Surface-treated steel sheet and method of producing same

MYPI2025002294A0Undetermined Publication Date: 2024-05-24JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025002294
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-11-24
Filing Date
2023-07-07
Publication Date
2024-05-24

AI Technical Summary

Technical Problem

The existing surface-treated steel sheets have poor adhesion to BPA-free paints, which lacks sufficient corrosion resistance, and are manufactured using hexavalent chromium, which is being regulated due to environmental concerns.

Method used

A surface-treated steel sheet with a Sn plating layer and a film layer containing Zr oxide and Ti oxide, where the contact angle of ethylene glycol is 50° or less and the total atomic ratio of K, Na, Mg, and Ca is 5.0% or less, is manufactured without using hexavalent chromium, ensuring excellent adhesion to BPA-free paints.

Benefits of technology

The solution provides a surface-treated steel sheet with excellent adhesion to BPA-free paints, maintaining corrosion resistance and adhering to environmental regulations by eliminating hexavalent chromium in the manufacturing process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a surface-treated steel sheet that can be produced without the use of hexavalent chromium and that has excellent adhesion to BPA-free paint. A surface-treated steel sheet having, on at least one surface of a steel sheet, a Sn plating layer and a coating layer disposed on the Sn plating layer and containing at least one of Zr oxide and Ti oxide, wherein a contact angle of ethylene glycol is 50° or less, and a total atomic ratio of K, Na, Mg, and Ca adsorbed on a surface of the steel sheet to all elements is 5.0 % or less.
Need to check novelty before this filing date? Find Prior Art

Description

Surface-treated steel sheet and its manufacturing method

[0001] The present invention relates to a surface-treated steel sheet, particularly to a surface-treated steel sheet having excellent adhesion to BPA (bisphenol A)-free paint. The surface-treated steel sheet of the present invention can be suitably used for containers such as cans. The present invention also relates to a method for manufacturing the surface-treated steel sheet.

[0002] Sn-plated steel sheet (tinplate), a type of surface-treated steel sheet, is widely used as a material for various metal cans such as beverage cans, food cans, pail cans, and 18-liter cans because it has excellent corrosion resistance, weldability, and workability, and is easy to manufacture.

[0003] The surface of the surface-treated steel sheets used for these applications is coated with an organic resin coating, such as an epoxy-based paint, to accommodate various contents. When the organic resin coating is applied, a chromium oxide layer formed on the outermost surface by electrolyzing or immersing the steel sheet in an aqueous solution containing hexavalent chromium plays an important role. That is, the chromium oxide layer achieves excellent adhesion to the organic resin coating layer, thereby ensuring corrosion resistance against various contents (Patent Documents 1 to 5).

[0004] On the other hand, it has been suggested that BPA contained in epoxy-based paints may have harmful effects on humans. Therefore, development of BPA-free paints using polyester-based resins that do not contain BPA is underway (Patent Documents 6 and 7), and there is a demand for them to replace epoxy-based paints. However, tinplate, which has been used as steel sheet for cans until now, has poorer adhesion to BPA-free paints than to epoxy-based paints. Therefore, sufficient corrosion resistance against various contents cannot be ensured, and the application of BPA-free paints to various metal cans has not progressed at present.

[0005] Furthermore, in recent years, due to growing environmental awareness, there has been a trend toward restricting the use of hexavalent chromium worldwide, and therefore, in the field of surface-treated steel sheets used for various metal cans, there is a demand for the establishment of a manufacturing method that does not use hexavalent chromium.

[0006] As a method for producing a surface-treated steel sheet without using hexavalent chromium, for example, a method proposed in Patent Document 8 is known. In this method, a surface-treated steel sheet is proposed in which a coating containing a zirconium compound is formed on the surface of a Sn-plated steel sheet.

[0007] Japanese Patent Laid-Open No. 58-110695 Japanese Patent Laid-Open No. 55-134197 Japanese Patent Laid-Open No. 57-035699 Japanese Patent Laid-Open No. 11-117085 Japanese Patent Laid-Open No. 2007-231394 Japanese Patent Laid-Open No. 2013-144753 Japanese Patent Laid-Open No. 2008-050486 Japanese Patent Laid-Open No. 2018-135569

[0008] According to the method proposed in Patent Document 8, a surface treatment layer can be formed without using hexavalent chromium, and according to Patent Document 8, the method can provide a surface-treated steel sheet having excellent adhesion to an epoxy-based paint.

[0009] However, the surface-treated steel sheet obtained by the conventional method proposed in Patent Document 8 has excellent adhesion to epoxy-based paints, but poor adhesion to BPA-free paints, resulting in insufficient corrosion resistance to BPA-free paints. Therefore, it has not been possible to replace the BPA-free paint with a BPA-free paint while maintaining corrosion resistance to various contents.

[0010] Therefore, there is a demand for a surface-treated steel sheet that can be produced without using hexavalent chromium and has excellent adhesion to BPA-free paints.

[0011] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a surface-treated steel sheet that can be produced without using hexavalent chromium and has excellent adhesion to a BPA-free paint.

[0012] As a result of extensive research into achieving the above object, the inventors of the present invention have discovered the following (1) and (2).

[0013] (1) In a surface-treated steel sheet having a coating layer containing at least one of Zr oxide and Ti oxide on a Sn-plated layer, the contact angle of ethylene glycol and the total atomic ratio of K, Na, Mg, and Ca adsorbed on the surface to all elements can be controlled within specific ranges, thereby providing a surface-treated steel sheet with excellent adhesion to BPA-free paints.

[0014] (2) The above-mentioned surface-treated steel sheet can be produced by forming a coating, conditioning the surface under predetermined conditions, and then performing a final water wash using water having an electrical conductivity of a predetermined value or less.

[0015] The present invention has been completed based on the above findings. The gist of the present invention is as follows.

[0016] 1. A surface-treated steel sheet having a Sn-plated layer on at least one surface of the steel sheet, and a coating layer containing at least one of Zr oxide and Ti oxide disposed on the Sn-plated layer, wherein the surface-treated steel sheet has a contact angle with ethylene glycol of 50° or less, and the total atomic ratio of K, Na, Mg, and Ca adsorbed on the surface to all elements is 5.0% or less.

[0017] 2. The Sn plating layer has an Sn coating amount of 0.1 to 20.0 g / m per one side of the steel sheet. 2 2. The surface-treated steel sheet according to 1 above,

[0018] 3. The total amount of Zr oxide and Ti oxide deposited in the coating layer is 0.3 to 50.0 mg / m per side of the steel sheet in terms of the amount of metal Zr and the amount of metal Ti. 2 3. The surface-treated steel sheet according to 1 or 2 above,

[0019] 4. The coating layer further contains P, and the P deposition amount is 50.0 mg / m per one side of the steel sheet. 2 4. The surface-treated steel sheet according to any one of claims 1 to 3, wherein:

[0020] 5. The coating layer further contains Mn, and the Mn coating amount is 50.0 mg / m per one side of the steel sheet. 2 5. The surface-treated steel sheet according to any one of claims 1 to 4, wherein:

[0021] 6. The surface-treated steel sheet according to any one of the above items 1 to 5, further comprising a Ni-containing layer disposed below the Sn-plated layer.

