Conductive paste and method for manufacturing electronic component
Patent Information
- Application Number
- MYPI2025002352
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-19
- Filing Date
- 2023-10-13
- Publication Date
- 2024-04-19
AI Technical Summary
Conductive pastes using copper as the main component face challenges in forming thin, dense, and highly continuous terminal electrodes when fired at low temperatures, as existing methods struggle to efficiently remove binders and prevent carbon residues from trapping, leading to issues like blister failure and inadequate sintering.
A conductive paste comprising copper-based conductive powder with specific particle size distribution and surface treatment, combined with fine glass frit, allows for improved filling and debinding properties, enabling the formation of thin, dense terminal electrodes even at lower firing temperatures by ensuring uniform sintering and binder removal.
The solution enables the production of thin, dense, and highly continuous terminal electrodes with high productivity, even when firing at temperatures as low as 720°C, by ensuring effective binder removal and uniform sintering, thus overcoming the limitations of existing methods.
Smart Images

Figure PI2025002352_DRAWING_001
Abstract
Description
Conductive paste and method for manufacturing electronic components
[0001] The present invention relates to a conductive paste using a conductive powder containing copper as a main component. In particular, the present invention relates to a conductive paste for forming terminal electrodes of multilayer electronic components such as multilayer ceramic capacitors, multilayer inductors, and multilayer piezoelectric actuators. The present invention also relates to a method for manufacturing multilayer electronic components. In particular, the present invention relates to a method for manufacturing electronic components by forming terminal electrodes on a multilayer base body for a multilayer electronic component.
[0002] Multilayer ceramic electronic components such as multilayer ceramic capacitors, multilayer inductors, and multilayer piezoelectric actuators are generally manufactured as follows.
[0003] First, a conductive paste for the internal electrodes is printed in a predetermined pattern on a dielectric ceramic green sheet such as a barium titanate ceramic. Then, multiple such sheets are stacked and pressed together to obtain an unfired laminate in which ceramic green sheets and internal electrode paste layers are alternately stacked. The resulting laminate is cut into chips of a predetermined shape to obtain a laminated element. The laminated element may be fired at a high temperature at this stage, or it may not be fired at this stage but may be co-fired later with a terminal electrode paste layer formed using a conductive paste for the terminal electrodes. In either case, the laminate in its state before the formation of the terminal electrode paste layer is referred to as a "laminated element."
[0004] Thereafter, a conductive paste for terminal electrodes, which contains components such as conductive powder, binder resin, organic solvent, and glass frit, is printed on the exposed ends of the internal electrodes of the laminated body by a dip printing method or the like to form a conductive paste layer, which is then dried as necessary and further fired at a high temperature to form the terminal electrodes.
[0005] Furthermore, thereafter, a plating layer of nickel, tin, or the like may be formed on the terminal electrodes by electroplating or the like, if necessary.
[0006] Traditionally, precious metals such as palladium, silver-palladium, and platinum have been used as internal electrode materials. However, there are demands for resource conservation and cost reduction, and particularly for sintered types, there is a demand for preventing delamination and cracking caused by oxidative expansion of palladium and silver-palladium during sintering. In recent years, therefore, the use of base metals such as nickel, cobalt, and copper has become mainstream. For this reason, copper, nickel, cobalt, or alloys of these metals, which easily form good electrical connections with base metal internal electrodes, have been used as terminal electrode materials instead of the conventional silver and silver-palladium.
[0007] When base metals are used for the internal electrodes and terminal electrodes in this way, the terminal electrodes are usually fired in a non-oxidizing atmosphere with as low an oxygen partial pressure as possible, for example, in an inert gas atmosphere with an oxygen content of several ppm to several tens of ppm, at a high peak temperature of 800°C, so as to prevent the base metals from being oxidized during firing.
[0008] However, particularly when firing copper-based metal powder in a low-oxygen atmosphere, it is difficult to properly remove the binder, which burns, decomposes, and scatters organic components such as binder resin. If the binder is not removed sufficiently at the relatively low temperature in the early stages of firing, before the glass fluidizes and the copper powder sinters, carbon and organic residues become trapped in the film after sintering begins, causing various problems such as blister defects at the subsequent high-temperature stages.
[0009] Therefore, in the past, an important issue for conductive pastes using metal powders whose main component is base metals, particularly copper, has been how to efficiently remove the binder in the early stages of firing and reduce residual carbon before the sintering of the copper powder progresses at high temperatures.
[0010] As a method for solving this problem, for example, Patent Document 1 discloses a conductor paste for terminal electrodes that uses an aliphatic amine as a surface treatment agent for copper-based conductive powder, thereby improving the dispersibility of the conductive powder and significantly improving the binder removal properties, thereby making it possible to form dense terminal electrodes that are excellent in adhesion and conductivity.
[0011] Patent Document 2 discloses a conductive paste comprising copper powder, glass frit, and an organic vehicle, the copper powder being a mixture of 0 to 70 vol% of coarse copper powder having an average particle size of 1.0 μm to 3.0 μm and 30 to 100 vol% of fine copper powder having an average particle size of 0.1 to 0.8 μm. Patent Document 2 also discloses an electronic component comprising a laminate having a plurality of ceramic layers and internal electrodes, and external electrodes formed on the outer surfaces of the laminate and electrically connected to the internal electrodes by baking the conductive paste, wherein the carbon content in the external electrodes when the sintering density of the external electrodes is 80% is 0.007 wt% or less.
[0012] JP 2006-004734 A JP 2011-187225 A
[0013] Recently, there has been a demand for lower firing temperatures when forming the terminal electrodes in order to reduce environmental impact, manufacturing costs, and thermal stress on the laminated body. In addition, there is a demand for smaller electronic components, which in turn requires thinner terminal electrodes. That is, there is a demand for a conductive paste that can be appropriately debindered, can be fired at a lower temperature, and is suitable for thinning.
[0014] The conductive pastes described in Patent Documents 1 and 2 are designed assuming firing at high temperatures such as 800° C. Therefore, when firing at 800° C., sintering proceeds sufficiently after binder removal, resulting in a dense fired film. However, when the present inventors attempted firing at a low temperature such as 720° C. using the above-mentioned paste, they were unable to achieve sufficient sintering after binder removal within firing times of several tens of minutes or several hours.
[0015] Therefore, an object of the present invention is to provide a conductive paste that can form thin, dense, and highly continuous terminal electrodes while maintaining high productivity, even when fired at a low temperature.An object of the present invention is also to provide a method for manufacturing electronic components that include thin, dense, and highly continuous terminal electrodes while maintaining high productivity, even when fired at a low temperature.
[0016] As a result of intensive research to solve the above problems, the present inventors have discovered a method for producing a polymer having copper as a main component and a volume-based cumulative 50% particle diameter D50 measured by laser diffraction particle size distribution measurement. C A fine conductive powder having a particle diameter of 0.3 μm or more and 4.5 μm or less, a ratio of an average major diameter X to an average minor diameter Y of 1.0 or more and 3.0 or less, and a ratio of an average major diameter X to an average thickness Z of 1.1 or more and 9.0 or less, and a volume-based cumulative 50% particle diameter D50 measured by laser diffraction particle size distribution measurement. G The present inventors have discovered that by combining a fine glass frit having a particle size of 0.3 μm or more and 2.0 μm or less, it is possible to form a thin, dense, and highly continuous terminal electrode while maintaining high productivity, even when firing at a low temperature, and have thus completed the present invention.
[0017] That is, the present invention (1) is a conductive paste containing a conductive powder mainly composed of copper, glass frit, a binder resin, and an organic solvent, wherein the conductive powder mainly composed of copper has a volume-based cumulative 50% particle diameter D50 in laser diffraction particle size distribution measurement. C a ratio of an average major diameter X to an average minor diameter Y is 1.0 to 3.0, and a ratio of an average major diameter X to an average thickness Z defined below is 1.1 to 9.0, and the volume-based cumulative 50% particle diameter D50 of the glass frit measured by laser diffraction particle size distribution measurement is G The conductive paste is characterized in that the thickness of the conductive paste is 0.3 μm or more and 2.0 μm or less. (Average Thickness) The conductive paste containing the copper-based conductive powder is cast onto a PET film using an applicator to form a coating film with a thickness of 250 μm, and the coating film is dried in an air atmosphere at 150° C. for 10 minutes to form a dry film. A cross section of the dry film is exposed by ion milling, and the cross section of the dry film is observed with a scanning electron microscope. 500 conductive particles are randomly selected and the minor axis is measured as the thickness to determine the average value of the thicknesses, and this average value is defined as the "average thickness."
