Stretched polyethylene film, packaging material, and food packaged body

MYPI2025001857A0Undetermined Publication Date: 2024-03-30RM TOHCELLO CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025001857
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-30
Filing Date
2023-09-26
Publication Date
2024-03-30

AI Technical Summary

Technical Problem

Packaging films face challenges in recycling due to complex multilayer structures, which compromise their recyclability despite achieving desired properties like strength and gas barrier properties.

Method used

A stretched polyethylene film with a three-layer structure comprising high-density polyethylene and medium-density polyethylene layers, optimized for improved flexibility through specific density, melt flow rate, and thermal properties, allowing for enhanced recyclability while maintaining performance.

Benefits of technology

The solution provides a flexible packaging film with improved puncture resistance, bending resistance, and tear strength, facilitating easier recycling and maintaining performance balance of transparency, rigidity, and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025001857_DRAWING_001
    Figure PI2025001857_DRAWING_001
Patent Text Reader

Abstract

A stretched polyethylene film includes a high density polyethylene layer 1 (101), a medium density polyethylene layer (102), and a high density polyethylene layer 2 (103) in this order, and when a first differential scanning calorimetry (1st Run) including a process of raising the temperature from -50°C to 200°C at a temperature rising rate of 10°C / min, an isothermal process of holding the temperature at 200°C for 10 minutes, and a process of lowering the temperature from 200°C to -50°C at a temperature falling rate of 10°C / min, and a second differential scanning calorimetry (2nd Run) including a process of raising the temperature from -50°C to 200°C at a temperature rising rate of 10°C / min are continuously performed using a differential scanning calorimeter, in a DSC curve 1 obtained by the first differential scanning calorimetry, an endothermic peak A is observed in a range of equal to or higher than 10°C and equal to or lower than 160°C, and an amount of heat of fusion (ΔHm) of the endothermic peak A is equal to or more than 110 J / g and equal to or less than 162 J / g.
Need to check novelty before this filing date? Find Prior Art

Description

Stretched polyethylene film, packaging material and food packaging body

[0001] The present invention relates to a stretched polyethylene film, a packaging material, and a food package.

[0002] In the field of packaging films, attempts to improve various performances by devising materials used, layer structures, etc. are known.

[0003] Patent Document 1 discloses a laminated film that includes a base layer and a heat seal layer, has a stiffness of 70 mN or more in the TD direction measured under conditions of a loop length of 50 mm and a push-in length of 10 mm, and has a polyethylene content of 90 mass% or more, and describes that this laminated film can be recycled and can fully ensure the self-supporting properties of a standing pouch.

[0004] Patent Document 2 discloses a polyethylene laminate for use in packaging materials, which comprises at least an oriented polyethylene film, an adhesive layer, and a heat-sealable polyethylene layer, wherein the adhesive layer contains a solvent-free adhesive, and the oriented polyethylene film contains at least one of high-density polyethylene (HDPE) and medium-density polyethylene (MDPE), and describes that this polyethylene laminate for use in packaging materials can significantly reduce the burden on the environment, and has high printability and strength.

[0005] Patent Document 3 discloses a polyethylene co-extruded film comprising a polyethylene film substrate and a polyethylene film layer, wherein the polyethylene film substrate is an electron beam irradiated layer containing polyethylene, a light stabilizer, and a crosslinking agent, and the polyethylene film layer contains polyethylene, and the surface opposite to the surface on which the polyethylene film substrate is provided has heat-sealability. It is described that this polyethylene co-extruded film can suppress deterioration over time and further has improved heat resistance and strength.

[0006] Patent Document 4 describes a multilayer film in which a gas barrier layer formed by applying a dispersion containing an inorganic layered compound and a water-soluble polymer onto at least one surface of a base layer made of a thermoplastic resin, an overcoat layer containing a cationic resin and a resin having a hydroxyl group, an adhesive layer, and a sealant layer are laminated in this order, and it is described that this multilayer film has excellent heat sealability and gas barrier properties.

[0007] JP 2022-053864 A JP 2022-079510 A JP 2018-008455 A JP 2009-241359 A

[0008] With the recent rise in environmental awareness, particularly the focus on the problem of marine plastic pollution, packaging films have come under scrutiny from society. This has led to a greater demand than ever before for the promotion of packaging film recycling. In other words, there is a growing demand for packaging films to be designed and manufactured with "ease of recycling" in mind.

[0009] Many conventional packaging films have achieved desired effects (strength, gas barrier properties, etc.) by laminating multiple materials. For example, the multilayer film described in Patent Document 4 has at least four layers: a gas barrier layer, an overcoat layer, an adhesive layer, and a sealant layer. However, laminating multiple materials has led to difficulties in recycling. From the perspective of facilitating the recycling of packaging films, for example, it is conceivable to make the packaging film have as simple a layer structure as possible.

[0010] In terms of simplifying the layer structure, the ultimate goal is to make the packaging film "single-layer." Furthermore, there are examples such as Patent Documents 1 to 3, in which a multi-layer structure in which a single material is blended at a high content overall is used to facilitate recycling, even if the film is not single-layer. The present inventors conducted a preliminary study on various properties that may be required of packaging films using polyethylene film, a relatively low-cost and general-purpose packaging material. As a result of the study, it was found that polyethylene "single-layer" films have poor flexibility.

[0011] The present invention provides a stretched polyethylene film having improved flexibility and a packaging material constructed from such a stretched polyethylene film.

[0012] [1] A stretched polyethylene film comprising, in this order, a high-density polyethylene layer 1, a medium-density polyethylene layer, and a high-density polyethylene layer 2, wherein, when a first differential scanning calorimetry (1st Run) consisting of a process of increasing the temperature from -50°C to 200°C at a heating rate of 10°C / min, an isothermal process of maintaining the temperature at 200°C for 10 minutes, and a process of decreasing the temperature from 200°C to -50°C at a heating rate of 10°C / min, and a second differential scanning calorimetry (2nd Run) consisting of a process of increasing the temperature from -50°C to 200°C at a heating rate of 10°C / min, are successively performed using a differential scanning calorimeter, an endothermic peak A is observed in a range of 10°C to 160°C in DSC curve 1 obtained by the first differential scanning calorimetry, and the heat of fusion of the endothermic peak A (ΔH m [2] The density of the medium-density polyethylene layer measured in accordance with JIS K 7112:1999 is 910 kg / m 3 More than 935kg / m 3 [3] The stretched polyethylene film according to [1] or [2], wherein the amorphous thickness, determined from peaks in the MD direction at a diffraction angle 2θ of 0.2 to 0.4° by small-angle X-ray scattering (SAXS) measurement, is less than 12.5 nm. [4] The stretched polyethylene film according to any one of [1] to [3], wherein the total amount of high-density polyethylene layer 1 and high-density polyethylene layer 2 in the stretched polyethylene film is 25% by mass or more and 85% by mass or less, when the entire stretched polyethylene film is taken as 100% by mass. [5] The density of high-density polyethylene layer 1 and high-density polyethylene layer 2, measured in accordance with JIS K 7112:1999, is 940 kg / m or less. 3 More than 970kg / m 3[6] The stretched polyethylene film according to any of [1] to [5], wherein the high-density polyethylene layer 1 and the high-density polyethylene layer 2 each have an MFR of 0.01 g / 10 min or more and 20 g / 10 min or less, as measured in accordance with ASTM D1238 at 190°C under a load of 2.16 kg. [7] The stretched polyethylene film according to any of [1] to [6], wherein the medium-density polyethylene layer has an MFR of 0.01 g / 10 min or more and 20 g / 10 min or less, as measured in accordance with ASTM D1238 at 190°C under a load of 2.16 kg. [8] The stretched polyethylene film according to any one of [1] to [7], wherein the stretched polyethylene film has a peak full width at half maximum (FWHM) of 0.21° or less in the MD diffraction angle 2θ range of 0.2 to 0.4° as determined by small-angle X-ray scattering (SAXS) measurement. [9] The stretched polyethylene film according to any one of [1] to [8], wherein the stretched polyethylene film has a haze of 16.0% or less per sheet as measured in accordance with JIS K 7136:2000.

[10] The stretched polyethylene film has a TD tensile modulus T of 16.0% or less as measured in accordance with JIS K7127:1999 using a tensile tester under conditions of a measurement temperature of 23±2°C, 50±5% RH, and a pulling rate of 5 mm / min. 2

[11] The stretched polyethylene film according to any one of [1] to [9], wherein the tensile modulus T in the MD direction of the stretched polyethylene film is measured in accordance with JIS K7127:1999 using a tensile tester under conditions of a measurement temperature of 23±2°C, 50±5% RH, and a pulling rate of 5 mm / min. 1 and the tensile modulus in the TD direction T 2The stretched polyethylene film according to any one of [1] to

[10] , wherein the sum of the values ​​of tensile strength (V) and compressive strength (V) is 1500 MPa or more and 2900 MPa or less.

[12] The stretched polyethylene film according to any one of [1] to

[11] , wherein the stretched polyethylene film has a heat shrinkage rate in the MD direction of 6.0% or less when heat-treated at 100°C for 15 minutes in accordance with JIS C2151:2019.

[13] The stretched polyethylene film according to any one of [1] to

[12] , wherein the stretched polyethylene film has a heat shrinkage rate in the MD direction of 25.0% or less when heat-treated at 120°C for 15 minutes in accordance with JIS C2151:2019.

