Cut-and-processed product, and guardrail
Patent Information
- Application Number
- MYPI2025001560
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-29
- Filing Date
- 2023-09-19
- Publication Date
- 2024-03-29
AI Technical Summary
Conventional methods for improving corrosion resistance of cut ends in plated steel products face challenges such as red rust occurrence and cathode peeling of repair coatings, leading to inadequate long-term corrosion protection.
A cut product made from Zn-Al-Mg-based plated steel with a Zn-Al-Mg-based plating layer covering 50-99% of the cut end surface, combined with a repair coating containing Zn-based metal powder and a binder resin, providing initial and long-term corrosion resistance by suppressing cathode peeling and enhancing sacrificial anticorrosion action.
The solution effectively prevents cathode peeling and maintains excellent corrosion resistance from the initial stage to the long term, ensuring the cut end surface remains protected against corrosion.
Smart Images

Figure PI2025001560_DRAWING_001 
Figure PI2025001560_DRAWING_002 
Figure PI2025001560_DRAWING_003
Abstract
Description
Cutting products and guardrails
[0001] The present disclosure relates to cutting workpieces and guardrails.
[0002] When plated steel is processed into a product shape, it is cut, and part of the cut cross section exposes the steel base material. Since the cut edge not covered with the plated layer has reduced corrosion resistance, it is necessary to improve the corrosion resistance of the cut edge.
[0003] Various methods and technologies have been investigated to improve the corrosion resistance of cut end surfaces of plated steel products. For example, known rust prevention processing technologies for cut end surfaces include the inclined end surface method (Patent Document 1, etc.), the slit method (Patent Document 2, etc.), and the laser cutting method (Patent Document 3, etc.), which cover a larger portion of the end surface cross section with a plating layer than the cross section of the end surface obtained by conventional shearing. However, it is difficult to cover the entire surface of the cut cross section with a plating layer, and there are problems such as the occurrence of red rust on the partially exposed cut end surface during early exposure.
[0004] Therefore, a conventional anticorrosion technique for cut edges is to generally apply a repair paint containing Zn-based metal powder (see, for example, Patent Document 4) to the exposed steel surface of the cut edge.
[0005] JP 2020-32437 A JP 2017-192989 A JP 2021-087988 A JP 2017-122186 A
[0006] It was hoped that by combining the above-mentioned anti-rust processing technology for cut edges with repair painting, it would be possible to impart even greater corrosion resistance to cut edges.
[0007] However, at the cut end surface, the area of the steel substrate, which acts as the cathode, is significantly smaller than the plating layer, which acts as the anode, so the reduction reaction of water or oxygen is concentrated, causing cathodic peeling of the repair coating, making it impossible to maintain sufficient corrosion resistance, especially in terms of suppressing red rust in the early stages of corrosion.Furthermore, because of the cathodic peeling of the repair coating, the long-term corrosion resistance was not as good as expected.
[0008] Therefore, an object of the present disclosure is to provide a cut product that suppresses cathodic peeling of a repair coating film and has excellent corrosion resistance at the cut end surface from the beginning to the long term, and a guardrail that utilizes the cut product.
[0009] Means for solving the problems include the following aspects: <1> A cut product of a Zn-Al-Mg-plated steel material having a base steel material and a Zn-Al-Mg-plated layer coated on the surface of the base steel material, wherein a cut end surface of the cut product is coated with the Zn-Al-Mg-plated layer at a coverage rate of 50 to 99% of the cut end surface, a non-plated surface of the base steel material and the Zn-Al-Mg-plated layer around the non-plated surface at the cut end surface of the cut product are coated with a repair coating film, and an initial coating resistance value R1 of the repair coating film is 10 to 1000 Ω / cm 2 and the coating resistance value R2 after immersion of the cut product in 5 mass % salt water for 3 hours is 5 to 50 Ω / cm 2<2> The cut product according to <1>, wherein the repair coating film has a thickness of 10 μm or more. <3> The cut product according to <1> or <2>, wherein a cut end surface of the cut product has: a first inclined surface including a first sagging surface continuous from a first surface of the cut product and a first shear surface continuous from the first sagging surface, and inclining from the first surface of the cut product toward the center in the plate thickness direction; a second inclined surface including a second sagging surface continuous from a second surface of the cut product and a second shear surface continuous from the second sagging surface, and inclining from the second surface of the cut product toward the center in the plate thickness direction; and a fracture surface formed between the first inclined surface and the second inclined surface, wherein at least a part of the base steel located on the first inclined surface and the second inclined surface of the cut end surface of the cut product is coated with the Zn-Al-Mg-based plating layer, and wherein an unplated surface of the base steel including the fracture surface and the Zn-Al-Mg-based plating layer around the unplated surface of the cut end surface of the cut product are coated with the repair coating film. <4> The cut product according to <1> or <2>, wherein the cut end surface of the cut product has: a side surface that includes a sagging surface continuing from a first surface of the cut product and a shear surface continuing from the sagging surface, and that is inclined along the plate thickness direction or from the first surface of the cut product toward the center; and a fracture surface that is continuing from the side surface and reaches a second surface of the cut product, wherein at least a portion of the base steel located on the side surface of the cut end surface of the cut product is coated with the Zn-Al-Mg-based plating layer, and wherein the non-plated surface of the base steel including the fracture surface and the Zn-Al-Mg-based plating layer around the non-plated surface of the cut end surface of the cut product are coated with the repair coating. <5> The cut product according to <1> or <2>, wherein the initial coating resistance value R1 of the repair coating is 300 to 500 Ω / cm 2 <6> The cut product according to any one of <1> to <4>, wherein the coating resistance value R2 of the repair coating film after immersion is 10 to 45 Ω / cm 2The cut product according to any one of <1> to <5>, wherein the Zn-based metal powder contains Zn and Al. <7> The cut product according to <2>, wherein the Zn-based metal powder contains Zn and Al. <8> The cut product according to <7>, wherein the Al content relative to the Zn in the Zn-based metal powder containing Zn and Al is 20 to 45 mass%. <9> The cut product according to <7>, wherein the Al content relative to the Zn in the Zn-based metal powder containing Zn and Al is 28 to 34 mass%. <10> The cut product according to <2>, <7>, <8>, or <9>, wherein the content ratio of the Zn-based metal powder to the entire repair coating is 60 to 80 mass% of the metal powder. <11> The cut product according to <2> or any one of <7> to <10>, wherein the binder resin is at least one selected from the group consisting of polystyrene resin and epoxy resin. <12> A guardrail having the cut product according to any one of <1> to <11>.
[0010] According to the present disclosure, it is possible to provide a cut product that suppresses cathodic peeling of a repair coating film and has excellent corrosion resistance at the cut end surface from the beginning to the long term, and a guardrail that uses the cut product.
