in the thickness direction of the plating layer (hereinafter also referred to as the "Z-axis direction"). Specifically, the surface of the plating layer is dry-polished with a #1200 grit polishing sheet, and then finish-polished using a finishing solution containing alumina with an average particle size of 3 μm, a finishing solution containing alumina with an average particle size of 1 μm, and a finishing solution containing colloidal silica, in that order. The Zn intensity of the plating layer surface before and after polishing is measured by XRF (X-ray fluorescence analysis), and the point at which the Zn intensity after polishing is half of the Zn intensity before polishing is defined as half the thickness of the plating layer. Since the Zn—Al—Mg alloy layer occupies more than half the thickness of the plating layer, the polished surface polished to half the thickness of the plating layer is the polished surface of the Zn—Al—Mg alloy layer. Therefore, analyzing the polished surface allows the metal structure contained in the Zn—Al—Mg alloy layer to be identified.
[0049] Next, the polished surface is observed under a scanning electron microscope (SEM) at a magnification of 500 times to obtain a backscattered electron image (hereinafter also referred to as a "SEM backscattered electron image"). The SEM observation conditions are an acceleration voltage of 15 kV, a probe current of 10 nA, and a field of view of 244 μm × 198 μm.
[0050] Furthermore, a mapping analysis was performed using an electron probe microanalyzer (FE-EPMA) at an acceleration voltage of 15 kV, an irradiation current of 30 nA, a beam diameter of approximately 100 nm, an irradiation time per point of 5 ms, a measurement pitch of 300 nm, and a magnification of 500x. The area can then be roughly divided into an area where the detection points of Mg and Zn overlap, an area where the detection points of Al and Zn overlap, and an area where Zn is detected alone. The area where the detection points of Mg and Zn overlap is referred to as MgZn. 2 The area where the detected points of Al and Zn overlap is defined as Al crystal. Furthermore, in the area where Zn is detected alone, a line analysis of 10 μm length is performed by FE-EPMA at a magnification of 2000 times. At this time, the area where Mg or Al is detected at 1% or more in the measurement area is defined as Zn / Al / MgZn. 2 Regions where less than 1% of the ternary eutectic, Mg, and Al are detected can be identified as Zn crystals. These are then subjected to computer image processing to determine the area ratio (the area (pixels) of each phase in the field of view is calculated).
[0051] Next, the Mg-enriched layer will be described. The Mg-enriched layer is a Zn / Al / MgZn layer present on the surface of the Zn-Al-Mg alloy layer. 2 This is a layer in which the Mg concentration is enriched due to the densification of Mg-containing phases such as ternary eutectic. If the Mg-enriched layer is thin, corrosion resistance will be inferior. On the other hand, if the Mg-enriched layer is too thick, discoloration resistance will be deteriorated. Therefore, the thickness of the Mg-enriched layer is set to 0.8 μm or more (thickness of the plating layer × 1 / 2). The thickness of the Mg-enriched layer is preferably 0.9 μm or more and 25 μm or less, more preferably 1.0 μm or more and 22.5 μm or less. The thickness of the plating layer is preferably 5 μm or more and 50 μm or less, more preferably 10 μm or more and 45 μm or less.
[0052] The Mg-enriched layer is a layer defined as follows.
[0053] First, the plating layer is sputtered from the surface side in the depth direction using glow discharge optical emission spectroscopy (quantitative GDS), and the depth distribution of the intensity of each element contained in the plating layer (e.g., Zn, Al, Mg, Fe) is measured (see Figure 1) (measurement equipment: Horiba, Ltd., model number: GD-Profiler 2, measurement conditions: DC mode, voltage 900 V, current 20 mA). If a chemical conversion coating or the like is present on the plating layer, the depth distribution of the intensity of the element that constitutes the main component of the coating (e.g., carbon (C) in the case of an organic coating, or the main element in the case of an inorganic coating) is also measured. In the case of an inorganic coating, the main element is, for example, zirconium (Zr) in the case of a zirconium oxide coating, or silicon (Si) in the case of a coating containing a silane coupling agent. The measurement is carried out to a depth where the plating layer disappears and the base steel is sufficiently exposed. The depth [μm] of the hole after measurement is measured, and the sputtering rate [μm / s] is calculated by dividing the measured value by the GDS measurement time [s]. Multiplying this sputtering rate by the elapsed time from the start of measurement at the target measurement location yields the depth [μm] from the surface of the target measurement location. Here, when observing the change in Fe intensity from the plating surface direction, the point (A) is defined as the point where the increase in Fe intensity per 0.1 μm exceeds 0.003. The Mg intensity at point (A) is defined as 1, and point (B) where the relative Mg intensity is 1.03 when viewed from the base steel (i.e., base steel) side toward the plating layer surface is defined as the interface between the Mg-enriched layer and the Zn-Al-Mg alloy layer. When viewing the plating layer surface from this point, point (C) where the Mg intensity and the carbon (C) intensity become equal is defined as the top of the Mg-enriched layer. The carbon (C) intensity that determines point (C) (the carbon (C) intensity when no chemical conversion coating or the like is present on the plating layer) is the intensity of carbon (C) derived from dirt or oil adhering to the plating layer surface. However, when a chemical conversion coating or the like is present on the plating layer, point (C) is the point where the intensity is the same as that of the element that is the main component of the coating, and is taken as the upper end of the Mg-enriched layer. The Mg-enriched layer is defined as the layer between points (B) and (C), and the thickness of the Mg-enriched layer is defined as the average value of the differences in depth between points (B) and (C) measured at three locations.
