Element transfer sheet
Patent Information
- Application Number
- MYPI2025001760
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2023-09-21
- Publication Date
- 2024-03-22
AI Technical Summary
Element transfer sheets with uneven adhesive surfaces struggle to increase the distance between elements when expanded, leading to reduced holding force and limited interval widening between elements.
An element transfer sheet with a base material having uneven tensile stress in specific directions, combined with an adhesive layer featuring convex portions, allows for increased spacing and uniformity between elements upon expansion.
The solution effectively increases the distance between elements while maintaining uniformity, facilitating easier peeling and transfer by adjusting tensile stress and adhesive layer design.
Smart Images

Figure PI2025001760_DRAWING_001 
Figure PI2025001760_DRAWING_002 
Figure PI2025001760_DRAWING_003
Abstract
Description
Element transfer sheet
[0001] The present invention relates to a sheet for element transfer.
[0002] Element transfer sheets used for transferring elements are known. Such sheets can be used to temporarily hold an object and transfer it to a desired position. It is also known to expand the element transfer sheet while it is holding the object.
[0003] For example, Patent Document 1 describes dicing a semiconductor wafer attached to a dicing film, expanding the dicing film after dicing to separate the chips, and then picking up and transferring the chips to another substrate. Patent Document 1 also discloses using a material having a specific density and specific components as the dicing film material to form uniform gaps between the chips in the expanding process. Furthermore, Non-Patent Documents 2 and 3 describe attaching a wafer to adhesive tape, irradiating the intended cutting portion with laser light, and expanding the adhesive tape to cut the wafer along the intended cutting portion.
[0004] JP 2021-014557 A JP 2023-013022 A JP 2023-013023 A
[0005] The present inventors have investigated providing irregularities on the surface of the adhesive layer of an element transfer sheet. According to this configuration, by expanding the sheet, the holding force of the element by the sheet can be reduced, making it easier to peel the element from the sheet. However, it has been found that even if the sheet is expanded while elements are held on an element transfer sheet having such irregularities, the spacing between the elements may not be large enough.
[0006] An object of the present invention is to increase the spacing between elements held by an element transfer sheet having an adhesive layer with an uneven surface when the sheet is expanded.
[0007] After extensive research, the inventors discovered that by appropriately adjusting the tensile stress of the substrate of the element transfer sheet, the spacing between the elements held by the sheet can be increased when the sheet is expanded, thereby solving the above-mentioned problem. After further research, they completed the present invention.
[0008] That is, the present invention relates to the following items [1] to [9]. [1] A device transfer sheet comprising a substrate and an adhesive layer having an uneven surface, wherein the tensile stress in a first direction at 100% elongation of the substrate is higher than the tensile stress in a second direction perpendicular to the first direction, the tensile stress in the first direction being 12 MPa or more and the tensile stress in the second direction being 9 MPa or more. [2] The device transfer sheet according to [1], wherein the tensile stress in the first direction is 40 MPa or less and the tensile stress in the second direction is 30 MPa or less. [3] The device transfer sheet according to any one of [1] to [2], wherein the tensile modulus of the substrate is 2500 MPa or less. [4] The device transfer sheet according to any one of [1] to [3], wherein the breaking elongation of the substrate is 105% or more. [5] The device transfer sheet according to any one of [1] to [4], wherein the substrate is a polyolefin film or a vinyl chloride copolymer film. [6] The element transfer sheet according to any one of [1] to [5], wherein the adhesive layer has a plurality of convex portions spaced apart by concave portions, the plurality of convex portions having a pitch of 1 μm to 100 μm. [7] The element transfer sheet according to any one of [1] to [6], wherein the adhesive layer has a plurality of convex portions, the heights of the plurality of convex portions being uniform. [8] The element transfer sheet according to any one of [1] to [7], wherein, after forming a plurality of elements by dicing a wafer substrate held on the adhesive layer, the element transfer sheet is expanded by 180% in the first direction and the second direction, the coefficient of variation of the spacing between the plurality of elements is 0.2 or less. [9] The element transfer sheet according to any one of [1] to [8], wherein, after forming a plurality of elements by dicing a wafer substrate held on the adhesive layer, the element transfer sheet is expanded by 80 mm in the first direction and the second direction, the average spacing between the plurality of elements is 1 mm or more.
[0009] When the element transfer sheet having an adhesive layer with an uneven surface is expanded, the spacing between the elements held by the sheet can be made larger.
[0010] 1 is a cross-sectional view of a sheet according to an embodiment; 2 is a cross-sectional view showing an example of unevenness on a sheet; 3 is a cross-sectional view showing an example of unevenness on a sheet; 4 is a top view showing an example of unevenness on a sheet; 5 is a top view showing an example of unevenness on a sheet; 6 is a cross-sectional view showing an example of unevenness on a sheet; 7 is a cross-sectional view showing an example of unevenness on a sheet; 8 is a cross-sectional view showing an example of unevenness on a sheet; 9 is a cross-sectional view showing an example of unevenness on a sheet; 10 is a diagram for explaining a method of expanding a sheet; 11 is a diagram for explaining a method of expanding a sheet; 12 is a flowchart of an element transferring method according to an embodiment;
[0011] Hereinafter, the embodiments will be described in detail with reference to the accompanying drawings. Note that the following embodiments do not limit the scope of the invention as claimed, and not all combinations of features described in the embodiments are necessarily essential to the invention. Two or more of the features described in the embodiments may be combined in any desired manner. Furthermore, the same reference numerals are used to designate identical or similar components, and redundant descriptions will be omitted.
[0012] (Definitions) In this specification, the mass average molecular weight (Mw) and number average molecular weight (Mn) are values measured by size exclusion chromatography in terms of standard polystyrene, specifically, values measured in accordance with JIS K7252-1: 2016. In addition, in this specification, "(meth)acrylic acid" is a term that refers to both "acrylic acid" and "methacrylic acid," and the same applies to other similar terms.
[0013] In this specification, when one or more lower limits and one or more upper limits of a numerical range (e.g., a range of content, etc.) are described, it can be understood that any combination of the lower limit and upper limit therein is described. For example, the description "preferably 1 or more, more preferably 2 or more, even more preferably 3 or more, and preferably 9 or less, more preferably 8 or less, even more preferably 7 or less" clearly means that the numerical range may be any of 1 or more to 9 or less, 1 or more to 8 or less, 1 or more to 7 or less, 2 or more to 9 or less, 2 or more to 8 or less, 2 or more to 7 or less, 3 or more to 9 or less, 3 or more to 8 or less, and 3 or more to 7 or less.
[0014] (Sheet Configuration) An element transfer sheet according to one embodiment of the present invention comprises a substrate 120 and an adhesive layer 110 having an uneven surface. The element transfer sheet is used to temporarily hold an element and transfer it to a destination. For example, the element transfer sheet can be used to receive an element held on another holding substrate, temporarily hold the element, and transfer the element to a desired position on the destination. The substrate 120 can support the adhesive layer 110. The configuration of such a sheet will be described below with reference to FIG. 1, which is a schematic diagram of a sheet according to one embodiment. In this specification, the element transfer sheet may be simply referred to as a sheet.
[0015] (Base material)
[0016] The substrate 120 functions as a support for supporting the adhesive layer 110. The substrate 120 is located on the surface of the adhesive layer 110 opposite to the surface having the irregularities.
[0017] As will be described later, the sheet according to this embodiment can be expanded. From this perspective, a flexible substrate can be used as the substrate 120. Furthermore, by using a flexible substrate as the substrate 120, it is possible to improve cushioning properties when holding elements, facilitate stacking of sheets, or form the sheet into a roll. For example, a resin film can be used as the substrate 120. The resin film is a film in which a resin-based material is used as the main material, and may be made of a resin material or may contain an additive in addition to the resin material. The resin film may be laser light transmissive.
[0018] In this embodiment, the tensile stress in the first direction of the substrate 120 at 100% elongation is higher than the tensile stress in the second direction perpendicular to the first direction. Furthermore, in this embodiment, the tensile stresses in the first and second directions of the substrate 120 at 100% elongation are sufficiently high. The tensile stress in the first direction of the substrate 120 at 100% elongation is 12 MPa or more, preferably 14 MPa or more, more preferably 18 MPa or more, and even more preferably 22 MPa or more. Furthermore, the tensile stress in the second direction of the substrate 120 at 100% elongation is 9 MPa or more, preferably 12 MPa or more, and more preferably 15 MPa or more. By using a substrate 120 having such a tensile stress, the spacing between the multiple elements held by the sheet tends to increase when the sheet is expanded. Furthermore, by using a substrate 120 having such a tensile stress, the variation in the spacing between the multiple elements held by the sheet tends to decrease when the sheet is expanded. By using such a sheet according to this embodiment, it becomes easy to selectively transfer elements held on the sheet.
