Glass composition for flat cross-section glass fibers, flat cross-section glass fibers, and method for manufacturing flat cross-section glass fibers from glass material containing glass recycling material
Patent Information
- Application Number
- MYPI2025002234
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-02-08
- Publication Date
- 2024-08-08
AI Technical Summary
The production of flat cross-section glass fibers using recycled glass materials is hindered by the presence of foreign substances like platinum and crushed bricks, leading to instability in flattening, flatness ratio, and spinning stability, which is not adequately addressed by conventional E-glass compositions.
A glass composition with specific ranges of SiO2, Al2O3, B2O3, CaO, MgO, Fe2O3, TiO2, Na2O, and K2O, where the ratio of K2O/Na2O is between 0.05 and 0.50, and the ratio of MgO/Fe2O3 is between 4.10 and 10.00, along with the formula (C×M×T/NK)1/2 satisfying 3.00≦(C×M×T/NK)≦3.75, is used to enhance the stability of flat cross-section glass fibers when produced with recycled materials.
This composition ensures excellent flattening stability, flatness ratio stability, and glass fiber spinning stability, even when using recycled materials, by maintaining the mechanical strength and reducing the viscosity of the melt, thus improving the productivity and quality of flat cross-section glass fibers.
Abstract
Description
Glass composition for flat cross section glass fiber, flat cross section glass fiber, and method for producing flat cross section glass fiber from glass raw material containing recycled glass material
[0001] The present invention relates to a glass composition for flat cross section glass fibers, flat cross section glass fibers, and a method for producing flat cross section glass fibers from glass raw materials including recycled glass materials.
[0002] Glass fibers have been widely used in various applications to improve the performance of resin compositions. In recent years, demand for glass fibers (hereinafter sometimes referred to as flat cross-section glass fibers) made of a characteristic glass composition for glass fiber and including a plurality of glass filaments having a flat cross-sectional shape with a major axis and a minor axis each having a length within a predetermined range has been expanding, because the glass fibers impart the characteristics derived from the glass composition for glass fiber to glass fiber-reinforced molded products and have excellent resin composition reinforcement properties, such as improving the tensile strength and impact strength of glass fiber-reinforced resin compositions (see, for example, Patent Document 1).
[0003] Among glass compositions for glass fibers, E-glass composition is the most widely used, and among flat cross section glass fibers, flat cross section glass fibers made of E-glass composition are produced in the largest volume.
[0004] The E-glass composition contains SiO in the range of 52.0 to 56.0 mass % based on the total amount of the glass composition for the glass fiber. 2 and Al in the range of 12.0 to 16.0 mass% 2 O 3 and a total of 20.0 to 25.0 mass% of MgO and CaO, and 5.0 to 10.0 mass% of B. 2 O 3 The composition includes:
[0005] On the other hand, in recent years, due to the increasing environmental consciousness, the glass fiber waste generated in the manufacturing process is decontaminated and crushed (recycled glass material) is reused as a glass raw material. Among flat cross section glass fibers, flat cross section glass fibers having an E-glass composition are produced in the largest amount, so if it is possible to manufacture flat cross section glass fibers having an E-glass composition using recycled glass material, it will contribute greatly to the environment.
[0006] International Publication No. 2017 / 171101
[0007] However, compared with pure glass raw materials made from minerals, the recycled glass material contains fine foreign matter such as platinum and broken bricks, and these foreign matter affect the productivity of flat cross section glass fibers. Therefore, when an attempt is made to produce flat cross section glass fibers made from a conventional E-glass composition as described in Patent Document 1, for example, there is the disadvantage that the flattening stability, flattening ratio stability, and glass fiber spinning stability are impaired.
[0008] The present invention aims to eliminate such inconveniences and provide a glass composition for flat cross section glass fiber, which can provide flat cross section glass fiber having excellent flattening stability, flattening ratio stability, and glass fiber spinning stability, even when flat cross section glass fiber is produced using recycled glass material.
[0009] Another object of the present invention is to provide a flat cross section glass fiber made from the glass composition for a flat cross section glass fiber, and a method for producing a flat cross section glass fiber from a glass raw material containing a recycled glass material.
[0010] In order to achieve this object, the glass composition for flat cross section glass fiber of the present invention contains SiO in the range of 50.00 to 60.00 mass % based on the total amount of the glass composition for flat cross section glass fiber. 2 and Al in the range of 9.00 to 18.00 mass% 2 O 3 and B in the range of 3.00 to 9.00% by weight. 2 O 315.00 to 30.00 mass% CaO; 0.10 to 5.00 mass% MgO; and 0.01 to 1.00 mass% Fe. 2 O 3 and TiO in the range of 0.01 to 1.00 mass%. 2 and a total of 0.10 to 2.00 mass% of Na 2 O and K 2 O, and the Na 2 K content relative to O content 2 The ratio of the content of O (K 2 O / Na 2 O) is in the range of 0.05 or more and less than 0.50, 2 O 3 The ratio of the MgO content to the Fe content (MgO / Fe 2 O 3 ) is in the range of 4.10 or more and less than 10.00, the content of CaO is C, the content of MgO is M, the content of TiO 2 The content of T, 2 O and K 2 When the total content of O is NK, the C, M, T, and NK satisfy the following formula (1): 3.00≦(C×M×T / NK). 1/2 ≦3.75 (1)
[0011] According to the glass composition for flat cross section glass fiber of the present invention, SiO 2 , Al 2 O 3 , B 2 O 3 , CaO, MgO, Fe 2 O 3 , TiO 2 The content of and Na 2 O and K 2 The total content of O and Na 2 K content relative to O content 2 The ratio of the content of O (K 2 O / Na 2 O) and Fe 2 O 3 The ratio of the MgO content to the Fe content (MgO / Fe 2 O 3) are each within the above ranges, and C, M, T, and NK satisfy the above formula (1), so that even when flat cross section glass fibers are produced using recycled glass materials, flat cross section glass fibers having excellent flattening stability, flattening ratio stability, and glass fiber spinning stability can be obtained.
[0012] The flat cross section glass fiber of the present invention is a flat cross section glass fiber comprising a plurality of flat cross section glass filaments having a flat cross section with a major axis of a predetermined length range and a minor axis of a predetermined length range, and is characterized in that the flat cross section glass filaments are made from the glass composition for flat cross section glass fiber of the present invention.
