Photosensitive composition, cured product, electronic component, and method for producing cured product
Patent Information
- Application Number
- MYPI2025001748
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-28
- Filing Date
- 2023-09-14
- Publication Date
- 2024-03-28
AI Technical Summary
Current photosensitive compositions used in semiconductor manufacturing face challenges in achieving excellent mechanical properties, migration resistance, and suppressing development residues, especially when heated at low temperatures, while maintaining high electrical insulation reliability.
A photosensitive composition containing a binder resin with specific structural units, such as imide, amide, and siloxane structures, along with a photosensitizer and radically polymerizable compounds, which promotes crosslinking and ring-closing reactions, thereby enhancing mechanical properties and migration resistance, and includes specific organic acids and ions to control polarization and charge balance.
The composition effectively suppresses development residues, achieves excellent mechanical properties at low temperatures, and provides enhanced migration resistance, ensuring high reliability in electronic components.
Smart Images

Figure PI2025001748_DRAWING_001
Abstract
Description
Photosensitive composition, cured product, electronic component, and method for producing the cured product
[0001] The present invention relates to a photosensitive composition, a cured product, an electronic component, and a method for producing the cured product.
[0002] In recent years, electronic terminal devices have become increasingly sophisticated, smaller, thinner, and lighter. These electronic terminal devices are equipped with semiconductor devices, such as processors and memories. Typical materials for surface protection layers and interlayer insulating layers of semiconductor devices, insulating layers of organic electroluminescence (hereinafter, "organic EL") displays, and planarizing layers of thin-film transistor (hereinafter, "TFT") substrates include resins such as polyimide and polybenzoxazole, which have excellent heat resistance and electrical insulation properties. Furthermore, to improve productivity, research is also being conducted on photosensitive polyimide / polybenzoxazole materials and photosensitive polyimide precursors / polybenzoxazole precursors that have been imparted with positive or negative photosensitivity.
[0003] As the applications of semiconductors expand and their performance improves, efforts are being made to reduce costs and increase integration by streamlining manufacturing processes, and semiconductor devices that form multilayer metal rewiring are attracting attention. Materials used for interlayer insulating layers in such multilayer metal rewiring are required to have high mechanical properties to withstand the stress associated with multilayering. Furthermore, they must also be able to suppress development residues when forming positive or negative patterns by photolithography. In addition, as wiring becomes finer with the increasing integration of semiconductor devices, reliability in terms of electrical insulation is also required, so high migration resistance is also required.
[0004] Furthermore, molding resins used in recent memory and semiconductor package fabrication have low heat resistance and are therefore restricted in their ability to be used in high-temperature processes. Therefore, materials used in surface protection layers and interlayer insulating layers of semiconductor devices are required to be curable at low temperatures of 250°C or less, and more preferably 220°C or less, and to have high mechanical properties.
[0005] Examples of materials with improved mechanical properties include a composition in which a flexible polyoxyalkylene structure is introduced into the main chain of a polyimide (see, for example, Patent Document 1). Examples of materials that can be cured by heating at low temperatures include a composition containing a resin such as polyimide or polybenzoxazole and a thermal crosslinking agent (see, for example, Patent Document 2).
[0006] JP 2012-208360 A JP 2007-016214 A
[0007] However, the compositions described in Patent Document 1 and Patent Document 2 have problems in providing a cured product that suppresses development residue while having excellent mechanical properties and migration resistance even when heated at low temperatures. Therefore, further improvement in the properties of photosensitive compositions has been desired. An object of the present invention is to provide a cured product that suppresses development residue while having excellent mechanical properties and excellent migration resistance and that can be used in electronic components. Another object of the present invention is to provide an electronic component that has excellent migration resistance.
[0008] In order to solve the above-mentioned problems, the photosensitive composition and electronic part of the present invention have the following constitutions [1] to
[20] .
[0009] [1] A photosensitive composition comprising (A) a binder resin and (C) a photosensitizer, and further comprising (B) a radical polymerizable compound and / or (F) a crosslinking agent, wherein the (A) binder resin comprises the following (A1) resin and / or (A2) resin, and the photosensitive composition satisfies the following condition (α): (A1) Resin: a resin containing one or more selected from the group consisting of an imide structure, an amide structure, an oxazole structure, and a siloxane structure in a structural unit in the main chain of the resin. (A2) Resin: a resin having a phenolic hydroxyl group in a structural unit in the main chain of the resin. (α) The photosensitive composition further contains one or more selected from the group consisting of sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing fluorine element, and satisfies the following condition (1x): (1x) the total content of sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing fluorine element in the total solid content of the photosensitive composition is 0.010 to 1,000 ppm by mass.
[0010] [2] The photosensitive composition according to [1] above, wherein the sulfonic acid, and the phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, and hypophosphite ester (hereinafter referred to as "organic acid containing phosphorus") have the following specific substituent a, the fluorine-containing carboxylic acid has the following specific substituent b, and the condition (α) is the following condition (α2), and the following condition (α2) is satisfied: (α2) Further, the compound contains one or more selected from the group consisting of a sulfonic acid having the following specific substituent a, a phosphorus-containing organic acid having the following specific substituent a, and a fluorine-containing carboxylic acid having the following specific substituent b, and satisfies the condition (1y) below: specific substituent a: one or more selected from the group consisting of a mono- or divalent aliphatic group having 1 to 18 carbon atoms, a mono- or divalent alicyclic group having 4 to 18 carbon atoms, a mono- or divalent aromatic group having 6 to 15 carbon atoms, a mono- or divalent fluorine-containing aliphatic group having 1 to 18 carbon atoms, a mono- or divalent fluorine-containing alicyclic group having 4 to 18 carbon atoms, and a mono- or divalent fluorine-containing aromatic group having 6 to 15 carbon atoms; specific substituent b: one or more selected from the group consisting of a mono- or divalent fluorine-containing aliphatic group having 1 to 18 carbon atoms, a mono- or divalent fluorine-containing alicyclic group having 4 to 18 carbon atoms, and a mono- or divalent fluorine-containing aromatic group having 6 to 15 carbon atoms. (1y) The total content of the sulfonic acid having the specific substituent a, the phosphorus-containing organic acid having the specific substituent a, and the fluorine-containing carboxylic acid having the specific substituent b in the total solid content of the photosensitive composition is 0.010 to 1,000 ppm by mass.
[0011] [3] The photosensitive composition according to [2] above, wherein the condition (α2) is the following condition (α3), and the following condition (α3) is satisfied: the sulfonic acid contains one or more selected from the group consisting of methanesulfonic acid, cyclohexanesulfonic acid, benzenesulfonic acid, toluenesulfonic acid, xylenesulfonic acid, trifluoromethanesulfonic acid, hexafluorocyclohexanesulfonic acid, hexafluorobenzenesulfonic acid, pentafluorotoluenesulfonic acid, tetrafluoroxylenesulfonic acid, trifluoromethylbenzenesulfonic acid, trifluoromethyltoluenesulfonic acid, and trifluoromethylxylenesulfonic acid; and the fluorine-containing carboxylic acid contains one or more selected from the group consisting of trifluoroacetic acid, trifluoropropionic acid, hexafluorocyclohexanecarboxylic acid, hexafluorobenzoic acid, and trifluoromethylbenzoic acid. (α3) The photosensitive composition further contains a sulfonic acid and / or a carboxylic acid containing a fluorine element, and satisfies the following condition (1z): (1z) the total content of the sulfonic acid and the carboxylic acid containing a fluorine element is 0.010 to 1,000 ppm by mass based on the total solid content of the photosensitive composition.
[0012] [4] The photosensitive composition according to any one of [1] to [3] above, further satisfying the following condition (β): (β) further containing one or more ions selected from the group consisting of chloride ions, bromide ions, sulfate ions, sulfite ions, nitrate ions, nitrite ions, phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions, and satisfying the following condition (2x): (2x) the total content of chloride ions, bromide ions, sulfate ions, sulfite ions, nitrate ions, nitrite ions, phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions is 0.010 to 1,000 ppm by mass based on the total solid content of the photosensitive composition.
[0013] [5] The photosensitive composition according to any one of [1] to [4] above, further satisfying the following condition (γ): (γ) further containing one or more selected from the group consisting of benzene, toluene, xylene, and naphthalene, and satisfying the following condition (3): (3) the total content of benzene, toluene, xylene, and naphthalene in the photosensitive composition is 0.010 to 1,000 ppm by mass.
[0014] [6] The photosensitive composition according to any one of [1] to [5] above, wherein the binder resin (A) contains the resin (A1), and the resin (A1) contains one or more resins selected from the group consisting of the following resins: (A1-1) resin, (A1-2) resin, (A1-3) resin, (A1-4) resin, (A1-5) resin, (A1-6) resin, and copolymers consisting of two or more resins thereof: (A1-1) resin: polyimide, (A1-2) resin: polyimide precursor, (A1-3) resin: polybenzoxazole, (A1-4) resin: polybenzoxazole precursor, (A1-5) resin: polyamideimide, and (A1-6) resin: polyamideimide precursor.
[0015] [7] The photosensitive composition according to any one of [1] to [6] above, further comprising one or more compounds selected from the group consisting of a cyclic amide compound represented by general formula (20), an amide compound represented by general formula (21), a cyclic urea compound represented by general formula (22), a urea compound represented by general formula (23), an oxazolidone compound represented by general formula (24), and an isoxazolidone compound represented by general formula (25), and satisfying the following condition (4): (4) The total content of the cyclic amide compound represented by general formula (20), the amide compound represented by general formula (21), the cyclic urea compound represented by general formula (22), the urea compound represented by general formula (23), the oxazolidone compound represented by general formula (24), and the isoxazolidone compound represented by general formula (25) in the total solid content of the photosensitive composition is 0.010 to 5.0 mass%.
[0016]
[0017] In the general formulas (20) to (25), R 46 ~R 56R each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, a cycloalkyl group having 4 to 10 carbon atoms, an aryl group having 6 to 15 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, or a hydroxyalkyl group having 1 to 6 carbon atoms. 130 represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a hydroxyalkyl group having 1 to 6 carbon atoms, a hydroxyalkoxy group having 1 to 6 carbon atoms, a hydroxy group, an amino group, a monoalkylamino group having 1 to 6 carbon atoms, or a dialkylamino group having 2 to 12 carbon atoms. 131 ~R 142 each independently represents an alkyl group having 1 to 6 carbon atoms. α, β, and γ each independently represent an integer of 0 to 6. a, b, c, e, f, g, h, i, j, k, l, and m each independently represent an integer of 0 to 2. When α is 0, a is 0. When β is 0, b is 0. When γ is 0, c is 0.
[0018] [8] The photosensitive composition according to any one of [1] to [7] above, further containing one or more components selected from the group consisting of a component containing elemental sodium, a component containing elemental potassium, a component containing elemental magnesium, a component containing elemental calcium, a component containing elemental iron, a component containing elemental copper, and a component containing elemental chromium, and satisfying the following condition (5): (5) The total content of elemental sodium, elemental potassium, elemental magnesium, elemental calcium, elemental iron, elemental copper, and elemental chromium in the total solid content of the photosensitive composition is 0.010 to 500 ppm by mass.
[0019] [9] The photosensitive composition according to any one of [1] to [8] above, wherein the (C) photosensitizer contains (C1) a photopolymerization initiator, and the (C1) photopolymerization initiator contains (C1-1) an oxime ester compound and / or (C1-2) a phosphine oxide compound.
[0020]
[10] The photosensitive composition according to any one of [1] to [9] above, further containing one or more selected from the group consisting of acetic acid, propionic acid, cyclopentanecarboxylic acid, cyclohexanecarboxylic acid, benzoic acid, methylbenzoic acid, and trimethylbenzoic acid, and satisfying the following condition (6): and / or further containing an aldoxime compound and / or a ketoxime compound, and satisfying the following condition (7): (6) The total content of acetic acid, propionic acid, cyclopentanecarboxylic acid, cyclohexanecarboxylic acid, benzoic acid, methylbenzoic acid, and trimethylbenzoic acid in the total solid content of the photosensitive composition is 0.010 to 500 ppm by mass, or (7) The total content of aldoxime compounds and ketoxime compounds in the total solid content of the photosensitive composition is 0.010 to 500 ppm by mass.
[0021]
[11] The photosensitive composition according to any one of [1] to
[10] above, further containing one or more components selected from the group consisting of a component containing elemental chlorine, a component containing elemental bromine, and a component containing elemental sulfur, and satisfying the following condition (8) and / or (9): and / or further containing water, and satisfying the following condition (10): (8) The total content of elemental chlorine and elemental bromine in the total solid content of the photosensitive composition is 0.010 to 500 ppm by mass, (9) The content of elemental sulfur in the total solid content of the photosensitive composition is 0.010 to 500 ppm by mass, and (10) The content of water in the photosensitive composition is 0.010 to 3.0% by mass.
[0022]
[12] The photosensitive composition according to any one of [1] to
[11] above, further satisfying the following condition (1α): (1α) the content of elemental fluorine in the total solid content of the photosensitive composition is 1,000 ppm by mass or less.
[0023]
[13] The photosensitive composition according to any one of [1] to
[12] above, further satisfying at least one of the following conditions (δ), (ε), and (ζ): (δ) The (B) radical polymerizable compound contains the following (B1) first polymerizable compound and (B2) second polymerizable compound. (ε) The (B) radical polymerizable compound contains the following (B3) third polymerizable compound and (B4) fourth polymerizable compound. (ζ) The (B) radical polymerizable compound contains the following (B1) first polymerizable compound or (B2) second polymerizable compound, and further contains the following (B3) third polymerizable compound or (B4) fourth polymerizable compound. (B1) First polymerizable compound: A compound having the following (I-b1) structure and further having at least two radical polymerizable groups. (I-b1) Structure: A structure containing an alicyclic structure and / or a heteroalicyclic structure. (B2) Second polymerizable compound: A compound having the following (I-b2) structure and (II-b2) structure and further having at least two radical polymerizable groups. (I-b2) Structure: A structure containing an aromatic structure. (II-b2) Structure: A structure containing an aliphatic structure. (B3) Third polymerizable compound: A compound having at least two (meth)acryloyl groups and further having the following structure (I-b3). (I-b3) Structure: At least two (meth)acryloyl groups are connected by a minimum of 4 to 10 atoms, and a structure containing an aliphatic structure. (B4) Fourth polymerizable compound: A compound having at least two (meth)acryloyl groups and further having the following structure (I-b4). (I-b4) Structure: At least two (meth)acryloyl groups are connected by a minimum of 11 to 45 atoms, and a structure containing an aliphatic structure.
[0024]
[14] The photosensitive composition according to any one of [1] to
[13] above, further comprising (G) inorganic particles, wherein the (G) inorganic particles comprise one or more particles selected from the group consisting of silica particles, alumina particles, titania particles, vanadium oxide particles, chromium oxide particles, iron oxide particles, cobalt oxide particles, copper oxide particles, zinc oxide particles, zirconium oxide particles, niobium oxide particles, tin oxide particles, and cerium oxide particles.
[0025]
[15] A photosensitive composition comprising (A) a binder resin and (C) a photosensitizer, and further comprising (B) a radically polymerizable compound and / or (F) a crosslinking agent, wherein the (A) binder resin comprises the following (A1) resin and / or (A2) resin, and the photosensitive composition satisfies one or more of the following conditions (α), (β), and (γ): (A1) Resin: A resin containing one or more selected from the group consisting of an imide structure, an amide structure, an oxazole structure, and a siloxane structure in a structural unit in the main chain of the resin. (A2) Resin: A resin having a phenolic hydroxyl group in a structural unit in the main chain of the resin. (α) Further, the photosensitive composition contains one or more selected from the group consisting of sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing fluorine element, and satisfies the following condition (1x): (1x) The total content of the sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing fluorine element in the total solid content of the photosensitive composition is 0.010 to 1,000 ppm by mass. (β) further contains one or more ions selected from the group consisting of chloride ions, bromide ions, sulfate ions, sulfite ions, nitrate ions, nitrite ions, phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions, and satisfies the following condition (2x): (2x) the total content of chloride ions, bromide ions, sulfate ions, sulfite ions, nitrate ions, nitrite ions, phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions is 0.010 to 1,000 ppm by mass relative to the total solids content of the photosensitive composition; (γ) further contains one or more ions selected from the group consisting of benzene, toluene, xylene, and naphthalene, and satisfies the following condition (3): (3) the total content of benzene, toluene, xylene, and naphthalene in the photosensitive composition is 0.010 to 1,000 ppm by mass.
[0026]
[16] A photosensitive composition film having a photosensitive composition coating formed from the photosensitive composition according to any one of [1] to
[15] above and a support.
[0027]
[17] A cured product obtained by curing the photosensitive composition according to any one of [1] to
[15] above.
[0028]
[18] An electronic component comprising the cured product according to
[17] above.
[0029]
[19] A method for producing a cured product, comprising: (1) a step of forming a coating film of the photosensitive composition according to any one of [1] to
[15] above on a substrate; (2) a step of irradiating the coating film of the photosensitive composition with actinic rays through a photomask; (3) a step of developing the coating film with a developer to form a pattern of the photosensitive composition; and (4) a step of heating the pattern to obtain a cured pattern of the photosensitive composition.
[0030]
[20] An electronic component having a cured product, the cured product containing the following resin (XA1) and / or resin (XA2), and satisfying the following condition (Xα): (XA1) resin: a resin containing one or more structures selected from the group consisting of imide structures, amide structures, oxazole structures, and siloxane structures in structural units in the main chain of the resin; (XA2) resin: a resin having a phenolic hydroxyl group in structural units in the main chain of the resin; (Xα) further containing one or more structures selected from the group consisting of sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing a fluorine element, and satisfying the following condition (X1x): (X1x) the total content of the sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing a fluorine element in the cured product is 0.010 to 1,000 ppm by mass.
[0031] The photosensitive composition of the present invention can suppress residues after development, and by improving the degree of crosslinking of the resin and promoting the ring-closing reaction, it is possible to provide a cured product that has excellent mechanical properties even when heated at low temperatures. In addition, it is possible to provide a cured product that is used in electronic components that have excellent migration resistance. Furthermore, the electronic components of the present invention can provide electronic components that have excellent migration resistance.
[0032] 1 is a schematic cross-sectional view showing an enlarged cross section of a pad portion of a semiconductor device having bumps;
[0033] The following describes a photosensitive composition according to a first aspect of the present invention and a photosensitive composition according to a second aspect of the present invention. When referring to the photosensitive composition of the present invention, it refers to the photosensitive composition according to the first and second aspects of the present invention. On the other hand, when referring to a specific aspect of a photosensitive composition, it is referred to as the photosensitive composition according to the first aspect of the present invention. However, the present invention is not limited to the following embodiments, and various modifications are naturally possible as long as the object of the invention can be achieved and the gist of the invention is not deviated from. The main chain of a resin refers to the longest chain among the chains constituting a resin containing structural units. The side chain of a resin refers to a chain branched from or bonded to the main chain among the chains constituting a resin containing structural units, which is shorter than the main chain. The term "terminal end of a resin" refers to a structure that blocks the main chain, such as a structure derived from a terminal blocking agent. Furthermore, a hydrocarbon group or alkylene group containing a "*** bond" or a "*** group" refers to a hydrocarbon group or alkylene group bound to a "*** bond" or a "*** group", or at least two hydrocarbon groups or at least two alkylene groups linked by a "*** bond" or a "*** group".
[0034] <Photosensitive Composition> The photosensitive composition according to a first embodiment of the present invention has the structure described in [1] above. The photosensitive composition according to a second embodiment of the present invention has the structure described in
[15] above. Sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing elemental fluorine may hereinafter be collectively referred to as "specific organic acid." Chloride ion, bromide ion, sulfate ion, sulfite ion, nitrate ion, nitrite ion, phosphate ion, phosphite ion, hypophosphite ion, formate ion, and fluoride ion may hereinafter be collectively referred to as "specific anion." Benzene, toluene, xylene, and naphthalene may hereinafter be collectively referred to as "specific aromatic compound."
[0035] By adopting the above-described configuration, the photosensitive composition of the present invention can suppress residues after development, and by improving the degree of crosslinking of the resin and promoting the ring-closing reaction, it is possible to provide a cured product with excellent mechanical properties even when heated at low temperatures. In addition, it is possible to provide a cured product with excellent migration resistance that can be used in electronic components. This is presumably because, by incorporating trace amounts of the above-described specific aromatic compounds, specific anions, or specific organic acids into the photosensitive composition, when forming a pattern of the photosensitive composition on wiring, the wiring surface corresponding to the openings is surface-modified by these specific aromatic compounds, specific anions, or specific organic acids. Therefore, it is believed that preventing residue adhesion to the wiring surface effectively suppresses residues after development.
[0036] Furthermore, it is presumed that the above-mentioned specific aromatic compounds are in a locally oriented state due to π-electron interactions between resins having aromatic rings, such as polyimides, polybenzoxazoles, and their precursors, and coordinate bonds via π-electrons with resins containing silicon atoms having a 3d orbital, an empty atomic orbital, such as polysiloxanes. As a result, crosslinking reactions between resins and ring-closure reactions between resins proceed efficiently, which is believed to result in excellent mechanical properties even when heated at low temperatures. Meanwhile, the above-mentioned specific anions and specific organic acids are believed to function as catalysts that promote crosslinking reactions on aromatic rings and ring-closure reactions between resins having aromatic rings, such as polyimides, polybenzoxazoles, and their precursors, and crosslinking reactions in resins having silanol groups, such as polysiloxanes. As a result, crosslinking reactions and ring-closure reactions proceed efficiently, which is believed to result in excellent mechanical properties even when heated at low temperatures.
[0037] Furthermore, intentionally incorporating trace amounts of these specific aromatic compounds, specific anions, or specific organic acids is believed to control the polarization structure and charge balance in the cured product of the photosensitive composition. Furthermore, aromatic rings in resins such as polyimides, polybenzoxazoles, and their precursors, and silanol groups in resins such as polysiloxanes, are also believed to contribute to the control of polarization structure and charge balance. This is believed to suppress ion migration and electromigration caused by metal impurities and ionic impurities that adversely affect electrical insulation, thereby achieving excellent migration resistance. Furthermore, suppressing metal migration and aggregation in wiring is believed to contribute to the high reliability of electronic components, semiconductor devices, display devices, and metal-clad laminates.
[0038] <(A) Binder Resin> The photosensitive composition of the present invention contains (A) a binder resin. The (A) binder resin is a heat-resistant resin, at least a portion of which remains in a cured product obtained by curing the composition. The (A) binder resin is preferably a resin that cures by forming a crosslinked structure through a reaction. The reaction is not particularly limited and may be caused by heating, irradiation with energy rays, or the like, and a crosslinked structure may also be formed by a (F) crosslinking agent described below. The (A) binder resin is preferably a thermosetting resin.
[0039] The (A) binder resin is preferably an alkali-soluble resin or an organic solvent-soluble resin. An alkali-soluble resin refers to a resin that has an acidic group and is soluble in an alkaline developer. An organic solvent-soluble resin refers to a resin that has an organic solvent-soluble structure and is soluble in an organic solvent developer. The alkali-soluble resin and organic solvent-soluble resin in the photosensitive composition of the present invention are preferably resins that are imparted with positive or negative photosensitivity by the (C) photosensitizer described below and that have a solubility that allows the formation of a positive or negative pattern by development with an alkaline developer or an organic solvent. The (A) binder resin more preferably has an acidic group in its structural unit. The acidic group contained in the (A) binder resin is preferably a phenolic hydroxyl group, a hydroxyimide group, a hydroxyamide group, a silanol group, a 1,1-bis(trifluoromethyl)methylol group, a mercapto group, a carboxy group, a carboxylic acid anhydride group, or a sulfonic acid group. When the binder resin (A) satisfies the following condition (P1a) and / or (P2a) described later, or when the photosensitive composition of the present invention satisfies the following condition (1α) described later, the acidic group contained in the binder resin (A) is preferably a phenolic hydroxyl group, a hydroxyimide group, a hydroxyamide group, a silanol group, a mercapto group, a carboxy group, a carboxylic anhydride group, or a sulfonic acid group.
[0040] The (A) binder resin preferably has a radical polymerizable group, more preferably has a radical polymerizable group in a structural unit of the resin. The radical polymerizable group preferably has an ethylenically unsaturated double bond group, more preferably a photoreactive group, an alkenyl group having 2 to 5 carbon atoms, or an alkynyl group having 2 to 5 carbon atoms. The photoreactive group is preferably a styryl group, a cinnamoyl group, a maleimide group, a nadimide group, or a (meth)acryloyl group, and from the viewpoints of improving sensitivity during exposure and promoting radical polymerization during heating at low temperatures, a (meth)acryloyl group is more preferred. On the other hand, the alkenyl group having 2 to 5 carbon atoms or the alkynyl group having 2 to 5 carbon atoms is preferably a vinyl group, an allyl group, a 2-methyl-2-propenyl group, a crotonyl group, a 2-methyl-2-butenyl group, a 3-methyl-2-butenyl group, a 2,3-dimethyl-2-butenyl group, an ethynyl group, or a 2-propargyl group, and from the viewpoints of improving sensitivity during exposure and promoting radical polymerization during heating at low temperatures, a vinyl group or an allyl group is more preferred.
[0041] <(A1) Resin, (A2) Resin, and (A3) Resin> In the photosensitive composition of the present invention, the binder resin (A) contains the following (A1) resin and / or (A2) resin. Furthermore, in the photosensitive composition of the present invention, it is preferable that the binder resin (A) further contains the following (A3) resin. (A1) Resin: A resin containing one or more structures selected from the group consisting of an imide structure, an amide structure, an oxazole structure, and a siloxane structure in a structural unit in the main chain of the resin. (A2) Resin: A resin having a phenolic hydroxyl group in a structural unit in the main chain of the resin. (A3) Resin: A resin having a radically polymerizable group.
[0042] The (A1) resin is a resin containing one or more structural units selected from the group consisting of imide structures, amide structures, oxazole structures, and siloxane structures in the main chain of the resin, such as polyimide, polybenzoxazole, precursors thereof, and copolymers of two or more of them. The (A3) resin is a resin having a radical polymerizable group such as a (meth)acryloyl group in at least one of the main chain, side chain, and terminal of the resin. Examples and preferred descriptions of the radical polymerizable group are as described above for the (A) binder resin.
[0043] Note that among the (A1) resin, (A2) resin, and (A3) resin, if each of them has a structure or group constituting a different resin, it will be classified as one of them according to the following rules. When a resin can fall into two or more of the (A1) resin, (A2) resin, and (A3) resin, the resin to which it falls will be determined as follows. That is, if a resin containing one or more structures selected from the group consisting of imide structures, amide structures, oxazole structures, and siloxane structures (hereinafter referred to as "imide structures, etc.") in the structural units of the resin's main chain has a phenolic hydroxyl group in the structural units of the resin's main chain, the resin is considered to be an (A1) resin. Furthermore, if a resin having a structural unit containing an imide structure, etc., has a radically polymerizable group, the resin is considered to be an (A1) resin. Furthermore, if a resin having a phenolic hydroxyl group in the structural units of the resin's main chain has a radically polymerizable group, the resin is considered to be an (A2) resin. Furthermore, when a resin having a structural unit containing an imide structure or the like has a phenolic hydroxyl group in the structural unit in the main chain of the resin and further has a radical polymerizable group, the resin is considered to fall under the category of resin (A1).
