Biaxially oriented polypropylene film, packaging body for food, and food packaging body

MYPI2025001893A0Undetermined Publication Date: 2024-03-28RM TOHCELLO CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025001893
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-28
Filing Date
2023-09-22
Publication Date
2024-03-28

AI Technical Summary

Technical Problem

Conventional biaxially oriented polypropylene films lack sufficient thermal dimensional stability, leading to issues with heat wrinkles during bag manufacturing and thermal elongation during vapor deposition and coating processes.

Method used

The thermal dimensional stability of biaxially oriented polypropylene films is improved by adjusting the crystal long period in the TD direction to 28.0 nm or less, as determined by small-angle X-ray scattering (SAXS) measurements, along with specific amorphous and crystal thicknesses, and crystal ratios, which enhances the film's performance in terms of heat sealing strength and thermal expansion coefficients.

Benefits of technology

This adjustment significantly reduces heat wrinkles during bag manufacturing and thermal elongation, improving the film's overall thermal dimensional stability, mechanical properties, and packaging performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025001893_DRAWING_001
    Figure PI2025001893_DRAWING_001
Patent Text Reader

Abstract

A biaxially oriented polypropylene film (100) including a biaxially oriented film layer (101) containing a propylene-based polymer, in which a crystal long period in a TD direction obtained from small angle X-ray scattering (SAXS) measurement is equal to or less than 28.0 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Biaxially oriented polypropylene film, food packaging and food packaging

[0001] The present invention relates to a biaxially oriented polypropylene film, a food package, and a food package.

[0002] Biaxially oriented polypropylene films (hereinafter also referred to as OPP films) have an excellent balance of performance such as processability, water vapor barrier properties, transparency, mechanical strength, and rigidity, and are used, for example, as packaging films for packaging food.

[0003] Examples of technologies relating to food packaging films using such OPP films include those described in Patent Document 1 (JP-A-2008-73926) and Patent Document 2 (JP-A-2004-82499).

[0004] Patent Document 1 describes a biaxially oriented multilayer polypropylene film comprising a biaxially oriented film made of a propylene polymer composition containing 75 to 90% by mass of a propylene homopolymer (A) and 25 to 10% by mass of a tackifier (D), the biaxially oriented film having, on one side thereof, a layer made of a propylene-α-olefin random copolymer (C) having a melting point in the range of 125 to 145°C, via a layer made of a propylene polymer (B) having a melting point of 155°C or higher, and the biaxially oriented film having, on the other side thereof, a layer made of a propylene polymer (E). Patent Document 1 also describes that the biaxially oriented multilayer polypropylene film can inhibit the seepage of petroleum resins and the like onto the film surface and has excellent lamination strength and moisture resistance.

[0005] Patent Document 2 describes a multilayer resin film that further includes a polyvinyl alcohol resin layer on at least one surface of a biaxially oriented polypropylene resin layer containing 10 to 40% by mass of a highly crystalline resin and 6 to 15% by mass of a petroleum resin, via an adhesive layer, and that has an oxygen permeability of 600 mL / m at a relative humidity of 85% RH and a temperature of 23°C. 2 day MPa or less, and the water vapor transmission rate at a relative humidity of 90% RH and a temperature of 40°C is 3.5 g / m 2Patent Document 2 describes a multilayer resin film characterized by a thickness of 20 μm or less per day. Patent Document 2 describes that the multilayer resin film has excellent oxygen gas barrier properties and moisture resistance.

[0006] JP 2008-73926 A JP 2004-82499 A

[0007] In recent years, from the perspective of environmental issues, there has been a demand for mono-material packaging materials. However, conventional, general biaxially oriented polypropylene films have sometimes lacked sufficient thermal dimensional stability in terms of suppressing thermal wrinkles at the seal area during bag production and suppressing thermal expansion during vapor deposition and coating processes. In other words, further improvement in the thermal dimensional stability of biaxially oriented polypropylene films is required in terms of suppressing thermal wrinkles at the seal area during bag production and suppressing thermal expansion during vapor deposition and coating processes.

[0008] The present invention has been made in view of the above circumstances, and provides a biaxially oriented polypropylene film, a food packaging material, and a food packaging material having improved thermal dimensional stability.

[0009] The present inventors have conducted extensive research to solve the above problems, and as a result have found that the thermal dimensional stability of biaxially oriented polypropylene films can be improved by adjusting the crystalline long period in the TD direction, as determined by small-angle X-ray scattering (SAXS) measurements, to a specific range, thereby completing the present invention.

[0010] That is, according to the present invention, there are provided the following biaxially oriented polypropylene film, food packaging material, and food packaging material.

[0011] [1] A biaxially stretched polypropylene film comprising a biaxially stretched film layer containing a propylene-based polymer, wherein the crystalline long period in the TD direction as determined by small-angle X-ray scattering (SAXS) measurement is 28.0 nm or less. [2] The biaxially stretched polypropylene film according to [1] above, wherein the amorphous thickness in the TD direction as determined by SAXS measurement is 15.5 nm or less. [3] The biaxially stretched polypropylene film according to [1] or [2] above, wherein the crystalline thickness in the TD direction as determined by SAXS measurement is 13.5 nm or less. [4] The biaxially stretched polypropylene film according to any one of [1] to [3] above, wherein the crystalline ratio at 165°C or less as determined by differential scanning calorimetry is 38% or more. [5] The biaxially stretched polypropylene film according to any one of [1] to [4] above, wherein the main melting point of the biaxially stretched polypropylene film as determined by differential scanning calorimetry is 165°C or higher and 180°C or lower. [6] The biaxially oriented polypropylene film according to any one of [1] to [5], wherein the biaxially oriented polypropylene film has a heat of fusion (ΔH) of 100 J / g or more and 150 J / g or less for the entire film, as determined by differential scanning calorimetry. [7] The biaxially oriented polypropylene film according to any one of [1] to [6], wherein the biaxially oriented polypropylene film has a heat of fusion (ΔH) of 40 J / g or more at 165°C or less, as determined by differential scanning calorimetry. [8] The biaxially oriented polypropylene film according to any one of [1] to [7], wherein the biaxially oriented polypropylene film has a crystal content of 20% or more at 165°C or less. [9] The biaxially oriented polypropylene film according to any one of [1] to [8], wherein the amount of structural units derived from α-olefins other than propylene contained in the biaxially oriented polypropylene film is 0.05 mol% or more, when the total amount of structural units derived from monomers contained in the biaxially oriented polypropylene film is taken as 100 mol%.

[10] The biaxially stretched polypropylene film according to any one of [1] to [9], which expands in the TD direction when heat-treated at 120 ° C. for 15 minutes in accordance with JIS C2151:2019.

[11] The biaxially oriented polypropylene film according to any one of [1] to

[10] above, which expands in the TD direction and shrinks in the MD direction when heat-treated at 120°C for 15 minutes in accordance with JIS C2151: 2019.

[12] The biaxially oriented polypropylene film according to any one of [1] to

[11] above, which has a thermal expansion coefficient of 0.1% or more and 2.0% or less when heat-treated at 120°C for 15 minutes in accordance with JIS C2151: 2019.

[13] The biaxially oriented polypropylene film according to any one of [1] to

[12] above, which has a heat shrinkage coefficient of 5.0% or less in the MD direction when heat-treated at 120°C for 15 minutes in accordance with JIS C2151: 2019.

[14] The biaxially oriented polypropylene film according to any one of [1] to

[13] , which has a heat shrinkage rate in the TD direction of 8.5% or less when heat-treated at 150°C for 15 minutes in accordance with JIS C2151: 2019.

[15] The biaxially oriented polypropylene film according to any one of [1] to

[14] , which has a heat shrinkage rate in the MD direction of 8.0% or less when heat-treated at 150°C for 15 minutes in accordance with JIS C2151: 2019.

[16] The heat shrinkage rates in the TD direction and the MD direction when heat-treated at 150°C for 15 minutes in accordance with JIS C2151: 2019 are each X. TD [%] and X MD When [%] is used, X TD +X MD

[17] The biaxially oriented polypropylene film according to any one of [1] to

[16] above, having a heat-sealing strength of 4.0 N / 15 mm or less when the biaxially oriented polypropylene film is heat-sealed to itself at 200°C.

[18] The biaxially oriented polypropylene film according to any one of [1] to

[17] above, having a heat-sealing strength of 1.0 N / 15 mm or less when the biaxially oriented polypropylene film is heat-sealed to itself at 170°C.

[19] The biaxially oriented polypropylene film according to any one of [1] to

[18] , wherein the propylene polymer comprises homopolypropylene (A) and at least one polymer (B) selected from the group consisting of random polypropylene (B1) and α-olefin copolymer (B2), and the MFR of the polymer (B) is 0.01 g / 10 min or more and 30 g / 10 min or less, as measured in accordance with ASTM D1238 at 230°C under a load of 2.16 kg.

[20] The biaxially oriented polypropylene film according to

[19] , wherein the homopolypropylene (A) has an isotactic mesopentad fraction (mmmm) of 96.0% or more.

[21] The biaxially oriented polypropylene film according to

[19] or

[20] , wherein the content of the polymer (B) is 1% by mass or more and 50% by mass or less, when the total mass of the biaxially oriented film layer is taken as 100% by mass.

[22] The biaxially oriented polypropylene film according to any one of

[19] to

[21] above, wherein the melting point of the polymer (B) is 50° C. or more and 155° C. or less.

[23] The biaxially oriented polypropylene film according to any one of

[19] to

[22] above, wherein the weight average molecular weight (Mw) of the polymer (B) is 100,000 or more and 1,000,000 or less.

[24] The biaxially oriented polypropylene film according to any one of

[19] to

[23] above, wherein the weight average molecular weight (Mw) / number average molecular weight (Mn) of the polymer (B) is 1.5 or more and 8.0 or less.

[25] The biaxially oriented polypropylene film according to any one of

[19] to

[24] , wherein the α-olefin copolymer (B2) comprises a random copolymer of propylene with one or more α-olefins selected from the group consisting of ethylene and α-olefins having from 4 to 10 carbon atoms.

[26] The biaxially oriented polypropylene film according to any one of [1] to

[25] , further comprising a surface resin layer on at least one side of the biaxially oriented film layer.

[27] The biaxially oriented polypropylene film according to

[26] , wherein the surface resin layer comprises homopolypropylene (A).

[28] The biaxially oriented polypropylene film according to

[27] , wherein the content of the homopolypropylene (A) in the surface resin layer is 75% by mass or more and 100% by mass or less, when the entire surface resin layer is taken as 100% by mass.

[29] The biaxially oriented polypropylene film according to any one of

[26] to

[28] , wherein the thickness of the surface resin layer is 0.1 μm or more and 10.0 μm or less.

[30] The biaxially oriented polypropylene film according to any one of [1] to

[29] , wherein the thickness of the biaxially oriented film layer is 5 μm or more and 100 μm or less.

[31] The tensile modulus T of the biaxially oriented polypropylene film in the MD direction is measured in accordance with JIS K7127 (1999) using a tensile tester under conditions of a measurement temperature of 23±2°C, 50±5% RH, and a pulling rate of 5 mm / min. 1 and the tensile modulus in the TD direction T 2 The sum of (T 1 +T 2

[32] The biaxially oriented polypropylene film according to any one of [1] to

[31] above, which is a food packaging film.

[33] A food package using the biaxially oriented polypropylene film according to any one of [1] to

[32] above.

[34] A food package comprising the food package according to

[33] above and a food product contained in the food package.

[0012] According to the present invention, it is possible to provide a biaxially oriented polypropylene film, a food packaging material, and a food packaging material having improved thermal dimensional stability.

[0013] Fig. 1 is a cross-sectional view schematically showing an example of the structure of a biaxially oriented polypropylene film of the present embodiment. Fig. 2 is a cross-sectional view schematically showing an example of the structure of a biaxially oriented polypropylene film of the present embodiment. Fig. 3 is a cross-sectional view schematically showing an example of the structure of a biaxially oriented polypropylene film of the present embodiment.

[0014] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Note that the drawings are schematic and do not correspond to the actual dimensional ratios. Note that "-" between numbers in the text indicates "above" to "below" unless otherwise specified.

[0015] 1 to 3 are cross-sectional views schematically illustrating an example of the structure of a biaxially oriented polypropylene film 100 according to this embodiment. The biaxially oriented polypropylene film 100 according to this embodiment includes a biaxially oriented film layer 101 containing a propylene-based polymer, and has a crystalline long period in the TD direction determined by small-angle X-ray scattering (SAXS) measurement of 28.0 nm or less.

[0016] As described above, further improvement in thermal dimensional stability is required for biaxially oriented polypropylene films from the viewpoint of suppressing thermal wrinkles at the seal portion during bag formation and suppressing thermal elongation during vapor deposition and coating processes. Here, the inventors have discovered through their studies that the thermal dimensional stability of the biaxially oriented polypropylene film 100 can be improved by setting the crystal long period in the TD direction determined by SAXS measurement to 28.0 nm or less, thereby arriving at the present invention. That is, the biaxially oriented polypropylene film 100 of this embodiment can improve thermal dimensional stability. Furthermore, because the biaxially oriented polypropylene film 100 of this embodiment has improved thermal dimensional stability, it can suppress thermal wrinkles at the seal portion during bag formation, thereby improving bag formability.

[0017] The crystal long period S in the TD direction of the biaxially stretched polypropylene film 100 obtained from the SAXS measurement 2is 28.0 nm or less, but from the viewpoint of further improving the thermal dimensional stability of the biaxially oriented polypropylene film 100, it is preferably 27.8 nm or less, more preferably 27.6 nm or less, even more preferably 27.0 nm or less, even more preferably 25.0 nm or less, even more preferably 23.0 nm or less, even more preferably 20.0 nm or less, even more preferably 18.0 nm or less, and even more preferably 15.0 nm or less, and from the viewpoint of further improving the performance balance between the transparency and water vapor barrier property of the biaxially oriented polypropylene film 100, it is preferably 5.0 nm or more, more preferably 8.0 nm or more, even more preferably 10.0 nm or more, even more preferably 12.0 nm or more, even more preferably 15.0 nm or more, even more preferably 18.0 nm or more, even more preferably 20.0 nm or more, even more preferably 23.0 nm or more, even more preferably 25.0 nm or more, and even more preferably 27.0 nm or more.