[0054] Next, the Al-Fe alloy layer will be described. The Al-Fe alloy layer may be formed on the surface of the base steel material (specifically, between the base steel material and the Zn-Al-Mg alloy layer), and has an Al structure. 5 The Fe phase is the main phase layer. The Al-Fe alloy layer is formed by mutual atomic diffusion between the base steel material and the coating bath. Since the steel material of the present disclosure has a coating layer formed by hot-dip coating, an Al-Fe alloy layer is likely to be formed in the coating layer containing Al element. Since the coating bath contains Al at a certain concentration or more, Al 5 The Fe phase is formed most frequently. However, atomic diffusion takes time, and there are also areas where the Fe concentration is high near the base steel material. Therefore, the Al-Fe alloy layer is partially composed of AlFe phase, Al 3 Fe phase, Al 5 Fe 2 In addition, since the plating bath contains a certain concentration of Zn, the Al-Fe alloy layer also contains a small amount of Zn.
[0055] In terms of corrosion resistance, Al 5 Fe phase, Al 3 Fe phase, AlFe phase, and Al 5 Fe 2 There is no significant difference between the two phases. The corrosion resistance here refers to the corrosion resistance in the areas not affected by welding.
[0056] Here, when the plating layer contains Si, Si is particularly likely to be incorporated into the Al-Fe alloy layer, and may form an Al-Fe-Si intermetallic compound phase. Identified intermetallic compound phases include the AlFeSi phase, and isomers such as α-, β-, q1-, and q2-AlFeSi phases exist. Therefore, these AlFeSi phases may be detected in the Al-Fe alloy layer. An Al-Fe alloy layer containing these AlFeSi phases is also referred to as an Al-Fe-Si alloy layer. Furthermore, since the Al-Fe-Si alloy layer is thinner than the Zn-Al-Mg alloy layer, its effect on the corrosion resistance of the entire plating layer is small.
[0057] Furthermore, when various pre-plated steel materials are used as the base steel material, the structure of the Al-Fe alloy layer may change depending on the amount of pre-plating applied. Specifically, when the pure metal layer used for pre-plating remains around the Al-Fe alloy layer, an intermetallic compound phase (e.g., Al 3 Ni phase, etc.) forms an alloy layer, an Al—Fe alloy layer in which some of the Al atoms and Fe atoms are substituted, or an Al—Fe—Si alloy layer in which some of the Al atoms, Fe atoms, and Si atoms are substituted.
[0058] That is, the Al—Fe alloy layer is made of Al 5 In addition to the alloy layer mainly composed of an Fe phase, the layer includes alloy layers of the above-mentioned various modes.
[0059] When a plating layer is formed on a pre-Ni plated steel material among various pre-plated steel materials, an Al-Ni-Fe alloy layer is formed as the Al-Fe alloy layer.
[0060] The thickness of the Al—Fe alloy layer is, for example, 0 μm or more and 7 μm or less, and is preferably 0.05 μm or more and 5 μm or less from the viewpoints of improving the adhesion of the plating layer (specifically, the Zn—Al—Mg alloy layer) and ensuring corrosion resistance and workability.
