Photo- and heat-curable silicone composition and production method for cured product thereof
Patent Information
- Application Number
- MYPI2025001485
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-28
- Filing Date
- 2023-08-01
- Publication Date
- 2024-03-28
AI Technical Summary
Existing two-step curing silicone compositions face challenges in managing first-stage and second-stage curing processes, with thermal curing methods requiring strict temperature control and generating outgas components that can lead to cracks, while photo- and thermosetting compositions lack efficient control over curing stages.
A composition containing (meth)acrylic group-containing organopolysiloxane, alkenyl group-containing organopolysiloxane, and organohydrogenpolysiloxane, along with a photopolymerization initiator and hydrosilylation reaction catalyst, allowing for first-stage curing by light and second-stage curing by heat, enabling individual and easy management of curing processes.
This approach allows for instantaneous first-stage curing by UV irradiation and controlled second-stage curing by heat, providing a stable and reproducible method for producing high-hardness silicone products, suitable for adhesive films and electronic device encapsulation.
Abstract
Description
Photo- and heat-curable silicone composition and method for producing the cured product
[0001] The present invention relates to a photo- and heat-curable silicone composition, and more specifically to a two-stage curing liquid silicone composition that is brought to a semi-cured state by radical curing with ultraviolet light in the presence of a photopolymerization initiator and a hydrosilylation reaction catalyst, and then completely cured by a hydrosilylation reaction upon heating, as well as a method for producing a cured product of said composition.
[0002] Two-stage curing liquid silicone materials are attractive because they allow for separate manufacturing process control. For example, in the encapsulant layer of an optical device, the degree of phosphor dispersion affects the light extraction efficiency, so strict control of the degree of dispersion is necessary. However, when a heat-curing material is used as the encapsulant, the viscosity of the base material decreases during heat curing, making the phosphor more likely to settle, making it difficult to control the degree of dispersion and cure simultaneously. Using a two-stage curing material for the encapsulant layer allows for consistent phosphor dispersion control through the first curing step, and then increases the hardness to the desired level through the second curing step, allowing for mounting on a semiconductor device. Thus, to simplify difficult manufacturing processes and contribute to the development of new, innovative manufacturing processes, two-stage curing silicone materials have been proposed for a wide range of applications, including adhesive films, optical device encapsulants, temporary fixing agents for electronic device components, and adhesives, and are actively being researched and developed.
[0003] Patent Document 1 reports that a liquid silicone composition containing an alkenyl group-containing organopolysiloxane, a platinum catalyst for hydrosilylation reactions, and a high-energy ray-activated platinum catalyst is subjected to a heated environment from room temperature to cause primary curing through an addition reaction, yielding a thermoplastic silicone that does not have fluidity in a room temperature environment, and that the thermoplastic silicone is then irradiated with high-energy rays, followed by a heated environment from room temperature to cause a further hydrosilylation reaction, thereby yielding a highly hardened silicone cured product.
[0004] Patent Document 2 reports that a liquid silicone adhesive composition containing an alkenyl group-containing organopolysiloxane, a hydrosilylation reaction catalyst, and a thermal radical reaction initiator is exposed to an environment ranging from room temperature to 100°C to carry out a first stage of curing via an addition reaction, yielding a silicone cured product, and that the resulting silicone cured product is then exposed to an environment at a temperature higher than the first stage curing temperature, such as 150 to 190°C, to carry out a second stage of curing via a thermal radical reaction, thereby yielding a silicone cured product with a high hardness.
[0005] Patent Document 3 reports that a liquid silicone adhesive composition containing an organopolysiloxane having a condensation reactive group, an alkenyl group-containing organopolysiloxane, a condensation reaction catalyst, and a thermal radical reaction initiator is subjected to a condensation reaction in the presence of moisture to carry out a first-stage curing to obtain a silicone cured product, and that the obtained silicone cured product is then subjected to a heated environment to carry out a second-stage curing by a thermal radical reaction, thereby obtaining a silicone cured product with a high hardness.
[0006] The methods described in Patent Documents 1 and 2 employ a curing mechanism in which heating is the starting point for both the first and second curing stages. It is generally difficult to control the state during thermal curing, and therefore, in order to reproducibly obtain the cured state of the silicone cured product obtained by the first curing, it is necessary to strictly control the temperature profile, making the methods described in Patent Documents 1 and 2 difficult to use in practice. On the other hand, the method described in Patent Document 3 generally performs the first curing by a condensation reaction, which generates a lot of outgassing components, and then performs thermal radical curing, which can lead to problems such as reversion and cracking due to the evaporation of outgassing components.
