Cut-and-processed product, and guardrail
Patent Information
- Application Number
- MYPI2025001559
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-29
- Filing Date
- 2023-09-19
- Publication Date
- 2024-03-29
AI Technical Summary
Conventional methods for improving corrosion resistance of cut ends in plated steel products, such as using Zn-based metal powders, often result in cathode peeling of the repair coating, leading to inadequate protection against red rust, especially in the early stages of corrosion.
A cut product made from Zn-Al-Mg-based plated steel with a linear coating of the Zn-Al-Mg-based plating layer covering 60-90% of the cut end surface, combined with a repair coating containing Zn-based metal powder and a binder resin, providing an initial coating resistance of 10-1000 Ω/cm and a resistance of 5-50 Ω/cm after immersion in salt water, which suppresses cathode peeling and maintains corrosion resistance over the long term.
The solution effectively prevents cathode peeling and maintains excellent corrosion resistance from the initial stage to long-term exposure, ensuring the cut end surface remains protected against red rust.
Smart Images

Figure PI2025001559_DRAWING_001 
Figure PI2025001559_DRAWING_002
Abstract
Description
Cutting products and guardrails
[0001] The present disclosure relates to cutting workpieces and guardrails.
[0002] When plated steel is processed into a product shape, it is cut, and part of the cut cross section exposes the steel base material. Since the cut edge not covered with the plated layer has reduced corrosion resistance, it is necessary to improve the corrosion resistance of the cut edge.
[0003] Various methods and technologies have been investigated to improve the corrosion resistance of cut end surfaces of plated steel products. For example, known rust prevention processing technologies for cut end surfaces include the inclined end surface method (Patent Document 1, etc.), the slit method (Patent Document 2, etc.), and the laser cutting method (Patent Document 3, etc.), which cover a larger portion of the end surface cross section with a plating layer than the cross section of the end surface obtained by conventional shearing. However, it is difficult to cover the entire surface of the cut cross section with a plating layer, and there are problems such as the occurrence of red rust on the partially exposed cut end surface during early exposure.
[0004] Therefore, a conventional anticorrosion technique for cut edges is to generally apply a repair paint containing Zn-based metal powder (see, for example, Patent Document 4) to the exposed steel surface of the cut edge.
[0005] JP 2020-32437 A JP 2017-192989 A JP 2021-087988 A JP 2017-122186 A
[0006] It was hoped that by combining the above-mentioned anti-rust processing technology for cut edges with repair painting, it would be possible to impart even greater corrosion resistance to cut edges.
[0007] However, at the cut end surface, the area of the steel substrate, which acts as the cathode, is significantly smaller than the plating layer, which acts as the anode, so the reduction reaction of water or oxygen is concentrated, causing cathodic peeling of the repair coating, making it impossible to maintain sufficient corrosion resistance, especially in terms of suppressing red rust in the early stages of corrosion.Furthermore, because of the cathodic peeling of the repair coating, the long-term corrosion resistance was not as good as expected.
[0008] Therefore, an object of the present disclosure is to provide a cut product that suppresses cathodic peeling of a repair coating film and has excellent corrosion resistance at the cut end surface from the beginning to the long term, and a guardrail that utilizes the cut product.
[0009] Means for solving the problems include the following aspects: <1> A cut product of a Zn-Al-Mg-plated steel material having a base steel material and a Zn-Al-Mg-plated layer coated on the surface of the base steel material, wherein a cut end surface of the cut product is coated with a linear coating in which components of the Zn-Al-Mg-plated layer have flowed in linearly, and the coverage of the linear coating with respect to the cut end surface is 60 to 90%, a non-plated surface of the base steel material and the linear coating around the non-plated surface at the cut end surface of the cut product are covered with a repair coating, and an initial coating resistance value R1 of the repair coating is 10 to 1000 Ω / cm 2 and the coating resistance value R2 after immersion of the cut product in 5 mass % salt water for 3 hours is 5 to 50 Ω / cm 2 and the repair coating has a thickness of 10 μm or more. <2> The cut product according to <1>, wherein the repair coating contains a Zn-based metal powder and a binder resin. <3> The cut product according to <1> or <2>, wherein the maximum length of the linear coating at the cut end surface of the cut product is 70 to 100% of the plate thickness of the cut product. <4> The initial coating resistance value R1 of the repair coating is 300 to 500 Ω / cm 2 <5> The cut product according to any one of <1> to <3>, wherein the coating resistance value R2 of the repair coating film after immersion is 10 to 45 Ω / cm 2The cut product according to any one of <1> to <4>, wherein the Zn-based metal powder contains Zn and Al. <6> The cut product according to <2>, wherein the Zn-based metal powder contains Zn and Al. <7> The cut product according to <6>, wherein the Al content relative to the Zn in the Zn-based metal powder containing Zn and Al is 20 to 45 mass%. <8> The cut product according to any one of <6>, wherein the Al content relative to the Zn in the Zn-based metal powder containing Zn and Al is 28 to 34 mass%. <9> The cut product according to any one of <2> or <6> to <8>, wherein the content of the Zn-based metal powder relative to the entire repair coating is 60 to 80 mass% of the metal powder. <10> The cut product according to <2> or any one of <6> to <9>, wherein the binder resin is at least one selected from the group consisting of polystyrene resin and epoxy resin. <11> A guardrail having the cut product according to any one of <1> to <10>.