[0019] On the other hand, the tensile stress in the first direction when the substrate 120 is 100% elongated is preferably 40 MPa or less, more preferably 30 MPa or less, and even more preferably 25 MPa or less. Also, the tensile stress in the second direction when the substrate 120 is 100% elongated is preferably 30 MPa or less, more preferably 25 MPa or less, and even more preferably 20 MPa or less. By not making the tensile stress of the substrate 120 too high in this way, uniform expansion of the sheet is facilitated.
[0020] Furthermore, from the viewpoint of increasing the spacing between the multiple elements held by the sheet while reducing the variation in this spacing when the sheet is expanded, the tensile stress in the first direction at 100% elongation of the substrate 120 is preferably 12 MPa or more, more preferably 14 MPa or more, while preferably 40 MPa or less, and more preferably 16 MPa or less. From the same viewpoint, the tensile stress in the second direction at 100% elongation of the substrate 120 is preferably 9 MPa or more, more preferably 10 MPa or more, and even more preferably 10.5 MPa or more, while preferably 30 MPa or less, more preferably 15 MPa or less, and even more preferably 12 MPa or less.
[0021] The first direction may be the direction in which the tensile stress is highest. The first direction may also be the MD direction. MD in the MD direction is an abbreviation for Machine Direction, and for example, the MD direction of the substrate means the longitudinal direction during the manufacture of the substrate. On the other hand, the second direction may be the direction in which the tensile stress is lowest. The second direction may also be the TD direction. TD in the TD direction is an abbreviation for Transverse Direction, and for example, the TD direction of the substrate means the width direction during the manufacture of the substrate. In this way, the MD direction and the TD direction are perpendicular to each other. In addition, in this specification, the tensile stress is measured as shown in the examples.
[0022] The inventors of the present application believe that by increasing the tensile stress of the substrate 120 as described above, the force that the elements receive when the sheet is expanded increases, resulting in an increase in the spacing between the elements and a decrease in spacing variation. The tensile stress of the substrate 120 can be adjusted, for example, by selecting the resin material or combination of resin materials that make up the substrate 120, or by adding additives. Furthermore, when a copolymer is used as the material for the substrate 120, the tensile stress of the substrate 120 can be adjusted by selecting the combination or ratio of the constituent units.
[0023] In addition, by increasing the tensile stress of the substrate 120 as in this embodiment, even if there is a difference between the tensile stress in the first direction and the tensile stress in the second direction of the substrate 120, it is possible to reduce the variation in the spacing between the multiple elements held by the sheet. Furthermore, in this embodiment, the unevenness of the adhesive layer 110 on the substrate 120 is also thought to contribute to reducing the variation in spacing in such cases. From this perspective, the absolute value of the difference between the tensile stress in the first direction and the tensile stress in the second direction when the substrate 120 is 100% elongated may be 2.0 MPa or more, 3.0 MPa or more, or 4.0 MPa or more.
[0024] Specific examples of resin films include polyethylene films such as low-density polyethylene (LDPE) film, linear low-density polyethylene (LLDPE) film, and high-density polyethylene (HDPE) film; polyolefin films such as polypropylene film, polybutene film, polybutadiene film, poly(4-methyl-1-pentene) film, ethylene-norbornene copolymer film, and norbornene resin film; ethylene copolymer films such as ethylene-vinyl acetate copolymer film, ethylene-(meth)acrylic acid copolymer film, and ethylene-(meth)acrylic acid ester copolymer film; polyvinyl chloride films such as polyvinyl chloride film and vinyl chloride copolymer film; polyester films such as polyethylene terephthalate film and polybutylene terephthalate film; polyurethane film; polyimide film; polystyrene film; polycarbonate film; and fluororesin films. Films containing a mixture of two or more materials, crosslinked films in which the resins forming these films are crosslinked, and modified films such as ionomer films may also be used. Furthermore, the substrate 120 may be a laminate film in which two or more resin films are laminated.
[0025] From the viewpoint of facilitating sheet expansion, the substrate 120 is preferably a polyolefin film or a vinyl chloride copolymer film. Examples of polyolefin films include polyethylene films, polypropylene films, and copolymers containing unsubstituted olefins such as ethylene or propylene as structural units, such as ethylene-based copolymers containing ethylene-methacrylic acid copolymer (EMAA). Examples of vinyl chloride copolymer films include vinyl chloride-vinylidene chloride copolymer films, vinyl chloride-vinyl acetate copolymer films, and vinyl chloride-ethylene copolymer films. The form of such copolymers is not particularly limited and may be any of block copolymers, random copolymers, alternating copolymers, and graft copolymers. These films may also contain other resin components or additives.
[0026] The thickness of the substrate 120 is not particularly limited, but from the viewpoint of achieving both supportability and roll winding properties, it is preferably 10 μm or more, more preferably 25 μm or more, and even more preferably 40 μm or more, while it is preferably 500 μm or less, more preferably 200 μm or less, even more preferably 150 μm or less, still more preferably 150 μm or less, even more preferably 120 μm or less, and particularly preferably 90 μm or less.
[0027] To facilitate uniform expansion of the sheet, the tensile modulus of the substrate 120 is preferably 50 MPa or more, more preferably 80 MPa or more, even more preferably 120 MPa or more, and is preferably 2500 MPa or less, more preferably 1000 MPa or less, even more preferably 500 MPa or less. In this specification, the tensile modulus is measured in accordance with JIS K7161-1:2014.
[0028] Similarly, to facilitate expansion of the sheet, the breaking elongation of the substrate 120 is preferably 105% or more, more preferably 150% or more, and even more preferably 200% or more. In this specification, the breaking elongation is measured in accordance with JIS K 7127:1999.
[0029] (Adhesive Layer) The adhesive layer 110 is a layer having adhesive properties and may contain a resin. As described above, the adhesive layer 110 has an uneven surface. The sheet may have two or more adhesive layers 110. For example, the sheet may have a laminate of one type or two or more types of adhesive layers 110.
[0030] (Composition of Adhesive Layer) Examples of resins contained in the adhesive layer 110 include rubber-based resins such as polyisobutylene-based resins, polybutadiene-based resins, and styrene-butadiene-based resins, acrylic-based resins, urethane-based resins, polyester-based resins, olefin-based resins, silicone-based resins, and polyvinyl ether-based resins. The adhesive layer may be heat-resistant, and examples of materials for the adhesive layer 110 that have such heat resistance include polyimide-based resins and silicone-based resins. The adhesive layer 110 may contain a copolymer having two or more types of structural units. The form of such a copolymer is not particularly limited, and may be any of a block copolymer, a random copolymer, an alternating copolymer, and a graft copolymer.
[0031] The resin contained in the adhesive layer 110 is preferably an adhesive resin that exhibits adhesiveness by itself. The resin is preferably a polymer having a mass average molecular weight (Mw) of 10,000 or more. From the viewpoint of improving retention, the mass average molecular weight (Mw) of the resin is preferably 10,000 or more, more preferably 70,000 or more, and even more preferably 140,000 or more. From the viewpoint of suppressing the storage modulus to a predetermined value or less, the mass average molecular weight (Mw) of the resin is preferably 2,000,000 or less, and even more preferably 1,200,000 or less. From the viewpoint of improving retention, the number average molecular weight (Mn) of the resin is preferably 10,000 or more, more preferably 50,000 or more, and even more preferably 100,000 or more. From the viewpoint of suppressing the storage modulus to a predetermined value or less, the number average molecular weight (Mn) of the resin is preferably 2,000,000 or less, more preferably 1,500,000 or less, and even more preferably 1,200,000 or less. As described below, when the adhesive layer 110 contains a resin derived from an energy reactive resin, the mass average molecular weight (Mw) and number average molecular weight (Mn) refer to the mass average molecular weight (Mw) and number average molecular weight (Mn) before the crosslinking reaction due to energy application. The glass transition temperature (Tg) of the resin is preferably −75° C. or higher, more preferably −70° C. or higher, and preferably 5° C. or lower, more preferably −20° C. or lower. When Tg is within this range, the retention properties and storage modulus of the obtained adhesive layer 110 can be easily set within the ranges described below.