[0007] International Publication No. 2019 / 088066 Japanese Patent Application Laid-Open No. 2007-191629 International Publication No. 2018 / 186165
[0008] The present invention has been made in view of the above circumstances, and has as its object to provide a two-stage curing silicone composition in which the first and second stages of curing can be controlled separately and simply.
[0009] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have found that a composition containing a (meth)acrylic group-containing organopolysiloxane, an alkenyl group-containing organopolysiloxane, and an organohydrogenpolysiloxane in specified ratios can undergo a first-stage light-induced curing and a second-stage heat-induced curing in the presence of a photopolymerization initiator and a hydrosilylation reaction catalyst, which allows for separate and simple control of the first-stage light-induced curing and the second-stage heat-induced curing, thereby completing the present invention.
[0010] That is, the present invention provides: 1. a photo- and thermosetting silicone composition comprising: (A) an organopolysiloxane having at least three (meth)acrylic groups per molecule; (B) an organopolysiloxane having at least two alkenyl groups and no (meth)acrylic groups per molecule; (C) an organohydrogenpolysiloxane having at least two hydrosilyl groups per molecule; (D) a photopolymerization initiator; and (E) a hydrosilylation reaction catalyst; wherein the amount of (meth)acrylic groups contained in component (A) is 1 to 15 mmol per 100 g of the composition; the ratio of the number of alkenyl groups in the composition to the number of (meth)acrylic groups contained in component (A) is 0.5 or greater; and the ratio of the number of hydrosilyl groups to the number of alkenyl groups and (meth)acrylic groups contained in components (A) and (B) is 0.8 to 3.0; 1. A photo- and thermo-curable silicone composition, wherein the component (A) is the following (A-i), (A-ii), or both: (A-i) an organopolysiloxane represented by the following formula (1): (In the formula, R 1 are each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms; R 2 each independently represents an oxygen atom or an alkylene group having 1 to 20 carbon atoms; R 3are each independently an acryloyloxyalkyl group, a methacryloyloxyalkyl group, an acryloyloxyalkyloxy group, or a methacryloyloxyalkyloxy group; k is an integer from 0 to 1,000; m is an integer from 0 to 20; a and b are each independently an integer from 0 to 3; and a+b+m is an integer of 3 or greater. The siloxane units in the parentheses followed by k and m may be arranged in any order. (A-ii) An organopolysiloxane A represented by the following formula (2) and having a number average molecular weight (Mn) of 3,000 to 100,000: p (R 1 3SiO 1 / 2 ) q (SiO 4 / 2 ) r (2) (wherein, R 1 represents the same meaning as above, A is a siloxane unit represented by the following formula (3), and p, q, and r are numbers that satisfy p>0, q>0, and r>0, and p+q+r=1, respectively. (In the formula, R 1 , R 2 and R 3 represents the same meaning as above, n represents an integer of 0 to 10, and c represents an integer of 1 to 3. 3. Photo- and thermosetting silicone composition 1, wherein the component (B) is the following (B-iii), (B-iv), or both: (B-iii) A linear organopolysiloxane R represented by the following formula (4), having a viscosity at 23°C of 50 to 10,000,000 mPa s: 4 R 1 2Si (OSiR 1 2) S OSiR 1 2nd Race 4 (4) (wherein, R 1 has the same meaning as above, and R 4 represents an alkenyl group having 2 to 20 carbon atoms, and s represents an integer of 1 to 10,000. (B-iv) Organopolysiloxanes represented by the following formula (5): 1 3SiO 1 / 2 ) t (R 4 R 1 2SiO 1 / 2 ) u (SiO4 / 2 ) v (5) (wherein, R 1 and R 4 represents the same meaning as above, and t, u, and v are numbers that satisfy t>0, u>0, v>0, and (t+u+v)=1.) 4. The photo- and thermosetting silicone composition of 1, wherein the component (C) is a linear organohydrogenpolysiloxane represented by the following formula (7), (R 1 3SiO 1 / 2 ) w (H (3-f) R 1 f SiO 1 / 2 ) 2-w (HR 1 1SiO 2 / 2 ) x (R 1 2SiO 2 / 2 ) y (7) (wherein, R 1 represents the same meaning as above, f represents 1 or 2, w represents an integer satisfying 0≦w≦2, and x and y represent positive integers satisfying 2≦x+y≦800 and 0.6≦x / (x+y+2)≦1.0.) 5. The photo- and thermosetting silicone composition of 1, wherein the component (D) is a photoradical polymerization initiator that does not contain nitrogen atoms, sulfur atoms, or phosphorus atoms; 6. A method for producing a cured product, comprising: (α) a step of irradiating any of the photo- and thermosetting silicone compositions of 1 to 5 with ultraviolet light to partially cure the composition and form a semi-cured composition; and (β) a step of heating the obtained semi-cured composition to completely cure it.