[0010] According to the present disclosure, it is possible to provide a cut product that suppresses cathodic peeling of a repair coating film and has excellent corrosion resistance at the cut end surface from the beginning to the long term, and a guardrail that uses the cut product.
[0011] Fig. 1 is a schematic cross-sectional perspective view showing a cut product of the present disclosure. Fig. 2 is a schematic cross-sectional view of the cut product of the present disclosure, cut along a direction perpendicular to the cut end surface of the cut product and perpendicular to the plate thickness direction. Fig. 3 is a schematic perspective view showing the state of the cut end surface when cut by a conventional shearing method. Fig. 4 is a schematic view for explaining a sample for measuring coating film resistance value.
[0012] An example of a coated steel sheet according to the present disclosure will be described below. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the upper and lower limits. In a numerical range described in stages, the upper or lower limit described in a certain numerical range may be replaced with the upper or lower limit of another numerical range described in stages. In a numerical range, the upper or lower limit described in a certain numerical range may be replaced with a value shown in an example. The term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. A "combination of preferred embodiments" is a more preferred embodiment.
[0013] In this specification, the "Zn-Al-Mg-based plating layer" is also referred to as the "plating layer." The "Zn-Al-Mg-based plated steel material" is also referred to as the "plated steel material." The "non-plated surface" refers to the surface of the base steel material of the plated steel material that is not covered with the Zn-Al-Mg-based plating layer.
[0014] The cut product of the present disclosure is a cut product of a Zn-Al-Mg-plated steel material having a base steel material and a Zn-Al-Mg-plated layer coated on the surface of the base steel material. The cut end surface of the cut product is coated with a linear coating formed by the components of the Zn-Al-Mg-plated layer flowing in linearly, and the coverage rate of the linear coating with respect to the cut end surface is 60 to 90%. The non-plated surface of the base steel material and the linear coating around the non-plated surface at the cut end surface of the cut product are covered with a repair coating. The initial coating resistance of the repair coating is 10 to 1000 Ω / cm 2 and the coating resistance value after immersion in 5 mass % salt water for 3 hours (hereinafter also referred to as "coating resistance value after immersion in salt water") is 5 to 50 Ω / cm 2 The thickness of the repair coating is 10 μm or more.
[0015] In the cut product of the present disclosure, the cut end surface of the cut product is coated with a linear coating in which components of the Zn-Al-Mg-based plating layer have flowed in linearly, and the non-plated surface of the base steel is coated with a repair coating. The repair coating has the above-mentioned properties, which suppress cathodic peeling and inhibit a decrease in corrosion resistance in the early stages of corrosion. In addition, the sacrificial corrosion protection effects of the components of the Zn-Al-Mg-based plating layer and the repair coating maintain high corrosion resistance from the early stages of corrosion through to the long-term corrosion. Therefore, the cut product of the disclosure suppresses cathodic peeling of the repair coating and has excellent corrosion resistance of the cut end surface from the early stages through to the long term.
[0016] The cut product of the present disclosure will now be described in detail.
[0017] (Plated steel material) Plated steel material is a steel material that can be cut. Plated steel material is a Zn-Al-Mg-based plated steel material having a base steel material and a plating layer coated on the surface of the base steel material. Specifically, plated steel material preferably has a plating layer on both sides of the base steel material.
[0018] The base steel is a steel material on which a coating layer is to be formed. The base steel is not particularly limited. Examples of the base steel include steel sheets of ultra-low C type (a ferrite-based structure), Al-k type (a structure containing pearlite in ferrite), two-phase type (e.g., a structure containing martensite in ferrite, or a structure containing bainite in ferrite), deformation-induced transformation type (a structure containing retained austenite in ferrite), and fine crystal type (a ferrite-based structure).
[0019] The plating layer is a Zn-Al-Mg-based plating layer containing at least zinc, aluminum, and magnesium. The Zn-Al-Mg-based plating layer has higher corrosion resistance than a Zn plating layer or an Al plating layer due to the inclusion of Al and Mg. Examples of the plating layer include a zinc-aluminum-magnesium plating layer, as well as well-known Zn-Al-Mg-based plating layers such as a zinc-aluminum-magnesium-tin plating layer, a zinc-aluminum-magnesium-silicon plating layer, and a zinc-aluminum-magnesium-tin-silicon plating layer.
