Chemical agent for forming solid lubrication coating film, method for manufacturing chemical agent, method for applying chemical agent, oil country tubular goods, and threaded joint for oil country tubular goods

MYPI2025001214A0Undetermined Publication Date: 2024-02-25JFE STEEL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025001214
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-08-25
Filing Date
2023-08-14
Publication Date
2024-02-25

AI Technical Summary

Technical Problem

Conventional methods for lubricating oil country tubular goods face challenges such as the difficulty of mixing metal soap with water-based polymers, slow drying times, reliance on volatile organic compounds (VOCs), and the need for environmentally friendly solutions that avoid heavy metals and PFAS, while also ensuring effective lubrication and corrosion resistance under severe well conditions.

Method used

A chemical agent using a water-soluble or water-dispersible polymer as a binder resin and metal soap as a solid lubricant, dissolved in a solvent system that includes lower alcohols and ammonia to achieve quick drying and dispersion of metal soap particles, ensuring effective lubrication and corrosion resistance without VOCs or harmful substances.

Benefits of technology

The solution provides a solid lubricant film that dries quickly, maintains lubrication and corrosion resistance under severe conditions, and complies with environmental regulations, suitable for use in well environments where traditional methods fail.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025001214_DRAWING_001
    Figure PI2025001214_DRAWING_001
  • Figure PI2025001214_DRAWING_002
    Figure PI2025001214_DRAWING_002
  • Figure PI2025001214_DRAWING_003
    Figure PI2025001214_DRAWING_003
Patent Text Reader

Abstract

Provided are an environmentally friendly chemical agent and a solid lubrication coating film. The chemical agent is used to form a solid lubrication coating film on a metal surface. The chemical agent contains a solid lubricant, a binder resin, and a solvent, as main components. The solvent contains water as a main component and a lower alcohol having three or fewer carbon atoms which is added as an additive to the water, and the additive has a volume of 0.5 or more and 45 or less in terms of 100 set as a volume of the water. The water and the additive account for 95% or more of the volume of the solvent. As the solid lubricant, at least a metal soap is contained, and a metal soap component accounts for 95% or more of a sum of total weights of metal soap and alkaline soap components. A condition that a particle size of the metal soap does not exceed a film thickness of the solid lubrication coating film is set. The binder resin is composed of a water-soluble or water-dispersible polymer and a copolymer, and a polymer having an acrylate or methacrylate structure and the copolymer account for 90% or more of a total weight of the binder resin.
Need to check novelty before this filing date? Find Prior Art

Description

Agent for forming solid lubricating coating, agent manufacturing method, agent application method, oil well tubular goods, and oil well tubular goods threaded joint

[0001] The present disclosure relates to an agent for forming a solid lubricant coating that imparts lubricity and corrosion resistance to metal surfaces, and to a technology using the agent. The present disclosure also relates to an agent that can simultaneously improve lubrication and prevent rust between two sliding objects made of metal surfaces, and to a solid lubricant coating formed thereby. The present disclosure primarily relates to a solid lubricant coating intended for the lubrication and rust prevention of oil country pipe threads. The present disclosure also aims to simultaneously achieve sufficient lubrication and rust prevention in the operating environment, even under actual make-up and make-back conditions in wells. The present disclosure also aims to enable rapid drying during film formation, including methods such as air drying, air blower drying, hot air blower drying, infrared irradiation, ultraviolet irradiation, and heat treatment.

[0002] At the same time, consider what happens when there is trouble in the well or during workover. Consider the case where the full-length pins are removed one by one or in groups of two or three and recovered near the well. In onshore wells, for example, the full-length pins are removed one by one. In offshore wells, for example, they are removed in groups of two or three. In this case, the oil well tubular goods are lined up and cleaned. The present disclosure is also intended to be utilized as a chemical agent applied to the thread surface for rust prevention protection, and as a coating formed by the agent.

[0003] Techniques similar to those disclosed herein include those described in Patent Documents 1 to 3, for example. Patent Document 1 exemplifies an example of a steel pipe threaded joint that is primarily made of an ultraviolet-curing resin film and has an acrylic / silicone surface layer. Patent Document 1 exemplifies an epoxy acrylic-based UV-curing resin, and while oil-based and water-based systems are also acceptable, it also clearly states that oil-based systems are preferred. In other words, it does not actively promote the use of water-based systems. Patent Document 1 also exemplifies a quick-drying lacquer-based acrylic / silicone surface film, and exemplifies one that contains metal soap as a solid lubricant.

[0004] Patent Document 2 is an example of an oil country pipe threaded joint in which a dry solid coating is further formed on a viscous liquid or semi-solid lubricating coating. It exemplifies the formation of either a water-soluble or water-dispersible polymer compound or an organic solvent-based composition in the dry lubricating coating. Patent Document 2 also exemplifies the use of a metal soap in a viscous liquid or semi-solid lubricating coating. However, Patent Document 2 is an example in which the metal soap is used as a thickener. It should be noted that Patent Document 2 does not aim to achieve the effect of the metal soap as a solid lubricant.

[0005] Patent Document 3 specifies a lubricating coating made of one or both of rosin and calcium fluoride, metal soap, wax, and basic aromatic organic acid metal salt. Examples of optional additives include thermoplastic resins and acrylic resins. Examples of solvents include those using volatile organic compounds.

[0006] Furthermore, examples of prior art that take into consideration tightening in actual wells include Patent Documents 4 and 5, and Non-Patent Document 1. Patent Document 4 describes using a vertical power tong and a 7" short pin to test the initial set at an angle of 6 degrees, assuming misalignment. Patent Document 5 is an example of a test evaluation using a vertical power tong and a 9-5 / 8" short pin to test and evaluate misalignment at 5 degrees. Non-Patent Document 1 is a paper that evaluates lubrication using a vertical power tong. Non-Patent Document 1 also describes placing a 5 kN weight on the tip of the short pin opposite the tightening side, that is, on the top end of the pin when tightening the pin upright.

[0007] JP 2016-028211 A JP 2008-537062 A Republished JP 2009-057754 A JP 2002-327874 A WO2017 / 110685

[0008] Tsutome et al.: Journal of the Japan Petroleum Technology Association, Vol. 61, No. 6 (1996), pp. 527-536. Kawamura Kasei Kogyo Co., Ltd., Solubility of Metal Soaps, Internet: <https: / / www.kawamura-kasei.co.jp / solubility_table.html>

[0009] This disclosure relates to an agent that simultaneously improves lubrication between two sliding objects and provides rust prevention, and to a solid lubricant coating realized thereby. This disclosure is primarily directed to a solid lubricant coating intended for lubrication and rust prevention of oil country tubular goods threads. This disclosure also aims to simultaneously achieve sufficient lubrication and rust prevention in the operating environment, even under actual well tightening and tightening conditions. To achieve these goals, this disclosure relates to an agent containing a water-soluble or water-dispersible polymer containing a component primarily composed of a metal soap as a solid lubricant. This disclosure also relates to a solid lubricant coating formed using this agent. Note that water-soluble or water-dispersible polymers are water-based polymers. The term "water-based polymer" as used herein refers to a polymer that has hydrophilic properties due to the inclusion of polar or charged functional groups in its structure. For example, this refers to a polymer containing a carboxyl group, an amine functional group, a sulfonic acid group, or the like in its main chain or side chain.

[0010] In contrast, the following problems have been encountered in the past. (1) There has been no idea of ​​a technology for mixing a metal soap into a water-based polymer solvent without using oils, ethers, or VOCs (volatile organic compounds), and without using chemicals known as thinners. Metal soaps are inherently thought to be insoluble in water and alcohol, so there has been no idea of ​​how to make them cloudy when mixed with water-based acrylic. (2) When alkaline soap is added to a water-based polymer, the soap dissolves in water. Therefore, when alkaline soap is added to a water-based polymer, the water solvent tends to become highly viscous and gelatinous. This has not been addressed in the past with respect to oil country tubular goods. (3) When chemicals using a water-based polymer and a water-based solvent are used, there is a high concern that they will take a long time to dry.

[0011] Here, among solvents other than water, volatile organic solvents such as xylene, toluene, and benzene must be avoided. These cannot be used in a no-open flame environment, and consideration must be given to the safety and health of workers, as well as the installation of drafts and other facilities. For this reason, it is preferable to avoid the use of VOCs (volatile organic compounds), especially the group of chemicals known as thinners. The methods exemplified in Patent Documents 1 to 3 use highly volatile VOCs and are not designed for use in a no-open flame environment, such as at a wellhead. For this reason, they cannot be used with oil well tubular goods.

[0012] It is also conceivable to use highly volatile but nonflammable fluorine-based solvents or fluorine-based binder resins to achieve rapid drying. However, these are practically unusable. Under the U.S. Toxic Substances Control Act (TSCA), the rule revision at the end of April 2021 will retroactively prohibit the use of all chemicals containing PFAS, even if they have previous permits or licenses. PFAS refers to fluorine-containing acrylic groups, including PFOS and PFOA. Furthermore, given the recent rise in environmental awareness, other countries may follow suit. Therefore, while methods other than fluorine-based or VOA cannot achieve rapid drying (i.e., immediate drying) for water-based polymers, it is preferable to achieve rapid drying within 30 minutes at room temperature. The rapid drying performance should preferably be within 15 minutes, and more preferably within 5 minutes. Furthermore, extreme conditions exist near oil and gas drilling sites, where open flames are strictly prohibited. Since neither heat treatment furnaces nor electricity can be used, it is necessary to assume an environment where the material is simply left in the open air. Therefore, it is not possible to imagine a process of removing the solvent by heat treatment at around 50-300°C at the wellhead. The UV-curable resin described in Patent Document 1 also requires equipment capable of irradiating UV rays at the wellhead. Therefore, Patent Document 1 requires equipment capable of doing so and facilities such as an electricity distribution system, which makes it difficult to say that it is feasible.

[0013] Factories that manufacture products with solid lubricant coatings on their surfaces are not in environments where open flames are strictly prohibited, such as wellheads. In these cases, it is easy to prepare drying enhancement equipment such as large fans, hot air dryers, heat treatment, infrared light, and ultraviolet light. When drying using such equipment designed to accelerate drying, it is preferable to dry within five minutes, preferably within three minutes, and even more preferably within one minute. To accommodate this without slowing down the conventional line speed, it is necessary to dry within the takt time of the production line.

[0014] (4) In response to the recent increase in environmental awareness, there is a need to design the system so as not to use heavy metals and a set of chemicals containing PFAS. However, this problem is thought to be solved automatically if the above-mentioned problem is solved. (5) The inventors have found that it is important to evaluate the lubrication performance of the solid lubricant coatings and chemicals disclosed herein using an evaluation method that is suited to the environment in which they will be used in an actual well, and to set upper and lower limits for the parameters. In other words, there is a problem in that conventional laboratory evaluations using short pins of about 1 m do not provide an evaluation method that is suited to actual use conditions.

[0015] For example, as in the methods shown in Patent Documents 4 and 5, even if a misalignment of 5 or 6 degrees is set and a make-up test is performed using a short pin, parameters that should be considered to be failing are erroneously judged as pass. As a result, the methods shown in Patent Documents 4 and 5 have the problem of not being able to verify the upper and lower limit specifications for parameters. Consider the case where a make-up / loosening test is performed using a short pin with a misalignment of 5 or 6 degrees. In this case, the inclination of the pin thread is mechanically determined by the incomplete thread portion of the box thread and the tapered portion at the tip of the pin thread. For this reason, the structure of the thread makes it difficult to set and insert the pin at a 5 or 6 degree inclination. Oil well pipe threads have a tapered thread structure, and their taper angle is approximately this level. However, it is structurally impossible for the pin to be inclined at this angle relative to the coupling. However, the threads can be simply placed without engaging each other. However, this does not affect the lubrication behavior. The only difference is the very initial setting position, and then it simply tightens along the screw taper.

[0016] Furthermore, the pin screw should be inserted and set along the taper of the screw. The inclination should exist due to the play between the threads when the screw is inserted. When inserting the pin screw into the box screw, it is structurally difficult to set a constant inclination of about 5 degrees. Due to the play between the threads, it is estimated that only an inclination of about 1 to 2 degrees can be set. In reality, even in this state, once the threads engage, the pin screw immediately straightens out. Therefore, even if the threads are barely engaging, a 5-degree inclination will cause minimal damage to the solid lubricant coating, and it is estimated that this cannot simulate actual well conditions.

[0017] Furthermore, the method described in Non-Patent Document 1, in which a 500 kN weight is placed on the pin screw to apply the load equivalent to a single actual pin, also presents problems for evaluation. As will be explained in detail in the following description of the invention, the initial setting position is important for simulating the rattle of the pin screw in an actual well. As shown in Figure 5 of Non-Patent Document 1, if the screw is manually tightened to a position where it can be tightened about half a turn, the weight acts as a balancer, resulting in a straight, ideal pin. Therefore, it is not possible to simulate the harsh conditions in an actual well, where the pin screw is tightened and retightened with rattle, based on the fact that the long pin is slightly bent in its elastic range. A harsh condition would be, for example, a condition similar to that of an actual well.

[0018] The inventors have found that unless the initial setting of the pin screw is intentionally set as follows and then tightened and tightened, it is impossible to estimate results that correspond to the conditions in an actual well or a simulated well. This setting involves exposing the pin screw from the box screw and placing a weight equivalent to one to three full-size pins on the end of the pin. It should be noted that, unlike lubrication using conventional viscous liquid compounds, evaluation results using a simple short pin tend to deviate from the results in an actual well. Specifically, the evaluation results tend to be too lenient. In other words, a pass rating in a test using a short pin does not necessarily mean a pass rating in an actual well. Therefore, in the case of solid lubricating coatings, unless proper lubrication evaluation is performed, the upper and lower limit specifications for parameters will not provide evidence that the lubrication will be tolerable in a well.

[0019] The present disclosure has been made in response to the above-mentioned problems, and aims to provide a solid lubricating coating that is environmentally friendly even when it is a water-soluble agent, using a water-soluble or water-dispersible polymer as the binder resin and a metal soap as the main solid lubricant, and that has lubrication properties that can withstand use in an actual well.

[0020] With regard to the lubrication of oil well pipe threads, growing environmental awareness has recently led to a trend toward limiting the chemicals and lubricant film components that can be used. Traditionally, the lubrication of oil well pipe threads has consisted of a combination of lubricating compounds containing harmful heavy metals and a surface treatment on the box thread side. The surface treatment, for example, consists of a manganese phosphate undercoat or an electroplated layer. However, the commonly used API-mod compounds, i.e., wet lubricants, have become difficult to use in environmentally conscious areas and regions. Specifically, API-mod compounds contain harmful heavy metals such as Pb and Zn as their main components. Therefore, there is a concern that harmful heavy metals may be washed away or overflow to the outside during tightening, resulting in marine pollution.

[0021] This disclosure employs a solid lubricant coating instead of these lubricating compounds. Furthermore, this disclosure employs a water-soluble or water-dispersible polymer as the binder resin for the solid lubricant coating. This aims to avoid the issue of harmful heavy metals leaking out. The chemicals used in this application for forming solid lubricants use water as the solvent, which is considered to be environmentally resistant. It is sufficient for the binder resin and solid lubricant to comply with international chemical regulations and rules. This will simultaneously achieve HSE and ensure the safety and health of workers. Replacing conventional lubrication of oil country pipe threads with a solid lubricant coating is also effective in resolving HSE issues. HSE stands for health, safety, and environment.

[0022] Furthermore, in many cases, the wet compounds used in conventional lubrication methods are different for lubrication and storage. Technology that replaces wet-compound lubrication methods with solid lubricating coatings must also ensure that dry films are used for rust prevention during storage. Furthermore, using conventional wet compounds to protect pin threads from rust is not particularly desirable, except in emergencies. In other words, we believe it is preferable for solid lubricating coatings to be designed as both a lubricating film and a coating that provides rust prevention during storage.

[0023] Furthermore, it is important to note that conventional lubricating and corrosion-resistant compounds are viscous liquids. Therefore, these compounds function while wet. In other words, there is no need to consider drying time for wet compounds. On the other hand, solid lubricating coatings are dry films that function in a dry state. Therefore, when forming a solid lubricating coating, the chemical design must take into account the process of evaporating the solvent from the applied coating and the time required for this. There are already existing technologies for designing dry, soft polymer-based resin films using chemicals with water-soluble or water-dispersible polymers as matrix components, particularly for use in surface lubrication of oil well pipe threaded joints. Furthermore, there are also existing technologies for solid lubricants that use metal soaps as the main component to achieve high lubrication.

[0024] However, there are no known solid lubricants in which metal soap is dispersed as the main component in a dry, soft polymer-based resin film formed using a simple water-soluble or water-dispersible polymer, which corresponds to a combination of these. The polymer-based resin film is a matrix component. It has traditionally been considered difficult to incorporate water-repellent, water-insoluble metal soaps into a water-based solvent alone, assuming that no oil or thinner is mixed in. While the idea of ​​using metal soaps as solid lubricants in a water-based solvent alone is not completely unheard of, it is difficult to achieve under the conditions targeted by this disclosure. Metal soaps are water-repellent, and even if you try to simply mix them with water, they float to the surface and do not disperse or dissolve.

[0025] This disclosure relates to a design in which a dry, soft polymer-based resin film is formed using a water-soluble or water-dispersible polymer, and a solid lubricant is dispersed and distributed within the film. Furthermore, this disclosure positions metal soap as the main component of the solid lubricant. Metal soap itself is water-repellent and insoluble in water. At the same time, metal soap itself is also said to be insoluble in alcohols. Substances in which metal soap itself is said to be slightly soluble are VOCs (volatile organic compounds), specifically, chemicals in the group known as thinners. However, these chemicals are often considered harmful to health and are often broadly referred to as thinners. These chemicals are classified as VOCs or ethers, such as toluene, xylene, benzene, and mineral spirits, as well as oils, such as those broadly known as mineral oils. This information is widely known and publicly available.

[0026] Therefore, it has been considered difficult to directly mix metal soaps with water-based polymers. Therefore, metal soaps have traditionally been dissolved in the VOCs listed above and then mixed with a water-based solvent. Methods using thinners or the like are described in, for example, Patent Documents 1 to 3. However, as will be described later, due to concerns about worker safety and the environment, and due to environmental considerations, this method is unlikely to be usable in places where open flames are strictly prohibited, such as in oil / gas drilling environments.

[0027] The present disclosure also contemplates the case where an alkaline soap is also dispersed. Here, the alkaline soap is either a sodium salt or a potassium salt of a fatty acid, or both. Hereinafter, the alkaline soap will also be referred to simply as soap. Rather, the present disclosure contemplates the use of a small amount of alkaline soap to assist and reinforce lubrication. To reiterate, the present disclosure is designed such that a water-soluble or water-dispersible polymer forms a dry, soft polymer-based resin film, and a solid lubricant is dispersed and distributed within the film.

[0028] Unlike metal soaps, soaps are soluble in water. Therefore, alkaline soaps have the disadvantage of being difficult to use with the chemicals and solid lubricant coatings considered in this disclosure. Furthermore, there have been few examples of their application to date. When a water-based polymer is designed with a certain amount of alkaline soap added, the entire liquid gels and solidifies. This results in increased fluidity, which is characteristic of water-based systems. This means that the easy-to-apply feature disappears and quick drying tends to be difficult. Meanwhile, there are many soap-based lubricants available commercially, even for industrial use, that are used while wet. However, these lubricants utilize the lubrication in a hard gel state without drying. Therefore, this technology is different from that of the present disclosure.

[0029] As mentioned above, conventionally, water-based polymers refer to polymers that use water as a solvent, and the water component must be dried and removed before film formation. Water-based polymers are either water-soluble or water-dispersible. Because water is the solvent, water-based polymers require heating of the coated object. Alternatively, the target area can be heated before application. In either case, without a process to promote water evaporation, the coated product must remain in the production plant until it dries. This significantly reduces production efficiency. In other words, drying in the air requires a significant drying time, necessitating the securing of a drying space. Therefore, unless a method is found to rapidly dry water-based polymers, production efficiency declines, resulting in higher production costs. In other words, rapid drying requires the use of drying equipment and heat treatment furnaces. However, this leads to increased installation and running costs.

[0030] On the other hand, a technique for quickly drying a water-based polymer by adding a volatile organic solvent and effectively utilizing the volatile heat generated to form a film is also known. Patent Document 1 states that since the acrylic silicone surface film becomes a dry film at a relatively low temperature in a short time, it is advisable to select an oil-based film, and that it is particularly preferable to use a room temperature curing type. In other words, Patent Document 1 is an example of using the evaporation of an oil-based solvent to achieve rapid drying without selecting a water-based system.

[0031] Patent Document 2 exemplifies a purely water-based system, a system of water and a volatile organic solvent, and a system using an ultraviolet-curable resin. Of these three, the latter two are capable of rapid drying. However, the first, a purely water-based polymer system, requires some method for evaporating the water. However, Patent Document 2 does not explicitly state how this method should be done.

