AI Technical Summary
Existing methods for producing alumina particles result in high surface residual Na concentration and aggregation, leading to poor curing and voltage resistance issues in resin compositions, and contamination risks due to crushing for powdering.
A method involving washing and drying of alumina slurry using a predetermined method to directly dry and powderize without crushing, achieving spherical alumina particles with low surface residual Na and minimal aggregation, and incorporating these particles into a resin composite composition.
The method produces alumina particles with low surface residual Na and reduced aggregation, preventing poor curing and contamination, and enabling efficient use as fillers in semiconductor packages without the need for crushing, ensuring improved fluidity and moldability.
Smart Images

Figure PI2025001927_DRAWING_001
Abstract
Description
Spherical alumina particles, their production method, and resin composite composition containing them
[0001] The present invention relates to spherical alumina particles, particularly spherical alumina particles having a reduced surface residual Na concentration and a low degree of aggregation, a method for producing the same, and a resin composite composition containing the same.
[0002] In recent years, the increasing functionality and speed of electronic devices such as mobile phones has led to an increase in the amount of heat generated by the electronic components inside the devices. To ensure the normal operation of electronic devices, efficiently dissipating the generated heat to the outside has become an important issue. Thermally conductive sheets and thermally conductive adhesives are widely used for heat dissipation. These are attached or applied between the heat-generating element and the heat-dissipating fin and then pressed together to eliminate the gap between the heat-generating element and the heat-dissipating fin, allowing for efficient heat dissipation. Furthermore, the semiconductors inside electronic components also generate significant amounts of heat due to their similarly high functionality and high speed, and the encapsulating materials that protect the semiconductors are also required to have heat dissipation properties.
[0003] Generally, heat dissipation sheets, heat dissipation adhesives, and semiconductor encapsulants are composed of thermally conductive inorganic fillers and resins. Thermally conductive inorganic fillers are made from inexpensive aluminum hydroxide and aluminum oxide (hereafter referred to as alumina), as well as materials such as silicon carbide, boron nitride, and aluminum nitride, which are expected to have high thermal conductivity. Alumina, in particular, is often used as a thermally conductive inorganic filler because it is inexpensive and chemically stable.
[0004] JP 2012-21710 A JP 2008-120673 A
[0005] The Bayer process is a widely known method for producing alumina. In the Bayer process, bauxite is treated with caustic soda (sodium hydroxide) to dissolve aluminum as sodium aluminate, and impurities such as iron, titanium, and silicon are precipitated as red mud. This is then filtered, and the filtrate (sodium aluminate solution) is mixed with hydrous alumina Al. 2 O 3 ・3H 2By adding 0 seeds and stirring for several days, hydrous alumina is precipitated in the liquid and recovered. The recovered hydrous alumina is calcined to obtain high-purity alumina Al 2 O 3 can be obtained.
[0006] The Bayer process involves treatment with caustic soda (sodium hydroxide), so sodium may remain in the finished alumina. If a large amount of sodium is present on the filler surface, it reacts with the resin or moisture in the air, releasing hydroxide ions. These hydroxide ions react with the epoxy groups present in the epoxy resin, inhibiting the polymerization reaction between the resins and causing poor curing. Furthermore, if sodium or potassium ions are present in the resin composition created by kneading with epoxy groups, the voltage resistance will be impaired. For these reasons, it is desirable to have a low amount of sodium. To remove or reduce this sodium, the alumina is washed with water and then dried.
[0007] Patent Document 1 discloses an apparatus that can efficiently perform washing, filtration, and drying of powder such as alumina in the same container. More specifically, it proposes that by introducing compressed gas into the container, washing, filtration, and drying of the powder can be performed in the same container without the need for a stirring blade inside the container. It also discloses the use of heating by electricity or steam, or microwave irradiation to improve the drying speed.
[0008] Thus, when drying the washed alumina slurry, it is often heated. However, prolonged heating during the heat drying process can cause sodium ions remaining inside the alumina to migrate outward and potentially dissolve onto the surface of the alumina that has been cleaned by washing. Furthermore, the smaller the particle size of the alumina particles contained in the slurry, the more likely they are to aggregate with each other when heated and dried, resulting in the dried product becoming a strong agglomerate. These agglomerates require crushing for powderization. Crushing can result in contamination of the alumina powder product with foreign matter from the crusher.
[0009] Furthermore, Patent Document 2 discloses a fine spherical aluminum oxide powder using fine low-soda aluminum oxide as a raw material, with a maximum particle size of 7 μm or less and an average particle size in the range of 0.2 to 0.9 μm. This powder is disclosed as being produced by subjecting the raw material powder to a strong crushing treatment before introducing it into a flame, and then continuously introducing the powder into the flame immediately after sufficient crushing and dispersion of agglomerated particles, thereby stably producing a spherical inorganic oxide powder free of coarse particles and with an average particle size of less than 1 μm. However, as in Patent Document 1, there is a risk of foreign matter from the crusher being mixed into the finished alumina powder during crushing. The concentration of the sodium component in this powder is not disclosed.