[0018] In addition, the crystal long period S in the MD direction of the biaxially stretched polypropylene film 100 obtained from the SAXS measurement 1 From the viewpoint of further improving the thermal dimensional stability of the biaxially oriented polypropylene film 100, it is preferably 16.5 nm or less, more preferably 16.0 nm or less, even more preferably 15.8 nm or less, and even more preferably 15.5 nm or less, and from the viewpoint of further improving the performance balance between the transparency and water vapor barrier property of the biaxially oriented polypropylene film 100, it is preferably 5.0 nm or more, more preferably 8.0 nm or more, even more preferably 10.0 nm or more, even more preferably 12.0 nm or more, and even more preferably 14.0 nm or more.

[0019] The crystal long period S in the MD direction of the biaxially stretched polypropylene film 100 obtained from the SAXS measurement 1 and the crystal long period S in the TD direction 2 The sum of (S 1 +S 2) is preferably 44.5 nm or less, more preferably 44.0 nm or less, even more preferably 43.5 nm or less, even more preferably 43.0 nm or less, even more preferably 40.0 nm or less, even more preferably 35.0 nm or less, even more preferably 32.0 nm or less, even more preferably 30.0 nm or less, and even more preferably 28.0 nm or less from the viewpoint of further improving the thermal dimensional stability of the biaxially oriented polypropylene film 100, and is preferably 15.0 nm or more, more preferably 20.0 nm or more, even more preferably 25.0 nm or more, even more preferably 28.0 nm or more, even more preferably 30.0 nm or more, even more preferably 32.0 nm or more, even more preferably 35.0 nm or more, even more preferably 38.0 nm or more, even more preferably 40.0 nm or more, and even more preferably 42.0 nm or more from the viewpoint of further improving the performance balance between the transparency and water vapor barrier property of the biaxially oriented polypropylene film 100. The crystal long period S 1 and the crystal long period S in the TD direction 2 can be measured by the method described in the Examples.

[0020] The amorphous thickness S in the TD direction of the biaxially oriented polypropylene film 100 obtained from SAXS measurement 4 From the viewpoint of further improving the thermal dimensional stability of the biaxially oriented polypropylene film 100, the amorphous thickness S is preferably 15.5 nm or less, more preferably 15.2 nm or less, even more preferably 15.0 nm or less, even more preferably 14.5 nm or less, even more preferably 13.0 nm or less, even more preferably 11.0 nm or less, even more preferably 10.0 nm or less, and even more preferably 8.0 nm or less, and from the viewpoint of further improving the performance balance between formability and transparency of the biaxially oriented polypropylene film 100, the amorphous thickness S that is easily mobile when heated is preferably 3.0 nm or more, more preferably 5.0 nm or more, even more preferably 8.0 nm or more, even more preferably 10.0 nm or more, and even more preferably 13.0 nm or more. 4 When the value is equal to or less than the upper limit, the thermal dimensional stability of the biaxially oriented polypropylene film 100 can be further improved.

[0021] In addition, the amorphous thickness S in the MD direction of the biaxially stretched polypropylene film 100 obtained by SAXS measurement 3 From the viewpoint of further improving the thermal dimensional stability of the biaxially oriented polypropylene film 100, it is preferably 9.5 nm or less, more preferably 9.0 nm or less, even more preferably 8.8 nm or less, even more preferably 8.6 nm or less, and even more preferably 8.0 nm or less, and from the viewpoint of further improving the performance balance of formability and transparency of the biaxially oriented polypropylene film 100, it is preferably 3.0 nm or more, more preferably 5.0 nm or more, even more preferably 7.0 nm or more, even more preferably 7.5 nm or more, and even more preferably 8.0 nm or more.

[0022] The amorphous thickness S in the MD direction of the biaxially oriented polypropylene film 100 obtained from SAXS measurement 3 and the amorphous thickness S in the TD direction 4 The sum of (S 3 +S 4 ) is preferably 24.5 nm or less, more preferably 24.0 nm or less, even more preferably 23.5 nm or less, even more preferably 23.0 nm or less, even more preferably 20.0 nm or less, even more preferably 18.0 nm or less, even more preferably 16.0 nm or less, and even more preferably 15.0 nm or less from the viewpoint of further improving the thermal dimensional stability of the biaxially oriented polypropylene film 100, and is preferably 5.0 nm or more, more preferably 8.0 nm or more, even more preferably 10.0 nm or more, even more preferably 13.0 nm or more, even more preferably 15.0 nm or more, even more preferably 17.0 nm or more, even more preferably 20.0 nm or more, even more preferably 22.0 nm or more, and even more preferably 23.0 nm or more from the viewpoint of further improving the balance of formability and transparency of the biaxially oriented polypropylene film 100. 3 and the amorphous thickness S in the TD direction 4 can be measured by the method described in the Examples.

[0023] The crystal thickness S in the TD direction of the biaxially oriented polypropylene film 100 obtained from SAXS measurement 6 From the viewpoint of further improving the performance balance between the formability and thermal dimensional stability of the biaxially oriented polypropylene film 100, it is preferably 13.5 nm or less, more preferably 13.0 nm or less, even more preferably 12.5 nm or less, even more preferably 12.0 nm or less, even more preferably 10.0 nm or less, and even more preferably 8.0 nm or less, and from the viewpoint of further improving the performance balance between the transparency and water vapor barrier property of the biaxially oriented polypropylene film 100, it is preferably 3.0 nm or more, more preferably 5.0 nm or more, even more preferably 8.0 nm or more, even more preferably 10.0 nm or more, even more preferably 12.0 nm or more, and even more preferably 12.5 nm or more.

[0024] In addition, the crystal thickness S in the MD direction of the biaxially stretched polypropylene film 100 obtained from the SAXS measurement 5 is preferably 9.0 nm or less, more preferably 8.0 nm or less, and even more preferably 7.5 nm or less, from the viewpoint of further improving the performance balance of the formability and thermal dimensional stability of the biaxially oriented polypropylene film 100, and is preferably 3.0 nm or more, more preferably 5.0 nm or more, and even more preferably 6.5 nm or more, from the viewpoint of further improving the performance balance of the transparency and water vapor barrier property of the biaxially oriented polypropylene film 100.

[0025] The crystal thickness S in the MD direction of the biaxially oriented polypropylene film 100 obtained from SAXS measurement 5 and the crystal thickness S in the TD direction 6 The sum of (S 5 +S 6) is preferably 21.0 nm or less, more preferably 20.5 nm or less, even more preferably 20.0 nm or less, even more preferably 19.0 nm or less, even more preferably 18.0 nm or less, even more preferably 17.0 nm or less, even more preferably 16.0 nm or less, and even more preferably 15.5 nm or less, from the viewpoint of further improving the performance balance between the formability and thermal dimensional stability of the biaxially oriented polypropylene film 100, and is preferably 5.0 nm or more, more preferably 8.0 nm or more, even more preferably 10.0 nm or more, even more preferably 13.0 nm or more, even more preferably 15.0 nm or more, even more preferably 16.0 nm or more, even more preferably 18.0 nm or more, and even more preferably 19.0 nm or more, from the viewpoint of further improving the performance balance between the transparency and water vapor barrier property of the biaxially oriented polypropylene film 100. The crystal thickness S in the MD direction of the biaxially oriented polypropylene film 100 determined by SAXS measurement 5 and the crystal thickness S in the TD direction 6 can be measured by the method described in the Examples.

[0026] The crystalline long period, amorphous thickness, and crystalline thickness of the biaxially stretched polypropylene film 100 can be adjusted, for example, by adjusting the type and content ratio of the propylene-based polymer contained in the biaxially stretched film layer 101, the thickness and stretching ratio of the biaxially stretched film layer 101, the constituent material and thickness of the surface resin layer 103, etc.

[0027] The crystalline ratio of the biaxially oriented polypropylene film 100 of this embodiment at 165°C or less, as determined by differential scanning calorimetry, is preferably 38% or more, from the viewpoint of further improving the thermal dimensional stability of the biaxially oriented polypropylene film 100.

[0028] As described above, biaxially oriented polypropylene films are required to have further improved thermal dimensional stability in order to suppress thermal wrinkles at the seal portions during bag formation and to suppress thermal elongation during vapor deposition and coating processes. Here, the inventors' studies have revealed that the amount of crystalline components at temperatures below 165°C affects thermal dimensional stability. Based on this knowledge, the inventors conducted further studies and found that the thermal dimensional stability of the biaxially oriented polypropylene film 100 can be improved by increasing the crystalline fraction at temperatures below 165°C to 38% or more. That is, the biaxially oriented polypropylene film 100 of this embodiment, which has a crystalline fraction at temperatures below 165°C of 38% or more, can further improve thermal dimensional stability. Furthermore, because such biaxially oriented polypropylene film 100 has improved thermal dimensional stability, it can further suppress thermal wrinkles at the seal portions during bag formation, thereby further improving bag formability.

[0029] The crystalline fraction of the biaxially oriented polypropylene film 100 at 165°C or below, as determined by differential scanning calorimetry, is preferably 38% or higher, but from the viewpoint of further improving the thermal dimensional stability of the biaxially oriented polypropylene film 100, it is more preferably 39% or higher, even more preferably 40% or higher, even more preferably 41% or higher, even more preferably 42% or higher, and even more preferably 43% or higher, and from the viewpoint of further improving the performance balance between the formability and thermal dimensional stability of the biaxially oriented polypropylene film 100, it is preferably 70% or lower, more preferably 65% ​​or lower, even more preferably 60% or lower, even more preferably 55% or lower, and even more preferably 50% or lower. The crystalline fraction of the biaxially oriented polypropylene film 100 at 165°C or below can be measured by the method described in the Examples.

[0030] The main melting point of the biaxially oriented polypropylene film 100, as determined by differential scanning calorimetry, is preferably 165°C or higher, more preferably 168°C or higher, and even more preferably 170°C or higher, from the viewpoint of further improving the thermal dimensional stability of the biaxially oriented polypropylene film 100, and is preferably 180°C or lower, more preferably 178°C or lower, even more preferably 175°C or lower, and even more preferably 173°C or lower, from the viewpoint of further improving the performance balance between the formability and thermal dimensional stability of the biaxially oriented polypropylene film 100. The main melting point of the biaxially oriented polypropylene film 100 can be measured by the method described in the Examples. Herein, the peak temperature of the maximum melting peak in the DSC curve is defined as the main melting point.

[0031] The heat of fusion (ΔH) of the entire biaxially oriented polypropylene film 100, as determined by differential scanning calorimetry, is preferably 100 J / g or more, more preferably 105 J / g or more, even more preferably 110 J / g or more, even more preferably 113 J / g or more, even more preferably 115 J / g or more, and even more preferably 117 J / g or more, from the viewpoint of further improving the thermal dimensional stability of the biaxially oriented polypropylene film 100. Furthermore, from the viewpoint of further improving the performance balance between the formability and thermal dimensional stability of the biaxially oriented polypropylene film 100, it is preferably 150 J / g or less, more preferably 140 J / g or less, even more preferably 130 J / g or less, and even more preferably 128 J / g or less. The heat of fusion (ΔH) of the entire biaxially oriented polypropylene film 100 can be measured by the method described in the Examples. Herein, when multiple melting peaks appear in the DSC curve, the heat of fusion (ΔH) is defined as the sum of the areas of the multiple melting peaks.

[0032] The heat of fusion (ΔH) of the biaxially oriented polypropylene film 100 at 165°C or less, as determined by differential scanning calorimetry, is preferably 40 J / g or more, more preferably 42 J / g or more, even more preferably 43 J / g or more, even more preferably 45 J / g or more, even more preferably 48 J / g or more, and even more preferably 50 J / g or more, from the viewpoint of further improving the thermal dimensional stability of the biaxially oriented polypropylene film 100. Furthermore, the heat of fusion (ΔH) of the biaxially oriented polypropylene film 100 at 165°C or less is preferably 90 J / g or less, more preferably 85 J / g or less, even more preferably 80 J / g or less, even more preferably 75 J / g or less, even more preferably 70 J / g or less, even more preferably 65 J / g or less, and even more preferably 60 J / g or less, from the viewpoint of further improving the performance balance between the formability and the thermal dimensional stability of the biaxially oriented polypropylene film 100. The heat of fusion (ΔH) of the biaxially oriented polypropylene film 100 at 165°C or less can be measured by the method described in the Examples.

[0033] The crystallinity of the biaxially oriented polypropylene film 100, as determined by differential scanning calorimetry, is preferably 40% or more, more preferably 45% or more, even more preferably 50% or more, even more preferably 53% or more, and even more preferably 55% or more, from the viewpoint of further improving the thermal dimensional stability of the biaxially oriented polypropylene film 100, and is preferably 80% or less, more preferably 75% or less, even more preferably 70% or less, even more preferably 65% ​​or less, even more preferably 62% or less, and even more preferably 60% or less, from the viewpoint of further improving the performance balance between the formability and thermal dimensional stability of the biaxially oriented polypropylene film 100. The crystallinity of the biaxially oriented polypropylene film 100 can be measured by the method described in the examples.

[0034] The crystal content of the biaxially oriented polypropylene film 100 at 165°C or less, as determined by differential scanning calorimetry, is preferably 20% or more, more preferably 22% or more, even more preferably 23% or more, and even more preferably 24% or more, from the viewpoint of further improving the thermal dimensional stability of the biaxially oriented polypropylene film 100, and is preferably 40% or less, more preferably 38% or less, even more preferably 36% or less, preferably 35% or less, and even more preferably 30% or less, from the viewpoint of further improving the performance balance between the formability and thermal dimensional stability of the biaxially oriented polypropylene film 100. The crystal content of the biaxially oriented polypropylene film 100 at 165°C or less can be measured by the method described in the Examples.

[0035] The above-mentioned properties of the biaxially oriented polypropylene film 100 determined by differential scanning calorimetry can be adjusted, for example, by adjusting the type and content ratio of the propylene-based polymer contained in the biaxially oriented film layer 101, the thickness and stretching ratio of the biaxially oriented film layer 101, the constituent material and thickness of the surface resin layer 103, etc.

