Coating agent composition

MYPI2025001852A0Undetermined Publication Date: 2024-04-07THREE BOND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025001852
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-07
Filing Date
2023-10-03
Publication Date
2024-04-07

AI Technical Summary

Technical Problem

Outdoor installations such as signboards and vending machines are prone to scratches and corrosion due to exposure to rain and wind, and existing coating agents often peel or crack, impairing the design and failing to hide scratches effectively.

Method used

A coating composition comprising a silicone oligomer with alkoxy, phenyl, and alkyl groups, a compound with an alkoxy group and amino or mercapto group, another silicone oligomer with alkoxy and alkyl groups, and a curing catalyst, which forms a cured product with excellent adhesion, scratch hiding properties, and resistance to impact and weathering.

Benefits of technology

The coating composition effectively conceals scratches, provides excellent adhesion and impact resistance, and maintains weather resistance, preventing peeling and cracking, thus maintaining the design integrity of outdoor installations.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A problem of a conventional coating agent has been that, even in the case of coating with such a coating agent in advance, design of an outdoor installation object is impaired due to peeling with a strong impact for reason of the outdoor and / or due to scratching of such a coating agent itself. Another problem has also been that no scratch can be covered even by coating with such a coating agent after scratching and thus design is impaired. A coating agent composition including the following components (A) to (D): component (A): a silicone oligomer having only an alkoxy group, a phenyl group and an alkyl group in its molecule; component (B): a compound having an alkoxy group and having an amino group and / or a mercapto group in its molecule; component (C): a silicone oligomer having only an alkoxy group and an alkyl group in its molecule; and component (D): a curing catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Coating composition

[0001] The present invention relates to a coating composition.

[0002] Outdoor installations such as signs and vending machines, which are often installed outdoors, are prone to scratches caused by exposure to wind and rain, which can impair the design of the outdoor installation and lead to corrosion at the scratched areas. Methods for removing scratches include polishing with a compound or painting with the same color, but these require high skill from the installer. Since it is difficult to repair scratches on outdoor installations after they have been damaged, a method is known in which a coating agent is used in advance to make the body less susceptible to scratches (Patent Document 1, Patent Document 2).

[0003] JP 2007-161989 A JP 2015-183014 A

[0004] However, even if a coating agent is applied beforehand, there are problems such as peeling or cracking of the coating agent due to strong impacts caused by outdoor use, and such cracking can damage the design of outdoor installations.Furthermore, even if a coating agent is applied after an outdoor installation has been scratched, the scratch cannot be concealed, resulting in a loss of design.

[0005] Therefore, an object of the present invention is to provide a coating composition that can conceal scratches and has excellent adhesion when cured.

[0006] As a result of intensive research into achieving the above object, the inventors discovered a method for producing a coating composition that has excellent design and adhesion, and that can conceal scratches on outdoor installations by applying a coating over the scratches, thereby completing the present invention.

[0007] The gist of the present invention will now be described.

[0008] [1] A coating composition comprising the following components (A) to (D):

[0009] Component (A): A silicone oligomer having only alkoxy groups, phenyl groups, and alkyl groups within the molecule. Component (B): A compound having an alkoxy group and an amino group and / or a mercapto group within the molecule. Component (C): A silicone oligomer having only alkoxy groups and alkyl groups within the molecule. Component (D): A curing catalyst.

[0010] [2] The coating composition according to [1], wherein the alkyl group in component (A) is a silicone oligomer in which the alkyl group is a methyl group.

[0011] [3] The coating composition according to [1] or [2], wherein the alkoxy group in the component (A) is a methoxy group.

[0012] [4] The coating composition according to any one of [1] to [3], wherein the component (B) is a silicone oligomer having an alkoxy group and an amino group and / or a mercapto group in the molecule.

[0013] [5] The coating agent composition according to any one of [1] to [4], wherein the content of the component (B) is 0.1 to 15 parts by mass per 100 parts by mass of the component (A).

[0014] [6] The coating agent composition according to any one of [1] to [5], wherein the content of the component (C) is 0.1 to 15 parts by mass per 100 parts by mass of the component (A).

[0015] [7] The coating composition according to any one of [1] to [6], wherein the component (D) is a metal alkoxide.

[0016] [8] The coating composition according to any one of [1] to [7], further comprising an organic solvent.

[0017] [9] An outdoor object coated with a cured product of the coating composition according to any one of [1] to [8].

[0018] The present invention provides a coating composition, particularly an outdoor coating composition, which provides a cured product capable of concealing scratches and exhibiting excellent adhesion. The present invention also provides a coating composition which is resistant to peeling and cracking even when subjected to impact. Furthermore, the present invention also provides a coating composition which provides a cured product with excellent flex resistance and weather resistance.

[0019] The present invention will be described in detail below. The present invention is not limited to the following embodiments. Unless otherwise specified, in this specification, operations and measurements of physical properties are performed at room temperature (20°C to 25°C) and a relative humidity of 40% RH to 50% RH. "A and / or B" includes each of A and B and all combinations of one or more of them. Specifically, it refers to at least one of A and B, and also refers to A, B, and combinations of A and B. In this specification, "X to Y" is used to mean "X to Y" and includes the numerical values ​​(X and Y) before and after it as upper and lower limits. When multiple "X to Y" are listed, for example, when "X1 to Y1 or X2 to Y2" is listed, the disclosure of each numerical value as the upper limit, the disclosure of each numerical value as the lower limit, and the combination of the upper and lower limits are all disclosed (i.e., they serve as a legitimate basis for amendment). Specifically, amendments to X1 or more, amendments to Y2 or less, amendments to X1 or less, amendments to Y2 or more, amendments between X1 and X2, amendments between X1 and Y2, etc. must all be deemed lawful.

