Spherical silica particles, resin composite composition containing same, and production method thereof

MYPI2025001928A0Undetermined Publication Date: 2024-03-30NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025001928
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-30
Filing Date
2023-10-02
Publication Date
2024-03-30

AI Technical Summary

Technical Problem

The miniaturization of semiconductor packages requires encapsulating materials with higher flowability and thermal conductivity, but increasing the filler filling rate to achieve this reduces fluidity, and existing methods struggle to optimize particle size distribution for both fluidity and thermal performance.

Method used

Spherical silica particles with a controlled particle size distribution, specifically limiting coarse particles ≥3 μm and ≥5 μm, and a specific surface area, are used in a resin composite composition, along with a method involving thermal spraying and classification to enhance fluidity and thermal conductivity.

Benefits of technology

The controlled particle size distribution of spherical silica particles improves the fluidity and filling properties of the resin composite, reducing defective rates in semiconductor products and enhancing thermal performance, particularly in small or thin semiconductor packages.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

ABSTRACT SPHERICAL SILICA PARTICLES, RESIN COMPOSITE COMPOSITION CONTAINING SAME, AND PRODUCTION METHOD THEREOF Spherical silica particles excellent in fluidity, a resin composite composition containing the spherical silica particles, and a method of production of the same, that is, spherical silica particle wherein, among the 1 m or more and 30 m or less particles detected by a Coulter counter, a number frequency of 3 m or more particles is 300 ppm or more and 50000 ppm or less, a number frequency of 5 m or more particles is 100 ppm or less, and a specific surface area by the BET method is 5.0 m2 / g or more and 20 m2 / g or less, a resin composite composition containing the spherical silica particles, and a method of production of the same.
Need to check novelty before this filing date? Find Prior Art

Description

Spherical silica particles, resin composite composition containing the same, and method for producing the same

[0001] The present invention relates to spherical silica particles, particularly particles having a size of 1 μm or more and 30 μm or less as detected by a Coulter counter, in which the number frequency of particles having a size of 3 μm or more is 300 ppm or more and 50,000 ppm or less, the number frequency of particles having a size of 5 μm or more is 100 ppm or less, and the specific surface area measured by the BET method is 5.0 m 2 / g or more 20m 2 The present invention relates to spherical silica particles having excellent fluidity due to a viscosity of 1 / g or less, a resin composite composition containing the same, and a method for producing the same.

[0002] Semiconductor packages such as ICs and CPUs are becoming smaller and thinner, which has led to a growing need for thinner bonding wires with narrower pitches. Meanwhile, the increased heat generated by semiconductor devices due to their higher performance has made it increasingly important to improve the heat dissipation capabilities of semiconductor packages. The encapsulating materials used in semiconductor packages are also required to have higher flowability and thermal conductivity to improve filling into narrow spaces. Resin composite compositions containing epoxy resins filled with silica particles as a filler have been used as encapsulating materials for semiconductor packages. However, due to the increasing need for high flowability in recent years, spherical silica particles have become increasingly popular as fillers. The use of spherical silica particles has significantly improved the flowability of encapsulating materials compared to conventional crushed silica particles.

[0003] However, as the need for higher thermal conductivity in encapsulants increases, it is becoming necessary to increase the filler filling rate, which has a higher thermal conductivity than resin, in order to increase the thermal conductivity of the encapsulant. Increasing the filler filling rate is also necessary to increase the strength of the encapsulant while lowering its thermal expansion coefficient. However, increasing the filler filling rate reduces fluidity, so attempts have been made to optimize the particle size distribution. Furthermore, a common method for increasing the space filling rate of filler particles is to blend particles with several different particle size distributions.

[0004] JP 2022-037681 A JP 2007-015884 A JP 2022-90679 A

[0005] As described above, the resin composite composition or its filler to be used as the sealing material has been studied from various viewpoints such as fluidity or filling property, heat dissipation property (thermal conductivity), and strength.

[0006] For example, Patent Document 1 proposes that the particle size distribution and specific surface area of ​​the amorphous silica powder contained in the resin composite composition be appropriately adjusted in order to obtain high fluidity of the resin composite composition. More specifically, in the particle size frequency distribution, the most frequent diameter is in the range of 1 to 10 μm, the frequency of particles with a particle size of less than 0.50 μm is 1.0% or more, and the most frequent diameter is in the range of 1 to 12 μm. 2 The document discloses an amorphous silica powder characterized by having a specific surface area of ​​1 / g.

