Film and method for producing semiconductor package

MYPI2025001248A0Undetermined Publication Date: 2024-03-01AGC INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025001248
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-01
Filing Date
2023-08-29
Publication Date
2024-03-01

AI Technical Summary

Technical Problem

The separation of release and antistatic layers in complex semiconductor packages often results in the release layer remaining attached to the package, leading to damage and poor mold releasability due to static electricity generation during the peeling process.

Method used

A film with a base material, an antistatic layer, and a release layer, where the elongation rate is between 90% and 255%, and the layers are designed to prevent peeling by ensuring strong cohesive forces and improved adhesion between the antistatic and release layers, using specific polymers and crosslinking agents to enhance interlayer adhesion.

Benefits of technology

The film effectively prevents the release and antistatic layers from peeling off, ensuring reliable semiconductor package manufacturing with improved mold releasability and reduced static-induced damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025001248_DRAWING_001
    Figure PI2025001248_DRAWING_001
Patent Text Reader

Abstract

This film is a film including a base material, an antistatic layer provided on one surface of the base material, and a release layer provided on a surface of the antistatic layer opposite to the base material, and having an elongation rate of more than 90% and less than 255% as measured by a tensile test at 25°C and at a speed of 100 mm / min and determined by the following formula: Elongation rate (%) = (elongation at break (mm)) × 100 / (distance between grips before applying tension (mm))
Need to check novelty before this filing date? Find Prior Art

Description

Film and semiconductor package manufacturing method

[0001] This disclosure relates to a method for manufacturing a film and a semiconductor package. This application claims priority to Japanese Patent Application No. 2022-139307, filed on September 1, 2022, the contents of which are incorporated herein by reference.

[0002] Semiconductor elements are sealed in a package and mounted on a substrate to protect them from the outside air. A curable resin such as epoxy resin is used to seal the semiconductor elements. Resin sealing is performed by placing the semiconductor element in a predetermined location in a mold, filling the mold with curable resin, and then curing it. Transfer molding and compression molding are commonly known sealing methods. When sealing semiconductor elements, a release film is often placed on the inner surface of the mold to improve the releasability of the package from the mold.

[0003] When a release film is used in the manufacture of a semiconductor package, static electricity is generated when the sealed semiconductor package is peeled from the film, causing the film to become charged, and the semiconductor package may be damaged by discharge from the charged film. In order to prevent the film from becoming charged, Patent Document 1 proposes providing an antistatic layer between the substrate and the release layer.

[0004] International Publication No. 2016 / 125796

[0005] In recent years, semiconductor package shapes have become more complex, and semiconductor packages with exposed portions have an increased height difference, leading to an increasing use of films that conform to complex shapes. The present inventors have found that when the film described in Patent Document 1 is used to conform to a complex shape, the release layer and the antistatic layer are likely to peel off. If the release layer and the antistatic layer peel off, the release layer is likely to remain attached to the semiconductor package when the sealed semiconductor package is peeled off from the film.

[0006] The present disclosure provides a film in which a release layer and an antistatic layer are unlikely to peel off from each other, and a method for manufacturing a semiconductor package using the film.

[0007] The present disclosure provides a method for manufacturing a film and a semiconductor package having the following configurations [1] to

[15] : [1] A film comprising a substrate, an antistatic layer provided on one surface of the substrate, and a release layer provided on the surface of the antistatic layer opposite the substrate, wherein the film has an elongation calculated by the following formula when measured at 25°C and a speed of 100 mm / min in a tensile test: Elongation (%) = (Elongation at break (mm)) x 100 / (Distance between grippers before tensile testing (mm)) [2] The film of [1], wherein the substrate comprises at least one material selected from the group consisting of fluororesin, polymethylpentene, syndiotactic polystyrene, polycycloolefin, silicone rubber, polyester elastomer, polybutylene terephthalate, polyethylene terephthalate, and polyamide. [3] The film of [2] above, wherein the fluororesin comprises at least one selected from the group consisting of an ethylene-tetrafluoroethylene copolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, a tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymer, and a tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer. [4] The film of any of [1] to [3] above, wherein the release layer comprises a reaction-cured product of a hydroxyl group-containing (meth)acrylic polymer and a difunctional or higher isocyanate compound. [5] The film of [4] above, wherein the ratio of isocyanate groups of the isocyanate compound to 100 mol % of hydroxyl groups of the hydroxyl group-containing (meth)acrylic polymer is 20 to 115 mol %. [6] The film of any of [1] to [5] above, wherein the antistatic layer comprises a reaction-cured product of a carboxyl group-containing (meth)acrylic polymer and at least one selected from the group consisting of a difunctional or higher aziridine compound and a difunctional or higher epoxy compound. [7] The film according to the above [6], wherein the total ratio of the aziridine groups of the aziridine compound and the epoxy groups of the epoxy compound to 100 mol % of the carboxy groups of the carboxy group-containing (meth)acrylic polymer is 15 to 130 mol %. [8] The film according to any one of the above [1] to [7], wherein the thickness of the substrate is 25 to 250 μm.[9] The film of any of [1] to [8] above, wherein the thickness of the release layer is 0.05 to 3 μm.

[10] The film of any of [1] to [9] above, which is a release film used in a step of encapsulating a semiconductor element with a curable resin.

[11] A method for manufacturing a semiconductor package, comprising: placing the film of any of [1] to

[10] above on an inner surface of a mold; placing a substrate to which a semiconductor element is fixed within the mold with the film placed therein; encapsulating the semiconductor element within the mold with a curable resin to produce an encapsulated body; and releasing the encapsulated body from the mold.

[0008] According to the present disclosure, it is possible to provide a film in which the release layer and the antistatic layer are not easily peeled off, and a method for manufacturing a semiconductor package using the film.

[0009] FIG. 1 is a schematic cross-sectional view showing one embodiment of the present film.

[0010] Hereinafter, embodiments of the present disclosure will be described in detail. However, the embodiments of the present disclosure are not limited to the following embodiments. In the following embodiments, components (including element steps, etc.) are not essential unless otherwise specified. The same applies to numerical values ​​and their ranges, and do not limit the embodiments of the present disclosure.

[0011] In the present disclosure, the term "process" includes not only processes that are independent of other processes, but also processes that cannot be clearly distinguished from other processes as long as the purpose of the process is achieved. In the present disclosure, numerical ranges indicated using "to" include the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In numerical ranges described in stages in the present disclosure, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another staged numerical range. Furthermore, in numerical ranges described in the present disclosure, the upper or lower limit of that numerical range may be replaced with a value shown in the examples. In the present disclosure, each component may contain multiple corresponding substances. When multiple substances corresponding to each component are present in a composition, the content or amount of each component refers to the total content or amount of the multiple substances present in the composition, unless otherwise specified. In the present disclosure, when embodiments are described with reference to drawings, the configuration of the embodiment is not limited to the configuration shown in the drawings. Furthermore, the sizes of components in the drawings are conceptual, and the relative size relationships between components are not limited thereto.

[0012] In this disclosure, the term "unit" of a polymer refers to a portion derived from a monomer that exists in the polymer and constitutes the polymer. A unit also refers to a unit obtained by chemically converting the structure of a unit after polymer formation. In some cases, units derived from individual monomers are referred to by the name of the monomer followed by "unit." In this disclosure, films and sheets are referred to as "films" regardless of their thickness. In this disclosure, acrylate and methacrylate are collectively referred to as "(meth)acrylate," acrylic and methacrylic are collectively referred to as "(meth)acrylic," and (meth)acryloyl and methacryloyl are collectively referred to as "(meth)acryloyl." In this disclosure, a (meth)acrylic polymer is a polymer having units based on a monomer having a (meth)acryloyl group or (meth)acrylic acid. Hereinafter, a monomer having a (meth)acryloyl group or (meth)acrylic acid is also referred to as a "(meth)acrylic monomer."

[0013] [Film] A film according to one embodiment of the present disclosure (hereinafter also referred to as "the film") comprises a substrate, an antistatic layer provided on one side of the substrate, and a release layer provided on the side of the antistatic layer opposite the substrate, and has an elongation calculated by the following formula when measured at 23°C and a speed of 100 mm / min in a tensile test: more than 90% and less than 255%. The elongation of the film is preferably 125% or more and less than 255%, more preferably 175% or more and less than 255%, and particularly preferably 225% or more and less than 255%. Elongation (%) = (elongation at break (mm)) x 100 / (distance between grippers before tension (mm))

[0014] The "tensile test" can be performed by the method described in "Elongation" in the Examples. Specifically, the film is cut into a strip (50 mm wide, 100 mm long). This film is clamped and set between the grips of a tensile tester (for example, RTC-131-A manufactured by Orientec Co., Ltd.). The film is stretched at a gripping distance of 10 mm before tensioning and at a speed of 100 mm / min until the film breaks, and the elongation (mm) at break is measured. The measurement was performed at 23°C.

