Easily adhesive polyamide film and method for producing same
Patent Information
- Application Number
- MYPI2025001952
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-07-06
- Filing Date
- 2023-09-26
- Publication Date
- 2024-03-29
AI Technical Summary
Conventional polyamide films used for packaging face issues with adhesion after hot water treatment, blocking resistance, printability, and transparency, particularly during boiling or retort processing, due to insufficient adhesive strength and susceptibility to delamination.
A polyamide film with a primer layer containing a combination of polyurethane resin A without silanol groups and polyurethane resin B with silanol groups, having different glass transition temperatures, is used to enhance adhesion, blocking resistance, and printability, while maintaining transparency and reducing the need for curing agents.
The film achieves high adhesion and blocking resistance even after hot water treatment, with improved printability and transparency, making it suitable for food packaging and other industrial applications.
Smart Images

Figure PI2025001952_DRAWING_001 
Figure PI2025001952_DRAWING_002
Abstract
Description
Highly adhesive polyamide film and method for producing the same
[0001] The present invention relates to a novel highly adhesive polyamide film and a method for producing the same, and more particularly to a highly adhesive polyamide film suitable for use as a packaging material, an electrical insulating material, a general industrial material, etc., and a method for producing the same.
[0002] Biaxially oriented polyamide films are widely used as packaging films for packaging foods and other items because they have excellent mechanical properties, optical properties, thermal properties, barrier properties, and the like, as well as excellent abrasion resistance, impact resistance, pinhole resistance, and the like. In these applications, the surface of the substrate film is usually subjected to various secondary processes, such as coating with various coating agents, printing, vapor deposition, and lamination with other films. For this reason, attempts have been made to modify the surface of the substrate film and improve adhesion between the substrate film and the coating formed by the secondary process by subjecting the substrate film to physical surface treatments such as corona discharge treatment and plasma treatment, or chemical surface treatments that activate the film surface using chemicals such as acids and alkalis.
[0003] However, while physical surface treatments are relatively simple, the resulting adhesion is insufficient, while chemical surface treatments are complicated and have problems such as a poor working environment.
[0004] When polyamide films are used for food packaging, a method is generally adopted in which a sealant film is laminated on the film after printing as necessary. However, if the adhesive strength between the two films is weak, peeling between the polyamide film substrate and the sealant film, known as delamination, may occur during boiling or retort treatment for sterilizing the contents.
[0005] To solve this problem, in addition to the above-mentioned physical or chemical surface treatment methods, there is a method of forming an easily adhesive coating film (hereinafter referred to as a "primer layer") by applying a primer having adhesive activity to a substrate film. This method is widely used because it allows the primer component to be selected according to the type of top coat layer.
[0006] As a component of the primer layer, aqueous resins are often used from the viewpoints of workability, safety, and cost. Among them, polyurethane resins, polyester resins, acrylic resins, etc. are particularly used to improve adhesion with coating layers, ink layers, vapor deposition layers, etc. as top coat layers (Patent Documents 1 to 7).
[0007] Among these, for example, a method is known in which the surface properties of the coating film are improved and adhesion after hot water treatment is improved by controlling the thickness of the primer layer of an easy-adhesion polyamide film, the physical properties of the polyurethane resin used as the easy-adhesion coating agent, and the amount of volatile base components remaining in the primer layer (Patent Document 7). According to Patent Document 7, with regard to the volatile base components, by not including a curing agent (crosslinking agent) in the primer layer, the total amount of volatile base components can be reduced, which not only prevents a decrease in water resistance but also increases safety when used as a packaging material for food, etc.
[0008] JP 2022-38956, JP 2020-121496, JP 2014-22080, JP 2000-26798, JP 3-55302, International Publication WO2008 / 75461, International Publication WO2010 / 110282
[0009] However, these conventional films require further improvement in terms of blocking resistance. Specifically, when the film is handled in roll form, a phenomenon known as "blocking" tends to occur, in which films stick to each other. This phenomenon tends to be particularly pronounced when the primer layer does not contain a curing agent, as disclosed in Patent Document 7 and elsewhere. Furthermore, when the surface opposite the primer layer is subjected to a corona discharge treatment in order to be used as an intermediate layer in a multilayer laminate, blocking becomes even more likely to occur, leading to processing problems. In this case, one method for suppressing blocking is to add a lubricant to the primer layer, but adding a large amount of lubricant increases haze, impairing transparency and potentially reducing print visibility.
[0010] Furthermore, there is still room for improvement in the printability of conventional films, which is due to the primer layer. Product packaging is being printed in a wide variety of ways to express individuality as well as to promote environmental friendliness, so there is a trend toward higher demands for print appearance. In this regard, there is also the problem of localized deterioration in print appearance caused by the coating film properties of the primer layer applied to conventional films, and there is also room for improvement in this regard.
[0011] Furthermore, in recent years, with the aging of consumers and the diversification of products, there has been an increasing demand for long-term storage of food packaging, and the need for hot water retort treatment in the sterilization and pasteurization process has also increased. In addition, since boiling treatment is sometimes performed in an aerated state, there is a demand for the laminate to be able to maintain high strength even in harsher environments.
[0012] Thus, there is a demand for the development of materials that can maintain high adhesion even after hot water treatment such as boiling or retort treatment, and that also have excellent blocking resistance, printability, transparency, etc. However, there is still room for further improvement in these respects with conventional films.
[0013] Therefore, a main object of the present invention is to provide an easily adhesive polyamide film which has high adhesion even after hot water treatment and is also excellent in blocking resistance, printability, transparency, etc.
[0014] As a result of extensive research into the problems of the prior art, the inventors discovered that the above object can be achieved by forming a primer layer containing specific components on a polyamide film, and thus completed the present invention.
[0015] That is, the present invention relates to the following easy-to-adhere polyamide film and its manufacturing method. 1. A polyamide film having a primer layer formed on at least one surface of a polyamide substrate film, characterized in that (1) the primer layer contains a polyurethane resin A having no silanol groups and a polyurethane resin B having silanol groups, and (2) the polyurethane resin A and the polyurethane resin B have different glass transition temperatures (Tg). 2. The easy-to-adhere polyamide film according to item 1, wherein the polyurethane resin A has a glass transition temperature (Tg) in the range of 5 to 50°C, and the polyurethane resin B has a glass transition temperature (Tg) in the range of 60°C or higher. 3. The easy-to-adhere polyamide film according to item 1, wherein, when the total of the polyurethane resin A and the polyurethane resin B is 100 parts by mass, the polyurethane resin A is 25 to 80 parts by mass and the polyurethane B is 20 to 75 parts by mass. 4. 5. The highly adhesive polyamide film according to item 1, wherein polyurethane resin A has a film elongation of 300% or more and a tensile strength of 20 to 50 MPa, and polyurethane resin B has a film elongation of 200% or more and a tensile strength of 40 to 60 MPa. 2Item 1, wherein, when the areas of 300 halftone dots in the area are measured at any 10 locations in the TD direction of the printed film, the ratio of the smallest to the largest area (average of the 20 smallest areas / average of the 20 largest areas) is in the range of 0.8 to 1. 6. The easy-to-adhere polyamide film according to item 1, wherein the adhesion strength after one week in an environment of 40°C after overlapping primer layers and applying a load of 10 kg / cm is 40 g / 15 mm or less. 7. The easy-to-adhere polyamide film according to item 1, wherein the haze is 8% or less. 8. The easy-to-adhere polyamide film according to item 1, which is a biaxially stretched film. 9. A laminate comprising at least a laminating adhesive layer and a heat-sealing layer laminated in this order on the primer layer of the easy-to-adhere polyamide film according to any one of items 1 to 8, either directly or via a printed layer. 10. 11. A method for producing an easily adhesive polyamide film, comprising the steps of: (1) applying an aqueous coating agent containing a polyurethane resin A that does not have silanol groups and a polyurethane resin B that has silanol groups to at least one surface of an unstretched polyamide substrate film; and (2) biaxially stretching the polyamide film coated with the aqueous coating agent, followed by heat treatment. 12. A method for producing an easily adhesive polyamide film, comprising the steps of: (1) uniaxially stretching an unstretched polyamide substrate film in a first direction, (2) applying an aqueous coating agent containing a polyurethane resin A that does not have silanol groups and a polyurethane resin B that has silanol groups to at least one surface of the uniaxially stretched polyamide substrate film, and (3) uniaxially stretching the polyamide substrate film coated with the aqueous coating agent in a second direction perpendicular to the first direction, followed by heat treatment.
[0016] According to the present invention, it is possible to provide an easily adhesive polyamide film that has high adhesion even after hot water treatment and is also excellent in blocking resistance, printability, transparency, etc.
[0017] In particular, the highly adhesive polyamide film of the present invention uses two specific polyurethane resins with different glass transition temperatures in the primer layer, so that even after hot water treatment, it can achieve adhesion (lamination strength) equal to or better than that before the treatment and exhibit excellent blocking resistance. As a result, the content of lubricants and other additives can be reduced, making it possible to provide a film with high transparency. At the same time, it can maintain excellent adhesion performance even after hot water treatment, such as boiling or retorting.
[0018] Although the mechanism of action of using the above two types of polyurethane resins is unclear, it is presumed that by using polyurethane resin B having silanol groups, the silanol groups react with each other during the film drying and stretching process to form a crosslinked structure, which allows the primer layer to be cured without the need for a curing agent, resulting in improved blocking resistance. On the other hand, polyurethane resin A having no silanol groups does not form such a crosslinked structure, but it is presumed to function to improve printability while maintaining affinity with polyurethane resin B in the primer layer. In this way, it is believed that the combined use of two types of polyurethane resins makes it possible to exhibit excellent blocking resistance, printability, etc., while maintaining high adhesion even after hot water treatment.