[0020] The plating layer may contain cobalt, molybdenum, tungsten, nickel, titanium, chromium, iron, magnesium, lead, bismuth, antimony, tin, copper, cadmium, arsenic, etc. as a different metal element or impurity.
[0021] In particular, from the viewpoint of corrosion resistance, the zinc-based plating layer is preferably a plating layer containing aluminum in addition to zinc, or a plating layer containing aluminum and magnesium. In other words, using a zinc alloy-plated steel sheet as the base sheet is preferable because it provides better corrosion resistance than a zinc-plated steel sheet. Specifically, the plating layer can be, for example, a plating layer containing, by mass, 65.0% Zn, 5.0% to 25.0% Al, and 2.0% to 12.5% Mg. More specifically, the plating layer has the following composition, in mass %, Zn: 65.0%, Al: 5.0% to 25.0%, Mg: 2.0% to 12.5%, Sn: 0% to 20.0%, Bi: 0% to 5.0%, In: 0% to 2.0%, Ca: 0% to 3.00%, Y: 0% to 0.5%, La: 0% to 0.5%, Ce: 0% to 0.5%, Si: 0% to 2.5%, Cr: 0% to 0.25%, Ti: 0% to 0.25%, Zr: 0% to 0.25%, Mo: 0% to 0.25%, W: 0% to 0.25%, Ag: 0% to 0.25%, P: 0% to 0.25%, An example of a plating layer having a chemical composition consisting of Ni: 0% to 0.25%, Co: 0% to 0.25%, V: 0% to 0.25%, Nb: 0% to 0.25%, Cu: 0% to 0.25%, Mn: 0% to 0.25%, Li: 0% to 0.25%, Na: 0% to 0.25%, K: 0% to 0.25%, Fe: 0% to 5.0%, Sr: 0% to 0.5%, Sb: 0% to 0.5%, Pb: 0% to 0.5%, B: 0% to 0.5%, and impurities.
[0022] The method for forming the plating layer is not particularly limited, and any of the known methods such as electroplating, hot dip plating, vapor deposition plating, dispersion plating, and vacuum plating may be used.
[0023] The coating weight of the plating layer is not particularly limited, but is preferably 15 g m -2 140g・m or more-2 It is preferable that the weight is 30 g m or less. -2 90g・m or more -2 The coating weight of the plating layer is 15 g m or less. -2 When the coating weight is 140 g m or more, the occurrence of unplated areas due to an excessively small coating weight is suppressed. -2 When the content is less than this, the corrosion resistance is high and the phenomenon of the plating layer turning black is suppressed.
[0024] (Cut end surface of cut product) - Linear coating - The cut end surface of the cut product according to the present disclosure is covered with a linear coating formed by components of the Zn-Al-Mg-based plating layer flowing in linearly. The line width of the linear coating is, for example, about 10 to 100 μm.
[0025] For example, when plated steel is cut using a laser cutting method, the plating layer formed on the surface of the base steel near the cut is melted by the heat of the laser. The components of the molten plating layer flow into the cut edge in a trickle and resolidify. As a result, the cut edge is covered with a linear film containing the components of the plating layer (see Figure 1). On the other hand, when plated steel is cut using a conventional shearing method, the plating layer formed on the surface of the base steel near the cut follows the shearing blade and penetrates into the cut edge. As a result, the cut edge is covered with a strip-shaped plating layer (see Figure 3). In Figure 1, 101 denotes the cut product, 101C denotes the cut edge, 10 denotes the plated steel, 12 denotes the base steel, 14 denotes the plating layer, 16 denotes the linear film, and 18 denotes the repair coating. In FIG. 3, 201 denotes a cut product, 201C denotes a cut end surface, 20 denotes a plated steel material, 22 denotes a base steel material, 24 denotes a plated layer, and CD denotes a cutting direction.
[0026] - Coverage of linear coating - The coverage of the linear coating on the cut end surface is 60 to 90%. If the coverage of the linear coating is less than 60%, the coverage of the linear coating on the cut end surface is too low, resulting in reduced corrosion resistance. On the other hand, when plated steel is cut, the plating layer on the surface of the plated steel melts in part of the cut end surface, and the components of the molten plating layer flow into the cut end surface. However, it is difficult to cause the components of the molten plating layer to flow over the entire cut end surface. Therefore, the coverage of the linear coating is set to the above range. The coverage of the plating layer is preferably 70 to 90%.