[0013] The flat cross section glass fiber of the present invention can have excellent flattening stability, flattening ratio stability, and glass fiber spinning stability even when produced using recycled glass materials.
[0014] Furthermore, the method for producing a flat cross section glass fiber from a glass raw material containing a recycled glass material of the present invention is a method for producing a flat cross section glass fiber from a glass raw material containing a recycled glass material, which method comprises using a glass raw material containing recycled glass material to obtain flat cross section glass filaments having a flat cross section with a major axis of a length within a predetermined range and a minor axis of a length within a predetermined range, and bundling a plurality of the flat cross section glass filaments, wherein the glass raw material contains recycled glass material in a range of 1.0 to 50.0 mass % relative to the total amount, and the flat cross section glass filaments are made of the glass composition for flat cross section glass fiber of the present invention.
[0015] According to the method for producing a flat cross section glass fiber from a glass raw material containing a recycled glass material of the present invention, even when produced using recycled glass material, as long as the amount of recycled glass material relative to the total amount is within the above range, it is possible to produce a flat cross section glass fiber having excellent flattening stability, flattening ratio stability, and glass fiber spinning stability.
[0016] Here, the expression "the flat cross section glass fiber has excellent flattening stability" means that when glass raw materials are melted, the resulting molten glass is drawn out from a bushing equipped with 400 nozzle tips at a flow rate of 1.5 g / min of the molten glass passing through each nozzle to obtain 400 flat cross section glass filaments, and these flat cross section glass filaments are bundled to produce a flat cross section glass fiber, the average ratio of the major axis to the minor axis (major axis / minor axis) of the 400 flat cross section glass filaments constituting the flat cross section glass fiber is 3.0 or more.
[0017] Furthermore, the expression "the flat cross section glass fiber has excellent aspect ratio stability" means that when glass raw materials are melted, the resulting molten glass is drawn out from a bushing equipped with 400 nozzle tips at a flow rate of 1.3 g / min of the molten glass passing through each nozzle to obtain 400 flat cross section glass filaments, and these flat cross section glass filaments are bundled to produce a flat cross section glass fiber, the 400 flat cross section glass filaments constituting the flat cross section glass fiber do not contain any flat cross section glass filaments having a ratio of the major axis to the minor axis (major axis / minor axis) of 2.0 or less.
[0018] Furthermore, the flat cross section glass fiber having excellent glass fiber spinning stability means that when a glass raw material is melted, the resulting molten glass is drawn out from a bushing equipped with 400 nozzle tips at a flow rate of 1.3 g / min of molten glass passing through each nozzle to obtain 400 flat cross section glass filaments, and these flat cross section glass filaments are bundled to produce a flat cross section glass fiber, the number of times that the flat cross section glass filaments constituting the flat cross section glass fiber are broken is 105 or less.
[0019] Next, the embodiment of the present invention will be described in more detail.
[0020] The glass composition for flat cross section glass fiber of this embodiment contains SiO in the range of 50.00 to 60.00 mass % based on the total amount of the glass composition for flat cross section glass fiber. 2and Al in the range of 9.00 to 18.00 mass% 2 O 3 and B in the range of 3.00 to 9.00 mass% 2 O 3 15.00 to 30.00 mass% CaO; 0.10 to 5.00 mass% MgO; and 0.01 to 1.00 mass% Fe. 2 O 3 and TiO in the range of 0.01 to 1.00 mass%. 2 and a total of 0.10 to 2.00 mass% of Na 2 O and K 2 O, and the Na 2 K content relative to O content 2 The ratio of the content of O (K 2 O / Na 2 O) is in the range of 0.05 or more and less than 0.50, 2 O 3 The ratio of the MgO content to the Fe content (MgO / Fe 2 O 3 ) is in the range of 4.10 or more and less than 10.00, the content of CaO is C, the content of MgO is M, the content of TiO 2 The content of T, 2 O and K 2 When the total content of O is NK, the C, M, T, and NK satisfy the following formula (1): 3.00≦(C×M×T / NK). 1/2 ≦3.75 (1)
[0021] According to the glass composition for flat cross section glass fiber of this embodiment, SiO 2 , Al 2 O 3 , B 2 O 3 , CaO, MgO, Fe 2 O 3 , TiO 2 The content of and Na 2 O and K 2 O and total content, and Na 2 K content relative to O content 2 The ratio of the content of O (K 2 O / Na 2 O) and Fe2 O 3 The ratio of the MgO content to the Fe content (MgO / Fe 2 O 3 ) are each within the above ranges, and C, M, T, and NK satisfy the above formula (1), so that even when flat cross section glass fibers are produced using recycled glass materials, flat cross section glass fibers having excellent flattening stability, flattening ratio stability, and glass fiber spinning stability can be obtained.
[0022] The glass composition for flat cross section glass fiber of this embodiment contains SiO 2 If the content of SiO is less than 50.00 mass %, the mechanical strength of the flat cross section glass fiber made from the glass composition for flat cross section glass fiber is significantly reduced, and the ability of the flat cross section glass fiber to reinforce the resin composition is impaired. 2 If the content exceeds 60.00 mass %, the 1000 poise temperature and liquidus temperature of the glass composition for the flat cross section glass fiber become high, making it difficult to produce the flat cross section glass fiber.
[0023] In the glass composition for flat cross section glass fiber of this embodiment, SiO 2 The content is preferably in the range of 50.50 to 56.60 mass%, more preferably in the range of 51.00 to 54.44 mass%, even more preferably in the range of 52.00 to 54.40 mass%, particularly preferably in the range of 53.00 to 54.35 mass%, and most preferably in the range of 53.60 to 54.30 mass%.
[0024] The glass composition for flat cross section glass fiber of this embodiment contains Al based on the total amount of the glass composition for flat cross section glass fiber. 2 O 3 If the content of Al is less than 9.00% by mass, the mechanical strength of the flat cross section glass fiber made from the glass composition for flat cross section glass fiber is significantly reduced, and the ability of the flat cross section glass fiber to reinforce the resin composition is impaired. 2 O 3If the content exceeds 18.00 mass %, the 1000 poise temperature and liquidus temperature of the glass composition for the flat cross section glass fiber become high, making it difficult to produce the flat cross section glass fiber.
