Polytetrafluoroethylene (PTFE) membranes with gradient pore structures and methods for preparing the same
Patent Information
- Application Number
- MYPI2025001417
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-12-19
- Filing Date
- 2023-12-19
- Publication Date
- 2024-06-19
AI Technical Summary
It is difficult for existing porous polytetrafluoroethylene membranes to maintain high filtration accuracy and mechanical strength while improving the filtration rate and dirt-holding capacity. Moreover, the preparation method of asymmetric membrane materials has problems such as difficulty in operation and uneven stress between layers.
A polytetrafluoroethylene membrane with a gradient pore structure is used. Through the mixing of isoparaffin and PTFE dispersion resin, lamination of different thicknesses and thermal stretching process, the first porous outer surface is formed with island-like microstructure and the second porous A membrane material with an H-shaped ladder-like microstructure on its outer surface.
The combination of low flow resistance, high flow rate and high filtration precision is achieved, which improves filtration efficiency and pollutant capture capabilities, while avoiding the problems of weakened membrane thickness and operational difficulty.
Smart Images

Figure PI2025001417_DRAWING_001 
Figure PI2025001417_DRAWING_002 
Figure PI2025001417_DRAWING_003
Abstract
Description
A polytetrafluoroethylene membrane with a gradient pore structure and a preparation method thereof Technical Field
[0001] The present invention relates to the technical field of polymer filtration membrane materials, in particular to a polytetrafluoroethylene membrane with a gradient pore structure and a preparation method thereof. Background Art
[0002] Expanded polytetrafluoroethylene (PTFE) membranes with porous structures have been widely used in liquid and gas filtration. These membranes are highly chemically inert and thermally stable at extreme temperatures, allowing them to be used in very harsh working conditions.
[0003] As described in U.S. Patent No. 3,953,566A, PTFE resin and lubricant are mixed to form a raw material. The PTFE mixed raw material is then formed into a paste and extruded. After removing the lubricant from the extruded material, the PTFE product is stretched to produce a porous PTFE product. Expanded PTFE material is characterized by a porous microstructure with nodes connected by fibrils. The pore size is relatively uniform within the membrane and on both surfaces, resulting in a symmetrical pore structure.
[0004] Filter materials with symmetrical pore structures can achieve high filtration accuracy. The smaller the pore size, the more precise the filtration or separation. However, smaller pore sizes generally reduce the permeability of liquids or gases through the membrane, failing to provide high dirt holding capacity. Conversely, increasing the pore size of the filter material to increase the flow capacity of the membrane will result in a decrease in the number of particles captured by the membrane, and the filtration efficiency will decrease.
[0005] In order to increase the processing volume per unit area and per unit time and improve the filtration rate, it is necessary to significantly increase the number of pores or minimize the thickness of the membrane material while ensuring a certain pore size. Under specific production conditions, it is very difficult to significantly increase the number of pores per unit area. In addition, although the filtration rate can be increased by reducing the thickness of the filter material, it will lead to a decrease in the mechanical strength of the film. The focus of developing filter materials is to find an ideal combination of high permeability and high filtration accuracy, while ensuring filtration efficiency, having low resistance, high flow rate and high dirt holding capacity. As a technology to overcome this shortcoming, asymmetric porous membranes have greater processing capacity under the same filtration or separation conditions.
[0006] Although the filtration properties of porous PTFE membranes are constantly improving, being able to provide PTFE filtration membranes with small particle size and low flow resistance at the same time remains one of the technical difficulties in this field.
[0007] Filter materials with asymmetric pore structures can ensure high filtration accuracy while having the advantages of small pressure difference and long service life. They are widely used in the field of filtration and separation. For example, Chinese patent CN107810047A discloses an asymmetric polytetrafluoroethylene composite with a macro-textured surface, and the two membrane surfaces of the polytetrafluoroethylene composite have different bubble point pressure values. In this method, the second PTFE membrane needs to be wetted, that is, when the lubricant is not removed, to expand the rolled strip in the longitudinal or transverse direction. This operation is difficult to implement and can easily cause irreversible damage to the PTFE strip. Although the membrane prepared by this method has a unique macro-textured surface, there are one or more strands on the membrane surface that bulge from the membrane surface, which may cause uneven force between layers when compounded with other supporting layers.
[0008] For example, U.S. Patent No. 4,248,924A provides a porous film material composed of polytetrafluoroethylene with an asymmetric structure, produced by stretching the film using a pair of rotating rollers with a temperature difference of 50°C or higher. The combination of a temperature gradient across the thickness created by the temperature difference between the front and back surfaces of the membrane and a compressive force across the thickness creates an asymmetric structure in the resulting porous film material, characterized by a different fiber structure on the front surface than on the back surface. However, due to the thinness of the stretched film, this method often produces a limited temperature gradient across the thickness, making it difficult to effectively control the asymmetric structure of the membrane material.