[0011] The photo- and heat-curable silicone composition of the present invention has two different curing-inducing methods, making it easy to control and handle the curing. That is, the first curing step using light can be carried out at room temperature in a short time because the polymerization reaction proceeds instantaneously during ultraviolet irradiation. Furthermore, the semi-cured composition after the first curing step is easy to handle and does not change in hardness over a long period of time in a low-temperature environment such as refrigeration, ensuring ample time before the second curing step using heat. The photo- and heat-curable silicone composition of the present invention, which has these properties, is particularly useful as an adhesive film, an optical device encapsulating material, or an adhesive for electronic device components.
[0012] The present invention will be described in detail below. The photo- and heat-curable silicone composition according to the present invention contains the following components (A) to (E).
[0013] [1] Component (A) Component (A) in the photo- and thermosetting silicone composition of the present invention is an organopolysiloxane having at least three (meth)acrylic groups per molecule, and is preferably the following (A-i), (A-ii), or both: In the present invention, the term "(meth)acrylic group" refers to an acrylic group or a methacrylic group.
[0014] (Ai) Organopolysiloxane represented by the following formula (1):
[0015] (In the formula, R 1 are each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms; R 2 each independently represents an oxygen atom or an alkylene group having 1 to 20 carbon atoms; R 3are each independently an acryloyloxyalkyl group, a methacryloyloxyalkyl group, an acryloyloxyalkyloxy group, or a methacryloyloxyalkyloxy group; k is an integer from 0 to 1,000; m is an integer from 0 to 20; a and b are each independently an integer from 0 to 3; and a+b+m is an integer of 3 or greater. The siloxane units in the parentheses to which k and m are attached may be arranged in any order.
[0016] (A-ii) Organopolysiloxane A represented by the following formula (2) and having a number average molecular weight (Mn) of 3,000 to 100,000: p (R 1 3SiO 1 / 2 ) q (SiO 4 / 2 ) r (2) (wherein, R 1 represents the same meaning as above, A is a siloxane unit represented by the following formula (3), and p, q, and r are numbers that satisfy p>0, q>0, and r>0, and p+q+r=1, respectively.
[0017] (In the formula, R 1 , R 2 and R 3 represents the same meaning as above, n represents an integer of 0 to 10, and c represents an integer of 1 to 3.
[0018] R 1 The alkyl group having 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms, may be linear, branched, or cyclic, and specific examples thereof include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-hexyl, cyclohexyl, n-octyl, 2-ethylhexyl, and n-decyl groups. 1Specific examples of the aryl group having 6 to 20 carbon atoms, preferably 6 to 10 carbon atoms, include phenyl, tolyl, xylyl, naphthyl, etc. In addition, some or all of the hydrogen atoms bonded to these carbon atoms may be substituted with other substituents, specific examples of which include halogen-substituted hydrocarbon groups such as chloromethyl, bromoethyl, trifluoropropyl, and cyanoethyl groups, and cyano-substituted hydrocarbon groups. Among these, R 1 As the alkyl group, an alkyl group having 1 to 5 carbon atoms and a phenyl group are preferred, and a methyl group, an ethyl group and a phenyl group are more preferred.
[0019] R 2 The alkylene group having 1 to 20 carbon atoms may be linear, branched, or cyclic, and specific examples thereof include methylene, ethylene, propylene, trimethylene, tetramethylene, isobutylene, pentamethylene, hexamethylene, heptamethylene, octamethylene, and nonamethylene groups. 2 is preferably an oxygen atom, a methylene group, an ethylene group or a trimethylene group, more preferably an oxygen atom or an ethylene group.
[0020] R 3 Specific examples of the compound include, but are not limited to, those represented by the following formulas:
[0021] (In the formula, g represents an integer of 1 to 4.)
