Coated ultrahigh-strength steel with low spot welding crack sensitivity and manufacturing method therefor

MYPI2025001734A0Undetermined Publication Date: 2024-03-23BAOSHAN IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025001734
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-23
Filing Date
2023-09-25
Publication Date
2024-03-23

AI Technical Summary

Technical Problem

Existing zinc-coated ultra-high-strength steel is prone to cracks during spot welding, resulting in a decrease in welding performance, and it is difficult to effectively suppress the formation of cracks with existing technology.

Method used

By optimizing the chemical composition of the steel substrate, including the ratio of carbon, silicon, manganese, boron, molybdenum and other elements, a coated ultra-high-strength steel with low spot welding crack sensitivity is designed, and adopts thin slab continuous casting, hot rolling, acid The manufacturing method of washing, continuous annealing and plating zinc-containing coatings controls the microstructure and coating thickness of the steel plate and reduces the occurrence of surface cracks in solder joints.

Benefits of technology

It achieves high strength and high welding performance while significantly reducing the sensitivity of spot welding cracks. The maximum length of the cracks on the surface of the welding spot is less than 5% of the plate thickness, and improving the tensile strength and elongation of the steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025001734_DRAWING_001
    Figure PI2025001734_DRAWING_001
Patent Text Reader

Abstract

The present invention discloses coated ultrahigh-strength steel with low spot welding crack sensitivity, comprising a steel substrate and a zinc-containing coating on the surface of the steel substrate. The steel substrate contains Fe and inevitable impurity elements. The steel substrate further contains the following chemical elements in percentage by mass: 0.10-0.30% of C, 0.30-0.90% of Si, 1.00-2.20% of Mn, 0.001-0.003% of B, and 0.30-1.00% of Al. Correspondingly, the present invention further discloses a manufacturing method for the coated ultrahigh-strength steel. The coated ultrahigh-strength steel in the present invention can be effectively prepared by using the manufacturing method, the final yield strength is 600-850 MPa, the tensile strength is 980-1150 MPa, the uniform elongation is not less than 13%, and the elongation at break is not less than 15%.
Need to check novelty before this filing date? Find Prior Art

Description

A coated ultra-high strength steel with low spot welding crack sensitivity and a manufacturing method thereof Technical Field

[0001] The present invention relates to high-strength steel and a manufacturing method thereof, and in particular to ultra-high-strength steel with a coating and a manufacturing method thereof. Background Art

[0002] At present, with the advancement of automobile lightweighting and the increasing requirements of the automotive industry for vehicle corrosion resistance, many automakers are increasingly demanding coated ultra-high-strength steel. For cold-stamped steel, the coating is mainly zinc-containing coating, such as hot-dip pure zinc, hot-dip galvanized iron, and electroplated pure zinc. Resistance spot welding has become the most important connection method in automotive welding production due to its advantages such as fast welding speed and low cost. Many zinc-coated ultra-high-strength steel joints often exhibit good quasi-static mechanical properties when spot welded, but a welding crack appears on the surface of the steel plate in contact with the electrode and in the surrounding area. This welding crack is called a spot welding crack. Figure 1 schematically shows a schematic diagram of a spot welding crack in zinc-coated ultra-high-strength steel. However, it is very difficult to suppress the formation of this crack. Therefore, this crack has become a major obstacle and bottleneck in the application of zinc-coated ultra-high-strength steel in the automotive field.

[0003] There are some known technical solutions for controlling welding cracks in the prior art, but there are still many disadvantages:

[0004] For example, the Chinese patent document with publication number CN108015401A, publication date May 11, 2018, and titled “Resistance spot welding method for galvanized high-strength steel with good joint performance” discloses a method for suppressing spot weld surface cracks while ensuring that the performance of the weld joint is not reduced through innovation in the spot welding process.

[0005] For example, the Chinese patent document with publication number CN109385515A, published on February 26, 2019, and titled "Multi-layer steel and method for reducing liquid metal embrittlement", discloses a method for suppressing the occurrence of spot welding cracks in high-strength steel. The method suppresses the occurrence of spot welding cracks by first decarburizing the high-strength steel and then galvanizing it, so that the thickness of the decarburized layer is between 10 and 50 microns.

[0006] Another example is the Chinese patent document CN110892087A, published on March 17, 2020, and titled "Zinc-Coated Steel Sheet with High Resistance Spot Weldability." It discloses a technical solution for reducing spot weld cracking by increasing the dew point to form an inner oxide layer on the steel sheet, thereby improving the surface composition distribution. However, this technical solution suffers from the difficulty in controlling the thickness and uniformity of the inner oxide layer and the uniformity of the surface composition distribution of the steel sheet.

[0007] Summary of the Invention

[0008] One of the purposes of the present invention is to provide a coated ultra-high-strength steel with low spot welding crack sensitivity. The coated ultra-high-strength steel has very excellent quality and performance. While meeting the user's requirements for the performance of coated high-strength steel and the mechanical properties of spot welding joints, it also has low spot welding crack sensitivity and has good prospects for promotion and application.

