Hot stamping part and method for manufacturing same

MYPI2025001328A0Undetermined Publication Date: 2024-02-29HYUNDAE STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025001328
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-08-31
Filing Date
2023-03-17
Publication Date
2024-02-29

AI Technical Summary

Technical Problem

The hot stamping process faces challenges in efficiently forming holes and reducing scrap material, as existing methods either increase processing time with laser equipment or compromise shear surface quality when using press molds.

Method used

The method involves simultaneously forming and cooling blanks to create holes, allowing for increased coil yield and reduced scrap, by heating the blank to a specific temperature range and transferring it to a press mold for hot pressing and piercing, followed by trimming and additional piercing steps using either laser or cold press molds.

Benefits of technology

This approach enhances the productivity and quality of hot stamping parts while improving raw material yield, reducing processing time and costs, and maintaining high shear surface quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025001328_DRAWING_001
    Figure PI2025001328_DRAWING_001
  • Figure PI2025001328_DRAWING_002
    Figure PI2025001328_DRAWING_002
  • Figure PI2025001328_DRAWING_003
    Figure PI2025001328_DRAWING_003
Patent Text Reader

Abstract

The present disclosure provides a method of manufacturing a hot stamping component, the method including preparing a blank, heating the blank, transferring the heated blank to a press mold, forming and first piercing the transferred blank by hot-pressing the transferred blank into a shape of a hot stamping component and forming at least two holes in the transferred blank, and trimming the formed blank by cutting an outer portion of the formed blank using the at least two holes.
Need to check novelty before this filing date? Find Prior Art

Description

Hot stamping parts and their manufacturing method

[0001] The present invention relates to a hot stamping part and a method for manufacturing the same.

[0002] As environmental and fuel efficiency regulations tighten globally, the need for lighter vehicle materials is increasing. Consequently, research and development on ultra-high-strength steel and hot-stamping steel is actively underway.

[0003] Hot stamping is a process for manufacturing high-strength parts by heating steel plates to high temperatures in a furnace, then forming and rapidly cooling them within a press. Additionally, a piercing process may be performed to cut and machine holes within the high-strength parts.

[0004] The piercing process uses laser equipment or press molds, but when laser equipment is used, processing time may increase, and when press molds are used, the cross-sectional quality may deteriorate.

[0005] As a technology related to this, there is Korean Patent Publication No. 10-2020-0080721 (Title of invention: Hot stamping part manufacturing device and hot stamping part manufacturing method using the same).

[0006] Embodiments of the present invention are characterized in that by forming holes in the blank simultaneously with forming and cooling the blank, the quantity of blanks obtainable from the coil can be increased and the amount of scrap discarded can be reduced.

[0007] One embodiment of the present invention provides a method for manufacturing a hot stamping part, comprising: a preparation step of preparing a blank; a heating step of heating the blank; a transfer step of transferring the heated blank to a press mold; a forming and first piercing step of hot-pressing the transferred blank to form a shape of a hot stamping part and forming at least two holes in the transferred blank; and a trimming step of cutting an outer portion of the formed blank using the at least two holes.

[0008] In the present embodiment, the preparation step may be a step of cutting the coil into the blank using a laser or a cold press mold.

[0009] In this embodiment, the blank may include an outer portion of the coil.

[0010] In the present embodiment, in the heating step, the blank can be heated to a temperature of Ac3 to 1000°C.

[0011] In the present embodiment, the temperature of the blank before the forming and first piercing steps may be equal to or higher than the Ms temperature.

[0012] In the present embodiment, in the forming and first piercing steps, the transferred blank can be cooled within the press mold.

[0013] In this embodiment, the transferred blank can be cooled for a time of 3 seconds or more and 20 seconds or less.

[0014] In this embodiment, the trimming step may be a step of cutting the outer portion of the molded blank using a laser or a cold press mold.

[0015] In the present embodiment, a second piercing step may further be included in which an additional hole is formed in the molded blank using the at least two holes.

[0016] In the present embodiment, after the trimming step, a step of removing a burr formed in the blank may be further included.

[0017] Another embodiment of the present invention provides a hot stamping part comprising: a first shear surface having a first hole defined therein; and a second shear surface formed on an edge of the hot stamping part; wherein a first shear line having a first length is formed in a portion adjacent to the first shear surface; and a second shear line or a first diagonal pattern having a second length smaller than the first length is formed in a portion adjacent to the second shear surface.

[0018] In this embodiment, the first length may be 50 μm or more, and the second length may be less than 50 μm.

[0019] In the present embodiment, a third shear surface may further be defined by a second hole spaced apart from the first hole.

[0020] In the present embodiment, a third short-line or second diagonal pattern having a third length smaller than the first length may be formed in a portion adjacent to the third shear surface.

[0021] In the present embodiment, a fourth shear surface may further be defined by a third hole spaced apart from the first hole.

[0022] In the present embodiment, a fourth short-circuit line having a fourth length greater than the second length may be formed in a portion adjacent to the fourth shear surface.

[0023] In this embodiment, the edge of the hot stamping part may have a curved shape.

[0024] In the present embodiment, the hot stamping part further includes a plating layer, and the plating layer may be provided along an edge of the hot stamping part.

[0025] Other aspects, features and advantages other than those described above will become apparent from the following detailed description, claims and drawings for carrying out the invention.

[0026] According to one embodiment of the present invention as described above, the productivity and quality of hot stamping parts can be improved, and at the same time, the raw material input yield can be enhanced.

[0027] FIG. 1 is a flowchart schematically illustrating a method for manufacturing a hot stamping part according to one embodiment of the present invention.

[0028] FIG. 2 is a flowchart schematically illustrating a preparation step of a method for manufacturing a hot stamping part according to one embodiment of the present invention.

[0029] Figure 3 is a plan view schematically illustrating a blank according to one embodiment of the present invention.

[0030] FIG. 4 is a flowchart schematically illustrating a heating step of a method for manufacturing a hot stamping part according to one embodiment of the present invention.

[0031] FIG. 5 is a drawing illustrating a heating furnace having a plurality of sections in a heating step of a method for manufacturing a hot stamping part according to one embodiment of the present invention.

[0032] FIGS. 6 and 7 are cross-sectional views illustrating the forming and first piercing steps of a manufacturing process of a hot stamping part according to one embodiment of the present invention.

[0033] FIG. 8 is a perspective view schematically illustrating a blank of a manufacturing process of a hot stamping part according to one embodiment of the present invention.

[0034] FIG. 9 is a perspective view illustrating a second piercing step of a manufacturing process of a hot stamping part according to one embodiment of the present invention.

[0035] FIG. 10 is a perspective view schematically illustrating a hot stamping part according to one embodiment of the present invention.

[0036] FIG. 11 is a cross-sectional view schematically illustrating a frontal section of a first hole of a hot stamping part according to one embodiment of the present invention.

[0037] FIG. 12 is a cross-sectional view schematically illustrating a front surface of a first additional hole or a front surface of a first edge of a hot stamping part according to one embodiment of the present invention.

[0038] FIGS. 13 and 14 are plan views and cross-sectional views schematically illustrating a frontal surface of a first additional hole or a frontal surface of a first edge of a hot stamping part according to one embodiment of the present invention.

[0039] FIG. 15 is a cross-sectional view schematically illustrating a shear surface of a second edge of a hot stamping part according to one embodiment of the present invention.

[0040] Figures 16 and 17 are drawings illustrating the difference according to the length of the short-circuit line formed around the cross-section.

[0041] FIGS. 18 and 19 are plan views showing the effect of applying a manufacturing method according to one embodiment of the present invention.

[0042] The present invention is capable of various modifications and embodiments. Specific embodiments are illustrated in the drawings and described in detail in the detailed description. The effects and features of the present invention, as well as the methods for achieving them, will become clearer with reference to the embodiments described in detail below, along with the drawings. However, the present invention is not limited to the embodiments disclosed below and can be implemented in various forms.

