Spherical alumina particles, method of production of same, and resin composite composition containing same

MYPI2025001837A0Undetermined Publication Date: 2024-03-30NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025001837
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-30
Filing Date
2023-10-02
Publication Date
2024-03-30

AI Technical Summary

Technical Problem

Existing methods for producing spherical alumina particles with small particle size and low metal Al concentration are limited by agglomeration issues, contamination risks, and equipment wear, which affect their thermal conductivity and safety in semiconductor applications.

Method used

A method involving a raw material preparation step with alumina, boehmite, or aluminum hydroxide, followed by surface treatment with a silicon atom-containing agent and spheroidization in a flame, to produce spherical alumina particles with controlled particle size, low metal Al concentration, and specific surface area, reducing agglomeration and equipment wear.

Benefits of technology

The method effectively produces spherical alumina particles with low metal Al concentration, small particle size, and controlled gelatinization rate, enhancing thermal conductivity and safety for semiconductor applications while maintaining equipment durability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

ABSTRACT SPHERICAL ALUMINA PARTICLES, METHOD OF PRODUCTION OF SAME, AND RESIN COMPOSITE COMPOSITION CONTAINING SAME Spherical alumina particles having a low metal Al concentration and small particle size, a method of production of the same, and a resin composite composition containing the same, that is, spherical alumina particles having a metal Al concentration of 1000 ppm or less, an average particle size of 0.3 to 2.0 um, a specific surface area of 2.5 to 5.0 m2 / g, a roundness of 0.80 or more, and an - phase ratio of 5.0% or less, a method of production of the same, and a resin composite composition containing the same.
Need to check novelty before this filing date? Find Prior Art

Description

Spherical alumina particles, their production method, and resin composite composition containing them

[0001] The present invention relates to spherical alumina particles, particularly spherical alumina particles having a reduced concentration of metallic Al, a method for producing the same, and a resin composite composition containing the same.

[0002] In recent years, the increasing functionality and speed of electronic devices such as mobile phones has led to an increase in the amount of heat generated by the electronic components inside the devices. To ensure the normal operation of electronic devices, efficiently dissipating the generated heat to the outside has become an important issue. Thermally conductive sheets and thermally conductive adhesives are widely used for heat dissipation. These are attached or applied between the heat-generating element and the heat-dissipating fin and then pressed together to eliminate the gap between the heat-generating element and the heat-dissipating fin, allowing for efficient heat dissipation. Furthermore, the semiconductors inside electronic components also generate significant amounts of heat due to their similarly high functionality and high speed, and the encapsulating materials that protect the semiconductors are also required to have heat dissipation properties.

[0003] Generally, heat dissipation sheets, heat dissipation adhesives, and semiconductor encapsulants are composed of thermally conductive inorganic fillers and resins. Thermally conductive inorganic fillers are made from inexpensive aluminum hydroxide and aluminum oxide (hereafter referred to as alumina), as well as materials such as silicon carbide, boron nitride, and aluminum nitride, which are expected to have high thermal conductivity. Alumina, in particular, is often used as a thermally conductive inorganic filler because it is inexpensive and chemically stable.

[0004] Thermally conductive inorganic fillers such as alumina are also required to be small in particle size and spherical. This is because semiconductor packages such as ICs and CPUs are becoming smaller and thinner, and as a result, bonding wires are becoming thinner and narrower in pitch. In other words, thermally conductive inorganic fillers such as alumina used in semiconductor packages are also required to be small in particle size and spherical in order to improve their ability to fill narrow spaces inside semiconductors.

[0005] Japanese Patent No. 6771078 Japanese Patent No. 5036984 Japanese Patent Laid-Open No. 2008-120673

[0006] Several methods are known for producing small particle size spherical alumina particles, typically 2.0 μm or less in size.

[0007] A common method for producing spherical alumina is the flame fusion method, which uses aluminum oxide as a raw material. The raw material aluminum oxide is sprayed into a flame, and the surface of the aluminum oxide is heated and melted to form spheroids. However, the molten particles may stick together, forming large aggregates, and the desired small particle size may not be obtained.

[0008] Patent Document 1 discloses a method for suppressing the aggregation of aluminum oxide by adding silica particles to raw aluminum oxide and then thermally spraying the mixture. However, this method inevitably results in the inclusion of silica particles in the spherical alumina particles obtained in the end.

[0009] Patent Document 2 discloses a method of suppressing the aggregation of aluminum oxide by placing a collision plate at the tip of a thermal spray burner, causing raw aluminum oxide to collide with the collision plate, and then performing a thermal spraying process.

[0010] Patent Document 3 discloses that fine-grained low-soda aluminum oxide raw material powder is passed through a device with a crushing and dispersing function, dispersed in a carrier gas, and then continuously introduced into a flame immediately thereafter to obtain spherical alumina with an average particle diameter of less than 1 μm and very little metal impurities. The spherical alumina obtained here is said to have a metal Al concentration of <0.010%. However, with this method, the crushed and dispersed particles re-agglomerate due to the small amount of moisture in the carrier gas, making it impossible to obtain small-diameter spherical alumina. Furthermore, since the alumina particles contain a large amount of hard alpha alumina, there is a concern that the device may be worn when passed through the crushing and dispersing device. Furthermore, the basic properties of the obtained spherical alumina, such as the specific surface area and circularity, are unclear.

[0011] As a method other than the flame fusion method, the deflagration method (VMC method) is also known. Specifically, it is said that metallic aluminum powder is dispersed in an oxygen stream, ignited, and oxidized. The reaction heat converts the metal and oxide into vapor or liquid, and then cooling can be used to obtain fine alumina particles, for example, with a particle size of 2.0 μm or less. However, since an explosive reaction is used, there is a risk of a dust explosion. Furthermore, there is a possibility that some of the metallic aluminum will not react, i.e., will not convert to alumina, and will remain. In particular, if the remaining metallic aluminum is contained in a semiconductor package, etc., it may lead to serious accidents such as a short circuit in the semiconductor. Note that neither Patent Document 1 nor Patent Document 2 mentions or suggests the remaining metallic aluminum.