[0009] In view of this, it is necessary to improve the asymmetric membrane materials and preparation methods thereof in the prior art to solve the above problems.
[0010] Summary of the Invention
[0011] The purpose of the present invention is to disclose a polytetrafluoroethylene membrane material with a gradient pore structure, which combines the characteristics of low flow resistance and small pore size, so that it has excellent filtration rate and reliable retention accuracy in liquid and gas filtration.
[0012] To achieve the above objectives, the present invention provides a polytetrafluoroethylene membrane with a gradient pore structure, wherein the cross-section of the polytetrafluoroethylene membrane has a gradient pore structure, and the first porous outer surface and the second porous outer surface of the polytetrafluoroethylene membrane have fibers and nodes with different microstructures; the first porous outer surface has an island-like microstructure constructed by a plurality of interconnected smaller nodes, and the second porous outer surface has an H-shaped ladder-like microstructure constructed by a plurality of interconnected larger nodes.
[0013] In some embodiments, the smaller nodes are circular structures with an average diameter of 0.30 to 1.50 μm.
[0014] In some embodiments, the smaller nodes are formed by connecting a number of thick and short microfibers, the average length of the thick and short microfibers is in the range of 0.2 to 2.5 μm, the average diameter is in the range of 0.05 to 0.2 μm, and the aspect ratio is 2 to 20.
[0015] In some embodiments, the larger nodes are oblong structures with an average length of 0.5 to 10 μm and an average width of 0.5 to 2 μm.
[0016] In some embodiments, the larger node is formed by connecting a plurality of elongated microfibers, wherein the elongated microfibers have an average length ranging from 1 to 10 μm, an average diameter ranging from 5 to 200 nm, and an aspect ratio of 10 to 200.
[0017] Another object of the present invention is to provide a method for preparing a PTFE porous membrane with a gradient pore structure, comprising the following steps:
[0018] (1) First, isoparaffin and PTFE dispersion resin are uniformly mixed to obtain a PTFE resin mixture, and then the PTFE resin mixture is pressed into a cylindrical preform;
[0019] (2) using an extruder to extrude the cylindrical preform into three continuous strips of equal width with different thicknesses and rectangular cross-sections through T-shaped extrusion dies of different specifications, namely, a first sheet, a second sheet, and a third sheet;
[0020] (3) The first sheet, the second sheet, and the third sheet are stacked in the same width direction in increasing or decreasing thickness, and are fed into a pair of metal rollers along the length direction and rolled in the thickness direction to a range of 0.05 to 1 mm to form a laminate;
[0021] (4) drying the laminate at 200-250° C., and then expanding the laminate in the direction of the speed at 250-350° C. at a stretching rate of 20% / s to 3000% / s and an expansion ratio of 50% to 900% to form a uniaxially stretched product;
[0022] (5) Expanding the uniaxially stretched product in a direction perpendicular to the speed at a temperature of 200 to 400° C., at a stretching rate of 5% / s to 500% / s, and at a ratio of 300% to 3000%, to finally form a PTFE membrane material with a gradient pore structure.
[0023] In some embodiments, in step (1), isoparaffin and PTFE dispersed resin are uniformly mixed in a weight ratio of 15 to 30% to obtain a PTFE resin mixture, and the mixture is dried at a temperature of not less than 20° C. for more than 12 hours, and the PTFE resin mixture is pressed into a cylindrical preform.
[0024] In some embodiments, in step (2), the cylindrical preform is extruded into three continuous strips of equal width with different thicknesses having rectangular cross-sections through T-shaped extrusion dies of different specifications at a compression ratio of 20 to 500, namely the first sheet, the second sheet and the third sheet, wherein: the thickness of the second sheet is at least 1.2 times the thickness of the first sheet, the thickness of the third sheet is at least 1.2 times the thickness of the second sheet, and the compression ratio of the first sheet is at least 2.5 times that of the second sheet and 3 times that of the third sheet.
[0025] In some embodiments, in step (4), the laminate is expanded along the speed direction at a stretching rate of 50% / s to 2000% / s and an expansion ratio of 80% to 800% to form a uniaxially stretched product.
[0026] In some embodiments, in step (5), the PTFE membrane material having a gradient pore structure is finally formed by expanding in a direction perpendicular to the speed at a stretching rate of 20% / s to 300% / s and a ratio of 500% to 2500%.