[0019] The highly adhesive polyamide film of the present invention having these characteristics can be suitably used, for example, as a packaging material, an electrical insulating material, a general industrial material, etc. In particular, it is suitable as a food packaging material that is printed on the film and then subjected to boiling or retort treatment.
[0020] Furthermore, the highly adhesive polyamide film of the present invention has the advantages of being easily obtained by applying an aqueous coating agent containing a polyurethane resin to a polyamide film and then drying it, and of being easy to control the thickness, etc. As a result, the highly adhesive polyamide film of the present invention has excellent productivity and is industrially advantageous.
[0021] According to the manufacturing method of the present invention, by incorporating the process of forming a primer layer by applying an aqueous coating agent into the film manufacturing process, the coating agent can be dried simultaneously during the heat treatment process aimed at thermal setting of the polyamide film, thereby simplifying the process. Furthermore, the temperature conditions of the heat treatment process can be higher than the heating conditions when a coating agent is applied to a film and then dried after molecular crystallization and orientation (hereinafter also referred to as "oriented crystallization") by biaxial stretching is completed. This is advantageous for reducing the volatile base components in the primer layer. In contrast, when a curing agent is added separately to the aqueous coating agent, a network-like crosslinked structure is formed during in-line drying, and localized unevenness in the primer layer originating from the curing points deteriorates the print appearance. Furthermore, if the primer layer contains only a polyurethane resin without a curing agent, blocking is likely to occur due to changes over time when the film is stored in roll form after film formation. According to the present invention, by incorporating a silanol group-containing polyurethane at a specific blend ratio, water-resistant adhesion and improved print appearance can be achieved without compromising blocking properties.
[0022] 1 is a diagram showing an example of the layer structure of an easily adhesive polyamide film of the present invention. 2 is a diagram showing an example of the layer structure of a laminate of the present invention. 3 is a diagram showing an outline of a method for evaluating the printability of a film in Test Example 1.
[0023] 1. Highly Adhesive Polyamide Film The highly adhesive polyamide film of the present invention (the film of the present invention) is a polyamide film having a primer layer formed on at least one surface of a polyamide substrate film, characterized in that: (1) the primer layer contains a polyurethane resin A having no silanol groups and a polyurethane resin B having silanol groups; and (2) the glass transition temperatures (Tg) of the polyurethane resin A and the polyurethane resin B are different from each other.
[0024] In the present invention, a polyamide substrate film having a primer layer formed on at least one side thereof and no other layers laminated thereon is referred to as a "film of the present invention," and a film of the present invention having other layers laminated on one or both sides thereof is referred to as a "laminate."
[0025] The basic layer structure of the film of the present invention is shown in Figure 1. In the film 10 of Figure 1A, a primer layer 12 is formed on one surface of a polyamide substrate film 11. In Figure 1A, the primer layer 12 is formed over the entire surface of one surface of the polyamide substrate film 11, but it may be formed on only a portion of the surface as long as the effects of the present invention are not impaired. In the film 10' of Figure 1B, the primer layer 12 is formed on both surfaces (front and back) of the polyamide substrate film 11. In Figure 1B, the primer layer 12 is formed over the entire surface of both surfaces of the polyamide substrate film 11, but it may be formed on only a portion of the surface as long as the effects of the present invention are not impaired.
[0026] 1A and 1B, a transparent film can be suitably used as the polyamide substrate film 11. Similarly, it is desirable that the primer layer 12 is also transparent. By configuring the film of the present invention from these transparent layers, the haze value described below can be more reliably achieved.
[0027] Polyamide Substrate Film The polyamide substrate film is composed mainly of a polyamide resin and functions as a core layer of the film of the present invention or the laminate described below.
[0028] An example of a polyamide resin is nylon 6, which is obtained by ring-opening polymerization of a raw material containing ε-caprolactam. Other examples of polyamide resins include polyamide resins obtained by polycondensation of raw materials containing a lactam with a three- or higher ring member, an ω-amino acid, a dibasic acid, a diamine, etc. The above raw materials are not limited, and, for example, conventional petroleum-derived monomers as well as monomers obtained by depolymerization through chemical recycling can also be used.
[0029] Furthermore, the polyamide resin may be a remelted resin obtained by melting a polyamide resin. In the present invention, from the viewpoints of environmental conservation and effective utilization of resources, waste polyamide resin (particularly polyamide 6 resin) may be used as the remelted resin. More specifically, examples of the remelted resin include pellets formed by remelting unstretched waste, edge trimming waste, slit waste, defective products, etc., generated during the production of polyamide film.
[0030] Specific examples of such polyamide resins include at least one of nylon 6, 7, 10, 11, 12, 4.10, 5.6, 6.6, 6.9, 6.10, 6.11, 6.12, 10.10, 6T, 9T, 10T, 6I, MXD6 (poly(metaxylylene adipamide), 6 / 6.6, 6 / 12, 6 / 6T, 6 / 6I, and 6 / MXD6. Of these, nylon 6 is preferred because of its excellent balance between heat resistance and mechanical properties.
[0031] The content of the polyamide resin in the polyamide substrate film is not limited, but can usually be set within a range of about 90 to 100% by mass, and can also be set to, for example, 95 to 99% by mass.
[0032] The polyamide substrate film may contain components other than the polyamide resin as long as the effects of the present invention are not impaired, such as at least one of various additives such as antioxidants, ultraviolet absorbers, preservatives, antistatic agents, antiblocking agents, and inorganic fine particles.
[0033] In particular, a lubricant may be blended to further improve the slip properties of the film. At least one of inorganic and organic lubricants can be used as the lubricant. Examples of inorganic lubricants include clay, talc, calcium carbonate, magnesium carbonate, zinc carbonate, wollastonite, silica, alumina, calcium oxide, magnesium oxide, calcium silicate, sodium aluminate, calcium aluminate, magnesium aluminosilicate, glass balloons, carbon black, zinc oxide, antimony trioxide, zeolite, hydrotalcite, layered silicate, sodium silicate, aluminum hydroxide, iron oxide, zirconium oxide, barium sulfate, titanium oxide, and carbon black. Examples of organic lubricants include acrylic crosslinked polymers, styrene crosslinked polymers, phenolic resins, nylon resins, polyethylene wax, and ethylene bisstearic acid amide. Among these, silica is preferred.
[0034] The content of the lubricant in the polyamide substrate film is not particularly limited, but from the viewpoint of ensuring the transparency of the film, it is preferably 0.5% by mass or less, and more preferably 0.3% by mass or less, in the polyamide substrate film. The lower limit can be, for example, 0.01% by mass, but is not limited thereto. Note that when used in applications where transparency is not required, the content may exceed 0.5% by mass.
[0035] The polyamide substrate film may be composed of a single layer, or may be composed of multiple layers formed by simultaneous melt extrusion, lamination, etc. In particular, in the present invention, a polyamide substrate film composed of a single layer is preferred because it can be easily produced.
[0036] As the polyamide substrate film, a pre-made or commercially available polyamide film can be used, or a film formed by a known film forming method can also be used.
[0037] When producing a polyamide substrate film, for example, a molten polymer is extruded through a T-die and then cooled with a casting roll to produce an unstretched sheet. This is then subjected to simultaneous biaxial stretching or sequential biaxial stretching. The stretched film thus obtained is subjected to a short-term heat treatment, for example, at a temperature of about 200°C, to improve dimensional stability. In this way, a polyamide substrate film can be obtained. That is, the polyamide substrate film in the film of the present invention is preferably a biaxially stretched film.
[0038] Furthermore, the polyamide substrate film may be subjected to a surface treatment such as a corona discharge treatment, if necessary, within the scope that does not impair the effects of the present invention.
[0039] The thickness of the polyamide substrate film is not limited and can be appropriately set depending on the application, location of use, etc., but it is usually sufficient to set it within the range of about 3 to 50 μm.
[0040] Primer Layer The primer layer is formed on one or both sides of the polyamide substrate film and has the function of imparting excellent adhesion to the polyamide substrate film. The primer layer of the film of the present invention contains a polyurethane resin A that does not have a silanol group and a polyurethane resin B that has a silanol group. By containing both polyurethane resin A and polyurethane resin B in the primer layer, it is possible to achieve lamination strength after hot water treatment that could not be achieved with polyurethane resin A alone or polyurethane resin B alone, and it is also possible to obtain good blocking resistance, printability, etc.
[0041] Polyurethane Resin A The polyurethane resin A may be any resin that does not contain silanol groups in the molecule, and may be, for example, a polyurethane resin obtained by reacting a compound containing at least two isocyanate groups in one molecule (hereinafter referred to as an "isocyanate group-containing compound") with a compound containing at least two active hydrogen groups in one molecule (hereinafter referred to as an "active hydrogen group-containing compound"). Polyurethane resin A may be a known or commercially available product, or may be one obtained by a known production method.
[0042] The isocyanate group-containing compound may be any of aliphatic diisocyanates, alicyclic diisocyanates, aromatic diisocyanates, araliphatic diisocyanates, etc. These may be used alone or in combination of two or more.