[0010] The present invention has been made in view of the above circumstances, and its object is to provide spherical alumina particles having a low surface residual Na concentration and a low degree of aggregation, a method for producing the same, and a resin composite composition containing the same.
[0011] The present inventors have found that by drying an alumina slurry that has been washed with water by a predetermined method, the slurry can be directly dried and powdered without the need for crushing.
[0012] Based on the above findings, the gist of the present invention is as follows: [1] An average particle size of 0.4 to 1.9 μm and a specific surface area of 1.0 to 5.0 m 2 / g, surface residual Na is 20 ppm or less, contained Na 2 [2] Spherical alumina particles according to [1], characterized in that the degree of gelatinization is 10.0% or less.
[0013] [3] A method for producing spherical alumina particles, comprising: a water slurry preparation step of mixing raw material spherical alumina with water to prepare a water slurry containing the raw material spherical alumina; and a drying step of drying the water slurry. [4] A method for producing spherical alumina particles according to [3], comprising: a raw material spherical alumina washing step of washing the raw material spherical alumina with water before the water slurry preparation step.
[0014] [5] A resin composite composition comprising the spherical alumina particles according to [1] or [2]. [6] The resin composite composition according to [5], further comprising at least one inorganic filler selected from the group consisting of amorphous spherical silica particles, crystalline spherical silica particles, titania particles, magnesia particles, aluminum nitride particles, boron nitride particles, barium titanate particles, calcium titanate particles, and carbon fibers.
[0015] The present invention provides spherical alumina particles with a low surface residual Na concentration and a low degree of aggregation, and a resin composite composition containing the same. Because the spherical alumina particles have a low surface residual Na concentration, when used as a filler, poor curing and loss of voltage resistance can be avoided. Furthermore, because the degree of aggregation is low, crushing is not required, and contamination due to crushing can be avoided. Furthermore, the spherical alumina particles can be easily produced by a manufacturing method that is one aspect of the present invention.
[0016] FIG. 1 is a diagram showing the state of alumina particles in the case of conventional heat drying and in the case of freeze drying according to the present embodiment.
[0017] [Spherical alumina particles]
[0018] (Average particle size) The spherical alumina particles according to one embodiment of the present invention have an average particle size of 0.4 to 1.9 μm. An average particle size of less than 0.4 μm is undesirable because the particles tend to aggregate more, significantly reducing the fluidity of the resin composition when used as a filler. An average particle size of more than 1.9 μm can cause the particles to get caught in the narrow spaces between the mounting substrate and the chip in semiconductor packages, which are becoming increasingly smaller and thinner, reducing the fluidity of the liquid encapsulant and reducing moldability.
[0019] Here, the average particle size refers to the average particle size (D50), and means the median diameter D50 at 50% cumulative volume in the volume-based particle size distribution measured by a laser diffraction / scattering particle size distribution measurement method. The laser diffraction / scattering particle size distribution measurement method involves irradiating a dispersion containing spherical alumina particles with laser light and determining the particle size distribution from the intensity distribution pattern of the diffracted / scattered light emitted from the dispersion. In the present invention, a laser diffraction / scattering particle size distribution measurement device "Mastersizer 3000" (manufactured by Malvern) is used. The average particle size of the raw material for spherical alumina particles can also be determined in a similar manner.
[0020] (Specific Surface Area) In one embodiment of the present invention, the spherical alumina particles have a specific surface area of 1.0 m2 measured by the BET method. 2 / g or more 5.0m 2 / g or less.
[0021] The specific surface area of the spherical particles is 1.0 m 2 If the specific surface area of the spherical particles is less than 5.0 m / g, the particles are unlikely to form a close-packed structure, which may reduce the fluidity of the liquid encapsulant containing the particles. 2 If the particle size exceeds 1 / g, the tendency for aggregation between particles increases, which may also reduce the fluidity of the liquid encapsulant.
[0022] The specific surface area is measured by the BET method. Typically, the specific surface area is measured by the following procedure. Approximately 5 g of a sample is weighed out and vacuum dried at 250°C for 5 minutes. Next, the sample is placed in an automatic specific surface area measuring device (Macsorb, manufactured by Mountec Co., Ltd.), and the nitrogen gas adsorption amount is measured at a relative pressure P / P0 of 0.291 at a measurement temperature of 77 K using pure nitrogen and a nitrogen-helium mixed gas (mixture ratio: nitrogen 30%, He 70%), and the BET specific surface area is calculated by the one-point method.