[0061] Since the Zn-Al-Mg alloy layer is usually thicker than the Al-Fe alloy layer, the contribution of the Al-Fe alloy layer to the corrosion resistance of the plated steel is smaller than that of the Zn-Al-Mg alloy layer. However, as can be inferred from the results of component analysis, the Al-Fe alloy layer contains Al and Zn, which are corrosion-resistant elements, at a certain concentration or higher. Therefore, the Al-Fe alloy layer has a certain degree of corrosion resistance against the base steel.
[0062] Furthermore, when a plating layer having the chemical composition specified in the present disclosure is formed by hot-dip plating, an Al—Fe alloy layer having a thickness of 100 nm or more is often formed between the base steel material and the Zn—Al—Mg alloy layer.
[0063] From the viewpoint of corrosion resistance, the thicker the Al—Fe alloy layer, the better. Therefore, the thickness of the Al—Fe alloy layer is preferably 0.05 μm or more. However, a thick Al—Fe alloy layer significantly deteriorates workability, so the thickness of the Al—Fe alloy layer is preferably 7 μm or less. When the thickness of the Al—Fe alloy layer is 7 μm or less, the amount of cracks and powdering that originate from the Al—Fe alloy layer is reduced, improving workability. The thickness of the Al—Fe alloy layer is more preferably 5 μm or less, and even more preferably 2 μm or less.
[0064] The thickness of the Al—Fe alloy layer is measured as follows. After embedding the sample in resin and polishing it, the thickness of the identified Al—Fe alloy layer is measured at any five locations on an SEM backscattered electron image (magnification: 10,000x, field of view: 50 μm long x 200 μm wide, field of view in which the Al—Fe alloy layer is visible) of the cross section of the plating layer (a cross section of the plating layer cut along the sheet thickness direction). The arithmetic average of the measurements at the five locations is then taken as the thickness of the Al—Fe alloy layer. The thickness of the plating layer is also measured at any five locations on the cross section SEM backscattered electron image (magnification: 500x, field of view: 198 μm long x 244 μm wide, field of view in which the entire plating layer is visible). The arithmetic average of the measurements at the five locations is then taken as the thickness of the plating layer.
[0065] (Method for Producing Plated Steel Product) Hereinafter, an example of a method for producing a plated steel product according to the present disclosure will be described.
[0066] The plated steel material of the present disclosure is obtained by forming a plating layer having the above-mentioned predetermined chemical composition and metal structure on the surface (i.e., one side or both sides) of a base steel material (such as a base steel sheet) by a hot-dip galvanizing method.
[0067] Specifically, as an example, hot-dip galvanizing is performed under the following conditions. Hereinafter, a method for producing a plated steel sheet will be described as an example of a method for producing a plated steel material according to the present disclosure. First, a base steel sheet serving as a base steel material is immersed in a galvanizing bath and then removed from the galvanizing bath. The steel sheet is then cooled in a temperature range of 450 to 395°C at an average cooling rate of 15°C / s or less. Next, the steel sheet is cooled in a temperature range of 395 to 340°C at an average cooling rate of 3°C / s or less. Next, the steel sheet is cooled in a temperature range of 340 to 280°C at an average cooling rate of 10 to 20°C / s or more. Here, the coating is performed using a continuous hot-dip metal coating method such as the Sendzimir method. After cooling, the steel sheet is subjected to skin-pass rolling under conditions of a skin-pass roll surface roughness Ra of 1 to 5 μm and a skin-pass rolling force of 100 to 500 tons.
[0068] Here, the plating layer is composed of Al crystals and MgZn crystallized around the Al crystals. 2 Crystal, Zn / Al / MgZn 2 It solidifies in the order of ternary eutectic.
[0069] Therefore, Al crystals are grown by cooling at an average cooling rate of 15°C / s or less in the temperature range of 450 to 395°C. Then, MgZn is grown around the Al crystals by cooling at an average cooling rate of 3°C / s or less in the temperature range of 395 to 340°C. 2 This ensures that the Zn / Al / MgZn 2 The ternary eutectic can be refined.
[0070] The upper limit of the average cooling rate in the temperature range of 450 to 395°C is 15°C / s, preferably 13°C / s, and more preferably 11°C / s. The lower limit is not particularly limited, but from the viewpoint of productivity, it is preferably 1°C / s, and more preferably 2°C / s or more. If the average cooling rate in the temperature range of 450 to 395°C exceeds 15°C / s, the Al crystals will be too finely crystallized, resulting in a Zn / Al / MgZn alloy. 2 The ternary eutectic is also excessively refined, which makes it difficult to form an Mg-enriched layer by skin-pass rolling, which will be described later.