[0012] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide spherical alumina particles having a low metal Al concentration, a low rate of alpha conversion, and a small particle size, a method for producing the same, and a resin composite composition containing the same.

[0013] The present inventors have found that by spraying a raw material containing at least one of alumina, boehmite, and aluminum hydroxide having a predetermined particle size in a flame fusion method, it is possible to obtain small-sized spherical alumina particles with a low concentration of metallic aluminum while suppressing aggregation of the raw material particles.

[0014] Based on the above findings, the gist of the present invention is as follows.

[0015] [1] Metallic Al concentration is 1000 ppm or less, average particle size is 0.3 to 2.0 μm, and specific surface area is 2.5 to 5.0 m 2 / g, a circularity of 0.80 or more, and a gelatinization rate of 5.0% or less. [2] The spherical alumina particles according to [1], having a gelatinization rate of 1.0% or less. [3] A method for producing spherical alumina particles, comprising: a raw material preparation step of preparing a raw material containing at least one of alumina, boehmite, and aluminum hydroxide and having a particle size of 0.2 to 2.0 μm; a surface treatment step of surface-treating the raw material with a silicon atom-containing surface treatment agent; and a spheroidization step of introducing the surface-treated raw material into a flame to melt it, and then quenching it to spheroidize it. [4] A resin composite composition characterized by containing the spherical alumina particles according to [1] or [2]. [5] The resin composite composition according to [4], further containing at least one inorganic filler selected from amorphous spherical silica particles, crystalline spherical silica particles, titania particles, magnesia particles, aluminum nitride particles, boron nitride particles, barium titanate particles, calcium titanate particles, and carbon fibers.

[0016] The present invention provides small-diameter spherical alumina particles with a low metallic aluminum concentration, a very low gelatinization rate, and a controlled specific surface area, as well as a resin composite composition containing the same. Because of their small particle size, they can be used in miniaturized and thinned semiconductor packages, and the low metallic aluminum concentration reduces the occurrence of serious accidents such as short circuits. Furthermore, the very low gelatinization rate results in a very smooth alumina particle surface, which has the advantages of enhanced fluidity and reduced equipment wear. Furthermore, the spherical alumina particles can be easily produced by a manufacturing method according to one aspect of the present invention.

[0017] [Spherical Alumina Particles] (Metal Al Concentration) The spherical alumina particles according to one embodiment of the present invention have a metal Al concentration of 1000 ppm or less. Alumina is an oxide of metal Al and can be produced by oxidizing and dehydrating metal Al or an aluminum compound containing metal Al (e.g., aluminum hydroxide). During the alumina production process, metal Al contained in the raw materials may not be sufficiently oxidized, resulting in metal Al remaining in the alumina product. In particular, the deflagration method (VMC method) utilizes an explosive reaction to oxidize metal Al, which is likely to result in uneven oxidation, i.e., not converting to alumina, and metal aluminum remaining. Metal Al has much higher electrical conductivity than alumina (aluminum oxide). In applications requiring high insulation, such as semiconductor packaging, the presence of metal Al can cause serious accidents such as unexpected short circuits. From this perspective, a lower metal Al concentration is preferable. The spherical alumina particles according to one embodiment of the present invention have a metal Al concentration of 1000 ppm or less, which suppresses the occurrence of serious accidents such as short circuits. More preferably, the metal Al concentration may be 800 ppm or less or 700 ppm or less. The lower limit of the metal Al concentration is not particularly limited and may be 0 ppm, but since this may result in a large burden and difficulty in production management, it may be set to several ppm, specifically 1 ppm or more, or 5 ppm or more. The lower limit of the metal Al concentration may be adjusted depending on the actual application and the target allowable range of insulating properties, and may be, for example, 10 ppm or more, 20 ppm or more, or 30 ppm or more.

[0018] The metal Al concentration is analyzed as follows: Approximately 1 g of spherical alumina particle sample is weighed out and placed in a beaker. 60 ml of 1 mol / L hydrochloric acid is added to the beaker and stirred at room temperature for 5 hours. After stirring, the supernatant of the sample solution is removed and the volume is adjusted to 100 ml, and the solution is analyzed for Al content using ICP-MS.

[0019] (Particle size) The spherical alumina particles according to one embodiment of the present invention have an average particle size of 0.3 to 2.0 μm. A particle size of less than 0.3 μm is undesirable because the particles tend to aggregate more, significantly reducing the fluidity of the resin composition when used as a filler. A particle size of more than 2.0 μm can cause the particles to get caught in the narrow spaces between the mounting substrate and the chip in semiconductor packages, which are becoming increasingly smaller and thinner, reducing the fluidity of the liquid encapsulant and reducing moldability.

[0020] Here, the average particle size refers to the average particle size (D50), and means the median diameter D50 at 50% cumulative volume in the volume-based particle size distribution measured by a laser diffraction / scattering particle size distribution measurement method. The laser diffraction / scattering particle size distribution measurement method involves irradiating a dispersion containing spherical alumina particles with laser light and determining the particle size distribution from the intensity distribution pattern of the diffracted / scattered light emitted from the dispersion. In the present invention, a laser diffraction / scattering particle size distribution measurement device "Mastersizer 3000" (manufactured by Malvern) is used. The average particle size of the raw material for spherical alumina particles can also be determined in a similar manner.

