Substrate for semiconductor device and method for producing same
Patent Information
- Application Number
- MYPI2025001983
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-09-29
- Publication Date
- 2024-03-29
AI Technical Summary
The existing semiconductor device substrates face challenges with thermal expansion due to high voltage and current applications, leading to potential separation of ceramic substrates and electrodes, requiring enhanced bonding strength between the copper plate and ceramic substrate.
A substrate with a copper plate bonded to a ceramic substrate, where the ceramic substrate is composed of alumina and zirconia, with a Cu existing region depth of 11.0 to 20.0 μm and a CuO-rich copper oxide layer formed through wet oxidation, promoting higher bonding strength by facilitating copper diffusion and reducing thermal stress.
The described configuration significantly improves the bonding strength between the copper plate and ceramic substrate, ensuring reliable performance under thermal stress conditions, as evidenced by increased load per unit width for peeling and optimized Cu mass concentration profiles.
Smart Images

Figure PI2025001983_DRAWING_001 
Figure PI2025001983_DRAWING_002 
Figure PI2025001983_DRAWING_003
Abstract
Description
Substrate for semiconductor device and manufacturing method thereof
[0001] The present invention relates to a substrate for a semiconductor device and a method for manufacturing the same.
[0002] BACKGROUND ART As a substrate for a semiconductor device used in a power transistor module or the like, a DBOC (Direct Bonding of Copper Substrate) substrate having a copper plate on the surface of a ceramic substrate is known (for example, Patent Documents 1 to 3).
[0003] International Publication No. 2022 / 118802
[0004] However, in the substrate for the semiconductor device described above, the application of high voltage and high current to the semiconductor generates heat, which can cause thermal expansion of the components, potentially resulting in separation between the ceramic substrate and the electrodes. Therefore, in order to improve the reliability of the device, high bonding strength is required at the bonding interface between the ceramic substrate and the electrodes.
[0005] The present invention has been made to solve the above problems, and an object of the present invention is to provide a substrate for a semiconductor device and a manufacturing method thereof that can improve the bonding strength between a copper plate and a ceramic substrate.
[0006] Item 1. A substrate for a semiconductor device, comprising: a ceramic substrate; and a copper plate bonded to at least one surface of the ceramic substrate, wherein the ceramic substrate has a Cu-existing region having a Cu-existing depth of 11.0 to 20.0 μm from the bonding interface with the copper plate when the cumulative Cu mass concentration is 90%.
[0007] Item 2. The substrate for a semiconductor device according to Item 1, wherein the ceramic substrate contains alumina, and zirconia or partially stabilized zirconia, and in the Cu-existing region, the content of copper in crystal grains of the zirconia is greater than the content of copper in crystal grains of the alumina.
[0008] Item 3. The substrate for a semiconductor device according to Item 1 or 2, wherein a load per unit width for peeling the copper plate from the ceramic substrate is 5.5 kg / cm or more.
[0009] Item 4. A method for manufacturing a substrate for a semiconductor device, comprising: a step of oxidizing a copper plate by a wet oxidation method; and a step of bonding the copper plate to at least one surface of a ceramic substrate by a direct bonding method, wherein the oxidized copper plate contains CuO and CuO before being bonded to the ceramic substrate, and the CuO-rich copper oxide layer is formed on the surface.
[0010] Item 5. The method for manufacturing a substrate for a semiconductor device according to Item 3 or 4, wherein the Cu presence depth at which an integrated Cu mass concentration of 90% is shown from the bonding interface with the copper plate on each surface of the ceramic substrate is 11.0 to 20.0 μm.
[0011] According to the present invention, the bonding strength between the ceramic substrate and the copper plate can be improved.
[0012] 5(a) is a backscattered electron image near the bonding interface between the copper plate and the ceramic substrate, and FIG. 5(b) is a schematic diagram illustrating a method for segmenting and averaging the EPMA mapping image for profiling the cross section of the substrate for a semiconductor device of Example 1 according to the present invention. 5(b) is a diagram showing the correlation of the mass concentrations of Cu and Al with respect to the depth from the bonding interface in the ceramic substrate direction in the ceramic substrate according to the present invention. 5(c) is a diagram showing the integral of the Cu mass concentration with respect to the depth from the bonding interface in the ceramic substrate direction in the ceramic substrate according to the present invention.
