Receiving substrate, laser lift-off method, lift method, holding method, and method for cleaning microstructure

MYPI2025002385A0Undetermined Publication Date: 2024-04-21SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025002385
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-21
Filing Date
2023-10-10
Publication Date
2024-04-21

AI Technical Summary

Technical Problem

Existing methods for transferring microstructures like mini LEDs and micro LEDs face issues with damage, misalignment, tilting, and falling during laser lift-off and cleaning, particularly due to uneven loading and the use of aqueous hydrochloric acid which affects solder components.

Method used

A receiving substrate with a curable resin layer is used to prevent local stress and misalignment during laser lift-off, and to securely hold microstructures by burying protrusions in the resin layer, which is then cured to increase hardness and adhesion, allowing for reliable transfer and cleaning without displacement or tilting.

Benefits of technology

The solution effectively prevents damage, misalignment, and tilting of microstructures during transfer and cleaning, ensuring reliable adhesion and positioning, even with protrusions, and maintains the integrity of solder components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025002385_DRAWING_001
    Figure PI2025002385_DRAWING_001
  • Figure PI2025002385_DRAWING_002
    Figure PI2025002385_DRAWING_002
  • Figure PI2025002385_DRAWING_003
    Figure PI2025002385_DRAWING_003
Patent Text Reader

Abstract

The present invention is a receiving substrate for receiving a microstructure formed on a supply substrate and transferred by laser lift-off, wherein the receiving substrate includes a curable resin layer on a face to which the microstructure is to be transferred. Thus, the present invention can provide a receiving substrate that is capable of receiving a microstructure while suppressing damage, and also holding the microstructure while controlling displacement and a tilt thereof. Fig. 1
Need to check novelty before this filing date? Find Prior Art

Description

Receiving substrate, method for manufacturing receiving substrate, lifting method, holding method, and method for cleaning microstructure

[0001] The present invention relates to a receiving substrate used when transferring a microstructure such as a mini light-emitting diode (hereinafter also referred to as a mini LED) or a micro light-emitting diode (hereinafter also referred to as a micro LED), a method for manufacturing the receiving substrate, a laser-induced forward transfer (LIFT) method for transferring the microstructure, a holding method for holding the microstructure on the receiving substrate, and a method for cleaning the microstructure.

[0002] In recent years, with the miniaturization of semiconductor elements, microstructure transfer technology using adhesive resins has attracted attention as a means of assembling electrical and electronic products using semiconductor elements. In particular, there has been active development of technology for manufacturing LED displays for applications such as signage, TVs, medical devices, in-vehicle displays, and smartphones by transferring tens of thousands of mini-LEDs (LED elements with short sides of 100 μm to several hundred μm) or micro-LEDs (LED elements with short sides of 100 μm or less, or even 50 μm or less) at once.

[0003] We have previously developed a method for transferring microstructures such as microLEDs onto circuit boards using silicone adhesive cured materials as donor substrates or transfer stamp materials (Patent Document 1).

[0004] On the other hand, a known method for electrically connecting a transferred microstructure, such as an LED element, to a circuit board involves applying solder particles (hereinafter also referred to as bumps) to the electrodes of the microstructure, mounting the microstructure on the wiring of the circuit board, and then reflowing the solder particles to melt the solder components contained in the bumps and establish electrical continuity. When transferring a microstructure containing such a bump, the bumps are often rounded, which can lead to problems with the mounting orientation on the donor plate being uneven and tilting relative to the plate plane. Furthermore, for example, after laser lift-off (hereinafter also referred to as LLO) of a blue LED element, Ga adheres to the surface of the microstructure. Using a hydrochloric acid solution as a cleaning solution to remove this Ga also dissolves the solder components, changing their composition. This raises the melting point during reflow and affects subsequent processes. Furthermore, the impact of cleaning often causes the microstructure to fall off.

[0005] Japanese Patent Application Laid-Open No. 2021-34610

[0006] The present invention has been made to solve the above problems, and aims to provide a receiving substrate that can receive a microstructure while minimizing damage and can hold the microstructure while minimizing misalignment and tilting, a method for manufacturing such a receiving substrate, a lifting method that can transfer a microstructure from a supply substrate to a receiving substrate while minimizing damage and hold the microstructure while minimizing misalignment and tilting, a holding method that can minimize misalignment and tilting of the microstructure, and a cleaning method that can clean a microstructure while minimizing falling off, misalignment, and tilting.

[0007] In order to solve the above problem, the present invention provides a receiving substrate for transferring and receiving a microstructure formed on a supply substrate by laser lift-off, the receiving substrate having a curable resin layer on the surface onto which the microstructure is transferred.

[0008] The receiving substrate of the present invention can prevent local stress from being applied to the microstructure during laser lift-off (LLO) and can firmly hold the microstructure. Therefore, the receiving substrate of the present invention can receive the microstructure while suppressing damage, and can also hold the microstructure while suppressing misalignment and tilt.

[0009] For example, the curable resin layer is photocurable or thermosetting.

[0010] The curable resin layer is not particularly limited as long as it is curable, and may be, for example, photocurable or thermosetting.

[0011] For example, the curable resin layer may be in a B-stage state.

[0012] The curable resin layer may be in a B-stage state, i.e., a semi-cured state. After receiving the microstructure, this resin layer can be subjected to a secondary curing treatment to hold the microstructure without causing displacement or tilt.

[0013] The curable resin layer is preferably in a gel state.

[0014] If the resin layer is in a gel state, damage to the microstructure during laser lift-off can be more reliably prevented.

[0015] For example, the curable resin layer may be a silicone-based gel layer.

[0016] The curable resin layer is not limited, but may be, for example, a silicone-based gel layer.

[0017] The curable resin layer preferably has tackiness to the minute structure.

[0018] Such a resin layer can further prevent the received minute structure from being misaligned.

[0019] The hardening resin layer preferably increases in hardness upon curing.

[0020] If the resin layer has a hardness that increases as it hardens, it is possible to further suppress the positional deviation and tilt of the minute structure after hardening.

[0021] Alternatively, it is also preferable that the curable resin layer is one that, upon curing, increases its adhesive strength to the minute structure or its holding power for the minute structure.

[0022] With such a resin layer, it is possible to more reliably prevent the positional deviation and tilt of the minute structure after hardening.

[0023] Alternatively, it is also preferable that the curable resin layer becomes rubbery upon curing.

[0024] If the resin layer becomes rubbery upon hardening, it is possible to further suppress the positional deviation and tilt of the minute structure after hardening.

[0025] In this case, for example, the storage modulus of the curable resin layer may be 10 to 1000 Pa at 25° C., and may be increased to 1 MPa to 30 GPa upon curing.

[0026] The curable resin layer may be one whose storage modulus increases upon curing in this manner, for example.

[0027] The present invention also provides a method for manufacturing a receiving substrate having a curable resin layer, comprising the steps of: forming a layer of a resin capable of undergoing at least two types of curing reactions on one surface of a substrate for preparing a receiving substrate; and partially curing the resin by carrying out the first type of curing reaction.