[0044] The photosensitive composition of the present invention preferably contains an (A1) resin from the viewpoint of improving mechanical properties and migration resistance when heated at low temperatures, and more preferably contains an (A1) resin and an (A2) resin from the viewpoint of suppressing residue after development and improving mechanical properties when heated at low temperatures. Furthermore, the photosensitive composition of the present invention preferably contains an (A1) resin and / or an (A2) resin, and further contains an (A3) resin, from the viewpoint of improving sensitivity during exposure and improving mechanical properties when heated at low temperatures. Furthermore, from these viewpoints, the photosensitive composition of the present invention more preferably contains an (A1) resin, an (A2) resin, and an (A3) resin.
[0045] <(A1) Resin> From the viewpoint of improving mechanical properties and migration resistance when heated at low temperatures, the (A1) resin preferably contains one or more resins selected from the group consisting of the following (A1-1) resin, (A1-2) resin, (A1-3) resin, (A1-4) resin, (A1-5) resin, (A1-6) resin, (A1-7) resin, (A1-8) resin, maleimide resin, maleimide-styrene resin, maleimide-triazine resin, maleimide-oxazine resin, and copolymers consisting of two or more resins thereof. It is more preferable that the resin (A1) contains one or more resins selected from the group consisting of (A1-3) resin, (A1-4) resin, (A1-5) resin, (A1-6) resin, (A1-7) resin, (A1-8) resin, and copolymers consisting of two or more of these resins, and it is even more preferable that the resin (A1) contains one or more resins selected from the group consisting of (A1-1) resin, (A1-2) resin, (A1-3) resin, (A1-4) resin, (A1-5) resin, (A1-6) resin, (A1-7) resin, and copolymers consisting of two or more of these resins (hereinafter referred to as "polyimide resins"). The resin (A1) may be either a single resin or a copolymer thereof. (A1-1) Resin: Polyimide (A1-2) Resin: Polyimide precursor (A1-3) Resin: Polybenzoxazole (A1-4) Resin: Polybenzoxazole precursor (A1-5) Resin: Polyamideimide (A1-6) Resin: Polyamideimide precursor (A1-7) Resin: Polyamide (A1-8) Resin: Polysiloxane.
[0046] The (A1) resin as described above has an imide structure, an amide structure, an oxazole structure, or a siloxane structure in the structural units of the resin main chain, which is effective in improving mechanical properties. Furthermore, it is presumed that these structures capture metal impurities and ionic impurities that adversely affect electrical insulation, thereby suppressing ion migration and electromigration and improving migration resistance.
[0047] The (A) binder resin preferably contains an (A1) resin, and from the viewpoint of improving mechanical properties and migration resistance when heated at low temperatures, the (A1) resin preferably contains one or more resins selected from the group consisting of the above-mentioned (A1-1) resin, (A1-2) resin, (A1-3) resin, (A1-4) resin, (A1-5) resin, (A1-6) resin, and copolymers consisting of two or more of them, and more preferably contains one or more resins selected from the group consisting of (A1-1) resin, (A1-2) resin, (A1-3) resin, (A1-4) resin, and copolymers consisting of two or more of them. Furthermore, from the viewpoint of improving mechanical properties when heated at low temperatures, the (A1) resin further preferably contains an (A1-1) resin, (A1-3) resin, and copolymers consisting of two or more of them. On the other hand, from the viewpoint of improving sensitivity during exposure, it is more preferable that the (A1) resin contains a (A1-2) resin, a (A1-4) resin, or a copolymer of two or more of these resins.
[0048] The binder resin (A) preferably contains a resin (A1), and the resin (A1) preferably has a radical polymerizable group from the viewpoints of improving sensitivity during exposure and improving mechanical properties during heating at low temperatures. Examples and preferred descriptions of the radical polymerizable group are as described above for the binder resin (A).
[0049] From the viewpoints of improving sensitivity during exposure and improving mechanical properties during heating at low temperatures, the (A1-1) resin, (A1-2) resin, (A1-3) resin, (A1-4) resin, (A1-5) resin, (A1-6) resin, and copolymers of two or more of these resins preferably have a radical polymerizable group. Examples and preferred descriptions of the radical polymerizable group are as described above for the (A) binder resin.
[0050] The radical polymerizable group is preferably one or more types selected from the group consisting of general formulae (51), (52), (53), (54) and (55).
[0051]
[0052] In the general formulae (51) to (55), X 21~X 24 each independently represents an alkylene group having 1 to 10 carbon atoms, a cycloalkylene group having 4 to 10 carbon atoms, or an arylene group having 6 to 15 carbon atoms. 25 represents a divalent to hexavalent organic group. 26 represents a direct bond or a divalent to hexavalent organic group. 181 ~R 202 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 15 carbon atoms. a, b, c, d, and e each independently represent 0 or 1. f and g each independently represent an integer of 1 to 5.
[0053] In the general formulae (51) to (55), X 25 is preferably a divalent to hexavalent aliphatic group, more preferably a divalent to hexavalent alkylene group having 1 to 10 carbon atoms. 26 is preferably a direct bond or a divalent to hexavalent aliphatic group, more preferably a divalent to hexavalent alkylene group having 1 to 10 carbon atoms. The above-mentioned alkyl group, aryl group, alkylene group, cycloalkylene group, and arylene group may have a heteroatom, and may be either unsubstituted or substituted.
[0054] The radical polymerizable group is preferably obtained by reacting a part of the phenolic hydroxyl group and / or carboxyl group of the resin with a compound having a radical polymerizable group. Examples of the compound having a radical polymerizable group include isocyanate compounds, epoxy compounds, aldehyde compounds, ketone compounds, acetate compounds, carboxylic acid compounds, carboxylic acid derivatives, alkyl halide compounds, alkyl azide compounds, alkyl sulfonate compounds, alkyl cyanide compounds, and alcohol compounds. These compounds also preferably have a urea bond or a urethane bond.
[0055] Examples of alcohol compounds having a radical polymerizable group include 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 4-hydroxyhexyl (meth)acrylate, glycerol di(meth)acrylate, trimethylolpropane di(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, and trispentaerythritol hepta(meth)acrylate.
[0056] The (A) binder resin preferably contains an (A1) resin, and the (A1) resin preferably contains an (A1) resin that does not have a radical polymerizable group and an (A1) resin that has a radical polymerizable group, from the viewpoints of improving sensitivity during exposure, suppressing residue after development, improving mechanical properties during heating at low temperatures, and improving migration resistance.
[0057] It is believed that by adopting the above-mentioned configuration, the resin (A1) having no radical polymerizable group exhibits the effects of suppressing residues after development due to the acidic group or organic solvent-soluble structure and capturing metal impurities, ionic impurities, etc., while the resin (A1) having a radical polymerizable group exhibits the effects of improving sensitivity during exposure and promoting radical polymerization during heating at low temperatures, etc. It is presumed that such functional separation in the resin (A1) results in a remarkable effect of improving multiple properties.
[0058] From the viewpoint of improving sensitivity during exposure, the acid equivalent of the (A1) resin is preferably 200 g / mol or more, more preferably 250 g / mol or more, and even more preferably 300 g / mol or more. On the other hand, from the viewpoint of suppressing residue after development, the acid equivalent of the (A1) resin is preferably 600 g / mol or less, more preferably 500 g / mol or less, and even more preferably 450 g / mol or less. Herein, exposure refers to irradiation with activated actinic rays (radiation), and examples thereof include irradiation with visible light, ultraviolet light, electron beams, or X-rays. Hereinafter, exposure refers to irradiation with activated actinic rays (radiation).
[0059] From the viewpoint of suppressing residues after development, the double bond equivalent of the resin (A1) is preferably 200 g / mol or more, more preferably 400 g / mol or more, even more preferably 500 g / mol or more, even more preferably 700 g / mol or more, and particularly preferably 1,000 g / mol or more. On the other hand, from the viewpoint of improving sensitivity during exposure, the double bond equivalent of the resin (A1) is preferably 3,000 g / mol or less, more preferably 2,000 g / mol or less, and even more preferably 1,500 g / mol or less.
[0060] <(A1) Resin; Polyimide Resin> Examples of polyimide precursors include polyamic acid, polyamic acid ester, polyamic acid amide, and polyisoimide. Examples of polyimides include resins obtained by dehydrating and cyclizing a polyimide precursor by heating or a reaction using a catalyst. The polyimide preferably has a structural unit represented by general formula (1). The polyimide precursor preferably has a structural unit represented by general formula (2).
[0061]
[0062] In the general formula (1) and the general formula (2), R 1 and R 5 R each independently represents a tetravalent to decavalent organic group. 2 and R 6 R each independently represents a divalent to decavalent organic group. 3 , R 4 , and R 9 R each independently represents a phenolic hydroxyl group, a sulfonic acid group, a mercapto group, or a substituent represented by general formula (7) or general formula (8). 7 represents a substituent represented by general formula (7) or general formula (8). 8 represents a phenolic hydroxyl group, a sulfonic acid group, or a mercapto group. p represents an integer of 0 to 6. q represents an integer of 0 to 8. t represents an integer of 2 to 8, u represents an integer of 0 to 6, and 2≦t+u≦8. v represents an integer of 0 to 8. However, R 3 or R 4 represents a phenolic hydroxyl group, R bonded to the phenolic hydroxyl group 1 or R2 contains an aromatic structure in its structure. 8 or R 9 represents a phenolic hydroxyl group, R bonded to the phenolic hydroxyl group 5 or R 6 contains an aromatic structure in its structure.
[0063] In the general formula (1) and the general formula (2), R 1 , R 5 , R 2 , and R 6 Preferably, each independently has an aliphatic structure having 2 to 20 carbon atoms, an alicyclic structure having 4 to 20 carbon atoms, or an aromatic structure having 6 to 30 carbon atoms. q is preferably an integer of 1 to 8. v is preferably an integer of 1 to 8. R 1 and R 5 R each independently represents a carboxylic acid residue. 2 and R 6 each independently represents an amine residue. The above-mentioned aliphatic structure, alicyclic structure, and aromatic structure may have a heteroatom, and may be either unsubstituted or substituted.
[0064]
[0065] In the general formula (7) and the general formula (8), R 28 ~R 30 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an acyl group having 2 to 6 carbon atoms, or an aryl group having 6 to 15 carbon atoms. 28 ~R 30 are each independently preferably a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an acyl group having 2 to 4 carbon atoms, or an aryl group having 6 to 10 carbon atoms. The above-mentioned alkyl group, acyl group, and aryl group may have a heteroatom, and may be either unsubstituted or substituted.
[0066] The polyimide precursor may be a polyimide having a structural unit represented by general formula (2) R 7 is a substituent represented by general formula (7), R 28A structural unit in which R is a hydrogen atom is called an amic acid structural unit. 7 is a substituent represented by general formula (7), R 28 A structural unit in which R is an alkyl group having 1 to 10 carbon atoms, an acyl group having 2 to 6 carbon atoms, or an aryl group having 6 to 15 carbon atoms is called an amic acid ester structural unit. 7 is a substituent represented by general formula (8), the structural unit is called an amic acid amide structural unit. From the viewpoint of improving mechanical properties when heated at low temperatures, the polyimide precursor preferably has an amic acid ester structural unit and / or an amic acid amide structural unit. Furthermore, the polyimide precursor may have an imide ring-closed structural unit in which a part of the amic acid structural unit, amic acid ester structural unit, or amic acid amide structural unit is ring-closed into an imide ring.
[0067] Examples of polybenzoxazole precursors include polyhydroxyamides. Examples of polybenzoxazoles include resins obtained by dehydrating and cyclizing polybenzoxazole precursors by heating or by a reaction using a catalyst. The polybenzoxazole preferably has a structural unit represented by general formula (3). The polybenzoxazole precursor preferably has a structural unit represented by general formula (4).
[0068]
[0069] In the general formula (3) and the general formula (4), R 10 and R 14 R each independently represents a divalent to decavalent organic group. 11 and R 15 R each independently represents a tetravalent to decavalent organic group having an aromatic structure. 12 , R 13 , and R 16 R each independently represents a phenolic hydroxyl group, a sulfonic acid group, a mercapto group, or a substituent represented by the above general formula (7) or general formula (8). 17 represents a phenolic hydroxyl group. 18represents a sulfonic acid group, a mercapto group, or a substituent represented by the above general formula (7) or general formula (8). r represents an integer of 0 to 8. s represents an integer of 0 to 6. w represents an integer of 0 to 8. x represents an integer of 2 to 8, and y represents an integer of 0 to 6, with 2≦x+y≦8. However, R 12 or R 13 represents a phenolic hydroxyl group, R bonded to the phenolic hydroxyl group 10 or R 11 contains an aromatic structure in its structure. 16 represents a phenolic hydroxyl group, R bonded to the phenolic hydroxyl group 14 contains an aromatic structure in its structure. 17 R bonded to 15 contains an aromatic structure in its structure.
[0070] In the general formula (3) and the general formula (4), R 10 , R 14 , R 11 , and R 15 Preferably, each independently has an aliphatic structure having 2 to 20 carbon atoms, an alicyclic structure having 4 to 20 carbon atoms, or an aromatic structure having 6 to 30 carbon atoms. s is preferably an integer of 1 to 6. 10 and R 14 R each independently represents a carboxylic acid residue. 11 and R 15 each independently represents an amine residue. The above-mentioned aliphatic structure, alicyclic structure, and aromatic structure may have a heteroatom, and may be either unsubstituted or substituted.
[0071] Examples of polyamideimide precursors include resins obtained by reacting tricarboxylic anhydrides with diamines. Examples of polyamideimides include resins obtained by dehydrating and cyclizing polyamideimide precursors by heating or by a reaction using a catalyst. The polyamideimide preferably has a structural unit represented by general formula (5). The polyamideimide precursor preferably has a structural unit represented by general formula (6).
[0072]
[0073] In the general formula (5) and the general formula (6), R 19 and R 23 R each independently represents a trivalent to decavalent organic group. 20 and R 24 R each independently represents a divalent to decavalent organic group. 21 , R 22 , and R 27 R each independently represents a phenolic hydroxyl group, a sulfonic acid group, a mercapto group, or a substituent represented by the above general formula (7) or general formula (8). 25 represents a substituent represented by general formula (7) or general formula (8). 26 represents a phenolic hydroxyl group, a sulfonic acid group, or a mercapto group. m represents an integer of 0 to 7. n represents an integer of 0 to 8. a represents an integer of 0 to 7. b represents an integer of 0 to 8. However, R 21 or R 22 represents a phenolic hydroxyl group, R bonded to the phenolic hydroxyl group 19 or R 20 contains an aromatic structure in its structure. 26 or R 27 represents a phenolic hydroxyl group, R bonded to the phenolic hydroxyl group 23 or R 24 contains an aromatic structure in its structure.
[0074] In the general formula (5) and the general formula (6), R 19 , R 23 , R 20 , and R 24 Preferably, each independently has an aliphatic structure having 2 to 20 carbon atoms, an alicyclic structure having 4 to 20 carbon atoms, or an aromatic structure having 6 to 30 carbon atoms. n is preferably an integer of 1 to 8. b is preferably an integer of 1 to 8. R 19 and R 23 R each independently represents a carboxylic acid residue. 20 and R 24 each independently represents an amine residue. The above-mentioned aliphatic structure, alicyclic structure, and aromatic structure may have a heteroatom, and may be either unsubstituted or substituted.
[0075] Examples of polyamides include resins obtained by reacting a dicarboxylic acid or a corresponding dicarboxylic acid activated diester with a diamine or a diisocyanate compound. The above polyimides, polyimide precursors, polybenzoxazoles, polybenzoxazole precursors, polyamideimides, and polyamideimide precursors may be copolymers with polyamides.
[0076] From the viewpoint of improving sensitivity during exposure, the polyimide resin preferably contains a carboxylic acid residue having a fluorine atom and / or an amine residue having a fluorine atom. The total content of the carboxylic acid residues having a fluorine atom and the amine residues having a fluorine atom relative to the total carboxylic acid residues and the total amine residues of each resin is preferably 10 to 100 mol%, more preferably 30 to 100 mol%, and even more preferably 50 to 100 mol%. The total content of the amine residues having a fluorine atom relative to the total amine residues of each resin is preferably 10 to 100 mol%, more preferably 30 to 100 mol%, and even more preferably 50 to 100 mol%. The total content of the carboxylic acid residues having a fluorine atom relative to the total carboxylic acid residues of each resin is preferably 10 to 100 mol%, more preferably 30 to 100 mol%, and even more preferably 50 to 100 mol%.
[0077] From the viewpoint of improving storage stability, the polyimide resin preferably has a structure in which the terminal of the resin is blocked with a monoamine, a dicarboxylic acid anhydride, or a monocarboxylic acid derivative. From the viewpoint of improving sensitivity during exposure and improving mechanical properties during heating at low temperatures, the polyimide resin preferably has a crosslinkable group or a radically polymerizable group capable of reacting with resins, etc., at the terminal of the resin, and more preferably has a maleimide group or a nadiimide group. The maleimide group and the nadiimide group at the terminal of the resin are preferably an amine residue and / or a carboxylic acid residue. Examples of such acid monomers include maleic anhydride and nadic anhydride.
[0078] <Fluorine Element Content in the Structure of the (A) Binder Resin> From the viewpoint of suppressing residue after development and improving migration resistance, the (A) binder resin preferably satisfies the following condition (P1a). The (A) binder resin more preferably satisfies the following condition (P2a). Similarly, when the (A) binder resin is a polyimide-based resin, from the viewpoint of suppressing residue after development and improving migration resistance, it also preferably satisfies the following condition (P1a), and more preferably satisfies the following condition (P2a). (P1a) The fluorine element content in the structure of the (A) binder resin is 10,000 ppm by mass or less. (P2a) The fluoride ion content in the structure of the (A) binder resin is 10,000 ppm by mass or less.
[0079] From the viewpoint of the effects of the present invention, the content of elemental fluorine in the structure of the (A) binder resin is preferably 0 ppm by mass or more, more preferably 0.010 ppm by mass or more, even more preferably 0.030 ppm by mass or more, even more preferably 0.050 ppm by mass or more, particularly preferably 0.070 ppm by mass or more, and most preferably 0.10 ppm by mass or more. On the other hand, from the viewpoint of the effects of the present invention, the content of elemental fluorine is preferably 10,000 ppm by mass or less, more preferably 5,000 ppm by mass or less, even more preferably 1,000 ppm by mass or less, even more preferably 500 ppm by mass or less, particularly preferably 300 ppm by mass or less, and most preferably 100 ppm by mass or less. Furthermore, the fluorine content is preferably 50 ppm by mass or less, more preferably 30 ppm by mass or less, even more preferably 10 ppm by mass or less, even more preferably 5 ppm by mass or less, particularly preferably 3 ppm by mass or less, and most preferably 1 ppm by mass or less.
[0080] The preferred range of the content of fluoride ions in the structure of the binder resin (A) is the same as the preferred range of the content of fluorine element in the structure of the binder resin (A) described above.
[0081] The content of fluorine element in the structure of (A) binder resin may be 0 ppm by mass, and the content of fluoride ion in the structure of (A) binder resin may also be 0 ppm by mass.
[0082] By incorporating a binder resin (A) having a fluorine content of a specific value or less into the photosensitive composition, the content of fluorine element, fluoride ions, or fluorine-containing anions derived from these resins in these resins is reduced to a specific value or less. It is therefore believed that protons in the photosensitive composition are locally activated due to interactions such as hydrogen bonding between the components in the photosensitive composition. Therefore, the effect of promoting dissolution in the developer is thought to be significant in suppressing residue after development. Furthermore, intentionally reducing the content of the above components in the resin to a specific value or less is thought to reduce the content of the above components in the cured product of the photosensitive composition, thereby controlling the polarization structure and charge balance in the cured product. As a result, it is believed that ion migration and electromigration caused by metal impurities and ionic impurities that adversely affect electrical insulation are suppressed, thereby improving migration resistance.
[0083] <(A1) Resin; Other Resins> Examples of polysiloxanes include resins obtained by hydrolyzing and dehydrating condensation of one or more selected from the group consisting of trifunctional organosilanes, tetrafunctional organosilanes, bifunctional organosilanes, and monofunctional organosilanes. The polysiloxane preferably has a trifunctional organosilane unit represented by general formula (9) and / or a tetrafunctional organosilane unit represented by general formula (10).
[0084]
[0085] In the general formula (9) and the general formula (10), R 41 represents a hydrogen atom or a monovalent organic group. 1 ~* 3 R each independently represents a bonding point in the resin. 41is preferably a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 4 to 10 carbon atoms, an aryl group having 6 to 15 carbon atoms, a halogenated alkyl group having 1 to 10 carbon atoms, a halogenated cycloalkyl group having 4 to 10 carbon atoms, or a halogenated aryl group having 6 to 15 carbon atoms. The above-mentioned alkyl group, cycloalkyl group, aryl group, halogenated alkyl group, halogenated cycloalkyl group, and halogenated aryl group may have a heteroatom, and may be either unsubstituted or substituted.
[0086] A maleimide resin is a resin having at least two maleimide groups in at least one of the main chain, side chain, and terminal of the resin. Note that maleimide resins are different from polyimide-based resins.
[0087] Examples of maleimide-styrene resins include resins obtained by radical copolymerizing the above-mentioned maleimide resin with a styrene derivative, and resins obtained by radical copolymerization of a maleimide compound, a styrene derivative, and another copolymerization component such as a (meth)acrylic acid derivative.
[0088] Examples of maleimide-triazine resins include resins obtained by further reacting the above-mentioned maleimide resin with a compound having a triazine structure and / or an aromatic cyanate ester compound, and resins obtained by reacting a maleimide compound with a compound having a triazine structure and / or an aromatic cyanate ester compound.
[0089] Examples of maleimide-oxazine resins include resins obtained by further reacting the above-mentioned maleimide resin with a compound having a benzoxazine structure, and resins obtained by reacting a maleimide compound with a compound having a benzoxazine structure.
[0090] <(A2) Resin> The (A) binder resin preferably contains an (A2) resin, and the (A2) resin preferably contains one or more resins selected from the group consisting of phenolic resins, polyhydroxystyrene, phenolic group-containing epoxy resins, and phenolic group-containing acrylic resins. The (A2) resin may be a single resin or a copolymer thereof.
[0091] Examples of the phenolic resin include resins obtained by reacting a phenolic compound with one or more compounds selected from the group consisting of an aldehyde compound, a ketone compound, an alkoxymethyl compound, and a methylol compound. The phenolic resin is preferably a novolac resin, a resol resin, or a phenol aralkyl resin.
[0092] The phenolic resin preferably contains one or more structural units selected from the group consisting of general formulae (31), (32), (33), (34), (35), (38), (39) and (40).
[0093]
[0094] In the general formulas (31) to (35), X 31 ~X 37 each independently represents an aliphatic structure having 1 to 2 carbon atoms. 33 represents an alkylene group having 1 to 10 carbon atoms. 35 represents a direct bond, an alkylene group having 1 to 6 carbon atoms, an alkylidene group having 1 to 6 carbon atoms, a halogenated alkylene group having 1 to 6 carbon atoms, a halogenated alkylidene group having 1 to 6 carbon atoms, an aromatic group, a condensed polycyclic structure, a condensed polycyclic heterocyclic structure, a structure in which an aromatic ring skeleton and an alicyclic skeleton are directly linked, or a structure in which at least two aromatic ring skeletons are directly linked. 71 ~R 82 R each independently represents a halogen atom, an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 15 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkenyloxy group having 2 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms, a carboxy group, an amino group, or a ring-forming group. The rings connected by the ring-forming group represent a monocyclic or condensed polycyclic hydrocarbon ring.83 ~R 88 each independently represents an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 4 to 10 carbon atoms, an aryl group having 6 to 15 carbon atoms, or a hydroxy group. a represents an integer of 1 to 4. b represents an integer of 1 to 5. m represents an integer of 0 to 3. n represents an integer of 0 to 4. c represents an integer of 1 to 4. o and p each independently represent an integer of 0 to 3. q represents an integer of 0 to 4. d represents an integer of 1 to 4. r and s each independently represent an integer of 0 to 3. t represents an integer of 0 to 4. e represents an integer of 1 to 4. f, g, v, and w each independently represent an integer of 0 to 4. u represents an integer of 0 to 3. h represents an integer of 1 to 3. x represents an integer of 0 to 2. y and z each independently represent 0 or 1. α, β, γ, δ, ε, and ζ each independently represent an integer of 0 to 4. 1 and * 2 each independently represents a bonding point in the resin.
[0095]
[0096] In the general formulae (38) to (40), Z 31 ~Z 34 each independently represents an aliphatic structure having 1 to 2 carbon atoms. 32 represents an aromatic group, a fused polycyclic structure, a fused polycyclic heterocyclic structure, a structure in which an aromatic ring skeleton and an alicyclic skeleton are directly linked, or a structure in which at least two aromatic ring skeletons are directly linked. 34 represents a direct bond, an alkylene group having 1 to 6 carbon atoms, an alkylidene group having 1 to 6 carbon atoms, a halogenated alkylene group having 1 to 6 carbon atoms, a halogenated alkylidene group having 1 to 6 carbon atoms, an aromatic group, a condensed polycyclic structure, a condensed polycyclic heterocyclic structure, a structure in which an aromatic ring skeleton and an alicyclic skeleton are directly linked, or a structure in which at least two aromatic ring skeletons are directly linked. 91 ~R 96R each independently represents a halogen atom, an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 15 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkenyloxy group having 2 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms, a carboxy group, an amino group, or a ring-forming group. The rings connected by the ring-forming group represent a monocyclic or condensed polycyclic hydrocarbon ring. 97 ~R 99 each independently represents an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 4 to 10 carbon atoms, an aryl group having 6 to 15 carbon atoms, or a hydroxy group. a represents an integer of 1 to 4. m represents an integer of 0 to 3. n represents an integer of 0 to 5. b represents an integer of 1 to 4. o represents an integer of 0 to 3. p represents an integer of 0 to 10. However, W 32 where X is the valence of the formula (I), 0≦p≦(X-2). c and d each independently represent an integer of 1 to 4. q and r each independently represent an integer of 0 to 3. α, β, and γ each independently represent an integer of 0 to 4.
[0097] The phenolic resin also preferably has a structural unit represented by general formula (36).
[0098]
[0099] In the general formula (36), X 38 represents an aliphatic structure having 1 to 6 carbon atoms. 89 represents a halogen atom, an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 15 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkenyloxy group having 2 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms, a carboxy group, an amino group, or a ring-forming group. The rings connected by the ring-forming group represent monocyclic or condensed polycyclic hydrocarbon rings. R 90 represents an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 4 to 10 carbon atoms, or an aryl group having 6 to 15 carbon atoms. a represents an integer of 1 to 4. b represents an integer of 0 to 3. α represents an integer of 0 to 4.
[0100] In the general formulae (31) to (36) and (38) to (40), the aliphatic structure, alkyl group, cycloalkyl group, aryl group, alkenyl group, alkoxy group, alkenyloxy group, acyl group, ring-forming group, alkylene group, alkylidene group, aromatic group, fused polycyclic structure, fused polycyclic heterocyclic structure, aromatic ring skeleton, and alicyclic skeleton may have a heteroatom and may be unsubstituted or substituted. The fused polycyclic hydrocarbon ring formed by the ring-forming group is preferably a naphthalene ring, an anthracene ring, a pyrene ring, an indane ring, an indene ring, a tetrahydronaphthalene ring, a fluorene ring, a xanthene ring, or an isoindolinone ring.
[0101] Examples of polyhydroxystyrene include resins obtained by radical copolymerization of a hydroxystyrene derivative with a styrene derivative and / or other copolymerizable components, such as (meth)acrylic acid derivatives or (meth)acrylic acid ester derivatives.
