Electrically conductive paste, electronic component, and multilayer ceramic capacitor

MYPI2025001700A0Undetermined Publication Date: 2024-03-21SUMITOMO METAL MINING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025001700
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-21
Filing Date
2023-08-29
Publication Date
2024-03-21

AI Technical Summary

Technical Problem

Multilayer ceramic capacitors face challenges in achieving smaller size and higher capacity due to issues with adhesion between internal electrode layers and green sheets, leading to problems like peeling, misalignment, and decreased insulation resistance, which are exacerbated by the use of plasticizers and incompatible organic binder resins.

Method used

A conductive paste is developed containing conductive powder, ceramic powder, a dispersant, and a binder resin with a polymer compound where cellulose and polyvinyl acetal are bonded by sulfur atoms, along with an anionic polymer dispersant, to enhance adhesion and dispersibility, resulting in a smooth dry film and improved electrode formation.

Benefits of technology

The conductive paste achieves excellent adhesion and dispersibility, enabling the formation of thin, uniform internal electrode layers with improved reliability and capacitance in multilayer ceramic capacitors, addressing issues of peeling, misalignment, and insulation resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025001700_DRAWING_001
    Figure PI2025001700_DRAWING_001
  • Figure PI2025001700_DRAWING_002
    Figure PI2025001700_DRAWING_002
Patent Text Reader

Abstract

Provided are an electrically conductive paste using an electrically conductive powder or a ceramic powder which is refined for a size reduction and a thickness reduction of a multilayer ceramic electronic component, the electrically conductive paste being capable of forming an internal electrode layer having a smooth dry film and excellent adhesive properties, an electronic component, and a multilayer ceramic capacitor. The electrically conductive paste contains an electrically conductive powder, a ceramic powder, a dispersant, a binder resin, and an organic solvent, in which the binder resin contains cellulose, polyvinyl acetal, and a polymer compound obtained by bonding a cellulose-based compound and a polyvinyl acetal-based compound by sulfur atoms, a molar ratio of the sulfur atoms contained in the polymer compound to a total of the cellulose and the cellulose-based compound is 0.3 to 1.7, and the dispersant is an anionic polymer compound. Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Conductive paste, electronic components and multilayer ceramic capacitors

[0001] The present invention relates to a conductive paste, an electronic component, and a multilayer ceramic capacitor.

[0002] As electronic devices such as mobile phones and digital devices become smaller and more powerful, there is a demand for smaller and higher-capacity electronic components, including multilayer ceramic capacitors. Multilayer ceramic capacitors have a structure in which multiple dielectric layers and multiple internal electrode layers are alternately stacked, and by reducing the thickness of these dielectric layers and internal electrode layers, it is possible to achieve smaller size and higher capacity.

[0003] For example, a multilayer ceramic capacitor is manufactured as follows: First, barium titanate (BaTiO 3 A conductive paste for internal electrodes is printed (applied) in a predetermined electrode pattern onto the surface of a green sheet containing a dielectric powder such as ethylenediaminetetraacetic acid (EPO) and a binder resin such as polybutyral resin, and then dried to form a dry film. Next, the dried film and the green sheet are alternately stacked and heat-pressed to form an integrated laminate. This laminate is then cut, subjected to an organic binder removal treatment in an oxidizing or inert atmosphere, and then fired to obtain fired chips. Next, a paste for external electrodes is applied to both ends of the fired chip, and after firing, the surfaces of the external electrodes are nickel-plated or the like to obtain multilayer ceramic capacitors (MLCCs).

[0004] In recent years, there has been a demand for MLCCs to be even smaller and have larger capacities, and for example, thinner electrode films with excellent density and continuity for internal electrodes using nickel or the like, and ceramic dielectric materials and dielectric layers using such materials are being studied to have higher dielectric constants and thinner layers, with dielectric layer thicknesses of 1.0 μm or less already in practical use. It is also desirable to reduce the electrode film thickness to 1.0 μm or less.

[0005] One of the required characteristics for miniaturizing and increasing the capacity of MLCCs is the suppression of a decrease in insulation resistance under high temperatures and high voltages, i.e., high reliability. The decrease in insulation resistance is said to be caused by the occurrence of unevenness on the surface of the Ni electrode layer sandwiching the dielectric layer during the sintering process, which causes the electric field to concentrate on the uneven surfaces. During the sintering process, the Ni electrode layer is formed through a process of sintering and densification of the Ni powder. However, because fine Ni powder sinters quickly, the electrode is prone to breakage and spheroidization. As a result, the effective electrode area of ​​the Ni electrode layer decreases, reducing capacity, and the unevenness on the Ni electrode layer surface leads to a decrease in insulation resistance.

[0006] As MLCCs become thinner, the adhesion between the green sheets and the internal electrode layers decreases, causing frequent problems such as peeling and misalignment due to insufficient adhesion during lamination. Therefore, for example, internal electrode pastes containing plasticizers are used. However, the plasticizer significantly reduces the elastic modulus of the printed film, making it soft and prone to deformation. Even though the adhesion to the green sheets is improved, this can lead to serious problems such as poor cutting of the internal electrode layers. Furthermore, the plasticizer increases the amount of gas generated during the organic binder removal process, which can cause cracks.

[0007] When ceramic green sheets are stacked and pressed in the thickness direction, poor adhesion between the green sheets results in poor adhesion between the green sheets. This poor adhesion can lead to short circuits, for example, in multilayer ceramic capacitors. In particular, the need for multilayer MLCCs requires the use of fine-particle dielectric powder to reduce the thickness of each dielectric layer and increase the number of layers, making it desirable to improve the poor adhesion. Weak adhesion between green sheets can cause structural defects such as delamination, voids, and cracks during firing, reducing the yield of MLCCs.

[0008] To improve such poor adhesion, the following measures 1) and 2) can be considered. 1) Increasing the amount of binder or tackifier in the conductive paste is conceivable, but simply increasing these amounts does not significantly improve adhesion. Conversely, increasing these amounts increases the amount of organic substances, such as organic binders and tackifiers, in the conductive paste. These organic substances make it difficult to remove the organic binder. Even after the organic binder removal process, the remaining organic substances (residual carbon) can cause structural defects during the subsequent firing process. 2) When stacking multiple ceramic green sheets with conductive paste films, smoothing the surface of the coating film made of conductive paste increases the contact area between the conductive paste film and the ceramic green sheets, thereby improving adhesion.

[0009] While the goal of improving adhesion between the internal electrodes and green sheets is to prevent cracking, using butyral resin as the resin can prevent electrode peeling during cutting. Until now, cellulose-based resins such as ethyl cellulose have been primarily used as organic binders. However, while cellulose-based resins are highly compatible with various solvents and are effective in imparting the desired rheological properties to conductive pastes, they have the drawback of not being very thermoplastic themselves, meaning that the dried portion of the conductive paste retains almost no adhesion to the upper green sheet during thermocompression bonding. As a result, no conductive paste for multilayer ceramic capacitor internal electrodes has been developed that can further improve thermocompression bonding between the internal electrodes of green sheets on which the conductive paste is screen-printed and the upper green sheet, prevent electrode misalignment within the chip, improve electrode alignment, and prevent chip cracking and peeling, thereby enabling high stacking density.

[0010] Therefore, the internal electrode paste can contain an organic resin, and the organic binder resin is preferably a mixture of ethyl cellulose (EC) and polyvinyl butyral (PVB).