[0043] Examples of the aliphatic diisocyanate include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, 2,6-diisocyanate methyl caproate, and mixtures thereof; examples of the alicyclic diisocyanate include 1, 3-cyclopentane diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (isophorone diisocyanate), 4,4'-methylenebis(cyclohexyl isocyanate), methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 1,4-bis(isocyanatomethyl)cyclohexane or 1,3-bis(isocyanatomethyl)cyclohexane or a mixture thereof (hydrogenated xylylene diisocyanate), or a mixture thereof; as aromatic diisocyanates, for example, m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4- or 2,6-tolylene diisocyanate or a mixture thereof, 4,4'-toluidine diisocyanate, dianisidine diisocyanate, 4,4'-diphenyl ether diisocyanate, etc., or a mixture thereof Examples of aromatic and aliphatic diisocyanates include 1,3- or 1,4-xylylene diisocyanate or mixtures thereof, ω,ω'-diisocyanato-1,4-diethylbenzene, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene or mixtures thereof; examples of triisocyanates include triphenylmethane-4,4',4"-triisocyanate, 1,3,5-triisocyanatobenzene, 2,4,6-triisocyanatotoluene, 1,3,5-triisocyanatohexane, and the like;Examples of polyisocyanate monomers include 4,4'-diphenyldimethylmethane-2,2'-5,5'-tetraisocyanate, and dimers and trimers derived from the above polyisocyanate monomers.
[0044] Examples of the active hydrogen group-containing compound include compounds having an amino group, a hydroxyl group, or a mercapto group as a group having an active hydrogen group. However, from the viewpoints of the reaction rate with the isocyanate group and the mechanical properties of the resulting coating, compounds having a hydroxyl group (particularly polyols) are preferred.
[0045] Examples of the compound having a hydroxyl group include polyester polyol, polyolefin polyol, polyether polyol, polyether ester polyol, polyester amide polyol, acrylic polyol, polycarbonate polyol, polyhydroxyalkane, castor oil, polyurethane polyol, and mixtures thereof.
[0046] Examples of the polyester polyol include polyester polyols obtained by reacting a dibasic acid such as terephthalic acid, isophthalic acid, adipic acid, azelaic acid, or sebacic acid, or a dialkyl ester thereof, or a mixture thereof, with a glycol such as ethylene glycol, propylene glycol, diethylene glycol, butylene glycol, neopentyl glycol, 1,6-hexane glycol, 3-methyl-1,5-pentanediol, 3,3'-dimethylolheptane, polyoxyethylene glycol, polyoxypropylene glycol, or polytetramethylene ether glycol, or a mixture thereof.
[0047] Examples of the polyolefin polyol include polyethylene polyol, polypropylene polyol, polyisobutene polyol, hydrogenated polyisoprene polyol, and hydrogenated polybutadiene polyol.
[0048] Examples of the polyether polyol include polyether polyols obtained by polymerizing an oxirane compound such as ethylene oxide, propylene oxide, butylene oxide, or tetrahydrofuran using a low-molecular-weight polyol such as water, ethylene glycol, propylene glycol, trimethylolpropane, or glycerin as an initiator.
[0049] Examples of the polyetherester polyol include polyetherester polyols obtained by reacting the dibasic acids, their dialkyl esters, or mixtures thereof with the polyether polyols. Examples of the polyesteramide polyol include those obtained by adding an aliphatic diamine having an amino group, such as ethylenediamine, propylenediamine, or hexamethylenediamine, as a raw material to the raw materials for the polyesterification reaction and reacting them.
[0050] Examples of the acrylic polyol include those obtained by copolymerizing a polymerizable monomer having one or more hydroxyl groups in one molecule, such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, etc., with (meth)acrylic acid or an ester thereof. These can be used alone or in combination of two or more.
[0051] Examples of the polycarbonate polyol include those obtained by reacting at least one of ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,9-nonanediol, 1,8-nonanediol, neopentyl glycol, diethylene glycol, dipropylene glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, bisphenol A, and hydrogenated bisphenol A with dimethyl carbonate, diphenyl carbonate, ethylene carbonate, phosgene, etc. These can be used alone or in combination of two or more.
[0052] Examples of the polyhydroxyalkane include liquid rubber obtained by copolymerizing isoprene, butadiene, or butadiene with acrylamide or the like.
[0053] Examples of the polyurethane polyol include polyols having a urethane bond in one molecule, and examples of the polyol include those obtained by reacting a polyether polyol, a polyester polyol, a polyether ester polyol, or the like with an isocyanate group-containing compound having at least two isocyanate groups per molecule, as described below, in a molar ratio (NCO group / OH group) of less than 1.
[0054] In addition to the above-mentioned compounds having a hydroxyl group, glycols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, 1,8-nonanediol, neopentyl glycol, diethylene glycol, dipropylene glycol, 1,4-cyclohexanediol, and 1,4-cyclohexanedimethanol; low molecular weight polyols such as glycerin, trimethylolpropane, and pentaerythritol; and monools such as methanol, ethanol, propanols, butanols, 2-ethylhexanol, lauryl alcohol, and stearyl alcohol may also be mixed. These may be used alone or in combination of two or more.
[0055] Furthermore, it is preferable that an anionic functional group (hydrophilic group) be introduced into the polyurethane resin A. Examples of the anionic functional group include a carboxyl group, a sulfonic acid group, and a phosphate group. Methods for introducing an anionic functional group into the polyurethane resin include a method using a diol having an anionic functional group as a polyol component, and a method using a diol having an anionic functional group as a chain extender. Examples of diols having an anionic functional group include aliphatic carboxylic acids such as glyceric acid, dioxymaleic acid, dioxyfumaric acid, tartaric acid, dimethylolpropionic acid, dimethylolbutanoic acid, 2,2-dimethylolvaleric acid, 2,2-dimethylolpentanoic acid, 4,4-di(hydroxyphenyl)valeric acid, and 4,4-di(hydroxyphenyl)butyric acid, and aromatic carboxylic acids such as 2,6-dioxybenzoic acid. These may be used alone or in combination of two or more.
[0056] The content of polyurethane resin A in the primer layer is not limited, but is usually about 15 to 75 mass %, particularly preferably 15 to 70 mass %, and even more preferably 20 to 60 mass %.
[0057] Polyurethane Resin B The polyurethane resin B may be any resin containing at least one silanol group in the molecule. As the polyurethane resin B, known or commercially available resins can be used, or those obtained by known production methods can also be used.
[0058] The positions where the silanol groups contained in polyurethane resin B are present (bonded) are not particularly limited, and they may be present (bonded) at both ends, either end, or any position in the middle of the polyurethane resin.
[0059] Furthermore, it is preferable that an anionic functional group (hydrophilic group) be introduced into the polyurethane resin B. Examples of the anionic functional group include a carboxyl group, a sulfonic acid group, and a phosphate group. Methods for introducing an anionic functional group into the polyurethane resin include using a diol having an anionic functional group as a polyol component, or using a diol having an anionic functional group as a chain extender. Examples of diols having an anionic functional group include aliphatic carboxylic acids such as glyceric acid, dioxymaleic acid, dioxyfumaric acid, tartaric acid, dimethylolpropionic acid, dimethylolbutanoic acid, 2,2-dimethylolvaleric acid, 2,2-dimethylolpentanoic acid, 4,4-di(hydroxyphenyl)valeric acid, and 4,4-di(hydroxyphenyl)butyric acid, and aromatic carboxylic acids such as 2,6-dioxybenzoic acid. These may be used alone or in combination of two or more.
[0060] Examples of polyurethane resin B include polyurethane resins in which silanol groups have been introduced into the molecule by reacting a polyurethane compound obtained by reacting an isocyanate group-containing compound with an active hydrogen group-containing compound with a compound containing at least one active hydrogen group and at least one hydrolyzable silicon group per molecule (hereinafter referred to as a "hydrolyzable silicon group-containing compound").
[0061] As in the case of anionic functional groups, methods for introducing silanol groups include a method using a diol having a silanol group as a polyol component, a method using a diol having a silanol group as a chain extender, etc. Examples of diols having silanol groups include at least one of silanediol, 1,3-disiloxane-1,3-diol, diphenylsilanediol, etc.
[0062] The isocyanate group-containing compound, active hydrogen group-containing compound, etc. may be the same as those described above for polyurethane resin A.
[0063] The hydrolyzable silicon group-containing compound may be any compound containing at least one active hydrogen group and at least one hydrolyzable silicon group per molecule. Examples of the hydrolyzable silicon group include groups in which a hydrolyzable group is bonded to a silicon atom, which is generated when hydrolyzed in the presence or absence of a silanol condensation catalyst. Examples of the hydrolyzable group include at least one of a hydrogen atom, a halogen atom, an alkoxy group, an acyloxy group, a ketoximate group, an amino group, an amide group, an aminooxy group, a mercapto group, and an alkenyloxy group. Generally, 1 to 3 hydrolyzable groups may be bonded to one silicon atom.
[0064] Specific examples of hydrolyzable silicon group-containing compounds include compounds in which the active hydrogen group is a mercapto group and the hydrolyzable group is an alkoxy group, such as at least one of γ-mercaptopropyltrimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropyltriethoxysilane, γ-mercaptopropylmethyldiethoxysilane, etc. Furthermore, examples of compounds in which the active hydrogen group is an amino group and the hydrolyzable group is an alkoxy group, such as at least one of γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropylmethyldiethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropylmethyldimethoxysilane, γ-aminopropylmethyldiethoxysilane, γ-aminopropyltrimethoxysilane, etc.
[0065] The content of polyurethane resin B in the primer layer is not particularly limited, but is usually about 15 to 75 mass %, particularly preferably 15 to 70 mass %, and even more preferably 20 to 60 mass %.
[0066] The ratio of polyurethane resin A to polyurethane resin B is not limited, but when the total of both is 100 parts by mass, polyurethane resin A should be 25 to 80 parts by mass (preferably 30 to 80 parts by mass, more preferably 40 to 80 parts by mass, particularly preferably 55 to 80 parts by mass, and most preferably 65 to 80 parts by mass), and polyurethane resin B should be 20 to 75 parts by mass (preferably 20 to 70 parts by mass, more preferably 20 to 60 parts by mass, particularly preferably 20 to 45 parts by mass, and most preferably 20 to 35 parts by mass). If the polyurethane resin A in the primer layer exceeds 80 parts by mass, blocking resistance may decrease when the highly adhesive polyamide film is handled in roll form, which may cause problems. Furthermore, if the polyurethane resin B exceeds 75 parts by mass, the optimal amount of silanol crosslinking structure may be exceeded, resulting in localized surface unevenness and a deterioration in print appearance. Furthermore, adhesion to processed materials such as prints and adhesives applied to the primer layer may be reduced.