[0028] This manufacturing method allows a receiving substrate having a curable resin layer to be manufactured by performing a step of partially curing the resin through a first curing reaction. This receiving substrate can prevent localized stress from being applied to the microstructure during laser lift-off and can firmly hold the microstructure. Therefore, the manufactured receiving substrate can receive the microstructure by laser lift-off with reduced damage and can hold the microstructure with reduced misalignment and tilt.

[0029] For example, the at least two types of curing reactions may include a combination of a photocuring reaction and a thermal curing reaction, a combination of thermal curing reactions having different curing initiation temperatures, or a combination of photocuring reactions having different curing wavelengths.

[0030] The combination of the above curing reactions is not particularly limited, but the above-mentioned combinations can be used, for example.

[0031] In this case, for example, the at least two types of curing reactions may include a combination of at least two selected from the group consisting of a radical curing system, a cationic curing system, an anionic curing system, an addition curing system, and a condensation curing system.

[0032] The combination of the above curing reactions is not particularly limited, but the above-mentioned combinations can be used, for example.

[0033] The present invention also provides a lifting method for transferring a microstructure formed on a supply substrate to a receiving substrate by laser lift-off, wherein the surface of the microstructure facing the receiving substrate has a protrusion, the surface of the receiving substrate onto which the microstructure is transferred has a curable resin layer, the microstructure is pressed against the curable resin layer so that the protrusion is embedded in the curable resin layer, the curable resin layer is cured with the protrusion embedded in the curable resin layer to hold the microstructure on the receiving substrate, and laser lift-off is performed with the microstructure held on the receiving substrate.

[0034] With this type of lifting method, laser lift-off is performed with the protrusions of the microstructure buried in the curable resin layer, thereby preventing local stress from being applied to the microstructure during laser lift-off. Therefore, with the lifting method of the present invention, even microstructures with protrusions can be transferred from a supply substrate to a receiving substrate while preventing damage. Furthermore, the curable resin layer of the receiving substrate used in the lifting method of the present invention can be hardened while holding the microstructure, thereby increasing its hardness. Therefore, with the lifting method of the present invention, the microstructure can be held on the receiving substrate while suppressing misalignment and tilting of the received microstructure.

[0035] The present invention also provides a holding method for holding a microstructure having protrusions on a receiving substrate, wherein the receiving substrate has a curable resin layer on the surface that holds the microstructure, the microstructure is pressed against the curable resin layer so that the protrusions are embedded in the curable resin layer, and the curable resin layer is hardened while the protrusions are embedded in the curable resin layer, thereby holding the microstructure on the receiving substrate.

[0036] With this holding method, the protrusions of the microstructure are embedded in the curable resin layer, and the curable resin layer is hardened, thereby preventing damage, misalignment, and tilting of the microstructure, allowing the microstructure to be held on the receiving substrate.

[0037] The present invention also provides a method for cleaning a microstructure, which comprises transferring the microstructure to the receiving substrate using the lifting method of the present invention, and then cleaning the microstructure with an acid or alkaline cleaning solution.

[0038] As described above, the lifting method of the present invention can hold the received microstructure on the receiving substrate while suppressing misalignment and tilting of the microstructure. Therefore, the cleaning method of the present invention can clean the microstructure while suppressing the microstructure from falling off, being misaligned, or being tilted.

[0039] The present invention also provides a cleaning method for a microstructure having protrusions, which comprises pressing the microstructure against a curable resin layer so that the protrusions are embedded in the curable resin layer, and after the curable resin layer is cured, cleaning the microstructure with an acid or alkaline cleaning solution in a state in which the protrusions of the microstructure are tightly covered by the resin layer and no air bubbles are present in the resin layer within 5 μm around the protrusions.

[0040] With this cleaning method, the protrusions of the microstructure are embedded in a curable resin layer, and after this curable resin layer is hardened, the microstructure is cleaned in a state where the protrusions of the microstructure are covered tightly by the resin layer and there are no air bubbles in the resin layer within 5 μm around the protrusions, thereby preventing the microstructure from falling off, shifting in position, or tilting due to cleaning.

[0041] As described above, the receiving substrate of the present invention can receive the microstructure by laser lift-off while suppressing damage, and can also suppress displacement and tilt of the microstructure.

[0042] Furthermore, the method for manufacturing a receiving substrate of the present invention makes it possible to receive a microstructure by laser lift-off while suppressing damage, and to manufacture a receiving substrate that can suppress positional deviation and tilt of the microstructure.

[0043] Furthermore, the lifting method of the present invention can transfer even microstructures having protrusions from a supply substrate to a receiving substrate while preventing damage. Furthermore, the lifting method of the present invention can hold the microstructure on the receiving substrate while suppressing misalignment and tilt of the received microstructure.

[0044] Furthermore, with the holding method of the present invention, it is possible to hold the microstructure on the receiving substrate while suppressing positional deviation and tilt of the microstructure.

[0045] Furthermore, the cleaning method of the present invention makes it possible to clean a minute structure while suppressing falling off, displacement, and tilting.

[0046] 5(B) is a schematic diagram showing an example of a receiving substrate of the present invention; FIG. 5(C) is a schematic diagram showing an example of a method for manufacturing a receiving substrate of the present invention; FIG. 5(D) is a schematic diagram showing an example of a supply substrate that can be used in the present invention; FIG. 5(E) is a schematic diagram showing an example of a lifting method of the present invention; FIG. 5(F) is a schematic diagram showing bonding and secondary curing in an example of lifting of the present invention; FIG. 5(F) is a detailed diagram of FIG. 5(C) is a schematic diagram of another side of the laminated substrate shown in FIG. 6; FIG. 5(F) is a schematic diagram showing LLO and peeling in an example of a lifting method of the present invention; FIG. 5(F) is a schematic diagram showing an example of a cleaning method of the present invention; FIG. 5(F) is a photograph of a microstructure after transfer according to Example 1, a microstructure after peeling following this transfer, and a microstructure after cleaning following this peeling; FIG. 5(F) is a photograph of a microstructure after transfer according to a reference example, a microstructure after peeling following this transfer, and a microstructure after cleaning following this peeling.

[0047] As described above, there was a need to develop a receiving substrate that can receive a microstructure while minimizing damage and can hold the microstructure while minimizing misalignment and tilting, a method for manufacturing such a receiving substrate, a lifting method that can transfer a microstructure from a supply substrate to a receiving substrate while minimizing damage and hold the microstructure while minimizing misalignment and tilting, a holding method that can minimize misalignment and tilting of the microstructure, and a cleaning method that can clean the microstructure while minimizing falling off, misalignment, and tilting.

[0048] After extensive research into the above-mentioned problems, the inventors discovered that by using a receiving substrate containing a curable resin layer, it is possible to receive the microstructure by laser lift-off while minimizing damage, and to reduce the positional shift and tilt of the microstructure, thereby completing the present invention.

[0049] That is, the present invention is a receiving substrate for transferring and receiving a microstructure formed on a supply substrate by laser lift-off, and the receiving substrate has a curable resin layer on the surface onto which the microstructure is transferred.

[0050] The present invention also provides a method for manufacturing a receiving substrate having a curable resin layer, comprising the steps of: forming a layer of a resin capable of undergoing at least two types of curing reactions on one surface of a substrate for preparing a receiving substrate; and partially curing the resin by carrying out a first type of curing reaction.