[0011] Ethyl cellulose (EC) can be suitably used as a binder for the internal electrode paste due to its good solubility in solvents, printability, combustion decomposition properties, etc. Furthermore, by using polyvinyl butyral (PVB), which is used for the green sheet, together as an organic binder resin, it is possible to increase the adhesive strength between the green sheet and the dried film of the internal electrode paste.

[0012] Patent Documents 1 and 2 disclose a conductive paste containing a cellulose-based resin and a polyvinyl butyral resin as a binder resin, and disclose that the paste improves adhesion to ceramic green sheets.

[0013] Patent No. 5299904 Patent No. 5224722

[0014] However, when two different organic binder resins are mixed, they are generally incompatible (immiscible) combinations. When two organic binder resins are incompatible, the two organic binder resins are basically not soluble in each other and exist independently, so not only are they unable to exhibit the expected performance, but their functionality is often significantly reduced.

[0015] Furthermore, when the resin becomes less soluble in the solvent, the smoothness of the dried paste film deteriorates. For example, when EC and PVB are mixed, a typical "sea-island structure" is observed, confirming phase separation. As a result, the distribution of inorganic particles (conductive particles, ceramic powder) in the dried film becomes non-uniform. In this way, the combination of organic materials in the paste composition affects the dispersibility of inorganic particles (conductive particles, ceramic powder) in the dried film.

[0016] By making polymers that are normally immiscible compatible with each other, the advantages of both can be combined, the interface between the different polymers can be stabilized, and a uniform and stable dispersion state can be achieved.

[0017] Furthermore, the conductive pastes disclosed in Patent Documents 1 and 2 contain polyvinyl butyral resin, which improves the adhesion between the dried film and the green sheet. However, these techniques use a combination of cellulose-based resin and polyvinyl butyral resin, which results in poor compatibility between the two resins, resulting in insufficient dispersion of the conductive powder and ceramic powder in the conductive paste, and in insufficient density and smoothness of the dried film of the conductive paste. Such dried film properties are not sufficient to meet the increasing capacitance of multilayer ceramic capacitors in recent years.

[0018] In view of the above circumstances, an object of the present invention is to provide a conductive paste using a finely divided conductive powder or ceramic powder for reducing the size and thickness of a multilayer ceramic electronic component, which is capable of forming an internal electrode layer having a smooth dried film and excellent adhesion, an electronic component, and a multilayer ceramic capacitor.

[0019] In order to solve the above problems, the conductive paste of the present invention comprises a conductive powder, a ceramic powder, a dispersant, a binder resin, and an organic solvent, wherein the binder resin comprises cellulose, polyvinyl acetal, and a polymer compound in which a cellulose-based compound and a polyvinyl acetal-based compound are bonded together via sulfur atoms, the molar ratio of sulfur atoms contained in the polymer compound to the total of the cellulose and the cellulose-based compound is 0.3 to 1.7, and the dispersant is an anionic polymer compound.

[0020] The dispersant may comprise a carboxy group or a carboxylic acid anhydride group.

[0021] The cellulose compound may be a cellulose derivative having a thiol group or a vinyl group, the polyvinyl acetal compound may be a polyvinyl acetal resin having a thiol group or a vinyl group, and if the cellulose derivative has a thiol group, the polyvinyl acetal resin may have a vinyl group that reacts with the thiol group, and if the cellulose derivative has a vinyl group, the polyvinyl acetal resin may have a thiol group that reacts with the vinyl group.

[0022] The cellulose derivative may be ethyl cellulose having a thiol group or a vinyl group, and the polyvinyl acetal resin may be polyvinyl butyral having a thiol group or a vinyl group.

[0023] The cellulose-based compound may be a first esterification reaction product obtained by dehydration condensation of a carboxy group of a carboxylic acid having a thiol group or a vinyl group with a hydroxyl group of cellulose; the polyvinyl acetal-based compound may be a second esterification reaction product obtained by dehydration condensation of a carboxy group of a carboxylic acid having a thiol group or a vinyl group with a hydroxyl group of polyvinyl acetal; if the first esterification reaction product has a thiol group, the second esterification reaction product may have a vinyl group; if the first esterification reaction product has a vinyl group, the second esterification reaction product may have a thiol group; and the polymer compound may be a thiol-ene reaction product of the first esterification reaction product and the second esterification reaction product.

[0024] The first esterification reaction product may be an esterification reaction product obtained by dehydration condensation of a carboxy group of 3-allyloxypropionic acid and a hydroxy group of ethyl cellulose, and the second esterification reaction product may be an esterification reaction product obtained by dehydration condensation of a carboxy group of 3-mercaptopropionic acid and a hydroxy group of polyvinyl butyral.

[0025] The conductive powder may be nickel powder.

[0026] The number average particle size of the conductive powder may be 0.05 μm or more and 1.0 μm or less.

[0027] The ceramic powder may include barium titanate.

[0028] The ceramic powder may have a number average particle size of 0.01 μm or more and 0.5 μm or less.

[0029] The content of the ceramic powder may be 1% by mass or more and 20% by mass or less.

[0030] The conductive paste of the present invention may be used for internal electrodes of multilayer ceramic components.

[0031] In order to solve the above-mentioned problems, the electronic component of the present invention is an electronic component formed using the conductive paste of the present invention.

[0032] In order to solve the above-mentioned problems, the multilayer ceramic capacitor of the present invention is a multilayer ceramic capacitor having at least a laminate in which dielectric layers and internal electrode layers are laminated, and the internal electrode layers are formed using the conductive paste of the present invention.

[0033] The conductive paste of the present invention has excellent dispersibility of the conductive powder and a high surface smoothness when dried after application. Furthermore, the electrode pattern of an electronic component such as a multilayer ceramic capacitor formed using the conductive paste of the present invention has excellent adhesion of the conductive paste even when forming a thin electrode.

[0034] 1A and 1B are a perspective view and a cross-sectional view showing the multilayer ceramic capacitor according to the embodiment, respectively, and are graphs showing evaluation results of adhesion between a green sheet and a dried film formed by printing and drying a conductive paste.

[0035] Hereinafter, an embodiment of the conductive paste, electronic component, and multilayer ceramic capacitor of the present invention will be described.

[0036] [Conductive Paste] The conductive paste of this embodiment contains a conductive powder, a ceramic powder, a dispersant, a binder resin, and an organic solvent. Each component will be described in detail below.

[0037] (Conductive Powder) The conductive powder is not particularly limited, and metal powders can be used. For example, powders of one or more elements selected from Ni, Pd, Pt, Au, Ag, Cu, and alloys thereof can be used. Among these, powders of Ni or its alloys are preferred from the viewpoints of conductivity, corrosion resistance, and cost. Examples of Ni alloys that can be used include alloys of Ni with at least one element selected from the group consisting of Mn, Cr, Co, Al, Fe, Cu, Zn, Ag, Au, Pt, and Pd (Ni alloys). The Ni content in the Ni alloy is, for example, 50% by mass or more, preferably 80% by mass or more. Furthermore, the Ni powder may contain several hundred ppm of S to suppress rapid gas generation due to partial thermal decomposition of the binder resin during binder removal treatment.

[0038] The method for producing the conductive powder is not particularly limited, and examples thereof include a method in which chloride vapor is directly precipitated from the gas phase in hydrogen gas, an atomization method from molten metal, a spray pyrolysis method using an aqueous solution, and a wet method in which a raw material metal salt is reduced in an aqueous solution.