[0011] FIG. 1 is a schematic cross-sectional view showing a cut product 101 according to a first embodiment of the present disclosure. FIG. 2 is a schematic view for explaining a method for manufacturing the cut product 101 according to the first embodiment of the present disclosure. FIG. 3 is a schematic cross-sectional view showing the cut product 101 according to a second embodiment of the present disclosure. FIG. 4 is a schematic view for explaining a method for manufacturing the cut product 101 according to the second embodiment of the present disclosure. FIG. 5 is a schematic cross-sectional view showing the cut product 101 according to a third embodiment of the present disclosure. FIG. 6 is a schematic view for explaining a method for manufacturing the cut product 101 according to the third embodiment of the present disclosure. FIG. 7 is a schematic view for explaining a sample for measuring a coating resistance value.
[0012] An example of a coated steel sheet according to the present disclosure will be described below. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the upper and lower limits. In a numerical range described in stages, the upper or lower limit described in a certain numerical range may be replaced with the upper or lower limit of another numerical range described in stages. In a numerical range, the upper or lower limit described in a certain numerical range may be replaced with a value shown in an example. The term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. A "combination of preferred embodiments" is a more preferred embodiment.
[0013] In this specification, the "Zn-Al-Mg-based plating layer" is also referred to as the "plating layer." The "Zn-Al-Mg-based plated steel material" is also referred to as the "plated steel material." The "non-plated surface" refers to the surface of the base steel material of the plated steel material that is not covered with the Zn-Al-Mg-based plating layer.
[0014] The cut product of the present disclosure is a cut product of a Zn-Al-Mg-plated steel material having a base steel material and a Zn-Al-Mg-plated layer coated on the surface of the base steel material. The cut end surface of the cut product is coated with the Zn-Al-Mg-plated layer at a coverage rate of 50 to 99% of the cut end surface, and the non-plated surface of the base steel material and the Zn-Al-Mg-plated layer around the non-plated surface at the cut end surface of the cut product are coated with a repair coating. The initial coating resistance of the repair coating is 10 to 1000 Ω / cm 2 and the coating resistance value after immersion in 5 mass % salt water for 3 hours (hereinafter also referred to as "coating resistance value after immersion in salt water") is 5 to 50 Ω / cm 2 The thickness of the repair coating is 10 μm or more.
[0015] In the cut product disclosed herein, 50 to 99% of the cut end surface of the cut product is covered with a Zn-Al-Mg-based plating layer, and the non-plated surface of the cut end surface and the plating layer surrounding the non-plated surface are covered with a repair coating having the above-mentioned resistance characteristics. This configuration suppresses cathodic peeling of the repair coating, thereby preventing a decrease in corrosion resistance in the early stages of corrosion. In addition, the sacrificial corrosion protection effects of the components of the Zn-Al-Mg-based plating layer and the components of the repair coating maintain high corrosion resistance from the early stages of corrosion through to the long-term corrosion. Therefore, the cut product disclosed herein suppresses cathodic peeling of the repair coating and exhibits excellent corrosion resistance of the cut end surface from the early stages through to the long term.
[0016] The cut product of the present disclosure will now be described in detail.
[0017] (Plated steel material) Plated steel material is a steel material that can be cut. Plated steel material is a Zn-Al-Mg-based plated steel material having a base steel material and a plating layer coated on the surface of the base steel material. Specifically, plated steel material preferably has a plating layer on both sides of the base steel material.
[0018] The base steel is a steel material on which a coating layer is to be formed. The base steel is not particularly limited. Examples of the base steel include steel sheets of ultra-low C type (a ferrite-based structure), Al-k type (a structure containing pearlite in ferrite), two-phase type (e.g., a structure containing martensite in ferrite, or a structure containing bainite in ferrite), deformation-induced transformation type (a structure containing retained austenite in ferrite), and fine crystal type (a ferrite-based structure).
[0019] The plating layer is a Zn—Al—Mg-based plating layer, which contains at least zinc, aluminum, and magnesium. Compared to a Zn plating layer or an Al plating layer, the Zn—Al—Mg-based plating layer has higher corrosion resistance due to the inclusion of Al and Mg. Examples of the plating layer include a zinc-aluminum-magnesium plating layer, as well as well-known Zn—Al—Mg-based plating layers such as a zinc-aluminum-magnesium-tin plating layer, a zinc-aluminum-magnesium-silicon plating layer, and a zinc-aluminum-magnesium-tin-silicon plating layer.
[0020] The plating layer may contain cobalt, molybdenum, tungsten, nickel, titanium, chromium, iron, magnesium, lead, bismuth, antimony, tin, copper, cadmium, arsenic, etc. as a different metal element or impurity.
[0021] In particular, from the viewpoint of corrosion resistance, the zinc-based plating layer is preferably a plating layer containing aluminum in addition to zinc, or a plating layer containing aluminum and magnesium. In other words, using a zinc alloy-plated steel sheet as the base sheet is preferable because it provides better corrosion resistance than a zinc-plated steel sheet. Specifically, the plating layer can be, for example, a plating layer containing, by mass, 65.0% Zn, 5.0% to 25.0% Al, and 2.0% to 12.5% Mg. More specifically, the plating layer has the following composition, in mass %, Zn: 65.0%, Al: 5.0% to 25.0%, Mg: 2.0% to 12.5%, Sn: 0% to 20.0%, Bi: 0% to 5.0%, In: 0% to 2.0%, Ca: 0% to 3.00%, Y: 0% to 0.5%, La: 0% to 0.5%, Ce: 0% to 0.5%, Si: 0% to 2.5%, Cr: 0% to 0.25%, Ti: 0% to 0.25%, Zr: 0% to 0.25%, Mo: 0% to 0.25%, W: 0% to 0.25%, Ag: 0% to 0.25%, P: 0% to 0.25%, An example of a plating layer having a chemical composition consisting of Ni: 0% to 0.25%, Co: 0% to 0.25%, V: 0% to 0.25%, Nb: 0% to 0.25%, Cu: 0% to 0.25%, Mn: 0% to 0.25%, Li: 0% to 0.25%, Na: 0% to 0.25%, K: 0% to 0.25%, Fe: 0% to 5.0%, Sr: 0% to 0.5%, Sb: 0% to 0.5%, Pb: 0% to 0.5%, B: 0% to 0.5%, and impurities.
[0022] The method for forming the plating layer is not particularly limited, and any of the known methods such as electroplating, hot dip plating, vapor deposition plating, dispersion plating, and vacuum plating may be used.
[0023] The coating weight of the plating layer is not particularly limited, but is preferably 15 g m -2140g・m or more -2 It is preferable that the weight is 30 g m or less. -2 90g・m or more -2 The coating weight of the plating layer is 15 g m or less. -2 When the coating weight is 140 g m or more, the occurrence of unplated areas due to an excessively small coating weight is suppressed. -2 When the content is less than this, the corrosion resistance is high and the phenomenon of the plating layer turning black is suppressed.