[0020] One aspect of the present invention provides a coating composition comprising the following components (A) to (D): component (A): a silicone oligomer having only alkoxy groups, phenyl groups, and alkyl groups in the molecule, component (B): a compound having an alkoxy group and an amino group and / or a mercapto group in the molecule, component (C): a silicone oligomer having only alkoxy groups and alkyl groups in the molecule, and component (D): a curing catalyst. This provides a coating composition, particularly a coating composition for outdoor use, in which the cured product (also simply referred to as the "cured product" in this specification) obtained by curing the coating composition (also simply referred to as the "composition" in this specification) can conceal scratches and has excellent adhesion.

[0021] In this specification, a silicon oligomer having a functional group A refers to a silicon oligomer having a main chain skeleton formed of siloxane bonds (Si—O—Si) and functional groups A present at molecular chain terminals, side chains, etc. The silicon oligomer having the functional group A is derived from a silane compound having the functional group A. Specifically, when the silane compound having the functional group A has a hydrolyzable group bonded to a silicon atom, hydrolysis and dehydration condensation reactions proceed, forming siloxane bonds (Si—O—Si), and oligomerization of the silane compound having the functional group A proceeds, thereby obtaining a silicon oligomer having functional groups A at molecular chain terminals, side chains, etc. In one embodiment, the hydrolyzable group may be the functional group A. The functional group A may be one type, or may be composed of two or more types. In one embodiment, of the hydrolyzable groups contained in the silane compound, only a portion of the hydrolyzable groups are used for hydrolysis, and the remaining hydrolyzable groups may remain in the structure of the silicon oligomer.

[0022] In this specification, a silicon oligomer having only functional group A refers to a silicon oligomer that has a main chain skeleton formed of siloxane bonds (Si—O—Si) and also necessarily has only functional group A at the molecular chain terminals, side chains, etc. In one embodiment, the functional group may be of one type, or may be composed of two or more types.

[0023] In this specification, a silicone oligomer having an alkoxy group refers to a silicone oligomer having a main chain skeleton formed of siloxane bonds (Si—O—Si) and alkoxy groups at the molecular chain terminals, side chains, etc. The silicone oligomer having an alkoxy group is a polymer obtained by partially hydrolyzing and partially hydrolyzing and condensing a silane compound having an alkoxy group with a known catalyst such as an acid, a base, or an organotin compound or an organotitanium compound, and is a silicone compound having alkoxy groups derived from the silane compound at the molecular chain terminals, side chains, etc., and having a linear structure, branched structure, or three-dimensional network structure.

[0024] Preferred forms of silane compounds having an alkoxy group for obtaining the above-mentioned silicone oligomer include polyfunctional alkoxysilane compounds such as dialkoxysilane compounds, trialkoxysilane compounds, and tetraalkoxysilane compounds, and monoalkoxysilane compounds (monofunctional alkoxysilane compounds). That is, the above-mentioned silicone oligomer is preferably a partial hydrolysis condensate of an alkoxysilane compound represented by the following formula (1). The alkoxysilane compounds represented by the following formula (1) may be used alone, or two or more types may be used in combination. Furthermore, the silicone oligomer may be used alone, or two or more types may be used in combination.

[0025]

[0026] In the above formula (1), R 1 and R 2 are each independently a group selected from the group consisting of substituted or unsubstituted aliphatic hydrocarbon groups having 1 to 10 carbon atoms and aromatic hydrocarbon groups having 6 to 20 carbon atoms, and x is an integer of 0 to 3. 1 and R 2 are preferably each independently a group selected from the group consisting of substituted or unsubstituted aliphatic hydrocarbon groups having 1 to 5 carbon atoms and aromatic hydrocarbon groups having 6 to 10 carbon atoms, and more preferably are each independently a group selected from the group consisting of a methyl group, an ethyl group, a propyl group, and a phenyl group.

[0027] As used herein, the term "substituted" refers to a hydrogen atom being replaced with another group, such as, but not limited to, a methyl group, an ethyl group, a propyl group, a butyl group, and the like.

[0028] In the above formula (1), x is an integer of 0 to 3. When the alkoxysilane compound represented by the above formula (1) is used alone, x is preferably an integer of 0 to 2, and more preferably 1 or 2. Furthermore, when two or more types of alkoxysilane compounds are used, it is preferable to use in combination at least a first alkoxysilane compound in which x is an integer of 1 to 3 and a second alkoxysilane compound in which x is an integer of 0 to 3 (however, this does not include the case where x = 3 for both the first alkoxysilane compound and the second alkoxysilane compound).