[0018] The present invention (2) also provides the conductive paste according to (1), wherein the conductive powder containing copper as a main component has an aliphatic amine on at least a part of the surface thereof.
[0019] The present invention (3) also provides the conductive paste according to (2), in which the aliphatic amine is contained in an amount of 0.01 part by mass or more and 1.0 part by mass or less per 100 parts by mass of the conductive powder containing copper as a main component.
[0020] In addition, the present invention (4) is characterized in that the cumulative 10% particle diameter of the glass frit on a volume basis in a laser diffraction particle size distribution measurement is D10 G The cumulative 90% particle size is D90 G When this is done, (D90 G -D10 G ) / D50 G The present invention provides a conductive paste according to any one of (1) to (3), in which the value of the resistance is 7.5 or less.
[0021] In addition, the present invention (5) is characterized in that the volume-based cumulative 10% particle diameter of the conductive powder containing copper as a main component in laser diffraction particle size distribution measurement is D10 C The cumulative 90% particle size is D90 C When this is done, (D90 C -D10 C ) / D50 C The present invention provides a conductive paste according to any one of (1) to (4), in which the value of the resistance is 7.5 or less.
[0022] In addition, the present invention (6) has a shear rate of 40 s when measured at 25 ° C. -1 Viscosity at a shear rate of 0.4 s -1 and (5) a phase difference δ between a strain of 1% applied to the conductive paste at an angular frequency of 1 Hz and a stress generated by the strain is 45° or more and 80° or less.
[0023] The present invention (7) provides a conductive paste according to any one of (1) to (6), which satisfies all of the following criteria: the electrode area ratio of the terminal electrodes is 90% or more, the average maximum thickness of the terminal electrodes is 40 μm or less, and the average minimum thickness of the terminal electrodes is 1.0 μm or more, as calculated by the following evaluation tests. <Test for Evaluating Electrode Area Ratio of Terminal Electrodes> Evaluation test samples prepared by the following method for preparing evaluation test samples are observed with a scanning electron microscope, with 10 visual fields per sample, and the ratio of the electrode area in the observed visual fields is calculated as the electrode area ratio of the terminal electrodes. <Test for Evaluating Maximum Thickness of Terminal Electrodes> Evaluation test samples prepared by the following method for preparing evaluation test samples are observed with a scanning electron microscope, and the maximum thickness of each evaluation test sample is measured at the point where a perpendicular line is longest when a perpendicular line is drawn from the outer periphery of the terminal electrode to the end face of the laminated body. The maximum thicknesses of 20 electronic components whose maximum thicknesses were measured are averaged to calculate the average maximum thickness of the terminal electrodes. <Terminal Electrode Minimum Thickness Evaluation Test> An evaluation test sample prepared by the evaluation test sample preparation method described below is observed with a scanning electron microscope, and the thickness of the evaluation test sample is measured at the point where the length of a perpendicular line drawn from the outer periphery of the terminal electrode to the end face of the laminated body is the shortest, and the thickness of the point where the distance between the corner of the laminated body and the outer periphery of the terminal electrode is the shortest. The thickness of the thinnest of these points is measured as the minimum thickness, and the minimum thicknesses of 20 electronic components whose minimum thicknesses have been measured are averaged to calculate the average minimum thickness of the terminal electrodes.<Method of Preparing Evaluation Test Samples> A rectangular parallelepiped laminated body having a length of 0.6 mm, a width of 0.3 mm, and a height of 0.3 mm, in which a plurality of dielectric layers containing barium titanate and internal electrode layers containing nickel are stacked, is prepared. The conductive paste is applied to the end of the laminated body where the internal electrodes are exposed by dip printing, with the laminated body lowered at a rate of 300 μm / s and pulled up at a rate of 100 μm / s. The laminated body is then held in an air atmosphere at 150°C for 10 minutes, and then heated in a nitrogen atmosphere at a heating rate of 50°C / min. After reaching 720°C, the temperature is held for 15 minutes to form terminal electrodes, thereby producing 20 electronic components equipped with terminal electrodes. The 20 electronic components are each embedded in resin, and each electronic component is cut in the stacking direction (perpendicular to the dielectric layers and internal electrode layers) so as to pass through the center of each end face of the electronic component to expose a cross section of the electronic component, thereby preparing an evaluation test sample.
[0024] The present invention (8) also provides a method for manufacturing an electronic component, comprising: a laminated body preparation step of preparing a laminated body for a multilayer electronic component, which comprises a plurality of ceramic layers and a plurality of internal electrode layers; and a terminal electrode formation step of applying a conductive paste to exposed ends of the internal electrodes of the laminated body, and then firing the applied conductive paste to form terminal electrodes, wherein the conductive paste is the conductive paste described in any one of (1) to (7).
[0025] The present invention (9) also provides the method for producing an electronic component according to (7), wherein the peak temperature of the firing is 720° C. or less.
[0026] In addition, the present invention (10) is a conductive paste that is fired before use, and the peak temperature of the firing is T 1 When the temperature was 100°C, the glass frit was placed in a cylindrical container having an inner diameter of 5 mm, and a pressure of 3 MPa was applied in the axial direction for 10 seconds to prepare a cylindrical green compact having a diameter of 5 mm and a height of 1 mm. The green compact was then placed on a copper plate having a surface roughness Ra of 100 nm so that the flat surface of the green compact was in contact with the copper plate, and the green compact was heated at a heating rate of 10°C / min in a nitrogen atmosphere. 1(7) The conductive paste according to any one of (1) to (7), wherein when the temperature of the powder compact is raised to 100°C and the powder compact is heated to melt the glass constituting the powder compact, the contact angle of the glass with the copper plate is 80° or less.
[0027] In addition, the present invention (11) has a shear rate of 4 s when measured at 25 ° C. -1 The present invention provides a conductive paste according to any one of (1) to (7) and (10), which has a viscosity of 10.0 Pa·s or more and 80.0 Pa·s or less at 1000 kJ / min.
[0028] The present invention (12) also provides the method for manufacturing an electronic component according to (8) or (9), in which the electrode area ratio of the terminal electrodes calculated by the following calculation method is 90% or more. <Method for calculating the electrode area ratio of terminal electrodes> Twenty of the electronic components are embedded in resin, and each electronic component is cut in the lamination direction (perpendicular to the dielectric layers and internal electrode layers) so as to pass through the center of each end face of the electronic component to expose a cross section of each electronic component, and the cross section is observed using a scanning electron microscope in 10 visual fields for each electronic component, and the ratio of the electrode area within the observed visual field is calculated as the electrode area ratio.
[0029] The present invention (13) also provides the method for manufacturing an electronic component according to any one of (8), (9), and (12), in which the average maximum thickness of the terminal electrodes calculated by the following calculation method is 40 μm or less. <Method for calculating the average maximum thickness of terminal electrodes> Twenty of the electronic components are embedded in a resin, and each electronic component is cut in the stacking direction (perpendicular to the dielectric layers and internal electrode layers) so as to pass through the center of each end face of the electronic component to expose a cross section of each electronic component, and the cross section is observed with a scanning electron microscope. When a perpendicular line is drawn from the outer periphery of the terminal electrode to the end face of the laminated body on the cross section, the point where the length of the perpendicular line is longest is measured as the maximum thickness, and the maximum thicknesses of the 20 electronic components whose maximum thicknesses have been measured are averaged to calculate the average maximum thickness of the terminal electrodes.
[0030] The present invention (14) also provides a method for manufacturing an electronic component according to any one of (8), (9), (12), and (13), in which the average minimum thickness of the terminal electrodes calculated by the following calculation method is 1.0 μm or more. <Method for calculating the average minimum thickness of terminal electrodes> Twenty of the electronic components are embedded in resin, and each electronic component is cut in the stacking direction (perpendicular to the dielectric layers and internal electrode layers) so as to pass through the center of each end face of the electronic component to expose a cross section of each electronic component. The cross section is observed with a scanning electron microscope, and the thickness of a point on the cross section where the length of a perpendicular line drawn from the outer periphery of the terminal electrode to the end face of the laminated body is smallest and the thickness of a point where the distance between a corner of the laminated body and the outer periphery of the terminal electrode is shortest are measured, and the thickness of the thinnest part of these is measured as the minimum thickness, and the average minimum thickness of the terminal electrodes is calculated by averaging the minimum thicknesses of the 20 electronic components whose minimum thicknesses have been measured.
[0031] According to the present invention, even when firing at a low temperature, thin, dense, and highly continuous terminal electrodes can be formed while maintaining high productivity.Furthermore, even when firing at a low temperature, electronic components including thin, dense, and highly continuous terminal electrodes can be manufactured while maintaining high productivity.