[0021] (Galactose ratio) Here, the alpha-alumina ratio refers to the proportion of alpha-alumina crystals in the crystalline phase. The spherical alumina particles according to one embodiment of the present invention have a galactose ratio of 5.0% or less. Alumina is known to be crystalline, with typical crystalline forms known as alpha-alumina, θ-alumina, and δ-alumina. The spherical alumina particles according to one embodiment of the present invention, as will be described in detail later, can be produced based on a thermal spraying method in which a raw material is introduced into a flame, melted, and then rapidly cooled. In this case, the resulting alumina can have a high amorphous content, making it easy to obtain spherical alumina particles with a galactose ratio of 5.0% or less. Controlling the galactose ratio within this range results in a smooth alumina particle surface, which is effective in maintaining high fluidity when mixed with a resin, and excellent in low equipment wear due to the low amount of hard alpha-alumina particles. On the other hand, if the galactose ratio is low, the amount of alpha-alumina contained in the alumina particles will be too small, resulting in a decrease in the thermal conductivity of the particles and a risk of a decrease in the thermal conductivity of the resin composition. The lower limit of the gelatinization rate is not particularly limited and may be 0.0%, but may be 0.1% or 0.2% from the viewpoint of the burden of production management and the thermal conductivity characteristics of the resin composition. The upper limit of the gelatinization rate may be 3.0%, 1.5%, 1.0%, 0.9%, or 0.8%.

[0022] The alpha-phase ratio of the alumina particle powder is measured using a powder X-ray diffractometer. The integrated area of ​​the obtained diffraction peaks is determined, and the ratio of the diffraction peak area derived from alpha-alumina to the total area is analyzed by the Rietveld method. Specifically, an X-ray diffraction pattern is obtained using a D2PHASER manufactured by Bruker in the 2θ range of 10° to 90°. The alpha-phase ratio is calculated from the obtained pattern by the Rietveld method using a DIFFRAC.TOPAS manufactured by Bruker. During the calculation, analysis is performed assuming the presence of only three types of crystalline phases: alpha-alumina, delta-alumina, and theta-alumina, and the alpha-alumina content is calculated.

[0023] (Specific Surface Area) The spherical alumina particles of the present invention have a specific surface area of ​​2.5 m2 measured by the BET method. 2 / g or more 5.0m 2 / g or less.

[0024] The specific surface area of ​​the spherical particles is 2.5 m 2 If the specific surface area of ​​the spherical particles is less than 5.0 m / g, the particles are unlikely to form a close-packed structure, which may reduce the fluidity of the liquid encapsulant containing the particles. 2 If the particle size exceeds 3.0 m / g, the tendency for aggregation between particles increases, and the fluidity of the liquid encapsulant may also decrease. 2 / g. The preferred upper limit is 4.0 m 2 / g.

[0025] The specific surface area of ​​spherical particles can also be measured by the BET method, and is typically measured by the following procedure. Approximately 5 g of sample is weighed out and vacuum dried at 250°C for 5 minutes. Next, the sample is placed in an automatic specific surface area measuring device (Macsorb, manufactured by Mountec Co., Ltd.), and the nitrogen gas adsorption amount is measured at a relative pressure P / P of 0.291 at a measurement temperature of 77 K using pure nitrogen and a nitrogen-helium mixed gas (mixture ratio: nitrogen 30%, He 70%), and the BET specific surface area is calculated by the one-point method.

[0026] (Circularity) In one embodiment of the present invention, the spherical alumina particles may have a circularity of 0.80 or more. The higher the circularity of the spherical particles, the lower the viscosity of a resin composite composition containing the alumina particles and the more improved the moldability. The circularity may be 0.85 or more, 0.90 or more, or 0.93 or more. Theoretically, the upper limit of the circularity is 1.0, but from the viewpoint of production control, it may be 0.98 or less, or 0.95 or less.

[0027] The circularity can be measured using an electron microscope, an optical microscope, and an image analyzer. For example, Sysmex FPIA. These devices are used to measure the circularity of particles (perimeter of the equivalent circle / perimeter of the projected image of the particle). The circularity of 100 or more particles is measured, and the average value is taken as the circularity of the powder.

[0028] (Converted Powder Resistivity) The spherical alumina particles according to one embodiment of the present invention have a converted powder resistivity of 3.0×10 9The alumina particles are sometimes used in applications requiring high insulation, such as semiconductor packages, and the higher the converted powder resistivity, the more preferable it is. In this regard, the converted powder resistivity of spherical alumina particles is 3.1 × 10 9 Ω・cm or more, 3.2×10 9 Ω・cm or more, 4.0×10 9 Ω・cm or more, 5.0×10 9 The upper limit is not particularly limited, but it may be 1.0 × 10 11 Ω・cm or less, 1.0×10 10 It may be Ω·cm or less.

[0029] The converted powder resistivity of the alumina particle powder (hereinafter also simply referred to as "converted powder resistivity") is calculated by the powder resistivity and the Na 2 The resistivity is calculated by multiplying the powder resistivity by the NaO content. In other words, it is calculated using the formula: (converted powder resistivity) = (powder resistivity of alumina particle powder) x (NaO content of spherical alumina particles). The powder resistivity of alumina particle powder is measured using the MCP-PD51 powder resistivity measurement system. As a pretreatment for measurement, the powder is heated and dried in air at 200°C for 5 hours. The dried powder is introduced into the powder resistivity measurement probe unit, and the sample is gradually pressurized using the attached hydraulic pump. When the load reaches 20 kN, measurement is performed using a high resistivity meter.

[0030] (Na 2 O content) The spherical alumina particles according to one embodiment of the present invention contain Na 2 The O content may be 1000 ppm or less. 2 When O is contained, Na is contained in the resin composite composition containing the alumina particles. 2 O acts as an impurity, and there is a risk that the desired properties will not be obtained. 2 The lower the O content, the better. 2 The upper limit of the O content may be 750 ppm or less, or 500 ppm or less. 2The lower limit of the O content is not particularly limited and may be 0 ppm, but since this may make production management difficult, it may be set to several ppm, specifically 1 ppm or more, or 5 ppm or more. 2 The lower limit of the O content may be adjusted, for example, to 10 ppm or more, 20 ppm or more, or 30 ppm or more.