[0029] The component (A) used in the present invention is a silicone oligomer having only alkoxy groups, phenyl groups, and alkyl groups in the molecule. In other words, the component (A) is a silicone oligomer that always has alkoxy groups, phenyl groups, and alkyl groups in the molecule. When the component (A) is such a silicone oligomer, the cured product of the composition of the present invention after curing and drying has excellent adhesion, particularly adhesion to impact and bending, and weather resistance, is less likely to crack even when subjected to impact, and has good scratch concealment properties. The component (A) is a compound represented by the following formula (2):

[0030]

[0031] (In the above formula (2), R 3 is a phenyl group, and R 4 is an alkyl group, and Y is an integer of 1 to 3), and a compound represented by the following formula (3):

[0032]

[0033] (In the above formula (3), R 5 and R 6 is an alkyl group, and Z is an integer of 1 to 3. In one embodiment, component (A) is a partial hydrolysis condensate of an alkoxysilane compound represented by the above formula (2) or formula (3) and a tetraalkoxysilane compound (in the above formula (1), R 1 and R 2are each independently a substituted or unsubstituted aliphatic hydrocarbon group having 1 to 10 carbon atoms, and x=0) and an alkoxysilane compound.

[0034] In addition to the alkoxysilane compounds represented by the above formulas (2) and (3), compounds having both an alkyl group and a phenyl group and represented by the following formula (4):

[0035]

[0036] (In the above formula (4), R 7 is a phenyl group, and R 8 and R 9 The silicone oligomer of component (A) may be synthesized by partial hydrolysis and condensation using one or more alkoxysilane compounds represented by formula (2): (wherein p is an alkyl group, p is an integer of 1 or 2, q is an integer of 1 or 2, and p+q≦3). From the viewpoint of flexibility and adhesion of the cured product, component (A) is preferably a condensate of an alkoxysilane compound represented by formula (2) and an alkoxysilane compound represented by formula (3). In one embodiment, component (A) may be a silicone oligomer obtained from a tetraalkoxysilane compound represented by formula (2), formula (3), or formula (4).

[0037] In one embodiment, R in formula (2) 4 may each independently be a methyl group, an ethyl group, a propyl group, or a butyl group, and from the viewpoint of curability, is preferably a methyl group or an ethyl group, more preferably a methyl group.

[0038] In one embodiment, R in formula (3) 5 and R 6 may each independently be a methyl group, an ethyl group, a propyl group, or a butyl group, and from the viewpoint of adhesion, preferably each independently be a methyl group or an ethyl group, and more preferably both be methyl groups.

[0039] In one embodiment, the alkoxy groups contained in the tetraalkoxysilane compound for obtaining component (A) include, but are not limited to, methoxy, ethoxy, propoxy, and butoxy groups. Of the four alkoxy groups contained in the tetraalkoxysilane compound for obtaining component (A), one or more, two or more, three or more, or all four may be methoxy groups.

[0040] In one embodiment, R in formula (4) 8 and R 9 may each independently be a methyl group, an ethyl group, a propyl group, or a butyl group, and from the viewpoints of curing drying properties, adhesion, and the like, preferably each independently be a methyl group or an ethyl group, and more preferably both be methyl groups.

[0041] The alkoxy group in component (A) is preferably an alkoxy group having 1 to 5 carbon atoms, and more preferably an alkoxy group having 1 to 3 carbon atoms. Examples of the alkoxy group having 1 to 3 carbon atoms include a methoxy group, an ethoxy group, and a propoxy group. From the viewpoint of the curing and drying properties of the composition, and the flexibility and adhesion of the cured product obtained by curing the composition, a methoxy group is preferred.

[0042] The alkyl group in component (A) is preferably an alkyl group having 1 to 5 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms. Examples of the alkyl group having 1 to 3 carbon atoms include, but are not limited to, methyl, ethyl, and propyl groups. From the viewpoints of flexibility and adhesion, a methyl group is preferred.

[0043] The kinematic viscosity of the component (A) at 25°C is 1 to 500 mm 2 s -1 It is preferable that the range is 10 to 350 mm. 2 s -1 and more preferably 15 to 300 mm 2 s -1 and even more preferably 30 to 280 mm 2 s -1 and particularly preferably 50 to 270 mm 2s -1 The kinematic viscosity of the component (A) is 1 mm 2 s -1 By setting the thickness to 500 mm or more, a uniform coating can be formed. 2 s -1 In addition, the kinematic viscosity of the component (A) is 50 mm or less, which is favorable for workability. 2 s -1 When the kinematic viscosity is above 100%, the cured product obtained from the composition of the present invention exhibits particularly excellent weather resistance and can suppress discoloration of the cured product. In this specification, the kinematic viscosity is measured by a viscosity measurement method in accordance with JIS Z 8803:2011. For example, the kinematic viscosity can be measured using a single cylindrical rotational viscometer (B-type viscometer).

[0044] Commercially available products of component (A) include, but are not limited to, KR-401N, KR-510, KR-9218, X-40-9227, and X-40-9312 (manufactured by Shin-Etsu Chemical Co., Ltd.), etc. These may be used alone or in combination of two or more.