[0036] The tensile modulus T of the biaxially stretched polypropylene film 100 in the MD direction is measured using a tensile tester under the conditions of a measurement temperature of 23±2°C, 50±5% RH, and a pulling speed of 5 mm / min in accordance with JIS K7127 (1999). 1 and the tensile modulus in the TD direction T 2 The sum of (T 1 +T 2 ) is preferably 3000 MPa or more, more preferably 3500 MPa or more, even more preferably 4000 MPa or more, even more preferably 5000 MPa or more, even more preferably 6000 MPa or more, even more preferably 6500 MPa or more, and is preferably 10000 MPa or less, more preferably 8000 MPa or less, even more preferably 7500 MPa or less. 1 and the tensile modulus in the TD direction T 2 The sum of (T 1 +T 2) is equal to or greater than the lower limit, the biaxially oriented polypropylene film 100 can have a better balance of performances such as thermal dimensional stability, formability, water vapor barrier properties, mechanical properties, transparency, bag-making properties, and handling properties. Furthermore, the stiffness of the biaxially oriented polypropylene film 100 can be improved, which can prevent film positional deviation during heat sealing and prevent sealing defects. That is, the tensile modulus T 1 and the tensile modulus in the TD direction T 2 The sum of (T 1 +T 2 When the tensile modulus T in the MD direction is equal to or greater than the lower limit, the biaxially oriented polypropylene film 100 can have a better balance of thermal dimensional stability, formability, water vapor barrier property, mechanical properties, transparency, bag-making properties, handling properties, and packaging suitability. 1 and the tensile modulus in the TD direction T 2 The sum of (T 1 +T 2 ) is not more than the above upper limit, problems such as breakage are less likely to occur during molding of the biaxially stretched polypropylene film 100, continuous stretch molding of the film is facilitated, and industrial continuous productivity can be further improved. Such tensile modulus is a substitute value for quantitatively measuring the stiffness of the film, and can be adjusted by, for example, adjusting the type and content ratio of the propylene-based polymer contained in the biaxially stretched film layer 101, the thickness and stretch ratio of the biaxially stretched film layer 101, the constituent material and thickness of the surface resin layer 103, etc.

[0037] In addition, the tensile modulus T of the biaxially oriented polypropylene film 100 in the MD direction 1is preferably 1000 MPa or more, more preferably 1200 MPa or more, even more preferably 1300 MPa or more, even more preferably 1400 MPa or more, even more preferably 1500 MPa or more, even more preferably 1800 MPa or more, even more preferably 2000 MPa or more, and even more preferably 2300 MPa or more, from the viewpoint of further improving the performance balance of the biaxially oriented polypropylene film 100, including thermal dimensional stability, antistatic properties, bag formability, and packaging suitability; and is preferably 4000 MPa or less, more preferably 3500 MPa or less, even more preferably 3000 MPa or less, even more preferably 2800 MPa or less, and even more preferably 2600 MPa or less, from the viewpoint of further improving the performance balance of the biaxially oriented polypropylene film 100, including thermal dimensional stability, antistatic properties, bag formability, and packaging suitability.

[0038] From the viewpoint of further improving the thermal dimensional stability of the biaxially oriented polypropylene film 100, the biaxially oriented polypropylene film 100 of this embodiment preferably has the property of expanding in the TD direction and shrinking in the MD direction when heat-treated at 120°C for 15 minutes in accordance with JIS C2151:2019.

[0039] As described above, further improvement in thermal dimensional stability is required for biaxially oriented polypropylene films from the viewpoint of suppressing thermal wrinkles at the sealed portion during bag making and suppressing thermal elongation during vapor deposition and coating processes. The inventors have discovered that the thermal dimensional stability of biaxially oriented polypropylene films 100 can be improved by having the property of expanding in the TD direction and shrinking in the MD direction when heated at 120°C for 15 minutes. Generally, a roll of biaxially oriented polypropylene film is unwound in the MD direction and subjected to tension during bag making, coating, vapor deposition, and other processes. Since the TD direction is not tensioned, the biaxially oriented polypropylene film is susceptible to thermal shrinkage when heated, leading to thermal wrinkles at the sealed portion. Furthermore, since the MD direction is tensioned, if the film has low heat resistance, it is prone to thermal elongation in the MD direction when heated. On the other hand, the biaxially oriented polypropylene film 100 of this embodiment has the property of expanding in the TD direction and shrinking in the MD direction when heated at 120°C for 15 minutes, and is therefore thought to be less susceptible to thermal shrinkage in the TD direction or thermal elongation in the MD direction when heated. Therefore, it is presumed that the biaxially oriented polypropylene film 100 of this embodiment, which has the property of expanding in the TD direction and shrinking in the MD direction when heated at 120°C for 15 minutes in accordance with JIS C2151:2019, has improved thermal dimensional stability, thereby making it possible to further suppress thermal wrinkles in the sealed portion. In other words, the biaxially oriented polypropylene film 100 of this embodiment, which has the property of expanding in the TD direction and shrinking in the MD direction when heated at 120°C for 15 minutes in accordance with JIS C2151:2019, can further improve thermal dimensional stability. Furthermore, since such biaxially oriented polypropylene film 100 has improved thermal dimensional stability, it is possible to suppress heat wrinkles in the sealed portion during bag production, thereby further improving bag production properties.

[0040] From the viewpoint of further improving the performance balance between thermal dimensional stability and bag formability, the biaxially oriented polypropylene film 100 preferably expands in the TD direction when heat-treated at 120°C for 15 minutes in accordance with JIS C2151:2019. More specifically, the thermal expansion coefficient in the TD direction of the biaxially oriented polypropylene film 100 when heat-treated at 120°C for 15 minutes is preferably 0.1% or more, more preferably 0.2% or more, even more preferably 0.3% or more, even more preferably 0.4% or more, and even more preferably 0.5% or more from the viewpoint of further improving the performance balance between thermal dimensional stability and bag formability and from the viewpoint of further suppressing thermal wrinkles in the sealed portions and obtaining bag products with good thermal wrinkles in the sealed portions, and is preferably 2.0% or less, more preferably 1.5% or less, even more preferably 1.2% or less, even more preferably 1.0% or less, and even more preferably 0.8% or less from the viewpoint of further improving the performance balance between thermal dimensional stability and bag formability. Generally, a roll of biaxially oriented polypropylene film is unwound in the MD direction, and bag-making, coating, vapor deposition, etc. are performed while tension is applied. Since no tension is applied in the TD direction, the biaxially oriented polypropylene film is susceptible to thermal shrinkage when heated, and thermal wrinkles are likely to occur in the sealed portion. On the other hand, if the thermal expansion coefficient in the TD direction when heated at 120°C for 15 minutes is within the above range, the biaxially oriented polypropylene film 100 is less likely to undergo thermal shrinkage in the TD direction even when heated, thereby making it possible to further suppress thermal wrinkles in the sealed portion. Furthermore, the thermal expansion coefficient in the TD direction of the biaxially oriented polypropylene film 100 when heated at 120°C for 15 minutes is calculated using the following method. First, a 10 cm x 10 cm test piece is cut from the biaxially oriented polypropylene film 100, and this test piece is heat-treated at 120°C for 15 minutes. Next, the TD length of the test piece after heat treatment is measured. 1 [cm], the thermal expansion coefficient in the TD direction [%] is 100 × (TD 1 -10) / 10.

[0041] Furthermore, the heat shrinkage rate in the MD direction of the biaxially oriented polypropylene film 100 when heat-treated at 120°C for 15 minutes is preferably 5.0% or less, more preferably 4.0% or less, even more preferably 3.0% or less, even more preferably 2.5% or less, even more preferably 2.2% or less, and even more preferably 2.0% or less, from the viewpoint of further improving the performance balance between thermal dimensional stability and bag-formability, and further suppressing thermal elongation of the film during processing. It may also be 0.1% or more, 0.3% or more, or 0.5% or more. Generally, a roll of biaxially oriented polypropylene film is unwound in the MD direction, and bag-forming, coating, vapor deposition, and the like are carried out while applying tension. That is, because tension is applied in the MD direction, if the film has low heat resistance, it is prone to thermal elongation in the MD direction when heated. On the other hand, if the heat shrinkage in the MD direction when heated at 120°C for 15 minutes is within the above range, it is possible to further suppress the thermal elongation in the MD direction when the biaxially oriented polypropylene film 100 is heated. The heat shrinkage in the MD direction of the biaxially oriented polypropylene film 100 when heated at 120°C for 15 minutes is calculated by the following method. First, a 10 cm x 10 cm test piece is cut out from the biaxially oriented polypropylene film 100, and this test piece is heat-treated at 120°C for 15 minutes. Next, the length in the MD direction of the test piece after heat treatment is measured. 1 When the heat shrinkage rate in the MD direction is [cm], the heat shrinkage rate [%] in the MD direction is 100 × (10 - MD 1 ) / 10.

[0042] In addition, the thermal shrinkage rate X in the TD direction of the biaxially stretched polypropylene film 100 when heat-treated at 150° C. for 15 minutes TD From the viewpoint of further improving the performance balance between thermal dimensional stability and bag formability, is preferably 8.5% or less, more preferably 7.0% or less, even more preferably 5.0% or less, even more preferably 3.0% or less, even more preferably 2.0% or less, even more preferably 1.0% or less, and even more preferably 0.8% or less, and may be 0.0% or more, 0.1% or more, or 0.2% or more.

[0043] In addition, the heat shrinkage rate X in the MD direction of the biaxially stretched polypropylene film 100 when heat-treated at 150° C. for 15 minutes is MD From the viewpoint of further improving the performance balance between thermal dimensional stability and bag formability, is preferably 8.0% or less, more preferably 7.0% or less, even more preferably 6.0% or less, even more preferably 5.5% or less, even more preferably 5.0% or less, and even more preferably 4.8% or less, and may be 0.1% or more, 0.5% or more, 1.0% or more, 1.5% or more, 2.0% or more, or 2.5% or more.

[0044] The heat shrinkage rate in the TD direction and the heat shrinkage rate in the MD direction when the biaxially stretched polypropylene film 100 was heated at 150°C for 15 minutes were respectively X TD [%] and X MD When [%] is used, X TD +X MD From the viewpoint of further improving the balance between the thermal dimensional stability and bag formability of the biaxially oriented polypropylene film 100, the X of the biaxially oriented polypropylene film 100 is preferably less than 6.0%, more preferably less than 5.0%. TD [%] and X MD [%] is calculated by the following method. First, a 10 cm x 10 cm test piece is cut out from a biaxially stretched polypropylene film 100, and this test piece is heat-treated at 150°C for 15 minutes. Then, the length in the TD direction of the test piece after the heat treatment is 1 The length of the test piece in the MD direction after heat treatment is defined as MD [cm]. 1 When [cm], X TD [%] is 100 × (10-TD 1 ) / 10, and X MD [%] is 100 x (10-MD 1 ) / 10.

[0045] The thermal expansion coefficient and thermal shrinkage coefficient of the biaxially stretched polypropylene film 100 can be adjusted by, for example, adjusting the type and content ratio of the propylene-based polymer contained in the biaxially stretched film layer 101, the thickness and stretching ratio of the biaxially stretched film layer 101, and the constituent material and thickness of the surface resin layer 103. The thermal expansion coefficient and thermal shrinkage coefficient of the biaxially stretched polypropylene film 100 can be measured in accordance with JIS C2151:2019.

[0046] The heat-seal strength (hereinafter also referred to as "heat-seal strength at 200°C") when biaxially oriented polypropylene films 100 are heat-sealed together at 200°C is preferably 4.0 N / 15 mm or less from the viewpoint of further improving the balance between thermal dimensional stability and bag-forming performance. In this specification, the heat-seal strength is used as an indicator of the heat-seal resistance of the biaxially oriented polypropylene film surface. The lower the heat-seal strength, the better the heat-seal resistance of the biaxially oriented polypropylene film surface can be determined. Here, the heat-seal strength when heat-sealed at 200°C can be measured by the following method. First, two biaxially oriented polypropylene films 100 are heat-sealed under conditions of 200°C, 2.0 kgf pressure, and 1.0 second sealing time to obtain a laminated film. Next, the two biaxially oriented polypropylene films 100 are peeled together under conditions of 15 mm width, 90-degree peel, peel speed 300 mm / min, and tension in the TD direction, and the peel strength at this time is taken as the heat-seal strength.

[0047] As described above, biaxially oriented polypropylene films are required to have further improved thermal dimensional stability in order to suppress thermal wrinkles at the sealed portions during bag production and to suppress thermal elongation during vapor deposition and coating processes. The inventors' studies have revealed that biaxially oriented polypropylene films having a heat-sealing strength of 4.0 N / 15 mm or less when heat-sealed at 200°C can have improved thermal dimensional stability. That is, the biaxially oriented polypropylene film 100 of the present embodiment, which has a heat-sealing strength of 4.0 N / 15 mm or less when heat-sealed at 200°C, can further improve thermal dimensional stability. Furthermore, because such biaxially oriented polypropylene film 100 has improved thermal dimensional stability, it can suppress thermal wrinkles at the sealed portions during bag production, thereby further improving bag formability. Furthermore, from the perspective of environmental issues, mono-material packaging materials are being sought. Therefore, a film surface with improved heat resistance compared to conventional biaxially oriented polypropylene films is required in order to suppress thermal wrinkles at the sealed portions during bag production and to suppress thermal fusion of the film to the seal bar. The biaxially oriented polypropylene film 100 of this embodiment has a heat fusion strength of 4.0 N / 15 mm or less when heat-sealed at 200°C, and has an improved performance balance between thermal dimensional stability and heat resistance of the film surface, which can further suppress heat wrinkles in the sealed area during bag production and heat fusion of the film to the seal bar.