[0031] Spherical alumina particles Na 2 The O content is measured using an atomic absorption spectrophotometer. 0.5 g of sample is placed in a pressure vessel, 10 ml of sulfuric acid (1+3) is added, the vessel is capped, and the vessel is heated at 230°C for 16 hours in a heating and drying oven. After allowing the heated solution to cool, the solution is diluted to 100 ml and measured using an atomic absorption spectrophotometer. Note that sulfuric acid (1+3) refers to a solution diluted by adding 3 parts pure water to 1 part concentrated sulfuric acid by volume.

[0032] (Fluidity) The spherical alumina particles according to one embodiment of the present invention may be those for which the fluidity evaluation by the following measurement method is good, i.e., ◯ (Good). The spherical alumina particles can be used as a filler for a resin composite composition, and from the viewpoint of production control, it is preferable that the fluidity is within an appropriate range. The fluidity varies depending on the conditions of the matrix resin, etc., but the evaluation criteria for fluidity in this specification are shown as a guideline.

[0033] The fluidity evaluation method used in this specification is as follows. First, 30 g of a spherical alumina particle sample is weighed out and placed in a bag. Next, 70 g of AZ10-75 (alumina powder manufactured by Nippon Steel Chemical & Material Co., Ltd., average particle size 10 μm) is weighed out and placed in the bag containing the spherical alumina particles. The bag is then tied and thoroughly mixed. 43.5 g of the mixed alumina particle powder is weighed out and placed in a 200 ml plastic container. 6.5 g of silicone resin CY52-276A liquid manufactured by Dow Toray is added, and the mixture is vacuum mixed using a Thinky vacuum mixer called "Awatori Rentaro." The mixing conditions are 15 seconds of premixing and 90 seconds of vacuum mixing. After mixing, the plastic container containing the mixture is placed in a water bath adjusted to 25°C and cooled for 1 hour. 10 g of the kneaded and prepared compound (resin composite composition) is placed on a plate with a smooth surface. There are no particular restrictions on the material of the plate, but in this example, an iron plate was used. The plate on which the compound was placed was tilted 60 degrees from the horizontal to check the degree of flow of the compound. In this test, if the compound had flowed 15 cm or more after 5 hours of tilting, the fluidity was evaluated as O (Good), and if it had not flowed 15 cm or more, the fluidity was evaluated as × (Not Good).

[0034] [Method for producing spherical alumina particles] One embodiment of the present invention provides a method for producing spherical alumina particles. This method is a method that can suitably produce the alumina particles described above, and includes the following steps: (1) a raw material preparation step of preparing a raw material containing at least one of alumina, boehmite, and aluminum hydroxide and having a particle size of 0.3 to 2.00 μm; (2) a surface treatment step of surface-treating the raw material with a silicon atom-containing surface treatment agent; and (3) a spheroidization step of introducing the raw material into a flame to melt it, and then rapidly cooling it to form spherical particles.

[0035] Although the order of the steps may vary, the spheroidizing step (3) will be explained first.

[0036] The spheroidization process (3) involves introducing the raw material into a flame, melting it, and then rapidly cooling it to form spheroids. The raw material can be introduced into the flame while suspended in a carrier gas. Examples of the carrier gas include air, oxygen, and propane gas. The flame formation method is not particularly limited. For example, a flame can be formed by supplying a flame-forming fuel (e.g., propane) to a burner via a route separate from the introduction of the raw material; a flame can be formed by pre-mixing fuel and a combustion-supporting gas (e.g., air or oxygen) and supplying it to the burner; or a flame can be formed by mixing the raw material, fuel, and combustion-supporting gas and supplying it to the burner. The flame is preferably formed in a heat-resistant furnace. The flame is preferably formed at the top of the heat-resistant furnace, the raw material is supplied into the flame, and the resulting alumina particle material is collected from below as it settles due to gravity. By preventing the formation of a flame in the lower part of the heat-resistant furnace, the alumina particle material that settles to the bottom is rapidly cooled and granulated.

[0037] In the raw material preparation step (1), raw materials to be introduced in the spheroidization step (3) are prepared. The raw materials contain at least one of alumina, boehmite, and aluminum hydroxide, and are prepared so that the particle size is 0.2 to 2.0 μm. Boehmite is alumina monohydrate, and Al 2 O 3 ・H 2 O, and aluminum hydroxide is Al(OH) 3 In both cases, when the raw material is put into the flame in the spheroidizing process (3), the hydrated content (H 2 O) or hydroxyl groups (OH) are converted into water vapor (H 2 O) and alumina (Al 2 O 3 ) particles are produced. 2 O 3) particles are melted at least on the surface and spheroidized. When alumina is used as the raw material, examples include calcined alumina obtained by sintering aluminum hydroxide, alumina obtained by electrofusion of aluminum hydroxide, low-soda alumina produced from aluminum hydroxide, and high-purity alumina produced by ammonia-alum pyrolysis, aluminum alkoxide hydrolysis, aluminum water discharge, or other methods. From the viewpoint of productivity and cost, alumina obtained by calcining low-soda aluminum hydroxide is more preferred. Among the above raw materials, boehmite and aluminum hydroxide contain sufficient moisture (hydration water and hydroxyl groups). Therefore, as described below, the increase in particle size of the raw material is particularly effectively suppressed in the spheroidization step, and spherical alumina particles with an average particle size of less than 1 μm can be efficiently obtained, making them more preferred.

[0038] Conventionally, a method for producing spherical alumina involves introducing alumina particles into a flame to spheroidize them. However, in this spheroidization process, the alumina particles, whose surfaces are melted, fuse together and aggregate, which can lead to an increase in particle size and a decrease in circularity of the resulting particles. However, this embodiment solves these problems.

[0039] First, since the raw material in this embodiment contains moisture (hydration water and hydroxyl groups), water vapor (H 2 It takes time for the alumina particles (O) to separate. In other words, there is little opportunity (short time) for the surfaces of the alumina particles to melt in the flame, causing the alumina particles to fuse together and aggregate. As a result, the particle size of the alumina particles after passing through the flame is prevented from excessively increasing beyond the particle size of the raw material (0.2 to 2.0 μm).