[14] The stretched polyethylene film according to any one of [1] to

[13] , wherein at least one surface of the stretched polyethylene film is a corona-treated surface.

[15] The stretched polyethylene film according to any one of [1] to

[14] , wherein the stretched polyethylene film has a laminate strength in the machine direction of 0.7 N / 15 mm or more and 10.0 N / 15 mm or less, as measured using a tensile tester under conditions of T-peel and a crosshead speed of 300 mm / min in accordance with JIS Z 0238: 1998.

[16] The stretched polyethylene film has a pinhole count of 2500 / m, as measured after 3000 bending tests using a Gelbo flex tester at a bending angle of 440°, a bending speed of 40 times / min, and an atmosphere of -30°C. 2The stretched polyethylene film according to any one of [1] to

[15] , wherein the stretched polyethylene film has a tear strength in the MD direction of 100 mN or more and 600 mN or less, as measured using a light-load tear tester under the following conditions: test piece size: MD direction: 63.5 mm, TD direction: 50.0 mm, pendulum weight: 96.09 g, tear length: 12.7 mm, and pendulum lift angle: 90°.

[18] The stretched polyethylene film according to any one of [1] to

[17] , wherein the stretched polyethylene film has a total thickness of 10 μm or more and 100 μm or less.

[19] The stretched polyethylene film according to any one of [1] to

[18] , which is a food packaging film.

[20] A packaging material using the stretched polyethylene film according to any one of [1] to

[19] .

[21] A food package comprising the packaging material according to

[20] and food inside the packaging material.

[0013] According to the present invention, a stretched polyethylene film having improved flexibility can be provided.

[0014] FIG. 1 is a cross-sectional view schematically illustrating an example of the structure of a stretched polyethylene film according to an embodiment of the present invention.

[0015] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. In this specification, unless otherwise specified, the numerical range "A to B" indicates A or more and B or less.

[0016] <Stretched Polyethylene Film> The stretched polyethylene film (100) according to this embodiment comprises a high-density polyethylene layer 1 (101), a medium-density polyethylene layer (102), and a high-density polyethylene layer 2 (103) in this order. When a first differential scanning calorimetry (1st Run) consisting of a process of increasing the temperature from -50°C to 200°C at a heating rate of 10°C / min, an isothermal process of maintaining the temperature at 200°C for 10 minutes, and a process of decreasing the temperature from 200°C to -50°C at a heating rate of 10°C / min, and a second differential scanning calorimetry (2nd Run) consisting of a process of increasing the temperature from -50°C to 200°C at a heating rate of 10°C / min, are successively performed using a differential scanning calorimeter, an endothermic peak A is observed in the range of 10°C to 160°C in DSC curve 1 obtained by the first differential scanning calorimetry, and the heat of fusion of the endothermic peak A (ΔH m ) is 110 J / g or more and 162 J / g or less.

[0017] According to the investigations of the present inventors, a three-layer structure including a high-density polyethylene layer 1, a medium-density polyethylene layer, and a high-density polyethylene layer 2 in this order was used, and the heat of fusion (ΔH m It has been found that flexibility can be improved by setting the tensile strength (T) to the above range. In this specification, flexibility is expressed by puncture resistance, bending resistance, and tear strength, and can be evaluated by the balance of performance among puncture resistance, bending resistance, and tear strength. In this specification, flexibility means that the film is flexible yet resistant to breaking and tearing.

[0018] In the stretched polyethylene film of this embodiment, the heat of fusion (ΔH mFrom the viewpoint of further suppressing thickness unevenness of the stretched polyethylene film, the heat of fusion (ΔH m ) is measured as follows. A test piece of about 5.0 mg is cut out from a stretched polyethylene film. Next, using a differential scanning calorimeter, the test piece is subjected to a first differential scanning calorimetry (1st Run) consisting of a process of heating from -50°C to 200°C at a heating rate of 10°C / min, an isothermal process of maintaining the temperature at 200°C for 10 minutes, and a process of cooling from 200°C to -50°C at a heating rate of 10°C / min, followed by a second differential scanning calorimetry (2nd Run) consisting of a process of heating from -50°C to 200°C at a heating rate of 10°C / min. In the DSC curve 1 obtained by the first differential scanning calorimetry, the heat of fusion (ΔH m ) (J / g) is calculated. Here, the calorific value of the endothermic peak A is calculated by determining the area enclosed by the melting endothermic curve including the endothermic peak A and the baseline. The baseline is defined as a line connecting the point where the change in the Deriv. Heat Flow begins (i.e., the point where the flat region of the Deriv. Heat Flow ends) and the point where the change in the Deriv. Heat Flow ends (i.e., the point where the Deriv. Heat Flow enters the flat region) before and after the endothermic peak A. In addition, when multiple endothermic peaks are observed in the range of 10°C to 160°C, the maximum peak is defined as the endothermic peak A.

[0019] The materials constituting the stretched polyethylene film will be described below.

[0020] In the stretched polyethylene film according to the present embodiment, the density of the medium-density polyethylene layer, measured in accordance with JIS K 7112:1999, is preferably 910 kg / m from the viewpoint of making the amorphous thickness of the stretched polyethylene film a predetermined value or less and further improving the flexibility of the stretched polyethylene film. 3 More preferably, 913 kg / m 3 More preferably, 915 kg / m 3 or more, and preferably 935 kg / m 3 or less, more preferably 933 kg / m 3 More preferably, 932 kg / m or less 3 More preferably, 930 kg / m or less 3 More preferably, 928 kg / m or less 3 More preferably, 925 kg / m or less 3 More preferably, 922 kg / m or less 3 More preferably, 920 kg / m or less 3 In the stretched polyethylene film according to the present embodiment, the density of the medium-density polyethylene layer measured in accordance with JIS K 7112:1999 is preferably 917 kg / m or less, from the viewpoint of further improving the balance of flexibility and thermal dimensional stability. 3 More preferably, 918 kg / m 3 That's all.

[0021] According to the stretched polyethylene film of this embodiment, the medium-density polyethylene layer has a three-layer structure sandwiched between high-density polyethylene layer 1 and high-density polyethylene layer 2, and by setting the density of the medium-density polyethylene layer within the above range, flexibility can be further improved.

[0022] The density of the medium-density polyethylene constituting the medium-density polyethylene layer, measured in accordance with JIS K 7112:1999, is preferably 910 kg / m from the viewpoint of making the amorphous thickness of the stretched polyethylene film a predetermined value or less and further improving flexibility. 3 More preferably, 913 kg / m 3 More preferably, 915 kg / m 3and preferably 935 kg / m 3 or less, more preferably 933 kg / m 3 More preferably, 932 kg / m or less 3 More preferably, 930 kg / m or less 3 More preferably, 928 kg / m or less 3 More preferably, 925 kg / m or less 3 More preferably, 922 kg / m or less 3 More preferably, 920 kg / m or less 3 The following is the result.

[0023] The melt flow rate (MFR) of the medium-density polyethylene layer, measured in accordance with ASTM D1238 under conditions of 190°C and a load of 2.16 kg, is preferably 0.01 g / 10 min or more, more preferably 0.1 g / 10 min or more, even more preferably 0.5 g / 10 min or more, and still more preferably 1.0 g / 10 min or more, from the viewpoint of further improving processability; and from the viewpoint of improving the stiffness of the stretched polyethylene film while maintaining the tearability of the stretched polyethylene film, is preferably 20 g / 10 min or less, more preferably 10 g / 10 min or less, even more preferably 5 g / 10 min or less, even more preferably 4 g / 10 min or less, and still more preferably 3 g / 10 min or less.

[0024] The melting point of the medium-density polyethylene layer, as measured by a differential scanning calorimeter (DSC), is preferably 110°C or higher, more preferably 115°C or higher, from the viewpoint of improving heat resistance and stiffness while maintaining processability and adhesiveness, and is preferably 135°C or lower, more preferably 130°C or lower, even more preferably 128°C or lower, and even more preferably 125°C or lower, from the viewpoint of improving adhesiveness while maintaining heat resistance.

[0025] The melt flow rate (MFR) of the medium-density polyethylene constituting the medium-density polyethylene layer, measured in accordance with ASTM D1238 under conditions of 190°C and a load of 2.16 kg, is preferably 0.01 g / 10 min or more, more preferably 0.1 g / 10 min or more, even more preferably 0.5 g / 10 min or more, and still more preferably 1.0 g / 10 min or more, from the viewpoint of further improving processability; and from the viewpoint of improving the stiffness of the stretched polyethylene film while maintaining the tearability of the stretched polyethylene film, is preferably 20 g / 10 min or less, more preferably 10 g / 10 min or less, even more preferably 5 g / 10 min or less, even more preferably 4 g / 10 min or less, and still more preferably 3 g / 10 min or less.

[0026] The melting point of the medium-density polyethylene constituting the medium-density polyethylene layer, as measured by a differential scanning calorimeter (DSC), is preferably 110°C or higher, more preferably 115°C or higher, from the viewpoint of improving heat resistance and stiffness while maintaining processability and adhesiveness, and is preferably 135°C or lower, more preferably 130°C or lower, even more preferably 128°C or lower, and even more preferably 125°C or lower, from the viewpoint of improving adhesiveness while maintaining heat resistance.

[0027] When two or more types of polyethylene are used as the polyethylene constituting the medium-density polyethylene layer, the density, MFR, and melting point of the medium-density polyethylene layer can be measured values ​​for a mixture obtained by melt-blending two or more types of polyethylene by a known method. The melting point of the medium-density polyethylene layer can be the peak temperature of the maximum melting peak.