[0007] Furthermore, Patent Document 2 relates to a method for producing spherical inorganic fine powder by thermally spraying raw material powder into a flame to form spherical particles, and proposes a method for suppressing the coarsening of the obtained powder (particles) and achieving a particle size within a desired range. More specifically, it discloses that by mixing a dispersion surface treatment agent with an inorganic raw material powder of a specific average particle size and then thermally spraying it, it is possible to prevent particle size increase during thermal spraying due to aggregation of the raw material powder.

[0008] Furthermore, Patent Document 3 discloses a spherical silica powder which comprises steps of forming spherical silica particles by a sol-gel method, firing the spherical silica particles, and then crushing the fired particles.

[0009] However, further improvements in the properties of the resin composite composition or its filler used as an encapsulant are required. In particular, with the recent trend toward smaller semiconductor packages, there is a demand for smaller particle sizes of fillers used in encapsulants. However, the decrease in flowability due to the smaller particle size of the filler has become a problem.

[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide spherical silica particles having excellent fluidity, a resin composite composition containing the same, and a method for producing the same.

[0011] The present inventors have found that the above-mentioned problems can be solved by precisely cutting out coarse particles in the particle size distribution of spherical silica particles, more specifically by limiting the number of coarse particles having a particle size equal to or larger than a certain particle size.

[0012] Based on the above findings, the gist of the present invention is as follows.

[0013] [1] Among particles of 1 μm or more and 30 μm or less detected by a Coulter counter, the number frequency of particles of 3 μm or more is 300 ppm or more and 50,000 ppm or less, the number frequency of particles of 5 μm or more is 100 ppm or less, and the specific surface area measured by the BET method is 5.0 m 2 / g or more 20m 2 / g or less. [2] Spherical silica particles according to [1], having a D50 of 0.4 to 3.0 μm as measured by a laser diffraction scattering method. [3] Spherical silica particles according to [1] or [2], having a circularity of 0.85 or more. [4] Spherical silica particles according to any one of [1] to [3], having a B / A ratio of 0.002 to 0.20, where A is the number frequency of particles of 1 to 2 μm and B is the number frequency of particles of 2 to 30 μm, among the number of particles of 1 μm to 30 μm measured by a Coulter counter. [5] Spherical silica particles according to any one of [1] to [4], having less than 10 ppm of particles of 10 μm or more, among the particles of 1 μm to 30 μm measured by a Coulter counter. [6] A resin composite composition comprising the spherical silica particles according to any one of [1] to [5]. [7] The resin composite composition according to [6], further comprising at least one inorganic filler selected from amorphous spherical alumina particles, crystalline spherical silica particles, alumina particles, titania particles, magnesia particles, aluminum nitride particles, boron nitride particles, barium titanate particles, calcium titanate particles, and carbon fibers. [8] A resin composite composition according to [6], further comprising a step of spheroidizing natural silica stone by introducing it into a flame to melt it and then cooling it, and a step of classifying the resulting material using a classifier and / or a sieve after the spheroidizing step, wherein, among particles of 1 μm to 30 μm in size detected by a Coulter counter, the number frequency of particles of 3 μm or larger is 300 ppm to 50,000 ppm, the number frequency of particles of 5 μm or larger is 100 ppm or less, and the specific surface area measured by the BET method is 5.0 m 2 / g or more 20m 2 / g or less, [1] to [5].

[0014] The spherical silica particles and resin composite compositions containing the spherical silica particles according to the present invention have a particle size distribution, particularly the number frequency of particles of 3 μm or larger and the number frequency of particles of 5 μm or larger, controlled within specific ranges. Therefore, they have excellent fluidity, i.e., excellent narrow-area filling ability. As a result, they can reduce the defect rate in semiconductor products, particularly in recent small or thin semiconductor products such as wafer-level packages (WLPs). Furthermore, the spherical silica particles can be obtained by the method for producing spherical silica particles according to the present invention.