[0015] The present inventors have found that this film is particularly effective in preventing peeling between the antistatic layer and the release layer when manufacturing semiconductor packages having complex shapes. When the elongation exceeds 90%, when a coating liquid for a release layer is applied to the antistatic layer to form the release layer, the antistatic layer is slightly dissolved by the solvent in the coating liquid, roughening the surface of the antistatic layer, and the release layer penetrates into the roughened surface, improving the adhesion between the antistatic layer and the release layer. Furthermore, when the elongation is less than 255%, the release layer and the antistatic layer each have sufficient cohesive strength, preventing cohesive failure in each layer when the film is peeled from the semiconductor package.

[0016] The present film is not particularly limited in other configuration as long as it comprises a substrate, an antistatic layer, and a release layer. FIG. 1 is a schematic cross-sectional view showing one embodiment of the present film. The film 1 shown in FIG. 1 comprises a substrate 2, an antistatic layer 3, and a release layer 4, in this order. When the film 1 is used to encapsulate a semiconductor element, the substrate 2 is disposed so as to contact a mold, and after resin encapsulation, the release layer 4 contacts the encapsulant (i.e., a semiconductor package in which a semiconductor element is encapsulated). The film 1 may comprise other layers in addition to the substrate 2, the antistatic layer 3, and the release layer 4. Each component of the present film will be described in detail below.

[0017] (Substrate) The material of the substrate is not particularly limited. The substrate typically contains a resin. Examples of resins include fluororesin, polymethylpentene, syndiotactic polystyrene, polycycloolefin, silicone rubber, polyester elastomer, polybutylene terephthalate, polyethylene terephthalate, and polyamide. In one embodiment, from the viewpoint of excellent releasability of the film, the substrate preferably contains a resin having releasability (hereinafter also referred to as "releasable resin"). The releasable resin refers to a resin in which the layer composed of the resin has releasability. Examples of releasable resins include fluororesin, polymethylpentene, syndiotactic polystyrene, polycycloolefin, silicone rubber, polyester elastomer, polybutylene terephthalate, and polyamide. From the viewpoint of excellent releasability, heat resistance, strength, and elongation at high temperatures, fluororesin, polymethylpentene, syndiotactic polystyrene, and polycycloolefin are preferred, and from the viewpoint of excellent releasability, fluororesin is more preferred. The resin contained in the substrate may be one type or two or more types. It is particularly preferable that the substrate is composed solely of a fluororesin. However, even if the substrate is composed solely of a fluororesin, it does not preclude the inclusion of a resin other than the fluororesin as long as the effects of the invention are not impaired.

[0018] As the fluororesin, a fluoroolefin polymer is preferred from the viewpoint of excellent mold releasability and heat resistance. The fluoroolefin polymer is a polymer having units based on a fluoroolefin. The fluoroolefin polymer may further have units other than the units based on a fluoroolefin. Examples of the fluoroolefin include tetrafluoroethylene (hereinafter also referred to as "TFE"), vinyl fluoride, vinylidene fluoride, trifluoroethylene, hexafluoropropylene (hereinafter also referred to as "HFP"), and chlorotrifluoroethylene. One type of fluoroolefin may be used alone, or two or more types may be used in combination.

[0019] Examples of the fluoroolefin polymer include ethylene-TFE copolymer (hereinafter also referred to as "ETFE"), TFE-HFP copolymer (hereinafter also referred to as "FEP"), TFE-perfluoro(alkyl vinyl ether) copolymer, and TFE-HFP-vinylidene fluoride copolymer. From the viewpoint of mechanical properties, at least one selected from the group consisting of ETFE and FEP is preferred. One type of fluoroolefin polymer may be used alone, or two or more types may be used in combination.

[0020] From the viewpoint of large elongation at high temperatures, ETFE is preferred as the fluoroolefin polymer. ETFE is a copolymer having units based on TFE (hereinafter also referred to as "TFE units") and units based on ethylene (hereinafter also referred to as "E units"). ETFE is preferably a polymer having TFE units, E units, and units based on a third monomer other than TFE and ethylene. Depending on the type and content of the units based on the third monomer, the crystallinity of ETFE can be easily adjusted, thereby making it easy to adjust the storage modulus or other tensile properties of the substrate. For example, when ETFE has units based on a third monomer (especially a monomer having a fluorine atom), the tensile strength and elongation at high temperatures (especially around 180 ° C) tend to be improved.

[0021] The third monomer may be a monomer having a fluorine atom or a monomer not having a fluorine atom. The fluorine atom-containing monomer may be the following monomers a1 to a5. Monomer a1: Fluoroolefins having 2 or 3 carbon atoms. Monomer a2: X(CF 2 ) n CY=CH 2 (wherein X and Y each independently represent a hydrogen atom or a fluorine atom, and n represents an integer of 2 to 8.) Monomer a3: a fluorovinyl ether. Monomer a4: a functional group-containing fluorovinyl ether. Monomer a5: a fluorine-containing monomer having an aliphatic ring structure.

[0022] Specific examples of the monomer a1 include fluoroethylenes (such as trifluoroethylene, vinylidene fluoride, vinyl fluoride, and chlorotrifluoroethylene), and fluoropropylenes (such as hexafluoropropylene (HFP) and 2-hydropentafluoropropylene).

[0023] As the monomer a2, a monomer in which n is 2 to 6 is preferred, and a monomer in which n is 2 to 4 is more preferred. A monomer in which X is a fluorine atom and Y is a hydrogen atom, i.e., (perfluoroalkyl)ethylene, is also preferred. Specific examples of the monomer a2 include the following compounds: CF 3 CF 2 CH=CH 2 , C.F. 3 CF 2 CF 2 CF 2 CH=CH 2 ((Perfluorobutyl)ethylene (hereinafter also referred to as "PFBE")), CF 3 CF 2 CF 2 CF 2 CF=CH 2 , C.F. 2 HCF 2 CF 2 CF=CH 2 , C.F. 2 HCF 2 CF 2 CF 2 CF=CH2 .

[0024] Specific examples of the monomer a3 include the following compounds. Among the following, the diene monomer is a monomer that can be cyclopolymerized. CF 2 = CFOCF 3 , C.F. 2 = CFOCF 2 CF 3 , C.F. 2 = CFO (CF 2 ) 2 CF 3 (perfluoro(propyl vinyl ether) (hereinafter also referred to as "PPVE")), CF 2 = CFOCF 2 CF (CF 3 ) O(CF 2 ) 2 CF 3 , C.F. 2 = CFO (CF 2 ) 3 O (CF 2 ) 2 CF 3 , C.F. 2 = CFO (CF 2 CF (CF 3 ) O) 2 (CF 2 ) 2 CF 3 , C.F. 2 = CFOCF 2 CF (CF 3 ) O(CF 2 ) 2 CF 3 , C.F. 2 = CFOCF 2 CF = CF 2 , C.F. 2 = CFO (CF 2 ) 2 CF = CF 2 .

[0025] Specific examples of the monomer a4 include the following compounds: CF 2 = CFO (CF 2 ) 3 CO 2 CH 3 , C.F. 2 = CFOCF2 CF (CF 3 ) O(CF 2 ) 3 CO 2 CH 3 , C.F. 2 = CFOCF 2 CF (CF 3 ) O(CF 2 ) 2 SO 2 F.

[0026] Specific examples of the monomer a5 include perfluoro(2,2-dimethyl-1,3-dioxole), 2,2,4-trifluoro-5-trifluoromethoxy-1,3-dioxole, and perfluoro(2-methylene-4-methyl-1,3-dioxolane).

[0027] Examples of the monomer not having a fluorine atom include the following monomers b1 to b4: Monomer b1: olefins; Monomer b2: vinyl esters; Monomer b3: vinyl ethers; Monomer b4: unsaturated acid anhydrides.

[0028] Specific examples of monomer b1 include propylene and isobutene. Specific examples of monomer b2 include vinyl acetate. Specific examples of monomer b3 include ethyl vinyl ether, butyl vinyl ether, cyclohexyl vinyl ether, and hydroxybutyl vinyl ether. Specific examples of monomer b4 include maleic anhydride, itaconic anhydride, citraconic anhydride, and 5-norbornene-2,3-dicarboxylic anhydride.