[0027] Compared to existing technologies, the present invention offers the following advantages: the polytetrafluoroethylene membrane material with a gradient pore structure produced by this method exhibits low resistance and high flow rate without compromising thickness or filtration accuracy. This improved filtration efficiency enhances pollutant capture. For a given transmembrane pressure drop, the high permeability or high flow capacity of the membrane reduces resistance losses, shortens filtration time, and thus reduces energy costs. Furthermore, these advantages enable the creation of a system with a smaller installation space and greater cost savings. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] FIG1 is a cross-sectional view of a polytetrafluoroethylene film laminate according to the present invention;
[0029] FIG2 is a 2000x scanning electron micrograph of the first porous outer surface of the polytetrafluoroethylene membrane shown in Example 1 of the present invention;
[0030] FIG3 is a 2000x scanning electron micrograph of the second porous outer surface of the polytetrafluoroethylene membrane shown in Example 1 of the present invention;
[0031] FIG4 is a 2000x scanning electron micrograph of the first porous outer surface of the polytetrafluoroethylene membrane shown in Example 2 of the present invention;
[0032] FIG5 is a 2000x scanning electron micrograph of the second porous outer surface of the polytetrafluoroethylene membrane shown in Example 2 of the present invention;
[0033] FIG6 is a scanning electron micrograph at 2000 times magnification of the first porous outer surface of the polytetrafluoroethylene membrane shown in Example 3 of the present invention;
[0034] FIG7 is a 2000x scanning electron micrograph of the second porous outer surface of the polytetrafluoroethylene membrane shown in Example 3 of the present invention;
[0035] FIG8 is a 2000x scanning electron micrograph of the first porous outer surface of the polytetrafluoroethylene membrane shown in Example 4 of the present invention;
[0036] FIG9 is a 2000x scanning electron micrograph of the second porous outer surface of the polytetrafluoroethylene membrane shown in Example 4 of the present invention;
[0037] FIG10 is a 2000x scanning electron micrograph of the first porous outer surface of the polytetrafluoroethylene membrane shown in Example 5 of the present invention;
[0038] FIG11 is a scanning electron micrograph at 2000 times magnification of the second porous outer surface of the polytetrafluoroethylene membrane shown in Example 5 of the present invention;
[0039] FIG12 is a 2000x scanning electron micrograph of the first porous outer surface of the polytetrafluoroethylene membrane shown in Example 6 of the present invention;
[0040] FIG13 is a scanning electron micrograph at 2000 times magnification of the second porous outer surface of the polytetrafluoroethylene membrane shown in Example 6 of the present invention. DETAILED DESCRIPTION
[0041] The present invention is described in detail below with reference to the various embodiments shown in the accompanying drawings, but it should be noted that these embodiments are not limitations of the present invention, and any equivalent transformations or substitutions in functions, methods, or structures made by ordinary technicians in this field based on these embodiments are all within the scope of protection of the present invention.
[0042] The method for preparing a polytetrafluoroethylene membrane having a gradient pore structure of the present invention comprises the following specific steps:
[0043] (1) First, an isoparaffin lubricant and a polytetrafluoroethylene (PTFE) dispersion resin are uniformly mixed in a weight ratio of 15 to 30% to obtain a PTFE resin mixture, which is then dried at a temperature of not less than 20° C. for more than 12 hours and pressed into a cylindrical preform.
[0044] (2) Using an extruder, at a compression ratio of 20 to 500, preferably 30 to 250, the cylindrical preform is extruded through T-shaped extrusion dies of different specifications into three continuous strips of equal width with rectangular cross-sections of different thicknesses, namely the first sheet, the second sheet, and the third sheet.
[0045] Among them: the thickness of the second sheet is at least 1.2 times the thickness of the first sheet, preferably 1.2 to 5 times; the thickness of the third sheet is at least 1.2 times the thickness of the second sheet, preferably 1.2 to 5 times; the compression ratio of the first sheet is at least 2.5 times that of the second sheet and 3 times that of the third sheet.
[0046] (3) The first sheet, the second sheet, and the third sheet are stacked in the same width direction in increasing or decreasing thickness, and are fed into a pair of metal rollers along the length direction and rolled in the thickness direction to a range of 0.05 to 1 mm, preferably to a range of 0.15 to 0.6 mm, to form a laminate, as shown in FIG1 .
[0047] (4) The laminate is dried at 200-250°C, and then expanded along the speed direction at 250-350°C at a stretching rate of 20% / s to 3000% / s, preferably at a stretching rate of 50% / s to 2000% / s, and an expansion ratio of 50% to 900%, preferably at an expansion ratio of 80% to 800%, to form a uniaxially stretched product.
[0048] (5) The uniaxially stretched product is stretched at a temperature of 200 to 400° C. at a stretching rate of 5% / s to 500% / s, preferably at a stretching rate of 20% / s to 300% / s, and at a ratio of 300% to 3000%, preferably at a ratio of 500% to 2500%, and is expanded in a direction perpendicular to the speed to ultimately form a polytetrafluoroethylene (PTFE) membrane material having a gradient pore structure.
[0049] The cross section of the membrane material has a gradient pore structure. The polytetrafluoroethylene (PTFE) membrane material has two outer surfaces, a first porous outer surface and a second porous outer surface, which respectively have fibers and nodes with different microstructures.