[0015] The spherical silica particles according to the present invention have a particle size of 1 μm or more and 30 μm or less, and the number frequency of particles of 3 μm or more is 300 ppm or more and 50,000 ppm or less, and the number frequency of particles of 5 μm or more is 100 ppm or less, among particles of 1 μm or more and 30 μm or less, as detected by a Coulter counter. The specific surface area measured by the BET method is 5.0 m 2 / g or more 20m 2 / g or less.

[0016] The Coulter Counter measures particles using an electrical resistance method known as the Coulter Principle, and is free from errors in particle surface morphology, internal structure, refractive index, color, etc., which can be seen in optical measurement methods, resulting in high measurement accuracy. In particular, the particle size obtained by this method can be expressed as a number distribution, making it possible to precisely control the particle size distribution.

[0017] Spherical silica particles and 150 mL of electrolyte were placed in a 200 mL glass beaker and dispersed for 30 seconds using an ultrasonic homogenizer (ULTRA SONIC HOMOGENIZER UH-300, manufactured by SMT Corporation). This dispersion was then added to the electrolyte prepared in another beaker to adjust the concentration. The particle size of each spherical silica particle in the concentration-adjusted dispersion was measured using a Coulter counter (Multisizer 3, manufactured by Beckman Coulter) with an aperture diameter of 50 μm. The number of particles measured per measurement was approximately 100,000, and the same sample was measured three times. Of the particles detected by the Coulter counter with a particle size of 1 μm or more and 30 μm or less, the number of particles with a particle size of 3 μm or more and 5 μm or more was calculated, and this was taken as the frequency (ppm) of coarse particles relative to the total number of particles measured.

[0018] Measurement using this Coulter counter reveals that the number frequency of particles 3 μm or larger relative to the total number of spherical silica particles 1 μm or larger and 30 μm or smaller is 300 ppm or larger and 50,000 ppm or smaller, and the number frequency (ratio) of coarse particles 5 μm or larger is 100 ppm or smaller. For example, 100 ppm or smaller means that, when there are 100,000 particles 1 μm or larger and 30 μm or smaller, there are 10 or fewer particles 5 μm or larger. The present inventors have found that if the number frequency of coarse particles 5 μm or larger exceeds 100 ppm, such coarse particles clog the narrow spaces between the mounting substrate and the chip, reducing fluidity and, as a result, reducing the defect rate of semiconductor products filled with the particles.

[0019] The lower the number frequency of coarse particles of 5 μm or more, the better the fluidity, so this number frequency may be 90 ppm or less, 80 ppm or less, 70 ppm or less, 60 ppm or less, or 50 ppm or less. The number frequency of coarse particles of 5 μm or more may be 0 ppm, but completely eliminating these coarse particles, i.e., achieving 0 ppm, can be difficult due to the large burden on production management, so it may be set to several ppm, specifically 1 ppm or more, or 5 ppm or more. The lower limit of this number frequency may be adjusted depending on the actual application and the allowable range of the target yield, and may be, for example, 10 ppm or more, 20 ppm or more, or 30 ppm or more.

[0020] On the other hand, the number frequency of coarse particles of 3 μm or more needs to be controlled to ensure the fluidity of the resin composite composition. If the number frequency is less than 300 ppm, the number of particles with a large specific surface area of ​​less than 3 μm increases, causing an increase in viscosity and resulting in a decrease in fluidity. On the other hand, if the number frequency exceeds 50,000 ppm, it becomes difficult to prevent the inclusion of particles of 5 μm or more, causing clogging in the narrow space between the mounting substrate and the chip, resulting in a decrease in fluidity. The preferred upper limit of the number frequency is 30,000 ppm, more preferably 20,000 ppm. The preferred lower limit of the number frequency is 500 ppm, more preferably 1,000 ppm, and even more preferably 2,000 ppm.

[0021] Furthermore, among particles of 1 μm to 30 μm detected by a Coulter counter, it is preferable that the number frequency of particles of 10 μm or larger is less than 10 ppm. The lower the number frequency of coarse particles of 10 μm or larger, the better the fluidity, so this is preferable. If the number frequency of coarse particles of 10 μm or larger is 10 ppm or higher, such coarse particles will clog the narrow spaces between the mounting substrate and the chip, reducing fluidity. It is more preferable that the number frequency is less than 5 ppm, even more preferably less than 1 ppm, even more preferably less than 0.1 ppm, and most preferably zero.