[0032] Patent Document 3 discloses a method for shortening drying time by using a volatile solvent with a flash point of 30°C or higher. However, in hot regions such as desert regions in midsummer, a flash point of around 30°C raises concerns that a spark or other risk factor could ignite the wellhead. Furthermore, even if the material is processed in a workshop some distance from the well, the risk of ignition cannot be ruled out. Thus, materials with low flash points pose a high risk of fire and other accidents unless used in a well-controlled environment. In other words, there has traditionally been a challenge in how to achieve safe and rapid drying. Materials with low flash points are easily flammable.

[0033] In contrast, the present disclosure uses a solid lubricating coating primarily composed of a water-soluble or water-dispersible polymer. To speed up the drying of aqueous solvents, it is conceivable to use VOCs (volatile organic compounds), particularly thinners, to take advantage of their volatility. However, due to VOC emission control regulations and to avoid placing workers in a harsh environment, the inventors have determined that the use of toluene, xylene, benzene, and other organic solvents, no matter how volatile they are and how effective they are in speeding up drying, should be avoided. Even providing an exhaust system would require significant capital investment. Furthermore, when forming a solid lubricating coating, it is difficult to use volatile organic solvents, which are harmful to the body, as chemicals. Therefore, the inventors have determined that the use of VOCs (volatile organic compounds) and thinners, which are both harmful to health and too volatile, is not possible to achieve rapid drying. Furthermore, there has been a recent trend toward discouraging the use of fluorine-based solvents, which are inherently fast-drying, and fluorine-based resins, which can be dissolved in them to form binder resin components in paints. Fluorine-based solvents are substitutes for fluorocarbons.

[0034] Traditionally, fluorine compounds have been treated as the king of surface treatments due to their quick drying properties, excellent lubrication and corrosion prevention. However, due to the recent tightening of rules, fluorine compounds are becoming unusable. The US TSCA (Toxic Substances Control Act) and the European REACH chemical agent regulations prohibit the use of fluorine-based alkyl compounds (F-(CF 2 ) nUntil now, only PFOS (perfluorooctanesulfonic acid) and PFOA (perfluorooctanoic acid) were subject to restrictions (chemical species containing 8 carbon atoms). Substances with fewer carbon atoms were usable without any particular issues. However, the April 2021 revision of the U.S. TSCA retroactively banned the import, use, and production of PFAS (organic fluorine compounds: perfluoroalkyl and polyfluoroalkyl compounds) into the U.S. This means that binder resins containing fluorine compounds (PFAS) are no longer usable. In other words, the only fluorine-containing chemicals and products that can be used are Teflon® (PTFE: polytetrafluoroethylene) and PFPE (perfluoropolyether), which are exempt from TSCA. Furthermore, the international trend toward designing solid lubricant coatings without using fluorine can no longer be ignored.

[0035] Based on the above, this disclosure proposes an environmentally friendly approach to using water as a solvent, making the binder resin water-soluble, and then combining it with appropriate solid lubricants and other additives to form a solid lubricant coating. However, water as a solvent is difficult to volatilize, and evaporation takes time. Furthermore, drying requires large-scale capital investment, such as a heat treatment furnace, and other issues remain.

[0036] Furthermore, when applying a solid lubricant coating to the threads of oil country tubular goods (OCTG), the tubular goods are produced and transported away from the oil / gas wells. Therefore, when creating a solid lubricant coating based on a water-soluble or water-dispersible polymer at the production site, it may seem that all issues related to quick drying or rapid drying can be addressed. In other words, because water-based polymers are difficult to dry, measures may be taken, such as creating equipment to dry them slowly or using heat treatment equipment to accelerate drying. In this case, if heat treatment equipment is not used, adding a volatile organic solvent to accelerate drying may be considered. Furthermore, in many cases, this can be achieved by providing an exhaust system and taking measures to prevent ignition.

[0037] However, when solid lubricant coating agents and the solid lubricant coatings formed using them are used on OCTG threaded joints, and the OCTG threaded joints are then used in wells, the following issues arise. Specifically, solid lubricant coatings are not necessarily manufactured or formed exclusively at production sites far from the well. When considering potential problems with the lubricant coatings formed on OCTG, it is necessary to consider the possibility of using the agents for forming solid lubricant coatings at the wellhead. Open flames are strictly prohibited at the wellhead, and there are also situations where the footing is not stable. Furthermore, when applying water-soluble or water-dispersible polymers at the wellhead, they must dry quickly.

[0038] This is because, when a well malfunctions, tubing threads are often pulled up from the well in groups of one to three, often while being tightened. In this case, the pulled pins (oil well pipes) must be lined up side by side, their surfaces cleaned with water or steam, and then coated with a similar anti-corrosion coating. In contrast, conventional OCTG thread techniques do not involve the application of wet lubricating compounds containing Pb and Zn, such as API-mod compounds, but rather the application of a compound known as a wet storage compound. In contrast, in the case of solid lubricating coatings, unlike wet compounds, a fast-drying solid coating base must be formed at the wellhead in order to achieve complete application using solid lubricating coating technology alone. However, open flames are strictly prohibited at the wellhead. The use of organic solvents with low flash points and good volatility, which promote fast drying, is not permitted due to their danger.

[0039] The descriptions in Patent Documents 1 to 3 are examples, but in all of these, highly volatile organic solvents with low or likely low flash points have been used to quickly form a film. Furthermore, it is believed that the chemicals are designed on the assumption that oil country tubular goods are produced and transported away from oil / gas wells. Chemicals based on low flash points are extremely dangerous to use near oil / gas wells, where open flames are strictly prohibited. This disclosure provides a chemical that minimizes the use of highly volatile organic solvents.

[0040] Furthermore, the inventors do not intend to address the corrosion resistance and lubrication issues addressed in this disclosure at a level that can be evaluated simply through simple laboratory experiments or simulations, as is often done on a daily basis. The inventors have examined conventional laboratory tests and found that they must be designed to withstand the most severe conditions imaginable. In this disclosure, corrosion resistance is not limited to corrosion protection in the as-deposited state, but rather assumes a situation in which the solid lubricant coating is damaged. It is assumed that corrosion resistance must be maintained after the solid lubricant coating surface of an oil country pipe thread is tightened and loosened with a protector under the most severe conditions imaginable. In other words, this disclosure assumes that corrosion resistance must be maintained even when the solid lubricant coating is damaged by contact with a protector.

[0041] At the same time, this disclosure assumes that good lubricity must be guaranteed under sliding conditions involving high loads. When considering actual wells, it is necessary to assume that a certain amount of solid lubricant coating will inevitably be scraped off during make-up and tightening. The inventors have discovered that the scraped-off debris can cause seizure problems in the following cases: when it gets stuck in the gap between the box thread or pin thread, or when a high or uneven load is applied to the joint, causing part of the film to be completely torn off. Furthermore, they have discovered that unless upper and lower limits for the components of the solid lubricant coating are set by simulating conditions in an actual well or similar to those in a well, the specifications for lubrication performance will be meaningless in an actual well.

[0042] A commonly used test is a laboratory make-up test using a short pin of approximately 1 m. In this test, a NG result for the lubrication of solid lubricant coatings, which is the subject of this disclosure, also results in a NG result in an actual well. However, the inventors have learned that even if a test using a short pin of approximately 1 m results in a pass, this does not guarantee that the result will be passable in an actual well. However, the ranges specified for the lubrication performance of solid lubricant coatings in past patent documents are rarely specified with such considerations in mind. In the case of viscous liquid lubricating compounds commonly used to lubricate conventional oil well pipe threads, there is little difference between laboratory make-up and remake evaluations using a short pin and actual well conditions. Furthermore, actual well results tend to correlate with laboratory evaluations. This is because the lubricating compound is a viscous liquid, and it is assumed that the compound moves in tandem during make-up and remake.

[0043] On the other hand, in the case of solid lubricating coatings, the debris that is inevitably scraped off does not necessarily move in conjunction with tightening and loosening. For this reason, in actual wells where debris is inevitably generated in large amounts, the debris is likely to clog the well. Furthermore, when significant peeling occurs, seizure occurs in areas where the solid lubricating coating has become thin or has disappeared. Based on this knowledge, the inventors have come to the realization that solid lubricating coatings must be evaluated taking this into account.

[0044] This finding will be explained in more detail. In actual wells, the situation in which a full-length pin thread is tightened into a box thread is not idealized as described in textbooks. In an ideal situation, one would imagine a full-length pin standing upright in the box thread, inserted and set, and then tightened straight. However, this is not the case in reality. The structure of OCTG threads has an incomplete thread portion when the pin thread is inserted into the box thread in an inserting manner. This backlash (play, allowance) often causes the pin to be set slightly at an angle during initial setting. When the threads are first tightened, the pin threads move around freely due to the play. Therefore, by the time the threads engage, the solid lubricant coating is subjected to a combination of the large load of the pin's own weight and the unbalanced load caused by the pin's uneven movement. This inevitably increases the risk of the solid lubricant coating being abnormally scraped off or completely peeled off. On the other hand, wet lubricating compounds are viscous liquid lubricants that move in conjunction with the tightening and un-tightening of the well, which is in stark contrast to the fact that the results of lubrication evaluation in the lab using a short pin are nearly identical to those in an actual well.

[0045] This is specifically shown in Figures 2 and 3. The examples shown in Figures 2 and 3 are examples where the tightening and tightening test conditions were 15 to 25 rpm until torque was reached, and then 2.5 to 1.5 rpm after torque was reached. This is the result of testing under strict conditions, i.e., at a high rotation speed, that exceed the conditions specified in the screw handling instructions, i.e., the tightening instructions in the technical package. The examples shown in Figures 2 and 3 are examples where the well tightening material and strength grade are 9-5 / 8" 53.5# Q125 material, with JFELION TM This is an example of evaluation of a solid lubricant coating on a screw.

[0046] Figure 2 shows a torque turn chart based on a conventional laboratory evaluation method using a short pin of approximately 1 m and tightened with vertical power tongs. Because the pin is short, handling is not difficult and the pin can be set straight. Therefore, the pin can be set by hand until the pin threads are barely exposed (Figure 2(b)). In this case, the torque turn chart shows that torque begins to build up from the beginning of tightening, and the tightening is completed after the shoulder torque bending point has been exceeded. In other words, this results in a very typical chart (Figure 2(a)). The reason the torque builds up so quickly is because the pin thread and box thread are fully engaged during the initial setting stage and tightening is performed from a preset position.

[0047] On the other hand, Figure 3 shows the torque-turn chart for Range-3, using a single full-scale pin just over 40 feet (just over 12 m). Figure 3 also shows the results of a test conducted in a simulated well. The units (size) on the horizontal axis are different from those in Figure 2. Note that the simulated well is not an actual oil and gas producing well, but an experimental well with a simulated hole drilled so that just over three full-scale pins can be inserted underground. The simulated well also refers to a laboratory facility with a rig above which two or three connected pins can be suspended and set, allowing for tightening and tightening tests. This example shows the trend under conditions similar to those observed in an actual well, but differs from the case of the short-length pin shown in Figure 2. In this example, steady torque does not develop until approximately 6.3 rotations, and irregular spikes of torque are occasionally observed during this rotation. The inventors have discovered that this phenomenon is directly linked to damage to the solid lubricant coating, and that this fact suggests the importance of evaluating the solid lubricant coating.

[0048] The torque chart example in Figure 3 shows what happens when setting and tightening a Range-3 pin, or a pin just over 40 feet (just over 12 m). In this case, because the actual pin is approximately 12 m, it cannot be set perfectly straight and is almost always inserted at an angle. This is similar to the condition in a real well. As a result, even when setting the pin by hand, the pin thread and the box thread will partially butt up too tightly. As a result, when tightening by hand, five or more threads on the pin, often about half of the total threads, will be exposed from the box, preventing further advancement. From this state, tightening with tongs begins. In most cases, the threads are not fully engaged, and some parts are inadvertently butt up too tightly, preventing further advancement. As a result, with actual-size pins, the box thread and the pin thread will butt up under uneven loads before they are fully engaged. In other words, this means damaging each other. With this in mind, we have come to the realization that, without evaluating solid lubricant coatings, as already mentioned above, a simple "NG" result in an evaluation using a short pin means an "NG" result in an actual well, but an "OK" result in an evaluation using a short pin does not necessarily mean an "OK" result in an actual well. For this reason, we have come to the realization that in previous inventions, evaluations based on "OK" results in an evaluation using a short pin, in terms of upper and lower limits for components, conditions, and other parameters, do not necessarily indicate a satisfactory range in an actual well. Here, the methods of Patent Documents 4 and 5 are examples of test evaluations using a short pin, and do not necessarily indicate a satisfactory range.

[0049] Furthermore, in Non-Patent Document 1, lubrication is evaluated by placing a 5 kN weight on the top end of the pin when tightening it upright. Here, judging from the torque turn chart for a 7"29# pin, Non-Patent Document 1 appears to be intending to apply the weight of one actual length pin, that is, a pin of approximately 40 feet (approximately 12 m). However, judging from the torque turn chart, i.e., Fig. 5 in Non-Patent Document 1, it appears to be premised on conducting the test with a tightening behavior closer to that of Fig. 2 rather than that of Fig. 3. In other words, Non-Patent Document 1 appears to be premised on conducting the tightening test from a state in which the initial set position is tightened by hand to a level where the pin thread is not exposed and the pin thread and box thread are sufficiently engaged. For this reason, it is not necessarily possible to determine a favorable range.

[0050] From the above, the problems that can be extracted from the present disclosure are described below. This disclosure is based on the premise that oils and volatile organic solvents such as thinners are not used. Based on this premise, this disclosure considers creating a chemical agent by dispersing solid lubricant components, primarily metal soap, in a binder resin made of a water-soluble or water-dispersible polymer. It also considers using this chemical agent to create a corrosion-resistant lubricating film made of a solid lubricant coating. It has been discovered that such a configuration has the following problems. For this reason, it has been discovered that further ingenuity is needed.

[0051] (First issue) This is an issue when mixing metal soap into water-based polymers. That is, when mixing water-insoluble metal soap, it is necessary to devise a way to make it cloudy without using oils or volatile organic compounds, and moreover, without using a group of chemicals called thinners.

[0052] (Second problem) When alkaline soap is added to a water-based polymer, the solvent tends to become viscous and gelatinous because the alkaline soap dissolves in water. Therefore, even if the alkaline soap is intended to provide lubrication, it may take a long time to form a film when the alkaline soap is added to a water-based polymer. At the same time, it is necessary to specify the appropriate amount of alkaline soap to form a dry solid lubricating coating.

[0053] (Third Issue) Because a water-based polymer is used and water is the solvent, there is a high concern that drying after application will take a long time. Therefore, some kind of ingenuity is needed to achieve rapid drying, which is an issue. Essentially, it is preferable to have a coating that can be applied anywhere and dry quickly. In extreme situations, such as in an open-fire environment, neither heat treatment furnaces nor electricity can be used, and the coating may simply be left exposed to the air. However, this disclosure anticipates that this solid lubricant coating and chemicals can be used not only at oil country tubular goods manufacturing sites but also at wellheads. Therefore, to improve quick-drying performance, it is necessary to avoid the use of thinner-based VOCs at wellheads where open flames are strictly prohibited. At the same time, consideration must be given to the safety and health of workers, including the installation of drafts, etc. Therefore, it is necessary to design solid lubricant coatings and chemicals with the assumption that the use of thinner-based VOCs should be avoided.

[0054] (Fourth Issue) In response to the recent increase in environmental awareness, it is necessary to avoid the use of a set of chemicals containing heavy metals and PFAS (fluorine-containing acrylic groups, including PFOS and PFOA). PFAS is a fluorine-containing acrylic group, including PFOS and PFOA.

[0055] (Fifth Problem) It is important to evaluate the feasibility of lubrication and other properties of the solid lubricant coatings and chemicals disclosed herein using an evaluation method suited to the environment in which they will be used in an actual well, and to set upper and lower limits for parameters. However, conventional evaluation methods using short pins of about 1 m do not provide an evaluation method suited to actual usage conditions.

[0056] The means for solving each problem in this disclosure are described below. The present disclosure relates to a chemical agent in which a water-soluble or water-dispersible polymer, i.e., a water-based polymer, is used as the binder resin, a metal soap is used as the main component of the solid lubricant, and water is used as the main component of the solvent. It also relates to a solid lubricant coating formed by this chemical agent. The metal soap functions as a water-repellent solid lubricant. Water-repellent means that the agent is not soluble in water. Assuming that the metal soap can be successfully formulated in the chemical agent, it is considered that good lubricity, corrosion resistance, quick drying, and other properties can be achieved within the ranges specified in this disclosure. In order to solve the above problems, the present disclosure defines the following solutions and constitutes an invention.

[0057] The solution to the first problem involves a technique for effectively mixing metal soap with water as a solvent. Metal soaps are generally described as insoluble in both water and alcohol, and are said to dissolve in thinner-based volatile organic solvents, ether-based solvents, and oil-based solvents. For example, Non-Patent Document 2 clearly states that metal soaps are insoluble in ethyl alcohol, methyl alcohol, and butyl alcohol. In other words, metal soaps can be dissolved by selecting water as the solvent, using a VOC that is easily volatile even at room temperature, and using a thinner-based solvent that requires workers to wear special masks or draft equipment. However, until now, it has been thought that there was no solution for dissolving metal soap in water unless such substances were used. Furthermore, considering the lubrication of oil well pipe threads and the application of chemicals at the wellhead, the use of thinner-based solvents is strictly prohibited in wellhead environments where open flames are strictly prohibited. Although thinner-based solvents are solvents that do not leave a residue on the formed film, they cannot be used.

[0058] The inventors conducted an experiment to investigate mixing a water-insoluble metal soap with a water-soluble or water-dispersible polymer, i.e., water, which is a solvent for water-based polymers. During the experiment, they noticed that although the metal soap is insoluble in both water and ethanol, when actually dissolved, the dispersibility of the metal soap differs when compared with water and lower alcohols such as ethanol.

[0059] Specifically, they found that in lower alcohols such as ethanol, metal soaps tend to be less likely to clump and more likely to form fine particles, allowing them to remain in fine particle form. After mixing the metal soap with alcohol, they can be stirred vigorously or vibrated with ultrasound. On the other hand, in water, the metal soaps aggregate and grow into clumps, preventing them from becoming uniformly dispersed. From this, they discovered that by first dissolving the metal soap in lower alcohols such as ethanol, it is possible to disperse the metal soap, albeit in an insoluble state. They then discovered that by spreading it in a water-based polymer and mixing it, they could approach a homogeneous drug.

[0060] When the agent disclosed herein is left standing, the metal soap separates over time. However, if the container containing the agent disclosed herein is shaken or otherwise re-mixed before application, and the solvent water is evaporated after application, a homogeneous solid lubricating coating is formed. Furthermore, if the metal soap is directly dissolved in water, the metal soap tends to clump, raising concerns that the resulting solid lubricating coating will be inhomogeneous.

[0061] The reasons for this are not entirely clear. Qualitatively, water is simply a polar solvent. On the other hand, lower alcohols such as ethanol tend to dissolve in water and also slightly dissolve in oil. Metal soaps are insoluble in water, but are generally described as insoluble in alcohol as well. However, metal soaps can dissolve in oil and VOCs such as paint thinners. Therefore, it is presumed that the level of insolubility is likely to be responsible for the differences in phenomena described above, as there are differences at the molecular level.

[0062] On the other hand, lower alcohols such as ethanol are also highly volatile and fall into the VOC category. Therefore, there is a concern that they may be flammable in environments where open flames are strictly prohibited. For this reason, it is necessary to specify upper limits for the amount of lower alcohol that can be used to dissolve the above-mentioned metal soap and its concentration in the agent. From this perspective, the present disclosure specifies an upper limit for the amount of lower alcohol. Furthermore, the more metal soap dissolved, the better for use as a solid lubricant. However, the upper limit for the amount of metal soap that can be dissolved is determined by the alcohol dissolving limit, as well as the volatility and flash point. The lower limit for the metal soap is determined by the minimum amount at which lubrication can be achieved.

[0063] The second issue is how to mix in a small amount of alkaline soap to support lubrication. That is, how to mix a small amount of alkaline soap into a system that uses a water-based polymer as the binder resin, a metal soap as the main component of the solid lubricant, and water as the solvent, without adding VOCs such as thinner.

[0064] Alkaline soap dissolves in water, making it easy to incorporate. However, if too much alkaline soap is incorporated, the water solvent tends to become viscous and gelatinous. This makes the applied agent slow to dry and takes a long time to dry as a solid film. Even when it dries, it becomes a semi-solid, highly viscous film. A semi-solid to viscoelastic film leaves a sticky surface, making it prone to adhesion of dirt and sand. Once dirt and other debris are attached, they become difficult to remove. This creates resistance during tightening and loosening, potentially preventing the necessary lubrication. Therefore, to support the solid lubrication effect by the inclusion of alkaline soap and avoid changing the viscosity of the water solvent, it is necessary to add a small amount of alkaline soap and set an upper limit. From this perspective, the present disclosure specifies the amount of alkaline soap to be added.

[0065] The third issue is that because water-based polymers use water as a solvent, drying may take a long time after application. In this disclosure, adding large amounts of VOCs and using their volatility to evaporate water is not adopted, considering environments where open flames are strictly prohibited. Toluene, xylene, and benzene-based VOCs, commonly known as thinners, cannot be used, taking into consideration the health and safety of workers. Furthermore, it is necessary to safely dry the film, even in environments where electric heaters cannot be used or where the film will dry and form simply by being left outdoors in the local environment.