[0051] The present invention also provides a lifting method for transferring a microstructure formed on a supply substrate to a receiving substrate by laser lift-off, wherein the surface of the microstructure facing the receiving substrate has a protrusion, the surface of the receiving substrate onto which the microstructure is transferred has a curable resin layer, the microstructure is pressed against the curable resin layer so that the protrusion is embedded in the curable resin layer, the curable resin layer is hardened while the protrusion is embedded in the curable resin layer, and the microstructure is held on the receiving substrate, and laser lift-off is performed while the microstructure is held on the receiving substrate.

[0052] The present invention also provides a holding method for holding a microstructure having protrusions on a receiving substrate, wherein the receiving substrate has a curable resin layer on the surface that holds the microstructure, the microstructure is pressed against the curable resin layer so that the protrusions are embedded in the curable resin layer, and the curable resin layer is hardened while the protrusions are embedded in the curable resin layer, thereby holding the microstructure on the receiving substrate.

[0053] The present invention also provides a method for cleaning a microstructure, which comprises transferring the microstructure to the receiving substrate using the lifting method of the present invention, and then cleaning the microstructure with an acid or alkaline cleaning solution.

[0054] The present invention also provides a cleaning method for a microstructure having protrusions, which comprises pressing the microstructure against a curable resin layer so that the protrusions are embedded in the curable resin layer, and after the curable resin layer has hardened, cleaning the microstructure with an acid or alkaline cleaning solution in a state in which the protrusions of the microstructure are tightly covered by the resin layer and no air bubbles are present in the resin layer within 5 μm of the protrusions.

[0055] The present invention will be described in detail below, but the present invention is not limited thereto.

[0056] [Receiving Substrate] FIG. 1 shows a schematic diagram of an example of the receiving substrate of the present invention.

[0057] 1 is a receiving substrate 10 for receiving a microstructure formed on a supply substrate by transferring it thereon by laser lift-off. The supply substrate and the microstructure will be described later.

[0058] The receiving substrate 10 has a curable resin layer 12 on one surface 10A (the surface onto which the microstructure is transferred) as shown in Fig. 1. The receiving substrate 10 of the example shown in Fig. 1 further includes a support substrate 11 that supports the curable resin layer 12.

[0059] The curable resin layer 12 is a layer of resin that can be cured, and can be said to be in a first cured state, a B-stage state, or a semi-cured state.

[0060] The resin of the curable resin layer 12 can deform to conform to the surface shape of the microstructure. When the curable resin layer 12 is cured (e.g., second curing), the resin of the curable resin layer 12 becomes highly hard and maintains its conformity to the surface shape of the microstructure. This prevents local stress from being applied to the microstructure even during laser lift-off (LLO) and firmly holds the microstructure. Therefore, the receiving substrate 10 of the present invention can receive the microstructure while suppressing damage and also prevents misalignment and tilting.

[0061] The curable resin layer 12 and the support substrate 11 will be described in more detail below.

[0062] <Curable Resin Layer> The resin of the curable resin layer 12 used in the present invention is not particularly limited as long as it is curable, and may be, for example, photocurable or thermosetting.

[0063] The resin of the curable resin layer 12 may be, for example, a B-stage two-stage curing resin. After receiving the microstructure, the resin layer 12 is subjected to a secondary curing process, thereby enabling the microstructure to be held without displacement or tilt.

[0064] The B-stage resin of the two-stage curing resin may be, for example, a two-stage curing silicone composition that has been subjected to primary curing.

[0065] A two-stage curing silicone composition is a silicone composition that can be cured in at least two stages by combining at least two types of curing reactions selected from, for example, an addition curing reaction, a photoradical polymerization reaction, a thermal radical polymerization reaction, a cationic curing reaction, an anionic curing reaction, and a condensation curing reaction. The curing modes may be freely combined as long as they do not inhibit each other's curing reactions. Among these, a combination of an addition curing reaction and a photoradical polymerization reaction, a combination of an addition curing reaction and a thermal radical polymerization reaction, and a photoradical polymerization reaction and a thermal radical polymerization reaction are preferred from the standpoint of ease of resin design or curing, and a combination of an addition curing reaction and a photoradical polymerization reaction is particularly preferred from the standpoint of ease of design and curing. The number of at least two types of curing reactions is not particularly limited as long as it is two or more, but can be, for example, two or more and four or less.

[0066] After the application process to the support substrate 11, for example, in the case of first curing by a hydrosilylation reaction, the composition is heated and cured for 5 to 90 minutes in an environment of preferably 20 to 200°C, or in the case of first curing by a photoradical polymerization reaction, the composition is heated and cured for 5 to 3000 mW / cm using 365 nm light as an index in a nitrogen environment. 2 and 100 to 20,000 mJ / cm 2The first cured curable silicone-based resin layer can be formed under curing conditions suitable for the silicone-based composition, such as by irradiating the composition with ultraviolet light at an integrated light amount of 1000 nm or more.

[0067] Here, the storage modulus of the curable resin layer 12 after the first curing is desirably 10 to 1000 Pa at 25° C., and particularly preferably 100 to 500 Pa. Unlike a liquid resin layer, a resin layer having a storage modulus in the range of 10 to 1000 Pa at 25° C. can easily maintain in-plane uniformity, and the curable resin layer can easily follow the irregularities of the microstructure.

[0068] When the obtained curable resin layer 12 is secondarily cured, for example, when the second curing is performed by a hydrosilylation reaction, the curing is preferably performed by heating in an environment of 20 to 200°C for 5 to 90 minutes, or when the second curing is performed by a photoradical polymerization reaction, the curing is preferably performed in a nitrogen environment with 365 nm light as an index at 50 to 3000 mW / cm. 2 and 100 to 20,000 mJ / cm 2 The second cured resin layer (e.g., a silicone-based resin layer) can be formed under curing conditions suitable for the curable silicone-based composition, such as by irradiating the composition with ultraviolet light at an integrated light amount of

[0069] Here, the curable resin layer 12 preferably has a storage modulus of 1 MPa to 30 GPa at 25°C after curing (secondary curing), and more preferably 4 MPa to 5 GPa. If the storage modulus at 25°C after secondary curing is 1 MPa or more, sufficient holding power for the microstructure can be ensured, and, for example, falling off during cleaning can be sufficiently suppressed. Furthermore, if the storage modulus at 25°C after secondary curing is 30 GPa or less, sufficient holding power can be exhibited to be applicable to the next process.

[0070] The curable resin layer 12 is preferably in a gel state, such as a silicone-based gel layer. A gel-like resin layer can more reliably prevent damage to the microstructure during laser lift-off. In the present invention, "gel-like" refers to a jelly-like state in which the liquid has lost its fluidity and has surface tackiness.

[0071] The curable resin layer 12 preferably has tackiness to the microstructure, which can further prevent the received microstructure from being displaced.

[0072] The hardness of the curable resin layer 12 is preferably increased by curing. If the hardness of the resin layer increases by curing, the positional deviation and tilt of the microstructure can be further suppressed after curing.