[0028] From the viewpoint of making the amorphous thickness of the stretched polyethylene film a predetermined value or less and further improving flexibility, the content of medium-density polyethylene in the medium-density polyethylene layer is preferably 80% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, and still more preferably 98% by mass or more, relative to the entire medium-density polyethylene layer. There is no upper limit to the content of medium-density polyethylene in the medium-density polyethylene layer, but it is, for example, 100% by mass or less.

[0029] In the stretched polyethylene film according to the present embodiment, the total amount of high-density polyethylene layer 1 and high-density polyethylene layer 2 is preferably 25% by mass or more, more preferably 30% by mass or more, even more preferably 35% by mass or more, even more preferably 40% by mass or more, and still more preferably 45% by mass or more, based on the total amount of the stretched polyethylene film, from the viewpoint of further improving the performance balance among transparency, rigidity, heat resistance, slip property, heat-fusion strength, and flexibility; and from the viewpoint of setting the amorphous thickness of the stretched polyethylene film to a predetermined value or less and further improving the flexibility of the stretched polyethylene film, the total amount is preferably 85% by mass or less, more preferably 83% by mass or less, even more preferably 80% by mass or less, even more preferably 70% by mass or less, even more preferably 65% ​​by mass or less, and still more preferably 60% by mass or less.

[0030] In the stretched polyethylene film of the present embodiment, the high-density polyethylene layer 1 and the high-density polyethylene layer 2 may be formed using the same material or different materials. However, when different materials are used, it is preferable that the high-density polyethylene layer 1 and the high-density polyethylene layer 2 satisfy the following configuration.

[0031] From the viewpoint of further improving the balance of transparency, rigidity, heat resistance, slip properties, and heat fusion strength, the content of high-density polyethylene in the high-density polyethylene layer 1 and the high-density polyethylene layer 2 is preferably 80% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, and even more preferably 98% by mass or more, based on the total content of each of the high-density polyethylene layer 1 and the high-density polyethylene layer 2. There is no upper limit to the content of high-density polyethylene in the high-density polyethylene layer 1 and the high-density polyethylene layer 2, but it is, for example, 100% by mass or less.

[0032] The densities of the high-density polyethylene layer 1 and the high-density polyethylene layer 2, as measured in accordance with JIS K 7112:1999, are preferably 940 kg / m, respectively, from the viewpoint of achieving a better balance of various properties such as heat resistance, transparency, mechanical properties, and rigidity.3 More preferably, 943 kg / m 3 More preferably, 945 kg / m 3 or more, and from the viewpoint of achieving a better balance between flexibility and rigidity, it is preferably 970 kg / m 3 or less, more preferably 968 kg / m 3 More preferably, 965 kg / m or less 3 More preferably, 960 kg / m or less 3 More preferably, 955 kg / m or less 3 More preferably, 950 kg / m or less 3 The following is the result.

[0033] The density of the high-density polyethylene constituting the high-density polyethylene layer 1 and the high-density polyethylene layer 2, as measured in accordance with JIS K 7112:1999, is preferably 940 kg / m, from the viewpoint of achieving a better balance of various properties such as heat resistance, transparency, mechanical properties, and rigidity. 3 More preferably, 943 kg / m 3 More preferably, 945 kg / m 3 or more, and from the viewpoint of achieving a better balance between flexibility and rigidity, it is preferably 970 kg / m 3 or less, more preferably 968 kg / m 3 More preferably, 965 kg / m or less 3 More preferably, 960 kg / m or less 3 More preferably, 955 kg / m or less 3 More preferably, 950 kg / m or less 3 The following is the result.

[0034] The melt flow rates (MFR) of the high-density polyethylene layer 1 and the high-density polyethylene layer 2, measured in accordance with ASTM D1238 under conditions of 190°C and a load of 2.16 kg, are each preferably 0.01 g / 10 min or more, more preferably 0.1 g / 10 min or more, even more preferably 0.5 g / 10 min or more, and still more preferably 1.0 g / 10 min or more, from the viewpoint of further improving fluidity and moldability; and are preferably 20 g / 10 min or less, more preferably 10 g / 10 min or less, even more preferably 5 g / 10 min or less, even more preferably 3 g / 10 min or less, even more preferably 2 g / 10 min or less, and still more preferably 1.5 g / 10 min or less, from the viewpoint of improving the stiffness of the stretched polyethylene film while maintaining the tearability of the stretched polyethylene film.

[0035] The melt flow rate (MFR) of the high-density polyethylene constituting the high-density polyethylene layer 1 and the high-density polyethylene layer 2, measured in accordance with ASTM D1238 under conditions of 190°C and a load of 2.16 kg, is preferably 0.01 g / 10 min or more, more preferably 0.1 g / 10 min or more, even more preferably 0.5 g / 10 min or more, and still more preferably 1.0 g / 10 min or more, from the viewpoint of further improving fluidity and moldability; and from the viewpoint of improving the stiffness of the stretched polyethylene film while maintaining the tearability of the stretched polyethylene film, is preferably 20 g / 10 min or less, more preferably 10 g / 10 min or less, even more preferably 5 g / 10 min or less, even more preferably 3 g / 10 min or less, even more preferably 2 g / 10 min or less, and still more preferably 1.5 g / 10 min or less.

[0036] The melting points of the high-density polyethylene layer 1 and the high-density polyethylene layer 2, as measured by a differential scanning calorimeter (DSC), are each preferably 120°C or higher, more preferably 125°C or higher, and preferably 135°C or lower, more preferably 133°C or lower, and even more preferably 130°C or lower, from the viewpoint of further improving the balance of thermal dimensional stability, heat resistance, mechanical properties, rigidity, bag-formability, flowability, moldability, and the like.

[0037] The melting points of the high-density polyethylenes constituting the high-density polyethylene layer 1 and the high-density polyethylene layer 2, as measured by a differential scanning calorimeter (DSC), are preferably 120°C or higher, more preferably 125°C or higher, and are preferably 135°C or lower, more preferably 133°C or lower, and even more preferably 130°C or lower, from the viewpoint of further improving the balance of thermal dimensional stability, heat resistance, mechanical properties, rigidity, bag-formability, flowability, moldability, and the like.

[0038] When two or more types of polyethylene are used as the polyethylene constituting the high-density polyethylene layer, the density, MFR, and melting point of the high-density polyethylene layer can be measured values ​​for a mixture obtained by melt-blending two or more types of polyethylene by a known method. The melting point of the high-density polyethylene layer can be the peak temperature of the maximum melting peak.

[0039] At least one surface of the stretched polyethylene film of this embodiment is preferably a corona-treated surface (a surface modified by corona discharge irradiation). By making at least one surface of the stretched polyethylene film of this embodiment a corona-treated surface, the printing properties, coating properties, and lamination properties with other films of the stretched polyethylene film of this embodiment can be further improved.

[0040] The high-density polyethylene layer 1, the high-density polyethylene layer 2, and the medium-density polyethylene layer may contain various additives within the scope of the present invention, such as heat stabilizers, weather stabilizers, antioxidants, ultraviolet absorbers, lubricants, slip agents, nucleating agents, antiblocking agents, antistatic agents, antifogging agents, pigments, dyes, inorganic or organic fillers, etc.

[0041] The thicknesses of high-density polyethylene layer 1 and high-density polyethylene layer 2 are each preferably 1 μm or more, more preferably 3 μm or more, from the viewpoint of further improving the balance between transparency, rigidity, heat resistance, slip property, and heat-fusion strength, and preferably 17 μm or less, more preferably 15 μm or less, even more preferably 10 μm or less, and even more preferably 7 μm or less. The thicknesses of high-density polyethylene layer 1 and high-density polyethylene layer 2 may be the same or different, but are preferably the same from the viewpoint of uniforming the mechanical strength of the stretched polyethylene film on the high-density polyethylene layer 1 side and the high-density polyethylene layer 2 side. The thickness of the medium-density polyethylene layer is preferably 2 μm or more, more preferably 3 μm or more, even more preferably 5 μm or more, even more preferably 8 μm or more, from the viewpoint of improving the flexibility of the stretched polyethylene film, and is preferably 30 μm or less, more preferably 25 μm or less, even more preferably 20 μm or less, even more preferably 15 μm or less, even more preferably 13 μm or less, and even more preferably 11 μm or less. The overall thickness of the stretched polyethylene film is preferably 10 μm or more, more preferably 13 μm or more, and even more preferably 15 μm or more, from the viewpoint of maintaining the tearability and further improving the mechanical strength of the stretched polyethylene film, and is preferably 100 μm or less, more preferably 70 μm or less, even more preferably 50 μm or less, even more preferably 40 μm or less, even more preferably 30 μm or less, and even more preferably 25 μm or less, from the viewpoint of further improving the tearability, handleability, formability, bag-making suitability, lightness, etc. of the stretched polyethylene film.

[0042] Next, the physical properties of the stretched polyethylene film will be described.