[0050] The first porous outer surface has an island-like microstructure constructed from a plurality of interconnected smaller nodes. The smaller nodes are circular in structure and have an average diameter of 0.30 to 1.50 μm. The smaller nodes are formed by connecting a plurality of short and thick microfibers, each having an average length ranging from 0.2 to 2.5 μm, an average diameter ranging from 0.05 to 0.2 μm, and an aspect ratio of 2 to 20.
[0051] The second porous outer surface has an H-shaped ladder-like microstructure constructed from a plurality of interconnected larger nodes. The larger nodes are oblong structures with an average length of 0.5-10 μm and an average width of 0.5-2 μm. The larger nodes are formed by connecting a plurality of slender microfibers, each with an average length ranging from 1-10 μm, an average diameter ranging from 5-200 nm, and an aspect ratio of 10-200.
[0052] Testing method for polytetrafluoroethylene membrane material
[0053] 1. Thickness measurement
[0054] The film thickness was measured by placing the film or sheet between the probe and anvil of a Mitutoyo Model 7327 Thickness Micrometer. The average of three measurements was used.
[0055] 2. Bubble point measurement
[0056] Bubble point and mean flow pore size were measured using a capillary flow porometer (Porolux 500, Porometer NV, Belgium) according to the general guidelines of ASTM F316-03. The sample membrane was placed in the sample chamber and wetted with a test fluid with a surface tension of 16 dynes / cm. The values expressed for bubble point and mean flow pore size are the average of two measurements.
[0057] 3. Scanning electron microscope images
[0058] SEM images were generated using a cold field emission scanning electron microscope (Hitachi Regulus 8100).
[0059] 4. Node and fiber size measurement
[0060] SolidWorks 2014 software (Dassault Systemes, France) was used to perform proportional measurements on the SEM images, and the measurement results were converted into the actual sizes of nodes and fibers using the scale of the SEM images.
[0061] The present invention will be described in detail with reference to the following examples, but the present invention is not limited by these examples.
[0062] Example 1
[0063] Daikin F-106 polytetrafluoroethylene (PTFE) dispersion resin was uniformly mixed with 18.3% by weight of isoparaffin (ExxonMobil ISOPAR M) and placed in a constant temperature oven at 25°C for 18 hours. The PTFE resin mixture was pressed into a cylindrical preform, which was then extruded through a T-die at a compression ratio of 195 to obtain a continuous first sheet with a rectangular cross-section and a thickness of 0.4 mm.
[0064] Asahi Glass CD-126E polytetrafluoroethylene (PTFE) dispersion resin was uniformly mixed with 25.6% by weight of isoparaffin (ExxonMobil ISOPAR K) and placed in a constant temperature oven at 25°C for 18 hours. The PTFE resin mixture was then pressed into a cylindrical preform. The preforms were then extruded through T-dies of different specifications at a compression ratio of 49 to produce a second continuous sheet with a rectangular cross-section and a thickness of 0.9 mm. A third continuous sheet with a rectangular cross-section and a thickness of 1.2 mm was extruded at a compression ratio of 37.
[0065] Three sheets of different specifications are stacked in increasing or decreasing thickness along the same width direction. They are then fed into a pair of metal rollers along the length direction and rolled to 0.3mm in the thickness direction to form a laminate. The dried laminate, after removing the additive oil, is longitudinally stretched by a longitudinal stretching mechanism at a stretching roller temperature of 300°C, a stretching rate of 117% / s, and a stretch expansion ratio of 230%. The uniaxially stretched product (base tape) is then transversely stretched by a transverse expander at a stretching temperature of 250°C, a stretching rate of 22% / s, and a stretch expansion ratio of 2000%. Finally, it is heat-set to form a film.
[0066] As described above, the obtained polytetrafluoroethylene (PTFE) microporous membrane has a first porous outer surface and a second porous outer surface with different microstructures. As shown in Figures 2-3, Figure 2 is a scanning electron micrograph (SEM) of the first porous outer surface of the PTFE membrane, taken at a magnification of 2000 times, showing an island-like microstructure constructed by several interconnected smaller nodes; Figure 3 is a scanning electron micrograph (SEM) of the second porous outer surface of the PTFE membrane, taken at a magnification of 2000 times, showing an H-shaped ladder-like microstructure constructed by several interconnected larger nodes.
[0067] Solidworks 2014 software was used to measure the nodes in Figure 2 in proportion, and the node sizes are shown in Table 1 below.
[0068] Table 1 Node size of the first porous outer surface
[0069] The fibers in Figure 2 were measured in proportion using Solidworks 2014 software, and the fiber sizes are shown in Table 2 below.
[0070] Table 2 Fiber size of the first porous outer surface
[0071] Solidworks 2014 software was used to measure the nodes in Figure 3 in proportion, and the node sizes are shown in Table 3 below.
[0072] Table 3 Node size of the second porous outer surface
[0073] Solidworks 2014 software was used to measure the fibers in Figure 3 in proportion, and the fiber dimensions are shown in Table 4 below.