[0073] Alternatively, it is also preferable that the curable resin layer 12 has an adhesive strength to the microstructure or an increased holding power for the microstructure upon curing, which can further reduce the positional deviation or tilt of the microstructure after curing.

[0074] Alternatively, it is also preferable that the curable resin layer 12 becomes rubbery upon curing. If the resin layer becomes rubbery upon curing, it can further suppress the positional deviation and tilt of the microstructure after curing. In the present invention, "rubbery" means a state in which the resin layer exhibits resilience against loads and impacts and has excellent stretchability and elasticity.

[0075] Furthermore, the curable resin layer 12 may be cured into a resin cured product such as a high-hardness plastic, instead of a rubber-like material.

[0076] <Support Substrate> Examples of the support substrate 11 used in the receiving substrate 10 include a synthetic quartz glass substrate and float glass, with a synthetic quartz glass substrate being particularly preferred from the standpoints of flatness and transparency.

[0077] Furthermore, the size of the support substrate 11 used for the receiving substrate 10 is preferably the same as or larger than the diameter of the supply substrate (described in detail below) used. Specifically, when a sapphire substrate with an outer diameter of 10.16 cm (4 inches) is used as the supply substrate, a receiving substrate 10 with an outer diameter of 10.16 to 20.32 cm (4 to 8 inches) can be used.

[0078] In order to reliably transfer some or all of the multiple microstructures from the supply substrate to the receiving substrate 10, it is preferable that when the multiple microstructures formed on one side of the supply substrate are bonded to the receiving substrate 10 having a curable resin layer 12 on a support substrate 11, each microstructure is temporarily and uniformly fixed to the curable resin layer 12 of the receiving substrate 10.

[0079] In order to temporarily fix the microstructure with high precision, the support substrate 11 used for the receiving substrate 10 has a spatial frequency of 1 mm obtained by measuring an area of ​​6.01 mm x 6.01 mm with a pixel number of 1240 x 1240 using a white light interferometer. -1 The power spectral density above is 10 12 nm 4 In particular, when the minute structure is a micro LED, taking into consideration the distance between the minute structures, a spatial frequency of 10 mm obtained by measuring an area of ​​6.01 mm x 6.01 mm with a white light interferometer at a pixel count of 1240 x 1240 is preferably 10 mm or less. -1 More than 50 mm -1 The power spectral density at 9 nm 4 It is preferable that:

[0080] Furthermore, since the receiving substrate 10 temporarily fixes the microstructure with high precision, it is preferable that the supporting substrate 11 used for the receiving substrate 10 has a small thickness variation. For example, the thickness variation (TTV) measured by a wavelength conversion Fizeau flatness tester manufactured by Mizojiri Optical Industries Co., Ltd. is preferably 2 μm or less, more preferably 1 μm or less, and even more preferably 0.5 μm or less.

[0081] The microstructure to be held by the receiving substrate 10 of the present invention may be a microstructure having protrusions or a microstructure without protrusions.

[0082] [Method for manufacturing a receiving substrate] The receiving substrate of the present invention can be manufactured by the method for manufacturing a receiving substrate of the present invention, which will be described below with reference to Fig. 2. However, the receiving substrate of the present invention can also be manufactured by a method other than the method for manufacturing a receiving substrate of the present invention, which will be described below.

[0083] 2A, a substrate for preparing a receiving substrate (support substrate) 11 is prepared. For details of the support substrate to be used, see the previous description.

[0084] Next, as shown in FIG. 2B, a step of forming a layer 12a of at least two types of resin capable of undergoing a curing reaction on one surface of the support substrate 11 is carried out, thereby obtaining a composite 10a.

[0085] This step can include, for example, coating the support substrate 11 with at least two types of resin capable of undergoing a curing reaction.

[0086] The resin used here is not particularly limited as long as it is capable of undergoing at least two types of curing reactions, for example, the two-stage curing silicone composition described above can be used.

[0087] When the two-stage curing silicone composition described above is used as the resin capable of at least two types of curing reactions, the two-stage curing silicone composition may be applied to the support substrate 11 in any desired shape using spin coating, slit coating, screen printing, or the like. The thickness of the two-stage curing silicone composition may be determined as desired, taking into account the shape and thickness of the microstructure to be transferred, but is preferably 1 to 500 μm, more preferably 5 to 200 μm, and even more preferably 10 to 100 μm from the viewpoints of ease of application and maintaining uniformity in film thickness after curing. Furthermore, a support substrate 11 that has been pre-treated with a primer may be used to improve adhesion or bondability at the interface between the support substrate 11 and the curable silicone resin 12a.

[0088] Next, a first curing reaction (so-called primary curing) is carried out to partially cure the resin capable of at least two types of curing reactions in the resin layer 12a. This causes the resin layer 12a to undergo primary curing, becoming a curable resin layer 12. As a result, the receiving substrate 10 of the present invention shown in FIG. 2(C) can be obtained.

[0089] The curable resin layer 12 can be subjected to secondary curing. The curable resin layer 12 can become a second-cured resin layer 12b shown in Fig. 2(D) by secondary curing. That is, the receiving substrate 10b shown in Fig. 2(D) has a support substrate 11 and a second-cured resin layer 12b formed on the support substrate 11.

[0090] The at least two types of curing reactions (e.g., primary curing and secondary curing) described above can include, for example, a combination of a photocuring reaction and a thermal curing reaction, a combination of thermal curing reactions having different curing initiation temperatures, or a combination of photocuring reactions having different curing wavelengths.

[0091] In another aspect, the at least two types of cure reactions described above (e.g., primary cure and secondary cure) can include, for example, a combination of at least two selected from the group consisting of a radical cure system, a cationic cure system, an anionic cure system, an addition cure system, and a condensation cure system.

[0092] [Lifting Method] The lifting method of the present invention is a lifting method for transferring a microstructure formed on a supply substrate to a receiving substrate by laser lift-off. An example of the lifting method of the present invention will be described with reference to FIGS.

[0093] As the receiving substrate used in the lifting method of the present invention, the receiving substrate 10 of the present invention described above can be used.

[0094] A supply substrate that can be used in the present invention is, for example, a supply substrate 20 having a plurality of microstructures 100 formed on one surface of a support substrate 21, and having protrusions 130 on a surface 100A of the microstructures 100 facing the receiving substrate 10, as shown in Figure 3. In Figure 3, protrusions 130 such as bumps are formed on the element body 120 of the microstructure 100. Recesses 110 are formed between the protrusions 130. Note that by using the receiving substrate of the present invention described above, microstructures without protrusions can also be transferred by laser lift-off.

[0095] The support substrate 21 used in the supply substrate 20 may be, for example, a sapphire substrate, a GaAs substrate (gallium arsenide substrate), a Si substrate, or a SiC substrate, and may have any diameter.

[0096] Furthermore, examples of the microstructure 100 include elements obtained by providing a basic structure as a device on a support substrate 21 through processes carried out in typical semiconductor pre-processing steps such as epitaxial growth, ion implantation, wet etching, dry etching, vapor deposition, and electrode formation, and then separating the element by conventional methods such as blade dicing, dry etching, and laser dicing to a depth required to separate the element.