[0032] The amount of resin contained in the adhesive layer 110 relative to the total amount of components constituting the adhesive layer 110 can be set appropriately depending on the desired retention and storage modulus of the adhesive layer 110, but is preferably 30% by mass or more, more preferably 50% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and is preferably 99.99% by mass or less, more preferably 99.95% by mass or less, even more preferably 99.90% by mass or less, even more preferably 99.80% by mass or less, and even more preferably 99.50% by mass or less.
[0033] The storage modulus of the adhesive layer 110 is preferably 0.001 MPa or more, more preferably 0.01 MPa or more, even more preferably 0.03 MPa or more, and even more preferably 0.07 MPa or more, from the viewpoint of the morphological stability of the uneven shape of the adhesive layer surface. On the other hand, a low storage modulus of the adhesive layer 110 is preferable in that it can suppress misalignment when holding an element. From this viewpoint, the storage modulus of the adhesive layer 110 is preferably 100 MPa or less, more preferably 50 MPa or less, even more preferably 20 MPa or less, and particularly preferably 5 MPa or less. In this specification, the storage modulus is measured in accordance with JIS K7244-1:1998. Specifically, the storage modulus of the adhesive layer 110 can be measured by preparing a cylindrical sample having a thickness of 3 mm and a diameter of 8 mm, and measuring the storage modulus of the sample using a viscoelasticity measuring device by a torsional shear method at 1 Hz and 23°C.
[0034] In one embodiment, the resin contained in the adhesive composition forming the adhesive layer 110 may include a thermoplastic resin. That is, the adhesive layer 110 may be formed from a thermoplastic resin. When a thermoplastic resin is used, it becomes easy to form irregularities in the adhesive layer 110 by heating and softening the resin, and it also becomes easy to maintain the irregular shape formed by cooling. Examples of thermoplastic resins include rubber-based resins, acrylic-based resins, urethane-based resins, and olefin-based resins. Examples include polybutadiene-based thermoplastic elastomers using butadiene as a monomer, styrene-based thermoplastic elastomers using styrene as a monomer, and acrylic-based thermoplastic elastomers using (meth)acrylic acid or a (meth)acrylic acid ester as a monomer.
[0035] The following describes examples of the composition of the adhesive layer 110. However, the composition of the adhesive layer 110 is not limited to the following.
[0036] (Acrylic Resin (A)) In one embodiment, the pressure-sensitive adhesive composition forming the pressure-sensitive adhesive layer 110 contains an acrylic resin. The acrylic resin is a resin containing (meth)acrylic acid or a (meth)acrylic acid ester as a monomer. From the viewpoint of improving adhesive strength, the mass average molecular weight (Mw) of the acrylic resin is preferably 10,000 or more, more preferably 100,000 or more, and even more preferably 500,000 or more. Furthermore, from the viewpoint of suppressing the storage modulus to a predetermined value or less, the mass average molecular weight (Mw) is preferably 2,000,000 or less, more preferably 1,500,000 or less, and even more preferably 1,200,000 or less.
[0037] The glass transition temperature (Tg) of the acrylic resin is preferably −75° C. or higher, more preferably −70° C. or higher, and preferably 5° C. or lower, more preferably −20° C. or lower. When the Tg is within this range, it becomes easier to obtain adhesive layer 110 having the above-mentioned storage modulus.
[0038] When an acrylic resin has two or more structural units, the glass transition temperature (Tg) of the acrylic resin can be calculated using the Fox equation. The Tg of the monomer from which the structural unit is derived can be calculated using the value listed in the Polymer Data Handbook or the Adhesive Handbook.
[0039] Examples of (meth)acrylic acid esters constituting acrylic resins include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isooctyl (meth)acrylate. The alkyl group constituting the alkyl ester has a chain structure having 1 to 18 carbon atoms (methacrylate), such as acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, myristyl (meth)acrylate, pentadecyl (meth)acrylate, palmityl (meth)acrylate, heptadecyl (meth)acrylate, and stearyl (meth)acrylate. (meth)acrylic acid alkyl esters; (meth)acrylic acid cycloalkyl esters such as isobornyl (meth)acrylate and dicyclopentanyl (meth)acrylate; (meth)acrylic acid aralkyl esters such as benzyl (meth)acrylate; (meth)acrylic acid cycloalkenyl esters such as dicyclopentenyl (meth)acrylate; (meth)acrylic acid cycloalkenyloxyalkyl esters such as dicyclopentenyloxyethyl (meth)acrylate; imide (meth)acrylates; glycidyl (meth)acrylate and other glycidyl (meth)acrylates. Examples of the acrylate include ricidyl group-containing (meth)acrylic acid esters; hydroxyl group-containing (meth)acrylic acid esters such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and substituted amino group-containing (meth)acrylic acid esters such as N-methylaminoethyl (meth)acrylate.Here, the term "substituted amino group" refers to a group having a structure in which one or two hydrogen atoms of an amino group are substituted with a group other than a hydrogen atom.
[0040] The acrylic resin may be, for example, a resin obtained by copolymerizing one or more monomers selected from the group consisting of (meth)acrylic acid esters or (meth)acrylic acid, itaconic acid, vinyl acetate, acrylonitrile, styrene, and N-methylolacrylamide.
[0041] The acrylic resin may be composed of one kind of monomer or two or more kinds of monomers, and when two or more kinds of monomers are used, the combination and ratio thereof can be selected arbitrarily.
[0042] In one embodiment, the acrylic resin contains a monomer having a hydroxyl group as a constituent unit. The acrylic resin may also have functional groups capable of bonding to other compounds, such as vinyl groups, (meth)acryloyl groups, amino groups, carboxy groups, and isocyanate groups, in addition to the hydroxyl groups. These functional groups, including the hydroxyl groups of the acrylic resin, may bond to other compounds via a crosslinking agent (C) described below, or may bond directly to other compounds without the crosslinking agent (C).
[0043] The amount of acrylic resin in the total amount of resin in the adhesive composition can be set appropriately depending on the desired adhesive strength and storage modulus of the adhesive layer 110, but is preferably 0% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, even more preferably 50% by mass or more, and is preferably 100% by mass or less, more preferably 95% by mass or less, even more preferably 80% by mass or less, even more preferably 60% by mass or less.
[0044] (Energy Reactive Resin (B)) In one embodiment, the pressure-sensitive adhesive composition forming the pressure-sensitive adhesive layer 110 contains an energy reactive resin (B). The energy reactive resin (B) refers to a resin whose elastic modulus improves upon application of energy. The energy reactive resin may be a resin derived from an energy-reactive monomer. In this case, the energy reactive resin is a resin obtained by polymerizing the energy-reactive monomer by application of energy.
[0045] Examples of energy reactive resins include energy ray reactive resins and heat reactive resins. Energy ray reactive resins refer to resins whose elastic modulus improves when irradiated with energy rays. For example, energy reactive resins can be energy ray curable resins. Heat reactive resins refer to resins whose elastic modulus improves when heated. The resin contained in the adhesive layer 110 is more preferably derived from a thermoplastic energy reactive resin, and even more preferably derived from a thermoplastic energy ray reactive resin. The type of energy ray is not particularly limited, and examples include ultraviolet rays, electron beams, and ionizing radiation. Preferred energy rays are ultraviolet rays, i.e., the resin is preferably an ultraviolet reactive resin.
[0046] A thermoplastic energy reactive resin refers to an energy reactive resin that has thermoplastic properties at least before energy is applied. Furthermore, a resin derived from an energy reactive resin means that the resin is obtained from an energy reactive resin. For example, a resin derived from an energy reactive resin is a crosslinked energy reactive resin.
[0047] When such an energy reactive resin is used, the formed uneven shape can be easily maintained by providing energy (for example, by irradiating with energy rays) after forming the unevenness in the resin.
[0048] Such energy reactive resins can be polymers having polymerizable functional groups introduced therein. The polymerizable functional groups are functional groups that are crosslinked by the application of energy (e.g., irradiation with energy rays). Examples of such polymerizable functional groups include alkenyl groups such as vinyl groups and allyl groups, (meth)acryloyl groups, oxetanyl groups, and epoxy groups.
[0049] For example, a diene rubber composed of a polymer having a polymerizable functional group at the end of the main chain and / or at a side chain can be used as the energy reactive resin. Diene rubber refers to a rubbery polymer having a double bond in the polymer main chain. Specific examples of diene rubber include polymers using butadiene or isoprene as a monomer (i.e., having butenediyl groups or pentenediyl groups as structural units). Preferred examples of the energy reactive resin include polybutadiene resin (PB resin), styrene-butadiene-styrene block copolymer (SBS resin), and styrene-isoprene-styrene block copolymer. These resins can be used as ultraviolet-reactive resins.