[0022] 7. The Ni-containing layer has a Ni deposition amount of 2 mg / m per one side of the steel sheet. 2 ~2000mg / m 2 7. The surface-treated steel sheet according to claim 6, wherein:

[0023] 8. A method for producing a surface-treated steel sheet having a Sn plating layer on at least one surface of the steel sheet and a coating layer containing at least one of Zr oxide and Ti oxide disposed on the Sn plating layer, the method comprising: a coating formation step of treating the surface of a steel sheet having a Sn plating layer on at least one surface with an aqueous solution containing at least one of Zr ions and Ti ions to form the coating layer on the Sn plating layer; and applying the aqueous solution to the surface of the coating layer in an amount of 1.0 to 30.0 g / m. 2 a surface conditioning step of holding the steel sheet in a state where the surface is present for 0.1 to 20.0 seconds; and a water rinsing step of rinsing the steel sheet with water at least once after the surface conditioning step, wherein in the water rinsing step, water having an electrical conductivity of 100 μS / m or less is used in at least the final water rinsing.

[0024] 9. The method for producing a surface-treated steel sheet according to the above item 8, wherein the surface-treated steel sheet further has a Ni-containing layer disposed below the Sn-plated layer.

[0025] According to the present invention, it is possible to provide a surface-treated steel sheet that has excellent adhesion to BPA-free paint without using hexavalent chromium. The surface-treated steel sheet of the present invention can be suitably used as a material for containers, etc.

[0026] A method for carrying out the present invention will be specifically described below. Note that the following description shows an example of a preferred embodiment of the present invention, and the present invention is not limited thereto.

[0027] A surface-treated steel sheet according to one embodiment of the present invention has a Sn-plated layer on at least one surface of the steel sheet, and a coating layer disposed on the Sn-plated layer, the coating layer containing at least one of Zr oxide and Ti oxide. It is important in the present invention that the contact angle of ethylene glycol with the surface-treated steel sheet is 50° or less, and that the total atomic ratio of K, Na, Mg, and Ca adsorbed on the surface to all elements is 5.0% or less. Each of the constituent elements of the surface-treated steel sheet is described below.

[0028] [Steel Sheet] The steel sheet is not particularly limited and any steel sheet can be used, but it is preferable to use a steel sheet for cans. For example, an ultra-low carbon steel sheet or a low carbon steel sheet can be used as the steel sheet. The manufacturing method of the steel sheet is also not particularly limited and a steel sheet manufactured by any method can be used, but typically a cold-rolled steel sheet can be used. The cold-rolled steel sheet can be manufactured by a general manufacturing process that includes, for example, hot rolling, pickling, cold rolling, annealing, and temper rolling.

[0029] The composition of the steel sheet is not particularly limited, but the steel sheet may contain C, Mn, Cr, P, S, Si, Cu, Ni, Mo, Al, and unavoidable impurities within a range that does not impair the effects of the present invention. In this case, for example, a steel sheet having a composition specified in ASTM A623M-09 can be suitably used as the steel sheet.

[0030] In one embodiment of the present invention, the composition is, in mass%, C: 0.0001 to 0.13%, Si: 0 to 0.020%, Mn: 0.01 to 0.60%, P: 0 to 0.020%, S: 0 to 0.030%, Al: 0 to 0.20%, N: 0 to 0.040%, Cu: 0 to 0.20%, Ni: 0 to 0.15%, Cr: 0 to 0.10%, Mo: 0 to 0.05%, Ti: 0 to 0.020%, Nb: 0 to 0.020%, B: 0 to 0.020%, Ca: 0 to 0.020%, Sn: 0 to 0.020%, Sb: 0 to 0.020%, It is preferable to use a steel sheet having a composition consisting of Cr, P, S, Al, and N, and the balance being Fe and unavoidable impurities. Of the above composition, the lower the content of Si, P, S, Al, and N, the more preferable it is. Cu, Ni, Cr, Mo, Ti, Nb, B, Ca, Sn, and Sb are components that can be added as desired.

[0031] The lower limit of the thickness of the steel plate is not particularly limited, but the thickness is preferably 0.10 mm or more. The upper limit of the thickness is not particularly limited, but the thickness is preferably 0.60 mm or less. Here, "steel plate" is defined to include "steel strip."

[0032] [Sn-plated layer] The Sn-plated layer may be provided on at least one surface of the steel sheet, or may be provided on both surfaces. The Sn-plated layer may cover at least a portion of the steel sheet, or may cover the entire surface on which the Sn-plated layer is provided. The Sn-plated layer may be a continuous layer or a discontinuous layer. An example of the discontinuous layer is a layer having an island structure.

[0033] The Sn-plated layer also includes a layer in which a portion of the Sn-plated layer is alloyed. For example, a layer in which a portion of the Sn-plated layer is turned into a Sn alloy layer by a heat-melting treatment after Sn plating is also included in the Sn-plated layer. Examples of the Sn alloy layer include an Fe—Sn alloy layer and an Fe—Sn—Ni alloy layer.

[0034] For example, by heating and melting the Sn by electrical heating or the like after Sn plating, a part of the Sn-plated layer on the steel sheet side can be made into an Fe—Sn alloy layer. Also, by plating a steel sheet having a Ni-containing layer on its surface with Sn and then heating and melting the Sn by electrical heating or the like, a part of the Sn-plated layer on the steel sheet side can be made into one or both of an Fe—Sn—Ni alloy layer and an Fe—Sn alloy layer.

[0035] The Sn coating weight in the Sn plating layer is not particularly limited and can be any amount. However, from the viewpoint of further improving the appearance and corrosion resistance of the surface-treated steel sheet, it is preferable that the Sn coating weight is 20.0 g / m per one side of the steel sheet. 2 From the same viewpoint, it is preferable that the Sn deposition amount is 0.1 g / m or less. 2 It is preferable that the density is 0.2 g / m or more. 2 From the viewpoint of further improving the workability, the Sn deposition amount is more preferably 1.0 g / m or more. 2 More preferably, it is set to the above.

[0036] The Sn deposition amount can be measured by the electrolytic stripping method specified in JIS G 3303.

[0037] The formation of the Sn plating layer is not particularly limited and can be performed by any method, such as electroplating or hot-dip plating. When the Sn plating layer is formed by electroplating, any plating bath can be used. Examples of plating baths that can be used include a phenolsulfonic acid Sn plating bath, a methanesulfonic acid Sn plating bath, and a halogen-based Sn plating bath.

[0038] After the Sn plating layer is formed, a reflow treatment may be performed. When the reflow treatment is performed, the Sn plating layer is heated to a temperature equal to or higher than the melting point of Sn (231.9°C), thereby forming an alloy layer such as an Fe—Sn alloy layer underneath (on the steel sheet side of) the unalloyed Sn plating layer. Furthermore, if the reflow treatment is omitted, a Sn-plated steel sheet having an unalloyed Sn plating layer is obtained.

[0039] The surface side of the Sn-plated layer may contain Sn oxides, or may not contain any Sn oxides at all. However, from the viewpoint of improving coating secondary adhesion, which is adhesion to a paint in a humid environment, and sulfide staining resistance, it is preferable that the surface side of the Sn-plated layer contain Sn oxides. Sn oxides can be formed during a reflow treatment or by dissolved oxygen contained in the rinsing water after Sn plating, but it is preferable to control the amount of Sn oxides contained in the Sn-plated layer by a pretreatment, which will be described later.

[0040] [Ni-containing layer] The surface-treated steel sheet may further include an optional Ni-containing layer. For example, the surface-treated steel sheet according to one embodiment of the present invention may further include an Ni-containing layer disposed below the Sn-plated layer. In other words, the surface-treated steel sheet according to one embodiment of the present invention may include, on at least one surface of the steel sheet, a Ni-containing layer, a Sn-plated layer disposed on the Ni-containing layer, and a coating layer containing at least one of Zr oxide and Ti oxide disposed on the Sn-plated layer.