[0043] In the examples below, the terms first, second, etc. are not used in a limiting sense, but are used for the purpose of distinguishing one component from another.

[0044] In the examples below, singular expressions include plural expressions unless the context clearly indicates otherwise.

[0045] In the following examples, terms such as “include” or “have” mean that a feature or component described in the specification is present, and do not preclude the possibility that one or more other features or components may be added.

[0046] In the following examples, when a part such as a film, region, component, etc. is said to be on or above another part, it includes not only a case where it is directly on top of the other part, but also a case where another film, region, component, etc. is interposed in between.

[0047] For convenience of explanation, the sizes of components in the drawings may be exaggerated or reduced. For example, the sizes and thicknesses of each component shown in the drawings are arbitrarily shown for convenience of explanation, and the present invention is not necessarily limited to what is shown.

[0048] In this specification, “A and / or B” refers to the case where it is A, or B, or both A and B. In addition, in this specification, “at least one of A and B” refers to the case where it is A, or B, or both A and B.

[0049] In the following examples, when referring to "planar", it means when the target portion is viewed from above, and when referring to "cross-sectional", it means when the target portion is viewed from the side in a cross-section cut vertically. In the following examples, when referring to "overlapping", it includes "planar" and "cross-sectional" overlapping.

[0050] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings, and when describing with reference to the drawings, identical or corresponding components will be given the same drawing reference numerals.

[0051] FIG. 1 is a flowchart schematically illustrating a method for manufacturing a hot stamping part according to one embodiment of the present invention.

[0052] Referring to FIG. 1, a method for manufacturing a hot stamping part according to one embodiment may include a preparation step (S100), a heating step (S200), a transfer step (S300), a forming and first piercing step (S400), and a trimming step (S500). Specifically, the method for manufacturing a hot stamping part according to one embodiment may include a preparation step (S100) of preparing a blank, a heating step (S200) of heating the blank, a transfer step (S300) of transferring the heated blank to a press mold, a forming and first piercing step (S400) of hot-pressing the transferred blank to form a shape of a hot stamping part and forming at least two holes in the transferred blank, and a trimming step (S500) of cutting an outer portion of the formed blank using the at least two holes.

[0053] FIG. 2 is a flowchart schematically illustrating a preparation step of a method for manufacturing a hot stamping part according to one embodiment of the present invention, and FIG. 3 is a plan view schematically illustrating a blank according to one embodiment of the present invention.

[0054] Referring to FIGS. 2 and 3, the preparation step (S100) may be a step of preparing a blank (100) for hot stamping. In one embodiment, the preparation step (S100) may include a hot rolling step (S110), a cooling / coiling step (S120), a cold rolling step (S130), an annealing step (S140), a plating step (S150), and a cutting step (S160).

[0055] First, a reheating step of the steel slab may be performed. In the reheating step of the steel slab, the steel slab obtained through the continuous casting process is reheated to a predetermined temperature, so that the components segregated during casting can be re-dissolved. In one embodiment, the slab reheating temperature (SRT) may be about 1,200°C to about 1,400°C. If the slab reheating temperature (SRT) is lower than about 1,200°C, the components segregated during casting may not be sufficiently re-dissolved, making it difficult to significantly see the homogenization effect of the alloy elements and the solid solution effect of titanium (Ti). A higher slab reheating temperature (SRT) is advantageous for homogenization, but if the slab reheating temperature (SRT) exceeds about 1,400°C, the austenite crystal grain size increases, making it difficult to secure strength, and the manufacturing cost of the steel plate may increase due to the excessive heating process.

[0056] In the hot rolling step (S110), the reheated plate may be hot rolled at a predetermined finishing rolling temperature. A hot-rolled steel plate may be manufactured through the hot rolling step (S110). In one embodiment, the finishing rolling temperature (Finishing Delivery Temperature: FDT) may be about 880°C to about 950°C. At this time, if the finishing rolling temperature (FDT) is lower than about 880°C, it is difficult to secure the workability of the steel plate due to the occurrence of a mixed grain structure caused by abnormal region rolling, and not only may the workability be reduced due to microstructural non-uniformity, but also a problem of sheet passing during hot rolling may occur due to a rapid phase change. If the finishing rolling temperature (FDT) exceeds about 950°C, the austenite grains may become coarser, and the TiC precipitates may become coarser, which may deteriorate the performance of the hot stamping part.

[0057] In the cooling / coiling step (S120), the hot-rolled hot-rolled steel sheet may be cooled to a predetermined coiling temperature (Coiling Temperature, CT) and coiled. In one embodiment, the coiling temperature of the cooling / coiling step (S120) may be about 550°C to about 800°C. The coiling temperature affects the redistribution of carbon, and when the coiling temperature is lower than about 550°C, the low-temperature phase fraction due to overcooling may increase, which may increase the strength, and there is a concern that the rolling load may be severe during cold rolling, and the ductility may rapidly decrease. Conversely, when the coiling temperature exceeds about 800°C, abnormal crystal grain growth or excessive crystal grain growth may cause formability deterioration and strength deterioration.

[0058] In the cold rolling step (S130), the coiled hot-rolled steel sheet may be uncoiled, pickled, and then cold rolled. The pickling process may be performed to remove scale from the coiled hot-rolled steel sheet, i.e., the hot-rolled coil manufactured through the hot rolling process. Through the cold rolling step (S130), a cold-rolled steel sheet may be manufactured.

[0059] The annealing step (S140) may anneal the cold-rolled cold-rolled steel sheet at a temperature of about 700°C or higher. For example, the annealing step (S140) may include heating the cold-rolled cold-rolled steel sheet and cooling the heated cold-rolled steel sheet at a predetermined cooling rate. The cold-rolled steel sheet may be annealed in the annealing step (S140). The annealing step (S140) may be performed in an annealing furnace.

[0060] In one embodiment, the annealing temperature of the cold-rolled steel sheet may be between about 750°C and about 900°C. If the annealing temperature of the cold-rolled steel sheet is lower than about 750°C, the desired structure may not be obtained, and recrystallization may not be sufficiently completed. On the other hand, if the annealing temperature of the cold-rolled steel sheet exceeds about 900°C, the annealing temperature may be too high, reducing the efficiency of the manufacturing process. Therefore, if the annealing temperature of the cold-rolled steel sheet satisfies the range of about 750°C to about 900°C, the desired structure may be obtained, recrystallization may be sufficiently completed, and the efficiency of the manufacturing process may be improved.

[0061] The plating step (S150) may be a step of forming a plating layer on an annealed cold-rolled steel sheet. In one embodiment, a plating layer may be formed on the annealed cold-rolled steel sheet through the plating step (S150). At this time, the plating layer may include a zinc (Zn)-based plating layer or an aluminum (Al)-based plating layer.

[0062] Specifically, in the plating step (S150), the annealed cold-rolled steel sheet can be immersed in a plating bath. At this time, the plating bath can maintain a temperature of about 400°C to about 700°C. The plating amount is about 40 g / m on both sides of the base material of the cold-rolled steel sheet. 2 About 200 g / m 2 It can be done. After the plating step (S150), the cold rolled steel sheet with the plating layer formed can be wound into a coil shape.

[0063] Although Fig. 2 illustrates that a cold rolling step (S130), an annealing step (S140), and a plating step (S150) are performed after a cooling / coiling step (S120), the present invention is not limited thereto. At least one of the cold rolling step (S130), the annealing step (S140), and the plating step (S150) may be omitted. For example, the cold rolling step (S130) and the annealing step (S140) may be omitted. In this case, the hot-rolled steel sheet on which a plating layer is formed after the plating step (S150) may be coiled into a coil shape.