[0023] (Surface Residual Sodium) In one embodiment of the present invention, the spherical alumina particles have a surface residual sodium content of 20 ppm or less. Surface residual sodium refers to residual sodium adhering to the alumina surface and was measured using ion chromatography. When large amounts of sodium are present on the filler surface, i.e., the alumina surface, they react with the resin or moisture in the air to release hydroxide ions. These hydroxide ions react with epoxy groups present in the epoxy resin, inhibiting the polymerization reaction between the resins and causing poor curing. Furthermore, the presence of sodium or potassium ions in a resin composition prepared by kneading with epoxy groups impairs voltage resistance. A sodium content of 20 ppm or less can avoid poor curing and loss of voltage resistance. From the above perspective, a lower sodium content is preferable, but complete removal is costly, so a sodium content of 0.1 ppm or more is used. Surface residual sodium is measured using ion chromatography. Typically, the measurement is performed using the following procedure. 4 g of sample and 40 ml of distilled water are added to a centrifuge tube, the tube is capped, and the tube is thoroughly shaken to mix. After mixing, the sample and sample solution are separated using a centrifuge. The sample solution was separated and analyzed for sodium ions using an ion chromatograph manufactured by Toa Medical Electronics.
[0024] (Contains Na 2 O) In one embodiment of the present invention, the spherical alumina particles contain Na 2 The content of Na is 1000 ppm or less. 2 O is the total amount of Na present on the surface and inside of alumina, and is measured by atomic absorption spectrometry to determine the amount of Na oxide. 2 It is quantified as O. 2 If a large amount of O is present in alumina, sodium is present not only on the surface of the alumina but also inside the alumina, and when the alumina is heat-treated, the sodium component is liberated on the particle surface, which may increase the residual surface Na content. 2 If the O content is 1000 ppm or less, the sodium content is low and the amount of sodium released onto the particle surface can be reduced. 2The lower the O content, the better, but since it is difficult to completely remove it in terms of production control, the lower limit may be set to 50 ppm or more. 2 The amount of O contained in the alumina particles may be measured by an elemental analysis method known to those skilled in the art, for example, by an atomic absorption spectrophotometer, and converted into oxide.
[0025] (Agglomeration Degree) In one embodiment of the present invention, the spherical alumina particles have an agglomeration degree of 1.0% or less. The agglomeration degree here is an index indicating whether particles are agglomerated, and was measured by a sieving measurement method. When the washed alumina slurry is heated and dried, the particles aggregate together and form large clumps. The agglomeration requires crushing to separate the particles. Crushing results in equipment wear and increased costs due to contact with the crushing device. Furthermore, the agglomeration of particles may result in insufficient dispersion in the resin, which may deteriorate the fluidity and viscosity of the resin composition. Agglomeration degree of 1.0% or less indicates few clumps, which means that crushing is unnecessary. From the above perspective, a lower agglomeration degree is desirable, but since it is difficult to completely prevent agglomeration, the lower limit may be set to 0.0001% or more. The agglomeration degree is measured as follows: Two standard sieves with mesh sizes of 4.75 mm and 212 μm are stacked in order. The sieves were stacked in order, with the 212 μm mesh sieve at the bottom, and the sieves with gradually increasing mesh sizes on top of it. 50 g of sample was placed on the top 4.75 mm mesh sieve and set in a sieve shaker. The sieve shaker used was an Endecotts OCTAGON 200. After the sieves were set, the shaker was set to an amplitude of 5 and a shaking time of 3 minutes. After shaking was completed, the particle weights of the particles remaining on each sieve mesh and the particles that passed through the 212 μm mesh were measured. If the amount of particles on the 4.75 mm mesh is Ag, the amount of particles on the 212 μm mesh is Bg, and the amount of particles that passed through the 212 μm mesh is Cg, then the degree of agglomeration was calculated as A / (B+C)×100(%).
[0026] (Circularity) In one embodiment of the present invention, the spherical alumina particles have a circularity of 0.90 or more. The higher the circularity of the spherical particles, the lower the viscosity of a resin composite composition containing the alumina particles and the more improved the moldability. The circularity may be 0.91 or more, 0.92 or more, or 0.93 or more. Theoretically, the upper limit of the circularity is 1.0, but from the viewpoint of production control, it may be 0.98 or less, or 0.95 or less.
[0027] The circularity can be measured using an electron microscope, an optical microscope, and an image analyzer. For example, Sysmex FPIA. These devices are used to measure the circularity of particles (perimeter of the equivalent circle / perimeter of the projected image of the particle). The circularity of 100 or more particles is measured, and the average value is taken as the circularity of the powder.