[0066] In the present disclosure, the lower alcohols mentioned in the first problem, i.e., alcohols such as ethanol, methanol, isopropyl alcohol, normal propyl alcohol, and industrial ethanol, are used to dissolve the metal soap. As described above, they can be formulated within a range that allows for compatibility with open flame environments without causing any problems due to their volatility and flash point. To enable compatibility with open flame environments, the flash point of the agent must be 60°C or higher, preferably 150°C or higher, and more preferably 250°C or higher. Under these conditions, an excess of lower alcohols is added beyond that required to dissolve the metal soap, thereby utilizing their volatility. However, the higher the flash point, the lower the amount or content of alcohol added. However, it is preferable to include at least 0.5% of lower alcohols.

[0067] At the same time, the addition of ammonia water and its volatility may be utilized. Ammonia water may also be used to adjust the pH of paint. When used for pH adjustment, additional ammonia water is added to the formulation to shift the pH toward the upper limit of the specified pH of the agent, i.e., toward the high pH side. Furthermore, if no pH adjustment is specified, ammonia water (28-30%) may be added up to 1% vol / vol% relative to the water solvent to promote volatility. In this disclosure, experiments were conducted to clarify the conditions for simultaneous use of ethanol and ammonia and to clarify the optimal range. Ammonia water is commercially available in dilute concentrations such as 10% and 5%. However, this disclosure will be discussed based on concentrated ammonia water (28-30%).

[0068] At the same time, in this disclosure, a small particle size of the metal soap is selected. Then, by dispersing the metal soap in the agent to prevent aggregation, the contact surface area of ​​the metal soap is increased, realizing rapid drying. The average particle size of the metal soap is 10 μm or less, preferably 5 μm or less, and more preferably 1 μm or less, to promote drying of the applied agent. Furthermore, to disperse and mix these into the agent, the agent is prepared by dissolving them in a lower alcohol such as ethanol, as explained in the response to the first problem. Adjusting the viscosity of the agent is also important. It is also important to lower the viscosity to create a thin application situation and make it difficult to apply thickly.

[0069] If the agent is applied to the metal surface of a cylinder while rotating the cylinder, excess agent will inevitably drip off from the 6 o'clock position, i.e., the lowest position. Similarly, if the cylinder is not rotated, the excess agent will inevitably drip off from the 6 o'clock position, although the 6 o'clock position tends to be applied somewhat thickly. Even when applying to a plate-shaped object, if the object is placed at an angle, excess agent will drip off under its own weight. This creates conditions that facilitate rapid drying. Therefore, to achieve rapid drying, the following conditions must be met to ensure rapid drying, even when the coated metal surface is left indoors or outdoors in an atmospheric environment. These conditions are a combination of the use of the aforementioned alcohol and ammonia, selecting the particle size of the metal soap to prevent the metal soap from aggregating and clumping, and adjusting the viscosity of the agent to prevent thick application.

[0070] The fourth problem is a method for designing a system that does not use heavy metals and a set of chemicals containing PFAS. PFAS refers to fluorine-containing acrylic groups, including PFOS and PFOA. In contrast, the present disclosure is constructed using a water-based polymer that does not use harmful substances, so by implementing solutions to the above problems 1 to 3, the system can be automatically solved. The fifth problem is the need to define upper and lower limits for each material by evaluating the properties of this lubricating and anticorrosive film using appropriate evaluation methods.

[0071] First, the corrosion resistance and corrosion prevention properties of this disclosure are based on the most stringent conditions, assuming the lubrication of oil country pipe threaded joints. Simply evaluating the corrosion resistance of a film applied to a plate or the lubrication behavior using a short pin may result in NG results, but it cannot be said to be a pass. In this disclosure, corrosion resistance is not based solely on the corrosion resistance of a film formed by applying a chemical agent; in other words, it is necessary to assume that when tightening with a protector, partial contact between the film and the protector will occur, causing damage to the film.

[0072] Regarding lubrication, in actual wells, a Range-3 full-length pin, i.e., a pin of about 40 feet (about 12 m) is set up and then hung and tightened by a derrick crane, etc. In the worst case scenario, the entire weight of the full-length pin may be applied to the box screw side. 3(b)。 English: Incidentally, one 9-5 / 8" 53.8# piece is equivalent to about one ton. Because of this large load, it is necessary to consider the possibility of significant damage to the solid lubricant coating. Regarding the initial setting position of a full-length pin, unlike short pins, it is assumed that the pin cannot be set until almost all of its threads are hidden by the box threads. In other words, it is necessary to evaluate lubrication by assuming a situation where the threads cannot be advanced any further, that is, a situation where the pin can only be tightened up to the position where the threads are exposed. For example, in an actual well, the pin threads can only be set to a position equivalent to the symbol 1a (10) in Figure 3(b). However, evaluating the solid lubrication behavior of OCTG threads in an actual well or a simulated well is not realistic from the standpoint of cost and the time required to arrange experiments.

[0073] The solution to this problem is as follows: A weight equivalent to one to three full-length pins is attached to the upper end of the short pin. Furthermore, the initial setting position of the screw is set to a position where approximately half of the pin thread is exposed from the box screw. This allows a weight to be applied during tightening and not during tightening, simulating tightening in an actual well and determining the upper and lower parameter limits in accordance with actual conditions. That is, in this disclosure, the initial setting position of the pin screw is intentionally set to a position where the pin thread is exposed from the box screw. Furthermore, in this disclosure, weights equivalent to one to three full-length pins are placed on the end of the pin, and tightening and tightening are performed for evaluation. During tightening, weights equivalent to one to three full-length pins are applied. Note that the weight equivalent to one pin is intended for onshore wells, and the weight equivalent to three pins is intended for offshore wells. During tightening, the weight is suspended by an overhead crane to adjust the load, and tightening is performed with reduced loads, including zero load. If the weight is left on during tightening, the weight acts as a balancer, causing the pin to rise straight up without rattling. This results in the solid lubricant coating not being damaged at all on either the box screw or the pin thread, which means that the simulation does not mimic what happens in an actual well.

[0074] The agent disclosed herein is an agent in which the main component of the solid lubricant is a metal soap, the main component of the binder resin is a water-soluble or water-dispersible polymer, and the main component of the solvent is water. While based on the above-mentioned configuration, the agent disclosed herein can provide an environmentally friendly agent that does not use a group of agents known as thinners, heavy metals, or a set of agents including PFAS. Furthermore, the agent disclosed herein can achieve rapid drying without the use of a group of agents known as thinners. Therefore, it can be used even in environments where open flames are strictly prohibited. PFAS refers to a fluorine-containing acrylic group, including PFOS and PFOA. Furthermore, the agent disclosed herein can provide a solid lubricant coating with lubricity and corrosion resistance that can withstand use in actual wells.

[0075] 7 is a diagram showing an oil country pipe and an oil country pipe threaded joint. FIG. 7(a) is a diagram of a tightening chart in a conventional laboratory test, and FIG. 7(b) is a diagram showing the initial set position at that time. FIG. 7(a) is a diagram of a tightening chart in an actual well, and FIG. 7(b) is a diagram showing the initial set position at that time. Schematic diagrams of tightening charts, where (a) is for an actual well and (b) is for a conventional laboratory test. FIG. 7(b) is a diagram explaining new laboratory test conditions (weight tongs). FIG. 7(b) is a diagram showing an example of weight placement under new laboratory test conditions (weight tongs). FIG. 7(c) is a diagram illustrating the state of setting of a pin screw and a box screw. Threads and the like are omitted in FIG. 7. FIG. 7(d) is a diagram showing an example of a method of applying paint to a pipe using a brush.

[0076] This disclosure relates to a solid lubricating coating and an agent for forming the same, which is formed on one or both sides of a lubrication surface, for example, when two opposing objects made of the same metal are required to slide against each other with high lubrication. This disclosure is particularly directed to a solid lubricating coating and an agent for forming the same in the lubrication of thread profiles, and further to the lubrication of oil country tubular goods threads.

[0077] In addition, this disclosure intends to simultaneously provide corrosion protection through the lubricating film. This disclosure intends to achieve sufficient lubrication of threaded parts even under actual tightening and tightening conditions in oil and natural gas wells. This disclosure employs a solid lubricant component primarily composed of metal soap, with a water-soluble or water-dispersible polymer as the binder resin. Furthermore, when applying the agent and forming it into a solid lubricating coating, instant drying, such as drying from the applied surface, is not expected. However, this disclosure aims to achieve rapid drying, such as drying in about 30 minutes when left to dry in the air after application.

[0078] The present disclosure provides a protective coating for corrosion prevention by covering the threads with a soft film. Furthermore, the present disclosure aims to achieve lubrication using this soft film, which also functions as a lubricating film. The present disclosure also contemplates a chemical agent for creating such a film. This disclosure focuses on environmental resistance and compliance with international chemical regulations, and was designed to be easy to use, including quick drying. The chemical agent of the present disclosure is also intended for use in the event of well trouble or workover. The chemical agent of the present disclosure is also intended to be used when full-length pins are removed one by one or in groups of two or three, collected near the well, lined up, and cleaned, and then formed as a protective coating on the thread surface for corrosion prevention. Removing full-length pins one by one is intended for onshore wells, while removing them in groups of two or three is intended for offshore wells.

[0079] Next, an embodiment of the present invention will be described. In this embodiment, an oil well tubular good is assumed as a metal part having a surface to which lubrication performance is imparted. However, the present invention may be applied to other metal parts.

[0080] (Configuration) <Chemical Agent> The chemical agent of this embodiment is an agent for imparting lubrication performance and corrosion resistance to the metal surface of a metal part such as an oil country tubular good. The chemical agent is composed of a solid lubricant, a binder resin, and a solvent component, and may contain small amounts of additive components depending on the situation.

[0081] [Solvent Component] The solvent component is primarily composed of water. A lower alcohol having 3 or less carbon atoms is added to the water as an additive. The volume of the additive relative to the water is 0.5 to 45 parts by volume per 100 parts by volume of water. One of the characteristics of the composition of the solvent disclosed herein is that 95% or more of the volume of the solvent is composed of the water and the lower alcohol, making it a component system primarily composed of water. The lower alcohol is, for example, one or more lower alcohols selected from methanol, ethanol, isopropyl alcohol, normal propyl alcohol, and industrial ethanol.

[0082] The additive may further contain at least one of aqueous ammonia and a primary amine. The content of at least one of aqueous ammonia and a primary amine is, for example, 2 parts by volume or less per 100 parts by volume of water. The addition of the lower alcohol, aqueous ammonia, and primary amine is intended to utilize their volatility to promote rapid drying of the coating. At the same time, the lower alcohol functions as follows in the solvent of the present disclosure, which is characterized by its water-solubility, i.e., in a solvent mainly composed of water. That is, when dissolving a solid lubricant, the lower alcohol functions effectively when dissolving a water-repellent solid lubricant. The lower alcohol also helps to dissolve and disperse the solid lubricant throughout the solvent, avoiding extreme association.

[0083] If the lower alcohol with 3 or less carbon atoms is not added in a ratio of 0.5 or more per 100 parts by volume of water, the water-repellent solid lubricant will not be uniformly dispersed and will phase separate from the water. In many cases, the lower alcohol will remain on the water surface. On the other hand, lower alcohols have low flash points. Consider a situation where lower alcohols are used to lubricate oil well pipe threads and are applied at the wellhead in an environment where open flames are strictly prohibited. In this case, there is a concern that lower alcohols could cause fires and become extremely dangerous chemicals. Therefore, the upper limit for the amount of lower alcohol added is set at 45 parts.

[0084] The solid lubricating coating formed by drying does not contain any solvent components, including lower alcohols. The solvent components only affect the drying time of the agent. Therefore, unless the environment is open flame-free, a large amount of lower alcohol may be used to speed up drying. The preferred range of lower alcohol content is 20% or less. While this correlates with the vaporization point (described below), a content of 20% or less facilitates rapid drying. Furthermore, this range ensures a vaporization point of 70°C or higher, or a level that is considered non-flammable, further enhancing the safety of use at wellheads where open flames are prohibited. Furthermore, in the worst case scenario, adding a large amount of lower alcohol in the hope of rapid drying can lead to the following problem. This means that the solid lubricating coating may dry too quickly, increasing its inhomogeneity and potentially cracking, resulting in deterioration of film quality.

[0085] [Solid Lubricant] The solid lubricant contains a soap component containing at least a metal soap among metal soap and alkaline soap components. The metal soap component accounts for 95% or more of the total weight of the metal soap and alkaline soap components. In other words, the main component of the solid lubricant is the metal soap. The weight of the metal soap is 95% or more of the combined weight of the metal soap and alkaline soap. If the alkaline soap content is high, it may dissolve in the aqueous solvent, causing the viscosity of the solvent to become too high, making it difficult to apply uniformly and slowing down the drying of the film. In other words, by reducing the alkaline soap content, the above concerns are alleviated. However, since the lubrication improvement effect of alkaline soap cannot be expected when there is no alkaline soap, it is preferable to design the components to contain it.

[0086] At the same time, the particle size of the metal soap must not exceed the thickness of the solid lubricating coating. A preferred range is an average particle size of 10 μm or less. If the particle size exceeds the thickness of the solid lubricating coating, it means that the metal soap penetrates the solid lubricating coating and is present. In this case, tightening and loosening with a strong torque will cause greater damage to the solid lubricating coating than when the metal soap is dispersed within the solid lubricating coating. For example, there is a risk of significant peeling, resulting in poor lubrication properties. Therefore, the particle size must be equal to or less than the thickness of the solid lubricating coating. On the other hand, assuming a thin film thickness necessary for the solid lubricating coating to achieve lubrication and rust prevention, a film thickness of at least 10 μm is required. For this reason, a particle size of 10 μm or less is preferred.

[0087] The metal soap and alkaline soap components constituting the solid lubricant contain one or more soaps that are compounds consisting of a fatty acid selected from the following Group A and a metal element selected from the following Group B. Group A: stearic acid, behenic acid, lauric acid, 12-hydroxystearic acid, oleic acid, montanic acid Group B: Na, K, Mg, Ca, Zn

[0088] [Binder Resin] The binder resin is a polymer or copolymer made of a water-soluble or water-dispersible polymer, containing a polymer having an acrylate or methacrylate structure in an amount of 90% or more based on the total weight of the binder resin. The water-soluble or water-dispersible polymer constituting the binder resin is, for example, a polymer made of one or more monomers selected from the following (1) to (4), or a copolymer made of two or more monomers:

[0089] (1) Monomers mainly consisting of acrylates, methacrylates, and their respective derivatives. (2) Monomers to which alkyl esters, vinyl esters, styrene esters, carboxylic acid esters, and monomers containing their respective derivatives are attached to acrylates, methacrylates, and their respective derivatives. (3) Monomers grafted onto the above (1) and (2). (4) Monomers of either or both of vinyl compounds and urethane compounds.

[0090] In this specification, the phrase "comprised of a water-soluble or water-dispersible polymer, containing a polymer having an acrylate or methacrylate structure at 90% or more of the total weight of the binder resin" is interpreted as follows: In other words, in the case of a copolymer, if even a portion of the copolymer structure contains an acrylate or methacrylate structure, the binder resin of the copolymer is treated as a "polymer having an acrylate or methacrylate structure," regardless of the weight of the incorporated acrylate or methacrylate structure or other components. A polymer that is permissible to be mixed in at less than 10% refers to one that does not form a copolymer with the polymer having an acrylate or methacrylate structure targeted by this application. In other words, structures containing acryloyl groups, vinyl groups, etc., in the monomer are excluded.

[0091] Furthermore, since the agent of the present disclosure is dissolved in an aqueous solvent, in addition to the above information, the polymer that can be mixed must be water-soluble. Examples include water-soluble polyamideimide resin, phenolic resin, and urea resin (urea formaldehyde). For example, when the volume of the solvent is converted to weight assuming a specific gravity of 1, the weight of the solvent is preferably 0.7 to 100 times the total weight of the solid lubricant and binder resin. Furthermore, the weight of the solid lubricant is preferably 0.1 to 1.0 times the weight of the binder resin. By adjusting the above components, it is preferable to set the flash point of the agent to a flash point above 60°C or to make it flame-retardant (non-flammable). Furthermore, it is preferable to adjust the viscosity of the agent to 1000 mPa·sec or less by adjusting the above components.

[0092] The appropriate and preferred ranges for these parameters can be defined as follows. First, the lower limit of the solvent weight is 0.7 or more because it is defined as the amount of solvent required to dissolve the solid lubricant. In fact, as shown in the examples below, metal soap, the main component of solid lubricants, was soluble up to 0.7. Furthermore, 0.7 was set as the lower limit because 0.5 would result in the lubricating components to be incorporated being insufficiently dissolved. The lubricating components to be incorporated include metal soap components, alkali soap components, and others. A maximum weight ratio of 100 times or less is expected, but a preferred range is 10 times or less. A high solvent weight ratio means a high amount of chemicals and a thin film component. Film components include binder resin components, solid lubricant components, and others. If multiple recoating, such as repeated application and drying, is desired, a maximum weight ratio of 100 times is not particularly problematic. On the other hand, if the effort of multiple coatings and drying is not a problem, a ratio exceeding 100 times may be possible. At the same time, there is a high concern that the thinness of the agent will make the film more prone to unevenness. This will result in a slightly worse number of times of tightening and loosening, but it may still be usable. Hereinafter, "number of times of tightening and loosening" will also be referred to as "number of times of M / B."

[0093] The preferred range is 10 times or less. A ratio of 10 times or less makes it easier to form the required film thickness with a conceivable coating method, for example, one to three coats, with a good M / B count and no particular deterioration. In the examples described below, it has been confirmed that a solid lubricating coating can be formed without any problems and the required lubrication properties can be achieved up to a weight ratio of 7.6 or less. Therefore, a ratio of 7.6 or less can be said to be an even more preferred range. Regarding rust prevention, a lower solvent weight is also preferable, as will be described later. In the present application, the solvent is primarily water. Therefore, to avoid rust in insufficiently dried areas, a ratio of 2 times or less is even more desirable.

[0094] Next, the ratio of the weight of the solid lubricant to the weight of the binder resin is preferably in a range of 0.1 times or more and 1.0 times or less. If the amount of solid lubricant is small relative to the binder resin, the total amount of solid lubricant, which is mainly responsible for lubrication, is small, and lubrication tends to deteriorate. Conversely, if the amount is too large, more than necessary may be contained, causing interference between the solid lubricants, resulting in saturation or deterioration of the tendency to improve lubrication properties. In the examples shown below, the actual M / B counts at the lower limit of the pass range were 0.08 at the lower limit and 5.0 at the upper limit within the experimental range, and the properties deteriorated to a passing level.

[0095] The flash point range is preferably 60°C or higher, and more preferably, it should be defined as non-flammable. On the other hand, in oil and gas wells, if there are locations or areas where the operating environment allows use in a temperature range below 60°C, the agents and films used to create the solid lubricating coatings of the present application can be used. These are parameters determined purely based on the safety of workers and the well site. They are not factors that affect lubrication, which is evaluated by the number of M / B runs. With the exception of alternative fluorocarbons, a low flash point often means high volatility, which affects the agent's early drying and film formation behavior. Considering the operating environment in wells, the flash point should be set to 60°C or higher, and more preferably, it should be designed to be even higher or to be classified as non-flammable.

[0096] The viscosity of a chemical agent is defined as the result of mixing the agent with a solvent, solid lubricant, binder resin, and other additives. Viscosity varies depending on the mixing concentration. In this application, the viscosity is preferably 1000 mPa·sec or less in order to prevent uneven application of the chemical agent and uneven film thickness. This is because high viscosity increases the tendency for uneven film thickness to occur. In the examples below, no particular deterioration was observed at 740 mPa·sec or less, so this can be said to be a more preferable range. Furthermore, by adjusting the above components, the chemical agent can be applied to the metal surface at an amount of 0.1 g / mm 2 Consider the case where the agent is applied as follows. In this case, it is preferable to adjust the agent so that it has quick drying properties, so that it can dry within 30 minutes when left to dry in a windless atmospheric environment at room temperature. Alternatively, by adjusting the above components, the agent can be applied to the metal surface in an amount of 0.1 g / mm 2 Consider the case where the coating is applied as follows. In this case, it is preferable to adjust the coating to have quick drying properties that allow it to dry within 5 minutes when dried in an atmospheric environment at room temperature with air blown at a speed of 1 m / sec or more. Note that "room temperature" here refers to a temperature in the range of 15 to 30°C.

[0097] Coating amount: 0.1 g / mm 2 "Below" refers to a typical coating amount achieved by a spin coating method using a 50 mm bristle width JIS No. 20 brush, with the brush being drawn in one direction only once. The drying time at this time is also defined. It is preferable to achieve a drying time of 30 minutes or less when left to dry, and 5 minutes or less when dried with airflow of 1 m / sec or more. This is achieved using multiple parameters specified in this application. The volatility of at least one of lower alcohol and aqueous ammonia is utilized by incorporating it, and the volatility surface area is increased by incorporating metal soap as a solid lubricant in a dispersed form with an appropriate size, thereby enhancing drying.