[0024] (Cut end surface of cut product) - Coverage of plating layer - A cut end surface of the cut product according to the present disclosure is partially covered with a Zn-Al-Mg-based plating layer. Compared to a Zn-plated layer or an Al-plated layer, the Zn-Al-Mg-based plating layer has high corrosion resistance due to the Al and Mg content, so that the cut end surface is also provided with high corrosion resistance.
[0025] The coverage of the plating layer on the cut end surface is 50 to 99%. If the coverage of the plating layer is less than 50%, the coverage of the plating layer on the cut end surface is too low, resulting in reduced corrosion resistance. On the other hand, when plated steel is cut, the plating layer on the surface of the plated steel will wrap around to the plating layer on the cut end surface in part of the cut end surface. However, it is difficult to make the plating layer wrap around the entire cut end surface. Therefore, the coverage of the plating layer is set to the above range. The coverage of the plating layer is preferably 70 to 99%, and more preferably 90 to 99%.
[0026] The coverage of the plating layer is measured as follows. The cut end surface of the cut-processed part to be measured is immersed in a solvent that dissolves the repair coating (i.e., binder resin) and then cleaned in an ultrasonic cleaner for at least one minute to completely remove the repair coating. Next, a sample is prepared by depositing gold on the cut end surface to a thickness of approximately 10 nm. The elemental distribution of Zn, Al, and Mg among the components of the plating layer is measured using an electron probe microanalyzer (EPMA) in a direction perpendicular to the plate thickness. The coverage of the plating layer is then determined as the proportion of the area in which Zn, Al, or Mg is detected relative to the cut cross section. Here, in measuring the elemental distribution of the components of the plating layer using EPMA, the components of the plating layer are distinguished from the components of the base steel by determining whether any of the plating components, Zn, Al, or Mg, is present at 1 atm% or more as determined by EPMA quantification. The area where the presence of any of the plating components Zn, Al, and Mg was confirmed to be 1 atm% or more by quantitative EPMA analysis was determined to be the area covered with the plating layer. This operation was performed three times, and the average value was calculated. The EPMA measurement conditions were as follows: measurement area = cross-section width (i.e., plate thickness) x 10 mm, acceleration voltage = 25 kV, and electron beam diameter = 10 μmφ.
[0027] - Repair coating film - At the cut end surface of the cut product according to the present disclosure, the non-plated surface of the base steel and the Zn-Al-Mg-based plating layer around the non-plated surface are coated with a repair coating film. Specifically, for example, the repair coating film may be coated on the non-plated surface of the base steel and on the plating layer to a depth of at least 100 μm from the edge of the plating layer (i.e., the boundary between the non-plated surface of the base steel and the plating layer). Preferably, the repair coating film is coated so as to cover the sagging surface and the entire cut end surface.
[0028] The formation state of the repair coating is confirmed as follows: The cut-processed part to be measured is cut along a direction perpendicular to the cut end surface and parallel to the plate thickness direction. Next, the steel plate to be measured is embedded in an embedding resin mixed with an embedding hardener at a predetermined ratio, and the embedded sample is mechanically polished to expose the cut surface of the cut-processed part, creating a specimen with the cut surface as the observation surface. The observation surface of the sample is observed at a magnification of 50 to 100 using a scanning electron microscope (SEM) equipped with an energy dispersive X-ray spectrometer (EDS). The elemental distributions of Zn, Al, and Mg, among the components of the plating layer, are also measured. The edge of the plating layer is then determined based on the area where Zn, Al, or Mg is detected. The distance between the edge of the plating layer and the edge of the repair coating is then determined from the SEM image. Note that the distance between the edge of the plating layer and the edge of the repair coating is the distance along the surface of the plating layer. This procedure allows the formation of the repair coating to be confirmed. The EDS measurement conditions are: measurement area = cross-section width (i.e., plate thickness) x cutting direction 200 μm, acceleration voltage = 15 V, and electron beam diameter = 10 μm.
[0029] --Composition of Repair Coating-- The repair coating contains a component that has a sacrificial anticorrosion effect. Specifically, the repair coating preferably contains a zinc-based metal powder and a binder resin. The repair coating may also contain other additives as needed.
[0030] The Zn-based metal powder is a metal powder containing Zn. The Zn-based metal powder may be a metal powder containing Zn alone, or may be a metal powder containing Zn and a metal other than Zn. The metal powder containing Zn and a metal other than Zn may be a mixed metal powder of a metal powder containing Zn alone and a metal powder containing a metal other than Zn alone, or may be an alloy metal powder containing Zn and a metal other than Zn.
[0031] Examples of metals other than Zn include Al, Si, Mg, Co, Ti, V, Cr, Mn, Fe, Co, Ni, stainless steel, etc. Among these, Al is preferred as the metal other than Zn. In other words, it is preferred that the Zn-based metal powder contains Zn and Al. When Al is contained in the metal powder, Zn and Al have excellent corrosion resistance against the base steel material. 6 Al 2 (OH) 16 CO 3 ・4H 2 O is more likely to be generated, improving corrosion resistance.
[0032] Here, in the Zn-based metal powder containing Zn and Al, the Al content relative to Zn is preferably 20 to 45% by mass, more preferably 25 to 35% by mass, and particularly preferably 28 to 34% by mass. An Al content of 20% by mass or more suppresses excessive decreases in the coating resistance values R1 and R2 initially and after saltwater immersion, improving corrosion resistance. An Al content of 45% by mass or less suppresses excessive increases in the coating resistance value R2 after saltwater immersion, making cathodic peeling of the repair coating less likely to occur. In the Zn-based metal powder containing Zn and Al, the total content of Zn and Al relative to the Zn-based metal powder is preferably 90% by mass or more, more preferably 95% by mass or more, and particularly preferably 100% by mass. In other words, the total content of metals other than Zn and Al (especially the V content) is preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably 0% by mass relative to the Zn-based metal powder.
[0033] The average particle size of the Zn-based metal powder is preferably 1 to 20 μm, and more preferably 1 to 10 μm. When the average particle size of the Zn-based metal powder is within the above range, the surface area of the Zn metal powder increases, making it easier for the sacrificial corrosion protection to work, thereby improving corrosion resistance. Note that the "average particle size" is the particle size that is 50% cumulative from the smallest diameter side in the number-based particle size distribution determined by dynamic light scattering. Note that the particle size of the Zn-based metal powder is measured by dissolving the repair coating (i.e., the binder resin) in a solvent, recovering the Zn-based metal powder by centrifugation, and measuring the particle size.