[0045] The content of the (A) component may be 10% by weight or more, 15% by weight or more, or 20% by weight or more, and 98% by weight or less, 50% by weight or less, or 40% by weight or less, based on the entire composition. The content of the (A) component may be 10 to 98% by weight, 15 to 50% by weight, or 20 to 40% by weight, based on the entire composition. Furthermore, when the composition of the present invention contains an organic solvent, the content of the (A) component may be 80 to 98% by weight or 90 to 95% by weight, based on the entire composition excluding the organic solvent. When the content of the (A) component is 80 to 98% by weight, based on the entire composition excluding the organic solvent, the cured product obtained from the composition of the present invention has excellent flexibility and is crack-resistant. When two or more components are used, the content of the (A) component refers to the combined total.

[0046] The component (B) used in the present invention is a compound having an alkoxy group and an amino group and / or a mercapto group in the molecule. In one embodiment, the component (B) may be a compound having a silicon atom. In one embodiment, the component (B) may be a silane compound, such as a silane coupling agent having an alkoxy group and an amino group or a mercapto group at the ends of a hydrocarbon chain. Silane compounds that can be used as the component (B) include, but are not limited to, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, and 3-aminopropyltrimethoxysilane. The component (B) may or may not have a main chain structure, and even if it has a main chain structure, the main chain structure is not particularly limited. The component (B) may be a silicone oligomer having an alkoxy group and an amino group and / or a mercapto group on the side chain or terminal of the polysiloxane chain. Among these, a silane compound and / or a silicone oligomer having an amino group is preferred from the viewpoint of excellent drying properties, and a silicone oligomer is even more preferred.

[0047] The alkoxy group in component (B) is preferably an alkoxy group having 1 to 10 carbon atoms, and more preferably an alkoxy group having 1 to 5 carbon atoms. Examples of the alkoxy group in component (B) include, but are not limited to, a methoxy group, an ethoxy group, a propoxy group, and a butoxy group. In terms of excellent long-term weather resistance, a methoxy group or an ethoxy group is preferred, and a methoxy group is even more preferred. Furthermore, component (B) may have an alkoxysilyl group (e.g., a monoalkoxysilyl group, a dialkoxysilyl group, or a trialkoxysilyl group) as a partial structure. The alkoxy group contained in the alkoxysilyl group may be the same as the alkoxy group in component (B).

[0048] The component (B) may contain either an amino group or a mercapto group, or may contain both, but it preferably contains a mercapto group in terms of excellent adhesion.

[0049] In one embodiment, the component (B) is preferably a silicone oligomer or silane compound having an alkyl group, more preferably a silicone oligomer having an alkyl group, and even more preferably a silicone oligomer having a methyl group. When the component (B) has an alkyl group, the cured product obtained from the composition of the present invention exhibits excellent adhesion and weather resistance.

[0050] Commercially available products of component (B) include, but are not limited to, KR-518, KR-519, KBM-573, KBM-603, KBM-803, and KBM-903 (manufactured by Shin-Etsu Chemical Co., Ltd.).

[0051] The content of the component (B) is preferably 0.1 to 15 parts by mass, more preferably 0.5 to 10 parts by mass, and most preferably 0.5 to 5 parts by mass, per 100 parts by mass of the component (A). An amount of 0.1 part by mass or more provides excellent adhesion, while an amount of 15 parts by mass or less minimizes the impact on weather resistance. When two or more types are used, the content of the component (B) refers to the total value.

[0052] The component (C) used in the present invention is a silicone oligomer having only alkoxy groups and alkyl groups in the molecule (excluding component (A)). In other words, the component (C) is a silicone oligomer that always has alkoxy groups and alkyl groups in the molecule. The component (C) is a compound represented by the following formula (5):

[0053]

[0054] (In the above formula (5), R 10 and R 11are each independently an alkyl group, for example, an alkyl group having 1 to 5 carbon atoms (saturated aliphatic hydrocarbon group), and r is an integer of 1 to 3. The compound represented by formula (5) above may be used alone, or multiple types may be used. Component (C) may also be a silicone oligomer obtained from an alkoxysilane compound represented by formula (5) above and a tetraalkoxysilane compound. Furthermore, the silicone oligomer used as component (C) may be used alone, or two or more types may be used in combination. R in formula (5) above 10 Examples of the groups include a methyl group, an ethyl group, a propyl group, and a butyl group. From the viewpoint of adhesion, however, the component (C) is preferably R 10 is a silicone oligomer that is a condensation product of an alkoxysilane compound in which methyl groups can be used.

[0055] The alkoxy group in component (C) is preferably an alkoxy group having 1 to 5 carbon atoms, and more preferably an alkoxy group having 1 to 3 carbon atoms. Examples of the alkoxy group having 1 to 3 carbon atoms include a methoxy group, an ethoxy group, and a propoxy group. From the viewpoints of the curing and drying properties of the composition and the adhesion of the cured product, a methoxy group is preferred.

[0056] The alkyl group in component (C) is preferably an alkyl group having 1 to 5 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms. Examples of the alkyl group having 1 to 3 carbon atoms include methyl, ethyl, and propyl groups, but from the viewpoint of adhesion of the cured product, a methyl group is preferred.

[0057] The kinematic viscosity of the component (C) at 25°C is 1 to 500 mm 2 s -1 It is preferable that the range is 10 to 350 mm. 2 s -1 and more preferably 40 to 200 mm 2 s -1 and more preferably 60 to 90 mm 2 s -1 The kinematic viscosity is 1 mm 2 s -1By setting the thickness to 500 mm or more, a uniform coating can be formed. 2 s -1 The following conditions make work easier.