[0050] The average number of polymerizable functional groups per molecule in these energy reactive resins is preferably 1.5 or more, more preferably 2 or more, from the viewpoint of easily maintaining the uneven shape of the adhesive layer 110. On the other hand, from the viewpoint of improving the adhesiveness and flexibility of the adhesive layer 110, this average value is preferably 20 or less, more preferably 15 or less, and even more preferably 10 or less.
[0051] The adhesive layer 110 may contain one type of resin or two or more types of resins. In one embodiment, the adhesive layer 110 contains a liquid resin, a resin derived from an energy-reactive liquid resin, or a resin derived from an energy-reactive monomer, in addition to a thermoplastic resin or a resin derived from a thermoplastic energy-reactive resin. The liquid resin refers to a resin that is liquid at room temperature (25°C) before mixing. The energy-reactive liquid resin refers to an energy-reactive resin that is liquid at room temperature (25°C) before mixing and before energy is applied. The resin derived from an energy-reactive monomer refers to a resin obtained by polymerizing an energy-reactive monomer by applying energy. Adding such a liquid resin or monomer makes it easier to control the retention and storage modulus of the adhesive layer 110.
[0052] It is preferable that adhesive layer 110 according to an embodiment contains a resin derived from an energy reactive liquid resin, since it is easy to maintain the uneven shape of adhesive layer 110. An example of such a liquid resin is a diene rubber, and a specific example is a polybutadiene resin in which butadiene is used as a monomer.
[0053] According to another embodiment, the adhesive layer 110 includes a combination of any resin and an energy-reactive liquid resin or a resin derived from an energy-reactive monomer. For example, the adhesive layer 110 may include an acrylic resin (A) and an energy-reactive liquid resin or a resin derived from an energy-reactive monomer. Even with this combination, by forming irregularities on a film of a mixture of the acrylic resin (A) and the energy-reactive liquid resin or the energy-reactive monomer and then applying energy (e.g., irradiating with energy rays), the energy-reactive liquid resin or the energy-reactive monomer is polymerized, making it easy to maintain the irregularities that have been formed.
[0054] Examples of energy-reactive monomers include bifunctional or polyfunctional compounds incorporating polymerizable functional groups such as alkenyl groups (e.g., vinyl groups and allyl groups), (meth)acryloyl groups, oxetanyl groups, and epoxy groups. Preferred examples of energy-reactive monomers include polyvalent (meth)acrylates, such as difunctional (meth)acrylates. Thus, the adhesive layer 110 can include an energy-ray-curable resin containing a polyvalent (meth)acrylate as a structural unit. Specific examples of polyvalent (meth)acrylates include cycloalkyl di(meth)acrylates, such as tricyclodecane dimethanol diacrylate.
[0055] Furthermore, the ratio of the energy reactive resin (B) to the total amount of components constituting the adhesive layer 110 can be selected depending on the desired retention and storage modulus of the adhesive layer 110. For example, this ratio is preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 8% by mass or more, and even more preferably 10% by mass or more, and is preferably 30% by mass or less, and more preferably 25% by mass or less.
[0056] Furthermore, when the adhesive layer 110 contains an acrylic resin (A) and an energy reactive resin (B), the amount of the energy reactive resin relative to the acrylic resin can be selected depending on the desired retention and storage modulus of the adhesive layer 110. For example, the amount of the energy reactive resin relative to 100 parts by mass of the acrylic resin is preferably 1 part by mass or more, more preferably 5 parts by mass or more, even more preferably 8 parts by mass or more, particularly preferably 10 parts by mass or more, and preferably 30 parts by mass or less, more preferably 25 parts by mass or less. In this case, the energy reactive resin is, for example, an energy ray-curable resin, such as a resin derived from an energy ray-curable monomer. Here, parts by mass are based on the mass of the solid content, and hereinafter also based on mass unless otherwise specified.
[0057] (Other Components of Adhesive Layer) The adhesive composition forming the adhesive layer 110 may contain components other than the resin. For example, the adhesive composition may contain one or more of a crosslinking agent (C), a photopolymerization initiator (D), and other additives.
[0058] Examples of the crosslinking agent (C) include an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, an aziridine-based crosslinking agent, a metal chelate-based crosslinking agent, etc. These crosslinking agents may be used alone or in combination of two or more.
[0059] Among these crosslinking agents, isocyanate-based crosslinking agents are preferred from the viewpoints of increasing cohesive strength and improving adhesive strength, ease of availability, etc. Examples of the isocyanate-based crosslinking agent include polyvalent isocyanate compounds such as aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate; alicyclic polyisocyanates such as dicyclohexylmethane-4,4'-diisocyanate, bicycloheptane triisocyanate, cyclopentylene diisocyanate, cyclohexylene diisocyanate, methylcyclohexylene diisocyanate, methylenebis(cyclohexyl isocyanate), 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate, and hydrogenated xylylene diisocyanate; and acyclic aliphatic polyisocyanates such as hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, and lysine diisocyanate. Further, examples of the isocyanate crosslinking agent include a trimethylolpropane adduct modified product of the polyisocyanate compound, a biuret modified product obtained by reacting the polyisocyanate compound with water, and an isocyanurate modified product containing an isocyanurate ring.
[0060] The pressure-sensitive adhesive composition may contain one type of crosslinking agent or may contain two or more types of crosslinking agents. From the viewpoint of appropriately carrying out the crosslinking reaction, the content of the crosslinking agent in the pressure-sensitive adhesive composition is preferably 0.01 mass% or more, more preferably 0.1 mass% or more, even more preferably 0.5 mass% or more, particularly preferably 0.8 mass% or more, and preferably 5 mass% or less, more preferably 4 mass% or less, even more preferably 2 mass% or less.
[0061] For example, the crosslinking agent may be a crosslinking agent for the acrylic resin (A). For example, an isocyanate-based crosslinking agent of an isocyanurate-type modified compound can be used as a crosslinking agent for an acrylic resin containing a monomer having a hydroxyl group as a constituent unit. In this case, the amount of crosslinking agent relative to the acrylic resin can be selected so that the crosslinking reaction can be carried out appropriately. For example, the amount of crosslinking agent relative to 100 parts by mass of the acrylic resin is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 0.5 parts by mass or more, particularly preferably 1.0 parts by mass or more, and preferably 5 parts by mass or less, more preferably 4 parts by mass or less, and even more preferably 2 parts by mass or less.
[0062] The photopolymerization initiator (D) initiates a crosslinking reaction in response to the application of energy (e.g., irradiation with energy rays). When the pressure-sensitive adhesive composition contains the energy reactive resin (B), the pressure-sensitive adhesive layer 110 further contains the photopolymerization initiator (D), and thus the crosslinking reaction proceeds even when a relatively low amount of energy is applied.
[0063] Examples of the photopolymerization initiator (D) include 1-hydroxycyclohexyl phenyl ketone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzyl phenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, dibenzyl, diacetyl, 8-chloroanthraquinone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.
[0064] The pressure-sensitive adhesive composition may contain one type of polymerization initiator or two or more types of polymerization initiators. The content of the photopolymerization initiator in the pressure-sensitive adhesive composition is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 2% by mass or less.
[0065] Other additives that may be contained in the adhesive layer 110 are not particularly limited, but include, for example, ultraviolet absorbers such as benzotriazole-based compounds, oxazolic acid amide compounds, or benzophenone-based compounds; light stabilizers such as hindered amine-based, benzophenone-based, or benzotriazole-based compounds; resin stabilizers such as imidazole-based resin stabilizers, dithiocarbamate-based resin stabilizers, phosphorus-based resin stabilizers, or sulfur ester-based resin stabilizers; antioxidants such as phenol-based compounds such as hindered phenol-based compounds, aromatic amine-based compounds, sulfur-based compounds, or phosphorus-based compounds such as phosphate ester-based compounds, fillers, pigments, extenders, and softeners.
[0066] When the adhesive layer 110 contains these additives, the content of the additives in the adhesive layer 110 is preferably 0.0001% by mass or more, more preferably 0.01% by mass or more, particularly preferably 0.1% by mass or more, even more preferably 1% by mass or more, and preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less.
[0067] (Shape of Adhesive Layer) The surface of the adhesive layer 110 according to this embodiment has projections and depressions. In one embodiment, the adhesive layer 110 has a plurality of projections on its surface that are spaced apart and bounded by depressions. Each of the projections may be spaced apart by a depression that is continuous across the entire adhesive layer 110.