[0013] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A ceramic substrate and a substrate for a semiconductor device using the same according to an embodiment of the present invention will now be described with reference to the accompanying drawings. Fig. 1 is a cross-sectional view of a semiconductor device having a substrate for a semiconductor device according to this embodiment.
[0014] <1. Overview of Semiconductor Device> The semiconductor device according to this embodiment is used as a power module in various electronic devices such as smartphones, personal computers, large home appliances, railways, electric vehicles, power generation (wind power generation, solar power generation, fuel cells, etc.), air conditioners, industrial robots, commercial elevators, home microwave ovens, induction electric rice cookers, and UPS (uninterruptible power supplies).
[0015] As shown in FIG. 1, the semiconductor device 1 according to this embodiment includes a substrate 2 for a semiconductor device, a first bonding material 5, a second bonding material 5', a semiconductor chip 6, bonding wires 7, and a heat sink 8.
[0016] The substrate 2 for a semiconductor device is a so-called DBOC (Direct Bonding of Copper Substrate) substrate, and includes a plate-shaped ceramic substrate 3, which is an insulator, a first copper plate 4 bonded to one surface (top surface) of the ceramic substrate 3, and a second copper plate 4' bonded to the other surface (bottom surface). Details of the ceramic substrate 3 will be described later.
[0017] A transmission circuit is formed on the first copper plate 4. On the other hand, the second copper plate 4' is formed in a flat plate shape.
[0018] A semiconductor chip 6 is bonded to the upper surface of the semiconductor device substrate 2, i.e., to a part of the upper surface of the first copper plate 4, via a first bonding material 5. The semiconductor chip 6 and the first copper plate 4 are also connected by bonding wires 7.
[0019] On the other hand, a heat sink 8 is bonded to the lower surface of the semiconductor device substrate 2, i.e., the lower surface of the second copper plate 4′, via a second bonding material 5′. The heat sink 8 is a known material and can be made of a metal such as copper.
[0020] 2. Structure of Ceramic Substrate Next, the ceramic substrate 3 will be described in detail. The ceramic substrate 3 contains alumina (AlO), zirconia (ZrO), yttria (YO), a glass component, and the remainder. The glass component contains silica (SiO). The contents of the constituent elements of the ceramic substrate 3 will be described below.
[0021] The matrix component of the ceramic substrate 3 is made of alumina. The alumina content is, for example, preferably 75% by mass or more and 90% by mass or less, and more preferably 85% by mass or more and 90% by mass or less.
[0022] The zirconia content is preferably 10% by mass or more and 25% by mass or less, and more preferably 10% by mass or more and 15% by mass or less. A zirconia content of 10% by mass or more can improve the strength of the ceramic substrate 3. It is also thought that this can prevent the linear thermal expansion coefficient of the ceramic substrate 3 from becoming too small, thereby reducing the difference in the linear thermal expansion coefficient between the ceramic substrate 3 and the first and second copper plates 4, 4'. As a result, it is thought that this can reduce thermal stress occurring at the bonding interface, contributing to the prevention of cracks occurring in the ceramic substrate 3 at the bonding interface.
[0023] Furthermore, as will be shown in the examples described later, Cu diffused from the copper plates 4, 4' bonded to the ceramic substrate 3 diffuses into the ceramic substrate 3 preferentially through the zirconia crystal grains rather than through the alumina crystal grains that constitute the matrix component, thereby forming a Cu-containing region. Therefore, when the zirconia content is set as described above, the diffusion of Cu is promoted, and as will be described later, the bonding strength of the copper plates 4, 4' is increased, which is preferable.