[0071] The upper limit of the average cooling rate in the temperature range of 395°C to 340°C is 3°C / s, preferably 2.5°C / s. The lower limit is not particularly limited, but from the viewpoint of productivity, it is preferably 0.5°C / s, more preferably 1°C / s or more. If the average cooling rate in the temperature range of 395°C to 340°C exceeds 3°C / s, the MgZn crystals around the Al crystals may be cooled. 2 The crystals could not be grown sufficiently, and the Zn / Al / MgZn 2 The ternary eutectic crystal is not sufficiently refined, which makes it difficult to form an Mg-enriched layer by skin-pass rolling, which will be described later.
[0072] Next, the Zn / Al / MgZn alloy is cooled in the temperature range of 340 to 280°C at an average cooling rate of 10°C / s or more. 2 The ternary eutectic is refined. This makes it easier for a Mg-enriched layer to be formed by skin-pass rolling, which will be described later. However, if the average cooling rate in the temperature range of 340 to 280°C exceeds 20°C / s, the Zn / Al / MgZn 2 The ternary eutectic becomes excessively fine, making it difficult to form a Mg-enriched layer by skin-pass rolling, which will be described later. The average cooling rate in the temperature range below 280°C is not limited. For example, furnace cooling may be used, or heat retention may be performed to adjust the properties of the steel material. Water cooling may also be performed using mist cooling or the like. The average cooling rate in the method exemplified here is, for example, 50°C / second or less.
[0073] Next, after cooling, skin pass rolling is performed under the conditions that the surface roughness Ra of the skin pass roll is 1 μm or more and the skin pass rolling force is 100 tons or more, thereby removing the soft Mg-containing crystals (Zn / Al / MgZn) present in the surface layer of the Zn-Al-Mg alloy layer. 2 The Mg-enriched layer is formed by extending the Mg-containing crystals (e.g., ternary eutectic). However, if the surface roughness Ra of the skin-pass roll exceeds 5 μm, the surface area of the coating layer increases, causing the Mg-enriched layer to become too thick and resulting in poor discoloration resistance. On the other hand, if the surface roughness Ra of the skin-pass roll is less than 1 μm, the base steel sheet slips during skin-pass rolling, preventing uniform rolling and making it impossible to ensure corrosion resistance and discoloration resistance. Furthermore, if the skin-pass rolling force exceeds 500 tons, the soft Mg-containing crystals (Zn / Al / MgZn 2If the skin-pass rolling force is less than 100 tons, the Mg-enriched layer is difficult to thicken and corrosion resistance is deteriorated. If the skin-pass rolling force is within the appropriate range and the surface roughness Ra of the skin-pass roll is large, point (B) in Figure 1 tends to move to the right, and the thickness of the Mg-enriched layer increases.
[0074] The surface roughness Ra of the skin-pass roll is measured as follows: The roughness of the surface of the skin-pass roll is measured at three locations in the width direction of the roll using a stylus-type portable roughness meter, and the average value is calculated.
[0075] The post-treatments that can be applied to the plated steel material of the present disclosure will be described below.
[0076] The plated steel material of the present disclosure may have a coating formed on the plating layer. The coating may be one layer or two or more layers. Examples of types of coatings that may be formed directly on the plating layer include chromate coatings, phosphate coatings, and chromate-free coatings. The chromate treatment, phosphate treatment, and chromate-free treatment that form these coatings can be performed by known methods.
[0077] Chromate treatments include electrolytic chromate treatments that form a chromate film by electrolysis, reactive chromate treatments that form a film by utilizing a reaction with the material and then wash away excess treatment solution, and paint-on chromate treatments that apply a treatment solution to the substrate and dry it without rinsing with water to form a film. Any of these treatments may be used.
[0078] Examples of electrolytic chromate treatments include electrolytic chromate treatments using chromic acid, silica sol, resin (acrylic resin, vinyl ester resin, vinyl acetate acrylic emulsion, carboxylated styrene butadiene latex, diisopropanolamine-modified epoxy resin, etc.), and hard silica.
[0079] Examples of the phosphate treatment include zinc phosphate treatment, zinc calcium phosphate treatment, and manganese phosphate treatment.
[0080] Chromate-free treatments are particularly suitable because they place no burden on the environment. Chromate-free treatments include electrolytic chromate-free treatments that form a chromate-free film by electrolysis, reactive chromate-free treatments that form a film by utilizing a reaction with the material and then wash away excess treatment liquid, and paint-on chromate-free treatments that apply a treatment liquid to the substrate and dry it without rinsing with water to form a film. Any of these treatments may be used.