[0040] Furthermore, water vapor (H 2O) expands when heated in the flame, and acts to increase the distance between the remaining raw materials, i.e., between the alumina particles. In other words, the chances of alumina particles fusing together are further reduced. As a result, the particle size of the alumina particles after passing through the flame is prevented from excessively increasing compared to the particle size of the raw material (0.2 to 2.0 μm). In addition, since there is little contact between the particles, the spheroidization of each particle is also promoted.

[0041] Next, the surface treatment step (2) will be described.

[0042] In the surface treatment step (2), the raw material obtained in the raw material preparation step (1) is surface-treated prior to the spheroidization step (3). Examples of surface treatment agents for the raw material include silane compounds (e.g., silane coupling agents), silazanes, and Al coupling agents. While the amount of surface treatment agent can be adjusted appropriately depending on the raw material's properties, it is preferable to incorporate these surface treatment agents at a concentration of 1% by mass or more relative to the raw material, which reduces the likelihood of raw material powder particles adsorbing to each other. This effectively prevents clogging of burners and piping due to adhesion and supply rate variations. Furthermore, it effectively prevents coarsening due to aggregation of raw material powder particles. On the other hand, if an excessive amount of surface treatment agent is present, the treatment agents react with each other, crosslinking the particles via the surface treatment agent. This may result in the original dispersion effect not being achieved, and from an economical standpoint, adding an excessive amount of treatment agent is undesirable. The preferred upper limit of the amount of surface treatment agent incorporated is 10% by mass relative to the raw material. Of the above surface treatment agents, silicon atom-containing compounds (also referred to as "silicon atom surface treatment agents") such as silane coupling agents, alkoxysilane compounds, and silazane compounds are preferred from the standpoint of economy and reactivity. Known substances can be used as these silicon atom surface treatment agents. Examples of silane coupling agents include vinyltrimethoxysilane and N-phenyl-3-aminopropyltrimethoxysilane. Examples of alkoxysilane compounds include hexyltrimethoxysilane and octyltriethoxysilane. Examples of silazane compounds include hexamethyldisilazane and trimethylsilane. From the standpoint of excellent reactivity, silazane compounds are more preferred. Hexamethyldisilazane and trimethylsilane are more preferred.

[0043] The surface treatment method includes the following first step (heating step) and second step (surface treatment step). First step (heating step): A raw material powder containing alumina, aluminum hydroxide, or boehmite is heated at a temperature of 100°C to 500°C for 30 minutes or more. The preferred heating conditions are 150°C or higher for 2 or 5 hours. Heating the raw material powder in this step removes excess moisture from the powder particle surface, thereby enhancing the reactivity of the treatment agent with the particle powder in the subsequent surface treatment step. This is because moisture on the raw material surface can react with the surface treatment agent, preventing the surface treatment agent from properly reacting with the raw material. While there is no particular restriction on the raw material heating method, commonly used methods such as an electric drying furnace, tunnel kiln, or shuttle kiln are preferred. The drying temperature is preferably 500°C or less to suppress particle size coarsening due to moisture generated from the raw material during spheroidization. Heating at 500°C or higher causes complete desorption of moisture from the aluminum hydroxide or boehmite, resulting in no moisture being generated during spheroidization. The lower limit of the drying temperature is preferably 100°C or higher in order to evaporate the moisture. After heating, the product may be cooled and used in the next step, or it may not be cooled. Preferably, the next step, the surface treatment step, is carried out without cooling.

[0044] Second Step (Surface Treatment Step) The raw material powder heat-treated in the previous step is placed in an arbitrary mixer and stirred. Stirring may be performed at room temperature or after heating. To enhance the reactivity of the silane compound, the mixture is preferably heated to 50°C or higher, more preferably 80°C or higher, before stirring. After stirring for 30 seconds to 10 minutes, the surface treatment agent is sprayed while continuing to stir. The types of surface treatment agents are as described above, and preferred are hexamethyldisilazane and trimethylsilane. The amount to be sprayed is preferably 1 to 5 times the amount calculated from the minimum coverage area of ​​the surface treatment agent, the specific surface area of ​​the raw material powder being treated, and the input weight (see the formula below). Amount of surface treatment agent to be sprayed = (specific surface area of ​​raw material powder) x (input weight of raw material powder) / (minimum coverage area of ​​surface treatment agent)

[0045] The method for stirring the surface treatment agent is not particularly limited, but a method in which the surface treatment agent, such as the silane coupling agent, is mixed with the raw material powder using a commonly used mixer such as a ball mill, vibration mill, planetary mill, jet mill, mechanical stirring blade mixer, or container rotary mixer is preferred. The raw materials may also be heated during mixing. The heating method is not particularly limited, but the outside of the mixing container may be covered with a jacket and heated with steam, heated water, oil, or the like. Heating can increase the reactivity of the surface treatment agent, making it possible to efficiently surface treat the raw materials.

[0046] Furthermore, prior to the surface treatment step (2), the raw material may be passed through an auxiliary device with a crushing and dispersing function. In the case of a dry method, examples of such devices include a jet mill or other device that swirls powder particles in a high-speed airflow, causing collision and pulverization, and a device that causes dust-containing gases to collide with each other to cause collision and pulverization. In the case of a wet method, examples include a high-pressure wet jet mill-type crushing device that crushes powder particles by collision, and an ultrasonic dispersing device that can irradiate powerful ultrasonic waves into a slurry delivery pipe. When passing through such a device with a crushing and dispersing function, it is desirable to line the powder-contacting parts of the device to prevent contact and wear between the alumina particles and the metal parts of the device. The lining material is not particularly limited, but examples include urethane, boron carbide, alumina, silicon carbide, and Teflon (registered trademark). However, since alumina particles are a very hard substance, an alumina lining is more preferable.

[0047] The raw material according to this embodiment may include at least one of boehmite and aluminum hydroxide, which contain more surface OH groups than alumina and are therefore more amenable to surface treatment, and the effects of the treatment are more readily apparent. In other words, the raw materials are more effectively dispersed, and as a result, spherical alumina particles with the desired small particle size and high circularity can be more easily obtained.