[0029] The third monomer may be used alone or in combination of two or more. As the third monomer, from the viewpoint of easy adjustment of the crystallinity and excellent tensile strength and elongation at high temperatures (particularly around 180°C), monomer a2, HFP, PPVE, and vinyl acetate are preferred, and HFP, PPVE, CF 3 CF 2 CH=CH 2and PFBE are more preferred, and PFBE is particularly preferred. That is, as ETFE, a copolymer having TFE units, E units, and units based on PFBE (hereinafter also referred to as "PFBE units") is particularly preferred.

[0030] In ETFE, the molar ratio of TFE units to E units (TFE units / E units) is preferably 80 / 20 to 40 / 60, more preferably 70 / 30 to 45 / 55, and even more preferably 65 / 35 to 50 / 50. When the TFE units / E units is within the above range, the ETFE has excellent heat resistance and mechanical strength.

[0031] The ratio of the units based on the third monomer in ETFE is preferably 0.01 to 20 mol%, more preferably 0.10 to 15 mol%, and even more preferably 0.20 to 10 mol%, relative to the total (100 mol%) of all units constituting ETFE. When the ratio of the units based on the third monomer is within the above range, ETFE is excellent in heat resistance and mechanical strength.

[0032] When the units based on the third monomer contain PFBE units, the proportion of the PFBE units is preferably 0.5 to 4.0 mol%, more preferably 0.7 to 3.6 mol%, and even more preferably 1.0 to 3.6 mol%, relative to the total (100 mol%) of all units constituting ETFE. When the proportion of the PFBE units is within the above range, the tensile strength and elongation of the film at high temperatures, particularly at around 180°C, are improved.

[0033] The substrate may consist of only resin, or may further contain other components in addition to resin. Examples of other components include lubricants, antioxidants, antistatic agents, plasticizers, and mold release agents. From the viewpoint of preventing mold contamination, it is preferable that the substrate does not contain other components.

[0034] The thickness of the substrate is preferably 25 to 250 μm, more preferably 50 to 150 μm, and even more preferably 75 to 125 μm. When the thickness of the substrate is equal to or less than the upper limit of the above range, the film is easily deformable and exhibits excellent mold conformability. When the thickness of the substrate is equal to or greater than the lower limit of the above range, the film is easy to handle, for example, in a roll-to-roll process, and wrinkles are less likely to occur when the film is stretched and placed to cover the cavity of a mold. The thickness of the substrate can be measured in accordance with ISO 4591:1992 (JIS K7130:1999) B1 method (method for measuring the thickness of a sample taken from a plastic film or sheet by the mass method). The same applies hereinafter to the thickness of each layer of the film.

[0035] The surface of the substrate may have surface roughness. The arithmetic mean roughness Ra of the substrate surface is preferably 0.2 to 3.0 μm, more preferably 0.5 to 2.5 μm. When the arithmetic mean roughness Ra of the substrate surface is equal to or greater than the lower limit of the above range, the mold releasability is better. When the arithmetic mean roughness Ra of the substrate surface is equal to or less than the upper limit of the above range, pinholes are less likely to form in the film. The arithmetic mean roughness Ra is measured based on JIS B0601:2013 (ISO 4287:1997, Amd.1:2009). The reference length lr (cutoff value λc) for the roughness curve is 0.8 mm.

[0036] The substrate may be unstretched or stretched. For example, unstretched polyamide film, biaxially stretched polyamide film, biaxially stretched PET (polyethylene terephthalate) film, biaxially stretched PEN (polyethylene phthalate) film, biaxially stretched syndiotactic polystyrene film, and unstretched PBT (polybutylene terephthalate) film are commercially available. Other usable films include polyimide film, polyphenylene sulfide resin film, and crosslinked polyethylene film.

[0037] The surface of the substrate adjacent to other layers may be subjected to any surface treatment. Examples of surface treatment include corona treatment, plasma treatment, coating with a silane coupling agent, and coating with an adhesive. From the viewpoint of adhesion between the substrate and other layers, corona treatment or plasma treatment is preferred.

[0038] From the viewpoint of adhesion between the substrate and the adjacent layer, the wetting tension of the surface of the substrate on the antistatic layer side is preferably 20 mN / m or more, more preferably 30 mN / m or more, and particularly preferably 35 mN / m or more. The upper limit of the wetting tension is not particularly limited, and may be 80 mN / m or less.

[0039] The substrate may be a single layer or may have a multilayer structure. Examples of a multilayer structure include a structure in which multiple layers, each containing a resin, are laminated. In this case, the resins contained in the multiple layers may be the same or different. From the viewpoints of mold followability, tensile elongation, and production costs, the substrate is preferably a single layer. From the viewpoint of film strength, the substrate preferably has a multilayer structure. The multilayer structure may be, for example, a structure in which a layer containing the aforementioned release resin (preferably a fluororesin) is laminated on a resin film (which may be a film containing only resin) containing a resin such as polyester, polybutylene terephthalate, polystyrene (preferably syndiotactic), or polycarbonate, or a structure in which a layer containing a first release resin, the resin film, and a layer containing a second release resin are laminated in this order. The layer containing the release resin and the resin film may be laminated via an adhesive. One or both sides of each release resin layer may be subjected to corona treatment or plasma treatment. When the substrate has such a multilayer structure, it is preferable that the layer containing the release resin be disposed on the antistatic layer side. When the substrate has such a multilayer structure, the surface of the layer containing a release resin disposed on the antistatic layer side is preferably subjected to a corona treatment or plasma treatment.

[0040] (Antistatic Layer) The antistatic layer is not particularly limited as long as it is a layer having an antistatic function. The antistatic layer may be provided on the substrate adjacent to the substrate, or may be provided on the substrate via another layer adjacent to the substrate.

[0041] The antistatic layer may contain an antistatic agent. Examples of the antistatic agent include an ionic liquid, a conductive polymer, and a conductive filler. One type of antistatic agent may be used alone, or two or more types may be used in combination.

[0042] Examples of ionic liquids include onium compounds such as pyridinium and imidazolium, as well as fluorine-based compounds. Conductive polymers are polymers in which electrons move and diffuse along the polymer backbone. Examples of conductive polymers include polyaniline-based polymers, polyacetylene-based polymers, polyparaphenylene-based polymers, polypyrrole-based polymers, polythiophene-based polymers, and polyvinylcarbazole-based polymers. Examples of conductive fillers include metal ion-conductive salts, metal compounds (e.g., metal oxides), fillers coated with metal compounds (e.g., metal oxides), conductive carbon, and conductive carbon nanotubes. Examples of metal ion-conductive salts include lithium salt compounds. Examples of metal oxides used as fillers and metal oxides coating fillers include tin oxide, tin-doped indium oxide, antimony-doped tin oxide, phosphorus-doped tin oxide, zinc antimonate, and antimony oxide.

[0043] As the antistatic agent, from the viewpoint of excellent heat resistance and conductivity, at least one selected from the group consisting of polyaniline polymers, polyacetylene polymers, polyparaphenylene polymers, polypyrrole polymers, polythiophene polymers, and polyvinylcarbazole polymers is preferred.

[0044] The antistatic agent is preferably dispersed in the binder resin. That is, the antistatic layer is preferably a layer in which the antistatic agent is dispersed in the binder resin. The binder resin is preferably heat-resistant. For example, when the film is used in the encapsulation process of semiconductor elements, a binder resin having heat resistance at approximately 180°C is preferred. From the viewpoint of excellent heat resistance, the binder resin preferably contains at least one selected from the group consisting of (meth)acrylic resin, silicone resin, urethane resin, polyester resin, polyamide resin, vinyl acetate resin, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, chlorotrifluoroethylene-vinyl alcohol copolymer, and tetrafluoroethylene-vinyl alcohol copolymer. Among these, from the viewpoint of excellent mechanical strength, it is preferable that the binder resin is composed of at least one selected from the group consisting of (meth)acrylic resin, silicone resin, urethane resin, polyester resin, polyamide resin, vinyl acetate resin, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, chlorotrifluoroethylene-vinyl alcohol copolymer, and tetrafluoroethylene-vinyl alcohol copolymer (for example, only (meth)acrylic resin). Furthermore, from the viewpoint of excellent heat resistance and dispersibility of the antistatic agent, at least one selected from the group consisting of polyester resins and (meth)acrylic resins is preferred. In the antistatic layer, the binder resin may be crosslinked. When the binder resin is crosslinked, the strength, heat resistance, and solvent resistance are superior to those when it is not crosslinked.