[0022] Furthermore, among the number of particles measuring 1 μm to 30 μm in size as detected by a Coulter counter, if the particle frequency of 1 to 2 μm is A and the particle frequency of 2 to 30 μm is B, then the ratio B / A is preferably 0.002 to 0.20. This means that it is preferable to contain an excess of 1 to 2 μm particles relative to the 2 to 30 μm particles, but if there are too many 1 to 2 μm particles with large surface areas, the flowability will deteriorate. By setting the ratio within this range, the flowability of the resin composite composition is appropriately ensured and the filling (blending) effect of the filler is fully exhibited. A more preferred lower limit of B / A is 0.01, more preferably 0.03, more preferably 0.05, and even more preferably 0.10. On the other hand, a more preferred upper limit of B / A is 0.19.

[0023] Classification may be performed to obtain a desired particle size distribution. Conventionally known methods can be used for classification, and either wet classification or dry classification may be used. Gravitational field classification, inertial field classification, or centrifugal field classification may also be used. In the case of centrifugal field classification, either a free vortex type or a forced vortex type may be used. A preferred example is a method of using a precision wind classifier (also called an "air classifier") to separate the coarse and fine powders. However, in the present invention, the number frequency is measured using a Coulter counter in classification control, and precise control of the particle size distribution can contribute to the excellent properties of the spherical silica particles, such as fluidity.

[0024] The spherical silica particles of the present invention exhibit the effects of the invention regardless of the degree of crystallinity. However, since amorphous silica has a lower coefficient of thermal expansion than crystalline silica, in order to more effectively reduce the coefficient of thermal expansion of the resin composition, the degree of crystallinity is preferably 20% or less. More preferably, it is 10% or less, and even more preferably, it is 5% or less. Even more preferably, it is 1% or less. Even more preferably, it is 0.1% or less. Here, "degree of crystallinity" refers to the proportion of amorphous and crystalline silica present in the spherical silica particles. The degree of crystallinity can be determined by XRD. In XRD measurement, the proportion of the crystalline phase can be calculated using the sum of the integrated intensities of the crystalline peaks (Ic) and the integrated intensity of the amorphous halo portion (Ia) using the following formula: X (crystalline phase proportion) = Ic / (Ic + Ia) × 100 (%). In the present invention, XRD measurement was performed within the range of 2Θ = 10° to 90°. The crystalline phase ratio was determined from the sum of the crystalline peak intensities appearing in the 2Θ measurement range and the integrated intensity of the broad halo portion due to amorphous matter appearing around 2Θ = 22°. In this invention, an X-ray diffractometer "D2 PHASER" (manufactured by Bruker) was used.

[0025] The spherical silica particles of the present invention can be produced by a method such as a thermal spraying method. In the thermal spraying method, natural silica powder, which has been pulverized to a desired particle size, is passed through a flame, whereby the particles melt and become spherical due to surface tension. By such a thermal spraying method, spherical silica particles having a circularity of 0.80 or more, preferably 0.85 or more, can be produced. They can also be obtained by burning metals. For example, a chemical flame is formed in an oxygen-containing atmosphere with a mixture of metal powder such as silicon powder or silicon powder together with a carrier gas, and the desired silica (SiO 2 The degree of crystallinity can be controlled by the conditions of heat treatment (melting, cooling, etc. of the particles) in the process of producing the spherical silica particles.

[0026] The spherical silica particles may be mixed with other inorganic fillers to the extent that desired properties are obtained. Here, other inorganic fillers include those of different types, such as alumina powder, magnesia powder, titania powder, etc., as well as those with different particle size distributions. The types of other inorganic fillers will be described later.

[0027] In one embodiment of the present invention, the spherical silica particles may have a D50 of 0.4 to 3.0 μm as measured by a laser diffraction scattering method.

[0028] The particle size distribution of spherical silica particles can also be measured by a laser diffraction scattering method, and can be measured using a particle size distribution measuring device such as a "Mastersizer 3000" (manufactured by Malvern). In the measurement, the refractive index of water, which is the solvent, is set to 1.33, and the refractive index of the powder is determined by taking into account the refractive index of the powder material. For example, the refractive index of amorphous silica is measured as 1.54.