[0039] The number average particle size of the conductive powder is not particularly limited and may be selected depending on the size of the electronic component to be used. For example, for multilayer ceramic capacitors, which are becoming increasingly thin, the number average particle size of the conductive powder is preferably 0.5 μm or less, and more preferably 0.3 μm or less. If the average particle size exceeds 0.5 μm, the internal electrode surface becomes significantly uneven, which may degrade the electrical characteristics of the capacitor, which is undesirable. The lower limit of the average particle size of the conductive powder is not particularly limited, but is, for example, 0.03 μm or more. If the number average particle size is less than 0.03 μm, handling becomes extremely difficult.

[0040] The number average particle size of the conductive powder is a value determined by observation using a scanning electron microscope (SEM), and is the average value obtained by measuring the particle size of each of multiple particles from an image observed with an SEM at a magnification of 10,000 times.

[0041] The content of the conductive powder is preferably 30% by mass or more and less than 70% by mass, more preferably 40% by mass or more and 60% by mass or less, based on the total amount of the conductive paste. When the content of the conductive powder is in the above range, the conductive paste has excellent conductivity and dispersibility.

[0042] (Ceramic Powder) The ceramic powder is not particularly limited, and for example, in the case of a conductive paste for an internal electrode of a multilayer ceramic capacitor, a known ceramic powder is appropriately selected depending on the type of multilayer ceramic capacitor to be applied. Examples of the ceramic powder include perovskite-type oxides containing Ba and Ti, and preferably barium titanate (BaTiO 3 )

[0043] The ceramic powder may be a ceramic powder containing barium titanate as a main component and an oxide as a secondary component. Examples of the oxide include oxides of Mn, Cr, Si, Ca, Ba, Mg, V, W, Ta, Nb, and one or more rare earth elements. Examples of the ceramic powder include barium titanate (BaTiO 3 Alternatively, a ceramic powder of a perovskite-type oxide ferroelectric may be used in which the Ba atoms or Ti atoms of the above-mentioned alloy are substituted with other atoms such as Sn, Pb, or Zr.

[0044] In the conductive paste for the internal electrodes, powder of the same composition as the dielectric ceramic powder constituting the green sheets of the multilayer ceramic capacitor may be used as the ceramic powder. This suppresses the occurrence of cracks due to a mismatch in shrinkage at the interface between the dielectric layer and the internal electrode layer during the sintering process. In addition to the above, examples of such ceramic powders include ZnO, ferrite, PZT, BaO, and Al. 2 O 3 , Bi 2 O 3 , R (rare earth element) 2 O 3 , TiO 2 , Nd 2 O 3 The ceramic powder may be one type or two or more types.

[0045] The number average particle diameter of the ceramic powder is, for example, 0.01 μm or more and 0.5 μm or less, preferably 0.01 μm or more and 0.3 μm or less. When the number average particle diameter of the ceramic powder is in the above range, when used as an internal electrode paste, a sufficiently fine, thin, and uniform internal electrode can be formed. The number average particle diameter is a value determined by observation with a scanning electron microscope (SEM), and is the average value obtained by measuring the particle diameter of each of a plurality of particles in an image observed with the SEM at a magnification of 50,000 times.

[0046] The content of the ceramic powder is preferably 1 part by mass or more and 30 parts by mass or less, and more preferably 3 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the conductive powder. When the content of the conductive powder is within the above range, the conductivity and dispersibility are excellent.

[0047] The content of the ceramic powder is preferably 1% by mass or more and 20% by mass or less, more preferably 5% by mass or more and 20% by mass or less, based on the total amount of the conductive paste. When the content of the conductive powder is in the above range, the conductive paste has excellent conductivity and dispersibility.

[0048] (Binder Resin) The binder resin used in the conductive paste of the present embodiment contains cellulose, polyvinyl acetal, and a polymer compound in which a cellulose-based compound and a polyvinyl acetal-based compound are bonded together by sulfur atoms, and the molar ratio of sulfur atoms contained in the polymer compound to the total of the cellulose and the cellulose-based compound is 0.3 to 1.7.

[0049] That is, the binder resin used in the conductive paste of this embodiment contains a polymer compound in which a cellulose compound and a polyvinyl acetal compound are bonded together. The number average molecular weight (Mn) of this polymer compound is preferably 20,000 to 200,000, as calculated using standard polystyrene standards by gel permeation chromatography (GPC). The content of the polymer compound in which a cellulose compound and a polyvinyl acetal compound are bonded together is preferably 1 part by mass or more and 10 parts by mass or less, more preferably 1 part by mass or more and 8 parts by mass or less, per 100 parts by mass of the conductive powder.

[0050] The polymer compound molecules of this embodiment contain both cellulose-based and polyvinyl acetal-based compounds, allowing the dried film obtained from the conductive paste of this embodiment to have the surface smoothness provided by the cellulose-based compound and the adhesion to the green sheet provided by the polyvinyl acetal-based compound. Furthermore, the polymer compound contains the structures of the cellulose-based compound and the polyvinyl acetal-based compound, which are incompatible with each other, within the same molecule, thereby eliminating poor dispersion of the conductive paste.

[0051] Here, even if the molar ratio of sulfur atoms contained in the polymer compound to the total of the cellulose and the cellulose-based compound is 0.5 to 2, the surface roughness of the dried film is superior to that of a conventional conductive paste that uses cellulose and a polyvinyl acetal resin in combination as a binder resin, but if the molar ratio is 0.3 to 1.7, the surface roughness and dry film density of the dried film of the conductive paste are even superior. The molar ratio of sulfur atoms contained in the polymer compound to the total of the cellulose and the cellulose-based polymer compound is 0.3 to 1.7, and more preferably 0.5 to 1.5.

[0052] The polymer compound in which the cellulose-based compound and the polyvinyl acetal-based compound are bonded, which can be used in this embodiment, will be described in more detail.

[0053] Both cellulose and polyvinyl acetal have hydroxyl groups within their molecules. A cellulose-based compound is prepared by introducing functional groups capable of reacting with other compounds to form bonds into the hydroxyl groups of the cellulose, thereby chemically modifying the reactive functional groups. On the other hand, a polyvinyl acetal-based polymer compound is prepared by introducing functional groups capable of reacting with other compounds to form bonds, but different from the functional groups introduced into the cellulose-based compound, thereby chemically modifying the reactive functional groups. In other words, the reactive functional groups introduced into the cellulose-based compound and the reactive functional groups introduced into the polyvinyl acetal-based compound are different. Note that while the functional groups introduced into the cellulose-based compound and the functional groups introduced into the polyvinyl acetal-based compound react, the same functional groups do not react easily. The reason for the low reactivity between the same functional groups is to prevent bonding between cellulose-based compounds and between polyvinyl acetal-based compounds.

[0054] Then, by bonding the functional group introduced into the cellulose-based compound with the functional group introduced into the polyvinyl acetal-based compound, a polymer compound in which the cellulose-based compound and the polyvinyl acetal-based compound are bonded can be obtained. Specifically, by introducing a thiol group into cellulose to form a cellulose-based compound and a vinyl group into a polyvinyl acetal resin to form a polyvinyl acetal-based compound, the thiol group and the vinyl group bond via the double bond of the vinyl group and the sulfur atom of the thiol group in the presence of a nucleophile or under conditions that generate radicals. As the polymer compound of the binder resin used in the conductive paste of this embodiment, a polymer compound in which the cellulose-based compound and the polyvinyl acetal-based compound are bonded can be obtained by utilizing the bonding reaction between the thiol group and the vinyl group. Of course, it is also possible to introduce a vinyl group into the hydroxyl group of cellulose to form a cellulose-based compound, and then introduce a thiol group into the hydroxyl group of the polyvinyl acetal resin to form a polyvinyl acetal-based compound.