[0009] To achieve the above objectives, the present invention provides a coated ultra-high-strength steel with low spot welding crack sensitivity, comprising a steel substrate and a zinc-containing coating on the surface of the steel substrate, wherein the steel substrate contains Fe and unavoidable impurity elements, and further contains the following chemical elements in the following mass percentages:

[0010] C: 0.10~0.30%; Si: 0.30~0.90%; Mn: 1.00~2.20%; B: 0.001~0.003%; Al: 0.30~1.00%.

[0011] Furthermore, in the coated ultra-high strength steel of the present invention, the mass percentage of each chemical element of the steel substrate is:

[0012] C: 0.10-0.30%; Si: 0.30-0.90%; Mn: 1.00-2.20%; B: 0.001-0.003%; Al: 0.30-1.00%; the remainder being Fe and unavoidable impurity elements.

[0013] Furthermore, in the coated ultra-high strength steel of the present invention, the chemical elements of the steel substrate further include Mo: 0.10-2.00%.

[0014] In the above-mentioned technical solution of the present invention, a chemical composition design based on carbon, silicon, manganese, boron or boron-molybdenum composite is adopted, which fully utilizes the role of carbon, silicon, manganese, boron and molybdenum elements in the phase transformation of the material, thereby achieving the unification of high mechanical properties and high spot welding performance of the ultra-high strength steel described in the present invention, and ultimately obtaining a coated ultra-high strength steel product with low spot welding crack sensitivity.

[0015] In the coated ultra-high strength steel of the present invention, the design principles of the chemical elements are as follows:

[0016] C: In the coated ultra-high-strength steel with low spot welding crack sensitivity described in the present invention, the solubility of carbon in austenite is much higher than its solubility in ferrite, which can prolong the incubation period before austenite transformation and reduce the Ms temperature. The higher the mass percentage of carbon in the steel, the greater the fraction of retained austenite, and the higher the enrichment of carbon in the retained austenite during partitioning, which is beneficial to enhancing the stability of retained austenite, producing the TRIP effect, and improving the ductility of the material. In addition, carbon is also the most basic solid solution strengthening element in steel. However, it should be noted that the carbon content in steel should not be too high. When the mass percentage of carbon is too high, the weldability of the steel will be reduced, and in particular, the tendency of surface cracks to occur at the weld point of the joint will be significantly increased. Based on this, in order to give full play to the beneficial effects of element C, in the present invention, the mass percentage of element C is controlled to be 0.10-0.30%.

[0017] Of course, in some preferred embodiments, in order to obtain better implementation effects, the mass percentage of the C element may be further preferably controlled to be between 0.15 and 0.20%.

[0018] Si: In the coated ultra-high strength steel with low spot welding crack sensitivity described in the present invention, the solubility of silicon in carbides is extremely small, which can strongly inhibit the formation of cementite during the partitioning treatment, promote the enrichment of carbon in the retained austenite, and improve the stability of the retained austenite. However, it should be noted that excessive silicon should not be added to the steel. Too high a silicon mass percentage will reduce the high-temperature plasticity of the steel and form stable oxides on the surface of the steel plate, reducing the wettability of the steel plate. In particular, the inventors of this case have found that silicon is an element that significantly increases the tendency of surface cracks in welds. Based on this, in the coated ultra-high strength steel with low spot welding crack sensitivity described in the present invention, the mass percentage of the Si element is specifically controlled to be 0.30 to 0.90%.

[0019] Of course, in some preferred embodiments, in order to obtain better implementation effects, the mass percentage of Si element may be further preferably controlled to be between 0.40 and 0.80%.

[0020] Mn: In the ultra-high strength steel with low spot welding crack sensitivity of the present invention, manganese can expand the austenite phase region and reduce Ac3, M s and M fPoint, improve austenite stability and steel hardenability, reduce the critical transformation rate, which is conducive to preserving retained austenite to room temperature. At the same time, manganese can also play a solid solution strengthening effect in steel. When the Mn content in the steel is too low, ferrite and pearlite banded structures will be produced at a low cooling rate due to segregation. In addition, the mass percentage of manganese in the steel should not be too high. When the mass percentage of manganese in the steel is too high, it will aggravate the grain coarsening trend, reduce the plasticity and toughness of the steel, and deteriorate the corrosion resistance. In particular, it will increase the enrichment of manganese in the shallow surface layer of the base material under the coating, increase the surface crack sensitivity of the weld spot of the joint, and deteriorate the welding performance. Based on this, in order to give full play to the beneficial effects of the Mn element, in the ultra-high strength steel with low spot welding crack sensitivity with coating described in the present invention, the mass percentage of the Mn element is controlled to be 1.00-2.20%.

[0021] Of course, in some preferred embodiments, in order to obtain better implementation effects, the mass percentage of the Mn element may be further preferably controlled between 1.00 and 2.00%.

[0022] B: In the coated ultra-high-strength steel with low spot weld crack sensitivity described herein, boron significantly improves the steel's hardenability. On the one hand, boron tends to segregate at grain boundaries, filling grain boundary defects and reducing grain boundary energy. This makes it more difficult for new phases to nucleate at austenite grain boundaries, which are typically ferrite nucleation sites, thereby enhancing austenite stability and improving hardenability. On the other hand, the addition of boron reduces the steel's demand for hardenability-enhancing elements such as carbon and manganese.