[0025] In the glass composition for flat cross section glass fiber of this embodiment, Al relative to the total amount of the glass composition for flat cross section glass fiber 2 O 3 The content is preferably in the range of 12.00 to 16.00 mass%, more preferably in the range of 12.50 to 15.50 mass%, even more preferably in the range of 13.00 to 15.00 mass%, particularly preferably in the range of 13.50 to 14.50 mass%, and most preferably in the range of 13.75 to 14.25 mass%.
[0026] The glass composition for flat cross section glass fiber of this embodiment is B relative to the total amount of the glass composition for flat cross section glass fiber. 2 O 3 If the content of B is less than 3.00% by mass, the viscosity of the molten glass composition for the flat cross section glass fiber increases at high temperatures, and devitrification is likely to occur in the bushing, which may cause breakage of the glass filaments constituting the flat cross section glass fiber during glass fiber spinning, or may cause flat cross section glass fibers containing devitrification. 2 O 3 If the content exceeds 9.00% by mass, the amount of volatile components from the melt of the glass composition for the flat cross section glass fiber increases, which leads to a deterioration in spinning productivity when the operation period is extended, or shortens the life of the furnace, making it impossible to obtain the desired productivity.
[0027] In the glass composition for flat cross section glass fiber of this embodiment, B relative to the total amount of the glass composition for flat cross section glass fiber 2 O 3The content is preferably in the range of 4.60 to 7.90 mass%, more preferably in the range of 4.70 to 7.00 mass%, even more preferably in the range of 4.80 to 6.80 mass%, particularly preferably in the range of 5.00 to 6.50 mass%, particularly preferably in the range of 5.10 to 6.4 mass%, and most preferably in the range of 5.55 to 5.94 mass%.
[0028] In the glass composition for flat cross section glass fiber of this embodiment, if the CaO content is less than 15.00 mass% relative to the total amount of the glass composition for flat cross section glass fiber, the viscosity of the molten glass composition for flat cross section glass fiber at high temperatures increases, resulting in poor flattening ratio stability and flattening stability. Also, if the CaO content exceeds 30.00 mass%, devitrification is likely to occur in the bushing, which can cause breakage during spinning or can cause flat cross section glass fibers containing devitrification.
[0029] In the glass composition for flat cross section glass fiber of this embodiment, the content of CaO relative to the total amount of the glass composition for flat cross section glass fiber is preferably in the range of 20.00 to 28.00 mass%, more preferably in the range of 20.50 to 26.0 mass%, even more preferably in the range of 21.00 to 25.00 mass%, particularly preferably in the range of 21.50 to 24.50 mass%, and most preferably in the range of 22.00 to 24.00 mass%.
[0030] In the glass composition for flat cross section glass fiber of this embodiment, if the MgO content is less than 0.10 mass % relative to the total amount of the glass composition for flat cross section glass fiber, the viscosity of the molten glass composition for flat cross section glass fiber increases at high temperatures, resulting in poor aspect ratio stability and flattening stability. Also, if the MgO content exceeds 5.00 mass %, striae will occur in the molten glass composition for flat cross section glass fiber, and the glass filaments constituting the flat cross section glass fiber may be easily broken during spinning.
[0031] In the glass composition for flat cross section glass fiber of this embodiment, the content of MgO relative to the total amount of the glass composition for flat cross section glass fiber is preferably in the range of 0.20 to 2.90 mass%, more preferably in the range of 0.50 to 2.50 mass%, even more preferably in the range of 0.80 to 2.40 mass%, particularly preferably in the range of 0.90 to 2.30 mass%, especially preferably in the range of 1.00 to 2.20 mass%, and most preferably in the range of 1.10 to 2.10 mass%.
[0032] The glass composition for flat cross section glass fiber of this embodiment contains Fe relative to the total amount of the glass composition for flat cross section glass fiber. 2 O 3 If the content of Fe is less than 0.01% by mass, the defoaming property of the molten glass composition for the flat cross section glass fiber may be reduced, and breakage due to bubbles may easily occur in the glass filaments constituting the flat cross section glass fiber during spinning. 2 O 3 If the content exceeds 1.00 mass %, the molten glass composition for the flat cross section glass fiber will be colored, and this coloring will cause the radiant heat absorption to become non-uniform, resulting in a deterioration in the melt uniformity of the molten glass composition for the flat cross section glass fiber, and therefore a deterioration in the aspect ratio stability and flattening stability.
[0033] In the glass composition for flat cross section glass fiber of this embodiment, Fe relative to the total amount of the glass composition for flat cross section glass fiber 2 O 3 The content is preferably in the range of 0.05 to 0.90 mass%, more preferably in the range of 0.10 to 0.60 mass%, even more preferably in the range of 0.15 to 0.55 mass%, particularly preferably in the range of 0.18 to 0.45 mass%, particularly preferably in the range of 0.20 to 0.42 mass%, and most preferably in the range of 0.21 to 0.40 mass%.
[0034] The glass composition for flat cross section glass fiber of this embodiment contains TiO relative to the total amount of the glass composition for flat cross section glass fiber. 2If the content of TiO is less than 0.01% by mass, the viscosity of the molten glass composition for the flat cross section glass fiber increases at high temperatures, resulting in poor flattening ratio stability and flattening stability. 2 If the content exceeds 1.00 mass %, the 1000 poise temperature and liquidus temperature of the glass composition for the flat cross section glass fiber become high, making it difficult to produce the flat cross section glass fiber.
[0035] In the glass composition for flat cross section glass fiber of this embodiment, TiO 2 The content is preferably in the range of 0.05 to 0.90 mass%, more preferably in the range of 0.06 to 0.50 mass%, even more preferably in the range of 0.07 to 0.35 mass%, particularly preferably in the range of 0.08 to 0.24 mass%, particularly preferably in the range of 0.09 to 0.22 mass%, and most preferably in the range of 0.10 to 0.20 mass%.
[0036] In the glass composition for flat cross section glass fiber of this embodiment, Na relative to the total amount of the glass composition for flat cross section glass fiber 2 O and K 2 It is difficult to make the total O content less than 0.10 mass % when mineral materials are used as glass raw materials. 2 O and K 2 If the total content of O exceeds 2.00 mass %, the mechanical strength of the flat cross section glass fiber made from the glass composition for the flat cross section glass fiber is significantly reduced, and the ability of the flat cross section glass fiber to reinforce the resin composition is impaired.