[0055] That is, the cellulose compound may be a cellulose derivative having a thiol group or a vinyl group, and the polyvinyl acetal compound may be a polyvinyl acetal resin having a thiol group or a vinyl group. When the cellulose derivative has a thiol group, the polyvinyl acetal resin has a vinyl group that reacts with the thiol group, and when the cellulose derivative has a vinyl group, the polyvinyl acetal resin has a thiol group that reacts with the vinyl group.

[0056] The cellulose-based polymer compound used as the binder resin of the conductive paste of this embodiment is preferably a polymer compound chemically modified by bonding a compound to the hydroxyl group of cellulose, a natural polymer. Note that this chemical modification is different from the chemical modification that introduces the above-mentioned reactive functional group.

[0057] Examples of bonding of a compound with the hydroxyl group of cellulose include alkyl etherification and esterification. Examples of celluloses having hydroxyl groups include methyl cellulose, ethyl cellulose, propyl cellulose, butyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxybutyl methyl cellulose, cellulose acetate (acetyl cellulose, diacetyl cellulose, triacetyl cellulose, etc.), cellulose acetate propionate, cellulose acetate butyrate, nitrocellulose, etc. Only one of these celluloses may be used, or two or more may be used in combination.

[0058] Since the conductive paste of the embodiment contains an organic solvent, it is preferable that the cellulose also dissolves in the organic solvent. From the viewpoints of solubility in the organic solvent and smoothness of the dried film of the conductive paste, it is more preferable to use ethyl cellulose as the cellulose.

[0059] The molecular weight of the cellulose affects the viscosity of the conductive paste of this embodiment. The number average molecular weight (Mn) of the cellulose, as calculated using standard polystyrene standards by GPC, is preferably 10,000 to 100,000, and more preferably 10,000 to 80,000.

[0060] If the number average molecular weight of the cellulose is less than 10,000, the viscosity of the conductive paste will be low, whereas if the number average molecular weight of the cellulose exceeds 100,000, the viscosity of the conductive paste will be too high.

[0061] Not all of the hydroxyl groups in cellulose are chemically modified. The glucose rings that make up cellulose have three hydroxyl groups attached, but on average, 0.1 to 1 hydroxyl group per glucose ring of cellulose remains as a hydroxyl group and is not chemically modified. Reactive functional groups are introduced into these unmodified hydroxyl groups.

[0062] On the other hand, polyvinyl acetal is usually a polymer composed of vinyl acetal / vinyl alcohol / vinyl acetate monomer units, and can be obtained by saponifying polyvinyl acetate to polyvinyl alcohol and then acetalizing the polyvinyl alcohol.Specific examples include butyralized polyvinyl alcohol (polyvinyl butyral) and formalized polyvinyl alcohol (polyvinyl formal).

[0063] The polyvinyl acetal may be a commercially available product, and various polyvinyl acetals differing in the degree of butyralization, degree of formalization, amount of acetyl groups, amount of hydroxyl groups, molecular weight, etc. are sold by Sekisui Chemical Co., Ltd., Kuraray Co., Ltd., etc. Only one type of polyvinyl acetal may be used, or two or more types may be used in combination.

[0064] The polyvinyl acetal is preferably one that is soluble in an organic solvent, and more preferably polyvinyl butyral because of its high solubility in an organic solvent.

[0065] The molecular weight of polyvinyl acetal affects the film strength and the viscosity of the solution, and therefore the number average molecular weight of polyvinyl acetal, as calculated using standard polystyrene standards by GPC, is preferably in the range of 5,000 to 150,000, and more preferably in the range of 10,000 to 100,000.

[0066] If the number-average molecular weight of the polyvinyl acetal is less than 5,000, the solution viscosity will be extremely low, making it difficult to adjust the viscosity of the inorganic particle-containing composition (paste or slurry). Furthermore, the strength and adhesion of the film formed by applying and drying the inorganic particle-containing composition may be reduced.

[0067] Polyvinyl acetal has at least one hydroxyl group per molecule. Generally, polyvinyl acetal has 20 to 40 mol % of hydroxyl groups as vinyl alcohol units constituting the polymer. These hydroxyl groups are chemically modified by introducing reactive functional groups.

[0068] The compound that reacts with the hydroxyl groups of cellulose to chemically modify it can be a compound that has a thiol or vinyl group at one end and a carboxyl group at the other end, whose carboxyl group undergoes dehydration condensation with the hydroxyl groups of the cellulose-based polymer compound to form an ester bond.

[0069] A method for synthesizing the polymer compound used in this embodiment will now be described. Cellulose-based compounds and polyvinyl acetal-based compounds can be obtained by esterifying or etherifying a compound having a functional group reactive with a hydroxyl group and a functional group reactive with other compounds with the hydroxyl groups of cellulose or the hydroxyl groups of polyvinyl acetal. Examples of functional groups reactive with hydroxyl groups include carboxyl groups and hydroxyl groups.

[0070] The esterification reaction can be carried out using, for example, a condensing agent. Examples of the condensing agent include carbodiimide, diphenylphosphoric acid azide, and 1-hydroxybenzotriazole. One type of condensing agent may be used alone, or two or more types may be used in combination. Among these, carbodiimide is preferred because it has excellent versatility and reactivity and allows the reaction to proceed under low temperature conditions and without being affected by moisture in the reaction environment.

[0071] Examples of carbodiimides include dicyclohexylcarbodiimide, diisopropylcarbodiimide, N-[3-(dimethylamino)propyl]-N'-ethylcarbodiimide, and N-[3-(dimethylamino)propyl]-N'-ethylcarbodiimide methiodide. Among these, dicyclohexylcarbodiimide and diisopropylcarbodiimide are preferred from the viewpoint of availability. When using a carbodiimide, it is also preferred to use a base such as dimethylaminopyridine or triethylamine as a reaction accelerator in the range of 0.01 mol % to 10 mol % relative to the carbodiimide.

[0072] The etherification reaction can be carried out efficiently by using an alkali metal hydroxide such as KOH or NaOH, or an alkali metal hydride such as NaH or KH as a reaction catalyst.

[0073] To obtain a cellulose-based compound, it is also preferable to dissolve cellulose in an aprotic solvent such as ethyl acetate, mix with a compound having a carboxyl group that forms an ester bond with a hydroxyl group and a vinyl group or a thiol group that is a functional group that reacts with other compounds, and use a condensing agent and a base such as dimethylaminopyridine as a nucleophile to promote the esterification reaction in the range of 0.01 mol % to 10 mol %.

[0074] The polymer compound used in this embodiment has a molar ratio of sulfur atoms to the total of cellulose and cellulose-based compounds of 0.3 to 1.7, so it is necessary to add 0.3 to 1.7 mol of a compound having a functional group that reacts with other compounds per 1 mol of cellulose.

[0075] The reaction temperature for synthesizing cellulose compounds is preferably in the range of room temperature to 50°C. In a system where the synthesis reaction of a cellulose compound is complete, there is a mixture of unreacted cellulose, in which no functional group reactive with other compounds has been introduced to the hydroxyl group, cellulose compounds in which one reactive functional group has been introduced, and cellulose compounds in which multiple reactive functional groups have been introduced. Chemical modification is a matter of probability, but the majority of cellulose compounds have one hydroxyl group of cellulose chemically modified. Once the synthesis of the cellulose compound is complete, the solvent can be removed by distillation.