[0043] In the stretched polyethylene film of this embodiment, the tensile modulus T of the stretched polyethylene film in the MD direction is measured using a tensile tester in accordance with JIS K7127:1999 under the conditions of a measurement temperature of 23±2°C, 50±5% RH, and a tension speed of 5 mm / min. 1is preferably 800 MPa or more, more preferably 850 MPa or more, even more preferably 900 MPa or more, even more preferably 950 MPa or more, even more preferably 1000 MPa or more, even more preferably 1050 MPa or more, even more preferably 1100 MPa or more, and even more preferably 1200 MPa or more, from the viewpoint of further improving the balance of the thermal dimensional stability, bag formability, and packaging suitability of the stretched polyethylene film; and is preferably 1500 MPa or less, more preferably 1450 MPa or less, even more preferably 1400 MPa or less, and even more preferably 1350 MPa or less, from the viewpoint of further improving the balance of the thermal dimensional stability, bag formability, and packaging suitability of the stretched polyethylene film. 2 is preferably 700 MPa or more, more preferably 750 MPa or more, even more preferably 800 MPa or more, even more preferably 850 MPa or more, even more preferably 900 MPa or more, even more preferably 920 MPa or more, and even more preferably 925 MPa or more, from the viewpoint of further improving the balance of the formability, mechanical properties, transparency, bag-formability, handleability, and packaging suitability of the stretched polyethylene film; and is preferably 1400 MPa or less, more preferably 1300 MPa or less, even more preferably 1200 MPa or less, even more preferably 1180 MPa or less, even more preferably 1150 MPa or less, and even more preferably 1130 MPa or less, from the viewpoint of further improving the balance of the bag-formability and packaging suitability of the stretched polyethylene film.

[0044] In the stretched polyethylene film of this embodiment, the tensile modulus T of the stretched polyethylene film in the MD direction is measured using a tensile tester in accordance with JIS K7127:1999 under the conditions of a measurement temperature of 23±2°C, 50±5% RH, and a tension speed of 5 mm / min. 1 and the tensile modulus in the TD direction T 2The total value of and is preferably 1500 MPa or more, more preferably 1600 MPa or more, even more preferably 1700 MPa or more, even more preferably 1800 MPa or more, even more preferably 1900 MPa or more, even more preferably 2000 MPa or more, and even more preferably 2050 MPa or more, from the viewpoints of achieving a better performance balance between transparency, rigidity, heat resistance, heat-fusion strength, and thermal dimensional stability, and further improving the stiffness of the stretched polyethylene film; and from the viewpoints of making problems such as breakage less likely to occur during molding of the stretched polyethylene film, facilitating continuous stretch molding of the film, and further improving industrial continuous productivity, the total value is preferably 2900 MPa or less, more preferably 2800 MPa or less, even more preferably 2700 MPa or less, even more preferably 2600 MPa or less, even more preferably 2500 MPa or less, and even more preferably 2400 MPa or less. Such a tensile modulus is a substitute value for quantitatively measuring the stiffness of a film, and can be adjusted, for example, by adjusting the types and contents of the high-density polyethylene layer 1, the high-density polyethylene layer 2, and the medium-density polyethylene layer contained in the stretched polyethylene film, the thickness of the stretched polyethylene film, the stretching ratio, etc.

[0045] In the stretched polyethylene film of this embodiment, the haze per sheet of stretched polyethylene film measured in accordance with JIS K 7136: 2000 is, from the viewpoint of further improving the transparency of the stretched polyethylene film, preferably 16.0% or less, more preferably 15.8% or less, even more preferably 15.5% or less, even more preferably 15.3% or less, and still more preferably 15.0% or less. There is no lower limit for the haze per sheet of stretched polyethylene film, but it may be, for example, 0.1% or more, 1.0% or more, 3.0% or more, or 5.0% or more.

[0046] In the stretched polyethylene film according to this embodiment, the amorphous thickness determined from the peak in the MD diffraction angle 2θ range of 0.2 to 0.4° by small-angle X-ray scattering (SAXS) measurement is preferably less than 12.5 nm, more preferably 12.4 nm or less, even more preferably 12.2 nm or less, even more preferably 12.0 nm or less, even more preferably 11.7 nm or less, and even more preferably 11.5 nm or less, from the viewpoint of improving the flexibility of the stretched polyethylene film. There is no lower limit to the amorphous thickness determined from the peak in the MD diffraction angle 2θ range of 0.2 to 0.4° by small-angle X-ray scattering (SAXS) measurement, but it may be, for example, 9.0 nm or more, 9.5 nm or more, 10.0 nm or more, 10.5 nm or more, or 11.0 nm or more. Such amorphous thickness can be adjusted, for example, by adjusting the types and contents of the high-density polyethylene layer 1, the high-density polyethylene layer 2, and the medium-density polyethylene layer contained in the stretched polyethylene film, the thickness of the stretched polyethylene film, the stretching ratio, etc.

[0047] The stretched polyethylene film according to this embodiment has a three-layer structure in which the medium-density polyethylene layer is sandwiched between high-density polyethylene layer 1 and high-density polyethylene layer 2, and the amorphous thickness of the stretched polyethylene film is set to the above-mentioned upper limit or less, thereby further improving the flexibility of the stretched polyethylene film.

[0048] In the stretched polyethylene film of this embodiment, the full width at half maximum (FWHM) of the peak at a diffraction angle 2θ in the MD direction in the range of 0.2 to 0.4°, as determined by small-angle X-ray scattering (SAXS) measurement, is preferably 0.21° or less, more preferably 0.20° or less, even more preferably 0.19° or less, and even more preferably 0.18° or less, from the viewpoints of increasing the crystallinity of the surface layer of the stretched polyethylene film, suppressing the formation of a brittle layer, and improving slip properties. The full width at half maximum (FWHM) of the peak at a diffraction angle 2θ in the MD direction in the range of 0.2 to 0.4° of the stretched polyethylene film is preferably 0.05° or more, more preferably 0.10° or more, even more preferably 0.13° or more, even more preferably 0.15° or more, even more preferably 0.16° or more, and even more preferably 0.17° or more, from the viewpoints of further improving film formability, bag formability, lamination strength, and thermal dimensional stability. The full width at half maximum (FWHM) of the peak in the MD diffraction angle 2θ range of 0.2 to 0.4°, which is determined from such small-angle X-ray scattering (SAXS) measurement, can be adjusted by, for example, adjusting the types and contents of the high-density polyethylene layer 1, the high-density polyethylene layer 2, and the medium-density polyethylene layer contained in the stretched polyethylene film, the thickness of the stretched polyethylene film, the stretch ratio, etc.

[0049] In the stretched polyethylene film of this embodiment, from the viewpoint of further improving thermal dimensional stability and bag-formability, the heat shrinkage rate in the MD direction of the stretched polyethylene film when heat-treated at 100°C for 15 minutes is preferably 6.0% or less, more preferably 5.5% or less, even more preferably 5.0% or less, even more preferably 4.5% or less, even more preferably 4.3% or less, even more preferably 4.1% or less, and even more preferably 4.0% or less, and may be 0.1% or more, 0.5% or more, 1.0% or more, 1.5% or more, 2.0% or more, or 2.5% or more. The heat shrinkage rate of the stretched polyethylene film can be measured in accordance with JIS C2151:2019.

[0050] In the stretched polyethylene film of the present embodiment, the heat shrinkage rate in the MD direction of the stretched polyethylene film when heat-treated at 120°C for 15 minutes is, from the viewpoint of further improving the thermal dimensional stability and bag-formability, preferably 25.0% or less, more preferably 23.0% or less, even more preferably 22.5% or less, even more preferably 22.0% or less, even more preferably 21.0% or less, and still more preferably 20.0% or less, and may be 1.0% or more, 3.0% or more, 5.0% or more, 10.0% or more, or 15.0% or more.

[0051] When at least one of the stretched polyethylene films is non-corona-treated, the heat fusion strength when the non-corona-treated sides of the stretched polyethylene films are bonded together at 140°C is preferably 4.0 N / 15 mm or less, more preferably 3.8 N / 15 mm or less, from the viewpoint of improving heat resistance. There is no lower limit for the heat fusion strength, but it is, for example, 0.1 N / 15 mm or more. The heat fusion strength is measured as follows. The non-corona-treated surfaces of two stretched polyethylene films cut to a width of 15 mm are heat-fused together at 140°C, a pressure of 2.0 kgf, and a sealing time of 1.0 second to obtain a laminated film. Next, using the laminated film cut to a width of 15 mm, the two stretched polyethylene films are peeled at a 90° angle, at a peel speed of 300 mm / min, and pulled in the machine direction. The peel strength measured at this time is the heat fusion strength (N / 15 mm).

[0052] In the stretched polyethylene film of this embodiment, the laminate strength measured in accordance with JIS Z 0238:1998 is preferably 0.7 N / 15 mm or more, more preferably 0.8 N / 15 mm or more, and preferably 10.0 N / 15 mm or less, more preferably 5.0 N / 15 mm or less, even more preferably 3.0 N / 15 mm or less, and even more preferably 2.0 N / 15 mm or less, from the viewpoint of achieving a better balance between adhesiveness and easy-opening properties. The laminate strength is measured as follows: A 297 cm x 210 cm test piece is cut out from the stretched polyethylene film, and the corona-treated surface of the test piece is bonded to the corona-treated surface of a 50 μm-thick cast LLDPE film, one side of which has been corona-treated, with an ester-based adhesive, followed by aging at 40°C for 3 days. Next, a test piece with a width of 15 mm is cut out, and the peel strength when peeled in the MD direction using a tensile tester in accordance with JIS Z 0238:1998 at a peel angle of 90°, a chuck distance of 100 mm, and a crosshead speed of 300 mm / min is determined, and this is taken as the laminate strength.