[0098] <Method of Producing the Agent> The agent is preferably prepared by dispersing and clouding the metal soap in a lower alcohol, and then adding the resulting mixture to the water solvent.

[0099] <Method of applying the agent> Before applying the agent, it is preferable to shake and stir the container containing the agent before applying it. Furthermore, when applying the agent of this embodiment to the surface of a tubular part, it is preferable to apply the agent in the circumferential direction while rotating the tubular part about its axis.

[0100] <Oil country tubular goods and oil country tubular goods threaded joint> An oil country tubular goods is a box 2 having a female thread 2a and a pin 1 having a male thread 1a, as shown in Fig. 1. An oil country tubular goods threaded joint, as shown in Fig. 1, is composed of a box 2, such as a coupling, having a female thread 2a, and a pin 1 having a male thread 1a. A lubricating coating comprising the solid lubricating coating of the present disclosure is formed on the contact surface (fastening surface 10) of the threaded portion of at least one of the box 2 and the pin 1.

[0101] In this embodiment, a lubricating coating having a solid lubricating coating is formed on the thread portion of the oil country tubular good. The solid lubricating coating has a binder resin and a solid lubricant dispersed in the binder resin. The solid lubricant contains a soap component containing at least a metal soap from among metal soap and alkali soap components, and the metal soap component accounts for 95% or more of the total weight of the metal soap and alkali soap components. The metal soap and alkali soap components constituting the solid lubricant include, for example, one or more soaps that are compounds composed of a fatty acid selected from Group A below and a metal element selected from Group B below. Group A: stearic acid, behenic acid, lauric acid, 12-hydroxystearic acid, oleic acid, montanic acid Group B: Na, K, Mg, Ca, Zn

[0102] The weight of the metal soap is, for example, 95% or more of the total weight of the metal soap and the alkali soap. The particle size of the metal soap is preferably 10 μm or less. The binder resin is made of a water-soluble or water-dispersible polymer, and the polymer is a polymer or copolymer containing 90% or more of monomers belonging to acrylate or methacrylate. The water-soluble or water-dispersible polymer constituting the binder resin is, for example, a polymer composed of one or more monomers selected from the following (1) to (4). The copolymer is a copolymer composed of two or more of these monomers.

[0103] (1) Monomers mainly consisting of acrylates, methacrylates, and their respective derivatives. (2) Monomers to which alkyl esters, vinyl esters, styrene esters, carboxylic acid esters, and monomers containing their respective derivatives are attached to acrylates, methacrylates, and their respective derivatives. (3) Monomers grafted onto the above (1) and (2). (4) Monomers of either or both of vinyl compounds and urethane compounds.

[0104] The phrase "comprised of a water-soluble or water-dispersible polymer, containing a polymer having an acrylate or methacrylate structure in an amount of 90% or more of the total weight of the binder resin" is interpreted as follows: In the case of a copolymer, if even a portion of the copolymer structure contains an acrylate or methacrylate structure, the binder resin of the copolymer is treated as a "polymer having an acrylate or methacrylate structure" regardless of the weight of the incorporated components other than the acrylate or methacrylate structure. It does not simply mean the weight of "acrylate or methacrylate."

[0105] The solid lubricating coating has a thickness of, for example, 1 μm or more and 100 μm or less, and is soft, with a pencil hardness of H or less. A base film (not shown) may be provided underneath the solid lubricating coating. At least one of the oil country tubular goods of the box and the pin is made of oil country tubular goods on which the lubricating coating of the present disclosure is formed. When one of the box and the pin is made of oil country tubular goods on which the lubricating coating of the present disclosure is formed, it is preferable that a coating having a harder hardness than the solid lubricating coating is formed on the thread portion of the other oil country tubular goods.

[0106] The lower limit of 1 μm or more for the film thickness is determined to comply with regulations requiring a film thickness sufficient for lubrication and below a thickness where the size of the metal soap does not penetrate the solid lubricant film. The upper limit of 100 μm or less is determined by the gap between the female and male threads (coupling / pin) of the OCTG thread. The solid lubricant film is inevitably scraped to some extent during tightening and loosening. Furthermore, the scraped solid lubricant film-derived material either moves in conjunction with the powder material during tightening and loosening, reforms and reattaches, or fails to do so and becomes clogged in the thread gap, resulting in increased risk of seizure. Depending on the type of thread, the thread gap (between the pin crest and the coupling valley) is approximately 100 μm wide. Meanwhile, the thread gap (between the pin valley and the coupling crest) is tightly fitted. If the solid lubricant film exceeds 100 μm, the absolute amount of the solid lubricant film inevitably increases to a certain extent when tightening and loosening, and it is estimated that the amount exceeds the amount that can be absorbed by the above-mentioned gap, and in fact, seizure occurs frequently. Therefore, the upper limit is set to 100 μm or less as the preferred range. If it exceeds that, it is difficult to say that it is always NG, but the number of M / Bs will not meet the specified number, and seizure will easily occur.

[0107] As described above, the agent disclosed herein has a binder resin component primarily composed of a water-soluble or water-dispersible polymer. Furthermore, a metal soap is used as the main component of the solid lubricant, to which trace amounts of alkaline soap and other additives with solid lubricant-like properties are added. Furthermore, the agent disclosed herein is composed of a component system that includes a water-based solvent and allows the addition of small amounts of organic solvents. This agent allows for rapid drying after application, and the solid lubricant coating formed using this agent provides lubrication and rust prevention that can withstand use in wells. This disclosure is intended for use in the most severe conditions, namely, the lubrication of threaded joints in oil well pipes.

[0108] The definitions of each element are explained in detail below. In this disclosure, the chemicals and the solid lubricating coatings formed using these chemicals are expected to provide rapid drying, corrosion resistance, and lubrication properties. However, the parameters that realize each required property are interrelated with the required properties and must be achieved within the upper and lower limit ranges specified in this disclosure. First, the required target properties will be described, followed by the ranges and meanings of each parameter.

[0109] "Regarding the target quick drying, corrosion resistance, and lubrication properties" In this disclosure, quick drying refers to the ability to dry within 5 minutes, preferably within 1 minute, without heating and by drying with air blowing. Alternatively, it means that when left outdoors or indoors at room temperature, it can dry within 30 minutes or less, preferably 15 minutes, and even more preferably within 5 minutes. Drying here refers to a level that goes beyond dry to the touch, and reaches a semi-hardened or hardened dry level. The paint terms dry to the touch and semi-hardened are defined in accordance with JIS K5500-2000.

[0110] However, when applied to oil well pipe threads, this disclosure aims to develop a coating agent with low viscosity and good fluidity. Therefore, it is conceivable that the coating agent will inevitably collect at the 6 o'clock position, i.e., the lowest position, causing the liquid to pool or drip in that area. Therefore, in the discussion of the above-mentioned rapid drying, we will focus on the dryness of the screw positions on the upper side of the watch, from 8 o'clock to 4 o'clock, as in a watch. The areas between 4 o'clock and 8 o'clock, or more precisely, the 5 o'clock to 7 o'clock positions where the coating agent pools or drips and remains undried, are excluded from the rapid drying analysis. The reason for excluding this area is as follows: Although the coating agent may remain partially wet, the lowest layer of the coating liquid applied to those areas constitutes a solid lubricating coating, and this does not affect the integrity of the film in terms of corrosion prevention. In other words, there are only insufficiently dried areas between the dried lowest layer of film from the pipe surface and the outermost layer of film in contact with the atmosphere, but in terms of rust prevention, a solid lubricating film formed by drying at the lowest layer is achieved.

[0111] The corrosion resistance of the present disclosure does not only refer to the corrosion resistance of the surface after the chemical agent has been applied and the water has evaporated. The corrosion resistance of the present disclosure assumes the most severe conditions, that is, a tubular structure with a thread, such as an oil country pipe thread. Furthermore, the present disclosure targets corrosion resistance after a protective cover, such as a protector, has been tightened and tightened, i.e., after it has been attached once and then removed again, with the protector removed. This assumes conditions that are slightly more severe than the actual required characteristics. With actual oil country pipe threads, after a solid lubricating coating has been formed, it is conceivable that when the protector is attached, the solid lubricating coating may partially come into contact with the protector, causing damage to the film. This is because the protector is attached in this state and the thread is left standing indoors or outdoors.

[0112] In this disclosure, the lubrication characteristics are ensured by evaluation results in actual wells, simulated wells, or make-up tests using power tongs, which can approximate these. This disclosure does not evaluate the lubricity of a solid lubricant simply by a conventional make-up / make-back test using a short pin. The inventors have found that a solid lubricant coating cannot be properly evaluated using a conventional make-up / make-back test using a short pin. Here, lubrication using a lubricating compound has traditionally been, and still is, the mainstream method for lubricating oil country pipe threaded joints. Because lubricating compounds are viscous liquids, they move in conjunction with make-up and make-back, improving lubrication. Therefore, there is little difference between lubrication evaluations in a laboratory using a short pin and evaluations in an actual well. However, when using a solid lubricant coating as disclosed in this disclosure, the solid lubricant coating may inevitably be scraped off, and the resulting debris or powder may not be able to move in conjunction with make-up and make-back, as compounds do. This will be discussed in more detail later, but the laboratory will devise a method for evaluation under conditions similar to those of an actual well, and the suitability of the solid lubricant coating will be determined based on the lubrication behavior evaluated in this devised test.

[0113] Regarding water-soluble or water-dispersible polymers: In this disclosure, water-soluble or water-dispersible polymers are defined as binder resins. Because this disclosure assumes that a film will form after the water evaporates, i.e., after evaporation or volatilization, the term "polymer" in this disclosure refers to a synthetic polymer in the narrow sense. The polymers in this disclosure exclude well-known natural polymers such as pectin, agar, starch-based materials, cellulose-based materials, and natural gums (alginate-based materials). The polymers in this disclosure also exclude polymers that remain semi-dry and moist even after drying, i.e., after the water has evaporated. Polymers that do not completely dry raise concerns about water-induced corrosion when applied to carbon steel. Specifically, the water-soluble or water-dispersible polymers in this disclosure include those composed of a single polymer and copolymers composed of two or more monomers. The individual monomers correspond to the following monomers (1) to (4):

[0114] (1) Monomers mainly consisting of acrylates, methacrylates, and their respective derivatives. (2) Furthermore, because these acrylates, methacrylates, and their respective derivatives are water-based, monomers containing alkyl esters, vinyl esters, styrene esters, carboxylic acid esters, and their respective derivatives. (3) Monomers grafted onto the above (1) and (2). (4) Monomers of either or both vinyl compounds and urethane compounds.

[0115] The present disclosure includes at least one polymer or copolymer of two or more monomers defined in (1) to (4), or a copolymer of either or both of a polymer consisting of a single monomer of (1) to (3) or a copolymer of (1) to (3) with (4) or other compounds. The other compounds refer to monomers such as maleic acid, sulfonic acid, styrene, carboxylic acid, and salts thereof.

[0116] The phrase "comprised of a water-soluble or water-dispersible polymer, containing a polymer having an acrylate or methacrylate structure in an amount of 90% or more of the total weight of the binder resin" is interpreted as follows: In the case of a copolymer, if even a portion of the copolymer structure contains an acrylate or methacrylate structure, the binder resin of the copolymer is treated as a "polymer having an acrylate or methacrylate structure," regardless of the weight of the components other than the incorporated acrylate or methacrylate structure. This does not simply mean the weight of "acrylate or methacrylate." The water-based polymer referred to here refers to a polymer that has hydrophilic properties due to the inclusion of polar or charged functional groups in the polymer structure. For example, it refers to a polymer that contains a carboxyl group, an amine functional group, a sulfonic acid, or the like in the main chain or side chain.

[0117] The binder resin of the present disclosure is dissolved in a solvent whose main component is water, and when the agent is applied, the water is removed, i.e., evaporated and volatilized, to form a film. Since the present disclosure is based on the basic premise of being environmentally friendly, the agent of the present disclosure is designed without using materials containing heavy metals such as lead, which have recently become a problem, or alkyl groups containing F (fluorine), such as those in the group known as PFAS. The requirements for achieving rapid drying of the film after application of the agent directly and indirectly affect the film properties of the agent. Next, the items related to rapid drying will be described in detail.

[0118] At the final film stage, it is desirable for the polymer or copolymer to contain 90% or more of acrylate and methacrylate monomers. Furthermore, copolymers containing acrylate and methacrylate with other monomers during copolymerization are considered acrylate and methacrylate polymers and satisfy the above requirement of 90% or more. The requirement of 90% or more means that the polymer is mostly composed of acrylate and methacrylate polymers, and it is acceptable to contain 10% or less of other polymers. In practice, the copolymer is expected to be close to 100% acrylate and methacrylate polymers.

[0119] "Why Rapid Drying is Necessary and Why Its Target Value is Required" The reason for the need for rapid drying is simply because the chemicals disclosed herein and the solid lubricant coatings formed using them are required to be used at the manufacturing site and also at the site of use. In particular, when considering application to oil well pipe thread joints, the following chemicals are also anticipated. That is, the chemicals are anticipated to be used when temporarily pulling up oil well pipe for tubing due to a problem at the wellhead, or when seizure occurs and the oil well pipe needs to be removed and sent to a workshop. In this case, the work must be completed within the category of a clean, green solid lubricant coating. After the oil well pipe is pulled up from the well, it is washed with water or the like, and a solid lubricant anti-corrosion film can be formed using the chemicals disclosed herein to prevent rust on the threads. Such demand is naturally present when used at the wellhead.

[0120] In this case, if you use a conventional wet compound, you will usually apply a preservative compound. TM In contrast, this disclosure assumes that the agent will be applied in a wellhead environment, forming a solid lubricant film. In other words, this disclosure requires that the agent be applied in a fire-free environment, without the use of heaters or other fire-causing devices, and that the agent will dry as quickly as possible to form a solid lubricant film.

[0121] From another perspective, there is a need to address the issue of inadequate production systems at individual workshops when threading on-site. Threading workshops have sufficient machining equipment. With conventional compound methods, surface treatment of box threads is often outsourced and rarely performed in-house. Surface treatments include, for example, manganese phosphate treatment and copper plating. At the same time, pin threads are not required to be coated with a viscous liquid storage compound and allowed to dry. For this reason, pin threads are typically shipped with a protector attached after application, without undergoing a drying process. If the agent disclosed herein were to be used at such sites, it would be difficult to rely on heat treatment equipment such as air blowers or hot air dryers. Therefore, we determined that the agent disclosed herein must be able to dry by leaving it indoors or outdoors for 30 minutes or less, preferably 15 minutes, and even more preferably within 5 minutes.

[0122] The 30-minute period is assumed to be the time required for one worker to lay out and line up approximately 30 pin screws or box screws, paint one end of each OCTG from end to end, return to the original position, and paint the other end from end to end, repeating this process. The 30-minute period is also assumed to be the time required for the worker to return to the original position and be nearly dry. It is also set as the time required for the worker to prepare the protectors and tighten them one by one without waiting. A drying time of 15 minutes would be sufficient even when processing a smaller number of pipes. Drying in 5 minutes or less is the most desirable goal.

[0123] However, factories that manufacture products coated with lubricating coatings are likely to have ventilation equipment and other facilities. Therefore, drying can be accelerated not only by leaving the coating to dry in the atmosphere but also by passing the coating through a ventilation system such as a jet fan, a heater ventilation system capable of emitting hot air, or a heat treatment furnace. In such cases, drying is preferably performed within five minutes, preferably within three minutes, and more preferably within one minute. This drying time is preferable to avoid interfering with the line speed and handling at the manufacturing site of products coated with solid lubricating coatings with excellent lubricity and corrosion resistance, or to keep such interfering levels to a low level. When describing the airflow rate of electric fans and blowers, a typical electrically driven fan has an airflow rate of 2 to 4 m / s. However, since this disclosure assumes that drying can be performed using a weak handheld fan, the drying time will be evaluated assuming an airflow rate of 1 m / s.

[0124] "Method of applying the agent" The basic composition of the agent disclosed herein is a solvent (water + trace amounts of lower alcohol, ammonia, and primary amine), a binder resin (mainly a water-based polymer), and a solid lubricant (metal soap + trace amounts of alkaline soap). The viscosity of the agent is also an important parameter. As one element for achieving rapid drying, it is preferable to design the liquid so that the viscosity of the agent is low. In this case, when applied to an inclined surface, it tends to flow rather than remain there. In other words, it is preferable to adjust the viscosity of the agent so that it flows when applied.

[0125] For example, a viscosity of 1000 mPa·sec or less is preferred. This level is the level at which, when applied to an obliquely placed member or tubular member, the agent feels like it flows along the slope. Note that the viscosity in this disclosure refers to the viscosity when the agent is opened or at the beginning of application. This viscosity specification can prevent the inadvertent formation of a thick film when applying the agent. There is no set lower limit for viscosity, but it is set to, for example, 40 mPa·sec or more. When a water-soluble or water-dispersible polymer material is added and mixed with a water-soluble solvent, the viscosity tends to increase, rather than reaching the viscosity of water (1 mPa·sec). Therefore, the minimum viscosity is approximately 40 mPa·sec.

[0126] By reducing the viscosity of the agent to 1000 mPa·sec or less, it becomes difficult to apply multiple coats or build-up paint, but it has the advantage of being able to achieve a uniform coating thickness and a thin film. Viscosity can be adjusted by selecting the monomers that make up the water-based polymer, adjusting the concentration of the metal soap and alkaline soap, and adjusting the blend ratio, including the solvent. On the other hand, because the viscosity of the agent is 1000 mPa·sec or less, it has low viscosity and is easy to flow. As a result, the agent in the wet areas tends to drip, accumulating at the 6 o'clock position on a clock. This area then unintentionally forms a thick film, so even if the base has dried and formed a film, the accumulated area may not dry within the drying time.

[0127] For this reason, when lubricating a tubular structure, the target drying time is determined by the dryness of the upper half of the lubricant at 12 o'clock on a clock, or more broadly, from 9 o'clock to 3 o'clock. While some liquid does accumulate at the 6 o'clock position, this is simply a collection of wet chemicals on top of the already dry portion. Therefore, the lower portion is dry at the initial stage of application. Any application method, including brushing, spraying, dipping, hand application, or machine application, is acceptable. Taking advantage of the tendency for the liquid to drip, after application, the object being treated can be turned downward or tilted to allow the paint to drip downward. Furthermore, for tubular metal parts, it is better to rotate the metal part while applying the paint with a brush or spray rather than leaving it to stand. This enhances drying and allows any remaining chemicals that did not form a film to be evenly reapplied to the metal surface as it rotates, helping to create a uniform film. It also prevents the paint from accumulating in one place.

[0128] "Ideas for Achieving Rapid Drying Properties" In the present disclosure, essential and preferred configurations consisting of the following four components have been devised and utilized to achieve rapid drying properties of water-soluble or water-dispersible polymers.

[0129] <Essential Components> One of the essential components is a lower alcohol. In other words, lower alcohol is a volatile organic solvent whose concentration is adjusted to have a flash point of 60°C or higher, so that it can be used in environments where open flames are strictly prohibited. This allows for quick drying. The flash point of the agent should preferably be adjusted to 150°C or higher, and more preferably 250°C or higher. Furthermore, the use of thinner-based VOCs should be avoided. This is to ensure the safety and health of workers and to allow work to be carried out without the need for exhaust equipment such as drafts.

[0130] Another option is aqueous ammonia. Depending on the situation, the volatility of aqueous ammonia can also be utilized to control the concentration within an appropriate range, allowing use without a draft facility. One of the components is the concentration and particle size of the metal soap. Controlling the concentration and particle size of the contained metal soap within an appropriate range enables rapid drying. The particle size of the metal soap should be 10 μm or less. Using a particle size of 5 μm or less, preferably 1 μm or less, increases the surface area of ​​the metal soap and enhances drying. At this time, it is necessary to take measures to prevent the metal soaps from associating with each other and forming clumps, which would result in their apparent size exceeding their individual sizes. This is achieved by first dissolving the metal soap in the above-mentioned lower alcohol and then mixing it with a mixture of a water-based solvent and an aqueous polymer.

[0131] The metal soap also functions as the main component of the lubricant, and the total weight of the solid lubricant, including the alkaline soap described below, should consist of at least 95% metal soap. As for the overall mixing ratio, when the solvent has evaporated and a solid lubricant coating has been formed, the total weight of the solid lubricant should be 0.05 to 1.0 per 100 weight parts of the binder resin. The total weight of the solid lubricant should consist of at least 95% metal soap.

[0132] In the present disclosure, alkaline soap may be used to support lubrication. However, adding soap that dissolves easily in water can, conversely, cause the solvent water to become viscous and gelatinous. This has the adverse effect of increasing the viscosity of the agent and slowing film formation. Excessive gelation prevents the water from being completely removed, making it impossible to achieve a dry solid lubricant coating. Therefore, it is necessary to specify an upper limit for the appropriate amount of alkaline soap at a trace level. This should be within the appropriate viscosity range described below. Furthermore, the main component of the solid lubricant, the metal soap, should account for 95% or more, meaning the alkaline soap component should be limited to 5% or less.