[0064] Thereafter, in the cutting step (S160), a steel plate (e.g., a cold-rolled steel plate or a hot-rolled steel plate) wound in a coil shape is uncoiled, and then the steel plate can be cut into a blank (100) using a laser or a cold press mold. At this time, the blank (100) may include an outer portion (or edge) of the coil. For example, the blank (100) may include an outer portion (or edge) of the steel plate.

[0065] Referring to Fig. 1, after the preparation step (S100) of preparing a blank (100), a heating step (S200) of heating the blank (100) may be performed. The heat source method in the heating step (S200) may be direct heating or indirect heating. The heat source method in the heating step (S200) may use either direct heating or indirect heating, or a combination of direct heating and indirect heating.

[0066] In one embodiment, in the heating step (S200), the blank (100) may be heated within a heating furnace. The heating furnace may be provided with one section having one temperature range (or, a single temperature), or may be provided with multiple sections having different temperature ranges. When the heating furnace is provided with one section having one temperature range, the blank (100) may be heated within the heating furnace to a target temperature within one temperature range. At this time, the target temperature may be Ac3 to about 1,000°C. That is, the blank (100) may be heated within a heating furnace having a temperature range of Ac3 to about 1,000°C until the temperature of the blank (100) reaches Ac3 to about 1,000°C.

[0067] On the other hand, if the furnace is equipped with multiple sections having different temperature ranges, the blank (100) can be heated to the target temperature in different temperature ranges within the furnace.

[0068] FIG. 4 is a flowchart schematically illustrating a heating step of a method for manufacturing a hot stamping part according to one embodiment of the present invention, and FIG. 5 is a drawing illustrating a heating furnace having a plurality of sections in the heating step of a method for manufacturing a hot stamping part according to one embodiment of the present invention.

[0069] Referring to FIGS. 4 and 5, in the heating step (S200), the blank (100, see FIG. 3) may be heated in a heating furnace having multiple sections having different temperature ranges. As illustrated in FIG. 4, the heating step (S200) may include a multi-stage heating step (S210) and a soaking heating step (S220). The multi-stage heating step (S210) and the soaking heating step (S220) may be steps in which the blank (100) is heated while passing through multiple sections provided in the heating furnace.

[0070] In one embodiment, the overall temperature of the furnace may be about 680°C to about 1,000°C. Specifically, the overall temperature of the furnace in which the multi-stage heating step (S210) and the soaking heating step (S220) are performed may be about 680°C to about 1,000°C. At this time, the temperature of the furnace in which the multi-stage heating step (S210) is performed may be about 680°C to about Ac3, and the temperature of the furnace in which the soaking heating step (S220) is performed may be about Ac3 to about 1,000°C.

[0071] In the multi-stage heating step (S210), the blank (100) may be heated (or heated) in stages while passing through multiple sections provided in the heating furnace. There may be multiple sections among the multiple sections provided in the heating furnace in which the multi-stage heating step (S210) is performed, and the temperature is set for each section so that the temperature increases from the inlet of the heating furnace into which the blank (100) is introduced toward the outlet of the heating furnace from which the blank (100) is taken out, so that the blank (100) may be heated (or heated) in stages.

[0072] After the multi-stage heating step (S210), a soaking heating step (S220) may be performed. In the soaking heating step (S220), the multi-stage heated blank may be heated (or soaked heated) while passing through a section of a heating furnace set to a temperature of about Ac3 to about 1,000°C. Among the multiple sections provided in the heating furnace, at least one section may be used for the soaking heating step (S220).

[0073] According to one embodiment, a heating furnace may have a plurality of sections having different temperature ranges. Specifically, the heating furnace may have a first section (P1) having a first temperature range (T1), a second section (P2) having a second temperature range (T2), a third section (P3) having a third temperature range (T3), a fourth section (P4) having a fourth temperature range (T4), a fifth section (P5) having a fifth temperature range (T5), a sixth section (P6) having a sixth temperature range (T6), and a seventh section (P7) having a seventh temperature range (T7).

[0074] In one embodiment, in the multi-stage heating step (S611), the blank may be heated stepwise while passing through the first section (P1) to the fourth section (P4) defined within the heating furnace. Additionally, in the crack heating step (S612), the blank that has been multi-stage heated in the first section (P1) to the fourth section (P4) may be crack heated while passing through the fifth section (P5) to the seventh section (P7).

[0075] The first section (P1) to the seventh section (P7) may be arranged sequentially within the furnace. The first section (P1) having the first temperature range (T1) may be adjacent to the inlet of the furnace into which the blank is fed, and the seventh section (P7) having the seventh temperature range (T7) may be adjacent to the outlet of the furnace from which the blank is taken out. Accordingly, the first section (P1) having the first temperature range (T1) may be the first section of the furnace, and the seventh section (P7) having the seventh temperature range (T7) may be the last section of the furnace.

[0076] The temperatures of the plurality of sections provided in the furnace, for example, the temperatures of the first section (P1) to the seventh section (P7), may increase from the inlet of the furnace into which the blank is fed to the outlet of the furnace from which the blank is taken out. However, the temperatures of the fifth section (P5), the sixth section (P6), and the seventh section (P7) may be the same. In addition, the temperature difference between two adjacent sections among the plurality of sections provided in the furnace may be greater than 0°C and less than or equal to 100°C. For example, the temperature difference between the first section (P1) and the second section (P2) may be greater than 0°C and less than or equal to 100°C.

[0077] The furnace temperature of the soaking heating step (S220) may be Ac3 to about 1,000°C. If the furnace temperature of the soaking heating step (S220) is less than Ac3, the manufactured hot stamping part may not have the desired material. On the other hand, if the furnace temperature of the soaking heating step (S220) exceeds about 1,000°C, carbide-forming elements or nitride-forming elements such as Ti, V, Nb, and Mo in the blank (100) may be dissolved into the parent material, making it difficult to suppress grain coarsening.

[0078] Although FIG. 5 illustrates a heating furnace according to one embodiment as having seven sections with different temperature ranges, the present invention is not limited thereto. The heating furnace may also have five, six, or eight sections with different temperature ranges.

[0079] In one embodiment, the heating step (S200) is provided with a multi-stage heating step (S210) and a crack heating step (S220), so that the temperature of the heating furnace can be set in stages, thereby improving the energy efficiency of the heating furnace.

[0080] In one embodiment, the furnace may have a length of about 20 m to about 40 m along the transport path of the blank (100). The furnace may have a plurality of sections having different temperature ranges, and a ratio of the length of a section in which the blank is multi-heated among the plurality of sections to the length of a section in which the blank is crack-heated among the plurality of sections may satisfy about 1:1 to about 4:1. If the length of the section in which the blank is crack-heated within the furnace increases so that the ratio of the length of the section in which the blank is multi-heated to the length of the section in which the blank is crack-heated exceeds about 1:1, the amount of hydrogen penetrating into the blank in the crack-heating section may increase, which may increase delayed fracture. On the other hand, if the length of the section in which the blank is crack-heated decreases so that the ratio of the length of the section in which the blank is multi-heated to the length of the section in which the blank is crack-heated is less than about 4:1, the crack-heating section (or time) may not be sufficiently secured, which may result in uneven strength of the manufactured hot stamped part. For example, the length of a uniform heating section among the plurality of sections provided in the furnace may be about 20% to about 50% of the total length of the furnace.

[0081] In one embodiment, the total heating time for which the heating step (S200) is performed may be about 2 min to about 20 min. That is, the total time for which the blank remains in the heating furnace may be about 2 min to about 20 min. If the total heating time for which the heating step (S200) is performed is about 2 min or less, the heating time may be insufficient, and thus the manufactured hot stamping part may not have a desired material. On the other hand, if the total heating time for which the heating step (S200) is performed is about 20 min or more, the heating time may be too long, which may lower the production speed and reduce the economic efficiency. Therefore, if the total heating time for which the heating step (S200) is performed satisfies about 2 min to about 20 min, the manufactured hot stamping part may have a desired material, and at the same time, the deterioration of the economic efficiency of the manufacturing process may be prevented or minimized.