[0074] Table 4 Fiber size of the second porous outer surface
[0075] The bubble point was determined using two test conditions run using a capillary flow porometer. In the first test, the first porous outer surface of the PTFE membrane faced the metal mesh; in the second test, the second porous outer surface of the PTFE membrane faced the metal mesh. The bubble points were measured to be 1.97 bar and 1.62 bar, respectively.
[0076] Example 2
[0077] Daikin F-106 polytetrafluoroethylene (PTFE) dispersion resin was uniformly mixed with 19.5% by weight of isoparaffin (ExxonMobil ISOPAR M) and placed in a constant temperature oven at 25°C for 20 hours. The PTFE resin mixture was pressed into a cylindrical preform, which was then extruded through a T-die at a compression ratio of 195 to obtain a continuous first sheet with a rectangular cross-section and a thickness of 0.4 mm.
[0078] Asahi Glass CD-126E polytetrafluoroethylene (PTFE) dispersion resin was uniformly mixed with 23.5% by weight of isoparaffin (ExxonMobil ISOPAR K) and placed in a constant temperature oven at 25°C for 20 hours. The PTFE resin mixture was then pressed into a cylindrical preform. The preforms were then extruded through T-dies of different specifications at a compression ratio of 56 to produce a second continuous sheet with a rectangular cross-section and a thickness of 0.8 mm. A third continuous sheet with a rectangular cross-section and a thickness of 1.0 mm was extruded at a compression ratio of 45.
[0079] Three sheets of different specifications are stacked in the same width direction in increasing or decreasing thickness. They are then fed into a pair of metal rollers along the length direction and rolled to 0.28mm in the thickness direction to form a laminate. The dried laminate, after removing the additive oil, is longitudinally stretched by a longitudinal stretching mechanism at a stretching roller temperature of 300°C, a stretching rate of 150% / s, and a stretch expansion ratio of 250%. The uniaxially stretched product (base tape) is then transversely stretched by a transverse expander at a stretching temperature of 250°C, a stretching rate of 22% / s, and a stretch expansion ratio of 2000%. Finally, it is heat-set to form a film.
[0080] As described above, the obtained polytetrafluoroethylene membrane has a first porous outer surface and a second porous outer surface with different microstructures, as shown in Figures 4-5. Figure 4 is a scanning electron micrograph (SEM) of the first porous outer surface of the polytetrafluoroethylene (PTFE) membrane taken at a magnification of 2000 times, showing an island-like microstructure constructed by several smaller nodes connected to each other; Figure 5 is a scanning electron micrograph (SEM) of the second porous outer surface of the polytetrafluoroethylene (PTFE) membrane taken at a magnification of 2000 times, showing an H-shaped ladder-like microstructure constructed by several larger nodes connected to each other.
[0081] Solidworks 2014 software was used to measure the nodes in Figure 4 in proportion, and the node sizes are shown in Table 5 below.
[0082] Table 5 Node size of the first porous outer surface
[0083] The fibers in Figure 4 were measured in proportion using Solidworks 2014 software, and the fiber sizes are shown in Table 6 below.
[0084] Table 6 Fiber size of the first porous outer surface
[0085] Solidworks 2014 software was used to measure the nodes in Figure 5 in proportion, and the node sizes are shown in Table 7 below.
[0086] Table 7 Node size of the second porous outer surface
[0087] The fibers in Figure 5 were measured in proportion using Solidworks 2014 software, and the fiber sizes are shown in Table 8 below.
[0088] Table 8 Fiber size of the second porous outer surface
[0089] The bubble point was determined using a capillary flow porometer running two test conditions. In the first test, the first porous outer surface of the PTFE membrane faced the metal mesh; in the second test, the second porous outer surface of the PTFE membrane faced the metal mesh. The bubble points were measured to be 1.78 bar and 1.53 bar, respectively.
[0090] Example 3
[0091] Daikin F-106 polytetrafluoroethylene (PTFE) dispersion resin was uniformly mixed with 21.3% by weight of isoparaffin (ExxonMobil ISOPAR M) and placed in a constant temperature oven at 25°C for 22 hours. The PTFE resin mixture was pressed into a cylindrical preform, which was then extruded through a T-die at a compression ratio of 195 to obtain a continuous first sheet with a rectangular cross-section and a thickness of 0.4 mm.
[0092] Asahi Glass CD-126E polytetrafluoroethylene (PTFE) dispersion resin was uniformly mixed with 25.5% by weight of isoparaffin (ExxonMobil ISOPAR K) and placed in a constant temperature oven at 25°C for 22 hours. The PTFE resin mixture was then pressed into a cylindrical preform. The preforms were then extruded through T-dies of different specifications at a compression ratio of 56 to produce a second continuous sheet with a rectangular cross-section and a thickness of 0.8 mm. A third continuous sheet with a rectangular cross-section and a thickness of 1.2 mm was extruded at a compression ratio of 37.