[0034] The content of the Zn-based metal powder is preferably 60 to 80 mass % of the entire repair coating, and more preferably 65 to 75 mass %. When the content of the Zn-based metal powder is 60 mass % or more, excessive increases in the coating resistance value at the initial stage and after immersion in salt water are suppressed, and cathodic peeling of the repair coating becomes less likely to occur. When the content of the Zn-based metal powder is 80 mass % or less, excessive decreases in the coating resistance value at the initial stage and after immersion in salt water are suppressed, and corrosion resistance is improved. Therefore, the content of the Zn-based metal powder is preferably in the above range.
[0035] Examples of binder resins include well-known resins such as polystyrene resin, polyester resin, epoxy resin, urethane resin, polyolefin resin, acrylic resin, and phenol resin. Among these, the binder resin is preferably at least one selected from the group consisting of polystyrene resin and epoxy resin. Use of these resins makes it easy to control the coating film resistance value after saltwater immersion within a preferred range, and facilitates improving corrosion resistance.
[0036] The binder resin may be a crosslinked resin or a non-crosslinked resin, but a crosslinked resin is preferred from the viewpoint of improving corrosion resistance. As a crosslinking agent for forming the crosslinked resin, well-known crosslinking agents such as melamine, isocyanate, silane compounds, zirconium compounds, and titanium compounds can be used depending on the type of resin to be crosslinked.
[0037] The content of the binder resin is preferably 20 to 40% by mass, more preferably 25 to 35% by mass, of the repair coating film. When the content of the binder resin is 20% by mass or more, excessive decreases in the coating film resistance value at the initial stage and after immersion in salt water are suppressed, and corrosion resistance is improved. When the content of the binder resin is 40% by mass or less, excessive increases in the coating film resistance value at the initial stage and after immersion in salt water are suppressed, and cathodic peeling of the repair coating film is less likely to occur. Therefore, the content of the binder resin is preferably within the above range.
[0038] Other additives in the repair coating include pigments (MgO, Al 2 O 3、Examples of suitable additives include precipitated barium sulfate, barium carbonate, calcium carbonate, carbon, magnesium carbonate, etc.), dispersants, antifoaming agents, preservatives, thickeners, and film-forming aids.
[0039] --Film Thickness of Repair Coating-- If the thickness of the repair coating is too low, corrosion resistance will decrease. There is no particular upper limit for the repair coating thickness, but if the thickness is too thick, not only will the coating cost per cut end surface increase, but the drying time after application of the repair paint will also increase. Therefore, the thickness of the repair coating is 10 μm or more. The thickness of the repair coating is preferably 10 to 100 μm, and more preferably 20 to 30 μm.
[0040] The thickness of the repair coating is measured as follows: The cut-processed part to be measured is cut along a direction perpendicular to the cut end surface and parallel to the plate thickness direction. Next, the cut-processed part to be measured is embedded in an embedding resin mixed with an embedding hardener at a predetermined ratio, and the embedded sample is mechanically polished to expose the cut surface of the cut-processed part, preparing a specimen with the surface perpendicular to the cut end surface as the observation surface. The observation surface of the sample is observed using a scanning electron microscope (SEM) at a magnification of 50 to 100, and the thickness of the repair coating formed at any location on the non-plated surface of the base steel is measured. This thickness measurement is performed on three embedded samples, and the average of the three measurements is calculated.
[0041] --Repaired coating film resistance value-- The initial coating film resistance value R1 of the repaired coating film is 10 Ω / cm 2 If the initial resistance value R1 of the repair coating is less than 1000 Ω / cm, the metal powder in the repair coating will gradually oxidize, and the sacrificial corrosion protection property of the repair coating will be deactivated early, resulting in a decrease in corrosion resistance. 2 If the resistance is higher than this, the sacrificial corrosion protection of the repair coating film will not work at all, and red rust or the like may occur on the steel substrate under the repair coating film due to the influence of water in the atmosphere, etc., and the corrosion resistance will decrease. Therefore, the initial coating film resistance value R1 should be 10 to 1000 Ω / cm 2The initial coating resistance value R1 of the repair coating film indicates the coating resistance value when the proportion of uncorroded metal particles in the total amount of metal particles in the repair coating film is 80% or more. If the proportion of uncorroded metal particles in the total amount of metal particles in the repair coating film is 80% or more, the coating resistance value R1 in this state is 10 to 1000 Ω / cm 2 From the above viewpoint, the initial coating resistance value R1 is 300 to 500 Ω / cm 2 is preferred.
[0042] Here, the initial coating resistance value R1 refers to the coating resistance value when the cut product is stored in a non-corrosive environment and when it is used in a corrosive environment, provided that the proportion of uncorroded metal powder in the total amount of metal powder in the coating is 80% or more. Specifically, the coating resistance value of the repair coating of a cut product that has been stored in a non-corrosive environment from the time the cut product is produced until the cut product is put to use (for example, until the cut product is installed as a guardrail beam) corresponds to the "initial coating resistance value R1." Furthermore, the coating resistance value of the repair coating of a cut product that has been used in a corrosive environment as a guardrail beam also corresponds to the "initial coating resistance value R1" provided that the proportion of uncorroded metal powder in the total amount of metal powder in the repair coating is 80% or more.
[0043] The corrosion rate of the total amount of metal powder is the sum of the oxidation rate and hydroxide rate of the metal powder. The method for measuring the corrosion rate of metal powder is to analyze the cross-sectional image of the repair coating film. Specifically, it is as follows.
[0044] The central area of the cut end surface of the cut-processed part to be measured, excluding a 10 mm range from the edge of the repair coating, is cut along a direction perpendicular to the cut end surface and parallel to the plate thickness direction. The cut-processed part to be measured is then embedded in an embedding resin mixed with an embedding hardener at a predetermined ratio, and the embedded sample is mechanically polished to expose the cut surface between the cut-processed part and the repair coating. A specimen is then prepared, with the observation surface being a surface perpendicular to the cut end surface. The observation surface of the specimen is then subjected to mapping analysis using a scanning electron microscope (SEM) equipped with energy dispersive x-ray spectroscopy (EDS). The observation magnification is set so that the entire repair coating can be observed in the film thickness direction from the interface between the repair coating and the base steel to the coating surface, and the interface between the repair coating and the base steel can be observed at a depth of 100 μm or more. This field observation is performed at three locations per embedded sample, for a total of nine locations per three embedded samples, and the corrosion rate of the metal powder in each field is calculated. The corrosion rate (%) of the metal powder is calculated by "(number of corroded metal powders / total number of metal powders) x 100" in the field of view. Corroded metal powder can be identified by mapping analysis using an SEM equipped with EDS, where the detection positions of metal elements such as Zn and oxygen coincide. However, this corroded metal powder contains MgO, Al, etc., which were originally added to the paint in an oxidized state. 2 O 3 The percentage of the corroded metal powder excluding these additives is calculated as follows: First, the corrosion rate of the metal powder is calculated by visual observation, and then the additives (MgO, Al) added to the raw material paint are calculated. 2 O 3 Specifically, the corrosion rate (%) of the metal particles obtained by visual observation is subtracted from the MgO, Al, etc., ratio of the total metal particles contained in the paint material. 2 O 3The additive percentages (%) that were added from the beginning are subtracted. In other words, the corrosion percentage (%) of metal powder is calculated by "(number of corroded metal powder particles - number of additives) / total number of metal powder particles x 100" in the visual field. In this way, the additive percentage measurements are subtracted from the corrosion percentage measurements in the nine visual fields mentioned above, and the average value of the obtained percentages is calculated. The value obtained by subtracting the average percentage (%) obtained from 100% (= 100 - average percentage obtained) is the "non-corroded percentage of the total amount of metal powder in the repair coating." Note that MgO, Al, etc., which are contained in the paint in an oxidized state, are also included. 2 O 3 For additives such as these, it is possible to distinguish them from corroded metal powder by calculating the increase in oxides in the repair coating from the oxides derived from the additives in the paint.