[0076] To synthesize a polyvinyl acetal compound, it is also preferable to dissolve polyvinyl acetal in an aprotic solvent such as ethyl acetate, mix it with a compound having a carboxy group that forms an ester bond with a hydroxyl group and a vinyl group or a thiol group that is a functional group that reacts with other compounds, and use a condensing agent and a base such as dimethylaminopyridine as a nucleophile to promote the esterification reaction in the range of 0.01 mol % to 10 mol %.

[0077] The reaction temperature for chemically modifying the hydroxyl groups of polyvinyl acetal is preferably in the range of room temperature to 50° C. After the synthesis of the polyvinyl acetal compound is completed, the solvent can be removed by distillation.

[0078] The polymer compound used in this embodiment is prepared by dissolving a cellulose-based compound and a polyvinyl acetal-based compound in a solvent, adding a radical generator, and heating the resulting mixture, whereby a vinyl group in either the cellulose-based compound or the polyvinyl acetal-based compound reacts with a thiol group in the other, bonding the cellulose-based compound and the polyvinyl acetal-based compound together.

[0079] Alternatively, the cellulose compound and the polyvinyl acetal compound may be dissolved in a solvent, and a nucleophilic agent such as a base such as an amine may be added thereto, followed by heating.

[0080] The temperature for the reaction to bond the cellulose compound and the polyvinyl acetal compound can be appropriately selected, but is preferably 60° C. or higher.

[0081] The solvent may be an acetate-based solvent such as dihydroterpineol acetate, isobornyl acetate, isobornyl propionate, isobornyl butyrate, isobornyl isobutyrate, ethylene glycol monobutyl ether acetate, or dipropylene glycol methyl ether acetate, or a terpene-based solvent such as terpineol or dihydroterpineol. If the solvent used in the conductive paste is used as the solvent, the resulting polymer compound can be dissolved in the solvent to form a vehicle.

[0082] In this embodiment, in addition to the polymer compound in which a cellulose compound and a polyvinyl acetal compound are bonded, it is also possible to add cellulose resins such as methyl cellulose, ethyl cellulose, ethylhydroxyethyl cellulose, and nitrocellulose, acrylic resins, and butyral resins such as polyvinyl acetal resins. The molecular weight of the resins that can be added in this way is about 20,000 to 200,000 in GCP.

[0083] The content of the binder resin is preferably 0.5% by mass or more and 10% by mass or less, more preferably 1% by mass or more and 6% by mass or less, based on the total amount of the conductive paste. When the content of the binder resin is in the above range, the conductive paste has excellent conductivity and dispersibility.

[0084] For example, the cellulose derivative may be ethyl cellulose having a thiol group or a vinyl group, and the polyvinyl acetal resin may be polyvinyl butyral having a thiol group or a vinyl group.

[0085] Specifically, the cellulose-based compound may be a first esterification reaction product obtained by dehydration condensation of a carboxy group of a carboxylic acid having a thiol group or a vinyl group with a hydroxyl group of cellulose, and the polyvinyl acetal-based compound may be a second esterification reaction product obtained by dehydration condensation of a carboxy group of a carboxylic acid having a thiol group or a vinyl group with a hydroxyl group of polyvinyl acetal. Furthermore, when the first esterification reaction product has a thiol group, the second esterification reaction product may have a vinyl group; when the first esterification reaction product has a vinyl group, the second esterification reaction product may have a thiol group; and the polymer compound may be a thiol-ene reaction product of the first esterification reaction product and the second esterification reaction product.

[0086] More specifically, the first esterification reaction product may be an esterification reaction product obtained by dehydration condensation of a carboxy group of 3-allyloxypropionic acid and a hydroxy group of ethyl cellulose, and the second esterification reaction product may be an esterification reaction product obtained by dehydration condensation of a carboxy group of 3-mercaptopropionic acid and a hydroxy group of polyvinyl butyral.

[0087] (Organic Solvent) The organic solvent is not particularly limited, and any known organic solvent capable of dissolving the binder resin can be used. Examples of organic solvents include acetate-based solvents such as dihydroterpinyl acetate, isobornyl acetate, isobornyl propionate, isobornyl butyrate, isobornyl isobutyrate, ethylene glycol monomethyl ether acetate, ethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, and dipropylene glycol methyl ether acetate; terpene-based solvents such as terpineol and dihydroterpineol; hydrocarbon-based solvents such as tridecane, nonane, and cyclohexane; and petroleum-based hydrocarbon solvents such as mineral spirits. One or more organic solvents may be used.

[0088] The content of the organic solvent is preferably 40 parts by mass or more and 100 parts by mass or less, more preferably 65 parts by mass or more and 95 parts by mass or less, relative to 100 parts by mass of the conductive powder. When the content of the organic solvent is within the above range, the conductive powder has excellent conductivity and dispersibility.

[0089] The content of the organic solvent is preferably 20% by mass or more and 60% by mass or less, and more preferably 35% by mass or more and 55% by mass or less, based on the total amount of the conductive paste. When the content of the organic solvent is in the above range, the conductive paste has excellent conductivity and dispersibility.

[0090] (Dispersant) The conductive paste of this embodiment contains a polymer dispersant. The role of the polymer dispersant is to adsorb to the surfaces of the inorganic powders (conductive powder and ceramic powder) to suppress aggregation of the inorganic powders and to improve wettability with the organic vehicle to disperse the inorganic powders in the conductive paste.

[0091] The polymer dispersant is preferably anionic and has a carboxyl group or a carboxylic anhydride group. By using an anionic polymer dispersant, the dispersibility of inorganic powders such as conductive powders and ceramic powders in an organic vehicle can be further improved. Here, a carboxylic anhydride group is a group formed by the bonding of two carboxyl groups to H. 2This refers to the anhydride state where O is dehydrated. Examples include acid anhydrides such as phthalic anhydride and maleic anhydride, which are molecular units composed of two dehydrated carboxyl groups.

[0092] Anionic polymer dispersants preferably have graft chains, which are expected to improve solubility in various organic solvents.

[0093] The mass average molecular weight of the anionic polymer dispersant is preferably 1,000 to 100,000, more preferably 5,000 to 70,000, and even more preferably 10,000 to 60,000. By making the mass average molecular weight of the polymer dispersant 1,000 or more, the dispersibility of the inorganic powder in the organic vehicle can be improved. If the mass average molecular weight is greater than 100,000, the compatibility with the organic vehicle and organic solvent may decrease, particles such as conductive powder and ceramic powder may aggregate, and the dispersibility and storage stability may decrease.

[0094] Such polymer dispersants have carboxyl or carboxylic anhydride groups as functional groups in the main chain. For anionic polymer dispersants, it is desirable to further include oxyethylene groups in the graft chains in order to adsorb inorganic powders.

[0095] The anionic polymer dispersant may contain one or more types. That is, multiple types of polymer dispersants may be contained depending on the length of the main chain, the length of the graft chain, the presence or absence of the graft chain, etc. The content of the anionic polymer dispersant in the conductive paste can be appropriately selected taking into consideration the viscosity, stickiness, long-term storage stability, etc. of the conductive paste, and may be contained within a range that does not impair the effects of the present invention.

[0096] For example, the amount of anionic polymer dispersant added per 100 parts by mass of conductive metal powder is preferably 0.01 to 5.00 parts by mass, and more preferably 0.20 to 2.00 parts by mass. If the amount of dispersant added is less than 0.01 part by mass, sufficient dispersibility tends to be difficult to obtain. On the other hand, if the amount of dispersant added exceeds 5.00 parts by mass, problems such as poor drying properties and a decrease in dry film density may occur.