[0027] The coverage of the linear coating is measured as follows. The cut end surface of the cut-processed part to be measured is immersed in a solvent that dissolves the repair coating (i.e., the binder resin) and then cleaned in an ultrasonic cleaner for at least one minute to completely remove the repair coating. Next, a sample is prepared by depositing gold on the cut end surface to a thickness of approximately 10 nm. The element distributions of Zn, Al, and Mg are measured from the direction perpendicular to the thickness of the cut end surface of the sample using an electron probe microanalyzer (EPMA) in the base steel, plating layer, carbon, and oxygen. The coverage of the linear coating is then calculated as the percentage of the area where Zn, Al, or Mg is detected relative to the cut cross section. Here, in measuring the element distribution of the components of the coating layer using EPMA, the components of the coating layer are distinguished from the components of the base steel by determining whether any of the coating components, Zn, Al, and Mg, is present at 1 atm% or more by EPMA quantitative analysis. The area where it is confirmed that any of the coating components, Zn, Al, and Mg, is present at 1 atm% or more by EPMA quantitative analysis is considered to be the area covered by the linear coating. This operation is performed three times, and the average value is calculated. The EPMA measurement conditions are: measurement area = cross-section width (i.e., sheet thickness) x 10 mm, acceleration voltage = 25 kV, and electron beam diameter = 10 μm.
[0028] - Maximum length of linear coating - The maximum length of the linear coating is preferably 70 to 100% of the thickness of the cut product. When the maximum length of the linear coating is 70% or more, there is no bias toward one end of the cut end surface in the thickness direction, and the cut end surface is covered with the linear coating from one end to the other end in the thickness direction of the cut end surface. This makes it easier to improve corrosion resistance. Therefore, the maximum length of the linear coating is preferably in the above range. The maximum length of the linear coating is more preferably 90 to 100%.
[0029] The maximum length of the linear coating is measured as follows. The cut end surface of the cut-processed part to be measured is immersed in a solvent that dissolves the repair coating (i.e., the binder resin) and then cleaned in an ultrasonic cleaner for at least one minute to completely remove the repair coating. Next, gold is vapor-deposited on the cut end surface to a thickness of approximately 10 nm to prepare a sample using the cut end surface as the observation surface. The element distribution of Zn, Al, and Mg, among the components of the plating layer, is measured on the observation surface of the sample using an electron probe microanalyzer (EPMA). Then, the length of the longest linear region in which any of Zn, Al, and Mg is detected is measured. The length of the linear region is defined as the length along the thickness direction of the sample (see T in Figure 1). The ratio of the length of the longest linear region to the sample thickness is then calculated. This procedure is performed three times, and the average value is calculated. Except for the above, the method for measuring the maximum length of the linear coating is the same as the method for measuring the coverage rate of the linear coating.
[0030] -Repair Coating- At the cut end surface of the cut product according to the present disclosure, the non-plated surface of the base steel and the linear coating around the non-plated surface are coated with a repair coating (see Figures 1 and 2). Specifically, for example, the repair coating may be applied to the non-plated surface of the base steel and the linear coating up to at least 100 μm from the edge of the linear coating (i.e., the boundary between the non-plated surface of the base steel and the linear coating). Preferably, the repair coating is applied so as to cover the entire cut end surface. Note that Figure 2 is a schematic cross-sectional view of the cut product cut along a direction perpendicular to the cut end surface and perpendicular to the thickness direction of the cut product. In Figure 2, 101C denotes the cut end surface of the cut product, 12 denotes the base steel of the plated steel, 16 denotes the linear coating, and 18 denotes the repair coating.
[0031] The formation state of the repair coating is confirmed as follows: The cut-processed part to be measured is cut along a direction perpendicular to the cut end surface and perpendicular to the plate thickness direction. Next, the steel plate to be measured is embedded in an embedding resin mixed with an embedding hardener at a predetermined ratio, and the embedded sample is mechanically polished to expose the cut surface of the cut-processed part, creating a specimen with the cut surface as the observation surface. The observation surface of the sample is observed at a magnification of 50 to 100 using a scanning electron microscope (SEM) equipped with an energy dispersive X-ray spectrometer (EDS). The elemental distributions of Zn, Al, and Mg, among the components of the plating layer, are also measured. The edge of the linear coating is then determined based on the area where Zn, Al, or Mg is detected. The distance between the edge of the linear coating and the edge of the repair coating is then determined from the SEM image. Note that the distance between the edge of the linear coating and the edge of the repair coating is the distance along the surface of the linear coating. This procedure allows the formation of the repair coating to be confirmed. The EDS measurement conditions are: measurement area = cross-section width (i.e., plate thickness) x cutting direction 200 μm, acceleration voltage = 15 V, and electron beam diameter = 10 μm.
[0032] --Composition of Repair Coating-- The repair coating contains a component that has a sacrificial anticorrosion effect. Specifically, the repair coating preferably contains a zinc-based metal powder and a binder resin. The repair coating may also contain other additives as needed.
[0033] The Zn-based metal powder is a metal powder containing Zn. The Zn-based metal powder may be a metal powder containing Zn alone, or may be a metal powder containing Zn and a metal other than Zn. The metal powder containing Zn and a metal other than Zn may be a mixed metal powder of a metal powder containing Zn alone and a metal powder containing a metal other than Zn alone, or may be an alloy metal powder containing Zn and a metal other than Zn.