[0045] On the other hand, the coating resistance value R2 of the repair coating after immersion in salt water was 5 Ω / cm 2 If the resistance value R2 of the repair coating film after immersion in salt water is less than 50 Ω / cm, the metal powder in the repair coating film will be rapidly consumed in a corrosive environment, and the sacrificial corrosion protection properties of the repair coating film will be quickly deactivated, resulting in a decrease in corrosion resistance. 2 If the resistance value is higher than this, the reduction reaction of oxygen in a corrosive environment will be concentrated in the exposed steel substrate directly below the repair coating, and the resulting basic environment will make it difficult for intermolecular forces such as hydrogen bonds to function, resulting in cathodic peeling of the repair coating and ultimately a decrease in corrosion resistance. The resistance value R2 of the repair coating after immersion in salt water is 10 to 45 Ω / cm 2 is preferably 25 to 40 Ω / cm 2 is more preferred.
[0046] Here, the coating film resistance value after saltwater immersion of the repair coating film is the coating film resistance value after immersing the cut product in 5% by mass saltwater for 3 hours. More specifically, it is the coating film resistance value after immersing at least the cut end surface of the cut product in 5% by mass saltwater at a liquid temperature of 25°C for 3 hours.
[0047] The initial and post-saltwater immersion coating film resistance values R1 and R2 of the repair coating film can be adjusted, for example, by the film thickness of the repair coating film and the type and amount of metal powder.
[0048] The coating resistance value is measured as follows. The cut product to be measured is cut into 10 mm square pieces to obtain a cut piece having a cut end surface on which a repair coating film is formed. The cut end surface of the obtained cut piece is used as the measurement surface, and a conductor is connected to the portion other than the measurement surface by spot welding, soldering, or other means that does not interfere with electrical continuity. A certain area of the cut end surface to be measured is exposed, and the remaining portion is insulated and sealed to obtain a sample of the repair coating film (see Figure 7). The coating resistance value of the obtained sample is measured by measuring the AC impedance of the repair coating film at the exposed cut end surface. This operation is performed twice, and the average coating resistance value is calculated. In Figure 7, 400 denotes the sample, 402 denotes the cut piece of the cut product, 404 denotes the conductor, 404A denotes the conductor connection portion, 406 denotes the insulating seal, and 408 denotes the repair coating film at the exposed cut end surface.
[0049] (Specific Forms of Cut End Surface of Cut Product) As specific forms of the cut end surface of the cut product of the present disclosure, cut products according to first to third embodiments of the present disclosure will be described with reference to the drawings. In the following description, the "first surface and second surface of the cut product" refer to surfaces that face each other in the thickness direction. A "sagging surface" refers to a surface that is plastically deformed into a curved shape due to tensile stress acting on the surface of the plated steel material when the plated steel material is cut. A "shear surface" refers to a surface that is cut by shear force when the plated steel material is cut. A "fracture surface" refers to a surface that is formed when the plated steel material is fractured, originating from cracks that occur in the plated steel material during cutting. The "sagging surface," "shear surface," and "fracture surface" are continuous surfaces that constitute the cut end surface of the cut product.
[0050] 1 to 6, the plate length direction of the plated steel material is the X direction, the plate width direction is the Y direction, and the plate thickness direction is the Z direction. In Fig. 1 to 6, the same members or parts are denoted by the same reference numerals.
[0051] First Embodiment A cut end surface 101C of a cut product 101 according to a first embodiment of the present disclosure has a first inclined surface 102, a second inclined surface 104, and a fractured surface 106, as shown in FIG.
[0052] The first inclined surface 102 includes a first sagging surface 102A that continues from the first surface 101A of the cut product 101, and a first shearing surface 102B that continues from the first sagging surface 102A. The first inclined surface 102 is inclined in the thickness direction from the first surface 101A toward the center of the cut product 101. In other words, the first shearing surface 102B is a surface that has a predetermined inclination angle with respect to the thickness direction of the plated steel material 10.
[0053] The second inclined surface 104 includes a second sagging surface 104A continuing from the second surface 101B of the cut product 101, and a second shearing surface 104B continuing from the second sagging surface 104A. The second inclined surface 104 is inclined in the thickness direction from the second surface 101B of the cut product 101 toward the center. In other words, the second inclined surface 104 is a surface having a predetermined inclination angle with respect to the thickness direction of the plated steel material 10.
[0054] The fracture surface 106 is formed between the first inclined surface 102 and the second inclined surface 104. The fracture surface 106 is formed when the plated steel material 10 breaks when the plated steel material is cut. For this reason, the fracture surface 106 is difficult to be covered with the plating layer 14, and becomes a non-plated surface of the base steel material 12.
[0055] Of the cut end surface 101C of the cut product 101, at least a portion of the base steel material 12 located on the first inclined surface 102 and the second inclined surface 104 is coated with a plating layer 14. Specifically, the first inclined surface 102 is coated with a plating layer 14 that covers the base steel material 12 located on the first surface 101A when the plated steel material 10 is cut. The second inclined surface 104 is coated with a plating layer 14 that covers the base steel material located on the second surface 101B when the plated steel material 10 is cut. In other words, the first inclined surface 102 and the second inclined surface 104 are each coated with a plating layer 14 that is continuous with the plating layer 14 of the cut product 101.
[0056] The coverage rate of the plating layer 14 with respect to the cut end surface of the cut product 101 is adjusted by adjusting the area of the plating layer 14 that covers the base steel 12 located on the first inclined surface 102 and the second inclined surface 104. Note that the entire surface of the base steel 12 located on the first inclined surface 102 and the second inclined surface 104 may be covered with the plating layer 14.
[0057] On the other hand, of the cut end surface 101C of the cut product 101, the non-plated surface of the base steel material 12 including the fracture surface 106 and the plating layer 14 around the non-plated surface are covered with a repair coating film 16.