[0024] On the other hand, by setting the zirconia content to 25% by mass or less, it is believed that excessive reaction at the bonding interface during copper plate bonding can be suppressed, and the generation of voids at the bonding interface can be suppressed. This is due to the difference in wettability between alumina and zirconia and the Cu-O eutectic liquid phase during copper plate bonding. Furthermore, by setting the zirconia content to 25% by mass or less, it is possible to improve the impedance of the ceramic substrate 3 without increasing the silica content, as will be described later.
[0025] The yttria content is preferably 0.8 mass% or more and 1.9 mass% or less. By setting the content to 0.8 mass% or more, it is thought that the proportion of the monoclinic phase in the zirconia crystal phase can be prevented from becoming excessive, while the proportion of the tetragonal phase can be increased. As a result, it is thought that the mechanical strength of the ceramic substrate 3 can be improved and that this contributes to preventing cracks from occurring in the ceramic substrate 3 at the bonding interface.
[0026] The ratio of the yttria content to the zirconia content is preferably 4.5 mass % or more and 7.9 mass % or less, which is thought to maintain the stability of the tetragonal phase of zirconia in an appropriate state and contribute to suppressing a decrease in the mechanical strength of the ceramic substrate 3.
[0027] On the other hand, by setting the yttria content to 1.9 mass % or less, it is thought that the proportion of cubic crystals in the zirconia crystal phase can be prevented from becoming excessive, while the proportion of tetragonal crystals can be increased, which is thought to improve the mechanical strength of the ceramic substrate 3 and contribute to preventing cracks from occurring in the ceramic substrate 3 at the bonding interface.
[0028] Next, the glass components will be described. The silica content is preferably 0.1 mass % or more and 2.5 mass % or less. If the silica content is 0.1 mass % or more, the oxygen ion conductivity of the ceramic substrate 3 is suppressed, and the impedance can be improved, as described below. On the other hand, if the silica content is too high, there is a risk of a decrease in the strength of the ceramic substrate 3. To prevent this, the silica content is preferably 2.5 mass % or less.
[0029] In particular, when the zirconia content is 10% by mass or more and 15% by mass or less, the silica content is preferably 0.7% by mass or more and 1.5% by mass or less. Furthermore, when the zirconia content is more than 15% by mass but not more than 25% by mass, the silica content is preferably 1.5% by mass or more and 2.0% by mass or less. Thus, by changing the silica content depending on the zirconia content, the impedance of the ceramic substrate 3 can be effectively improved.
[0030] The glass component may contain at least one of magnesia (MgO) and calcia (CaO). For example, the magnesia content is preferably 0.1% by mass or more and 0.8% by mass or less, and more preferably 0.15% by mass or more and 0.3% by mass or less. By setting the magnesia content to 0.1% by mass or more, the ceramic substrate 3 can be sintered without excessively high firing temperatures, and coarsening of alumina and zirconia particles is thought to be suppressed. As a result, the mechanical strength of the ceramic substrate 3 can be improved, contributing to the suppression of cracks occurring in the ceramic substrate 3 at the bonding interface. Furthermore, a sufficient amount of MgAl2O4 crystals (hereinafter referred to as "spinel crystals") can be generated in the ceramic substrate 3, which is thought to improve wettability with the Cu-O eutectic liquid phase during copper plate bonding. As a result, it is thought to contribute to the suppression of voids occurring at the bonding interface.
[0031] On the other hand, it is believed that by setting the magnesia content to 0.8 mass % or less, it is possible to suppress the excessive formation of spinel crystals, which have low mechanical strength, and improve the mechanical strength of the ceramic substrate 3. As a result, it is believed that this contributes to suppressing the occurrence of cracks in the ceramic substrate 3 at the bonding interface.
[0032] When the glass component contains calcia, the calcia content is preferably 0.03% by mass or more and 0.35% by mass or less. This is thought to enable the ceramic substrate 3 to be sintered without an excessively high firing temperature, and to prevent the alumina and zirconia particles from becoming coarse. As a result, the mechanical strength of the ceramic substrate 3 can be improved, and this is thought to contribute to preventing cracks from occurring in the ceramic substrate 3 at the bonding interface.