[0037] In the glass composition for flat cross section glass fiber of this embodiment, Na 2 O and K 2 The total content of O is preferably in the range of 0.20 to 1.80 mass%, more preferably in the range of 0.30 to 1.50 mass%, even more preferably in the range of 0.40 to 1.20 mass%, particularly preferably in the range of 0.51 to 1.10 mass%, and most preferably in the range of 0.60 to 0.94 mass%.
[0038] In the glass composition for flat cross section glass fiber of this embodiment, Na 2 K content relative to O content 2 The ratio of the content of O (K 2 O / Na 2 If Na is less than 0.05, the fiber formability of the molten glass composition for the flat cross section glass fiber deteriorates, and the surface tension of the molten glass composition for the flat cross section glass fiber increases, resulting in a deterioration in the aspect ratio stability of the glass composition for the flat cross section glass fiber. 2 K content relative to O content 2 The ratio of the content of O (K 2 O / Na 2 If the value of (O) is 0.50 or more, it becomes difficult to sufficiently clarify the melt of the glass composition for the flat cross section glass fiber, and the flattening stability of the glass composition for the flat cross section glass fiber deteriorates.
[0039] In the glass composition for flat cross section glass fiber of this embodiment, Na 2 K content relative to O content 2 The ratio of the content of O (K 2 O / Na 2 O) is preferably in the range of 0.07 or more and 0.44 or less, more preferably in the range of 0.08 or more and 0.40 or less, even more preferably in the range of 0.09 or more and 0.36 or less, particularly preferably in the range of 0.10 or more and 0.035 or less, particularly preferably in the range of 0.11 or more and 0.33 or less, and most preferably in the range of 0.12 or more and 0.32 or less.
[0040] In the glass composition for flat cross section glass fiber of this embodiment, Fe 2 O 3 The ratio of the MgO content to the Fe content (MgO / Fe 2 O 3 If the value of Fe is less than 4.10, the melting property of the molten glass composition for the flat cross section glass fiber deteriorates due to coloration of the molten glass composition, and the aspect ratio stability deteriorates. 2 O 3 The ratio of the MgO content to the Fe content (MgO / Fe 2 O 3If the value of (a) is 10.00 or more, the melting property of the molten glass composition for the flat cross section glass fiber deteriorates, and the aspect ratio stability deteriorates.
[0041] In the glass composition for flat cross section glass fiber of this embodiment, Fe 2 O 3 The ratio of the MgO content to the Fe content (MgO / Fe 2 O 3 ) is preferably in the range of 4.30 to 9.94, more preferably in the range of 6.60 to 9.40, and even more preferably in the range of 7.10 to 8.90.
[0042] In the glass composition for flat cross section glass fiber of this embodiment, the (C × M × T / NK) 1/2 If the value of (C×M×T / NK) is less than 3.00, the amount of volatile components from the melt of the glass composition for the flat cross section glass fiber, which may cause breakage of the glass filaments constituting the flat cross section glass fiber during glass fiber spinning, tends to increase, and the glass fiber spinning stability deteriorates. 1/2 If the value exceeds 3.75, Cr-based crystals, specifically uvarovite crystals, which cause breakage of the glass filaments constituting the flat cross section glass fiber during glass fiber spinning, tend to be more likely to occur, and the glass fiber spinning stability deteriorates.
[0043] In the glass composition for flat cross section glass fiber of this embodiment, the (C × M × T / NK) 1/2 The value of is preferably in the range of 3.03 to 3.65, more preferably in the range of 3.04 to 3.40, and even more preferably in the range of 3.05 to 3.15.
[0044] The glass composition for flat cross section glass fiber of this embodiment contains F in the range of 0 mass % or more and less than 1.00 mass % relative to the total amount of the glass composition for flat cross section glass fiber. 2 In the glass composition for flat cross section glass fiber of this embodiment, F relative to the total amount of the glass composition for flat cross section glass fiber may be contained. 2From the viewpoint of reducing the environmental load, the content is preferably less than 0.10% by mass, more preferably less than 0.01% by mass, even more preferably 0.004% by mass or less, and particularly preferably 0% by mass.
[0045] Furthermore, the glass composition for flat cross section glass fiber of this embodiment may contain ZnO in a range of 0 mass% or more and less than 3.00 mass% relative to the total amount of the glass composition for flat cross section glass fiber. When the glass composition for flat cross section glass fiber of this embodiment contains ZnO, the content of ZnO relative to the total amount of the glass composition for flat cross section glass fiber is preferably less than 2.50 mass%, more preferably less than 1.50 mass%, even more preferably less than 0.50 mass%, particularly preferably less than 0.10 mass%, especially preferably less than 0.05 mass%, and most preferably less than 0.01 mass%.
[0046] The glass composition for flat cross section glass fiber of this embodiment can be prepared by mixing a glass recycled material and a mineral material or mineral-derived refined material in a range of 1.0 to 50.0 mass % relative to the total amount of the glass composition for flat cross section glass fiber. The glass composition for flat cross section glass fiber of this embodiment has the content ratio of the glass recycled material and the mineral material or mineral-derived refined material determined based on the components contained in the glass recycled material and the mineral material or mineral-derived refined material, the content of each component, and the amount of volatilization of each component during the melting process when making into glass raw materials, so as to obtain the above-mentioned glass composition.
[0047] Examples of the recycled glass material include waste glass fibers generated during the glass fiber manufacturing process due to reasons such as cutting, poor quality, or non-compliance with standards, or glass fibers recovered from glass fiber-reinforced resin compositions, which have been pulverized after organic components adhering to the surface have been removed by incineration, etc. Preferably, the recycled glass material is a recycled glass material recovered from a glass fiber-reinforced resin composition containing E-glass fiber.
[0048] Examples of the mineral materials include silica sand, feldspar, clay, and limestone, and examples of the mineral-derived refined materials include silica powder, dolomite, talc, clay, alumina, and soda ash.