[0058] Commercially available products of component (C) include, but are not limited to, KC-89S, KR-500, X-40-9225, X-40-9246, and X-40-9250 (manufactured by Shin-Etsu Chemical Co., Ltd.).

[0059] The content of the component (C) is preferably 0.1 to 15 parts by mass, more preferably 0.5 to 10 parts by mass, and most preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the component (A). An amount of 0.1 part by mass or more provides a coating composition with excellent adhesion, and an amount of 15 parts by mass or less provides a coating composition with excellent flexibility and no cracking. When two or more components are used, the content of the component (C) refers to the total value.

[0060] The component (D) used in the present invention is a curing catalyst. Component (D) is a compound that causes the alkoxy groups contained in components (A) to (C) to react with moisture in the air and undergo a condensation reaction. Component (D) can be appropriately selected from conventionally known compounds, such as organotin compounds, organozinc compounds, organotitanium compounds, organozirconium compounds, organoaluminum compounds, organonickel compounds, inorganic acid compounds, organic acid compounds, inorganic base compounds, and organic base compounds, and can be selected from these compounds to meet the required characteristics in terms of reactivity, storage stability, colorability, and the like. These compounds may be used alone or in combination of two or more.

[0061] Examples of the organic tin compound include dibutyltin dilaurate, dibutyltin dioctate, dibutyltin diacetate, dioctyltin dilaurate, dioctyltin dioctate, dioctyltin diacetate, dibutyltin bisacetylacetate, and dioctyltin bisacetyllaurate.

[0062] Examples of organic zinc compounds include zinc triacetylacetonate, zinc-2-ethylhexoate, zinc naphthenate, and zinc stearate.

[0063] Examples of the organic titanium compound include tetrabutyl titanate, tetranonyl titanate, tetrakisethylene glycol methyl ether titanate, tetrakisethylene glycol ethyl ether titanate, and bis(acetylacetonyl)dipropyl titanate.

[0064] Examples of the organic zirconium compound include zirconium tetraacetylacetonate, zirconium tributoxyacetylacetonate, zirconium dibutoxydiacetylacetonate, zirconium tetra-normal propoxide, zirconium tetraisopropoxide, zirconium tetra-normal butoxide, zirconium acylate, zirconium tributoxystearate, zirconium octoate, zirconyl (2-ethylhexanoate), and zirconium (2-ethylhexoate).

[0065] Examples of the organic aluminum compounds include aluminum salt compounds such as aluminum octylate, aluminum triacetate, and aluminum tristearate; aluminum alkoxide compounds such as aluminum trimethoxide, aluminum triethoxide, aluminum triallyloxide, and aluminum triphenoxide; aluminum methoxybis(ethyl acetoacetate), aluminum methoxybis(acetylacetonate), aluminum ethoxybis(ethyl acetoacetate), aluminum ethoxybis(acetylacetonate), aluminum isopropoxybis(ethyl acetoacetate), and aluminum isopropoxybis(methyl acetoacetate); Examples of aluminum chelate compounds include aluminum isopropoxybis(t-butylacetoacetate), aluminum butoxybis(ethylacetoacetate), aluminum dimethoxy(ethylacetoacetate), aluminum dimethoxy(acetylacetonate), aluminum diethoxy(ethylacetoacetate), aluminum diethoxy(acetylacetonate), aluminum diisopropoxy(ethylacetoacetate), aluminum diisopropoxy(methylacetoacetate), aluminum tris(ethylacetoacetate), aluminum tris(acetylacetonate), and aluminum octylacetoacetate diisoproprate.

[0066] As the component (D), it is preferable to use a curing catalyst other than an organotin compound from the viewpoint of legal regulations. Among them, from the viewpoint of achieving both curability and storage stability, a metal alkoxide is more preferable, a titanium alkoxide is more preferable, and tetrabutyl titanate is most preferable.

[0067] The content of the component (D) is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 15 parts by mass, and most preferably 1 to 10 parts by mass, per 100 parts by mass of the component (A). An amount of 0.1 part by mass or more provides a coating agent composition with excellent curability, while an amount of 20 parts by mass or less provides a coating agent composition with excellent storage stability. When two or more types are used, the content of the component (D) refers to the total value.

[0068] The coating composition of the present invention preferably contains an organic solvent from the viewpoint of workability and application properties. The inclusion of an organic solvent allows the components (A) to (D) to be uniformly dissolved or dispersed, and also allows for dilution to form a uniform thin film. The organic solvent is not particularly limited as long as it is a substance that can uniformly dissolve or disperse the components (A) to (D) and is liquid at 25°C and does not react with the components (A) to (D). Examples of the organic solvent include naphthenic hydrocarbons and their halides, paraffinic hydrocarbons and their halides, isoparaffinic hydrocarbons and their halides, ether compounds, alcohol compounds, phenolic compounds, glycol compounds, ketone compounds, ester compounds, and crude oil fractions. When selecting a substance made of a compound that easily absorbs water in a system, such as low-molecular-weight alcohols, ethers, or acetone, it is desirable to use a substance that has been purified by distillation or other methods to remove as much water as possible.