[0048] The raw material according to this embodiment may contain components other than boehmite or aluminum hydroxide, such as alumina, as long as the effects of the present invention are not affected.

[0049] Furthermore, the raw material according to this embodiment is adjusted to a particle size equivalent to or slightly smaller than the particle size of the alumina particles to be produced, i.e., 0.2 to 2.0 μm. Preferably, the particle size may be 0.3 μm or more, or 1.9 μm or less. The particle size may be adjusted by pulverization or classification to achieve the desired particle size. As described above, in the production method according to this embodiment, the particle size distribution of the raw material is generally inherited as the particle size distribution of the alumina particulate material to be produced.

[0050] [Resin Composite Composition] According to one embodiment of the present invention, a composite composition of the spherical alumina particles and a resin can be finally produced. The composition of the resin composite composition will be described in more detail below.

[0051] Using a slurry composition containing spherical alumina particles and a resin, it is possible to obtain a resin composite composition such as a semiconductor encapsulant (particularly a solid encapsulant), an interlayer insulating film, etc. Furthermore, by curing these resin composite compositions, it is possible to obtain a resin composite such as an encapsulant (cured product), a substrate for a semiconductor package, etc.

[0052] When producing the resin composite composition, for example, in addition to the spherical alumina particles and resin, a curing agent, a curing accelerator, a flame retardant, a silane coupling agent, etc. are blended as needed, and composited by a known method such as kneading, etc. Then, the composite is molded into pellets, films, etc. depending on the application.

[0053] Furthermore, when producing the resin composite composition, in addition to the spherical alumina particles and resin, other inorganic fillers may be blended. Examples of the inorganic fillers include amorphous spherical silica particles, crystalline spherical silica particles, titania particles, magnesia particles, aluminum nitride particles, boron nitride particles, barium titanate particles, calcium titanate particles, and carbon fibers. The blending ratio of the inorganic fillers can be adjusted appropriately depending on the application of the resin composite composition, but from the viewpoint of exerting the effects of the spherical alumina particles of the present invention, it is preferable that the blending ratio of the spherical alumina particles to the other inorganic fillers is 95:5 to 60:40.

[0054] Furthermore, when the resin composite composition is cured to produce a resin composite, for example, the resin composite composition is heated to melt it, processed into a shape according to the intended use, and then heated to a temperature higher than that used for melting to completely cure it. In this case, a known method such as a transfer molding method can be used.

[0055] For example, when manufacturing semiconductor-related materials such as package substrates and interlayer insulating films, known resins can be used as the resin for the resin composite composition, but epoxy resins are preferred. The epoxy resin is not particularly limited, but examples include bisphenol A epoxy resins, bisphenol F epoxy resins, biphenyl epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, naphthalene epoxy resins, and phenoxy epoxy resins. One of these resins can be used alone, or two or more resins with different molecular weights can be used in combination. Among these, epoxy resins having two or more epoxy groups per molecule are preferred from the viewpoints of curability, heat resistance, and the like. Specific examples include biphenyl-type epoxy resins, phenol novolac-type epoxy resins, orthocresol novolac-type epoxy resins, epoxidized novolac resins of phenols and aldehydes, glycidyl ethers of bisphenol A, bisphenol F, bisphenol S, etc., glycidyl ester acid epoxy resins obtained by reacting polybasic acids such as phthalic acid or dimer acid with epochlorohydrin, linear aliphatic epoxy resins, alicyclic epoxy resins, heterocyclic epoxy resins, alkyl-modified polyfunctional epoxy resins, β-naphthol novolac-type epoxy resins, 1,6-dihydroxynaphthalene-type epoxy resins, 2,7-dihydroxynaphthalene-type epoxy resins, bishydroxybiphenyl-type epoxy resins, and epoxy resins into which halogens such as bromine have been introduced to impart flame retardancy. Among these epoxy resins having two or more epoxy groups per molecule, bisphenol A-type epoxy resins are particularly preferred.

[0056] Furthermore, resins other than epoxy resins can also be used as resin composite compositions for applications other than semiconductor encapsulation composite materials, such as prepregs for printed circuit boards and various engineering plastics. Specific examples of resins that can be used in addition to epoxy resins include silicone resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyamides such as polyimides, polyamideimides, and polyetherimides; polyesters such as polybutylene terephthalate and polyethylene terephthalate; polyphenylene sulfide, aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS resins, AAS (acrylonitrile-acrylic rubber-styrene) resins, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resins.

[0057] The curing agent used in the resin composite composition may be any known curing agent for curing the resin, such as a phenol-based curing agent, such as a phenol novolac resin, an alkylphenol novolac resin, or a polyvinylphenol, which may be used alone or in combination.

[0058] The amount of the phenolic curing agent blended is preferably such that the equivalent ratio to the epoxy resin (phenolic hydroxyl group equivalent / epoxy group equivalent) is 0.1 or more and less than 1.0, thereby eliminating any unreacted phenolic curing agent from remaining and improving moisture absorption and heat resistance.

[0059] The amount of the spherical alumina particles of the present invention added to the resin composite composition is preferably large from the viewpoints of heat resistance and thermal expansion coefficient, but is typically 70% by mass to 95% by mass, preferably 80% by mass to 95% by mass, and more preferably 85% by mass to 95% by mass. This is because if the amount of spherical alumina particles is too small, it is difficult to achieve effects such as improving the strength of the sealing material and suppressing thermal expansion. Conversely, if the amount is too large, segregation due to aggregation of the spherical alumina particles is likely to occur in the composite material regardless of the surface treatment of the spherical alumina particles, and the viscosity of the composite material will become too high, making it difficult to use as a sealing material. Note that when the aforementioned "other filler" is used in combination, the preferred amount added to the resin composite composition is the total amount of the spherical alumina particles and the "other filler."

[0060] In addition to the resin, known additives such as a silane coupling agent, a curing agent, a colorant, and a hardening retarder can be used.