[0133] The viscosity of the drug is formulated to be 1000 mPa·sec or less. This viscosity is necessary when the drug is formulated, including water-soluble or water-dispersible polymer materials, additives such as metal soaps, and the above-mentioned lower alcohols. The aim is to achieve a low viscosity and a thin liquid viscosity. There is no set lower limit for viscosity, but it will be approximately 40 mPa·sec or more. When a water-soluble or water-dispersible polymer material is added and formulated into a water-soluble solvent, the viscosity will not be the same as that of water (1 mPa·sec), but will be high. This level will be approximately 40 mPa·sec.

[0134] <Preferred Configuration> When applying the agent to a tubular metal component, which is a structure, it is preferable to apply the agent while rotating the tubular structure. It is also preferable to continue rotating the tubular structure after application. This is because rotation prevents wet agent from accumulating at the 6 o'clock position after application, and can be expected to have the same effect as promoting drying using air blowing, etc. Furthermore, in the case of tubular metal components (structures), liquid inevitably accumulates at the 6 o'clock position, causing only the outermost layer to take a long time to dry. Complete drying, including this, takes a long time. For this reason, when applying the agent to the outside of the tube, it is preferable to take advantage of dripping from the 6 o'clock position. Alternatively, whether on the outside or inside of the tube, it is preferable to tilt the tube at an angle to expel the agent that tends to accumulate at the 6 o'clock position. Furthermore, rapid drying can be achieved by utilizing processes that enhance drying, such as air blower drying, hot air blower drying, infrared irradiation, ultraviolet irradiation, and heat treatment. In this case, a synergistic effect with the above configuration can be expected.

[0135] "Utilization of lower alcohols, ammonia, and primary amines, and the flash point of the entire agent" In this disclosure, the volatility of lower alcohols and ammonia is utilized, and a fine metal soap, the main component of the solid lubricant, is selected. This increases the surface area, allowing for quick drying, reducing the viscosity of the agent itself and increasing its fluidity. This prevents the formation of a thick film and promotes the volatilization and evaporation of water. The term "lower alcohol" as used herein refers to one or a combination of two or more selected from, for example, methanol, ethanol, isopropyl alcohol, normal propyl alcohol, and industrial ethanol.

[0136] Among lower alcohols, those with four or more carbon atoms, i.e., butanol or higher, tend to be less soluble in water. For this reason, the present disclosure uses lower alcohols with three or fewer carbon atoms. However, these have low flash points at high concentrations and cannot be used in environments where open flames are strictly prohibited. Therefore, the agent is formulated so that the flash point of the final formulated agent is 60°C or higher, preferably 150°C or higher. More preferably, it is formulated to a level that can be classified as non-flammable. By containing at least 0.5% or more of the lower alcohol group, volatility can be utilized to achieve rapid drying. Most desirable is a situation in which no flash point is established or measured, which is defined as non-flammable.

[0137] The lower alcohols not only strengthen the drying process, but also help to prevent the metal soap additive from clumping and from associating with the size it was when added. If you simply dissolve the metal soap in water, the water-repellent properties of the metal soap will prevent it from mixing with the water and instead cause the particles to associate with each other and form clumps. Even if you try to mix metal soap particles with particle sizes below the specified value into a coating paint, if you mix the metal soap directly into water, it will not disperse sufficiently. As a result, even if a film is formed, it will be unevenly distributed, which is not good for lubrication or corrosion resistance.

[0138] In this disclosure, a metal soap is first dissolved in a lower alcohol. Then, a mixture of lower alcohol and metal soap is mixed with a dispersion of a water-soluble or water-dispersible polymer and water. The concentration of the lower alcohol and the content of the metal soap must be adjusted to fall within the ranges specified in this disclosure. Furthermore, to enhance rapid drying, a lower alcohol may be used as the primary agent, and the volatility of ammonia or primary amines may also be utilized. The ammonia referred to here is aqueous ammonia. This is a commercially available agent, prepared at a concentration of 28-30%. Incidentally, aqueous ammonia itself is nonflammable. Commercially available aqueous ammonia is also available in dilute concentrations such as 10% and 5%. However, this disclosure will be discussed based on concentrated aqueous ammonia (28-30%).

[0139] Aqueous ammonia may be used as a chemical to prepare aqueous polymers in the neutral pH range, specifically, a pH of about 5 to 9, which is considered to be preferable. Aqueous ammonia may be used in conjunction with the volatilizing effect of lower alcohols. The use of highly volatile primary amines is also permitted as long as the pH does not exceed the above range. The primary amine may be added to shift the pH toward the alkaline side. The ammonia and primary amine added to shift the pH from the neutral side to the alkaline side are then used to utilize their combined volatility.

[0140] However, when it comes to primary amines, care must be taken when handling methylamine in particular. Aqueous ammonia can be handled as non-flammable. On the other hand, methylamine is highly flammable, so adding large amounts increases the risk of accidents. Therefore, while small amounts of primary amines can be used, they should be handled with care. In order to dry and strengthen the solvent by evaporation, the weight of lower alcohols, ammonia, and primary amines must be 30% or less of the total solvent. The upper limit is limited by factors such as flash point.

[0141] The chemicals disclosed herein do not contain water-insoluble alternative fluorocarbon solvents, halogenated solvents such as trichloroethylene and tetrachloroethylene, or thinners. These chemicals are not recommended for use due to their adverse effects on the global environment and health. Furthermore, thinners, a VOC, are often considered harmful to health and include toluene, xylene, benzene, mineral spirits, and ethers, as well as oils broadly referred to as mineral oils.

[0142] The reason for setting the flash point of the agent of the present disclosure to 60°C is as follows. The temperature that can be expected to occur at an actual wellhead when laying an oil well pipe threaded joint while tightening it is thought to be at most below 60°C. For this reason, the first step is to ensure that the temperature does not fall below this temperature. This reduces the risk of ignition and fire caused by a volatile agent, essentially eliminating it. The reason for setting the flash point as 150°C and the more desirable flash point as 250°C is as follows. That is, 250°C is the highest temperature at the wellhead, and 150°C is the highest temperature that can be expected to reach the wellhead after heat transfer, so these settings were made. To eliminate the risk, the flash point must be unmeasurable and the agent must be classified as non-flammable.

[0143] "Metal soap particle size and content concentration, alkaline soap content" In this disclosure, metal soap and alkaline soap function as solid lubricants. Furthermore, to enhance early drying, metal soaps increase the surface area by reducing the particle size of the metal soap, thereby accelerating drying. Alkaline soaps are first dissolved in a water-based solvent and then incorporated into the film, or precipitated soap appears on the surface or inside the film. However, since alkaline soaps are not ultimately liquid, they are treated as solid lubricants. In the following explanation, solid lubricants refer to soap components containing metal soap and alkaline soap.

[0144] In this disclosure, the enhancement of rapid drying is achieved by simultaneously achieving multiple factors. The volatility of the aforementioned additives, consisting of the volatile lower alcohol group, ammonia, and primary amine, is utilized by adding appropriate amounts to the solvent. Based on promoting the evaporation of the aqueous solvent, the size of the metal soap is specified and dispersed uniformly without clumping. Furthermore, the viscosity of the agent is set to 1000 mPa·sec or less to prevent the agent from being applied too thickly. At the same time, the amounts of metal soap and alkaline soap added must be adjusted to simultaneously achieve lubricity and corrosion resistance.

[0145] The particle size of the metal soap should be 10 μm or less, preferably 5 μm or less, and even more preferably 1 μm or less. This increases the surface area of ​​the metal soap, thereby enhancing drying. The smaller the particle size of the metal soap, the faster the chemical dries. However, it is important that the metal soap particles are dispersed, maintaining their particle size and preventing clumping. At the same time, to ensure the integrity of the solid lubricant coating, the particle size of the metal soap must not exceed the film thickness of the solid lubricant coating. If the film thickness is exceeded, the metal soap will appear to protrude from the film. This will result in significant damage to the film, such as peeling or scraping, when a strong torque is applied. On the other hand, there are no size restrictions for alkaline soaps, as they are soluble in water.

[0146] Metal soap is the main component of the solid lubricant and is key to dry strengthening. On the other hand, alkaline soap is formulated to play a supplementary lubricating role. In actual wells, when a full-size pin is set into a box screw, it is rare for the pin thread to be inserted straight into the box screw and then manually tightened, as is ideal. In reality, the pin thread is inevitably set at a slight angle. As a result, even when manually tightened, only about half of the pin threads are exposed. This often results in uneven contact between the threads during the initial tightening process, which can damage the surface of the solid lubricant coating. In this case, the alkaline soap is expected to provide lubrication support, sliding the box screw and pin screw from a fully engaged state to a stable position. The alkaline soap is expected to provide lubrication by sliding the box screw and pin screw into a stable position, preventing the spike-like torque seen in Figure 3 from building up before torque is applied.

[0147] Additionally, metal soaps are water-repellent. Therefore, even if the solid lubricant coating is slightly damaged, its water-repellent effect is expected to effectively improve corrosion resistance. In other words, corrosion resistance is ensured by metal soap. The solid lubricant must account for 95% or more by weight of metal soap and alkaline soap. In essence, the inclusion of about 5% of another solid lubricant is permitted, but the intention is that most of the solid lubricant should be made up of materials broadly classified as soap.

[0148] As mentioned above, the content of metal soap or alkaline soap is considered based on the balance of the total chemicals. In this case, when the volume of the solvent is converted to weight with a specific gravity of 1, it is formulated so that it accounts for 0.7 to 100 times the weight of all solid lubricant components that form the film. The weight of all solid lubricant components is the sum of the weights of the solid lubricant and the binder resin. In other words, a wide range of formulation is acceptable for water-based solvents, except for extremely concentrated or diluted states. If the ratio exceeds 100, there is too much water, making drying difficult. Furthermore, because there is a concern that water itself may cause rust, it is preferable that the ratio be 10 times or less, and more preferably 2 times or less.

[0149] The solvent evaporates during drying, leaving only the binder resin component and solid lubricant as the film. It is desirable that the weight ratio of solid lubricant to binder resin be 0.01 to 1, with the metal soap accounting for 95% or more of the weight of the solid lubricant. The lower limit is 0.1:1 because, if the ratio is less than that, there is too little support for the solid lubricant, and the lubrication improvement effect cannot be expected. In this case, if a strong force is applied to the binder resin, the film is likely to peel off completely, resulting in a high risk of seizure. The upper limit is 1:1 because if the metal soap content is too high relative to the solvent, the film itself will lose its integrity, and even a slight load will significantly increase the risk of the film cracking and being exposed to the environment. Furthermore, this concentration can be said to be the limit for maintaining the metal soap in a fine size without clumping.

[0150] "Types of Metal Soaps and Alkaline Soaps" In this disclosure, the metal soaps and alkaline soaps are assumed to be the following. That is, the metal soaps and alkaline soaps are composed of one or a combination of two or more soaps made from compounds of fatty acids of Group A and metal elements of Group B below. - Group A (stearic acid, behenic acid, lauric acid, 12-hydroxystearic acid, oleic acid, montanic acid) - Group B (Na, K, Mg, Ca, Zn)

[0151] In this disclosure, metal soaps are defined as consisting of one or more metal salts of group B, namely, magnesium salts, calcium salts, and zinc salts of fatty acids of group A. Metal salts of alkali soaps are consisting of either or both of sodium salts and potassium salts of group B. Other alkali metal salts are commercially available, but these other metal salts are excluded because they are not used in applications such as dissolving in water for cleaning.

[0152] "Amount of Agent Applied and Drying Time" As described above, the enhancement of rapid drying was explained as being achieved by simultaneously achieving multiple factors. That is, the above-mentioned volatile lower alcohols, ammonia, and primary amines are added to the solvent in appropriate amounts, with the limitation that the flash point does not become too low. These volatilities are then utilized to promote the evaporation of the aqueous solvent, and the size of the metal soap is reduced and the metal soap is dispersed uniformly without clumping. Furthermore, the viscosity of the agent is adjusted to 1000 mPa·sec or less to prevent the agent from being applied too thickly.

[0153] Furthermore, as a condition for ensuring rapid drying, while keeping the above conditions as a premise, the coating amount is actually 0.1 g / mm 2 It is preferable for rapid drying to apply the coating uniformly to the following conditions. Under these conditions, when left in the air at room temperature (15°C-30°C, for example, 24°C), it can be expected to dry within 30 minutes. Furthermore, when drying with air blowing at 3 mm / sec or more, rapid drying properties can be expected, allowing drying within 5 minutes at room temperature. The coating amount is, for example, 0.2 to 0.05 g / mm 2is the preferred range. If it is applied thicker than this, the drying time tends to be slower and some of it will drip. In addition, there are cases where only the surface layer of that part does not dry. 2 Turning off the heat tends to speed up drying, but this can cause concerns about corrosion resistance.

[0154] "Film Properties: Film Thickness, Pencil Hardness" In the present disclosure, when the coating agent dries to form a solid lubricating coating, it is preferable that the coating thickness be in the range of 1 μm to 100 μm and have a soft pencil hardness of H or less. Ideally, a uniform coating thickness of approximately 10 μm to 50 μm is sufficient. However, when a coating agent with the above-mentioned viscosity is applied, the low viscosity means that the paint that cannot form a film tends to drip and move, no matter how much drying is performed. In a structure with threads, such as an oil well pipe thread structure, the coating agent tends to accumulate in the valleys of the threads, especially at the 6 o'clock position on a watch. Furthermore, the surface tension of the coating solution tends to thin the corners of the thread structure. Therefore, to achieve both lubrication and corrosion resistance, the coating thickness is preferably within the above range. If the coating thickness is less than 1 μm at its thinnest point, there is a high risk of seizure. Furthermore, if the coating thickness exceeds 100 μm, it tends to be scraped off during lubrication, and the resulting peeled pieces and powdery material can cause seizure. There is also a possibility that the roots will peel off and burn.

[0155] Here, the film thickness refers to the film thickness at the stage when the agent has dried and become a solid lubricating coating, as described above. The film thickness can be determined, for example, by cutting the threaded portion longitudinally at four locations (e.g., four locations spaced 90 degrees apart) along the circumferential direction and observing each cross section obtained under a microscope. The film thickness at the thickest and thinnest portions of the coating is identified through this observation. It is then confirmed whether each film thickness falls within the above-mentioned range. If the tendency of the film thickness distribution is known from past measurement results, the film thickness can also be estimated as follows. That is, if the agent application and drying method is the same, it is also possible to estimate the maximum and minimum film thickness values ​​for the entire threaded portion by measuring the film thickness at predetermined specific locations with an electromagnetic film thickness meter.

[0156] The hardness of the solid lubricating coating is preferably a pencil hardness of H or less. This is because the solid lubricating coating of the present disclosure is intentionally made soft to achieve lubrication properties, assuming that it will wear away slightly when hit hard. Furthermore, if the pencil hardness exceeds H, it may peel off completely, increasing the risk of seizure. Film hardness is measured by pencil hardness. The measurement method is specified in JIS K 5600-5-4 (1999). The JIS standard states that this standard is a translation of "ISO / DIS 15184, Paints and Varnishes—Determination of Film Hardness by Pencil Test." The pencil hardness test method of the present disclosure evaluates the pencil hardness in accordance with the JIS standard. That is, 6B to 6B to 6H to 6H to 9H are the evaluation targets, and hardness of 9H or more is evaluated as ≦6B and ≧9H, respectively.

[0157] "Coating of both sides of oil country tubular goods constituting a threaded joint, coating of one side, and coating of one side but with a different type of solid lubricant coating on the opposing surface" This disclosure encompasses all cases, including when the solid lubricant coating of the present disclosure, made with the agent of the present disclosure, is coated on both sides of the surfaces to be lubricated, and when it is coated on only one side and nothing is coated on the other. When the solid lubricant coating of the present disclosure is formed on only one component, it is preferable that the pencil hardness of the solid lubricant coating of the present disclosure be softer than that of the other type of lubricant coating on the opposing surface. The solid lubricant coating of the present disclosure is designed to be a soft film. This is because the lubricating properties are achieved assuming slight abrasion during lubrication, and this effect cannot be achieved if the coating itself is hard.

[0158] "Method for Evaluating the Corrosion Resistance of Solid Lubricant Coatings" In the corrosion resistance evaluation in this disclosure, a protector used to protect the threads of a structure with a thread structure, such as an oil country pipe thread, is tightened and then loosened, and then the protector is removed, and salt spray is applied to the solid lubricant coating. The evaluation was based on the criteria that the appearance of red rust all over the surface was deemed NG. In essence, the corrosion resistance was evaluated by first inflicting possible damage on the film and then evaluating it with salt spray. The salt spray conditions were in accordance with JIS K 5600-7-1, using neutral salt spray conditions of 5% NaCl (35°C, humidity 98-99%, spray rate 1-2 mL / Hr / 80 cm). 2 , pH 6.5-7.2) and based on evaluation at 8 hours.

[0159] Here, the metal surfaces of metal parts covered by this disclosure include, for example, lathe-machined or machined surfaces, polished surfaces, etc. Note that for the corrosion resistance evaluation, areas with remaining mill scale were excluded. Depending on the roundness and eccentricity of the tubular structure, samples may have mill scale embedded in the thread structure. However, if mill scale is cleaned before forming a solid lubricating coating, water can penetrate into tiny defects, holes, and scratches in the mill scale. Furthermore, when a solid lubricating coating is formed on top of the mill scale, even if the solid lubricating coating is sound, rust spots may appear on the underlying steel. However, such rust spots are not rust on the solid lubricating coating and are therefore excluded from the evaluation.

[0160] "Lubrication Evaluation Method" This is considered to be the most severe lubrication condition among the environments in which the solid lubricant coating of the present disclosure is used. In other words, lubrication is evaluated under the tightening and tightening conditions of OCTG threads that are similar to those used in actual wells. However, evaluating the solid lubrication behavior of OCTG threads in actual wells or simulated wells is not realistic in terms of both cost and the time required to arrange experiments. For this reason, in the present disclosure, evaluation was performed using an apparatus such as that shown in Figures 5 and 6.

[0161] This solution involves attaching weights (one to three full-length pins) to the upper end of the short pin to allow for load application. The screw is initially set in a position where the pin threads are approximately half exposed relative to the box screw, and then tightened with tongs. A weight is applied during tightening, but not during back-tightening, destabilizing the pin threads and simulating the tightening conditions in an actual well. This allows the upper and lower limits of each parameter regarding the lubrication characteristics to be set to values ​​consistent with actual conditions. This evaluation method is also referred to as "weight-tong evaluation." The inventors have confirmed that this weight-tong evaluation can adequately reproduce the evaluation of tightening and back-tightening in an actual well. The reason for using this weight-tong evaluation is as follows: Relying on evaluations using horizontal power tongs with short pins approximately 1 m long or vertical power tongs with simply short pins could lead to a false assessment of superiority in the "solid lubricant coating evaluation" that is the subject of this disclosure. In other words, the upper and lower limits of the parameters that define the invention become meaningless.

[0162] Solid lubricant coatings can inevitably be damaged when tightening and loosening, and flaked or powdery debris does not always move in tandem with tightening and loosening. If they do not move in tandem, they can get stuck in the thread gap and cause seizure. However, evaluations using conventional short pins are less susceptible to damage, so there is a concern that something that is actually bad may be evaluated as good. On the other hand, with lubrication using conventional compounds, the compound is a viscous liquid, so it moves in tandem with tightening and loosening. For this reason, there is no significant discrepancy between the evaluation results using short pins and the evaluation in an actual well.

[0163] In past patent documents, there are occasional reports that lubrication tests based on solid lubricating coatings can be performed up to 15-20 times, even with large diameter sizes such as 9-5 / 8" and 13-3 / 8". However, such a number is virtually impossible with solid lubricating coatings, which have inferior lubrication properties compared to grease-like compounds. These results are likely based on evaluations using horizontal or vertical power tongs using short pins, which are commonly seen in laboratories. If so, such evaluation values ​​are possible, but in actual well cases where large-diameter OCTG using solid lubricating coatings are used for make-up and make-up in wells, a make-up of 15-20 times is rarely possible. Based on this consideration, the evaluation method in the examples described below was a weight-tongs test using the equipment shown in Figures 5 and 6. The conditions simulated are those that occur in make-up and make-up tests in actual wells and simulated wells, and the lubricity of solid lubricating coatings is evaluated under these conditions, such as those seen in Figures 3 and 4(a).

