Copper etchant
Patent Information
- Application Number
- MYPI2025002168
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-22
- Filing Date
- 2023-08-18
- Publication Date
- 2024-05-22
AI Technical Summary
Existing copper etching agents, particularly those based on sulfuric acid and hydrogen peroxide, fail to maintain the smoothness of copper surfaces effectively, especially during continuous etching processes in semiconductor and printed wiring board manufacturing.
A copper etching agent comprising hydrogen peroxide, sulfuric acid, an aromatic compound with a hydroxyl or carboxyl group bonded to a benzene ring, and a chlorine ion, which helps in stabilizing the smoothness of the copper surface by controlling the etching rate and preventing undercutting.
The etching agent effectively maintains the smoothness of copper surfaces, reduces side etching, and ensures stable etching performance even during continuous processing, suitable for removing seed layers in semi-additive copper wiring formation methods.
Smart Images

Figure PI2025002168_DRAWING_001 
Figure PI2025002168_DRAWING_002
Abstract
Description
Copper Etching Agent
[0001] The present invention relates to copper etchants.
[0002] In the manufacturing process of semiconductors and printed wiring boards, wet etching is used to pattern metals and form recesses. For example, in the manufacturing process of semiconductors, wet etching is used to form grooves and recesses. In the manufacturing process of printed wiring boards, wet etching is used to pattern metal layers made of copper or other materials to form metal wiring.
[0003] In the formation of copper wiring using the semi-additive method, which is a type of wiring formation method, a copper layer called a "seed layer" is formed on an insulating substrate by electroless plating, a plating resist is formed on the seed layer, and then pattern plating is performed in the resist openings on the seed layer by electrolytic copper plating. The plating resist is then removed, and the seed layer remaining between the wiring is removed by wet etching, thereby forming copper wiring. In this seed layer removal by wet etching, not only the seed layer but also the copper wiring is etched by the etching agent, which can affect the wiring shape and characteristics.
[0004] Etching agents for removing such seed layers are described, for example, in Patent Documents 1 and 2. Patent Document 1 describes an etching agent containing sulfuric acid and hydrogen peroxide, and further containing a benzotriazole compound and an amine compound. Patent Document 1 describes that such an etching agent can suppress undercutting of copper wiring during seed layer removal. Patent Document 2 describes an etching agent containing sulfuric acid and hydrogen peroxide, and further containing an amino acid, a nitrogen-containing heterocyclic compound such as an azole, a halogen, etc. Patent Document 2 describes that such an etching agent can maintain a smooth surface shape of copper wiring, etc. even after seed layer removal.
[0005] However, in the etching using the so-called sulfuric acid / hydrogen peroxide-based etching agent described in Patent Documents 1 and 2, the smoothness of the copper surface after etching is insufficient, and there is a problem that it is difficult to stably maintain the smoothness after etching, particularly when etching treatments are performed successively.
[0006] Japanese Patent Publication No. 2011-202242 Japanese Patent Publication No. 2021-195572
[0007] The present invention has been made in view of the above-mentioned problems of the prior art, and an object of the present invention is to provide a copper etching agent that can stably maintain the smoothness of the copper surface after etching.
[0008] The present invention comprises hydrogen peroxide, sulfuric acid, an aromatic compound, and chloride ions, and the aromatic compound comprises a structure in which a hydroxyl group and / or a carboxyl group is bonded to a benzene ring.
[0009] The content of the chloride ions may be 0.000020% by mass or more and 0.02% by mass or less.
[0010] The aromatic compound may be at least one selected from the group consisting of phenols, benzoic acid compounds, 2-hydroxybenzoic acid, 5-sulfosalicylic acid, methyl salicylate, sodium salicylate, isoamyl salicylate, and acetylsalicylic acid.
[0011] It may further contain triazoles.
[0012] The triazoles may be one or more selected from the group consisting of 1,2,4-triazole, 1,2,3-triazole, 3-amino-5-mercapto-1,2,4-triazole, 3,5-diamino-1,2,4-triazole, 3,5-dimethyl-1,2,4-triazole, 3-mercapto-1,2,4-triazole, 4-amino-1,2,4-triazole, 3-amino-1,2,4-triazole, 4-amino-3-mercapto-4H-1,2,4-triazole, and 3-amino-5-methylthio-1H-1,2,4-triazole.