[0022] In the above formula (1), a and b are integers from 0 to 3, and the sum (a + b + m) with the above m is 3 or greater. If a + b + m is less than 3, the photocuring reaction is less likely to occur, and the resulting silicone cured product may have insufficient hardness. In particular, it is preferable that a and b are 2 and m is 4. k is an integer from 0 to 1,000, and if k exceeds 1,000, polymerizability may be poor. From the standpoint of the resistance to volatilization and polymerizability of component (A-i), k is preferably an integer from 30 to 500, and more preferably an integer from 50 to 400. m is an integer from 0 to 20, preferably an integer from 0 to 10, and more preferably 0. If m exceeds 20, the composition may become cloudy during curing.
[0023] In the above formula (2), p, q, and r are numbers that satisfy p>0, q>0, r>0, and p+q+r=1, respectively. From the standpoint of ease of handling of the composition and the hardness of the resulting silicone cured product, p is preferably 0.05 to 0.07, q is preferably 0.33 to 0.35, and r is preferably 0.58 to 0.62.
[0024] The number average molecular weight of component (A-ii) is in the range of 3,000 to 100,000, preferably 5,000 to 10,000. If the number average molecular weight is below 3,000, the number of (meth)acrylic groups contained per molecule may fall below 3, which may result in insufficient hardness of the silicone cured product obtained after the two-stage curing. If the number average molecular weight exceeds 100,000, the compatibility of component (A-ii) may decrease. Note that the number average molecular weight in the present invention is a value calculated in terms of standard polystyrene as measured by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as the developing solvent.
[0025] The component (A) may be used alone or in combination of two or more. Furthermore, since the component (A-ii) may become solid in the usage environment, it may be dissolved in the component (A-i) or a liquid organic compound containing a (meth)acrylic group before use. From the viewpoint of ease of handling, the viscosity of the entire component (A) at 23°C is preferably 100,000 mPa·s or less (typically 1 to 100,000 mPa·s), and more preferably 10,000 mPa·s or less (for example, 5 to 10,000 mPa·s). The viscosity in the present invention is measured using a B-type rotational viscometer.
[0026] The amount of (meth)acrylic groups contained in component (A) is within the range of 1 to 15 mmol, preferably 1.5 to 14 mmol, per 100 g of the composition. If it is less than 1 mmol / 100 g, the first-stage curing may be insufficient, while if it exceeds 15 mmol / 100 g, the first-stage curing may result in an excessively high hardness, thereby negating the benefit of performing the two-stage curing.
[0027] [2] Component (B) The component (B) in the photo- and thermosetting silicone composition of the present invention is an organopolysiloxane having at least two alkenyl groups in each molecule and no (meth)acrylic groups, and is preferably the following (B-iii), (B-iv), or both:
[0028] (B-iii) A linear organopolysiloxane R having a viscosity of 50 to 10,000,000 mPa·s at 23°C, represented by the following formula (4): 4 R 1 2Si (OSiR 1 2) S OSiR 1 2nd Race 4 (4) (wherein, R 1 has the same meaning as above, and R 4 represents an alkenyl group having 2 to 20 carbon atoms, and s represents an integer of 1 to 10,000. (B-iv) Organopolysiloxanes represented by the following formula (5) (R 1 3SiO 1 / 2 ) t (R 4 R 12SiO 1 / 2 ) u (SiO 4 / 2 ) v (5) (wherein, R 1 and R 4 has the same meaning as above, and t, u, and v are numbers that satisfy t>0, u>0, and v>0, and (t+u+v)=1.
[0029] In the above formula (4), R 1 Examples of R include the same as those of formula (1), but a methyl group and a phenyl group are preferred. 4 The alkenyl group having 2 to 20 carbon atoms may be linear, branched, or cyclic, and specific examples thereof include vinyl, allyl, butenyl, pentenyl, hexenyl, and octenyl groups, with vinyl being preferred. s is an integer of 1 to 10,000, and preferably an integer of 100 to 1,000.
[0030] The viscosity of component (B-iii) at 25°C is 50 to 10,000,000 mPa·s, and preferably 100 to 100,000 mPa·s.
[0031] In the above formula (5), R 1 Examples of R include the same as those of formula (1), but a methyl group and a phenyl group are preferred. 4 The alkenyl group having 2 to 20 carbon atoms may be linear, branched, or cyclic, and specific examples thereof include vinyl, allyl, butenyl, pentenyl, hexenyl, and octenyl groups, with the vinyl group being preferred. t, u, and v are numbers that satisfy t > 0, u > 0, and v > 0, respectively, and (t + u + v) = 1, and from the viewpoints of curability and hardness of the cured product, (t + u) / v is preferably 0.3 to 2.0, and more preferably 0.5 to 1.0.