[0102] Examples of phenol group-containing epoxy resins include resins obtained by reacting a polyfunctional epoxy compound with a phenol compound having an epoxy reactive group. Phenol group-containing epoxy resins include those having a fluorene structure, a xanthene structure, an isoindolinone structure, a naphthalene structure, a tricyclo[5.2.1.0] structure, a hydroxybenzoate ... 2,6 ] It is preferable that the aryl group has a decane structure or a biphenyl structure.
[0103] Examples of phenol group-containing acrylic resins include resins obtained by the following (a) to (e): (a) a resin obtained by further reacting an acrylic resin described below with a phenol compound having an addition reactive group, (b) a resin obtained by further reacting a polyfunctional carboxylic acid dianhydride or a polyfunctional carboxylic acid compound with the resin obtained by (a) above, (c) a resin obtained by radical copolymerization of a copolymerization component having a phenolic hydroxyl group with another copolymerization component such as a (meth)acrylic acid derivative, (d) a resin obtained by further reacting a phenol compound having an addition reactive group with the resin obtained by (c) above, and (e) a resin obtained by further reacting a polyfunctional carboxylic acid dianhydride or a polyfunctional carboxylic acid compound with the resin obtained by (d) above.
[0104] The phenol group-containing acrylic resin is a resin different from polyhydroxystyrene. The phenol group-containing acrylic resin preferably has a unit derived from a (meth)acrylic acid ester derivative having a condensed polycyclic structure, a condensed polycyclic heterocyclic structure, or an aromatic structure, or a unit derived from a styrene derivative.
[0105] <(A3) Resin> The (A) binder resin preferably further contains an (A3) resin, and the (A3) resin preferably contains one or more resins selected from the group consisting of polycyclic side chain-containing resins, acid-modified epoxy resins, and acrylic resins. The (A3) resin may be a single resin or a copolymer thereof.
[0106] Examples of polycyclic side chain-containing resins include resins obtained by reacting a polyfunctional epoxy compound with a carboxylic acid compound having a radical polymerizable group, with a polyfunctional carboxylic acid dianhydride. Other examples include resins obtained by reacting a polyfunctional phenol compound with a polyfunctional carboxylic acid dianhydride, with an epoxy compound having a radical polymerizable group. The polycyclic side chain-containing resin is preferably a cardo resin having a fluorene structure, a xanthene structure, or an isoindolinone structure.
[0107] Examples of acid-modified epoxy resins include resins obtained by reacting a polyfunctional epoxy compound with a carboxylic acid compound having a radical polymerizable group, and then reacting the resulting compound with a polyfunctional carboxylic acid dianhydride. Acid-modified epoxy resins include those having a naphthalene structure, tricyclo[5.2.1.0] 2,6 ] Epoxy (meth)acrylate resins having a decane structure or a biphenyl structure are preferred.
[0108] Examples of the acrylic resin include resins obtained by radical copolymerization of one or more selected from the group consisting of (meth)acrylic acid derivatives, (meth)acrylic acid ester derivatives, styrene derivatives, and other copolymerization components.
[0109] The total content of the (A1) resins relative to 100% by mass of the total of the (A) binder resins is preferably 10% by mass or more, more preferably 30% by mass or more, even more preferably 50% by mass or more, and particularly preferably 70% by mass or more, from the viewpoint of improving the mechanical properties and migration resistance when heated at low temperatures. On the other hand, the total content of the (A1) resins is preferably 100% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less, from the viewpoint of improving the mechanical properties when heated at low temperatures.
[0110] The total content of the (A2) resins relative to 100% by mass of the total of the (A) binder resins is preferably 5.0% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and particularly preferably 30% by mass or more, from the viewpoints of suppressing residue after development and improving mechanical properties upon heating at low temperatures. On the other hand, the total content of the (A2) resins is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less, from the viewpoints of improving mechanical properties upon heating at low temperatures.
[0111] The total content of the (A3) resins relative to 100% by mass of the total of the (A) binder resins is preferably 5.0% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and particularly preferably 30% by mass or more, from the viewpoint of improving sensitivity during exposure and mechanical properties upon heating at low temperatures. On the other hand, the total content of the (A3) resins is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less, from the viewpoint of improving mechanical properties upon heating at low temperatures.
[0112] The content ratio of the (A) binder resin in the total solid content of the photosensitive composition of the present invention is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more, from the viewpoint of improving mechanical properties and migration resistance when heated at low temperatures. On the other hand, the content ratio of the (A) binder resin is preferably 75% by mass or less, more preferably 65% by mass or less, and even more preferably 55% by mass or less, from the viewpoint of improving mechanical properties when heated at low temperatures. The total solid content of the composition refers to the sum of the masses of all components in the composition excluding the solvent. The solid content concentration can be calculated by heating 1 g of the composition at 150°C for 30 minutes to evaporate and dry, measuring the mass remaining after heating, and calculating the solid content concentration from the masses before and after heating.
[0113] <(B) Radically Polymerizable Compound> The photosensitive composition of the present invention contains a (B) radically polymerizable compound (hereinafter referred to as "(B) compound") and / or a (F) crosslinking agent. The (B) compound refers to a compound having a radically polymerizable group, and a compound having at least two radically polymerizable groups is preferred. Examples and preferred descriptions regarding the radically polymerizable group are as described above for the (A) binder resin.
[0114] The photosensitive composition of the present invention preferably contains a photosensitizer (C) described below and further contains a compound (B) and / or a crosslinking agent (F); from the viewpoint of accelerating the photoreaction, it is more preferable that the photopolymerization initiator (C1) described below and further contains a compound (B). When the composition has negative photosensitivity, the inclusion of the compound (B) significantly improves the sensitivity during exposure. On the other hand, when the composition has positive photosensitivity, the inclusion of the compound (B) significantly improves the pattern shape control after thermal curing.
[0115] The radical polymerizable group of the (B) compound preferably has an ethylenically unsaturated double bond group, and from the viewpoint of improving sensitivity during exposure and promoting radical polymerization during heating at low temperatures, a (meth)acryloyl group is more preferred. The number of radical polymerizable groups of the (B) compound is preferably 2 or more, more preferably 3 or more, and even more preferably 4 or more, from the viewpoint of improving sensitivity during exposure and improving mechanical properties during heating at low temperatures. On the other hand, the number of radical polymerizable groups is preferably 12 or less, more preferably 10 or less, even more preferably 8 or less, and particularly preferably 6 or less, from the viewpoint of improving mechanical properties during heating at low temperatures and improving migration resistance.
[0116] When the photosensitive composition of the present invention contains the binder resin (A) and the compound (B), the content of the binder resin (A) is preferably 25 parts by mass or more, more preferably 35 parts by mass or more, and even more preferably 45 parts by mass or more, based on 100 parts by mass of the total of the binder resin (A) and the compound (B), from the viewpoints of improving the mechanical properties upon heating at low temperatures and improving the migration resistance. On the other hand, the content of the binder resin (A) is preferably 85 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 75 parts by mass or less, from the viewpoints of improving the sensitivity upon exposure and improving the mechanical properties upon heating at low temperatures.
[0117] <Compound (B1) to Compound (B5)> From the viewpoint of improving sensitivity during exposure and improving mechanical properties during heating at low temperatures, it is preferable that the photosensitive composition of the present invention further satisfy at least one of the following conditions (δ), (ε), and (ζ): (δ) The (B) compound contains the following (B1) first polymerizable compound (hereinafter, "(B1) compound") and (B2) second polymerizable compound (hereinafter, "(B2) compound"). (ε) The (B) compound contains the following (B3) third polymerizable compound (hereinafter, "(B3) compound") and (B4) fourth polymerizable compound (hereinafter, "(B4) compound"). (ζ) The (B) compound contains the following (B1) compound or (B2) compound, and further contains the following (B3) compound or (B4) compound. (B1) compound: a compound having the following (I-b1) structure and further having at least two radically polymerizable groups. (I-b1) structure: a structure containing an alicyclic structure and / or a structure containing a heteroalicyclic structure. (B2) compound: a compound having the following (I-b2) structure and (II-b2) structure and further having at least two radically polymerizable groups. (I-b2) structure: a structure containing an aromatic structure. (II-b2) Structure: A structure containing an aliphatic structure. (B3) Compound: A compound having at least two (meth)acryloyl groups and further having the following structure (I-b3). (I-b3) Structure: At least two (meth)acryloyl groups are connected by a minimum of 4 to 10 atoms, and a structure containing an aliphatic structure. (B4) Compound: A compound having at least two (meth)acryloyl groups and further having the following structure (I-b4). (I-b4) Structure: At least two (meth)acryloyl groups are connected by a minimum of 11 to 45 atoms, and a structure containing an aliphatic structure.
[0118] In the compound (B1), the alicyclic structure in the structure (I-b1) is preferably a fused polycyclic alicyclic structure from the viewpoint of improving mechanical properties when heated at low temperatures, and more preferably a tricyclo[5.2.1.0] 2,6]decane structure is more preferred. Furthermore, from the viewpoint of improving mechanical properties and migration resistance when heated at low temperatures, the heteroalicyclic structure in the (I-b1) structure is preferably a nitrogen-containing cyclic structure, more preferably a cyclic structure having at least two nitrogen atoms, and even more preferably an isocyanuric acid structure and / or a triazine structure. In the (B1) compound, the number of nitrogen atoms in the heteroalicyclic structure in the (I-b1) structure is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more. Meanwhile, the number of nitrogen atoms is preferably 6 or less, more preferably 4 or less.
[0119] The compound (B1) preferably further has the following structure (II-b1): Structure (II-b1): Structure containing an aliphatic structure In the compound (B1), the aliphatic structure in the structure (II-b1) is preferably an alkylene group, an oxyalkylene group, an alkylene group containing a hydroxy group, an oxyalkylene group containing a hydroxy group, an alkylenecarbonyl group, an oxyalkylenecarbonyl group, or an aminoalkylenecarbonyl group, from the viewpoints of improving sensitivity during exposure and improving migration resistance.
[0120] In the compound (B2), the aromatic structure in the structure (I-b2) is preferably a benzene structure or a biphenyl structure from the viewpoint of improving mechanical properties when heated at low temperatures. From the same viewpoint, the aromatic structure in the structure (I-b2) is preferably a fused polycyclic structure, more preferably a fluorene structure, an indane structure, or a naphthalene structure. From the same viewpoint, the aromatic structure in the structure (I-b2) is preferably a fused polycyclic heterocyclic structure, more preferably a xanthene structure, an indolinone structure, or an isoindolinone structure.
[0121] In the compound (B2), from the viewpoints of improving sensitivity during exposure and improving migration resistance, the aliphatic structure in the structure (II-b2) is preferably an alkylene group, an oxyalkylene group, an alkylene group containing a hydroxy group, an oxyalkylene group containing a hydroxy group, an alkylenecarbonyl group, an oxyalkylenecarbonyl group, or an aminoalkylenecarbonyl group.
[0122] When the (B3) compound or the (B4) compound has two (meth)acryloyl groups, the minimum number of atoms in the (I-b3) structure or the (I-b4) structure refers to the minimum number of atoms, including carbon atoms and heteroatoms, between the carbonyl carbons of the two (meth)acryloyl groups. The atoms bonded to the carbon atoms and heteroatoms between the carbonyl carbons are not included in the calculation of the minimum number of atoms. For example, when an oxygen atom, a propylene group, and an oxygen atom are present between the carbonyl carbons, the minimum number of atoms is five. Furthermore, when the (B3) compound or the (B4) compound has three or more (meth)acryloyl groups, the minimum number of atoms refers to the minimum number of atoms, including carbon atoms and heteroatoms linking the carbonyl carbons of all of the (meth)acryloyl groups. Similarly, the atoms bonded to the carbon atoms and heteroatoms linking the carbonyl carbons are not included in the calculation of the minimum number of atoms.
[0123] By setting the minimum number of atoms in the (I-b3) structure within a specific range for the (B3) compound, the amount of low molecular weight molecules derived from the (B) compound in the cured product can be further reduced, resulting in a significant improvement in migration resistance. The minimum number of atoms in the (I-b3) structure is preferably 5 or more, more preferably 6 or more. Meanwhile, the minimum number of atoms in the (I-b3) structure is preferably 9 or less, more preferably 8 or less. Meanwhile, by setting the minimum number of atoms in the (I-b4) structure within a specific range for the (B4) compound, the molecular mobility is improved, thereby increasing the probability of collisions between (meth)acryloyl groups and between (meth)acryloyl groups and other radically polymerizable groups, resulting in a significant improvement in sensitivity during exposure. The minimum number of atoms in the (I-b4) structure is preferably 13 or more, more preferably 15 or more, even more preferably 17 or more, and particularly preferably 20 or more. On the other hand, the minimum number of atoms in the above (I-b4) structure is preferably 40 or less, more preferably 35 or less, even more preferably 30 or less, and particularly preferably 25 or less.
[0124] In the (B3) compound and the (B4) compound, the aliphatic structure in the (I-b3) structure and the (I-b4) structure is preferably an alkylene group, an oxyalkylene group, an alkylene group containing a hydroxy group, an oxyalkylene group containing a hydroxy group, an alkylenecarbonyl group, an oxyalkylenecarbonyl group, or an aminoalkylenecarbonyl group, from the viewpoint of improving sensitivity during exposure and improving migration resistance. Furthermore, the aliphatic structure in the (I-b3) structure and the (I-b4) structure is preferably a structure derived from an aliphatic polyfunctional alcohol. The (B3) compound and the (B4) compound are different compounds from the (B1) compound and the (B2) compound, and do not have a structure containing an alicyclic structure, a structure containing a heteroalicyclic structure, or a structure containing an aromatic structure.
[0125] The (B) compounds as described above not only have the effect of improving the degree of crosslinking of the cured product due to the generation of radicals during exposure or heating at low temperatures, but also have the effect of improving the degree of crosslinking due to reaction with the side chain or terminal radical polymerizable groups of the resin, and are therefore presumed to improve mechanical properties when heated at low temperatures. Furthermore, the (B) compounds having an aliphatic structure in the (II-b1), (II-b2), (I-b3), or (I-b4) structure described above are presumed to suppress ion migration and electromigration by reducing the low-molecular-weight components derived from the (B) compounds in the cured product, thereby improving migration resistance.
[0126] From the viewpoint of improving mechanical properties when heated at low temperatures, it is also preferable that the (B) compound further contains the following (B5) compound. Note that the (B5) compound is a compound different from the above-mentioned (B2) compound and does not have the above-mentioned (II-b2) structure. (B5) compound: a compound having a structure containing a fused polycyclic structure and / or a structure containing a fused polycyclic heterocyclic structure, and further having at least two radically polymerizable groups. In the (B5) compound, the above-mentioned fused polycyclic structure is preferably a fluorene structure, an indane structure, or a naphthalene structure. In the (B5) compound, the above-mentioned fused polycyclic heterocyclic structure is preferably a xanthene structure, an indolinone structure, or an isoindolinone structure.
[0127] The (B) compound preferably contains one or more compounds selected from the group consisting of the (B1) compound, the (B2) compound, the (B3) compound, the (B4) compound, and the (B5) compound. The (B) compound preferably contains two or more compounds selected from the group consisting of the (B1) compound, the (B2) compound, the (B3) compound, and the (B4) compound, and more preferably further contains the (B5) compound. The preferred contents of these (B) compounds are the same as those described above.
[0128] The total content of the (B1) compound, the (B2) compound, the (B3) compound, the (B4) compound, and the (B5) compound is preferably 15 parts by mass or more, more preferably 20 parts by mass or more, and even more preferably 25 parts by mass or more, while the total content of the (B1) compound, the (B2) compound, the (B3) compound, the (B4) compound, and the (B5) compound is preferably 75 parts by mass or less, more preferably 65 parts by mass or less, and even more preferably 55 parts by mass or less.
[0129] <(C) Photosensitizer> The photosensitive composition of the present invention contains (C) a photosensitizer. (C) The photosensitizer refers to a compound that undergoes bond cleavage, reaction, or structural change upon exposure to generate another compound, thereby imparting positive or negative photosensitivity to the composition.
[0130] The (C) photosensitizer preferably contains one or more selected from the group consisting of a (C1) photopolymerization initiator, a (C2) naphthoquinone diazide compound, a (C3) photoacid generator, and a (C4) photobase generator. When negative photosensitivity is imparted to the composition, the (C1) photopolymerization initiator is preferably contained, and more preferably, one or more selected from the group consisting of a (C2) naphthoquinone diazide compound, a (C3) photoacid generator, and a (C4) photobase generator. When positive photosensitivity is imparted to the composition, the (C2) naphthoquinone diazide compound is preferably contained, and more preferably, one or more selected from the group consisting of a (C1) photopolymerization initiator, a (C3) photoacid generator, and a (C4) photobase generator.
[0131] The content of the (C) photosensitizer is preferably 1.0 part by mass or more, more preferably 3.0 parts by mass or more, and even more preferably 5.0 parts by mass or more, from the viewpoint of improving sensitivity during exposure, where the total of the (A) binder resin and the (B) compound is taken as 100 parts by mass, while the content of the (C) photosensitizer is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, from the viewpoint of suppressing residues after development.
[0132] <(C1) Photopolymerization Initiator> The (C1) photopolymerization initiator refers to a compound that generates radicals by bond cleavage and / or reaction upon exposure. The inclusion of the (C1) photopolymerization initiator is suitable for negative pattern formation, and the effect of improving sensitivity during exposure is significant. The (C1) photopolymerization initiator is preferably an α-hydroxyketone compound, an α-aminoketone compound, a biimidazole compound, a phosphine oxide compound, or an oxime ester compound. The preferred contents of these (C) photosensitizers are the same as those described above.
[0133] From the viewpoints of improving sensitivity during exposure and improving mechanical properties during heating at low temperatures, the (C) photosensitizer contains a (C1) photopolymerization initiator, and the (C1) photopolymerization initiator preferably contains a (C1-1) oxime ester compound (hereinafter referred to as "(C1-1) compound") and / or a (C1-2) phosphine oxide compound (hereinafter referred to as "(C1-2) compound"), and more preferably contains a (C1-1) compound. The (C1-1) compound refers to a compound having an oxime ester structure in the molecule as a structure that undergoes bond cleavage and / or reaction upon exposure to generate radicals. The (C1-2) compound refers to a compound that has a phosphine oxide structure in the molecule and an acyl group as a structure that undergoes bond cleavage and / or reaction upon exposure to generate radicals. The preferred contents of these (C) photosensitizers are the same as those described above.
[0134] From the viewpoint of improving sensitivity during exposure and improving mechanical properties during heating at low temperatures, the (C1-1) compound preferably has one or more selected from the group consisting of the following (I) and (II): (I) a structure in which at least one oxime ester structure is bonded to a fused polycyclic structure, a fused polycyclic heterocyclic structure, a diphenyl sulfide structure, or a benzene structure (α-oxime structure) or a structure in which at least one oxime ester carbonyl structure is bonded to a fused polycyclic structure, a fused polycyclic heterocyclic structure, a diphenyl sulfide structure, or a benzene structure; (II) one or more selected from the group consisting of a nitro group, a group substituted with a halogen atom, a naphthylcarbonyl structure, a trimethylbenzoyl structure, a thiophenylcarbonyl structure, a furylcarbonyl structure, at least two oxime ester structures, and a structure in which at least two oxime ester carbonyl structures are bonded (hereinafter referred to as "specific substituents").
[0135] The fused polycyclic structure is preferably a fluorene structure, a benzofluorene structure, a dibenzofluorene structure, an indene structure, an indane structure, a benzoindene structure, or a benzoindane structure. The fused polycyclic heterocyclic structure is preferably a carbazole structure, a dibenzofuran structure, a dibenzothiophene structure, a benzocarbazole structure, an indole structure, an indoline structure, a benzoindole structure, a benzoindoline structure, a phenothiazine structure, or a phenothiazine oxide structure. The (C1-1) compound more preferably has a structure in which a specific substituent is bonded to a fused polycyclic structure, a fused polycyclic heterocyclic structure, a diphenyl sulfide structure, or a benzene structure.
[0136] From the viewpoint of improving sensitivity during exposure and improving mechanical properties during heating at low temperatures, the (C1-1) compound preferably has a group substituted with a halogen atom, more preferably a group substituted with a fluorine atom. The group substituted with a halogen atom is preferably a trifluoromethyl group, a trifluoropropyl group, a trichloropropyl group, a tetrafluoropropyl group, a fluorocyclopentyl group, a fluorophenyl group, or a pentafluorophenyl group. When the polyimide resin has a carboxylic acid residue having a fluorine atom and / or an amine residue having a fluorine atom, it is presumed that the (C1-1) compound as described above improves compatibility with the binder resin (A), and promotes radical polymerization from the film surface to the depth of the film.
[0137] From the viewpoint of photobleaching properties, the (C1-1) compound preferably has a fluorene structure, a benzofluorene structure, a dibenzofluorene structure, an indole structure, a benzoindole structure, a phenothiazine structure, a phenothiazine oxide structure, or a diphenyl sulfide structure, and also preferably has a structure in which at least one oxime ester carbonyl structure is bonded to a fused polycyclic structure, a fused polycyclic heterocyclic structure, a diphenyl sulfide structure, or a benzene structure. When the (C1-1) compound has photobleaching properties, the effects of improving sensitivity during exposure and improving pattern processability in thick films become significant. Furthermore, it is presumed that the reduction of low-molecular-weight components derived from the (C1-1) compound in the cured product suppresses ion migration and electromigration, thereby improving migration resistance. The photobleachability refers to a decrease in absorbance at wavelengths in the ultraviolet region (e.g., 400 nm or less) and / or absorbance at wavelengths of visible light (380 to 780 nm) due to bond cleavage and / or reaction upon exposure to light.
[0138] The (C1-1) compound as described above is presumed to have the effect of improving the degree of crosslinking of the cured product and promoting the ring-closing reaction of the resin due to the generation of radicals when heated at low temperatures and the interaction of the oxime ester structure, thereby improving the mechanical properties when heated at low temperatures.
[0139] Examples of the (C1-2) compound include 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-(2,4,4-trimethylpentyl)phosphine oxide.
[0140] The (C1-2) compound as described above is presumed to have the effect of improving the degree of crosslinking of the cured product and accelerating the ring-closing reaction of the resin due to the generation of radicals when heated at low temperatures and the interaction of the phosphine oxide structure, thereby improving the mechanical properties when heated at low temperatures.
[0141] <(C2) Naphthoquinone Diazide Compound> The (C2) naphthoquinone diazide compound refers to a compound that undergoes a structural change upon exposure to generate an indene carboxylic acid and / or a sulfoindene carboxylic acid. The inclusion of a (C2) naphthoquinone diazide compound is suitable for forming a positive-tone pattern. The (C2) naphthoquinone diazide compound is preferably a 1,2-naphthoquinone diazide-5-sulfonic acid ester or a 1,2-naphthoquinone diazide-4-sulfonic acid ester of a compound having a phenolic hydroxyl group. The preferred contents of these (C) photosensitizers are the same as those described above.
[0142] <(C3) Photoacid Generator> The (C3) photoacid generator refers to a compound that generates an acid by bond cleavage and / or reaction upon exposure. The inclusion of a (C3) photoacid generator is suitable for negative pattern formation from the viewpoint of promoting cationic polymerization, etc. On the other hand, when a resin or the like has an acidic group protected by an acid-dissociable group, it is suitable for positive pattern formation from the viewpoint of liberating the acidic group upon exposure. Examples of the (C3) photoacid generator include ionic compounds and nonionic compounds. Preferred ionic compounds are triorganosulfonium salt compounds. Preferred nonionic compounds are halogen-containing compounds, diazomethane compounds, sulfone compounds, sulfonate ester compounds, carboxylate ester compounds, sulfonimide compounds, phosphate ester compounds, or sulfonebenzotriazole compounds. The preferred content of each of these (C) photosensitizers is the same as described above.
[0143] <(C4) Photobase Generator> The (C4) photobase generator refers to a compound that generates a base by bond cleavage and / or reaction upon exposure. The inclusion of a (C4) photobase generator is suitable for negative-tone pattern formation from the viewpoint of promoting anionic polymerization, etc. On the other hand, when a resin or the like has a base-dissociable protected acidic group, it is suitable for positive-tone pattern formation from the viewpoint of liberating the acidic group upon exposure. Examples of the (C4) photobase generator include ionic compounds and nonionic compounds. Preferred ionic compounds are diazabicycloalkene salt compounds, triazabicycloalkene salt compounds, α-keto quaternary ammonium salt compounds, benzyl quaternary ammonium salt compounds, guanidine salt compounds, and biguanide salt compounds. Preferred ionic compounds have a ketoprofen structure, an oxoxanthene structure, a benzofuran structure, or a naphthalene structure. The nonionic compound is preferably a nitrobenzyl carbamate compound, an anthracenyl carbamate compound, a benzoin-based carbamate compound, an anthraquinone-based carbamate compound, a hydroxycinnamamide-based compound, or a coumarinamide-based compound. The preferred content of each of these (C) photosensitizers is the same as above.
[0144] <(D) Colorant> The photosensitive composition of the present invention preferably further contains a (D) colorant. The (D) colorant refers to a compound that imparts color by absorbing light of a visible light wavelength (380 to 780 nm). The inclusion of the (D) colorant makes it possible to adjust the chromaticity of transmitted or reflected light through a film of the composition and to impart light-blocking properties to the film of the composition. The (D) colorant is preferably a pigment or a dye. From the viewpoint of improving light-blocking properties, the (D) colorant preferably contains a black agent.
[0145] The term "black" in the case of a (D) colorant refers to a color index generic name (hereinafter referred to as "C.I. number") containing "BLACK." When a colorant without a C.I. number is contained, the colorant is black when formed into a cured film. The term "black" when formed into a cured film refers to a cured film in which the transmittance per 1.0 μm film thickness at a wavelength of 550 nm is converted to a film thickness of 0.10 to 1.5 μm based on the Beer-Lambert equation so that the transmittance at a wavelength of 550 nm is 10%, and the converted transmittance at wavelengths of 450 to 650 nm in the transmission spectrum is 25% or less. The transmission spectrum of the cured film can be determined based on the method described in paragraph
[0285] of WO 2019 / 087985.
[0146] The content ratio of the colorant (D) relative to the total solid content of the photosensitive composition of the present invention is preferably 5.0% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, even more preferably 20% by mass or more, and particularly preferably 30% by mass or more, from the viewpoints of improving light-shielding property and improving reliability. On the other hand, the content ratio of the colorant (D) relative to the total solid content of the photosensitive composition of the present invention is preferably 70% by mass or less, more preferably 50% by mass or less, from the viewpoints of improving sensitivity during exposure and suppressing residues after development.
[0147] The (D) colorant preferably contains a black pigment, more preferably an organic black pigment and / or an inorganic black pigment. The organic black pigment is preferably a benzofuranone-based black pigment, a perylene-based black pigment, an azomethine-based black pigment, an anthraquinone-based black pigment, an aniline-based black pigment, an azo-based black pigment, or carbon black. The inorganic black pigment is preferably a metal element fine particle, oxide, composite oxide, sulfide, sulfate, nitrate, carbonate, nitride, carbide, or oxynitride. The metal element is preferably Ti, Zr, V, Cr, Mn, Co, Ni, Y, Nb, Hf, Ta, W, Re, Fe, Cu, Zn, or Ag. The inorganic black pigment preferably contains an element other than these metal elements, more preferably B, Al, Si, Mn, Co, Ni, Fe, Cu, Zn, or Ag. The (D) colorant also preferably contains a black dye. The black dye preferably contains a black dye containing elemental chromium and / or an azo-based black dye. The preferred content ratios of these colorants (D) are the same as those described above.