[0164] What actually happens in actual wells is that because full-length pins (approximately 12 meters long) are used, it is impossible to "set the pin perfectly straight" during initial setting, and the pin is almost always inserted at an angle. Even when attempting to set a full-length pin thread perfectly straight using a stubbing guide or compensator, it is impossible to set it perfectly straight. The pin thread ends up being set at a slight angle. It is virtually impossible to tighten the pin thread until the threads are hidden by the box screw. When the pin screw is inserted into the box screw and further tightened by hand, the threads partially touch each other midway. As a result, the pin thread cannot be advanced any further until five or more threads, or about half of the total threads, are exposed. Therefore, when initially tightening with tongs, it takes several turns until the load is applied—for example, approximately 6.3 turns in Figure 3—before the pin thread and box screw begin to mesh in the correct position. Like many other threaded structures, oil well pipe threads have a tapered structure, so that the threads ultimately mesh in a stable position. To exaggerate, the circled area in Figure 7 is severely damaged. Cracks, peeling, and the like inevitably occur in the film at a microscopic level. That is, because the pin thread 1a is set at a slight angle, the following occurs in relation to the thread portion 2a of the box screw 2. The positions where the pin thread contacts, namely, the tip of the pin thread 1a, near the center of the threads of the thread portion 2a of the box screw, and near the center of the pin thread 1a and near the entrance of the thread portion 2a of the box screw, tend to be severely damaged. "Near the center of the thread" refers to the vicinity of the position where the pin screw contacts the box screw when inserted. "Near the entrance of the thread portion 2a of the box screw" refers to the vicinity of the entrance of the box screw 2a when the pin screw is inserted.

[0165] In Figure 3, irregular spikes of torque are observed during the first few rotations before the stable position is reached, i.e., before a steady torque is generated. This is directly related to damage to the solid lubricant coating due to uneven contact between the pin thread and the box thread. This fact is essential for evaluating the lubrication of solid lubricant coatings. Uneven contact between the threads inevitably causes wear of the solid lubricant coating. These peeled pieces and debris do not necessarily move in conjunction with the tightening and loosening of the threads. If debris becomes lodged in the thread gap, it becomes a major cause of seizure. This is due to a combination of rattle caused by the initial setting position of the pin thread and the weight of the actual length pin. This results in uneven, unbalanced loads contacting the pin thread and the box thread, inevitably causing the solid lubricant coating to peel off or break into powder. The impact of these debris lodging in the thread gap and seizure was evaluated using a laboratory simulation method.

[0166] Figure 5 shows the overall concept of the test method, and Figure 6 shows an enlarged view of the area involving the weight 3. The weight-tongs test uses a vertical power tongs 4. The short screw 1 and box screw 2 are then tightened using the threads of the pin thread 1a and the box thread 2a. To simulate a situation where the threads do not mesh, the initial temporary tightening position is set so that half of the total number of threads on the pin thread 1a are exposed from the box screw 2. This is one of the causes of wobble. From this position, tightening with the power tongs 4 begins. At this time, the weight 3 is attached to the opposite side of the tightening screw of the pin 1. The weight of the weight 3 is calculated based on the outer diameter and thickness of the actual pins, equivalent to a load of one to three actual-size pins. For 9-5 / 8" 53.5#, one piece will weigh approximately 1 ton (2,200 lbs), and three pieces connected together will weigh approximately 3 tons (6,600 lbs). One piece is intended for use in onshore wells, and three pieces are intended for use in offshore wells.

[0167] The weight 3 in Figure 5 has an insertion rod 13 welded to the weight body 3A at an axially symmetrical position, as shown in Figure 6. The insertion rod 13 is inserted from above the pin 1 to attach the weight to the upper end of the pin 1. Through holes 1d and 13a are pre-drilled in the pin 1 and the insertion rod 13. A piercing rod 12 is inserted and set into the through holes 1d and 13a to integrate the weight 3 and pin 1. A swivel-type hook 11 is welded to the axial center of the upper part of the weight 3, and the weight is suspended from a hanging device 20 on the ceiling via a hanging chain 21. When tightening, the weight load is applied to the box screw, and the screw is tightened at 5 to 20 rpm until torque is established. The initial temporary tightening position and the high-speed tightening and loosening rotation serve as a simulation of play. Once the torque is reached, reduce the rotation speed to 0.5 to 2 rpm and tighten the bolts to the tightening position.

[0168] To simulate a tightening / retraction test in an actual well, the weight 3 may or may not be applied, especially during loosening. It is preferable not to apply the weight 3 during retraction. In the following example, the weight 3 is not applied during retraction. If retraction is performed with the weight applied, the weight acts as a "weight" or balancer when loosening from the tightened position, loosening the pin thread as if it were rising straight up. This prevents the pin from rattling, and damage to the solid lubricant coating is not caused during retraction. Even under conditions where the load is not set to zero, the load is lifted and the test is performed. Even under conditions where the load is not set to zero, loosening the load allows for testing under conditions where rattling is more severe and more likely to damage the solid lubricant coating. The rotational speed during backlash is such that when the torque is high, loosening begins at a speed of 0.5 to 2 rpm, and when the torque reaches about 1 / 10 of the tightening torque value, loosening is increased to a high speed of 5 to 20 rpm. In this example, after backlash is complete, the pin thread and box thread are separated from each other by backlash, and the surfaces of each are air-blowed to remove debris from the solid lubricant coating, the surfaces are checked, and then the backlash is continued again.

[0169] Lubrication evaluation is performed using the following methods and criteria. According to ISO 13679, casing sizes are considered acceptable if they have been tightened and loosened three times or more, and tubing sizes are considered acceptable if they have been tightened and loosened ten times or more. However, when considering lubrication using a solid lubricant film, the number of M / B cycles tends to be lower than when using conventional lubrication with a grease-like compound. The reasons for this are as follows: With conventional methods using a grease-like compound, after each tightening and loosening, the grease-like compound on the surface is washed off with an organic solvent, the surface is inspected, and then a new grease-like compound is applied. This means that the main source of lubrication is resupplied. On the other hand, with lubrication using a solid lubricant film, the thread surface is cleaned with an air blower, but no lubricating components are added during the process. As a result, it is undeniable that the number of tightening and loosening cycles when using a solid lubricant film tends to be lower.

[0170] Therefore, as the criteria for the number of tightening and loosening times in this disclosure, a casing size that was tightened and loosened three or more times was judged to pass. A tubing size that was tightened and loosened five or more times was judged to pass. Furthermore, the casing size was determined to be 7 inches or more, and the tubing was determined to be less than 7 inches, and judgment was made by drawing a line. In addition to the number of M / B times, once the casing was completely loosened after tightening, the pin was released to the top, and the pin thread surface and box thread surface were observed after air blowing to directly visually confirm whether or not there was any seizure. In addition, the torque turn chart was checked to see if there were any abnormalities.

[0171] The NG judgment was made as follows: If the screw did not loosen during the M / B number of tightening and loosening operations, it was judged that seizure had occurred at that number of tightening and loosening operations, and the number of tightening and loosening operations was judged as the previous number of tightening and loosening operations. For screws that were completely loosened and the surface could be observed, if slight seizure had occurred in the seal area, it was judged as NG on the spot. Then, the number of tightening and loosening operations was judged to be the number that would cause seizure at the next number of tightening and loosening operations, and the tightening test using the weight tongs was completed on the spot. If the screw part had very slight seizure, it was repaired and the test continued as is. The number of tightening and loosening operations performed in this way was sorted into good and bad using the judgment criteria described above.

[0172] Examples according to the present disclosure are described below. (Example 1: Method of Mixing Metal Soap and Method of Mixing Uniformly) In the study group of Example 1, the conditions for the metal soap mixing method were selected based on how it was mixed into the liquid. The metal soap mixing conditions were investigated using chemicals with the following mixing ratios. The solvent used was a mixture of water as the main component, industrial ethanol, and aqueous ammonia. Ca stearate (metal soap: particle size 8-10 μm or less) and sodium stearate (alkali soap) were mixed at a weight ratio of 99:1 as the solid lubricant. A copolymer of vinyl acetate and methacrylic acid was used as the binder resin, with 10 parts by weight of methacrylic acid mixed with 100 parts by weight of vinyl acetate. Note that the copolymer referred to here corresponds to 100% "polymer having an acrylate or methacrylate structure" as described in this disclosure.

[0173] The blending ratio for each was 3:1 of the solvent (water) (measured by volume and converted to weight assuming a specific gravity of 1) relative to the total weight of the solid lubricant (metal soap + alkali soap) and binder resin. The blending weight ratio of the solid lubricant was 0.1:1 relative to the weight of the binder resin. To carry out these blends, a mixture of water and monomers for creating a vinyl acetate / methacrylic acid copolymer was prepared. As shown below, the metal soap was blended with industrial ethanol, and then ammonia water was added to adjust the pH to 7-8. Finally, sodium stearate was blended and mixed. We considered ways to mix the metal soap into this basic chemical.

[0174] <Condition 1> Condition 1 is a case where calcium stearate was added directly to the base chemicals according to the above blending ratio and stirred. Condition 1 is a case where no industrial ethanol was used. In condition 1, the metal soaps were not mixed thoroughly, and some of the metal soaps floated on the surface and aggregated together. In other words, they could not be mixed homogeneously. This result supports the conventional knowledge that metal soaps are insoluble in water.

[0175] <Condition 2> In condition 2, calcium stearate was added to the base chemicals according to the above mixing ratio and stirred. Then, industrial ethanol was added in a vol / vol ratio of 100 parts water to 20 parts ethanol. In condition 2, the mixture was not thoroughly mixed, with some floating on the surface and clumping together. In other words, it was not possible to mix it homogeneously. Condition 2 shows that the metal soap did not mix well even if ethanol was added later.

[0176] <Condition 3> Condition 3 is an example in which calcium stearate was stirred in a separate container with industrial ethanol (100 parts water, 20 parts industrial ethanol), i.e., homogeneously mixed, and then added to the base chemical and stirred. Condition 3 can be considered an example of a nearly homogeneous mixture. Although calcium stearate is said to be insoluble in both water and alcohol, we confirmed that in alcohol (ethanol), the particles of calcium stearate can be finely dispersed without forming lumps, as the particles do not associate with each other. Therefore, we found that by first dissolving it in ethanol (alcohol), and then adding that state to the base chemical and stirring it, a homogeneous solution of the metal soap can be created.

[0177] <Condition 4> In Condition 4, calcium stearate was thoroughly stirred in a separate container with industrial ethanol (1 part water to 1 part industrial ethanol) before being added to the base chemicals. In Condition 4, 19 parts industrial ethanol was subsequently added to the base chemicals and stirred. In Condition 4, when the metal soap calcium stearate was added to a small amount of ethanol to create a turbid mixture, the metal soap did not mix well, and some of it floated to the surface and aggregated together, forming lumps. In other words, this is an example where the metal soap was mixed into the base chemicals, but was not mixed homogeneously.

[0178] <Condition 5> In Condition 5, calcium stearate was thoroughly stirred in a separate container with 15 parts industrial ethanol to 100 parts water, and then added to the base chemicals. Condition 5 is an example in which 5 parts industrial ethanol was subsequently added to the base chemicals and stirred. In the system under Condition 5, the metal soap calcium stearate was already homogeneously mixed with the 15 parts industrial ethanol. Therefore, even when further industrial ethanol was added from that state, it can be said that this is an example in which the mixture remained almost homogeneously mixed.

[0179] The following was learned from these examples of conditions 1 to 5. That is, a suitable amount of lower alcohol, that is, an amount that allows the metal soap to be mixed sufficiently, is first prepared, and a homogeneous solution of the appropriate amount or less of metal soap is added to the main chemical and stirred. In this case, the metal soap can be mixed into a solvent that is mainly water. Furthermore, it was found that if the amount of metal soap is too large to be mixed uniformly with the volume of lower alcohol, it is highly likely that the metal soap will not mix even if additional industrial ethanol is added after it has been added to the basic chemical.

[0180] In the following examples, further examples are provided on the assumption that the chemical is a uniformly mixed chemical containing metal soap. (Example 2: Rapid drying property, application amount, and drying method) In the study group of this Example 2, the chemical was applied to the structure of an oil country pipe thread, and the quality was judged based on the degree of drying. The mixing ratio of alcohol to ammonia water, different types of alcohol, and the size of the metal soap were investigated. The conditions of each of the following chemicals were systematically changed to investigate rapid drying property.

[0181] The solvent was composed of alcohol and aqueous ammonia relative to 100 parts water, and the solid lubricant was composed of metal soap and alkaline soap. The binder resin was a copolymer prepared by blending 100 parts by weight of acrylic acid with 6 parts by weight of polyvinyl alcohol as the monomer. The polyvinyl alcohol was, for example, saponified polyvinyl acetate obtained by polymerizing vinyl acetate monomer with poval. The blending ratios corresponded to the contents of this study. For the solvent system, when the solvent (water) was taken as 100 parts (measured by volume and converted to weight with a specific gravity of 1), various blending conditions were prepared for industrial ethanol and aqueous ammonia.

[0182] Additionally, we prepared samples with different total weights of solid lubricant (metal soap + alkali soap) and binder resin, different blending balances with the solvent, and different weight ratios of metal soap and alkali soap in the solid lubricant coating. Furthermore, we prepared samples with different sizes of metal soap. We then examined the drying conditions for each. For the blending method, sodium stearate was blended and mixed just before the final blend. Finally, ammonia water (approximately 28%) was added at the end to adjust the pH to 6.5-8.5. We used the method identified in the study group of Example 1 above, namely, mixing the metal soap with "lower alcohol (ethanol: Example 1)" beforehand and then mixing it in. "Industrial ethanol" here refers to highly pure ethanol. However, it refers to ethanol containing methanol or isopropyl alcohol at levels not subject to the Liquor Tax Act.

[0183] The common experimental conditions were: the oil well pipe screw material was carbon steel, L80 grade, size was 5.5" 23#, and the screw was JFEBEAR. TM A pin screw with a short length of 700-1000 mm and machined on both ends was prepared. To apply the agent, a regular paint brush (Japanese standard: No. 20 brush, 50 mm width) was first dipped in the agent. The short pin was then placed on two rollers that rotated at the same rate, and the agent was applied while rotating at a speed of about 10 to 20 seconds per rotation (see Figure 8). The two rollers were two axially rotating rollers that came into contact with a 5.5" 23# pin screw at approximately the 5 o'clock and 7 o'clock positions. The brush 30 was moved in the longitudinal direction of the pipe 31, with the brush 30 contacting perpendicularly to the rotation of the screw, and sweeping only once in one direction, so as not to coat the same part of the screw at the same position of the brush. The coated areas were the entire screw, the end face of the tip of the pin screw, about 10 mm inward, and up to about 30 to 50 mm of the non-threaded area at the end of the thread (runout portion). Both ends were evaluated as one set. Note that the brush will inevitably paint about 10 mm inward as it wraps around. The non-threaded area of ​​about 30 to 50 mm will inevitably be painted as the brush will wrap around.

[0184] First, as an example of leaving to dry in the air, one side was painted and then left. Subsequently, as an example of leaving to dry in the air, the other side was painted while rotating in the same way, and while continuing to rotate, the hand dryer was operated in atmospheric air blowing mode with a two-stage airflow rate setting at the lowest, for example, 1 m / sec, to dry. The drying time was then recorded. After that, the rotation of the pipe was stopped, and the drying time for the stationary drying side was also recorded. When touched with a hand, if no fingerprints remained and the surface was not sticky, it was judged to be dry.

[0185] Dryness was judged at the upper part of the pipe, between 8 and 4 o'clock on a clock. The same judgment position was used for the left-to-dry side. When a large amount of coating was applied, the coating liquid accumulated at the 6 o'clock position when left to dry. However, since all but the very surface had already hardened, this judgment standard was used, judging that this was not a problem for the paint drying. If the left-to-dry time was not considered dry within 30 minutes, it was recorded as 30 minutes or more. The indoor temperature on the day was 25-28°C, and it remained at approximately that temperature during drying. The forced drying conditions were simply blown air, which is slower and more severe than hot air blowing conditions. However, if these drying conditions were acceptable, any forced drying conditions could be judged as acceptable, so this was considered to be the most severe possible condition.

[0186] The application weight was calculated from the difference in brush weight. However, because the agent had low viscosity and high fluidity, it appeared as if semi-dried paint had accumulated at the 6 o'clock position, especially on the side that was left after application. Ultimately, some dripping occurred from the 6 o'clock position, but this amount was ignored and the application amount was calculated as the difference in brush weight before and after application. Furthermore, the viscosity of the liquid was approximately 850 mPa·sec, with some exceptions, and did not change significantly under any condition. The exceptions were when the solvent blend ratio was increased, falling below 850 mPa·sec. Examples of low fluidity include Nos. 2-10 to 2-14 below. An example of an increase in the solvent blend ratio would be when a thinly mixed agent with a water-based solvent was used.

[0187] In the following examples, we will explain the film weight but will not discuss the film thickness. There was only one example where film thickness was measured, and cross-sectional microscopy was performed on No. 2-5. The pin thread shape of the oil well pipe thread had a root of 20 to 50 μm and a crest of approximately 20 to 40 μm. Furthermore, the stabbing flank (the vertical wall of the thread that contacts when tightening) and the load flank (the vertical wall of the thread that contacts when loosening) were 5 to 10 μm. Depending on the brush contact, for example, there was variation in the brush joint. The brush joint refers to an unsteady portion, such as when the brush is re-dipped in the agent and re-applied, or when the brush is pressed hard to squeeze out the coating liquid when the coating liquid flow rate is low. Therefore, in the study of this example, the brush was applied, and the pipe itself was rotating. This was intended to achieve a uniform coating. However, because the viscosity of the liquid itself is low, a film forms from the dry areas, but on the other hand, the paint that has not dried tends to accumulate in the undried areas due to rotation. In other words, the paint moving to the grooves of the thread roots appears to be the cause of this difference in film thickness. The characteristics were evaluated with this level of film thickness difference. However, when evaluating the drying itself, as long as the pipe is rotated, there is a high tendency for the paint to dry uniformly, so the completion of drying was determined by the drying time of the slowest part.

[0188] The details are shown in Tables 1 to 3. These are examples of investigations into drying time. Note that the lubrication characteristics of oil country pipe threads, as represented by the number of M / Bs, are not subject to evaluation and judgment in Tables 1 to 3. "*" in the tables means that it is outside the specified range. "**" means that it is outside the preferred range. The evaluation here was made according to the following criteria: Inventive example (drying OK) / Inventive example (△: drying time outside the preferred range) / Comparative example.

[0189] The examples of the present invention (drying OK) were determined to have drying times within the appropriate ranges defined in claims 10 and 11 of the present application, and also to satisfy the ranges defined in claims 1 to 9. The examples of the present invention (△: drying time outside the preferred range) include cases where the conditions are not acceptable in terms of drying time. In other words, they are outside the preferred range. However, they are within the inventive range defined in this disclosure. However, no tightening / retraction test is shown. The comparative examples include cases where the drying time is not acceptable, or where the formation of the solid coating is not satisfactory and passing the M / B number is not expected. As a result, the tightening / retraction test itself is difficult, resulting in an inadequate result. Furthermore, they refer to cases where the inventive range defined in this disclosure is not acceptable.

[0190]

[0191]

[0192]

[0193] No. 2-1 to No. 2-3 are examples that do not contain alkaline soap. At the same time, No. 2-1 is also an example that does not contain alcohol or aqueous ammonia as a solvent. No. 2-1 examines the drying state of the binder resin (acrylic acid and vinyl alcohol copolymer) examined in the examples, slightly exceeding the limit for thick coating. This represents the drying characteristics of the binder resin with this formulation. This corresponds to a comparative example. Specifically, the solvent is water alone, without alcohol or aqueous ammonia. Because it is water alone, calcium stearate, which is characterized by its water-repellent properties, may not be homogeneously dispersed and dissolved even at the chemical stage. As a result, even when a solid coating is formed, much of the calcium stearate component is not incorporated into the film but remains on top of the film, making it unsuitable as a solid lubricating coating. This example also requires a long drying time, making it a comparative example.

[0194] In both No. 2-2 and No. 2-3, the volume ratio (Vol / Vol) of ethanol to water is 6:100. The former does not contain aqueous ammonia, while the latter contains aqueous ammonia at a ratio of 0.5. In both cases, the application amount is within the target range, and both the blown air drying and the standing drying met the target values. In other words, they are examples of the present invention (drying OK). No. 2-3 has a slightly shorter drying time, which is an improvement. This suggests that the inclusion of aqueous ammonia may have contributed to a more or less favorable progress in volatility.

[0195] No. 2-4 is a case where a small amount of alkaline soap component was added compared to No. 2-3. Metal soap (calcium stearate) and alkaline soap (sodium stearate) were added in a weight ratio of 99:1. Its drying time was comparable to that of No. 2-3 and is an example of the present invention. No. 2-5 is a case where the ammonia water of No. 2-4 was replaced with the primary amine methylamine. Its drying performance was similar to that of No. 2-4 and is an example of the present invention. The above-mentioned No. 2-4 and Nos. 2-6 to 2-9 are cases where the proportion of industrial ethanol was increased, respectively, to 6, 10, 25, 25, and 43 parts per 100 parts of water. Furthermore, these cases correspond to ammonia concentrations of 0.5, 1.0, 1.0, no addition, and 2.0 parts, respectively.

[0196] Generally speaking, the drying time was shorter for Nos. 2-4, 2-5, 2-7, and 2-8, 2-9, in that order, whether drying by air drying or standing. This example shows that the more industrial ethanol used, the faster the drying. All of these are examples of the present invention (drying OK). Example No. 2-7 shows that drying can be enhanced without ammonia, simply by the volatilization ability of industrial ethanol. From examples Nos. 2-4, 2-5, 2-6, and 2-8, it can be interpreted that ammonia has a positive effect on rapid drying. Furthermore, example No. 2-9 is an example where the sum of alcohol and ammonia water is 45 parts by volume relative to the water volume, meaning that there are no problems with drying up to this range.