[0032] The number-average molecular weight of component (B-iv) is preferably 500 to 500,000, and more preferably 1,000 to 100,000. If the number-average molecular weight is less than 500, the number of alkenyl groups contained per molecule may fall below 2, which may result in insufficient hardness of the silicone cured product obtained after the two-stage curing. If the number-average molecular weight exceeds 500,000, the compatibility of component (B-iv) may decrease.
[0033] The component (B) may be used alone or in combination of two or more. Furthermore, since the component (B-iv) may become solid in the usage environment, it may be dissolved in the component (B-iii) before use. From the viewpoint of ease of handling, the viscosity of the entire component (B) at 23°C is preferably 100,000 mPa s or less (typically 1 to 100,000 mPa s), and more preferably 10,000 mPa s or less (for example, 5 to 10,000 mPa s).
[0034] The amount of component (B) to be blended is an amount such that the ratio of the number of alkenyl groups in the composition to the number of (meth)acrylic groups in component (A) is 0.5 or more, preferably 0.5 to 30. If the ratio is less than 0.5, the change in hardness due to the second-stage curing will be minimal, and the benefit of performing two-stage curing may be lost.
[0035] [3] Component (C) Component (C) is an organohydrogenpolysiloxane having at least two hydrosilyl groups per molecule, and specific examples thereof include those represented by the following average composition formula (6): 1 d H e SiO (4-d-e) / 2 (6) (wherein, R 1 has the same meaning as above, d is 0.7 to 2.1, e is 0.001 to 1.0, and is a number that satisfies 0.8≦d+e≦3.0.
[0036] In the above formula (6), d is preferably 1.0 to 1.8, e is preferably 0.1 to 1, and d+e is preferably 1≦d+e≦2.4, more preferably 1.6≦d+e≦2.2. Within these ranges, foaming during curing can be suppressed, the hardness of the resulting cured product is further improved, and changes in hardness over time are less likely to occur.
[0037] In particular, the component (C) is preferably a linear organohydrogenpolysiloxane represented by the following formula (7): (R 1 3SiO 1 / 2 ) w (H (3-f) R 1 f SiO 1 / 2 ) 2-w (HR 1 1SiO 2 / 2 ) x (R 1 2SiO 2 / 2 ) y (7) In formula (7), R 1 Examples of x include the same as those in formula (1) above, but a methyl group is preferred. f is 1 or 2, but 2 is preferred. w is an integer satisfying 0≦w≦2, but is preferably 0 or 2, and more preferably 2. x and y are positive integers satisfying 2≦x+y≦800 and 0.6≦x / (x+y+2)≦1.0, and are preferably positive integers satisfying 7≦x+y≦700 and 0.7≦x / (x+y+2)≦0.9.
[0038] The kinematic viscosity of component (C) at 23°C is 0.5 to 1,000 mm 2 / s is preferred, and 1 to 100 mm 2 Here, the kinematic viscosity is a value measured using a Cannon-Fenske viscometer.
[0039] The component (C) may be used alone or in combination of two or more. The amount of component (C) is such that the ratio of the number of hydrosilyl groups to the number of alkenyl groups and (meth)acrylic groups contained in components (A) and (B) is in the range of 0.8 to 3.0, preferably 0.9 to 2.0. If the ratio is less than 0.8, the curability in the second curing stage and the hardness of the resulting cured product may be insufficient, while if it exceeds 3.0, the hardness of the resulting cured product changes significantly over time.
[0040] [4] Component (D) Component (E) is a photopolymerization initiator that generates organic radical species by absorbing ultraviolet light, which act as the initiation point for the polymerization reaction of the (meth)acrylic group. The photopolymerization initiator for component (D) preferably does not contain nitrogen atoms, sulfur atoms, or phosphorus atoms so as not to inhibit the addition reaction, which is the first-stage curing mechanism. Specific examples of such photopolymerization initiators include 2,2-diethoxyacetophenone, 2,2-dimethoxy-1,2-diphenylethan-1-one (Omnirad 651, manufactured by IGM Resins B.V.), 1-hydroxycyclohexylphenylketone (Omnirad 184, manufactured by IGM Resins B.V.), 2-hydroxy-2-methyl-1-phenylpropan-1-one (Omnirad 1173, manufactured by IGM Resins B.V.), and 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methylpropan-1-one (Omnirad 1174, manufactured by IGM Resins B.V.). 127), and methyl phenylglyoxylate (Omnirad MBF, manufactured by IGM Resins B.V.). Among these, 2,2-diethoxyacetophenone and 2-hydroxy-2-methyl-1-phenyl-propan-1-one (Omnirad 1173, manufactured by IGM Resins B.V.) are preferred from the viewpoint of compatibility with components (A) and (B).