[0041] The Ni-containing layer can be any layer containing nickel, and for example, one or both of a Ni layer and a Ni alloy layer can be used. Examples of the Ni layer include a Ni plating layer. Examples of the Ni alloy layer include a Ni—Fe alloy layer. Furthermore, by forming a Sn plating layer on the Ni-containing layer and then performing a reflow treatment, an Fe—Sn—Ni alloy layer or an Fe—Sn alloy layer can be formed below the unalloyed Sn plating layer (on the steel sheet side).

[0042] The method for forming the Ni-containing layer is not particularly limited, and any method can be used, such as electroplating. When a Ni—Fe alloy layer is formed as the Ni-containing layer, the Ni layer can be formed on the steel sheet surface by a method such as electroplating, and then annealed to form the Ni—Fe alloy layer.

[0043] The Ni deposition amount of the Ni-containing layer is not particularly limited, but from the viewpoint of improving resistance to sulfide blackening, the Ni deposition amount per one surface of the steel sheet is set to 2 mg / m 2 From the viewpoint of cost, it is preferable that the Ni deposition amount per one side of the steel sheet is 2000 mg / m or more. 2 It is preferable to do the following:

[0044] The Ni deposition weight of the Ni-containing layer is measured by a calibration curve method using fluorescent X-rays. First, a plurality of steel sheets with known Ni deposition weights are prepared, and the fluorescent X-ray intensities derived from Ni are measured for the steel sheets in advance. A calibration curve is then obtained by linearly approximating the relationship between the measured fluorescent X-ray intensities and the Ni deposition weights. Next, the fluorescent X-ray intensities derived from Ni of the surface-treated steel sheet are measured, and the Ni deposition weight of the Ni-containing layer can be determined using the calibration curve.

[0045] [Coating Layer] A coating layer containing at least one of Zr oxide and Ti oxide is present on the Sn-plated layer. The inclusion of at least one of Zr oxide and Ti oxide in the coating layer is necessary to obtain excellent adhesion with BPA-free paint.

[0046] There is no particular lower limit to the total amount of Zr oxide and Ti oxide attached in the coating layer. However, from the viewpoint of further improving adhesion to the BPA-free paint, the total amount of Zr oxide and Ti oxide attached is preferably 0.3 mg / m2 per one side of the steel sheet in terms of the amount of metal Zr and the amount of metal Ti. 2 More than 0.4 mg / m 2 More preferably, 0.5 mg / m or more 2 The above is more preferable. On the other hand, there is no particular upper limit on the total adhesion amount of Zr oxide and Ti oxide in the coating layer. However, if the total adhesion amount of Zr oxide and Ti oxide is excessively large, cohesive failure of the coating layer may occur, which may impair adhesion to the BPA-free paint. Therefore, from the viewpoint of ensuring more stable adhesion to the BPA-free paint, the total adhesion amount of Zr oxide and Ti oxide, in terms of the amount of metal Zr and the amount of metal Ti, is 50.0 mg / m per one side of the steel sheet. 2 Preferably, 45.0 mg / m or less 2More preferably, 40.0 mg / m or less 2 The following is more preferable: When calculating the total adhesion weight of Zr oxide and Ti oxide, the adhesion weight of Zr oxide is calculated as a value converted into the amount of metallic Zr, and the adhesion weight of Ti oxide is calculated as a value converted into the amount of metallic Ti.

[0047] The amount of Zr oxide attached in the coating layer is measured by a calibration curve method using fluorescent X-rays. First, a plurality of steel sheets with known amounts of attached metal Zr are prepared, and the fluorescent X-ray intensity derived from Zr for the steel sheets is measured in advance. A calibration curve is then created by linearly approximating the relationship between the measured fluorescent X-ray intensity and the amount of attached metal Zr. Next, the fluorescent X-ray intensity derived from Zr of the surface-treated steel sheet is measured, and the amount of attached Zr oxide in the coating layer can be determined in terms of metallic Zr using the calibration curve.

[0048] The amount of Ti oxide in the coating layer is measured by a calibration curve method using fluorescent X-rays. First, a plurality of steel sheets with known amounts of Ti deposited are prepared, and the fluorescent X-ray intensity derived from Ti is measured for each steel sheet in advance. A calibration curve is then prepared by linearly approximating the relationship between the measured fluorescent X-ray intensity and the amount of Ti deposited. Next, the fluorescent X-ray intensity derived from Ti in the surface-treated steel sheet is measured, and the above-mentioned calibration curve can be used to determine the amount of Ti oxide deposited in the coating layer in terms of metallic Ti.

[0049] The coating layer may contain P from the viewpoint of further improving adhesion with the BPA-free paint. There is no particular upper limit on the amount of P contained in the coating layer, but since cohesive failure of the coating layer may impair adhesion with the BPA-free paint, it is recommended to limit the amount to 50.0 mg / m per steel sheet surface. 2 The lower limit of the amount of P contained in the coating layer is not particularly limited, and is, for example, 0.0 mg / m 2 or may not be contained at all.

[0050] The amount of P deposited in the coating layer is measured by a calibration curve method using fluorescent X-rays. First, a plurality of steel sheets with known amounts of P deposited are prepared, and the fluorescent X-ray intensity derived from P is measured for the steel sheets in advance. A calibration curve is then prepared by linearly approximating the relationship between the measured fluorescent X-ray intensity and the amount of P deposited. Next, the fluorescent X-ray intensity derived from P of the surface-treated steel sheet is measured, and the amount of P deposited in the coating layer can be determined using the calibration curve.

[0051] The coating layer may contain Mn from the viewpoint of further improving adhesion with the BPA-free paint. There is no particular upper limit on the amount of Mn contained in the coating layer, but since cohesive failure of the coating layer may impair adhesion with the BPA-free paint, it is recommended to limit the amount to 50.0 mg / m per side of the steel sheet. 2 The lower limit of the amount of Mn contained in the coating layer is not particularly limited, and is, for example, 0.0 mg / m 2 or may not be contained at all.

[0052] The Mn deposition amount in the coating layer is measured by a calibration curve method using fluorescent X-rays. First, a plurality of steel sheets with known Mn deposition amounts are prepared, and the fluorescent X-ray intensity derived from Mn for the steel sheets is measured in advance. A calibration curve is then prepared by linearly approximating the relationship between the measured fluorescent X-ray intensity and the Mn deposition amount. Next, the fluorescent X-ray intensity derived from Mn of the surface-treated steel sheet is measured, and the Mn deposition amount in the coating layer can be determined using the calibration curve.

[0053] The coating layer may contain Sn. The upper limit of the Sn content in the coating layer is not particularly limited. The coating layer may not contain Sn, and the upper limit is 0.0 mg / m 2 It may be.

[0054] The coating layer may contain C. There is no particular upper limit to the C content in the coating layer. The coating layer may not contain C, and the upper limit is 0.0 mg / m 2 It may be.

[0055] The coating layer may contain elements other than Zr, Ti, O, Sn, Mn, P, Ni, and C, as well as K, Na, Mg, and Ca, as described below. Examples of elements other than these include metal impurities such as Cu, Zn, and Fe, and elements such as S, N, F, Cl, Br, and Si, which are contained in the aqueous solution used in the coating formation process described below. However, if elements other than Zr, Ti, O, Sn, Mn, P, Ni, C, K, Na, Mg, and Ca are present in excess, adhesion to the BPA-free paint may be reduced. Therefore, the total content of elements other than Zr, Ti, O, Sn, Mn, P, Ni, C, K, Na, Mg, and Ca in the coating layer is preferably 30% or less, and more preferably 20% or less, in atomic ratio. The coating layer may not contain elements other than Zr, Ti, O, Sn, Mn, P, Ni, C, K, Na, Mg, and Ca, and may be 0% in atomic ratio. The content of the above elements can be measured by XPS (X-ray photoelectron spectroscopy).