[0048] In a package produced using the biaxially oriented polypropylene film 100, from the viewpoint of further improving the performance balance between the ability to prevent the film from fusing to the seal bar during bag making processing and the seal appearance, the heat-seal strength (TD tensile direction) of a portion of the biaxially oriented polypropylene film 100 heat-sealed under conditions of 200°C, a pressure of 2.0 kgf, and a sealing time of 1.0 second (hereinafter also referred to as "heat-seal strength at 200°C") is preferably 4.0 N / 15 mm or less, more preferably 3.5 N / 15 mm or less, even more preferably 3.0 N / 15 mm or less, even more preferably 2.5 N / 15 mm or less, even more preferably 2.0 N / 15 mm or less, even more preferably 1.5 N / 15 mm or less, and even more preferably 1.3 N / 15 mm or less. The lower limit of the heat-sealing strength of the biaxially oriented polypropylene film 100 at 200°C is not particularly limited, but may be 0.01 N / 15 mm or more, 0.05 N / 15 mm or more, 0.1 N / 15 mm or more, 0.3 N / 15 mm or more, 0.5 N / 15 mm or more, or 0.8 N / 15 mm or more. In this specification, the heat-sealing strength is used as an index of the heat-sealing resistance of the biaxially oriented polypropylene film surface. It can be determined that the lower the heat-sealing strength, the better the heat-sealing resistance of the biaxially oriented polypropylene film surface. Here, the heat-sealing strength at 200°C can be measured by the following method. First, two biaxially oriented polypropylene films 100 are heat-sealed at 200°C under conditions of 2.0 kgf pressure and 1.0 second sealing time to obtain a laminated film. Next, two biaxially oriented polypropylene films 100 were peeled off under the conditions of a width of 15 mm, 90-degree peeling, a peeling speed of 300 mm / min, and tension in the TD direction, and the peel strength at this time was defined as the heat-sealing strength. The heat-sealing strength at 200°C can be adjusted, for example, by adjusting the types and contents of the homopolypropylene (A) and polymer (B) contained in the biaxially oriented film layer 101, the thickness and stretching ratio of the biaxially oriented film layer 101, the constituent material and thickness of the surface resin layer 103, etc.

[0049] The heat-seal strength when two biaxially oriented polypropylene films 100 are heat-sealed at 170°C (hereinafter also referred to as "heat-seal strength at 170°C") is preferably 1.0 N / 15 mm or less, more preferably 0.8 N / 15 mm or less, even more preferably 0.5 N / 15 mm or less, even more preferably 0.3 N / 15 mm or less, and even more preferably 0.2 N / 15 mm or less, from the viewpoint of further improving the performance balance between thermal dimensional stability and bag formability. The lower limit of the heat-seal strength of the biaxially oriented polypropylene film 100 at 170°C is not particularly limited, but may be 0.01 N / 15 mm or more, 0.03 N / 15 mm or more, or 0.05 N / 15 mm or more. Here, the heat-seal strength when heat-sealed at 170°C can be measured by the following method. First, two biaxially oriented polypropylene films 100 are heat-sealed together at 170°C under a pressure of 2.0 kgf and a sealing time of 1.0 second to obtain a laminated film. Next, the two biaxially oriented polypropylene films 100 are peeled together at a width of 15 mm, at a 90-degree peel angle, at a peel rate of 300 mm / min, and pulled in the TD direction, and the peel strength measured at this time is defined as the heat-seal strength. The heat-seal strength at 170°C can be adjusted by, for example, adjusting the type and content of the propylene-based polymer contained in the biaxially oriented film layer 101, the thickness and stretch ratio of the biaxially oriented film layer 101, and the constituent material and thickness of the surface resin layer 103.

[0050] The haze of the biaxially stretched polypropylene film 100, measured using a haze meter in accordance with JIS K7136:2000, is preferably 5.0% or less, more preferably 3.0% or less, even more preferably 2.5% or less, even more preferably 2.0% or less, even more preferably 1.5% or less, and even more preferably 1.0% or less, from the viewpoint of further improving the transparency of the biaxially stretched polypropylene film 100. Such a haze can be adjusted, for example, by adjusting the type and content ratio of the propylene-based polymer contained in the biaxially stretched film layer 101, the thickness and stretch ratio of the biaxially stretched film layer 101, the constituent material and thickness of the surface resin layer 103, etc.

[0051] Here, food packaging produced using the biaxially oriented polypropylene film 100 exhibits sufficient water vapor barrier properties, and therefore, the biaxially oriented polypropylene film 100 is particularly suitable for use as a food packaging film for packaging foods that require water vapor barrier properties.

[0052] From the viewpoint of stably obtaining food packaging with improved water vapor barrier properties, the water vapor permeability of the biaxially oriented polypropylene film 100, measured by the following method, is preferably 20.0 g / (m 2 24h) or less, more preferably 15.0 g / (m 2 24h) or less, more preferably 12.0 g / (m 2 24h) or less, more preferably 10.0 g / (m 2 24h) or less, more preferably 8.0 g / (m 2 (Measurement Method) The biaxially oriented polypropylene film 100 is folded and two sides are heat-sealed to form a bag. Then, calcium chloride is placed inside as the contents. Next, the other side is heat-sealed to form a bag with a surface area of ​​0.01 m2 or less. 2 The resulting bag is then stored for 72 hours at 40°C and 90% RH. The mass of calcium chloride is measured before and after storage, and the difference between the masses is used to determine the water vapor permeability (g / (m 2 Such water vapor permeability can be adjusted by, for example, adjusting the type and content of the propylene-based polymer contained in the biaxially stretched film layer 101, the thickness and stretching ratio of the biaxially stretched film layer 101, the constituent material and thickness of the surface resin layer 103, etc.

[0053] The amount of structural units derived from α-olefins other than propylene contained in the biaxially oriented polypropylene film 100 is preferably 0.05 mol% or more, more preferably 0.1 mol% or more, even more preferably 0.3 mol% or more, even more preferably 0.5 mol% or more, even more preferably 1.0 mol% or more, even more preferably 3.0 mol% or more, even more preferably 5.0 mol% or more, and even more preferably 8.0 mol% or more, from the viewpoint of further improving the performance balance of the formability, thermal dimensional stability, and bag formability of the biaxially oriented polypropylene film 100, when the total amount of structural units derived from monomers contained in the biaxially oriented polypropylene film 100 is taken as 100 mol%. % or more, and more preferably 10.0 mol% or more, and from the viewpoint of further improving the performance balance of the thermal dimensional stability, water vapor barrier property, bag formability, and transparency of the biaxially oriented polypropylene film 100, it is preferably 50.0 mol% or less, more preferably 30.0 mol% or less, even more preferably 25.0 mol% or less, even more preferably 20.0 mol% or less, even more preferably 15.0 mol% or less, even more preferably 12.0 mol% or less, even more preferably 10.0 mol% or less, even more preferably 8.0 mol% or less, even more preferably 5.0 mol% or less, even more preferably 2.0 mol% or less, and even more preferably 1.0 mol% or less. When the amount of structural units derived from α-olefins other than propylene contained in the biaxially stretched polypropylene film 100 is within the above range, the softening effect of the structural units derived from α-olefins exhibits an effect of suppressing the yield point stress at the start of stretching in the stretching process, improving ease of formability, and in addition, the effect of lowering the melting point of the structural units derived from α-olefins more efficiently relieves residual stress in the heat setting process during film formation, improving formability and suppressing thickness unevenness, resulting in further improved thermal dimensional stability of the biaxially stretched polypropylene film 100. The amount of structural units derived from α-olefins other than propylene in the biaxially stretched polypropylene film 100 can be measured by the method described in the Examples.

[0054] The thickness of the biaxially oriented polypropylene film 100 is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 12 μm or more, and even more preferably 15 μm or more, from the viewpoint of further improving the balance of performance such as thermal dimensional stability, formability, water vapor barrier property, cost, mechanical properties, transparency, bag formability, handleability, appearance, and lightness, and is preferably 100 μm or less, more preferably 50 μm or less, even more preferably 40 μm or less, even more preferably 30 μm or less, and even more preferably 25 μm or less.

[0055] Each layer constituting the biaxially oriented polypropylene film 100 will be described below.

[0056] [Biaxially oriented film layer] The biaxially oriented film layer 101 (also referred to as a biaxially oriented polypropylene-based film layer) contains a propylene-based polymer. The biaxially oriented film layer 101 is formed, for example, by biaxially stretching a film made of a propylene-based polymer composition containing a propylene-based polymer.

[0057] The biaxially stretched film layer 101 may be a single layer or may have a structure in which a plurality of layers made of a propylene-based polymer composition are laminated, but it is necessary that the biaxially stretched film layer 101 is biaxially stretched.

[0058] The thickness of the biaxially oriented film layer 101 is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 12 μm or more, and even more preferably 15 μm or more, from the viewpoint of further improving the performance balance of the biaxially oriented polypropylene film 100, such as thermal dimensional stability, formability, water vapor barrier property, cost, mechanical properties, transparency, bag formability, handleability, appearance, and lightness, and is preferably 100 μm or less, more preferably 50 μm or less, even more preferably 40 μm or less, even more preferably 30 μm or less, and even more preferably 20 μm or less.

[0059] In the biaxially oriented polypropylene film 100, the ratio of the thickness of the biaxially oriented film layer 101 to the total thickness of the biaxially oriented polypropylene film 100 is preferably 50% or more, more preferably 60% or more, even more preferably 70% or more, even more preferably 75% or more, and preferably 100% or less, more preferably 99% or less, even more preferably 95% or less, even more preferably 90% or less.

[0060] (Propylene-Based Polymer Composition) The propylene-based polymer composition of the present embodiment contains a propylene-based polymer. From the viewpoint of further improving the balance of performance of the biaxially stretched polypropylene film 100, such as thermal dimensional stability, environmental compatibility, heat resistance, water vapor barrier property, transparency, cost, mechanical properties, rigidity, bag formability, flowability, moldability, handleability, appearance, and lightness, the content of the propylene-based polymer in the propylene-based polymer composition of the present embodiment, i.e., the biaxially stretched film layer 101, is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, and still more preferably 98% by mass or more, when the entire propylene-based polymer composition is taken as 100% by mass.

[0061] (Propylene-Based Polymer) The propylene-based polymer of this embodiment is a polymer containing structural units derived from propylene, and examples thereof include homopolypropylene (A); and at least one polymer (B) selected from the group consisting of random polypropylene (B1) and an α-olefin copolymer (B2). From the viewpoint of further improving the balance of thermal dimensional stability and antistatic properties of the biaxially stretched polypropylene film 100, the propylene-based polymer of this embodiment preferably contains homopolypropylene (A) and at least one polymer (B) selected from the group consisting of random polypropylene (B1) and an α-olefin copolymer (B2), and more preferably contains homopolypropylene (A) and at least one polymer (B) selected from the group consisting of random polypropylene (B1) and an α-olefin copolymer (B2), and the MFR of the polymer (B) measured in accordance with ASTM D1238 under conditions of 230°C and a load of 2.16 kg is 0.01 g / 10 min or more and 30.0 g / 10 min or less.

[0062] As described above, biaxially oriented polypropylene films are required to have further improved thermal dimensional stability in order to suppress thermal wrinkles at the seal portion during bag making and to suppress thermal elongation during vapor deposition and coating processes. However, when highly crystalline homopolypropylene is used to improve thermal dimensional stability, its high crystallinity results in a high yield stress during molding, which causes the stretching point to become unstable, making it difficult to achieve sufficient improvement in thermal dimensional stability. The inventors have discovered that using a combination of homopolypropylene (A) and at least one polymer (B) selected from the group consisting of random polypropylene (B1) and an α-olefin copolymer (B2) as the propylene polymer constituting the OPP film efficiently relieves the residual stress in the film, thereby improving the thermal dimensional stability of the biaxially oriented polypropylene film. Specifically, the biaxially oriented polypropylene film 100 of this embodiment, which contains homopolypropylene (A) and at least one polymer (B) selected from the group consisting of random polypropylene (B1) and an α-olefin copolymer (B2), can further improve thermal dimensional stability. Furthermore, since such biaxially oriented polypropylene film 100 has improved thermal dimensional stability, it is possible to more effectively prevent thermal wrinkles in the sealed portion during bag production, thereby further improving bag production properties.

[0063] (Homopolypropylene (A)) Examples of the homopolypropylene (A) include propylene homopolymers and propylene-based copolymers having a content of structural units derived from α-olefins other than propylene of 2.0 mol% or less. When the total content of the structural units constituting the homopolypropylene (A) is taken as 100 mol%, the content of structural units derived from propylene in the homopolypropylene (A) is 98.0 mol% or more, preferably 98.5 mol% or more, more preferably 98.7 mol% or more, even more preferably 99.0 mol% or more, even more preferably 99.5 mol% or more, and still more preferably 99.8 mol% or more, and is, for example, 100.0 mol% or less.

[0064] The α-olefin other than propylene includes, for example, one or more selected from the group consisting of ethylene and α-olefins having from 4 to 20 carbon atoms, preferably one or more selected from the group consisting of ethylene and α-olefins having from 4 to 6 carbon atoms, more preferably at least one selected from the group consisting of ethylene and 1-butene, and even more preferably ethylene. The content of structural units derived from α-olefins other than propylene, when the entire homopolypropylene (A) is taken as 100 mol%, is preferably 2.0 mol% or less, more preferably 1.5 mol% or less, even more preferably 1.3 mol% or less, even more preferably 1.0 mol% or less, even more preferably 0.5 mol% or less, and even more preferably 0.2 mol% or less. The homopolypropylene (A) in the biaxially stretched film layer 101 may be used singly or in combination of two or more types.

[0065] The isotactic mesopentad fraction (mmmm) of the homopolypropylene (A) is preferably 96.0% or more, more preferably 96.5% or more, even more preferably 97.0% or more, even more preferably 97.3% or more, even more preferably 97.5% or more, even more preferably 97.8% or more, and even more preferably 98.0% or more, from the viewpoint of further improving the performance balance of the biaxially oriented polypropylene film 100, such as thermal dimensional stability, heat resistance, water vapor barrier property, mechanical properties, rigidity, and bag formability. The upper limit of the isotactic mesopentad fraction (mmmm) of the homopolypropylene (A) is not particularly limited, but from the viewpoint of ease of production, it is 99.5% or less, more preferably 99.3% or less, and even more preferably 99.0% or less. The isotactic mesopentad fraction (mmmm) is an index of stereoregularity, 13 It can be determined by a known method from a C-nuclear magnetic resonance (NMR) spectrum. When two or more types of homopolypropylenes are used as the homopolypropylene (A), the isotactic mesopentad fraction of the homopolypropylene (A) can be the isotactic mesopentad fraction of a mixture obtained by melt blending two or more types of homopolypropylene (A) by a known method.