[0068] 2A-B are side views showing the shape of the adhesive layer 110, and FIGS. 3A-C are top views showing the shape of the adhesive layer 110. FIGS. 2A and 3A show an example of the adhesive layer 110 before expansion, and FIGS. 2B and 3B show an example of the adhesive layer 110 after expansion. In addition, while FIGS. 2A-B depict the element 140 held by the convex portions 111 of the adhesive layer 110, FIGS. 3A-C omit the element 140 held by the convex portions 111.
[0069] As shown in Figures 2A and 3A, the protrusions 111 may be regularly arranged on the surface of the adhesive layer 110. Regularly arranging the protrusions means that the protrusions are lined up in a straight line at regular intervals. On the other hand, the protrusions 111 may be arranged so that the intervals between them vary regularly. For example, the intervals between the protrusions may be short in the center of the sheet and long in the peripheral area of the sheet. Furthermore, the protrusions may be arranged irregularly.
[0070] 3C is a top view showing another shape of the adhesive layer 110. As shown in FIG. 3C, stripe-shaped convex portions 111 may be provided on the surface of the adhesive layer 110. In FIG. 3C, linear convex portions 111 having a constant width are arranged at regular intervals. The width or interval of these linear convex portions 111 may vary regularly, or the linear convex portions 111 may be arranged irregularly.
[0071] In this embodiment, the sheet is expanded, and the adhesive layer 110 shown in Figures 2A and 3A is transformed into the adhesive layer 110' shown in Figures 2B and 3B. Comparing the adhesive layer 110 and the adhesive layer 110', the pitch P of each convex portion 111 in the adhesive layer 110' has been increased due to the expansion, and the number of convex portions 111 that hold one element 140 has been reduced. As a result, in the adhesive layer 110', the force with which the convex portions 111 hold the element 140 is reduced compared to the adhesive layer 110.
[0072] The pitch P of the convex portions 111 before expansion is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, and even more preferably 15 μm or more, from the viewpoint of adjusting the holding force. On the other hand, from the viewpoint of increasing the contact area between the adhesive layer 110 and the element and thereby increasing the holding force, this pitch P is preferably 100 μm or less, more preferably 75 μm or less, even more preferably 50 μm or less, even more preferably 35 μm or less, and even more preferably 25 μm or less. Here, the pitch P of the convex portions 111 refers to the distance between the center point of one arbitrarily selected convex portion 111 and the center point of another convex portion 111 closest to that convex portion 111. For example, in the case of FIG. 2A, the pitch P of the convex portions 111 represents the distance between the center point of the convex portion 111 on a straight line on which the convex portions 111 are arranged at regular intervals and the center point of another convex portion 111 closest to that convex portion 111. When the convex portions 111 are arranged on a plurality of straight lines, the pitch P represents the distance between the center points of the convex portions on the straight line on which the convex portions 111 are arranged at the shortest pitch. In this specification, the spacing between the convex portions 111 means the spacing between the centers of the convex portions.
[0073] The specific shape of the protrusions 111 is not particularly limited. For example, the protrusions 111 may have a pillar (column) shape. As a specific example, the protrusions 111 may have a cylindrical shape or a prismatic shape. Furthermore, as described above, the protrusions 111 may extend in a line shape, or may extend in a curved shape such as a wavy shape. Furthermore, these protrusions 111 may be tapered.
[0074] 4A shows a cross-sectional view of an adhesive layer 110 according to one embodiment, taken perpendicular to the surface of the adhesive layer 110 and passing through a protruding portion 111. The protruding portion 111 shown in FIG. 4A is tapered, i.e., the protruding portion 111 is tapered. Furthermore, as shown in FIG. 4B, the tip of the protruding portion 111 may be curved. This configuration further reduces the impact when the adhesive layer 110 holds the element, making it easier for the adhesive layer 110 to hold the element without slipping. Alternatively, the tip of the protruding portion may be flat.
[0075] 4A, the surface of the adhesive layer 110 may have flat recesses and protruding portions 111 protruding from the recesses. In this manner, the adhesive layer 110 has a plurality of protruding portions 111 that are spaced apart from one another and may be bounded by the recesses.
[0076] As another example, the convex portions may be hemispherical or partial spheres as shown in Figure 4B. Furthermore, the convex portions 111 may be T-shaped as shown in Figure 4C. As yet another example, the convex portions 111 may have a shape of a collection of particles, a mushroom shape, the surface of a lotus leaf, or a needle shape. As yet another example, the surface of the adhesive layer 110 may be rough or fibrous, and such a surface may also be said to have irregularities.
[0077] From the viewpoint of maintaining the holding force of the element, the width or diameter of each protrusion 111 is preferably 1 μm or more, more preferably 2 μm or more, even more preferably 5 μm or more, and even more preferably 10 μm or more. On the other hand, from the viewpoint of improving the ease of peeling the element, the width or diameter is preferably 100 μm or less, more preferably 50 μm or less, even more preferably 30 μm or less, and even more preferably 20 μm or less. Here, the width and diameter of the protrusion 111 refer to the minimum distance and maximum distance (represented by D in FIG. 4A ) between two parallel lines that contact the protrusion 111 from both sides on the surface of the recess.
[0078] In addition, the area of each of the protrusions 111 is preferably 10 μm from the viewpoint of maintaining the holding force of the element. 2 More preferably, 20 μm or more 2 More preferably, 30 μm or more 2 On the other hand, from the viewpoint of increasing the ease of peeling off the element, it is preferable that the thickness is 2000 μm. 2 Less than 1000 μm, more preferably 2 More preferably, 500 μm or less 2 Here, the area of the convex portion 111 means the area of the portion protruding from the surface of the concave portion (the area of a circle with a diameter D in the case of FIG. 4A).
[0079] In one embodiment, the height of each protrusion 111 is preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more, from the viewpoint of improving the ease of peeling of the element. On the other hand, from the viewpoint of improving dimensional stability, the height of each protrusion 111 is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less. This allows the element's holding power to be changed. Here, the height of the protrusion 111 is represented by H in FIG. 4A. Also, in one embodiment, the heights of the multiple protrusions in the adhesive layer 110 are uniform. In another embodiment, the adhesive layer 110 may have a first multiple protrusions having a first uniform height and a second multiple protrusions having a different height. Here, the second multiple protrusions may have a second uniform height. For example, the protrusions 111 may be composed of such first protrusions and second protrusions. In a further embodiment, the adhesive layer 110 may have multiple protrusions of random heights.
[0080] Furthermore, the total area of the protrusions 111 relative to the area of the adhesive layer 110 is preferably 1% or more, more preferably 5% or more, even more preferably 10% or more, even more preferably 18% or more, and even more preferably 40% or more, from the viewpoint of maintaining the holding force of the element. On the other hand, the total area of the protrusions relative to the area of the adhesive layer 110 is preferably 95% or less, more preferably 75% or less, and even more preferably 60% or less, from the viewpoint of improving the ease of peeling the element.
[0081] The unevenness of the adhesive layer 110 may be designed according to the shape of the element held by the sheet. For example, the ratio of the adhesive area between the adhesive layer 110 and one element to the area of one element is preferably 1% or more, more preferably 2% or more, even more preferably 3% or more, even more preferably 4% or more, even more preferably 5% or more, even more preferably 7% or more, and even more preferably 10% or more, relative to the area of one element (100%), from the viewpoint of maintaining the holding force of the element. On the other hand, the ratio of the adhesive area between the adhesive layer 110 and one element to the area of one element is preferably 95% or less, more preferably 70% or less, even more preferably 50% or less, and even more preferably 30% or less, from the viewpoint of improving the ease of peeling the element. In the case of FIG. 4A, the adhesive area corresponds to the area of a circle with a diameter T. Note that the adhesive area may change if the holding position of the element on the sheet is shifted. In this case, it is preferable that the adhesive area ratio falls within the above range, regardless of the position of the workpiece.
[0082] (Release Sheet) Furthermore, as shown in Fig. 1 , the element transfer sheet according to this embodiment may include a release sheet 150 that is in contact with the adhesive layer 110 and has an uneven surface that is complementary to the uneven surface of the adhesive layer 110. For the sake of explanation, Fig. 1 shows a state in which the adhesive layer 110 and the release sheet 150 are separated.