[0049] Furthermore, the glass composition for flat cross section glass fiber of this embodiment may contain oxides of Ba, Co, Ni, Cu, Mo, Sr, Nb, W, Ce, Y, La, Bi, Gd, Pr, Sc, or Yb as impurities originating from the glass raw materials containing the recycled glass material, in a range of 3.00 mass% or less in total relative to the total amount of the glass composition for the flat cross section glass fiber. In the glass composition for flat cross section glass fiber of this embodiment, the content of the impurities relative to the total amount of the glass composition for the flat cross section glass fiber is preferably 2.00 mass% or less, and more preferably less than 1.00 mass%.
[0050] In particular, the glass composition for flat cross section glass fiber of this embodiment contains BaO, CuO, SrO, Ni as impurities. 2 O 3 , Nb 2 O 4 , W.O. 3 , CeO 2 , Y 2 O 3 , La 2 O 3 , Bi 2 O 3 , Gd 2 O 3 , Pr 2 O 3 , Sc 2 O 3 , or Yb 2 O 3 When it contains, the content thereof is, independently of the total amount of the glass composition for the flat cross section glass fiber, preferably in the range of less than 0.40 mass%, more preferably in the range of less than 0.20 mass%, even more preferably in the range of less than 0.10 mass%, particularly preferably in the range of less than 0.05 mass%, particularly preferably in the range of 0.04 mass% or less, particularly preferably less than 0.015 mass%, and most preferably in the range of less than 0.01 mass%.
[0051] The content of each component of the glass composition for the flat cross section glass fiber of this embodiment can be measured using an ICP optical emission spectrometer for the light element Li, and the content of other elements can be measured using a wavelength dispersive X-ray fluorescence analyzer.
[0052] The measurement method can be as follows: First, a glass batch is placed in a platinum crucible and melted in an electric furnace at a temperature of 1650°C for 6 hours while stirring, thereby obtaining a homogeneous molten glass. Alternatively, glass fibers are placed in a platinum crucible and melted in an electric furnace at a temperature of 1650°C for 6 hours while stirring, thereby obtaining a homogeneous molten glass.
[0053] The glass batch is prepared by mixing glass raw materials. If organic matter is attached to the surface of the glass fiber or if the glass fiber is contained mainly as a reinforcing material in an organic material (resin), the glass fiber is used after removing the organic matter by, for example, heating in a muffle furnace at 300 to 650°C for about 0.5 to 24 hours.
[0054] Next, the obtained molten glass is poured onto a carbon plate to produce glass cullet, and then the glass cullet is crushed and powdered to obtain glass powder.
[0055] Next, the light element Li is quantitatively analyzed using an ICP optical emission spectrometer after the glass powder is thermally decomposed with acid. Other elements are quantitatively analyzed using a wavelength-dispersive X-ray fluorescence analyzer after the glass powder is formed into a disk shape using a press. Specifically, quantitative analysis using a wavelength-dispersive X-ray fluorescence analyzer can be performed by preparing a calibration curve sample based on the results measured using the fundamental parameter method and analyzing it using the calibration curve method. The content of each component in the calibration curve sample can be quantitatively analyzed using an ICP optical emission spectrometer. The results of these quantitative analyses are converted into oxides to calculate the content and total amount of each component, and the content (mass %) of each component can be determined from these values.
[0056] Next, the flat cross section glass fiber of this embodiment is a flat cross section glass fiber containing a plurality of flat cross section glass filaments having a flat cross section with a major axis of a predetermined length range and a minor axis of a predetermined length range, and the flat cross section glass filaments are made from the glass composition for the flat cross section glass fiber of this embodiment.
[0057] The flat cross section glass fiber of this embodiment can be produced by the method of producing a flat cross section glass fiber from a glass raw material containing a recycled glass material of this embodiment, which involves using a glass raw material containing a recycled glass material to obtain flat cross section glass filaments having a flat cross section with a major axis having a length within a predetermined range and a minor axis having a length within a predetermined range, and then bundling a plurality of the flat cross section glass filaments.
[0058] In the method for producing a flat cross section glass fiber from a glass raw material containing a recycled glass material of the present embodiment, the glass raw material contains the recycled glass material in a range of 1.0 to 50.0 mass% relative to the total amount, and the flat cross section glass filaments are made of the glass composition for flat cross section glass fiber of the present embodiment.
[0059] The flat cross section glass fiber of this embodiment can be formed, for example, from the glass composition for the flat cross section glass fiber of this embodiment as follows. First, glass raw materials prepared so as to have the above-mentioned composition when melted are supplied to a melting furnace and melted at a temperature range of 1000 poise or higher, specifically at a temperature in the range of 1450 to 1650°C. Then, the molten glass melted at this temperature is discharged from 1 to 8000 nozzle tips or holes controlled to a predetermined temperature, and cooled and solidified while being stretched by being wound up at high speed, thereby forming the glass fiber.
[0060] Here, the glass single fiber (glass filament) discharged from one nozzle tip or hole and cooled and solidified usually has a perfectly circular cross-sectional shape and a diameter in the range of 2.0 to 35.0 μm. On the other hand, when the nozzle tip has a non-circular shape and has a protrusion or notch that rapidly cools the molten glass, the flat cross-sectional glass filament of this embodiment having a non-circular (e.g., elliptical or oval) flat cross-sectional shape can be obtained by controlling the temperature conditions. The non-circular shape is, for example, an ellipse or oval (a shape in which the short sides of a rectangle are replaced with semicircles whose diameter is the short sides), etc.
[0061] In the flat cross section glass filament of this embodiment, the ratio of the major axis to the minor axis of the cross section shape (major axis / minor axis) is, for example, in the range of 2.0 to 10.0, and the fiber diameter when the cross section area is converted into that of a perfect circle (converted fiber diameter) is, for example, in the range of 2.0 to 35.0 μm.
[0062] The flat cross section glass fiber of this embodiment is usually in the form of a glass fiber bundle (glass strand) in which the flat cross section glass filaments are bundled in the range of 10 to 8,000 pieces, and has a weight in the range of 0.3 to 10,000.0 tex (g / km) and an elastic modulus in the range of 70.0 to 79.4 GPa. In the flat cross section glass fiber of this embodiment, the elastic modulus can be measured, for example, as follows.