[0023] In addition, the inventors of this case also discovered that boron can reduce the segregation of manganese at grain boundaries, thereby reducing the formation of a manganese enrichment layer in the steel matrix under the coating, thereby significantly reducing the formation of spot welding cracks. However, the higher the boron content, the better. When the grain boundary defects are filled, if there is still more non-equilibrium boron segregation, a "boron phase" precipitate will form at the grain boundary, increasing the grain boundary energy. At the same time, the "boron phase" will serve as the core of the new phase, promoting the increase in nucleation rate, reducing the stability of austenite, and reducing hardenability. In other words, the obvious precipitation of "boron phase" has a negative impact on hardenability, and a large amount of "boron phase" precipitation will make the steel brittle, which has a negative impact on the mechanical properties of the steel; and the brittle grain boundaries will promote the occurrence and expansion of spot welding cracks.

[0024] The inventors of this case have discovered that a boron content of 0.0030% is the inflection point for grain boundary embrittlement. Based on this, to maximize the beneficial effects of boron, the mass percentage of boron in the coated ultra-high-strength steel with low spot weld crack sensitivity described in this invention is controlled to 0.001-0.003%.

[0025] Of course, in some preferred embodiments, in order to obtain better implementation effects, the mass percentage of the B element may be further preferably controlled to be between 0.0015% and 0.003%.

[0026] Al: In the coated ultra-high-strength steel with low spot welding crack sensitivity described in the present invention, aluminum, when present in a solid solution, can increase stacking fault energy, inhibit cementite precipitation and the transformation from γ to martensite, and improve austenite stability. Furthermore, aluminum forms fine, dispersed, insoluble particles with carbon and nitrogen, which can refine grains. However, aluminum's strengthening effect is weaker than silicon, and its ability to stabilize austenite is also weaker than silicon. Furthermore, when the weight percentage of aluminum in the steel is too high, a large amount of oxide inclusions is easily formed, which is not conducive to steelmaking and continuous casting. Therefore, in the coated ultra-high-strength steel with low spot welding crack sensitivity described in the present invention, the weight percentage of Al is controlled to be between 0.30 and 1.00%.

[0027] Mo: In the coated ultra-high-strength steel with low spot welding crack sensitivity described herein, molybdenum shifts the C curve to the right and lowers the Ms point, thereby improving the steel's hardenability and increasing both strength and elongation. Furthermore, molybdenum is a strong carbide-forming element. During smelting, it forms fine, dispersed MoC particles, which are subsequently distributed in the martensite as a hard second phase during phase transformation, significantly enhancing the steel's toughness. More importantly, the inventors of this application have discovered that the addition of molybdenum significantly improves the steel's resistance to spot welding cracking. Based on this, and taking into account the aforementioned factors and the cost of molybdenum addition, the weight percentage of Mo in the coated ultra-high-strength steel with low spot welding crack sensitivity described herein is controlled between 0.10 and 2.00%. In some embodiments, the weight percentage of Mo is controlled between 0.15 and 2.00%.

[0028] Of course, in some preferred embodiments, in order to obtain better implementation effects, the mass percentage of the Mo element can be further preferably controlled between 0.10 and 1.00%. In some embodiments, the mass percentage of the Mo element is controlled between 0.15 and 1.00% or between 0.20 and 1.00%.

[0029] Furthermore, in the coated ultra-high strength steel of the present invention, the mass percentage of each chemical element of the steel substrate satisfies at least one of the following:

[0030] C: 0.15~0.20%;

[0031] Si: 0.40~0.80%;

[0032] Mn: 1.00~2.00%;

[0033] B: 0.0015~0.003%;

[0034] Mo: 0.10~1.00%.

[0035] Furthermore, in the coated ultra-high strength steel of the present invention, the mass percentage of the inevitable impurity elements of the steel substrate satisfies: P≤0.01%, S≤0.005%.

[0036] In the above technical solution, P and S elements are both impurity elements in the coated ultra-high-strength steel described in the present invention. When technical conditions permit, in order to obtain steel with better performance and higher quality, the content of impurity elements in the coated ultra-high-strength steel should be reduced as much as possible.

[0037] In the present invention, P and S are both impurity elements. Although P can play a role in solid solution strengthening, inhibit the formation of carbides, and is beneficial to improving the stability of retained austenite, too high a mass percentage of P will weaken the grain boundaries, increase the brittleness of the material, and deteriorate the welding performance. In other words, the positive effect of the P element is weaker than its negative effect. Therefore, the mass percentage of P is preferably controlled to P≤0.01%.

[0038] Accordingly, the S element in steel tends to form a low-melting eutectic at the grain boundaries. When its mass percentage is too high, the plasticity of the material will be significantly deteriorated. Therefore, the mass percentage of the S element is controlled to S≤0.005%.

[0039] Furthermore, in the coated ultra-high strength steel of the present invention, the microstructure of the steel substrate is ferrite+martensite+retained austenite.

[0040] Furthermore, in the coated ultra-high strength steel of the present invention, the volume proportion of ferrite is 25% to 45%; and / or the volume proportion of martensite is 45% to 65%.