[0093] Three sheets of different specifications are stacked in the same width direction in increasing or decreasing thickness. They are then fed into a pair of metal rollers along the length direction and rolled to 0.32mm in the thickness direction to form a laminate. The dried laminate, after removing the additive oil, is longitudinally stretched by a longitudinal stretching mechanism at a stretching roller temperature of 300°C, a stretching rate of 66.7% / s, and a stretch expansion ratio of 200%. The uniaxially stretched product (base tape) is then transversely stretched by a transverse expander at a stretching temperature of 250°C, a stretching rate of 22% / s, and a stretch expansion ratio of 2000%. Finally, the laminate is heat-set to form a film.
[0094] As described above, the obtained polytetrafluoroethylene (PTFE) membrane has a first porous outer surface and a second porous outer surface with different microstructures, as shown in Figures 6-7. Figure 6 is a scanning electron micrograph (SEM) of the first porous outer surface of the polytetrafluoroethylene (PTFE) membrane taken at a magnification of 2000 times, showing an island-like microstructure constructed by several interconnected smaller nodes; Figure 7 is a scanning electron micrograph (SEM) of the second porous outer surface of the polytetrafluoroethylene (PTFE) membrane taken at a magnification of 2000 times, showing an H-shaped ladder-like microstructure constructed by several interconnected larger nodes.
[0095] Solidworks 2014 software was used to measure the nodes in Figure 6 in proportion, and the node sizes are shown in Table 9 below.
[0096] Table 9 Node size of the first porous outer surface
[0097] Solidworks 2014 software was used to measure the fibers in Figure 6 in proportion, and the fiber dimensions are shown in Table 10 below.
[0098] Table 10 Fiber size of the first porous outer surface
[0099] Solidworks 2014 software was used to measure the nodes in Figure 7 in proportion, and the node sizes are shown in Table 11 below.
[0100] Table 11 Node size of the second porous outer surface
[0101] The fibers in Figure 7 were measured in proportion using Solidworks 2014 software, and the fiber dimensions are shown in Table 12 below.
[0102] Table 12 Fiber size of the second porous outer surface
[0103] The bubble point was determined using two test conditions run using a capillary flow porometer. In the first test, the first porous outer surface of the PTFE membrane faced the metal mesh; in the second test, the second porous outer surface of the PTFE membrane faced the metal mesh. The bubble points were measured to be 2.16 bar and 1.51 bar, respectively.
[0104] Example 4
[0105] A polytetrafluoroethylene (PTFE) dispersion resin was uniformly mixed with 19.5% by weight of an isoparaffin and then placed in a constant temperature oven at 25°C for 20 hours. The PTFE resin mixture was pressed into a cylindrical preform, which was then extruded through a T-die at a compression ratio of 190°C to obtain a continuous first sheet with a rectangular cross-section and a thickness of 0.5 mm.
[0106] A polytetrafluoroethylene (PTFE) dispersion resin was uniformly mixed with 23.5% by weight of isoparaffin and placed in a constant-temperature oven at 25°C for 20 hours. The PTFE resin mixture was then pressed into a cylindrical preform. The cylindrical preforms were then extruded through T-dies of different specifications at a compression ratio of 56 to produce a second continuous sheet with a rectangular cross-section and a thickness of 0.8 mm. A third continuous sheet with a rectangular cross-section and a thickness of 1.0 mm was extruded at a compression ratio of 45.
[0107] Three types of sheets are stacked in the same width direction, in increasing or decreasing thickness. They are then fed into a pair of metal rollers along the length direction and rolled to 0.28mm in the thickness direction to form a laminate. The dried laminate, after removing the additive oil, is longitudinally stretched by a longitudinal stretching mechanism at a stretching roller temperature of 300°C, a stretching rate of 150% / s, and a stretch expansion ratio of 250%. The uniaxially stretched product (base tape) is then transversely stretched by a transverse expander at a stretching temperature of 250°C, a stretching rate of 22% / s, and a stretch expansion ratio of 2000%. Finally, it is heat-set to form a film.
[0108] As described above, the obtained polytetrafluoroethylene (PTFE) membrane has a first porous outer surface and a second porous outer surface with different microstructures, as shown in Figures 8-9. Figure 8 is a scanning electron micrograph (SEM) of the first porous outer surface of the polytetrafluoroethylene (PTFE) membrane taken at a magnification of 2000 times, showing an island-like microstructure constructed by several interconnected smaller nodes; Figure 9 is a scanning electron micrograph (SEM) of the second porous outer surface of the polytetrafluoroethylene (PTFE) membrane taken at a magnification of 2000 times, showing an H-shaped ladder-like microstructure constructed by several interconnected larger nodes.
[0109] The bubble point was determined by running two test conditions using a capillary flow porometer. In the first test, the first porous outer surface of the PTFE membrane faced the metal mesh, and in the second test, the second porous outer surface of the PTFE membrane faced the metal mesh. The bubble points were measured to be 2.89 bar and 1.61 bar, respectively.