[0041] The component (D) may be used alone or in combination of two or more. The amount of component (D) added is preferably in the range of 0.01 to 20 mass% based on the total mass of components (A), (B), and (C). Within this range, good curability and excellent deep curing properties are achieved.
[0042] [5] Component (E) Component (E) is a hydrosilylation catalyst that promotes the addition reaction between the alkenyl groups in components (A) and (B) and the Si—H groups in component (C). Specific examples include platinum metal-supported carbon powder, platinum black, platinic chloride, chloroplatinic acid, reaction products of chloroplatinic acid and monohydric alcohols, complexes of platinum and vinylsiloxanes such as divinyltetramethyldisiloxane, complexes of chloroplatinic acid and olefins, platinum-based catalysts such as platinum bisacetoacetate, palladium-based catalysts, and rhodium-based catalysts. Among these, platinum-containing catalysts are preferred from the standpoint of reactivity, and complexes of platinum and vinylsiloxanes are more preferred.
[0043] There are no particular restrictions on the amount of component (E) that may be added, provided that it is an amount that promotes the hydrosilylation reaction. However, an amount that results in a metal content in component (E) of 0.01 to 500 ppm by mass, based on the total mass of components (A), (B), and (C), is preferred, an amount that results in a metal content in component (E) of 0.01 to 500 ppm by mass, more preferably 0.05 to 100 ppm, and even more preferably 0.01 to 50 ppm.
[0044] [6] Other Components In addition to the above-mentioned components (A) to (E), the photo- and thermosetting silicone composition of the present invention may contain other components as long as the purpose of the present invention is not impaired. Examples of other components include reaction control agents such as 3-methyl-1-butyn-3-ol and ethynylmethyldecylcarbinol that control the reactivity of the platinum catalyst; adhesion promoters having adhesion-imparting groups such as carbonyl groups, epoxy groups, and alkoxysilyl groups; thixotropy control agents such as fumed silica; reinforcing agents such as crystalline silica; antioxidants; light stabilizers; heat resistance improvers such as metal oxides and metal hydroxides; pigments such as titanium oxide; dyes; thermal conductivity-imparting fillers such as alumina; viscosity modifiers such as non-reactive silicone oils that do not have reactive functional groups; and conductivity-imparting agents such as metal powders of silver, gold, etc.
[0045] The photo- and thermosetting silicone composition of the present invention can be prepared by mixing the above components (A) to (E) and other components, if necessary, by a known method. In this case, the composition of the present invention may be prepared as a one-part composition, or as a two-part composition or a composition divided into three or more parts, which are then mixed in any desired ratio at the time of use.
[0046] The method for producing a cured product of the photo- and heat-curable silicone composition of the present invention includes the steps of: (α) irradiating the photo- and heat-curable silicone composition with ultraviolet light to partially cure the composition and form a semi-cured composition; and (β) heating the resulting semi-cured composition to completely cure it.
[0047] The ultraviolet light irradiated in step (α) preferably has a wavelength of 200 to 500 nm, more preferably 200 to 350 nm. From the viewpoint of preventing discoloration, the irradiation temperature is preferably 20 to 40°C, and the irradiation intensity is preferably 30 to 2,000 mW / cm. 2 More preferably, the exposure dose is 150 to 100,000 mJ / cm 2is preferred. Usable light sources for ultraviolet rays include 365 nm UV-LED lamps, metal halide lamps, and high-pressure mercury lamps. Examples of ultraviolet irradiation methods include irradiating the composition with an appropriate amount of ultraviolet rays. However, when the composition is applied to a transparent substrate such as glass or a resin film, ultraviolet rays may be irradiated through the glass or film. During ultraviolet irradiation, it is preferable to irradiate the composition in a nitrogen or argon atmosphere to suppress the influence of oxygen, which inhibits curing. The heating conditions in step (β) are preferably in an environment of 50 to 150°C, more preferably 80 to 120°C, for 10 minutes to 1 day, more preferably 30 minutes to 1 hour.
[0048] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. In the following, the viscosity at 23°C was measured using a Brookfield rotational viscometer, and the kinematic viscosity at 23°C was measured using a Cannon-Fenske viscometer. Vi represents a vinyl group, and Me represents a methyl group.