[0066] The melt flow rate (MFR) of the homopolypropylene (A), measured in accordance with ASTM D1238 under conditions of 230°C and a load of 2.16 kg, is preferably 0.5 g / 10 min or more, more preferably 1.0 g / 10 min or more, and even more preferably 2.0 g / 10 min or more, from the viewpoint of further improving the balance of fluidity and moldability, and is preferably 20.0 g / 10 min or less, more preferably 10.0 g / 10 min or less, and even more preferably 7.0 g / 10 min or less, from the viewpoint of further stabilizing moldability. When two or more types of homopolypropylenes are used as the homopolypropylene (A), the MFR of the homopolypropylene (A) can be the MFR of a mixture obtained by melt-blending two or more types of homopolypropylenes (A) by a known method.

[0067] The melting point of the homopolypropylene (A) is preferably 150° C. or higher, more preferably 155° C. or higher, even more preferably 160° C. or higher, and even more preferably 163° C. or higher, from the viewpoint of further improving the balance of performance such as thermal dimensional stability, heat resistance, water vapor barrier property, mechanical properties, rigidity, bag formability, flowability, and moldability of the biaxially oriented polypropylene film 100, and is preferably 180° C. or lower, more preferably 175° C. or lower, even more preferably 170° C. or lower, and even more preferably 168° C. or lower. When two or more types of homopolypropylenes are used as the homopolypropylene (A), the melting point of the homopolypropylene (A) is the peak temperature of the maximum melting peak.

[0068] The homopolypropylene (A) can be produced by various methods, for example, by using a known catalyst such as a Ziegler-Natta catalyst or a metallocene catalyst.

[0069] (Polymer (B)) The polymer (B) contains at least one selected from the group consisting of random polypropylene (B1) and α-olefin copolymer (B2), and preferably contains random polypropylene (B1).

[0070] The melt flow rate (MFR) of polymer (B), measured in accordance with ASTM D1238 under conditions of 230°C and a load of 2.16 kg, is preferably 0.01 g / 10 min or more, more preferably 0.1 g / 10 min or more, even more preferably 0.5 g / 10 min or more, even more preferably 1.0 g / 10 min or more, and even more preferably 2.0 g / 10 min or more, from the viewpoint of further improving the performance balance between formability and thermal dimensional stability of the biaxially oriented polypropylene film 100, and is preferably 30.0 g / 10 min or less, more preferably 20.0 g / 10 min or less, even more preferably 15.0 g / 10 min or less, even more preferably 12.0 g / 10 min or less, and even more preferably 10.0 g / 10 min or less. When two or more polymers are used as polymer (B), the MFR of a mixture obtained by melt-blending two or more polymers (B) by a known method can be used.

[0071] The melting point of the polymer (B) is preferably 50° C. or higher, more preferably 60° C. or higher, even more preferably 70° C. or higher, even more preferably 80° C. or higher, and even more preferably 90° C. or higher, from the viewpoint of further improving the balance of performance such as thermal dimensional stability, heat resistance, water vapor barrier property, mechanical properties, rigidity, bag formability, flowability, and moldability of the biaxially oriented polypropylene film 100, and is preferably 155° C. or lower, more preferably 150° C. or lower, even more preferably 148° C. or lower, and even more preferably 145° C. or lower. When two or more polymers are used as the polymer (B), the melting point of the polymer (B) is the peak temperature of the maximum melting peak.

[0072] The weight average molecular weight (Mw) of the polymer (B) is preferably 100,000 or more, more preferably 150,000 or more, even more preferably 200,000 or more, and even more preferably 220,000 or more, from the viewpoint of further improving the performance balance of the biaxially oriented polypropylene film 100 among formability, thermal dimensional stability, blocking resistance, and sheet payout property; and is preferably 1,000,000 or less, more preferably 800,000 or less, more preferably 600,000 or less, even more preferably 500,000 or less, and even more preferably 450,000 or less, from the viewpoint of further improving the thermal dimensional stability.

[0073] The weight-average molecular weight (Mw) / number-average molecular weight (Mn) ratio of polymer (B) is preferably 1.5 or more, more preferably 1.8 or more, from the viewpoint of further improving the performance balance of the biaxially oriented polypropylene film 100 in terms of formability, thermal dimensional stability, blocking resistance, and sheet payout ability. Also, from the viewpoint of further improving the performance balance of the biaxially oriented polypropylene film 100 in terms of formability, thermal dimensional stability, blocking resistance, and sheet payout ability, it is preferably 8.0 or less, more preferably 7.5 or less, even more preferably 7.0 or less, and even more preferably 6.8 or less. When two or more polymers are used as polymer (B), the weight-average molecular weight (Mw) and number-average molecular weight (Mn) of polymer (B) can be determined by the method described in the examples.

[0074] The content of polymer (B) is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, when the entire biaxially oriented film layer 101 is taken as 100% by mass, from the viewpoint of further improving the performance balance between the formability and thermal dimensional stability of the biaxially oriented polypropylene film 100; and from the viewpoint of further improving the performance balance of the biaxially oriented polypropylene film 100, such as thermal dimensional stability, water vapor barrier property, transparency, mechanical properties, rigidity, bag formability, fluidity, and formability, the content is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, even more preferably 25% by mass or less, even more preferably 22% by mass or less, and even more preferably 20% by mass or less.

[0075] (Random Polypropylene (B1)) The random polypropylene (B1) comprises a random copolymer of propylene and an α-olefin other than propylene, in which the content of structural units derived from the α-olefin other than propylene is more than 2.0 mol % and not more than 15.0 mol %. The α-olefin other than propylene comprises, for example, one or more selected from the group consisting of ethylene and α-olefins having from 4 to 20 carbon atoms, preferably one or more selected from the group consisting of ethylene and α-olefins having from 4 to 6 carbon atoms, more preferably at least one selected from ethylene and 1-butene, and even more preferably ethylene.

[0076] The content of structural units derived from α-olefins other than propylene in the random polypropylene (B1), when the entire random polypropylene (B1) is taken as 100 mol%, is preferably more than 2.0 mol%, more preferably 2.5 mol% or more, even more preferably 3.0 mol% or more, even more preferably 3.5 mol% or more, and even more preferably 4.0 mol% or more, from the viewpoint of further improving the performance balance of formability, thermal dimensional stability, and bag formability of the biaxially oriented polypropylene film 100. Furthermore, it is preferably 15.0 mol% or less, more preferably 12.0 mol% or less, even more preferably 10.0 mol% or less, even more preferably 8.0 mol% or less, and even more preferably 6.5 mol% or less, from the viewpoint of further improving the performance balance of thermal dimensional stability, water vapor barrier property, bag formability, and transparency of the biaxially oriented polypropylene film 100. The amount of structural units derived from α-olefins other than propylene can be measured by the method described in the Examples.

[0077] The random polypropylene (B1) preferably comprises one or more selected from the group consisting of a propylene-ethylene random copolymer, a propylene-ethylene-1-butene random copolymer, and a propylene-1-butene random copolymer, more preferably comprises one or more selected from the group consisting of a propylene-ethylene random copolymer and a propylene-1-butene random copolymer, and even more preferably comprises a propylene-ethylene random copolymer. The random polypropylene (B1) in the biaxially stretched film layer 101 may be used alone or in combination of two or more.

[0078] (α-Olefin Copolymer (B2)) The α-olefin copolymer (B2) is a copolymer of two or more types of α-olefins, and includes, for example, an α-olefin copolymer in which the content of structural units derived from an α-olefin other than propylene exceeds 15.0 mol%. The α-olefin copolymer (B2) includes a random copolymer of propylene and an α-olefin other than propylene, in which the content of structural units derived from an α-olefin other than propylene exceeds 15.0 mol%. The α-olefin other than propylene includes, for example, one or more selected from the group consisting of ethylene and α-olefins having from 4 to 10 carbon atoms, preferably one or more selected from the group consisting of α-olefins having from 4 to 8 carbon atoms, more preferably at least one selected from 1-butene and 1-octene, and even more preferably 1-butene.

[0079] The content of structural units derived from α-olefins other than propylene in the α-olefin copolymer (B2), when the entire α-olefin copolymer (B2) is taken as 100 mol%, is preferably more than 15.0 mol%, more preferably 20.0 mol% or more, even more preferably 30.0 mol% or more, even more preferably 50.0 mol% or more, even more preferably 70.0 mol% or more, and even more preferably 80.0 mol% or more, from the viewpoint of further improving the performance balance of formability, thermal dimensional stability, and bag formability of the biaxially oriented polypropylene film 100. Furthermore, it is preferably 99.0 mol% or less, more preferably 98.0 mol% or less, even more preferably 95.0 mol% or less, even more preferably 92.0 mol% or less, and even more preferably 90.0 mol% or less, from the viewpoint of further improving the performance balance of thermal dimensional stability, water vapor barrier property, bag formability, and transparency of the biaxially oriented polypropylene film 100. The amount of structural units derived from α-olefins other than propylene in the α-olefin copolymer (B2) can be measured by the method described in the Examples.

[0080] The α-olefin copolymer (B2) preferably comprises a random copolymer of propylene and one or more α-olefins selected from the group consisting of ethylene and α-olefins having from 4 to 10 carbon atoms, more preferably a random copolymer of propylene and one or two α-olefins selected from the group consisting of 1-butene and 1-octene, and even more preferably a random copolymer of propylene and 1-butene. The α-olefin copolymer (B2) in the biaxially stretched film layer 101 may be used singly or in combination of two or more.

[0081] The polymer (B) can be produced by various methods, for example, by using a known catalyst such as a Ziegler-Natta catalyst or a metallocene catalyst.

[0082] (Other Components) If necessary, various additives such as a tackifier, a heat stabilizer, a weather stabilizer, an antioxidant, an ultraviolet absorber, a lubricant, a slipping agent, a nucleating agent, an antiblocking agent, an antistatic agent, an antifogging agent, a pigment, a dye, and an inorganic or organic filler may be added to the propylene polymer composition of the present embodiment, within a range that does not impair the object of the present embodiment.

[0083] (Method for preparing propylene polymer composition) The propylene polymer composition of the present embodiment can be prepared by mixing or melting and kneading the components using a dry blend, a tumbler mixer, a Banbury mixer, a single-screw extruder, a twin-screw extruder, a high-speed twin-screw extruder, a heated roll, or the like.

[0084] [Surface Resin Layer] The biaxially oriented polypropylene film 100 preferably further comprises a surface resin layer 103 on at least one surface of the biaxially oriented film layer 101, from the viewpoint of imparting functions such as heat fusion resistance, heat sealing properties, antistatic properties, blocking resistance, printability, and slip properties to the film surface depending on the purpose. The surface resin layer 103 may be provided on both surfaces of the biaxially oriented film layer 101. By providing the surface resin layer 103 on both surfaces of the biaxially oriented film layer 101, different functions can be imparted to each surface of the film. Furthermore, the surface resin layer 103 is preferably provided on the outermost layer of the biaxially oriented polypropylene film 100, from the viewpoint of further improving functions such as heat fusion resistance, heat sealing properties, antistatic properties, blocking resistance, printability, and slip properties of the biaxially oriented polypropylene film 100 depending on the purpose.

[0085] The surface resin layer 103 is preferably provided so as to be in direct contact with the surface of the biaxially oriented film layer 101. This simplifies the manufacturing process of the biaxially oriented polypropylene film 100.

[0086] In the biaxially oriented polypropylene film 100, the thickness of the surface resin layer 103 is preferably 0.1 μm or more, more preferably 0.2 μm or more, even more preferably 0.5 μm or more, even more preferably 1.0 μm or more, and even more preferably 1.5 μm or more, from the viewpoint of further improving the heat-sealing resistance, antistatic properties, blocking resistance, printability, slip properties, and other properties of the biaxially oriented polypropylene film 100. Furthermore, from the viewpoint of further improving the balance of performance, such as heat-sealing resistance, thermal dimensional stability, formability, cost, mechanical properties, transparency, environmental compatibility, and light weight, of the biaxially oriented polypropylene film 100, the thickness is preferably 10.0 μm or less, more preferably 8.0 μm or less, even more preferably 6.0 μm or less, even more preferably 5.0 μm or less, and even more preferably 3.0 μm or less. Here, the thickness of the surface resin layer 103 refers to the thickness of the surface resin layer 103 provided on one side of the biaxially oriented film layer 101. That is, in this embodiment, when the surface resin layer 103 is provided on both sides of the biaxially stretched film layer 101, the above thickness of the surface resin layer 103 indicates the thickness of the surface resin layer 103 provided on one side of the biaxially stretched film layer 101.

[0087] In the biaxially oriented polypropylene film 100, the surface resin layer 103 is preferably a single layer, which can further simplify the manufacturing process of the biaxially oriented polypropylene film 100.

[0088] The surface resin layer 103 is preferably formed by biaxially stretching simultaneously with the biaxially stretched film layer 101 in a state before biaxial stretching. This allows the biaxially stretched polypropylene film 100 to be produced by a molding method such as co-extrusion, i.e., using a laminated film produced in a single molding process, thereby further simplifying the manufacturing process of the biaxially stretched polypropylene film 100. Therefore, the surface resin layer 103 is preferably biaxially stretched.

[0089] The surface resin layer 103 may be subjected to a surface treatment in order to further improve the balance between printability and blocking resistance of the biaxially oriented polypropylene film 100. Specifically, the surface may be subjected to a surface activation treatment such as corona treatment, flame treatment, plasma treatment, primer coating treatment, or ozone treatment.