[0056] [Contact Angle of Ethylene Glycol] In the present invention, it is important that the contact angle of ethylene glycol of the surface-treated steel sheet is 50° or less. By controlling the surface of the surface-treated steel sheet so that the contact angle of ethylene glycol is 50° or less, a strong bond is formed between the polyester resin contained in the BPA-free paint and the surface-treated steel sheet, resulting in high adhesion to the BPA-free paint. From the viewpoint of further improving adhesion to the BPA-free paint, the contact angle of ethylene glycol is preferably 48° or less, and more preferably 45° or less. Since the lower the contact angle of ethylene glycol, the better from the viewpoint of improving adhesion to the BPA-free paint, the lower limit is not particularly limited and may be 0°. However, from the viewpoint of ease of production, it may be 5° or more, or even 8° or more.

[0057] Furthermore, the surface of the surface-treated steel sheet of the present invention, i.e., the surface state of the coating layer containing at least one of Zr oxide and Ti oxide, is stable against heat, and the contact angle of ethylene glycol does not change significantly, even after heat treatment equivalent to paint baking. It is believed that the thermal stability of such a surface state also contributes to improved adhesion with BPA-free paint. Therefore, the contact angle of ethylene glycol of the surface-treated steel sheet after heat treatment equivalent to paint baking is preferably 50° or less, more preferably 48° or less, and even more preferably 45° or less. Furthermore, the lower limit of the contact angle of ethylene glycol of the surface-treated steel sheet after heat treatment equivalent to paint baking is not particularly limited and may be 0°, but the contact angle may be 5° or more, or even 8° or more. The conditions for the heat treatment equivalent to paint baking are a maximum temperature of 200°C and a holding time at the maximum temperature of 10 minutes.

[0058] Although the mechanism by which the contact angle of ethylene glycol on the surface-treated steel sheet becomes 50° or less is not clear, it is thought that the micro-roughness of the surface is adjusted in the surface conditioning step described below, and the surface is modified to have a high affinity for ethylene glycol. If the surface conditioning step described below is not carried out, even if the surface of the surface-treated steel sheet has a high affinity for ethylene glycol immediately after production, the coating layer cannot be fixed in a state with such high affinity, and the contact angle of ethylene glycol exceeds 50°.

[0059] The contact angle of ethylene glycol can be measured by the θ / 2 method. In this measurement, the temperature of the surface-treated steel sheet to be measured is set to 20°C, and ethylene glycol at a temperature of 20°C is dropped onto the surface of the surface-treated steel sheet. The contact angle 1 second after the drop is calculated by the θ / 2 method. More specifically, the contact angle can be measured by the method described in the Examples. The surface of the surface-treated steel sheet may be coated with an anti-rust oil such as CSO (cottonseed oil), DOS (dioctyl sebacate), or ATBC (acetyl tributyl citrate). If the surface-treated steel sheet is coated with oil, the coating-equivalent heat treatment is performed to evaporate the coated oil, and the contact angle measured by the method described in the Examples is used as the contact angle of ethylene glycol on the coated surface-treated steel sheet. As described above, the surface-treated steel sheet of the present invention is stable against heat treatment. Therefore, it is believed that the effects of the present invention can also be achieved on the surface-treated steel sheet before the heat treatment, provided that the contact angle measured after the heat treatment and the atomic ratio of the adsorbed element, described below, satisfy the conditions of the present invention. Although additive components such as rust inhibitors contained in the applied oil may remain on the surface of the coated steel sheet even after heat treatment equivalent to painting, the amount is so small that it does not affect the contact angle of ethylene glycol or the atomic ratio of the adsorbed elements described above.

[0060] It has been reported that in surface-treated steel sheets manufactured using conventional hexavalent chromium baths such as those proposed in Patent Documents 1 to 5, the composition of the chromium hydrate oxide layer present on the surface significantly affects adhesion to epoxy-based paints in humid environments. In humid environments, water that penetrates the epoxy-based paint film inhibits adhesion at the interface between the epoxy-based paint film and the chromium hydrate oxide layer. Therefore, it was thought that the presence of a large number of hydrophilic OH groups in the chromium hydrate oxide layer would promote water spreading and wetting at the interface, resulting in a decrease in adhesive strength. Therefore, in conventional surface-treated steel sheets, the reduction of OH groups due to the progression of oxidation of chromium hydrate oxide, i.e., the hydrophobicization of the surface, improved adhesion to epoxy-based paints in humid environments.

[0061] In contrast, the present invention focuses on ethylene glycol rather than water and has found that by adjusting the surface to have a high affinity for ethylene glycol, strong adhesion with BPA-free paints can be ensured. Therefore, it can be said that the present invention is based on a technical concept that is completely different from the above-mentioned prior art. The mechanism by which adjusting the surface to have a high affinity for ethylene glycol improves adhesion with BPA-free paints is unclear. However, because ethylene glycol is one of the hydroxyl group monomers that constitute the polyester resin that makes up BPA-free paints, it is presumed that adjusting the surface to have a high affinity for ethylene glycol improves adhesion with BPA-free paints.

[0062] [Atomic Ratio of Adsorbed Elements] As described above, the surface of the surface-treated steel sheet of the present invention has a contact angle with ethylene glycol of 50° or less, and its surface is chemically active. Therefore, cations of elements such as K, Na, Mg, and Ca are easily adsorbed onto the surface of the surface-treated steel sheet. The inventors have found that simply reducing the contact angle with ethylene glycol to 50° or less does not achieve the intended adhesion due to the influence of the adsorbed cations. In the present invention, the adhesion to BPA-free paint can be improved by reducing the amount of the cations adsorbed on the surface of the surface-treated steel sheet.

[0063] Specifically, the total atomic ratio of K, Na, Mg, and Ca adsorbed on the surface of the surface-treated steel sheet relative to all elements is set to 5.0% or less, preferably 3.0% or less, and more preferably 1.0% or less. Since the lower the total atomic ratio, the better, the lower limit is not particularly limited and may be 0.0%. The total atomic ratio can be measured by XPS. In this measurement, the atomic ratios of K, Na, Mg, and Ca relative to all elements can be determined by the relative sensitivity factor method from the integrated intensities of the narrow spectra of K2p, Na1s, Ca2p, and Mg1s at the outermost surface of the surface-treated steel sheet. More specifically, the measurement can be performed using the method described in the Examples. Note that if the surface-treated steel sheet is oiled, the atomic ratios measured by the method described in the Examples after the oiling process are determined as the atomic ratios of the adsorbed elements on the surface-treated steel sheet after oiling, after the coating-equivalent heat treatment is performed to vaporize the oil.

[0064] [Manufacturing Method] In a manufacturing method of a surface-treated steel sheet according to one embodiment of the present invention, a surface-treated steel sheet having the above-described properties can be manufactured by the method described below.

[0065] A method for producing a surface-treated steel sheet according to one embodiment of the present invention is a method for producing a surface-treated steel sheet having a Sn-plated layer and a coating layer disposed on the Sn-plated layer on at least one surface of the steel sheet, and includes the following steps (1) to (3). Each step will be described below. (1) Coating formation step (2) Surface conditioning step (3) Water washing step

[0066] In one embodiment of the present invention, the surface-treated steel sheet may further have a Ni-containing layer disposed under the Sn-plated layer. When producing a surface-treated steel sheet having a Ni-containing layer, a steel sheet having a Ni-containing layer on at least one surface and a Sn-plated layer disposed on the Ni-containing layer may be subjected to the film formation step.