[0032] FIG. 1 is a schematic diagram illustrating a method for measuring the fired film thickness of a terminal electrode formed from a conductive paste.
[0033] <Conductive Paste> The conductive paste of the present invention contains a conductive powder containing copper as a main component, glass frit, a binder resin, and an organic solvent, wherein the conductive powder has a volume-based cumulative 50% particle diameter D50C of 0.3 μm or more and 4.5 μm or less, a ratio of the average major diameter X to the average minor diameter Y of 1.0 or more and 3.0 or less, and a ratio of the average major diameter X to the average thickness Z of 1.1 or more and 9.0 or less, and the glass frit has a volume-based cumulative 50% particle diameter D50C of 0.3 μm or more and 4.5 μm or less, both measured by laser diffraction particle size distribution measurement. GIn particular, when the copper-based conductive powder of the present invention has an aliphatic amine (described later) on at least a portion of its surface, the effects of the present invention are more pronounced.
[0034] By using the conductive powder containing copper as the main component, the filling property of the conductive powder in the coating film of the conductive paste is improved, so that the sintering of the conductive powder can be easily progressed even when firing at a low temperature. G By using a glass frit having a D50 within the above range, the fine glass frit is uniformly dispersed even inside the film before firing in which the conductive powder is densely packed, so that the conductive powder is easily sintered uniformly throughout the film, and a binder removal path can be properly secured throughout the film, resulting in the formation of a thin, dense, and highly continuous terminal electrode. G By setting the upper limit of the above range, it is possible to reduce discontinuous portions of the terminal electrodes due to voids that occur after the glass flows.
[0035] Surface-treating the conductive powder improves the dispersibility of the conductive powder, further improving the packing of the conductive powder in the coating film. However, improved packing narrows the debindering path, reducing the debindering ability. Furthermore, the surface treatment agent itself must also be debindered, which can lead to poor sintering or other problems such as blistering due to insufficient debindering. In a preferred embodiment of the present invention, the use of an aliphatic amine, described below, as the surface treatment agent enables appropriate debindering even when the conductive powder is densely packed. That is, by using the conductive powder of the present invention surface-treated with an aliphatic amine, the conductive powder is packed even more densely in the coating film before firing. Furthermore, the use of the glass frit of the present invention and the aliphatic amine as the surface treatment agent for the conductive powder improves the packing ability, which facilitates sintering even when firing at a low temperature, making it easier to obtain a dense fired film.
[0036] The conductive paste of the present invention is preferably used by applying the conductive paste to a laminated body or the like to form a coating film, drying the coating film as needed to form a dry film, and then firing the paste. The peak firing temperature is not particularly limited, and firing is possible at a temperature of 600°C or higher, which is lower than conventional firing temperatures. From the viewpoints of reducing the environmental load, reducing production costs, and reducing thermal stress on the laminated body, a temperature of 600°C or higher and 720°C or lower is preferred, and a temperature of 600°C or higher and 700°C or lower is particularly preferred.
[0037] <Conductive Powder> The conductive powder of the present invention may be any powder containing copper as a main component. Preferably, the copper content in the conductive powder is 80% by mass or more and 100% by mass or less, more preferably 90% by mass or more and 100% by mass or less, even more preferably 95% by mass or more and 100% by mass or less, and particularly preferably 100% by mass (pure copper). When the copper content in the conductive powder is within the above range, the conductive powder particles are easily sintered together, making it easier to obtain a dense fired film. Note that, as long as the conductive powder of the present invention contains copper as a main component, it may be a mixed powder of copper powder and other element metal powders such as nickel powder or silver powder, or an alloy powder of copper and other element metals such as nickel or silver. Furthermore, it may be a composite powder in which copper powder is coated with glass, ceramic, or the like, or may have an oxide film on the surface. Furthermore, it may be surface-treated with an organometallic compound, a surfactant, or the like, or two or more of these conductive powders may be mixed and used. In this specification, the term "main component" means that the component in question accounts for more than 50 mass% of the total, and in particular, in the case of a conductive powder containing copper as the main component, this means that the copper component accounts for more than 50 mass% of the total conductive powder contained in the conductive paste of the present invention, including the above-mentioned mixed powder, alloy powder, etc.
[0038] The volume-based cumulative 50% particle diameter D50 of the conductive powder containing copper as the main component in the present invention measured by laser diffraction particle size distribution measurement CThe D50 of the copper-based conductive powder may be 0.3 μm or more and 4.5 μm or less, preferably 0.3 μm or more and 4.0 μm or less, more preferably 0.5 μm or more and 4.0 μm or less, more preferably 0.5 μm or more and 3.0 μm or less, more preferably 0.7 μm or more and 3.0 μm or less, even more preferably 1.0 μm or more and 3.0 μm or less, and particularly preferably 1.5 μm or more and 2.5 μm or less. C When the temperature is within the above range, the sintering of the conductive powder proceeds easily even when the firing is performed at a low temperature, and a dense fired film can be easily formed. In addition, a thin fired film can be easily formed.
[0039] The copper-based conductive powder of the present invention may have a ratio of the average major diameter X to the average minor diameter Y of 1.0 or more and 3.0 or less, preferably 1.0 or more and 2.5 or less. When the ratio of the average major diameter X to the average minor diameter Y of the copper-based conductive powder is within the above range, sintering proceeds easily even when firing at a low temperature, making it easier to form a dense fired film. In addition, it makes it easier to form a thin fired film (terminal electrode) with excellent continuity.
[0040] The above-mentioned average major axis X and average minor axis Y can both be measured, for example, by scanning electron microscope observation. That is, they can be measured by randomly selecting a plurality of conductive particles (e.g., 500 particles) using a scanning electron microscope, measuring the major axis and minor axis, and calculating the average value of each. Alternatively, they can be measured, for example, by a flow particle image analyzer. That is, they can be measured by using a flow particle image analyzer to measure the major axis and minor axis of a plurality of conductive particles (e.g., 500 particles) and calculating the average value of each. As a flow particle image analyzer, for example, an FPIA-3000S manufactured by Sysmex Corporation can be used.
[0041] The copper-based conductive powder of the present invention may have a ratio of the average major diameter X to the average thickness Z, as defined below, of 1.1 to 9.0, preferably 1.1 to 7.5, more preferably 1.2 to 7.5, more preferably 1.2 to 6.0, more preferably 1.5 to 5.0, more preferably 1.6 to 4.5, more preferably 1.6 to 4.0, even more preferably 1.7 to 3.0, and particularly preferably 1.8 to 2.5. When the ratio of the average major diameter X to the average thickness Z of the copper-based conductive powder is within the above range, sintering proceeds easily even when sintered at a low temperature, making it easier to form a dense sintered film. Furthermore, it is easier to form a thin sintered film (terminal electrode) with excellent continuity. (Average Thickness) The conductive paste containing the copper-based conductive powder is cast onto a PET film using an applicator to form a coating film with a thickness of 250 μm, and the coating film is dried in an air atmosphere at 150° C. for 10 minutes to form a dry film. The cross section of the dry film is exposed by ion milling, and the cross section of the dry film is observed with a scanning electron microscope. 500 conductive particles are randomly selected, and the minor axis is measured as the thickness to determine the average value of the thickness. This average value is defined as the "average thickness" in this specification (the present invention).
[0042] The average thickness Z can be measured, for example, by scanning electron microscope observation of the cross section of a dried film formed using the conductive paste of the present invention. More specifically, for example, the conductive paste of the present invention is cast on a PET film using an applicator to form a coating film with a thickness of 250 μm, and the coating film is dried under conditions of atmospheric air, 150 ° C., and 10 minutes to form a dried film. The cross section of the dried film is exposed using an ion milling device (e.g., IM4000 manufactured by Hitachi High-Technologies Corporation), and the cross section of the dried film is observed using a scanning electron microscope (e.g., SU-8020 manufactured by Hitachi High-Technologies Corporation). A plurality of conductive particles (e.g., 500 particles) are randomly selected from the observation, and the minor axis is measured as the thickness, and the average value of the thicknesses is calculated. For example, the conductive paste of the present invention may be prepared by mixing 100 parts by mass of a conductive powder containing copper as a main component, an acrylic resin (7 parts by mass as resin) dissolved in terpineol, and 10 parts by mass of glass frit, followed by kneading using a triple roll mill, diluting with terpineol, and then heating at 25° C. and a shear rate of 4 s -1 It is possible to use a conductive powder whose viscosity is adjusted to 30 Pa s at 2000 kJ / min. Even when other powders such as glass frit are contained in addition to the conductive powder whose main component is copper, the average thickness of the conductive powder whose main component is copper can be measured by distinguishing it from the other powders. For example, the conductive powder whose main component is copper can be distinguished from other powders by observing the element distribution in the cross section of the dried film using EDX (Energy Dispersive X-ray spectroscopy).