[0033] The content of the balance is preferably 0.05 mass% or less in terms of oxide. This is thought to prevent the ceramic substrate 3 from being excessively sintered even when the firing temperature is not excessively high, and to reduce the porosity of the ceramic substrate 3. As a result, it is thought to improve the mechanical strength of the ceramic substrate 3 and contribute to preventing cracks from occurring in the ceramic substrate 3 at the bonding interface. The element contained in the balance may be an element that is intentionally added, or an element that is unavoidably mixed in. The element contained in the balance is not particularly limited, but examples thereof include Fe (iron), Ti (titanium), and Mn (manganese).
[0034] In this embodiment, the contents of the constituent elements of the ceramic substrate 3 are calculated in terms of oxides as described above, but the constituent elements of the ceramic substrate 3 may or may not exist in the form of oxides. For example, at least one of Y, Mg, and Ca may not exist in the form of an oxide but may be solid-solved in ZrO. For example, yttria may be solid-solved in zirconia to form PSZ (partially stabilized zirconia).
[0035] The content of the constituent elements of the ceramic substrate 3 in terms of oxide is calculated as follows. First, the constituent elements of the ceramic substrate 3 are qualitatively analyzed using an X-ray fluorescence analyzer (XRF) or an energy dispersive analyzer (EDS) attached to a scanning electron microscope (SEM). Next, each element detected by this qualitative analysis is quantitatively analyzed using an ICP optical emission spectrometer. Next, the content of each element measured by this quantitative analysis is converted into its oxide.
[0036] Here, XRF is an abbreviation for X-ray Fluorescence Analysis, SEM is an abbreviation for Scanning Electron Microscope, EDS is an abbreviation for Energy Dispersive X-ray Spectroscopy, and ICP is an abbreviation for Inductively Coupled Plasma.
[0037] 3. Manufacturing Method of Ceramic Substrate Next, a method of manufacturing a ceramic substrate will be described. First, powder materials of the above-described constituent elements are mixed. Next, the mixed powder materials are pulverized and mixed using, for example, a ball mill.
[0038] Next, an organic binder (for example, polyvinyl butyral), a solvent (xylene, toluene, etc.), and a plasticizer (dioctyl phthalate, etc.) are added to the pulverized and mixed powder material to form a slurry material.
[0039] Subsequently, the slurry material is molded into a desired shape by a desired molding method (for example, die pressing, cold isostatic pressing, injection molding, doctor blade method, extrusion molding, etc.) to produce a ceramic molded body.
[0040] The ceramic compact is then fired in an oxygen atmosphere or an air atmosphere (at 1555° C. to 1565° C. for 0.7 to 1.0 hour), whereby the ceramic sintered body 3 is completed.
[0041] 4. Manufacturing Method of Substrate for Semiconductor Device First, the copper plates 4, 4' are oxidized by wet treatment using a wet oxidation method. The wet treatment method is, for example, as follows. First, oil and organic residues from copper plate processing are removed by degreasing and cleaning. Next, a fine unevenness treatment is performed on the copper plates 4, 4' by microetching. Subsequently, the copper plates 4, 4' are immersed in an oxidation treatment solution for a predetermined time. For example, the copper plates 4, 4' are immersed for 5 minutes in an oxidation treatment solution adjusted to a pH of 14. As a result, an oxide film containing CuO and CuO and rich in CuO is formed on the surface of the copper plates 4, 4' before bonding to the ceramic substrate 3.
[0042] Next, a laminate is formed by disposing the copper plates 4, 4', the surfaces of which have been oxidized as described above, on the upper and lower surfaces of the ceramic substrate 3, and this is heated in a nitrogen atmosphere at 1065°C to 1083°C for approximately 10 to 60 minutes. By heating, a Cu-O eutectic liquid phase is generated at the interface where the ceramic substrate 3 and the copper plates 4, 4' are joined. The thickness of each copper plate 4, 4' can be, for example, 0.1 to 2.0 mm.