[0197] Cases No. 2-10 to No. 2-15 are the results of examining the weight ratio of solvent to solid content (weight of solid lubricant components + total weight of binder resin). Note that the weight of solvent refers to the weight change when the volume of a solvent consisting of water, alcohol, and ammonia is assumed to have a specific gravity of 1. No. 2-10 to No. 2-11 are cases examined where the volume of industrial ethanol is 25 parts per 100 parts of water. No. 2-12 to No. 2-15 are cases examined where the volume of industrial ethanol is 40 parts. The former group includes cases where the weight ratio of solvent to solid content is 0.7 and 30, respectively. The latter group includes cases where the weight ratios are 20, 50, 100, and 130, respectively.

[0198] When the weight ratio of solvent to solids is up to 100, the target drying time of this disclosure is met, and the examples are examples of the present invention (drying OK) (Nos. 2-11 to 2-14). On the other hand, in the case of No. 2-15, where the ratio exceeds 100 and is 130, the drying time during standing does not meet the target, and the example is an example of the present invention (△: drying time outside the preferred range). This means that although the drying time standard is not met, the basic structure of the present disclosure is satisfied. However, the lubrication behavior is not listed in Example 2.

[0199] Nos. 2-16 to 2-20 are the results of investigations when the alkaline soap content was increased. These are cases where the amount of solvent was relatively high (solvent weight ratio was 2.5) and the alcohol content was also high. The weight ratios of metal soap to alkaline soap were 99:1, 99:1, 95:5, 90:10, and 80:20, respectively. Furthermore, the application amounts differ between No. 2-16 and 2-17, with the former being 6g and the latter being 12g, and the latter being 0.1g / mm2, which was the target application amount. 2 This is also a case where the number slightly exceeded this.

[0200] No. 2-16 and 2-17 cleared the standard for blow drying. However, when left to dry, the former cleared the standard, while the latter did not. The latter was applied with twice the amount of paint than the former, so it is presumed that the drying time exceeded the standard. The amount of paint applied was the specified value: 0.1 g / mm 2This suggests that if the drying time exceeds 100%, the drying time may not meet the criteria for the preferred range, especially when left to dry. The former corresponds to an example of the present invention (drying OK), while the latter corresponds to an example of the present invention (△: drying time outside the preferred range). This is because, except for the preferred drying time, the range specified in the present application is met.

[0201] No. 2-18 is an example where the alkaline soap content is at the upper limit of the specified value. Although the drying time is longer than No. 2-15, it still meets the target. It is an example of the present invention (drying OK). On the other hand, Nos. 2-19 and 2-20 exceeded the target, containing too much alkaline soap component (sodium stearate), increasing the viscosity of the solvent and making it difficult to apply evenly. Furthermore, even after application, it took too long to dry, failing to meet the target value. This shows that adding too much alkaline soap is not a good idea. In particular, No. 2-20 is an example where the drying time exceeded the standard for the preferred range and the viscosity increased too much, making it difficult to apply evenly. No. 2-20 had unevenness and dripping, resulting in very slow drying in some areas, making it impossible to accurately determine the drying time. Therefore, Nos. 2-19 and 2-20 are comparative examples.

[0202] Cases No. 2-21 to 2-26 are a series of investigations into lower alcohols. No. 2-21 is methanol, No. 2-22 to 2-24 are isopropyl alcohol, No. 2-25 is normal propyl alcohol, and No. 2-26 is isobutyl alcohol. Nos. 2-22 to 2-24 are the results of an investigation that also investigated the effect of the film thickness of the solid lubricant coating (solid lubricant coating).

[0203] Nos. 2-21 to 2-25 are examples of compounds with up to 3 carbon atoms. When using methanol, ethanol (Nos. 2-2 to 2-20), isopropyl alcohol, or normal propyl alcohol, the metal soap content is the specified amount. At the same time, the target film thickness is 0.1 g / mm 2This indicates that the drying target can be met if the following conditions are met. Nos. 2-21 to 2-23 and 2-25 are examples of the present invention (drying OK). On the other hand, No. 2-24 is a case where the film thickness exceeded the target value using isopropyl alcohol, and the target value for the preferred drying time range was not met. Since the basic structure of the present disclosure is satisfied (experimental data omitted), this is an example of the present invention (△: drying time outside the preferred range).

[0204] No. 2-26 was an example of isobutyl alcohol with four carbon atoms. A problem that arose even before application was that the metal soap did not mix well with the aqueous solvent when the agent was formulated, and so this was designated a comparative example. As the number of carbon atoms increases, the ability to dissolve in water gradually deteriorates. From this, even if the metal soap can be uniformly dispersed and dissolved in isobutyl alcohol, if this is dispersed and mixed in water and considered as a paint, the following can be said. In other words, it is presumed that the dissolved isobutyl alcohol and metal soap did not mix well with the water-based solvent. Therefore, before discussing the drying time, this was positioned as a comparative example because a uniform coating film was not formed.

[0205] Cases No. 2-27 to 2-33 are the results of investigating the effects of the type of metal soap and alkaline soap, and the particle size of the metal soap. No. 2-27 to 2-29 are cases of calcium stearate and sodium stearate. No. 2-30 is a case of zinc stearate and sodium oleate. No. 2-31 is a case of magnesium stearate and potassium stearate. No. 2-32 is a case of calcium montanate and sodium 12-hydroxystearate, and No. 2-33 is a case of calcium behenate and sodium laurate. The effects of fine particles of metal soap were also investigated.

[0206] As in Example No. 2-29, when the particle size of the metal soap is 25 μm, the drying time exceeds the specified range. However, in the other examples where the particle size is 10 μm or less, the drying time meets the preferred range and rapid drying is possible. In other words, although adding metal soap tends to intensify drying, keeping the particle size 10 μm or less tends to meet the drying time target. Furthermore, it was found that the types of metal soap and alkaline soap can be applied without any particular problems within the scope of this disclosure.

[0207] No. 2-29 can be judged as an example of the present invention (△: drying time outside the preferred range), while Nos. 2-27 to 2-34 are examples of the present invention (drying OK). The reason why No. 2-29 is an example of the present invention (△: drying time outside the preferred range) is as follows: the metal soap (calcium stearate) is 25 μm, and as mentioned above, there are often regions where the film thickness on the vertical wall portion, stabbing flank, and load flank of the oil country pipe thread is smaller than the particle size of the metal soap. For this reason, it is possible that the integrity of the film cannot be maintained at all times during lubrication, and that problems may arise with long-term rust prevention.

[0208] (Example 3: Effect of each condition on lubricity) The study group of this Example 3 explains the invention by examining the lubrication behavior through a weight-tongs test, in which a coating of agent was applied to the structure of an oil country pipe thread and a film was formed. The weight was applied in its entirety during tightening. On the other hand, during untightening, the weight load was reduced to nearly zero, and the thread was lifted by the overhead crane 20 shown in Figure 5, in order to simulate wobble. Various combinations of conditions were systematically prepared for study, and the lubrication behavior, that is, the number of M / B runs, was used to determine whether or not the test was successful. Reflecting the results of the study in Example 1, the metal soap component was dispersed and uniformly dissolved in a lower alcohol in advance to ensure homogeneous dispersion, and then used as the agent.

[0209] As already mentioned above, the criteria for judging the lubrication properties using weight tongs were that a casing size was judged to pass if it could be tightened and loosened three times or more. A tubing size was judged to pass if it could be tightened and loosened five times or more. Furthermore, judgment was made by drawing a line between casing sizes of 7 inches or more and tubing sizes of less than 7 inches. In thread test standards such as API-5C5, the standard for tubing-equivalent materials with conventional lubrication requirements that use an API-mod compound is to achieve 10 or more M / B cycles. However, with a solid lubricating coating, the film itself inevitably wears away gradually, so the number of cycles tends to decrease. Therefore, in this application, the pass range is set at 5 or more cycles.

[0210] In addition to the number of M / B times, once the screw was completely loosened after tightening, the pin was released to the top. Then, the pin thread surface and the box thread surface were observed after air blowing to directly visually confirm whether or not there was seizure. In addition, a torque turn chart was checked to confirm whether there were any abnormalities. The judgment method was as follows: If the screw did not loosen during the tightening and loosening of the M / B number of times, it was judged that seizure had occurred at that tightening and loosening count, and the number of tightening and loosening was judged as the previous number.

[0211] For those that were completely loosened and the surface could be observed, if there was any seizure, even slight, in the sealing area, it was judged as NG. Then, the number of tightening / rewinding attempts was judged to be the next time seizure occurred, and the number of tightening attempts using the weight tongs was recorded on the spot, and the tightening / rewinding test was completed. If there was very slight seizure in the threaded area rather than the sealing area, it was repaired and the test continued as is. The number of tightening / rewinding attempts performed in this way was used to sort the results into good and bad according to the judgment criteria described above. The conditions and results are shown in Tables 4 to 12. The symbol "*" next to each parameter in the tables means that it is outside the specified range. The symbol "**" means that it is outside the preferred range.

[0212]

[0213]

[0214]

[0215]

[0216]

[0217]

[0218]

[0219]

[0220]

[0221] The "Solid lubricant coating A with pencil hardness 3H" that appears frequently in the table is as follows: In the case of carbon steel, it is a manganese phosphate conversion coating, and in the case of stainless steel, it is a solid lubricant coating formed on top of a base layer of Cu-Sn electroplated film (Sn: 45-47%). In these cases, the binder resin is a polyamideimide film, and the solid lubricant is PTFE and a trace amount of MoS. 2 The structure can be considered to be nearly uniformly dispersed from the total thickness (1-3%). This refers to a solid lubricant coating with a thickness of 50-80 μm. The film thickness is the measured value of the film thickness on the thread. It refers to the same solid lubricant coating, including the pencil hardness of 3H. The film thickness distribution on each part of the thread is as follows. Specifically, the thread design of oil country pipe threads has an inverted hook structure. For this reason, even if a uniform film thickness is aimed for by applying chemicals in an ingenious way, the film thickness on the vertical wall parts of the threads at the load flank and stabbing flank inevitably tends to be less. However, by innovating the solid lubricant coating formation, it was possible to ensure a film thickness of more than half the measured film thickness on the vertical wall parts of the thread.

[0222] No. 3-1 to 3-12 are made of carbon steel P110 material, 7"38# JFELION TMThe chemical agent used for the screws was a styrene-acrylic acid copolymer (500 parts by weight of styrene for 100 parts by weight of acrylate). This is an example where this was applied to the pin thread side. The box thread side was also coated with the above-mentioned "Solid Lubricant Coating A with a pencil hardness of 3H." In this case, a manganese phosphate conversion coating was applied to the base. A tightening / loosening test was conducted using a 2-ton weight, equivalent to the tightening force when three screws are connected, to determine whether or not the test was successful.

[0223] In Examples No. 3-1 to 3-8, the solvent was composed of 15 parts industrial ethanol and 2 parts aqueous ammonia per 100 parts water by volume. The blending ratios were also the same, and the blending conditions were the same within the specified range. The study cases differed in the size of the metal soap, the presence or absence of alkaline soap, and the film thickness. Examples No. 3-1 to 3-4 were cases in which the particle size of the metal soap (calcium stearate) was 5 μm, 1 μm, 10 μm (this example was the only one that did not contain alkaline soap), and 10 μm, respectively. Examples No. 3-1, 3-2, and 3-4 showed good lubrication behavior with more than 10 M / B cycles using weight tongs (topped at 10 cycles), and are examples of the present invention. Example No. 3-3 was only M / B three times, and is also an example of the present invention. However, Example No. 3-3 was different from Example No. 3-2, which contained alkaline soap components. The lubrication properties were worse than those of 3-1, 2, and 4. This indicates that the addition of alkaline soap is effective in improving lubrication.

[0224] In Nos. 3-5 to 3-8, the metal soap size was 25 μm. However, the solid lubricant coating thicknesses were 20 μm, 50 μm, 100 μm, and 180 μm, respectively. Furthermore, the drying times for these cases were 7 minutes of air drying, 23 minutes of air drying, 8 minutes of hot air drying, and 10 minutes of hot air drying, respectively. Nos. 3-7 and 3-8 were dried using a hot air blower (1000 W output). Generally, the drying times tend to be longer than those for Nos. 3-1 to 3-4. This change is thought to be due to the larger solid lubricant film and the particle size of the metal soap. Smaller, more dispersed metal soap particles increase the surface area and the number of drying points within the film. As a result, accelerated drying can be expected. However, in these cases, this was not possible due to the larger particle size, and this can be explained by the increased volume required for drying due to the film thickness.

[0225] No. 3-5 is an example where the film thickness is 20 μm, and the size of the metal soap is large compared to the film thickness. These are examples where the film integrity is difficult to maintain when the metal soap is larger than the film thickness, resulting in destruction and seizure in those areas. No. 3-6 (film thickness 50 μm) corresponds to an inventive example with six or seven M / B cycles. Nos. 3-7 and 3-8 are examples where the influence of film thickness was investigated. In the former, the number of M / B cycles was met with a film thickness of 100 μm, but in the latter, with a film thickness of 180 μm, some M / B cycles did not meet the standard of three. This shows that lubrication performance can deteriorate when the film thickness exceeds 100 μm.

[0226] Nos. 3-9 and 10 are comparative examples where the drying method was changed. These will be explained in comparison with No. 3-1. No. 3-1 above is an example where the number of M / Bs was more than 10 (it was capped at 10). No. 3-9 is the same up to the point where one coat was applied with a brush while the pipe was rotating. However, in this example, only the pin thread pipe was rotated and allowed to dry in the air, and it dried in 15 minutes. In No. 3-10, after the spin coating, the rotation was stopped and the pipe was left to dry in a stationary state, and it took extra time to dry.

[0227] As mentioned above, the drying assessment was performed on the upper side of the pipe from the 8 o'clock to 4 o'clock positions. This assessment was possible because the lower part of the coating film had already formed a film, which could be estimated by the drying from the 8 o'clock to 4 o'clock positions. Furthermore, in this case, the 5 o'clock to 7 o'clock positions, where the liquid pools were present, were also dry on the surface, but not completely dry to the inside, so corrosion resistance could be considered acceptable. As shown in this example, the lubrication behavior was slightly inferior to that of Nos. 3-1 and 3-9, but still within the acceptable range. The lubrication performance could be considered excellent, making this an example of the present invention. This is because the agent had low viscosity, resulting in high fluidity, which appeared to correlate with the fact that the paint that was not completely dry at the end of application moved along the threads (dripping). The 5 o'clock to 7 o'clock positions were dry on the surface, but this could be attributed to the influence of the paint not yet completely dry to the inside, but still within the acceptable range.

[0228] Cases No. 3-11 and 3-12 are cases where the binder resin contained a binder resin component other than an acrylate or methacrylate. Cases No. 3-11 and No. 3-12 are cases where 11 parts by weight and 35 parts by weight of water-soluble phenolic resin were mixed, respectively, per 100 parts by weight of binder resin components other than methacrylate. The former are examples of the present invention, while the latter are comparative examples, in which the amount mixed exceeded the upper limit of the standard.

[0229] The weight percentages of binder resins other than acrylate or methacrylate resins in the total binder resin are 90% and 74%, respectively (less than the standard 90%). The former meets the M / B count requirement and is an inventive example. The former is an example with a solvent / (solid lubricant + binder resin) blend ratio of 1.8, a solid lubricant / binder resin weight ratio of 0.12, and a viscosity of 650 mPa·sec. The latter are examples with viscosities of 1.8, 0.12, and 1300 mPa·sec, respectively. On the other hand, the latter was applied with a target thickness of 25 μm, but did not dry completely. Furthermore, even after waiting overnight after application, it did not dry and remained semi-wet, making it impossible to perform a tightening / untightening test, and was therefore considered a comparative example.

[0230] The examples of No. 3-13 to 3-17 are made of carbon steel Q125 material, 9-5 / 8" 53.5# JFELION TM The chemicals used for the threads were vinyl acetate-butyl acrylate and polyvinyl polymer (420:100:75). This example shows a case where this was applied to the pin thread side. The box thread side was also coated with the above-mentioned "Solid Lubricant Coating A with a pencil hardness of 3H." A manganese phosphate conversion coating was then applied to the base under these conditions. A tightening / untightening test was conducted using a 3-ton weight, equivalent to the tightening force when three threads are connected, to determine whether or not the test would be successful. This example shows a study where the amount of lower alcohol (ethanol) added was increased to increase volatility and strengthen drying.

[0231] The solvents used were 35, 35, 35, 45, and 60 parts industrial ethanol per 100 parts water, respectively. The application methods were, in order, spin coating / air drying, spin coating / air drying, static application (hand coating) / static drying, spin coating / static drying, and static application (hand coating) / static drying. Only No. 3-17, which contained 60 parts lower alcohol, exceeding the standard limit of 45, failed to meet the tightening / retraction number standard. When tightening / retraction tests were performed using weight tongs, the results were 5, 1, and 2 times, which were acceptable, but the overall M / B number was poor. Therefore, it was selected as a comparative example. This suggests that the coating may dry too quickly, resulting in inconsistent film thickness. Furthermore, the flash point is 40°C, and assuming application at the wellhead, there is a risk of an explosion or other accident, which is why it can be deemed a failure.

[0232] In the other cases, the number of M / B cycles met the pass standard criteria. The reason why the number of M / B cycles in No. 3-13 was limited to the lower limit of 3 is presumably because the solid lubricant / binder resin ratio exceeded the preferred range of 1.0. It is presumed that this is due to the slightly inferior film integrity in solid lubricant films containing a large amount of solid lubricant. Furthermore, from the study examples No. 3-15 to 3-17, the cases where the coating was applied by hand and / or left to dry (without air blowing) tended to have slightly lower M / B cycles. It is presumed that this is due to uneven film thickness caused by the wet chemical gradually flowing down and forming a film at the 6 o'clock position during drying.

[0233] The examples of No. 3-18 to 3-34 are made of martensitic stainless steel HP2-13CR-110 (13Cr-5Ni-2Mo type), size: 9-5 / 8" 43.5# JFELION TM The agent used for the threads was ethylene-methacrylic acid copolymer resin. However, the ethylene in this case was a polymerized ethylene-methacrylic acid based on a random copolymer of ethylene oxide and propylene oxide, and this example was formed on the pin thread side. The box thread side was formed under the conditions of "Solid Lubricant Coating A with a pencil hardness of 3H," with a Cu-Sn binary electroplated indicator film formed on the base. A tightening / untightening test was conducted using a 2-ton weight to determine whether or not the test was successful, and the applied weight was equivalent to the tightening force when connecting just under three wells in an actual well.

[0234] Nos. 3-19 to 3-22 and 3-24 to 33 were within the acceptable range for the number of tightening / retraction operations in the weight-tong tightening / retraction test, and are examples of the present invention. Nos. 3-18, 3-23, and 3-34 are comparative examples. Nos. 3-18 to 3-21 are examples investigating the lower limit of the lower alcohol content. No. 3-18 is an example of a purely water-based solvent without added alcohol. It was dried with hot air at 100°C, and the drying time was not particularly long. However, it failed the weight-tong tightening / retraction test after only one attempt, making it a comparative example. Because the solvent was water only, the metal soap, the main component of the solid lubricant, is water-repellent. This, in part, may be related to the inhomogeneous film quality even after the solid lubricant film is formed due to the inability to disperse uniformly.

[0235] Nos. 3-19 to 3-21 are examples where the industrial ethanol content is 0.5, 1, and 5, respectively. It can be seen that the M / B count was within the acceptable range from No. 3-19 (industrial ethanol: 0.5). Nos. 3-22 to 3-24 are examples where a third solid lubricant other than metal soap and alkali soap was added, with graphite, graphite, and BN added, respectively. Nos. 3-22 and 3-24, which were adjusted within the specified range, had an acceptable M / B count and are examples of the present invention. No. 3-23 is an example where the third solid lubricant (graphite in this case) was included in a large amount, and the metal soap and alkali soap exceeded the specified weight percentage of the total solid lubricant. In these examples, the M / B count did not meet the acceptable criteria and was rejected, corresponding to a comparative example. In reality, the graphite formed a tape-like product exceeding 20 mm in length along the groove of the thread, which caused seizure.

[0236] Cases No. 3-25 to No. 27 use the same solvent, binder resin, and solid lubricant, but the application and drying methods were changed to compare cases where the solid lubricant coating was completely dried and cases where some semi-dried areas remained. No. 3-25 is a case where the coating was applied with a brush while the pipe was rotating, and then air-dried while the pipe was still rotating. The completely dried film passed the M / B test using weighted tongs and is an example of the present invention. No. 3-26 and No. 27 follow the same process as No. 3-25 up to the application stage, but the drying method is different; the solid lubricant coating was formed by leaving it to dry. No. 3-26 is a case where the coating was completely dried, while No. 3-27 appears to have some insufficiently dried areas. To be precise, there are some areas of the liquid paint that have not completely dried between the 5 and 7 o'clock positions. Furthermore, the paint film formation (drying) begins with the outermost layer (the surface in contact with the atmosphere) and the surface in contact with the screw steel, so in this case, a semi-dried portion remains near the center of the film thickness. This is an example where the contact surface between the screw and the paint film is also dry. Although the application and drying times were the same, there was some variation in the application method, which is presumed to have had an effect, but there were no problems with lubrication, and both are examples of the present invention.