[0043] The conductive powder containing copper as a main component in the present invention has a D50 C The shape is not particularly limited as long as the diameter is 0.3 μm or more and 4.5 μm or less, the ratio of the average major diameter X to the average minor diameter Y is 1.0 or more and 3.0 or less, and the ratio of the average major diameter X to the average thickness Z is 1.1 or more and 9.0 or less, and may be, for example, a flat, cylindrical, elliptical cylindrical, truncated conical, truncated elliptical conical, rectangular parallelepiped, or other shape. Note that the conductive powder of the present invention does not exclude powders of other shapes such as spherical, and the conductive powder as a whole may be referred to as having a "D50 CIt is sufficient that the "ratio of average major diameter X to average minor diameter Y" and "ratio of average major diameter X to average thickness Z" satisfy the above-mentioned numerical ranges. In this case, the content of the conductive powder satisfying the numerical ranges relative to the total conductive powder is not particularly limited, but is preferably more than 50 mass%, more preferably 55 mass% or more, more preferably 60 mass% or more, more preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, and particularly preferably 95 mass% or more.
[0044] The conductive powder containing copper as a main component in the present invention has a volume-based cumulative 10% particle diameter D10 measured by laser diffraction particle size distribution measurement. C The cumulative 90% particle size is D90 C When this is done, (D90 C -D10 C ) / D50 C is preferably 7.5 or less, more preferably 6.5 or less, still more preferably 5.0 or less, still more preferably 4.0 or less, still more preferably 3.0 or less, and particularly preferably 2.0 or less. (D90 C -D10 C ) / D50 C The lower limit of the D90 of the conductive powder containing copper as the main component is not particularly limited, but can be set to, for example, 0.2 or more. C -D10 C ) / D50 C In other words, the narrow particle size distribution of the conductive powder allows the conductive powder to be sintered uniformly throughout the entire film. This means that localized sintering within the film can be suppressed, ensuring an appropriate binder removal path throughout the film, resulting in the formation of a thin, dense, and highly continuous terminal electrode. Furthermore, the terminal electrode can be prevented from becoming too thick due to excessively large conductive powder particles.
[0045] The specific surface area of the conductive powder is preferably 0.2 m 2 / g or more 3.0m 2 / g or less, particularly preferably 0.3m 2 / g or more 2.0m 2When the specific surface area of the conductive powder containing copper as a main component is within the above range, sintering proceeds easily even when firing at a low temperature, and a dense fired film is easily formed. In addition, a thin fired film is easily formed.
[0046] The method for producing the conductive powder of the present invention is not particularly limited, and the conductive powder can be produced, for example, by producing a spherical conductive powder by spray pyrolysis, physical vapor deposition, chemical vapor deposition, liquid phase reduction, atomization, or the like, then, if necessary, surface-treating the conductive powder with a surface treatment agent such as an aliphatic amine described below, and then pulverizing the powder using a bead mill, ball mill, stamp mill, etc. Furthermore, if necessary, classification can be performed before or after the pulverization to adjust the particle size distribution.
[0047] <Glass Frit> The cumulative 50% particle diameter D50 of the glass frit in the present invention is determined by laser diffraction particle size distribution measurement. G The D50 of the glass frit may be 0.3 μm or more and 2.0 μm or less, and is preferably 0.5 μm or more and 1.5 μm or less. G When the content is in the above range, a dense fired film can be easily formed, and a fired film (terminal electrode) with excellent continuity can be easily formed.
[0048] The cumulative 10% particle diameter of the glass frit in the present invention measured by laser diffraction particle size distribution measurement is D10 G The cumulative 90% particle size is D90 G When this is done, (D90 G -D10 G ) / D50 G is preferably 7.5 or less, more preferably 6.5 or less, still more preferably 5.0 or less, even more preferably 3.5 or less, and particularly preferably 2.5 or less. (D90 G -D10 G ) / D50 G The lower limit of the (D90) of the glass frit is not particularly limited, but can be, for example, 0.2 or more. G -D10 G ) / D50 GIn other words, the narrow particle size distribution of the glass frit allows uniformly sized glass frit to be uniformly distributed within the pre-fired film, which is densely packed with conductive powder, facilitating uniform sintering of the conductive powder throughout the film. This also suppresses localized sintering within the film, ensuring appropriate debindering paths throughout the film, resulting in the formation of thin, dense, and highly continuous terminal electrodes. The lack of extremely small glass frit, which exists in agglomerates and is prone to softening and flow, facilitates the suppression of localized sintering and localized debindering failures resulting from the sintering. The lack of extremely large glass frit also suppresses exposure of the laminated body due to voids formed where the glass frit flows during the firing process, thereby improving the continuity of the terminal electrodes.
[0049] The conductive paste of the present invention is a sintered conductive paste used after sintering, and the peak temperature of the sintering is T 1 When the temperature was 100°C, the glass frit was placed in a cylindrical container having an inner diameter of 5 mm, and a pressure of 3 MPa was applied in the axial direction for 10 seconds to prepare a cylindrical green compact having a diameter of 5 mm and a height of 1 mm. The green compact was then placed on a copper plate having a surface roughness Ra of 100 nm so that the flat surface of the green compact was in contact with the copper plate, and the green compact was heated at a heating rate of 10°C / min in a nitrogen atmosphere. 1When the temperature of the powder compact is raised to °C and the powder compact is heated to melt the glass constituting the powder compact, the contact angle of the glass with the copper plate is preferably 80° or less, more preferably 75° or less, more preferably 70° or less, more preferably 65° or less, even more preferably 60° or less, and particularly preferably 55° or less. The lower limit of the contact angle of the glass with the copper plate is not particularly limited, but may be, for example, 10° or more. When the contact angle of the glass with the copper plate is in the above range, the wettability of the glass with the copper-based conductive powder is improved, and while flow of the glass is suppressed up to a desired temperature for appropriate binder removal, the glass can quickly wet and spread in the vicinity of the conductive powder once the desired temperature is reached, making it easier to form a thin, dense, and highly continuous terminal electrode.
[0050] The composition of the glass frit in the present invention is not particularly limited, and examples thereof include BaO-ZnO-based, BaO-ZnO-B 2 O 3 RO-ZnO-B 2 O 3 -MnO 2 RO-ZnO system, RO-ZnO-MnO system 2 RO-ZnO-SiO 2 ZnO-B 2 O 3 system, SiO 2 -B 2 O 3 -R' 2 O-based, SiO 2 -RO-R' 2 Glasses such as O-based (where R is an alkaline earth metal element and R' is an alkali metal element) can be used.
[0051] The glass transition point of the glass frit in the present invention is preferably 400° C. or higher and 550° C. or lower. When the glass transition point of the glass frit is within the above range, the glass easily wets and spreads throughout the film even when fired at a low temperature, making it easier to form a dense fired film.
[0052] The softening point of the glass frit in the present invention is preferably 500° C. or higher and 650° C. or lower. When the softening point of the glass frit is in the above range, the glass easily wets and spreads throughout the film even when fired at a low temperature, making it easier to form a dense fired film.
[0053] The specific surface area of the glass frit is preferably 2.0 m 2 / g or more 7.0m 2 / g or less, particularly preferably 3.0m 2 / g or more 6.0m 2 When the specific surface area of the glass frit is in the above range, the glass frit is easily dispersed uniformly in the film, and therefore a dense fired film is easily formed.
[0054] The amount of glass frit relative to 100 parts by mass of the conductive powder is preferably 1 part by mass or more and 20 parts by mass or less, more preferably 4 parts by mass or more and 18 parts by mass or less, even more preferably 6 parts by mass or more and 16 parts by mass or less, and particularly preferably 8 parts by mass or more and 14 parts by mass or less. When the amount of glass frit is within the above range, a dense fired film can be easily formed.
[0055] <Surface Treatment Agent> The copper-based conductive powder of the present invention preferably has an aliphatic amine on at least a portion of its surface. By having an aliphatic amine on at least a portion of its surface, the copper-based conductive powder can prevent oxidation of the copper-based conductive powder and improve the dispersibility of the conductive powder in the paste. This improves the packing of the conductive powder in the coating film of the conductive paste of the present invention, thereby enabling the formation of a fired film with excellent density even when fired at a low temperature. Furthermore, the improved dispersibility of the conductive powder in the paste makes it easier to form thin, highly continuous terminal electrodes.