[0067] In the present invention, polyurethane resin A and polyurethane resin B are used that have different glass transition temperatures (Tg). This allows for good blocking resistance, flexibility, and the like to be obtained in the temperature range between the respective glass transition temperatures (Tg). The glass transition temperature (Tg) of polyurethane resin A is usually preferably about 5 to 50°C. Among these, the lower limit of the Tg of polyurethane resin A is usually preferably 5°C or higher, more preferably 10°C or higher, even more preferably 15°C or higher, and most preferably 20°C or higher. If the Tg is less than 5°C, the blocking resistance of the wound roll film may be reduced. On the other hand, if the Tg exceeds 50°C, the flexibility of the primer layer may be reduced, and stretchability may be impaired, potentially damaging the appearance of the polyamide film.
[0068] The glass transition temperature (Tg) of polyurethane resin B is usually preferably 60°C or higher, more preferably 70°C or higher, even more preferably 85°C or higher, and most preferably 100°C or higher. If the Tg is lower than 60°C, the heat resistance of the entire primer layer may be reduced, and blocking resistance may be reduced. The upper limit of the Tg of polyurethane resin B can be set to, for example, about 120°C, but is not limited to this.
[0069] The polyurethane resin A and / or B used in the present invention preferably has a film elongation of 200% or more. If the elongation of polyurethane resin A or B is less than 200%, the cohesive strength of the resin film will be improved, but the flexibility and impact resistance of the film may be reduced, which may result in reduced adhesion to the processed product after processing such as coating or printing of the primer layer.
[0070] The polyurethane resins A and / or B used in the present invention preferably have a tensile strength of 20 MPa or more, particularly 25 MPa or more, and even more preferably 30 MPa or more. If the tensile strength of polyurethane resins A and B is less than 20 MPa, the adhesion between the primer layer and the processed material after processing such as coating or printing and before hot water treatment is improved, but the heat resistance of the primer layer may be reduced. Therefore, when the primer layer is processed such as coating or printing, the adhesion between the primer layer and the processed material after hot water treatment is likely to be significantly impaired. Furthermore, the cohesive strength of the resin film may be reduced, which may result in reduced blocking resistance.
[0071] Taking all the above points into consideration, in the present invention, it is particularly preferable that polyurethane resin A has a film elongation of 300% or more and a tensile strength of 20 to 50 MPa, and polyurethane resin B has a film elongation of 200% or more and a tensile strength of 40 to 60 MPa.
[0072] In the film of the present invention, other additives may be contained in the primer layer to the extent that the effects of the present invention are not impaired, however, it is preferable that a small amount or no curing agent (crosslinking agent) is contained for the above-mentioned reasons, and therefore the amount of the curing agent (crosslinking agent) in the primer layer is 0.1 mass % or less.
[0073] In particular, a lubricant can be blended to impart higher blocking resistance to the primer layer. For example, when the lubricant is particulate, a lubricant with an average particle size of 5 to 300 nm (particularly 10 to 200 nm) can be used. The content is not limited, but typically ranges from 0 to 10% by mass in the primer layer. Therefore, the content can be, for example, 0.1 to 10% by mass. From the viewpoint of improving blocking resistance and transparency, the content can also be, for example, 0.1 to 5% by mass, preferably 0.3 to 3% by mass, and more preferably 0.5 to 2% by mass.
[0074] The lubricant may be at least one of an organic lubricant and an inorganic lubricant. Examples of the inorganic lubricant include at least one of clay, talc, calcium carbonate, magnesium carbonate, zinc carbonate, wollastonite, silica, alumina, calcium oxide, magnesium oxide, calcium silicate, sodium aluminate, calcium aluminate, magnesium aluminosilicate, glass balloons, carbon black, zinc oxide, antimony trioxide, zeolite, hydrotalcite, layered silicate, sodium silicate, aluminum hydroxide, iron oxide, zirconium oxide, barium sulfate, titanium oxide, and carbon black. Examples of the organic lubricant include at least one of an acrylic crosslinked polymer, a styrene crosslinked polymer, a phenolic resin, a nylon resin, polyethylene wax, and ethylene bisstearamide.
[0075] In the film of the present invention, the total amount of volatile base components generated from the primer layer is preferably 0.50 ppm or less, and more preferably 0.20 ppm or less. If the volatile base components remain in the primer layer at more than 0.50 ppm, the water resistance of the primer layer may be reduced, and when the primer layer is subjected to processing such as coating or printing, the adhesion to the processed material upon contact with water may be reduced. In addition, the effect of improving safety when the highly adhesive polyamide film is used as a packaging material for food, etc., is likely to be impaired.
[0076] The thickness of the primer layer (thickness after stretching) is not limited, but can typically be about 0.025 to 0.250 μm, with 0.050 to 0.120 μm being particularly preferred. If the thickness is less than 0.025 μm, it becomes difficult to form a uniform, defect-free coating on the film. As a result, when the primer layer is subjected to processing such as coating or printing, adhesion to the processed material after hot water treatment such as boiling or retorting may be reduced. On the other hand, if the thickness exceeds 0.250 μm, water resistance may be reduced. Furthermore, since the terminal groups are more likely to bleed out to the surface, blocking properties may be reduced and the amount of volatile base components remaining in the primer layer may increase. Furthermore, further improvement in adhesion is minimal, which may be economically inefficient.
[0077] The thickness of the film of the present invention is not particularly limited, but is usually about 3 to 50 μm, and preferably 10 to 25 μm. The film of the present invention is preferably a stretched film, and more preferably a biaxially stretched film (a film biaxially oriented and crystallized).
[0078] The film of the present invention has excellent blocking resistance. Therefore, when two primer layers are superposed on each other and a load of 10 kg / cm is applied and the film is left in a 40°C environment for one week, the adhesion strength is preferably 40 g / 15 mm or less, more preferably 30 g / 15 mm or less, even more preferably 20 g / 15 mm or less, particularly preferably 15 g / 15 mm or less, and most preferably 10 g / 15 mm or less. Furthermore, when two primer layers are superposed on each other and a load of 10 kg / cm is applied and the film is left in a 40°C environment for one week, the adhesion strength is preferably 10 g / 15 mm or less, more preferably 5 g / 15 mm or less, and particularly preferably 3 g / 15 mm or less. The lower limit of blocking resistance is not particularly limited, but in all of the above cases, it is usually about 1 g / 15 mm.
[0079] Furthermore, the film of the present invention has excellent printability. Therefore, the 2.5 mm halftone print of 50% gradation printed on the primer layer 2 When the areas of the 300 halftone dots in the area are measured at any 10 locations in the TD direction of the print film, the minimum to maximum area ratio (average of the 20 smallest areas / average of the 20 largest areas) is preferably in the range of 0.8 to 1, more preferably in the range of 0.85 to 1, and most preferably in the range of 0.9 to 1. If it is in this range, printing unevenness will be minimal and a uniform print state will be obtained.
[0080] The film of the present invention also has good transparency, so that print visibility is also good. In this case, the haze value of the film of the present invention is usually preferably 8% or less, more preferably 7% or less, and most preferably 6% or less. The lower limit of the haze is not particularly limited, but is usually about 1%. As described above, the film of the present invention has excellent blocking resistance, so that even when a lubricant is used, a relatively small amount is sufficient. This makes it possible to simultaneously achieve excellent blocking resistance and high transparency.
[0081] The highly adhesive polyamide film of the present invention exhibits excellent adhesion to processed materials, such as paints and inks, when the surface of its primer layer is subjected to various secondary processing treatments, such as painting and ink printing, and also exhibits excellent adhesion to sealant films due to the presence of a laminating adhesive layer. Therefore, it can be used as a laminated product subjected to secondary processing, such as laminating a sealant film, and is highly useful as a base film for packaging, general industrial use, etc. Furthermore, since it maintains excellent adhesion even after hot water treatments such as boiling and retorting, and also has excellent printability, it is particularly suitable for use in the field of food packaging.
[0082] 2. Method for Producing Highly Adhesive Polyamide Film The method for producing the film of the present invention is not limited, but can be suitably carried out particularly by the following first method or second method.
[0083] (A) First Method The first method is a method for producing an easily adhesive polyamide film, and includes the following steps: (1) applying an aqueous coating agent containing a polyurethane resin A that does not have silanol groups and a polyurethane resin B that has silanol groups to at least one surface of an unstretched polyamide film (coating step); and (2) biaxially stretching the polyamide film coated with the aqueous coating agent, followed by heat treatment (stretching step).
[0084] Coating Step In the coating step, an aqueous coating agent containing a polyurethane resin A having no silanol groups and a polyurethane resin B having silanol groups is applied to at least one surface of an unstretched polyamide film.
[0085] The unstretched polyamide film described above will ultimately become the polyamide substrate film of the present invention. Therefore, its composition and the like can be those described above in "1. Highly Adhesive Polyamide Film." The unstretched polyamide film can be produced by molding a melt-kneaded product containing a polyamide resin into a sheet. The melt-kneaded product itself can be prepared according to a known method. For example, raw materials containing a polyamide resin are charged into an extruder equipped with a heating device, heated to a predetermined temperature to melt the material, and then extruded through a T-die and cooled and solidified using a casting drum or the like to obtain an unstretched sheet, which is a sheet-shaped molded product. The average thickness of the unstretched sheet in this case can be appropriately set depending on the final thickness and the like, and can be, for example, about 15 to 250 μm, or about 50 to 235 μm, but is not limited thereto.