[0090] The surface resin layer 103 is composed of, for example, a polyolefin-based resin composition (A) containing a polyolefin. The polyolefin constituting the surface resin layer 103 includes, for example, one or more selected from the group consisting of homopolymers or copolymers of α-olefins such as ethylene, propylene, 1-butene, hexene-1,4-methyl-pentene-1, and 1-octene; high-pressure low-density polyethylene; linear low-density polyethylene (LLDPE); high-density polyethylene; homopolypropylene; random copolymers of propylene and α-olefins having from 2 to 10 carbon atoms; ethylene-vinyl acetate copolymers (EVA); and ionomer resins. Among these, homopolypropylene is preferred as the polyolefin constituting the surface resin layer 103 from the viewpoint of further improving the balance of performance of the biaxially oriented polypropylene film 100, such as heat fusion resistance, thermal dimensional stability, heat resistance, water vapor barrier properties, transparency, mechanical properties, rigidity, bag formability, flowability, and moldability. Here, a preferred embodiment of the homopolypropylene constituting the surface resin layer 103 is the same as the homopolypropylene (A) described above. That is, the homopolypropylene constituting the surface resin layer 103 preferably contains the homopolypropylene (A) described above.

[0091] From the viewpoint of further improving the performance balance of the biaxially oriented polypropylene film 100, such as heat fusion resistance, thermal dimensional stability, heat resistance, water vapor barrier property, transparency, mechanical properties, rigidity, bag formability, fluidity, and moldability, the content of polyolefin in the polyolefin resin composition (A), i.e., the surface resin layer 103, is preferably 75% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, even more preferably 99% by mass or more, and preferably 100% by mass or less, when the entire polyolefin resin composition (A), i.e., the entire surface resin layer 103, is taken as 100% by mass. From the viewpoint of further improving the balance of performance such as heat fusion resistance, thermal dimensional stability, heat resistance, water vapor barrier property, transparency, mechanical properties, rigidity, bag formability, flowability, and moldability of the biaxially oriented polypropylene film 100, the content of homopolypropylene (A) in the polyolefin resin composition (A), i.e., the surface resin layer 103, is preferably 75% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, even more preferably 99% by mass or more, and preferably 100% by mass or less, when the entire polyolefin resin composition (A), i.e., the entire surface resin layer 103, is taken as 100% by mass.

[0092] (Other Components) If necessary, various additives such as a tackifier, a heat stabilizer, a weather stabilizer, an antioxidant, an ultraviolet absorber, a lubricant, a slipping agent, a nucleating agent, an antiblocking agent, an antistatic agent, an antifogging agent, a pigment, a dye, and an inorganic or organic filler may be added to the polyolefin resin composition (A) constituting the surface resin layer 103, within a range that does not impair the object of this embodiment.

[0093] (Method for preparing polyolefin resin composition (A)) The polyolefin resin composition (A) can be prepared, for example, by mixing or melting and kneading the components using a dry blend, a tumbler mixer, a Banbury mixer, a single-screw extruder, a twin-screw extruder, a high-speed twin-screw extruder, a heat roll, or the like.

[0094] <Method for Producing Biaxially Stretched Polypropylene Film> The biaxially oriented polypropylene film 100 can be obtained by, for example, co-extrusion molding a propylene-based polymer composition for forming the biaxially oriented film layer 101 and, if necessary, a polyolefin-based resin composition (A) for forming the surface resin layer 103 into a film, and then biaxially stretching the resulting film using a known biaxially oriented film production method such as simultaneous biaxial stretching, sequential biaxial stretching, or inflation biaxial stretching. The molding apparatus and molding conditions are not particularly limited, and conventionally known molding apparatuses and molding conditions can be used. Examples of molding apparatus that can be used include a T-die extruder, a multilayer T-die extruder, an inflation molding machine, and a multilayer inflation molding machine. For example, known OPP film production conditions can be used for the biaxial stretching conditions. More specifically, in the sequential biaxial stretching method, for example, the stretching temperature in the MD direction may be 100°C to 145°C, the stretching ratio in the MD direction may be in the range of 4.5 to 6 times, the stretching temperature in the TD direction may be 130°C to 190°C, and the stretching ratio in the TD direction may be in the range of 9 to 11 times. The biaxially stretched polypropylene film 100 can also be obtained by separately molding the biaxially stretched film layer 101 and, if necessary, the surface resin layer 103, and laminating and molding these together.

[0095] <Uses of Biaxially Stretched Polypropylene Film> The biaxially oriented polypropylene film 100 can also be suitably used as a food packaging film that constitutes a food package.

[0096] The food packaging of this embodiment is a packaging that uses the biaxially oriented polypropylene film 100, and is, for example, a packaging bag used for containing food. Furthermore, the food packaging of this embodiment may use the biaxially oriented polypropylene film 100 in only a portion thereof, or the biaxially oriented polypropylene film 100 may be used for the entire food packaging, depending on the application.

[0097] The food package of this embodiment includes the food package of this embodiment and food contained in the food package. That is, the food package of this embodiment is the food package of this embodiment that contains food.

[0098] Although the embodiments of the present invention have been described above with reference to the drawings, these are merely examples of the present invention, and various other configurations may be adopted. The biaxially oriented polypropylene film 100 may further include one or more layers selected from the group consisting of a sealant layer and a coating layer. The biaxially oriented polypropylene film 100 may also be used as a raw sheet for coating.

[0099] The present embodiment will be described in detail below with reference to examples and comparative examples, but the present embodiment is not limited to the descriptions of these examples.

[0100] 1. Raw Materials The raw materials used in the Examples and Comparative Examples are as follows: (1) Homopolypropylene (A) h-PP1: Homopolypropylene (MFR: 3.0 g / 10 min, melting point: 165°C, isotactic mesopentad fraction (mmmm): 98.0%, Mw: 370,000, Mn: 68,000, Mw / Mn: 5.4, content of propylene-derived structural units: 100 mol%) (2) Polymer (B) r-PP1: Random polypropylene (MFR: 7.0 g / 10 min, melting point: 139°C, Mw: 322,000, Mn: 50,700, Mw / Mn: 6.4, content of ethylene-derived structural units: 3.2 mol%, content of 1-butene-derived structural units: 2.9 mol%, content of propylene-derived structural units: 93.9 mol%) BPR1: 1-butene propylene copolymer (MFR: 9.0 g / 10 min, melting point: 100°C, Mw: 227,000, Mn: 114,000, Mw / Mn: 2.0, content of structural units derived from 1-butene: 88.9 mol%, content of structural units derived from propylene: 11.1 mol%)

[0101] 2. Measurement and Evaluation Methods (1) Isotactic mesopentad fraction (mmmm) of homopolypropylene (A) The isotactic mesopentad fraction (mesopentad fraction, (mmmm)) was measured using a nuclear magnetic resonance apparatus (AVANCE III cryo-500 model, manufactured by Bruker Biospin). 13Measurement was performed by C-NMR. The sample was dissolved in the following measurement solvent and the measurement was performed, and the evaluation was performed based on the integrated intensity of each signal. [Measurement conditions] Measurement nucleus: 13 C (125 MHz) Measurement mode: Single pulse proton broadband decoupling Pulse width: 45° Number of points: 64 k Repetition time: 5.5 seconds Measurement solvent: orthodichlorobenzene / heavy benzene (4:1) Sample concentration: 50 mg / 0.6 mL Measurement temperature: 120 °C Window function: exponential (BF: 0.5 Hz) Chemical shift reference: mmmm (CH 3 ): 21.59ppm

[0102] (2) MFR of homopolypropylene (A) and polymer (B) Measured in accordance with ASTM D1238 at 230° C. and under a load of 2.16 kg.

[0103] (3) Melting points of homopolypropylene (A) and polymer (B) Using a differential scanning calorimeter (product name: Q200DSC manufactured by TA Instruments), homopolypropylene (A) and polymer (B) were subjected to a first differential scanning calorimetry (1st Run) consisting of a process of increasing the temperature from -30°C to 250°C at a heating rate of 10°C / min and a process of decreasing the temperature from 250°C to -30°C at a heating rate of 10°C / min under a nitrogen stream, and a second differential scanning calorimetry (2nd Run) consisting of a process of increasing the temperature from -30°C to 250°C at a heating rate of 10°C / min. The peak temperature of the maximum melting peak in the DSC curve in the 2nd Run was taken as the melting point.

[0104] (4) Weight-average molecular weight (Mw) and number-average molecular weight (Mn) of homopolypropylene (A) and polymer (B) The weight-average molecular weight (Mw) and number-average molecular weight (Mn) of homopolypropylene (A) and polymer (B) were measured by gel permeation chromatography (GPC). The GPC method was performed using a gel permeation chromatograph (Tosoh Corporation, HLC-8321 GPC / HT type) as follows. The separation columns were two TSKgel GNH6-HT and two TSKgel GNH6-HTL, each with a diameter of 7.5 mm and a length of 300 mm. The column temperature was 145°C, the mobile phase contained o-dichlorobenzene and 0.025% by mass of BHT as an antioxidant, and was moved at a rate of 1.0 mL / min. The sample concentration was 0.1% (w / v), the sample injection volume was 400 μL, and a differential refractometer was used as the detector. The molecular weight was calculated as polypropylene equivalent using monodisperse polystyrene as the standard.

[0105] (5) Measurement of the content of structural units derived from α-olefins other than propylene in the homopolypropylene (A) and polymer (B), and the content of structural units derived from α-olefins other than propylene contained in the biaxially stretched polypropylene film. The content of structural units derived from α-olefins other than propylene in the homopolypropylene (A) and polymer (B), and the content of structural units derived from α-olefins other than propylene contained in the biaxially stretched polypropylene film were measured using a nuclear magnetic resonance apparatus (AVANCE III cryo-500 model, manufactured by Bruker Biospin). 13 Measurement was performed by C-NMR. The sample was dissolved in the following measurement solvent and the measurement was performed, and evaluation was performed based on the integrated intensity of each signal. 13C-NMR spectroscopy was performed using the following methods: Macromolecules (1982) Ethylene-1-Butene Copolymers. 1. Commoner Sequence Distribution and Macromolecules (1977) Carbon-13 Nuclear Magnetic Resonance Determination of Monomer Composition and Sequence Distribution in Ethylene-Propylene Copolymers Prepared with a Stereoregular Catalyst. Signals were assigned with reference to the FTIR System and the like, and the content (mol %) of ethylene-derived structural units, the content (mol %) of propylene-derived structural units, and the content (mol %) of 1-butene-derived structural units in each polymer were quantified. [Measurement conditions] Measurement nucleus: 13 C (125 MHz) Measurement mode: Single pulse proton broadband decoupling Pulse width: 45° Number of points: 64 k Repetition time: 5.5 seconds Measurement solvent: orthodichlorobenzene / heavy benzene (4:1) Sample concentration: 50 mg / 0.6 mL Measurement temperature: 120°C Window function: exponential (BF: 0.5 Hz) Furthermore, to measure the content of structural units derived from α-olefins other than propylene contained in a biaxially stretched polypropylene film, a biaxially stretched polypropylene film was used as a sample.

[0106] (6) Tensile Modulus A 15 mm x 15 cm test piece was cut out from a biaxially stretched polypropylene film. Then, the tensile modulus T of the test piece in the MD direction was measured using a tensile tester manufactured by Orientec Co., Ltd., in accordance with JIS K7127 (1999) under the conditions of a measurement temperature of 23±2°C, 50±5% RH, and a pulling speed of 5 mm / min. 1 and tensile modulus in the TD direction T 2 were measured respectively.

[0107] (7) Small-Angle X-Ray Scattering (SAXS) Measurement of Biaxially Stretched Polypropylene Film For the biaxially stretched polypropylene film of each example, the MD direction of the film was set to the top and bottom, the TD direction to the left and right, and the measurement film was set in the following device so that the angle between the X-ray source direction and the film surface was perpendicular. For the TD direction measurement, the TD direction was set to the top and bottom, and the MD direction to the left and right, and small-angle X-ray scattering (SAXS) measurement was performed with the following device and conditions. Device: RIGAKU Corporation, product name: Ultima IV (small-angle scattering attachment system) X-ray incident direction: normal to the film X-ray wavelength: 0.15418 nm Optical unit specifications: 1. Optical system selection slit: 0.03 mm for small-angle scattering (= 1st slit) 2. DS: anti-scattering slit 1.00 mm (= 2nd slit) 3. 1. 1st to 2nd slit distance: 70 mm 2. 2nd to sample distance: 98 mm 3. Vacuum path length: 100 mm (installed on a dedicated stand in front of the receiving slit box) 4. RS, SS: scattering slit 0.20 mm, receiving slit 0.10 mm 5. Camera length: 285 mm 6. Receiving side Soller slit: 5° using a flexible optical system 7. Monochromatization: None (monochromatization on the incident side using a multilayer mirror) 8. Camera length: 285 mm 9. Receiving side Soller slit: 5° using a flexible optical system 10. Monochromatization: None (monochromatization on the incident side using a multilayer mirror) 11. Detector: RIGAKU scintillation detector (HV: 762V) (one-dimensional) X-ray irradiation conditions: A. Scan axis: 2 theta B. Measurement method: continuous C. Scan start angle: 0.1° D. Scan end angle: 1.0° E. Sampling width: 0.02° F. Scan speed: 0.5° / min G. Voltage / current: 40 kV-40 mA H. Number of sample stacks: To obtain sufficient scattering intensity, the samples were stacked to a distance of approximately 0.5 mm with the sample orientation aligned. The X-ray scattering pattern obtained under the above measurement conditions was subjected to detector background correction and air scattering correction to obtain a SAXS profile I(q). The Bragg angle θ was calculated from the magnitude of the scattering vector of the peak derived from the crystal long period in the SAXS profile using the following formula (1), and this was substituted into the following Bragg formula (2) to calculate the crystal long period (d).q = 4π sin θ / λ (1) θ: Bragg angle q: magnitude of scattering vector λ: X-ray wavelength 2d sin θ = λ (2) d: crystalline long period θ: Bragg angle λ: X-ray wavelength Also, referring to the structural analysis of crystalline polymer materials by scattering method in Nichias Technical Times (2014) No. 2, No. 365, the electron density correlation function γ (r) was calculated by Fourier transforming the scattering intensity profile I (q) using the following equation (3). γ (r) has special properties that can be directly used for structural characterization, and the amorphous thickness (da) of the biaxially stretched polypropylene film obtained as structural information was calculated. Furthermore, r indicates distance (nm).