[0041] Furthermore, in the coated ultra-high strength steel of the present invention, in the ferrite, the volume proportion of grains with a size of less than 10 μm is ≥85%, and the volume proportion of grains with a size of less than 5 μm is ≥55%.

[0042] Furthermore, in the coated ultra-high strength steel of the present invention, the average grain size of the retained austenite is ≤2 μm; and / or the average C content in the retained austenite is ≥1.0%, such as 1.0-1.3%.

[0043] Furthermore, in the coated ultra-high-strength steel described in the present invention, the "low spot welding crack sensitivity" means that no surface cracks are generated at the weld point when welding is performed using the spot welding process, or, if surface cracks are generated at the weld point, the maximum length of the surface cracks at the weld point is less than 5% of the plate thickness, preferably less than 3% of the plate thickness, and more preferably less than 1% of the plate thickness.

[0044] Furthermore, in the coated ultra-high-strength steel described in the present invention, its mechanical properties meet the following requirements: its yield strength is ≥600MPa, such as ≥700MPa, preferably ≥750MPa; its tensile strength is ≥980MPa, preferably ≥1040MPa; its uniform elongation is ≥13%, preferably ≥15.5%; its elongation at break is ≥15%, preferably ≥20%, and more preferably ≥22.5%.

[0045] Furthermore, in the coated ultra-high strength steel described in the present invention, its mechanical properties meet the following requirements: its yield strength is 600MPa~850MPa, its tensile strength is 980MPa~1150MPa, its uniform elongation is not less than 13%, and its elongation at break is not less than 15%.

[0046] Furthermore, in the coated ultra-high strength steel described in the present invention, its mechanical properties meet the following requirements: its yield strength is 755-845 MPa, its tensile strength is 1040-1140 MPa, its uniform elongation is 14.7-16.4%, and its elongation at break is between 22.6-25.4%.

[0047] Furthermore, in the coated ultra-high strength steel described in the present invention, the coating is a pure zinc coating, a zinc-iron alloy coating, a zinc-aluminum-magnesium coating or an aluminum-zinc coating.

[0048] Furthermore, in the coated ultra-high strength steel of the present invention, the coating weight is 30 to 120 g / m 2 , preferably 50 to 100 g / m 2 .

[0049] Accordingly, another object of the present invention is to provide a method for manufacturing coated ultra-high strength steel, which is simple to produce and the resulting high-strength steel has significantly improved spot welding performance, especially the ability to resist surface cracks in weld spots, under the same mechanical property conditions.

[0050] In order to achieve the above object, the present invention proposes a method for manufacturing coated ultra-high strength steel, which specifically comprises the following steps:

[0051] (1) Smelting and thin plate continuous casting;

[0052] (2) heating;

[0053] (3) Hot rolling: The thickness of the oxide scale on the surface of the steel strip after hot rolling is controlled to be ≤4 μm, and the mass percentage of FeO+Fe3O4 in the oxide scale on the surface of the steel strip after hot rolling is ≤50 wt%;

[0054] (4) pickling, or pickling + cold rolling;

[0055] (5) Continuous annealing: annealing at 800-920°C, then slowly cooling to 700-770°C at a cooling rate of 3-10°C / s; then rapidly cooling to 200-300°C at a cooling rate of 50-500°C / s (e.g., 100-500°C / s, 200-500°C / s, or 400-500°C / s); then heating to 360-460°C, holding for 50-600s; finally cooling to room temperature;

[0056] (6) Coating with zinc coating.

[0057] In the technical solution described in this invention, the manufacturing method utilizes a thin slab continuous casting process in conjunction with pickling or pickling rolling, followed by continuous annealing and coating, to produce coated ultra-high-strength steel with low spot welding crack sensitivity. The coated ultra-high-strength steel produced by this manufacturing method can be welded using conventional spot welding processes used in automotive plants, with the maximum length of surface cracks at the welds being less than 5% of the plate thickness, demonstrating very low spot welding crack sensitivity and excellent quality.

[0058] In the above step (1) of the present invention, since thin slab continuous casting is used, the rough rolling process can be omitted, the hot rolling deformation is reduced, and the steel plate performance in the subsequent steps (4) and (5) is guaranteed. In addition, since thin slab continuous casting is used in step (1), it can fully utilize the heat of the slab and reduce the energy consumption required for heating, thereby obtaining a more uniform ferrite or ferrite + pearlite structure, which is conducive to maintaining a certain amount of fine-grained ferrite in the microstructure of the finished substrate in step (6), thereby improving the uniformity of the structure.

[0059] In step (2), controlling the thickness of the oxide scale on the surface of the hot-rolled steel strip to be ≤4 μm and the content of (FeO+Fe3O4) in the oxide scale on the surface of the hot-rolled steel strip to be ≤50 wt% is beneficial to the subsequent step (4) and has an important influence on the performance of the steel plate obtained after continuous annealing. This is because: in the technical solution described in the present invention, FeO and Fe3O4 are more difficult to pickle than Fe2O3, and controlling the thickness of the oxide scale on the surface of the hot-rolled steel strip prepared by the present invention and the content of (FeO+Fe3O4) in the oxide scale on the surface of the hot-rolled steel strip to be ≤50 wt% can effectively improve the pickling effect and obtain a pickled plate surface that can be used for direct continuous annealing. Since the pickled plate can be directly annealed continuously, the deformation of the hot-rolled structure is small, and the steel plate structure is mainly pearlite and ferrite. Therefore, under the same continuous annealing conditions, the material strength can be reduced, the structure can be made more uniform, and excellent ductility can be obtained.