[0086] The aqueous coating agent can be prepared by dispersing polyurethane resin A, polyurethane resin B, etc. in water. In particular, when polyurethane resin A and polyurethane resin B are anionic polyurethane resins, it is desirable to use a volatile base to disperse them in water. The volatile base is not particularly limited, and examples thereof include at least one of ammonia, methylamine, ethylamine, dimethylamine, diethylamine, triethylamine, morpholine, ethanolamine, etc. Among these, triethylamine is more preferred because it provides good liquid stability to the water-dispersed polyurethane resin and has a relatively low boiling point, resulting in a small amount remaining in the primer layer.
[0087] A surfactant may also be added to the aqueous coating to improve the coating properties when applying the coating to the substrate film. Such surfactants can promote wetting of the aqueous coating onto the substrate film. Examples include anionic surfactants such as polyethylene alkyl phenyl ether, polyoxyethylene-fatty acid ester, glycerin fatty acid ester, fatty acid metal soap, alkyl sulfate, alkyl sulfonate, and alkyl sulfosuccinate, and nonionic surfactants such as acetylene glycol. These surfactants can be used alone or in combination. The surfactant content is not limited, but is preferably 0.01 to 1% by mass in the aqueous coating. If the surfactant content exceeds 1% by mass, the surfactant may bleed out or remain in the primer layer, potentially reducing adhesion after hot water treatment such as boiling or retorting. For this reason, it is preferable that the surfactant used be one that volatilizes during heat treatment in the manufacturing process of the highly adhesive polyamide film.
[0088] As the aqueous coating agent, known or commercially available water-dispersible polyurethane resins (particularly anionic water-dispersible polyurethane resins) can also be used. Examples of the water-dispersible polyurethane resin A include those with the product names "HYDRAN ADS-110," "HYDRAN ADS-120," "HYDRAN KU-400SF," "HYDRAN HW-311," "HYDRAN HW-312B," "HYDRAN HW-333," "HYDRAN AP-20," "HYDRAN AP-201," "HYDRAN AP-80," "HYDRAN APX-101H," and "HYDRAN AP-60LM" (all manufactured by DIC Corporation), and those with the product name "SUPERFLEX 107" (all manufactured by DIC Corporation). M," "Superflex 150," "Superflex 150HS," "Superflex 410," "Superflex 420NS," "Superflex 460," "Superflex 460S," "Superflex 700," "Superflex 750," and "Superflex 840" (all manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.); product names "Takelac W-6010," "Takelac W-6020," "Takelac W-511," and "Takelac W-5030" (all manufactured by Mitsui Chemicals, Inc.); and product names "NeoRez R9679," "NeoRez R9637," "NeoRez R966," and "NeoRez R972" (all manufactured by DSM). Examples of the water-dispersible polyurethane resin B include products under the names "Takelac WS-4000," "Takelac WS-4022," "Takelac WS-5000," "Takelac WS-5100," and "Takelac WS-6010" (all manufactured by Mitsui Chemicals, Inc.).
[0089] The solids concentration of the polyurethane resin in the aqueous coating is not limited and can be changed as appropriate, for example, depending on the specifications of the coating equipment and drying / heating equipment. In this case, a solution that is too dilute may require a long drying process. On the other hand, if the solids concentration is too high, it may be difficult to obtain a uniform coating and may also hinder coatability. From this perspective, it is usually preferable that the solids concentration in the aqueous coating be in the range of about 3 to 35% by mass.
[0090] The method for applying the aqueous coating material to the polyamide film is not particularly limited, and examples thereof include conventional methods such as gravure roll coating, reverse roll coating, wire bar coating, and air knife coating.
[0091] After the aqueous coating material is applied, a drying step can be carried out as necessary. The drying method can be either natural drying or heat drying, but a method of drying by heating at, for example, 100 to 180°C can be preferably used.
[0092] In the stretching process, the polyamide film coated with the aqueous coating agent is biaxially stretched and then heat-treated. More specifically, in the first method, an aqueous coating agent containing an anionic water-dispersible polyurethane resin as a main component is applied to at least one side of an unstretched polyamide substrate film to form a coating film, and then the unstretched polyamide film is biaxially stretched together with the coating film, followed by heat treatment to biaxially orient the crystals of the polyamide film.
[0093] In the first method, simultaneous biaxial stretching can be suitably employed as the stretching method. The stretching temperature is usually about 70 to 250°C, and preferably 100 to 230°C. The stretching ratio can be appropriately set depending on, for example, the application, desired physical properties, etc., and can be, for example, about 2 to 4 times in the MD direction and about 2 to 4 times in the TD direction, but is not limited thereto.
[0094] After stretching, a heat treatment is carried out. For example, a film that has been stretched while both ends in the width direction are held can be suitably heat-treated (i.e., heat-set) while both ends in the width direction are still held.
[0095] In the manufacturing method of the present invention, the heat setting temperature is usually preferably 180 to 250°C, and more preferably 210 to 230°C. If the heat setting temperature is less than 180°C, the thermal dimensional stability of the stretched and oriented film will be high, and the amount of volatile base components remaining in the primer layer will be large. As a result, the adhesion of the primer layer to the processed material when wetted with water, which is the objective of the present invention, is likely to decrease. Furthermore, if the heat setting temperature exceeds 250°C, the temperature will be above the melting point of the polyamide resin, and the desired stretched film may not be obtained.
[0096] (B) Second Method The second method is a method for producing an easily adhesive polyamide film, and includes the following steps: (1) uniaxially stretching an unstretched polyamide film in a first direction (first stretching step); (2) applying an aqueous coating containing a polyurethane resin A that does not have silanol groups and a polyurethane resin B that has silanol groups to at least one side of the uniaxially stretched polyamide film (coating step); and (3) uniaxially stretching the polyamide film coated with the aqueous coating in a second direction perpendicular to the first direction, followed by heat treatment (second stretching step).
[0097] First Stretching Step In the first stretching step, an unstretched polyamide film is uniaxially stretched in a first direction. More specifically, the unstretched polyamide film is stretched in the first direction by passing it through a group of rollers heated to 45 to 80°C (preferably 50 to 60°C) and operating at different peripheral speeds. The stretching ratio in this case can be appropriately set depending on, for example, the intended use and desired physical properties, and can be, for example, 2 to 4 times in the MD or TD direction, but is not limited thereto. The unstretched polyamide film will ultimately become the polyamide substrate film of the film of the present invention. Therefore, its composition, etc., can be as described above. The unstretched polyamide film can be produced in the same manner as in the first method.
[0098] In the coating step, at least one surface of the uniaxially stretched polyamide film is coated with an aqueous coating agent containing a polyurethane resin A having no silanol groups and a polyurethane resin B having silanol groups. The aqueous coating agent and coating conditions may be the same as those in the first method.
[0099] Second Stretching Step In the second stretching step, the polyamide substrate film coated with the aqueous coating agent is uniaxially stretched in a second direction perpendicular to the first direction, and then heat-treated.
[0100] The film is gripped at both widthwise ends and stretched in the second direction at a temperature of 70 to 150° C. (preferably 80 to 120° C.) The stretching ratio in this case can be appropriately set depending on, for example, the application, desired physical properties, etc., and can be, for example, about 2 to 4 times in the TD or MD direction, but is not limited thereto.
[0101] The stretching temperature of the sequential biaxial stretching method employed in the second method is lower than that of the simultaneous biaxial stretching method employed in the first method because, if stretching is performed at high temperatures using the sequential biaxial stretching method, the crystallinity of the polyamide film becomes too high, making it impossible to stretch at the required magnification or significantly impairing the physical properties required of the polyamide film.
[0102] The film of the present invention obtained by the first or second method may be subjected to a surface treatment such as a corona discharge treatment or an adhesion-improving treatment, provided that the effects of the present invention are not impaired. Furthermore, for example, an adhesion-improving layer, a barrier coat layer, a printing layer, etc. may be appropriately provided as needed. In particular, by subjecting the surface opposite the primer layer to a corona discharge treatment, the film is suitable for surface printing and can also be suitably used as an intermediate layer in a multilayer laminate.
[0103] 3. Use of Highly Adhesive Polyamide Film The film of the present invention (particularly the biaxially stretched film) obtained as described above has excellent mechanical properties such as tensile elongation, tensile strength, and elastic modulus, which are typical of polyamide resin films, as well as excellent transparency, color tone, wettability, printability, and the like, and is therefore particularly suitable for use as a packaging material.
[0104] The film of the present invention can be used alone or in the form of a laminate in which it is laminated with other layers.
[0105] The other layers are not limited to, and may include, for example, a barrier layer, a printed layer, a laminating adhesive layer, a heat-sealing layer, a resin film, etc., as needed. In particular, the present invention also encompasses a laminate (laminating body of the present invention) in which at least a laminating adhesive layer and a heat-sealing layer are laminated in this order on the primer layer of the film of the present invention, either directly or via a printed layer. For example, as shown in FIG. 2 , a primer layer 12 is formed on one side of a polyamide substrate film 11, a printed layer 13 is laminated on the primer layer, and a laminating adhesive layer 14 and a heat-sealing layer 15 are further formed on the printed layer. The laminating adhesive layer or heat-sealing layer may be a resin layer containing, for example, a polyolefin such as polyethylene or polypropylene. These may be known or commercially available materials. In the present invention, such a laminate including additional layers is also encompassed in the laminate of the present invention.