[0056] In the present invention, the aliphatic amine is preferably present in an amount of 0.01 to 1.0 part by mass, more preferably 0.02 to 1.0 part by mass, more preferably 0.03 to 1.0 part by mass, more preferably 0.04 to 1.0 part by mass, still more preferably 0.05 to 1.0 part by mass, and particularly preferably 0.1 to 0.5 part by mass, relative to 100 parts by mass of the copper-based conductive powder. When the amount of the aliphatic amine is within the above range, the dispersibility of the conductive powder in the paste is improved, and the binder removal property during firing is also improved, making it easier to form thin, dense, and highly continuous terminal electrodes.
[0057] As the aliphatic amine in the present invention, various types can be used, including primary amines such as octylamine, laurylamine, myristylamine, stearylamine, oleylamine, tallowamine, and tallowpropylenediamine; secondary amines such as distearylamine; and tertiary amines such as triethylamine, dimethyloctylamine, dimethylmyristylamine, dimethylpalmitylamine, dimethylstearylamine, dimethylbehenylamine, dimethyllaurylamine, and trioctylamine. Two or more of these amines may be used in combination, and mixtures of several aliphatic amines that are typically commercially available as "aliphatic amines" can also be used. In particular, from the standpoints of ease of coating treatment on copper powder and metal adsorption, alkylamines having a main chain of approximately 8 to 20 carbon atoms, or aliphatic amines containing such alkylamines as the main component, are preferred.
[0058] <Binder Resin> The binder resin in the present invention is not particularly limited, but preferably contains an acrylic resin. The ratio of the acrylic resin to the total binder resin is preferably more than 50% by mass, more preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more. When an acrylic resin is used, it has excellent thermal decomposition properties in a nitrogen atmosphere, so the binder resin can be successfully removed without oxidizing copper.
[0059] The amount of binder resin per 100 parts by mass of conductive powder is not particularly limited, but is preferably 3 parts by mass to 11 parts by mass, more preferably 4 parts by mass to 10 parts by mass, even more preferably 5 parts by mass to 9 parts by mass, and particularly preferably 6 parts by mass to 8 parts by mass. When the amount of binder resin is within the above range, it becomes easier to form a terminal electrode that is thin, dense, and has excellent continuity.
[0060] The weight-average molecular weight of the acrylic resin is not particularly limited, but may be, for example, from 20,000 to 1,000,000. Two or more types of acrylic resins having different weight-average molecular weights, structures, etc. may be used in combination.
[0061] <Organic Solvent> The organic solvent in the present invention is not particularly limited, and examples thereof include terpineol, dihydroterpineol, dihydroterpineol acetate, secondary butyl alcohol, butyl carbitol, butyl carbitol acetate, and benzyl alcohol.
[0062] <Additives> In addition to the above components, the conductive paste of the present invention may contain additives such as antifoaming agents, plasticizers, dispersants, and rheology modifiers, as needed, as long as the effects of the present invention are not impaired. Examples of plasticizers include dimethyl phthalate, diethyl phthalate, dibutyl phthalate, di-2-ethylhexyl phthalate, di-n-octyl phthalate, butyl benzyl phthalate, dioctyl adipate, diisononyl adipate, dibutyl sebacate, diethyl sebacate, dioctyl sebacate, tricresyl phosphate, chlorinated paraffin, and cyclohexane 1,2-dicarboxylic acid diisononyl ester. Examples of rheology modifiers include silica powder.
[0063] <Physical Properties of Conductive Paste> The shear rate of the conductive paste of the present invention measured at 25°C was 4 s -1 The viscosity of the conductive paste is not particularly limited, but is preferably 10.0 Pa s or more and 80.0 Pa s or less, and particularly preferably 20.0 Pa s or more and 60.0 Pa s or less. When the viscosity of the conductive paste is in the above range, it becomes easier to form thin, dense, and highly continuous terminal electrodes.
[0064] The conductive paste of the present invention has a shear rate of 40 s when measured at 25°C. -1 Viscosity at a shear rate of 0.4 s -1 The viscosity ratio in the conductive paste is not particularly limited, but is preferably 2.0 or more and 20.0 or less, and particularly preferably 3.0 or more and 8.0 or less. When the viscosity ratio of the conductive paste is in the above range, it becomes easier to form a thin, dense, and highly continuous terminal electrode.
[0065] When a strain of 1% is applied to the conductive paste of the present invention at an angular frequency of 1 Hz, the value of the phase difference δ between the strain and the stress generated by the strain is not particularly limited, but is preferably 45° to 80°, and particularly preferably 45° to 78°. When the phase difference δ of the conductive paste is within the above range, it becomes easier to form thin, dense, and highly continuous terminal electrodes.
[0066] The conductive paste of the present invention can be used to calculate the electrode area ratio of the terminal electrodes, the average maximum thickness of the terminal electrodes, and the average minimum thickness of the terminal electrodes, as described below, using an evaluation test sample prepared, for example, by the following method. The evaluation test sample can be prepared, for example, by preparing a rectangular parallelepiped laminated body having a length of 0.6 mm, a width of 0.3 mm, and a height of 0.3 mm, in which a plurality of dielectric layers containing barium titanate and internal electrode layers containing nickel are stacked, and applying the conductive paste to the end of the laminated body where the internal electrodes are exposed by dip printing, with the laminated body lowered at a rate of 300 μm / s and pulled up at a rate of 100 μm / s, and then holding the body in an air atmosphere at 150°C for 10 minutes, and then heating the body in a nitrogen atmosphere at a heating rate of 50°C / min, and after reaching 700°C or 720°C, holding the body for 15 minutes to form terminal electrodes, thereby producing 20 electronic components equipped with terminal electrodes, and embedding each of the 20 electronic components in resin. Each electronic component can be prepared by cutting the electronic component so as to pass through the center of each end face of the electronic component and in the stacking direction (perpendicular to the dielectric layers and internal electrode layers) to expose a cross section of the electronic component.
[0067] <Method for manufacturing electronic components> The conductive paste of the present invention is suitable as a conductive paste for forming electrodes on an electrode-forming body (hereinafter also referred to as an electrode-forming body for electronic components) on which electrodes are to be formed in the manufacture of electronic components, and is particularly suitable as a conductive paste for forming terminal electrodes on a laminate base body for multilayer electronic components.
[0068] A preferred method for manufacturing an electronic component using the conductive paste of the present invention includes a preparation step of preparing an electrode-forming body for electronic components, and an electrode-forming step of applying a conductive paste to the outer surface of the electrode-forming body for electronic components and then firing the applied conductive paste to form an electrode, and the method includes forming an electrode on the electrode-forming body for electronic components using the conductive paste of the present invention. By using the conductive paste of the present invention in the above-mentioned method for manufacturing an electronic component, even when firing is performed at a low temperature in the electrode-forming step, thin, dense, and highly continuous electrodes can be formed while maintaining high productivity. In other words, according to the above-mentioned method for manufacturing an electronic component, even when firing is performed at a low temperature in the electrode-forming step, electronic components having thin, dense, and highly continuous electrodes can be manufactured while maintaining high productivity.
[0069] The preparation step is a step of preparing an electrode-forming body for electronic components. The electrode-forming body for electronic components refers to an object on which an electrode is formed in the manufacturing process of an electronic component. Examples of the electrode-forming body for electronic components include a laminate for a multilayer electronic component consisting of multiple ceramic layers and multiple internal electrode layers, and a cathode-forming body for a solid electrolytic capacitor consisting of an anode and a dielectric layer formed on the surface of the anode.
[0070] The electrode forming step is a step of applying a conductive paste to the outer surface of an electrode-forming body for electronic components and firing the applied conductive paste to form an electrode. Examples of methods for applying the conductive paste include dip printing, screen printing, and roll coating. Among these, dip printing is preferred.
[0071] In the electrode formation step, the position, method, thickness, number of electrodes, type of metal constituting the electrodes, shape of the conductive powder used to form the electrodes, etc. are appropriately selected depending on the electronic component to be manufactured.
[0072] In the electrode forming step, after forming electrodes on the body for forming an electrode for electronic components, appropriate steps can be included depending on the type of electronic component. For example, in the case of a multilayer electronic component, in the electrode forming step, electrodes are formed at predetermined positions on the multilayer body for electronic components, and then a plating layer is formed on the surface of the electrode.