[0061] As for the silane coupling agent, any known coupling agent may be used, but those having an epoxy-based functional group are preferred.

[0062] A slurry composition containing spherical alumina particles and a resin can be used to obtain a heat-dissipating sheet, a heat-dissipating grease, and the like.

[0063] When obtaining the heat dissipation sheet, the spherical alumina particles, resin, and additives are appropriately blended and compounded by a known method such as kneading, etc. The obtained composite is molded into a sheet by a known method.

[0064] For example, when producing a heat dissipation sheet, known resins can be used in the resin composite composition, including silicone resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyamides such as polyimides, polyamideimides, and polyetherimides; polyesters such as polybutylene terephthalate and polyethylene terephthalate; polyphenylene sulfide, aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS resins, AAS (acrylonitrile-acrylic rubber-styrene) resins, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resins. Among these, silicone resins are preferred. The silicone resin is not particularly limited, but examples include peroxide-curable, addition-curable, condensation-curable, and ultraviolet-curable resins.

[0065] In addition to the resin, known additives such as a silane coupling agent, a curing agent, a colorant, and a hardening retarder can be used.

[0066] When preparing the thermally conductive grease, the spherical alumina particles, resin, and additives are appropriately blended and compounded by a known method such as kneading. The resin used in the thermally conductive grease is also called the base oil.

[0067] For example, when producing a thermally conductive grease, known resins can be used in the resin composite composition, and specific examples include silicone resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyamides such as polyimide, polyamideimide, and polyetherimide; polyesters such as polybutylene terephthalate and polyethylene terephthalate; polyphenylene sulfide, aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS resins, AAS (acrylonitrile-acrylic rubber-styrene) resins, AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resins, mineral oils, synthetic hydrocarbon oils, ester oils, polyglycol oils, silicone oils, and fluorine oils.

[0068] In addition to the resin, known additives such as silane coupling agents, colorants, thickeners, etc. Examples of the thickener that can be used include calcium soap, lithium soap, aluminum soap, calcium complex, aluminum complex, lithium complex, barium complex, bentonite, urea, PTFE, sodium terephthalamate, silica gel, and organic bentonite.

[0069] The present invention will be described below through examples and comparative examples, but the present invention should not be construed as being limited to the following examples.

[0070] Example 1: Boehmite raw material (D50 = 0.4 μm) was preheated in a heating furnace at 150°C for 5 hours, and the heated raw material was then charged into a Henschel mixer. After charging, hexamethyldisilazane was added while stirring to perform surface treatment. The amount of hexamethyldisilazane added was 1.5 wt% based on the weight of the raw material. Oxygen was then supplied as a carrier gas into a high-temperature flame formed by the combustion of LPG and oxygen, and a melting and spheroidizing treatment was performed to produce spherical alumina particles as described in Example 1 of Table 1.

[0071] Example 2 Spherical alumina particles shown in Example 2 in Table 1 were produced in the same manner as in Example 1, except that alumina powder (D50=0.7 μm) was used as the raw material.

[0072] Example 3 Spherical alumina particles shown in Example 3 in Table 1 were produced in the same manner as in Example 1, except that boehmite raw material (D50=0.2 μm) was used as the raw material.

[0073] (Comparative Examples 1 to 7) Under the conditions shown in Table 1, various raw materials (metallic aluminum powder, boehmite, or alumina) were supplied to a high-temperature flame formed by the combustion of LPG and oxygen using air as a carrier gas, and oxidation and spheroidization treatment were carried out to produce spherical alumina particles shown in the comparative examples in Table 1.

[0074] Example 4 The spherical alumina particles obtained in Example 1 and aluminum nitride particles (D50 = 30 μm) were mixed in a ratio of 90:10 (spherical alumina particle weight):(aluminum nitride particle weight) to prepare a spherical alumina particle mixture A. Furthermore, the spherical alumina particle mixture A was mixed with Dow Toray's silicone resin CY52-276A liquid so that the amount of spherical alumina particle mixture A added to the resin composite composition was 90 mass %, and the mixture was vacuum-kneaded using a Thinky vacuum kneader "Awatori Rentaro" to obtain a resin composite composition. The kneading conditions were 15 seconds of pre-kneading and 90 seconds of vacuum kneading.

[0075] Example 5 The spherical alumina particles obtained in Example 2 were mixed with boron nitride particles (D50 = 20 μm) in a ratio of 90:10 (spherical alumina particle weight):(boron nitride particle weight) to prepare spherical alumina particle mixture B. Furthermore, spherical alumina particle mixture B was mixed with silicone resin CY52-276A liquid manufactured by Dow Toray so that the amount of spherical alumina particle mixture B in the resin composite composition was 90% by mass, and the mixture was vacuum-kneaded using a Thinky vacuum kneader "Awatori Rentaro" to obtain a resin composite composition. The kneading conditions were 15 seconds of pre-kneading and 90 seconds of vacuum kneading.

[0076] Table 1 shows the physical properties of the produced spherical alumina particles.

[0077]

[0078] The methods for measuring the various physical properties are described below.

[0079] (Average particle size by laser diffraction scattering method) The laser diffraction / scattering particle size distribution measurement method is a method in which a dispersion liquid containing spherical alumina particles is irradiated with laser light, and the particle size distribution is determined from the intensity distribution pattern of the diffracted / scattered light emitted from the dispersion liquid. In the present invention, a laser diffraction / scattering particle size distribution measurement device "Mastersizer 3000" (manufactured by Malvern) was used.

[0080] (Specific Surface Area) The specific surface area is measured by the BET method. Typically, the specific surface area is measured by the following procedure. Approximately 5 g of a sample is weighed out and vacuum dried at 250°C for 5 minutes. Next, the sample is placed in an automatic specific surface area measuring device (Macsorb, manufactured by Mountec Co., Ltd.), and the nitrogen gas adsorption amount is measured at a measurement temperature of 77 K using pure nitrogen and a nitrogen-helium mixed gas (mixture ratio: nitrogen 30%, He 70%) at a relative pressure P / P0 of 0.291, and the BET specific surface area is calculated by the one-point method.