[0013] According to the present invention, it is possible to provide a copper etching agent that can stably maintain the smoothness of the copper surface after etching.
[0014] Figure 1 is a chart showing the results of analyzing the surface of a test substrate using an EDS device. Figure 2 is a chart showing the results of analyzing the surface of a test substrate using an EDS device. Figure 3 is a graph showing the relationship between changes in chloride ion concentration and Sdr value.
[0015] Hereinafter, embodiments of the copper etching agent (hereinafter also simply referred to as etching agent) of the present invention will be described.
[0016] The copper etching agent of this embodiment contains hydrogen peroxide, sulfuric acid, an aromatic compound, and chloride ions, and the aromatic compound is an etching agent containing a structure in which a hydroxyl group and / or a carboxyl group is bonded to a benzene ring.
[0017] [Copper] The copper to be etched with the etching agent of the present embodiment may be copper (pure copper) or a copper alloy containing copper. Hereinafter, in this specification, "copper" refers to copper or a copper alloy.
[0018] [Hydrogen Peroxide] Hydrogen peroxide acts as an oxidizing agent for copper in the etching agent. The concentration of hydrogen peroxide in the etching agent is, for example, in the range of 4% by mass to 25% by mass, or 5% by mass to 20% by mass. When the concentration of hydrogen peroxide is in the above range, it can function appropriately as an oxidizing agent for copper.
[0019] [Sulfuric acid] Sulfuric acid acts as a component that dissolves oxidized copper in the etching agent. In the etching agent, copper is converted to copper oxide by hydrogen peroxide, and this copper oxide is dissolved in the solution by acid, resulting in the copper being etched.
[0020] The concentration of sulfuric acid during etching is, for example, in the range of 5% by mass to 30% by mass, or 10% by mass to 20% by mass, whereby oxidized copper can be appropriately dissolved in the etching agent.
[0021] [Aromatic Compound] An aromatic compound is a compound having a structure in which a hydroxyl group and / or a carboxyl group is bonded to a benzene ring. In the aromatic compound of this embodiment, it is preferable that at least one of the hydroxyl group and the carboxyl group is directly bonded to a carbon atom constituting the benzene ring. Examples of aromatic compounds having a structure in which a hydroxyl group is bonded to a benzene ring include phenols such as phenol, methylphenol, and dimethylphenol. Among these, phenols having a structure in which only a hydroxyl group is bonded to a benzene ring are preferred. Examples of aromatic compounds having a structure in which a carboxyl group is bonded to a benzene ring include benzoic acid compounds such as adducts of benzoic acid, such as benzoic acid, nitrobenzoic acid, and aminobenzoic acid, to which other functional groups are added, and benzoic acid salts such as sodium benzoate. Examples of aromatic compounds having a structure in which a hydroxyl group and a carboxyl group are bonded to a benzene ring include 2-hydroxybenzoic acid (salicylic acid), 5-sulfosalicylic acid, methyl salicylate, sodium salicylate, isoamyl salicylate, and acetylsalicylic acid. When a compound having a structure in which both a hydroxyl group and a carboxyl group are bonded to a benzene ring is used as the aromatic compound, there is an advantage that smoothness after etching can be maintained in a particularly preferable state.
[0022] The concentration of the aromatic compound in the etching agent is, for example, in the range of 0.0001% by mass to 1% by mass, or 0.0005% by mass to 0.5% by mass, or 0.0008% by mass to 0.1% by mass. When the concentration of the aromatic compound is in the above range, smoothness after etching can be maintained in a more suitable state.
[0023] [Chloride ions] Chloride ions act as a component that inhibits copper etching. Chloride ions can be incorporated into the etching agent by including a chloride ion source in the etching agent. Examples of chloride ion sources include sodium chloride, calcium chloride, aluminum chloride, magnesium chloride, and ammonium chloride.