[0081] Furthermore, one or more organic resin coatings may be provided on the coating directly on the plating layer. The organic resin is not limited to a specific type, and examples thereof include polyester resin, polyurethane resin, epoxy resin, acrylic resin, polyolefin resin, and modified versions of these resins. Here, the modified version refers to a resin obtained by reacting a reactive functional group contained in the structure of these resins with another compound (such as a monomer or a crosslinking agent) containing a functional group capable of reacting with the functional group.
[0082] Such organic resins may be a mixture of one or more unmodified organic resins, or a mixture of one or more organic resins obtained by modifying at least one other organic resin in the presence of at least one organic resin. The organic resin film may also contain any coloring pigment or anti-rust pigment. Water-based organic resins obtained by dissolving or dispersing them in water may also be used.
[0083] (Examples) A predetermined amount of pure metal ingot was used and melted in a vacuum melting furnace to obtain a coating layer with the chemical composition shown in Tables 1 and 2. A coating bath was then prepared in the atmosphere. A hot-dip coating simulator was used to prepare the coated steel sheets. A 2.3 mm thick general-purpose hot-rolled steel sheet (C concentration <0.1%) was used as the base steel. The surface to be coated of the base steel was brush-polished, and then degreased and pickled immediately before the coating process. In some examples, a pre-Ni-plated steel sheet was used as the base steel, which was a 2.3 mm thick general-purpose hot-rolled steel sheet that had been pre-Ni-plated. The Ni deposition amount was 1 g / m 2 ~3g / m 2In addition, examples in which pre-Ni plated steel was used as the base steel are indicated as "Pre-Ni" in the "Base steel" column in the table. A contact-type K thermocouple was attached to the backside of the surface to be plated of the base steel in order to monitor the temperature of the steel during the plated steel sheet production process.
[0084] In the preparation of all samples, the same reduction treatment method was carried out on the base steel material up to the stage of immersion in the plating bath. 2 -H 2 (5%) (dew point -40°C or less, oxygen concentration less than 25 ppm), the temperature was raised from room temperature to 800°C by electrical heating, and after holding for 60 seconds, N 2 The steel sheets were cooled to a temperature 10°C higher than the plating bath temperature by gas blowing, and immediately immersed in the plating bath. The immersion time in the plating bath for each steel sheet was as shown in the table. 2 The gas wiping pressure was adjusted to prepare plated steel sheets with a plating thickness of 30 μm (±1 μm).
[0085] The coating bath temperature was 500°C. The immersion time in the coating bath was 2 seconds. After the base steel material was pulled out of the coating bath, a coating layer was obtained by a cooling process in which the average cooling rates in the following first to third stages shown in Tables 1 and 2 were set as shown in Tables 1 and 2. - First stage average cooling rate: Average cooling rate in the temperature range of 450 to 395°C - Second stage average cooling rate: Average cooling rate in the temperature range of 395 to 340°C - Third stage average cooling rate: Average cooling rate in the temperature range of 340 to 280°C During the cooling process, N was added to the coated steel material. 2 The steel material was cooled by blowing gas onto it. At this time, N was blown onto the steel material so as to achieve a predetermined cooling rate within the above temperature range. 2 The cooling was carried out while adjusting the amount of gas blown.
[0086] -Various measurements- Samples were cut out from the obtained plated steel sheets. Then, the following items were measured according to the methods described above. -Thickness of the plated layer -Thickness of the Mg-enriched layer -Thickness of the Al-Fe alloy layer (however, in the case of examples where a pre-Ni plated steel sheet was used as the base steel, the thickness of the Al-Ni-Fe alloy layer is shown). -The ratio of Al crystals, MgZn, 2Crystal, Zn / Al / MgZn 2 Total area ratio of ternary eutectic (referred to as specific structure area ratio in the table)
[0087] - Corrosion resistance - Samples were cut out from the obtained plated steel sheets. Then, the samples were placed vertically and subjected to 21 cycles of a combined cyclic corrosion test (CCT) in accordance with the accelerated corrosion test (JASO M609-91). After the corrosion test, the corrosion weight loss was 20 g / m 2 The following cases are evaluated as "A": 2 Super was rated as "NG".