[0034] Examples of metals other than Zn include Al, Si, Mg, Co, Ti, V, Cr, Mn, Fe, Co, Ni, stainless steel, etc. Among these, Al is preferred as the metal other than Zn. In other words, it is preferred that the Zn-based metal powder contains Zn and Al. When Al is contained in the metal powder, Zn and Al have excellent corrosion resistance against the steel sheet substrate. 6 Al 2 (OH) 16 CO 3 ・4H 2 O is more likely to be generated, improving corrosion resistance.
[0035] Here, in the Zn-based metal powder containing Zn and Al, the Al content relative to Zn is preferably 20 to 45 mass%, more preferably 25 to 35 mass%, and particularly preferably 28 to 34 mass%. When the Al content is 20 mass% or more, excessive decreases in the coating film resistance values R1 and R2 initially and after saltwater immersion are suppressed, improving corrosion resistance. When the Al content is 45 mass% or less, excessive increases in the coating film resistance value R2 after saltwater immersion are suppressed, making cathodic peeling of the repair coating less likely to occur. In the Zn-based metal powder containing Zn and Al, the total content of Zn and Al relative to the Zn-based metal powder is preferably 90 mass% or more, more preferably 95 mass% or more, and particularly preferably 100 mass%. In other words, the total content of metals other than Zn and Al (especially the V content) is preferably 10 mass% or less, more preferably 5 mass% or less, and particularly preferably 0 mass% relative to the Zn-based metal powder.
[0036] The average particle size of the Zn-based metal powder is preferably 1 to 20 μm, and more preferably 1 to 10 μm. When the average particle size of the Zn-based metal powder is within the above range, corrosion resistance is improved. The "average particle size" is the particle size that is 50% cumulative from the smallest diameter side in the number-based particle size distribution determined by dynamic light scattering. The particle size of the Zn-based metal powder is measured by dissolving the repair coating (i.e., the binder resin) in a solvent, recovering the Zn-based metal powder by centrifugation, and measuring the particle size.
[0037] The content of the Zn-based metal powder is preferably 60 to 80 mass % of the entire repair coating, and more preferably 65 to 75 mass %. When the content of the Zn-based metal powder is 60 mass % or more, excessive increases in the coating resistance value at the initial stage and after immersion in salt water are suppressed, and cathodic peeling of the repair coating becomes less likely to occur. When the content of the Zn-based metal powder is 80 mass % or less, excessive decreases in the coating resistance value at the initial stage and after immersion in salt water are suppressed, and corrosion resistance is improved. Therefore, the content of the Zn-based metal powder is preferably in the above range.
[0038] Examples of binder resins include well-known resins such as polystyrene resin, polyester resin, epoxy resin, urethane resin, polyolefin resin, acrylic resin, and phenol resin. Among these, the binder resin is preferably at least one selected from the group consisting of polystyrene resin and epoxy resin. Use of these resins makes it easy to control the coating film resistance value after saltwater immersion within a preferred range, and facilitates improving corrosion resistance.
[0039] The binder resin may be a crosslinked resin or a non-crosslinked resin, but a crosslinked resin is preferred from the viewpoint of improving corrosion resistance. As a crosslinking agent for forming the crosslinked resin, well-known crosslinking agents such as melamine, isocyanate, silane compounds, zirconium compounds, and titanium compounds can be used depending on the type of resin to be crosslinked.
[0040] The content of the binder resin is preferably 20 to 40% by mass, more preferably 25 to 35% by mass, of the repair coating film. When the content of the binder resin is 20% by mass or more, excessive decreases in the coating film resistance value at the initial stage and after immersion in salt water are suppressed, and corrosion resistance is improved. When the content of the binder resin is 40% by mass or less, excessive increases in the coating film resistance value at the initial stage and after immersion in salt water are suppressed, and cathodic peeling of the repair coating film is less likely to occur. Therefore, the content of the binder resin is preferably within the above range.
[0041] Other additives in the repair coating include pigments (MgO, Al 2 O 3、 Examples of suitable additives include precipitated barium sulfate, barium carbonate, calcium carbonate, carbon, magnesium carbonate, etc.), dispersants, antifoaming agents, preservatives, thickeners, and film-forming aids.
[0042] --Film Thickness of Repair Coating-- If the thickness of the repair coating is too low, corrosion resistance will decrease. There is no particular upper limit to the repair coating thickness, but if the thickness is too thick, not only will the coating cost per cut end surface increase, but the drying time after application of the repair paint will also increase. Therefore, the thickness of the repair coating is 10 μm or more. The thickness of the repair coating is preferably 10 to 100 μm, and more preferably 20 to 30 μm.