[0081] (Circularity) Circularity can be measured using an electron microscope, an optical microscope, and an image analyzer. For example, Sysmex FPIA. Using these devices, the circularity of particles (perimeter of the equivalent circle / perimeter of the projected image of the particle) is measured. The circularity of 100 or more particles is measured, and the average value is taken as the circularity of the powder.

[0082] (Gallitic Ratio) The alpha-phase ratio of the alumina particle powder is measured using a powder X-ray diffractometer. The integrated area of ​​the obtained diffraction peaks is determined, and the ratio of the diffraction peak area derived from alpha-alumina to the total area is analyzed by the Rietveld method. Specifically, an X-ray diffraction pattern is obtained using a D2PHASER manufactured by Bruker in the 2θ range of 10° to 90°. The alpha-phase ratio is calculated from the obtained pattern by the Rietveld method using a DIFFRAC.TOPAS manufactured by Bruker. During the calculation, analysis is performed assuming the presence of only three types of crystalline phases, alpha-alumina, delta-alumina, and theta-alumina, and the alpha-alumina content is calculated.

[0083] (Metal Al Concentration) The metal Al remaining in the alumina particles is measured using the following procedure. Approximately 1 g of a spherical alumina particle sample is weighed out and placed in a beaker. 60 ml of 1 mol / L hydrochloric acid is added to the beaker and stirred at room temperature for 5 hours. After stirring, the supernatant of the sample solution is removed and the volume is adjusted to 100 ml, and the solution is analyzed for Al content using ICP-MS.

[0084] (Converted Powder Resistivity) The converted powder resistivity of the alumina particle powder (hereinafter also simply referred to as "converted powder resistivity") is the powder resistivity and the Na 2In other words, (converted powder resistivity) = (powder resistivity of alumina particle powder) × (Na content of spherical alumina particles) 2 The powder resistivity of the alumina particle powder is measured using the powder resistivity measurement system MCP-PD51. As a pretreatment for the measurement, the powder is heated and dried in air at 200°C for 5 hours. The dried powder is introduced into a powder resistivity measurement probe unit, and the sample is gradually pressurized using the attached hydraulic pump. When the load reaches 20 kN, measurement is performed using a high resistivity meter.

[0085] (Na of particles 2 O content) Na content of alumina particles 2 The O content was measured using an atomic absorption spectrophotometer. 0.5 g of a sample was placed in a pressure vessel, 10 ml of sulfuric acid (1+3) was added, and the vessel was then capped and heated in a heating and drying oven at 230°C for 16 hours. The heated solution was allowed to cool, then the solution was diluted to 100 ml and measured using an atomic absorption spectrophotometer.

[0086] (Fluidity) 30 g of spherical alumina particle sample was weighed out and placed in a bag. 70 g of AZ10-75 (alumina powder, average particle size 10 μm, manufactured by Nippon Steel Chemical & Material Co., Ltd.) was then weighed out and placed in the bag containing the spherical alumina particles. The bag was then tied and thoroughly mixed. 43.5 g of the mixed alumina particle powder was weighed out and placed in a 200 ml plastic container. 6.5 g of silicone resin CY52-276A liquid manufactured by Dow Toray was added, and the mixture was vacuum mixed using a Thinky vacuum mixer called "Awatori Rentaro." The mixing conditions were 15 seconds of premixing and 90 seconds of vacuum mixing. After mixing, the plastic container containing the mixture was placed in a water bath adjusted to 25°C and cooled for 1 hour. 10 g of the mixed compound (resin composite composition) was placed on a smooth-surfaced plate. There are no particular restrictions on the material of the plate, but in this example, an iron plate was used. The plate on which the compound was placed was tilted 60 degrees from the horizontal to check the degree of flow of the compound. In this test, if the compound had flowed 15 cm or more after 5 hours of tilting, the fluidity was evaluated as O (Good), and if it had not flowed 15 cm or more, the fluidity was evaluated as × (Not Good).

[0087] It was confirmed that spherical alumina particles having a low metallic aluminum concentration, a low gelatinization rate, and a small particle size could be obtained. It was also confirmed that a resin composite composition containing the spherical alumina particles could be obtained.

[0088] The spherical alumina particles of the present invention have a small particle size, making them suitable for use in miniaturized and thinned semiconductor packages, and their low metallic aluminum concentration prevents serious accidents such as short circuits. Furthermore, the spherical alumina particles can be easily produced by a manufacturing method according to one embodiment of the present invention. Resin composite compositions containing the spherical alumina particles exhibit good fluidity and can be used for purposes other than semiconductor encapsulation. Specifically, they can also be used as prepregs for printed circuit boards and various engineering plastics.

Claims

1. Metallic Al concentration is 1000 ppm or less, average particle size is 0.3 to 2.0 μm, and specific surface area is 2.5 to 5.0 m 2 / g, a circularity of 0.80 or more, and a degree of gelatinization of 5.0% or less.

2. The spherical alumina particles according to claim 1, wherein the gelatinization rate is less than 1.0%.

3. A method for producing spherical alumina particles, comprising: a raw material preparation step of preparing a raw material containing at least one of alumina, boehmite, and aluminum hydroxide and having a particle size of 0.2 to 2.0 μm; a surface treatment step of surface-treating the raw material with a silicon atom-containing surface treatment agent; and a spheroidization step of introducing the surface-treated raw material into a flame to melt it, and then rapidly cooling it to form spherical particles.

4. A resin composite composition containing the spherical alumina particles according to claim 1 or 2.

5. The resin composite composition according to claim 4, further comprising at least one inorganic filler selected from the group consisting of amorphous spherical silica particles, crystalline spherical silica particles, titania particles, magnesia particles, aluminum nitride particles, boron nitride particles, barium titanate particles, calcium titanate particles, and carbon fibers.