[0110] Example 5
[0111] Daikin F-106 polytetrafluoroethylene (PTFE) dispersion resin was uniformly mixed with 19.5% by weight of isoparaffin and placed in a constant-temperature oven at 25°C for 18 hours. The PTFE resin mixture was pressed into a cylindrical preform, which was then extruded through a T-die at a compression ratio of 190°C to obtain a continuous first sheet with a rectangular cross-section and a thickness of 0.5 mm.
[0112] Asahi Glass CD-126E polytetrafluoroethylene (PTFE) dispersion resin was uniformly mixed with 21.6% by weight of isoparaffin and placed in a constant-temperature oven at 25°C for 18 hours. The PTFE resin mixture was then pressed into a cylindrical preform. This cylindrical preform was then extruded through T-dies of different specifications at a compression ratio of 49 to produce a second continuous sheet with a rectangular cross-section and a thickness of 0.9 mm. A third continuous sheet with a rectangular cross-section and a thickness of 1.2 mm was extruded at a compression ratio of 37.
[0113] Three types of sheets are stacked in the same width direction, in increasing or decreasing thickness. They are then fed into a pair of metal rollers along the length direction and rolled to 0.32mm in the thickness direction to form a laminate. The dried laminate, after removing the additive oil, is longitudinally stretched by a longitudinal stretching mechanism at a stretching roller temperature of 300°C, a stretching rate of 66.7% / s, and a stretch expansion ratio of 200%. The uniaxially stretched product (base tape) is then transversely stretched by a transverse expander at a stretching temperature of 250°C, a stretching rate of 22% / s, and a stretch expansion ratio of 2000%. Finally, it is heat-set to form a film.
[0114] As described above, the obtained PTFE microporous membrane has a first porous outer surface and a second porous outer surface with different microstructures. As shown in Figures 10-11, Figure 10 is a scanning electron micrograph (SEM) of the first porous outer surface of the PTFE membrane, taken at a magnification of 2000 times, showing an island-like microstructure constructed by a plurality of interconnected smaller nodes; Figure 11 is a scanning electron micrograph (SEM) of the second porous outer surface of the PTFE membrane, taken at a magnification of 2000 times, showing an H-shaped ladder-like microstructure constructed by a plurality of interconnected larger nodes.
[0115] The bubble point was determined using a capillary flow porometer running two test conditions. In the first test, the first porous outer surface of the PTFE membrane faced the metal mesh, and in the second test, the second porous outer surface of the PTFE membrane faced the metal mesh. The bubble points were measured to be 2.35 bar and 1.77 bar, respectively.
[0116] Example 6
[0117] A polytetrafluoroethylene (PTFE) dispersion resin was uniformly mixed with 21.3% by weight of an isoparaffin (ExxonMobil ISOPAR M) and placed in a 30°C oven for 15 hours. The PTFE resin mixture was pressed into a cylindrical preform, which was then extruded through a T-die at a compression ratio of 190 to obtain a continuous first sheet with a rectangular cross-section and a thickness of 0.5 mm.
[0118] A polytetrafluoroethylene (PTFE) dispersion resin was uniformly mixed with 26.2% by weight of an isoparaffin (ExxonMobil ISOPAR K) and placed in a 30°C oven for 15 hours. The PTFE resin mixture was then pressed into a cylindrical preform. The preforms were then extruded through T-dies of different specifications at a compression ratio of 56 to produce a second continuous sheet with a rectangular cross-section and a thickness of 0.8 mm. A third continuous sheet with a rectangular cross-section and a thickness of 1.2 mm was extruded at a compression ratio of 37.
[0119] Three types of sheets are stacked in increasing or decreasing thickness along the same width direction. They are then fed into a pair of metal rollers along the length direction and rolled to 0.3mm in the thickness direction to form a laminate. The dried laminate, after removing the additive oil, is longitudinally stretched by a longitudinal stretching mechanism at a stretching roller temperature of 300°C, a stretching rate of 117% / s, and a stretch expansion ratio of 230%. The uniaxially stretched product (base tape) is then transversely stretched by a transverse expander at a stretching temperature of 250°C, a stretching rate of 22% / s, and a stretch expansion ratio of 2000%. Finally, it is heat-set to form a film.
[0120] As described above, the obtained PTFE microporous membrane has a first porous outer surface and a second porous outer surface with different microstructures. As shown in Figures 12-13, Figure 12 is a scanning electron micrograph (SEM) of the first porous outer surface of the PTFE membrane, taken at a magnification of 2000 times, showing an island-like microstructure constructed by a plurality of interconnected smaller nodes; Figure 13 is a scanning electron micrograph (SEM) of the second porous outer surface of the PTFE membrane, taken at a magnification of 2000 times, showing an H-shaped ladder-like microstructure constructed by a plurality of interconnected larger nodes.