[0082] Referring to FIG. 1, a transfer step (S300) may be performed after the heating step (S200). In the transfer step (S300), a heated blank (100) may be transferred to a press mold (400, see FIG. 6). For example, the heated blank (100) may be taken out from the heating furnace and then transferred to the press mold (400).

[0083] In the transport step (S300), the heated blank (100) may be cooled to ambient temperature (or room temperature). That is, the heated blank (100) may be air-cooled at ambient temperature during transport. If the heated blank (100) is not air-cooled, the mold entry temperature (e.g., molding start temperature) may increase, causing wrinkles (or bends) to occur on the surface of the manufactured hot stamping part. In addition, since the use of a refrigerant may affect the subsequent process (hot stamping), it may be desirable for the heated blank (100) to be air-cooled during transport.

[0084] FIGS. 6 and 7 are cross-sectional views illustrating the forming and first piercing steps of a manufacturing process of a hot stamping part according to one embodiment of the present invention, and FIG. 8 is a perspective view schematically illustrating a blank of a manufacturing process of a hot stamping part according to one embodiment of the present invention. Specifically, FIG. 6 is a cross-sectional view of a blank and a press mold before the forming and first piercing steps are performed, FIG. 7 is a cross-sectional view of a blank and a press mold during the forming and first piercing steps, and FIG. 8 is a perspective view schematically illustrating a blank after the forming and first piercing steps.

[0085] Referring to FIGS. 1, 6, 7, and 8, a forming and first piercing step (S400) may be performed after the transfer step (S300). The forming and first piercing step (S400) may be a step of hot-pressing the transferred blank (100) to form it into the shape of a hot stamping part and forming at least two holes (110) in the transferred blank (100).

[0086] In one embodiment, the forming and first piercing step (S400) may be performed in a press mold (400). The press mold (400) may include a lower mold (410), an upper mold (420), and a punch (430). The lower mold (410) may have a shape of a bottom surface of a hot stamping part. The upper mold (420) may face the lower mold (410) and have a shape of a top surface of the hot stamping part. The press mold (400) may have at least one punch (430), preferably at least two punches (430). In one embodiment, the punches (430) may include a first punch and a second punch.

[0087] For example, as will be described later, since a laser process or a cold piercing process must be performed using the holes formed through hot piercing, at least two or more holes may be formed through hot piercing. Specifically, since the blank (100) must be seated on a tool using the holes formed through hot piercing as a guide pattern (or, reference point) and then subsequent processes must be performed, at least two or more holes may be formed in the blank (100) through hot piercing.

[0088] However, the present invention is not limited thereto. For example, various modifications are possible, such as a press mold (400) being provided with only one punch (430) or three or more punches (430).

[0089] Although not shown, when the press mold (400) is equipped with only one punch (430), a foam bead may be formed at the edge of the blank (100) during molding of the blank (100).

[0090] In one embodiment, the clearance between the punch (430) and the mold (e.g., the lower mold (410) and / or the upper mold (420)) may be from about 2% to about 30%. If the clearance is less than about 2%, the punch (430) may become stuck in the mold due to thermal expansion of the mold. On the other hand, if the clearance exceeds about 30%, the vibration of the punch (430) may become severe, which may lead to uneven quality, including the formation of short-circuit lines on the cross-section. For example, the uniformity of the short-circuit lines may deteriorate, such as when many short-circuit lines are formed only on a portion of the cross-section. Accordingly, when the clearance between the punch (430) and the mold (e.g., the lower mold (410) and / or the upper mold (420)) is about 2% to about 30%, the punch (430) can be prevented from being caught in the mold due to thermal expansion, and the short-circuit lines formed around the shear surface can be uniformly formed.

[0091] In one embodiment, the blank (100) may be hot pressed in the forming and first piercing step (S400). Specifically, the blank (100) may be hot pressed to form the shape of a hot stamping part by using a press mold (400) including a lower mold (410) and an upper mold (420) that are transferred (or heated). Specifically, the blank (100) may be hot pressed by pressing (e.g., hot pressing) the lower mold (410) having the shape of the bottom surface of the hot stamping part with the upper mold (420) having the shape of the top surface of the hot stamping part, thereby forming the blank (100) into the shape of the hot stamping part.

[0092] In one embodiment, in the forming and first piercing step (S400), hot forming of the blank (100) may be performed simultaneously with hot piercing of the blank (100). Specifically, when hot forming the blank (100), the punch (430) included in the press die (400) may be lowered to perform hot piercing of the blank (100). Alternatively, in the forming and first piercing step (S400), after hot forming of the blank (100) is completed, the punch (430) included in the press die (400) may be lowered to perform hot piercing of the blank (100). That is, in the forming and first piercing step (S400), the punch (430) included in the press mold (400) may be lowered to perform hot piercing on the blank (100) simultaneously with the hot forming of the blank (100) or after the hot forming of the blank (100) is completed.

[0093] In one embodiment, when hot forming a blank (100) using a press mold (400), a first punch and a second punch included in the press mold (400) may be lowered to form at least two holes (110a, 110b) in the blank (100). Specifically, in the process of hot forming the blank (100) by pressing the lower mold (410) and the blank (100) with the upper mold (420), the first punch and the second punch may be lowered to form a first hole (110a) and a second hole (110b) in the blank (100). The hot piercing may be performed simultaneously with the hot forming. Alternatively, the hot piercing may be performed after the hot forming is completed. That is, the hot piercing may be performed simultaneously with the hot forming or after the hot forming is completed.

[0094] Although FIGS. 6 and 7 illustrate that a punch (430) included in a press mold (400) is lowered to form a hole (110) in a blank (100), the present invention is not limited thereto. Although not illustrated, a hole (110) may also be formed in a blank (100) through a separately provided external device.

[0095] In one embodiment, the temperature of the blank (100) before the forming and first piercing step (S400) is performed may be equal to or higher than the Ms temperature. If the temperature of the blank (100) before the forming and first piercing step (S400) is lower than the Ms temperature, a large load may be generated during the forming and first piercing, which may cause damage to the press die (400) and / or the punch (430). Preferably, the hot piercing may be performed at a temperature of about 350°C or higher and about 750°C or lower. More preferably, the hot piercing may be performed at a temperature of about 400°C or higher and about 700°C or lower.

[0096] In one embodiment, the blank (100) may be cooled while being formed into the final part shape in the press mold (400) (or during hot forming). The press mold (400) may be provided with cooling channels (440) through which a coolant circulates therein. For example, the interiors of the lower mold (410) and the upper mold (420) may each have cooling channels (440). Specifically, the cooling channels (440) may be arranged within the lower mold (410) and the upper mold (420) along the surface of the lower mold (410) and the surface of the upper mold (420). The blank (100), which has been heated by the circulation of the coolant supplied through the cooling channels (440) provided in the press mold (400), may be rapidly cooled. At this time, in order to prevent a spring back phenomenon of the plate material and to maintain a desired shape, the rapid cooling may be performed while applying pressure in a closed state. When forming and cooling a heated blank (100), the average cooling rate can be at least about 10°C / s or more to the martensite end temperature. Preferably, the cooling can be at least about 20°C / s or more.