[0069] Preferred examples of the organic solvent include ketone compounds, ester compounds, ether compounds, alcohol compounds, paraffins, isoparaffins, or naphthenic hydrocarbon compounds, or crude oil distillation components, and more preferred are paraffins, isoparaffins, or naphthenic hydrocarbon compounds, or crude oil distillation components. In one embodiment, the organic solvent is preferably a linear or branched saturated hydrocarbon having 5 to 15 carbon atoms, more preferably a linear or branched saturated hydrocarbon having 6 to 14 carbon atoms, and even more preferably a branched saturated hydrocarbon having 6 to 14 carbon atoms. Among these, 2,2,4,6,6-pentamethylheptane can be preferably used as the organic solvent from the viewpoints of workability and coatability.

[0070] The content of the organic solvent is preferably 50 to 90% by mass, more preferably 60 to 80% by mass, and most preferably 65 to 75% by mass, based on the total amount of the coating composition. A content of 50% by mass or more provides a coating composition that is excellent in workability and application, while a content of 90% by mass or less provides a coating composition that is excellent in scratch concealment. When two or more organic solvents are used, the content of the organic solvents refers to the total value.

[0071] In addition to the above-mentioned components, various additives may be added as optional components to the coating composition of the present invention, as needed, within the range that does not impair the effects of the present invention. Examples of additives include silane coupling agents (excluding component (B)), plasticizers, fillers, storage stabilizers, tackifiers, organic or inorganic pigments, rust inhibitors, antifoaming agents, dispersants, surfactants, viscoelasticity adjusters, and thickeners.

[0072] The method for preparing the coating composition of the present invention is not particularly limited, and conventionally known methods can be appropriately employed. For example, predetermined amounts of components (A), (B), (C), (D), and any optional components are weighed and added to a stirring vessel sequentially or simultaneously in any order, and then mixed using a mixing means such as a three-one motor, preferably while vacuum degassing. Preferably, component (D) is added last. Adding component (D) last can prevent the curing reaction from proceeding at an undesired stage. The mixing temperature is preferably 10 to 50°C, and the mixing time is preferably 0.1 to 5 hours.

[0073] The coating composition of the present invention may be applied by any known method, without any particular limitations. Examples include hand application using fibers impregnated with the composition, brush application, and machine application using an automated machine. Preferably, a suitable amount of the coating composition of the present invention is impregnated into fibers such as a dried sponge or rag, and the impregnated coating composition is manually spread thinly over the surface of a steel plate or coated plate. Volatilization of volatile components is then achieved by natural drying or forced drying using a dryer or the like. During this process, reactive components (A) to (C) contained in the coating composition come into contact with moisture in the air, and a hydrolysis reaction proceeds due to the action of component (D). Concurrently with the evaporation of volatile components, crosslinking and curing occur on the steel plate or coated plate, forming a cured product. In one embodiment, the cured product obtained by curing the coating composition may contain a portion of the organic solvent remaining in the cured product without volatilization.

[0074] The coating composition applied by the above application method preferably has a film thickness after drying of 1 to 15 μm, more preferably 2 to 10 μm, and most preferably 4 to 7 μm. If it is 1 μm or more, it will have excellent scratch concealing properties, and if it is 15 μm or less, the coating will not crack due to impact or bending.

[0075] The coating composition of the present invention can be applied to substrates such as various metals, glass, ceramics, resins, and color steel plates. Since it has excellent adhesion to impacts and conceals scratches, it is particularly suitable for outdoor installations such as signs, labels, and vending machines. In one embodiment of the present invention, an outdoor installation coated with a cured product of the coating composition is also provided.

[0076] Although the embodiments of the present invention have been described in detail, it is clear that this is for illustrative and exemplary purposes only and not for limitation, and that the scope of the present invention should be interpreted by the appended claims.

[0077] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples. Furthermore, unless otherwise specified, tests were conducted in an environment of 25°C and 55% RH. [Examples 1 to 7 and Comparative Examples 1 to 9] The following components were prepared to prepare coating compositions. Hereinafter, the coating composition will also be simply referred to as the composition.