[0108] The crystalline thickness (dc) was calculated by subtracting the amorphous thickness (da) from the crystalline long period (d).

[0109] (8) Differential Scanning Calorimetry of Biaxially Stretched Polypropylene Film A test piece of approximately 5.0 mg was cut out from the biaxially stretched polypropylene film. Next, a first differential scanning calorimetry (1st Run) was performed on the sample using a differential scanning calorimeter (product name: Q200DSC, manufactured by TA Instruments) under a nitrogen gas flow. The first run consisted of a temperature increase from -50°C to 250°C at a temperature increase rate of 5°C / min and a temperature decrease from 250°C to -50°C at a temperature decrease rate of 5°C / min. From the resulting DSC curve, the main melting point (°C), the heat of fusion ΔH (J / g) of the entire film, and the heat of fusion ΔH (J / g) below 165°C were determined. Here, the peak temperature of the maximum melting peak in the DSC curve was taken as the main melting point. The heat of fusion ΔH (J / g) of the entire film was calculated from the area of ​​the melting peak on the DSC curve in accordance with JIS K 7122:1987 (with the exception that the heating rate was 5°C / min). When multiple melting peaks appear on the DSC curve, the total area of ​​the multiple melting peaks was used as the heat of fusion (ΔH) of the entire film. The heat of fusion ΔH (J / g) at 165°C or less is the heat of fusion in the range of 165°C or less out of the heat of fusion ΔH (J / g) of the entire film.

[0110] Next, the crystalline ratio (%) below 165 ° C, crystallinity (%), amorphous amount (%), and crystalline amount below 165 ° C were each calculated from the following formula. The heat of fusion of fully crystalline polypropylene used in the calculation was 209 J / g as described in Macro Molecular Chemie, Rapid Communication, Vol. 9, item 75 (1988). Crystallinity ratio below 165 ° C (%) = 100 × heat of fusion ΔH (J / g) below 165 ° C / heat of fusion ΔH (J / g) of the entire film Crystallinity (%) = 100 × heat of fusion ΔH (J / g) of the entire film / fully crystalline heat of fusion of polypropylene (209 J / g) Amorphous amount (%) = 100 - crystallinity (%) Crystallinity amount below 165 ° C (%) = crystallinity (%) × crystalline ratio below 165 ° C (%) / 100

[0111] (9) Water Vapor Permeability The biaxially oriented polypropylene film was folded back so that the surface resin layer 1 was on the inner side, and the two sides were heat-sealed to form a bag. Calcium chloride was then placed inside the bag. The other side was then heat-sealed to form a bag with a surface area of ​​0.01 m. 2 The resulting bags were then stored at 40°C and 90% RH for 72 hours. The mass of calcium chloride was measured before and after storage, and the difference between the masses was used to determine the water vapor permeability (g / (m 2 ・24h)) were calculated respectively.

[0112] (10) Thermal expansion coefficient and thermal shrinkage coefficient of biaxially stretched polypropylene film at 120°C The thermal expansion coefficient and thermal shrinkage coefficient of biaxially stretched polypropylene film at 120°C were measured in accordance with JIS C2151:2019. First, a 10 cm x 10 cm test piece was cut out from the biaxially stretched polypropylene film. Then, the test piece was heat-treated at 120°C for 15 minutes. At this time, the test piece was heated by hanging it without applying force in a hot air circulation type thermostatic oven (manufactured by ADVANTEC, product name: DRM620DE). Next, after cooling the test piece to room temperature, the length of the test piece was measured. Next, the length in the TD direction of the test piece after heat treatment was measured. 1 [cm], and the thermal expansion coefficient in the TD direction [%] is 100 × (TD 1The length of the test piece in the MD direction after the heat treatment was calculated as follows: MD 1 [cm], and the heat shrinkage rate [%] in the MD direction is calculated as 100 × (10 - MD 1 The above measurement was carried out three times, and the average values ​​of the obtained measurements were used as the thermal expansion coefficient and thermal shrinkage coefficient of the biaxially stretched polypropylene film at 120°C, respectively.

[0113] (11) Heat shrinkage of biaxially stretched polypropylene film at 150°C The heat shrinkage of biaxially stretched polypropylene film at 150°C was measured in accordance with JIS C2151:2019. First, a 10 cm x 10 cm test piece was cut out from the biaxially stretched polypropylene film. Then, the test piece was heat-treated at 150°C for 15 minutes. At this time, the test piece was heated in a hot air circulation type thermostatic chamber (manufactured by ADVANTEC, product name: DRM620DE) while hanging without applying force. Next, after cooling the test piece to room temperature, the length of the test piece was measured. Next, the length in the TD direction of the test piece after heat treatment was measured. 1 The length of the test piece in the MD direction after heat treatment is defined as MD [cm]. 1 When [cm], X TD [%] is 100 × (10-TD 1 ) / 10, and X MD [%] is 100 x (10-MD 1 The above measurement was carried out three times, and the average value of the obtained measurements was used as the heat shrinkage rate of the biaxially stretched polypropylene film at 150°C.

[0114] (12) Haze The haze of the biaxially stretched polypropylene film was measured in accordance with JIS K7136:2000 using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., NDH5000).

[0115] (13) Heat-sealing strength at 170°C or 200°C Two biaxially oriented polypropylene films cut to a width of 15 mm were heat-sealed together at the surface resin layer 1 (heat-sealing layer) under conditions of 170°C or 200°C, a pressure of 2.0 kgf, and a sealing time of 1.0 second to obtain laminated films. The two biaxially oriented polypropylene films were then peeled off under conditions of 15 mm width, 90-degree peeling, a peeling rate of 300 mm / min, and tension in the TD direction, and the peel strength at this time was taken as the heat-sealing strength at 170°C or 200°C, respectively.

[0116] (14) Bag-forming properties (presence or absence of wrinkles upon heat sealing at 180°C) Two biaxially oriented polypropylene films cut to a width of 15 mm were heat-sealed together at the surface resin layer 1 (heat-resistant adhesive layer) under conditions of 180°C, a pressure of 2.0 kgf, and a sealing time of 1.0 second to obtain a laminated film. The presence or absence of heat wrinkles at the sealed portion was then visually observed.

[0117] (15) Thermal Dimensional Stability The thermal dimensional stability of the biaxially stretched polypropylene film was evaluated according to the following criteria: AA (very good): Heat shrinkage rate (X) at 150°C MD +X TD ) is less than 5.0% A (good): Heat shrinkage rate at 150 ° C (X MD +X TD ) is 5.0% or more and less than 6.0% B (bad): Heat shrinkage rate (X MD +X TD ) is 6.0% or more and less than 7.0% C (very bad): Heat shrinkage rate (X MD +X TD ) is 7.0% or more

[0118] [Examples 1 to 6 and Comparative Example 1] Polypropylene films were extruded with the compositions shown in Table 1, and then biaxially stretched to produce biaxially stretched polypropylene films, which were then evaluated. The extrusion conditions and biaxial stretching conditions were as follows. Corona treatment was also performed on the surface of the surface resin layer 2 side shown in Table 1. Extruder: 60 mmφ multilayer T-die extruder (screw: L / D = 27, manufactured by Screw Seiki Co., Ltd.) Extrusion setting temperature: 230 to 250°C, Processing speed: 20 m / min (take-up speed) MD stretching temperature [°C]: shown in Table 1 MD stretch ratio [times]: shown in Table 1 TD stretching temperature [°C]: shown in Table 1 TD stretch ratio [times]: shown in Table 1 Relaxation rate [%]: shown in Table 1 Here, the relaxation rate refers to the maximum stretch ratio width in the device settings divided by the tenter exit width. In addition, the notation "A / B / C" for the stretching temperature in Table 1 means "preheating temperature (temperature at which the raw film is heated before stretching) / stretching temperature (temperature at which stretching is performed) / heat setting temperature (temperature at which heat setting (annealing) is performed after stretching)."

[0119]

[0120] The biaxially oriented polypropylene films of the Examples had improved thermal dimensional stability compared to the biaxially oriented polypropylene films of the Comparative Examples.

[0121] This application claims priority based on Japanese Patent Application Nos. 2022-155360, 2022-155356, 2022-155359, 2022-155365, and 2022-155368, all filed on September 28, 2022, the disclosures of which are incorporated herein in their entireties.

[0122] The present invention can also take the following aspects.

[0123] [1a] A biaxially oriented polypropylene film comprising a biaxially oriented film layer containing a propylene-based polymer, the biaxially oriented polypropylene film having a crystalline fraction of 38% or more at temperatures below 165°C as determined by differential scanning calorimetry. [2a] The biaxially oriented polypropylene film according to [1a], wherein the biaxially oriented polypropylene film has a main melting point of 165°C or more and 180°C or less as determined by differential scanning calorimetry. [3a] The biaxially oriented polypropylene film according to [1a] or [2a], wherein the biaxially oriented polypropylene film has a heat of fusion (ΔH) of 110 J / g or more and 150 J / g or less as determined by differential scanning calorimetry. [4a] The biaxially oriented polypropylene film according to any one of [1a] to [3a], wherein the biaxially oriented polypropylene film has a heat of fusion (ΔH) of 40 J / g or more at temperatures below 165°C as determined by differential scanning calorimetry. [5a] The biaxially oriented polypropylene film according to any one of [1a] to [4a], wherein the biaxially oriented polypropylene film has a crystallinity of 20% or more at temperatures below 165°C as determined by differential scanning calorimetry. [6a] The biaxially oriented polypropylene film according to any one of [1a] to [5a], wherein the amount of structural units derived from α-olefins other than propylene contained in the biaxially oriented polypropylene film is 0.05 mol% or more, when the total amount of structural units derived from monomers contained in the biaxially oriented polypropylene film is taken as 100 mol%. [7a] The biaxially oriented polypropylene film according to any one of [1a] to [6a], further comprising a surface resin layer on at least one side of the biaxially oriented film layer. [8a] The biaxially oriented polypropylene film according to [7a], wherein the surface resin layer contains homopolypropylene (A). [9a] The biaxially oriented polypropylene film according to [8a], wherein the content of the homopolypropylene (A) in the surface resin layer is 75% by mass or more and 100% by mass or less, when the entire surface resin layer is taken as 100% by mass. [10a] The biaxially oriented polypropylene film according to any one of [7a] to [9a], wherein the thickness of the surface resin layer is 0.1 μm or more and 10.0 μm or less.[11a] The biaxially oriented polypropylene film according to any one of [1a] to [10a], wherein the thickness of the biaxially oriented film layer is 5 μm or more and 100 μm or less. [12a] The tensile modulus T of the biaxially oriented polypropylene film in the machine direction is measured in accordance with JIS K7127 (1999) using a tensile tester under conditions of a measurement temperature of 23±2°C, 50±5% RH, and a pulling rate of 5 mm / min. 1 and the tensile modulus in the TD direction T 2 The sum of (T 1 +T 2 [13a] The biaxially oriented polypropylene film according to any one of [1a] to [12a], wherein the compressive strength (TS) of the biaxially oriented polypropylene film is 3,000 MPa or more and 10,000 MPa or less. [13a] The biaxially oriented polypropylene film according to any one of [1a] to [12a], wherein the biaxially oriented polypropylene film expands in the TD direction when heat-treated at 120°C for 15 minutes in accordance with JIS C2151:2019. [14a] The biaxially oriented polypropylene film according to any one of [1a] to [13a], wherein the biaxially oriented polypropylene film is a food packaging film. [15a] A food package using the biaxially oriented polypropylene film according to any one of [1a] to [14a]. [16a] A food package comprising the food package according to [15a], and a food in the food package.

[0124] The present invention can also take the following aspects.

[0125] [1b] A biaxially oriented polypropylene film comprising a biaxially oriented film layer containing a propylene-based polymer, which expands in the TD direction and shrinks in the MD direction when heat-treated at 120°C for 15 minutes in accordance with JIS C2151: 2019. [2b] The biaxially oriented polypropylene film according to [1b], which has a thermal expansion coefficient in the TD direction of 0.1% or more and 2.0% or less when heat-treated at 120°C for 15 minutes in accordance with JIS C2151: 2019. [3b] The biaxially oriented polypropylene film according to [1b] or [2b], which has a heat shrinkage coefficient in the MD direction of 5.0% or less when heat-treated at 120°C for 15 minutes in accordance with JIS C2151: 2019. [4b] The biaxially oriented polypropylene film according to any one of [1b] to [3b], which has a heat shrinkage rate in the TD direction of 8.5% or less when heat-treated at 150°C for 15 minutes in accordance with JIS C2151: 2019. [5b] The biaxially oriented polypropylene film according to any one of [1b] to [4b], which has a heat shrinkage rate in the MD direction of 8.0% or less when heat-treated at 150°C for 15 minutes in accordance with JIS C2151: 2019. [6b] The heat shrinkage rate in the TD direction and the heat shrinkage rate in the MD direction are each X, Y, Z, and Z according to JIS C2151: 2019. TD [%] and X MD When [%] is used, X TD +X MD[7b] The biaxially oriented polypropylene film according to any one of [1b] to [5b], wherein the amount of structural units derived from α-olefins other than propylene contained in the biaxially oriented polypropylene film is 0.05 mol% or more, when the total amount of structural units derived from monomers contained in the biaxially oriented polypropylene film is taken as 100 mol%. [8b] The biaxially oriented polypropylene film according to any one of [1b] to [7b], further comprising a surface resin layer on at least one side of the biaxially oriented film layer. [9b] ​​The biaxially oriented polypropylene film according to [8b], wherein the surface resin layer contains homopolypropylene (A). [10b] The biaxially oriented polypropylene film according to [9b], wherein the content of the homopolypropylene (A) in the surface resin layer is 75% by mass or more and 100% by mass or less, when the entire surface resin layer is taken as 100% by mass. [11b] The biaxially oriented polypropylene film according to any one of [8b] to [10b], wherein the thickness of the surface resin layer is 0.1 μm or more and 10.0 μm or less. [12b] The biaxially oriented polypropylene film according to any one of [1b] to [11b], wherein the thickness of the biaxially oriented film layer is 5 μm or more and 100 μm or less. [13b] The tensile modulus T of the biaxially oriented polypropylene film in the MD direction measured using a tensile tester in accordance with JIS K7127 (1999) under conditions of a measurement temperature of 23±2°C, 50±5% RH, and a pulling speed of 5 mm / min. 1 and the tensile modulus in the TD direction T 2 The sum of (T 1 +T 2 [14b] The biaxially oriented polypropylene film according to any one of [1b] to [13b] above, which is a food packaging film. [15b] A food package using the biaxially oriented polypropylene film according to any one of [1b] to [14b] above. [16b] A food package comprising the food package according to [15b] above and a food product contained in the food package.