[0148] The benzofuranone-based black pigment preferably contains a compound having at least two benzofuran-2(3H)-one structures which may share a benzene ring or at least two benzofuran-3(2H)-one structures which may share a benzene ring, a geometric isomer thereof, a salt thereof, or a salt of a geometric isomer thereof. The perylene-based black pigment preferably contains a compound having a 3,4,9,10-perylenetetracarboxylic acid bisbenzimidazole structure, a geometric isomer thereof, a salt thereof, or a salt of a geometric isomer thereof. The azomethine-based black pigment preferably contains a compound having an azomethine structure and a carbazole structure or a salt thereof.
[0149] The (D) colorant preferably contains a mixture of two or more colors of colorants, more preferably (I) blue, red, and yellow, (II) blue, red, and orange, (III) blue, purple, and orange, or (IV) purple and yellow. The colorant mixture is more preferably a color pigment mixture and / or a color dye mixture. The color pigment is preferably an anthraquinone-based pigment, a diketopyrrolopyrrole-based pigment, a perylene-based pigment, an isoindoline-based pigment, an isoindolinone-based pigment, an imidazolone-based pigment, a quinacridone-based pigment, a pyranthrone-based pigment, a phthalocyanine-based pigment, an indanthrone-based pigment, or a dioxazine-based pigment. The color dye is preferably a squarylium-based dye, a xanthene-based dye, a triarylmethane-based dye, or a phthalocyanine-based dye. The preferred content ratios of these (D) colorants are the same as those described above.
[0150] In the photosensitive composition of the present invention, the pigment preferably has a coating layer. The coating layer refers to a layer that coats the surface of the pigment, and examples thereof include a layer formed by surface treatment with a silane coupling agent, surface treatment with a silicate, surface treatment with a metal alkoxide, or coating treatment with a resin. The coating layer preferably has one or more types selected from the group consisting of a silica coating layer, a metal oxide coating layer, and a metal hydroxide coating layer.
[0151] <(E) Dispersant> The photosensitive composition of the present invention preferably further contains a (E) dispersant. The (E) dispersant refers to a compound having a surface affinity structure that interacts with the pigment surface and a dispersion stabilizing structure that inhibits approach of pigments to each other. From the viewpoint of improving the dispersion stability of the pigment, the photosensitive composition of the present invention more preferably contains a pigment and further contains a (E) dispersant.
[0152] The dispersant (E) is preferably a dispersant having a basic group, a dispersant having a basic group and an acidic group, or a dispersant having a salt structure of a basic group. Note that the dispersant may also contain a dispersant having an acidic group, a dispersant having a salt structure of an acidic group, or a dispersant having neither a basic group nor an acidic group.
[0153] The basic group of the (E) dispersant is preferably a tertiary amino group or a nitrogen-containing ring structure. The acidic group of the (E) dispersant is preferably a carboxy group, a sulfonic acid group, or a phosphate group. The salt structure of the basic group of the (E) dispersant is preferably a quaternary ammonium salt structure or a salt structure of a nitrogen-containing ring structure. The counter anion in the salt structure of the basic group is preferably a carboxylate anion, a sulfonate anion, a sulfate anion, a nitrate anion, a phosphate anion, or a halogen anion. The polymer chain of the (E) dispersant is preferably a fluororesin, a silicone, an acrylic resin, a polyoxyalkylene ether, a polyester, a polyurethane, a polyol, a polyalkyleneamine, a polyethyleneimine, or a polyallylamine.
[0154] When the photosensitive composition of the present invention contains a pigment, the content of the dispersant (E) is preferably 5.0 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, based on 100 parts by mass of the pigment, from the viewpoint of improving the dispersion stability of the pigment. On the other hand, the content of the dispersant (E) is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, from the viewpoint of improving the sensitivity during exposure.
[0155] <(F) Crosslinking Agent> The photosensitive composition of the present invention contains the compound (B) and / or the crosslinking agent (F). The crosslinking agent (F) refers to a compound having a crosslinkable group, a cationically polymerizable group, or an anionically polymerizable group that can react with a resin, etc.
[0156] The photosensitive composition of the present invention preferably contains the above-mentioned (C) photosensitizer and further contains the (B) compound and / or the (F) crosslinking agent, and from the viewpoint of accelerating the photoreaction, it is more preferable that it contains the above-mentioned (C3) photoacid generator or (C4) photobase generator and further contains the (F) crosslinking agent. On the other hand, from the viewpoint of improving the degree of crosslinking of resins, etc., it is also preferable that it contains the above-mentioned (C2) naphthoquinone diazide compound and further contains the (F) crosslinking agent.
[0157] From the viewpoints of improving sensitivity during exposure and improving mechanical properties upon heating at low temperatures, the (F) crosslinking agent is preferably a compound having one or more groups selected from the group consisting of an alkoxyalkyl group, a hydroxyalkyl group, an epoxy group, an oxetanyl group, and a blocked isocyanate group (hereinafter referred to as "specific crosslinkable groups"). The alkoxyalkyl group is preferably an alkoxymethyl group or an alkoxyethyl group, and more preferably a methoxymethyl group or a methoxyethyl group. The hydroxyalkyl group is preferably a methylol group or an ethylol group. From the viewpoints of improving sensitivity during exposure and improving mechanical properties upon heating at low temperatures, the number of specific crosslinkable groups possessed by the (F) crosslinking agent is preferably 2 or more, more preferably 3 or more, even more preferably 4 or more, and particularly preferably 6 or more. On the other hand, from the viewpoints of improving mechanical properties upon heating at low temperatures, the number of specific crosslinkable groups is preferably 12 or less, more preferably 10 or less, and even more preferably 8 or less.
[0158] The content of the (F) crosslinking agent is preferably 1.0 part by mass or more, more preferably 3.0 parts by mass or more, and even more preferably 5.0 parts by mass or more, from the viewpoints of improving sensitivity during exposure and improving mechanical properties upon heating at low temperatures, relative to 100 parts by mass of the total of the (A) binder resin and the (B) compound. On the other hand, the content of the (F) crosslinking agent is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, from the viewpoints of suppressing residues after development and improving mechanical properties upon heating at low temperatures.
[0159] <Compound (F1) and Compound (F2)> From the viewpoints of suppressing residue after development and improving mechanical properties when heated at low temperatures, the (F) crosslinking agent preferably contains the following compound (F1) and / or compound (F2). The preferred contents of these (F) crosslinking agents are also the same as those described above. Compound (F1): a compound having at least two phenolic hydroxyl groups and at least two specific crosslinkable groups Compound (F2): a compound having a structure containing a heteroalicyclic structure and at least two specific crosslinkable groups.
[0160] The compound (F1) preferably has at least two structures in which a phenolic hydroxyl group and a specific crosslinkable group are bonded to one aromatic structure, and more preferably has at least two structures in which a phenolic hydroxyl group and at least two specific crosslinkable groups are bonded to one aromatic structure.
[0161] The heteroalicyclic structure in the compound (F2) is preferably a nitrogen-containing cyclic structure, more preferably a cyclic structure having at least two nitrogen atoms. The cyclic structure having at least two nitrogen atoms is preferably one or more selected from the group consisting of an isocyanuric acid structure, a triazine structure, a glycoluril structure, an imidazolidone structure, a pyrazole structure, an imidazole structure, a triazole structure, a tetrazole structure, and a purine structure, more preferably an isocyanuric acid structure and / or a triazine structure. The number of nitrogen atoms in the heteroalicyclic structure in the compound (F2) is preferably one or more, more preferably two or more, and even more preferably three or more. Meanwhile, the number of nitrogen atoms is preferably six or less, more preferably four or less.
[0162] <(G) Inorganic Particles> From the viewpoint of improving migration resistance, the photosensitive composition of the present invention preferably further contains (G) inorganic particles. (G) Inorganic particles refer to particles containing, as a main component, an element selected from the group consisting of a metal element, a metalloid element, and a semiconductor element. The main component refers to the component that is contained in the largest amount by mass among the constituent components. From the viewpoint of improving migration resistance, the (G) inorganic particles preferably have hydroxy groups and / or silanol groups on the particle surface.
[0163] From the viewpoint of improving migration resistance, the photosensitive composition of the present invention further contains (G) inorganic particles, and the (G) inorganic particles preferably contain one or more particles selected from the group consisting of silica particles, alumina particles, titania particles, vanadium oxide particles, chromium oxide particles, iron oxide particles, cobalt oxide particles, copper oxide particles, zinc oxide particles, zirconium oxide particles, niobium oxide particles, tin oxide particles, and cerium oxide particles, and from the viewpoint of improving migration resistance and suppressing external light reflection, it is more preferable that the (G) inorganic particles contain silica particles.
[0164] From the viewpoint of improving migration resistance, the silica particles preferably have a functional group on the surface. The functional group on the surface of the silica particles is preferably a radical polymerizable group, a thermally reactive group, a hydroxy group, a silanol group, an alkoxysilyl group, an alkylsilyl group, a dialkylsilyl group, a trialkylsilyl group, a phenylsilyl group, or a diphenylsilyl group. The radical polymerizable group or the thermally reactive group is also preferably a reactive residue of a surface modifying group containing a radical polymerizable group or a reactive residue of a surface modifying group containing a thermally reactive group. It is more preferable that the silica particles have a radical polymerizable group and / or a thermally reactive group on the surface. Examples and preferred descriptions of the radical polymerizable group are as described above in the binder resin (A).
[0165] From the viewpoint of improving migration resistance, the average primary particle diameter of the silica particles is preferably 5.0 nm or more, more preferably 7.0 nm or more, and even more preferably 10 nm or more. On the other hand, from the viewpoint of suppressing residues after development and external light reflection, the average primary particle diameter of the silica particles is preferably 200 nm or less, more preferably 100 nm or less, even more preferably 70 nm or less, even more preferably 50 nm or less, particularly preferably 30 nm or less, and most preferably 20 nm or less.
[0166] The average primary particle size of the silica particles is preferably more than 0.20 μm, more preferably 0.30 μm or more, and even more preferably 0.50 μm or more, from the viewpoint of increasing the elastic modulus and decreasing the thermal expansion coefficient, while the average primary particle size of the silica particles is preferably 100 μm or less, more preferably 50 μm or less, even more preferably 30 μm or less, still more preferably 10 μm or less, particularly preferably 5.0 μm or less, and most preferably 3.0 μm or less, from the viewpoint of suppressing residues after development.
[0167] The primary particle size of silica particles refers to the major axis diameter of the primary particles of silica particles. The average primary particle size of silica particles in a film can be calculated by imaging and analyzing the cross section of the film using a transmission electron microscope (hereinafter referred to as "TEM") and measuring 30 primary particles of silica particles as the average value. The average primary particle size of silica particles in a silica particle dispersion can be determined by measuring the particle size distribution by dynamic light scattering or laser diffraction / scattering. Examples of measuring instruments that can be used for the dynamic light scattering method include the SZ-100 manufactured by Horiba, Ltd., and for the laser diffraction / scattering method, the SLD3100 manufactured by Shimadzu Corporation or the LA-920 manufactured by Horiba, Ltd., or equivalents thereof.
[0168] The silica particles described above are believed to capture metal impurities, ionic impurities, and other substances that adversely affect electrical insulation due to the acidity and negative charge of the hydroxyl groups and / or silanol groups on the particle surface. Furthermore, the robust structure of the particles allows them to retain the captured impurities even after heat treatment or voltage application, which is thought to improve migration resistance. Furthermore, the silica particles unevenly distributed on the surface of the cured product are believed to reduce the reflection and scattering of incident external light.
[0169] From the viewpoint of improving migration resistance, the silica particles preferably contain silica particles containing sodium element. The sodium element may exist in the form of, for example, ions (Na +) or a salt with a silanol group (Si—ONa). The sodium content in the silica particles is preferably 1.0 ppm by mass or more, more preferably 5.0 ppm by mass or more, even more preferably 10 ppm by mass or more, even more preferably 50 ppm by mass or more, and particularly preferably 100 ppm by mass or more. On the other hand, the sodium content in the silica particles is preferably 10,000 ppm by mass or less, more preferably 5,000 ppm by mass or less, and even more preferably 1,000 ppm by mass or less. The sodium contained in the silica particles can be detected by imaging and analyzing the cross section of the film using transmission electron microscope-energy dispersive X-ray spectroscopy (hereinafter referred to as “TEM-EDX”). It is believed that intentionally incorporating a trace amount of sodium into the silica particles controls the polarization structure and charge balance in the cured product. This is thought to efficiently capture metal impurities and ionic impurities that adversely affect electrical insulation, thereby improving migration resistance.
[0170] The content of the (G) inorganic particles in the total solid content of the photosensitive composition of the present invention is preferably 5.0% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and particularly preferably 20% by mass or more, from the viewpoint of improving migration resistance, while the content of the (G) inorganic particles is preferably 90% by mass or less, more preferably 70% by mass or less, and even more preferably 50% by mass or less, from the viewpoint of suppressing residues after development.
[0171] <Other Additives> The photosensitive composition of the present invention preferably further contains one or more additives selected from the group consisting of a thermal color former, an oxidative color former, a dissolution promoter, an ink repellent, a sensitizer, a chain transfer agent, a polymerization inhibitor, a silane coupling agent, and a surfactant. Known additives may be used as these additives.
[0172] <Solvent> The photosensitive composition of the present invention preferably further contains a solvent. From the viewpoint of solubility of various resins and various additives, the solvent is preferably a compound having an alcoholic hydroxyl group, a carbonyl group, an ester bond, an amide bond, or at least three ether bonds.
[0173] When the photosensitive composition of the present invention contains a pigment and further contains a dispersant, the solvent is preferably a compound having a carbonyl group, an ester bond, or an amide bond, more preferably a compound having an alkylcarbonyl group, a dialkylcarbonyl group, a formyl group, a carboxy group, a carboxylic acid ester bond, a carbonate ester bond, a formate ester bond, an amide group, an imide group, a urea bond, or a urethane bond, and even more preferably a compound having an acetate bond, a propionate bond, or a butyrate bond.
[0174] <Contents of specific aromatic compound, specific anion, and specific organic acid> The photosensitive composition of the first aspect of the present invention satisfies the following condition (α): The photosensitive composition of the second aspect of the present invention satisfies one or more selected from the group consisting of the following conditions (α), (β), and (γ): (α) The composition further contains one or more ions selected from the group consisting of sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing fluorine element, and satisfies the following condition (1x): (1x) The total content of sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing fluorine element in the total solid content of the photosensitive composition is 0.010 to 1,000 ppm by mass; (β) The composition further contains one or more ions selected from the group consisting of chloride ions, bromide ions, sulfate ions, sulfite ions, nitrate ions, nitrite ions, phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions, and satisfies the following condition (2x): (2x) The total content of chloride ions, bromide ions, sulfate ions, sulfite ions, nitrate ions, nitrite ions, phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions in the total solid content of the photosensitive composition is 0.010 to 1,000 ppm by mass. (γ) The photosensitive composition further contains one or more members selected from the group consisting of benzene, toluene, xylene, and naphthalene, and satisfies the following condition (3): (3) The total content of benzene, toluene, xylene, and naphthalene in the photosensitive composition is 0.010 to 1,000 ppm by mass.
[0175] Sulfonic acid is an organic compound having at least one sulfonic acid group. The sulfonic acid has a substituent containing a carbon element, and is preferably a compound having a sulfonic acid group. Phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, and hypophosphite ester are preferably compounds having a substituent containing a carbon element and an acidic group containing a phosphorus element. The carboxylic acid containing a fluorine element is preferably a compound having a substituent containing a fluorine element and a carbon element, and having a carboxy group.
[0176] When the above condition (β) is satisfied, the photosensitive composition of the present invention preferably further contains a compound containing a specific anion. When the photosensitive composition of the present invention contains a compound containing a specific anion, it preferably further contains an ammonium ion, a primary ammonium ion, a secondary ammonium ion, a tertiary ammonium ion, or a quaternary ammonium ion as a cationic species.
[0177] The above phosphoric acid ester, phosphonic acid ester, phosphonic acid ester, phosphorous acid ester, phosphinic acid, and hypophosphite ester are preferably phosphoric acid monoester, phosphoric acid diester, phosphonic acid, phosphonic acid monoester, phosphorous acid monoester, phosphorous acid diester, phosphinic acid, or hypophosphite monoester.
[0178] The specific organic acid preferably has one or more selected from the group consisting of mono- to di-valent aliphatic groups having 1 to 18 carbon atoms, mono- to di-valent alicyclic groups having 4 to 18 carbon atoms, mono- to di-valent aromatic groups having 6 to 15 carbon atoms, mono- to di-valent fluorine-containing aliphatic groups having 1 to 18 carbon atoms, mono- to di-valent fluorine-containing alicyclic groups having 4 to 18 carbon atoms, and mono- to di-valent fluorine-containing aromatic groups having 6 to 15 carbon atoms.
[0179] The photosensitive composition of the second aspect of the present invention preferably satisfies two or more conditions selected from the group consisting of the above-mentioned condition (α), the above-mentioned condition (β), and the above-mentioned condition (γ), from the viewpoint of suppressing residues after development, improving mechanical properties when heated at low temperatures, and improving migration resistance. From the viewpoint of the effects of the present invention, it is more preferable that the photosensitive composition of the present invention satisfies the above-mentioned condition (α), and further satisfies the above-mentioned condition (β) and / or the above-mentioned condition (γ).
[0180] From the viewpoints of suppressing residue after development, improving mechanical properties when heated at low temperatures, and improving migration resistance, the photosensitive composition of the present invention preferably satisfies the above condition (α) and also satisfies the above condition (β).From the viewpoint of the effects of the present invention, the photosensitive composition of the present invention preferably satisfies the above condition (α) and also satisfies the above condition (γ).
[0181] From the viewpoints of suppressing residues after development, improving mechanical properties when heated at low temperatures, and improving migration resistance, it is preferred that the photosensitive composition of the present invention satisfy the above condition (γ) and also satisfy the above condition (α) and / or the above condition (β).
[0182] On the other hand, if the storage stability of the photosensitive composition is poor, for example, generation of foreign matter after storage at room temperature may become an issue. If foreign matter is generated during storage of the photosensitive composition, when a cured product of the photosensitive composition, such as the cured product in the electronic component of the present invention, is formed, the foreign matter will remain in the cured product or in the pattern opening. Such foreign matter can cause a decrease in the reliability of light-emitting elements in display devices and a decrease in migration resistance in electronic components. The photosensitive composition of the present invention exhibits a significant effect of improving storage stability by setting the content of the specific aromatic compound, the content of the specific anion, or the content of the specific organic acid within an appropriate range.
[0183] The total content of the specific aromatic compounds in the photosensitive composition is preferably 0.030 mass ppm or more, more preferably 0.050 mass ppm or more, even more preferably 0.070 mass ppm or more, and particularly preferably 0.10 mass ppm or more. On the other hand, the total content of the specific aromatic compounds is preferably 500 mass ppm or less, more preferably 300 mass ppm or less, and even more preferably 100 mass ppm or less. Furthermore, from the viewpoints of suppressing residue after development, improving mechanical properties in heating at low temperatures, and improving migration resistance, it is preferably 50 mass ppm or less, more preferably 30 mass ppm or less, even more preferably 10 mass ppm or less, even more preferably 5.0 mass ppm or less, particularly preferably 3.0 mass ppm or less, and most preferably 1.0 mass ppm or less.
[0184] The total content of the specific anions in the total solid content of the photosensitive composition is preferably 0.030 mass ppm or more, more preferably 0.050 mass ppm or more, even more preferably 0.070 mass ppm or more, and particularly preferably 0.10 mass ppm or more. On the other hand, the total content of the specific anions is preferably 500 mass ppm or less, more preferably 300 mass ppm or less, and even more preferably 100 mass ppm or less. Furthermore, from the viewpoints of suppressing residue after development, improving mechanical properties in heating at low temperatures, and improving migration resistance, it is preferably 50 mass ppm or less, more preferably 30 mass ppm or less, even more preferably 10 mass ppm or less, even more preferably 5.0 mass ppm or less, particularly preferably 3.0 mass ppm or less, and most preferably 1.0 mass ppm or less.
[0185] The total content of the specific organic acids in the total solid content of the photosensitive composition is preferably 0.030 mass ppm or more, more preferably 0.050 mass ppm or more, even more preferably 0.070 mass ppm or more, and particularly preferably 0.10 mass ppm or more. On the other hand, the total content of the specific organic acids is preferably 500 mass ppm or less, more preferably 300 mass ppm or less, and even more preferably 100 mass ppm or less. Furthermore, from the viewpoints of suppressing residue after development, improving mechanical properties in low-temperature heating, and improving migration resistance, it is preferably 50 mass ppm or less, more preferably 30 mass ppm or less, even more preferably 10 mass ppm or less, even more preferably 5.0 mass ppm or less, particularly preferably 3.0 mass ppm or less, and most preferably 1.0 mass ppm or less.
[0186] When the above condition (α) is satisfied, the photosensitive composition of the present invention preferably contains a sulfonic acid and / or a carboxylic acid containing a fluorine element, and more preferably contains a sulfonic acid. The total content of the sulfonic acid and / or the carboxylic acid containing a fluorine element in the total of the specific organic acids is preferably 50% by mass or more, more preferably 60% by mass or more. On the other hand, the total content of the sulfonic acid and / or the carboxylic acid containing a fluorine element is preferably 100% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less. It is more preferable that the content of the sulfonic acid is within the above-mentioned range.
[0187] When the above condition (β) is satisfied, the photosensitive composition of the present invention preferably contains one or more ions selected from the group consisting of phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions, and more preferably contains one or more ions selected from the group consisting of phosphate ions, phosphite ions, and hypophosphite ions. The total content of phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions in the total amount of specific anions is preferably 50% by mass or more, more preferably 60% by mass or more. On the other hand, the total content of phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions is preferably 100% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less. It is more preferable that the total content of phosphate ions, phosphite ions, and hypophosphite ions be within the above-mentioned range.
[0188] When the above condition (γ) is satisfied, the photosensitive composition of the present invention preferably contains one or more selected from the group consisting of benzene, toluene, and xylene, and more preferably contains benzene and / or toluene. The total content of benzene, toluene, and xylene in the total of the specific aromatic compounds is preferably 50% by mass or more, more preferably 60% by mass or more. On the other hand, the total content of benzene, toluene, and xylene is preferably 100% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less. Furthermore, it is more preferable that the total content of benzene and toluene is within the above-mentioned range.
[0189] When the photosensitive composition of the present invention has negative photosensitivity, it preferably satisfies the above-mentioned condition (γ) from the viewpoint of suppressing residues after development. Also, when the photosensitive composition of the present invention has negative photosensitivity and contains the above-mentioned (C1) photopolymerization initiator and (B) compound, it preferably satisfies the above-mentioned condition (γ) from the viewpoint of suppressing residues after development.
[0190] It is believed that the specific aromatic compound exhibits the effect of suppressing residues after development by stabilizing the compound through interaction with active radicals or active species in cationic polymerization or anionic polymerization through the π electrons on the aromatic ring. In particular, it is believed that the specific aromatic compound captures active radicals derived from the photopolymerization initiator (C1) and the compound (B), thereby significantly suppressing residues after development through control of radical polymerization during exposure.
[0191] From the viewpoints of suppressing residues after development, improving mechanical properties when heated at low temperatures, and improving migration resistance, it is preferable that the above condition (β) is the following condition (β2), and that the above condition (α) and / or the following condition (β2) are satisfied: (β2) The photosensitive composition of the present invention further contains one or more ions selected from the group consisting of phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions, and satisfies the following condition (2y): (2y) the total content of phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions in the total solid content of the photosensitive composition is 0.010 to 1,000 ppm by mass.
[0192] The preferred range of the total content of phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions in the total solid content of the photosensitive composition is the same as the content of each of the specific anions described above.
[0193] From the viewpoints of suppressing residues after development, improving mechanical properties when heated at low temperatures, and improving migration resistance, the photosensitive composition of the present invention is such that: the sulfonic acid, and the phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, and hypophosphite ester (hereinafter referred to as "organic acids containing phosphorus") have the following specific substituent a; the fluorine-containing carboxylic acid has the following specific substituent b; and it is preferable that the condition (α) is the following condition (α2), and that the following condition (α2) and / or the above condition (β) are satisfied, and it is more preferable that the following condition (α2) is satisfied: (α2) Further, the compound contains one or more selected from the group consisting of a sulfonic acid having the following specific substituent a, a phosphorus-containing organic acid having the following specific substituent a, and a fluorine-containing carboxylic acid having the following specific substituent b, and satisfies the condition (1y) below: specific substituent a: one or more selected from the group consisting of a mono- or divalent aliphatic group having 1 to 18 carbon atoms, a mono- or divalent alicyclic group having 4 to 18 carbon atoms, a mono- or divalent aromatic group having 6 to 15 carbon atoms, a mono- or divalent fluorine-containing aliphatic group having 1 to 18 carbon atoms, a mono- or divalent fluorine-containing alicyclic group having 4 to 18 carbon atoms, and a mono- or divalent fluorine-containing aromatic group having 6 to 15 carbon atoms; specific substituent b: one or more selected from the group consisting of a mono- or divalent fluorine-containing aliphatic group having 1 to 18 carbon atoms, a mono- or divalent fluorine-containing alicyclic group having 4 to 18 carbon atoms, and a mono- or divalent fluorine-containing aromatic group having 6 to 15 carbon atoms. (1y) The total content of the sulfonic acid having the specific substituent a, the phosphorus-containing organic acid having the specific substituent a, and the fluorine-containing carboxylic acid having the specific substituent b is 0.010 to 1,000 ppm by mass relative to the total solid content of the photosensitive composition.
[0194] The preferred range of the total content of the sulfonic acid having the specific substituent a, the phosphorus-containing organic acid having the specific substituent a, and the fluorine-containing carboxylic acid having the specific substituent b relative to the total solid content of the photosensitive composition is also the same as the content of each of the specific organic acids.
[0195] From the viewpoints of suppressing residues after development, improving mechanical properties when heated at low temperatures, and improving migration resistance, the photosensitive composition of the present invention preferably satisfies the following condition (α3) in place of the above condition (α2): the sulfonic acid preferably contains one or more selected from the group consisting of methanesulfonic acid, propanesulfonic acid, cyclohexanesulfonic acid, benzenesulfonic acid, toluenesulfonic acid, xylenesulfonic acid, trifluoromethanesulfonic acid, hexafluorocyclohexanesulfonic acid, hexafluorobenzenesulfonic acid, pentafluorotoluenesulfonic acid, tetrafluoroxylenesulfonic acid, trifluoromethylbenzenesulfonic acid, trifluoromethyltoluenesulfonic acid, and trifluoromethylxylenesulfonic acid; From the viewpoints of suppressing residues after development, improving mechanical properties when heated at low temperatures, and improving migration resistance, the fluorine-containing carboxylic acid preferably contains one or more selected from the group consisting of trifluoroacetic acid, trifluoropropionic acid, hexafluorocyclohexanecarboxylic acid, hexafluorobenzoic acid, and trifluoromethylbenzoic acid. (α3) The photosensitive composition further contains a sulfonic acid and / or a fluorine-containing carboxylic acid and satisfies the following condition (1z): (1z) the total content of the sulfonic acid and the fluorine-containing carboxylic acid relative to the total solid content of the photosensitive composition is 0.010 to 1,000 ppm by mass. The preferred ranges for the total content of the sulfonic acid and the fluorine-containing carboxylic acid relative to the total solid content of the photosensitive composition are also the same as those for the contents of the specific organic acids described above.