[0063] First, the flat cross section glass fiber of this embodiment is placed in a platinum crucible and melted in an electric furnace at a temperature of 1600°C for 6 hours while stirring, thereby obtaining a homogeneous molten glass. When the flat cross section glass fiber of this embodiment is contained in a glass fiber reinforced resin composition, the glass fiber reinforced resin composition is heated, for example, in a muffle furnace at 300 to 650°C for about 0.5 to 24 hours to decompose the organic matter, and the resulting flat cross section glass fiber is used.
[0064] Next, the obtained molten glass is poured onto a carbon plate to produce glass cullet, and then the obtained glass cullet is poured into a small cylindrical platinum bushing having one circular nozzle tip at the bottom of the container, and the bushing is heated to a predetermined temperature so that the viscosity of the poured glass cullet becomes 1000±150 poise, thereby melting the glass cullet and obtaining molten glass.
[0065] Next, the molten glass discharged from the nozzle tip of the platinum bushing is wound up at a predetermined speed by a winder so that the glass fiber diameter becomes 13±2 μm, and is cooled and solidified while being stretched, thereby obtaining a glass fiber having a perfectly circular cross section. A single fiber (monofilament) is collected between the nozzle tip of the platinum bushing and the winder, and a monofilament in a state in which deterioration due to contact and friction is minimized is selected.
[0066] Next, the obtained monofilament is aligned in the long side direction along a line connecting the center points of the short sides of a mount having two gripping portions and two support portions, as described below, and bonded to prepare a monofilament test piece. Next, the diameter of the obtained monofilament is measured using a scanning electron microscope (manufactured by Hitachi, Ltd., product name: S-3400), and the cross-sectional area of the monofilament is calculated from the obtained diameter.
[0067] Next, the two gripping portions in the mount are set in the upper and lower gripping portions of a tensile tester (manufactured by A&D Co., Ltd., product name: benchtop material testing machine STB-1225S) with the distance between the gripping portions set to 50 mm, and the two support portions in the mount are cut off, and the gripping portions are connected only with the monofilament, and then a tensile test is performed at a crosshead speed of 5 mm / min. Next, the stresses corresponding to the strains ε1 = 0.0005 and ε2 = 0.0025 between the two points are designated as σ1 and σ2, respectively, and the tensile modulus is calculated by dividing the stress difference (σ2 - σ1) by the strain difference (ε2 - ε1). Monofilament test pieces that experienced thread loss during measurement are excluded, and the modulus of elasticity of the flat cross section glass fiber of this embodiment can be measured by calculating the average value of the tensile modulus for n = 15.
[0068] The backing paper has short sides of 25 mm and long sides of 75 mm, and a cutout section with a short side of 15 mm and a long side of 50 mm in the center of its interior, with the short sides and long sides of the backing paper parallel to the short sides and long sides of the cutout, respectively.A gripping section that is set in the gripping tool of a tensile testing machine is provided between the short sides of the cutout and the short sides of the backing paper, and a support section that connects and supports the two gripping sections is provided between the long sides of the cutout and the long sides of the backing paper.
[0069] The flat cross section glass fiber of this embodiment can be obtained by further processing the glass strands in various forms, such as yarn, woven fabric, knitted fabric, nonwoven fabric, chopped strand, roving, powder, etc. The nonwoven fabric includes chopped strand mat and multiaxial nonwoven fabric.
[0070] The chopped strand is a glass fiber formed by bundling a plurality of glass filaments and cut into lengths in the range of 1 to 25 mm. The chopped strand is usually distributed in the form of a bag-like package containing a plurality of glass fiber pieces cut as described above.
[0071] The roving is a glass fiber formed by bundling a plurality of glass filaments and continuously winding it up. The roving is usually distributed in a state where glass fibers having a length of 1000 m or more are wound around a core material.
[0072] The flat cross section glass fiber of this embodiment may be surface-coated with an organic substance for the purposes of improving the bundling of the glass filaments, improving the adhesion between the glass fiber and the resin, improving the uniform dispersion of the flat cross section glass fiber in a mixture of the flat cross section glass fiber with the resin or inorganic material, etc. Examples of such organic substances include starch, urethane resin, epoxy resin, vinyl acetate resin, acrylic resin, modified polypropylene (particularly, carboxylic acid-modified polypropylene), copolymers of (poly)carboxylic acid (particularly, maleic acid) and unsaturated monomers, etc.
[0073] The flat cross section glass fiber of this embodiment may be coated with a resin composition containing, in addition to these resins, a silane coupling agent, a lubricant, a surfactant, etc. Alternatively, the flat cross section glass fiber of this embodiment may be coated with a treatment composition containing, without containing the resin, a silane coupling agent, a surfactant, etc. Such a resin composition or treatment composition coats the flat cross section glass fiber at a ratio in the range of 0.1 to 2.0 mass%, based on the mass of the flat cross section glass fiber of this embodiment in a state not coated with the resin composition or treatment composition. The coating of the flat cross section glass fiber with the organic substance can be carried out, for example, in the production process of the flat cross section glass fiber, by applying a resin solution or a resin composition solution to the flat cross section glass fiber using a known method such as a roller applicator, and then drying the flat cross section glass fiber to which the resin solution or resin composition solution has been applied. Furthermore, the flat cross section glass fiber of this embodiment in the form of a woven fabric with the organic material can be coated by immersing the flat cross section glass fiber in a solution of a treatment composition, and then drying the flat cross section glass fiber to which the treatment composition has been applied.
[0074] Examples of the silane coupling agent include aminosilane, chlorosilane, epoxysilane, mercaptosilane, vinylsilane, acrylicsilane, and cationic silane. These compounds can be used alone or in combination of two or more.
[0075] Examples of aminosilanes include γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-N'-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and γ-anilinopropyltrimethoxysilane.
[0076] Examples of chlorosilane include γ-chloropropyltrimethoxysilane.
[0077] Examples of epoxy silanes include γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.
[0078] Examples of mercaptosilane include γ-mercaptotrimethoxysilane.
[0079] Examples of vinylsilanes include vinyltrimethoxysilane and N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane.
[0080] Examples of the acrylic silane include γ-methacryloxypropyltrimethoxysilane.
[0081] Examples of cationic silanes include N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride and N-phenyl-3-aminopropyltrimethoxysilane hydrochloride.