[0045] In one embodiment, from the viewpoint of solvent resistance, the antistatic layer preferably contains, as a binder resin, a reaction cured product of a carboxyl group-containing (meth)acrylic polymer and at least one selected from the group consisting of a difunctional or higher functional aziridine compound (hereinafter also referred to as a "polyfunctional aziridine compound") and a difunctional or higher functional epoxy compound (hereinafter also referred to as a "polyfunctional epoxy compound"). In this case, the carboxyl group-containing (meth)acrylic polymer reacts with the at least one selected from the group consisting of the polyfunctional aziridine compound and the polyfunctional epoxy compound to crosslink and form a reaction cured product. The antistatic layer may also be a reaction cured product of a carboxyl group-containing (meth)acrylic polymer, at least one selected from the group consisting of the polyfunctional aziridine compound and the polyfunctional epoxy compound, and other components.

[0046] The proportion of units based on the (meth)acrylic monomer relative to the entire (meth)acrylic polymer is not particularly limited, and is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and particularly preferably 80% by mass or more.

[0047] The carboxy group of the carboxy group-containing (meth)acrylic polymer is a crosslinking functional group that reacts with an aziridine group in a polyfunctional aziridine compound or an epoxy group in a polyfunctional epoxy compound. The acid value of the carboxy group-containing (meth)acrylic polymer is preferably 1 to 80 mgKOH / g, more preferably 1 to 40 mgKOH / g, even more preferably 1 to 30 mgKOH / g, and particularly preferably 5 to 30 mgKOH / g. The acid value of the carboxy group-containing (meth)acrylic polymer is an indicator of the ease of crosslinking when reacted with a polyfunctional aziridine compound or a polyfunctional epoxy compound. When the acid value is equal to or less than the upper limit, the antistatic layer has excellent extensibility. When the acid value is equal to or greater than the lower limit, the antistatic layer has excellent adhesion. When multiple types of (meth)acrylic polymers are used in the antistatic layer, the above range is the preferred range for the acid value of the entire multiple types of (meth)acrylic polymers. The acid value of the (meth)acrylic polymer is measured by the method specified in JIS K0070:1992.

[0048] In the carboxy group-containing (meth)acrylic polymer, the carboxy group may be present in a side group, at a main chain terminal, or both in a side chain and a main chain. From the viewpoint of facilitating adjustment of the carboxy group content, it is preferable that the carboxy group be present at least in a side group.

[0049] Examples of carboxy group-containing (meth)acrylic polymers in which a carboxy group exists on a side group include (meth)acrylic polymers having units based on a carboxy group-containing monomer. Examples of carboxy group-containing monomers include carboxy group-containing (meth)acrylic monomers. Examples of carboxy group-containing (meth)acrylic monomers include carboxy group-containing (meth)acrylates and (meth)acrylic acid. Examples of carboxy group-containing (meth)acrylates include ω-carboxy-polycaprolactone mono(meth)acrylate and mono-2-((meth)acryloyloxy)ethyl succinic acid. These monomers may be used alone or in combination of two or more.

[0050] The carboxyl group-containing (meth)acrylic polymer may be composed solely of units based on a carboxyl group-containing monomer, or may further contain units based on a monomer other than the carboxyl group-containing monomer. Examples of the monomer other than the carboxyl group-containing monomer include (meth)acrylates that do not contain hydroxyl groups or carboxyl groups, and (meth)acrylates that contain hydroxyl groups. These monomers may be used alone or in combination of two or more.

[0051] Examples of (meth)acrylates that do not contain a hydroxyl group or a carboxy group include alkyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, benzyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, glycidyl (meth)acrylate, 2-aminoethyl (meth)acrylate, 3-(methacryloyloxypropyl)trimethoxysilane, trifluoromethylmethyl (meth)acrylate, and 2-trifluoromethylethyl (meth)acrylate. acrylate, 2-perfluoroethylethyl (meth)acrylate, 2-perfluoroethyl-2-perfluorobutylethyl (meth)acrylate, 2-perfluoroethyl (meth)acrylate, perfluoromethyl (meth)acrylate, diperfluoromethylmethyl (meth)acrylate, 2-perfluoromethyl-2-perfluoroethylmethyl (meth)acrylate, 2-perfluorohexylethyl (meth)acrylate, 2-perfluorodecylethyl (meth)acrylate, and 2-perfluorohexadecylethyl (meth)acrylate.

[0052] The alkyl (meth)acrylate is preferably a compound in which the alkyl group has 1 to 12 carbon atoms, and examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, and dodecyl (meth)acrylate.

[0053] Examples of hydroxyl group-containing (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1,4-cyclohexanedimethanol monoacrylate, and 2-acryloyloxyethyl-2-hydroxyethyl-phthalic acid.

[0054] The mass average molecular weight (hereinafter also referred to as "Mw") of the carboxy group-containing (meth)acrylic polymer is preferably 10,000 to 1,000,000, more preferably 50,000 to 800,000, and even more preferably 100,000 to 600,000. When Mw is equal to or greater than the lower limit, the strength of the antistatic layer is excellent. When Mw is equal to or less than the upper limit, the extensibility of the antistatic layer is excellent. The Mw of the carboxy group-containing (meth)acrylic polymer is a polystyrene-equivalent value obtained by measurement by gel permeation chromatography using a calibration curve prepared using standard polystyrene samples of known molecular weight.

[0055] A polyfunctional aziridine compound is a compound having two or more aziridine groups per molecule. The number of aziridine groups in the polyfunctional aziridine compound is preferably 6 or less, and particularly preferably 3 or less, from the viewpoint of obtaining high extensibility without excessively increasing the crosslink density of the antistatic layer. Examples of polyfunctional aziridine compounds include 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate], 4,4-bis(ethyleneiminocarbonylamino)diphenylmethane, and trimethylolpropane-tris(β-aziridinyl)propionate. One type of polyfunctional aziridine compound may be used alone, or two or more types may be used in combination.

[0056] Commercially available polyfunctional aziridine compounds may be used, including Araquat CL910 (trade name) manufactured by Arakawa Chemical Industries, Ltd., Chemitite (registered trademark) DZ-22E (trade name) manufactured by Nippon Shokubai Co., Ltd., and Chemitite (registered trademark) PZ-33 (trade name) manufactured by Nippon Shokubai Co., Ltd.

[0057] From the viewpoint of obtaining high extensibility without excessively increasing the crosslink density of the antistatic layer, the aziridine equivalent of the polyfunctional aziridine compound is preferably 50 g / eq or more, more preferably 75 g / eq or more, and even more preferably 100 g / eq or more. From the viewpoint of increasing the strength of the antistatic layer, the aziridine equivalent of the polyfunctional aziridine compound is preferably 300 g / eq or less, more preferably 250 g / eq or less, and even more preferably 200 g / eq. From such viewpoints, the aziridine equivalent of the polyfunctional aziridine compound is preferably 50 to 300 g / eq, more preferably 75 to 250 g / eq, and even more preferably 100 to 200 g / eq.

[0058] A polyfunctional epoxy compound is a compound having two or more epoxy groups in one molecule. The number of epoxy groups in the polyfunctional epoxy compound is preferably 6 or less, and particularly preferably 3 or less, from the viewpoint of not excessively increasing the crosslink density of the antistatic layer and obtaining high extensibility. Examples of polyfunctional epoxy compounds include N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, resorcinol diglycidyl ether, and glycerol polyglycidyl ether. One type of epoxy compound may be used alone, or two or more types may be used in combination.

[0059] Commercially available polyfunctional epoxy compounds may be used, examples of which include TETRAD-X (trade name) and TETRAD-C (trade name) manufactured by Mitsubishi Gas Chemical Company, Inc., and Denacol (registered trademark) EX-201 (trade name) and Denacol (registered trademark) EX-313 (trade name) manufactured by Nagase ChemteX Corporation.

[0060] From the viewpoint of obtaining high extensibility without excessively increasing the crosslink density of the antistatic layer, the epoxy equivalent of the polyfunctional epoxy compound is preferably 30 g / eq or more, more preferably 50 g / eq or more, and even more preferably 90 g / eq or more. From the viewpoint of increasing the strength of the antistatic layer, the epoxy equivalent of the polyfunctional epoxy compound is preferably 300 g / eq or less, more preferably 200 g / eq or less, even more preferably 150 g / eq or less, and particularly preferably 120 g / eq or less. From such viewpoints, the epoxy equivalent of the polyfunctional epoxy compound is preferably 30 to 300 g / eq, more preferably 50 to 200 g / eq, and even more preferably 90 to 120 g / eq.