[0067] [Film Formation Step] In the film formation step, a surface of a steel sheet having a Sn-plated layer on at least one side thereof is treated with an aqueous solution containing at least one of Zr ions and Ti ions to form a film layer on the Sn-plated layer. The formed film layer is a film layer containing at least one of Zr oxide and Ti oxide.

[0068] The treatment with the aqueous solution is not particularly limited and can be carried out by any method. The treatment can be carried out, for example, by electrolysis. When the treatment is carried out by electrolysis, it is preferable to subject the steel sheet having the Sn plating layer to cathodic electrolysis in the aqueous solution. For the cathodic electrolysis, conventional equipment used for chromate treatment and the like can be used as is. Therefore, from the viewpoint of reducing equipment costs, it is preferable to form the coating layer by cathodic electrolysis.

[0069] The method for preparing the aqueous solution is not particularly limited, but for example, the aqueous solution can be prepared by dissolving one or both of a Zr-containing compound as a Zr ion source and a Ti-containing compound as a Ti ion source in water. The water can be distilled water or deionized water, but is not limited thereto, and any water can be used.

[0070] The Zr-containing compound and the Ti-containing compound may be any compound capable of supplying Zr ions and Ti ions, respectively. Examples of the Zr-containing compound include ZrF 4 Zr salts such as H 2 ZrF 6 Ya K 2 ZrF 6 It is preferable to use a Zr complex such as ZrF. Zr ions become Zr oxide as the pH on the surface of the cathode increases, forming a film. Examples of the Ti-containing compound include TiF. 4 Ti salts such as, or H 2 TiF 6 Ya K 2 TiF 6 It is preferable to use a Ti complex such as Ti ions, which turn into Ti oxides as the pH on the surface of the cathode increases, forming a film.

[0071] The aqueous solution may further contain at least one selected from the group consisting of fluoride ions, nitrate ions, ammonium ions, phosphate ions, Mn ions, and sulfate ions. When the aqueous solution contains both nitrate ions and ammonium ions, treatment can be completed in a short time of several seconds to several tens of seconds, which is extremely advantageous industrially. Therefore, it is preferable that the aqueous solution contains both nitrate ions and ammonium ions in addition to at least one of Zr ions and Ti ions. Hereinafter, the unit of ion concentration, "ppm," refers to parts per million by mass unless otherwise specified.

[0072] When the aqueous solution contains Zr ions, the lower limit of the Zr ion concentration is not particularly limited, but is preferably 100 ppm or more. The upper limit of the Zr ion concentration is also not particularly limited, but is preferably 4000 ppm or less. Similarly, when the aqueous solution contains Ti ions, the lower limit of the Ti ion concentration is not particularly limited, but is preferably 100 ppm or more. The upper limit of the Ti ion concentration is also not particularly limited, but is preferably 4000 ppm or less.

[0073] Furthermore, when the aqueous solution contains fluoride ions, the lower limit of the fluoride ion concentration is not particularly limited, but is preferably 120 ppm or more. The upper limit of the fluoride ion concentration is also not particularly limited, but is preferably 4000 ppm or less. When the aqueous solution contains phosphate ions, the lower limit of the phosphate ion concentration is not particularly limited, but is preferably 50 ppm or more. The upper limit of the phosphate ion concentration is also not particularly limited, but is preferably 5000 ppm or less. When the aqueous solution contains Mn ions, the lower limit of the Mn ion concentration is not particularly limited, but is preferably 50 ppm or more. The upper limit of the Mn ion concentration is also not particularly limited, but is preferably 5000 ppm or less. When the aqueous solution contains ammonium ions, the lower limit of the ammonium ion concentration is not particularly limited, but may be 0 ppm. The upper limit of the ammonium ion concentration is also not particularly limited, but is preferably 20000 ppm or less. When the aqueous solution contains nitrate ions, the lower limit of the nitrate ion concentration is not particularly limited, but may be 0 ppm. The upper limit of the nitrate ion concentration is not particularly limited, but is preferably 20,000 ppm or less. When the aqueous solution contains sulfate ions, the lower limit of the sulfate ion concentration is not particularly limited, and may be 0 ppm. The upper limit of the sulfate ion concentration is not particularly limited, but is preferably 20,000 ppm or less.

[0074] The upper limit of the temperature of the aqueous solution during cathodic electrolysis is not particularly limited, but is preferably 50°C or lower, for example. Performing cathodic electrolysis at 50°C or lower makes it possible to produce a dense, uniform coating structure consisting of very fine particles. Furthermore, by setting the temperature of the aqueous solution to 50°C or lower, the occurrence of defects, cracks, microcracks, etc. in the coating layer to be formed can be suppressed, and adhesion to BPA-free paint can be further improved. Furthermore, the lower limit of the temperature of the aqueous solution during cathodic electrolysis is also not particularly limited, but is preferably 10°C or higher, for example. By setting the temperature of the aqueous solution to 10°C or higher, the efficiency of coating production can be improved. Furthermore, setting the temperature of the aqueous solution to 10°C or higher is economical because cooling of the aqueous solution is not required even when the outside temperature is high, such as in summer.

[0075] The lower limit of the pH of the aqueous solution is not particularly limited, but is preferably 3 or higher. If the pH is 3 or higher, the production efficiency of Zr oxide or Ti oxide can be further improved. Furthermore, the upper limit of the pH of the aqueous solution is also not particularly limited, but is preferably 5 or lower. If the pH is 5 or lower, it is possible to prevent a large amount of precipitation from occurring in the aqueous solution, and improve continuous productivity.

[0076] For the purpose of adjusting the pH or improving the efficiency of electrolysis, for example, nitric acid, aqueous ammonia, etc. may be added to the aqueous solution.

[0077] The lower limit of the current density during cathodic electrolysis is not particularly limited, but is, for example, 0.05 A / dm 2 It is preferable that the current is 1 A / dm or more. 2 It is more preferable that the current density is 0.05 A / dm or more. 2 If the current density is equal to or greater than 50 A / dm, the efficiency of producing Zr oxide or Ti oxide is improved. As a result, a coating layer containing more stable Zr oxide or Ti oxide can be produced, and the adhesion to the BPA-free paint can be further improved. Furthermore, the upper limit of the current density during cathodic electrolysis is not particularly limited, but it can be set to, for example, 50 A / dm 2 It is preferable that the current is 10 A / dm or less. 2It is more preferable that the current density is 50 A / dm or less. 2 If the temperature is below this level, the efficiency of producing Zr oxide or Ti oxide can be made appropriate, and the production of Zr oxide or Ti oxide, which is coarse and has poor adhesiveness, can be suppressed.

[0078] The electrolysis time in the cathodic electrolysis is not particularly limited, and may be adjusted appropriately depending on the current density so as to obtain the above-mentioned Zr deposition amount and Ti deposition amount.

[0079] The current pattern in the cathodic electrolysis treatment may be continuous or intermittent. Furthermore, the relationship between the aqueous solution and the steel sheet during the cathodic electrolysis is not particularly limited, and they may be stationary or moving relative to each other. However, from the viewpoint of promoting the reaction and improving uniformity, it is preferable to perform cathodic electrolysis while moving the steel sheet and the aqueous solution relative to each other. For example, the steel sheet and the aqueous solution can be moved relative to each other by continuously performing cathodic electrolysis while passing the steel sheet through a treatment tank containing an aqueous solution containing at least one of Zr ions and Ti ions.

[0080] When cathodic electrolysis is performed while moving the steel sheet and the aqueous solution relative to each other, the relative flow velocity between the aqueous solution and the steel sheet is preferably 50 m / min or more. If the relative flow velocity is 50 m / min or more, the pH on the steel sheet surface where hydrogen is generated with current application can be made more uniform, and the generation of coarse Zr oxides or Ti oxides can be effectively suppressed. There is no particular upper limit to the relative flow velocity.