[0237] Cases No. 3-28 to No. 3-32 compare the effects of the weight ratio of the solvent to the total weight of the solid lubricant and binder resin (calculated assuming the specific gravity of the solvent is 1) and the weight ratio of the solid lubricant to the binder resin. Both parameters were examined under the following conditions: 100-0.6, 150△-5.0△, 0.7-0.1, 0.5▽-0.08▽, and 0.6▽-1.1△. △ indicates exceeding the upper limit of the preferred range, and ▽ indicates reaching the lower limit of the preferred range. All conditions are examples of the invention. Those within the preferred range showed a good number of M / B cycles, with No. 3-28 reaching six cycles and No. 3-30 reaching ten cycles. However, those exceeding the preferred range only achieved lubrication performance of around three or four cycles.

[0238] Cases No. 3-33 and No. 3-34 are examples in which a solvent other than water and alcohol was added, such as DMSO (dimethyl sulfoxide). In the former case, 6 parts by volume of DMSO was added to a base agent with 14 parts industrial ethanol, assuming a volume of water of 100. Furthermore, these cases are examples in which the volume of water and lower alcohol constitutes 95% of the total solvent weight, and other solvents constitute 5%, representing a study of the solvent composition limits of the present application. These cases involve the use of a stable, non-volatile polar solvent, which can be dried in about 5 minutes with hot air drying. However, these cases do not dry within the specified 5 minutes with air drying at room temperature, and cannot be dried for 30 minutes even when left to dry. If a film can be formed, the lubrication level targeted by the present application can be met, and therefore are examples of the present invention.

[0239] On the other hand, No. 3-34 is a case in which even more DMSO was added, and the solvent contained a large amount of DMSO with a high boiling point (approximately 190°C). Therefore, it did not dry even when left to dry in the air or when blown dry (including hot air), and could not form a film. It could be formed into a film by heat treatment at 200°C or higher. However, due to the low viscosity of the formulated solvent, it was not possible to instantly form a film during the baking process, and dripping occurred even during baking. Specifically, a thick film formed at the 6 o'clock position, filling the pin thread valleys in some places, and in some places, further dripping occurred, leading to the formation of droplet-like film protrusions. As a result, even when a tightening / untightening test was performed, the required number of times was not reached, and seizure occurred, making it an NG and comparative example. These considerations indicate that the solvent must be composed of 95% or more of water and lower alcohol.

[0240] Cases No. 3-35 to 39 are made of carbon steel T95, size 5.5" 23# JFELION. TM In this example, the screw was treated with a mixture of diacetone acrylamide (DAAD: a type of acrylate) and a polymer of diphenylmethane diisocyanate (MDI: a urethane compound) at a ratio of 40 parts by weight to 100 parts by weight of the acrylate DAAD. The box screw was coated with a "solid lubricant coating A with a pencil hardness of 3H," with a Cu-Sn binary electroplating indicator film formed underneath. A tightening / untightening test using a 1-ton weight was conducted to determine whether the test was successful, and the applied weight was equivalent to the tightening force applied when connecting just under three wells in an actual well.

[0241] Nos. 3-35 to 3-39 are examples in which solid lubricating coatings were formed using different coating and drying methods. The five examples are, in order, spin coating - spin-transfer air drying, spin coating - static drying, static hand coating - static drying, spin coating - spin-transfer air drying, and spin coating - spin-transfer air drying. The weight tong M / B times were, in order, ≥ 10 times (stopped at 10 times), ≥ 10 times (stopped at 10 times), 9 times, 8 times, and 9 times. All passed and are examples of the present invention. Compared to Nos. 3-1 to 3-34, the use of smaller diameter materials resulted in a smaller tightening torque, indicating that they were not significantly affected by uneven film thickness distribution due to static hand coating or static drying. In Nos. 3-38 and 39, metal soap was used, and No. This is an example using a different type of metal soap than the calcium stearate and calcium / zinc stearate (mixture) used in examples 3-1 to 3-37. The former uses zinc stearate, and the latter uses barium stearate. In both cases, the other requirements are within the specified range, and the M / B count is within the acceptable range, making them examples of the present invention.

[0242] The examples of No. 3-40 to 3-43 are made of carbon steel T95, and the size is 3.5" 9.2# JFEBEAR. TM This example uses a copolymer of acrylic acid and polyvinyl acetate as a chemical agent for screws. It also uses a chemical agent where 30 parts by weight of polyvinyl acetate is mixed with 100 parts by weight of acrylic acid. In this example, "Solid Lubricant Coating A with a pencil hardness of 3H" is used on box screws, and the base is coated with a manganese phosphate chemical conversion coating. Other examples include use on pin screws, a case where both thread surfaces are formed using only the chemical agent, and a case where only a manganese phosphate chemical conversion coating is used. A 500 kg weight was applied to conduct a tightening / untightening test to determine whether the test was successful, which corresponds to the weight applied when three pipes are connected in an actual well.

[0243] No. 3-40 is the same as the previous series of examples, except that a solid lubricating coating was applied to the pin thread side and "Solid Lubricating Coating A with a pencil hardness of 3H" was applied to the box thread side. This is an example of the present invention in which the number of M / B cycles was ≥ 10 (maximum 10 cycles). No. 3-41 is an example in which a solid lubricating coating was applied to the pin thread side and the box thread only had a manganese phosphate coating and no "Solid Lubricating Coating A with a pencil hardness of 3H," but it was able to be tightened and untightened three times, making it an example of the present invention. No. 3-42 is an example in which the solid lubricating coating of the present disclosure was applied to both sides of the thread, and it was able to be tightened and untightened five times, making it also an example of the present invention. No. 3-43 is an example in which the box thread had a solid lubricating coating and "Solid Lubricating Coating A with a pencil hardness of 3H" was applied to the pin thread side, making it able to be tightened and untightened ≥ 10 times (maximum 10 cycles), making it also an example of the present invention.

[0244] (Example 4) Results of investigation into corrosion Table 13 shows the results.

[0245] In the corrosion resistance evaluation in this disclosure, a protector used to protect the thread structure of a structure with a thread structure, such as an oil country pipe thread, was tightened and then loosened, and then the protector was removed, and salt spray was then performed on the solid lubricant coating. The evaluation was based on the criteria that the appearance of red rust over the entire surface was considered to be NG. The evaluation was performed using salt spray after inflicting possible damage on the film. Corrosion resistance was examined using some of the materials and conditions examined in Tables 1 to 12. The salt spray conditions were in accordance with JIS K 5600-7-1, using neutral salt spray conditions of 5% NaCl (35°C, humidity 98-99%, spray rate 1-2 mL / Hr / 80 cm). 2 , pH 6.5-7.2) and based on evaluation at 8 hours.

[0246] Here, the metal surface of a metal part (oil country pipe thread surface) that is the subject of this disclosure includes, for example, lathe-machined or machined surfaces, polished surfaces, etc. Note that for the corrosion resistance evaluation, areas with remaining mill scale were excluded. Depending on the roundness and eccentricity of the tubular structure, samples may contain mill scale in the thread structure. However, if the mill scale is cleaned before forming a solid lubricant coating, the water-based agent may penetrate into tiny defects, holes, or scratches in the mill scale. For this reason, when a solid lubricant coating is formed on top of the mill scale, even if the solid lubricant coating is sound, rust spots may appear on the underlying steel. However, such rust spots are not rust on the solid lubricant coating and are therefore excluded from the evaluation.

[0247] The sample numbers in Table 13 indicate the drug compositions based on the ingredients and compositions used in Tables 1 to 12. The application method was different from that of the sample numbers in question; the application was done with a brush while rotating a pipe, and the drying method was rotation and air drying, resulting in complete drying. All materials were L80, 3.5" 9.2# JFELION. TM This is an example where the test pieces were aligned with the PIN threads (male threads) of the test pieces. After complete drying, a protector made of HDPE resin (high density polyethylene) was used to tighten and loosen the screws once, and then a salt spray test was conducted. As a comparison material, a general-purpose thin steel SPCC material was used, and the pin threads were coated with the agents Nos. 3-1, 13, 17, 20, 38, and 42. However, the comparative SPCC material was not coated with rust preventative oil, and the same process as tightening and loosening the protector once was not performed. The results clearly show that all of the materials coated with the agent of this application have excellent corrosion resistance.

[0248] (Other) The present disclosure may also have the following configurations: (1) An agent for forming a solid lubricating coating on a metal surface, comprising a solid lubricant, a binder resin, and a solvent as its main components, the solvent being primarily water to which a lower alcohol having 3 or fewer carbon atoms has been added as an additive, the volume of the additive being 0.5 to 45 parts by volume per 100 parts by volume of water in the solvent, the water and the additive accounting for 95% or more by volume of the solvent, the solid lubricant containing a soap component containing at least a metal soap from among a metal soap and an alkali soap component, the metal soap component accounting for 95% or more by weight of the total weight of the metal soap and alkali soap components, the particle size of the metal soap not exceeding the film thickness of the solid lubricating coating, the binder resin being composed of a water-soluble or water-dispersible polymer and copolymer, and the polymer and copolymer having an acrylate or methacrylate structure accounting for 90% or more by weight of the binder resin. (2) The additive further contains at least one of aqueous ammonia and a primary amine. (3) The lower alcohol is one or more lower alcohols selected from methanol, ethanol, isopropyl alcohol, normal propyl alcohol, and industrial ethanol, and the volume of the lower alcohol is 0.5 or more per 100 parts by volume of water in the solvent. (4) The metal soap and alkali soap components constituting the solid lubricant include one or more soaps that are compounds consisting of a fatty acid selected from Group A below and a metal element selected from Group B below, and the weight of the metal soap is 95% or more of the total weight of the metal soap and the alkali soap. Group A: stearic acid, behenic acid, lauric acid, 12-hydroxystearic acid, oleic acid, montanic acid Group B: Na, K, Mg, Ca, Zn (5) The particle size of the metal soap is 10 μm or less. (6) The water-soluble or water-dispersible polymer constituting the binder resin is a polymer composed of one or more monomers selected from the following (1) to (4), and the copolymer is a copolymer composed of two or more monomers selected from the following (1) to (4):(1) Monomers primarily composed of acrylate, methacrylate, and their respective derivatives. (2) Monomers of acrylate, methacrylate, or their respective derivatives, with monomers containing alkyl esters, vinyl esters, styrene esters, carboxylic acid esters, and their respective derivatives. (3) Monomers grafted onto (1) or (2). (4) Monomers of either or both vinyl compounds and urethane compounds. (7) The flash point of the agent is above 60°C or the agent is flame-retardant. (8) When the specific gravity of the solvent is 1 and the volume of the solvent is converted to weight, the weight of the solvent is 0.7 to 100 times the total weight of the solid lubricant and binder resin, and the weight of the solid lubricant is 0.1 to 1.0 times the weight of the binder resin. (9) The viscosity of the agent is 1000 mPa·sec or less. (10) The amount of coating on the metal surface is 0.1 g / mm. 2 When applied at the following rate, it has the rapid drying property of drying within 30 minutes when left to dry in a windless atmospheric environment at room temperature. (11) When applied at a rate of 0.1 g / mm to a metal surface 2When applied as described below, the agent dries quickly, drying within 5 minutes when dried in an atmospheric environment at room temperature with air blown at a speed of 1 m / sec or more. (12) A method for producing the agent for forming a solid lubricating coating of the present disclosure, in which the metal soap is prepared by dispersing and turbiding the metal soap in a lower alcohol and then adding the mixture to a water solvent. (13) A method for applying the agent for forming a solid lubricating coating of the present disclosure to the surface of a tubular part, in which the agent is applied while the tubular part is rotated about its axis. (14) An oil country tubular good having a lubricating coating formed on a thread portion, wherein the solid lubricating coating comprises a solid lubricant dispersed in a binder resin, the solid lubricant contains a soap component containing at least a metal soap from among metal soap and alkali soap components, the metal soap component accounts for 95% or more of the total weight of the metal soap and alkali soap components, the particle size of the metal soap does not exceed the film thickness of the solid lubricating coating, the binder resin is made of a water-soluble or water-dispersible polymer and copolymer, and the polymer and copolymer having an acrylate or methacrylate structure accounts for 90% or more of the total weight of the binder resin. (15) The metal soap and alkali soap components constituting the solid lubricant include one or more soaps which are compounds consisting of a fatty acid selected from Group A below and a metal element selected from Group B below, and the weight of the metal soap is 95% or more of the total weight of the metal soap and alkali soap. Group A: stearic acid, behenic acid, lauric acid, 12-hydroxystearic acid, oleic acid, montanic acid Group B: Na, K, Mg, Ca, Zn (16) The particle size of the metal soap is 10 μm or less. (17) The water-soluble or water-dispersible polymer constituting the binder resin is a polymer composed of one or more monomers selected from the following (1) to (4), and the copolymer is a copolymer composed of two or more monomers selected from the following (1) to (4).(1) Monomers mainly composed of acrylate, methacrylate, and their respective derivatives (2) Monomers of acrylate, methacrylate, and their respective derivatives, to which alkyl esters, vinyl esters, styrene esters, carboxylic acid esters, and monomers containing their respective derivatives are attached (3) Monomers grafted to the above (1) and (2) (4) Monomers of either or both of vinyl compounds and urethane compounds (18) The solid lubricating coating has a film thickness of 1 μm or more and 100 μm or less, and is soft, having a pencil hardness of H or less (19) An oil country tubular goods threaded joint connecting a box having an internal thread and a pin having an external thread, wherein the oil country tubular goods of at least one of the box and the pin is made of the oil country tubular goods on which the solid lubricating coating of the present disclosure is formed. (20) An oil country tubular goods threaded joint connecting a box having an internal thread and a pin having an external thread, wherein one of the box and the pin is made of an oil country tubular goods on which the solid lubricating coating of the present disclosure is formed, and the threaded portion of the other oil country tubular goods is formed with a coating having a harder coating than the solid lubricating coating.

[0249] The entire contents of Japanese Patent Application No. 2022-134375 (filed August 25, 2022), from which this application claims priority, are incorporated herein by reference. While the present application has described a limited number of embodiments, the scope of the invention is not limited thereto, and modifications of each embodiment based on the above disclosure would be obvious to one skilled in the art.

[0250] 1 Pin 1a Threaded portion 2 Box 2a Threaded portion

Claims

1. An agent for forming a solid lubricating coating on a metal surface, comprising a solid lubricant, a binder resin, and a solvent as its main ingredients, the solvent being primarily water to which a lower alcohol having 3 or less carbon atoms has been added as an additive, the volume of the additive being 0.5 to 45 parts by volume per 100 parts by volume of water in the solvent, the water and the additive accounting for 95% or more by volume of the solvent, the solid lubricant containing a soap component containing at least a metal soap from among metal soap and alkali soap components, the metal soap component accounting for 95% or more by weight of the total weight of the metal soap and alkali soap components, the particle size of the metal soap not exceeding the thickness of the solid lubricating coating, the binder resin being composed of a water-soluble or water-dispersible polymer and copolymer, and the polymer and copolymer having an acrylate or methacrylate structure accounting for 90% or more by weight of the binder resin.

2. The agent for forming a solid lubricating coating according to claim 1, further comprising at least one of aqueous ammonia and a primary amine as the additive.

3. A chemical for forming a solid lubricating coating according to claim 1 or claim 2, wherein the lower alcohol is one or more selected from the group consisting of methanol, ethanol, isopropyl alcohol, normal propyl alcohol, and industrial ethanol, and the volume of the lower alcohol is 0.5 or more per 100 parts by volume of water in the solvent.

4. An agent for forming a solid lubricating coating as set forth in any one of claims 1 to 3, wherein the metal soap and alkaline soap components constituting the solid lubricant contain one or more types of soap that are compounds consisting of a fatty acid selected from Group A below and a metal element selected from Group B below, and the weight of the metal soap is 95% or more of the total weight of the metal soap and alkaline soap. Group A: Stearic acid, behenic acid, lauric acid, 12-hydroxystearic acid, oleic acid, montanic acid Group B: Na, K, Mg, Ca, Zn 5. An agent for forming a solid lubricating coating according to any one of claims 1 to 4, wherein the particle size of the metal soap is 10 μm or less.

6. An agent for forming a solid lubricating coating according to any one of claims 1 to 5, wherein the water-soluble or water-dispersible polymer constituting the binder resin is a polymer composed of one or more monomers selected from the following (1) to (4), and the copolymer is a copolymer composed of two or more monomers selected from the following (1) to (4): (1) Monomers mainly consisting of acrylate, methacrylate, and their respective derivatives (2) Monomers in which acrylate, methacrylate, or their respective derivatives is attached with a monomer containing an alkyl ester, vinyl ester, styrene ester, carboxylic acid ester, or their respective derivatives (3) Monomers grafted to the above (1) and (2) (4) Monomers of either or both of vinyl compounds and urethane compounds 7. An agent for forming a solid lubricating coating according to any one of claims 1 to 6, wherein the flash point of the agent is above 60°C or the agent is flame-retardant.

8. An agent for forming a solid lubricating coating according to any one of claims 1 to 7, wherein, when the volume of the solvent is converted to weight assuming a specific gravity of 1, the weight of the solvent is 0.7 to 100 times the total weight of the solid lubricant and binder resin, and the weight of the solid lubricant is 0.1 to 1.0 times the weight of the binder resin.

9. An agent for forming a solid lubricating coating according to any one of claims 1 to 8, wherein the viscosity of the agent is 1000 mPa·sec or less.

10. Coating amount for metal surface: 0.1 g / mm 2 The agent for forming a solid lubricating coating according to any one of claims 1 to 9, which has rapid drying properties, being able to dry within 30 minutes when applied as follows and left to dry in a windless atmospheric environment at room temperature:

11. Coating amount for metal surface: 0.1 g / mm 2 The agent for forming a solid lubricating coating according to any one of claims 1 to 10, which has rapid drying properties, being able to dry within 5 minutes when applied at a temperature below 100°C and dried by air blowing at a speed of 1 m / sec or more in an atmospheric environment at room temperature.

12. A method for producing an agent for forming a solid lubricating coating according to any one of claims 1 to 11, comprising dispersing and turbidifying a metal soap in a lower alcohol, and then adding the resulting mixture to a water solvent to prepare the metal soap.

13. A method for applying a solid lubricating coating forming agent according to any one of claims 1 to 11 to the surface of a tubular part, comprising applying the agent while rotating the tubular part about its axis.

14. An oil country tubular good having a lubricating coating formed on a thread portion, wherein the solid lubricating coating comprises a solid lubricant dispersed in a binder resin, the solid lubricant containing a soap component containing at least a metal soap from among metal soap and alkaline soap components, the metal soap component accounting for 95% or more of the total weight of the metal soap and alkaline soap components, the particle size of the metal soap not exceeding the film thickness of the solid lubricating coating, and the binder resin comprising a water-soluble or water-dispersible polymer and copolymer, and wherein the polymer and copolymer having an acrylate or methacrylate structure account for 90% or more of the total weight of the binder resin.

15. The oil country tubular good according to claim 14, wherein the metal soap and alkali soap components constituting the solid lubricant contain one or more soaps which are compounds consisting of a fatty acid selected from Group A below and a metal element selected from Group B below, and the weight of the metal soap is 95% or more of the total weight of the metal soap and the alkali soap. Group A: stearic acid, behenic acid, lauric acid, 12-hydroxystearic acid, oleic acid, montanic acid Group B: Na, K, Mg, Ca, Zn 16. An oil country tubular good according to claim 14 or 15, wherein the particle size of the metal soap is 10 μm or less.

17. The oil country tubular good according to any one of claims 14 to 16, wherein the water-soluble or water-dispersible polymer constituting the binder resin is a polymer composed of one or more monomers selected from the following (1) to (4), and the copolymer is a copolymer composed of two or more monomers selected from the following (1) to (4): (1) Monomers mainly consisting of acrylate, methacrylate, and their respective derivatives; (2) Monomers in which acrylate, methacrylate, or their respective derivatives is attached with a monomer containing an alkyl ester, vinyl ester, styrene ester, carboxylic acid ester, or their respective derivatives; (3) Monomers grafted to the above (1) and (2); (4) Monomers of either or both of vinyl compounds and urethane compounds.

18. An oil country tubular good according to any one of claims 14 to 17, wherein the solid lubricating coating has a thickness of 1 μm or more and 100 μm or less, and is soft, having a pencil hardness of H or less.

19. An oil well pipe threaded joint connecting a box having a female thread and a pin having a male thread, wherein the oil well pipe of at least one of the box and the pin is made of the oil well pipe described in any one of claims 14 to 18.

20. An oil well pipe threaded joint connecting a box having a female thread and a pin having a male thread, wherein the oil well pipe of one of the box and the pin is made of the oil well pipe described in any one of claims 14 to 18, and the threaded portion of the other oil well pipe is formed with a coating having a harder coating than the solid lubricating coating.