[0060] Accordingly, in step (5), the inventors optimized the design of the continuous annealing process, which can form a homogenized austenite structure or austenite + ferrite structure by controlling the annealing temperature to 800-920 ° C.; then slowly cooling to 700-770 ° C at a cooling rate of 3-10 ° C / s to further adjust the ferrite content in the structure and obtain a certain proportion of ferrite, thereby improving the plasticity of the material; then cooling to 200-300 ° C (i.e., between M s (starting temperature of martensitic transformation) and M f (martensitic transformation end temperature), at which point the austenite partially transforms into martensite, which can ensure that the steel obtains higher strength; then, it is heated to 360-460℃ and kept warm for 50-600s, which can partition carbon in martensite and austenite, forming a certain amount of carbon-rich retained austenite, which is stable to room temperature. Due to the TRIP effect, the work hardening ability and formability of the steel can be significantly improved, and a high-strength steel plate with excellent ductility can be obtained.

[0061] In addition, in view of the inventors' understanding of the effects of carbon, silicon, manganese, boron or boron-molybdenum on spot welding cracks, especially the understanding that silicon and manganese are easily enriched in the shallow surface layer of the steel plate and significantly increase the sensitivity of the weld surface cracks, the present invention not only strictly limits the carbon, silicon, manganese, boron or boron-molybdenum content of the steel during composition design, but also reduces the content of carbon, silicon and manganese elements compared with steels of the same strength grade, and adds boron and molybdenum elements to increase the hardenability of the steel, thereby ensuring that the required microstructure composition is obtained in step (5), and ensuring that the ultra-high strength steel containing zinc coating obtained after step (6) has low spot welding crack sensitivity, that is, the maximum length of the weld surface crack is less than 5% of the plate thickness.

[0062] It should be noted that, when the zinc-containing coating is plated in step (6), the zinc-containing coating can be produced by, but is not limited to, hot-dip, electroplating, or vacuum plating techniques.

[0063] In summary, the coated ultra-high-strength steel designed in this invention utilizes a chemical composition of carbon, silicon, manganese, boron, aluminum, and molybdenum, along with ferrite grain refinement. Consequently, during continuous annealing, the number of nucleation sites for reverse austenite transformation increases, further refining the grain size. This results in a stable average retained austenite grain size of ≤2 μm at room temperature, and an average carbon content of ≥1.0% in the retained austenite.

[0064] Furthermore, in the method for manufacturing coated ultra-high strength steel of the present invention, in step (1), the thickness of the slab at the outlet end of the thin strip continuous casting is controlled to be 50 to 58 mm.

[0065] Furthermore, in the method for manufacturing coated ultra-high strength steel of the present invention, in step (1), the drawing speed of the thin strip continuous casting is controlled to be 2 to 5 m / min.

[0066] Furthermore, in the method for manufacturing coated ultra-high strength steel of the present invention, in step (2), the slab is heated to 1200-1250°C.

[0067] Furthermore, in the method for manufacturing coated ultra-high strength steel of the present invention, in step (3), the finishing rolling temperature is controlled to be 860-930°C, and the coiling temperature is controlled to be 450-600°C.

[0068] Furthermore, in the method for manufacturing coated ultra-high strength steel of the present invention, in step (4), when pickling + cold rolling is adopted, the cold rolling deformation is controlled to be 40% to 60%.

[0069] Furthermore, in the method for manufacturing coated ultra-high strength steel of the present invention, in step (5), the volume content of hydrogen in the reducing atmosphere in the continuous annealing furnace is controlled to be 10-15%.

[0070] Furthermore, in the method for manufacturing coated ultra-high strength steel according to the present invention, the annealing process parameters of step (5) satisfy at least one of the following:

[0071] Annealing temperature is 820~870℃;

[0072] Slowly cool to 700-730°C at a cooling rate of 3-10°C / s;

[0073] Rapid cooling to 250-300℃;

[0074] After rapid cooling, heat again to 400-430°C and keep warm for 180-300 seconds.

[0075] Compared with the prior art, the coated ultra-high strength steel with low spot welding crack sensitivity and the manufacturing method thereof of the present invention have the following advantages and beneficial effects:

[0076] In the coated ultra-high-strength steel designed by the present invention, its chemical element composition is based on C, Si, Mn, B, Al and Mo. By optimizing the ratio of each element, a coated ultra-high-strength steel with low spot welding crack sensitivity can be obtained.

[0077] The coated ultra-high strength steel with low spot welding crack sensitivity described in the present invention has very excellent quality and performance. While meeting the user's requirements for the performance of coated high-strength steel and the mechanical properties of spot welding joints, it also has low spot welding crack sensitivity.