[0196] <Content of specific nitrogen-containing compounds> From the viewpoint of improving migration resistance, the photosensitive composition of the present invention preferably further contains one or more compounds selected from the group consisting of cyclic amide compounds represented by general formula (20), amide compounds represented by general formula (21), cyclic urea compounds represented by general formula (22), urea compounds represented by general formula (23), oxazolidone compounds represented by general formula (24), and isoxazolidone compounds represented by general formula (25), and satisfies the following condition (4): (4) The total content of the cyclic amide compounds represented by general formula (20), amide compounds represented by general formula (21), cyclic urea compounds represented by general formula (22), urea compounds represented by general formula (23), oxazolidone compounds represented by general formula (24), and isoxazolidone compounds represented by general formula (25) (hereinafter referred to as "specific nitrogen-containing compounds") in the total solid content of the photosensitive composition is 0.010 to 5.0 mass%.
[0197] When the (A) binder resin contains the (A1) resin and the (A1) resin contains one or more resins selected from the group consisting of the (A1-1) resin, the (A1-2) resin, the (A1-3) resin, the (A1-4) resin, the (A1-5) resin, the (A1-6) resin, and copolymers consisting of two or more of these resins, from the viewpoint of improving migration resistance, it is more preferable that the photosensitive composition of the present invention further contains one or more resins selected from the group consisting of specific nitrogen-containing compounds and satisfies the above condition (4).
[0198]
[0199] In the general formulas (20) to (25), R 46 ~R 56 R each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, a cycloalkyl group having 4 to 10 carbon atoms, an aryl group having 6 to 15 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, or a hydroxyalkyl group having 1 to 6 carbon atoms. 130represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a hydroxyalkyl group having 1 to 6 carbon atoms, a hydroxyalkoxy group having 1 to 6 carbon atoms, a hydroxy group, an amino group, a monoalkylamino group having 1 to 6 carbon atoms, or a dialkylamino group having 2 to 12 carbon atoms. 131 ~R 142 each independently represents an alkyl group having 1 to 6 carbon atoms. α, β, and γ each independently represent an integer of 0 to 6. a, b, c, e, f, g, h, i, j, k, l, and m each independently represent an integer of 0 to 2. When α is 0, a is 0. When β is 0, b is 0. When γ is 0, c is 0. The above-mentioned substituents and structures may have heteroatoms, and may be either unsubstituted or substituted.
[0200] Examples of specific nitrogen-containing compounds include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-butyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N-vinyl-2-pyrrolidone, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N,N-dimethylpropionamide, N,N-dimethylisobutyramide, N,N-dimethyl-3-methoxypropionamide, N,N-dimethyl-3-butoxypropionamide, 1,3-dimethyl-2-imidazolidinone, 1,3-diethyl-2-imidazolidinone, N,N'-dimethylpropyleneurea, 1,1,3,3-tetramethylurea, and 1,1,3,3-tetraethylurea.
[0201] The total content of the specific nitrogen-containing compounds relative to the total solid content of the photosensitive composition is preferably 0.030% by mass or more, more preferably 0.050% by mass or more, even more preferably 0.070% by mass or more, and particularly preferably 0.10% by mass or more. On the other hand, the total content of the specific nitrogen-containing compounds is preferably 4.0% by mass or less, more preferably 3.5% by mass or less, and even more preferably 3.0% by mass or less. Furthermore, from the viewpoint of improving migration resistance, it is preferably 2.5% by mass or less, more preferably 2.0% by mass or less, even more preferably 1.5% by mass or less, even more preferably 1.0% by mass or less, particularly preferably 0.70% by mass or less, and most preferably 0.50% by mass or less.
[0202] It is presumed that the specific nitrogen-containing compounds described above have a nitrogen-containing structure having an unshared electron pair that captures metallic impurities, ionic impurities, and the like that adversely affect electrical insulation, thereby suppressing ion migration and electromigration and improving migration resistance.
[0203] <Content of Specific Metal Elements> From the viewpoint of improving mechanical properties and migration resistance when heated at low temperatures, the photosensitive composition of the present invention preferably further contains one or more components selected from the group consisting of a component containing elemental sodium, a component containing elemental potassium, a component containing elemental magnesium, a component containing elemental calcium, a component containing elemental iron, a component containing elemental copper, and a component containing elemental chromium (hereinafter referred to as "components containing specific metal elements"), and satisfies the following condition (5): (5) The total content of elemental sodium, elemental potassium, elemental magnesium, elemental calcium, elemental iron, elemental copper, and elemental chromium (hereinafter referred to as "specific metal elements") in the total solid content of the photosensitive composition is 0.010 to 500 ppm by mass.
[0204] When the photosensitive composition of the present invention contains one or more compounds selected from the group consisting of specific nitrogen-containing compounds and satisfies the above condition (4), it is more preferable that the photosensitive composition of the present invention further contains one or more compounds selected from the group consisting of components containing specific metal elements and satisfies the above condition (5), from the viewpoint of improving mechanical properties and migration resistance when heated at low temperatures.
[0205] The component containing a specific metal element is preferably a halide, oxide, nitride, hydroxide, sulfide, carbide, oxynitride, carboxylate, phosphate, carbonate, sulfate, nitrate, or metasilicate of the specific metal element.
[0206] The total content of the specific metal elements in the total solid content of the photosensitive composition is preferably 0.030 mass ppm or more, more preferably 0.050 mass ppm or more, even more preferably 0.070 mass ppm or more, and particularly preferably 0.10 mass ppm or more. On the other hand, the total content of the specific metal elements is preferably 300 mass ppm or less, more preferably 200 mass ppm or less, and even more preferably 100 mass ppm or less. Furthermore, from the viewpoint of improving mechanical properties and migration resistance when heated at low temperatures, it is preferably 50 mass ppm or less, more preferably 30 mass ppm or less, even more preferably 10 mass ppm or less, even more preferably 5.0 mass ppm or less, particularly preferably 3.0 mass ppm or less, and most preferably 1.0 mass ppm or less.
[0207] It is believed that the specific metal element described above captures metallic impurities and ionic impurities that adversely affect electrical insulation due to the positive charge of the metal element, thereby suppressing ionic migration and electromigration and improving migration resistance. It is believed that a metal complex is formed by intentionally incorporating a trace amount of a specific metal element in the photosensitive composition of the present invention in the presence of a specific nitrogen-containing compound. The formed metal complex is believed to function as a catalyst that promotes crosslinking reactions on aromatic rings and ring-closing reactions of resins having aromatic rings, such as polyimides, polybenzoxazoles, and their precursors, and crosslinking reactions in resins having silanol groups, such as polysiloxanes. As a result, crosslinking reactions and ring-closing reactions proceed efficiently, which is believed to result in excellent mechanical properties even when heated at low temperatures. It is also believed that the formed metal complex efficiently captures metallic impurities and ionic impurities that adversely affect electrical insulation due to the positive charge of the metal element and the nitrogen-containing structure, thereby improving migration resistance.
[0208] <Content of specific carboxylic acid> From the viewpoint of improving migration resistance, the photosensitive composition of the present invention preferably further contains one or more selected from the group consisting of acetic acid, propionic acid, cyclopentanecarboxylic acid, cyclohexanecarboxylic acid, benzoic acid, methylbenzoic acid, and trimethylbenzoic acid and satisfies the following condition (6), and / or further contains an aldoxime compound and / or a ketoxime compound described below and satisfies the following condition (7): (6) The total content of acetic acid, propionic acid, cyclopentanecarboxylic acid, cyclohexanecarboxylic acid, benzoic acid, methylbenzoic acid, and trimethylbenzoic acid (hereinafter referred to as "specific carboxylic acid") in the total solid content of the photosensitive composition is 0.010 to 500 ppm by mass.
[0209] As described above, the photosensitive composition of the present invention preferably further contains one or more selected from the group consisting of specific carboxylic acids and satisfies the above condition (6). Furthermore, when the (C) photosensitizer contains the (C1-1) oxime ester compound and / or the (C1-2) phosphine oxide compound, from the viewpoint of improving migration resistance, the photosensitive composition of the present invention more preferably further contains one or more selected from the group consisting of specific carboxylic acids and satisfies the above condition (6).
[0210] The total content of the specific carboxylic acids in the total solid content of the photosensitive composition is preferably 0.030 mass ppm or more, more preferably 0.050 mass ppm or more, even more preferably 0.070 mass ppm or more, and particularly preferably 0.10 mass ppm or more. On the other hand, the total content of the specific carboxylic acids is preferably 300 mass ppm or less, more preferably 200 mass ppm or less, and even more preferably 100 mass ppm or less. Furthermore, from the viewpoint of improving migration resistance, it is preferably 50 mass ppm or less, more preferably 30 mass ppm or less, even more preferably 10 mass ppm or less, even more preferably 5.0 mass ppm or less, particularly preferably 3.0 mass ppm or less, and most preferably 1.0 mass ppm or less.
[0211] The specific carboxylic acid is thought to capture metal impurities, ionic impurities, and the like that adversely affect electrical insulation due to the acidity and negative charge of the carboxy group. Furthermore, it is presumed that the specific carboxylic acid captures moisture in the cured product, thereby suppressing ionic migration and electromigration and improving migration resistance. Furthermore, in the photosensitive composition of the present invention, by controlling the content of the specific carboxylic acid within a specific range in the presence of the (C1-1) oxime ester compound and / or the (C1-2) phosphine oxide compound, it is presumed that the polarization structure and charge balance in the cured product can be controlled. This is thought to efficiently capture metal impurities, ionic impurities, and the like that adversely affect electrical insulation, thereby improving migration resistance. This effect is particularly pronounced when the photosensitive composition of the present invention contains the (C1-1) oxime ester compound.
[0212] <Content of specific oxime compound> As described above, from the viewpoint of improving migration resistance, the photosensitive composition of the present invention preferably further contains an aldoxime compound and / or a ketoxime compound and satisfies the following condition (7): (7) The total content of the aldoxime compound and the ketoxime compound (hereinafter referred to as "specific oxime compound") in the total solid content of the photosensitive composition is 0.010 to 500 ppm by mass.
[0213] When the (C) photosensitizer contains the (C1-1) oxime ester compound and / or the (C1-2) phosphine oxide compound, from the viewpoint of improving migration resistance, the photosensitive composition of the present invention more preferably further contains an aldoxime compound and / or a ketoxime compound and satisfies the above condition (7).
[0214] The total content of the specific oxime compounds relative to the total solid content of the photosensitive composition is preferably 0.030 mass ppm or more, more preferably 0.050 mass ppm or more, even more preferably 0.070 mass ppm or more, and particularly preferably 0.10 mass ppm or more. On the other hand, the total content of the specific oxime compounds is preferably 300 mass ppm or less, more preferably 200 mass ppm or less, and even more preferably 100 mass ppm or less. Furthermore, from the viewpoint of improving migration resistance, it is preferably 50 mass ppm or less, more preferably 30 mass ppm or less, even more preferably 10 mass ppm or less, even more preferably 5.0 mass ppm or less, particularly preferably 3.0 mass ppm or less, and most preferably 1.0 mass ppm or less.
[0215] The specific oxime compound is believed to capture metal impurities, ionic impurities, and the like that adversely affect electrical insulation due to the acidity and negative charge of the oxime group. Furthermore, it is believed that the specific oxime compound captures moisture in the cured product, thereby suppressing ionic migration and electromigration and improving migration resistance. Furthermore, in the photosensitive composition of the present invention, by controlling the content of the specific oxime compound within a specific range in the presence of the (C1-1) oxime ester compound and / or the (C1-2) phosphine oxide compound, it is believed that the polarization structure and charge balance in the cured product can be controlled. This is believed to efficiently capture metal impurities, ionic impurities, and the like that adversely affect electrical insulation, thereby improving migration resistance. This effect is particularly pronounced when the photosensitive composition of the present invention contains the (C1-1) oxime ester compound.
[0216] <Contents of chlorine, bromine, and sulfur> From the viewpoint of improving migration resistance, the photosensitive composition of the present invention preferably further contains one or more components selected from the group consisting of a component containing chlorine, a component containing bromine, and a component containing sulfur, and satisfies the following conditions (8) and / or (9), and / or further contains water, which will be described later, and satisfies the following condition (10), which will be described later: (8) The total content of chlorine and bromine in the total solid content of the photosensitive composition is 0.010 to 500 ppm by mass; and (9) The content of sulfur in the total solid content of the photosensitive composition is 0.010 to 500 ppm by mass.
[0217] As described above, it is preferred that the photosensitive composition of the present invention further contains one or more compounds selected from the group consisting of a chlorine-containing component, a bromine-containing component, and a sulfur-containing component, and satisfies the above conditions (8) and / or (9). Furthermore, when the photosensitive composition of the present invention contains one or more compounds selected from the group consisting of specific carboxylic acids and satisfies the above condition (6), or when the photosensitive composition of the present invention contains one or more compounds selected from the group consisting of specific oxime compounds and satisfies the above condition (7), it is more preferred that the photosensitive composition of the present invention further contains one or more compounds selected from the group consisting of a chlorine-containing component, a bromine-containing component, and a sulfur-containing component, and satisfies the above conditions (8) and / or (9), from the viewpoint of improving migration resistance.
[0218] The chlorine-containing component and the bromine-containing component are preferably alkyl chloride compounds, cycloalkyl chloride compounds, aryl chloride compounds, alkyl bromide compounds, cycloalkyl bromide compounds, or aryl bromide compounds, and the sulfur-containing component is preferably a thiol compound, sulfide compound, disulfide compound, sulfoxide compound, sulfone compound, sultone compound, or thiophene compound.
[0219] The total content of chlorine and bromine elements in the total solid content of the photosensitive composition is preferably 0.030 mass ppm or more, more preferably 0.050 mass ppm or more, even more preferably 0.070 mass ppm or more, and particularly preferably 0.10 mass ppm or more. On the other hand, the total content of chlorine and bromine elements is preferably 300 mass ppm or less, more preferably 200 mass ppm or less, and even more preferably 100 mass ppm or less. Furthermore, from the viewpoint of improving migration resistance, it is preferably 50 mass ppm or less, more preferably 30 mass ppm or less, even more preferably 10 mass ppm or less, even more preferably 5.0 mass ppm or less, particularly preferably 3.0 mass ppm or less, and most preferably 1.0 mass ppm or less.
[0220] The content of sulfur element in the total solid content of the photosensitive composition is preferably 0.030 mass ppm or more, more preferably 0.050 mass ppm or more, even more preferably 0.070 mass ppm or more, and particularly preferably 0.10 mass ppm or more. On the other hand, the content of sulfur element is preferably 300 mass ppm or less, more preferably 200 mass ppm or less, and even more preferably 100 mass ppm or less. Furthermore, from the viewpoint of improving migration resistance, it is preferably 50 mass ppm or less, more preferably 30 mass ppm or less, even more preferably 10 mass ppm or less, even more preferably 5.0 mass ppm or less, particularly preferably 3.0 mass ppm or less, and most preferably 1.0 mass ppm or less.
[0221] The chlorine, bromine, and sulfur elements described above capture metallic impurities and ionic impurities that adversely affect electrical insulation through unshared electron pairs and vacant 3d orbitals, which are atomic orbitals. This is believed to suppress ionic migration and electromigration and improve migration resistance. Furthermore, in the photosensitive composition of the present invention, intentionally incorporating trace amounts of these elements in the presence of a trace amount of a specific carboxylic acid and / or a trace amount of a specific oxime compound is believed to control the polarization structure and charge balance in the cured product. Additionally, the inclusion of trace amounts of these elements improves the storage stability of the (C1-1) oxime ester compound and / or the (C1-2) phosphine oxide compound, making this composition suitable for controlling the content of the specific carboxylic acid and the content of the specific oxime compound. These effects are believed to efficiently capture metallic impurities and ionic impurities that adversely affect electrical insulation, thereby improving migration resistance.
[0222] As one example, when the total content of the specific organic acid in the total solid content of the photosensitive composition is 100 ppm by mass and the content of elemental sulfur in the total solid content of the photosensitive composition is 100 ppm by mass, the above conditions (1x) and (9) are satisfied. As another example, when the total content of the specific organic acid in the total solid content of the photosensitive composition is 600 ppm by mass and the content of elemental sulfur in the total solid content of the photosensitive composition is 600 ppm by mass, the above condition (1x) is satisfied. As another example, when the total content of the specific organic acid in the total solid content of the photosensitive composition is 100 ppm by mass and the content of elemental sulfur in the total solid content of the photosensitive composition is 50 ppm by mass, the above conditions (1x) and (9) are satisfied.
[0223] <Water Content> As described above, from the viewpoint of improving migration resistance, the photosensitive composition of the present invention preferably further contains water and satisfies the following condition (10): (10) The content of water in the photosensitive composition is 0.010 to 3.0% by mass.
[0224] When the photosensitive composition of the present invention contains one or more compounds selected from the group consisting of specific carboxylic acids and satisfies the above condition (6), or when the photosensitive composition of the present invention contains one or more compounds selected from the group consisting of specific oxime compounds and satisfies the above condition (7), it is more preferable that the photosensitive composition of the present invention further contains water and satisfies the above condition (10) from the viewpoint of improving migration resistance. (10) The content of water in the photosensitive composition is 0.010 to 3.0 mass %.
[0225] The water content in the photosensitive composition is preferably 0.030% by mass or more, more preferably 0.050% by mass or more, even more preferably 0.070% by mass or more, and particularly preferably 0.10% by mass or more. On the other hand, the water content is preferably 2.5% by mass or less, more preferably 2.2% by mass or less, and even more preferably 2.0% by mass or less. Furthermore, from the viewpoint of improving migration resistance, it is preferably 1.7% by mass or less, more preferably 1.5% by mass or less, even more preferably 1.2% by mass or less, even more preferably 1.0% by mass or less, particularly preferably 0.70% by mass or less, and most preferably 0.50% by mass or less.
[0226] It is believed that the water captures metal impurities and ionic impurities that adversely affect electrical insulation through interactions such as the dipole moment of water molecules and hydrogen bonds, thereby suppressing ion migration and electromigration and improving migration resistance. Furthermore, in the photosensitive composition of the present invention, by controlling the water content within a specific range in the presence of a trace amount of a specific carboxylic acid and / or a trace amount of a specific oxime compound, the polarization structure and charge balance in the cured product are controlled. Additionally, controlling the water content within a specific range improves the storage stability of the (C1-1) oxime ester compound and / or the (C1-2) phosphine oxide compound, making this suitable for controlling the content of the specific carboxylic acid and the content of the specific oxime compound. These effects are believed to efficiently capture metal impurities and ionic impurities that adversely affect electrical insulation, thereby improving migration resistance.
[0227] <Fluorine Element Content> From the viewpoint of suppressing residue after development and improving migration resistance, the photosensitive composition of the present invention preferably further satisfies the following condition (1α): (1α) The fluorine element content of the total solid content of the photosensitive composition is 1,000 ppm by mass or less.
[0228] From the viewpoint of the effects of the present invention, the content of elemental fluorine in the total solid content of the photosensitive composition is preferably 0 ppm by mass or more, more preferably 0.010 ppm by mass or more, even more preferably 0.030 ppm by mass or more, even more preferably 0.050 ppm by mass or more, particularly preferably 0.070 ppm by mass or more, and most preferably 0.10 ppm by mass or more. On the other hand, from the viewpoint of the effects of the present invention, the content of elemental fluorine is preferably 1,000 ppm by mass or less, more preferably 500 ppm by mass or less, even more preferably 300 ppm by mass or less, and particularly preferably 100 ppm by mass or less. Furthermore, the content of elemental fluorine is preferably 50 ppm by mass or less, more preferably 30 ppm by mass or less, even more preferably 10 ppm by mass or less, even more preferably 5 ppm by mass or less, particularly preferably 3 ppm by mass or less, and most preferably 1 ppm by mass or less.
[0229] When the photosensitive composition of the present invention satisfies the above condition (α) and the specific organic acid contains a fluorine atom in its structure, it is preferable that the photosensitive composition of the present invention further satisfies the above condition (1α) in view of the effects of the present invention. When the photosensitive composition of the present invention satisfies the above condition (β) and the specific anion-containing compound contains a fluoride ion, it is preferable that the photosensitive composition of the present invention further satisfies the above condition (1α) in view of the effects of the present invention.
[0230] The content of elemental fluorine in the total solid content of the photosensitive composition may be 0 ppm by mass. When the content of elemental fluorine in the total solid content of the photosensitive composition exceeds 0 ppm by mass, the photosensitive composition of the present invention preferably contains a component in which the (A) binder resin, the (C) photosensitizer, the (B) compound, or the (F) crosslinking agent has a fluorine atom in its structure, or further contains a component containing elemental fluorine.
[0231] The fluorine-containing component is preferably a phenol compound, a fluorinated alkyl compound, a fluorinated cycloalkyl compound, or a fluorinated aryl compound having a substituent containing a fluorinated alkyl group, which is different from the above-mentioned specific organic acid and the above-mentioned compound containing the specific anion.
[0232] By controlling the content of compounds containing fluorine atoms in their structures or components containing fluorine atoms in the photosensitive composition to a specific value or less, the content of fluorine atoms in these components or anions containing fluorine atoms derived from these components is controlled to a specific value or less. Therefore, it is believed that protons in the photosensitive composition are locally activated due to interactions such as hydrogen bonding between the components in the photosensitive composition. Therefore, it is believed that the effect of promoting dissolution in the developer and suppressing residue after development is significant. Furthermore, it is believed that intentionally controlling the content of the above components to a specific value or less controls the polarization structure and charge balance in the cured product. As a result, it is believed that ion migration and electromigration caused by metal impurities and ionic impurities that adversely affect electrical insulation are suppressed, thereby improving migration resistance.
[0233] <Photosensitive Composition Coating and Photosensitive Composition Film of the Present Invention> The photosensitive composition coating of the present invention is a semi-cured (B-stage) film formed from the photosensitive composition of the present invention. The semi-cured state refers to a film in which a crosslinked structure is not formed or a crosslinked structure is formed by partial reaction, but the film retains fluidity, or to this state. For example, after application to a substrate or the like, the coating film is dried under reduced pressure to remove the solvent, or the coating film is dried by heating at 40 to 150°C, and refers to a state in which the film is soluble in an alkaline solution or an organic solvent. The photosensitive composition film of the present invention preferably has a photosensitive composition coating formed from the photosensitive composition of the present invention and a support. This configuration is suitable from the viewpoint of handleability. The photosensitive composition film has positive or negative photosensitivity. It is also preferable that the photosensitive composition film be capable of forming a free-standing film with a single film. The photosensitive composition film preferably has adhesive properties, and it is also preferable that multiple components are bonded to each other. Being able to form a free-standing film as a single film means being able to form a film having a width of 1.5 cm or more, a length of 5.0 cm or more, and a thickness of 5.0 μm or more without a support. In other words, the photosensitive composition film is also preferably a photosensitive composition coating that can form a free-standing film as a single film.
[0234] The photosensitive composition film of the present invention has positive or negative photosensitivity, and therefore can form a positive or negative pattern by developing the film with an alkaline developer or an organic solvent after patterning exposure. The photosensitive composition film of the present invention is suitable for forming a pattern on a substrate having a textured structure, forming a hollow structure, or as a dry film resist.
[0235] The support is preferably a flexible substrate from the viewpoints of improving adhesion to the photosensitive film of the present invention, flexibility, and ease of handling. The flexible substrate is preferably a polyimide substrate, a polyphenylene sulfide substrate, a silicone substrate, an acrylic resin substrate, an epoxy resin substrate, a polyethylene terephthalate substrate, a polybutylene terephthalate substrate, a polyethylene naphthalate substrate, or a polycarbonate substrate. The support may also be a rigid substrate. Examples of rigid substrates include a glass substrate, a quartz substrate, a crystal substrate, and a sapphire substrate. The surface of the support facing the photosensitive film of the present invention may be surface-treated with a silane coupling agent or the like from the viewpoints of improving adhesion to the film and improving peelability. The thickness of the support is preferably 10 to 200 μm from the viewpoint of ease of handling.
[0236] <Cured Product of the Photosensitive Composition of the Present Invention> The cured product of the present invention is obtained by curing the photosensitive composition of the present invention. Curing refers to the formation of a crosslinked structure by a reaction and the loss of fluidity of the film, or the state in which this occurs. The reaction is not particularly limited, and may be caused by heating, irradiation with energy rays, or the like, but is preferably caused by heating. The state in which a crosslinked structure is formed by heating and the film loses its fluidity is called thermal curing.
[0237] Heating conditions include, for example, heating at 150 to 500°C for 5.0 to 300 minutes. Heating methods include, for example, heating using an oven, a hot plate, infrared radiation, a flash annealing device, or a laser annealing device. Treatment atmospheres include, for example, air, oxygen, nitrogen, helium, neon, argon, krypton, or xenon atmospheres, gas atmospheres containing 1.0 to less than 10,000 ppm by mass (0.00010 to 1.0% by mass) of oxygen, gas atmospheres containing 10,000 ppm by mass or more (1.0% by mass) of oxygen, and vacuum.
[0238] The cured product of the present invention may be a product obtained by curing the photosensitive film of the present invention. Curing refers to the formation of a crosslinked structure by a reaction, resulting in the loss of film fluidity, or the state in which this occurs. The reaction here is as described above. Examples and preferred heating conditions are as described above.
[0239] The optical density of the cured product of the present invention per 1 μm of film thickness at a visible light wavelength (380 to 780 nm) is preferably 0.20 or more, more preferably 0.30 or more, even more preferably 0.50 or more, and particularly preferably 1.0 or more, from the viewpoint of improving light-blocking properties and reliability. On the other hand, from the viewpoint of improving sensitivity during exposure and reliability, the optical density is preferably 3.0 or less, more preferably 2.0 or less, more preferably 1.7 or less, and even more preferably 1.5 or less. The optical density is preferably the optical density of a cured product obtained by heating and curing the composition. By having the optical density within the above range, incident external light can be blocked, thereby achieving a significant effect of suppressing external light reflection. Furthermore, photodegradation of the cured product itself and layers inside it is suppressed, resulting in a significant effect of improving reliability.
[0240] The dielectric dissipation factor of the cured product of the present invention at a frequency of 1 GHz is preferably 0.00010 or more, more preferably 0.00030 or more, and even more preferably 0.00050 or more, from the viewpoint of improving reliability. On the other hand, from the viewpoint of low transmission loss, the dielectric dissipation factor is preferably 0.0100 or less, more preferably 0.0050 or less, even more preferably 0.0030 or less, and particularly preferably 0.0010 or less. The preferred ranges for the dielectric dissipation factor of the cured product of the present invention at frequencies of 10 GHz, 30 GHz, and 70 GHz are also the same as those described above. The dielectric dissipation factor is a value measured by a resonator method using a split post dielectric resonator (SPDR).
[0241] The cured product of the present invention preferably has a dielectric constant of 3.5 or less at a frequency of 1 GHz and / or a water absorption rate of 1.5 mass % or less.
[0242] The dielectric constant is preferably 2.0 or more, more preferably 2.3 or more, and even more preferably 2.5 or more. On the other hand, the dielectric constant is preferably 3.5 or less, more preferably 3.0 or less, even more preferably 2.9 or less, and particularly preferably 2.7 or less. The preferred ranges for the dielectric constant of the cured product of the present invention at frequencies of 10 GHz, 30 GHz, and 70 GHz are also the same as those described above.