[0053] In the stretched polyethylene film of this embodiment, the static friction coefficient (tan θ) of the surface of the stretched polyethylene film, measured with a slip tester, is preferably 0.20 or more, more preferably 0.25 or more, and preferably 0.65 or less, more preferably 0.60 or less, even more preferably 0.55 or less, and even more preferably 0.50 or less. When either the high-density polyethylene layer 1 or the high-density polyethylene layer 2 of the stretched polyethylene film is corona-treated, the static friction coefficient (tan θ) of the stretched polyethylene film surface may be measured between the treated surfaces, between the untreated surfaces, or between the treated and untreated surfaces. In particular, from the viewpoint of further improving the handleability of the stretched polyethylene film, it is preferable that the static friction coefficient (tan θ) of the surface on the corona-untreated side be within the above-mentioned range. The static friction coefficient (tan θ) of the surface on the corona-untreated side of the stretched polyethylene film is preferably 0.20 or more, more preferably 0.25 or more, and preferably 0.65 or less, more preferably 0.60 or less, even more preferably 0.55 or less, and even more preferably 0.50 or less.

[0054] The static friction coefficient (tan θ) of the corona-untreated surface of a stretched polyethylene film is measured by the following method. Two pieces of stretched polyethylene film (hereinafter referred to as stretched polyethylene films 1 and 2) cut to a size of 50 mm x 75 mm are prepared, and one of the stretched polyethylene films, stretched polyethylene film 1, is fixed to an inclined plate with the corona-untreated side facing up. Next, a friction body with a brass bottom (41 mm x 26 mm in size) is fixed to the center of the surface of the other stretched polyethylene film, stretched polyethylene film 2, opposite the corona-untreated side, and a weight is attached to the friction body so that the mass applied to the stretched polyethylene film 2 from the friction body is 150 g. Next, the corona-untreated surfaces of the two stretched polyethylene films 1 and 2 are placed face-to-face. Next, the inclined plate is tilted at a rate of 1° / sec, and the value of tan θ is determined from the angle θ when the upper stretched polyethylene film 2 begins to slide. When measuring the static friction coefficient (tan θ) of the corona-treated surface, the static friction coefficient (tan θ) of the corona-untreated surface is measured in the same manner as in the above method for measuring the static friction coefficient (tan θ) of the corona-untreated surface, except that the corona-untreated surface is replaced with the corona-treated surface.

[0055] In the stretched polyethylene film of the present embodiment, the puncture strength from the corona-treated surface toward the non-corona-treated surface, measured in accordance with JIS Z1707:1997 under conditions of 23±2°C and 50±5% RH, is, from the viewpoint of further suppressing tearing of the package, preferably 2.5 N or more, more preferably 3.0 N or more, even more preferably 4.0 N or more, and still more preferably 4.3 N or more, and is also preferably 8.0 N or less, more preferably 7.8 N or less, even more preferably 7.5 N or less, even more preferably 7.3 N or less, even more preferably 7.0 N or less, even more preferably 6.5 N or less, even more preferably 6.0 N or less, even more preferably 5.5 N or less, and even more preferably 5.0 N or less.

[0056] The tear strength in the MD direction of the stretched polyethylene film, measured using a light-load tear tester with a test weight of 96.09 g, is preferably 100 mN or more, more preferably 150 mN or more, even more preferably 180 mN or more, even more preferably 200 mN or more, even more preferably 230 mN or more, and even more preferably 250 mN or more, from the viewpoint of improving film-forming and bag-making processability. Furthermore, from the viewpoint of improving the tearability while maintaining the heat-sealability and stiffness of the stretched polyethylene film, it is preferably 600 mN or less, more preferably 580 mN or less, even more preferably 550 mN or less, even more preferably 530 mN or less, even more preferably 500 mN or less, even more preferably 490 mN or less, and even more preferably 450 mN or less. To achieve such tear strength, the density, thickness, etc. of the high-density polyethylene layer 1, high-density polyethylene layer 2, and medium-density polyethylene layer contained in the stretched polyethylene film may be appropriately adjusted. The tear strength in the MD direction is measured as follows. A test piece measuring 63.5 mm in the MD direction and 50 mm in the TD direction is cut out from the stretched polyethylene film. The tear strength (mN) of one test piece in the MD direction is measured using a light-load tear tester under the following conditions: pendulum weight: 96.09 g, tear length: 12.7 mm, pendulum lift angle: 90°. The light-load tear tester may be, for example, a Model D model manufactured by Toyo Seiki Seisakusho Co., Ltd.

[0057] In the stretched polyethylene film of this embodiment, the number of pinholes generated in the stretched polyethylene film is preferably 2500 / m, as measured by a Gelbo flex tester after 3000 bending cycles at a bending angle of 440 degrees and a bending speed of 40 cycles / min in an atmosphere of −30° C. 2 or less, more preferably 2300 particles / m 2 More preferably, 2200 pieces / m or less 2 More preferably, 2100 pieces / m or less 2 More preferably, 2000 pieces / m or less 2 There is no lower limit to the number of pinholes that occur in the stretched polyethylene film, but for example, it is set to 100 pinholes / m2 or more, and 2 It may be 500 pieces / m or more. 2 or more, and 2 It may be 1000 pieces / m or more. 2 or more. The number of pinholes generated represents an index of the flex resistance of the stretched polyethylene film of this embodiment, and the fewer the number of pinholes generated, the better the flex resistance. When the number of pinholes generated in the stretched polyethylene film is within the above range, the generation of pinholes due to flexing during low-temperature filling or low-temperature transportation can be further suppressed. The Gelbo Flex Tester that can be used is, for example, one manufactured by Tester Sangyo Co., Ltd.

[0058] <Identification of High-Density Polyethylene Layer and Medium-Density Polyethylene Layer> For example, it can be determined that the stretched polyethylene film of this embodiment is composed of high-density polyethylene layer 1, medium-density polyethylene layer, and high-density polyethylene layer 2 by cutting a cross section of the stretched polyethylene film and measuring the melting point of each layer. The melting points of high-density polyethylene layer 1 and high-density polyethylene layer 2 are, for example, in the range of 130°C or higher and 140°C or lower, and the melting point of the medium-density polyethylene layer is, for example, in the range of 110°C or higher and 129°C or lower.

[0059] <Method of manufacturing stretched polyethylene film> The stretched polyethylene film of the present embodiment is stretched uniaxially or biaxially from the viewpoint of improving the orientation crystallinity and increasing the mechanical strength, and is preferably stretched uniaxially from the viewpoint of improving productivity. Furthermore, by stretching the film uniaxially in the MD direction, the tensile modulus T 1This can further improve the properties. The stretched polyethylene film can be obtained by, for example, co-extrusion molding a high-density polyethylene resin for forming the high-density polyethylene layer 1, a medium-density polyethylene resin for forming the medium-density polyethylene layer, and a high-density polyethylene resin for forming the high-density polyethylene layer 2 in this order into a film, and then stretching the resulting film using a known stretched film production method such as a uniaxial stretching method, a simultaneous biaxial stretching method, or a sequential biaxial stretching method. The molding apparatus and molding conditions are not particularly limited, and conventionally known molding apparatuses and molding conditions can be used. Examples of molding apparatus that can be used include a T-die extruder, a multilayer T-die extruder, an inflation molding machine, and a multilayer inflation molding machine. Conditions for the uniaxial stretching and biaxial stretching methods can be, for example, those used for producing known stretched polyethylene films. More specifically, in the case of a uniaxial stretching method, the longitudinal stretching temperature may be 100°C to 145°C, and the longitudinal stretching ratio may be 4.5 to 6 times. In the sequential biaxial stretching method, for example, the longitudinal stretching temperature may be 100°C to 145°C, the longitudinal stretching ratio may be in the range of 4.5 to 6 times, the transverse stretching temperature may be 110°C to 160°C, and the transverse stretching ratio may be in the range of 9 to 11 times.

[0060] <Uses of Stretched Polyethylene Film / Packaging Material / Food Package> The stretched polyethylene film of this embodiment can be suitably used, specifically, as a food packaging film. The stretched polyethylene film of this embodiment can also be suitably used as a packaging material. When used as a packaging material, the stretched polyethylene film of this embodiment can be used alone, or other layers can be laminated to form the packaging material. Examples of such other layers include a substrate layer, a coating layer, an adhesive layer, and a heat-sealing layer. From the perspective of ease of recycling, it is preferable that these layers be formed from a polyethylene-based resin. The packaging material of this embodiment can also be suitably used for food packaging. The food packaging is used, for example, for the purpose of packaging food, and specifically includes the packaging material of this embodiment and the food contained therein. Depending on the application, only a portion of the food packaging may be made of the packaging material of this embodiment, or substantially the entire food packaging may be made of the packaging material of this embodiment.

[0061] There are no particular limitations on the method for producing a food package from the stretched polyethylene film or packaging material, and any method known in the field of packaging materials / packages, such as heat sealing or fusing, can be used.

[0062] The stretched polyethylene film according to this embodiment is preferably used for food packaging that requires good flexibility. The food packaging may be in the form of, for example, a two-sided bag or a standing pouch (pouch packaging). These forms are preferred because they can provide good flexibility.