[0061] The total ratio of the aziridine groups of the polyfunctional aziridine compound and the epoxy groups of the polyfunctional epoxy compound to 100 mol% of the carboxy groups of the carboxy group-containing (meth)acrylic polymer is preferably 15 to 130 mol%, more preferably 15 to 90 mol%, and particularly preferably 15 to 60 mol%. When the total ratio of the aziridine groups and the epoxy groups is not more than the upper limit, the crosslinking density is sufficiently low, resulting in excellent adhesion between the release layer and the antistatic layer. When the total ratio of the aziridine groups and the epoxy groups is not less than the lower limit, the crosslinking density is sufficiently high, resulting in excellent strength of the antistatic layer.

[0062] The antistatic layer may contain components other than the antistatic agent and binder resin. Examples of other components include lubricants, colorants, coupling agents, etc. Examples of lubricants include microbeads made of thermoplastic resin, fumed silica, and polytetrafluoroethylene (PTFE) fine particles. Examples of colorants include various organic and inorganic colorants, more specifically, cobalt blue, red iron oxide, and cyanine blue. Examples of coupling agents include silane coupling agents and titanate coupling agents.

[0063] From the viewpoint of fully exhibiting antistatic function, the content of the antistatic agent in the antistatic layer is preferably an amount that results in a surface resistance value of the film in the range described below. In one embodiment, when the antistatic layer is a layer in which an antistatic agent is dispersed in a binder resin, the content of the antistatic agent may be 3 to 50% by mass, or may be 5 to 20% by mass, relative to the binder resin. When the content of the antistatic agent is equal to or greater than the lower limit, the surface resistance value of the film tends to fall within a suitable range. When the content of the antistatic agent is equal to or less than the upper limit, the adhesion of the antistatic layer tends to be good.

[0064] The contents of the other components are appropriately set depending on the desired surface resistance and strength of the antistatic layer.

[0065] The thickness of the antistatic layer is preferably 0.05 to 3.0 μm, more preferably 0.1 to 2.5 μm. When the thickness of the antistatic layer is equal to or greater than the lower limit of the above range, electrical conductivity is exhibited and the antistatic function is excellent. When the thickness of the antistatic layer is equal to or less than the upper limit of the above range, the stability of the production process, including the appearance of the coated surface, is excellent.

[0066] (Release Layer) The release layer may be provided on the antistatic layer adjacent to the antistatic layer, or may be provided on the antistatic layer via another layer adjacent to the antistatic layer. The material of the release layer is not particularly limited. The release layer may be a layer that has adhesive properties to other members. In one embodiment, from the viewpoints of heat resistance sufficient for use in a transfer molding process in which the mold and encapsulating resin are exposed to high temperatures and compatibility with the antistatic layer, the release layer preferably includes a reaction cured product of a hydroxyl group-containing (meth)acrylic polymer and a bifunctional or higher isocyanate compound (hereinafter also referred to as a "polyfunctional isocyanate compound"). In this case, the hydroxyl group-containing (meth)acrylic polymer reacts with the polyfunctional isocyanate compound to crosslink and form a reaction cured product. The release layer may also be a reaction cured product of a hydroxyl group-containing (meth)acrylic polymer, a polyfunctional isocyanate compound, and other components.

[0067] The hydroxyl group of the hydroxyl group-containing (meth)acrylic polymer is a crosslinking functional group that reacts with the isocyanate group in the polyfunctional isocyanate compound. The hydroxyl value of the hydroxyl group-containing (meth)acrylic polymer is preferably 1 mgKOH / g or more, more preferably 29 mgKOH / g or more, and preferably 100 mgKOH / g or less. When multiple types of (meth)acrylic polymers are used in the release layer, the above range is the preferred range for the hydroxyl value of the entire multiple types of (meth)acrylic polymers. The hydroxyl value is measured by the method specified in JIS K0070:1992.

[0068] The hydroxyl group-containing (meth)acrylic polymer may or may not have a carboxy group. The carboxy group, like the hydroxyl group, is a crosslinking functional group that reacts with the isocyanate group in the polyfunctional isocyanate compound. The acid value of the hydroxyl group-containing (meth)acrylic polymer is preferably 100 mgKOH / g or less, more preferably 30 mgKOH / g or less, and may be 0 mgKOH / g.

[0069] The crosslinking functional group equivalent of the hydroxyl group-containing (meth)acrylic polymer, i.e., the total equivalent of hydroxyl groups and carboxyl groups, is preferably 500 g / mol or more, more preferably 1,000 g / mol or more, and preferably 2,000 g / mol or less. The crosslinking functional group equivalent corresponds to the molecular weight between crosslinking points and is a physical property value that governs the elastic modulus after crosslinking, i.e., the elastic modulus of the reaction-cured product. When the crosslinking functional group equivalent is equal to or greater than the lower limit, the elastic modulus of the reaction-cured product is low, resulting in excellent extensibility of the release layer. When the crosslinking functional group equivalent is equal to or less than the upper limit, the elastic modulus of the reaction-cured product is high, resulting in excellent release properties of the release layer against resins, electronic components, etc. In addition, migration of the components of the release layer to resins, electronic components, etc. is suppressed. The crosslinking functional group equivalent of the hydroxyl group-containing (meth)acrylic polymer is calculated by dividing the molecular weight of potassium hydroxide (56.1) by the sum of the hydroxyl value and acid value of the hydroxyl group-containing (meth)acrylic polymer, and multiplying the result by 1,000.

[0070] In the hydroxyl group-containing (meth)acrylic polymer, the hydroxyl groups may be present in side groups, at the terminals of the main chain, or both in the side chains and the main chain. In terms of ease of adjusting the hydroxyl group content, it is preferable that the hydroxyl groups be present at least in the side groups.

[0071] The hydroxyl group-containing (meth)acrylic polymer having hydroxyl groups present in side groups is preferably a copolymer having the following units c1 and c2: Unit c1: hydroxyl group-containing (meth)acrylate unit, Unit c2: unit other than unit c1.

[0072] An example of the unit c1 is a unit represented by the following formula 1: -(CH 2 -CR 1 (COO-R 2 —OH))— Formula 1 where R 1 is a hydrogen atom or a methyl group, and R 2 represents an alkylene group having 2 to 10 carbon atoms, a cycloalkylene group having 3 to 10 carbon atoms, or -R 3 -OCO-R 5 -COO-R 4 - is. R 3 and R 4 are each independently an alkylene group having 2 to 10 carbon atoms, and R 5 is a phenylene group.

[0073] R 1 is preferably a hydrogen atom. 2 , R 3 , R 4 The alkylene group in may be linear or branched.

[0074] Specific examples of the monomer that becomes unit c1 include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1,4-cyclohexanedimethanol monoacrylate, and 2-acryloyloxyethyl-2-hydroxyethyl-phthalic acid. The monomer that becomes unit c1 may be used alone or in combination of two or more. From the viewpoint of excellent reactivity of the hydroxyl group, the monomer R 2is preferably an alkylene group having 2 to 10 carbon atoms. That is, a unit based on a hydroxyalkyl (meth)acrylate having a hydroxyalkyl group having 2 to 10 carbon atoms is preferred.

[0075] The proportion of units c1 relative to the total (100 mol%) of all units constituting the hydroxyl group-containing (meth)acrylic polymer is preferably 3 mol% or more, and preferably 40 mol% or less, more preferably 30 mol% or less, and even more preferably 20 mol% or less. When the proportion of units c1 is above the lower limit, the crosslinking density of the polyfunctional isocyanate compound is sufficiently high, and the release layer has excellent releasability against resins, electronic components, etc. When the proportion of units c1 is below the upper limit, the release layer has excellent adhesion.