[0028] (Pregelatinization Ratio) In one embodiment of the present invention, the spherical alumina particles may have a pregelatinization ratio of 10.0% or less. Here, the pregelatinization ratio refers to the proportion of α-alumina crystals in the crystalline phase. Alumina is known to be crystalline, and typical crystalline forms include α-alumina, θ-alumina, and δ-alumina. The spherical alumina particles according to one embodiment of the present invention can be produced by a thermal spraying method, which involves introducing a raw material into a flame, melting it, and then quenching it, as described in detail below. In this case, the resulting alumina can have a high amorphous ratio, making it easy to obtain spherical alumina particles with a pregelatinization ratio of 10.0% or less. The upper limit of the pregelatinization ratio may be 5.0%, 3.0%, or 1.0%. The lower limit of the pregelatinization ratio is not particularly limited and may be 0.0%, but may be 0.1% or 0.4% from the perspective of reducing the burden of production management and the thermal conductivity characteristics of the resin composite composition.
[0029] The alpha-conversion rate is measured using a powder X-ray diffractometer. The integrated area of the obtained diffraction peaks is determined, and the ratio of the diffraction peak area derived from alpha-alumina to the total area is analyzed by the Rietveld method. Specifically, an X-ray diffraction pattern is obtained using a D2PHASER manufactured by Bruker in the 2θ range of 10° to 90°. The alpha-conversion rate is calculated from the obtained pattern by the Rietveld method using a DIFFRAC.TOPAS manufactured by Bruker. During the calculation, analysis is performed assuming the presence of only three types of crystalline phases: alpha-alumina, delta-alumina, and theta-alumina, and the alpha-alumina content is calculated.
[0030] (Purity) The purity of aluminum oxide in the alumina particles is preferably 99.99% or more and 100.00% or less. If the purity of aluminum oxide is less than 99.99%, the alumina particles tend to have an irregular shape.
[0031] Specific examples of devices that can be used to measure the purity of alumina fine particles include ICP emission spectrometry, which is highly sensitive and capable of quantifying impurity levels, and analytical devices such as AES and SIMS. The amount of impurities in the alumina particles in this example was measured by ICP emission spectrometry and atomic absorption spectrometry. The measurements were performed for each metal oxide according to the following JIS standard measurement methods. 2 O 3 (%): sulfuric acid (1+3) pressure acid decomposition, ICP method (JIS R 1649) SiO 2 (%): Sodium carbonate-boric acid fusion, ICP method (JIS H 1901) Na 2 O (%): sulfuric acid (1+3) pressure acid decomposition, atomic absorption spectrometry (JIS R 1649) The purity of the alumina particles was calculated using the following formula: where the value is rounded to two decimal places.
[0032] Purity of alumina particles [Al 2 O 3 (%)] = 100 (%) - [Fe 2 O 3 (%))]-[SiO 2 (%)]-[Na 2 O (%)]
[0033] [Method for producing spherical alumina particles] One embodiment of the present invention provides a method for producing spherical alumina particles. This method is a method that can suitably produce the alumina particles described above, and includes the following steps: (1) a step for producing raw alumina; (2) a step for spheroidizing the raw alumina to produce raw spherical alumina; (3) a water slurry preparation step for mixing the raw spherical alumina with water to prepare an aqueous slurry containing the raw spherical alumina; and (4) a drying step for drying the aqueous slurry.
[0034] (Raw Alumina) Raw alumina can be produced by a method such as thermal decomposition of ammonium aluminum carbonate, vapor phase oxidation, deflagration, Bayer method, or hydrolysis of aluminum alkoxide.
[0035] (Raw material spherical alumina) Raw material spherical alumina can be obtained by spheroidizing raw material alumina using a flame fusion method. The flame fusion method is a known thermal spraying method in which particles are sprayed into a flame to spheroidize the particles. The average sphericity can be adjusted by adjusting the amount of fuel gas fed into the flame per unit time and the type of fuel gas. The particle size of the spherical alumina powder can also be adjusted by adjusting the particle size of the particles used. The refrigerant is not particularly limited, but from the viewpoint of not reducing the purity of the spherical particles, a gas with few impurities and low activity such as air, nitrogen, or argon is preferable. Alternatively, raw material spherical alumina can be produced by a deflagration method in which a chemical flame is formed by a burner in an oxygen-containing atmosphere, and metallic aluminum powder is fed into the chemical flame in an amount sufficient to form a dust cloud, causing a deflagration to produce spherical alumina particles.
[0036] (Water Slurry) The raw spherical alumina described above is mixed with water to prepare a water slurry containing the raw spherical alumina. From the viewpoint of not reducing the purity of the spherical particles, the water to be mixed is preferably distilled water or ion-exchanged water that does not contain impurities such as sodium ions or chloride ions. The amount of water to be mixed can be appropriately adjusted taking into account the viscosity of the slurry, etc.