[0078] The coated ultra-high-strength steel prepared using the technical solution of the present invention includes a steel substrate and a zinc-containing coating on the surface of the steel substrate. Its mechanical properties meet the following requirements: a yield strength of 600MPa to 850MPa, a tensile strength of 980MPa to 1150MPa, a uniform elongation of not less than 13%, and an elongation at break of not less than 15%. Furthermore, when spot welding is actually performed, if surface cracks at the weld point occur, the maximum length of the surface cracks at the weld point is less than 5% of the plate thickness.

[0079] The manufacturing method designed in the present invention has a simple production process, and the obtained high-strength steel has significantly improved resistance to spot welding cracks under the same mechanical property conditions, and will have good application prospects in the production of safety structural parts for downstream users. BRIEF DESCRIPTION OF THE DRAWINGS

[0080] FIG1 schematically shows a schematic diagram of a spot weld crack of ultra-high strength steel with a zinc coating. DETAILED DESCRIPTION

[0081] The coated ultra-high strength steel with low spot welding crack sensitivity and the manufacturing method thereof described in the present invention will be further explained and illustrated below in conjunction with specific embodiments. However, such explanation and illustration do not constitute an undue limitation to the technical solution of the present invention.

[0082] Examples 1-28 and Comparative Examples 1-4

[0083] The coated ultra-high strength steels of Examples 1-28 of the present invention and the comparative steels of Comparative Examples 1-4 were prepared by the following steps:

[0084] (1) Smelting and thin strip continuous casting are carried out according to the chemical composition ratio designed in Table 1, wherein the slab thickness at the outlet end of the thin strip continuous casting is controlled to be 50-58 mm, and the pulling speed of the thin strip continuous casting is controlled to be 2-5 m / min to obtain the corresponding slab.

[0085] (2) Heating: Heat the slab to 1200-1250°C.

[0086] (3) Hot rolling: The thickness of the oxide scale on the surface of the steel strip after hot rolling is controlled to be ≤4μm, and the (FeO+Fe3O4) in the oxide scale on the surface of the steel strip after hot rolling is ≤50wt%. The finishing temperature is controlled to be 860-930℃, and the coiling temperature is controlled to be 450-600℃.

[0087] (4) Pickling, or pickling + cold rolling. When pickling + cold rolling is used, the cold rolling deformation is controlled to be 40% to 60%. When galvanizing or zinc alloy is directly plated after pickling, the cold rolling deformation in Table 2-2 is 0.

[0088] (5) Continuous annealing: Control the volume content of hydrogen in the reducing atmosphere in the continuous annealing furnace to be 10-15%; anneal at 800-920°C, preferably the annealing temperature can be controlled to be 820-870°C, then slowly cool to 700-770°C at a cooling rate of 3-10°C / s to obtain a certain proportion of ferrite, and the slow cooling final cooling temperature can be preferably controlled between 700-730°C; then quickly cool to 200-300°C at a cooling rate of 50-500°C / s to partially transform austenite into martensite, and the rapid cooling final cooling temperature can be preferably controlled between 250-300°C; then quickly cool and then heat to 360-460°C, preferably 400-430°C, and keep warm for 50-600s, preferably 180-300s; finally cool to room temperature.

[0089] (6) Coating with zinc or zinc alloy, wherein the coating can be specifically selected from pure zinc coating, zinc-iron alloy coating, zinc-aluminum-magnesium coating or aluminum-zinc coating.

[0090] It should be noted that the chemical composition designs and related manufacturing processes used in the coated ultra-high-strength steels of Examples 1-28 of the present invention all meet the specifications of the present invention. Accordingly, the chemical composition designs and related manufacturing processes used in the comparative steels of Comparative Examples 1-4 all contain process parameters that do not meet the design requirements of the present invention.

[0091] Table 1 lists the mass percentages of the chemical elements in the steel plate substrates of the coated ultra-high strength steels of Examples 1-28 and the comparative steels of Comparative Examples 1-4.

[0092] Table 1. (wt%, the balance is Fe and other inevitable impurities except P and S)

[0093] Accordingly, Table 2-1 and Table 2-2 list the specific process parameters of the coated ultra-high strength steel of Examples 1-28 and the comparative steel of Comparative Examples 1-4 in the above process steps (1) to (6).

[0094] Table 2-1. Note: In the above Table 2-1, "(FeO+Fe3O4) ratio" means the mass percentage of FeO and Fe3O4 in the oxide scale on the surface of the strip after hot rolling.

[0095] Table 2-2.

[0096] It should be noted that, before the plating process in step (6) above, in order to verify that the coated ultra-high strength steels of Examples 1-28 have excellent performance, the inventors sampled the coated ultra-high strength steel substrates of Examples 1-28 and the comparative steel substrates of Comparative Examples 1-4 obtained after the continuous annealing process in step (5), and observed the microstructures of the substrates of each Example and Comparative Example, and tested the mechanical properties of the substrates of each Example and Comparative Example. The microstructure observation results of the substrates of each Example and Comparative Example are listed in Table 3 below, and the mechanical property test results of the substrates of each Example and Comparative Example are listed in Table 4 below.

[0097] Table 3 lists the microstructural observation results of the coated ultra-high strength steel substrates of Examples 1 to 28 and the comparative steel substrates of Comparative Examples 1 to 4. The tests were performed according to the quantitative metallographic determination method in GB / T 15749-2008.

[0098] Table 3.