[0076] The unit c2 is not particularly limited as long as it is copolymerizable with the monomer that forms the unit c1. The unit c2 may have a carboxy group, but preferably does not have a reactive group other than the carboxy group that can react with an isocyanate group (e.g., an amino group). Examples of monomers that form the unit c2 include macromers having an unsaturated double bond, (meth)acrylates without a hydroxyl group, (meth)acrylic acid, and acrylonitrile. Examples of macromers having an unsaturated double bond include macromers having a polyoxyalkylene chain, such as (meth)acrylates of polyethylene glycol monoalkyl ether. Examples of (meth)acrylates not having a hydroxyl group include alkyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, benzyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, glycidyl (meth)acrylate, 2-aminoethyl (meth)acrylate, 3-(methacryloyloxypropyl)trimethoxysilane, trifluoromethylmethyl (meth)acrylate, and 2-trifluoromethylethyl (meth)acrylate. Examples thereof include 2-perfluoroethylethyl (meth)acrylate, 2-perfluoroethyl-2-perfluorobutylethyl (meth)acrylate, 2-perfluoroethyl (meth)acrylate, perfluoromethyl (meth)acrylate, diperfluoromethylmethyl (meth)acrylate, 2-perfluoromethyl-2-perfluoroethylmethyl (meth)acrylate, 2-perfluorohexylethyl (meth)acrylate, 2-perfluorodecylethyl (meth)acrylate, and 2-perfluorohexadecylethyl (meth)acrylate.

[0077] The alkyl (meth)acrylate is preferably a compound in which the alkyl group has 1 to 12 carbon atoms, and examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, and dodecyl (meth)acrylate.

[0078] It is preferable that unit c2 contains at least a unit based on alkyl (meth)acrylate. The proportion of alkyl (meth)acrylate units relative to the total (100 mol%) of all units constituting the hydroxyl group-containing (meth)acrylic polymer is preferably 60 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, and preferably 97 mol% or less. When the proportion of alkyl (meth)acrylate units is above the lower limit, the glass transition point and mechanical properties derived from the alkyl (meth)acrylate structure are exhibited, resulting in excellent mechanical strength and adhesiveness of the release layer. When the proportion of alkyl (meth)acrylate units is below the upper limit, the hydroxyl group content is sufficient, resulting in an increased crosslinking density and a high elastic modulus.

[0079] The Mw of the hydroxyl group-containing (meth)acrylic polymer is preferably 100,000 to 1,200,000, more preferably 200,000 to 1,000,000, and even more preferably 200,000 to 700,000. When the Mw is equal to or greater than the lower limit, the release layer has excellent releasability against resins, electronic components, and the like. When the Mw is equal to or less than the upper limit, the release layer has excellent adhesion. The Mw of the hydroxyl group-containing (meth)acrylic polymer is a polystyrene-equivalent value obtained by measurement by gel permeation chromatography using a calibration curve prepared using standard polystyrene samples of known molecular weight.

[0080] The glass transition temperature (Tg) of the hydroxyl group-containing (meth)acrylic polymer is preferably 20°C or lower, more preferably 0°C or lower. When Tg is equal to or lower than the upper limit, the release layer exhibits sufficient flexibility even at low temperatures, and is less likely to peel from the substrate. There is no particular restriction on the lower limit of Tg, but within the aforementioned molecular weight range, it is preferably -60°C or higher. Tg is the midpoint glass transition temperature measured by differential scanning calorimetry (DSC).

[0081] The polyfunctional isocyanate compound is a compound having two or more isocyanate groups in one molecule. The isocyanate group may be protected with a blocking agent. The number of isocyanate groups in the polyfunctional isocyanate compound is preferably 10 or less, particularly preferably 3 or less, from the viewpoint of obtaining high extensibility without excessively increasing the crosslinking density of the release layer. The polyfunctional isocyanate compound is most preferably bifunctional or trifunctional.

[0082] Examples of polyfunctional isocyanate compounds include hexamethylene diisocyanate (HDI), tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (NDI), tolidine diisocyanate (TODI), isophorone diisocyanate (IPDI), xylene diisocyanate (XDI), triphenylmethane triisocyanate, and tris(isocyanatophenyl)thiophosphate. Also included are isocyanurates (i.e., trimers) and biurets of these polyfunctional isocyanate compounds, and reaction products of these polyfunctional isocyanate compounds with polyol compounds (e.g., adducts, bifunctional prepolymers, trifunctional prepolymers, etc.). Also included are compounds in which the isocyanate groups of these polyfunctional isocyanate compounds are protected with a blocking agent. Examples of blocking agents include phenols such as m-cresol and guaiacol, benzenethiol, ethyl acetoacetate, diethyl malonate, and ε-caprolactam.

[0083] The bifunctional prepolymer is, for example, OCN-R 6 -NHC(=O)OR 7 -OC(=O)NH-R 6-NCO. 6 is a residue obtained by removing two isocyanate groups from a diisocyanate compound, and R 7 is a residue obtained by removing two hydroxyl groups from a diol compound. Examples of diisocyanate compounds include HDI, TDI, MDI, NDI, TODI, IPDI, and XDI, and HDI and IPDI are preferred from the viewpoint of resistance to yellowing. Examples of diol compounds include ethylene glycol and propylene glycol. Commercially available bifunctional prepolymers may be used. Examples of commercially available products include Duranate (registered trademark) D201 (trade name) and D101 manufactured by Asahi Kasei Corporation.

[0084] Examples of trifunctional prepolymers include isocyanurate forms of HDI (isocyanurate-type HDI), isocyanurate forms of TDI (isocyanurate-type TDI), isocyanurate forms of MDI (isocyanurate-type MDI), and reaction products of trifunctional polyols and bifunctional isocyanates. From the viewpoint of resistance to yellowing, isocyanurate-type HDI is preferred.

[0085] In one embodiment, the polyfunctional isocyanate compound preferably has an isocyanurate ring, from the viewpoint that the planarity of the ring structure allows the reaction cured product (i.e., the release layer) to exhibit a high elastic modulus. Examples of polyfunctional isocyanate compounds having an isocyanurate ring include isocyanurate-type HDI, isocyanurate-type TDI, and isocyanurate-type MDI.

[0086] The ratio of isocyanate groups of the polyfunctional isocyanate compound to 100 mol% of hydroxyl groups of the hydroxyl group-containing (meth)acrylic polymer is preferably 20 to 115 mol%, more preferably 20 to 80 mol%, and particularly preferably 20 to 70 mol%. When the ratio of isocyanate groups is equal to or less than the upper limit, the crosslink density is sufficiently low, resulting in excellent adhesion between the release layer and the antistatic layer. When the ratio of isocyanate groups is equal to or more than the lower limit, the crosslink density is sufficiently high, resulting in excellent releasability of the release layer against resins, electronic components, etc.

[0087] In the release layer, the content of the reaction cured product of the hydroxyl group-containing (meth)acrylic polymer and the polyfunctional isocyanate compound is preferably 50 mass% or more, more preferably 60 mass% or more, and even more preferably 70 mass% or more, based on the total mass of the release layer.

[0088] The release layer may contain components other than the reaction cured product, such as crosslinking catalysts (e.g., amines, metal compounds, acids, etc.), reinforcing fillers, coloring dyes, pigments, and antistatic agents.

[0089] The crosslinking catalyst may be any substance that functions as a catalyst for the reaction (urethanization reaction) between a hydroxyl group-containing (meth)acrylic copolymer and a polyfunctional isocyanate compound, and a general urethanization reaction catalyst can be used. Examples of crosslinking catalysts include amine compounds such as tertiary amines, organotin compounds, organolead compounds, and organozinc compounds, among other organometallic compounds. Examples of tertiary amines include trialkylamines, N,N,N',N'-tetraalkyldiamines, N,N-dialkylaminoalcohols, triethylenediamine, morpholine derivatives, and piperazine derivatives. Examples of organotin compounds include dialkyltin oxides, dialkyltin fatty acid salts, and stannous fatty acid salts. Preferred crosslinking catalysts are organotin compounds, with dioctyltin oxide, dioctyltin dilaurate, dibutyltin laurate, and dibutyltin dilaurate being more preferred. Alternatively, a dialkylacetylacetonetin complex catalyst can be used, which is synthesized by reacting a dialkyltin ester with acetylacetone in a solvent and has a structure in which two acetylacetone molecules are coordinated to one dialkyltin atom. The amount of the crosslinking catalyst used is preferably 0.01 to 0.5 parts by mass per 100 parts by mass of the hydroxyl group-containing (meth)acrylic polymer.

[0090] The thickness of the release layer is preferably 0.05 to 3.0 μm, more preferably 0.05 to 2.5 μm, and even more preferably 0.05 to 2.0 μm. When the thickness of the release layer is equal to or greater than the lower limit, the release properties are excellent. When the thickness of the release layer is equal to or less than the upper limit, the function of the antistatic layer is fully exhibited, and the surface resistance of the film on the release layer side is low.