[0081] [Surface Conditioning Step] Next, the coating layer obtained in the coating formation step is subjected to surface conditioning. Specifically, the aqueous solution is applied to the surface of the coating layer in an amount of 1.0 to 30.0 g / m 2 The surface is conditioned under the above conditions, and the coating layer is maintained in the presence of ethylene glycol for 0.1 to 20.0 seconds.

[0082] The mechanism by which the surface conditioning step enables the coating layer to be fixed in a state with high affinity for ethylene glycol is not clear, but is thought to be as follows: By contacting the coating layer with the aqueous solution, the surface of the coating layer is slightly etched, forming fine irregularities on the surface of the coating layer. The effect of these fine irregularities improves the affinity of the coating layer for ethylene glycol. This affinity is different from the affinity due to the presence of hydrophilic functional groups such as OH groups, and is due to the physical structure of the surface roughness, so it also has excellent thermal stability.

[0083] The state of the aqueous solution on the surface of the coating layer is not particularly limited, but from the viewpoint of uniformly progressing etching, it is preferable that the aqueous solution be in the form of a liquid film.

[0084] Amount of aqueous solution: 1.0 to 30.0 g / m 2 The amount of aqueous solution used for surface conditioning was 1.0 g / m 2 If the amount is less than 1.0 g / m, etching will not proceed sufficiently, and as a result, the contact angle of ethylene glycol will be greater than 50°. 2 or more, preferably 2.0 g / m 2 More preferably, 3.0 g / m 2 On the other hand, the amount of the aqueous solution is 30.0 g / m or more. 2 If the amount is more than 30.0 g / m, the affinity for ethylene glycol decreases, and as a result, the contact angle of ethylene glycol becomes larger than 50°. 2 or less, preferably 28.0 g / m 2 or less, more preferably 25.0 g / m 2 The following applies.

[0085] Holding time: 0.1 to 20.0 seconds. Furthermore, if the holding time is less than 0.1 seconds during the surface preparation, etching will not proceed sufficiently, resulting in a contact angle of ethylene glycol exceeding 50°. Therefore, the holding time is set to 0.1 seconds or more, preferably 0.2 seconds or more, and more preferably 0.3 seconds or more. On the other hand, if the holding time exceeds 20.0 seconds, the contact angle of ethylene glycol will also exceed 50°. This is thought to be because etching proceeds excessively, resulting in a surface state that is not suitable for developing affinity for ethylene glycol. Therefore, the holding time is set to 20.0 seconds or less, preferably 18.0 seconds or less, and more preferably 15.0 seconds or less.

[0086] The amount of the aqueous solution can be measured using a moisture meter based on a filter-type infrared absorption method. Specifically, the absorbance on the surface is measured using a moisture meter based on a filter-type infrared absorption method, and the amount of the aqueous solution is determined from the absorbance using a previously determined calibration curve. The calibration curve can be created by the following procedure. First, the steel sheet having the coating layer is placed on an electronic balance. The aqueous solution is dropped onto the steel sheet having the coating layer using a pipette to form a liquid film over the entire surface of the steel sheet having the coating layer. The weight of the aqueous solution present on the steel sheet having the coating layer is calculated from the weight of the steel sheet having the coating layer before and after the aqueous solution is dropped. The amount of aqueous solution per unit area is calculated by dividing the resulting weight of the aqueous solution by the area of ​​the steel sheet having the coating layer. Simultaneously, the absorbance on the surface of the steel sheet having the coating layer is measured using a moisture meter based on a filter-type infrared absorption method. The above measurements are performed multiple times while changing the amount of aqueous solution, and a calibration curve showing the correlation between the amount of aqueous solution and absorbance is created. The calibration curve may be a linear approximation of the correlation between the amount of aqueous solution and the absorbance.

[0087] The method for adjusting the amount of the aqueous solution present on the surface of the coating layer is not particularly limited, and any method can be used. For example, the amount of the aqueous solution on the surface of the steel sheet may be adjusted by squeezing the solution with a wringer roll or by wiping.

[0088] Prior to the film formation step, the steel sheet having the Sn-plated layer can be optionally pretreated. Pretreatment can remove, for example, a natural oxide film present on the surface of the Sn-plated layer. Removing the natural oxide film can adjust the amount of Sn oxide and activate the surface.

[0089] The pretreatment method is not particularly limited, and any method can be used, but it is preferable to perform one or both of electrolysis in an alkaline aqueous solution and immersion treatment in an alkaline aqueous solution as the pretreatment. One or both of cathodic electrolysis and anodic electrolysis can be used as the electrolysis treatment. It is preferable to perform any of the following treatments (1) to (4) as the pretreatment: (1) cathodic electrolysis in an alkaline aqueous solution (2) immersion treatment in an alkaline aqueous solution (3) cathodic electrolysis in an alkaline aqueous solution followed by anodic electrolysis in an alkaline aqueous solution (4) anodic electrolysis in an alkaline aqueous solution

[0090] The alkaline aqueous solution may contain one or more electrolytes. The electrolyte is not particularly limited and any electrolyte may be used. For example, carbonate is preferably used as the electrolyte, and sodium bicarbonate is more preferably used. The lower limit of the concentration of the alkaline aqueous solution is not particularly limited, but is preferably 1 g / L or more, and more preferably 5 g / L or more. The upper limit of the concentration of the alkaline aqueous solution is also not particularly limited, but is preferably 30 g / L or less, and more preferably 20 g / L or less.

[0091] The lower limit of the temperature of the alkaline aqueous solution is not particularly limited, but is preferably 10° C. or higher, and more preferably 15° C. or higher. The upper limit of the temperature of the alkaline aqueous solution is also not particularly limited, but is preferably 70° C. or lower, and more preferably 60° C. or lower.

[0092] In addition, when cathodic electrolysis is performed as the pretreatment, the lower limit of the electricity density in the cathodic electrolysis is not particularly limited, but is preferably 0.5 C / dm 2It is preferable that the curvature is 1.0 C / dm or more. 2 On the other hand, there is no particular upper limit to the electricity density of the cathodic electrolysis treatment, but if it is too high, the effect of the pretreatment will be saturated, so the electricity density should be 10.0 C / dm or more. 2 It is preferable to do the following:

[0093] When immersion treatment is performed as the pretreatment, the lower limit of the immersion time is not particularly limited, but is preferably 0.1 seconds or more, more preferably 0.5 seconds or more. On the other hand, the upper limit of the immersion time is also not particularly limited, but if it is too long, the effect of the pretreatment will be saturated, so the immersion time is preferably 10 seconds or less.

[0094] When the pretreatment is an anodic electrolysis treatment, the lower limit of the electricity density in the anodic electrolysis treatment is not particularly limited, but is preferably 0.5 C / dm 2 It is preferable that the curvature is 1.0 C / dm or more. 2 On the other hand, the upper limit of the electricity density in the anodic electrolysis treatment is not particularly limited, but if it is too high, the effect of the pretreatment will be saturated, so the electricity density is preferably 10.0 C / dm or more. 2 It is preferable to do the following:

[0095] After the pretreatment, it is preferable to wash the surface with water in order to remove the pretreatment liquid adhering to the surface.

[0096] Furthermore, when forming a Sn-plated layer on the surface of a substrate steel sheet, it is preferable to subject the substrate steel sheet to a pretreatment. Any pretreatment may be performed as the pretreatment, but it is preferable to perform at least one of degreasing, pickling, and water washing.