[0058] The cut product 101 can be manufactured, for example, by a cutting tool 121 shown in Fig. 2. As shown in Fig. 2, the cutting tool 121 has, when viewed from the plate width direction (Y direction), a punch 122 having a wedge-shaped first blade portion 122B on a first base portion 122A, and a die 124 having a wedge-shaped second blade portion 124B on a second base portion 124A. The wedge-shaped first blade portion 122B and second blade portion 124B extend in the plate width direction (Y direction), and the plated steel material 10 is cut along the extending direction of the first blade portion 122B and the second blade portion 124B.
[0059] The plated steel material 10 to be cut by the first blade portion 122B of the die 124 and the second blade portion 124B of the punch 122 is placed between the die 124 and the punch 122 with both ends held by blank holders (not shown). At this time, the die 124 and the punch 122 are installed with the first blade portion 122B and the second blade portion 124B facing each other. The punch 122 is then pressed relatively against the die 124 to cut the plated steel material 10.
[0060] When the punch 122 is pressed into the die 124, the cutting tool 121 causes the plating layer 14 on the surface of the plated steel material 10 to penetrate into the cut end surface 101C due to tensile stress generated between the first blade portion 122B and the second blade portion 124B and the plated steel material 10, so that a portion of the cut end surface 101C is covered with the plating layer 14. In other words, the plating layer 14 on the surface of the plated steel material 10 follows the movement of the first blade portion 122B and the second blade portion 124B relative to the plated steel material 10 when the punch 122 is pressed into the die 124, causing the plating layer 14 to penetrate into the cut end surface 101C. In this way, the plated steel material 10 is cut, and at least a portion of the first inclined surface 102 and the second inclined surface 104 of the cut end surface 101C of the cut product 101 can be covered with the plating layer 14.
[0061] The shape of the cut end surface 101C of the cut workpiece 101 cut by the cutting tool 112 is due to the shapes of the first blade portion 122B and the second blade portion 124B. Because the first blade portion 122B and the second blade portion 124B are wedge-shaped, the cut end surface 101C of the cut workpiece 101 does not have a shape along the thickness direction, but has a shape with a first inclined surface 102 and a second inclined surface 104 along the slope of the wedge shape.
[0062] In the cutting tool 121, by forming the first blade portion 122B and the second blade portion 124B into a wedge shape, when cutting the plated steel material 10, the plating layer 14 on the surface of the plated steel material 10 can easily follow the movement of the first blade portion 122B and the second blade portion 124B along the inclined surfaces of the wedge shape. As a result, the plating layer 14 on the surface of the plated steel material 10 can be made to follow not only the first sagging surface 102A and the second sagging surface 104A of the cut end surface 101C, but also the first shearing surface 102B and the second shearing surface 104B. Furthermore, by adjusting the inclination angles of the first shearing surface 102B and the second shearing surface 104B, the coverage rate of the plating layer 14 on the cut end surface 101C of the cut workpiece 101 can be adjusted. Specifically, by increasing the angle of the wedge-shaped slope of the first blade portion 122B and the second blade portion 124B relative to the thickness direction of the plated steel material 10, the plating coverage rate increases.
[0063] Second Embodiment A cut end surface 201C of a cut product 201 according to a second embodiment of the present disclosure has a side surface 202 and a fracture surface 206, as shown in FIG.
[0064] The side surface 202 includes a sagging surface 202A that continues from the first surface 201A of the cut product 201 and a shear surface 202B that continues from the sagging surface 202A. The side surface 202 is inclined in the thickness direction from the first surface 201A to the center of the cut product 201. In other words, the side surface 202 is a surface that has a predetermined inclination angle with respect to the thickness direction of the plated steel material 10.
[0065] The fracture surface 206 is a surface that continues from the side surface 202 and reaches the second surface 201B side of the cut product 201. The fracture surface 206 may have a return portion 206A (i.e., a burr) on the second surface 201B side of the cut product 201 that protrudes beyond the second surface 201B.
[0066] Of the cut end surface 201C of the cut product 201, at least a portion of the base steel material 12 located on the side surface 202 is coated with a plating layer 14. Specifically, the side surface 202 is coated with a plating layer 14 that covers the base steel material 12 located on the first surface 201A when the plated steel material 10 is cut. In other words, the side surface 202 is coated with a plating layer 14 that is continuous with the plating layer 14 of the cut product 201.
[0067] The coverage rate of the plating layer 14 with respect to the cut end surface of the cut product 201 is adjusted by adjusting the area of the plating layer 14 that covers the base steel material 12 located on the side surface 202. Note that the entire surface of the base steel material 12 located on the side surface may be covered with the plating layer 14.
[0068] On the other hand, of the cut end surface 201C of the cut product 201, the non-plated surface of the base steel material 12 including the fracture surface 206 and the plating layer 14 around the non-plated surface are covered with a repair coating film 16.
[0069] The cut product 201 can be manufactured by, for example, a cutting tool 221 shown in Fig. 4. The cutting tool 221 has an upper slit blade 222 and a lower slit blade 224. As shown in Fig. 4, when viewed from the plate width direction (Y direction), the upper slit blade 222 and the lower slit blade 224 have, on the surface facing the cut end surface 201C when cutting the plated steel material 10, a first surface 226A along the plate thickness direction of the plated steel material 10 and a tapered surface 226B inclined outward relative to the first surface 226A. The upper slit blade 222 and the lower slit blade 224 extend in the plate width direction (Y direction), and the plated steel material 10 is cut along the extension direction of the upper slit blade 222 and the lower slit blade 224.
[0070] The plated steel material 10 to be cut by the upper slitting blade 222 and the lower slitting blade 224 is positioned between the upper slitting blade 222 and the lower slitting blade 224 with both ends held by blank holders (not shown). The upper slitting blade 222 and the lower slitting blade 224 are then pressed relative to each other to cut the plated steel material 10.
[0071] When the upper slit blade 222 of the cutting tool 221 is pressed into the lower slit blade 224, tensile stress generated between the upper slit blade 222 and the lower slit blade 224 and the plated steel material 10 causes the plating layer 14 on the surface of the plated steel material 10 to penetrate into the cut end surface 201C, so that a portion of the cut end surface 201C is covered with the plating layer 14. In other words, when the upper slit blade 222 is pressed into the lower slit blade 224, the plating layer 14 on the surface of the plated steel material 10 follows the movement of the upper slit blade 222 and the lower slit blade 224 relative to the plated steel material 10, causing the plating layer 14 to penetrate into the cut end surface 201C. In this way, the plated steel material can be cut, and at least a portion of the side surface 202 of the cut end surface 201C of the cut product 201 can be covered with the plating layer 14.