[0091] (Other Layers) The film may or may not have layers other than the substrate, antistatic layer, and release layer. Examples of other layers include a gas barrier layer, a colored layer, etc. These layers may be used alone or in combination of two or more.

[0092] (Film Manufacturing Method) The present film is manufactured, for example, by the following method. An antistatic layer coating liquid containing an antistatic layer composition and a liquid medium is applied to one surface of a substrate and dried to form an antistatic layer. A release layer coating liquid containing a release layer composition and a liquid medium is applied to the surface of the formed antistatic layer opposite the substrate and dried to form a release layer. Any other layer may be formed. Heating may be performed to promote curing during the formation of each layer. Heating may be performed each time a layer is formed, or may be performed after forming multiple layers. The antistatic layer composition preferably contains an antistatic agent, a carboxyl group-containing (meth)acrylic polymer, and at least one selected from the group consisting of a polyfunctional aziridine compound and a polyfunctional epoxy compound. The antistatic layer composition does not contain a liquid medium. The release layer composition preferably contains a hydroxyl group-containing (meth)acrylic polymer and a polyfunctional isocyanate compound. The release layer composition does not contain a liquid medium.

[0093] (Surface Resistivity of Film) The surface resistance of the film is not particularly limited, and 17 Ω / □ or less, 11 Ω / □ or less is preferable, and 10 10 Ω / □ or less is more preferable, and 10 9 It is more preferably Ω / □ or less. There is no particular lower limit for the surface resistance value. The surface resistance value of the present film is measured in accordance with IEC 60093:1980: Double Ring Electrode Method, at an applied voltage of 500 V for 1 minute. As a measuring instrument, for example, an ultra-high resistance meter R8340 (Advantec) can be used.

[0094] (Uses of Film) The present film is also useful as a release film used in the process of encapsulating a semiconductor element with a curable resin, or as a surface protection film for a semiconductor element, a solar cell module, etc. In particular, it is particularly useful as a release film used in the process of producing a semiconductor package having a complex shape, for example, an encapsulated body in which a part of an electronic component is exposed from the resin.

[0095] [Method for manufacturing a semiconductor package] In one aspect, a method for manufacturing a semiconductor package includes: placing the film on the inner surface of a mold; placing a substrate having a semiconductor element fixed thereto within the mold on which the film is placed; encapsulating the semiconductor element within the mold with a curable resin to produce an encapsulated body; and releasing the encapsulated body from the mold.

[0096] Examples of semiconductor packages include integrated circuits that integrate semiconductor elements such as transistors and diodes, and light-emitting diodes that have light-emitting elements. The package shape of the integrated circuit may cover the entire integrated circuit, or may cover only a portion of the integrated circuit, i.e., expose only a portion of the integrated circuit.Specific examples include SIP (Single In-line Package), ZIP (Zigzag In-line Package), DIP (Dual In-line Package), SOJ (Small Outline J-leaded package), SON (Small Outline Non-leaded package), SOI (Small Outline I-leaded package), SOF (Small Outline F-leaded package), QFP (Quad Flat Package), QFJ (Quad Flat J-leaded package), QFN (Quad Flat Non-leaded package), QFF (Quad Flat F-leaded package), PGA (Pin Grid Array), LGA (Land Grid Array), BGA (Ball Grid Array), DTP (Dual Tape carrier Package), QTP (Quad Tape carrier Package), CSP (Chip Size Package / Chip Scale Package), WL-CSP (Wafer Lebel CSP), LLP (Leadless Lead frame Package), DFN (Dual Flatpack No-leaded), MCP (Multi Chip Package), MCM (Multi Chip Module), SiP (System in a Package), PoP (Package on a Package), PiP (Package in a Package), QIP (or QUI P) (Quad In-line Package), CFP (Ceramic Flat Package), LLCC (Lead Less Chip Carrier), FOWLP (Fan Out Wafer Level Package), COB (Chip On Board), COF (Chip On Film), COG (Chip On Glass), and SVP (Surface Vertical Package), etc.From the viewpoint of productivity, semiconductor packages are preferably manufactured through collective sealing and singulation, and examples thereof include integrated circuits sealed using the MAP (Molded Array Packaging) method or the WL (Wafer Level Packaging) method.

[0097] As the curable resin, thermosetting resins such as epoxy resins and silicone resins are preferred, and epoxy resins are more preferred.

[0098] In one aspect, the semiconductor package may or may not include electronic components such as a source electrode and a seal glass in addition to the semiconductor element, and may have some of the electronic components such as the semiconductor element, source electrode, and seal glass exposed from the resin.

[0099] The semiconductor package manufacturing method can be a known manufacturing method except for using the present film. For example, a transfer molding method can be used as a method for encapsulating a semiconductor element, and a known transfer molding device can be used as the device used in this method. The manufacturing conditions can also be the same as those in known semiconductor package manufacturing methods.

[0100] Next, embodiments of the present disclosure will be described in detail using examples, but the embodiments of the present disclosure are not limited to these examples. In the following examples, Examples 2 to 4, 7, 8, 10 to 13, 16, 17, and 19 are working examples, and Examples 1, 5, 6, 9, 14, 15, and 18 are comparative examples. "Parts" means "parts by mass."

[0101] (Evaluation Method) <Elongation> A film was cut into a strip (width 50 mm, length 100 mm). This film was clamped and set between the grips of a tensile tester (RTC-131-A manufactured by Orientec Co., Ltd.). The film was stretched at a grip distance of 10 mm before tensioning and a speed of 100 mm / min until the film broke, and the elongation (mm) at break was measured. The measurement was carried out at 23°C. The elongation was calculated from the measurement results using the following formula. The results are shown in Table 1. Elongation (%) = elongation at break (mm) / grip distance before tensioning (10 mm) × 100

[0102] <Surface Resistivity> The surface resistance (Ω / □) of the release layer side of the film was measured according to IEC 60093:1980: Double Ring Electrode Method. The measurement was performed using an ultra-high resistance meter R8340 (Advantec) at an applied voltage of 500 V for 1 minute.

[0103] <Preparation of Epoxy Resin Composition for Mold Release Test> The following materials were pulverized and mixed for 5 minutes in a supermixer to prepare an epoxy resin composition for a sealing test: 8 parts of a phenylene skeleton-containing phenol aralkyl epoxy resin (softening point 58°C, epoxy equivalent 277), 2 parts of a bisphenol A epoxy resin (melting point 45°C, epoxy equivalent 172), 2 parts of a phenylene skeleton-containing phenol aralkyl resin (softening point 65°C, hydroxyl equivalent 165), 2 parts of a phenol novolac resin (softening point 80°C, hydroxyl equivalent 105), 0.2 parts of a curing accelerator (triphenylphosphine), 84 parts of an inorganic filler (fused spherical silica with a median diameter of 16 μm), 0.1 part of carnauba wax, 0.3 parts of carbon black, and 0.2 parts of a coupling agent (3-glycidoxypropyltrimethoxysilane). The cured product of this epoxy resin composition had a glass transition temperature of 135°C, a storage modulus of 6 GPa at 130°C, and a storage modulus of 1 GPa at 180°C.

[0104] <Mold Release Test> Using the film of each example as the mold release film and the epoxy resin composition for mold release test described above as the curable resin, a mold release test was conducted using an encapsulation device (G-LINE Manual System transfer molding device, Apic Yamada Co., Ltd.) according to the following procedure. A semiconductor element was fixed to a 70 mm x 230 mm copper lead frame. Five 5 mm x 5 mm protrusions were evenly spaced on the upper die of a mold equipped with an upper and lower die, and a 190 mm wide film roll was set in a roll-to-roll fashion. The film was positioned so that the substrate was facing the five protrusions. After placing the lead frame with the semiconductor element fixed on the lower die, the film was vacuum-adsorbed onto the upper die, the die was clamped, and the curable resin was poured into the upper die. To expose a portion of the semiconductor element from the resin, the five protrusions on the upper die were brought into direct contact with the surface of the release layer of the film and the semiconductor element placed in the lower die, and the encapsulation resin was filled around this area. After applying pressure for 5 minutes, the mold was opened and the sealed body was removed.