[0099] Accordingly, when testing the mechanical properties of the substrates of each embodiment and comparative example, the relevant mechanical properties testing methods are as follows:

[0100] Tensile property test: GB / T228.1-2010 Tensile Tests of Metallic Materials Part 1: Room Temperature Test Method was used to conduct tensile tests to test the yield strength, tensile strength, uniform elongation, and elongation at break of the coated ultra-high-strength steel substrates of Examples 1-28 and the comparative steel substrates of Comparative Examples 1-4.

[0101] Table 4 lists the observation results of the mechanical properties of the coated ultra-high strength steel substrates of Examples 1-28 and the comparative steel substrates of Comparative Examples 1-4.

[0102] Table 4.

[0103] Accordingly, in order to verify that the finished products of Examples 1-28 with coated ultra-high strength steel prepared through the above steps (1)-(6) have relatively excellent low spot welding crack sensitivity, the inventors took samples of the finally prepared finished products of Examples 1-28 with coated ultra-high strength steel and the comparative steel plates of Comparative Examples 1-4, and conducted spot welding process welding tests on the finished steel plate samples of each embodiment and comparative example. The relevant spot welding process parameters are shown in Table 5 below.

[0104] Table 5 lists the specific spot welding process parameters of the coated ultra-high strength steels of Examples 1-28 and the comparative steel plates of Comparative Examples 1-4.

[0105] Table 5.

[0106] During the actual spot welding process, one tensile shear (TSS) specimen, one cross tensile (CTS) specimen, and one metallographic specimen were welded at each welding current. The TSS and CTS specimens were tested using a tensile testing machine according to ISO 14273-2016 and ISO 14272-2016 standards to measure the bearing capacity of the spot-welded joints of the finished steel plate samples of each embodiment and comparative example. The results are shown in Table 6 below.

[0107] Accordingly, for the metallographic specimens obtained, the coating on the surface of the joint was first removed with dilute hydrochloric acid, and the distribution and direction of the spot welding cracks were observed under a microscope. The cross section passing through the center of the weld nugget and where the most spot welding cracks could be cut was selected as the metallographic section of the joint. Wire cutting was used for sampling, and the cross section included all the welding characteristic areas of the spot welding joint. The surface of the cut specimens was rinsed to prevent foreign matter from interfering with the test results. The rinsed samples were dried. The dried specimens were mounted, ground and polished, and measured under a metallographic microscope. The maximum crack length was filled in Table 6.

[0108] Table 6 lists the mechanical properties of the welds and the crack test results of the welds of the coated ultra-high strength steels of Examples 1-28 and Comparative Examples 1-4 after spot welding.

[0109] Table 6. Note: The two values ​​of the nominal weight of the coating in Table 6 refer to the coating weight of the front and back of the steel plate. GI represents pure zinc coating, GA represents zinc-iron alloy coating, ZM represents zinc-aluminum-magnesium coating, and AZ represents aluminum-zinc coating.

[0110] As can be seen from Table 3 above, the microstructure of the steel substrates of Examples 1-28 and Comparative Examples 1-4 designed by the present invention is: ferrite + martensite + retained austenite. Furthermore, the microstructure of the substrates of each Example and Comparative Example meets the following requirements: the volume fraction of ferrite is 25% to 45%, and the volume fraction of martensite is 45% to 65%. The volume fraction of ferrite grains 10 μm or smaller is ≥ 85%, and the volume fraction of ferrite grains 5 μm or smaller is ≥ 55%. The average grain size of retained austenite is ≤ 2 μm, and the average carbon content in the retained austenite is ≥ 1.0%.

[0111] As can be seen from Table 4 above, the steel substrates of Examples 1-28 and Comparative Examples 1-4 designed by the present invention all have very excellent mechanical properties, and their mechanical properties all meet the design requirements of the present invention. The yield strength of the coated ultra-high-strength steel substrates of Examples 1-28 is specifically between 755 and 845 MPa, the tensile strength is between 1040 and 1140 MPa, the uniform elongation is between 14.7 and 16.4%, and the elongation at break is between 22.6 and 25.4%.

[0112] Table 6 also shows that for the finished coated ultra-high-strength steels of Examples 1-28 of this case, when the welding current was less than the spatter current, the welds exhibited no spot weld cracks; when the welding current was greater than the spatter current, the longest crack in the welds was less than 5% of the plate thickness. In contrast, for the comparative steel plates of Comparative Examples 1-4 designed in this case, cracks were observed in the welds regardless of whether the welding current was greater than the spatter current. The cracks in the spatter welds were more severe than those in the non-spatter welds, and the ratio of the maximum crack length to the plate thickness was significantly greater than 5%. This demonstrates that the coated ultra-high-strength steels of Examples 1-28, designed using the technical solution of the present invention, exhibit excellent low spot weld crack sensitivity while maintaining plate performance.

[0113] It should be noted that the combination of the various technical features in this case is not limited to the combination described in the claims of this case or the combination described in the specific embodiments. All technical features recorded in this case can be freely combined or combined in any way unless there is a contradiction between them.

[0114] It should also be noted that the embodiments listed above are merely specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made therefrom that can be directly derived from or easily conceived by those skilled in the art based on the disclosure of the present invention are intended to fall within the scope of protection of the present invention.