[0097] Known examples of such anionic polymer dispersants include copolymers of maleic anhydride and polyoxyalkylenes having terminal allyl groups, copolymers of acrylic acid and polyoxyalkylenes having terminal allyl groups, and copolymers of these compounds with styrene. Examples of structural formulas of such anionic polymer dispersants include the structural formulas (1) to (3) shown in the following [Chemical Formula 1] to [Chemical Formula 3]. For example, in Formulas (1) to (3), R is an alkyl group, m is an integer of 2 to 30, and n is an integer of 10 to 30. Furthermore, R is preferably an alkyl group having 5 to 30 carbon atoms, more preferably an alkyl group having 8 to 25 carbon atoms, and particularly preferably an alkyl group having 10 to 20 carbon atoms.

[0098]

[0099]

[0100]

[0101] The conductive paste of this embodiment may contain a dispersant other than the anionic polymer dispersant. For example, the dispersant (surfactant) may include an acid dispersant including a higher fatty acid, phosphoric acid, a polymer surfactant, etc., a cationic dispersant other than the acid dispersant, a nonionic dispersant, an amphoteric surfactant, and a polymer dispersant.

[0102] The content of the dispersant in the conductive paste can be appropriately selected in consideration of the viscosity, stickiness, long-term storage properties, etc. of the conductive paste, and may be contained within a range that does not impair the effects of the present invention.

[0103] Furthermore, for both anionic polymer dispersants and other dispersants, the mass-average molecular weight of the dispersant is preferably 200 to 100,000. It is more preferably 300 to 30,000. A mass-average molecular weight less than 200 may result in reduced particle dispersibility and storage stability. Typically, a paste with excellent dispersibility is obtained by adsorbing the dispersant to the particle surface to form a dispersant adsorption layer, which imparts electrostatic and steric repulsive forces to the particles. However, over time, collisions between particles are thought to overcome the repulsive forces of the adsorption layer, causing the particles to aggregate. Therefore, a mass-average molecular weight of 200 or greater is preferable. Furthermore, a mass-average molecular weight greater than 100,000 may result in reduced compatibility with organic vehicles and organic solvents, particle aggregation, and reduced dispersibility and storage stability. This may also result in increased paste viscosity.

[0104] The total amount of the anionic polymer dispersant and other dispersants added is preferably 0.01 to 5.00 parts by mass, and more preferably 0.20 to 2.00 parts by mass, per 100 parts by mass of the conductive metal powder. If the amount of dispersant is less than 0.01 part by mass, it tends to be difficult to obtain sufficient dispersibility. On the other hand, if the amount exceeds 5.00 parts by mass, problems such as poor drying properties and a decrease in dry film density may occur.

[0105] (Method for Producing Conductive Paste) The method for producing the conductive paste of this embodiment is not particularly limited, and conventionally known methods can be used. The conductive paste can be produced, for example, by preparing the above-mentioned components and stirring and kneading them using a triple-roll mill, a ball mill, a mixer, or the like. In this case, if a dispersant is applied to the surface of the conductive powder in advance, the conductive powder is sufficiently loosened without agglomeration, allowing the dispersant to be distributed evenly across the surface, making it easier to obtain a uniform conductive paste. Alternatively, the binder resin may be dissolved in an organic solvent for the vehicle to produce an organic vehicle, and the conductive powder, ceramic powder, organic vehicle, and dispersant may be added to the organic solvent for the paste, followed by stirring and kneading using a mixer to produce the conductive paste.

[0106] In addition, the organic solvent for the vehicle is preferably the same as the organic solvent for the paste that adjusts the viscosity of the conductive paste, in order to improve the compatibility of the organic vehicle. The content of the organic solvent for the vehicle is, for example, 5 parts by mass or more and 80 parts by mass or less relative to 100 parts by mass of the conductive powder. The content of the organic solvent for the vehicle is preferably 10% by mass or more and 40% by mass or less relative to the total amount of the conductive paste.

[0107] The surface smoothness of a dry film formed by printing a conductive paste can be evaluated by its surface roughness. The surface roughness of the conductive paste can be measured, for example, by the method described in the Examples (a method of measuring the arithmetic mean height Sa according to ISO 25178 using a VK-X120 manufactured by Keyence Corporation). When the surface smoothness of the dry film is evaluated by the arithmetic mean height Sa, the value is preferably 0.10 μm or less.

[0108] [Electronic Components, Multilayer Ceramic Capacitors] The conductive paste of the present invention can be suitably used in electronic components such as multilayer ceramic capacitors. The multilayer ceramic capacitor has dielectric layers formed using green sheets and internal electrode layers formed using the conductive paste.

[0109] In the multilayer ceramic capacitor, it is preferable that the dielectric ceramic powder contained in the green sheet and the ceramic powder contained in the conductive paste are powders of the same composition, and for example, barium titanate can be used. In the multilayer ceramic capacitor manufactured using the conductive paste of this embodiment, sheet attack and peeling failure of the green sheet are suppressed even when the thickness of the green sheet is, for example, 3 μm or less.

[0110] Hereinafter, embodiments of electronic components and the like of the present invention will be described with reference to the drawings. The drawings may be represented schematically or at a different scale as appropriate. Furthermore, the positions and directions of components will be described with reference to an XYZ Cartesian coordinate system as shown in FIG. 1 and other figures. In this XYZ Cartesian coordinate system, the X and Y directions are horizontal, and the Z direction is vertical (up-down).

[0111] 1A and 1B are a perspective view and a side cross-sectional view showing a multilayer ceramic capacitor 1, which is an example of an electronic component according to an embodiment. The multilayer ceramic capacitor 1 includes a ceramic laminate 10 in which dielectric layers 12 and internal electrode layers 11 are alternately stacked, and external electrodes 20.

[0112] A method for manufacturing a multilayer ceramic capacitor 1 using the above-described conductive paste will now be described. First, the conductive paste is printed on a dielectric layer made of a green sheet and dried to form a dry film. A plurality of dielectric layers, each having this dry film on its upper surface, are stacked and pressure-bonded to obtain a laminate, which is then fired and integrated to produce a ceramic laminate 10 in which internal electrode layers 11 and dielectric layers 12 are alternately stacked. A pair of external electrodes 20 is then formed on both ends of the ceramic laminate 10 to manufacture the multilayer ceramic capacitor 1. This method will now be described in more detail.

[0113] First, a green sheet is prepared, which is an unfired ceramic sheet made of a dielectric material. Examples of such green sheets include a dielectric layer paste obtained by adding an organic binder such as polyvinyl butyral and a solvent such as terpineol to a predetermined ceramic raw material powder such as barium titanate, and then coating the paste on a support film such as a PET film in a sheet form and drying it to remove the solvent. The thickness of the dielectric layer made of the green sheet is not particularly limited, but is preferably 0.05 μm or more and 3 μm or less in view of the demand for miniaturization of multilayer ceramic capacitors.

[0114] Next, the conductive paste is printed (applied) on one side of this green sheet by a known method such as screen printing, and then dried to form a dry film, to prepare a plurality of sheets. Note that, from the viewpoint of the requirement for thinning of the internal electrode layer 11, the thickness of the conductive paste (dry film) after printing is preferably set to a thickness such that the thickness of the dry film after drying is 1 μm or less.

[0115] Next, the green sheet is peeled off from the support film, and the dielectric layers made of the green sheet and the dry film formed on one side thereof are stacked alternately, and then a laminate is obtained by heat and pressure treatment. Note that a configuration in which protective green sheets not coated with conductive paste are further placed on both sides of the laminate may be adopted.