[0126] The present invention can also take the following aspects.

[0127] [1c] A biaxially oriented polypropylene film comprising a biaxially oriented film layer containing a propylene-based polymer, wherein the biaxially oriented polypropylene film has a heat-seal strength of 4.0 N / 15 mm or less when heat-sealed to itself at 200°C. [2c] The biaxially oriented polypropylene film according to [1c], wherein the heat-seal strength of 1.0 N / 15 mm or less when heat-sealed to itself at 170°C. [3c] The biaxially oriented polypropylene film according to [1c] or [2c], wherein the amount of structural units derived from α-olefins other than propylene contained in the biaxially oriented polypropylene film is 0.05 mol% or more when the total amount of structural units derived from monomers contained in the biaxially oriented polypropylene film is taken as 100 mol%. [4c] The biaxially oriented polypropylene film according to any one of [1c] to [3c], further comprising a surface resin layer on at least one side of the biaxially oriented film layer. [5c] The biaxially oriented polypropylene film according to [4c], wherein the surface resin layer contains homopolypropylene (A). [6c] The biaxially oriented polypropylene film according to [5c], wherein the content of homopolypropylene (A) in the surface resin layer is 75% by mass or more and 100% by mass or less, when the entire surface resin layer is taken as 100% by mass. [7c] The biaxially oriented polypropylene film according to any of [4c] to [6c], wherein the thickness of the surface resin layer is 0.1 μm or more and 10.0 μm or less. [8c] The biaxially oriented polypropylene film according to any of [1c] to [7c], wherein the thickness of the biaxially oriented film layer is 5 μm or more and 100 μm or less. [9c] The tensile modulus T of the biaxially oriented polypropylene film in the MD direction, measured using a tensile tester in accordance with JIS K7127 (1999) under conditions of a measurement temperature of 23±2°C, 50±5% RH, and a tensile speed of 5 mm / min. 1 and the tensile modulus in the TD direction T 2 The sum of (T 1 +T 2[10c] The biaxially oriented polypropylene film according to any one of [1c] to [8c] above, wherein the compressive strength (S) of the biaxially oriented polypropylene film is 3,000 MPa or more and 10,000 MPa or less. [10c] The biaxially oriented polypropylene film according to any one of [1c] to [9c] above, which is a food packaging film. [11c] A food package using the biaxially oriented polypropylene film according to any one of [1c] to [10c] above. [12c] A food package comprising the food package according to [11c] above and a food product contained in the food package.

[0128] The present invention can also take the following aspects.

[0129] [1d] A biaxially oriented polypropylene film comprising a biaxially oriented film layer containing homopolypropylene (A) and at least one polymer (B) selected from the group consisting of random polypropylene (B1) and α-olefin copolymer (B2), wherein the MFR of the polymer (B) is 0.01 g / 10 min or more and 30 g / 10 min or less, as measured in accordance with ASTM D1238 at 230°C under a load of 2.16 kg. [2d] The biaxially oriented polypropylene film according to [1d], wherein the amount of structural units derived from α-olefins other than propylene contained in the biaxially oriented polypropylene film is 0.05 mol% or more, relative to the total amount of structural units derived from monomers contained in the biaxially oriented polypropylene film, taken as 100 mol%. [3d] The biaxially oriented polypropylene film according to [1d] or [2d], wherein the isotactic mesopentad fraction (mmmm) of the homopolypropylene (A) is 96.0% or more. [4d] The biaxially oriented polypropylene film according to any one of [1d] to [3d] above, wherein the content of the polymer (B) is 1% by mass or more and 50% by mass or less, when the total mass of the biaxially oriented film layer is 100% by mass. [5d] The biaxially oriented polypropylene film according to any one of [1d] to [4d] above, wherein the melting point of the polymer (B) is 50°C or more and 155°C or less. [6d] The biaxially oriented polypropylene film according to any one of [1d] to [5d] above, wherein the weight average molecular weight (Mw) of the polymer (B) is 100,000 or more and 1,000,000 or less. [7d] The biaxially oriented polypropylene film according to any one of [1d] to [6d] above, wherein the weight average molecular weight (Mw) / number average molecular weight (Mn) of the polymer (B) is 1.5 or more and 8.0 or less. [8d] The biaxially oriented polypropylene film according to any one of [1d] to [7d] above, wherein the α-olefin copolymer (B2) comprises a random copolymer of propylene with one or more α-olefins selected from the group consisting of ethylene and α-olefins having a carbon number of 4 or more and 10 or less. [9d] The biaxially oriented polypropylene film according to any one of [1d] to [8d] above, further comprising a surface resin layer on at least one side of the biaxially oriented film layer.[10d] The biaxially oriented polypropylene film according to [9d], wherein the surface resin layer contains homopolypropylene (A). [11d] The biaxially oriented polypropylene film according to [10d], wherein the content of homopolypropylene (A) in the surface resin layer is 75% by mass or more and 100% by mass or less, when the entire surface resin layer is taken as 100% by mass. [12d] The biaxially oriented polypropylene film according to any of [9d] to [11d], wherein the thickness of the surface resin layer is 0.1 μm or more and 10.0 μm or less. [13d] The biaxially oriented polypropylene film according to any of [1d] to [12d], wherein the thickness of the biaxially oriented film layer is 5 μm or more and 100 μm or less. [14d] The tensile modulus T of the biaxially oriented polypropylene film in the machine direction, measured in accordance with JIS K7127 (1999) using a tensile tester under conditions of a measurement temperature of 23±2°C, 50±5% RH, and a pulling speed of 5 mm / min. 1 and the tensile modulus in the TD direction T 2 The sum of (T 1 +T 2 [15d] The biaxially oriented polypropylene film according to any one of [1d] to [14d], wherein the compressive strength (TS) of the biaxially oriented polypropylene film is 3,000 MPa or more and 10,000 MPa or less. [15d] The biaxially oriented polypropylene film according to any one of [1d] to [14d], wherein the biaxially oriented polypropylene film expands in the TD direction when heat-treated at 120°C for 15 minutes in accordance with JIS C2151:2019. [16d] The biaxially oriented polypropylene film according to any one of [1d] to [15d], which is a food packaging film. [17d] A food package using the biaxially oriented polypropylene film according to any one of [1d] to [16d]. [18d] A food package comprising the food package according to [17d] and a food in the food package.

[0130] 100 Biaxially oriented polypropylene film 101 Biaxially oriented film layer 103 Surface resin layer

Claims

1. A biaxially oriented polypropylene film having a biaxially oriented film layer containing a propylene-based polymer, wherein the crystalline long period in the TD direction determined by small-angle X-ray scattering (SAXS) measurement is 28.0 nm or less.

2. The biaxially oriented polypropylene film according to claim 1, wherein the amorphous thickness in the TD direction determined by SAXS measurement is 15.5 nm or less.

3. A biaxially oriented polypropylene film according to claim 1 or 2, in which the crystal thickness in the TD direction determined by SAXS measurement is 13.5 nm or less.

4. A biaxially oriented polypropylene film according to any one of claims 1 to 3, having a crystalline ratio of 38% or more at 165°C or less as determined by differential scanning calorimetry.

5. A biaxially oriented polypropylene film according to any one of claims 1 to 4, wherein the main melting point of the biaxially oriented polypropylene film determined by differential scanning calorimetry is 165°C or higher and 180°C or lower.

6. The biaxially oriented polypropylene film according to any one of claims 1 to 5, wherein the heat of fusion (ΔH) of the entire biaxially oriented polypropylene film, as determined by differential scanning calorimetry, is 100 J / g or more and 150 J / g or less.

7. The biaxially oriented polypropylene film according to any one of claims 1 to 6, wherein the heat of fusion (ΔH) of the biaxially oriented polypropylene film at 165°C or less, as determined by differential scanning calorimetry, is 40 J / g or more.

8. A biaxially oriented polypropylene film according to any one of claims 1 to 7, wherein the biaxially oriented polypropylene film has a crystal content of 20% or more at 165°C or less.

9. A biaxially oriented polypropylene film according to any one of claims 1 to 8, wherein the amount of structural units derived from α-olefins other than propylene contained in the biaxially oriented polypropylene film is 0.05 mol % or more, when the total amount of structural units derived from monomers contained in the biaxially oriented polypropylene film is 100 mol %.

10. A biaxially oriented polypropylene film according to any one of claims 1 to 9, which expands in the TD direction when heat-treated at 120°C for 15 minutes in accordance with JIS C2151:2019.

11. The biaxially oriented polypropylene film according to any one of claims 1 to 10, which expands in the TD direction and shrinks in the MD direction when heat-treated at 120°C for 15 minutes in accordance with JIS C2151:2019.

12. A biaxially oriented polypropylene film according to any one of claims 1 to 11, having a thermal expansion coefficient in the TD direction of 0.1% or more and 2.0% or less when heat-treated at 120°C for 15 minutes in accordance with JIS C2151:2019.

13. A biaxially oriented polypropylene film according to any one of claims 1 to 12, which has a heat shrinkage rate in the machine direction of 5.0% or less when heat-treated at 120°C for 15 minutes in accordance with JIS C2151:2019.

14. A biaxially oriented polypropylene film according to any one of claims 1 to 13, which has a thermal shrinkage rate in the TD direction of 8.5% or less when heat-treated at 150°C for 15 minutes in accordance with JIS C2151:2019.

15. A biaxially oriented polypropylene film according to any one of claims 1 to 14, which has a heat shrinkage rate in the machine direction of 8.0% or less when heat-treated at 150°C for 15 minutes in accordance with JIS C2151:2019.

16. In accordance with JIS C2151:2019, the thermal shrinkage in the TD direction and the thermal shrinkage in the MD direction when heated at 150°C for 15 minutes are measured as X TD [%] and X MD When [%] is used, X TD +X MD The biaxially oriented polypropylene film according to any one of claims 1 to 15, wherein the elongation is less than 6.0%.

17. A biaxially oriented polypropylene film according to any one of claims 1 to 16, wherein the heat fusion strength when the biaxially oriented polypropylene film is heat-sealed to itself at 200°C is 4.0 N / 15 mm or less.

18. A biaxially oriented polypropylene film according to any one of claims 1 to 17, wherein the heat fusion strength when the biaxially oriented polypropylene film is heat-sealed to itself at 170°C is 1.0 N / 15 mm or less.

19. A biaxially oriented polypropylene film according to any one of claims 1 to 18, wherein the propylene polymer comprises homopolypropylene (A) and at least one polymer (B) selected from the group consisting of random polypropylene (B1) and α-olefin copolymer (B2), and the MFR of the polymer (B) measured in accordance with ASTM D1238 at 230°C under a load of 2.16 kg is 0.01 g / 10 min or more and 30 g / 10 min or less.

20. The biaxially oriented polypropylene film according to claim 19, wherein the isotactic mesopentad fraction (mmmm) of the homopolypropylene (A) is 96.0% or more.

21. A biaxially oriented polypropylene film according to claim 19 or 20, wherein the content of the polymer (B) is 1% by mass or more and 50% by mass or less, when the entire biaxially oriented film layer is taken as 100% by mass.

22. A biaxially oriented polypropylene film according to any one of claims 19 to 21, wherein the melting point of the polymer (B) is 50°C or higher and 155°C or lower.

23. A biaxially oriented polypropylene film according to any one of claims 19 to 22, wherein the weight average molecular weight (Mw) of the polymer (B) is 100,000 or more and 1,000,000 or less.

24. A biaxially oriented polypropylene film according to any one of claims 19 to 23, wherein the weight average molecular weight (Mw) / number average molecular weight (Mn) of the polymer (B) is 1.5 or more and 8.0 or less.

25. A biaxially oriented polypropylene film according to any one of claims 19 to 24, wherein the α-olefin copolymer (B2) comprises a random copolymer of propylene with one or more α-olefins selected from the group consisting of ethylene and α-olefins having from 4 to 10 carbon atoms.

26. A biaxially oriented polypropylene film according to any one of claims 1 to 25, further comprising a surface resin layer on at least one side of the biaxially oriented film layer.

27. The biaxially oriented polypropylene film according to claim 26, wherein the surface resin layer comprises homopolypropylene (A).

28. A biaxially oriented polypropylene film as described in claim 27, wherein the content of the homopolypropylene (A) in the surface resin layer is 75% by mass or more and 100% by mass or less, when the entire surface resin layer is taken as 100% by mass.

29. A biaxially oriented polypropylene film according to any one of claims 26 to 28, wherein the thickness of the surface resin layer is 0.1 μm or more and 10.0 μm or less.

30. A biaxially oriented polypropylene film according to any one of claims 1 to 29, wherein the thickness of the biaxially oriented film layer is 5 μm or more and 100 μm or less.

31. The tensile modulus T of the biaxially oriented polypropylene film in the machine direction is measured using a tensile tester in accordance with JIS K7127 (1999) under the conditions of a measurement temperature of 23±2°C, 50±5% RH, and a tensile speed of 5 mm / min. 1 and the tensile modulus in the TD direction T 2 The sum of (T 1 +T 2 31. The biaxially oriented polypropylene film according to any one of claims 1 to 30, wherein the elongation stress (E) is 3000 MPa or more and 10000 MPa or less.

32. The biaxially oriented polypropylene film according to any one of claims 1 to 31, which is a food packaging film.

33. A food packaging product using the biaxially oriented polypropylene film according to any one of claims 1 to 32.

34. A food package comprising the food package of claim 33 and a food product within the food package.