[0097] For example, if the microstructure is an LED, an LED epitaxial substrate is prepared by forming a buffer layer on a 10.16 cm (4 inch) sapphire substrate, forming a 3 μm N-type GaN layer, followed by a known light-emitting layer structure and stacking P-type GaN epitaxial layers for a total thickness of 4 μm. After that, the N-type layer is locally exposed by dry etching, and then a P-type electrode is formed on the P-type layer by a known process, so that the N-type electrode is in contact with the exposed N-type layer. A bump is then formed on the electrode by a method such as plating, vapor deposition, or sputtering. Then, to separate LED elements of a predetermined size, laser dicing is performed until it reaches at least the sapphire substrate and the elements are completely separated, thereby obtaining the microstructure.

[0098] The size of the microstructure 100 is arbitrary, but for example, in the case of a power LED, it is about 1 mm square. In addition, in the case of an LED element, it is about 300 μm square, in the case of a mini LED, it is about 100 μm square, in the case of a micro LED, it is about 60 μm square or less, and in the case of an extremely small micro LED, it is 30 μm square or less.

[0099] Although the shape of the microstructure 100 described above is an example of a substantially square, the present invention is not limited to this. For example, in the case of a micro LED, the shape may be a rectangle with one side measuring 30 to 60 μm and the other side measuring 10 to 30 μm.

[0100] The thickness of the microstructure 100 depends on the thickness of the epitaxial growth on the support substrate 21, and is not particularly limited, but is preferably about 3 to 10 μm.

[0101] Now, in the lifting method of this example, the receiving substrate 10 and the supply substrate 20 are aligned with each other so that the surface 10A of the curable resin layer 12 of the receiving substrate 10 onto which the microstructure 100 is transferred faces the protrusion 130 provided on the surface 100A of the microstructure 100 of the supply substrate 20, as shown in Figure 4 (A).

[0102] 4B, the microstructure 100 is pressed against the curable resin layer 12 so that the protrusions 130 are embedded in the curable resin layer 12, thereby obtaining the laminated substrate 30. This process can also be called bonding.

[0103] 4(C), the curable resin layer 12 is cured with the protrusions 130 embedded in the curable resin layer 12, thereby holding the microstructure 100 on the receiving substrate 10. This step can also be called a second curing.

[0104] In another example, the bonding of the plurality of microstructures 100 formed on one surface of the supply substrate 20 to the curable resin layer (e.g., a silicone-based resin layer) 12 on the receiving substrate 10 and the second curing can be performed, for example, as shown in Fig. 5. Note that protrusions of the microstructures 100 are not shown in Fig. 5.

[0105] In this example, after being aligned as shown in Figure 5(A), the entire receiving substrate 10 and the supply substrate 20 are bonded together while applying pressure so that the microstructure 100 on the supply substrate 20 and the curable resin layer 12 on the receiving substrate 10 face each other, as shown in Figure 5(B), to obtain a laminate 30.

[0106] Thereafter, as shown in FIG. 5C, the curable resin layer 12 is subjected to a second curing to increase the hardness of the second-cured resin layer 12b, thereby obtaining a laminated substrate 40.

[0107] 6 and 7 show details of FIG. 5(C). FIG. 7 is a schematic diagram of the microstructure 100 observed through the support substrate 11 of the laminated substrate 40 in the state of FIG. 6. The microstructure 100 to be transferred by the lifting method of the present invention has protrusions 130 as described above. In FIGS. 6 and 7, the protrusions 130 such as bumps are completely covered with the secondary-cured resin layer 12b. Therefore, the recesses 110 of the microstructure 100 shown in FIG. 3 are filled with the resin layer 12b.

[0108] If no air bubbles exist within the resin layer 12b within 5 μm around the protrusion 130, the protrusion 130 can be prevented from coming into contact with the cleaning solution during the cleaning process, and this can prevent changes in the components that make up the protrusion 130. The absence of air bubbles within the resin 12b within a 5 μm range from the protrusion 130 can be confirmed using, for example, a laser microscope.

[0109] It is preferable that pressure be applied during lamination so that no air bubbles remain between the curable resin layer 12 and the microstructure 100. For example, it is preferable to apply a load of 0.05 to 1.0 MPa, more preferably 0.10 to 0.5 MPa, to perform lamination. In addition, at this time, pressure may be applied under reduced pressure so that the curable resin layer 12 can easily follow the shape of the microstructure. Furthermore, if the second curing of the curable resin is caused by heating, heating may be performed simultaneously with lamination to perform the second curing.

[0110] The second curing of the curable resin layer 12 is preferably carried out in a heating furnace in an environment of 80 to 200°C for 5 to 90 minutes when the second curing is carried out by a hydrosilylation reaction, or in a nitrogen environment in which 365 nm light is used as an index, with an intensity of 50 to 3000 mW / cm when the second curing is carried out by a photoradical polymerization reaction. 2 and 100 to 20,000 mJ / cm 2 The second cured resin layer 12b is formed under curing conditions suitable for the curable silicone resin used, such as by irradiating the composition with ultraviolet light with an integrated light amount of 1000 kJ / cm 2 or more.

[0111] 4(D) and 8(A) (protrusions of the microstructure 100 are omitted), laser lift-off is performed using laser light L while the microstructure 100 is held on the receiving substrate 10. Laser lift-off performed in this state can also be called contact laser lift-off (CLLO).

[0112] More specifically, the laminated substrate 40 obtained by the lamination and secondary curing process is irradiated with pulsed laser light L, for example, from the surface of the supply substrate 20 opposite to the surface on which the microstructure 100 is formed, to peel the microstructure 100 from the support substrate 21. This allows the microstructure 100 to be transferred from the supply substrate 20 to the second-cured resin layer 12b on the receiving substrate 10.

[0113] In the LLO process, for example, when the microstructure 100 is a gallium nitride microstructure fixed to a support substrate 21 of a supply substrate 20 such as a sapphire substrate, the gallium nitride in the irradiated portion is melted by irradiation with laser light from an excimer laser, a YAG laser, or the like, thereby enabling the gallium nitride microstructure 100 to be peeled off from the supply substrate 20. In this case, it is preferable to use KrF excimer laser light, particularly for microLEDs, from the viewpoint of the reliability of the microstructure 100.

[0114] Specifically, laser light is selectively irradiated to cause laser ablation at the interface between the microstructure 100 to be selected and the support substrate 21 of the supply substrate 20. As a result, in the case of a gallium nitride microstructure, for example, gallium nitride decomposes into metallic gallium and nitrogen to generate gas between the microstructure 100 to be selected and the support substrate 21 of the supply substrate 20, so that the microstructure 100 can be peeled off relatively easily.

[0115] After all of the microstructures 100 to be transferred are similarly irradiated with the laser light L and transferred, the receiving substrate 10b on which the microstructures 100 have been transferred can be peeled off from the support substrate 21 of the supply substrate 20, as shown in Fig. 4(E) and Fig. 8(B) (protrusions of the microstructures 100 are omitted), for example. This allows the receiving substrate 10c holding the microstructures 100 to be obtained.