[0037] (Washing) Before the water slurry preparation step, a raw material spherical alumina washing step may be carried out in which the raw material spherical alumina is washed with water. As with the slurry water, distilled water or ion-exchanged water that does not contain impurities such as sodium ions or chlorine ions may be used as the washing water. Alternatively, depending on the target to be removed by washing, washing may be carried out using a detergent, surfactant, or the like. By appropriately adjusting the conditions such as the temperature, number of times, and time of washing, the alumina particles can be brought to a desired washed state. Typically, the desired surface residual Na concentration and Na content are determined. 2 O concentration can be obtained. After washing, dehydration can be performed using a filter or the like until the desired particle concentration is reached. By performing dehydration, the Na content and cleaning agent dissolved in the water can be washed away, preventing re-adhesion after drying. Furthermore, water can be added to the raw spherical alumina after washing to dissolve the remaining impurity components in the water. If water is added, dehydration can be performed again to wash away the impurity components adhering to the alumina particle surfaces. In addition to achieving high purity, controlling the particle concentration to the desired level can improve the efficiency of the drying process in the subsequent process.
[0038] (Drying) To extract spherical alumina from an aqueous slurry containing raw spherical alumina, the water is dried and removed. Conventional drying involves heating the slurry for a long period of time while it is left stationary to evaporate the water from the slurry. As heating progresses, the water in the slurry evaporates and decreases, reducing the distance between the alumina particles in the slurry. When the water is completely removed from the slurry, the alumina particles may still be in contact with each other and form strong agglomerates. Furthermore, heating the slurry for a long period of time may cause sodium to migrate from the interior of the spherical alumina particles contained in the slurry to the surface and become liberated on the particle surface. In contrast, in this embodiment, the aqueous slurry containing the raw spherical alumina is dried by airflow heat or freeze-dried.
[0039] (Freeze-drying) In freeze-drying, water is frozen and immobilized, and the alumina particles are also immobilized. During freeze-drying, water gradually leaves the system (slurry) by sublimation, but the alumina particles are fixed, maintaining a certain distance between the alumina particles and suppressing contact and aggregation. In other words, when drying is complete and water is completely removed from the slurry, contact between the alumina particles is minimized, making aggregation less likely. Figure 1 is a schematic diagram showing the state of alumina particles in the case of conventional heat drying and the case of freeze-drying according to this embodiment. Thus, when freeze-drying according to this embodiment is performed, the resulting alumina particles exhibit reduced aggregation, eliminating the need to break down agglomerates of alumina particles. Generally, a mill or other crushing device is used to crush agglomerates, which can introduce foreign matter (contamination) from the crushing device. However, in this embodiment, crushing is not required, so naturally, the introduction of foreign matter (contamination) due to crushing is suppressed. Furthermore, since the heating temperature is low (10 to 90°C, more preferably 80°C), the exudation of sodium from inside the particles is minimized, and less sodium is released and re-adhered to the powder surface after drying.
[0040] (Airflow Heat Drying) Airflow heat drying is a method for extracting spherical alumina powder from a slurry by spraying it into a high-temperature airflow (100–300°C) to evaporate only the water. The slurry is sprayed into the high-temperature airflow using a nozzle such as a two-fluid nozzle. The sprayed slurry breaks into fine droplets due to the dispersion effect of the airflow. Compared to conventional heat drying methods, airflow heat drying has a significantly larger surface area because the slurry is formed into droplets using a nozzle. Because the amount of heat received by the slurry is proportional to the surface area in contact with the heat source, the water in the droplets evaporates and dries quickly. Compared to conventional heat drying methods, the shorter drying time (approximately 0.01–10 seconds) minimizes sodium leaching from the interior of the particles, resulting in less free reattachment of sodium to the dried powder. Furthermore, because the spherical alumina powder is sprayed into the airflow, aggregation between the spherical alumina powder particles is suppressed, eliminating the need to break down agglomerates of alumina particles.
[0041] [Resin Composite Composition] According to one embodiment of the present invention, a composite composition of the spherical alumina particles and a resin can be finally produced. The composition of the resin composite composition will be described in more detail below.
[0042] Using a slurry composition containing spherical alumina particles and a resin, it is possible to obtain a resin composite composition such as a semiconductor encapsulant (particularly a solid encapsulant), an interlayer insulating film, etc. Furthermore, by curing these resin composite compositions, it is possible to obtain a resin composite such as an encapsulant (cured product), a substrate for a semiconductor package, etc.
[0043] When producing the resin composite composition, for example, in addition to the spherical alumina particles and resin, a curing agent, a curing accelerator, a flame retardant, a silane coupling agent, etc. are blended as needed, and composited by a known method such as kneading, etc. Then, the composite is molded into pellets, films, etc. depending on the application.
[0044] In addition, when producing the resin composite composition, other inorganic fillers may be blended in addition to the spherical alumina particles and resin. Examples of the inorganic fillers include amorphous spherical silica particles, crystalline spherical silica particles, titania particles, magnesia particles, aluminum nitride particles, boron nitride particles, barium titanate particles, calcium titanate particles, and carbon fibers. The blending ratio of the inorganic fillers can be appropriately adjusted depending on the application of the resin composite composition.