Claims

1. A coated ultra-high strength steel with low spot welding crack sensitivity, comprising a steel substrate and a zinc-containing coating on the surface of the steel substrate, wherein the steel substrate contains Fe and unavoidable impurity elements, characterized in that: The steel substrate further contains the following chemical elements in the following mass percentages: C: 0.10~0.30%; Si: 0.30~0.90%; Mn: 1.00~2.20%; B: 0.001~0.003%; Al: 0.30~1.00%.

2. The coated ultra-high strength steel according to claim 1, wherein: The mass percentage of each chemical element of the steel substrate is: C: 0.10-0.30%; Si: 0.30-0.90%; Mn: 1.00-2.20%; B: 0.001-0.003%; Al: 0.30-1.00%; the remainder being Fe and unavoidable impurity elements.

3. The coated ultra-high strength steel according to claim 1 or 2, characterized in that: The mass percentage of each chemical element of the steel substrate satisfies at least one of the following: C: 0.15-0.20%; Si: 0.40-0.80%; Mn: 1.00-2.00%; B: 0.0015-0.003%.

4. The coated ultra-high strength steel according to claim 1 or 2, characterized in that: The chemical elements of the steel substrate further contain Mo: 0.10-2.00%; preferably, the mass percentage of Mo is 0.15-2.00%.

5. The coated ultra-high strength steel according to claim 4, wherein: The mass percentage of Mo in the steel substrate is 0.10-1.00%; preferably, the mass percentage of Mo is 0.15-1.00%.

6. The coated ultra-high strength steel according to claim 1 or 2, characterized in that: The mass percentage of the inevitable impurity elements of the steel substrate satisfies: P≤0.01%, S≤0.005%.

7. The coated ultra-high strength steel according to claim 1 or 2, characterized in that: The microstructure of the steel substrate is ferrite+martensite+retained austenite.

8. The coated ultra-high strength steel according to claim 7, wherein: The volume proportion of ferrite is 25% to 45%; and / or the volume proportion of martensite is 45% to 65%.

9. The coated ultra-high strength steel according to claim 7, wherein: In the ferrite, the volume proportion of grains with a size of less than 10 μm is ≥85%, and the volume proportion of grains with a size of less than 5 μm is ≥55%.

10. The coated ultra-high strength steel according to claim 7, wherein: The average grain size of the retained austenite is ≤2 μm; and / or the average C content in the retained austenite is ≥1.0%.

11. The coated ultra-high strength steel according to claim 1 or 2, characterized in that: When spot welding is used for welding, if surface cracks are generated at the weld point, the maximum length of the surface cracks at the weld point is less than 5% of the plate thickness.

12. The coated ultra-high strength steel according to claim 1 or 2, characterized in that: Its mechanical properties meet the following requirements: its yield strength is 600MPa-850MPa, its tensile strength is 980MPa-1150MPa, its uniform elongation is not less than 13%, and its elongation at break is not less than 15%.

13. The coated ultra-high strength steel according to claim 1 or 2, characterized in that: The coating is pure zinc coating, zinc-iron alloy coating, zinc-aluminum-magnesium coating or aluminum-zinc coating.

14. The method for manufacturing coated ultra-high strength steel according to any one of claims 1 to 13, wherein: Including steps: (1) Smelting and thin plate continuous casting; (2) heating; (3) Hot rolling: The thickness of the oxide scale on the surface of the steel strip after hot rolling is controlled to be ≤4 μm, and the mass percentage of FeO+Fe3O4 in the oxide scale on the surface of the steel strip after hot rolling is ≤50 wt%; (4) pickling, or pickling + cold rolling; (5) Continuous annealing: anneal at 800-920°C, then slowly cool to 700-770°C at a cooling rate of 3-10°C / s; then quickly cool to 200-300°C at a cooling rate of 50-500°C / s; then heat to 360-460°C, keep warm for 50-600s; finally cool to room temperature; (6) Coating with zinc coating.

15. The manufacturing method according to claim 14, characterized in that: In step (1), the thickness of the slab at the outlet end of the thin strip continuous casting is controlled to be 50 to 58 mm.

16. The manufacturing method according to claim 14, wherein: In step (1), the strip casting speed is controlled to be 2 to 5 m / min.

17. The manufacturing method according to claim 14, wherein: In step (2), the slab is heated to 1200-1250°C.

18. The manufacturing method according to claim 14, wherein: In step (3), the finishing temperature is controlled to be 860-930°C and the coiling temperature is controlled to be 450-600°C.

19. The manufacturing method according to claim 14, wherein: In step (4), when pickling + cold rolling is adopted, the cold rolling deformation is controlled to be 40% to 60%.

20. The manufacturing method according to claim 14, wherein: In step (5), the volume content of hydrogen in the reducing atmosphere in the continuous annealing furnace is controlled to be 10-15%.

21. The manufacturing method according to claim 14, wherein: The annealing process parameters of step (5) meet at least one of the following: Annealing temperature is 820~870℃; Slowly cool to 700-730°C at a cooling rate of 3-10°C / s; Rapid cooling to 250-300℃; After rapid cooling, heat again to 400-430°C and keep warm for 180-300 seconds.