[0097] The blank (100) may be held in the press mold (400) for about 3 seconds to about 20 seconds. For example, the engagement state of the press mold (400) may be held for about 3 seconds to about 20 seconds. If the holding time in the press mold (400) is less than about 3 seconds, sufficient cooling of the blank (100) may not occur, resulting in thermal deformation due to residual heat and temperature deviations between sections, which may deteriorate the dimensional quality. On the other hand, if the holding time in the press mold (400) exceeds about 20 seconds, the holding time in the press mold (400) may become longer, which may deteriorate productivity.

[0098] In one embodiment, the processes of hot press forming the heated blank (100), hot piercing the heated blank (100), and cooling the heated blank (100) can be performed simultaneously within the press die (400). For example, the hot pressing, hot piercing, and cooling of the blank (100) can be performed simultaneously with the press die (400) in a closed (or interlocked) state.

[0099] FIG. 9 is a perspective view illustrating a trimming step of a manufacturing process of a hot stamping part according to one embodiment of the present invention.

[0100] Referring to FIGS. 1 and 9, a trimming step (S500) may be performed after the forming and first piercing step (S400). The trimming step (S500) may be a step of cutting an outer portion of a formed blank (100) using at least two holes (110a, 110b) formed in the formed blank (100). In other words, the trimming step (S500) may be a step of cutting an outer portion of a blank (100) using two holes (110a, 110b) formed in the blank (100) through hot piercing.

[0101] In one embodiment, in the trimming step (S500), the edge of the blank (100) may be cut using at least two holes (110a, 110b) formed through hot piercing as reference points (or, guide patterns). In other words, the blank (100) may be seated in a tool using the at least two holes (110a, 110b) formed in the molded blank (100), and the edge of the molded blank (100) may be cut. For example, after inserting fixing pins (510a, 510b) into each of the at least two holes (110a, 100b) formed in the molded blank (100), the outer portion of the molded blank (100) may be cut.

[0102] In one embodiment, the trimming step (S500) may be performed using a laser or a press mold (e.g., a cold press mold).

[0103] A method for manufacturing a hot stamping part according to one embodiment of the present invention may include forming a hole (110) in a blank (100) through hot piercing, and then additionally cutting an outer portion of the blank (100) through cold trimming or laser trimming. That is, a method for manufacturing a hot stamping part according to one embodiment of the present invention may include performing a hot piercing process on a blank (100), cooling the blank (100), and then performing cold trimming or laser trimming.

[0104] In one embodiment, a second piercing step may be performed after the forming and first piercing step (S400). The second piercing step may be a step of forming an additional hole (120) in the formed blank (100) using at least two holes (110a, 110b) formed in the formed blank (100). In other words, the second piercing step may be a step of forming an additional hole (e.g., an additional hole (120)) in the blank (100) using two holes (110a, 110b) formed in the blank (100) through hot piercing.

[0105] In one embodiment, the second piercing step may be performed during the trimming step (S500). For example, the second piercing step and the trimming step (S500) may be performed simultaneously. Alternatively, the second piercing step may be performed before the trimming step (S500) or after the trimming step (S500). For example, the second piercing step and the trimming step (S500) may be performed sequentially.

[0106] Although FIG. 9 illustrates that two additional holes (120a, 120b) are formed through the second piercing step, the present invention is not limited thereto. One additional hole (120) may be formed, or three or more additional holes (120) may be formed.

[0107] In one embodiment, in the second piercing step, additional holes (120a, 120b) may be formed in the blank (100) using at least two holes (110a, 110b) formed through hot piercing as reference points (or, guide patterns). In other words, the blank (100) may be seated in a tool using the at least two holes (110a, 110b) formed in the molded blank (100), and additional holes (120a, 120b) may be formed in the molded blank (100). For example, fixing pins (510a, 510b) may be inserted into each of the at least two holes (110a, 110b) formed in the molded blank (100), and then the additional holes (120a, 120b) may be formed in the molded blank (100).

[0108] In one embodiment, the additional holes (120a, 120b) in the second piercing step may be formed using a laser or a cold press mold. While FIG. 9 illustrates two additional holes (120a, 120b) being formed through the second piercing step, the present invention is not limited thereto. One additional hole (120) may be formed, or three or more additional holes (120) may be formed.

[0109] A method for manufacturing a hot stamping part according to one embodiment of the present invention can form a hole (110) in a blank (100) through hot piercing, and then form an additional hole (e.g., an additional hole (120)) in the blank (100) through cold piercing or laser piercing. That is, a method for manufacturing a hot stamping part according to one embodiment of the present invention can perform a hot piercing process on a blank (100), cool the blank (100) on which the hot piercing process has been performed, and then perform a cold piercing process or a laser piercing process.

[0110] In one embodiment, a portion of the perimeter of the manufactured hot stamped part may be an edge of the coil raw material. That is, a portion of the perimeter of the manufactured hot stamped part may be an edge of the coil raw material without being cut.

[0111] In one embodiment, after the trimming step (S500) and / or the second piercing step are performed, a step for removing burrs formed in the blank may be performed. Through this, burrs formed during processes such as hot piercing, cold piercing, and cold trimming may be removed.

[0112] FIG. 10 is a perspective view schematically illustrating a hot stamping part according to one embodiment of the present invention.

[0113] Referring to FIG. 10, a hot stamping part (1000) according to one embodiment may include a hole (110) and an additional hole (120). The hot stamping part (1000) may include an edge (130). In addition, the hot stamping part (1000) may include cross-sections (150a, 150b, 150c, 150d, 150e, 150f) defined in the hole (110), the additional hole (120), and the edge (130), respectively.

[0114] As described above in the method for manufacturing a hot stamping part (1000), the hot stamping part (1000) may include at least two holes (110). The holes (110) may include a first hole (110a) and a second hole (110b). That is, the hot stamping part (1000) may include a first hole (110a) and a second hole (110b). In FIG. 10, the hot stamping part (1000) is illustrated as having two holes (110a, 110b), but the present invention is not limited thereto. For example, the hot stamping part (1000) may be provided with one or three or more holes.

[0115] Additionally, the hot stamping part (1000) may include at least one additional hole (120). For example, the hot stamping part (1000) may include a first additional hole (120a) and a second additional hole (120b). Although FIG. 10 illustrates two additional holes (120a, 120b), the present invention is not limited thereto. The number of additional holes (120) provided in the hot stamping part (1000) may be one or three or more.

[0116] At this time, the first hole (110a) and the second hole (110b) may be formed through the forming and first piercing step (S400), and the first additional hole (120a) and the second additional hole (120b) may be formed through the second piercing step. For example, the first hole (110a) and the second hole (110b) may be formed through hot piercing, and the first additional hole (120a) and the second additional hole (120b) may be formed through cold piercing or laser piercing.

[0117] Additionally, the hot stamping part (1000) may include an edge (130). Here, the edge (130) of the hot stamping part (1000) may refer to a surface extending along the long side of the hot stamping part (1000). The edge (130) may include a first edge (130a) and a second edge (130b). That is, the hot stamping part (1000) may include a first edge (130a) and a second edge (130b).

[0118] In one embodiment, the shear surface (150) may include a first shear surface (150a), a second shear surface (150b), a third shear surface (150c), a fourth shear surface (150d), a fifth shear surface (150e), and a sixth shear surface (150f). The first shear surface (150a), the second shear surface (150b), the third shear surface (150c), the fourth shear surface (150d), the fifth shear surface (150e), and the sixth shear surface (150f) may be formed together during the process in which the first hole (110a), the second hole (110b), the first additional hole (120a), the second additional hole (120b), the first edge (130a), and the second edge (130b) are formed, respectively. That is, the first shear surface (150a), the second shear surface (150b), the third shear surface (150c), the fourth shear surface (150d), the fifth shear surface (150e), and the sixth shear surface (150f) can be formed together when the first hole (110a), the second hole (110b), the first additional hole (120a), the second additional hole (120b), the first edge (130a), and the second edge (130b) are formed, respectively.