[0043] The thickness of the repair coating is measured as follows: The cut-processed part to be measured is cut along a direction perpendicular to the cut end surface and perpendicular to the plate thickness direction. Next, the cut-processed part to be measured is embedded in an embedding resin mixed with an embedding hardener in a predetermined ratio, and the embedded sample is mechanically polished to expose the cut surface of the cut-processed part, preparing a specimen with the surface perpendicular to the cut end surface as the observation surface. The observation surface of the sample is observed using a scanning electron microscope (SEM) at a magnification of 50 to 100, and the thickness of the repair coating formed at any location on the non-plated surface of the base steel is measured. This thickness measurement is performed on three embedded samples, and the average of the three measurements is calculated.
[0044] --Repaired coating film resistance value-- The initial coating film resistance value R1 of the repaired coating film is 10 Ω / cm 2 If the initial resistance value R1 of the repair coating is less than 1000 Ω / cm, the metal powder in the repair coating will gradually oxidize, and the sacrificial corrosion protection property of the repair coating will be deactivated early, resulting in a decrease in corrosion resistance. 2 If the resistance is higher than this, the sacrificial corrosion protection of the repair coating film will not work at all, and red rust or the like may occur on the steel substrate under the repair coating film due to the influence of water in the atmosphere, etc., and the corrosion resistance will decrease. Therefore, the initial coating resistance value R1 of the repair coating film should be 10 to 1000 Ω / cm 2 The initial coating resistance value R1 of the repair coating film indicates the coating resistance value when the proportion of uncorroded metal particles in the total amount of metal particles in the repair coating film is 80% or more. If the proportion of uncorroded metal particles in the total amount of metal particles in the repair coating film is 80% or more, the coating resistance value R1 in this state is 10 to 1000 Ω / cm 2 From the above viewpoint, the initial coating resistance value R1 is 300 to 500 Ω / cm 2 is preferred.
[0045] Here, the initial coating resistance value R1 refers to the coating resistance value when the cut product is stored in a non-corrosive environment and when it is used in a corrosive environment, provided that the proportion of uncorroded metal powder in the total amount of metal powder in the coating is 80% or more. Specifically, the coating resistance value of the repair coating of a cut product that has been stored in a non-corrosive environment from the time the cut product is produced until the cut product is put to use (for example, until the cut product is installed as a guardrail beam) corresponds to the "initial coating resistance value R1." Furthermore, the coating resistance value of the repair coating of a cut product that has been used in a corrosive environment as a guardrail beam also corresponds to the "initial coating resistance value R1" provided that the proportion of uncorroded metal powder in the total amount of metal powder in the repair coating is 80% or more.
[0046] The corrosion rate of the total amount of metal powder is the sum of the oxidation rate and hydroxide rate of the metal powder. The method for measuring the corrosion rate of metal powder is to analyze the cross-sectional image of the repair coating film. Specifically, it is as follows.
[0047] The central area of the cut end surface of the cut-processed part to be measured, excluding a 10 mm range from the edge of the repair coating, is cut along a direction perpendicular to the cut end surface and parallel to the plate thickness direction. The cut-processed part to be measured is then embedded in an embedding resin mixed with an embedding hardener at a predetermined ratio, and the embedded sample is mechanically polished to expose the cut surface between the cut-processed part and the repair coating. A specimen is then prepared, with the observation surface being a surface perpendicular to the cut end surface. The observation surface of the specimen is then subjected to mapping analysis using a scanning electron microscope (SEM) equipped with energy dispersive x-ray spectroscopy (EDS). The observation magnification is set so that the entire repair coating can be observed in the film thickness direction from the interface between the repair coating and the base steel to the coating surface, and the interface between the repair coating and the base steel can be observed at a depth of 100 μm or more. This field observation is performed at three locations per embedded sample, for a total of nine locations per three embedded samples, and the corrosion rate of the metal powder in each field is calculated. The corrosion rate (%) of the metal powder is calculated by "(number of corroded metal powders / total number of metal powders) x 100" in the field of view. Corroded metal powder can be identified by mapping analysis using an SEM equipped with EDS, where the detection positions of metal elements such as Zn and oxygen coincide. However, this corroded metal powder contains MgO, Al, etc., which were originally added to the paint in an oxidized state. 2 O 3 The percentage of the corroded metal powder excluding these additives is calculated as follows: First, the corrosion rate of the metal powder is calculated by visual observation, and then the additives (MgO, Al) added to the raw material paint are calculated. 2 O 3 Specifically, the corrosion rate (%) of the metal particles obtained by visual observation is subtracted from the MgO, Al, etc., ratio of the total metal particles contained in the paint material. 2 O 3The additive percentages (%) that were added from the beginning are subtracted. In other words, the corrosion percentage (%) of metal powder is calculated by "(number of corroded metal powder particles - number of additives) / total number of metal powder particles x 100" in the visual field. In this way, the additive percentage measurements are subtracted from the corrosion percentage measurements in the nine visual fields mentioned above, and the average value of the obtained percentages is calculated. The value obtained by subtracting the average percentage (%) obtained from 100% (= 100 - average percentage obtained) is the "non-corroded percentage of the total amount of metal powder in the repair coating." Note that MgO, Al, etc., which are contained in the paint in an oxidized state, are also included. 2 O 3 For additives such as these, it is possible to distinguish them from corroded metal powder by calculating the increase in oxides in the repair coating from the oxides derived from the additives in the paint.