[0097] By degreasing, rolling oil, rust-preventive oil, etc. adhering to the steel sheet can be removed. The degreasing can be carried out by any method without any particular limitation. After degreasing, it is preferable to wash the steel sheet with water to remove the degreasing treatment solution adhering to the surface of the steel sheet.

[0098] Furthermore, pickling can remove a natural oxide film present on the surface of the steel sheet and activate the surface. The pickling can be carried out by any method without any particular limitation. After pickling, the steel sheet is preferably washed with water to remove the pickling treatment solution adhering to the surface.

[0099] [Water-Rinsing Step] Next, the steel sheet after the surface conditioning step is rinsed with water at least once. By rinsing with water, the aqueous solution remaining on the surface of the steel sheet can be removed. The water-rinsing can be performed by any method without any particular limitation. For example, a water-rinsing tank can be provided downstream of the tank for film formation, and the steel sheet after the film-forming step can be continuously immersed in water. Alternatively, the steel sheet after the film-forming step can be rinsed by spraying water onto it.

[0100] The number of times that water washing is performed is not particularly limited, and may be one or more than two times. However, to avoid an excessive number of washing tanks, the number of times that water washing is performed is preferably five or less. Furthermore, when water washing is performed two or more times, each water washing may be performed using the same method or different methods.

[0101] In the present invention, it is important to use water having an electrical conductivity of 100 μS / m or less in at least the final rinse in the rinse treatment step. This reduces the amount of K, Na, Mg, and Ca adsorbed to the surface of the coated steel sheet, thereby improving adhesion. Water having an electrical conductivity of 100 μS / m or less can be produced by any method. The water having an electrical conductivity of 100 μS / m or less may be, for example, reverse osmosis water, ion-exchanged water, or distilled water. The electrical conductivity of the water used for rinsing can be measured using a conductivity meter.

[0102] When washing with water two or more times in the water washing treatment step, the above-mentioned effect can be obtained by using water having an electrical conductivity of 100 μS / m or less in the final wash, and therefore any water can be used for the washes other than the final wash. Water having an electrical conductivity of 100 μS / m or less may also be used for the washes other than the final wash. However, from the viewpoint of reducing costs, it is preferable to use water having an electrical conductivity of 100 μS / m or less only in the final wash, and to use ordinary water such as tap water or industrial water for the washes other than the final wash.

[0103] From the viewpoint of further reducing the amounts of K, Na, Mg, and Ca adsorbed on the surface of the coated steel sheet, the electrical conductivity of the water used in the final water rinse is preferably 50 μS / m or less, more preferably 30 μS / m or less. On the other hand, the lower limit of the electrical conductivity is not particularly limited and may be 0 μS / m. However, from the viewpoint of reducing costs, the electrical conductivity is preferably 1 μS / m or more.

[0104] The temperature of the water used in the washing treatment is not particularly limited and may be any temperature. However, an excessively high temperature places an excessive burden on the washing equipment, so the temperature of the water used for washing is preferably 95°C or less. On the other hand, the lower limit of the temperature of the water used for washing is not particularly limited, but is preferably 0°C or higher. The temperature of the water used for the washing may be room temperature.

[0105] The washing time per washing treatment is not particularly limited, but is preferably 0.1 seconds or more, more preferably 0.2 seconds or more, from the viewpoint of enhancing the effect of the washing treatment. The upper limit of the washing time per washing treatment is also not particularly limited, but is preferably 10 seconds or less, more preferably 8 seconds or less, in the case of production on a continuous line, because the line speed decreases and productivity decreases.

[0106] After the water washing step, drying may be optionally performed. The drying method is not particularly limited, and for example, a normal dryer or electric oven drying method can be applied. The temperature during the drying treatment is preferably 100°C or lower. If the temperature is within the above range, deterioration of the surface treatment film can be suppressed. The lower limit is not particularly limited, but is usually around room temperature.

[0107] The use of the surface-treated steel sheet of the present invention is not particularly limited, but it is particularly suitable as a surface-treated steel sheet for containers used in the manufacture of various containers such as food cans, beverage cans, pail cans, and 18-liter cans.

[0108] In order to confirm the effects of the present invention, surface-treated steel sheets were produced according to the procedures described below, and their properties were evaluated, although the present invention is not limited to these.

[0109] (Sn Plating) First, a steel sheet was subjected to electrolytic degreasing, water washing, pickling by immersion in dilute sulfuric acid, and water washing in sequence. Then, electroplating using a phenolsulfonic acid bath was performed to form a Sn plating layer on both sides of the steel sheet. The Sn deposition weight of the Sn plating layer was adjusted to the values ​​shown in Tables 2 and 3 by varying the current flow time. In some examples, prior to the Sn electroplating, the steel sheet was electroplated using a Watts bath to form a Ni plating layer as a Ni-containing layer on both sides of the steel sheet. The current flow time and current density were varied to achieve the Ni deposition weight of the Ni plating layer shown in Tables 2 and 3. The Sn deposition weight of the Sn plating layer was measured using the electrolytic stripping method specified in JIS G 3303. The Ni deposition weight of the Ni plating layer was measured using the fluorescent X-ray calibration curve method described above.

[0110] Furthermore, in some examples, after the Sn plating layer was formed, a reflow treatment was performed in which the substrate was heated by direct current heating at a heating rate of 50°C / sec for 5 seconds, and then immersed in water for rapid cooling.

[0111] As the steel sheet, a steel sheet for cans (T4 base sheet) having a thickness of 0.17 mm was used.

[0112] (Pretreatment of Sn-plated steel sheet) The obtained Sn-plated steel sheet was then subjected to the pretreatments shown in Tables 2 and 3. "C" indicates cathodic electrolysis, "A" indicates anodic electrolysis, "D" indicates immersion treatment, and "C→A" indicates cathodic electrolysis followed by anodic electrolysis. In the cathodic electrolysis, anodic electrolysis, and immersion treatments in the pretreatments, an aqueous sodium bicarbonate solution with a concentration of 10 g / L was used, and the temperature of the aqueous sodium bicarbonate solution was room temperature. The electrical density during cathodic electrolysis was 2.0 C / dm 2 The electrical density during anodic electrolysis was 4.0 C / dm 2 The immersion time in the immersion treatment was 1 second. For comparison, no pretreatment was performed in some examples.

[0113] (Film Forming Step) Next, the surface of the Sn-plated steel sheet was treated with an aqueous solution to form a film layer on the Sn-plated layer. Specifically, an aqueous solution having the composition shown in Table 1 was used as the aqueous solution, and a film layer was formed by performing cathodic electrolysis in the aqueous solution. The temperature of the aqueous solution was set to 35°C, and the pH was adjusted to 3 or more and 5 or less. The Zr deposition weight and Ti deposition weight were controlled by adjusting the electrical charge density. The Zr-containing compound was zirconium fluoride (ZrF 4 ) was used as the Ti-containing compound, and titanium fluoride (TiF 4 The aqueous solution was prepared by adjusting the concentration of each ion using compounds other than the Zr-containing compound and the Ti-containing compound so as to have the composition shown in Table 1.

[0114] (Surface Conditioning Step) After the above-mentioned film formation step, surface conditioning was carried out under the conditions shown in Tables 2 and 3. Specifically, at the time when the film formation step was completed, the steel sheet with the aqueous solution adhering to its surface was squeezed with a wringer roll, thereby adjusting the amount of aqueous solution present on the surface of the coating layer to the amount shown in Tables 2 and 3. The amount of the aqueous solution was measured with a moisture meter using the filter-type infrared absorption method, as described above. Thereafter, the solution was held for the holding time shown in Tables 2 and 3. In other words, the aqueous solution used in the surface conditioning step was the same as the aqueous solution used in the above-mentioned film formation step.