[0063] Furthermore, when a food package (such as a packaging bag) is constructed using the stretched polyethylene film or packaging material of this embodiment, it is preferable that the corona-treated surface is the inner surface and the non-corona-treated surface is the outer surface. Furthermore, as described above, when another layer is laminated on the stretched polyethylene film, it is preferable that the layer be laminated on the corona-treated surface. That is, when a laminate using the stretched polyethylene film of this embodiment is used for a food package (such as a packaging bag), it is preferable that the stretched polyethylene film of this embodiment be the outermost layer of the food package.

[0064] There are no limitations on the foods that can be packaged in the food packaging, but examples include baked goods, rice crackers, snacks, sprinkles, grain powders, and the like.

[0065] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various other configurations may be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of achieving the object of the present invention are included in the present invention.

[0066] <Raw Materials> The raw materials used in the Examples and Comparative Examples are listed below. The density was measured in accordance with JIS K 7112:1999. The MFR was measured in accordance with ASTM D1238 under conditions of 190°C and a load of 2.16 kg. The melting point was measured using a differential scanning calorimeter (DSC).

[0067] (High density polyethylene) High density polyethylene (HDPE1): Density: 949 kg / m 3 , MFR: 1.1 g / 10 min, melting point: 130°C (medium density polyethylene) Medium density polyethylene (MDPE1): Density: 916 kg / m 3 , MFR: 2.3 g / 10 min, melting point: 116 ° C. Medium density polyethylene (MDPE2): Density: 918 kg / m 3 , MFR: 3.8 g / 10 min, melting point: 116 ° C. Medium density polyethylene (MDPE3): Density: 923 kg / m 3 , MFR: 1.5 g / 10 min, melting point: 121 ° C. Medium density polyethylene (MDPE4): Density: 925 kg / m 3 , MFR: 1.9 g / 10 min, melting point: 122 ° C. Medium density polyethylene (MDPE5): Density: 937 kg / m 3 , MFR: 1.8 g / 10 min, melting point: 127 ° C. Medium density polyethylene (MDPE6): Density: 942 kg / m 3 , MFR: 2.9 g / 10 min, melting point: 127°C

[0068] <Production of Stretched Polyethylene Films> [Examples 1 to 3 and Comparative Example 1] High-density polyethylene, medium-density polyethylene, and high-density polyethylene in the Examples and Comparative Examples were extruded in this order using a T-die to form films using the formulations shown in Table 1, to obtain cast sheets, which were then subjected to uniaxial stretching. After uniaxial stretching, the second-layer high-density polyethylene side of the cast sheet was subjected to corona treatment, producing the stretched polyethylene film of each example. The extrusion and uniaxial stretching conditions are shown below. Multilayer extruder: 60 mmφ multilayer T-die extruder (L / D = 27, manufactured by Screw Seiki Co., Ltd.) Extrusion setting temperature: 230°C, processing speed: 25 m / min, longitudinal stretching temperature: 110 to 130°C, longitudinal stretching ratio: 5 times

[0069] The stretched polyethylene films obtained in each example were evaluated as follows. The results are shown in Table 1.

[0070] <Small-angle X-ray scattering (SAXS) measurement of stretched polyethylene film> For the stretched polyethylene film of each example, the MD direction of the film was set to the top and bottom, the TD direction to the left and right, and the measurement film was set in the following device so that the angle between the X-ray source direction and the film surface was perpendicular. Small-angle X-ray scattering (SAXS) measurement was carried out using the following device and conditions. Device: Manufactured by RIGAKU Corporation, product name: Ultima IV (small-angle scattering attachment system) X-ray incidence direction: normal to the film X-ray wavelength: 0.15418 nm Optical unit specifications: 1. Optical system selection slit: for small-angle scattering 0.03 mm (=1 st . Slit) 2. DS; Anti-scattering slit 1.00 mm (= 2 nd . Slit) 3. Soller slit on the entrance side: 5° flexible optical system used 4.1 st .~2 nd Distance between slits: 70 mm 5.2 nd. Distance between sample and sample: 98 mm 6. Vacuum path length: 100 mm (installed on a dedicated stand in front of the receiving slit box) 7. RS, SS: Scattering slit 0.20 mm, receiving slit 0.10 mm 8. Camera length: 285 mm 9. Receiving side Soller slit: 5° using a flexible optical system 10. Monochromatization: None (monochromatization on the incident side using a multilayer mirror) 11. Detector: RIGAKU scintillation detector (HV: 762 V) (one-dimensional) X-ray irradiation conditions: A. Scan axis: 2 theta B. Measurement method: continuous C. Scan start angle: 0.1° D. Scan end angle: 1.0° E. Sampling width: 0.02° F. Scan speed: 0.5° / min G. Voltage and current: 40 kV-40 mA H. Number of sample stacks: To obtain sufficient scattering intensity, the samples were aligned and stacked to a distance of approximately 0.5 mm. The X-ray scattering pattern obtained under the above measurement conditions was subjected to air scattering correction for the detector to obtain the SAXS profile I(q). The diffraction angle θ of the scattering vector magnitude of the peak derived from the crystal long period of the SAXS profile I(q) was calculated using equation (1), and this was substituted into Bragg's equation (2) to calculate the crystal long period (d). q = 4π sin θ / λ ... (1) θ: diffraction angle q: scattering vector magnitude λ: X-ray wavelength 2d sin θ = λ ... (2) d: crystal long period θ: diffraction angle λ: X-ray wavelength. Furthermore, referring to the structural analysis of crystalline polymer materials using scattering methods in Nichias Technical Review (2014) No. 2, No. 365, the electron density correlation function γ(r) was calculated by Fourier transforming the SAXS profile I(q) using the following (3). γ(r) has a special property that can be used directly for structural characterization, and the amorphous thickness (da) of each stretched polyethylene film obtained as structural information was calculated. r represents distance (nm).

[0071]

[0072] The difference value of the amorphous thickness from the crystalline long period (d) was calculated as the crystalline thickness (dc). Furthermore, the full width at half maximum (FWHM) of the peak in the MD direction diffraction angle 2θ range of 0.2 to 0.4° was calculated using X-ray analysis software PDXL-2 (manufactured by RIGAKU Corporation). Specifically, air scattering was removed from the SAXS profile I(q) obtained above. The obtained values ​​were separated into crystalline scattering and amorphous scattering using the above software, and the full width at half maximum (FWHM) of the peak in the MD direction diffraction angle 2θ range of 0.2 to 0.4° was calculated from the peak fitting results of crystalline scattering according to the following (analysis conditions). (Analysis conditions) Fitted peak shape: Split pseudo-Voigt function Crystallite size distribution type: Lorentz model

[0073] <Differential Scanning Calorimetry> A test piece of approximately 5.0 mg was cut out from the stretched polyethylene film of each example. Next, using a differential scanning calorimeter (product name: Q200DSC manufactured by TA Instruments), the test piece was subjected to a first differential scanning calorimetry (1st Run) consisting of a process of increasing the temperature from -50°C to 200°C at a heating rate of 10°C / min, an isothermal process of maintaining the temperature at 200°C for 10 minutes, and a process of decreasing the temperature from 200°C to -50°C at a heating rate of 10°C / min, and a second differential scanning calorimetry (2nd Run) consisting of a process of increasing the temperature from -50°C to 200°C at a heating rate of 10°C / min. In the DSC curve 1 obtained by the first differential scanning calorimetry, the heat of fusion (ΔH m ) (J / g) was calculated.

[0074] <Haze> The haze per sheet of the stretched polyethylene film of each example was measured in accordance with JIS K7136:2000 using a haze meter (NDH5000, manufactured by Nippon Denshoku Industries Co., Ltd.).

[0075] <Tensile modulus> A test piece of 15 mm x 15 cm was cut out from the stretched polyethylene film of each example. Then, the tensile modulus T of the test piece in the MD direction was measured using a tensile tester manufactured by Orientec Co., Ltd., in accordance with JIS K7127:1999 under the conditions of a measurement temperature of 23±2°C, 50±5% RH, and a pulling speed of 5 mm / min. 1and tensile modulus in the TD direction T 2 From the obtained values, T 1 and T 2 The total value was calculated.

[0076] <Heat shrinkage in MD direction of stretched polyethylene film at 100°C> The heat shrinkage in MD direction of stretched polyethylene film at 100°C was measured in accordance with JIS C2151:2019. A 10 cm x 10 cm test piece was cut out from the stretched polyethylene film of each example. The test piece was then heat-treated at 100°C for 15 minutes. At this time, the test piece was heated in a hot air circulation type thermostatic oven (manufactured by ADVANTEC, product name: DRM620DE) while being suspended without applying force. Next, after cooling the test piece to room temperature, the length of the test piece was measured. The length in the MD direction of the test piece after heat treatment was determined as the MD 100 [cm], and the heat shrinkage rate [%] in the MD direction is calculated as 100 × (10 - MD 100 The above measurement was carried out three times, and the average value of the obtained measurements was used as the heat shrinkage rate of the stretched polyethylene film at 100°C.

[0077] <Heat shrinkage in MD direction of stretched polyethylene film at 120°C> The heat shrinkage in MD direction of stretched polyethylene film at 120°C was measured in accordance with JIS C2151:2019. A 10 cm x 10 cm test piece was cut out from the stretched polyethylene film of each example. The test piece was then heat-treated at 120°C for 15 minutes. At this time, the test piece was heated in a hot air circulation type thermostatic oven (manufactured by ADVANTEC, product name: DRM620DE) while being suspended without applying force. Next, after cooling the test piece to room temperature, the length of the test piece was measured. The length in the MD direction of the test piece after heat treatment was determined as the MD 120 [cm], and the heat shrinkage rate [%] in the MD direction is calculated as 100 × (10 - MD 120 The above measurement was carried out three times, and the average value of the obtained measurements was used as the heat shrinkage rate of the stretched polyethylene film at 120°C.