[0073] A particularly preferred method for manufacturing electronic components using the conductive paste of the present invention includes a laminate body preparation step of preparing a laminate body for a multilayer electronic component comprising a plurality of ceramic layers and a plurality of internal electrode layers, and a terminal electrode formation step of applying a conductive paste to exposed ends of the internal electrodes of the laminate body and then firing the applied conductive paste to form terminal electrodes, in which the terminal electrodes are formed on the laminate body using the conductive paste of the present invention. By using the conductive paste of the present invention in the above-mentioned method for manufacturing electronic components, thin, dense, and highly continuous terminal electrodes can be formed while maintaining high productivity, even when firing is performed at a low temperature in the terminal electrode formation step. In other words, the above-mentioned method for manufacturing electronic components allows electronic components having thin, dense, and highly continuous terminal electrodes to be manufactured while maintaining high productivity, even when firing is performed at a low temperature in the terminal electrode formation step.
[0074] A laminate element for a multilayer electronic component comprises a plurality of ceramic layers and a plurality of internal electrode layers. In the laminate element for a multilayer electronic component, the ceramic layers and the internal electrode layers are alternately stacked. Examples of laminate elements for multilayer electronic components include laminate elements for multilayer ceramic capacitors, laminate elements for multilayer ceramic inductors, and laminate elements for piezoelectric actuators.
[0075] Examples of materials for forming the ceramic layers constituting the laminate element for a laminate-type electronic component include barium titanate, strontium titanate, calcium titanate, barium zirconate, strontium zirconate, calcium zirconate, and strontium calcium zirconate.
[0076] Examples of materials for forming the internal electrode layers constituting the laminated base body for a laminated electronic component include nickel, palladium, silver, copper, gold, etc., or alloys containing one or more of these (e.g., an alloy of silver and palladium, etc.).
[0077] In the terminal electrode forming step, the conductive paste of the present invention is applied to the exposed ends of the internal electrodes of the laminate element for a multilayer electronic component, and the applied conductive paste is fired to form the terminal electrodes. The method for applying the conductive paste is not particularly limited, and examples thereof include dip printing, screen printing, and roll coating. Of these, dip printing is preferred. Note that the conductive paste may be applied to the laminate element, dried, and then fired.
[0078] In this specification, both ends of the laminated element where the internal electrodes are exposed are referred to as "ends," the surfaces of the ends where the internal electrodes are particularly exposed are referred to as "end faces," and the outer edge portions of the end faces are referred to as "corners." Typically, when applying a conductive paste to the ends in the terminal electrode formation process, the conductive paste is applied so as to cover the end faces and corners.
[0079] The size of the laminated element in which the conductive paste of the present invention is used is not particularly limited, and the paste can be used, for example, in laminated elements for 2012-size multilayer ceramic capacitors, laminated elements for 1608-size multilayer ceramic capacitors, laminated elements for 1005-size multilayer ceramic capacitors, laminated elements for 0603-size multilayer ceramic capacitors, laminated elements for 0402-size multilayer ceramic capacitors, and laminated elements for 0201-size multilayer ceramic capacitors. Thinner terminal electrodes are particularly required in small multilayer ceramic capacitors, and the conductive paste of the present invention can be suitably used in laminated elements for 1005-size multilayer ceramic capacitors, laminated elements for 0603-size multilayer ceramic capacitors, laminated elements for 0402-size multilayer ceramic capacitors, and laminated elements for 0201-size multilayer ceramic capacitors.
[0080] The electrode area ratio of the terminal electrodes of the multilayer electronic component obtained by the present invention is not particularly limited, but is preferably 90% or more, and particularly preferably 99% or more. This makes it easier to prevent the plating solution from penetrating into the laminated body when plating the terminal electrodes. The electrode area ratio can be calculated, for example, by the following method. That is, a plurality of electronic components (e.g., 20 components) are embedded in resin, and each electronic component is cut through the center of each end face of the electronic component in the stacking direction (perpendicular to the dielectric layers and internal electrode layers) to expose a cross section of each electronic component. The cross section is observed with a scanning electron microscope (e.g., 10 fields of view for each electronic component), and the ratio of the electrode area to the observed field of view can be calculated as the electrode area ratio.
[0081] The maximum thickness of the terminal electrodes, measured by the method described below, is preferably 40 μm or less, more preferably 30 μm or less, more preferably 20 μm or less, even more preferably 15 μm or less, and particularly preferably 10 μm or less. The average maximum thickness of the terminal electrodes, calculated by the method described below, is preferably 40 μm or less, more preferably 30 μm or less, more preferably 20 μm or less, even more preferably 15 μm or less, and particularly preferably 10 μm or less. This allows the size of the multilayer electronic component to be reduced. Furthermore, for a multilayer electronic component of a given size, the thinner the terminal electrodes, the larger the size of the multilayer base body, i.e., the greater the electrode area and the number of layers can be increased, thereby improving the performance of the multilayer electronic component. The method for measuring the maximum thickness is not particularly limited, but for example, an electronic component is embedded in a resin, and the electronic component is cut in the lamination direction (perpendicular to the dielectric layers and internal electrode layers) so as to pass through the center of both end face portions of the electronic component to expose a cross section of the electronic component, and the cross section is observed with a scanning electron microscope. When a perpendicular line is drawn on the cross section from the outer periphery of the terminal electrode to the end face portion of the laminated body, the point where the length of the perpendicular line is longest can be measured as the maximum thickness. The method for calculating the average maximum thickness is not particularly limited, but for example, the average maximum thickness of the terminal electrode can be calculated by measuring the maximum thickness of each of the terminal electrodes using the above method for a plurality of electronic components (e.g., 20 electronic components) and averaging the maximum thicknesses.
[0082] The minimum thickness of the terminal electrodes measured by the method described below is preferably 1.0 μm or more, more preferably 2.5 μm or more, and particularly preferably 5.0 μm or more. The average value of the minimum thickness of the terminal electrodes calculated by the method described below is preferably 1.0 μm or more, more preferably 2.5 μm or more, and particularly preferably 5.0 μm or more. This makes it easier to prevent the plating solution from penetrating into the laminated body when plating the terminal electrodes. The method for measuring the minimum thickness is not particularly limited, but for example, an electronic component can be embedded in resin, cut through the center of both end face portions of the electronic component in the stacking direction (perpendicular to the dielectric layers and internal electrode layers) to expose a cross section of the electronic component, observe the cross section with a scanning electron microscope, measure the thickness of the point where the length of a perpendicular line drawn from the outer periphery of the terminal electrode to the end face portion of the laminated element body is smallest, and the thickness of the point where the distance between the corner portion of the laminated element body and the outer periphery of the terminal electrode is shortest, and the thickness of the thinnest of these points can be measured as the minimum thickness. Furthermore, the method for calculating the average of the minimum thicknesses is not particularly limited, but for example, the average of the minimum thicknesses can be calculated by measuring the minimum thickness of the terminal electrodes of a plurality of electronic components (e.g., 20 electronic components) using the above method and averaging the minimum thicknesses.
[0083] The present invention will be described below based on specific experimental examples, but the present invention is not limited to these.