[0115] (Water-Rinsing Step) Next, the steel sheet after the surface conditioning step was subjected to a water-rinsing treatment. The water-rinsing treatment was performed 1 to 5 times under the conditions shown in Tables 2 and 3. The water-rinsing method and the electrical conductivity of the water used for each treatment were as shown in Tables 2 and 3. In the treatments in which the water-rinsing method was "immersion," the steel sheet was immersed in water for water-rinsing. On the other hand, in the treatments in which the water-rinsing method was "spraying," the steel sheet was rinsed by spraying water onto it. The electrical conductivity was measured using a conductivity meter.

[0116] For each of the obtained surface-treated steel sheets, the deposition weights of Zr oxide, Ti oxide, P, and Mn in the coating layer were measured. The measurements were performed using the fluorescent X-ray calibration curve method described above. The measurement results are shown in Tables 4 and 5. In Tables 4 and 5, the deposition weights of Zr oxide and Ti oxide are shown as the amount of metal Zr and the amount of metal Ti, respectively.

[0117] For each of the obtained surface-treated steel sheets, the contact angle of ethylene glycol and the atomic ratio of the adsorbed elements were measured by the following procedure. The measurement results are shown in Tables 4 and 5.

[0118] (Contact angle of ethylene glycol) The contact angle of the obtained surface-treated steel sheet with ethylene glycol was measured using an automatic contact angle meter, model CA-VP, manufactured by Kyowa Interface Science Co., Ltd. The surface temperature of the surface-treated steel sheet was set to 20°C ± 1°C, and ethylene glycol used was special-grade reagent ethylene glycol manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., at 20°C ± 1°C. A 2 μl droplet of ethylene glycol was dropped onto the surface of the surface-treated steel sheet, and the contact angle was measured one second later using the θ / 2 method, and the arithmetic mean of the contact angles of five drops was taken as the contact angle of ethylene glycol.

[0119] In order to confirm the change in contact angle due to heat, the contact angle was also measured after the surface-treated steel sheet was heat-treated at 200°C for 10 minutes. The measurement conditions were the same as above. As a result, for the surface-treated steel sheet that satisfied the conditions of the present invention, the contact angle values ​​were substantially the same before and after the heat treatment. In contrast, for the surface-treated steel sheet that did not satisfy the conditions of the present invention, the contact angle values ​​changed significantly due to the heat treatment.

[0120] (Atomic ratio of adsorbed elements) The total atomic ratio of K, Na, Mg, and Ca adsorbed on the surface of the surface-treated steel sheet relative to all elements was measured by XPS. No sputtering was performed during the measurement. The atomic ratio relative to all elements detected was quantified using the relative sensitivity factor method from the integrated intensity of the narrow spectrum of K2p, Na1s, Ca2p, and Mg1s on the outermost surface of the sample, and (K atomic ratio + Na atomic ratio + Ca atomic ratio + Mg atomic ratio) was calculated. For the XPS measurement, a scanning X-ray photoelectron spectrometer PHI X-tool manufactured by ULVAC-PHI, Inc. was used, with a monochromatic AlKα ray source, a voltage of 15 kV, a beam diameter of 100 μmφ, and a take-off angle of 45°.

[0121] Furthermore, the adhesion of the obtained surface-treated steel sheets to BPA-free paint was evaluated by the following method. The evaluation results are shown in Tables 4 and 5.

[0122] (Preparation of Samples) BPA-free painted steel sheets were prepared as samples to be used for evaluating adhesion to BPA-free paints by the following procedure.

[0123] A polyester paint for the inner surface of a can (BPA-free paint) was applied to the surface of the obtained surface-treated steel sheet, and baked at 180°C for 10 minutes to produce a BPA-free painted steel sheet. The coating weight was 60 mg / dm 2 It was decided.

[0124] (Adhesion to BPA-free paint) Two BPA-free painted steel sheets prepared under the same conditions were laminated with the painted surfaces facing each other with a nylon adhesive film in between, and then subjected to a pressure of 2.94 × 10 5The specimens were laminated under pressure bonding conditions of 1 Pa, a temperature of 190°C, and a pressure bonding time of 30 seconds. This was then divided into 5 mm wide test pieces. The divided test pieces were immersed for 168 hours in a test liquid at 55°C consisting of a mixed aqueous solution containing 1.5 mass% citric acid and 1.5 mass% table salt. After immersion, the specimens were washed and dried, and the two steel plates of the divided test pieces were peeled apart using a tensile tester, and the tensile strength at the time of peeling was measured. The average value of the three test pieces was evaluated according to the following four levels. In practice, a result of 1 to 3 can be evaluated as having excellent adhesion to BPA-free paint. 1: 2.5 kgf or more 2: 2.0 kgf or more but less than 2.5 kgf 3: 1.5 kgf or more but less than 2.0 kgf 4: Less than 1.5 kgf

[0125] As is clear from the results shown in Tables 4 and 5, all of the surface-treated steel sheets satisfying the conditions of the present invention had excellent adhesion to BPA-free paints, even though they were produced without using hexavalent chromium.

[0126]

[0127]

[0128]

[0129]

[0130]

Claims

1. A surface-treated steel sheet having a Sn-plated layer on at least one surface of the steel sheet, and a coating layer containing at least one of Zr oxide and Ti oxide disposed on the Sn-plated layer, wherein the contact angle with ethylene glycol is 50° or less, and the total atomic ratio of K, Na, Mg, and Ca adsorbed on the surface to all elements is 5.0% or less.

2. The Sn plating layer has an Sn coating weight of 0.1 to 20.0 g / m per side of the steel sheet. 2 The surface-treated steel sheet according to claim 1 , 3. The total amount of Zr oxide and Ti oxide deposited in the coating layer is 0.3 to 50.0 mg / m2 per side of the steel sheet in terms of the amount of metal Zr and the amount of metal Ti. 2 The surface-treated steel sheet according to claim 1 or 2, 4. The coating layer further contains P, and the P coating amount is 50.0 mg / m per one side of the steel sheet. 2 The surface-treated steel sheet according to any one of claims 1 to 3, wherein:

5. The coating layer further contains Mn, and the Mn coating amount is 50.0 mg / m per one side of the steel sheet. 2 The surface-treated steel sheet according to any one of claims 1 to 4, wherein:

6. The surface-treated steel sheet according to any one of claims 1 to 5, further comprising a Ni-containing layer disposed below the Sn-plated layer.

7. The Ni-containing layer has a Ni deposition amount of 2 mg / m per side of the steel sheet. 2 ~2000mg / m 2 The surface-treated steel sheet according to claim 6, wherein:

8. A method for producing a surface-treated steel sheet having a Sn plating layer on at least one surface of the steel sheet and a coating layer containing at least one of Zr oxide and Ti oxide disposed on the Sn plating layer, the method comprising: a coating formation step of treating the surface of a steel sheet having a Sn plating layer on at least one surface with an aqueous solution containing at least one of Zr ions and Ti ions to form the coating layer on the Sn plating layer; and a step of applying the aqueous solution to the surface of the coating layer in an amount of 1.0 to 30.0 g / m. 2 a surface conditioning step of holding the steel sheet in a state where the surface is present for 0.1 to 20.0 seconds; and a water rinsing step of rinsing the steel sheet with water at least once after the surface conditioning step, wherein in the water rinsing step, water having an electrical conductivity of 100 μS / m or less is used in at least the final water rinsing.

9. The method for producing a surface-treated steel sheet according to claim 8, wherein the surface-treated steel sheet further has a Ni-containing layer disposed below the Sn-plated layer.