[0119] In other words, a first hole (110a) may be defined by a first shear plane (150a), a second hole (110b) may be defined by a second shear plane (150b), a first additional hole (120a) may be defined by a third shear plane (150c), a second additional hole (120b) may be defined by a fourth shear plane (150d), a first edge (130a) may be defined by a fifth shear plane (150e), and a second edge (130b) may be defined by a sixth shear plane (150f).

[0120] FIG. 11 is a cross-sectional view schematically illustrating a frontal surface of a first hole of a hot stamping part according to an embodiment of the present invention, FIG. 12 is a cross-sectional view schematically illustrating a frontal surface of a first additional hole or a first edge of a hot stamping part according to an embodiment of the present invention, FIGS. 13 and 14 are a plan view and a cross-sectional view schematically illustrating a frontal surface of a first additional hole or a first edge of a hot stamping part according to an embodiment of the present invention, and FIG. 15 is a cross-sectional view schematically illustrating a frontal surface of a second edge of a hot stamping part according to an embodiment of the present invention.

[0121] For example, Fig. 11 is a cross-sectional view schematically illustrating a shear surface on which hot piercing has been performed, Fig. 12 is a cross-sectional view schematically illustrating a shear surface on which cold piercing (or cold press mold) has been performed, Figs. 13 and 14 are plan views and cross-sectional views schematically illustrating the front and cross-section of a shear surface on which laser piercing or laser trimming has been performed, and Fig. 15 is a cross-sectional view schematically illustrating a shear surface when the shear surface is the edge of a coil raw material. Figs. 11, 12, and 15 correspond to cross-sections observed with an optical microscope after etching the cross-section, and Figs. 13 and 14 correspond to cross-sections observed with an optical microscope of the front of the shear surface without etching and cross-sections of the shear surface observed with an optical microscope. In Figs. 11 to 15, the shapes and characteristics of the shear surfaces are exemplarily illustrated for convenience of explanation.

[0122] Referring to FIGS. 10 and 11, a hot stamping part (1000) may include a first shear surface (150a) in which a first hole (110a) is defined, and when observed with an optical microscope after cross-sectional etching, first short-circuit lines (1100) having a first length may be formed in a portion adjacent to the first shear surface (150a). At this time, the first length may be about 50 μm or more. In addition, a first burr (1110) may be formed around the first shear surface (150a). At this time, the first length may be defined as an average length of the first short-circuit lines (1100) formed in a portion adjacent to the first shear surface (150a).

[0123] That is, if the first hole (110a) included in the hot stamping part (1000) is formed through hot piercing, a short-circuit line (e.g., the first short-circuit line (1100)) having a length of about 50 μm or more may exist in a portion adjacent to the first shear surface (150a) where the first hole (110a) is defined. Accordingly, if a short-circuit line (e.g., the first short-circuit line (1100)) having a length of about 50 μm or more exists in a portion adjacent to the first shear surface (150a) where the first hole (110a) is defined, it can be understood that the first hole (110a) is formed through hot piercing. In other words, when the short-circuit lines (e.g., the first short-circuit lines (1100)) formed in the portion adjacent to the first shear surface (150a) where the first hole (110a) is defined have an average length of about 50 μm or more, the first hole (110a) may be formed by hot piercing.

[0124] Referring to FIGS. 10 and 12, the hot stamping part (1000) may include a third shear surface (150c) in which a first additional hole (120a) is defined, and when observed with an optical microscope after cross-sectional etching, second short-circuit lines (1200) having a second length smaller than a first length may be formed in a portion adjacent to the third shear surface (150c). At this time, the second length may be less than about 50 μm. In addition, a second burr (1210) may be formed around the third shear surface (150c). However, the height of the second burr (1210) formed around the third shear surface (150c) may be smaller than the height of the first burr (1110) formed around the first shear surface (150a). Additionally, the second length can be defined as the average length of the second short-circuit lines (1200) formed in the portion adjacent to the third shear surface (150c).

[0125] That is, if the first additional hole (120a) included in the hot stamping part (1000) is formed through cold piercing (or cold press mold), a short-circuit line (e.g., a second short-circuit line (1200)) having a length of less than about 50 μm may exist in a portion adjacent to the third shear surface (150c) where the first additional hole (120a) is defined. Accordingly, if a short-circuit line (e.g., a second short-circuit line (1200)) having a length of less than about 50 μm exists in a portion adjacent to the third shear surface (150c) where the first additional hole (120a) is defined, it can be understood that the first additional hole (120a) is formed through cold piercing (or cold press mold). In other words, when the short-circuit lines (e.g., the second short-circuit lines (1200)) formed adjacent to the third shear surface (150c) where the first additional hole (120a) is defined have an average length of less than about 50 μm, the first additional hole (120a) may be formed by cold piercing (or cold press mold).

[0126] In addition, the hot stamping part (1000) may include a fifth shear surface (150e) having a first edge (130a) defined, and when observed with an optical microscope after cross-sectional etching, second short-circuit lines (1200) having a second length smaller than the first length may be formed in a portion adjacent to the fifth shear surface (150e). At this time, the second length may be less than about 50 ㎛. In addition, a second burr (1210) may be formed around the fifth shear surface (150e). However, the height of the second burr (1210) formed around the fifth shear surface (150e) may be smaller than the height of the first burr (1110) formed around the first shear surface (150a). In addition, the second length may be defined as an average length of the second short-circuit lines (1200) formed in a portion adjacent to the first edge (130a).

[0127] That is, if the first edge (130a) included in the hot stamping part (1000) is formed through cold trimming (or cold press mold), a short-circuit line (e.g., a second short-circuit line (1200)) having a length of less than about 50 μm may exist in a portion adjacent to the fifth shear surface (150e) where the first edge (130a) is defined. Accordingly, if a short-circuit line (e.g., a second short-circuit line (1200)) having a length of less than about 50 μm exists in a portion adjacent to the fifth shear surface (150e) where the first edge (130a) is defined, it can be understood that the first edge (130a) is formed through cold trimming (or cold press mold). In other words, when the short-circuit lines (e.g., the second short-circuit lines (1200)) formed in the portion adjacent to the fifth shear surface (150e) where the first edge (130a) is defined have an average length of less than about 50 μm, the first edge (130a) may be formed by cold trimming (or cold press mold).

[0128] Referring to FIGS. 10, 13, and 14, the hot stamping part (1000) may include a third shear surface (150c) in which a first additional hole (120a) is defined, and a short-circuit line may not be formed in a portion adjacent to the third shear surface (150c). However, the third shear surface (150c) may be provided with a diagonal pattern (1300) along the shear surface. In addition, a microstructure different from the base material may exist along the third shear surface (150c) with a thickness (or width) of about 20 μm or less in a direction perpendicular to the third shear surface (150c). In addition, a draw (1310) may exist on the lower side of the hot stamping part (1000).

[0129] That is, if the first additional hole (120a) included in the hot stamping part (1000) is formed through laser piercing, a diagonal pattern (1300) rather than a solid line may exist in a portion adjacent to the third shear surface (150c) where the first additional hole (120a) is defined. Accordingly, if a diagonal pattern (1300) exists in a portion adjacent to the third shear surface (150c) where the first additional hole (120a) is defined, it can be understood that the first additional hole (120a) was formed through laser piercing. In other words, if a diagonal pattern rather than a solid line exists in a portion adjacent to the third shear surface (150c) where the first additional hole (120a) is defined, the first additional hole (120a) may be formed through laser piercing.

[0130] In addition, the hot stamping part (1000) may include a fifth shear surface (150e) having a first edge (130a) defined therein, and a short-circuit line may not be formed in a portion adjacent to the fifth shear surface (150e). However, the fifth shear surface (150e) may be provided with a diagonal pattern (1300) along the shear surface. In addition, a microstructure different from the base material may have a thickness (or width) of about 20 μm or less along the shear surface in a direction perpendicular to the shear surface. In addition, a draw (1310) may be present on the lower side of the hot stamping part (1000).