[0106] For example, a laminate may be formed by subjecting the surface of the film of the present invention opposite to the primer layer to a corona discharge treatment, and then laminating an adhesive layer and a resin film in this order, either directly or via a printed layer. Specifically, (a) polyester resin film / laminating adhesive layer / polyamide substrate film / primer layer / laminating adhesive layer / heat seal layer, (b) polyester resin film / printing layer / laminating adhesive layer / polyamide substrate film / primer layer / laminating adhesive layer / heat seal layer, (c) polyester resin film / laminating adhesive layer / polyamide substrate film / primer layer / printing layer / laminating adhesive layer / heat seal layer, (d) polyamide resin film / laminating adhesive layer / polyamide substrate film / primer layer / laminating adhesive layer / heat seal layer, (e) polyamide resin film / printing layer / laminating adhesive layer / polyamide substrate film / primer layer / laminating adhesive layer / heat seal layer, (f) polypropylene resin film / laminating adhesive layer / polyamide substrate film / primer layer / laminating adhesive layer / heat seal layer, Examples of the film include, but are not limited to, (g) polypropylene resin film / printed layer / laminating adhesive layer / polyamide substrate film / primer layer / laminating adhesive layer / heat seal layer, (h) polypropylene resin film / laminating adhesive layer / polyamide substrate film / primer layer / printed layer / laminating adhesive layer / heat seal layer. Among these examples, the "polyamide substrate film / primer layer" corresponds to the film of the present invention. Specific examples of each layer are shown below.
[0107] The barrier layer is a layer for blocking, for example, air, moisture, etc. Examples of the barrier layer that can be used include aluminum foil, a vapor-deposited layer of aluminum, silicon oxide, etc., a polyvinylidene chloride (PVDC) coating, polycarboxylic acids, and a composite layer of a hydrogen-bonding resin and an inorganic layered compound.
[0108] The printed layer is a layer on which, for example, letters, designs, etc. are printed. The ink used to form the printed layer is not particularly limited. Examples include toluene-containing ink, non-toluene ink, and water-based ink. From an environmental perspective, at least one of non-toluene ink, water-based ink, etc. is preferred.
[0109] The adhesive for forming the laminating adhesive layer can be a known or commercially available adhesive. Examples include isocyanate-based, polyurethane-based, polyester-based, polyethyleneimine-based, polybutadiene-based, polyolefin-based, and alkyl titanate-based adhesives. Among these, at least one type of adhesive such as an isocyanate-based, polyurethane-based, or polyester-based adhesive is preferred from the viewpoints of adhesion, heat resistance, water resistance, and the like.
[0110] The heat seal layer is not particularly limited as long as it has heat sealability, and for example, at least one of low density polyethylene, linear low density polyethylene, high density polyethylene, ethylene-vinyl acetate copolymer, polypropylene, ionomer resin, etc. can be used.
[0111] The resin film is not limited to, but may be at least one of, for example, a polyester resin film, a polyamide resin film, a polypropylene resin film, and the like.
[0112] The laminate of the present invention can be produced by a known method such as dry lamination or extrusion lamination, which includes a step of laminating a laminating adhesive layer or a heat seal layer on a primer layer or a printed layer formed thereon as needed.
[0113] The laminate of the present invention can also be used as a packaging bag (bag body) by, for example, heat-sealing opposing laminate adhesive layers or heat-sealing layers together. The bag body can be in any form, such as a two-sided bag, a three-sided bag, a palm-seam bag, a gusset bag, a side-seal bag, a stand-up bag, or a stand-up zipper bag.
[0114] There are no limitations on the items to be packaged (contents), and the material can be used for a wide range of purposes, including packaging foods and beverages, pharmaceuticals, cosmetics, chemicals, and miscellaneous goods.
[0115] In the laminate of the present invention, regardless of whether a printed layer is present, the laminate strength (X) of the primer layer before and after hot water treatment in normal water exposure is preferably 3.0 N / cm or more, more preferably 3.5 N / cm or more, even more preferably 4.0 N / cm or more, particularly preferably 4.5 N / cm or more, and most preferably 5.0 N / cm or more. Furthermore, the ratio (Y / X) of the laminate strength (Y) in normal water exposure after hot water treatment at 120°C for 30 minutes to the laminate strength (X) in normal water exposure is preferably 0.5 or more. The ratio (Y / X) is preferably 0.6 or more, more preferably 0.7 or more, particularly preferably 0.8 or more, and most preferably 0.9 or more. If the ratio (Y / X) is less than 0.5, for example, when a packaging bag is formed from the laminate, filled with contents, sealed, and then further subjected to hot water treatment, bag breakage, opening defects, etc. are likely to occur.
[0116] The features of the present invention will be described in more detail below with reference to examples and comparative examples. However, the scope of the present invention is not limited to these examples. The urethane emulsions (water-dispersed polyurethane resins) used in the examples and comparative examples are all anionic polyurethane water dispersions.
[0117] 1. Regarding polyurethane resins used in the examples and comparative examples <Polyurethane resin A not having silanol groups> AP-201: Water-dispersible polyurethane resin "HYDRAN AP-201" manufactured by DIC Corporation AP-80: Water-dispersible polyurethane resin "HYDRAN AP-80" manufactured by DIC Corporation Polyurethane resin A-1: Polyurethane resin obtained by the following method Into a reaction vessel equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, 166.1 parts by mass of terephthalic acid, 36.5 parts by mass of adipic acid, 46.6 parts by mass of ethylene glycol, 67.6 parts by mass of 1,4-butanediol, and 0.1 parts by mass of dibutyltin oxide were charged while introducing nitrogen gas, and the mixture was subjected to a polycondensation reaction at 230°C for 6 hours until the acid value reached 1 or less, thereby obtaining a polyester polyol having a number average molecular weight of 1,500, an acid value of 0.1, and a hydroxyl value of 72.9. 300 parts by mass of the obtained polyester polyol was dehydrated by heating at 100°C under reduced pressure. Next, 144.2 parts by mass of methyl ethyl ketone was supplied to the reaction vessel adjusted to 80°C, followed by 26.8 parts by mass of 2,2-dimethylolpropionic acid and 18.0 parts by mass of 1,4-butanediol, and then 104.5 parts by mass of tolylene diisocyanate, and the mixture was reacted at 75°C for 8 hours. Next, 20.2 parts by mass of triethylamine was supplied to the reaction vessel adjusted to 50°C and neutralized, and then 300 parts by mass of water was supplied and mixed. Methyl ethyl ketone was removed from the mixture obtained above under reduced pressure, and water was then supplied to obtain polyurethane resin A-1 with a solids concentration of 25% by mass. Polyurethane resin A-2: polyurethane resin obtained by the following method Polyurethane resin A-2 was obtained in the same manner as for polyurethane resin A-1, except that 166.1 parts by mass of terephthalic acid and 219.2 parts by mass of adipic acid were used.Polyurethane resin A-3: Polyurethane resin obtained by the following method. While introducing nitrogen gas into a reaction vessel equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, 120.97 parts by mass of methyl ethyl ketone was supplied and the temperature was adjusted to 70°C. 26.8 parts by mass of 2,2-dimethylolpropionic acid, 106.4 parts by mass of 1,6-hexanediol, 13.4 parts by mass of trimethylolpropane, and 319.9 parts by mass of meta-xylylene diisocyanate were supplied and reacted at 70°C. It was confirmed that the reaction solution reached the predetermined amine equivalent. Next, 20.2 parts by mass of triethylamine was added to the reaction vessel adjusted to 35°C. Next, 1,440 parts by mass of water was added to a reaction vessel equipped with a homodisper capable of high-speed stirring, and the temperature was adjusted to 15°C. The mixture was stirred for 2,000 min. -1 While stirring and mixing at 40°C, the mixture obtained above was added and dispersed in water, and an amine aqueous solution prepared by mixing 41.7 parts by mass of 2-[(2-aminoethyl)amino]ethanol and 180 parts by mass of water was added, and a chain extension reaction was carried out. Subsequently, methyl ethyl ketone and a portion of the water were removed under reduced pressure to obtain a polyurethane resin A-3 having a solids concentration of 25% by mass. <Polyurethane Resin B Having Silanol Groups> WS-4022: "Takelac WS-4022" manufactured by Mitsui Chemicals, Inc. WS-5000: "Takelac WS-5000" manufactured by Mitsui Chemicals, Inc. Polyurethane Resin B-1: Polyurethane resin obtained by the following method Polyurethane Resin B-1 was obtained in the same manner as Polyurethane Resin A-3 above, except that an amine aqueous solution prepared by mixing 4.4 parts by mass of N-2-(aminoethyl)-3-aminopropyltrimethoxysilane and 18 parts by mass of water was added during the chain extension reaction.
[0118] 2. Examples and Comparative Examples [Example 1] (1) Preparation of Aqueous Coating (Aqueous Dispersion) DIC Corporation's water-dispersible polyurethane resin "Hydran AP-201" and Mitsui Chemicals' "Takelac WS-4022" were mixed in a 1:1 (solids mass ratio), and silica particles with an average particle size of 12 nm were added to the mixture to account for 0.25 mass% of the total. The mixture was then diluted with ion-exchanged water to prepare an aqueous coating with a solids mass of 10 mass%. (2) Preparation of Unstretched Polyamide Film Nylon 6 (relative viscosity: 3.03) containing 0.1 mass% of silica with an average particle size of 1.0 μm was extruded into a sheet from a T-die equipped extruder (75 mm diameter, L / D = 45, slow compression type single screw) at 270°C. The extruded sheet was then placed in close contact with a casting roll whose surface temperature was adjusted to 18°C and rapidly cooled to obtain an unstretched polyamide film with a thickness of 150 μm. This unstretched polyamide film was introduced into a water bath and adjusted to a water absorption of 4.0% by mass. (3) Production of Easy-Adhesion Polyamide Film The above-mentioned aqueous coating agent was applied to the water-absorbed unstretched polyamide film by air knife coating, and then dried in a dryer at 60°C for 10 seconds. The coated unstretched film was introduced into a simultaneous biaxial stretching machine and simultaneously biaxially stretched to 3.3 times in the longitudinal direction and 3.0 times in the transverse direction under conditions of a preheating temperature of 225°C, a preheating time of 5 seconds, a stretching temperature of 195°C, and a stretching time of 3 seconds. Next, a heat treatment was performed under conditions of a heat setting temperature of 215°C and a heat setting time of 5 seconds to produce an easy-adhesion polyamide film. The thickness of the polyamide substrate film in the obtained easy-adhesion polyamide film was 15 μm, and the thickness of the primer layer was 0.060 μm.