[0243] The water absorption is preferably 0.10% by mass or more, more preferably 0.30% by mass or more, while the water absorption is preferably 2.0% by mass or less, more preferably 1.5% by mass or less, even more preferably 1.0% by mass or less, even more preferably 0.70% by mass or less, and particularly preferably 0.50% by mass or less.
[0244] <Elements and Articles Comprising Cured Product> The element of the present invention comprises the cured product of the present invention. Furthermore, the article of the present invention comprises the cured product of the present invention. Examples of the article include electronic components, electronic devices, mobile objects, buildings, and windows. Examples of electronic components include semiconductor devices, antennas, displays, metal-clad laminates, wiring boards, semiconductor packages, active components including semiconductor devices, and passive components including semiconductor devices. Examples of semiconductor devices include transistors, diodes, integrated circuits, processors, and memories. Examples of passive components include resistors, capacitors, and inductors. Examples of electronic devices include industrial equipment, medical equipment, and construction equipment. Examples of mobile objects include vehicles, trains, airplanes, and heavy machinery. Examples of buildings include residences, stores, offices, buildings, and factories. Examples of windows include windows for electronic devices, mobile objects, and building structures.
[0245] The photosensitive composition of the present invention is preferably used to form electronic components, and is also preferably used to form one or more products selected from the group consisting of semiconductor devices, antennas, display devices, and metal-clad laminates.
[0246] Examples of semiconductor devices include semiconductor devices having a fan-out wafer-level package structure, a fan-out panel-level package structure, or an antenna-in-package structure. Examples of antennas include microstrip line antennas, strip line antennas, coplanar line antennas, grounded coplanar line (Conductor Back Coplanar; CBC) antennas, substrate integrated waveguide (SIW) antennas, post-wall waveguide (PWW) antennas, parallel two-wire line (Coplanar Strip; CPS) antennas, and slot line antennas. Examples of display devices include organic electroluminescence (EL) displays, quantum dot displays, micro light-emitting diode (LED) displays, mini-LED displays, and liquid crystal displays. Examples of metal-clad laminates include printed circuit boards.
[0247] The electronic component of the present invention includes the cured product of the present invention. The cured product of the present invention can have both excellent mechanical properties and high migration resistance even when heated at low temperatures. Therefore, the photosensitive composition of the present invention is preferably used to form an insulating layer for metal wiring, a protective layer for metal wiring, or an interlayer insulating layer for metal wiring in the electronic component.
[0248] The semiconductor device, antenna, display device, and metal-clad laminate of the present invention comprise the cured product of the present invention. For the same reasons as above, the photosensitive composition of the present invention is also preferably used to form an interlayer insulating layer for rewiring in a semiconductor device, an insulating layer for metal wiring in an antenna, a protective layer for metal wiring, or an interlayer insulating layer between metal wiring and ground wiring, and is also preferably used to form a pixel dividing layer, a TFT planarization layer, a TFT protective layer, an interlayer insulating layer for TFT, or a gate insulating layer in an organic EL display, a quantum dot display, or a micro LED display, and is also preferably used to form an insulating layer for metal wiring, a protective layer for metal wiring, or a solder resist layer for metal wiring in a metal-clad laminate.
[0249] An example of application of the cured product of the present invention to a semiconductor device having bumps will be described with reference to the drawings. Figure 1 is a schematic cross-sectional view showing an enlarged cross section of the pad portion of a semiconductor device having bumps. On a Si wafer 1, a passivation layer 3 is formed on an Al pad 2 for input / output, and via holes are formed in the passivation layer 3. A patterned insulating layer 4, which is the cured product of the present invention, is formed on the passivation layer 3. Furthermore, a metal layer 5, such as Cr or Ti, is formed to connect to the Al pad 2, and metal wiring 6, such as Al or Cu, is formed by electroplating or the like. The metal layer 5 is etched around the solder bumps 10 to insulate the pads. A barrier metal layer 8 and solder bumps 10 are formed on the insulated pads. The insulating layer 7 is a cured product of a patterned photosensitive composition, preferably the cured product of the present invention. The photosensitive composition forming the insulating layer 7 allows for thick-film patterning in the formation of scribe lines 9. When insulating layer 4 and / or insulating layer 7 is the cured product of the present invention, it has excellent mechanical properties when heated at low temperatures, thereby suppressing wafer warpage and significantly improving the accuracy of processes such as exposure and wafer transportation. Furthermore, it can also mitigate stress on the sealing resin during semiconductor packaging, thereby suppressing damage to the low-k layer and significantly improving the reliability of the semiconductor device.
[0250] <Hollow Structure> The hollow structure of the present invention comprises the cured product of the present invention. The electronic component of the present invention preferably comprises the hollow structure of the present invention. The hollow structure of the present invention comprises a hollow structure supporting material and a hollow structure roofing material. The hollow structure supporting material and hollow structure roofing material are preferably the cured product of the present invention. From the viewpoint of improving heat resistance and reliability, the hollow structure supporting material and hollow structure roofing material preferably contain the above-mentioned polyimide-based resin. The film thickness of the hollow structure supporting material is preferably 5 to 20 μm. The film thickness of the hollow structure roofing material is preferably 10 to 50 μm.
[0251] The photosensitive composition of the present invention is preferably used to form a hollow structure, more preferably to form a hollow structure support material and / or a hollow structure roofing material. The photosensitive film of the present invention is more suitable for forming a hollow structure, even more suitable for forming a hollow structure support material and / or a hollow structure roofing material, and particularly suitable for forming a hollow structure roofing material. Examples of electronic components having a hollow structure include MEMS (Micro Electro Mechanical Systems). Examples of MEMS include sensors, noise filters, SAW (Surface Acoustic Wave) filters, and BAW (Bulk Acoustic Wave) filters.
[0252] <Electronic Component> The electronic component of the present invention will be described below. However, the present invention is not limited to the following embodiments, and various modifications are possible as long as the object of the invention can be achieved and the gist of the invention is not deviated from.
[0253] The electronic component of the present invention has the configuration described above in
[20] . By adopting the above configuration, the present invention can provide an electronic component with excellent migration resistance. It is believed that intentionally incorporating a trace amount of the specific aromatic compound, specific anion, or specific organic acid into the cured product of the photosensitive composition controls the polarization structure and charge balance in the cured product of the photosensitive composition. It is also believed that aromatic rings in resins such as polyimide, polybenzoxazole, and their precursors, and silanol groups in resins such as polysiloxane, also contribute to controlling the polarization structure and charge balance. It is believed that this suppresses ion migration and electromigration caused by metal impurities and ionic impurities that adversely affect electrical insulation, thereby achieving excellent migration resistance. It is also believed that the suppression of metal migration and aggregation in wiring contributes to high reliability in electronic components, semiconductor devices, display devices, and metal-clad laminates.
[0254] <Resins and Compounds in the Cured Product> The electronic component of the present invention includes a cured product. The cured product in the electronic component of the present invention is preferably a cured product of a photosensitive composition, more preferably a cured product of a photosensitive composition containing a binder resin and a photosensitizer, and even more preferably a cured product of a photosensitive composition containing a binder resin and a photosensitizer and further containing a radically polymerizable compound and / or a crosslinking agent. The binder resin is preferably the binder resin (A) described above. The photosensitizer is preferably the photosensitizer (C) described above, more preferably the photopolymerization initiator (C1) described above. The radically polymerizable compound is preferably the compound (B) described above. The crosslinking agent is preferably the crosslinking agent (F) described above. Examples and preferred descriptions of the binder resin (A), the photosensitizer (C), the compound (B), and the crosslinking agent (F) are as described above.
[0255] The cured product in the electronic component of the present invention is also preferably a cured product of a photosensitive composition further containing one or more selected from the group consisting of a colorant, a dispersant, and inorganic particles. The colorant is preferably the above-mentioned (D) colorant. The dispersant is preferably the above-mentioned (E) dispersant. The inorganic particles are preferably the above-mentioned (G) inorganic particles. Examples and preferred descriptions of the (D) colorant, (E) dispersant, and (G) inorganic particles are as described above.
[0256] The cured product of the electronic component of the present invention contains the following (XA1) resin and / or (XA2) resin. Furthermore, it is preferable that the cured product of the electronic component of the present invention further contains the following (XA3) resin. (XA1) resin: a resin containing one or more structures selected from the group consisting of imide structures, amide structures, oxazole structures, and siloxane structures in the structural units of the resin main chain. (XA2) resin: a resin having a phenolic hydroxyl group in the structural units of the resin main chain. (XA3) resin: a resin having a radically polymerizable group.
[0257] The (XA1) resin in the cured product is preferably a resin having a structure derived from the above-mentioned (A1) resin. The (XA2) resin in the cured product is preferably a resin having a structure derived from the above-mentioned (A2) resin. The (XA3) resin in the cured product is preferably a resin having a structure derived from the above-mentioned (A3) resin. Examples and preferred descriptions of the (XA1) resin, (XA2) resin, and (XA3) resin in the cured product are the same as the examples and preferred descriptions of the (A1) resin, (A2) resin, and (A3) resin above.
[0258] From the viewpoint of improving migration resistance, the cured product in the electronic component of the present invention preferably contains an (A1) resin, more preferably contains an (A1) resin and an (A2) resin, and also preferably contains an (A3) resin. From the viewpoint of improving migration resistance, the cured product in the electronic component of the present invention further preferably contains an (A1) resin, an (A2) resin, and an (A3) resin.
[0259] It is presumed that the imide structure, amide structure, oxazole structure, or siloxane structure in the structural units of the main chain of the resin (A1) traps metal impurities, ionic impurities, and the like that adversely affect electrical insulation properties, thereby suppressing ion migration and electromigration and improving migration resistance.
[0260] The (XA1) resin preferably has one or more structural units selected from the group consisting of the above general formulae (1), (2), (3), (4), (5), (6), (9), and (10). The (XA2) resin preferably has one or more structural units selected from the group consisting of the above general formulae (31), (32), (33), (34), (35), (36), (38), (39), and (40). It is also preferable that a portion of the phenolic hydroxyl groups contained in these resins react with other resins or compounds to form crosslinked structures.
[0261] <Contents of specific aromatic compound, specific anion, and specific organic acid> The cured product of the electronic component of the present invention satisfies one or more selected from the group consisting of the following conditions (Xα), (Xβ), and (Xγ): The cured product of the electronic component of the present invention preferably satisfies the following condition (Xα). (Xα) further contains one or more ions selected from the group consisting of sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing fluorine element, and satisfies the condition (X1x) below. (X1x) The total content of sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing fluorine element in the cured product is 0.010 to 1,000 ppm by mass. (Xβ) further contains one or more ions selected from the group consisting of chloride ions, bromide ions, sulfate ions, sulfite ions, nitrate ions, nitrite ions, phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions, and satisfies the condition (X2x) below. (X2x) The total content of chloride ions, bromide ions, sulfate ions, sulfite ions, nitrate ions, nitrite ions, phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions in the cured product is 0.010 to 1,000 ppm by mass. (Xγ) The cured product further contains one or more members selected from the group consisting of benzene, toluene, xylene, and naphthalene, and satisfies the following condition (X3): (X3) The total content of benzene, toluene, xylene, and naphthalene in the cured product is 0.010 to 1,000 ppm by mass.
[0262] When the above condition (Xβ) is satisfied, the cured product of the electronic component of the present invention preferably further contains a compound containing a specific anion. When the cured product of the electronic component of the present invention contains a compound containing a specific anion, it preferably further contains an ammonium ion, a primary ammonium ion, a secondary ammonium ion, a tertiary ammonium ion, or a quaternary ammonium ion as a cationic species.
[0263] The above phosphoric acid ester, phosphonic acid ester, phosphonic acid ester, phosphorous acid ester, phosphinic acid, and hypophosphite ester are preferably phosphoric acid monoester, phosphoric acid diester, phosphonic acid, phosphonic acid monoester, phosphorous acid monoester, phosphorous acid diester, phosphinic acid, or hypophosphite monoester.
[0264] The specific organic acid preferably has one or more selected from the group consisting of mono- to di-valent aliphatic groups having 1 to 18 carbon atoms, mono- to di-valent alicyclic groups having 4 to 18 carbon atoms, mono- to di-valent aromatic groups having 6 to 15 carbon atoms, mono- to di-valent fluorine-containing aliphatic groups having 1 to 18 carbon atoms, mono- to di-valent fluorine-containing alicyclic groups having 4 to 18 carbon atoms, and mono- to di-valent fluorine-containing aromatic groups having 6 to 15 carbon atoms.
[0265] From the viewpoint of improving migration resistance, the cured product of the electronic component of the present invention preferably satisfies two or more selected from the group consisting of the above condition (Xα), the above condition (Xβ), and the above condition (Xγ). From the viewpoint of improving migration resistance, the cured product of the electronic component of the present invention more preferably satisfies the above condition (Xα) and further satisfies the above condition (β) and / or the above condition (γ). Furthermore, from the viewpoint of improving migration resistance, the cured product of the electronic component of the present invention preferably satisfies the above condition (Xγ) and also satisfies the above condition (Xα) and / or the above condition (Xβ).
[0266] The total content of the specific aromatic compounds in the cured product is preferably 0.030 mass ppm or more, more preferably 0.050 mass ppm or more, even more preferably 0.070 mass ppm or more, and particularly preferably 0.10 mass ppm or more. On the other hand, the total content of the specific aromatic compounds is preferably 500 mass ppm or less, more preferably 300 mass ppm or less, and even more preferably 100 mass ppm or less. Furthermore, from the viewpoint of improving migration resistance, it is preferably 50 mass ppm or less, more preferably 30 mass ppm or less, even more preferably 10 mass ppm or less, even more preferably 5.0 mass ppm or less, particularly preferably 3.0 mass ppm or less, and most preferably 1.0 mass ppm or less.
[0267] The total content of specific anions in the cured product is preferably 0.030 mass ppm or more, more preferably 0.050 mass ppm or more, even more preferably 0.070 mass ppm or more, and particularly preferably 0.10 mass ppm or more. On the other hand, the total content of specific anions is preferably 500 mass ppm or less, more preferably 300 mass ppm or less, and even more preferably 100 mass ppm or less. Furthermore, from the viewpoint of improving migration resistance, it is preferably 50 mass ppm or less, more preferably 30 mass ppm or less, even more preferably 10 mass ppm or less, even more preferably 5.0 mass ppm or less, particularly preferably 3.0 mass ppm or less, and most preferably 1.0 mass ppm or less.
[0268] The total content of the specific organic acids in the cured product is preferably 0.030 mass ppm or more, more preferably 0.050 mass ppm or more, even more preferably 0.070 mass ppm or more, and particularly preferably 0.10 mass ppm or more. On the other hand, the total content of the specific organic acids is preferably 500 mass ppm or less, more preferably 300 mass ppm or less, and even more preferably 100 mass ppm or less. Furthermore, from the viewpoint of improving migration resistance, it is preferably 50 mass ppm or less, more preferably 30 mass ppm or less, even more preferably 10 mass ppm or less, even more preferably 5.0 mass ppm or less, particularly preferably 3.0 mass ppm or less, and most preferably 1.0 mass ppm or less.
[0269] When the above condition (Xα) is satisfied, the cured product in the electronic component of the present invention preferably contains sulfonic acid and / or a carboxylic acid containing a fluorine element, more preferably sulfonic acid. The total content ratio of sulfonic acid and / or a carboxylic acid containing a fluorine element in the total of the specific organic acids is preferably 50 mass% or more, more preferably 60 mass% or more. On the other hand, the total content ratio of sulfonic acid and / or a carboxylic acid containing a fluorine element is preferably 100 mass% or less, more preferably 90 mass% or less, and even more preferably 80 mass% or less. It is also more preferable that the content ratio of sulfonic acid is the above-mentioned content ratio.
[0270] When the above condition (Xβ) is satisfied, the cured product in the electronic component of the present invention preferably contains one or more ions selected from the group consisting of phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions, and more preferably contains one or more ions selected from the group consisting of phosphate ions, phosphite ions, and hypophosphite ions. The total content of phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions in the total of the specific anions is preferably 50% by mass or more, more preferably 60% by mass or more. On the other hand, the total content of phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions is preferably 100% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less. It is more preferable that the total content of phosphate ions, phosphite ions, and hypophosphite ions be within the above-mentioned range.
[0271] When the above condition (Xγ) is satisfied, the cured product in the electronic component of the present invention preferably contains one or more selected from the group consisting of benzene, toluene, and xylene, and more preferably contains benzene and / or toluene. The total content of benzene, toluene, and xylene in the total of the specific aromatic compounds is preferably 50% by mass or more, more preferably 60% by mass or more. On the other hand, the total content of benzene, toluene, and xylene is preferably 100% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less. It is also more preferable that the total content of benzene and toluene is the above-mentioned content ratio.
[0272] From the viewpoint of improving migration resistance, the cured product in the electronic component of the present invention preferably satisfies the following condition (Xβ2) instead of the above condition (Xβ), and also satisfies the above condition (Xα) and / or the following condition (Xβ2): (Xβ2) The cured product further contains one or more ions selected from the group consisting of phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions, and also satisfies the following condition (X2y): (X2y) The total content of phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions in the cured product is 0.010 to 1,000 ppm by mass.
[0273] The preferred range of the total content of phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions in the cured product is the same as the preferred range of the content of each of the specific anions described above.
[0274] From the viewpoint of improving the migration resistance of the cured product in the electronic component of the present invention, it is preferable that the sulfonic acid, and the phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, and hypophosphite ester (hereinafter referred to as "organic acid containing phosphorus") have the following specific substituent a, the fluorine-containing carboxylic acid have the following specific substituent b, and the condition (Xα) is the following condition (Xα2), and the following condition (Xα2) and / or the above condition (Xβ) are satisfied, and it is more preferable that the following condition (Xα2) is satisfied. (Xα2) Further, the compound contains one or more selected from the group consisting of a sulfonic acid having the following specific substituent a, a phosphorus-containing organic acid having the following specific substituent a, and a fluorine-containing carboxylic acid having the following specific substituent b, and satisfies the condition (X1y) below: Specific substituent a: one or more selected from the group consisting of a mono- or divalent aliphatic group having 1 to 18 carbon atoms, a mono- or divalent alicyclic group having 4 to 18 carbon atoms, a mono- or divalent aromatic group having 6 to 15 carbon atoms, a mono- or divalent fluorine-containing aliphatic group having 1 to 18 carbon atoms, a mono- or divalent fluorine-containing alicyclic group having 4 to 18 carbon atoms, and a mono- or divalent fluorine-containing aromatic group having 6 to 15 carbon atoms; Specific substituent b: one or more selected from the group consisting of a mono- or divalent fluorine-containing aliphatic group having 1 to 18 carbon atoms, a mono- or divalent fluorine-containing alicyclic group having 4 to 18 carbon atoms, and a mono- or divalent fluorine-containing aromatic group having 6 to 15 carbon atoms. (X1y) The total content of the sulfonic acid having the specific substituent a, the phosphorus-containing organic acid having the specific substituent a, and the fluorine-containing carboxylic acid having the specific substituent b in the cured product is 0.010 to 1,000 ppm by mass.
[0275] The preferred range of the total content of the sulfonic acid having the specific substituent a, the phosphorus-containing organic acid having the specific substituent a, and the fluorine-containing carboxylic acid having the specific substituent b in the cured product is also the same as the content of each of the specific organic acids.
[0276] From the viewpoint of improving migration resistance, the cured product in the electronic component of the present invention preferably satisfies the following condition (Xα2) instead of the above condition (Xα3): The sulfonic acid preferably contains one or more selected from the group consisting of methanesulfonic acid, cyclohexanesulfonic acid, benzenesulfonic acid, toluenesulfonic acid, xylenesulfonic acid, trifluoromethanesulfonic acid, hexafluorocyclohexanesulfonic acid, hexafluorobenzenesulfonic acid, pentafluorotoluenesulfonic acid, tetrafluoroxylenesulfonic acid, trifluoromethylbenzenesulfonic acid, trifluoromethyltoluenesulfonic acid, and trifluoromethylxylenesulfonic acid The fluorine-containing carboxylic acid preferably contains one or more selected from the group consisting of trifluoroacetic acid, trifluoropropionic acid, hexafluorocyclohexanecarboxylic acid, hexafluorobenzoic acid, and trifluoromethylbenzoic acid, from the viewpoint of improving migration resistance. (Xα3) Further, it contains a sulfonic acid and / or a carboxylic acid containing a fluorine element, and satisfies the following condition (X1z): (X1z) The total content of the sulfonic acid and the carboxylic acid containing a fluorine element in the compound is 0.010 to 1,000 ppm by mass. The preferred range of the total content of the sulfonic acid and the carboxylic acid containing a fluorine element in the cured product is also the same as the content of the above-mentioned specific organic acid.
[0277] <Content of specific nitrogen-containing compound> When the cured product of the electronic device of the present invention contains the above (XA1) resin, from the viewpoint of improving migration resistance, the cured product of the electronic device of the present invention preferably further contains one or more compounds selected from the group consisting of the cyclic amide compound represented by the above general formula (20), the amide compound represented by the above general formula (21), the cyclic urea compound represented by the above general formula (22), the urea compound represented by the above general formula (23), the oxazolidone compound represented by the general formula (24), and the isoxazolidone compound represented by the general formula (25), and satisfies the following condition (X4). Examples and preferred descriptions of the specific nitrogen-containing compound are as described above. (X4) The total content of the cyclic amide compound represented by general formula (20), the amide compound represented by general formula (21), the cyclic urea compound represented by general formula (22), the urea compound represented by general formula (23), the oxazolidone compound represented by general formula (24), and the isoxazolidone compound represented by general formula (25) (hereinafter referred to as "specific nitrogen-containing compounds") in the cured product is 0.010 to 5.0 mass%.
[0278] The total content of the specific nitrogen-containing compounds in the cured product is preferably 0.030% by mass or more, more preferably 0.050% by mass or more, even more preferably 0.070% by mass or more, and particularly preferably 0.10% by mass or more. On the other hand, the total content of the specific nitrogen-containing compounds is preferably 4.0% by mass or less, more preferably 3.5% by mass or less, and even more preferably 3.0% by mass or less. Furthermore, from the viewpoint of improving migration resistance, it is preferably 2.5% by mass or less, more preferably 2.0% by mass or less, even more preferably 1.5% by mass or less, even more preferably 1.0% by mass or less, particularly preferably 0.70% by mass or less, and most preferably 0.50% by mass or less.
[0279] It is presumed that the specific nitrogen-containing compounds described above have a nitrogen-containing structure having an unshared electron pair that captures metallic impurities, ionic impurities, and the like that adversely affect electrical insulation, thereby suppressing ion migration and electromigration and improving migration resistance.
[0280] <Content of specific metal elements> When the cured product of the electronic device of the present invention contains one or more compounds selected from the group consisting of specific nitrogen-containing compounds and satisfies the above condition (X4), from the viewpoint of improving mechanical properties and migration resistance when heated at low temperatures, the photosensitive composition of the present invention preferably further contains one or more compounds selected from the group consisting of a component containing elemental sodium, a component containing elemental potassium, a component containing elemental magnesium, a component containing elemental calcium, a component containing elemental iron, a component containing elemental copper, and a component containing elemental chromium, and satisfies the following condition (X5): (X5) the total content of elemental sodium, elemental potassium, elemental magnesium, elemental calcium, elemental iron, elemental copper, and elemental chromium (hereinafter referred to as "specific metal elements") in the cured product is 0.010 to 500 ppm by mass.
[0281] The component containing a specific metal element is preferably a halide, oxide, nitride, hydroxide, sulfide, carbide, oxynitride, carboxylate, phosphate, carbonate, sulfate, nitrate, or metasilicate of the specific metal element.
[0282] The total content of the specific metal elements in the cured product is preferably 0.030 mass ppm or more, more preferably 0.050 mass ppm or more, even more preferably 0.070 mass ppm or more, and particularly preferably 0.10 mass ppm or more. On the other hand, the total content of the specific metal elements is preferably 300 mass ppm or less, more preferably 200 mass ppm or less, and even more preferably 100 mass ppm or less. Furthermore, from the viewpoint of improving migration resistance, it is preferably 50 mass ppm or less, more preferably 30 mass ppm or less, even more preferably 10 mass ppm or less, even more preferably 5.0 mass ppm or less, particularly preferably 3.0 mass ppm or less, and most preferably 1.0 mass ppm or less.
[0283] It is presumed that the specific metal element described above captures metallic impurities and ionic impurities that adversely affect electrical insulation due to the positive charge of the metal element, thereby suppressing ionic migration and electromigration and improving migration resistance. It is presumed that a metal complex is formed by intentionally incorporating a trace amount of a specific metal element in the cured product of the electronic component of the present invention in the presence of a specific nitrogen-containing compound. The formed metal complex efficiently captures metallic impurities and ionic impurities that adversely affect electrical insulation due to the positive charge of the metal element and the nitrogen-containing structure, thereby improving migration resistance.
[0284] <Contents of Elemental Chlorine, Elemental Bromine, and Elemental Sulfur> From the viewpoint of improving migration resistance, the cured product of the electronic component of the present invention preferably further contains one or more components selected from the group consisting of a component containing elemental chlorine, a component containing elemental bromine, and a component containing elemental sulfur, and satisfies the following conditions (X8) and / or (X9): (X8) The total content of elemental chlorine and elemental bromine in the cured product is 0.010 to 500 ppm by mass. (X9) The content of elemental sulfur in the cured product is 0.010 to 500 ppm by mass.
[0285] The chlorine-containing component and the bromine-containing component are preferably alkyl chloride compounds, cycloalkyl chloride compounds, aryl chloride compounds, alkyl bromide compounds, cycloalkyl bromide compounds, or aryl bromide compounds, and the sulfur-containing component is preferably a thiol compound, sulfide compound, disulfide compound, sulfoxide compound, sulfone compound, sultone compound, or thiophene compound.
[0286] The total content of chlorine and bromine elements in the cured product is preferably 0.030 mass ppm or more, more preferably 0.050 mass ppm or more, even more preferably 0.070 mass ppm or more, and particularly preferably 0.10 mass ppm or more. On the other hand, the total content of chlorine and bromine elements is preferably 300 mass ppm or less, more preferably 200 mass ppm or less, and even more preferably 100 mass ppm or less. Furthermore, from the viewpoint of improving migration resistance, it is preferably 50 mass ppm or less, more preferably 30 mass ppm or less, even more preferably 10 mass ppm or less, even more preferably 5.0 mass ppm or less, particularly preferably 3.0 mass ppm or less, and most preferably 1.0 mass ppm or less.
[0287] The content of sulfur element in the cured product is preferably 0.030 mass ppm or more, more preferably 0.050 mass ppm or more, even more preferably 0.070 mass ppm or more, and particularly preferably 0.10 mass ppm or more. On the other hand, the content of sulfur element is preferably 300 mass ppm or less, more preferably 200 mass ppm or less, and even more preferably 100 mass ppm or less. Furthermore, from the viewpoint of improving migration resistance, it is preferably 50 mass ppm or less, more preferably 30 mass ppm or less, even more preferably 10 mass ppm or less, even more preferably 5.0 mass ppm or less, particularly preferably 3.0 mass ppm or less, and most preferably 1.0 mass ppm or less.
[0288] The above-mentioned chlorine, bromine, and sulfur elements capture metal impurities and ionic impurities that adversely affect electrical insulation properties by using unshared electron pairs or 3d orbitals, which are empty atomic orbitals, and it is presumed that this suppresses ion migration and electromigration and improves migration resistance.
[0289] <Fluorine Element Content> From the viewpoint of improving migration resistance, the cured product of the electronic component of the present invention preferably satisfies the following condition (X1α): (X1α) The fluorine element content in the cured product is 1,000 ppm by mass or less.