[0084] <Preparation of Conductive Powder> First, multiple types of spherical copper powders and spherical silver powders with different particle sizes were prepared, and the particle size distribution and particle size were adjusted by classification. Next, zirconia beads with a diameter of 0.1 mm, the spherical copper powder, secondary butyl alcohol, and a predetermined surface treatment agent (aliphatic amine) were mixed and pulverized using a bead mill by appropriately adjusting the flow rate and number of passes. Further, classification was performed as necessary to adjust the particle size distribution and particle size, thereby obtaining copper powders 1 to 22 and silver powder 1 listed in Table 1. Note that the aforementioned pulverization process was not performed on copper powder 1, copper powder 3, and silver powder 1. Copper powder 3 and silver powder 1 were obtained by surface treatment using a predetermined surface treatment agent (aliphatic amine). For the obtained copper powders 1 to 22 and silver powder 1, the major and minor axes of 500 copper particles (silver particles in the case of silver powder 1, and copper and silver particles in the case of mixed powder C) were measured using a scanning electron microscope, and the average major and minor axes were calculated. The conductive pastes prepared in Experimental Examples 1 to 16 and 20 to 25 described below were cast onto a PET film using an applicator to form a coating film with a thickness of 250 μm, and the coating film was dried in an air atmosphere at 150°C for 10 minutes to form a dry film. The cross section of the dry film was exposed using an ion milling device (Hitachi High-Tech Corporation, model number: IM4000). The cross section of the dry film was observed using a scanning electron microscope (Hitachi High-Tech Corporation, model number: SU-8020). Based on the observation, 500 copper particles were randomly selected and their minor axes were measured. The minor axes were used as the thickness to calculate the average thickness. From the average major axis, average minor axis, and average thickness calculated as described above, the ratio of the average major axis to the average thickness and the ratio of the average major axis to the average minor axis were calculated. Furthermore, the volume-based cumulative 10% particle diameter D10, cumulative 50% particle diameter D50, and cumulative 90% particle diameter D90 were measured using a laser diffraction particle size distribution analyzer (LA-960, manufactured by HORIBA Co., Ltd.). Using these measured values, (D90-D10) / D50 was calculated.Mixed powder A was a powder obtained by mixing copper powder 3 and copper powder 5 in a mass ratio of 20:80 (used in Experimental Example 18 described below), mixed powder B was a powder obtained by mixing copper powder 3 and copper powder 5 in a mass ratio of 45:55 (used in Experimental Example 19 described below), and mixed powder C was a powder obtained by mixing copper powder 5 and silver powder 1 in a mass ratio of 90:10 (used in Experimental Example 17 described below). The "ratio of average major axis to average thickness," "ratio of average major axis to average minor axis," "D50," and "(D90-D10) / D50" of the mixed powders (i.e., the conductive powder as a whole) were measured and calculated using the methods described above. The average thicknesses of mixed powders A to C were measured and calculated using the same methods as described above, except that the conductive pastes prepared in Experimental Examples 17 to 19 were used. The average thickness of Silver Powder 1 was measured and calculated in the same manner as described above except that a conductive paste was prepared in the same manner as in Experimental Example 1, except that Silver Powder 1 was used instead of Copper Powder 1. The results are shown in Table 1.
[0085]
[0086] <Preparation of Glass Frit> BaO-ZnO based glass (BaO: 30 mol %, ZnO: 27 mol %, B 2 O 3 :25 mol%, SiO 2 :7 mol%, CaO: 7 mol%, Al 2 O 3 4 mol%) was prepared, and the particle size and particle size distribution were adjusted by pulverization and classification to prepare glass frits 1 to 8 shown in Table 2. The volume-based cumulative 10% particle diameter D10 of the prepared glass frits was measured using a laser diffraction particle size distribution analyzer (HORIBA, LA-960). G , Cumulative 50% particle diameter D50 G , cumulative 90% particle diameter D90 G Using the measured value, (D90 G -D10 G ) / D50 Gwas calculated. The glass transition point and softening point were also measured using the glass frit. The glass frit was placed in a cylindrical container with an inner diameter of 5 mm, and a pressure of 3 MPa was applied in the axial direction for 10 seconds to create a cylindrical green compact with a diameter of 5 mm and a height of 1 mm. The green compact was placed on a copper plate with a surface roughness Ra of 100 nm so that the flat surface of the green compact was in contact with the copper plate. The green compact was heated in a nitrogen atmosphere at a heating rate of 10°C / min up to 700°C to melt the glass constituting the green compact. The contact angle of the glass with the copper plate was then measured. The contact angle of glass frit 4 was also measured when the temperature was raised to 680°C and 720°C. The contact angle was 50°, similar to the contact angle at 700°C.
[0087]
[0088] <Preparation of Conductive Paste> Conductive powder, binder resin, and glass frit were blended in the blending ratios shown in Tables 3 to 6 to prepare conductive pastes. The amounts of surface treatment agent shown in the tables indicate the amount adhered to the powder surface by surface treatment when preparing the conductive powder. Copper Powders 1 to 22, Silver Powder 1 The ratio of average major diameter X to average thickness Z, the ratio of average major diameter X to average minor diameter Y, D50, and (D90-D10) / D50 are as shown in Table 1. Acrylic Resin 1: Mitsubishi Chemical Corporation, Model Number: DIANAL MB-2677, Weight-average molecular weight: 700,000 Acrylic Resin 2: Mitsubishi Chemical Corporation, Model Number: DIANAL BR-105, Weight-average molecular weight: 50,000 Glass Frits 1 to 8: D50 G , (D90 G -D10 G ) / D50 G The contact angle with respect to the copper plate, softening point and glass transition point are as shown in Table 2.
[0089] (Experimental Examples 1 to 35, 41, and 42) The conductive powder shown in Table 1, the glass frit shown in Table 2, and the acrylic resin 1 dissolved in terpineol were mixed in the blending ratios shown in Tables 3 to 6, and then kneaded using a three-roll mill (manufactured by Inoue Seisakusho). Then, the mixture was diluted with terpineol and heated at 25°C and a shear rate of 4 s -1Conductive pastes were prepared by adjusting the viscosity at 100°C to the values shown in Tables 3 to 6. The prepared conductive pastes were used to carry out the evaluations described below. The results are shown in Tables 3 to 6. Note that experimental examples marked with "*" are experimental examples outside the scope of the present invention.
[0090] (Experimental Examples 36 to 40) The conductive powder shown in Table 1, the glass frit shown in Table 2, and the acrylic resin 1 or acrylic resin 2 dissolved in terpineol were mixed in the blending ratios shown in Tables 3 to 6, and then kneaded using a three-roll mill (manufactured by Inoue Seisakusho). Then, the mixture was diluted with terpineol and, if necessary, dipropylene glycol-n-propyl ether, and heated at 25°C at a shear rate of 4 s -1 Conductive pastes were prepared by adjusting the viscosity and viscosity ratio at each temperature to the values shown in Table 6. The prepared conductive pastes were evaluated as described below. The results are shown in Table 6.
[0091] (Experimental Example 43) In this experimental example, the conductive paste prepared in Experimental Example 5 was used. When evaluating the terminal electrodes, the terminal electrodes were evaluated in the same manner as in Experimental Example 5, except that a laminated element having a length of 0.4 mm, a width of 0.2 mm, and a height of 0.2 mm, which was a substantially rectangular parallelepiped, and in which multiple dielectric layers containing barium titanate and internal electrode layers containing nickel were stacked was used.
[0092]
[0093]
[0094]
[0095]
[0096] <Evaluation of Physical Properties of Conductive Paste> (Viscosity) The viscosity of the conductive paste was measured at 25° C. and a shear rate of 4 s using a rotational viscometer (manufactured by Brookfield, model number: HADV-II+Pro). -1 The measurement was carried out under the following conditions.
[0097] (Viscosity Ratio) The viscosity of the conductive paste was measured at 25° C. and a shear rate of 0.4 s using a rotational viscometer (manufactured by Brookfield, model number: HADV-II+Pro). -1 and shear rate 40 s-1 Measurement was carried out under the following conditions: Shear rate 40 s -1 Viscosity at a shear rate of 0.4 s -1 The viscosity ratio was calculated as the ratio of the viscosities of the above.
[0098] (Retardation) The retardation value of the conductive paste was measured using a rheometer (manufactured by TA Instrument, model number: AR2000) under conditions of 25°C, an angular frequency of 1 Hz, and a strain of 1%, using parallel plates with a diameter of 40 mm.
[0099] <Evaluation Test of Terminal Electrodes> (Fabrication of Electronic Components with Terminal Electrodes) A laminated element having a length of 0.6 mm, a width of 0.3 mm, and a height of 0.3 mm was prepared, which was a roughly rectangular parallelepiped, and comprised multiple laminated layers of dielectric layers containing barium titanate and internal electrode layers containing nickel. A conductive paste was applied to the end of this laminated element, where the internal electrodes were exposed, by dip printing, with the laminated element lowered at a rate of 300 μm / s and raised at a rate of 100 μm / s. The laminated element was then held at 150°C in an air atmosphere for 10 minutes. The temperature was then increased at a rate of 50°C / min in a nitrogen atmosphere. After reaching the temperatures listed in Tables 3 to 6, the temperature was held for 15 minutes to form terminal electrodes, thereby fabricating electronic components with terminal electrodes.
[0100] (Preparation of Evaluation Test Samples) In each experimental example, 20 of the above-described electronic components were prepared. Each electronic component was embedded in resin, and cut through the center of each end face of each electronic component in the lamination direction (perpendicular to the dielectric layers and internal electrode layers) to expose the cross section of each electronic component, thereby preparing an evaluation test sample. The following evaluations were performed.