[0078] Component (A): Silicone oligomer having only alkoxy, phenyl, and alkyl groups in the molecule. X-40-9312 (Silicone oligomer having methoxy, methyl, and phenyl groups). Kinematic viscosity: 250 mm 2 s -1 Shin-Etsu Chemical Co., Ltd.) X-40-9227 (silicone oligomer having methoxy, methyl, and phenyl groups, kinematic viscosity: 15 mm 2 s -1 Shin-Etsu Chemical Co., Ltd.) KR-401N (silicone oligomer having methoxy, methyl, and phenyl groups, kinematic viscosity: 20 mm 2 s -1Shin-Etsu Chemical Co., Ltd.) KR-9218 (silicone oligomer having methoxy, methyl, and phenyl groups, kinematic viscosity: 40 mm 2 s -1 (Manufactured by Shin-Etsu Chemical Co., Ltd.) Component (A') or (C): Silicone oligomer other than component (A) KC-89S (Silicone oligomer having methoxy and methyl groups) Kinematic viscosity: 5 mm 2 s -1 Shin-Etsu Chemical Co., Ltd.) X-40-9225 (silicone oligomer having methoxy and methyl groups, kinematic viscosity: 100 mm 2 s -1 Shin-Etsu Chemical Co., Ltd.) X-40-9246 (silicone oligomer having methoxy and methyl groups, kinematic viscosity: 80 mm 2 s -1 (Manufactured by Shin-Etsu Chemical Co., Ltd.) Component (A'): Silicone oligomer other than component (A) KR-516 (Silicone oligomer having methoxy groups, methyl groups, and epoxy groups) Kinematic viscosity: 50 mm 2 s -1(Manufactured by Shin-Etsu Chemical Co., Ltd.) Component (B): a compound having an alkoxy group and at least one functional group selected from the group consisting of an amino group and a mercapto group in the molecule (excluding component (A)) KR-519 (a silicone oligomer having a methoxy group, a methyl group, and a mercapto group, manufactured by Shin-Etsu Chemical Co., Ltd.) KR-518 (a silicone oligomer having a methoxy group, an ethoxy group, and a mercapto group, manufactured by Shin-Etsu Chemical Co., Ltd.) KBM-803 (3-mercaptopropyltrimethoxysilane, a silane compound having a methoxy group and a mercapto group) KBM-603 (N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, a silane compound having a methoxy group and an amino group) Component (B'): a silane compound that does not contain at least one of an amino group and a mercapto group X-40-9296 (a silicone oligomer having a methoxy group, a methyl group, and a methacryl group, manufactured by Shin-Etsu Chemical Co., Ltd.) KR-511 (silicone oligomer having methoxy groups, phenyl groups, and vinyl groups, manufactured by Shin-Etsu Chemical Co., Ltd.) KR-513 (silicone oligomer having methoxy groups, methyl groups, and acrylic groups, manufactured by Shin-Etsu Chemical Co., Ltd.) X-41-1059A (silicone oligomer having methoxy groups, ethoxy groups, and epoxy groups, manufactured by Shin-Etsu Chemical Co., Ltd.) Component (C): silicone oligomer having only alkoxy groups and alkyl groups in the molecule (excluding components (A) and (B)) X-40-9250 (silicone oligomer having methoxy groups and methyl groups, kinematic viscosity: 80 mm 2 s -1 (manufactured by Shin-Etsu Chemical Co., Ltd.) Component (D): Curing catalyst - tetrabutyl titanate Organic solvent - 2,2,4,6,6-pentamethylheptane (isoparaffinic hydrocarbon compound) The compositions of Examples 1 to 7 and Comparative Examples 1 to 9 were produced as follows: Components (A) to (D) and the organic solvent were weighed and stirred for 15 minutes using a Three-One Motor manufactured by Shinto Scientific Co., Ltd. to obtain coating agent compositions. Detailed amounts prepared are shown in Tables 1 and 2, and all values ​​are expressed in parts by mass.

[0079] <Drying Time (minutes)> 2 ml of the composition was soaked into tissue paper. Next, the composition was uniformly applied to the entire white-painted surface of a white-painted plate (material: SPCC-SD (cold-rolled steel plate), standard: JIS G 3141:2017, dimensions: 0.8 mm × 70 mm × 150 mm, electrochemically electrodeposited and then coated with a white amino alkyd paint on one side, no clear coat, manufactured by Asahi B-Techno Co., Ltd.) using the tissue paper so that the coating thickness after drying was about 5 μm, and this was used as a test piece (in this specification, the "coating film after drying" refers to the film-like cured product of the composition and is also simply referred to as the "coating film"). Thereafter, the test piece was placed on a pedestal with its long side facing vertically against a wall, and left in an environment of 25 ° C. and 55% RH. The time until drying was measured to test the curing and drying properties. After the composition was applied to the coated surface of a test piece positioned 1 cm or more above the base, measurements were taken at 1-minute intervals on different coated surfaces to evaluate drying properties (i.e., "curing drying properties"; in this specification, "curing drying" is also simply referred to as "drying"). Drying time was measured in accordance with JIS K 5600-3-3:1999. Whether or not the test piece was in a dry state was determined by a method conforming to the tack-dry test of JIS K 5600-1-1:1999. The drying time is preferably within 60 minutes, more preferably within 30 minutes, and particularly preferably within 25 minutes.

[0080] <Tape Peeling Test> The composition was applied to a white-coated panel using the same method as in the drying time measurement. The composition was left to dry for 24 hours under conditions of 25°C and 55% RH. Approximately 3 cm of adhesive tape (cellophane tape, manufactured by Nichiban Co., Ltd.) was attached to the inner surface of the coating film of the prepared test piece, within 1 cm of the inner surface. The adhesive tape was then peeled off, and the white-coated panel was visually inspected to determine whether the coating film had been peeled off from the white-coated panel by the adhesive tape, using the following evaluation criteria.

[0081] Evaluation criteria: ◯: no peeling; ×: peeling.

[0082] <Scratch Concealment Test> The black painted surface of a black painted plate (material: SPCC-SD (cold rolled steel plate), standard: JIS G 3141:2017, dimensions: 0.8 mm × 70 mm × 150 mm, one side of which was coated with a black amino alkyd paint after chemical electrodeposition, with a clear coat, manufactured by Asahi B-Techno Co., Ltd.) was scratched with #40 sandpaper. The scratched area was cleaned with alcohol and allowed to dry, and then a composition was applied over the scratch using the same method as in the drying time measurement described above, and allowed to dry for 24 hours in an environment of 25°C and 55% RH. After curing, the test piece was placed upright against a wall with the long side vertical, and scratches made to the test piece were visually confirmed from a distance of 1 m from the test piece according to the following evaluation criteria. By making the scratches invisible, the design is also excellent.