[0024] The chloride ion concentration in the etching agent is, for example, in the range of 0.00001 mass % to 0.5 mass %, or 0.000015 mass % to 0.05 mass %, or 0.00002 mass % to 0.02 mass %. When the chloride ion concentration is in the above range, the copper etching rate can be appropriately suppressed, and the etching performance can be easily adjusted to a suitable range.
[0025] [Triazoles] The etching agent of this embodiment may further contain triazoles. In this embodiment, triazoles refer to 1,2,3-triazole, 1,2,4-triazole, and derivatives in which each functional group is bonded to a triazole skeleton. A triazole skeleton refers to a compound containing a five-membered nitrogen-containing heterocycle containing three nitrogen atoms. Examples of the derivatives include compounds in which an amino group, a mercapto group, a methyl group, an ethyl group, or other alkyl group is bonded to a triazole skeleton. Among these, triazole derivatives in which an amino group or a mercapto group is bonded are preferred.
[0026] More specific examples include 1,2,3-triazole, 1,2,4-triazole, 3-amino-5-mercapto-1,2,4-triazole, 3,5-diamino-1,2,4-triazole, 3,5-dimethyl-1,2,4-triazole, 3-mercapto-1,2,4-triazole, 4-amino-1,2,4-triazole, 3-amino-1,2,4-triazole, 4-amino-3-mercapto-4H-1,2,4-triazole, and 3-amino-5-methylthio-1H-1,2,4-triazole.
[0027] The concentration of triazoles in the etching agent is, for example, in the range of 0.00001% by mass to 1.0% by mass, or 0.00005% by mass to 0.5% by mass, or 0.00009% by mass to 0.48% by mass. When the triazole concentration is within the above range, smoothness after etching can be more easily maintained in a suitable state. Furthermore, the inclusion of triazole can easily improve the etching performance for electroless copper-plated copper. Therefore, an etching agent suitable for removing a seed layer formed by a semi-additive method without leaving any residue in areas other than the wiring can be obtained.
[0028] [Other Components] The etching agent of the present embodiment may contain other additives as needed. Examples of other components include additives that increase the solubility of each component, additives that suppress the decomposition of each component, a copper ion source as a component that promotes the oxidation of metallic copper, a pH adjuster, a surfactant, etc.
[0029] For example, when a copper ion source, which is a component that promotes the oxidation of metallic copper, is contained, examples of the copper ion source include copper sulfate, copper salts of organic acids, etc. When a copper ion source is contained, the content thereof is preferably about 1.4 mass % or more and 4.2 mass % or less.
[0030] The pH of the etching agent of this embodiment is not particularly limited, but may be in the range of 3 or less, or 2 or less, for example.
[0031] [Solvent] The etching agent can be easily prepared by dissolving the above-mentioned components in an appropriate solvent such as ion-exchanged water, pure water, or ultrapure water.
[0032] Unless otherwise specified, the exemplified components of the etching agent can be used alone or in combination of two or more.
[0033] The etching agent of this embodiment can be produced by mixing the above-mentioned components by a known method. Taking into consideration the solubility and decomposition of each component, some of the components may be mixed first, and then all of the components may be mixed immediately before use. Alternatively, a concentrated solution may be prepared by mixing some of the solvent, and then the remaining solvent may be added immediately before use to produce an etching agent of an appropriate concentration.
[0034] The method for etching copper with the etching agent of this embodiment is not particularly limited, and known methods can be used. Examples include etching treatment methods using immersion, spraying, etc. Treatment conditions such as treatment temperature and treatment time can also be adjusted as appropriate. For example, when etching by spraying, the spray pressure can be 0.05 to 0.20 MPa, the liquid temperature can be 20°C or higher and 35°C or lower, and the treatment time can be 20 seconds or higher and 300 seconds or lower. Furthermore, when etching by immersion, the liquid temperature can be 20°C or higher and 35°C or lower, and the treatment time can be 20 seconds or higher and 300 seconds or lower.