[0116] Since the supply substrate 20 and the microstructure 100 are separated by the LLO process, the supply substrate 20 can be easily peeled off using an appropriate jig.

[0117] With the lifting method of the present invention described above, laser lift-off is performed with the protrusions 130 of the microstructure 100 embedded in the curable resin layer 12, thereby preventing local stress from being applied to the microstructure 100 during laser lift-off. Therefore, with the lifting method of the present invention, even a microstructure 100 having protrusions 130 can be transferred from a supply substrate to a receiving substrate while preventing damage. Furthermore, the curable resin layer 12 of the receiving substrate 10 used in the lifting method of the present invention can be hardened and made highly hard while holding the microstructure 100. Therefore, with the lifting method of the present invention, the received microstructure 100 can be held on the receiving substrate 10 while suppressing misalignment and tilt.

[0118] The receiving substrate 10c may be used in the next step as it is, or may be used in the next step after undergoing a cleaning step using an acid or alkaline cleaning solution, or surface cleaning using oxygen plasma or argon plasma, as described below.

[0119] The microstructure 100 transferred onto the receiving substrate 10c via the lifting method of the present invention or further via the cleaning method described below can be mounted on a circuit board via a desired process, such as using a transfer stamp material described in Patent Document 1 or transferring the microstructure 100 again onto a polyimide layer. That is, the receiving substrate 10c can also be used as a supply substrate (donor substrate) that supplies the microstructure 100 to another substrate in another process.

[0120] [Holding Method] The bonding and secondary curing shown in Figures 4(B), 4(C), and 5 can also be referred to as the holding method of the present invention. That is, the holding method of the present invention for holding the microstructure 100 having the protrusions 130 on the receiving substrate 10 is a holding method in which the receiving substrate 10 has a curable resin layer 12 on the surface that holds the microstructure 100, the microstructure 100 is pressed against the curable resin layer 12 so that the protrusions 130 are embedded in the curable resin layer 12, and the curable resin layer 12 is cured in a state in which the protrusions 130 are embedded in the curable resin layer 12, thereby holding the microstructure 100 on the receiving substrate 10.

[0121] With this holding method, the protrusions 130 of the microstructure 100 are embedded in the curable resin layer 12, and the curable resin layer 12 is hardened, thereby preventing damage, misalignment, and tilting of the microstructure 100, and allowing the microstructure 100 to be held on the receiving substrate 10.

[0122] Furthermore, in the case of the receiving substrate of the present invention described above, even for microstructures that do not have protrusions, the contact surface of the microstructure can be pressed into the curable resin layer and the curable resin layer is then secondary cured, thereby making it possible to hold the microstructures that do not have protrusions on the receiving substrate of the present invention.

[0123] [Cleaning Method] In one aspect of the cleaning method of the present invention, after the microstructure 100 is received and transferred to the substrate 10 by the lift-off method of the present invention described above, the microstructure 100 is cleaned with an acid or alkaline cleaning solution.

[0124] In another aspect, the cleaning method of the present invention is a cleaning method for a microstructure 100 having protrusions 130, for example, as shown in Figure 3, in which the microstructure 100 is pressed against a curable resin layer 12, for example, as shown in Figure 5 (B), so that the protrusions 130 are embedded in the curable resin layer 12, and after the curable resin layer 12 is hardened, for example, as shown in Figures 6 and 7, the microstructure 100 is cleaned with an acid or alkaline cleaning solution in a state in which the protrusions 130 of the microstructure are covered tightly by the resin layer 12b and no air bubbles are present in the resin layer 12b within 5 μm around the protrusions 130.

[0125] The cleaning method of the present invention will be described in more detail below.

[0126] FIG. 9 shows an example of the cleaning method of the present invention, and schematically illustrates the state in which metal Ga is cleaned after the LLO step is completed and peeling is performed as shown in FIG.

[0127] In Figure 9(A), a second cured resin layer 12b holding the microstructure 100 is present on the receiving substrate 10c after the LLO process, and a metal (e.g., Ga) 140 is attached to the surface of the microstructure 100 opposite the resin layer 12b. Because the interface between the resin 12b and the microstructure 100 is in close contact, the receiving substrate 10c can be immersed or rinsed in an acid or alkaline cleaning solution, dissolving and removing the metal 140, as shown in Figure 9(B), to obtain a receiving substrate 10d with the transferred microstructure. Since the interface of the microstructure 100 on the resin 12b side is covered and held by the resin 12b, it is not affected by the acid or alkaline cleaning solution and is not evaporated during the cleaning process. The receiving substrate 10d can then be thoroughly washed with pure water and dried by air drying or other methods before being used in the next process.

[0128] In these cleaning steps, the microstructure 100 is held by the resin layer 12b and remains without falling off the surface of the resin 12b. Furthermore, by being held by the resin layer 12b, it is possible to suppress displacement and tilt.

[0129] In particular, in the example shown in Figure 9, the entire protrusion 130 of the microstructure 100 is covered with the resin layer 12b without any gaps, and there are no air bubbles in the resin 12b within 5 μm around the protrusion 130, so that the protrusion 130 can be prevented from being affected by acid or alkali during the cleaning process.

[0130] Furthermore, there is no air layer of 1 μm or more at the interface between the resin 12b and the element body 120 and the protrusion 130, and by subjecting them to the cleaning process in a state of close contact with each other, it is possible to prevent the composition of the interface of the element body 120 on the resin layer 12b side, and if the protrusion 130 is a bump, the composition of the bump from being affected, and the element can be used in the next process without any problems.

[0131] The cleaning solution used in this cleaning step can be an acid cleaning solution obtained by uniformly mixing concentrated hydrochloric acid, concentrated nitric acid, concentrated sulfuric acid, or the like with pure water in any ratio, or multiple aqueous acids can be used. In this case, the pH of the cleaning solution is preferably 0 to 4.0. A pH within this range allows for sufficient solubility of the metal (e.g., Ga) 140.

[0132] In addition, in the case of an alkaline cleaning solution, sodium hydroxide, potassium hydroxide, ammonium hydroxide, magnesium hydroxide, tetramethylammonium hydroxide, tetrabutylammonium hydroxide, sodium carbonate, sodium bicarbonate, or potassium acetate dissolved in pure water at any concentration can be used, and multiple alkaline cleaning solutions can also be used. In this case, the pH of the cleaning solution is preferably 9.5 to 14.0, and a pH within this range allows for sufficient solubility of the metal (e.g., Ga) 140.

[0133] As explained above, the receiving substrate of the present invention can also hold a microstructure without protrusions. Therefore, in a modified example of the cleaning method of the present invention, a microstructure without protrusions can also be cleaned while being held by the receiving substrate of the present invention.

[0134] The present invention described above can be applied to the manufacturing process of LED displays intended for use in signage, TVs, medical applications, in-vehicle displays, smartphones, and the like.

[0135] EXAMPLES The present invention will be specifically explained below using examples and comparative examples, but the present invention is not limited to these.