[0083] Evaluation criteria: ◯: Scratches are visible; ×: Scratches are not visible.

[0084] <Impact Peeling Test> A composition was applied to a steel plate (SPCC-SD (cold-rolled steel plate), standard: JIS G 3141:2017, dimensions: 0.8 mm x 70 mm x 150 mm) using the same method as for the drying time measurement. The drying conditions were to leave the plate to stand for 24 hours in an environment of 25°C and 55% RH. A weight drop resistance test was performed on the coated surface of the prepared test piece using a DuPont impact tester manufactured by Tester Sangyo, and the coating film was visually inspected according to the following evaluation criteria. The test was performed with a weight height of 500 mm and a weight mass of 500 g. Details of the test method follow JIS K 5600-5-3:1999.

[0085] Evaluation criteria: ◯: No peeling or cracking of the coating film; ×: Peeling or cracking of the coating film was observed.

[0086] <Bending Test> Test specimens were prepared using the same method as in the impact peel test. The test specimens were left to stand for 24 hours under drying conditions of 25°C and 55% RH. The prepared test specimens were subjected to a mandrel bending test using a mandrel bending tester manufactured by Ueshima Seisakusho, and the coating film was evaluated according to the following evaluation criteria. The diameter of the mandrel used was φ3 / 8 inches. Detailed test methods were in accordance with JIS K 5600-5-1:1999.

[0087] Evaluation criteria: ◯: No peeling or cracking of the coating film; ×: Peeling or cracking of the coating film was observed.

[0088] <Weather Resistance Test> The composition was applied to a white-painted panel using the same method as in the drying time measurement. The drying conditions were 25°C, 55% RH, and the panel was left to stand for 24 hours. The prepared test specimens were subjected to an accelerated weather resistance test using a xenon weather meter NX75 manufactured by Suga Test Instruments, and the coating film after 1000 hours and 2000 hours was evaluated according to the following evaluation criteria. The details of the tester were in accordance with JIS B 7754:1991, and the test method was in accordance with JIS D 0205:1987.

[0089] Evaluation criteria: ⊚: No peeling or cracking of the coating film after 2000 hours; ◯: No peeling or cracking of the coating film after 1000 hours (except for the case of ⊚); ×: Peeling or cracking of the coating film was observed after 1000 hours.

[0090]

[0091]

[0092] Examples 1 to 7 were compositions containing components (A) to (D), and were confirmed to have excellent scratch concealing properties, adhesion, and weather resistance. Furthermore, compositions using a silicone oligomer as component (B) were confirmed to have superior drying times. On the other hand, Comparative Examples 1 to 3 were compositions containing component (A') (or component (C)) instead of component (A), and Comparative Example 4 was a composition containing component (A') instead of component (A). However, these compositions exhibited poor impact resistance and flex resistance, and some exhibited peeling due to coating deformation during weather resistance testing. The composition of Comparative Example 5, which did not contain component (A), also exhibited poor adhesion in a flex test, and peeling of the coating film was confirmed. Comparative Examples 6 to 9 were compositions containing component (B') instead of component (B). In all cases, peeling or lifting of the coating film was confirmed during a tape peel test, resulting in poor adhesion to the coated plate. Furthermore, in Examples 1 and 5 to 7, no discoloration was observed in the coating film even after 2000 hours of accelerated weather resistance testing, demonstrating excellent weather resistance.

[0093] The coating composition of the present invention has excellent adhesion, particularly excellent adhesion against impact and bending, and can be applied to substrates such as various metals, glasses, ceramics, resins, etc. Furthermore, because it has scratch concealing properties, it is suitable for use on signs, labels, vending machines, and other items that are installed outdoors.

[0094] This application is based on Japanese Patent Application No. 2022-162524, filed on October 7, 2022, the disclosure of which is incorporated herein by reference in its entirety.

Claims

1. A coating composition comprising the following components (A) to (D): Component (A): a silicone oligomer having only alkoxy groups, phenyl groups, and alkyl groups in the molecule; Component (B): a compound having an alkoxy group and an amino group and / or a mercapto group in the molecule; Component (C): a silicone oligomer having only alkoxy groups and alkyl groups in the molecule; and Component (D): a curing catalyst.

2. The coating composition according to claim 1, wherein the alkyl group in component (A) is a methyl group.

3. The coating composition according to claim 1 or 2, wherein the alkoxy group in component (A) is a methoxy group.

4. The coating composition according to claim 1 or 2, wherein component (B) is a silicone oligomer having an alkoxy group, an amino group and / or a mercapto group in the molecule.

5. The coating composition according to claim 1 or 2, wherein the content of the component (B) is 0.1 to 15 parts by mass per 100 parts by mass of the component (A).

6. The coating composition according to claim 1 or 2, wherein the content of the component (C) is 0.1 to 15 parts by mass per 100 parts by mass of the component (A).

7. The coating composition according to claim 1 or 2, wherein the component (D) is a metal alkoxide.

8. The coating composition according to claim 1 or 2, further comprising an organic solvent.

9. An outdoor object coated with a cured product of the coating composition according to claim 1 or 2.