[0035] The smoothness of the copper surface etched with the etching agent of this embodiment can be evaluated, for example, by the following indexes. The developed area ratio (Sdr) value of the interface measured according to ISO 25178 is, for example, 0.20% or less, preferably 0.18% or less, and more preferably 0.175% or less. The Sdr value indicates the degree to which the developed area (surface area) of the measured surface has increased relative to the area of the measured surface, and the smaller this value, the smoother the surface. This value can be measured, for example, using a known shape analysis laser microscope. Details are measured by the method described in the Examples below.
[0036] Furthermore, the arithmetic mean roughness (Ra) measured in accordance with JIS B 0601 (2013) may be, for example, 0.11 μm or less, or 0.10 μm or less, or 0.095 μm or less. Furthermore, the root mean square roughness (Rq) measured in accordance with JIS B 0601 (2013) may be, for example, 0.125 μm or less, preferably 0.120 μm or less. Both Ra and Rq are measures of the roughness of the surface shape, with smaller values indicating fewer irregularities (smoother). This value can be measured, for example, using a known laser microscope. Details are measured using the method described in the Examples below.
[0037] The copper to be treated with the etching agent of this embodiment is not particularly limited, but is particularly suitable for use in removing a seed layer in the formation of copper wiring by a semi-additive process. In this case, a seed layer, which is a copper layer, is formed on an insulating substrate by electroless copper plating, a plating resist is formed on the seed layer, and then pattern plating is performed in the resist openings on the seed layer by electrolytic copper plating. The plating resist is then removed to form wiring, and the seed layer remaining between the wiring is removed by wet etching with the etching agent of this embodiment, thereby forming the wiring. Furthermore, in such wiring formation, the copper surface of the wiring is smoothed, and a suitable wiring shape with minimal wiring gouge (side etching) can be maintained. Maintaining the smoothness of the copper surface of wiring, etc., has the advantage of reducing transmission loss of electrical signals.
[0038] Furthermore, the etching agent of the present embodiment has etching performance suitable for removing a seed layer. For example, the etching rate for a copper layer formed by electroless copper plating is higher than the etching rate for a copper layer formed by electrolytic copper plating, and therefore the etching agent has high seed layer removability and causes little side etching of the wiring, making it suitable for removing a seed layer in a wiring formation process.
[0039] Furthermore, the etching agent of this embodiment can suppress a decrease in the smoothness of the treated copper surface even when etching is performed continuously. Therefore, a copper surface with high smoothness can be obtained stably. It is known that in etching for seed layer removal in the formation of copper wiring using a typical semi-additive method, chloride ions contained in the copper plating of the wiring or seed layer are mixed into the etching agent, and the chloride ion concentration in the etching agent increases as the number of treatments increases. In sulfuric acid / hydrogen peroxide-based etching agents, chloride ions contained in the etching agent within an appropriate concentration range have the effect of moderately suppressing etching and maintaining an appropriate etching rate, but if the concentration increases too much, the etching ability decreases drastically, making it difficult to sufficiently remove copper or reducing the smoothness after etching. The etching agent of this embodiment can suppress a decrease in etching performance even when the chloride ion concentration increases, thereby obtaining a copper surface with high smoothness stably. Therefore, a copper surface with high smoothness can be obtained stably even when treating a large number of substrates or other workpieces continuously.
[0040] The etching agent according to the present embodiment is as described above, but the disclosed embodiment should be considered to be illustrative in all respects and not restrictive. The scope of the present invention is defined by the claims rather than the above description, and it is intended to include all modifications within the meaning and scope of the claims.
[0041] The present invention will be explained in more detail below by showing examples, but the present invention is not limited to these examples.
[0042] [Test 1: Smoothness Test] (Etching Agent) Each etching agent used in this example was prepared. Each etching agent was an aqueous solution in which the following materials were dissolved in ion-exchanged water as a solvent to achieve the concentration of each component shown in Tables 1 to 3. Tables 1 to 3 also list the mass of each component, but ion-exchanged water was added in addition to the components listed in the tables to adjust the total amount to 1,000 g. Furthermore, according to the preparation method described below, 100 g of hydrogen peroxide was added in addition to the components shown in Tables 1 to 3, and a final amount of 1,100 g of etching agent was prepared.