[0119] Examples 2 to 4 Highly adhesive polyamide films were prepared in the same manner as in Example 1, except that the mixing ratio of the water-based polyurethane resin used in the water-based coating agent was changed as shown in Table 1.
[0120] [Example 5] An easily adhesive polyamide film was produced in the same manner as in Example 1, except that the mixing ratio of the aqueous polyurethane resin used in the aqueous coating was changed as shown in Table 1, and the average particle size of the lubricant added to the aqueous coating was changed to 20 nm and the amount added was changed to 0.25 mass%.
[0121] [Example 6] An easily adhesive polyamide film was produced in the same manner as in Example 1, except that the polyamide resin used was a polyamide resin obtained by chemically depolymerizing film scraps or defective products generated during the production of polyamide 6 resin films and resin scraps (resin waste) containing oligomers and the like generated during the polymerization of polyamide 6 resin, and using the resulting monomer as the polymerization raw material.
[0122] [Examples 7 to 9] Easy-adhesion polyamide films were produced in the same manner as in Example 1, except that the type of aqueous polyurethane resin (A) used in the aqueous coating was changed to "Hydran AP-80" manufactured by DIC Corporation, and the mixing ratio and the amount of lubricant added were changed as shown in Table 1.
[0123] [Example 10] An easily adhesive polyamide film was produced in the same manner as in Example 1, except that the type of aqueous polyurethane resin (B) used in the aqueous coating agent was changed to "Takelac WS-5000" manufactured by Mitsui Chemicals, Inc., and the mixing ratio was changed as shown in Table 1.
[0124] Examples 11 to 14 Highly adhesive polyamide films were prepared in the same manner as in Example 1, except that the type of water-based polyurethane resin used in the water-based coating agent was changed as shown in Table 1.
[0125] Example 15 An easily adhesive polyamide film was produced in the same manner as in Example 1, and then a corona discharge treatment was performed on the surface opposite to the surface on which the primer layer was formed, to produce an easily adhesive polyamide film.
[0126] [Comparative Examples 1 to 11, 16, 18, and 19] Easy-adhesion polyamide films were prepared in the same manner as in Example 1, except that the water-based polyurethane resin used in the water-based coating agent and the average particle size and amount of lubricant added were changed as shown in Table 1.
[0127] Comparative Example 12 An easily adhesive polyamide film was prepared in the same manner as in Example 1, except that the aqueous polyurethane resin used in the aqueous coating was changed to only "Hydran AP-201" manufactured by DIC Corporation, and an easily adhesive polyamide film was prepared in which a corona discharge treatment was performed on the surface opposite to the surface on which the primer layer was formed.
[0128] Comparative Examples 13 and 14 The aqueous polyurethane resin used in the aqueous coating was changed as shown in Table 1, and 4 parts by mass of a crosslinking agent carbodiimide (V-12-S manufactured by Nisshinbo) was added per 100 parts by mass of the polyurethane resin. Other than this, the average particle size and amount of the lubricant added were changed as shown in Table 1, and easy-adhesion polyamide films were produced in the same manner as in Example 1.
[0129] Comparative Example 15 Hydran KU-400SF was used as the aqueous polyurethane resin for the aqueous coating agent, and 6 parts by mass of melamine (Beckamin APM manufactured by DIC Corporation) was added as a crosslinking agent to 100 parts by mass of the polyurethane resin. Other than this, the average particle size and amount of the lubricant were changed as in Example 1, as shown in Table 1, and an easily adhesive polyamide film was produced in the same manner as in Example 1.
[0130] Comparative Example 17 A polyamide film was prepared in the same manner as in Example 1, except that no aqueous coating agent was used, and one side of the polyamide film was subjected to a corona discharge treatment.
[0131] [Test Example 1] The properties of the films obtained in Examples 1 to 15 and Comparative Examples 1 to 19 were investigated. The results are shown in Tables 1 and 2, along with the composition, properties, etc. of the aqueous coating agent (polyurethane resin) used to form the primer layer.
[0132] (1) Polyurethane Resin (1-1) Tensile Strength (MPa) and Elongation (%) Each polyurethane resin (dispersion) (Tables 1 to 2) used in the aqueous coating agent for forming the primer layer was cast onto a glass plate, dried at room temperature (about 20°C) for 24 hours, and then heat-treated at 150°C for 10 minutes to produce a film with a thickness of 50 μm. This film was cut into 5 mm wide strips, and the tensile strength and elongation of the test pieces were measured using a tensile tester (Shimadzu Corporation, AGS-100B) at a pulling rate of 300 mm / min.
[0133] (1-2) Glass transition temperature Tg (°C) Using a differential scanning calorimeter (Diamond DSC) manufactured by PerkinElmer, 10 mg of the film used in (1-1) above was heated once to Tg+20°C at 20°C / min, cooled, and then measured again at a heating rate of 5°C / min from -30°C to 250°C. The midpoint between the start temperature and end temperature at which the baseline of the secondary heating curve shifts was taken as the glass transition temperature.
[0134] (2) Film (2-1) Wet Tension (mN / m) In accordance with Japanese Industrial Standard JIS K6768, the primer layer-formed surface of the highly adhesive polyamide film obtained in each Example and Comparative Example was measured using a wet tension test mixture No. 36.0 to 54.0 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).
[0135] (2-2) Thickness of Primer Layer (μm) Using a JEOL "JEM-1230 TEM," the highly adhesive polyamide films obtained in each Example and Comparative Example were cut to an appropriate size, immersed in an aqueous phosphotungstic acid solution (PTA solution) for 3 hours, and then embedded in a visible light curing resin. Sections 80 nm thick were taken using an ultramicrotome, and RuO 4 After 1H gas-phase staining with the solution, transmission measurements were carried out at an accelerating voltage of 100 kV.
[0136] (2-3) Haze Using a haze meter "NDH4000" manufactured by Nippon Denshoku Co., Ltd., the haze was measured at the center of the film in the TD direction in accordance with Japanese Industrial Standard JIS K7136.
[0137] (2-4) Blocking Resistance The highly adhesive polyamide films obtained in each Example and Comparative Example were cut into A4 size pieces, and either (a) the primer layers were stacked together or (b) the primer layers were stacked on the opposite side of the primer layers. A load of 10 kg / cm was applied, and the pieces were left for one week in an atmosphere of 40°C and 70% RH. However, in Comparative Example 13, either (a) the corona discharge-treated surfaces were stacked together or (b) the corona discharge-treated surfaces were stacked on the opposite side of the corona discharge-treated surfaces. The pieces were then cut into 15 mm wide strips, and the peel force (g / 15 mm) required to peel the two sheets was measured using a tensile tester (Shimadzu Corporation, AGS-100B) using the T-type (90°) method at a tensile speed of 300 mm / min. This was used as an index of blocking resistance. A smaller value indicates better blocking resistance.