[0049] [1] Preparation of photo- and heat-curable silicone compositions [Examples 1-1 to 1-7, Comparative Examples 1-1 to 1-6] Components (A) to (E) shown below and other components were mixed in the amounts (parts by mass) shown in Tables 1 and 2 to prepare photo- and heat-curable silicone compositions.
[0050] Component (A) (A-i-1): Organopolysiloxane represented by the following formula (8) (viscosity at 23°C: 3,000 mPa·s, acrylic group content: 0.02 mol / 100 g) (In the formula, the arrangement of each siloxane unit in parentheses is random or block.)
[0051] (A-i-2): Organopolysiloxane represented by the following formula (9) (viscosity at 23°C: 1,000 mPa·s, acrylic group content: 0.026 mol / 100 g)
[0052] (A-ii-1): Siloxane unit represented by the following formula (10) / (ViMeSiO 1 / 2 Unit) / (MeSiO 1 / 2an organopolysiloxane having a molar ratio of (SiO units) / (SiO units) of 0.056 / 0.014 / 0.390 / 0.540 (number average molecular weight 5,700, average number of methacryl groups per molecule 3.7, amount of methacryl groups 0.0656 mol / 100 g, amount of vinyl groups 0.0164 mol / 100 g);
[0053] Component (B) (B-iii-1): an organopolysiloxane represented by the following formula (11) (viscosity at 23°C: 3,000 mPa·s, vinyl group content: 0.01 mol / 100 g) (In the formula, the arrangement of each siloxane unit in parentheses is random or block.)
[0054] (B-iii-2): Organopolysiloxane represented by the following formula (12) (viscosity at 23°C: 1,600 mPa s, vinyl group content: 0.013 mol / 100 g)
[0055] (B-iii-3): Organopolysiloxane represented by the following formula (13) (viscosity at 23°C: 5,000 mPa s, vinyl group content: 0.006 mol / 100 g)
[0056] (B-iv-1): Organopolysiloxane represented by the following average formula (14) (number average molecular weight: 4,500, average number of vinyl groups per molecule: 3.7, vinyl group amount: 0.082 mol / 100 g) (ViMeSiO 1 / 2 ) 0.058 (MeSiO 1 / 2 ) 0.402 (SiO 4 / 2 ) 0.540 (14)
[0057] Component (C) (C-1): an organohydrogenpolysiloxane represented by the following formula (15) (kinematic viscosity at 23°C: 4.5 mm 2 / s, silicon-bonded hydrogen atom content = 0.0145 mol / g)
[0058] (In the formula, the arrangement of each siloxane unit in parentheses is random or block.)
[0059] Component (D) (D-1): 2-hydroxy-2-methyl-1-phenyl-propan-1-one (Omnirad 1173, manufactured by IGM Resins B.V.)
[0060] Component (E) (E-1) Toluene solution of platinum 1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum content: 0.5% by mass)
[0061] (Other Components) Reaction inhibitor: ethynylmethyldecylcarbinol Diluent: disiloxane compound represented by the following structural formula (16)
[0062]
[0063]
[0064] [2] Production of cured products of photo- and heat-curable silicone compositions [Examples 2-1 to 2-7, Comparative Examples 2-1 to 2-6] The photo- and heat-curable silicone compositions obtained in Examples 1-1 to 1-7 and Comparative Examples 1-1 to 1-6 were subjected to irradiation in a nitrogen environment using a UV-LED lamp with a wavelength of 365 nm at 25°C with an irradiation intensity of 100 mW / cm. 2 and a dose of 3,000 mJ / cm 2 The first stage of curing was carried out by irradiating the sample with ultraviolet light so that the hardness reached 100%. The penetration or durometer A hardness of the resulting cured product was measured in accordance with JIS K 6249 using a penetrometer (1 / 4 cone) or durometer A hardness tester manufactured by Rigo Co., Ltd. Note that when the penetration was less than 1 and measurement was impossible, durometer A hardness was used. Subsequently, the cured product obtained by the first stage of curing was allowed to stand at 120°C for 1 hour to carry out the second stage of curing. The resulting cured product was cooled to 25°C, and then the hardness was measured in the same way as for the first stage of curing. The results are shown in Tables 3 and 4.