[0043] (Materials) Sulfuric acid: purified sulfuric acid manufactured by Nissan Chemical Industries, Ltd. Copper sulfate: manufactured by Meltex Corporation Triazoles 3,5-diamino-1,2,4-triazole: manufactured by Tokyo Chemical Industry Co., Ltd. 1,2,4-triazole: manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. 3-amino-5-mercapto-1,2,4-triazole: manufactured by Tokyo Chemical Industry Co., Ltd. 3-mercapto-1,2,4-triazole: manufactured by Otsuka Chemical Co., Ltd. 3-amino-1H-1,2,4-triazole: manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. 4-amino-3-mercapto-4H-1,2,4-triazole: manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. 3-amino-5-methylthio-1H-1,2,4-triazole: manufactured by Tokyo Chemical Industry Co., Ltd. 3,5-dimethyl-1,2,4-triazole: manufactured by Tokyo Chemical Industry Co., Ltd. Azoles 5-aminotetrazole: manufactured by Tokyo Chemical Industry Co., Ltd. Benzotriazole: Kishida Chemical Co., Ltd. Aromatic compounds 2-hydroxybenzoic acid (salicylic acid): Fujifilm Wako Pure Chemical Industries, Ltd. Phenol: Fujifilm Wako Pure Chemical Industries, Ltd. Benzoic acid: Tokyo Chemical Industry Co., Ltd. 5-sulfosalicylic acid dihydrate: Tokyo Chemical Industry Co., Ltd. Methyl salicylate: Fujifilm Wako Pure Chemical Industries, Ltd. Acetylsalicylic acid: Fujifilm Wako Pure Chemical Industries, Ltd. Amino acids β-alanine: Fujifilm Wako Pure Chemical Industries, Ltd. Hydrogen peroxide: ADEKA
[0044] The etching agent is prepared by mixing sulfuric acid, an aromatic compound, or an amino acid with deionized water (DI water), adding triazoles or azoles and dissolving them thoroughly, and then mixing copper sulfate as a copper ion source. Immediately before etching, hydrogen peroxide is added.
[0045] (Test Substrates) The following test substrates 1 and 2 were prepared. Substrate 1: A copper-clad laminate (CCL) with a thickness of 0.2 mm and a size of 340 x 510 mm was prepared by forming a plating layer (20 μm) using an electrolytic copper plating solution on the copper-clad laminate (CCL), and the substrate was cut to a size of 100 x 100 mm. Substrate 2: A wafer with a thickness of 725 μm and a diameter of 200 mm was laminated with an insulating resin (25 μm), a seed layer (0.4 μm) was formed on the insulating resin using an electroless copper plating solution, and a pattern layer with a thickness of 6 μm and an L / S = 10 / 10 μm was formed on the seed layer using an electrolytic copper plating solution. The substrate was then cut to a size of 10 x 10 mm.
[0046] (Test Method) Substrate 1 was etched using each etching agent. The treatment conditions were as follows: Using a sprayer, each etching agent was sprayed onto the substrate at a temperature of 25°C at a spray pressure of 0.1 MPa, and the etching time was adjusted so that the copper etching depth was 1.0 μm. The substrate was then washed with water and dried.
[0047] (Evaluation Method) The test substrates after etching were evaluated by the following method. (1) Measurement of Interface Developed Area Ratio (Sdr) Value The interface developed area ratio (Sdr) value was measured using a confocal microscope. The Sdr value was measured using a confocal microscope (OPTELICS HYBRID+, manufactured by Lasertec Corporation) with a 50x magnification objective lens. (2) Measurement Method of Arithmetic Average Roughness (Ra) and Root Mean Square Roughness (Rq) The arithmetic average roughness (Ra) and root mean square roughness (Rq) were measured using a confocal microscope (device used: OPTELICS HYBRID+, manufactured by Lasertec Corporation) with a 50x magnification objective lens. The arithmetic average roughness and root mean square roughness were measured in accordance with the standard (JIS B 0633:2001). The results are shown in Tables 1 to 3.