[0083] The release sheet 150 has a release layer 160. The release layer 160 is a layer that is easily peelable from the adhesive layer 110. The release layer 160 may have an uneven surface that is complementary to the uneven surface of the adhesive layer 110. That is, the release layer 160 has recesses 161, and the recesses 161 have a shape that is complementary to the protrusions 111. However, it is not essential that the recesses 161 have a shape that is complementary to the protrusions 111.
[0084] The release sheet 150 may have a substrate 170 on the surface that does not contact the adhesive layer 110. This substrate 170 can be designed similarly to the substrate 120, but does not need to have the same composition or structure as the substrate 120. For example, the material of the substrate 120 may be EMAA, and the material of the substrate 170 may be polyethylene terephthalate. Furthermore, the release sheet 150 may have an undercoat layer (not shown) between the release layer 160 and the substrate 170.
[0085] (Other Layers) The above sheet may have layers other than the substrate and the adhesive layer. For example, an additional adhesive layer may be provided on the surface of the substrate opposite to the adhesive layer. The sheet can be attached to another object via such an adhesive layer. The type of the additional adhesive layer is not particularly limited, and for example, the additional adhesive layer can be formed using a general adhesive.
[0086] (Characteristics of Element Transfer Sheet) From the viewpoint of suppressing misalignment when holding an element, the adhesive strength of the element transfer sheet is preferably 1 mN / 50 mm or more, more preferably 5 mN / 50 mm or more, even more preferably 10 mN / 50 mm or more, even more preferably 15 mN / 50 mm or more, and even more preferably 20 mN / 50 mm or more. From the viewpoint of peeling the held element from the adhesive layer 110 without damaging it, it is preferably 1000 mN / 50 mm or less, more preferably 500 mN / 50 mm or less, even more preferably 100 mN / 50 mm or less, and even more preferably 50 mN / 50 mm or less. In this specification, adhesive strength is measured as follows. That is, the element transfer sheet is cut into a size of 200 mm long x 50 mm wide, and the surface of the adhesive layer is pressed onto the mirror surface of a mirror silicon wafer using a laminator. After pressing, the sheet is left to stand for 1 hour in an environment of 23 ° C. and 50% RH (relative humidity) to prepare an adhesive strength measurement sample. The adhesive strength of the adhesive strength measurement sample thus prepared is measured using a tensile tester (manufactured by A&D Co., Ltd., product name "Tensilon (registered trademark)") under an environment of 23°C and 50% RH (relative humidity) at a peel angle of 180° and a pulling speed of 300 mm / min, in accordance with JIS Z0237:2000, except for the measurement conditions described above.
[0087] (Expansion of element transfer sheet) The expansion of the element transfer sheet will be described below. As described above, the element transfer sheet can be expanded in the surface direction while holding the elements. The method of expanding the sheet is not particularly limited. For example, the sheet may be expanded in one direction, two directions, or multiple other directions.
[0088] The expansion rate of the element transfer sheet is not particularly limited. Increasing the expansion amount tends to increase the spacing between elements after expansion. For example, the expansion rate of the sheet in one direction may be 50% or more, 100% or more, 150% or more, or 250% or more. Furthermore, the expansion rates of the sheet in two mutually perpendicular directions may be 50% or more, at least 100% or more, 150% or more, or 250% or more.
[0089] As a specific example, the sheet can be expanded by fixing the sheet to a frame and pressing a base against the sheet inside the frame. Such an example will be described with reference to FIGS. 5A and 5B. FIG. 5A shows a state in which the sheet holds elements 140a to 140d. As shown in FIG. 5A, the outer periphery of the sheet can be fixed to a frame 320. The shape of the frame 320 is not particularly limited. For example, the frame 320 may be a circular or rectangular frame-shaped member having an opening. In one embodiment, a circular ring frame is used as the frame. Using a ring frame allows the sheet to be expanded in all directions.
[0090] The sheet fixed to the frame 320 can be expanded by contacting the base 310 and then displacing (pulling down) the frame 320 toward the base 310 as shown in FIG. 5B . Furthermore, as the sheet expands, the spacing between the elements 140a-140d held by the sheet increases. The configuration of the base 310 is not particularly limited, and may be, for example, cylindrical or rectangular. The base 310 may also be mesh-shaped or ring-shaped. The frame 320 may be displaced relative to the base 310 at a speed of, for example, 0.1 mm / sec or more, or 1 mm / sec or more. In this case, the displacement amount of the frame 320, i.e., the pull-down amount, may be, for example, 20 mm or more, or 50 mm or more.
[0091] As described above, according to this embodiment, when the element transfer sheet is expanded while holding multiple elements, the spacing between the elements becomes larger. In one embodiment, multiple elements are formed by dicing the wafer substrate held by the adhesive layer 110. Then, when the element transfer sheet is expanded by 80 mm in a first direction and a second direction perpendicular to each other, the average spacing between the multiple elements is preferably 2.5 mm or more, more preferably 3.0 mm or more, even more preferably 3.5 mm or more, even more preferably 4.0 mm or more, and particularly preferably 5.0 mm or more. Here, the spacing between the multiple elements refers to the distance between adjacent elements. Furthermore, the average spacing between the multiple elements corresponds to the average value for a data group including the spacing between all pairs of adjacent elements in the first direction and the spacing between all pairs of adjacent elements in the second direction.
[0092] As a specific example, by pulling down frame 320 by 80 mm relative to base 310, the element transfer sheet can be expanded by 80 mm in a first direction and a second direction that are perpendicular to each other. For such measurements, a ring frame with an inner diameter of 194 mm can be used as frame 320. Furthermore, a cylindrical member with a diameter slightly smaller than the inner diameter of frame 320 can be used as base 310. As described above, expanding the transfer sheet by 80 mm in the first direction and the second direction that are perpendicular to each other can be achieved by pulling down such frame 320 by 80 mm relative to base 310. In this case, the element transfer sheet can be expanded by approximately 180% ((194 + 80 + 80) / 194 = approximately 180%).
[0093] Furthermore, according to this embodiment, when the element transfer sheet is expanded while holding multiple elements, the spacing between the elements becomes more uniform. In one embodiment, multiple elements are formed by dicing the wafer substrate held by the adhesive layer 110. The coefficient of variation of the spacing between the multiple elements when the element transfer sheet is then expanded 180% in the first and second directions perpendicular to each other is preferably 0.20 or less, and more preferably 0.15 or less. Here, the coefficient of variation is expressed by the mean value / standard deviation. The mean value of the spacing between the multiple elements is defined as above. The standard deviation of the spacing between the multiple elements corresponds to the standard deviation for a data group including the spacing between all pairs of adjacent elements in the first direction and the spacing between all pairs of adjacent elements in the second direction. In such measurements, as described above, approximately 180% expansion can be achieved by pulling the frame 320, which has an inner diameter of 194 mm, down 80 mm from the base 310.
[0094] (Method for manufacturing adhesive layer and sheet) There are no particular limitations on the method for manufacturing the adhesive layer and sheet. For example, a sheet having an adhesive layer 110 provided on a substrate 120 can be produced as follows. First, an organic solvent is added to a raw material composition containing each of the components of the adhesive layer 110 described above to prepare a solution of the raw material composition. This solution is then applied to the substrate 120 to form a coating film, which is then dried, thereby providing an adhesive layer on the substrate 120. Furthermore, by performing a process to provide irregularities on the surface of this adhesive layer, an adhesive layer 110 having irregularities can be formed.
[0095] Examples of organic solvents used to prepare the solution of the raw material composition include toluene, ethyl acetate, methyl ethyl ketone, etc. Examples of methods for applying the solution include spin coating, spray coating, bar coating, knife coating, roll coating, roll knife coating, blade coating, die coating, gravure coating, and printing methods (e.g., screen printing and inkjet printing).
[0096] There are no particular limitations on the process for providing the surface of the adhesive layer 110 with irregularities. For example, irregularities can be provided on the surface of the adhesive layer 110 using an imprinting method. In the imprinting method, a mold having a surface shape complementary to the irregularities to be provided can be used. Specifically, irregularities can be provided on the surface of the adhesive layer by heating the adhesive layer while pressing the adhesive layer provided on the substrate with the mold. A more specific method involves pressing the adhesive layer with the mold, heating the adhesive layer, and maintaining the temperature for a predetermined period of time, after which the adhesive layer is cooled and the mold is removed. When heating the adhesive layer, for example, the adhesive layer can be heated to a temperature higher than the softening point of the adhesive layer. The time for maintaining the adhesive layer in the heated state is also not particularly limited, and may be maintained for, for example, 10 seconds or more or 10 minutes or less. A specific method for heating the adhesive layer while pressing the adhesive layer with the mold includes vacuum laminating the adhesive layer provided on the substrate and the mold. Instead of performing the two-step process of forming the adhesive layer and forming the irregularities, an adhesive layer having irregularities on its surface may be formed on the substrate in a single step. Also, the release sheet 150 having the release layer 160 having irregularities as described above may be used as the mold.