[0082] Examples of the lubricant include modified silicone oil, animal oil and its hydrogenated product, vegetable oil and its hydrogenated product, animal wax, vegetable wax, mineral wax, condensation product of higher saturated fatty acid and higher saturated alcohol, polyethyleneimine, polyalkyl polyamine alkyl amide derivative, fatty acid amide, and quaternary ammonium salt.The lubricant can be used alone or in combination of two or more kinds.
[0083] Examples of animal oils include beef tallow.
[0084] Examples of vegetable oils include soybean oil, coconut oil, rapeseed oil, palm oil, castor oil, and the like.
[0085] Examples of animal waxes include beeswax and lanolin.
[0086] Examples of vegetable waxes include candelilla wax and carnauba wax.
[0087] Examples of mineral waxes include paraffin wax and montan wax.
[0088] Examples of the condensation products of higher saturated fatty acids and higher saturated alcohols include stearic acid esters such as lauryl stearate.
[0089] Examples of fatty acid amides include dehydration condensates of polyethylene polyamines such as diethylenetriamine, triethylenetetramine, and tetraethylenepentamine with fatty acids such as lauric acid, myristic acid, palmitic acid, and stearic acid.
[0090] Examples of the quaternary ammonium salt include alkyltrimethylammonium salts such as lauryltrimethylammonium chloride.
[0091] Examples of the surfactant include nonionic surfactants, cationic surfactants, anionic surfactants, and amphoteric surfactants. These surfactants can be used alone or in combination of two or more.
[0092] Examples of nonionic surfactants include ethylene oxide propylene oxide alkyl ethers, polyoxyethylene alkyl ethers, polyoxyethylene-polyoxypropylene block copolymers, alkyl polyoxyethylene-polyoxypropylene block copolymer ethers, polyoxyethylene fatty acid esters, polyoxyethylene fatty acid monoesters, polyoxyethylene fatty acid diesters, polyoxyethylene sorbitan fatty acid esters, glycerol fatty acid ester ethylene oxide adducts, polyoxyethylene castor oil ethers, hydrogenated castor oil ethylene oxide adducts, alkylamine ethylene oxide adducts, fatty acid amide ethylene oxide adducts, glycerol fatty acid esters, polyglycerin fatty acid esters, pentaerythritol fatty acid esters, sorbitol fatty acid esters, sorbitan fatty acid esters, sucrose fatty acid esters, polyhydric alcohol alkyl ethers, fatty acid alkanolamides, acetylene glycol, acetylene alcohol, ethylene oxide adducts of acetylene glycol, and ethylene oxide adducts of acetylene alcohol.
[0093] Examples of cationic surfactants include alkyldimethylbenzylammonium chloride, alkyltrimethylammonium chloride, alkyldimethylethylammonium ethyl sulfate, higher alkylamine acetate, higher alkylamine hydrochloride, ethylene oxide adducts of higher alkylamines, condensates of higher fatty acids and polyalkylene polyamines, salts of esters of higher fatty acids and alkanolamines, salts of higher fatty acid amides, imidazoline-type cationic surfactants, and alkylpyridinium salts.
[0094] Examples of anionic surfactants include higher alcohol sulfates, higher alkyl ether sulfates, α-olefin sulfates, alkylbenzene sulfonates, α-olefin sulfonates, reaction products of fatty acid halides and N-methyltaurine, dialkyl sulfosuccinates, higher alcohol phosphates, and phosphate salts of higher alcohol ethylene oxide adducts. Examples of amphoteric surfactants include amino acid-type amphoteric surfactants such as alkali metal salts of alkylaminopropionic acid, betaine-type surfactants such as alkyldimethylbetaine, and imidazoline-type amphoteric surfactants.
[0095] Next, examples of the present invention and comparative examples will be described.
[0096] [Examples 1 to 6 and Comparative Examples 1 to 6] First, a mineral-derived refined material and a recycled glass material were prepared to prepare glass frits of Examples 1 to 6 having the compositions shown in Table 1, and glass frits of Comparative Examples 1 to 6 having the compositions shown in Table 1. Each of the glass frits contained 10.0 mass% of the recycled glass material relative to the total amount. The recycled glass material was a recycled glass material recovered from a glass fiber-reinforced resin composition containing E-glass fiber.
[0097] Next, the glass raw materials were melted to obtain molten glass, and the obtained molten glass was drawn out from a bushing equipped with 400 nozzle tips at a flow rate of 1.3 g / min or 1.5 g / min per nozzle to obtain a plurality of flat cross section (oval cross section) glass filaments. Then, a plurality of the flat cross section (oval cross section) glass filaments were bundled to produce a flat cross section (oval cross section) glass fiber.
[0098] The nozzle tip has a hole portion having a flat cross-sectional shape with a minor axis length of 1.0 mm and a ratio of the major axis length to the minor axis length (minor axis / major axis) of 4.0, and a wall portion having a notch for cooling the molten glass.
[0099] Next, the flattening stability, flattening ratio stability, and glass fiber spinning stability of the flat cross section glass fibers obtained in each Example and Comparative Example were evaluated as follows. The results are shown in Tables 1 and 2.
[0100] [Flattening Stability] The glass raw materials were melted, and the resulting molten glass was drawn out from a bushing equipped with 400 nozzle tips at a flow rate of 1.5 g / min of the molten glass passing through each nozzle to obtain 400 flat cross section glass filaments. These flat cross section glass filaments were then bundled to produce a flat cross section glass fiber. When the average value of the ratio of the major axis to the minor axis (major axis / minor axis) of the 400 flat cross section glass filaments constituting the flat cross section glass fiber was 3.0 or more, the glass fiber was evaluated as "OK", and when the average value was less than 3.0, the glass fiber was evaluated as "NG".
[0101] [Flatness ratio stability] The glass raw materials were melted, and the resulting molten glass was drawn out from a bushing equipped with 400 nozzle tips at a flow rate of 1.3 g / min of the molten glass passing through each nozzle to obtain 400 flat cross section glass filaments. These flat cross section glass filaments were then bundled to produce a flat cross section glass fiber. When the 400 flat cross section glass filaments constituting the flat cross section glass fiber did not contain any flat cross section glass filaments having a ratio of the major axis to the minor axis (major axis / minor axis) of 2.0 or less, the result was evaluated as "OK", and when even one flat cross section glass filament having a ratio of the major axis to the minor axis (major axis / minor axis) of 2.0 or less was contained, the result was evaluated as "NG".