[0072] The shape of the cut end surface 201C of the cut workpiece 201 cut by the cutting tool 121 is due to the shapes of the upper slit blade 222 and the lower slit blade 224. The upper slit blade 222 and the lower slit blade 224 have a first surface 226A along the thickness direction of the plated steel material 10 and a tapered surface 226B inclined outward from the first surface 226A, so the cut end surface 201C of the cut workpiece 201 has a shape that has a side surface 202 that is along the slope of the tapered surface 226B rather than a shape that is along the thickness direction.
[0073] In the cutting tool 221, the upper slit blade 222 and the lower slit blade 224 have tapered surfaces 226B, which allows the plating layer 14 on the surface of the plated steel material 10 to easily follow the movement of the upper slit blade 222 and the lower slit blade 224 along the slope of the tapered surfaces 226B when cutting the plated steel material 10. As a result, the plating layer 14 on the surface of the plated steel material 10 can be made to follow not only the sagging surface 202A of the cut end surface 201C but also the shear surface 202B. Furthermore, by adjusting the width of the first surface 226A of the upper slit blade 222 and the lower slit blade 224 along the thickness direction of the plated steel material 10, the coverage of the plating layer 14 on the cut end surface 201C of the cut workpiece 201 can be adjusted.
[0074] Third Embodiment A cut end surface 301C of a cut product 301 according to a third embodiment of the present disclosure has a side surface 302 and a fracture surface 306, as shown in FIG.
[0075] The side surface 302 includes a sag surface 302A continuing from the first surface 301A of the cut product 301 and a shear surface 302B continuing from the sag surface 302A. The side surface 302 extends along the plate thickness direction.
[0076] The fracture surface 306 is a surface that continues from the side surface 302 and reaches the second surface 301B side of the cut product 301. The fracture surface 306 may have a return portion 306A (i.e., a burr) on the second surface 301B side of the cut product 301 that protrudes beyond the second surface 301B.
[0077] Of the cut end surface 301C of the cut product 301, at least a portion of the base steel material 12 located on the side surface 302 is coated with a plating layer 14. Specifically, the side surface 302 is coated with a plating layer 14 that covers the base steel material 12 located on the first surface 301A when the plated steel material 10 is cut. In other words, the side surface 302 is coated with a plating layer 14 that is continuous with the plating layer 14 of the cut product 301.
[0078] The coverage rate of the plating layer 14 with respect to the cut end surface of the cut product 301 is adjusted by adjusting the area of the plating layer 14 that covers the base steel material 12 located on the side surface 302. Note that the entire surface of the base steel material 12 located on the side surface may be covered with the plating layer 14.
[0079] On the other hand, of the cut end surface 301C of the cut product 301, the non-plated surface of the base steel material 12 including the fracture surface 306 and the plating layer 14 around the non-plated surface are covered with a repair coating film 16.
[0080] The cut product 301 can be manufactured by, for example, a cutting tool 321 shown in Fig. 6. The cutting tool 321 has an upper slit blade 322 and a lower slit blade 324. As shown in Fig. 6, the upper slit blade 322 and the lower slit blade 324 face the plated steel material 10 when viewed from the plate width direction (Y direction), and have curved portions 326A at corners that face the cut end surface 301C when the plated steel material 10 is cut. The upper slit blade 322 and the lower slit blade 324 extend in the plate width direction (Y direction), and the plated steel material 10 is cut along the extending direction of the upper slit blade 322 and the lower slit blade 324.
[0081] The plated steel material 10 to be cut by the upper slitting blade 322 and the lower slitting blade 324 is positioned between the upper slitting blade 322 and the lower slitting blade 324 with both ends held by blank holders (not shown). The upper slitting blade 322 and the lower slitting blade 324 are then pressed relative to each other to cut the plated steel material 10.
[0082] When the upper slit blade 322 of the cutting tool 321 is pressed into the lower slit blade 324, tensile stress generated between the upper slit blade 322 and the lower slit blade 324 and the plated steel material 10 causes the plating layer 14 on the surface of the plated steel material 10 to penetrate into the cut end surface 301C, so that a portion of the cut end surface 301C is covered with the plating layer 14. In other words, when the upper slit blade 322 is pressed into the lower slit blade 324, the plating layer 14 on the surface of the plated steel material 10 follows the movement of the upper slit blade 322 and the lower slit blade 324 relative to the plated steel material 10, causing the plating layer 14 to penetrate into the cut end surface 301C. In this way, the plated steel material can be cut, and at least a portion of the side surface 302 of the cut end surface 301C of the cut product 301 can be covered with the plating layer 14.
[0083] In the cutting tool 321, the upper slit blade 322 and the lower slit blade 324 have a curved portion 326A, which alleviates the tensile stress applied to the plating layer 14 on the surface of the plated steel material 10 when the plated steel material 10 is cut. As a result, the plating layer 14 on the surface of the plated steel material 10 can be made to follow not only the sagging surface 302A of the cut end surface 301C but also the shear surface 302B. Furthermore, by adjusting the radius of curvature of the curved portion 326A of the upper slit blade 322 and the lower slit blade 324, the coverage rate of the plating layer 14 on the cut end surface 301C of the cut workpiece 301 can be adjusted.
[0084] (Uses of Cut Products) The cut products of the present disclosure are applicable to uses such as steel sheets used for guardrails (specifically, guardrail components, especially guardrail beams), shaped steel for greenhouses or agricultural greenhouses, posts, beams, sound insulation walls, soundproof walls, electrical equipment components, environmental safety components, structural components, solar mounting frames, etc. The cut products of the present disclosure are obtained by cutting plated steel material and then subjecting it to processing such as press forming depending on the above-mentioned use, and then using the resulting product.
[0085] The present disclosure will be described in more detail below with reference to examples, although the present disclosure is not limited to these examples.
[0086] (Preparation of Plated Steel Sheet) Plated steel materials of the following steel type were prepared: Zn-6%Al-3%Mg: Zn-Al-Mg-based plated steel sheet (sheet thickness = 4.5 mm, coating composition = Al: 6 mass %, Mg: 3 mass %, balance: Zn, coating weight on one side = 120 g / m 2 ) Zn-11%Al-3%Mg: Zn-Al-Mg-based plated steel sheet (sheet thickness = 4.5 mm, coating composition = Al: 11 mass%, Mg: 3 mass%, balance: Zn, coating weight on one side = 120 g / m 2 ) Zn-19%Al-6%Mg: Zn-Al-Mg-based plated steel sheet (sheet thickness = 4.5 mm, coating composition = Al: 19 mass%, Mg: 6 mass%, balance: Zn, coating weight on one side = 120 g / m 2 ) Zn: hot-dip galvanized steel sheet (sheet thickness = 4.5 mm, coating weight = 120 g / m 2 )
[0087] (Repair Paint) A repair paint having the composition shown in Table 1 was prepared.