[0131] That is, if the first edge (130a) included in the hot stamping part (1000) is formed through laser trimming, a diagonal pattern (1300) rather than a solid line may exist in a portion adjacent to the fifth shear surface (150e) where the first edge (130a) is defined. Accordingly, if a diagonal pattern (1300) exists in a portion adjacent to the fifth shear surface (150e) where the first edge (130a) is defined, it can be understood that the first edge (130a) is formed through laser trimming. In other words, if a diagonal pattern rather than a solid line exists in a portion adjacent to the fifth shear surface (150e) where the first edge (130a) is defined, the first edge (130a) may be formed through laser trimming.

[0132] The first additional hole (120a) of the hot stamping part (1000) may be formed by a cold piercing (or cold press mold) or laser piercing process. Additionally, the first edge (130a) of the hot stamping part (1000) may be formed by a cold trimming (or cold press mold) or laser trimming process.

[0133] Referring again to FIGS. 10 and 11, the hot stamping part (1000) may include a second shear surface (150b) having a second hole (110b) defined therein, and first short lines (1100) having a third length greater than the second length may be formed adjacent to the second shear surface (150b). At this time, the third length may be about 50 μm or more. In addition, a first burr (1110) may be formed around the second shear surface (150b). At this time, the third length may be defined as an average length of the first short lines (1100) formed adjacent to the second shear surface (150b).

[0134] In one embodiment, the second additional hole (120b) may be provided in a manner identical to or similar to the first additional hole (120a) or the first edge (130a). In addition, the second edge (130b) may be provided in a manner identical to or similar to the first additional hole (120a) or the first edge (130a). However, the present invention is not limited thereto.

[0135] In one embodiment, the first edge (130a) and / or the second edge (130b) of the hot stamping part (1000) may be the edge of the coil raw material. For example, when the first edge (130a) and / or the second edge (130b) of the hot stamping part (1000) is observed under an optical microscope after cross-sectional etching, no portion damaged by a short circuit or external force is found, and the first edge (130a) and / or the second edge (130b) may form an arc shape (e.g., a curved shape). In this case, a plating layer (1420) may be formed along the cross-sectional edge.

[0136] In one embodiment, a hot stamping part (1000) may include a hole (110), an additional hole (120), and an edge (130), and when observed under an optical microscope after cross-section etching, a portion adjacent to a shear plane (e.g., a first shear plane (150a) and a second shear plane (150b)) where the hole (110) is defined may have a plurality of short lines (e.g., a first short line (1100)) having a length of about 50 μm or more, and a first burr (1110) may be formed. At this time, the length of the short lines may be an average length of the short lines.

[0137] In the portion adjacent to the shear plane (e.g., the third shear plane (150c), the fourth shear plane (150d), the fifth shear plane (150e), and the sixth shear plane (150f)) where the additional hole (120) and / or the edge (130) are defined, short-circuit lines (e.g., the second short-circuit lines (1200)) having a length of less than about 50 μm may be present, and a second burr (1210) may be formed. At this time, the length of the short-circuit lines may be the average length of the short-circuit lines.

[0138] Alternatively, a portion adjacent to a shear plane (e.g., a third shear plane (150c), a fourth shear plane (150d), a fifth shear plane (150e), and a sixth shear plane (150f)) where additional holes (120) and / or edges (130) are defined may have no short-circuit lines and a diagonal pattern (1300) along the shear plane, and a microstructure different from the parent material may exist along the shear plane with a thickness (or width) of about 20 μm or less in a direction perpendicular to the shear plane, and a draw (1310) may be formed adjacent to the shear plane.

[0139] After the heated blank is formed and cooled, a piercing process for cutting a hole within the cooled blank and a trimming process for cutting off unnecessary outer portions may be performed. The piercing process may utilize a laser or a press die (e.g., a cold press die). When the laser is used to perform the piercing process, the processing load is minimal and the cross-sectional quality is good, but the processing time is long and the processing cost may increase accordingly. On the other hand, when the press die is used to perform the piercing process, the processing time is fast and the processing cost is low, but the processing load is high and the cross-sectional quality may be inferior.

[0140] In one embodiment, hot piercing can be performed simultaneously during the process of forming and cooling the heated blank. That is, the processes of hot press forming the heated blank (100), hot piercing the heated blank (100), and cooling the heated blank (100) can be performed simultaneously (or together) within the press die (400). Therefore, by forming holes in the blank (100) in advance at a high temperature, the number of holes formed in the cooled blank (100) can be reduced. That is, by forming holes in the blank (100) in advance at a high temperature, the process of forming holes in the cooled blank (100) can be simplified, thereby reducing the processing time and thus the processing cost, and providing a hot stamping part (1000) with a small processing load and good cross-sectional quality.

[0141] In addition, when performing the piercing process and trimming process, arbitrary shapes may be formed in the outer area of ​​the blank (100) that is not included in the final product during hot pressing, and then the blank (100) may be seated in a tool using the arbitrary shapes and the piercing process and trimming process may be performed. However, due to this, the size of the blank (100) used in the method for manufacturing a hot stamping part may become larger than necessary compared to the final product, which may reduce the material yield and increase the amount of scrap waste, which may cause economic and environmental problems.

[0142] In one embodiment, at least two holes (110a, 110b) can be formed in the blank (100) through hot piercing simultaneously (or together) during the process of hot forming the blank (100), and by performing the cold piercing process and the cold trimming process using the at least two formed holes (110a, 110b) as guide patterns (or reference points), the size of the blank (100) used in the method for manufacturing a hot stamping part can be prevented from becoming unnecessarily large compared to the final product, so that the material yield can be increased, the amount of scrap can be reduced, and thus the economy can be improved and the environment can be protected.

[0143] In one embodiment, a short-flow line (e.g., a first short-flow line (1100)) having a length of about 50 μm or more may be present in a portion adjacent to a first shear surface (150a) where a first hole (110a) is defined, and a short-flow line (e.g., a second short-flow line (1200)) having a length of less than about 50 μm may be present in a portion adjacent to a third shear surface (150c) where a first additional hole (120a) is defined. That is, the length of the short-flow line formed in a portion adjacent to the first shear surface (150a) where a first hole (110a) is defined may be greater than the length of the short-flow line formed in a portion adjacent to the third shear surface (150c) where a first additional hole (120a) is defined. In this case, the length may be an average length of the short-flow lines.

[0144] When a fracture line is developed, the toughness of that area can be improved. That is, if the length of the fracture line formed in the area adjacent to the shear plane is long, the toughness of the shear plane and the area around the shear plane can be high.

[0145] The holes (110a, 110b) can be used as reference holes (tooling holes). For example, the holes (110a, 110b) formed in the hot stamping part (1000) can be used as guide patterns (or reference points) to secure the hot stamping part (1000) to the tool, and then subsequent processes such as additional hole formation, outer portion cutting, and dimensional quality inspection can be performed. In addition, the holes (110a, 110b) formed in the hot stamping part (1000) can be used as guide patterns (or reference points) for the sub-assembly process and the self-assembly process. The holes (110a, 110b) formed in the hot stamping part (1000) are repeatedly seated in the tool, and if the toughness of the holes (110a, 110b) formed in the hot stamping part (1000) and the area around the holes (110a, 110b) is low, the hot stamping part (1000) may be damaged or the tool may be worn or damaged. According to one embodiment of the present invention, a flow line (e.g., a first flow line (1100)) having a length of about 50 μm or more may exist around the holes (110a, 110b) formed in the hot stamping part (1000), and this may mean that the toughness around the holes (110a, 110b) formed in the hot stamping part (1000) is high. Accordingly, even if the holes (110a, 110b) formed in the hot stamping part (1000) are repeatedly placed in the tool, it is possible to prevent the hot stamping part (1000) from being damaged or the tool from being worn or damaged.