[0048] On the other hand, the coating resistance value R2 of the repair coating after immersion in salt water was 5 Ω / cm 2 If the resistance value R2 of the repair coating film after immersion in salt water is less than 50 Ω / cm, the metal powder in the repair coating film will be rapidly consumed in a corrosive environment, and the sacrificial corrosion protection properties of the repair coating film will be quickly deactivated, resulting in a decrease in corrosion resistance. 2 If it is higher, the reduction reaction of oxygen in a corrosive environment will be concentrated in the exposed steel substrate directly below the repair coating, and the resulting basic environment will make it difficult for intermolecular forces such as hydrogen bonds to work, causing cathodic peeling of the repair coating and ultimately reducing corrosion resistance. The coating resistance value R2 after immersion in salt water is 10 to 45 Ω / cm 2 is preferable, and 25 to 40 Ω / cm 2 is more preferable.
[0049] Here, the coating film resistance value after saltwater immersion of the repair coating film is the coating film resistance value after immersing the cut product in 5% by mass saltwater for 3 hours. More specifically, it is the coating film resistance value after immersing at least the cut end surface of the cut product in 5% by mass saltwater at a liquid temperature of 25°C for 3 hours.
[0050] The initial resistance value of the repair coating film and the resistance value after immersion in salt water can be adjusted by, for example, the thickness of the repair coating film and the type and amount of metal powder.
[0051] The coating resistance value is measured as follows. The cut product to be measured is cut into 10 mm square pieces to obtain a cut piece having a cut end surface on which a repair coating film is formed. The cut end surface of the obtained cut piece is used as the measurement surface, and a conductor is connected to the portion other than the measurement surface by spot welding, soldering, or other means that does not interfere with electrical continuity. A certain area of the cut end surface to be measured is exposed, and the remaining portion is insulated and sealed to obtain a sample of the repair coating film (see Figure 4). The coating resistance value is measured by measuring the AC impedance of the repair coating film on the exposed cut end surface of the obtained sample. This operation is performed twice, and the average coating resistance value is calculated. In Figure 4, 400 denotes the sample, 402 denotes the cut piece of the cut product, 404 denotes the conductor, 404A denotes the conductor connection portion, 406 denotes the insulating seal, and 408 denotes the repair coating film on the exposed cut end surface.
[0052] (Uses of Cut Products) The cut products of the present disclosure are applicable to uses such as steel sheets used for guardrails (specifically, guardrail components, especially guardrail beams), shaped steel for greenhouses or agricultural greenhouses, posts, beams, sound insulation walls, soundproof walls, electrical equipment components, environmental safety components, structural components, solar mounting frames, etc. The cut products of the present disclosure are obtained by cutting plated steel material and then subjecting it to processing such as press forming depending on the above-mentioned use, and then using the resulting product.
[0053] The present disclosure will be described in more detail below with reference to examples, although the present disclosure is not limited to these examples.
[0054] (Preparation of Plated Steel Sheet) Plated steel materials of the following steel type were prepared: Zn-6%Al-3%Mg: Zn-Al-Mg-based plated steel sheet (sheet thickness = 4.5 mm, coating composition = Al: 6 mass %, Mg: 3 mass %, balance: Zn, coating weight on one side = 120 g / m 2 ) Zn-11%Al-3%Mg: Zn-Al-Mg-based plated steel sheet (sheet thickness = 4.5 mm, coating composition = Al: 11 mass%, Mg: 3 mass%, balance: Zn, coating weight on one side = 120 g / m 2 ) Zn-19%Al-6%Mg: Zn-Al-Mg-based plated steel sheet (sheet thickness = 4.5 mm, coating composition = Al: 19 mass%, Mg: 6 mass%, balance: Zn, coating weight on one side = 120 g / m2 ) Zn: hot-dip galvanized steel sheet (sheet thickness = 4.5 mm, one-side coating weight = 120 g / m 2 )
[0055] (Repair Paint) A repair paint having the composition shown in Table 1 was prepared.