[0029] D50 (median diameter) refers to the particle diameter at which the cumulative volume is 50% in the cumulative particle size distribution of spherical silica particles, and D100 (maximum particle diameter) refers to the particle diameter at which the cumulative volume is 100% in the cumulative particle size distribution of spherical silica particles.

[0030] If D50 is less than 0.4, the particle size is small, and the viscosity of the encapsulant containing the particles may become too high. On the other hand, if D50 is more than 3.0 μm, the particles may settle during storage or during filling and curing, and the inclusion of particles of 5 μm or more may increase, causing the particles to get caught in the narrow space between the mounting substrate and the chip, resulting in poor fluidity of the encapsulant and reduced moldability. A more preferred lower limit is 1.0 μm. On the other hand, a more preferred upper limit is 2.0 μm.

[0031] The spherical silica particles according to the present invention have a specific surface area of ​​5 m2 as measured by the BET method. 2 / g or more 20m 2 / g or less.

[0032] The specific surface area of ​​the spherical silica particles can also be measured by the BET method, using a specific surface area measuring device manufactured by Mountech Co., Ltd. under the trade name "Macsorb Model HM-1208."

[0033] The specific surface area of ​​spherical silica particles is 5m 2 If the specific surface area is less than 6 m / g, the particles are unlikely to form a close-packed structure, which may reduce the fluidity of the sealing material containing the particles. 2 / g or more, 2 On the other hand, the specific surface area of ​​the spherical silica particles may be 20 m / g or more. 2 If the specific surface area is more than 15 m / g, the tendency for aggregation between particles increases, which may also reduce the fluidity of the sealing material. 2 / g or less, 2 / g or less.

[0034] In one embodiment of the present invention, the spherical silica particles may have a circularity of 0.85 or more. The higher the circularity of the spherical silica particles, the lower the viscosity of the resin composite composition containing the particles and the more improved the moldability. The circularity may be 0.90 or more, or 0.93 or more. Theoretically, the upper limit of the circularity is 1.0, but from the viewpoint of production control, it may be 0.98 or less, or 0.95 or less.

[0035] The circularity can be measured using an electron microscope, an optical microscope, and an image analyzer. For example, Sysmex FPIA. These devices are used to measure the circularity of particles (perimeter of the equivalent circle / perimeter of the projected image of the particle). The circularity of 100 or more particles is measured, and the average value is taken as the circularity of the powder.

[0036] In one embodiment of the present invention, a resin composite composition containing spherical silica particles is provided. Furthermore, a resin composite can be produced by curing the resin composite composition. The composition of the resin composite composition is described below.

[0037] Using a slurry composition containing spherical silica particles and a resin, it is possible to obtain a resin composite composition such as a semiconductor encapsulant (particularly a solid encapsulant), an interlayer insulating film, etc. Furthermore, by curing these resin composite compositions, it is possible to obtain a resin composite such as an encapsulant (cured product), a substrate for semiconductor packaging, etc.

[0038] When producing the resin composite composition, for example, in addition to the spherical silica particles and resin, a curing agent, a curing accelerator, a flame retardant, a silane coupling agent, etc. may be blended as needed, and the composite may be formed by a known method such as kneading, etc. Then, the composite may be molded into pellets, films, etc. depending on the application.

[0039] Furthermore, when producing the resin composite composition, in addition to the spherical silica particles and resin, other inorganic fillers may be blended. Examples of the inorganic fillers include amorphous spherical silica particles, amorphous spherical alumina particles, crystalline spherical silica particles, alumina particles, titania particles, magnesia particles, aluminum nitride particles, boron nitride particles, barium titanate particles, calcium titanate particles, and carbon fibers. The blending ratio of the inorganic fillers can be adjusted appropriately depending on the application of the resin composite composition, but from the viewpoint of exerting the effects of the spherical silica particles of the present invention, it is preferable that the blending ratio of the spherical silica particles to the other inorganic fillers is 95:5 to 60:40.

[0040] Furthermore, when the resin composite composition is cured to produce a resin composite, for example, the resin composite composition can be melted by applying heat, processed into a shape according to the intended use, and then completely cured by applying heat higher than that used for melting. In this case, known methods such as transfer molding and compression molding can be used.