[0045] Furthermore, when the resin composite composition is cured to produce a resin composite, for example, the resin composite composition is heated to melt it, processed into a shape according to the intended use, and then heated to a temperature higher than that used for melting to completely cure it. In this case, a known method such as a transfer molding method can be used.
[0046] For example, when manufacturing semiconductor-related materials such as package substrates and interlayer insulating films, known resins can be used as the resin for the resin composite composition, but epoxy resins are preferred. The epoxy resin is not particularly limited, but examples include bisphenol A epoxy resins, bisphenol F epoxy resins, biphenyl epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, naphthalene epoxy resins, and phenoxy epoxy resins. One of these resins can be used alone, or two or more resins with different molecular weights can be used in combination. Among these, epoxy resins having two or more epoxy groups per molecule are preferred from the viewpoints of curability, heat resistance, and the like. Specific examples include biphenyl-type epoxy resins, phenol novolac-type epoxy resins, orthocresol novolac-type epoxy resins, epoxidized novolac resins of phenols and aldehydes, glycidyl ethers of bisphenol A, bisphenol F, bisphenol S, etc., glycidyl ester acid epoxy resins obtained by reacting polybasic acids such as phthalic acid or dimer acid with epochlorohydrin, linear aliphatic epoxy resins, alicyclic epoxy resins, heterocyclic epoxy resins, alkyl-modified polyfunctional epoxy resins, β-naphthol novolac-type epoxy resins, 1,6-dihydroxynaphthalene-type epoxy resins, 2,7-dihydroxynaphthalene-type epoxy resins, bishydroxybiphenyl-type epoxy resins, and epoxy resins into which halogens such as bromine have been introduced to impart flame retardancy. Among these epoxy resins having two or more epoxy groups per molecule, bisphenol A-type epoxy resins are particularly preferred.
[0047] Furthermore, resins other than epoxy resins can also be used as resin composite compositions for applications other than semiconductor encapsulation composite materials, such as prepregs for printed circuit boards and various engineering plastics. Specific examples of resins that can be used in addition to epoxy resins include silicone resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyamides such as polyimides, polyamideimides, and polyetherimides; polyesters such as polybutylene terephthalate and polyethylene terephthalate; polyphenylene sulfide, aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS resins, AAS (acrylonitrile-acrylic rubber-styrene) resins, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resins.
[0048] The curing agent used in the resin composite composition may be any known curing agent for curing the resin, such as a phenol-based curing agent, such as a phenol novolac resin, an alkylphenol novolac resin, or a polyvinylphenol, which may be used alone or in combination.
[0049] The amount of the phenolic curing agent blended is preferably such that the equivalent ratio to the epoxy resin (phenolic hydroxyl group equivalent / epoxy group equivalent) is 0.1 or more and less than 1.0, thereby eliminating any unreacted phenolic curing agent from remaining and improving moisture absorption and heat resistance.
[0050] The amount of the spherical alumina particles of the present invention added to the resin composite composition is preferably large from the viewpoints of heat resistance and thermal expansion coefficient, but is usually 70% by mass to 95% by mass, preferably 80% by mass to 95% by mass, and more preferably 85% by mass to 95% by mass. This is because if the amount of the spherical alumina particles added is too small, it is difficult to obtain effects such as improving the strength of the sealing material and suppressing thermal expansion, and conversely, if the amount is too large, segregation due to aggregation of the spherical alumina particles is likely to occur in the composite material regardless of the surface treatment of the spherical alumina particles, and the viscosity of the composite material will also become too high, making it difficult to use as a sealing material.
[0051] In addition to the resin, known additives such as a silane coupling agent, a curing agent, a colorant, and a hardening retarder can be used.
[0052] As for the silane coupling agent, any known coupling agent may be used, but those having an epoxy-based functional group are preferred.
[0053] A slurry composition containing spherical alumina particles and a resin can be used to obtain a heat-dissipating sheet, a heat-dissipating grease, and the like.
[0054] When obtaining the heat dissipation sheet, the spherical alumina particles, resin, and additives are appropriately blended and compounded by a known method such as kneading, etc. The obtained composite is molded into a sheet by a known method.
[0055] For example, when producing a heat dissipation sheet, known resins can be used in the resin composite composition, including silicone resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyamides such as polyimides, polyamideimides, and polyetherimides; polyesters such as polybutylene terephthalate and polyethylene terephthalate; polyphenylene sulfide, aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS resins, AAS (acrylonitrile-acrylic rubber-styrene) resins, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resins. Among these, silicone resins are preferred. The silicone resin is not particularly limited, but examples include peroxide-curable, addition-curable, condensation-curable, and ultraviolet-curable resins.
[0056] In addition to the resin, known additives such as a silane coupling agent, a curing agent, a colorant, and a hardening retarder can be used.