[0097] As another method, the adhesive layer 110 having a rough surface can be provided by spray-coating a solution of the raw material composition. Furthermore, the adhesive layer 110 having a rough or fibrous surface can be provided by adding a filler to the solution of the raw material composition and coating such a solution. As yet another method, the adhesive layer 110 having a textured shape can be directly provided on the substrate 120 by coating the solution of the raw material composition according to a desired pattern using a printing method such as an inkjet method.
[0098] (Method of Using Element Transfer Sheet) The sheet according to this embodiment can be used to transfer elements. As a specific example, the sheet according to this embodiment can be used to transfer semiconductor chips obtained by dicing to desired positions. The element transfer method using the sheet according to this embodiment will be described with reference to the flowchart of FIG. 6.
[0099] (S10: Holding of Element) In S10, an element is held on the adhesive layer of the element transfer sheet according to this embodiment. The type of element is not particularly limited. The element may be, for example, a semiconductor chip such as an LED chip, a semiconductor chip with a protective film, or a semiconductor chip with a die attach film (DAF). The element may also be a micro light-emitting diode, a mini light-emitting diode, a power device, a MEMS (Micro Electro Mechanical Systems), or a controller chip, or a component thereof. The element may also be a singulated object such as a wafer, panel, or substrate. The element may have a circuit surface on which an integrated circuit having circuit elements such as transistors, resistors, and capacitors is formed. The element is not necessarily limited to a singulated object, and may also be various unsingulated wafers or substrates.
[0100] The size of the element is not particularly limited. For example, the size of the element is preferably 100 μm. 2 More preferably, 500 μm or more 2 More preferably, 1000 μm or more 2 On the other hand, the size of the element is preferably 100 mm 2 Less than 25 mm, more preferably 2 Less than 1 mm, more preferably 2 It may be the following:
[0101] Examples of wafers include semiconductor wafers such as silicon wafers, silicon carbide (SiC) wafers, and compound semiconductor wafers (e.g., gallium phosphide (GaP) wafers, gallium arsenide (GaAs) wafers, indium phosphide (InP) wafers, and gallium nitride (GaN) wafers). The size of the wafer is not particularly limited, but is preferably 6 inches (diameter approximately 150 mm) or larger, and more preferably 12 inches (diameter approximately 300 mm) or larger. The shape of the wafer is not limited to a circle, and may be an angular shape such as a square or rectangle.
[0102] The panel may be a fan-out type semiconductor package (e.g., FOWLP or FOPLP). That is, the workpiece may be a semiconductor package before or after singulation in a fan-out type semiconductor package manufacturing technique. The size of the panel is not particularly limited, but may be, for example, a rectangular substrate of about 300 to 700 mm.
[0103] The substrate may be a glass substrate, a sapphire substrate, or a compound semiconductor substrate.
[0104] In one embodiment, elements are transferred from a holding substrate to an element transfer sheet, and the element transfer sheet holds the transferred elements. For example, a semiconductor wafer can be attached to a wafer substrate, and the semiconductor wafer can then be diced. The elements on the wafer substrate obtained by dicing can then be brought into close contact with the adhesive layer 110 of the element transfer sheet. The adhesive strength between the wafer substrate and the elements can then be reduced by applying an external stimulus such as laser light. This process allows elements to be transferred from the wafer substrate to the semiconductor transfer sheet. Alternatively, elements obtained by dicing a semiconductor wafer can be transferred to a holding substrate to obtain a holding substrate with elements attached thereto. The elements attached to the holding substrate can then be transferred to the adhesive layer 110 of the element transfer sheet in a similar manner.
[0105] In another embodiment, an external stimulus may be used to separate an element attached to a holding substrate from the holding substrate. Specifically, the element moves away from the holding substrate. Alternatively, the element moves closer to the element transfer sheet. Then, the element comes into contact with the adhesive layer 110 of the sheet, separating the element from the holding substrate and capturing it on the sheet. The type of external stimulus is not particularly limited, but examples include application of energy, cooling, expansion of the holding substrate, and physical stimulation (e.g., pressing the back surface of the holding substrate with a pin, etc.). By using one or more of these external stimuli, the bonding force between the holding substrate and the element can be reduced, and the element can be separated from the holding substrate. For example, the element can be separated from the holding substrate by irradiation with laser light (laser lift-off method). In such an embodiment, pressure is generated between the element and the adhesive layer 110 as the separated element approaches the adhesive layer 110. However, the uneven surface of the adhesive layer 110 reduces the pressure generated between the element and the adhesive layer 110, making it easier to capture the element at the desired position on the sheet.
[0106] In a further embodiment, a semiconductor wafer is attached to the adhesive layer 110 of the element transfer sheet. Then, elements are formed by dicing the semiconductor wafer on the adhesive layer 110. This method also allows the element transfer sheet to hold elements.
[0107] (S20: Expanding the element transfer sheet) In S20, the element transfer sheet is expanded in the surface direction. Expanding the sheet increases the spacing between the elements. This makes it easier to handle the elements in the next step. In one embodiment, expanding the sheet reduces the element retention force, making it easier to peel off the elements in the next step. The specific method for expanding the sheet is as described above.
[0108] (S30: Peeling of Elements) In S30, the elements are peeled from the adhesive layer 110 of the element transfer sheet. In this embodiment, the elements are peeled from the adhesive layer 110 of the element transfer sheet expanded in the planar direction. The method for peeling the elements is not particularly limited. For example, the method described above can be used to transfer elements attached to a holding substrate to an element transfer sheet. Specifically, the element can be moved to the transfer destination by bringing the transfer destination substrate or sheet close to the surface of the element and pressing the surface of the sheet opposite the element using a pin or the like. As another method, specifically, the element can be peeled from the adhesive layer 110 of the sheet using an adsorption member such as a vacuum chuck and moved to the desired position at the transfer destination. If the holding force of the adhesive layer 110 is reduced by expanding the sheet, the element may be peeled from the adhesive layer 110 of the sheet without applying physical stimulation from the opposite surface of the adhesive layer 110 of the sheet. Furthermore, the adhesiveness between the element transfer sheet and the element may be reduced by bringing the elements held on the element transfer sheet into close contact with a substrate or sheet to which the elements are to be transferred, and then applying an external stimulus such as laser light. This method also allows the elements to be transferred from the element transfer sheet to the destination. In this case, expanding the element transfer sheet changes the relative arrangement of the elements before and after the sheet is expanded.
[0109] By this procedure, the element can be transferred to any desired destination using the element transfer sheet. Furthermore, by using this transfer method, electronic components or semiconductor devices having elements can be manufactured. The elements held by the element transfer sheet may be subjected to processing or treatment.
[0110] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples. In each example, parts and percentages are based on the mass of the solid content unless otherwise specified.
[0111] The following compounds were used in the examples and comparative examples. <Component (A): Acrylic Resin> As the acrylic resin, an acrylic copolymer (monomer mass ratio: 2-ethylhexyl acrylate / 2-hydroxyethyl acrylate / acrylic acid = 92.8 / 7.0 / 0.2, mass average molecular weight (Mw): 1,100,000) was used.
[0112] <Component (B): Energy Reactive Resin> Tricyclodecane dimethanol diacrylate was used as the energy reactive resin.
[0113] <Component (C): Crosslinking Agent> As the crosslinking agent, an isocyanurate type polyisocyanate derived from hexamethylene diisocyanate was used.
[0114] <Component (D): Photopolymerization Initiator> As the photopolymerization initiator, 2,4,6-trimethylbenzoyldiphenylphosphine oxide was used.
[0115] <Evaluation of Tensile Stress of Substrate> The tensile stress of the substrate used in each example was evaluated as follows. A substrate cut to 150 mm in the MD direction and 15 mm in the TD direction was used as a test sample. For this test sample, the tensile stress was measured in an environment of 23°C and 50% RH (relative humidity) in accordance with JIS K 7161-1:2014 and JIS K 7127:1999. For the measurement, a tensile tester (manufactured by Shimadzu Corporation, product name "Autograph (registered trademark) AG-IS 500N") was used. Specifically, after setting the chuck distance to 100 mm, a tensile test was performed on the test sample at a speed of 200 mm / min, and the tensile stress (MPa) in the MD direction at 100% elongation of the support was measured. In addition, a similar test was performed using a substrate cut into a size of 150 mm in the TD direction x 15 mm in the MD direction as a test sample, to measure the tensile stress (MPa) in the TD direction when the support was stretched 100%.