[0290] From the viewpoint of the effects of the present invention, the content of fluorine element in the cured product is preferably 0 mass ppm or more, more preferably 0.010 mass ppm or more, even more preferably 0.030 mass ppm or more, even more preferably 0.050 mass ppm or more, particularly preferably 0.070 mass ppm or more, and most preferably 0.10 mass ppm or more. On the other hand, from the viewpoint of the effects of the present invention, the content of fluorine element is preferably 1,000 mass ppm or less, more preferably 500 mass ppm or less, even more preferably 300 mass ppm or less, and particularly preferably 100 mass ppm or less. Furthermore, the content of fluorine element is preferably 50 mass ppm or less, more preferably 30 mass ppm or less, even more preferably 10 mass ppm or less, even more preferably 5 mass ppm or less, particularly preferably 3 mass ppm or less, and most preferably 1 mass ppm or less.
[0291] In addition, when the cured product of the electronic component of the present invention satisfies the above condition (Xα) and the specific organic acid contains a fluorine atom in its structure, it is preferable that the above condition (X1α) be satisfied in order to achieve the effects of the present invention. In addition, when the cured product of the electronic component of the present invention satisfies the above condition (Xβ) and the specific anion-containing compound contains a fluoride ion, it is preferable that the above condition (X1α) be satisfied in order to achieve the effects of the present invention.
[0292] The content of elemental fluorine in the cured product may be 0 ppm by mass. When the content of elemental fluorine in the cured product exceeds 0 ppm by mass, the cured product in the electronic component of the present invention preferably contains a binder resin having a fluorine atom in the structure thereof or further contains a component containing elemental fluorine.
[0293] The fluorine-containing component is preferably a phenol compound, a fluorinated alkyl compound, a fluorinated cycloalkyl compound, or a fluorinated aryl compound having a substituent containing a fluorinated alkyl group, which is different from the above-mentioned specific organic acid and the above-mentioned compound containing the specific anion.
[0294] It is believed that intentionally setting the fluorine content in the cured product below a specific value controls the polarization structure and charge balance in the cured product, thereby suppressing ion migration and electromigration caused by metal impurities and ionic impurities that adversely affect electrical insulation, thereby improving migration resistance.
[0295] <Method for producing a cured product> The method for producing a cured product of the present invention includes the following steps (1) to (4): (1) a step of forming a coating film of the photosensitive composition of the present invention on a substrate; (2) a step of irradiating the coating film of the photosensitive composition with actinic rays through a photomask; (3) a step of developing using a developer to form a pattern of the photosensitive composition; and (4) a step of heating the pattern to obtain a cured pattern of the photosensitive composition. In these steps, the methods described in paragraphs
[0453] to
[0481] of WO 2019 / 087985 may also be applied. In the step of forming a coating film, it is preferable to apply coating and then pre-bake to form a film. In the step of obtaining a cured pattern, it is preferable to heat the pattern to thermally cure it.
[0296] The present invention will be described in more detail below with reference to Examples, Reference Examples, and Comparative Examples, but the present invention is not limited to these examples. For compounds used in the following explanations or tables that use abbreviations, the names corresponding to the abbreviations are listed in Table 1-1.
[0297]
[0298] <Synthesis Examples of Each Resin> The compositions of the resins obtained in Synthesis Examples 1 to 25 as the (A) binder resin are summarized in Tables 1-2 to 1-4. Each resin was synthesized by a known method based on a method described in a known literature, with the monomer compounds to be used as monomers and the copolymerization ratios appropriately changed. The copolymerization ratios of the monomers are as shown in Tables 1-2 to 1-4.
[0299] The hydroxyl group-containing diamine (HA) having the following structure used in Synthesis Example 8 was synthesized by a known method based on the synthesis method described in Synthesis Example 1 in paragraphs
[0374] to
[0376] of WO 2016 / 056451. The resin obtained in Synthesis Example 5 using the hydroxyl group-containing diamine (HA) having the following structure is a polyimide precursor having an amic acid ester structural unit, an amic acid structural unit, and an imide ring-closed structure.
[0300]
[0301] In Synthesis Example 19, based on the synthesis methods described in Synthesis Examples 3 and 5 in paragraphs
[0109] to
[0122] of WO 2012 / 141165, a phenol compound having the following structure was synthesized as a condensation product of XLN and SAD instead of the condensation product of XLN and 4-hydroxybenzaldehyde, and the obtained phenol compound was used in a condensation reaction with an aldehyde compound.
[0302]
[0303] In Synthesis Examples 8 and 11, the amic acid structural units in the resin were reacted with the esterifying agent DFA, resulting in structural conversion to amic acid ester structural units having methyl groups. In Synthesis Examples 9 and 10, the tetracarboxylic dianhydride ODPA was reacted with HEMA or GDMA to effect ring-opening addition of all of the acid anhydride groups in the ODPA, and then the carboxy groups derived from the ODPA were reacted with the bisaminophenol compound BAHF and the end-capping agent EtOH. In Synthesis Example 18, the carboxy groups derived from the MAA in the resin were reacted with GMA having an epoxy group, resulting in ring-opening addition of all of the epoxy groups in the GMA. In Synthesis Example 24, the epoxy groups derived from the GMA in the resin were reacted with DHBA having a carboxy group, resulting in ring-opening addition of all of the epoxy groups in the GMA. In Synthesis Example 25, the phenolic hydroxyl groups derived from the HPMA in the resin were reacted with GMA having an epoxy group, resulting in ring-opening addition of all of the epoxy groups in the GMA.
[0304]
[0305]
[0306]
[0307] The structural units and structures of the resins obtained in each synthesis example and the resins used in each example, reference example, and comparative example are collectively shown in Table 2-1.
[0308]
[0309] Table 2-2 shows a list and description of the (D) colorant and (E) dispersant used in each example, reference example, and comparative example. Note that (A.R.52-B.B.7) is a dye obtained by mixing and stirring A.R.52 / B.B.7 at a molar ratio of 1 / 1, filtering the precipitated salt, washing it three times with water, and then drying it.
[0310]
[0311] <Each Colorant> Bk-CBF1 is a benzofuranone-based black pigment having a coating layer described in paragraphs
[0503] to
[0505] and Coating Example 1 of WO 2019 / 087985. Bk-CPR1 is a perylene-based black pigment having a coating layer obtained by the synthesis method described in paragraphs
[0186] to
[0188] and
[0191] and Example 18 of WO 2018 / 038083.
[0312] <Preparation Examples of Each Pigment Dispersion> The compositions of the pigment dispersions obtained in Preparation Examples Bk-1 to Bk-6 are summarized in Table 2-3. In Preparation Examples Bk-1 to Bk-6, each pigment dispersion was prepared by the following method.
[0313] Preparation Examples Bk-1 to Bk-6 Preparation of Pigment Dispersions (Bk-1) to (Bk-6) 35.0 g of ADP, a polyalkyleneamine-polyoxyalkylene ether-based dispersant (pigment dispersant 1 described in paragraphs
[0138] to
[0141] of JP 2020-070352 A, Synthesis Example 2) was weighed out as a dispersant, and 765.0 g of PGMEA was weighed out as a solvent and mixed. The mixture was stirred for 10 minutes to disperse the pigment. After that, 100.0 g of the black pigment described in Table 2-3 was weighed out as a colorant and mixed with the mixture and stirred for 30 minutes to obtain a pre-stirred liquid. A composite oxide of zirconium and hafnium (ZrO 2 -HfO 2 The grinding media is made of a composite oxide (zirconia (ZrO 2 ) / hafnium oxide (HfO 2 ) / yttrium oxide (Y 2 O 3 ) / aluminum oxide (Al 2 O 3 The pre-stirred solution was sent to a vertical bead mill in which a vessel was filled with a mixture of zirconia (ZrO ) = 93.3 / 1.5 / 4.9 / 0.3 (mass ratio), and a first wet media dispersion treatment was carried out using a circulation system at a peripheral speed of 8 m / s for 3 hours. 2 ) / hafnium oxide (HfO 2 ) / yttrium oxide (Y 2 O 3 ) / aluminum oxide (Al 2 O 3 The resulting dispersion was transferred to a vertical bead mill containing a vessel filled with a mixture of 1.5% by weight of 1.5% by weight of 1.5% by weight of 4.9% by weight of dispersant and 1.5% by weight of dispersant (mass ratio: 93.3 / 1.5 / 4.9 / 0.3), and subjected to a second wet media dispersion treatment at a peripheral speed of 9 m / s using a circulation system so that the average primary particle diameter of the pigment would be the value shown in Table 2-3. The resulting dispersion was then filtered through a 0.80 μmφ filter to obtain pigment dispersions (Bk-1) to (Bk-6) with a solids concentration of 15% by weight and a colorant / dispersant ratio of 100 / 35. The average primary particle diameters of the pigments in the resulting pigment dispersions are shown in Table 2-3.
[0314]
[0315] <Synthesis Example of Silica Particle Dispersion> Table 2-4 shows a list and description of the silica particles, which are inorganic particles, used in each of the Examples, Reference Examples, and Comparative Examples.
[0316] Synthesis Example 26 Synthesis of Silica Particle (SP-1) Dispersion To a three-neck flask, 104.5 g of MEK as a solvent, 142.5 g of MEK-ST-40 as a silica particle dispersion containing elemental sodium, and 0.01 g of MOP as a polymerization inhibitor were weighed, added, and mixed. After stirring for 10 minutes, the liquid temperature was raised to 50°C. Next, as a surface modifier, a solution prepared by dissolving 3.0 g of KBM-503 in 50.0 g of MEK was added dropwise over 10 minutes. After completion of the dropwise addition, the surface modifier was subjected to dehydration condensation by stirring at 50°C for 2 hours. After the reaction, the reaction solution was cooled to room temperature to obtain a dispersion of silica particles (SP-1). The obtained silica particles (SP-1) have a surface modifying group containing a methacryloyl group as a radically polymerizable group.
[0317] For the dispersion of silica particles (SP-2), (MSiP-1) was prepared by synthesizing silica particles having surface-modifying groups containing methylsilyl groups using MEK-ST-40 as a silica particle dispersion containing sodium element, KBM-13 as a surface modifier, and no MOP as a polymerization inhibitor, in the same manner as in Synthesis Example 20. For the dispersion of silica particles (SP-3), (MSiP-2) was prepared by synthesizing silica particles having surface-modifying groups containing methylsilyl groups using MEK-ST-L as a silica particle dispersion containing sodium element, KBM-13 as a surface modifier, and no MOP as a polymerization inhibitor, in the same manner as in Synthesis Example 20.
[0318]
[0319] <Evaluation Methods in Each Example, Reference Example, and Comparative Example> The evaluation methods in each Example, Reference Example, and Comparative Example are as follows. A glass substrate (manufactured by Geomatec Co., Ltd.; hereinafter referred to as "ITO / Ag substrate") was prepared by sputtering a 100 nm film of APC (silver / palladium / copper = 98.07 / 0.87 / 1.06 (mass ratio)) on glass, and then sputtering a 10 nm film of ITO on top of the APC layer. The glass substrate was then irradiated with UV-O for 100 seconds using a tabletop optical surface treatment device (PL16-110; manufactured by Sen Special Light Sources Co., Ltd.). 3 They were used after cleaning. Tempax glass substrates (manufactured by AGC Technoglass Co., Ltd.), polyethylene terephthalate (hereinafter "PET") films, polypropylene (hereinafter "PP") films, and alumina substrates were used without pretreatment. The other substrates were used after a dehydration bake treatment by heating at 130°C for 2 minutes using a hot plate (HP-1SA; manufactured by AS ONE Corporation). The film thickness was measured using a surface roughness and contour shape measuring instrument (SURFCOM1400D; manufactured by Tokyo Seimitsu Co., Ltd.) at a measurement magnification of 10,000x, a measurement length of 1.0 mm, and a measurement speed of 0.30 mm / s.
[0320] (1) Weight-average molecular weight of resins The polyimides (PI-1) to (PI-7), polyimide precursors (PIP-1) to (PIP-4), polybenzoxazole (PB-1), polybenzoxazole precursor (PBP-1), and polyamideimide (PAI-1) were each dissolved in N-methyl-2-pyrrolidone to prepare a 0.10% by mass N-methyl-2-pyrrolidone solution. The weight-average molecular weight in terms of polystyrene was measured using a GPC analyzer (Waters 2690; manufactured by Waters) under the following measurement conditions. <GPC measurement conditions> Detector: Waters 996 System controller: Waters 2690 Column oven: Waters HTR-B Thermocontroller: Waters TCM Column: TOSOH Guard Column Column: TOSOH TSK-GEL α-4000 Column: TOSOH TSK-GEL α-2500 Fluidized bed: N-methyl-2-pyrrolidone in which lithium chloride and phosphoric acid were dissolved at 0.050 mol / L each Development rate: 0.40 mL / min.
[0321] For other resins, the weight average molecular weight in terms of polystyrene was measured at around room temperature using a GPC analyzer (HLC-8220; manufactured by Tosoh Corporation) and tetrahydrofuran or N-methyl-2-pyrrolidone as the fluidized bed in accordance with JIS K7252-3 (2008).
[0322] (2) Average Primary Particle Diameter of Pigment in Pigment Dispersion Using a dynamic light scattering particle size distribution analyzer (SZ-100; manufactured by Horiba, Ltd.), D50 (median diameter) of the pigment dispersion was measured under the following conditions: laser wavelength: 532 nm, dilution solvent: PGMEA, dilution ratio: 250 (weight ratio), solvent viscosity: 1.25, solvent refractive index: 1.40, measurement temperature: 25°C, measurement mode: scattered light, and calculation conditions: polydispersity / broad. The measurement was performed twice, and the average value was taken as the average primary particle diameter of the pigment in the pigment dispersion.
[0323] (3) Average Primary Particle Diameter of Pigment in Cured Film A cured film of the composition was prepared by the method described in Example 1 below. The cross section of the cured film was photographed and analyzed using a transmission electron microscope to measure the primary particle diameter of the pigment. The average value of 30 primary particles of the pigment was determined as the average primary particle diameter of the pigment in the cured film.
[0324] (4) Contents of specific aromatic compounds, specific organic acids, specific nitrogen-containing compounds, specific carboxylic acids, and specific oxime compounds in the composition or cured film The contents of specific aromatic compounds, specific organic acids, specific nitrogen-containing compounds, specific carboxylic acids, and specific oxime compounds in the composition or cured film were measured by gas chromatography mass spectrometry and liquid chromatography mass spectrometry using calibration curves based on standard substances. The content relative to the total solid content of the composition was calculated from the obtained measured value and the following formula: (Content relative to the total solid content of the composition) = (Content in the composition) × 100 / (Solid content concentration of the composition [mass %]).
[0325] (5) Content of specific anions in the composition or cured film The content of specific anions in the composition or cured film was measured by ion chromatography under the following measurement conditions. The composition or cured film was added to a 10 mmol / L aqueous potassium hydroxide solution and shaken for 2 hours to extract ionic components. The extract was filtered under the following conditions, and then analyzed for cationic and anionic components by ion chromatography. The absence of an ion content indicates that the ion in question was not detected. The content relative to the total solid content of the composition was calculated from the obtained measured value and the following formula. (Content of total solid content of composition) = (Content in composition) × 100 / (Solid content concentration of composition [mass %]) <Filtration treatment conditions> Membrane filter: 0.22 μmφ, PVDF (manufactured by Merck Millipore) Solid phase extraction cartridge: InertSep Slim-J PLS-3 (manufactured by GL Sciences) Cation exchange cartridge: OnGuard II H (manufactured by Thermo Fisher Scientific) <Ion chromatography analysis conditions> Apparatus: ICS-5000 + (Manufactured by Thermo Fisher Scientific) Separation column: 2 mmφ×250 mm, IonPac AS11-HC-4 μm Eluent: potassium hydroxide / gradient Detector: electrical conductivity detector Sample injection volume: 100 μL.
[0326] (6) Content of specific metal element in composition or cured film The content of specific metal element in the composition or cured film was measured by inductively coupled plasma mass spectrometry and inductively coupled plasma atomic emission spectrometry using a calibration curve of a standard substance. The content relative to the total solid content of the composition was calculated from the obtained measured value and the following formula: (Content relative to the total solid content of the composition) = (Content in composition) × 100 / (Solid content concentration of the composition [mass %]).
[0327] (7) Contents of Fluorine, Chlorine, Bromine, and Sulfur in the Composition or Cured Film The contents of fluorine, chlorine, bromine, and sulfur in the composition or cured film were measured by combustion ion chromatography under the following measurement conditions. The composition or cured film was burned and decomposed in the combustion tube of an analyzer, the generated gas was absorbed in an absorption liquid, and a portion of the absorption liquid was analyzed by ion chromatography. An absence of an element content indicates that the element was not detected. The content relative to the total solid content of the composition was calculated from the obtained measured value and the following formula: (Content relative to the total solid content of the composition) = (Content in the composition) × 100 / (Solids concentration of the composition [mass %]) <Combustion and Absorption Conditions> System: AQF-2100H, GA-210 (manufactured by Mitsubishi Chemical Corporation) Electric furnace temperature: Inlet 900°C, Outlet 1000°C Gas: Ar / O 2 200mL / min, O 2 400 mL / min Absorption liquid: H 2 O 2 0.1 mass% Absorption solution volume: 5 mL <Conditions for ion chromatography and anion analysis> System: ICS1600 (manufactured by DIONEX) Mobile phase: 2.7 mmol / L Na 2 CO 3 , 0.3 mmol / L NaHCO 3 Flow rate: 1.50 mL / min Detector: electrical conductivity detector Injection volume: 100 μL.
[0328] (8) Water Content in Composition The water content in the composition was measured by volumetric titration in accordance with JIS K0113 (2005) using a Karl Fischer moisture meter (MKS-520; manufactured by Kyoto Electronics Manufacturing Co., Ltd.) and a Karl Fischer reagent as a titration reagent.
[0329] (9) Sensitivity A developed film of the composition was prepared by the method described in Example 1 below. The resolution pattern of the prepared developed film was observed using an FPD / LSI inspection microscope (OPTIPHOT-300; manufactured by Nikon Corporation). As an index of sensitivity, the exposure dose (value measured with an i-line illuminometer) at which a space pattern corresponding to an opening in a 20 μm line and space pattern could be formed with a dimensional width of 18 μm was taken as the sensitivity. The sensitivity was judged as follows, and a value of 90 mJ / cm was obtained. 2 A+, A, B+, B, C+, and C are considered pass, and the sensitivity is 60 mJ / cm 2 A+, A, B+, and B are considered good, and a sensitivity of 40 mJ / cm 2 The following were rated as excellent: A+ and A: Sensitivity is 30 mJ / cm 2 A: Sensitivity is 30 mJ / cm or less 2 and more than 40 mJ / cm 2 Below B+: Sensitivity is 40 mJ / cm 2 and more than 50 mJ / cm 2 B: Sensitivity is 50 mJ / cm or less 2 and more than 60 mJ / cm 2 Below C+: Sensitivity is 60 mJ / cm 2 and more than 75 mJ / cm 2 C: Sensitivity is 75 mJ / cm or less 2 and more than 90 mJ / cm 2 D: Sensitivity is 90 mJ / cm or less 2 and more than 150 mJ / cm 2 E: Sensitivity is 150 mJ / cm or less 2 Exceeded.
[0330] (10) Development Residue A developed film of the composition was prepared by the method described in Example 1 below. The resolution pattern of the prepared developed film was observed using an FPD / LSI inspection microscope (OPTIPHOT-300; manufactured by Nikon Corporation). As an indicator of development residue, the presence or absence of residue in a pattern corresponding to an opening in a 20 μm line and space pattern was observed. The evaluation was performed as follows, with A+, A, B+, B, C+, and C indicating that the area of residue was 20% or less being considered acceptable; A+, A, B+, and B indicating that the area of residue was 10% or less being considered good; and A+ and A indicating that the area of residue was 3% or less being considered excellent. A+: No residue A: The area where residue is present is 3% or less B+: The area where residue is present is more than 3% but not more than 6% B: The area where residue is present is more than 6% but not more than 10% C+: The area where residue is present is more than 10% but not more than 15% C: The area where residue is present is more than 15% but not more than 20% D: The area where residue is present is more than 20% but not more than 50% E: The area where residue is present is more than 50% but not more than 100%.
[0331] (11) Light-Shielding Property (Optical Density Value (hereinafter, "OD Value")) A cured film of the composition was prepared on a Tempax glass substrate (manufactured by AGC Technoglass Co., Ltd.) by the method described in Example 1 below. The incident light intensity (I ) at three points on the surface of the prepared cured film was measured using a transmission densitometer (X-Rite 361T(V); manufactured by X-Rite Co., Ltd.). 0 The optical density (OD) per 1 μm of film thickness was calculated as an index of light-shielding ability using the following formula, and the average value of the OD values at three points on the surface was calculated. OD value=log 10 (I 0 / I).
[0332] (12) Mechanical Properties (Elongation at Break) A 6-inch diameter SiO 2 A cured film of the composition was formed on a silicon wafer with a thickness of about 5 μm. 2The cured film was peeled off from the / Si wafer. The peeled cured film was cut into strips measuring 1.5 cm wide x 9.0 cm long. A tensile test was performed using a Tensilon (RTM-100; manufactured by Orientec Co., Ltd.) at a room temperature of 23.0°C and a humidity of 45.0% RH at a tensile speed of 50 mm / min to measure the elongation at break. Ten strips were measured per specimen. The average of the top five results was calculated as an index of mechanical properties. The results were judged as follows: A+, A, B+, B, C+, and C, which indicate an elongation at break of 5.0% or more, were considered pass; A+, A, B+, and B, which indicate an elongation at break of 10% or more, were considered good; and A+ and A, which indicate an elongation at break of 20% or more, were considered excellent. A+: Elongation at break is 30% or more. A: Elongation at break is 20% or more and less than 30%. B+: Elongation at break is 15% or more and less than 20%. B: Elongation at break is 10% or more and less than 15%. C+: Elongation at break is 7.5% or more and less than 10%. C: Elongation at break is 5.0% or more and less than 7.5%. D: Elongation at break is 1.0% or more and less than 5.0%. E: Elongation at break is less than 1.0% or cannot be measured.
[0333] (13) Migration Resistance (Insulation Reliability) Using the method described in Example 1 below, a cured film of the composition was prepared to a thickness of approximately 1.5 μm on a migration evaluation substrate (WALTS-TEG ME0102JY; manufactured by Waltz Corporation). Next, in a line-and-space pattern of comb-shaped copper wiring, conductor wires were soldered to the measurement terminals with 15 μm lines and 10 μm spaces to prepare an evaluation element. The prepared evaluation element was evaluated for insulation reliability under high temperature and high humidity conditions using an insulation degradation characteristic evaluation system (ETAC SIR13; manufactured by Kusumoto Chemicals Co., Ltd.). The evaluation element was placed in a high-temperature, high-humidity chamber set at a temperature of 85°C and a humidity of 85% RH, and a voltage of 5.0 V was applied. The change in resistance over time was measured at 5-minute intervals. When the resistance value was 1.0 × 10 6When the resistance reached Ω or less, it was judged to be insulation failure, and the test time at that point was measured as an index of migration resistance. The evaluation was made as follows, with A+, A, B+, B, C+, and C being pass when the test time was 200 hours or more, A+, A, B+, and B being good when the test time was 400 hours or more, and A+ and A being excellent when the test time was 800 hours or more. A+: Test time was 1,000 hours or more A: Test time was 800 hours or more but less than 1,000 hours B+: Test time was 600 hours or more but less than 800 hours B: Test time was 400 hours or more but less than 600 hours C+: Test time was 300 hours or more but less than 400 hours C: Test time was 200 hours or more but less than 300 hours D: Test time was 50 hours or more but less than 200 hours E: Test time was less than 50 hours or not measurable.
[0334] <Compounds used in each Example, Reference Example, and Comparative Example> The structures of the compounds (b-1) to (b-9), (c-1) to (c-9), (f-1) to (f-3), (i-1), (j-1), (k-1), and (NQD-1) used in each Example, Reference Example, and Comparative Example are shown below. Note that (b-1) and (b-2) correspond to the above-mentioned (B-1) compound, and (b-3) and (b-4) correspond to the above-mentioned (B-2) compound. (b-5) corresponds to the above-mentioned (B-3) compound, and the minimum number of atoms in the above-mentioned (I-b3) structure is 4. (b-6), (b-7), (b-8), and (b-9) correspond to the above-mentioned (B-4) compound, and the minimum number of atoms in the above-mentioned (I-b4) structure is 13 for (b-6), 23 for (b-7), 31 for (b-8), and 17 for (b-9). (i-1) is a dissolution promoter and has a hydrophobic structure (a phenyl group having 6 carbon atoms, to which two ethylene groups having 2 carbon atoms are bonded, each having a phenyl group having 6 carbon atoms), a hydrophilic structure (12 oxyethylene groups having 2 carbon atoms), and a hydrophilic group (a hydroxy group bonded to the oxyethylene group). (j-1) is a fluorenone compound that serves as a sensitizer. (k-1) is an organosilane compound that serves as a silane coupling agent and is an adhesion improver, and has an epoxy group.
[0335]
[0336]
[0337]
[0338]
[0339] Furthermore, specific aromatic compounds; compounds containing specific anions; specific organic acids; specific nitrogen-containing compounds; compounds containing specific metal elements; specific carboxylic acids; specific oxime compounds; and compounds containing fluorine, chlorine, bromine, or sulfur elements (hereinafter referred to as "compounds containing specific elements") used in each of the Examples, Reference Examples, and Comparative Examples are collectively shown in Tables 2-5.
[0340]
[0341] <Preparation of Photosensitive Composition 1> Compositions 1 to 157 were prepared according to the formulations shown in Tables 3-1 to 3-12. In Tables 3-1 to 3-12, the values in parentheses indicate the parts by mass of the solid content of each component. When a composition contained a pigment, a preparation not containing a pigment dispersion was first prepared, and then the pigment dispersion was mixed with the preparation to prepare the composition. A PGMEA / EL / GBL mixture in a mass ratio of 50 / 40 / 10 was used as the solvent, and the composition was prepared so that the solid content concentration was 20% by mass. The resulting composition solution was filtered through a 0.45 μmφ filter before use.
[0342] The amounts of the specific aromatic compound and water added were adjusted so that their contents in the composition would be those shown in Tables 3-1 to 3-12. The amounts of the compound containing a specific anion, the compound containing a specific metal element, and the compound containing a specific element added were adjusted so that the contents of the specific anion, the specific organic acid, the specific metal element, and the contents of elemental fluorine, elemental chlorine, elemental bromine, and elemental sulfur relative to the total solid content of the composition would be those shown in Tables 3-1 to 3-12. The amounts of the specific organic acid, the specific nitrogen-containing compound, the specific carboxylic acid, and the specific oxime compound added were adjusted so that their contents relative to the total solid content of the composition would be those shown in Tables 3-1 to 3-12.
[0343]
[0344]
[0345]
[0346]
[0347]
[0348]
[0349]
[0350]
[0351]
[0352]
[0353]
[0354]
[0355] Example 1 Composition 1 was applied to an ITO / Ag substrate using a spin coater (MS-A100; manufactured by Mikasa Corporation), and then prebaked for 120 seconds at 120°C using a buzzer hot plate (HPD-3000BZN; manufactured by AS ONE Corporation) to produce a prebaked film with a film thickness of approximately 1.8 μm. The prebaked film thus produced was spray-developed with a 2.38% by mass aqueous solution of TMAH or cyclopentanone using a compact photolithography developing device (AD-1200; manufactured by Takizawa Sangyo Co., Ltd.), and the time required for the prebaked film (unexposed areas) to completely dissolve (Breaking Point; hereinafter, "BP") was measured.