[0136] Supply substrates equipped with the following microstructures were prepared: <Supply substrate A and microstructure A> A sapphire substrate cut into a 1.5 cm square measuring 90 × 140 μm, a total thickness of 19 μm, and equipped with a mini LED element having a bump height of 7 μm. <Supply substrate B and microstructure B> A sapphire substrate cut into a 1.5 cm square measuring 18 × 36 μm, a total thickness of 9 μm, and equipped with a micro LED element having a bump height of 4 μm.

[0137] The following was prepared as a support substrate for the receiving substrate: <Support substrate used for receiving substrate> A synthetic quartz substrate having an outer diameter of 15.24 cm (6 inches), a thickness of 1 mm, and a total thickness variation (TTV) of 0.8 μm.

[0138] <Experimental Contents: Examples 1 to 5> [Preparation of Receiving Substrate] 3 g of the following two-stage curing silicone resin composition (Silicone A or B) was dropped onto a supporting substrate, and the composition was uniformly coated onto the supporting substrate using a spin coater to a film thickness of 30 μm. The resulting coating was subjected to the following first curing conditions to primarily cure the silicone resin composition into a gel state, thereby preparing a receiving substrate having a curable silicone resin.

[0139] [Bonding] The supply substrate and the receiving substrate were bonded together under pressure of 0.5 MPa so that the microstructures on the supply substrate, as shown in Table 1 below, came into contact with the curable silicone resin on the receiving substrate. The curable silicone resin was then subjected to secondary curing under the conditions shown below. A laser microscope was then used to check whether there were any air gaps of up to 1 μm or more between the supply substrate and the microstructures and the secondary cured silicone resin, and whether there were any air bubbles in the resin within 5 μm of the periphery of the protrusions.

[0140] [LLO and Peeling-Off] Next, LLO was performed by irradiating the microstructure with KrF excimer laser light from the rear surface of the supply substrate, and then the supply substrate was peeled off from the receiving substrate.

[0141] After peeling, the transfer rate and breakage rate of the microstructures from the supply substrate onto the receiving substrate were evaluated, and the results are shown in Table 1 below.

[0142] Thereafter, the surface of the microstructure was immersed for 3 minutes in an acid or alkaline cleaning solution shown below and in Table 1 for cleaning. Next, the process of immersing for 3 minutes in pure water for cleaning was repeated twice, and the structure was air-dried.

[0143] After air drying, the microstructures were checked for tilt and falling off. The results are shown below.

[0144] Acidic cleaning solution: 12% by mass hydrochloric acid aqueous solution Alkaline cleaning solution: 5% by mass potassium hydroxide aqueous solution

[0145] [Measurement of Elastic Modulus] The dynamic viscoelastic properties of the silicone gel cured product of the present invention are defined by a characteristic frequency and a storage modulus G' at a specific temperature. Measurements were performed using an ARES G-II viscoelasticity measuring device manufactured by TA Instruments. A silicone resin cured and molded to a size of 3 cm square and 500 μm thick was sandwiched between the circular measuring section of the testing device and a 20 mm diameter parallel plate, taking care not to trap air bubbles. The strain was measured for 10 minutes at a strain of 4% and a frequency of 1 Hz while maintaining a temperature of 25°C. The value 10 minutes after the start of measurement was read as the storage modulus G'. Measurements were also performed on the silicone resin after the second cure using the same procedure and conditions. The results are shown below.

[0146] Silicone A: First cured by addition reaction in an environment of 120°C x 1 h, becoming a gel with a storage modulus G' of 0.2 kPa, and then cured with 365 nm UV-LED 3000 mJ / cm under nitrogen. 2 (Illuminance: 100mW / cm 2 ) to undergo a photoradical reaction, resulting in a second cure, and becoming a rubber-like composition with a storage modulus G' of 8.2 MPa.

[0147] Silicone B: 365 nm UV-LED 3000 mJ / cm under nitrogen 2 (Illuminance: 100mW / cm 2) to undergo a photoradical reaction, resulting in a first cure, forming a gel-like substance with a storage modulus G' of 5 kPa, and then undergoing an addition reaction at 120°C for 1 hour, resulting in a second cure, forming a rubber-like substance with a storage modulus G' of 4 GPa.

[0148] <Experimental Contents: Comparative Examples 1 to 4> The transfer rate, breakage rate, and positional deviation of the microstructure in the LLO process, as well as tilt and detachment of the microstructure in the cleaning process, were confirmed by the same process as in the Examples, except that a receiving substrate was prepared by curing the silicone composition (silicone C) shown below into a rubber state under only a single curing condition. In other words, the receiving substrates used in Comparative Examples 1 to 4 did not have a curable resin layer.

[0149] The elastic modulus of the rubber-cured Silicone C was measured using the procedure described above.

[0150] Silicone C: A heat-curable silicone composition that hardens by addition reaction in an environment of 120°C for 1 hour, becoming a rubber-like composition with a storage modulus G' of 4.7 MPa.

[0151]

[0152] Also, Figure 10 shows photographs of the microstructure after transfer by LLO in Example 1 (Figure 10(A)), the microstructure after peeling following this transfer (Figure 10(B)), and the microstructure after cleaning following this peeling (Figure 10(C)).

[0153] The appearance of the microstructure after transfer by LLO in each of Examples 2 to 5, the microstructure after peeling following this transfer, and the microstructure after cleaning following this peeling were similar to those shown in Figures 10(A), 10(B), and 10(C).

[0154] As is clear from the results shown in Table 1 above and Figure 10, in Examples 1 to 5, the microstructures having protrusions were able to be transferred from the supply substrate to the receiving substrate at a transfer rate of 99% or more without damage or misalignment.

[0155] Furthermore, as is clear from the results shown in Table 1 above and FIG. 10, in Examples 1 to 5, neither falling off nor tilting of the minute structures was observed after cleaning.

[0156] These results are due to the fact that in Examples 1 to 5, the primarily cured silicone-based resin layer received the microstructure with its protrusions embedded in the primarily cured silicone-based resin layer, and the silicone-based resin layer was then secondarily cured in this state to increase its hardness, which allowed the secondarily cured silicone-based resin layer to adequately hold the microstructure, thereby preventing damage, detachment, misalignment, and tilting of the microstructure during the transfer, peeling, and cleaning processes using the LLO.

[0157] On the other hand, in Comparative Examples 1 to 4, a hardened rubber-like material was used, and a receiving substrate having a hardenable resin was not used, resulting in a breakage rate of 5% or more. Furthermore, in Comparative Examples 1 and 2, positional deviation of the microstructure was also confirmed. Furthermore, as is clear from the results shown in Table 1, tilting of the microstructure was observed after cleaning in Comparative Examples 1 to 4.

[0158] Furthermore, as a reference example, except that secondary curing of the curable resin layer was not performed during LLO, LLO, peeling, and cleaning were performed in the same manner as in Example 1. Figure 11 shows photographs of the microstructure after transfer by LLO in the reference example (Figure 11(A)), the microstructure after peeling following this transfer (Figure 11(B)), and the microstructure after cleaning following this peeling (Figure 11(C)).

[0159] In the reference example, the microstructures were misaligned during LLO and the transfer rate was low. Furthermore, in the reference example, cracks occurred in the microstructures that were not placed on the secondary-cured silicone-based resin layer during LLO.