[0041] For example, when manufacturing semiconductor-related materials such as package substrates and interlayer insulating films, known resins can be used as the resin for the resin composite composition, but epoxy resins are preferred. The epoxy resin is not particularly limited, but examples include bisphenol A epoxy resins, bisphenol F epoxy resins, biphenyl epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, naphthalene epoxy resins, and phenoxy epoxy resins. One of these resins can be used alone, or two or more resins with different molecular weights can be used in combination. Among these, epoxy resins having two or more epoxy groups per molecule are preferred from the viewpoints of curability, heat resistance, and the like. Specific examples include biphenyl-type epoxy resins, phenol novolac-type epoxy resins, orthocresol novolac-type epoxy resins, epoxidized novolac resins of phenols and aldehydes, glycidyl ethers of bisphenol A, bisphenol F, bisphenol S, etc., glycidyl ester acid epoxy resins obtained by reacting polybasic acids such as phthalic acid or dimer acid with epochlorohydrin, linear aliphatic epoxy resins, alicyclic epoxy resins, heterocyclic epoxy resins, alkyl-modified polyfunctional epoxy resins, β-naphthol novolac-type epoxy resins, 1,6-dihydroxynaphthalene-type epoxy resins, 2,7-dihydroxynaphthalene-type epoxy resins, bishydroxybiphenyl-type epoxy resins, and epoxy resins into which halogens such as bromine have been introduced to impart flame retardancy. Among these epoxy resins having two or more epoxy groups per molecule, bisphenol A-type epoxy resins are particularly preferred.

[0042] Furthermore, resins other than epoxy resins can also be used as resin composite compositions for applications other than semiconductor encapsulation composite materials, such as prepregs for printed circuit boards and various engineering plastics. Specific examples of resins that can be used in addition to epoxy resins include silicone resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyamides such as polyimides, polyamideimides, and polyetherimides; polyesters such as polybutylene terephthalate and polyethylene terephthalate; polyphenylene sulfide, aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS resins, AAS (acrylonitrile-acrylic rubber-styrene) resins, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resins.

[0043] The curing agent used in the resin composite composition may be any known curing agent for curing the resin, such as a phenol-based curing agent, such as a phenol novolac resin, an alkylphenol novolac resin, or a polyvinylphenol, which may be used alone or in combination.

[0044] The amount of the phenolic curing agent blended is preferably such that the equivalent ratio to the epoxy resin (phenolic hydroxyl group equivalent / epoxy group equivalent) is 0.1 or more and less than 1.0, thereby eliminating any unreacted phenolic curing agent from remaining and improving moisture absorption and heat resistance.

[0045] The amount of spherical silica particles added to the resin composite composition is preferably large from the viewpoints of heat resistance and thermal expansion coefficient, but is typically 70% by mass to 95% by mass, preferably 80% by mass to 95% by mass, and more preferably 85% by mass to 95% by mass. This is because if the amount of spherical silica particles is too small, it is difficult to achieve effects such as improving the strength of the sealing material and suppressing thermal expansion. Conversely, if the amount is too large, segregation due to aggregation of the spherical silica particles is likely to occur in the composite material regardless of the surface treatment of the spherical silica particles, and the viscosity of the composite material will also become too high, making it difficult to use as a sealing material. Note that when the aforementioned "other filler" is used in combination, the preferred amount added to the resin composite composition is the total amount of the spherical alumina particles and the "other filler."

[0046] As for the silane coupling agent, any known coupling agent may be used, but those having an epoxy-based functional group are preferred.

[0047] The fluidity (narrow section fluidity) of a resin composite composition containing spherical silica particles is measured, for example, by the following procedure. A transfer molding machine equipped with a measuring mold having a slit with a groove depth of 10 μm or less is used to measure the length of the resin composite composition containing each spherical silica particle flowing into the slit. The transfer molding conditions are a mold temperature of 175°C, a molding pressure of 7 MPa, and a dwell time of 180 seconds. The longer this length, the better the fluidity.