[0065]
[0066]
[0067] As shown in Tables 3 and 4, the photo- and heat-curable silicone compositions prepared in Examples 1-1 to 1-7 exhibit a large difference in hardness between the first-stage light-induced curing and the second-stage heat-induced curing. On the other hand, when the compositions of Comparative Examples 1-1, 1-5, and 1-6, in which the amount of (meth)acrylic groups in component (A) was less than 1 mmol per 100 g of composition, were used, the first-stage light-induced curing did not occur, and when the compositions of Comparative Examples 1-2 to 1-4, in which the amount of (meth)acrylic groups in component (A) was more than 15 mmol per 100 g of composition, the first-stage light-induced curing progressed too far, resulting in almost no difference in hardness after the second-stage curing and thus not forming a two-stage curing material.
Claims
1. A photo- and heat-curable silicone composition comprising: (A) an organopolysiloxane having at least three (meth)acrylic groups per molecule; (B) an organopolysiloxane having at least two alkenyl groups and no (meth)acrylic groups per molecule; (C) an organohydrogenpolysiloxane having at least two hydrosilyl groups per molecule; (D) a photopolymerization initiator; and (E) a hydrosilylation reaction catalyst; wherein the amount of (meth)acrylic groups contained in component (A) is 1 to 15 mmol per 100 g of the composition; the ratio of the number of alkenyl groups in the composition to the number of (meth)acrylic groups in component (A) is 0.5 or greater; and the ratio of the number of hydrosilyl groups to the number of alkenyl groups and (meth)acrylic groups contained in components (A) and (B) is 0.8 to 3.
0.
2. The photo- and thermosetting silicone composition according to claim 1, wherein the component (A) is the following (A-i), (A-ii), or both: (A-i) an organopolysiloxane represented by the following formula (1): (In the formula, R 1 are each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms; R 2 each independently represents an oxygen atom or an alkylene group having 1 to 20 carbon atoms; R 3 are each independently an acryloyloxyalkyl group, a methacryloyloxyalkyl group, an acryloyloxyalkyloxy group, or a methacryloyloxyalkyloxy group; k is an integer from 0 to 1,000; m is an integer from 0 to 20; a and b are each independently an integer from 0 to 3; and a+b+m is an integer of 3 or greater. The siloxane units in the parentheses followed by k and m may be arranged in any order. (A-ii) An organopolysiloxane A represented by the following formula (2) and having a number average molecular weight (Mn) of 3,000 to 100,000: p (R 1 3SiO 1 / 2 ) q (SiO 4 / 2 ) r (2) (wherein, R 1 represents the same meaning as above, A is a siloxane unit represented by the following formula (3), and p, q, and r are numbers that satisfy p>0, q>0, and r>0, and p+q+r=1, respectively. (In the formula, R 1 , R 2 and R 3 represents the same meaning as above, n represents an integer of 0 to 10, and c represents an integer of 1 to 3.
3. The photo- and heat-curable silicone composition according to claim 1, wherein the component (B) is the following (B-iii), (B-iv), or both: (B-iii) A linear organopolysiloxane R represented by the following formula (4) and having a viscosity at 23°C of 50 to 10,000,000 mPa·s: 4 R 1 2Si (OSiR 1 2) S OSiR 1 2nd Race 4 (4) (wherein, R 1 has the same meaning as above, and R 4 represents an alkenyl group having 2 to 20 carbon atoms, and s represents an integer of 1 to 10,000. (B-iv) Organopolysiloxanes represented by the following formula (5): 1 3SiO 1 / 2 ) t (R 4 R 1 2SiO 1 / 2 ) u (SiO 4 / 2 ) v (5) (wherein, R 1 and R 4 has the same meaning as above, and t, u, and v are numbers that satisfy t>0, u>0, v>0, and (t+u+v)=1.
4. The photo- and heat-curable silicone composition according to claim 1, wherein component (C) is a linear organohydrogenpolysiloxane represented by the following formula (7): (R 1 3SiO 1 / 2 ) w (H (3-f) R 1 f SiO 1 / 2 ) 2-w (HR 1 1SiO 2 / 2 ) x (R 1 2SiO 2 / 2 ) y (7) (wherein, R 1 represents the same meaning as above, f represents 1 or 2, w represents an integer satisfying 0≦w≦2, and x and y represent positive integers satisfying 2≦x+y≦800 and 0.6≦x / (x+y+2)≦1.
0.
5. The photo- and heat-curable silicone composition according to claim 1, wherein component (D) is a photoradical polymerization initiator that does not contain nitrogen, sulfur, or phosphorus atoms.
6. A method for producing a cured product comprising the steps of: (α) irradiating the photo- and heat-curable silicone composition according to any one of claims 1 to 5 with ultraviolet light to partially cure the composition and turn it into a semi-cured composition; and (β) heating the resulting semi-cured composition to completely cure it.