[0088] (Example) According to the conditions in Table 2, a plated steel sheet was cut using a cutting tool to obtain a sample having the cut end surface shown in FIG. 1 , FIG. 3 , or FIG. 5 . The shape of the cutting tool was adjusted to provide the coverage of the plating layer on the cut end surface as shown in Table 2. Next, according to the conditions in Table 2, a repair paint was applied to the non-plated surface of the base steel material of the plated steel sheet and the plating layer around the non-plated surface of the cut end surface of the sample to form a repair coating film. The film thickness of the repair coating film was set as shown in Table 2. The initial coating resistance value and the coating resistance value after immersion in saltwater (i.e., the coating resistance value after immersion of the cut product in 10% by mass saltwater for 3 hours) were also shown in Table 2.
[0089] Through these operations, cut samples were obtained.
[0090] (Evaluation) The cut end surfaces of the obtained cut product samples were subjected to the following evaluations.
[0091] - Cathodic peeling resistance - A combined cyclic corrosion test conforming to CCT-JASO M609 was carried out for 30 cycles. Thereafter, tape ("Cellotape (registered trademark)" manufactured by Nichiban Co., Ltd.) was applied to the surface of the cut end face of the cut-processed sample where the repair coating film had been formed, and then peeled off. The peeled tape was then observed, and the ratio of the area of the repair coating film peeled off from the tape to the area of the repair coating film adhered to the tape (hereinafter referred to as "peeled area ratio") was calculated and evaluated according to the following criteria. Pass was indicated by "A" or "B". A: Peeled area ratio 0% B: Peeled area ratio over 0% to 5% D: Peeled area ratio over 5%
[0092] - Long-term corrosion resistance 1 - A combined cyclic corrosion test in accordance with CCT-JASO M609 was carried out for 120 cycles. The area of red rust on the cut end surface of the cut sample was measured and evaluated according to the following criteria. Passing grades were rated as "A" and "B". A: Red rust area rate 0% B: Red rust area rate over 0% to 10% C: Red rust area rate over 10% to 20% D: Red rust area rate over 20% B or higher is passing grade
[0093] - Long-term corrosion resistance 2 - A combined cyclic corrosion test in accordance with CCT-JASO M609 was carried out for 180 cycles. The area of red rust on the cut end surface of the cut sample was measured and evaluated according to the following criteria. Passing grades were rated as "A" and "B". A: Red rust area rate 0% B: Red rust area rate over 0% to 20% D: Red rust area rate over 20% B or higher is passing grade
[0094]
[0095]
[0096] The above results show that the disclosed examples suppress cathodic peeling of the repair coating film compared to the comparative examples, and have excellent corrosion resistance of the cut end surface from the early stages to the long term.
[0097] The symbols are explained as follows: 10 Plated steel material 12 Base steel material 14 Zn-Al-Mg based plating layer 16 Repair coating film 101 Cut-processed product 101A First surface of cut-processed product 101B Second surface of cut-processed product 101C Cut end surface of cut-processed product 102 First inclined surface 102A Drooping surface 102B Shear surface 104 Second inclined surface 104A Second drooping surface 104B Second shear surface 106 Fracture surface 201 Cut-processed product 201A First surface of cut-processed product 201B Second surface of cut-processed product 201C Cut end surface of cut-processed product 202 Side surface 202A Drooping surface 202B Shear surface 206 Fracture surface 301 Cut-processed product 301A First surface of cut-processed product 301B Second surface of cut product 301C Cut end surface of cut product 302 Side surface 302A Droop surface 302B Shear surface 306 Fracture surface
[0098] The disclosure of Japanese Patent Application No. 2022-157062 is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually indicated to be incorporated by reference.
Claims
1. A cut product of Zn-Al-Mg-plated steel material having a base steel material and a Zn-Al-Mg-plated layer coated on the surface of the base steel material, wherein the cut end surface of the cut product is coated with the Zn-Al-Mg-plated layer at a coverage rate of 50 to 99% of the cut end surface, the non-plated surface of the base steel material and the Zn-Al-Mg-plated layer around the non-plated surface at the cut end surface of the cut product are coated with a repair coating, and the initial coating resistance value R1 of the repair coating is 10 to 1000 Ω / cm 2 and the coating resistance value R2 after immersion of the cut product in 5 mass % salt water for 3 hours is 5 to 50 Ω / cm 2 The cut product, wherein the repair coating film has a thickness of 10 μm or more.
2. The cut product according to claim 1, wherein the repair coating contains zinc-based metal powder and a binder resin.
3. A cut product according to claim 1, wherein the cut end surface of the cut product has: a first inclined surface which includes a first sagging surface continuing from a first surface of the cut product and a first shear surface continuing from the first sagging surface, and which inclines from the first surface of the cut product towards the centre in the plate thickness direction; a second inclined surface which includes a second sagging surface continuing from a second surface of the cut product and a second shear surface continuing from the second sagging surface, and which inclines from the second surface of the cut product towards the centre in the plate thickness direction; and a fracture surface formed between the first inclined surface and the second inclined surface; wherein at least a part of the base steel material located on the first inclined surface and the second inclined surface of the cut end surface of the cut product is coated with the Zn-Al-Mg-based plating layer; and wherein the non-plated surface of the base steel material including the fracture surface and the Zn-Al-Mg-based plating layer around the non-plated surface of the cut end surface of the cut product are coated with the repair coating film.
4. A cut product according to claim 1, wherein the cut end surface of the cut product has: a side surface that includes a sagging surface that is continuous from a first surface of the cut product and a shear surface that is continuous from the sagging surface, and that is inclined along the plate thickness direction or from the first surface of the cut product toward the center; and a fracture surface that is continuous from the side surface and reaches the second surface of the cut product; and at least a part of the base steel located on the side surface of the cut end surface of the cut product is coated with the Zn-Al-Mg-based plating layer; and the non-plated surface of the base steel including the fracture surface and the Zn-Al-Mg-based plating layer around the non-plated surface of the cut end surface of the cut product are coated with the repair coating film.
5. The initial coating resistance value R1 of the repair coating is 300 to 500 Ω / cm 2 2. The cut product according to claim 1, wherein 6. The coating resistance value R2 of the repair coating after immersion is 10 to 45 Ω / cm 2 2. The cut product according to claim 1, wherein 7. The cut product according to claim 2, wherein the Zn-based metal powder contains Zn and Al.
8. The cut product according to claim 7, wherein the content of Al relative to Zn in the Zn-based metal powder containing Zn and Al is 20 to 45 mass %.
9. The cut product according to claim 7, wherein the content of Al relative to Zn in the Zn-based metal powder containing Zn and Al is 28 to 34 mass %.
10. A cut product according to claim 2, wherein the content of the Zn-based metal powder in the entire repair coating is 60 to 80 mass % of the metal powder.
11. The cut product according to claim 2, wherein the binder resin is at least one selected from the group consisting of polystyrene resin and epoxy resin.