[0116] Next, the laminate is cut to a predetermined size to form green chips, and the green chips are subjected to a binder removal treatment and fired in a reducing atmosphere to produce the ceramic laminate 10. The binder removal treatment is preferably performed in air or an N2 gas atmosphere. The temperature during the binder removal treatment is, for example, 200°C or higher and 400°C or lower. The temperature is preferably maintained for 0.5 hours or higher and 24 hours or lower during the binder removal treatment. The firing is performed in a reducing atmosphere to suppress oxidation of the metals used in the internal electrode layers. The temperature during firing of the laminate is, for example, 1000°C or higher and 1350°C or lower, and the temperature is preferably maintained for 0.5 hours or higher and 8 hours or lower during the firing treatment.

[0117] By firing the green chip, the organic binder in the green sheet is completely removed, and the ceramic raw material powder is fired to form the ceramic dielectric layer 12. Also, the organic vehicle in the dried film is removed, and the nickel powder or the alloy powder mainly composed of nickel is sintered or melted and integrated to form the internal electrode layer 11, thereby forming a fired multilayer ceramic body in which a plurality of dielectric layers 12 and internal electrode layers 11 are alternately stacked. Note that, from the viewpoint of taking oxygen into the dielectric layer to increase reliability and suppressing reoxidation of the internal electrodes, the fired multilayer ceramic body may be subjected to an annealing treatment.

[0118] Then, a pair of external electrodes 20 is provided on the produced fired multilayer ceramic body, thereby producing the multilayer ceramic capacitor 1. For example, the external electrodes 20 include an external electrode layer 21 and a plating layer 22. The external electrode layer 21 is electrically connected to the internal electrode layer 11. Note that, for example, copper, nickel, or an alloy thereof can be suitably used as the material for the external electrodes 20. Note that the electronic component is not limited to a multilayer ceramic capacitor, and may be an electronic component other than a multilayer ceramic capacitor, such as a varistor.

[0119] EXAMPLES The present invention will be described in detail below based on examples and comparative examples, but the present invention is not limited to these examples.

[0120] [Materials Used] (Conductive Powder) Ni powder (number average particle size measured by SEM: 0.2 μm) was used as the conductive powder.

[0121] (Ceramic Powder) As the ceramic powder, barium titanate (BaTiO 3 (number average particle size measured by SEM: 0.05 μm) was used.

[0122] (Binder Resin) The binder resin was synthesized as follows.

[0123] (Synthesis of Cellulose-Based Compound (1a) Having a Vinyl Group) Ethyl cellulose ("Ethocel STD-100" manufactured by Dow Chemical, number average molecular weight Mn (value calculated as standard polystyrene by GPC): 63,420, average number of unetherified hydroxyl groups per glucose ring: 0.48) was prepared and dried.

[0124] A solution was obtained by dissolving 100 parts by mass of the dried ethyl cellulose in 900 parts by mass of ethyl acetate. To the obtained solution, 0.09 parts by mass of 3-allyloxypropionic acid, which corresponds to an average of 0.5 vinyl groups per molecule of ethyl cellulose, 0.10 parts by mass of diisopropylcarbodiimide as a condensing agent, and 0.002 parts by mass of dimethylaminopyridine as a reaction accelerator were added, and the mixture was stirred at a temperature of 40°C for 5 hours to carry out the reaction. Thereafter, the ethyl acetate was removed to obtain a cellulose-based compound (1a) in which vinyl groups had been introduced into ethyl cellulose as a solid.

[0125] A portion of the obtained solid was analyzed by FT-IR and H-NMR, confirming the formation of an ester bond and the introduction of vinyl groups into the ethyl cellulose in the same molar amount as the charged 3-allyloxypropionic acid.

[0126] In addition to the compound in which a vinyl group has been introduced into ethyl cellulose, the cellulose-based compound (1a) also contains unreacted ethyl cellulose. In the examples, this mixture is referred to as the cellulose-based compound (1a).

[0127] (Synthesis of Polyvinyl Butyral-Based Compound (1b) Having Thiol Groups) Polyvinyl butyral ("BM-SZ" manufactured by Sekisui Chemical Co., Ltd., number average molecular weight Mn (value calculated as standard polystyrene by GPC): 55,000, amount of hydroxyl groups: approximately 22 mol%) was prepared and dried. 100 parts by mass of the dried polyvinyl butyral was dissolved in 900 parts by mass of ethyl acetate. To the resulting solution, 0.10 parts by mass of 3-mercaptopropionic acid, corresponding to an average of 0.5 thiol groups introduced per molecule of polyvinyl butyral, 0.12 parts by mass of diisopropylcarbodiimide as a condensing agent, and 0.003 parts by mass of dimethylaminopyridine as a reaction accelerator were added, and the mixture was stirred at a temperature of 40°C for 5 hours to carry out a reaction. The ethyl acetate was then removed to obtain a solid polyvinyl butyral-based compound (1b) in which thiol groups had been introduced into polyvinyl butyral.

[0128] A portion of the obtained solid was analyzed by FT-IR and H-NMR, and it was confirmed that an ester bond was formed, and that a thiol group in the same molar amount as the charged 3-mercaptopropionic acid was introduced into the polyvinyl butyral.

[0129] The polyvinyl butyral-based compound (1b) contains a compound in which a thiol group has been introduced into polyvinyl butyral as well as unreacted polyvinyl butyral, and in the examples, this mixture is referred to as the polyvinyl butyral-based compound (1b).

[0130] (Synthesis of Polymer Compound 1) 5 parts by mass of cellulose compound (1a) and 4.35 parts by mass of polyvinyl butyral compound (1b) were dissolved in 60 parts by mass of dihydroterpineol solvent, and the solution was transferred to a glass flask reaction vessel. After nitrogen substitution, 0.1 parts by mass of azobisisobutyronitrile as a radical generator was added to the solution, and the reaction was carried out at 80 ° C. for 3 hours with stirring to obtain an organic vehicle 1 containing polymer compound 1. Here, the cellulose compound (1a) and the polyvinyl butyral compound (1b) have the same molar number, and as described above, an average of 0.5 thiol groups were introduced per molecule of polyvinyl butyral. Therefore, the molar ratio of sulfur atoms contained in polymer compound 1 to the total of cellulose and cellulose compound was 0.5. Organic vehicle 1 contained 13.5% by mass of polymer compound 1. Here, polymer compound 1 is a mixture of a polymer compound in which a cellulose compound (1a) and a polyvinyl butyral compound (1b) are bonded together, unreacted ethyl cellulose, and unreacted polyvinyl butyral, and in the examples, this mixture is referred to as polymer compound 1.

[0131] Furthermore, the produced polymer compound 1 was analyzed by FT-IR and 1H-NMR, and the presence of an -S- bond was confirmed, indicating that the target structure had been obtained. Furthermore, the number average molecular weight (Mn: standard polystyrene equivalent value measured by GPC) of polymer compound 1 was measured.

[0132] Table 1 shows the characteristics of the cellulose compound (1a) and polyvinyl acetal compound (1b) used in polymer compound 1.

[0133]

[0134] Example 1: A conductive paste was prepared by mixing 47% by weight of Ni powder, 4.7% by weight of ceramic powder, 26.67% by weight of organic vehicle 1, 0.4% by weight of an anionic polymer dispersant of polymeric polycarboxylic acid having the structural formula (1) above (R is an alkyl group having 5 to 30 carbon atoms, with a mass average molecular weight of 40,000), and 21.23% by weight of organic solvent (dihydroterpineol), for a total weight of 100%. The conductive paste was printed and dried as follows, and the surface roughness and adhesion to the green sheet were evaluated. The evaluation results are shown in Table 2 and Figure 2.