[0078] <Static Friction Coefficient> Two sheets of stretched polyethylene film of each example (hereinafter referred to as stretched polyethylene films 1 and 2) were prepared, cut to a size of 50 mm x 75 mm. One of the stretched polyethylene films, stretched polyethylene film 1, was fixed to an inclined plate with the non-corona-treated surface facing up. Next, a friction body with a bottom surface (41 mm x 26 mm) made of brass was fixed to the center of the surface of the other stretched polyethylene film, stretched polyethylene film 2, opposite the non-corona-treated surface. A weight was attached to the friction body so that the mass applied to the stretched polyethylene film 2 from the friction body was 150 g. Next, the non-corona-treated surfaces of the two stretched polyethylene films 1 and 2 were placed face-to-face. Next, the inclined plate was tilted at a rate of 1° / sec, and the value of tan θ was calculated from the angle θ at which the upper stretched polyethylene film 2 began to slide, and this was used as the static friction coefficient of the non-corona-treated surface.

[0079] <Heat-sealing strength> Two sheets of the stretched polyethylene film of each example, cut to a width of 15 mm, were heat-sealed together with their non-corona-treated surfaces at 140°C, a pressure of 2.0 kgf, and a sealing time of 1.0 second to obtain a laminated film. The resulting laminated film was then cut to a width of 15 mm, and the two sheets of stretched polyethylene film were peeled at a 90° peel angle, at a peel rate of 300 mm / min, and pulled in the MD direction. The peel strength at this time was recorded as the heat-sealing strength (N / 15 mm).

[0080] <Laminate Strength> A 297 cm x 210 cm test piece was cut from each stretched polyethylene film, and the corona-treated side of the test piece was bonded to the corona-treated side of a 50 μm thick cast LLDPE film (manufactured by Mitsui Chemicals Tohcello, TUX FCS #50) with one side corona-treated, using an ester-based adhesive (Mitsui Chemicals Takelac A310 / Takenate A3 / ethyl acetate) = 12 / 1 / 7), and aged at 40 ° C for 3 days. Next, a 15 mm wide test piece was cut out, and using a tensile tester (Orientec Co., Ltd. Tensilon Universal Testing Machine RTC-1225) in accordance with JIS Z 0238: 1998, the peel strength was measured when peeled in the MD direction at a peel angle of 90 °, a chuck distance of 100 mm, and a crosshead speed of 300 mm / min, and this was taken as the laminate strength.

[0081] <Puncture Strength> Puncture strength was measured as an index of flexibility as follows. Test pieces measuring 60 mm in width and 200 to 300 mm in length were cut out from each stretched polyethylene film. Next, the puncture strength (N) from the corona-treated surface toward the non-corona-treated surface was measured using a Tensilon RTC-1225 manufactured by Orientec Co., Ltd. in accordance with JIS Z1707:1997 under conditions of 23±2°C and 50±5% RH.

[0082] <Flexibility> As an index of flexibility, flexibility was evaluated as follows: A test piece measuring 297 cm × 210 cm was cut out from the stretched polyethylene film of each example, and a flex test was performed 3,000 times using a Gelbo Flex Tester (manufactured by Tester Sangyo Co., Ltd.) at a flex angle of 440° and a flex speed of 40 times / min in an atmosphere of −30° C. After the flex test, a bag was made from the test piece, and the number of pinholes generated was measured using Ageless Seal Check Solution (manufactured by Mitsubishi Gas Chemical Company).

[0083] <Tear Strength> As an index of flexibility, tear strength was measured as follows. A test piece measuring 63.5 mm in the MD direction and 50 mm in the TD direction was cut out from each stretched polyethylene film. The tear strength (mN) in the MD direction of one test piece was measured using a light-load tear tester (manufactured by Toyo Seiki Seisaku-sho, Ltd., Model-D) under the following conditions: pendulum weight: 96.09 g, tear length: 12.7 mm, pendulum lift angle: 90°.

[0084] The flexibility of the stretched polyethylene film was evaluated according to the following criteria: (Criteria) A (Good): All of the following (i) to (iii) are satisfied. B (Poor): One or more of the following (i) to (iii) are not satisfied. (i) Puncture strength is 2.5 N or more. (ii) Bending resistance (number of pinholes) is 2,500 / m. 2 (iii) The tear strength in the MD direction is 100 mN or more.

[0085]

[0086] When the stretched polyethylene film of the example was used, a food packaging film with improved flexibility (performance balance of puncture strength, bending resistance, and tear strength) could be obtained.

[0087] This application claims priority based on Japanese Patent Application Nos. 2022-157678, 2022-157993, and 2022-157996, filed on September 30, 2022, the disclosures of which are incorporated herein in their entireties.

[0088] The present invention can also take the following aspects.

[0089] [1a] A stretched polyethylene film comprising, in this order, a high-density polyethylene layer 1, a medium-density polyethylene layer, and a high-density polyethylene layer 2, wherein the medium-density polyethylene layer has a density of 910 kg / m as measured in accordance with JIS K 7112:1999. 3 More than 935kg / m 3 [2a] The stretched polyethylene film according to [1a], wherein the total amount of the high-density polyethylene layer 1 and the high-density polyethylene layer 2 in the stretched polyethylene film is 25% by mass or more and 85% by mass or less, when the entire stretched polyethylene film is taken as 100% by mass. [3a] The density of the high-density polyethylene layer 1 and the high-density polyethylene layer 2, measured in accordance with JIS K 7112:1999, is 940 kg / m or less. 3 More than 970kg / m 3[4a] The stretched polyethylene film according to any one of [1a] to [3a], wherein the high-density polyethylene layer 1 and the high-density polyethylene layer 2 each have an MFR of 0.01 g / 10 min or more and 20 g / 10 min or less, as measured in accordance with ASTM D1238 at 190°C under a load of 2.16 kg. [5a] The stretched polyethylene film according to any one of [1a] to [4a], wherein the medium-density polyethylene layer has an MFR of 0.01 g / 10 min or more and 20 g / 10 min or less, as measured in accordance with ASTM D1238 at 190°C under a load of 2.16 kg. [6a] The stretched polyethylene film according to any one of [1a] to [5a], wherein the stretched polyethylene film has a peak full width at half maximum (FWHM) of 0.20° or less in the MD diffraction angle 2θ range of 0.2 to 0.4°, as determined by small-angle X-ray scattering (SAXS) measurement. [7a] When the stretched polyethylene film is subjected to a first differential scanning calorimetry (1st Run) using a differential scanning calorimeter, the first differential scanning calorimetry (1st Run) comprises a process of increasing the temperature from -50°C to 200°C at a heating rate of 10°C / min, an isothermal process of maintaining the temperature at 200°C for 10 minutes, and a process of decreasing the temperature from 200°C to -50°C at a heating rate of 10°C / min, and a second differential scanning calorimetry (2nd Run) comprises a process of increasing the temperature from -50°C to 200°C at a heating rate of 10°C / min, an endothermic peak A is observed in the range of 10°C to 160°C in DSC curve 1 obtained by the first differential scanning calorimetry, and the heat of fusion of the endothermic peak A (ΔH m [8a] The stretched polyethylene film according to any one of [1a] to [7a], wherein the stretched polyethylene film has a haze of 16.0% or less per sheet as measured in accordance with JIS K 7136:2000. [9a] The stretched polyethylene film has a tensile modulus T in the machine direction of the stretched polyethylene film as measured in accordance with JIS K7127:1999 using a tensile tester under conditions of a measurement temperature of 23±2°C, 50±5% RH, and a pulling rate of 5 mm / min. 1and the tensile modulus in the TD direction T 2 The stretched polyethylene film according to any one of [1a] to [8a], wherein the total value of (a) and (b) is 1600 MPa or more and 2900 MPa or less. [10a] The stretched polyethylene film according to any one of [1a] to [9a], wherein the stretched polyethylene film has a heat shrinkage rate in the MD direction of 5.5% or less when heat-treated at 100°C for 15 minutes in accordance with JIS C2151:2019. [11a] The stretched polyethylene film according to any one of [1a] to [10a], wherein the stretched polyethylene film has a heat shrinkage rate in the MD direction of 25.0% or less when heat-treated at 120°C for 15 minutes in accordance with JIS C2151:2019. [12a] The stretched polyethylene film according to any one of [1a] to [11a], wherein at least one surface of the stretched polyethylene film is a corona-treated surface. [13a] The stretched polyethylene film according to any one of [1a] to [12a], wherein at least one surface of the stretched polyethylene film is non-corona treated, and wherein the heat fusion strength when the non-corona treated surfaces of the stretched polyethylene films are bonded together and heat-sealed at 140°C is 4.0 N / 15 mm or less. [14a] The stretched polyethylene film according to any one of [1a] to [13a], wherein the laminate strength in the MD direction of the stretched polyethylene film is 0.7 N / 15 mm or more and 10.0 N / 15 mm or less, as measured in accordance with JIS Z 0238:1998 using a tensile tester under conditions of T-peel and a crosshead speed of 300 mm / min. [15a] The stretched polyethylene film according to any one of [1a] to [14a], wherein the total thickness of the stretched polyethylene film is 10 μm or more and 100 μm or less. [16a] The stretched polyethylene film according to any one of [1a] to [15a], which is a food packaging film. [17a] A packaging material using the stretched polyethylene film according to any one of [1a] to [16a]. [18a] A food package comprising the packaging material according to [17a] and a food product placed inside the packaging material.