[0057] When preparing the thermally conductive grease, the spherical alumina particles, resin, and additives are appropriately blended and compounded by a known method such as kneading. The resin used in the thermally conductive grease is also called the base oil.
[0058] For example, when producing a thermally conductive grease, known resins can be used in the resin composite composition, and specific examples include silicone resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyamides such as polyimide, polyamideimide, and polyetherimide; polyesters such as polybutylene terephthalate and polyethylene terephthalate; polyphenylene sulfide, aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS resins, AAS (acrylonitrile-acrylic rubber-styrene) resins, AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resins, mineral oils, synthetic hydrocarbon oils, ester oils, polyglycol oils, silicone oils, and fluorine oils.
[0059] In addition to the resin, known additives such as silane coupling agents, colorants, thickeners, etc. Examples of the thickener that can be used include calcium soap, lithium soap, aluminum soap, calcium complex, aluminum complex, lithium complex, barium complex, bentonite, urea, PTFE, sodium terephthalamate, silica gel, and organic bentonite.
[0060] The present invention will be described below through examples and comparative examples, but the present invention should not be construed as being limited to the following examples.
[0061] The raw spherical alumina particles (Materials 1 to 4) listed in Table 1 were prepared and mixed with water to prepare a water slurry. When Materials 1 and 2 were used, the mixing ratio of ion-exchanged water and particles to prepare the water slurry was 200 kg of particle powder to 1000 L of water. When Material 3 was used, the mixing ratio was 300 kg of particle powder to 1000 L of ion-exchanged water. When Material 4 was used, the mixing ratio was 200 kg of particle powder to 1000 L of ion-exchanged water. The water slurry was mixed and stirred for 20 minutes to 1 hour, and then filtered using an appropriate filter until the water content was approximately 60 to 80 wt %.
[0062] (Examples 1 to 3) The prepared slurry was once pre-frozen under the condition of −40° C. Then, the inside of the apparatus was vacuum degassed and freeze-dried at 80° C. for 24 hours.
[0063] Example 4 The prepared slurry was air-dried at 200° C. using a jet turbo dryer manufactured by Hiraiwa Iron Works.
[0064] (Comparative Examples 1 to 3) The prepared slurry was left to stand in an oven without airflow and dried by a heat drying method at 230° C. for 40 hours.
[0065] Comparative Example 4 A slurry prepared using Material 4 was freeze-dried under the same conditions as in Example 1.
[0066] Comparative Example 5 A slurry prepared using Material 1 was once pre-frozen at −40° C. Thereafter, the slurry was freeze-dried at 95° C. for 24 hours while the inside of the apparatus was vacuum degassed.
[0067] Comparative Example 6 A slurry prepared using Material 1 was air-dried at 350° C. using a jet turbo drier manufactured by Hiraiwa Iron Works.
[0068] Example 5 The spherical alumina particles obtained in Example 1 and aluminum nitride particles (D50 = 30 μm) were mixed in a ratio of 90:10 (spherical alumina particle weight:aluminum nitride particle weight) to prepare a spherical alumina particle mixture A. Furthermore, the spherical alumina particle mixture A was mixed with Dow Toray's silicone resin CY52-276A liquid so that the amount of spherical alumina particle mixture A in the resin composite composition was 90% by mass. The mixture was then vacuum-kneaded using a Thinky vacuum kneader called "Awatori Rentaro" to obtain a resin composite composition. The kneading conditions were 15 seconds of pre-kneading and 90 seconds of vacuum kneading. After kneading, the plastic container containing the mixture was placed in a water bath adjusted to 25°C and cooled for 1 hour. 10 g of this resin composite composition was placed on a smooth-surfaced iron plate and tilted 60° from the horizontal to check the flowability of the resin composite composition. As a result, 5 hours after tilting, the resin composite composition flowed for 15 cm or more, demonstrating good fluidity.
[0069] Example 6: The spherical alumina particles obtained in Example 2 were mixed with boron nitride particles (D50 = 20 μm) at a ratio of 90:10 (spherical alumina particle weight:boron nitride particle weight) to prepare spherical alumina particle mixture B. Furthermore, spherical alumina particle mixture B was mixed with Dow Toray's silicone resin CY52-276A liquid so that the amount of spherical alumina particle mixture B in the resin composite composition was 90% by mass. The mixture was then vacuum-kneaded using a Thinky vacuum kneader called "Awatori Rentaro" to obtain a resin composite composition. The kneading conditions were 15 seconds of pre-kneading and 90 seconds of vacuum kneading. After kneading, the plastic container containing the mixture was placed in a water bath adjusted to 25°C and cooled for 1 hour. 10 g of this resin composite composition was placed on a smooth-surfaced iron plate and tilted 60° from the horizontal to check the flowability of the resin composite composition. As a result, 5 hours after tilting, the resin composite composition flowed for 15 cm or more, demonstrating good fluidity.