[0043] Subsequently, the laminate is cooled to solidify the Cu-O eutectic liquid phase, and the copper plates 4, 4' are bonded to the ceramic substrate 3. This completes the semiconductor device substrate 2. The transmission circuit formed on the copper plate 4 on the surface to which the semiconductor chip 6 is bonded can be formed by, for example, a subtractive method or an additive method.
[0044] <5. Copper-Present Region in Ceramic Substrate> As described above, a Cu-present region is formed inside the ceramic substrate 3 to which the copper plates 4, 4′ are bonded due to copper diffusing from the copper plates 4, 4′. This point will be described in detail in the Examples below. Upon examining the Cu-present region that exists from the interface between the copper plates 4, 4′ and the ceramic substrate 3 toward the interior of the ceramic substrate 3, the present inventors found that the bonding strength of the copper plates 4, 4′ is increased if the Cu-present depth from the interface with the ceramic substrate 3 in the Cu-present region is a predetermined depth. In particular, the inventors found that the bonding strength of the copper plates 4, 4′ is increased if the Cu-present depth, at which the cumulative Cu mass concentration in the Cu-present region is 90%, is 11.0 to 20.0 μm, preferably 13.0 to 18.0 μm, and even more preferably 13.0 to 16.0 μm.
[0045] That is, it was found that if the Cu presence depth showing an integrated Cu mass concentration of 90% is less than 11.0 μm, the copper presence region is narrow, and the bonding strength is weakened. On the other hand, it was also found that if the Cu presence depth showing an integrated Cu mass concentration of 90% exceeds 20.0 μm, the bonding strength is reduced.
[0046] In the examples described later, the load per unit width required to peel the copper plates 4, 4′ from the ceramic substrate 3 is measured, and this load is preferably 5.5 kg / cm or more, more preferably 6.0 kg / cm or more, and particularly preferably 8.0 kg / cm or more.
[0047] Furthermore, it has been found that when a copper plate is oxidized by the above-described wet oxidation method to form an oxide film containing CuO and CuO and rich in CuO on the surface of the copper plate 4, 4', the Cu diffusion region is wider as described above compared to a copper plate oxidized by a dry oxidation method. Even if a copper plate that has been oxidized by a method other than wet oxidation is used, the bonding strength between the copper plate 4, 4' and the ceramic substrate 3 can be improved as described above, as long as the substrate for a semiconductor device can achieve the above-described Cu presence depth. In other words, the Cu presence region described above may be formed by a method other than diffusing copper from the copper plate 4, 4' into the ceramic substrate 3.
[0048] In the above embodiment, the copper plates 4, 4' are bonded to both sides of the ceramic substrate 3, but it is also possible to use the ceramic substrate as a substrate for a semiconductor device by bonding a copper plate to only one side. When bonding the copper plates 4, 4' to both sides of the ceramic substrate 3, the Cu presence depth at which the integrated Cu mass concentration in the Cu presence region shows 90% does not need to be the same on each side of the ceramic substrate 3, and as described above, it is sufficient that it is within the range of 11.0 to 20.0 μm.
[0049] Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0050] <1. Preparation of Ceramic Substrate> Ceramic substrates according to Examples 1 and 2 and Comparative Examples 1 and 2 were prepared, each consisting of the following materials as its main component. That is, the ceramic substrates according to Examples 1 and 2 and Comparative Examples 1 and 2 were the same. Specifically, first, a powder material prepared by blending the compositions shown in Table 1 in predetermined proportions was pulverized and mixed in a ball mill. In Table 1, mass % is expressed as wt %. The values shown in Table 1 are values converted to the oxide of each element.
[0051] Next, polyvinyl butyral as an organic binder, xylene as a solvent, and dioctyl phthalate as a plasticizer were added to the pulverized and mixed powder material to form a slurry material.
[0052] Subsequently, the slurry material was formed into a sheet by a doctor blade method to prepare a ceramic molded body.
[0053] Subsequently, the ceramic compact was fired in an air atmosphere at 1565°C for 0.8 hours to obtain the ceramic substrates according to Examples 1 and 2 and Comparative Examples 1 and 2. The size of the ceramic substrate was 0.32 mm thick, 39 mm long, and 45 mm wide.