[0146] FIGS. 16 and 17 are drawings illustrating differences according to the lengths of the short-circuit lines formed around the shear surface. Specifically, FIG. 16 corresponds to a case where the length of the short-circuit lines formed around the shear surface (e.g., the average length of the short-circuit lines) is about 50 μm or more, and FIG. 17 corresponds to a case where the length of the short-circuit lines formed around the shear surface (e.g., the average length of the short-circuit lines) is less than about 50 μm. That is, FIG. 16 corresponds to a case where the short-circuit lines formed in a portion adjacent to the shear surface where a hole (110) is defined (e.g., the first short-circuit line (1100)) have an average length of about 50 μm or more, and FIG. 17 corresponds to a case where the short-circuit lines formed in a portion adjacent to the shear surface where an additional hole (120) and / or an edge (130) are defined (e.g., the second short-circuit line (1200)) have an average length of less than about 50 μm.

[0147] Referring to Fig. 16, when an arbitrary quadrilateral is drawn along the starting and ending points of the short-circuit lines formed on the periphery of the shear surface, if the length of the straight line AB of the edge of the shear surface is L1 and the length of the straight line CD inside the hot stamping part is L2, L2 / L1 may be about 1.2 to about 5.0. In addition, when the acute angle among the angles between the two diagonals AC and BD is θ1, θ1 may be about 10 degrees to about 45 degrees.

[0148] On the other hand, referring to Fig. 17, when an arbitrary quadrilateral is drawn along the start and end points of the short-circuit lines formed on the periphery of the shear surface, if the length of the straight line A'B' of the edge of the shear surface is L3 and the length of the straight line C'D' inside the hot stamping part is L4, L4 / L3 may have a value close to about 1. For example, L4 / L3 may be about 1.2 or less. In addition, when the acute angle among the angles between the two diagonals A'C' and B'D' is θ2, θ2 may be about 0 degrees to about 10 degrees.

[0149] That is, when the length of the short-circuit line formed around the shear surface is long, the straight line at the edge of the shear surface is shorter than the straight line inside the hot stamping part, and when the length of the short-circuit line formed around the shear surface is short, the straight line at the edge of the shear surface can be provided with a similar length to the straight line inside the hot stamping part. In addition, when the length of the short-circuit line formed around the shear surface is long, the acute angle among the angles between the two diagonals of any quadrilateral can be provided larger than when the length of the short-circuit line formed around the shear surface is short.

[0150] Accordingly, when the short-circuit lines (e.g., the first short-circuit lines (1100)) formed in a portion adjacent to the shear surface where the holes (110) are defined have an average length of about 50 ㎛ or more, the straight line of the edge of the shear surface may be provided to be shorter than the straight line inside the hot stamping part, and the acute angle among the angles between the two diagonals may be provided to be about 10 degrees to about 45 degrees. In addition, when the short-circuit lines (e.g., the second short-circuit lines (1200)) formed in a portion adjacent to the shear surface where the additional holes (120) and / or the edge (130) are defined have an average length of less than about 50 ㎛, the straight line of the edge of the shear surface may be provided to have a similar length to the straight line inside the hot stamping part, and the acute angle among the angles between the two diagonals may be provided to be about 0 degrees to about 10 degrees.

[0151] FIGS. 18 and 19 are plan views showing the effect of applying a manufacturing method according to one embodiment of the present invention.

[0152] Referring to FIGS. 18 and 19, it can be confirmed that when hot piercing is not performed during hot forming (or hot pressing) of a coil raw material of the same area, five blanks (100) can be obtained, but when hot piercing is performed during hot forming (or hot pressing), six blanks (100) can be obtained. That is, when hot piercing is performed during hot forming (or hot pressing), the number of blanks (100) that can be obtained from a coil raw material of the same area can increase, and the amount of scrap can be reduced, compared to when hot piercing is not performed during hot forming (or hot pressing).

[0153] Accordingly, if hot piercing is not performed during hot forming (or hot pressing), the size of the blank (100) used in the method for manufacturing a hot stamping part may become larger than necessary compared to the final product, thereby reducing the material yield. If hot piercing is performed during hot forming (or hot pressing), the size of the blank (100) used in the method for manufacturing a hot stamping part may be prevented from becoming larger than necessary compared to the final product, thereby increasing the material yield.

[0154] While the present invention has been described with reference to the embodiments illustrated in the drawings, these are merely exemplary, and those skilled in the art will appreciate that various modifications and equivalent alternative embodiments are possible. Therefore, the true scope of technical protection of the present invention should be determined by the technical spirit of the appended claims.

Claims

1. In the manufacturing method of hot stamping parts, Preparatory step to prepare the blank; A heating step for heating the above blank; A transfer step of transferring the heated blank to a press mold; A forming and first piercing step of hot pressing the transferred blank to form it into the shape of a hot stamping part and forming at least two holes in the transferred blank; and A trimming step of cutting the outer portion of the molded blank using at least two holes; A method for manufacturing a hot stamping part, comprising:

2. In paragraph 1, A method for manufacturing a hot stamping part, wherein the above preparation step is a step of cutting the coil into the blank using a laser or a cold press mold.

3. In paragraph 1, A method for manufacturing a hot stamping part, wherein the blank includes an outer portion of a coil.

4. In paragraph 1, A method for manufacturing a hot stamping part, wherein in the above heating step, the blank is heated to a temperature of Ac3 to 1000°C.

5. In paragraph 1, A method for manufacturing a hot stamping part, wherein the temperature of the blank before the forming and first piercing steps is equal to or higher than the Ms temperature.

6. In paragraph 1, In the above forming and first piercing steps, A method for manufacturing a hot stamping part, wherein the above-described transferred blank is cooled within the press mold.

7. In paragraph 6, A method for manufacturing a hot stamping part, wherein the above-mentioned transferred blank is cooled for a time period of 3 seconds or more and 20 seconds or less.

8. In paragraph 1, The above trimming step is, A method for manufacturing a hot stamping part, comprising the step of cutting the outer portion of the formed blank using a laser or cold press mold.

9. In paragraph 1, A method for manufacturing a hot stamped part, further comprising a second piercing step in which an additional hole is formed in the formed blank using at least two of the holes.

10. In paragraph 1, After the above trimming step, A method for manufacturing a hot stamping part, further comprising a step of removing a burr formed on the blank.

11. As a hot stamping part, A first shear plane having a first hole defined therein; and A second shear surface formed on the edge of the hot stamping part; Including, A first short-circuit line having a first length is formed in a portion adjacent to the first shear surface, A hot stamping part, wherein a second short-line or first diagonal pattern having a second length smaller than the first length is formed on a portion adjacent to the second shear surface.

12. In paragraph 11, A hot stamping part, wherein the first length is 50 μm or more and the second length is less than 50 μm.

13. In paragraph 11, A hot stamping part further comprising a third shear surface defined by a second hole spaced apart from the first hole.

14. In paragraph 13, A hot stamping part, wherein a third short-line or second diagonal pattern having a third length smaller than the first length is formed on a portion adjacent to the third shear surface.

15. In paragraph 11, A hot stamping part further comprising a fourth shear surface defined by a third hole spaced apart from the first hole.

16. In paragraph 15, A hot stamping part, wherein a fourth short-circuit line having a fourth length greater than the second length is formed in a portion adjacent to the fourth shear surface.

17. In paragraph 11, A hot stamping part having a curved edge.

18. In paragraph 17, The above hot stamping part further includes a plating layer, A hot stamping part, wherein the plating layer is provided along the edge of the hot stamping part.