[0090] The present invention can also take the following aspects.

[0091] [1b] A stretched polyethylene film comprising, in this order, a high-density polyethylene layer 1, a medium-density polyethylene layer, and a high-density polyethylene layer 2, wherein the amorphous thickness determined from a peak in the MD direction at a diffraction angle 2θ of 0.2 to 0.4° by small-angle X-ray scattering (SAXS) measurement is less than 12.5 nm. [2b] The tensile modulus T of the stretched polyethylene film in the TD direction, measured in accordance with JIS K7127:1999 using a tensile tester under conditions of a measurement temperature of 23±2°C, 50±5% RH, and a pulling rate of 5 mm / min, is 2 [3b] The medium-density polyethylene layer has a density of 910 kg / m or more as measured in accordance with JIS K 7112:1999. 3 More than 940kg / m 3 [4b] The stretched polyethylene film according to any one of [1b] to [3b], wherein the total amount of the high-density polyethylene layer 1 and the high-density polyethylene layer 2 in the stretched polyethylene film is 25% by mass or more and 85% by mass or less, when the entire stretched polyethylene film is taken as 100% by mass. [5b] The density of the high-density polyethylene layer 1 and the high-density polyethylene layer 2, measured in accordance with JIS K 7112:1999, is 940 kg / m or less, respectively. 3 More than 970kg / m 3 [6b] The stretched polyethylene film according to any one of [1b] to [4b], wherein the haze of the stretched polyethylene film per sheet measured in accordance with JIS K 7136:2000 is 16.0% or less. [7b] The tensile modulus T of the stretched polyethylene film in the MD direction, measured in accordance with JIS K7127:1999 using a tensile tester under conditions of a measurement temperature of 23±2°C, 50±5% RH, and a pulling rate of 5 mm / min, is 1 and the tensile modulus in the TD direction T 2The stretched polyethylene film according to any one of [1b] to [6b], wherein the sum of the values ​​of the tensile strength (MPa) and the compressive strength (MPa) is 1500 MPa or more and 2900 MPa or less. [8b] The stretched polyethylene film according to any one of [1b] to [7b], wherein the heat shrinkage rate in the MD direction of the stretched polyethylene film is 6.0% or less when heat-treated at 100°C for 15 minutes in accordance with JIS C2151:2019. [9b] ​​The stretched polyethylene film according to any one of [1b] to [8b], wherein at least one surface of the stretched polyethylene film is a corona-treated surface. [10b] The stretched polyethylene film according to any one of [1b] to [9b], wherein at least one surface of the stretched polyethylene film is an uncorona-treated surface, and wherein the heat-fusion strength when the uncorona-treated surfaces of the stretched polyethylene films are bonded together and heat-sealed at 140°C is 4.0 N / 15 mm or less. [11b] The stretched polyethylene film according to any one of [1b] to [10b], wherein the stretched polyethylene film has an overall thickness of 10 μm or more and 100 μm or less. [12b] The stretched polyethylene film according to any one of [1b] to [11b], which is a film for food packaging. [13b] A packaging material using the stretched polyethylene film according to any one of [1b] to [12b]. [14b] A food package comprising the packaging material according to [13b] and a food product placed inside the packaging material.

[0092] 100 Stretched polyethylene film 101 High density polyethylene layer 1 102 Medium density polyethylene layer 103 High density polyethylene layer 2

Claims

1. A stretched polyethylene film comprising, in this order, a high-density polyethylene layer 1, a medium-density polyethylene layer, and a high-density polyethylene layer 2, wherein when a first differential scanning calorimetry (1st Run) consisting of a process of increasing the temperature from -50°C to 200°C at a heating rate of 10°C / min, an isothermal process of maintaining the temperature at 200°C for 10 minutes, and a process of decreasing the temperature from 200°C to -50°C at a heating rate of 10°C / min, and a second differential scanning calorimetry (2nd Run) consisting of a process of increasing the temperature from -50°C to 200°C at a heating rate of 10°C / min, are successively performed using a differential scanning calorimeter, an endothermic peak A is observed in the range of 10°C to 160°C in DSC curve 1 obtained by the first differential scanning calorimetry, and the heat of fusion of the endothermic peak A (ΔH m ) is 110 J / g or more and 162 J / g or less.

2. The density of the medium-density polyethylene layer measured in accordance with JIS K 7112:1999 is 910 kg / m 3 More than 935kg / m 3 2. The stretched polyethylene film of claim 1, wherein:

3. The stretched polyethylene film according to claim 1 or 2, wherein the amorphous thickness determined from a peak in the MD direction diffraction angle 2θ range of 0.2 to 0.4° by small-angle X-ray scattering (SAXS) measurement is less than 12.5 nm.

4. A stretched polyethylene film according to any one of claims 1 to 3, wherein the total amount of the high-density polyethylene layer 1 and the high-density polyethylene layer 2 in the stretched polyethylene film is 25% by mass or more and 85% by mass or less, when the entire stretched polyethylene film is taken as 100% by mass.

5. The density of the high-density polyethylene layer 1 and the high-density polyethylene layer 2, measured in accordance with JIS K 7112:1999, is 940 kg / m 3 More than 970kg / m 3 The stretched polyethylene film according to any one of claims 1 to 4, wherein:

6. The stretched polyethylene film according to any one of claims 1 to 5, wherein the MFR of the first high-density polyethylene layer and the second high-density polyethylene layer, measured in accordance with ASTM D1238 at 190°C under a load of 2.16 kg, is 0.01 g / 10 min or more and 20 g / 10 min or less.

7. The stretched polyethylene film according to any one of claims 1 to 6, wherein the medium-density polyethylene layer has an MFR of 0.01 g / 10 min or more and 20 g / 10 min or less, as measured in accordance with ASTM D1238 at 190°C under a load of 2.16 kg.

8. The stretched polyethylene film according to any one of claims 1 to 7, wherein the full width at half maximum (FWHM) of a peak in the machine direction at a diffraction angle 2θ in the range of 0.2 to 0.4°, as determined by small-angle X-ray scattering (SAXS) measurement, is 0.21° or less.

9. The stretched polyethylene film according to any one of claims 1 to 8, wherein the haze per sheet of the stretched polyethylene film measured in accordance with JIS K 7136:2000 is 16.0% or less.

10. The tensile modulus T of the stretched polyethylene film in the transverse direction is measured using a tensile tester in accordance with JIS K7127:1999 under the conditions of a measurement temperature of 23±2°C, 50±5% RH, and a tension speed of 5 mm / min. 2 The stretched polyethylene film according to any one of claims 1 to 9, wherein the stretching strength is 700 MPa or more.

11. The tensile modulus T of the stretched polyethylene film in the machine direction is measured in accordance with JIS K7127:1999 using a tensile tester under the conditions of a measurement temperature of 23±2°C, 50±5% RH, and a pulling speed of 5 mm / min. 1 and the tensile modulus in the TD direction T 2 The stretched polyethylene film according to any one of claims 1 to 10, wherein the total value of is 1500 MPa or more and 2900 MPa or less.

12. A stretched polyethylene film according to any one of claims 1 to 11, wherein the stretched polyethylene film has a heat shrinkage rate in the machine direction of 6.0% or less when heat-treated at 100°C for 15 minutes in accordance with JIS C2151:2019.

13. A stretched polyethylene film according to any one of claims 1 to 12, wherein the stretched polyethylene film has a heat shrinkage rate in the machine direction of 25.0% or less when heat-treated at 120°C for 15 minutes in accordance with JIS C2151:2019.

14. The stretched polyethylene film according to any one of claims 1 to 13, wherein at least one surface of the stretched polyethylene film is corona-treated.

15. The stretched polyethylene film according to any one of claims 1 to 14, wherein the stretched polyethylene film has a laminate strength in the machine direction of 0.7 N / 15 mm or more and 10.0 N / 15 mm or less, as measured in accordance with JIS Z 0238:1998 using a tensile tester under conditions of T-peel and a crosshead speed of 300 mm / min.

16. The number of pinholes in the stretched polyethylene film is measured using a Gelbo flex tester at a bending angle of 440 degrees, a bending speed of 40 times / min, and an atmosphere of -30°C, after 3,000 bending cycles. The number of pinholes in the stretched polyethylene film is 2,500 / m. 2 The stretched polyethylene film according to any one of claims 1 to 15, wherein:

17. The stretched polyethylene film according to any one of claims 1 to 16, wherein the tear strength in the machine direction of the stretched polyethylene film is measured using a light-load tear tester under the following conditions: test piece size: machine direction: 63.5 mm, transverse direction: 50.0 mm, pendulum weight: 96.09 g, tear length: 12.7 mm, pendulum lift angle: 90°, and is 100 mN or more and 600 mN or less.

18. The stretched polyethylene film according to any one of claims 1 to 17, wherein the overall thickness of the stretched polyethylene film is 10 μm or more and 100 μm or less.

19. The stretched polyethylene film according to any one of claims 1 to 18, which is a food packaging film.

20. A packaging material using the stretched polyethylene film according to any one of claims 1 to 19.

21. A food package comprising the packaging material of claim 20 and a food product within the packaging material.