[0101] (Density of terminal electrodes (electrode area ratio)) The above-mentioned evaluation test samples were observed with a scanning electron microscope, with 10 visual fields per sample for a total of 200 visual fields, and the ratio of the electrode area to the visual fields was calculated as the electrode area ratio. The electrode area ratio value was evaluated based on the following evaluation criteria and given a rating of 1 to 3. A rating of 2 or more was considered to be acceptable. <Evaluation criteria> 3: Electrode area ratio is 99% or more 2: Electrode area ratio is 90% or more but less than 99% 1: Electrode area ratio is less than 90%
[0102] (Fired Film Thickness of Terminal Electrode) The above-mentioned evaluation test samples were observed with a scanning electron microscope, and the thickness of the thickest part (maximum thickness) and the thickness of the thinnest part (minimum thickness) of the terminal electrode (fired film) were measured, and the average value of the maximum thickness and the average value of the minimum thickness were calculated for each experimental example. The average values of the maximum thickness and the average value of the minimum thickness were evaluated based on the following evaluation criteria, and scores of 1 to 3 were given. A score of 2 or more was considered to be pass. <Evaluation Criteria> 3: Average maximum thickness ≦ 20 μm and average minimum thickness ≧ 2.5 μm 2: Average maximum thickness ≦ 40 μm and average minimum thickness ≧ 1.0 μm (excluding cases that fall under the above score 3) 1: Average maximum thickness > 40 μm or average minimum thickness < 1.0 μm
[0103] The method for measuring the fired film thickness will be described with reference to Figure 1. Figure 1 is a schematic diagram showing an evaluation test sample 10 obtained by forming terminal electrodes 4 on a laminated element 1 using a conductive paste. In the cross section of the evaluation test sample 10 observed with the scanning electron microscope described above, a perpendicular line is drawn from the outer periphery 5 of the terminal electrodes 4 to the end face 3 of the laminated element 1, and the length of the perpendicular line is defined as D. The thickness at the point where D is maximum is measured, and this thickness value is defined as the maximum thickness D. max Furthermore, the thickness Da at the point where the value of D is smallest and the thickness Db at the point where the distance between the corner portion 2 of the laminated element 1 and the outer periphery 5 of the terminal electrode 4 is shortest are measured, and the smaller of Da and Db is taken as the minimum thickness D min In addition, when the cross section of the evaluation test sample 10 observed with the scanning electron microscope described above had a portion where the laminated element body 1 was exposed due to a hole or the like in the terminal electrode 4, the minimum thickness was set to "0 μm."
[0104] As is clear from the above experimental examples, by using the conductive paste of the present invention, it was possible to form thin, dense, and highly continuous terminal electrodes while maintaining high productivity, even when firing at low temperatures such as 720°C or less.
[0105] 1 laminated element body 2 corner portion 3 end surface portion 4 terminal electrode 5 outer periphery portion 10 evaluation test sample D length of perpendicular line drawn from outer periphery portion to end surface portion Da thickness at the point where the value of D is smallest Db thickness at the point where the distance between the corner portion and outer periphery portion is shortest D max The thickness where D is the maximum min The smaller value of Da and Db
Claims
1. A conductive paste containing copper-based conductive powder, glass frit, binder resin, and organic solvent, wherein the volume-based cumulative 50% particle diameter D50 of the copper-based conductive powder measured by laser diffraction particle size distribution measurement is C a ratio of an average major diameter X to an average minor diameter Y is 1.0 to 3.0, and a ratio of an average major diameter X to an average thickness Z defined below is 1.1 to 9.0, and the volume-based cumulative 50% particle diameter D50 of the glass frit measured by laser diffraction particle size distribution measurement is G A conductive paste characterized in that the thickness of the conductive paste containing the copper-based conductive powder is 0.3 μm or more and 2.0 μm or less. (Average Thickness) The conductive paste containing the copper-based conductive powder is cast onto a PET film with an applicator to form a coating film with a thickness of 250 μm, and the coating film is dried in an air atmosphere at 150° C. for 10 minutes to form a dry film. A cross section of the dry film is exposed by ion milling, and the cross section of the dry film is observed with a scanning electron microscope. 500 conductive particles are randomly selected and the minor axis is measured as the thickness to determine the average value of the thicknesses, and this average value is defined as the “average thickness.” 2. The conductive paste according to claim 1, wherein the copper-based conductive powder has an aliphatic amine on at least a portion of its surface.
3. The conductive paste according to claim 2, characterized in that the aliphatic amine is contained in an amount of 0.01 to 1.0 parts by mass per 100 parts by mass of the conductive powder containing copper as the main component.
4. The cumulative 10% particle diameter of the glass frit on a volume basis measured by laser diffraction particle size distribution measurement is D10 G The cumulative 90% particle size is D90 G When this is done, (D90 G -D10 G ) / D50 G The conductive paste according to any one of claims 1 to 3, wherein the σ is 7.5 or less.
5. The volume-based cumulative 10% particle diameter of the copper-based conductive powder measured by laser diffraction particle size distribution measurement is D10 C The cumulative 90% particle size is D90 C When this is done, (D90 C -D10 C ) / D50 C The conductive paste according to any one of claims 1 to 4, wherein the value of the solubility coefficient of the conductive paste is 7.5 or less.
6. Shear rate 40 s when measured at 25 °C -1 Viscosity at a shear rate of 0.4 s -1 The conductive paste according to any one of claims 1 to 5, characterized in that the ratio of viscosities in the range of 2.0 to 20.0 is greater than or equal to 2.0, and when a strain of 1% is applied to the conductive paste at an angular frequency of 1 Hz, the value of the phase difference δ between the strain and the stress generated by the strain is greater than or equal to 45° and less than or equal to 80°.
7. The conductive paste according to any one of claims 1 to 6, characterized in that the electrode area ratio of the terminal electrodes is 90% or more, the average maximum thickness of the terminal electrodes is 40 μm or less, and the average minimum thickness of the terminal electrodes is 1.0 μm or more, as calculated by the following evaluation tests. <Terminal Electrode Area Ratio Evaluation Test> Evaluation test samples prepared by the following evaluation test sample preparation method are observed with a scanning electron microscope in 10 fields of view for each sample, and the ratio of the electrode area in the observed fields is calculated as the electrode area ratio of the terminal electrode. <Terminal Electrode Maximum Thickness Evaluation Test> Evaluation test samples prepared by the following evaluation test sample preparation method are observed with a scanning electron microscope, and the maximum thickness of the evaluation test sample is measured at the point where the length of a perpendicular line is longest when a perpendicular line is drawn from the outer periphery of the terminal electrode to the end face of the laminated body. The maximum thicknesses of 20 electronic components whose maximum thicknesses were measured are averaged to calculate the average maximum thickness of the terminal electrodes. <Terminal Electrode Minimum Thickness Evaluation Test> An evaluation test sample prepared by the evaluation test sample preparation method described below is observed with a scanning electron microscope, and the thickness of the evaluation test sample is measured at the point where the length of a perpendicular line drawn from the outer periphery of the terminal electrode to the end face of the laminated body is the shortest, and the thickness of the point where the distance between the corner of the laminated body and the outer periphery of the terminal electrode is the shortest. The thickness of the thinnest of these points is measured as the minimum thickness, and the minimum thicknesses of 20 electronic components whose minimum thicknesses have been measured are averaged to calculate the average minimum thickness of the terminal electrodes.<Method of Preparing Evaluation Test Samples> A rectangular parallelepiped laminated body having a length of 0.6 mm, a width of 0.3 mm, and a height of 0.3 mm, in which a plurality of dielectric layers containing barium titanate and internal electrode layers containing nickel are stacked, is prepared. The conductive paste is applied to the end of the laminated body where the internal electrodes are exposed by dip printing, with the laminated body lowered at a rate of 300 μm / s and pulled up at a rate of 100 μm / s. The laminated body is then held in an air atmosphere at 150°C for 10 minutes, and then heated in a nitrogen atmosphere at a heating rate of 50°C / min. After reaching 720°C, the temperature is held for 15 minutes to form terminal electrodes, thereby producing 20 electronic components equipped with terminal electrodes. The 20 electronic components are each embedded in resin, and each electronic component is cut in the stacking direction (perpendicular to the dielectric layers and internal electrode layers) so as to pass through the center of each end face of the electronic component to expose a cross section of the electronic component, thereby preparing an evaluation test sample.
8. A method for manufacturing electronic components, comprising: a laminated body preparation step of preparing a laminated body for a multilayer electronic component comprising a plurality of ceramic layers and a plurality of internal electrode layers; and a terminal electrode formation step of applying a conductive paste to the exposed ends of the internal electrodes of the laminated body and then firing the applied conductive paste to form terminal electrodes, wherein the conductive paste is the conductive paste defined in any one of claims 1 to 7.
9. The method for manufacturing an electronic component according to claim 8, wherein the peak temperature of the firing is 720°C or less.