[0056] (Example) According to the conditions in Table 2, plated steel sheets were cut by laser cutting or a conventional shearing method to obtain samples having the cut end surfaces shown in Figures 1 and 3. In the laser cutting method, the gas flow rate and gas pressure ejected from the laser nozzle were adjusted to obtain the linear coating coverage and maximum length of the linear coating on the cut end surface as shown in Table 2. In the shearing method, the clearance between the shear blade and the die was adjusted to obtain the plating layer coverage on the cut end surface as shown in Table 2. Next, according to the conditions in Table 2, repair paint was applied to the non-plated surface of the base steel material of the plated steel sheet and the linear coating or plating layer around the non-plated surface of the cut end surface of the sample to form a repair coating. The thickness of the repair coating was as shown in Table 2. The initial coating resistance value and the coating resistance value after immersion in salt water (i.e., the coating resistance value after immersion of the cut product in salt water of 100% by mass for 3 hours) were as shown in Table 2.
[0057] Through these operations, cut samples were obtained.
[0058] (Evaluation) The cut end surfaces of the obtained cut product samples were subjected to the following evaluations.
[0059] - Cathodic peeling resistance - A combined cyclic corrosion test conforming to CCT-JASO M609 was carried out for 30 cycles. Thereafter, tape ("Cellotape (registered trademark)" manufactured by Nichiban Co., Ltd.) was applied to the surface of the cut end face of the cut-processed sample where the repair coating film had been formed, and then peeled off. The peeled tape was then observed, and the ratio of the area of the repair coating film peeled off from the tape to the area of the repair coating film adhered to the tape (hereinafter referred to as "peeled area ratio") was calculated and evaluated according to the following criteria. Pass was indicated by "A" or "B". A: Peeled area ratio 0% B: Peeled area ratio over 0% to 5% D: Peeled area ratio over 5%
[0060] - Long-term corrosion resistance 1 - A combined cyclic corrosion test in accordance with CCT-JASO M609 was carried out for 120 cycles. The area of red rust on the cut end surface of the cut sample was measured and evaluated according to the following criteria. Passing grades were rated as "A" and "B". A: Red rust area rate 0% B: Red rust area rate over 0% to 5% C: Red rust area rate over 5% to 20% D: Red rust area rate over 20% B or higher is passing grade
[0061] - Long-term corrosion resistance 2 - A combined cyclic corrosion test based on CCT-JASO M609 was carried out for 180 cycles. The area of red rust on the cut end surface of the cut sample was measured and evaluated according to the following criteria. Passing grades were rated as "A" and "B". A: Red rust area rate 0% B: Red rust area rate over 0% to 20% D: Red rust area rate over 20% B or higher is passing grade
[0062]
[0063]
[0064] The above results show that the disclosed examples suppress cathodic peeling of the repair coating film compared to the comparative examples, and have excellent corrosion resistance of the cut end surface from the early stages to the long term.
[0065] The symbols are explained as follows: 10 Plated steel material 12 Base steel material 14 Plated layer 16 Linear coating 18 Repair coating 101 Cut product 101C Cut end surface
[0066] The disclosure of Japanese Patent Application No. 2022-157063 is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually indicated to be incorporated by reference.
Claims
1. A cut product of Zn-Al-Mg-plated steel material having a base steel material and a Zn-Al-Mg-plated layer coated on the surface of the base steel material, wherein the cut end surface of the cut product is coated with a linear film in which components of the Zn-Al-Mg-plated layer have flowed in linearly, and the coverage rate of the linear film with respect to the cut end surface is 60 to 90%, and the non-plated surface of the base steel material and the linear film around the non-plated surface at the cut end surface of the cut product are covered with a repair coating, and the initial coating resistance value R1 of the repair coating is 10 to 1000 Ω / cm 2 and the coating resistance value R2 after immersion of the cut product in 5 mass % salt water for 3 hours is 5 to 50 Ω / cm 2 The cut product, wherein the repair coating film has a thickness of 10 μm or more.
2. The cut product according to claim 1, wherein the repair coating contains zinc-based metal powder and a binder resin.
3. The cut product according to claim 1, wherein the maximum length of the linear coating on the cut end surface of the cut product is 70 to 100% of the plate thickness of the cut product.
4. The initial coating resistance value R1 of the repair coating is 300 to 500 Ω / cm 2 2. The cut product according to claim 1, wherein 5. The coating resistance value R2 of the repair coating after immersion is 25 to 40 Ω / cm 2 2. The cut product according to claim 1, wherein 6. The cut product according to claim 2, wherein the Zn-based metal powder contains Zn and Al.
7. The cut product according to claim 6, wherein the content of Al relative to Zn in the Zn-based metal powder containing Zn and Al is 20 to 45 mass %.
8. The cut product according to claim 6, wherein the content of Al relative to Zn in the Zn-based metal powder containing Zn and Al is 28 to 34 mass %.
9. The cut product according to claim 2, wherein the content of the Zn-based metal powder in the entire repair coating is 60 to 80 mass % of the metal powder.
10. The cut product according to claim 2, wherein the binder resin is at least one selected from the group consisting of polystyrene resin and epoxy resin.
11. A guardrail having the cut product according to any one of claims 1 to 10.