[0048]
[0049]
[0050]
[0051] As shown in Tables 1 to 3, in each Example, the Sdr value was 0.20% or less, Ra was 0.11 μm or less, and Rq was in the range of 0.125 μm, and the smoothness was better than that of the comparative example that was subjected to etching treatment (Comparative Example 1 is an untreated control).
[0052] [Test 2: Evaluation of Cu Remaining Property] Using the etching agents of Examples 1 and 8 (composed of the ingredients in the table plus 100 g of hydrogen peroxide) and substrate 2 from the above examples, treatment was performed with the treatment time adjusted so that the copper etching depth of the pattern layer of substrate 2 was 0.5 μm, and the copper remaining property after etching was examined. For the evaluation, three points on the surface of the resin portion between the patterns of the test substrate after etching were randomly selected, and the surface was analyzed using an EDS (Energy Dispersive X-ray Spectrometry) device. The device used was a JSM-IT200A (manufactured by JEOL Ltd.), and the analysis was performed at an accelerating voltage of 10 kV. The results of one of the three measured points are shown in Figures 1 and 2.
[0053] Figure 1 shows the results of etching with the etching agent of Example 1 containing triazole. Peaks were observed between the patterns at positions indicating the presence of C, Si, and O derived from the insulating resin, but no peaks appeared at positions indicating the presence of Cu. On the other hand, Figure 2 shows the results of etching with the etching agent of Example 8, which does not contain triazole. Peaks were observed between the patterns at positions indicating the presence of C, Si, and O derived from the insulating resin, as well as at positions indicating the presence of Cu. Similar results were obtained at the other two points. Therefore, it was found that the test substrate treated with the etching agent of the example containing triazole had good smoothness and also low residual copper in the seed layer.
[0054] [Test 3: Effect of Chloride Ion Concentration] Etching agents were prepared using deionized water as a solvent to achieve the concentrations of each component listed in Table 4. Assuming that prolonged etching of a copper-plated substrate would result in chloride ions dissolving in the etching agent, Substrate 1 was etched using 14 different etching agents based on the above etching agent, but with chloride ion concentrations ranging from 0.25 mg / L to 100 mg / L. The etching conditions were the same as in Test 1. As in Test 1, 100 g of hydrogen peroxide was added to the components listed in the table to prepare etching agents. The Sdr values after etching were measured using the same method as in Test 1, and the results are shown in Table 5 and Figure 3. The etching rate was calculated in μm / min by measuring the weight of the substrate before and after etching and dividing the weight by the area of the substrate and the etching time. These values are also shown in Table 5.
[0055]
[0056]
[0057] As shown in Table 5 and the graph in Figure 3, the Sdr value increased as the chloride ion concentration increased, but even when the chloride ion concentration was increased to 100 mg / L, the Sdr value was 0.2 or less. In addition, the etching rate was relatively stable.
Claims
1. A copper etching agent comprising hydrogen peroxide, sulfuric acid, an aromatic compound, and chloride ions, wherein the aromatic compound has a structure in which a hydroxyl group and / or a carboxyl group is bonded to a benzene ring.
2. The copper etching agent according to claim 1, containing 0.000020% by mass or more and 0.02% by mass or less of said chloride ions.
3. The copper etching agent according to claim 1, wherein the aromatic compound is at least one selected from the group consisting of phenols, benzoic acid compounds, 2-hydroxybenzoic acid, 5-sulfosalicylic acid, methyl salicylate, sodium salicylate, isoamyl salicylate, and acetylsalicylic acid.
4. The copper etchant of claim 1 further comprising a triazole.
5. The copper etching agent according to claim 4, wherein the triazole is at least one selected from the group consisting of 1,2,4-triazole, 1,2,3-triazole, 3-amino-5-mercapto-1,2,4-triazole, 3,5-diamino-1,2,4-triazole, 3,5-dimethyl-1,2,4-triazole, 3-mercapto-1,2,4-triazole, 4-amino-1,2,4-triazole, 3-amino-1,2,4-triazole, 4-amino-3-mercapto-4H-1,2,4-triazole, and 3-amino-5-methylthio-1H-1,2,4-triazole.