[0121] The bubble point was determined by running two test conditions using a capillary flow porometer. In the first test, the first porous outer surface of the PTFE membrane faced the metal mesh, and in the second test, the second porous outer surface of the PTFE membrane faced the metal mesh. The bubble points were measured to be 2.12 bar and 1.68 bar, respectively.
[0122] The series of detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present invention. They are not intended to limit the scope of protection of the present invention. Any equivalent implementation methods or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
[0123] In addition, it should be understood that although this specification is described in terms of implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.
Claims
1. A polytetrafluoroethylene membrane with a gradient pore structure, characterized in that: The cross-section of the polytetrafluoroethylene membrane has a gradient pore structure, and the first porous outer surface and the second porous outer surface of the polytetrafluoroethylene membrane have fibers and nodes with different microstructures; the first porous outer surface has an island-shaped microstructure constructed by a plurality of interconnected smaller nodes, and the second porous outer surface has an H-shaped ladder-shaped microstructure constructed by a plurality of interconnected larger nodes.
2. The polytetrafluoroethylene membrane with a gradient pore structure according to claim 1, characterized in that: The smaller nodes are circular in structure and have an average diameter of 0.30 to 1.50 μm.
3. The polytetrafluoroethylene membrane with a gradient pore structure according to claim 2, characterized in that: The smaller nodes are formed by connecting a number of thick and short microfibers. The average length of the thick and short microfibers is in the range of 0.2 to 2.5 μm, the average diameter is in the range of 0.05 to 0.2 μm, and the aspect ratio is 2 to 20.
4. The polytetrafluoroethylene membrane with a gradient pore structure according to claim 1, characterized in that: The larger nodes are long oval structures with an average length of 0.5 to 10 μm and an average width of 0.5 to 2 μm.
5. The polytetrafluoroethylene membrane with a gradient pore structure according to claim 4, characterized in that: The larger nodes are formed by connecting a number of slender microfibers, wherein the average length of the slender microfibers is in the range of 1 to 10 μm, the average diameter is in the range of 5 to 200 nm, and the aspect ratio is 10 to 200.
6. A method for preparing a polytetrafluoroethylene membrane having a gradient pore structure according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) First, isoparaffin and PTFE dispersion resin are uniformly mixed to obtain a PTFE resin mixture, and then the PTFE resin mixture is pressed into a cylindrical preform; (2) using an extruder to extrude the cylindrical preform into three continuous strips of equal width with different thicknesses and rectangular cross-sections through T-shaped extrusion dies of different specifications, namely, a first sheet, a second sheet, and a third sheet; (3) The first sheet, the second sheet, and the third sheet are stacked in the same width direction in increasing or decreasing thickness, and are fed into a pair of metal rollers along the length direction and rolled in the thickness direction to a range of 0.05 to 1 mm to form a laminate; (4) drying the laminate at 200-250° C., and then expanding the laminate in the direction of the speed at 250-350° C. at a stretching rate of 20% / s to 3000% / s and an expansion ratio of 50% to 900% to form a uniaxially stretched product; (5) Expanding the uniaxially stretched product in a direction perpendicular to the speed at a temperature of 200 to 400° C., at a stretching rate of 5% / s to 500% / s, and at a ratio of 300% to 3000%, to finally form a PTFE membrane material with a gradient pore structure.
7. The method for preparing a polytetrafluoroethylene membrane having a gradient pore structure according to claim 6, wherein: In step (1), isoparaffin and PTFE dispersed resin are uniformly mixed in a weight ratio of 15 to 30% to obtain a PTFE resin mixture, which is then dried at a temperature of not less than 20° C. for more than 12 hours, and the PTFE resin mixture is pressed into a cylindrical preform.
8. The method for preparing a polytetrafluoroethylene membrane having a gradient pore structure according to claim 7, wherein: In step (2), the cylindrical preform is extruded into three continuous strips of equal width with different thicknesses having rectangular cross-sections through T-shaped extrusion dies of different specifications at a compression ratio of 20 to 500, namely a first sheet, a second sheet and a third sheet, wherein: the thickness of the second sheet is at least 1.2 times the thickness of the first sheet, the thickness of the third sheet is at least 1.2 times the thickness of the second sheet, and the compression ratio of the first sheet is at least 2.5 times that of the second sheet and 3 times that of the third sheet.
9. The method for preparing a polytetrafluoroethylene membrane having a gradient pore structure according to claim 8, wherein: In step (4), the laminate is expanded along the speed direction at a stretching rate of 50% / s to 2000% / s and an expansion ratio of 80% to 800% to form a uniaxially stretched product.
10. The method for preparing a polytetrafluoroethylene membrane having a gradient pore structure according to claim 9, wherein: In step (5), the film is expanded in a direction perpendicular to the speed at a stretching rate of 20% / s to 300% / s and a ratio of 500% to 2500%, thereby finally forming a PTFE membrane material with a gradient pore structure.