[0135] [Evaluation Method] (Dispersibility: Surface Roughness of Dried Film and Adhesion to Green Sheet) <Surface Roughness> The prepared conductive paste was screen-printed onto a 2.54 cm (1 inch) square piece of heat-resistant tempered glass and dried at 120°C in air for 1 hour to prepare a 20 mm square dried film with a thickness of 1 to 3 μm. If the conductive paste has good dispersibility, the surface of the dried film will be smooth. If the dispersibility is poor, aggregation will occur within the conductive paste, causing the surface of the dried film to become rough and its surface smoothness to decrease. Therefore, the surface roughness Sa (arithmetic mean height) of the prepared dried film was measured using a laser microscope (Keyence VK-X120) in accordance with ISO 25178. The smaller the surface roughness Sa (arithmetic mean height), the smoother the surface of the dried film. The obtained dried film was also observed using a SEM.

[0136] <Adhesion between dried film and green sheet> The prepared conductive paste was applied to a 2.54 cm (1 inch) square BaTiO 3 The printing machine was adjusted so that the thickness of the printed film on the dielectric green sheet would be 3.6 μm, and a 2 cm square pattern was printed. After printing, the green sheet was dried at 120° C. for 20 minutes to form a dry film of the conductive paste on the surface of the green sheet. Next, BaTiO 3 The dielectric green sheet was placed on top, and the dried film of the conductive paste and the BaTiO 3 The dielectric green sheets were thermocompressed to form a laminate. The dried film of the conductive paste and the BaTiO 3By measuring the force required to peel off the dielectric green sheet, the dry film of the conductive paste and the BaTiO 3 The adhesion to the dielectric green sheet was evaluated. This adhesion was measured using a thin film adhesion strength measuring instrument (Romulus manufactured by Phototechnica Corporation). Specifically, the process of evaluating adhesion using the thin film adhesion strength measuring instrument was as follows: an aluminum stud pin coated with an epoxy adhesive was attached vertically to the center of the laminate, and a sample for adhesion evaluation with the stud pin attached vertically was prepared. The stud pin of the sample was then pulled away from the surface of the laminate, thereby separating the dried film of the conductive paste from the BaTiO 3 The adhesiveness of the dielectric green sheets was evaluated. The evaluation results of the adhesiveness are shown as relative evaluation results, with the adhesive strength of Comparative Example 1 described later being set at 100.

[0137] Comparative Example 1 A conductive paste was prepared and evaluated in the same manner as in Example 1, except that an anionic dispersant of an amide compound of an amino acid and a fatty acid (hereinafter referred to as Dispersant B, molecular weight 353) was used. The results are shown in Table 2 and FIG. 2.

[0138]

[0139] [Evaluation Results] As shown in Table 2, the dried film formed using the conductive paste of Example 1 had a surface roughness Sa (arithmetic mean height) of 0.06 μm, which was lower than that of Comparative Example 1. Furthermore, as shown in the SEM photograph in Table 2, it can be seen that the film had fewer irregularities than that of Comparative Example 1.

[0140] In contrast, the dry film formed using the conductive paste of Comparative Example 1 had a surface roughness Sa of 0.9 μm, which was rougher than that of Example 1. Furthermore, as shown in the SEM photograph in Table 2, the film had larger irregularities than that of Example 1.

[0141] Furthermore, according to FIG. 2, the dry film of Example 1, which has a superior surface roughness Sa, has a BaTiO 3 It is clear that the adhesiveness to the dielectric green sheet is excellent.

[0142] The conductive paste according to this embodiment, which uses finely divided conductive powders or ceramic powders, can provide a conductive paste having a smooth dry film and excellent adhesion, and can therefore be suitably used as a raw material for internal electrodes of multilayer ceramic capacitors, which are chip components (electronic components) in electronic devices such as mobile phones and digital devices.

[0143] REFERENCE SIGNS LIST 1 Multilayer ceramic capacitor 10 Ceramic laminate 11 Internal electrode layer 12 Dielectric layer 20 External electrode 21 External electrode layer 22 Plated layer

Claims

1. A conductive paste comprising a conductive powder, a ceramic powder, a dispersant, a binder resin, and an organic solvent, wherein the binder resin comprises cellulose, polyvinyl acetal, and a polymer compound in which a cellulose-based compound and a polyvinyl acetal-based compound are bonded together by sulfur atoms, the molar ratio of sulfur atoms contained in the polymer compound to the total of the cellulose and the cellulose-based compound is 0.3 to 1.7, and the dispersant is an anionic polymer compound.

2. The conductive paste according to claim 1, wherein the dispersant has a carboxy group or a carboxylic acid anhydride group.

3. The conductive paste according to claim 1 or 2, wherein the cellulose compound is a cellulose derivative having a thiol group or a vinyl group, the polyvinyl acetal compound is a polyvinyl acetal resin having a thiol group or a vinyl group, and when the cellulose derivative has a thiol group, the polyvinyl acetal resin has a vinyl group that reacts with the thiol group, and when the cellulose derivative has a vinyl group, the polyvinyl acetal resin has a thiol group that reacts with the vinyl group.

4. The conductive paste according to claim 3, wherein the cellulose derivative is ethyl cellulose having a thiol group or a vinyl group, and the polyvinyl acetal resin is polyvinyl butyral having a thiol group or a vinyl group.

5. The conductive paste according to claim 1, wherein the cellulose-based compound is a first esterification reaction product obtained by dehydration condensation of a carboxy group of a carboxylic acid having a thiol group or a vinyl group and a hydroxyl group of cellulose; the polyvinyl acetal-based compound is a second esterification reaction product obtained by dehydration condensation of a carboxy group of a carboxylic acid having a thiol group or a vinyl group and a hydroxyl group of polyvinyl acetal; when the first esterification reaction product has a thiol group, the second esterification reaction product has a vinyl group; when the first esterification reaction product has a vinyl group, the second esterification reaction product has a thiol group; and the polymer compound is a thiol-ene reaction product of the first esterification reaction product and the second esterification reaction product.

6. The conductive paste according to claim 5, wherein the first esterification reaction product is an esterification reaction product obtained by dehydration condensation of a carboxy group of 3-allyloxypropionic acid and a hydroxy group of ethyl cellulose, and the second esterification reaction product is an esterification reaction product obtained by dehydration condensation of a carboxy group of 3-mercaptopropionic acid and a hydroxy group of polyvinyl butyral.

7. The conductive paste according to claim 1 or 2, wherein the conductive powder is nickel powder.

8. The conductive paste according to claim 1, wherein the number average particle size of the conductive powder is 0.05 μm or more and 1.0 μm or less.

9. The conductive paste of claim 1, wherein the ceramic powder comprises barium titanate.

10. The conductive paste according to claim 1, wherein the number average particle size of the ceramic powder is 0.01 μm or more and 0.5 μm or less.

11. The conductive paste according to claim 1, wherein the content of the ceramic powder is 1% by mass or more and 20% by mass or less.

12. The conductive paste according to claim 1, which is used for internal electrodes of multilayer ceramic parts.

13. An electronic component formed using the conductive paste according to claim 1.

14. A multilayer ceramic capacitor comprising at least a laminate in which dielectric layers and internal electrode layers are laminated, the internal electrode layers being formed using the conductive paste according to claim 1.