[0054] Next, copper plates according to Examples 1 and 2 and Comparative Examples 1 and 2 were prepared and subjected to an oxidation treatment on their surfaces. In Examples 1 and 2, oxidation was performed using the wet oxidation method described above, while in Comparative Examples 1 and 2, oxidation was performed using the dry oxidation method. In the dry oxidation method, the copper plates according to Comparative Examples 1 and 2 were heated for 5 minutes in a heat treatment furnace heated to 300°C to form a CuO oxide film. The thickness of each copper plate was approximately 0.3 mm. Subsequently, the copper plates according to Examples and Comparative Examples with oxidized surfaces were placed on the top and bottom surfaces of a ceramic substrate and heated in a nitrogen atmosphere at 1065°C for the time shown in Table 2 below. In this manner, semiconductor device substrates according to Examples 1 and 2 and Comparative Examples 1 and 2 were obtained.
[0055] <2. Evaluation> <2-1. Surface Condition of Copper Plate> Prior to bonding to the ceramic substrate, X-ray diffraction (XRD) measurements were performed on the surfaces of the copper plates (Examples 1 and 2) processed by the wet oxidation method and the copper plates (Comparative Examples 1 and 2) processed by the dry oxidation method. The measurements were performed using a SmartLab (Rigaku Corporation) at a rated voltage of 45 kV and a rated current of 200 mA. The results are shown in FIG. 2. As shown in FIG. 2, the surface of the copper plate processed by the wet oxidation method shows a CuO peak, indicating that a CuO-rich copper oxide layer has been formed on the surface. On the other hand, the surface of the copper plate processed by the dry oxidation method shows a CuO peak, indicating that a CuO-rich copper oxide layer has been formed on the surface.
[0056] 2-2. Quantitative analysis of elements (point analysis method) In Example 1, quantitative analysis of O, Al, Cu, Y, and Zr elements contained in the ZrO particles (Point 1) and the AlO matrix (Point 2), both of which are located 1.5 μm deep from the bonding interface toward the ceramic substrate, was carried out by point analysis using a field emission electron probe microanalyzer. The analyzed points are shown in Figure 3, and the measurement results by the point analysis method are shown in Table 3.
[0057] The results in Table 3 show that the Cu mass concentration inside the ZrO particles (Point 1) is 2.7 times higher than that in the AlO matrix (Point 2), indicating that Cu preferentially diffuses through the ZrO particles, thus forming Cu-containing regions.
[0058] Quantitative analysis of elements (area analysis method) In Example 1, an area including the Cu electrode, the bonding interface, and the ceramic substrate was subjected to area analysis for Zr and Cu using a field emission electron probe microanalyzer (EPMA). The results are shown in FIG.
[0059] The distribution positions of Zr and Cu were roughly the same. It was also confirmed that the Cu concentration decreased as it progressed from the bonding interface toward the interior of the ceramic substrate. The above-mentioned Cu diffusion behavior (Table 3 and Figure 4) was not limited to Example 1, and it was confirmed that the same behavior was also observed in Example 2.
[0060] <2-4. Analysis of Cu and Al Content> To confirm the distribution of each element in detail, the following analysis was performed. Cross-sectional samples were obtained by cutting and polishing the semiconductor device substrate. The cross sections were analyzed using a scanning electron microscope (SEM) and a field-emission electron probe microanalyzer. Figure 5(a) shows a backscattered electron image of the vicinity of the bonding interface between the copper plate and the ceramic substrate. The image area for the backscattered electron image was 25 μm wide and 100 μm deep. This area was divided into 256 × 1,024 small areas. The elemental concentration in each small area was then calculated. Then, as shown in Figure 5(b), the elemental concentration (mass%) was averaged across the 256 small areas in the horizontal direction (X direction) (this is referred to as the X-direction average elemental concentration). The elemental concentration distribution was measured using a field-emission electron probe microanalyzer (EPMA). As the EPMA, a field emission electron probe microanalyzer FE-EPMA, JXA-8530F, manufactured by JEOL was used.