[0105] After the release test, the appearance of the release layer of the release film and the release surface of the cured product of the curable resin were visually inspected and evaluated according to the following criteria. A: The release layer was not attached to the surface of the cured product of the curable resin, and there was no peeling or damage to the release layer. B-1: The release layer was attached to the surface of the cured product of the curable resin, and no residue of the release layer was present on the release film side. It is believed that both the antistatic layer and the release layer were excessively cured, resulting in low interlayer adhesion and causing peeling at the interface. B-2: The release layer was attached to the surface of the cured product of the curable resin, and no residue of the release layer was present on the release film side. It is believed that a difference in shrinkage rate occurred due to a large or small amount of curing agent reactive group relative to the main agent of the antistatic layer and the release layer, causing peeling at the interface. C: The release layer was attached to the surface of the cured product of the curable resin, and residue of the release layer was present on the release film side. Because the amount of curing agent reactive groups relative to the main agent in both the antistatic layer and the release layer was extremely small, interlayer adhesion was good and interfacial peeling did not occur, but releasability was not expressed, and cohesive failure occurred within the release layer.

[0106] (Materials Used) <Substrate> ETFE film: Fluon (registered trademark) ETFE C-88AXP (manufactured by AGC) was fed into an extruder equipped with a T-die, and taken up between a pressing roll with an uneven surface and a metal roll with a mirror surface to form a film with a thickness of 100 μm. The temperature of the extruder and the T-die was 320 ° C, and the temperatures of the pressing roll and the metal roll were 100 ° C. The Ra of the surface of the obtained film was 2.0 μm on the pressing roll side and 0.2 μm on the mirror side. The mirror side was subjected to corona treatment so that the wetting tension based on ISO8296:1987 (JIS K6768:1999) was 40 mN / m or more. The obtained film was wound into a roll shape.

[0107] <Materials for Antistatic Layer> Base 1: ARAQUAT (registered trademark) AS601D (manufactured by Arakawa Chemical Industries, Ltd.), solid content 3.4 mass%, conductive polythiophene 0.4 mass%, carboxy group-containing (meth)acrylic polymer 3.0 mass%. Curing agent 1-1: ARAQUAT CL910 (manufactured by Arakawa Chemical Industries, Ltd.), solid content 10 mass%, trifunctional aziridine compound (2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate], aziridine equivalent 142 g / eq. Curing agent 1-2: CHEMITITE (registered trademark) DZ-22E (manufactured by Nippon Shokubai Co., Ltd.), solid content 25 mass%, bifunctional aziridine compound (4,4-bis(ethyleneiminocarbonylamino)diphenylmethane), aziridine equivalent 165 g / eq.

[0108] <Release Layer Materials> Base 2: Nissetsu (registered trademark) KP2562 (manufactured by Nippon Carbide Industries Co., Ltd.), solid content 35% by mass, hydroxyl group-containing (meth)acrylic polymer (hydroxyl value 70 mg KOH / g, crosslinking functional group equivalent 801 g / mol). Curing agent 2-1: Nissetsu CK157 (manufactured by Nippon Carbide Industries Co., Ltd.), solid content 100% by mass, trifunctional isocyanate compound (isocyanurate-type hexamethylene diisocyanate), NCO content 21% by mass. Curing agent 2-2: Duranate (registered trademark) D201 (manufactured by Asahi Kasei Corporation), solid content 100% by mass, bifunctional isocyanate compound (bifunctional prepolymer-type hexamethylene diisocyanate: OCN-R-NHC(=O)O-R'-OC(=O)NH-R-NCO), NCO content 15.8% by mass.

[0109] Example 1: 10 parts of base agent 1, 1 part of curing agent 1-1, and methanol were mixed to prepare an antistatic layer coating solution. The amount of methanol was such that the solids content of the antistatic layer coating solution was 2% by mass. The resulting antistatic layer coating solution was applied to the corona-treated surface of the substrate using a gravure coater and dried to form an antistatic layer with a thickness of 0.8 μm. Coating was performed using a direct gravure method, using a Φ100 mm x 250 mm wide grating 150#-depth 40 μm roll as the gravure plate. Drying was performed at 55°C for 1 minute through a roll-supported drying oven with an air flow of 19 m / s.

[0110] Next, 100 parts of base agent 2, 6 parts of curing agent 2-1, and ethyl acetate were mixed to prepare a coating liquid for a release layer. The amount of ethyl acetate was such that the solids content of the coating liquid for a release layer was 25% by mass. The obtained coating liquid for a release layer was applied to the surface of the substrate on which the antistatic layer was formed using a gravure coater, and dried to form a release layer with a thickness of 0.8 μm. Coating was performed using a direct gravure method, using a Φ100 mm x 250 mm wide grating 150#-depth 40 μm roll as a gravure plate. Drying was performed at 100 °C for 1 minute, passing through a roll-supported drying oven with an air flow of 19 m / s. The film was then aged at 40 °C for 120 hours to obtain a film.

[0111] (Examples 2 to 19) Films were prepared in the same manner as in Example 1, except that the amounts of the base agent and the type and amount of the curing agent blended in the coating liquid for the antistatic layer and the coating liquid for the release layer were changed as shown in Tables 1 and 2.

[0112] The elongation, surface resistance, and release test results of the obtained films are shown in Tables 1 and 2. In Tables 1 and 2, "aziridine groups relative to 100 mol% COOH" refers to the ratio of aziridine groups of the aziridine compound relative to 100 mol% of carboxy groups of the carboxy group-containing (meth)acrylic polymer. "NCO relative to 100 mol% OH" refers to the ratio of isocyanate groups of the isocyanate compound relative to 100 mol% of hydroxyl groups of the hydroxy group-containing (meth)acrylic polymer. "10^8" in the surface resistance value means 10 8 Shows.

[0113]

[0114]

[0115] As shown in Tables 1 and 2, the films of Examples 2 to 4, 7, 8, 10 to 13, 16, 17 and 19, which had elongation rates of more than 90% and less than 255%, were rated A in the release test.

[0116] The film of the present disclosure is such that the release layer and the antistatic layer are less likely to peel off when a semiconductor element is encapsulated with a curable resin. The film of the present disclosure can be used as a release film to produce semiconductor packages such as integrated circuits that integrate semiconductor elements such as transistors and diodes, source electrodes, sealing glass, and other electronic components. The film of the present disclosure can also be used as a protective film when processing, transporting, or storing semiconductor elements, solar cell modules, and the like.

[0117] REFERENCE SIGNS LIST 1 film 2 substrate 3 antistatic layer 4 release layer

Claims

1. A film comprising a substrate, an antistatic layer provided on one side of the substrate, and a release layer provided on the side of the antistatic layer opposite the substrate, wherein the film has an elongation of more than 90% and less than 255% when measured in a tensile test at 25°C at a speed of 100 mm / min using the following formula: Elongation (%) = (elongation at break (mm)) x 100 / (distance between grippers before tensioning (mm)).

2. The film according to claim 1, wherein the substrate comprises at least one material selected from the group consisting of fluororesin, polymethylpentene, syndiotactic polystyrene, polycycloolefin, silicone rubber, polyester elastomer, polybutylene terephthalate, polyethylene terephthalate, and polyamide.

3. The film according to claim 2, wherein the fluororesin comprises at least one selected from the group consisting of ethylene-tetrafluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymer, and tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer.

4. The film according to any one of claims 1 to 3, wherein the release layer comprises a cured product of a hydroxyl group-containing (meth)acrylic polymer and a difunctional or higher functional isocyanate compound.

5. The film according to claim 4, wherein the ratio of isocyanate groups of said isocyanate compound to 100 mol % of hydroxyl groups of said hydroxyl group-containing (meth)acrylic polymer is 20 to 115 mol %.

6. The film according to any one of claims 1 to 3, wherein the antistatic layer comprises a reaction-cured product of a carboxyl group-containing (meth)acrylic polymer and at least one compound selected from the group consisting of difunctional or higher functional aziridine compounds and difunctional or higher functional epoxy compounds.

7. The film according to claim 6, wherein the total ratio of the aziridine groups of said aziridine compound and the epoxy groups of said epoxy compound to 100 mol % of the carboxy groups of said carboxy group-containing (meth)acrylic polymer is 15 to 130 mol %.

8. The film according to any one of claims 1 to 3, wherein the thickness of the substrate is 25 to 250 µm.

9. The film according to any one of claims 1 to 3, wherein the release layer has a thickness of 0.05 to 3 µm.

10. The film according to any one of claims 1 to 3, which is a release film used in the process of encapsulating a semiconductor element with a curable resin.

11. A method for manufacturing a semiconductor package, comprising: placing the film according to any one of claims 1 to 3 on the inner surface of a mold; placing a substrate having a semiconductor element fixed thereto within the mold in which the film has been placed; encapsulating the semiconductor element within the mold with a curable resin to produce an encapsulated body; and releasing the encapsulated body from the mold.