[0048] The resin composite composition for measuring fluidity is prepared by mixing spherical silica particles with a resin of predetermined conditions at a mixing ratio. For example, the resin composite composition is prepared by mixing a biphenyl-based epoxy resin (YX4000H (manufactured by Mitsubishi Chemical Corporation) and spherical silica particles at a ratio of 25:75 (wt %), and further adding a curing agent, a curing accelerator, a mold release agent, and an epoxy-based silane coupling agent.

[0049] A method for producing spherical silica particles, which is one embodiment of the present invention, includes a step of introducing natural silica stone into a flame to melt it, followed by cooling to spheroidize it, and a step of classifying the particles using a classifier (e.g., a precision air classifier) ​​and / or a sieve after the spheroidization step. This production method produces spherical silica particles in which, among particles of 1 μm or more and 30 μm or less detected by a Coulter counter, the number frequency of particles of 3 μm or more is 300 ppm or more and 50,000 ppm or less, the number frequency of particles of 5 μm or more is 100 ppm or less, and the specific surface area measured by the BET method is 5.0 m. 2 / g or more 20m 2 / g or less.

[0050] The present invention will be described below through examples and comparative examples, but the present invention should not be construed as being limited to the following examples.

[0051] (Examples 1 to 6, Comparative Examples 1 to 4) Natural silica stone was crushed, and the crushed material was fed into a high-temperature flame formed by the combustion of LPG and oxygen, where it was melted and spheroidized to obtain spherical silica particles. The flame formation conditions, raw material particle size, raw material feed rate, classification conditions, mixing conditions, etc. were adjusted to produce various powders as shown in Table 1. Specifically, the particle size distribution was adjusted by adjusting the raw material particle size and by subjecting the powder after spheroidization to multistage sieving and classification, with classification performed using a precision air classifier as the final step. The number frequency of particles 5 μm or larger among particles 1 μm to 30 μm in size detected by a Coulter counter, D50 (or mode diameter) measured by laser diffraction scattering, specific surface area and circularity measured by the BET method, the ratio B / A of the number frequencies measured by the Coulter counter (where A is the number frequency of particles 1 to 2 μm and B is the number frequency of particles 2 to 30 μm), and the number frequency of particles 10 μm or larger measured by a Coulter counter were adjusted by adjusting the mixing amounts of several types of powder obtained by the above operations. For example, the number frequency and its ratio were adjusted by mixing particles with known number frequencies in appropriate ratios, the specific surface area was adjusted by adding ultrafine powders with various particle sizes and specific surface areas, and the circularity was controlled by adjusting the flame formation conditions and the feed rate of raw material.

[0052] Table 1 shows the physical properties of the spherical silica particles used.

[0053]

[0054] The methods for measuring the various physical properties are described below.

[0055] (Measurement by Coulter Counter Method) Spherical silica particles and 150 mL of electrolyte were placed in a 200 mL glass beaker and dispersed for 30 seconds using an ultrasonic homogenizer (ULTRA SONIC HOMOGENIZER UH-300, manufactured by SMT Corporation). This dispersion was then added to electrolyte prepared in another beaker to adjust the concentration. The concentration-adjusted dispersion was measured using a Coulter counter (Multisizer 3, manufactured by Beckman Coulter) with an aperture diameter of 50 μm to measure the individual particle diameters of the spherical silica particles. At this time, the number of particles measured per measurement was set to approximately 100,000, and the same sample was measured three times. Of these, the number of particles with particle diameters of 3 and 5 μm or more was calculated, and this was taken as the respective coarse particle frequencies (ppm) relative to the total number measured. Similarly, the number frequency A of particles having a particle size of 1 to 2 μm, the number frequency B of particles having a particle size of 2 to 30 μm, and the number frequency of particles having a particle size of 10 μm or more were also measured.

[0056] (D50 by laser diffraction scattering method) Measurement was performed using a particle size distribution analyzer "Mastersizer 3000" (manufactured by Malvern). In the measurement, the refractive index of water, which is the solvent, was set to 1.33, and the refractive index of the powder was determined taking into account the refractive index of the powder material. For example, the refractive index of amorphous silica was measured as 1.54.

[0057] (Specific Surface Area) The specific surface area (BET value) was determined by applying the BET theory to the adsorption isotherm measured by the gas adsorption method (BET method). The specific surface area was measured using a specific surface area measuring device, "Macsorb Model HM-1208" manufactured by Mountech Co., Ltd.