[0070] Table 2 shows the physical properties of the (dried) spherical alumina particles obtained under each condition.
[0071]
[0072]
[0073] The methods for measuring the various physical properties are described below.
[0074] (Average particle size by laser diffraction scattering method) The laser diffraction / scattering particle size distribution measurement method is a method in which a dispersion liquid containing spherical alumina particles is irradiated with laser light, and the particle size distribution is determined from the intensity distribution pattern of the diffracted / scattered light emitted from the dispersion liquid. In the present invention, a laser diffraction / scattering particle size distribution measurement device "Mastersizer 3000" (manufactured by Malvern) was used.
[0075] (Specific Surface Area) The specific surface area (BET value) was determined by applying the BET theory to the adsorption isotherm measured by the gas adsorption method (BET method). The specific surface area was measured using a specific surface area measuring device, "Macsorb Model HM-1208" manufactured by Mountech Co., Ltd.
[0076] (Residual surface sodium) The amount of ionic impurities adhering to the surface can be measured using ion chromatography. 4 g of sample and 40 ml of distilled water are added to a centrifuge tube, the tube is capped, and the tube is shaken thoroughly to mix. After mixing, the sample and sample solution are separated using a centrifuge. The sample solution is separated and analyzed for sodium ions using ion chromatography. Measurements were performed using an ion chromatograph manufactured by Toa Medical Electronics.
[0077] (Contains Na 2 O) 0.5 g of sample was placed in a pressure vessel, 10 ml of sulfuric acid (1 + 3) was added, the vessel was closed, and the vessel was heated in a heating and drying oven at 230 ° C for 16 hours. After the heated solution was allowed to cool, the solution was diluted to 100 ml and measured with an atomic absorption spectrophotometer. Note that sulfuric acid (1 + 3) refers to a solution diluted by adding 3 parts pure water to 1 part concentrated sulfuric acid by volume.
[0078] (Agglomeration Degree) Two standard sieves with mesh sizes of 4.75 mm and 212 μm were stacked in order. The sieve with 212 μm mesh was placed at the bottom, and the sieves with gradually increasing mesh sizes were stacked on top of it. 50 g of sample was placed on the top sieve with 4.75 mm mesh and set in a sieve shaker. The sieve shaker used was an OCTAGON 200 manufactured by Endecotts. After the sieves were set, the shaker was set to an amplitude of 5 and a shaking time of 3 minutes. After shaking was completed, the particle weights of the particles remaining on each sieve mesh and the particles that passed through the 212 μm mesh were measured. If the amount of particles on the 4.75 mm mesh is Ag, the amount of particles on the 212 μm mesh is Bg, and the amount of particles that passed through the 212 μm mesh is Cg, then the degree of agglomeration is calculated as A / (B+C)×100(%).
[0079] Through the above examples, it was confirmed that spherical alumina particles having a low surface residual Na concentration and a small degree of aggregation could be obtained, and that a resin composite composition containing the spherical alumina particles could be obtained.
[0080] The spherical alumina particles of the present invention have a low surface residual Na concentration, so when used as a filler, poor curing and loss of voltage resistance can be avoided. Furthermore, because of their low agglomeration, crushing is not required, and contamination due to crushing can be avoided. Therefore, they are suitable for use as a filler in miniaturized and thinned semiconductor packages, etc. Furthermore, the spherical alumina particles can be easily produced by a manufacturing method that is one aspect of the present invention. Resin composite compositions containing the spherical alumina particles exhibit good quality and can be used for purposes other than semiconductor encapsulation. Specifically, they can also be used as prepregs for printed circuit boards and various engineering plastics.
Claims
1. Average particle size is 0.4 to 1.9 μm, specific surface area is 1.0 to 5.0 m 2 / g, surface residual Na is 20 ppm or less, contained Na 2 Spherical alumina particles having an O content of 1000 ppm or less, an agglomeration degree of 1.0% or less, and a circularity of 0.9 or more.
2. Spherical alumina particles according to claim 1, characterized in that the gelatinization rate is 10.0% or less.
3. A method for producing spherical alumina particles, comprising: a water slurry preparation step of mixing raw spherical alumina with water to prepare a water slurry containing the raw spherical alumina; and a drying step of drying the water slurry.
4. The method for producing spherical alumina particles according to claim 3, further comprising: a raw material spherical alumina washing step of washing the raw material spherical alumina with water before the water slurry preparation step.
5. A resin composite composition containing the spherical alumina particles according to claim 1 or 2.
6. The resin composite composition according to claim 5, further comprising at least one inorganic filler selected from the group consisting of amorphous spherical silica particles, crystalline spherical silica particles, titania particles, magnesia particles, aluminum nitride particles, boron nitride particles, barium titanate particles, calcium titanate particles, and carbon fibers.