[0102] [Glass fiber spinning stability] The glass raw materials were melted, and the resulting molten glass was drawn out from a bushing equipped with 400 nozzle tips at a flow rate of 1.3 g / min of molten glass passing through each nozzle to obtain 400 flat cross section glass filaments. These flat cross section glass filaments were then bundled to produce a flat cross section glass fiber. This process was carried out continuously for 168 hours. When the number of times that the flat cross section glass filaments constituting the flat cross section glass fiber were cut was 105 or less, the result was evaluated as "OK", and when the number of times that the flat cross section glass filaments constituting the flat cross section glass fiber were cut was more than 105, the result was evaluated as "NG".
[0103]
[0104]
[0105] From Table 1, it is clear that the flat cross section glass fibers of Examples 1 to 6, which contain a plurality of flat cross section glass filaments made of the glass composition for flat cross section glass fiber of the present invention, have excellent flattening stability, flattening ratio stability, and glass fiber spinning stability.
[0106] On the other hand, from Table 2, Na 2 K content relative to O content 2 The ratio of the content of O (K 2 O / Na 2The flat cross section glass fiber of Comparative Example 1, which contains a plurality of flat cross section glass filaments made of a glass composition for flat cross section glass fiber in which the value of Na is less than 0.05, is unable to have sufficient flatness ratio stability. 2 K content relative to O content 2 The ratio of the content of O (K 2 O / Na 2 It is clear that the flat cross section glass fiber of Comparative Example 2, which contains a plurality of flat cross section glass filaments made of a glass composition for flat cross section glass fiber in which the value of (O) is 0.50 or more and 1.00, does not have sufficient flattening stability.
[0107] Also, from Table 2, Fe 2 O 3 The ratio of the MgO content to the Fe content (MgO / Fe 2 O 3 A flat cross section glass fiber of Comparative Example 3, which contains a plurality of flat cross section glass filaments made of a glass composition for flat cross section glass fiber, in which the tensile strength (Tb) of the glass composition for flat cross section glass fiber is 10.00 or more and 11.45, and Fe 2 O 3 The ratio of the MgO content to the Fe content (MgO / Fe 2 O 3 It is clear that the flat cross section glass fiber of Comparative Example 4, which contains a plurality of flat cross section glass filaments made of a glass composition for flat cross section glass fiber in which the aspect ratio is 3.65, which is less than 4.10, does not have sufficient aspect ratio stability.
[0108] Furthermore, the C, M, T, and NK do not satisfy the formula (1), and (C×M×T / NK) 1/2 The flat cross section glass fiber of Comparative Example 5 contains a plurality of flat cross section glass filaments made of a glass composition for a flat cross section glass fiber in which the value of C×M×T / NK is 4.02, which is greater than 3.75. 1/2 It is clear that the flat cross section glass fiber of Comparative Example 6, which contains a plurality of flat cross section glass filaments made of a glass composition for flat cross section glass fiber having a value of 2.86, which is less than 3.00, does not have sufficient glass fiber spinning stability.
Claims
1. A glass composition for flat cross section glass fiber, comprising 50.00 to 60.00 mass % of SiO based on the total amount of the glass composition for flat cross section glass fiber. 2 and Al in the range of 9.00 to 18.00 mass% 2 O 3 and B in the range of 3.00 to 9.00 mass% 2 O 3 %, CaO in the range of 15.00 to 30.00 mass%, MgO in the range of 0.10 to 5.00 mass%, and Fe in the range of 0.01 to 1.00 mass%. 2 O 3 and TiO in the range of 0.01 to 1.00 mass%. 2 and a total of 0.10 to 2.00 mass% Na 2 O and K 2 O, 2 K vs. O content 2 Ratio of O content (K 2 O / Na 2 O) is in the range of 0.05 or more and less than 0.50, 2 O 3 The ratio of the MgO content to the Fe content (MgO / Fe 2 O 3 ) is in the range of 4.10 or more and less than 10.00, the CaO content is C, the MgO content is M, and the TiO 2 The content of T, the Na 2 O and K 2 A glass composition for flat cross section glass fiber, characterized in that C, M, T and NK satisfy the following formula (1), where NK is the total content of O: 3.00≦(C×M×T / NK) 1/2 ≦3.75 ... (1) 2. A flat cross-section glass fiber comprising a plurality of flat cross-section glass filaments having a flat cross-sectional shape with a major axis of a predetermined range length and a minor axis of a predetermined range length, characterized in that the flat cross-section glass filaments are made of the glass composition for flat cross-section glass fiber according to claim 1.
3. A method for producing a flat cross-section glass fiber from a glass raw material containing a glass recycled material, comprising obtaining a flat cross-section glass filament having a flat cross-sectional shape with a major axis of a predetermined range and a minor axis of a predetermined range, and bundling a plurality of the flat cross-section glass filaments, wherein the glass raw material contains a glass recycled material in a range of 1.0 to 50.0 mass% based on the total amount, and the flat cross-section glass filament has SiO in a range of 50.00 to 60.00 mass% based on the total amount of the flat cross-section glass filament. 2 and Al in the range of 9.00 to 18.00 mass% 2 O 3 and B in the range of 3.00 to 9.00 mass% 2 O 3 %, CaO in the range of 15.00 to 30.00 mass%, MgO in the range of 0.10 to 5.00 mass%, and Fe in the range of 0.01 to 1.00 mass%. 2 O 3 and TiO in the range of 0.01 to 1.00 mass%. 2 and a total of 0.10 to 2.00 mass% Na 2 O and K 2 O, and the Na 2 K vs. O content 2 Ratio of O content (K 2 O / Na 2 O) is in the range of 0.05 or more and less than 0.50, 2 O 3 The ratio of the MgO content to the Fe content (MgO / Fe 2 O 3 ) is in the range of 4.10 or more and less than 10.00, and the CaO content C, the MgO content M, and the TiO 2 The content T of the Na 2 O and K 2 A method for producing a flat cross section glass fiber from a glass raw material containing a recycled glass material, characterized in that the total content NK of O satisfies the following formula (1): 3.00≦(C×M×T / NK) 1/2 ≦3.75 ... (1)