[0058] (Circularity) Circularity can be measured using an electron microscope, an optical microscope, and an image analyzer. For example, Sysmex FPIA. Using these devices, the circularity of particles (perimeter of the equivalent circle / perimeter of the projected image of the particle) is measured. The circularity of 100 or more particles is measured, and the average value is taken as the circularity of the powder.

[0059] (Fluidity (narrow section fluidity)) Using a transfer molding machine equipped with a measuring mold having a slit with a groove depth of 10 μm or less, the length of flow of each resin composite composition containing spherical silica particles into the slit was measured. The transfer molding conditions were a mold temperature of 175°C, a molding pressure of 7 MPa, and a dwell time of 180 seconds. The longer this length, the better the fluidity. A long length (2.5 cm or more) was marked as ○ (Excellent), a length of 1.5 cm or more but less than 2.5 cm was marked as △ (Good), and a short length (less than 1.5 cm) was marked as × (Not Good).

[0060] The resin composite composition for measuring the flowability was prepared by mixing a biphenyl-based epoxy resin (YX4000H (manufactured by Mitsubishi Chemical Corporation) and spherical silica particles in a ratio of 25:75 (wt %), and further adding a curing agent, a curing accelerator, a mold release agent, and an epoxy-based silane coupling agent.

[0061] (True Specific Gravity) The true specific gravity of the silica particles was measured by the pycnometer method (liquid phase displacement method) using a continuous automatic powder true density measuring device (manufactured by Seishin Enterprise Co., Ltd., trade name: AUTO TRUE DENSER MAT-7000).

[0062] Resin composite compositions containing silica particles of Examples 1 to 6 and Comparative Examples 1 to 4 were prepared, and the fluidity (narrow section fluidity) was measured. The measurement results are shown in Table 1. It was confirmed that spherical silica particles within the range of the present invention had good fluidity, rated ○ (Excellent) or △ (Good).

[0063] The spherical silica particles of the present invention and the resin composite composition containing the same exhibit good fluidity and can be used for purposes other than semiconductor encapsulation. Specifically, they can also be used as prepregs for printed circuit boards and various engineering plastics. Furthermore, the spherical silica particles can be obtained by the method for producing spherical silica particles according to the present invention.

Claims

1. Among particles between 1 μm and 30 μm detected by a Coulter counter, the number frequency of particles 3 μm or larger is between 300 ppm and 50,000 ppm, the number frequency of particles 5 μm or larger is 100 ppm or smaller, and the specific surface area measured by the BET method is 5.0 m 2 / g or more 20m 2 / g or less.

2. The spherical silica particles according to claim 1, having a D50 measured by a laser diffraction scattering method of 0.4 to 3.0 μm.

3. Spherical silica particles according to claim 1, having a circularity of 0.85 or more.

4. Spherical silica particles according to claim 1, wherein, among the number of particles of 1 μm or more and 30 μm or less detected by a Coulter counter, the particle number frequency of 1 to 2 μm is A and the particle number frequency of 2 to 30 μm is B, and the ratio B / A is 0.002 or more and 0.20 or less.

5. Spherical silica particles according to claim 1, in which, of particles of 1 μm or more and 30 μm or less, particles of 10 μm or more account for less than 10 ppm when detected by a Coulter counter.

6. A resin composite composition comprising the spherical silica particles according to any one of claims 1 to 5.

7. The resin composite composition according to claim 6, further comprising at least one inorganic filler selected from the group consisting of amorphous spherical alumina particles, crystalline spherical silica particles, alumina particles, titania particles, magnesia particles, aluminum nitride particles, boron nitride particles, barium titanate particles, calcium titanate particles, and carbon fibers.

8. A method for producing a natural silica stone, characterized by a step of introducing natural silica stone into a flame to melt it, and then cooling it to spheroidize it, and a step of classifying it using a classifier and / or a sieve after the spheroidization step, in which, among particles of 1 μm to 30 μm detected by a Coulter counter, the number frequency of particles of 3 μm or more is 300 ppm to 50,000 ppm, the number frequency of particles of 5 μm or more is 100 ppm or less, and the specific surface area measured by the BET method is 5.0 m 2 / g or more 20m 2 / g or less.