[0138] (2-5) Half-tone Printing Evaluation [Printing Process] (a) Printing Ink 1 Rio Alpha R39 Indigo (manufactured by TOYOINK) was mixed with diluent NKFS102 (manufactured by TOYOINK) and the viscosity (23°C) was adjusted to 15 seconds on a Zahn cup #3 scale. A printing roll film was prepared by slitting the film at positions 500 mm to the left and right of the center in the TD direction. The ink was applied to the primer layer of the film using a gravure printing cylinder, then dried at 50°C for 10 seconds and wound up to produce a printed film as shown in Figure 3. For Comparative Example 14, however, the ink was applied to the corona discharge-treated surface. The cylinder was helioengraved with 175 lines (175 halftone dots per inch) in the MD direction in the following order of gradation: 40%, 50%, 60%, 70%, 80%, 90%, and 100%. The depths of each tone were 10.0 μm, 12.5 μm, 15.0 μm, 17.5 μm, 20.0 μm, 22.5 μm, and 32.0 μm, respectively. The printing length in the MD direction for each tone was 60 mm, and the printing width in the TD direction was 0.8 m. Rio Alpha R39 Indigo is primarily composed of 10% pigment, 15% synthetic resin, 2.5% silica, 30% ethyl acetate, 15% isopropyl alcohol, 10% propyl acetate, 10% propylene glycol monomethyl ether, and 5% n-propyl alcohol by weight. The diluent NKFS102 is primarily composed of 50% ethyl acetate, 35% propyl acetate, 10% isopropyl alcohol, and 5% n-propyl alcohol by weight. (b) Printing Ink 2 A printed film was prepared in the same manner as above, except that Bellflora R Indigo 800MK (manufactured by Sakata Inx), an environmentally friendly ink containing plant-derived ingredients, was used as printing ink 2, along with the diluent L Solvent 2 (manufactured by Sakata Inx). Bellflora R Indigo 800MK is primarily composed of 45% by mass of n-propyl acetate, 15% by mass of isopropyl alcohol, 7.5% by mass of ethyl acetate, and 2.5% by mass of n-propyl alcohol. L Solvent 2 is primarily composed of 40% by mass of toluene, 40% by mass of methyl ethyl ketone, and 20% by mass of isopropyl alcohol.[Dot area evaluation] A total of 10 measurement points (area 2.5 mm) were measured at 50 mm intervals on a printed film prepared with printing ink 1, starting from a position 250 mm from the edge of a 50% gradation portion. 2 The sample was taken to an observable size (for example, 20 mm in MD direction x 50 mm in TD direction, centered on the measurement point), and observed at 50x magnification using a stereomicroscope (SteREO Discovery.V12 manufactured by ZEISS). 2 The diameters of 300 dots within the rectangle were measured and the area was calculated. If the dots were elliptical, the long and short sides were measured and the area was calculated as an ellipse. Of all the dot areas, the average of the smallest 20 dots / the average of the largest 20 dots was calculated. A larger value (closer to 1) indicates less uneven printing. [Evaluation of Print Appearance] Each gradation area of the produced printed film was visually inspected and rated on a four-point scale according to the following criteria. For practical purposes, a rating of "△" to "◎" is desirable. (Evaluation criteria) ◎: Very good (uniform shading in all gradation areas) ○: Good (uneven printing observed in some low gradation areas) △: Somewhat poor (unevenness observed in some parts of all gradation areas) ×: Poor (unevenness observed overall in all gradation areas)
[0139] (2-6) Lamination Strength of Printed Film [Lamination Step] A dry lamination adhesive for retort applications (manufactured by DIC Corporation, product name "DIC Dry LX500 / KR90S") was applied to the printed layer of the printed film prepared using Printing Ink 1 or Printing Ink 2 in (2-5) above, and then dried at 80°C for 10 seconds. The film was then dry-laminated with an unstretched polypropylene film (manufactured by Mitsui Chemicals Tohcello, product name "RXC-21", thickness 50 μm) at a nip pressure of 490 kPa on a metal roll heated to 80°C. After aging for the recommended time, a laminate film was obtained. [Lamination Strength Measurement] A 15 mm wide test piece was cut from the prepared laminate film, and the edge of the test piece was peeled off at the interface between the unstretched polypropylene film and the primer layer of the easy-adhesion polyamide film, and then the film was conditioned in a 23°C, 50% RH atmosphere for 24 hours. In the same atmosphere, the peel strength was measured using a tensile tester (Shimadzu Corporation, "AGS-100B") using the T-type (90°) method at a tensile speed of 300 mm / min. The measurement results were recorded as laminate strength (unit: N / cm). The prepared laminate film was cut into A4 size pieces, made into bags, filled with water, and retorted (120°C, 1.8 atmospheres, 30 minutes). The samples were then sampled and the laminate strength was measured in the same manner as above. In this peel test, based on actual use, a liquid was filled as the contents. Measurements were made while adhering water-soaked absorbent cotton to the peel interface, and the wet laminate strength was measured in a state where the peel interface was wet. Furthermore, for each laminate strength, the ratio (Y / X) of the laminate strength after treatment (Y) to the laminate strength before treatment (X) was calculated. The results are also shown in Table 2.
[0140] (2-7) Air-containing boil test [Lamination process] A dry laminating adhesive (manufactured by Mitsui Chemicals, Inc., product name "Takelac A-620 / Takenate A-65") was applied to the primer layer-formed surface of the easy-to-adhere polyamide film obtained in each Example and Comparative Example, and then dried at 80 ° C. for 10 seconds. The film was then dry-laminated with an unstretched polypropylene film (manufactured by Mitsui Chemicals Tocello, Inc., product name "TUX (HC-E)", thickness 50 μm) at a nip pressure of 490 kPa on a metal roll heated to 80 ° C. After aging for the recommended time, a laminate film was obtained. [Air-containing boil test] The prepared laminate film was three-way sealed to form a bag with a size of 150 mm x 150 mm (seal width 10 mm) under sealing conditions of a temperature of 150 ° C. at the top and 100 ° C. at a pressure of 0.3 MPa for 1 second. The resulting bags were filled with 200 ml of water and 180 ml of air and sealed with an impulse sealer. Ten bags of the produced air-filled packages were boiled at 95°C for 30 minutes, and the number of bags that broke after the boiling process was counted and evaluated according to the following criteria. For practical purposes, an evaluation of "○" or "◎" is desirable. (Evaluation criteria) ◎: Very good (no bags broken) ○: Fairly good (1 bag broken out of 10) △: Fairly poor (2-4 bags broken out of 10) ×: Poor (5 or more bags broken out of 10)
[0141]
[0142]
[0143] As is clear from the results in Tables 1 and 2, Examples 1 to 10 contained an appropriate amount of silanol-containing polyurethane in the primer layer of the adhesive polyamide film, and exhibited excellent transparency, minimal unevenness in the halftone dot area of halftone printing, and excellent blocking properties. Furthermore, the laminated films using the adhesive polyamide films of Examples 1 to 9 exhibited good lamination strength (X) after normal water exposure, and the ratio (Y / X) of the lamination strength after water exposure after hot water treatment (Y) to the lamination strength after normal water exposure (X) was 0.9 or higher, with some samples showing a lamination strength of 1.0 or higher (i.e., greater lamination strength after treatment than before treatment), and also performed well in the aerated boil test.
[0144] In Comparative Examples 1, 2, 5, 9, 10 and 12, the primer layer of the highly adhesive polyamide film did not contain polyurethane having a silanol group, and although there was no problem with halftone printing, blocking properties deteriorated.
[0145] Comparative Examples 3 and 4 are films in which the primer layer of the highly adhesive polyamide film does not contain polyurethane having silanol groups. Although there was no problem with blocking due to the increased amount of lubricant added, the haze value increased.
[0146] In Comparative Examples 6 to 8 and 19, the primer layer of the highly adhesive polyamide film was composed only of a polyurethane resin having silanol groups, but the halftone dot area ratio of the halftone printing was less than 0.8, and a deterioration in the appearance of the print was observed.
[0147] In Comparative Examples 13 to 15, a crosslinking agent having a crosslinking structure other than a silanol group was added to the primer layer of the highly adhesive polyamide film, so that localized unevenness occurred on the surface starting from the crosslinking points during the coating drying and stretching processes, and the dot area ratio when halftone printing was performed was less than 0.8, and a deterioration in the print appearance was observed. Also, the number of broken bags was somewhat high in the air-containing boil test.
[0148] In Comparative Example 16, the primer layer of the highly adhesive polyamide film was composed of a polyurethane resin having silanol groups and a polyurethane resin not having silanol groups, but the polyurethane resin not having silanol groups had a low glass transition temperature, resulting in poor blocking resistance.
[0149] Comparative Example 17 was a polyamide film having no primer layer, and therefore had good blocking resistance and halftone printing, but had low lamination strength and many bags broke in the air-containing boil test.
Claims
1. A polyamide film having a primer layer formed on at least one surface of a polyamide substrate film, characterized in that: (1) the primer layer contains a polyurethane resin A having no silanol groups and a polyurethane resin B having silanol groups; and (2) the glass transition temperatures (Tg) of the polyurethane resin A and the polyurethane resin B are different from each other.
2. The highly adhesive polyamide film according to claim 1, wherein the glass transition temperature (Tg) of the polyurethane resin A is in the range of 5 to 50°C, and the glass transition temperature (Tg) of the polyurethane resin B is in the range of 60°C or higher.
3. The highly adhesive polyamide film according to claim 1, wherein the polyurethane resin A is 25 to 80 parts by mass and the polyurethane B is 20 to 75 parts by mass, when the total of the polyurethane resin A and the polyurethane resin B is 100 parts by mass.
4. The highly adhesive polyamide film according to claim 1, wherein polyurethane resin A has a film elongation of 300% or more and a tensile strength of 20 to 50 MPa, and polyurethane resin B has a film elongation of 200% or more and a tensile strength of 40 to 60 MPa.
5. 2.5 mm of halftone printing 50% gradation part printed on the primer layer 2 2. The highly adhesive polyamide film according to claim 1, wherein, when the areas of 300 halftone dots in the area are measured at any 10 locations in the TD direction of the printed film, the ratio of the minimum to the maximum area (average of the 20 smallest areas / average of the 20 largest areas) is in the range of 0.8 to 1.
6. The highly adhesive polyamide film according to claim 1, wherein the adhesion strength is 40 g / 15 mm or less after one week in an environment of 40°C under a load of 10 kg / cm when the primer layers are stacked together.
7. The highly adhesive polyamide film according to claim 1, having a haze of 8% or less.
8. The highly adhesive polyamide film according to claim 1, which is a biaxially stretched film.
9. A laminate in which at least a laminating adhesive layer and a heat seal layer are laminated in this order directly or via a printed layer on a primer layer of the highly adhesive polyamide film according to any one of claims 1 to 8.
10. A method for producing an easily adhesive polyamide film, comprising: (1) applying an aqueous coating containing a polyurethane resin A that does not have silanol groups and a polyurethane resin B that has silanol groups to at least one side of an unstretched polyamide substrate film; and (2) biaxially stretching the polyamide film to which the aqueous coating has been applied, followed by heat treatment.
11. The method of claim 10, wherein the biaxial stretching is simultaneous biaxial stretching.
12. A method for producing an easily adhesive polyamide film, comprising: (1) a step of uniaxially stretching an unstretched polyamide substrate film in a first direction; (2) a step of applying an aqueous coating agent containing a polyurethane resin A that does not have silanol groups and a polyurethane resin B that has silanol groups to at least one side of the uniaxially stretched polyamide substrate film; and (3) a step of uniaxially stretching the polyamide substrate film to which the aqueous coating agent has been applied in a second direction perpendicular to the first direction, followed by a heat treatment.