[0160] Furthermore, in the reference example, as is clear from FIGS. 11B and 11C, the microstructures were observed to fall off, shift in position, or become tilted due to peeling and cleaning.

[0161] This specification includes the following aspects. [1] A receiving substrate for transferring and receiving a microstructure formed on a supply substrate by laser lift-off, the receiving substrate having a curable resin layer on the surface onto which the microstructure is transferred. [2] The receiving substrate according to [1], wherein the curable resin layer is photocurable or thermosetting. [3] The receiving substrate according to [1] or [2], wherein the curable resin layer is in a B-stage state. [4] The receiving substrate according to any one of [1] to [3], wherein the curable resin layer is in a gel state. [5] The receiving substrate according to any one of [1] to [4], wherein the curable resin layer is a silicone-based gel layer. [6] The receiving substrate according to any one of [1] to [5], wherein the curable resin layer has tackiness to the microstructure. [7] The receiving substrate according to any one of [1] to [6], wherein the curable resin layer increases in hardness upon curing. [8] The receiving substrate according to any one of [1] to [7], wherein the curable resin layer increases its adhesive strength to the microstructure or its holding strength for the microstructure upon curing. [9] The receiving substrate according to any one of [1] to [8], wherein the curable resin layer becomes rubbery upon curing.

[10] The receiving substrate according to any one of [1] to [9], wherein the curable resin layer has a storage modulus of 10 to 1000 Pa at 25°C and 1 MPa to 30 GPa upon curing.

[11] A method for manufacturing a receiving substrate having a curable resin layer, comprising the steps of forming a layer of a resin capable of at least two types of curing reactions on one side of a receiving substrate preparation substrate, and partially curing the resin by carrying out the first type of curing reaction.

[12] The method for manufacturing a receiving substrate according to

[11] , wherein the at least two types of curing reactions include a combination of a photocuring reaction and a thermal curing reaction, a combination of thermal curing reactions having different curing onset temperatures, or a combination of photocuring reactions having different curing wavelengths.

[13] The method for manufacturing a receiving substrate according to

[11] or

[12] , wherein the at least two types of curing reactions include a combination of at least two selected from the group consisting of a radical curing system, a cationic curing system, an anionic curing system, an addition curing system, and a condensation curing system.

[14] A lifting method for transferring a microstructure formed on a supply substrate to a receiving substrate by laser lift-off, wherein the surface of the microstructure facing the receiving substrate has protrusions, and the surface of the receiving substrate onto which the microstructure is transferred has a curable resin layer, the microstructure is pressed against the curable resin layer so that the protrusions are embedded in the curable resin layer, the curable resin layer is cured with the protrusions embedded in the curable resin layer to hold the microstructure on the receiving substrate, and laser lift-off is performed with the microstructure held on the receiving substrate.

[15] A holding method for holding a microstructure having protrusions on a receiving substrate, wherein the receiving substrate has a curable resin layer on a surface that holds the microstructure, the microstructure is pressed against the curable resin layer so that the protrusions are embedded in the curable resin layer, and the curable resin layer is cured with the protrusions embedded in the curable resin layer to hold the microstructure on the receiving substrate.

[16] A method for cleaning a microstructure, comprising transferring the microstructure to the receiving substrate by the lift-off method described in

[14] , and then cleaning the microstructure with an acid or alkaline cleaning solution.

[17] A method for cleaning a microstructure having protrusions, comprising pressing the microstructure against a curable resin layer so that the protrusions are embedded in the curable resin layer, and after curing the curable resin layer, cleaning the microstructure with an acid or alkaline cleaning solution in a state where the protrusions of the microstructure are covered tightly by the resin layer and there are no air bubbles in the resin layer within 5 μm around the protrusions.

[0162] The present invention is not limited to the above-described embodiments, which are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that provides similar effects is included within the technical scope of the present invention.

Claims

1. A receiving substrate for transferring and receiving a microstructure formed on a supply substrate by laser lift-off, the receiving substrate having a curable resin layer on the surface onto which the microstructure is transferred.

2. The receiving substrate according to claim 1, wherein said curable resin layer is photocurable or thermosetting.

3. The receiving substrate according to claim 1, wherein said curable resin layer is in a B-stage state.

4. The receiving substrate according to claim 1, wherein said curable resin layer is in a gel state.

5. The receiving substrate according to claim 1, wherein said curable resin layer is a silicone-based gel layer.

6. The receiving substrate according to claim 1, wherein said curable resin layer has tackiness to said minute structure.

7. The receiving substrate according to claim 1, wherein the hardening resin layer increases in hardness upon curing.

8. The receiving substrate according to claim 1, wherein the curable resin layer increases its adhesive strength to the minute structure or its holding power for the minute structure upon curing.

9. The receiving substrate according to claim 4, wherein said curable resin layer becomes rubbery upon curing.

10. The receiving substrate according to claim 4, wherein the storage modulus of said curable resin layer is 10 to 1000 Pa at 25° C. and becomes 1 MPa to 30 GPa upon curing.

11. A method for producing a receiving substrate having a curable resin layer, comprising: forming a layer of a resin capable of undergoing at least two types of curing reactions on one surface of a substrate for producing a receiving substrate; and partially curing the resin by carrying out the first type of curing reaction.

12. The method for manufacturing a receiving substrate according to claim 11, wherein the at least two types of curing reactions include a combination of a photocuring reaction and a thermal curing reaction, a combination of thermal curing reactions having different curing initiation temperatures, or a combination of photocuring reactions having different curing wavelengths.

13. The method for producing a receiving substrate according to claim 11, wherein the at least two types of curing reactions include a combination of at least two selected from the group consisting of a radical curing system, a cationic curing system, an anionic curing system, an addition curing system, and a condensation curing system.

14. A lifting method for transferring a microstructure formed on a supply substrate to a receiving substrate by laser lift-off, wherein the surface of the microstructure facing the receiving substrate has a protrusion, the surface of the receiving substrate onto which the microstructure is transferred has a curable resin layer, the microstructure is pressed against the curable resin layer so that the protrusion is embedded in the curable resin layer, the curable resin layer is cured with the protrusion embedded in the curable resin layer, thereby holding the microstructure on the receiving substrate, and laser lift-off is performed with the microstructure held on the receiving substrate.

15. A holding method for holding a microstructure having protrusions on a receiving substrate, wherein the receiving substrate has a curable resin layer on the surface that holds the microstructure, the microstructure is pressed against the curable resin layer so that the protrusions are embedded in the curable resin layer, and the curable resin layer is hardened while the protrusions are embedded in the curable resin layer, thereby holding the microstructure on the receiving substrate.

16. A method for cleaning a microstructure, comprising transferring the microstructure to the receiving substrate by the lifting method according to claim 14, and then cleaning the microstructure with an acid or alkaline cleaning solution.

17. A method for cleaning a microstructure having protrusions, comprising pressing the microstructure against a curable resin layer so that the protrusions are embedded in the curable resin layer, and after the curable resin layer has hardened, cleaning the microstructure with an acid or alkaline cleaning solution in a state in which the protrusions of the microstructure are tightly covered by the resin layer and there are no air bubbles in the resin layer within 5 μm of the periphery of the protrusions.