[0116] <Expansion Test> The expansion test of the sheet obtained in each example was carried out as follows: First, the adhesive layer of the sheet obtained in each example was attached to a ring frame (made of stainless steel, inner diameter 194 mm), and the sheet was cut to fit the outer diameter of the ring frame.
[0117] Next, a wafer substrate (mirror silicon wafer, 6 inches, 150 μm thick) was fixed to a separately prepared dicing tape. The wafer substrate was then diced into 10 mm x 10 mm squares to obtain multiple elements (silicon chips, element size 10 mm x 10 mm x 150 μm). The multiple elements obtained were attached to the adhesive layer of the sheet at the center of the inner side of the ring frame so that the mirror surface was attached to the adhesive layer. Attachment was performed by lamination at room temperature (23°C). The dicing tape was then peeled off to transfer the multiple elements from the dicing tape to the sheet. In this way, a sheet on which multiple elements were placed and supported by a ring frame was obtained as an evaluation sample.
[0118] The obtained evaluation sample was placed in the expanding device shown in FIG. 5A. With the element supported by the base 310 over the sheet, the ring frame 320 was pressed down at a speed of 1 mm / sec with a drop distance of 80 mm. After pressing down, the spacing between each chip (vertical and horizontal directions) was measured using a digital microscope. Here, the spacing between each chip refers to the distance between adjacent chips. Based on the spacing between each chip measured in this way, the average value and coefficient of variation of the spacing between each chip were calculated. The average value and coefficient of variation of the spacing between multiple chips correspond to the average value and coefficient of variation for a data group including the spacing between all pairs of adjacent chips in the first direction and the spacing between all pairs of adjacent chips in the second direction.
[0119] Example 1 A pressure-sensitive adhesive composition was prepared by dissolving 100 parts by solids by mass of an acrylic resin (A), 25 parts by solids by mass of an energy-reactive resin (B), 1.25 parts by solids by mass of a crosslinking agent (C), and 0.75 parts by solids by mass of a photopolymerization initiator (D) in toluene. This pressure-sensitive adhesive composition was applied to the release-treated surface of a release sheet (manufactured by Lintec Corporation, product name: SP-PET382150, a polyethylene terephthalate film laminated with a silicone-based release agent, thickness 38 μm), and the resulting coating was dried at 100°C for 2 minutes to form a pressure-sensitive adhesive layer with a thickness of 25 μm. The storage modulus of the resulting pressure-sensitive adhesive layer was 2.04 MPa.
[0120] Onto this adhesive layer, a PVC film (containing 35 parts by mass of di(2-ethylhexyl)phthalate as a plasticizer per 100 parts by mass of vinyl chloride copolymer, thickness 80 μm) was attached as a substrate. The tensile modulus and breaking elongation (TD direction and MD direction) of the substrate are shown in Figure 1.
[0121] After the release sheet was peeled off, the adhesive layer was attached to a replica mold on which a concave shape had been formed in advance, and vacuum laminated at 60° C. for 300 seconds. Next, an ultraviolet irradiator (manufactured by Heraeus) was used to irradiate the adhesive layer with an illuminance of 200 mW / cm. 2 , light intensity 800mJ / cm 2 A sheet having a textured surface was produced by irradiating ultraviolet light onto the sheet. The textured shape of the adhesive layer of the sheet was a grid-like arrangement of pillars, similar to that shown in FIG. 2A. The pitch P between pillars in the sheet was 20 μm. As shown in FIG. 4A, the height (H) of each pillar was 8 μm, the diameter (T) of the tip was 8 μm, and the diameter (D) of the base was 16 μm. The ratio of the area of the adhesive portion between the adhesive layer and the captured element (i.e., the area of the tip surface of the convex portion) to the area of the sheet was approximately 12.6%. The replica mold used had a surface shape complementary to the textured shape.
[0122] The sheet thus obtained was subjected to the expansion test as described above. The average value and coefficient of variation of the obtained tip spacing are shown in Table 1. Table 1 also shows the evaluation results of the expansion test, which were evaluated based on the size of the tip spacing and the variation in the tip spacing. In Table 1, "A" indicates a good evaluation result, and "F" indicates a poor evaluation result.
[0123] (Example 2) An EMAA film (ethylene-methacrylic acid copolymer film, acid content 9% by mass, one surface embossed to give a matte finish, thickness 80 μm) was used as the substrate, and a sheet was produced in the same manner as in Example 1, except that the non-embossed surface of the EMAA film was attached to the adhesive layer. The adhesive strength of the sheet of Example 2 was 23.5 mN / 50 mm.
[0124] Example 3 A sheet was produced in the same manner as in Example 1, except that a PO film (ethylene-block propylene copolymer, thickness 110 μm) was used as the substrate.
[0125] Comparative Example 1 A sheet was produced in the same manner as in Example 1, except that an LDPE film (amorphous low-density polyethylene, thickness 70 μm) was used as the substrate.
[0126]
[0127] As can be seen from a comparison between Examples 1 to 3 and Comparative Example 1, when the tensile stress in the first direction (e.g., MD direction) at 100% elongation of the substrate was 12 MPa or more and the tensile stress in the second direction (e.g., TD direction) was 9 MPa or more, the chip spacing increased and the chip spacing variation decreased, resulting in good evaluation results. In particular, as in Example 1, when the tensile stress in the first direction was 18 MPa or more and the tensile stress in the second direction was 12 MPa or more, the chip spacing increased and the chip spacing variation decreased, resulting in particularly good evaluation results. Furthermore, as in Example 3, when the tensile stress in the first direction was 12 MPa or more and 16 MPa or less and the tensile stress in the second direction was 9 MPa or more and 12 MPa or less, the chip spacing increased and the chip spacing variation decreased, resulting in particularly good evaluation results.
[0128] The invention is not limited to the above-described embodiment, and various modifications and variations are possible within the scope of the gist of the invention.
[0129] This application claims priority based on Japanese Patent Application No. 2022-151756 filed on September 22, 2022, Japanese Patent Application No. 2022-151757 filed on September 22, 2022, Japanese Patent Application No. 2023-058459 filed on March 31, 2023, Japanese Patent Application No. 2023-058460 filed on March 31, 2023, Japanese Patent Application No. 2023-058462 filed on March 31, 2023, and Japanese Patent Application No. 2023-058463 filed on March 31, 2023, the entire contents of which are incorporated herein by reference.
[0130] 110: adhesive layer, 120: substrate, 111: convex portion, 140: element, 150: release sheet, 160: release layer, 161: concave portion, 170: substrate, P: pitch
Claims
1. A device transfer sheet comprising a substrate and an adhesive layer having an uneven surface, wherein the tensile stress in a first direction when the substrate is 100% elongated is higher than the tensile stress in a second direction perpendicular to the first direction, the tensile stress in the first direction being 12 MPa or more, and the tensile stress in the second direction being 9 MPa or more.
2. The element transfer sheet according to claim 1, wherein the tensile stress in the first direction is 40 MPa or less, and the tensile stress in the second direction is 30 MPa or less.
3. The element transfer sheet according to claim 1, wherein the tensile modulus of the substrate is 2500 MPa or less.
4. The element transfer sheet according to claim 1, wherein the substrate has a breaking elongation of 105% or more.
5. The element transfer sheet according to claim 1, wherein the substrate is a polyolefin film or a vinyl chloride copolymer film.
6. The element transfer sheet according to claim 1, wherein the adhesive layer has a plurality of convex portions spaced apart from one another and bounded by concave portions, and the pitch of the plurality of convex portions is 1 μm or more and 100 μm or less.
7. The element transfer sheet according to claim 1, wherein the adhesive layer has a plurality of convex portions, the heights of the plurality of convex portions being uniform.
8. An element transfer sheet as described in claim 1, wherein, after forming a plurality of elements by dicing a wafer substrate held by the adhesive layer, when the element transfer sheet is expanded by 180% in the first direction and the second direction, the coefficient of variation of the spacing between the plurality of elements is 0.2 or less.
9. An element transfer sheet as described in claim 1, wherein, after forming multiple elements by dicing a wafer substrate held by the adhesive layer, when the element transfer sheet is expanded by 80 mm in the first direction and the second direction, the average spacing between the multiple elements is 1 mm or more.