[0356] A prebaked film was prepared in the same manner, and the prepared prebaked film was subjected to patterning exposure using a double-sided alignment single-sided exposure device (Mask Aligner PEM-6M; manufactured by Union Optical Co., Ltd.) through a grayscale mask for sensitivity measurement (MDRM MODEL 4000-5-FS; manufactured by Opto-Line International Co., Ltd.) with the i-line (wavelength 365 nm), h-line (wavelength 405 nm), and g-line (wavelength 436 nm) of an ultra-high pressure mercury lamp. After exposure, the film was developed with a 2.38% by mass TMAH aqueous solution using a compact photolithography developing device (AD-1200; manufactured by Takizawa Sangyo Co., Ltd.) and rinsed with water for 30 seconds to prepare a developed film. The development time was 1.3 times the measured BP. In cases where a pattern could not be formed after development with a 2.38% by weight TMAH aqueous solution, an exposed film was prepared in the same manner as above. After exposure, the film was developed with cyclopentanone using a small photolithography developing device (AD-1200; manufactured by Takizawa Sangyo Co., Ltd.) and rinsed with water for 30 seconds to produce a developed film. The development time was 1.3 times the measured BP. The developed pattern was observed, and the optimal exposure dose (value measured with an i-line illuminometer) capable of forming a space pattern with a dimensional width of 18 μm corresponding to the openings in a 20 μm line-and-space pattern was determined. After exposure at the optimal exposure dose, the developed pattern was thermally cured at 220°C for 60 minutes using a high-temperature inert gas oven (INH-9CD-S; manufactured by Koyo Thermo Systems Co., Ltd.) to produce a cured film with a film thickness of approximately 1.2 μm. The thermal curing conditions were as follows: in a nitrogen atmosphere with an oxygen concentration of 20 mass ppm or less, the temperature was raised to 220°C at a rate of 3.5°C / min, heat treatment was carried out at 220°C for 60 minutes, and then cooling to 50°C.
[0357] The cured film was analyzed using methods such as nuclear magnetic resonance spectroscopy, infrared spectroscopy, and time-of-flight secondary ion mass spectrometry to analyze the structural units of the resins contained therein. It was confirmed that the cured film of Composition 1 prepared by the above method contained the following resin. That is, the cured film of Composition 1 contained a resin having a structure derived from the resin contained in Composition 1. (XA1) Resin: Resin having a structural unit represented by General Formula (1); Resin having a structural unit represented by General Formula (2) <Examples 2 to 152 and Comparative Examples 1 to 5> Using each composition shown in Tables 3-1 to 3-12, the same procedures and evaluations as in Example 1 were performed. The evaluation results are summarized in Tables 4-1 to 4-12. For ease of comparison, the composition and evaluation results of Example 1 are listed in Tables 3-2 to 3-8 and Tables 4-2 to 4-8, respectively. Furthermore, the compositions and evaluation results of Examples 1, 115, and 119 are listed in Tables 3-9 and 4-9, respectively. Tables 3-10 and 4-10 show the composition and evaluation results of Example 123, respectively. In Examples 1 to 144 and Comparative Examples 1 to 5, the fluorine element content relative to the total solid content of the composition and the fluorine element content in the cured product exceeded 1,000 ppm by mass. In Examples 145 to 148, the fluorine element content relative to the total solid content of the composition and the fluorine element content in the cured product were 0 ppm by mass. In Examples 149 to 152, the fluorine element content relative to the total solid content of the composition is as shown in Table 3-11, and the fluorine element content in the cured product is as shown in Table 4-11.
[0358] The thermal curing conditions for Example 142 were as follows: in a nitrogen atmosphere with an oxygen concentration of 20 ppm by mass or less, the temperature was raised to 200°C at a heating rate of 3.5°C / min, and the composition was heated at 200°C for 60 minutes, followed by cooling to 50°C. Furthermore, in each of the above-described examples, when a positive-type photosensitive composition was used, a photomask in which the light-transmitting and light-shielding portions were inverted was used. The development time was set to 60, 90, or 120 seconds, and a grayscale mask (MDRM MODEL 4000-5-FS; manufactured by Opto-Line International) for sensitivity measurement was used to determine the optimal exposure dose (value measured with an i-line illuminometer) for forming a space pattern corresponding to the openings with a 20 μm width in a 20 μm line-and-space pattern. From these results, the optimal development time (60, 90, or 120 seconds) and the optimal exposure dose for that development time were determined. After exposure at the optimum exposure dose and development for the optimum development time, the pattern was thermally cured for 60 minutes at 200° C. The thermal curing conditions were as follows: in a nitrogen atmosphere with an oxygen concentration of 20 mass ppm or less, the temperature was raised to 200° C. at a temperature increase rate of 3.5° C. / min, heat treatment was carried out at 200° C. for 60 minutes, and then cooling to 50° C.
[0359]
[0360]
[0361]
[0362]
[0363]
[0364]
[0365]
[0366]
[0367]
[0368]
[0369]
[0370]
[0371] Comparative Examples 1 and 2 do not contain the specific aromatic compound, the specific anion-containing compound, or the specific organic acid, and therefore are inferior in development residue, mechanical properties, and migration resistance.
[0372] In Comparative Example 3, the content of the specific aromatic compound exceeds 1,000 ppm by mass. In Comparative Example 4, the content of the specific organic acid exceeds 1,000 ppm by mass. In Comparative Example 5, the content of the specific anion exceeds 1,000 ppm by mass. Comparative Examples 3, 4, and 5 do not satisfy any of the conditions (1x), (2x), and (3). Therefore, any one of the properties of development residue, mechanical properties, and migration resistance is inferior.
[0373] Comparative Example 6 Composition 155 was prepared in the same manner as in Comparative Example 3, except that the content of the specific aromatic compound in the composition was 1,500 ppm by mass. The resulting composition 155 was stored at 25° C. for one week. After storage, the composition was formed into a film on a substrate in the same manner as in Example 1. As a result, a large amount of foreign matter was generated, and the storage stability of the composition was poor.
[0374] Comparative Example 7 Composition 156 was prepared in Comparative Example 4, except that the content of the specific organic acid relative to the total solid content of the composition was 1,500 ppm by mass. The resulting composition 156 was stored at 25°C for one week. After storage, the composition was formed into a film on a substrate in the same manner as in Example 1. As a result, a large amount of foreign matter was generated, and the storage stability of the composition was poor.
[0375] Comparative Example 8 Composition 157 was prepared in the same manner as in Comparative Example 5, except that the content of the specific anion relative to the total solid content of the composition was 1,500 ppm by mass. The resulting composition 157 was stored at 25°C for one week. After storage, the composition was formed into a film on a substrate in the same manner as in Example 1. As a result, a large amount of foreign matter was generated, and the storage stability of the composition was poor.
[0376] Example 153 Composition 1 was prepared in the same manner as in Example 1, except that the content of the specific aromatic compound in the composition was 3 ppm by mass and the content of the specific organic acid in the total solid content of the composition was 3 ppm by mass. The resulting composition 1 was similarly stored at 25°C for one week. After storage, the composition was formed into a film on a substrate in the same manner as in Example 1. As a result, no foreign matter was generated and the storage stability of the composition was found to be good.
[0377] Example 154 Composition 14 was prepared in the same manner as in Example 14, except that the content of the specific aromatic compound in the composition was 3 ppm by mass and the content of the specific anion in the total solid content of the composition was 3 ppm by mass. The resulting composition 14 was similarly stored at 25°C for one week. After storage, the composition was formed into a film on a substrate in the same manner as in Example 1. As a result, no foreign matter was generated and the storage stability of the composition was found to be good.
[0378] <Preparation of Photosensitive Composition 2> Composition 158 was prepared using the same solid content as composition 1 described in Table 3-1 and GBL as a solvent so that the solid content concentration of the composition was 60 mass %. Similarly, composition 159 was prepared using the same solid content as composition 22 and GBL as a solvent so that the solid content concentration of the composition was 60 mass %. The resulting composition solution was filtered through a 1.0 μmφ filter before use.
[0379] Example 155 Composition 158 was applied onto a 50 μm-thick PET film using a comma roll coater, and then dried at 120° C. for 8 minutes. Next, a 30 μm-thick PP film was laminated as a protective film, to obtain a photosensitive composition film having a photosensitive composition coating of Composition 158, a PET film support, and a PP film protective film. The PP film protective film was peeled from the obtained photosensitive composition film, and the peeled surface was laminated onto a 5 cm x 5 cm alumina substrate using a vacuum diaphragm laminator (MVLP-500 / 600; manufactured by Meiki Seisakusho Co., Ltd.) under conditions of upper and lower heating platen temperatures of 80° C., a vacuuming time of 20 seconds, a vacuum pressing time of 30 seconds, and an application pressure of 0.5 MPa, thereby forming a photosensitive composition coating on the alumina substrate. Thereafter, the PET film serving as the support film was peeled off, and then a photomask having patterns with via sizes of 20 μmφ and 10 μmφ and patterns with line widths / space widths of 40 μm / 20 μm and 20 μm / 10 μm was set in an exposure device, and an exposure dose of 200 mJ / cm was applied using an ultra-high pressure mercury lamp equipped with an i-line bandpass filter under the condition of an exposure gap of 100 μm between the photomask and the photosensitive composition film. 2 , 300 mJ / cm 2 , 400 mJ / cm 2 , and 500 mJ / cm 2 The film was subjected to patterning exposure at 1000 kJ / cm² (value measured by an i-line illuminometer). After exposure, the film was developed by dip development using a 2.38% by mass aqueous solution of TMAH or cyclopentanone, and then rinsed with isopropyl alcohol or water for 30 seconds to produce a developed film in which the photosensitive composition film was patterned. The development time was twice the time required for the unexposed areas to completely dissolve. The developed pattern was thermally cured in the same manner as in Example 1 to produce a cured film of the photosensitive composition. Evaluation was carried out in the same manner as in Example 1. In Example 155, the content of elemental fluorine in the total solids content of the composition and the content of elemental fluorine in the cured product exceeded 1,000 ppm by mass. The sensitivity and development residue of the photosensitive composition film were evaluated using the methods described below. The evaluation results using a photosensitive composition film having a photosensitive composition film of composition 158 were as follows: sensitivity: A, development residue: A, mechanical properties: A, and migration resistance: B+.
[0380] The sensitivity of the photosensitive composition film was evaluated by the following method. A developed film was prepared by patterning the photosensitive composition film using the method described in Example 155 above. The resolution pattern of the developed film was observed using an FPD / LSI inspection microscope (OPTIPHOT-300; manufactured by Nikon Corporation). As an index of sensitivity, the exposure dose (value obtained with an i-line illuminometer) at which a space pattern corresponding to an opening with a dimensional width of 20 μm can be formed in a pattern with a line width / space width of 40 μm / 20 μm was used. The sensitivity was evaluated as follows, and a sensitivity of 900 mJ / cm was obtained. 2 A+, A, B+, B, C+, and C are considered acceptable, and the sensitivity is 600 mJ / cm 2 A+, A, B+, and B are considered good, and a sensitivity of 400 mJ / cm 2 The following were rated as excellent: A+ and A: Sensitivity is 300 mJ / cm 2 A: Sensitivity is 300 mJ / cm or less 2 and more than 400 mJ / cm 2 Below B+: Sensitivity is 400 mJ / cm 2 and more than 500 mJ / cm 2 B: Sensitivity is 500 mJ / cm or less 2 and more than 600 mJ / cm 2 Below C+: Sensitivity is 600 mJ / cm 2 and more than 750 mJ / cm 2 C: Sensitivity is 750 mJ / cm or less 2 and more than 900 mJ / cm 2 D: Sensitivity is 900 mJ / cm or less 2 and more than 1,500 mJ / cm 2 E: Sensitivity is 1,500 mJ / cm or less 2 Exceeded.
[0381] The development residue of the photosensitive composition film was evaluated by the following method. A developed film was prepared by patterning a photosensitive composition film using the method described in Example 155 above. The resolution pattern of the prepared developed film was observed using an FPD / LSI inspection microscope (OPTIPHOT-300; manufactured by Nikon Corporation). As an indicator of development residue, the presence or absence of residue in a pattern corresponding to an opening in a pattern with a line width / space width of 40 μm / 20 μm was observed. The evaluation was performed as follows, with A+, A, B+, B, C+, and C indicating a residue presence area of 20% or less being considered "pass," A+, A, B+, and B indicating a residue presence area of 10% or less being considered "good," and A+ and A indicating a residue presence area of 3% or less being considered "excellent." A+: No residue A: The area where residue is present is 3% or less B+: The area where residue is present is more than 3% but not more than 6% B: The area where residue is present is more than 6% but not more than 10% C+: The area where residue is present is more than 10% but not more than 15% C: The area where residue is present is more than 15% but not more than 20% D: The area where residue is present is more than 20% but not more than 50% E: The area where residue is present is more than 50% but not more than 100%.
[0382] Example 156 The same operations and evaluations as in Example 155 were carried out using composition 159. In Example 156, the content of elemental fluorine in the total solid content of the composition and the content of elemental fluorine in the cured product exceeded 1,000 ppm by mass. The evaluation results using a photosensitive composition film having a photosensitive composition coating of composition 159 were A for sensitivity, A+ for development residue, A+ for mechanical properties, and A+ for migration resistance.
[0383] REFERENCE SIGNS LIST 1 Si wafer 2 Al pad 3 Passivation layer 4 Insulation layer 5 Metal layer 6 Metal wiring 7 Insulation layer 8 Barrier metal layer 9 Scribe line 10 Solder bump
Claims
1. A photosensitive composition containing (A) a binder resin and (C) a photosensitizer, and further containing (B) a radical polymerizable compound and / or (F) a crosslinking agent, wherein the (A) binder resin contains the following (A1) resin and / or (A2) resin, and the photosensitive composition satisfies the following condition (α): (A1) Resin: A resin containing one or more selected from the group consisting of an imide structure, an amide structure, an oxazole structure, and a siloxane structure in a structural unit in the main chain of the resin. (A2) Resin: A resin having a phenolic hydroxyl group in a structural unit in the main chain of the resin. (α) Further, the photosensitive composition contains one or more selected from the group consisting of sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing fluorine element, and satisfies the following condition (1x): (1x) The total content of the sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing fluorine element in the total solid content of the photosensitive composition is 0.010 to 1,000 ppm by mass.
2. The photosensitive composition according to claim 1, wherein the sulfonic acid, and the phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, and hypophosphite ester (hereinafter referred to as "organic acids containing a phosphorus element") have the following specific substituent a, the fluorine-containing carboxylic acid has the following specific substituent b, and the condition (α) is the following condition (α2), and the following condition (α2) is satisfied: (α2) Further, the compound contains one or more selected from the group consisting of a sulfonic acid having the following specific substituent a, a phosphorus-containing organic acid having the following specific substituent a, and a fluorine-containing carboxylic acid having the following specific substituent b, and satisfies the condition (1y) below: specific substituent a: one or more selected from the group consisting of a mono- or divalent aliphatic group having 1 to 18 carbon atoms, a mono- or divalent alicyclic group having 4 to 18 carbon atoms, a mono- or divalent aromatic group having 6 to 15 carbon atoms, a mono- or divalent fluorine-containing aliphatic group having 1 to 18 carbon atoms, a mono- or divalent fluorine-containing alicyclic group having 4 to 18 carbon atoms, and a mono- or divalent fluorine-containing aromatic group having 6 to 15 carbon atoms; specific substituent b: one or more selected from the group consisting of a mono- or divalent fluorine-containing aliphatic group having 1 to 18 carbon atoms, a mono- or divalent fluorine-containing alicyclic group having 4 to 18 carbon atoms, and a mono- or divalent fluorine-containing aromatic group having 6 to 15 carbon atoms. (1y) the total content of the sulfonic acid having the specific substituent a, the phosphorus-containing organic acid having the specific substituent a, and the fluorine-containing carboxylic acid having the specific substituent b in the total solid content of the photosensitive composition is 0.010 to 1,000 ppm by mass; 3. The photosensitive composition according to claim 2, wherein the condition (α2) is the following condition (α3), and the following condition (α3) is satisfied: the sulfonic acid contains one or more selected from the group consisting of methanesulfonic acid, cyclohexanesulfonic acid, benzenesulfonic acid, toluenesulfonic acid, xylenesulfonic acid, trifluoromethanesulfonic acid, hexafluorocyclohexanesulfonic acid, hexafluorobenzenesulfonic acid, pentafluorotoluenesulfonic acid, tetrafluoroxylenesulfonic acid, trifluoromethylbenzenesulfonic acid, trifluoromethyltoluenesulfonic acid, and trifluoromethylxylenesulfonic acid; and the fluorine-containing carboxylic acid contains one or more selected from the group consisting of trifluoroacetic acid, trifluoropropionic acid, hexafluorocyclohexanecarboxylic acid, hexafluorobenzoic acid, and trifluoromethylbenzoic acid. (α3) The photosensitive composition further contains a sulfonic acid and / or a carboxylic acid containing a fluorine element, and satisfies the following condition (1z): (1z) the total content of the sulfonic acid and the carboxylic acid containing a fluorine element in the total solid content of the photosensitive composition is 0.010 to 1,000 ppm by mass; 4. The photosensitive composition according to claim 1, further satisfying the following condition (β): (β) further containing one or more ions selected from the group consisting of chloride ions, bromide ions, sulfate ions, sulfite ions, nitrate ions, nitrite ions, phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions, and also satisfying the following condition (2x): (2x) the total content of chloride ions, bromide ions, sulfate ions, sulfite ions, nitrate ions, nitrite ions, phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions in the total solid content of the photosensitive composition is 0.010 to 1,000 ppm by mass.
5. The photosensitive composition according to claim 1, further satisfying the following condition (γ): (γ) further containing one or more members selected from the group consisting of benzene, toluene, xylene, and naphthalene, and satisfying the following condition (3): (3) the total content of benzene, toluene, xylene, and naphthalene in the photosensitive composition is 0.010 to 1,000 ppm by mass 6. The photosensitive composition according to any one of claims 1 to 5, wherein the binder resin (A) comprises the resin (A1), and the resin (A1) comprises one or more resins selected from the group consisting of the following resins (A1-1), (A1-2), (A1-3), (A1-4), (A1-5), (A1-6), and copolymers consisting of two or more of them: (A1-1) resin: polyimide (A1-2) resin: polyimide precursor (A1-3) resin: polybenzoxazole (A1-4) resin: polybenzoxazole precursor (A1-5) resin: polyamideimide (A1-6) resin: polyamideimide precursor 7. The photosensitive composition according to claim 6, further comprising one or more compounds selected from the group consisting of cyclic amide compounds represented by general formula (20), amide compounds represented by general formula (21), cyclic urea compounds represented by general formula (22), urea compounds represented by general formula (23), oxazolidone compounds represented by general formula (24), and isoxazolidone compounds represented by general formula (25), and satisfying the following condition (4): (4) The total content of the cyclic amide compounds represented by general formula (20), amide compounds represented by general formula (21), cyclic urea compounds represented by general formula (22), urea compounds represented by general formula (23), oxazolidone compounds represented by general formula (24), and isoxazolidone compounds represented by general formula (25) is 0.010 to 5.0% by mass based on the total solid content of the photosensitive composition. (In general formulas (20) to (25), R 46 ~R 56 R each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, a cycloalkyl group having 4 to 10 carbon atoms, an aryl group having 6 to 15 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, or a hydroxyalkyl group having 1 to 6 carbon atoms. 130 represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a hydroxyalkyl group having 1 to 6 carbon atoms, a hydroxyalkoxy group having 1 to 6 carbon atoms, a hydroxy group, an amino group, a monoalkylamino group having 1 to 6 carbon atoms, or a dialkylamino group having 2 to 12 carbon atoms. 131 ~R 142 each independently represents an alkyl group having 1 to 6 carbon atoms. α, β, and γ each independently represent an integer of 0 to 6. a, b, c, e, f, g, h, i, j, k, l, and m each independently represent an integer of 0 to 2. When α is 0, a is 0. When β is 0, b is 0. When γ is 0, c is 0.
8. The photosensitive composition according to claim 7, further comprising one or more components selected from the group consisting of a component containing elemental sodium, a component containing elemental potassium, a component containing elemental magnesium, a component containing elemental calcium, a component containing elemental iron, a component containing elemental copper, and a component containing elemental chromium, and satisfying the following condition (5): (5) The total content of elemental sodium, elemental potassium, elemental magnesium, elemental calcium, elemental iron, elemental copper, and elemental chromium in the total solid content of the photosensitive composition is 0.010 to 500 ppm by mass.
9. The photosensitive composition according to claim 1, wherein the (C) photosensitizer contains (C1) a photopolymerization initiator, and the (C1) photopolymerization initiator contains (C1-1) an oxime ester compound and / or (C1-2) a phosphine oxide compound.
10. The photosensitive composition according to claim 9, further comprising one or more selected from the group consisting of acetic acid, propionic acid, cyclopentanecarboxylic acid, cyclohexanecarboxylic acid, benzoic acid, methylbenzoic acid, and trimethylbenzoic acid, and satisfying the following condition (6): and / or further comprising an aldoxime compound and / or a ketoxime compound, and satisfying the following condition (7): (6) The total content of acetic acid, propionic acid, cyclopentanecarboxylic acid, cyclohexanecarboxylic acid, benzoic acid, methylbenzoic acid, and trimethylbenzoic acid in the total solid content of the photosensitive composition is 0.010 to 500 ppm by mass, or (7) The total content of aldoxime compounds and ketoxime compounds in the total solid content of the photosensitive composition is 0.010 to 500 ppm by mass.
11. The photosensitive composition according to claim 10, further comprising one or more components selected from the group consisting of a component containing elemental chlorine, a component containing elemental bromine, and a component containing elemental sulfur, and satisfying the following conditions (8) and / or (9): and / or, further comprising water, and satisfying the following condition (10): (8) The total content of elemental chlorine and elemental bromine in the total solid content of the photosensitive composition is 0.010 to 500 ppm by mass; (9) The content of elemental sulfur in the total solid content of the photosensitive composition is 0.010 to 500 ppm by mass; and (10) The content of water in the photosensitive composition is 0.010 to 3.0% by mass.
12. The photosensitive composition according to any one of claims 1 to 5 and 9 to 11, further satisfying the following condition (1α): (1α) the content of elemental fluorine in the total solid content of the photosensitive composition is 1,000 mass ppm or less; 13. The photosensitive composition according to any one of claims 1 to 5 and 9 to 11, further satisfying at least one of the following conditions (δ), (ε), and (ζ): (δ) The (B) radical polymerizable compound contains the following (B1) first polymerizable compound and (B2) second polymerizable compound. (ε) The (B) radical polymerizable compound contains the following (B3) third polymerizable compound and (B4) fourth polymerizable compound. (ζ) The (B) radical polymerizable compound contains the following (B1) first polymerizable compound or (B2) second polymerizable compound, and further contains the following (B3) third polymerizable compound or (B4) fourth polymerizable compound. (B1) First polymerizable compound: A compound having the following (I-b1) structure and further having at least two radical polymerizable groups. (I-b1) Structure: A structure containing an alicyclic structure and / or a heteroalicyclic structure. (B2) Second polymerizable compound: A compound having the following (I-b2) structure and (II-b2) structure and further having at least two radical polymerizable groups. (I-b2) Structure: A structure containing an aromatic structure. (II-b2) Structure: A structure containing an aliphatic structure. (B3) Third polymerizable compound: A compound having at least two (meth)acryloyl groups and further having the following structure (I-b3). (I-b3) Structure: At least two (meth)acryloyl groups are connected by a minimum of 4 to 10 atoms, and a structure containing an aliphatic structure. (B4) Fourth polymerizable compound: A compound having at least two (meth)acryloyl groups and further having the following structure (I-b4). (I-b4) Structure: At least two (meth)acryloyl groups are connected by a minimum of 11 to 45 atoms, and a structure containing an aliphatic structure.
14. The photosensitive composition according to any one of claims 1 to 5 and 9 to 11, further comprising (G) inorganic particles, the (G) inorganic particles being one or more particles selected from the group consisting of silica particles, alumina particles, titania particles, vanadium oxide particles, chromium oxide particles, iron oxide particles, cobalt oxide particles, copper oxide particles, zinc oxide particles, zirconium oxide particles, niobium oxide particles, tin oxide particles, and cerium oxide particles.
15. A photosensitive composition containing (A) a binder resin and (C) a photosensitizer, and further containing (B) a radical polymerizable compound and / or (F) a crosslinking agent, wherein the (A) binder resin contains the following (A1) resin and / or (A2) resin, and the photosensitive composition satisfies one or more of the following conditions (α), (β), and (γ): (A1) Resin: A resin containing one or more selected from the group consisting of an imide structure, an amide structure, an oxazole structure, and a siloxane structure in a structural unit in the main chain of the resin. (A2) Resin: A resin having a phenolic hydroxyl group in a structural unit in the main chain of the resin. (α) Further, the photosensitive composition contains one or more selected from the group consisting of sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing fluorine element, and satisfies the following condition (1x): (1x) The total content of the sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing fluorine element in the total solid content of the photosensitive composition is 0.010 to 1,000 ppm by mass. (β) further contains one or more ions selected from the group consisting of chloride ions, bromide ions, sulfate ions, sulfite ions, nitrate ions, nitrite ions, phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions, and satisfies the following condition (2x): (2x) the total content of chloride ions, bromide ions, sulfate ions, sulfite ions, nitrate ions, nitrite ions, phosphate ions, phosphite ions, hypophosphite ions, formate ions, and fluoride ions in the total solids content of the photosensitive composition is 0.010 to 1,000 ppm by mass; (γ) further contains one or more ions selected from the group consisting of benzene, toluene, xylene, and naphthalene, and satisfies the following condition (3): (3) the total content of benzene, toluene, xylene, and naphthalene in the photosensitive composition is 0.010 to 1,000 ppm by mass.
16. A photosensitive composition film having a photosensitive composition coating and a support, the photosensitive composition being formed from the photosensitive composition according to any one of claims 1 to 5, 9 to 11, and 15.
17. A cured product obtained by curing the photosensitive composition according to any one of claims 1 to 5, 9 to 11, and 15.
18. An electronic component comprising the cured product according to claim 17.
19. A method for producing a cured product, comprising: (1) a step of forming a coating film of the photosensitive composition according to any one of claims 1 to 5, 9 to 11, and 15 on a substrate; (2) a step of irradiating the coating film of the photosensitive composition with actinic rays through a photomask; (3) a step of developing the coating film with a developer to form a pattern of the photosensitive composition; and (4) a step of heating the pattern to obtain a cured pattern of the photosensitive composition.
20. An electronic component having a cured product, the cured product containing the following resin (XA1) and / or resin (XA2), and satisfying the following condition (Xα): (XA1) resin: a resin containing one or more structures selected from the group consisting of imide structures, amide structures, oxazole structures, and siloxane structures in the structural units of the resin main chain; (XA2) resin: a resin having a phenolic hydroxyl group in the structural units of the resin main chain; (Xα) further containing one or more structures selected from the group consisting of sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing a fluorine element, and satisfying the following condition (X1x): (X1x) the total content of sulfonic acid, phosphate ester, phosphonic acid, phosphonate ester, phosphite ester, phosphinic acid, hypophosphite ester, and carboxylic acid containing a fluorine element in the cured product is 0.010 to 1,000 ppm by mass.