[0061] Figure 6 is a graph in which the Y direction in Figure 5, i.e., the depth direction of the ceramic substrate, is plotted on the vertical axis, and the average element concentration in the X direction at each depth is plotted on the vertical axis. The horizontal axis of this graph has the bonding interface between the copper plate and the ceramic substrate as the origin. The bonding interface is synonymous with the point where the Al concentration rises from 0 wt%. When plotting the Cu mass concentration, we randomly plotted 10 μm depth intervals from the bonding interface toward the ceramic substrate. If the slope of the Cu plot satisfies the condition of ≦0.10, the Cu mass concentration from the start of the interval was defined as 0 wt%. The results in Figure 6 indicate that the diffusion distance of Cu tends to increase when the copper plate is oxidized by wet processing and when the electrode bonding time is long.
[0062] 2-5. Relationship between Cu diffusion depth and bonding strength in semiconductor device substrate The bonding strength between a copper plate and a ceramic substrate was measured as follows. First, a predetermined length of the bonded rectangular copper plate was peeled off from the edge in the long-side direction and bent at a 90° angle. Next, the edge of the bent copper plate was clamped with a clip and pulled up vertically. The maximum value at this time was defined as the measured strength. In other words, bonding strength (kg / cm) = maximum pulling load (kg) / short-side length of the rectangle (cm). The results are shown in Table 4.
[0063] The Cu concentration in Figure 6 was integrated in the Y-axis direction and plotted as a graph in Figure 7. The Cu diffusion depth at which the cumulative Cu mass concentration in the Cu-diffused region reached 90% was determined. The bonding strength and Cu diffusion depth are shown in Table 4.
[0064] Comparing Example 1 and Example 2, as the bonding time increases, the Cu diffusion region tends to expand in the Y direction, while the bonding strength tends to decrease. Comparing Example 1 and Comparative Example 1, the bonding times are the same, but Comparative Example 1 has a narrower Cu diffusion region and lower bonding strength. This indicates that the melting point of the copper oxide layer is lowered, promoting Cu diffusion and resulting in higher bonding strength. However, there is no proportional relationship between the Cu diffusion region in the Y direction and the bonding strength; once the Cu diffusion region exceeds a certain level, the bonding strength begins to decrease.
[0065] Therefore, it was found that Examples 1 and 2, in which the Cu diffusion depth when the cumulative Cu mass concentration from the bonding interface is 90% is 11.0 to 20.0 μm, exhibit higher bonding strength than Comparative Examples 1 and 2.
[0066] 2... Substrate for semiconductor device 3... Ceramic substrate 4, 4'... Copper plate
Claims
1. A substrate for a semiconductor device comprising: a ceramic substrate; and a copper plate bonded to at least one surface of the ceramic substrate, wherein the ceramic substrate has a Cu-existing region having a Cu-existing depth of 11.0 to 20.0 μm from the bonding interface with the copper plate when the cumulative Cu mass concentration is 90%.
2. The substrate for a semiconductor device according to claim 1, wherein the ceramic substrate contains alumina and zirconia or partially stabilized zirconia, and in the Cu-existing region, the copper content in the zirconia crystal grains is greater than the copper content in the alumina crystal grains.
3. The substrate for a semiconductor device according to claim 1 or 2, wherein the load per unit width required to peel the copper plate from the ceramic substrate is 5.5 kg / cm or more.
4. A method for manufacturing a substrate for a semiconductor device, comprising: a step of oxidizing a copper plate by a wet oxidation method; and a step of bonding the copper plate to at least one surface of a ceramic substrate by a direct bonding method, wherein the oxidized copper plate contains CuO and Cu2O before being bonded to the ceramic substrate, and the CuO-rich copper oxide layer is formed on the surface.
5. A method for manufacturing a substrate for a semiconductor device according to claim 3 or 4, wherein the Cu presence depth at which an integrated Cu mass concentration of 90% is shown on each surface of the ceramic substrate from the bonding interface with the copper plate is 11.0 to 20.0 μm.