[0088] - Workability - Samples were cut out from the obtained plated steel sheets. After bending the samples by 1T, the bent portion was peeled off with tape and the area ratio of the plated layer adhered to the tape was evaluated. An area ratio of the plated layer adhered to the tape of 5% or less was evaluated as "A", and an area ratio of more than 5% was evaluated as "NG".
[0089] - Discoloration resistance - A sample was cut out from the obtained plated steel sheet. The sample was then placed at an angle of 60° to the horizontal in a constant temperature and humidity tester (KCL-2000 manufactured by EYELA) at 50°C and 80% RH, and the color difference ΔE after three days was evaluated. Regarding color difference, the L value, a* value, and b* value of the sample were measured using the SCE (specular reflection excluded) method with a colorimeter (CR-400 manufactured by Konica Minolta Optics) before and after the test, and the color difference ΔE was investigated at four locations and the average value was calculated. An average color difference ΔE of 10 or less after three days was evaluated as "A," and an average value of more than 10 was evaluated as "NG."
[0090] Examples are listed in Tables 1 and 2.
[0091]
[0092]
[0093]
[0094]
[0095]
[0096]
[0097]
[0098]
[0099] The above results show that the plated steel materials of the present disclosure, which are examples, are superior in corrosion resistance compared to the comparative examples, even in coastal areas where there is a high level of airborne salt and a severely corrosive environment. They also have excellent workability and discoloration resistance.
[0100] In Test No. 103, uniform rolling could not be achieved and the appearance varied greatly, so the thicknesses of the various plating layers were not measured.
[0101] Although the preferred embodiments and examples of the present disclosure have been described in detail above with reference to the accompanying drawings, the present disclosure is not limited to such examples. It is clear that a person skilled in the art to which the present disclosure pertains can conceive of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally fall within the technical scope of the present disclosure.
[0102] The disclosure of Japanese Patent Application No. 2022-138732 is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. A plated steel product having a base steel material and a plating layer including a Zn-Al-Mg alloy layer disposed on the surface of the base steel material and a Mg-enriched layer disposed on the surface of the Zn-Al-Mg alloy layer, wherein the plating layer contains, in mass %, Zn: more than 65.00%, Al: more than 5.00% but less than 25.00%, Mg: more than 3.00% but less than 12.50%, Sn: 0% to 3.00%, Bi: 0% to less than 5.00%, In: 0% to less than 2.00%, Ca: 0% to 3.00%, Y: 0% to 0.50%, La: 0% to less than 0.50%, Ce: 0% to less than 0.50%, Si: 0% to less than 2.5%, Cr: 0% to less than 0.25%, Ti: 0% to less than 0.25%, Zr: 0% to less than 0.25%, Mo: 0% to less than 0.25%, W: 0% to less than 0.25%, Ag: 0% to less than 0.25%, P: 0% to less than 0.25%, Ni: 0% to less than 0.25%, Co: 0% to less than 0.25%, V: 0% to less than 0.25%, Nb: 0% to less than 0.25%, Cu: 0% to less than 0.25%, Mn: 0% to less than 0.25%, Li: 0% to less than 0.25%, Na: 0% to less than 0.25%, K: 0% to less than 0.25%, Fe: 0% to 5.00%, Sr: 0% to less than 0.50%, The Zn-Al-Mg alloy layer has a chemical composition consisting of Sb: 0% to less than 0.50%, Pb: 0% to less than 0.50%, B: 0% to less than 0.50%, and impurities. 2 Crystal, Zn / Al / MgZn 2 A plated steel material, wherein a total area ratio of ternary eutectic is 90% or more, and the thickness of the Mg-enriched layer is 0.8 μm or more (½ times the thickness of the plated layer) or less.
2. The plated steel material according to claim 1, wherein the plated layer includes an Al-Fe alloy layer between the base steel material and the Zn-Al-Mg alloy layer.
3. A method for producing plated steel according to claim 1 or claim 2, comprising the steps of: immersing a base steel material in a coating bath, removing it from the coating bath, and then cooling it in a temperature range of 450 to 395°C at an average cooling rate of 15°C / s or less; cooling it in a temperature range of 395 to 340°C at an average cooling rate of 3°C / s or less; and cooling it in a temperature range of 340 to 280°C at an average cooling rate of 10 to 20°C / s or more; and after cooling, skin-pass rolling is performed under conditions of a skin-pass roll surface roughness Ra of 1 to 5 μm and a skin-pass rolling force of 100 to 500 tons.